Ferritic stainless steel sheet, its manufacturing method, and exhaust part
A ferritic stainless steel sheet with controlled composition and processing enhances high-temperature strength and manufacturability by suppressing Laves phase formation, addressing the deterioration issues in existing ferritic stainless steels.
Patent Information
- Application Number
- JP2020151130
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-09
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-09-09
AI Technical Summary
Ferritic stainless steel used in exhaust system parts experiences deterioration in high-temperature strength due to the formation of a precipitated phase called a Laves phase, leading to thermal fatigue and reduced manufacturability.
A ferritic stainless steel sheet with controlled chemical composition and metallographic structure, including specific limits on alloying elements and controlled precipitation of Nb-containing second phases, is produced through hot rolling, cold rolling, and annealing processes to suppress the formation of coarse Laves phases and enhance precipitation strengthening.
The solution effectively maintains high-temperature strength and manufacturability by preventing the coarsening of precipitates, ensuring the steel sheet retains strength even under prolonged exposure to high temperatures.
Smart Images

Figure 0007564664000001 
Figure 0007564664000002 
Figure 0007564664000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a ferritic stainless steel sheet, a manufacturing method thereof, and an exhaust part. [Background technology]
[0002] In recent years, stainless steels have come to be widely used in exhaust system parts such as exhaust manifolds, front pipes, and center pipes, in view of strengthening automobile exhaust gas regulations, improving engine performance, and reducing vehicle weight. Although these exhaust system parts vary depending on the type of vehicle or engine structure used, they are exposed to high-temperature exhaust gases at approximately 700 to 800°C. For this reason, materials used in exhaust parts are required to have a variety of properties, such as high-temperature strength, oxidation resistance, and thermal fatigue properties.
[0003] Among exhaust system parts, for example, if stainless steel with a large thermal expansion coefficient is used for parts that are repeatedly heated and cooled, such as exhaust manifolds, thermal fatigue failure is likely to occur due to thermal expansion and thermal contraction. For this reason, ferritic stainless steel, which is relatively inexpensive among stainless steels and has a small thermal expansion coefficient and good thermal fatigue properties, is sometimes used for exhaust parts.
[0004] On the other hand, ferritic stainless steels are inferior in high-temperature strength compared to other stainless steels, such as austenitic stainless steels. Therefore, in order to improve high-temperature strength, ferritic stainless steels have been developed to which alloy elements such as Nb, Mo, W, and Ti, which contribute to solid solution strengthening and precipitation strengthening, have been added. For example, the high-temperature strength of general-purpose steels SUS430J1 and SUS444 has been improved by adding Nb. In addition, the ferritic stainless steels disclosed in Patent Documents 1 to 6 have been improved by adding W. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2009-215648 A [Patent Document 2] JP 2009-235555 A [Patent Document 3] JP 2005-206944 A [Patent Document 4] JP 2008-189974 A [Patent Document 5] JP 2009-120893 A [Patent Document 6] JP 2009-120894 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, as disclosed in Patent Documents 1 to 6, when the above-mentioned alloy elements are added, there is a problem that the alloy elements form a precipitation phase called a Laves phase in a high-temperature environment, and the high-temperature strength deteriorates over time. In addition, cracks may occur during hot working, which may reduce manufacturability.
[0007] The present invention aims to solve the above problems and to provide a ferritic stainless steel sheet that suppresses deterioration of high-temperature strength even when exposed to high temperatures for long periods of time and has good manufacturability, a manufacturing method therefor, and an exhaust component. [Means for solving the problem]
[0008] The present invention has been made to solve the above problems, and the gist of the present invention is the following ferritic stainless steel sheet.
[0009] (1) Chemical composition, in mass%, C: 0.001 to 0.030%, N: 0.001 to 0.030%, Si: 2.00-4.00%, Mn: 0.01 to 2.00%, P: 0.010~0.050%, S: 0.0001 to 0.010%, Cr: 10.0-30.0%, Nb: 0.01 to 0.80%, Ti: 0 to 0.50%, B: 0~0.0009%, Al: 0-2.5%, Cu: 0-3.0%, Mo: 0-3.0%, W: 0 to 0.50%, V: 0~1.0%, Sn: 0-0.50%, Ni: 0-1.0%, Mg: 0 to 0.01%, Sb: 0-0.50%, Zr: 0-0.30%, Ta: 0 to 0.30%, Hf: 0~0.30%, Co: 0-0.30%, Ca: 0-0.01%, REM: 0~0.20%, Ga: 0 to 0.30%, The balance is Fe and impurities. In metal structure, The average crystal grain size of the matrix is 100 to 200 μm, When the second phase containing Nb is referred to as the Nb-containing second phase, A ferritic stainless steel sheet, in which the amount of precipitation of the Nb-containing second phase measured by extraction residue analysis is 0.15% by mass or less.
[0010] (2) The chemical composition is, in mass%, Ti: 0.01 to 0.50%, B: 0.0001~0.0009%, Al: 0.01-2.5%, Cu: 0.01-3.0%, Mo: 0.01-3.0%, W: 0.01 to 0.50%, V: 0.05-1.0%, Sn: 0.003-0.50%, Ni: 0.05 to 1.0%, Mg: 0.0002~0.01%, Sb: 0.0001 to 0.50%, Zr: 0.001 to 0.30%, Ta: 0.001 to 0.30%, Hf: 0.001~0.30%, Co: 0.01 to 0.30%, Ca: 0.0002-0.01%, REM: 0.001-0.20%, and Ga: 0.0002 to 0.30%, The ferritic stainless steel sheet according to the above (1), comprising one or more selected from the following:
[0011] (3) When aging heat treatment was performed at 750℃ for 100 hours, The amount of precipitation of the Nb-containing second phase measured by extraction residue analysis is 0.20% or more by mass%, The average particle size of the Nb-containing second phase is 200 nm or less, The ferritic stainless steel sheet according to (1) or (2) above, wherein the proportion of M6C carbides in the entire second phase is 50% or more by mass.
[0012] (4) A method for producing a ferritic stainless steel sheet according to any one of (1) to (3) above, (a) hot rolling a steel having the chemical composition described in (1) or (2) above to obtain a hot-rolled sheet; (b) coiling the hot-rolled sheet in a temperature range of 400 to 750 ° C.; (c) cold rolling the coiled hot-rolled sheet to obtain a cold-rolled sheet; (d) heating the cold-rolled sheet to a temperature range of 1100 to 1200°C, and then performing an annealing treatment by retaining the cold-rolled sheet in the temperature range for 30 seconds to 3 minutes.
[0013] (5) An exhaust part using the ferritic stainless steel sheet according to any one of (1) to (3) above. Effect of the Invention
[0014] According to the present invention, it is possible to obtain a ferritic stainless steel sheet, a manufacturing method, and an exhaust part that suppress deterioration of high-temperature strength even when exposed to high temperatures for a long period of time and have good manufacturability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present inventors have investigated the deterioration of high-temperature strength of ferritic stainless steel sheets and have obtained the following findings (a) to (c).
[0016] (a) The decrease in high-temperature strength due to the precipitation of the Laves phase is due to the following reasons. Normally, if the Laves phase is present at the stage of product shipment, it can cause a deterioration in toughness. For this reason, the above alloying elements are dissolved in the matrix by heat treatment, so that the Laves phase does not precipitate. On the other hand, when exposed to high temperatures of 600°C or higher in the usage environment, the above elements that were dissolved in the matrix form the Laves phase together with other elements.
[0017] In this way, the precipitation of the Laves phase reduces the amount of the alloying elements that contribute to solid solution strengthening in the parent phase, and the precipitation strengthening ability is reduced. In addition, when the precipitation state of the Laves phase is coarse and coarse, precipitation strengthening, more specifically, particle dispersion strengthening, does not occur. As a result, it is thought that the high-temperature strength is reduced. In particular, when the precipitation stability of the Laves phase is poor, the high-temperature strength in the usage environment is significantly deteriorated.
[0018] (b) Regarding this point, the inventors considered that even when alloying elements are contained, it is possible to suppress a decrease in high-temperature strength by controlling the Laves phase to precipitate in a manner that is unlikely to grow coarsely and by causing the Laves phase to precipitate finely within crystal grains.
[0019] (c) In the case of steel containing Nb, it was revealed that by appropriately controlling the Si content and the annealing conditions after cold rolling, a second phase containing Nb precipitates finely in the operating environment. The reason for this is due to the following mechanism.
[0020] During hot rolling and annealing after hot rolling, a second phase containing Nb is precipitated, but in the subsequent annealing process after cold rolling, the annealing temperature is increased to dissolve the second phase. As a result, the crystal grain size increases, the precipitation of the second phase at the grain boundaries is suppressed, and precipitation within the grains, which is effective for precipitation strengthening, is promoted.
[0021] Since element diffusion is slower within grains than at grain boundaries, precipitates are less likely to grow. This helps to prevent deterioration of high-temperature strength when used as a part. In addition, the second phase containing Nb that precipitates during use exists finely within the grains at high temperatures, effectively achieving precipitation strengthening. This is also expected to improve high-temperature strength.
[0022] The present invention has been made based on the above findings. Each of the features of the present invention will be described in detail below.
[0023] 1.Chemical composition The reasons for limiting the content of each element are as follows. In the following description, "%" for the content means "mass %."
[0024] C: 0.001 to 0.030% C deteriorates formability and corrosion resistance, and reduces high-temperature strength. For this reason, the C content is set to 0.030% or less. The C content is preferably set to 0.009% or less, and more preferably set to 0.007% or less. The lower the C content, the better. However, excessive reduction of C leads to an increase in refining costs, so the C content is set to 0.001% or more. The C content is preferably set to 0.003% or more.
[0025] N: 0.001 to 0.030% Like C, N deteriorates formability and corrosion resistance, and reduces high-temperature strength. For this reason, the N content is set to 0.030% or less. The N content is preferably set to 0.020% or less, and more preferably set to 0.015% or less. The lower the N content, the better. However, excessive reduction of N leads to an increase in refining costs, so the N content is set to 0.001% or more. The N content is preferably set to 0.003% or more, and more preferably set to 0.005% or more.
[0026] Si: 2.00-4.00% Silicon is a useful element as a deoxidizer, and also improves high-temperature strength, oxidation resistance, and high-temperature salt damage resistance. High-temperature strength, oxidation resistance, and high-temperature salt damage resistance improve with increasing Si content. In order to improve high-temperature strength, it is important to control the precipitation of precipitates, and this effect can be obtained by precipitating fine precipitates in large quantities. Silicon has the effect of precipitating fine precipitates during aging heat treatment, and this effect is stably expressed from 2.00%. For this reason, the Si content is set to 2.00% or more.
[0027] However, excessive Si content reduces room temperature ductility. Therefore, the Si content is set to 4.00% or less. In consideration of pickling properties and toughness, the Si content is preferably set to 2.90% or less. In consideration of manufacturability, the Si content is more preferably set to 2.80% or less.
[0028] Mn: 0.01 to 2.00% Mn is a useful element as a deoxidizer and also contributes to improving high-temperature strength in the medium temperature range. For this reason, the Mn content is set to 0.01% or more. However, if the Mn content exceeds 2.00%, Mn-based oxides are formed on the surface at high temperatures, which reduces scale adhesion and makes abnormal oxidation more likely to occur. In particular, when Mn is added in combination with Mo and W, abnormal oxidation tends to occur more easily depending on the Mn content. For this reason, the Mn content is set to 2.00% or less. Considering the pickling properties and room temperature ductility in steel sheet manufacturing, the Mn content is preferably set to 1.50% or less, and more preferably 1.00% or less.
[0029] P: 0.010~0.050% P is an impurity that is mainly mixed in from the raw materials during steel refining, and if the content is high, toughness and weldability decrease. In particular, if the P content exceeds 0.050%, the steel plate becomes significantly hard, and the corrosion resistance, toughness, and pickling properties deteriorate. For this reason, the P content is set to 0.050% or less. The P content is set to 0.040% or less. The lower the P content, the better, but if the P content is less than 0.010%, raw materials with a reduced P content must be used, resulting in increased costs. For this reason, the P content is set to 0.010% or more. It is more preferable that the P content is set to 0.020% or more.
[0030] S: 0.0001 to 0.010% S combines with Ti and / or C to improve workability. This effect is manifested from a content of 0.0001%, so the S content is set to 0.0001% or more. However, S deteriorates corrosion resistance and oxidation resistance. In addition, excessive S content reduces the amount of dissolved Ti and coarsens precipitates by combining with Ti and / or C. As a result, high-temperature strength is reduced. For this reason, the S content is set to 0.010% or less. Furthermore, in consideration of refining costs and high-temperature oxidation properties, the S content is preferably set to 0.0010 to 0.009%.
[0031] Cr: 10.0~30.0% Cr is an element necessary for ensuring oxidation resistance and corrosion resistance. It is also effective in improving high-temperature strength. For this reason, the Cr content is set to 10.0% or more. However, if the Cr content exceeds 30.0%, it will cause a decrease in workability and toughness. For this reason, the Cr content is set to 30.0% or less. The Cr content is preferably set to 18.0% or less. In consideration of manufacturability and scale spalling property, the Cr content is preferably set to 13.0 to 18.0%.
[0032] Nb: 0.01 to 0.80% Nb is an element effective in improving high-temperature strength by solid solution strengthening and precipitation strengthening of fine precipitates. It also fixes C and N as carbonitrides, improves the corrosion resistance of the product sheet, and has the effect of developing a recrystallized texture that affects the r-value. For this reason, the Nb content is set to 0.01% or more. The Nb content is preferably set to 0.30% or more. However, if the Nb content exceeds 0.80%, the steel sheet becomes significantly hard and the manufacturability is also deteriorated. For this reason, the Nb content is set to 0.80% or less. In consideration of the raw material cost and toughness, the Nb content is preferably set to 0.60% or less, and more preferably set to 0.50% or less.
[0033] In addition to the above elements, one or more elements selected from Ti, B, Al, Cu, Mo, W, V, Sn, Ni, Mg, Sb, Zr, Ta, Hf, Co, Ca, REM, and Ga may be contained within the ranges shown below. The reasons for limiting each element will be explained.
[0034] Ti: 0 to 0.50% Ti is an element that combines with elements such as C, N, and S to improve corrosion resistance, intergranular corrosion resistance, room temperature ductility, and deep drawability. In addition, when Ti is added in combination with Nb and Mo, the amount of solid solution of Nb and Mo during cold rolling annealing is increased, high temperature strength is improved, and thermal fatigue properties are improved. For this reason, Ti may be added as necessary. However, if Ti is added at more than 0.50%, the amount of solid solution Ti increases and room temperature ductility decreases. In addition, coarse Ti-based precipitates are formed, which become the starting point of cracks during hole expansion processing, and press workability is deteriorated. In addition, oxidation resistance is also deteriorated. Therefore, the Ti content is set to 0.50% or less. In addition, considering the occurrence of surface defects and toughness, the Ti content is preferably set to 0.25% or less. On the other hand, in order to obtain the above effect, the Ti content is preferably set to 0.01% or more. It is more preferable that the Ti content is set to 0.05% or more.
[0035] B: 0 to 0.0009% B has the effect of improving the secondary workability, high-temperature strength, and thermal fatigue properties during press working of the product. In addition, B causes fine precipitation of Laves phases, etc., and exhibits long-term stability of strengthening by these precipitates, suppressing strength reduction and improving thermal fatigue life. For this reason, B may be contained as necessary. However, excessive B content causes hardening of the steel sheet, deteriorating intergranular corrosion resistance and oxidation resistance. In addition, weld cracks occur. Therefore, the B content is set to 0.0009% or less. Considering corrosion resistance and manufacturing costs, the B content is preferably set to 0.0005% or less. On the other hand, in order to obtain the above effects, the B content is preferably set to 0.0001% or more.
[0036] Al: 0-2.5% Al has a deoxidizing effect. It also has the effect of improving oxidation resistance. It also has the effect of improving high-temperature strength as a solid solution strengthening element. For this reason, it may be contained as necessary. However, if Al is contained in excess, the steel sheet becomes hard, and the uniform elongation is significantly reduced, as well as the toughness is significantly reduced. Therefore, the Al content is set to 2.5% or less. Furthermore, in consideration of the occurrence of surface defects, weldability, and manufacturability, the Al content is preferably set to 2.2% or less, and more preferably to 0.5% or less. On the other hand, in order to obtain the above effects, the Al content is preferably set to 0.01% or more.
[0037] Cu: 0-3.0% Cu has the effect of improving corrosion resistance. It also has the effect of improving high-temperature strength by precipitation strengthening due to the precipitation of ε-Cu. Therefore, it may be contained as necessary. However, if Cu is contained in excess, hot workability decreases. Therefore, the Cu content is set to 3.0% or less. In addition, in consideration of thermal fatigue properties, manufacturability, and weldability, the Cu content is preferably set to 1.6% or less. On the other hand, in order to obtain the above effects, the Cu content is preferably set to 0.01% or more.
[0038] Mo: 0-3.0% Mo is an element effective for solid solution strengthening at high temperatures, and also has the effect of improving corrosion resistance and high-temperature salt damage resistance. Therefore, it may be contained as necessary. However, if Mo is contained in an amount exceeding 3.0%, room temperature ductility and oxidation resistance are significantly deteriorated. For this reason, the Mo content is set to 3.0% or less. In consideration of thermal fatigue properties and manufacturability, the Mo content is preferably set to 0.9% or less. On the other hand, in order to obtain the above effects, the Mo content is preferably set to 0.01% or more.
[0039] W: 0~0.50% Like Mo, W is an effective element for solid solution strengthening at high temperatures, and also produces a Laves phase (Fe2W) to bring about the effect of precipitation strengthening. In particular, when added in combination with Nb and Mo, the Laves phase of Fe2(Nb,Mo,W) precipitates, but the inclusion of W suppresses the coarsening of the Laves phase and improves the precipitation strengthening ability. Therefore, it may be included as necessary. However, if W is included in an amount exceeding 0.50%, the manufacturing cost increases and the room temperature ductility decreases. For this reason, the W content is set to 0.50% or less. Furthermore, in consideration of manufacturability, low temperature toughness, and oxidation resistance, the W content is preferably set to 0.40% or less, and more preferably set to 0.20% or less. On the other hand, in order to obtain the above effect, the W content is preferably set to 0.01% or more.
[0040] V: 0 to 1.0% V has the effect of improving corrosion resistance. Therefore, it is preferable to include V as necessary. However, if V is included in an amount exceeding 1.0%, the precipitates become coarse, the high-temperature strength decreases, and the oxidation resistance deteriorates. Therefore, the V content is set to 1.0% or less. In consideration of the manufacturing cost and manufacturability, the V content is preferably set to 0.5% or less. On the other hand, in order to obtain the above effect, the V content is preferably set to 0.05% or more. The V content is more preferably set to 0.08% or more.
[0041] Sn: 0 to 0.50% Sn has the effect of improving corrosion resistance and oxidation resistance. It also has the effect of improving high temperature strength in the medium temperature range. Therefore, it may be contained as necessary. However, if the Sn content exceeds 0.50%, the manufacturability and toughness are significantly reduced. Therefore, the Sn content is set to 0.50% or less. On the other hand, in order to obtain the above effect, the Sn content is preferably 0.003% or more. In consideration of oxidation resistance, the Sn content is more preferably 0.10% or more.
[0042] Ni: 0-1.0% Ni has the effect of improving acid resistance, toughness, and high-temperature strength. Therefore, it may be contained as necessary. However, if Ni is contained in an amount exceeding 1.0%, the manufacturing cost increases. Therefore, the Ni content is set to 1.0% or less. The Ni content is preferably set to 0.5% or less. On the other hand, in order to obtain the above effect, the Ni content is preferably set to 0.05% or more. The Ni content is more preferably set to 0.08% or more.
[0043] Magnesium: 0 to 0.01% Mg is an element that has a deoxidizing effect. It also has the effect of refining the structure of the slab and improving the formability. And, Mg oxides become the precipitation sites of carbonitrides such as Ti(C,N) and Nb(C,N) and have the effect of finely dispersing and precipitating them. As a result, it has the effect of improving toughness. Therefore, it may be contained as necessary. However, excessive Mg content leads to deterioration of weldability, corrosion resistance and surface quality. Therefore, the Mg content is 0.01% or less. The Mg content is preferably 0.001% or less. On the other hand, in order to obtain the above effect, the Mg content is preferably 0.0002% or more. In addition, in consideration of refining costs, the Mg content is more preferably 0.0003% or more.
[0044] Sb: 0 to 0.50% Sb has the effect of improving corrosion resistance and high-temperature strength. Therefore, it may be contained as necessary. However, if Sb is contained in an amount exceeding 0.50%, slab cracking and ductility reduction during steel plate production may occur excessively. Therefore, the Sb content is set to 0.50% or less. In consideration of manufacturability, the Sb content is preferably set to 0.30% or less. On the other hand, in order to obtain the above effect, the Sb content is preferably set to 0.0001% or more, and more preferably set to 0.0050% or more. In consideration of refining costs, the Sb content is more preferably set to 0.0100% or more.
[0045] Zr: 0 to 0.30% Zr, like Ti and Nb, is a carbonitride forming element and has the effect of improving corrosion resistance and deep drawability. Therefore, it may be contained as necessary. However, if Zr is contained in an amount exceeding 0.30%, manufacturability is significantly deteriorated. For this reason, the Zr content is set to 0.30% or less. In addition, taking into consideration the cost and surface quality, it is preferable to set it to 0.20% or less. On the other hand, in order to obtain the above effect, the Zr content is preferably set to 0.001% or more. The Zr content is more preferably set to 0.10% or more.
[0046] Ta: 0 to 0.30% Hf: 0~0.30% Ta and Hf have the effect of improving toughness by combining with C and N. Therefore, they may be contained as necessary. However, if the content of Ta and Hf exceeds 0.30%, not only will the cost increase, but manufacturability will also be significantly deteriorated. For this reason, the Ta content is set to 0.30% or less. The Ta content is preferably set to 0.08% or less. Similarly, the Hf content is set to 0.30% or less. The Hf content is preferably set to 0.08% or less.
[0047] On the other hand, in order to obtain the above-mentioned effects, the Ta content is preferably 0.001% or more. In consideration of refining costs, the Ta content is preferably 0.010% or more. Similarly, the Hf content is preferably 0.001% or more. In consideration of refining costs, the Hf content is preferably 0.010% or more.
[0048] Co: 0 to 0.30% Co has the effect of improving high-temperature strength. Therefore, it may be contained as necessary. However, if the Co content exceeds 0.30%, it leads to deterioration of toughness. Therefore, the Co content is set to 0.30% or less. In addition, taking into consideration refining costs and manufacturability, it is preferable to set it to 0.10% or less. On the other hand, in order to obtain the above effect, the Co content is preferably set to 0.01% or more.
[0049] Ca: 0-0.01% Ca is an element that has a desulfurization effect. Therefore, it may be contained as necessary. However, if Ca is contained in an amount exceeding 0.01%, coarse CaS is generated, which deteriorates toughness and corrosion resistance. Therefore, the Ca content is set to 0.01% or less. In consideration of manufacturability, the Ca content is preferably set to 0.0020% or less. On the other hand, in order to obtain the above effect, the Ca content is preferably set to 0.0002% or more. In consideration of refining costs, the Ca content is preferably set to 0.0003% or more.
[0050] REM: 0~0.20% REM has the effect of refining various precipitates and improving toughness and oxidation resistance. Therefore, it may be contained as necessary. However, if the REM content exceeds 0.20%, castability is significantly deteriorated and ductility is reduced. Therefore, the REM content is set to 0.20% or less. In consideration of manufacturability, the REM content is preferably set to 0.05% or less. On the other hand, in order to obtain the above effect, the REM content is preferably set to 0.001% or more.
[0051] REM refers to a total of 17 elements, including Sc, Y and lanthanides, and the above REM content refers to the total content of these elements. In industry, REM is often added in the form of misch metal.
[0052] Ga: 0 to 0.30% Ga has the effect of improving corrosion resistance and suppressing hydrogen embrittlement. Therefore, it may be contained as necessary. However, excessive Ga content increases manufacturing costs. Therefore, the Ga content is set to 0.30% or less. Furthermore, from the viewpoints of manufacturability and cost, and ductility and toughness, it is preferable that the Ga content is 0.002% or less. On the other hand, in order to obtain the above effects and from the viewpoint of the formation of sulfides and hydrides, the Ga content is preferably set to 0.0002% or more.
[0053] Other components are not particularly specified in the present invention, but in the present invention, Bi and the like may be contained in an amount of 0.001 to 0.1% as required.
[0054] In the chemical composition of the present invention, the balance is Fe and impurities. Here, the term "impurities" refers to The term "contaminants" refers to components that are mixed in industrially due to various factors in the manufacturing process and raw materials such as ores and scraps, and that are acceptable within the range that does not adversely affect the present invention. It is preferable to reduce the above-mentioned impurities as much as possible, including common harmful elements such as As and Pb.
[0055] 2.Metal structure 2-1. Average crystal grain size of the parent phase In the ferritic stainless steel sheet according to the present invention, the average crystal grain size of the ferrite phase, i.e., the matrix, is 100 to 200 μm or less. If the average crystal grain size of the matrix is less than 100 μm, the yield strength decreases in a high-temperature usage environment, and the high-temperature strength decreases. For this reason, the average crystal grain size of the matrix is 100 μm or more. The average crystal grain size of the matrix is preferably 120 μm or more.
[0056] On the other hand, if the average crystal grain size of the parent phase exceeds 200 μm, it is undesirable because the manufacturability decreases and the steel sheet surface becomes rough. Therefore, the average crystal grain size of the parent phase is set to 200 μm or less. In addition, taking into consideration the productivity, etc., the average crystal grain size of the parent phase is preferably set to 180 μm or less, and more preferably set to 150 μm or less.
[0057] The average crystal grain size of the parent phase may be measured by the following procedure. Specifically, in the L-section of the steel sheet, when the sheet thickness is t, a portion corresponding to 1 / 4t from the end of the steel sheet in the sheet thickness direction (hereinafter simply referred to as "1 / 4t portion") is observed using an optical microscope. The observation magnification is 50x, and five arbitrary locations (five fields of view) are observed. The crystal grain size is measured based on the observation results, and the average value is taken as the average crystal grain size. The measurement of the average crystal grain size complies with JIS G 0551:2013, and the calculation of the crystal grain size is rounded off to the nearest whole number.
[0058] 2-2.Nb-containing second phase Hereinafter, in the ferritic stainless steel sheet, the second phase containing Nb is described as the Nb-containing second phase, and in the steel sheet according to the present invention, the amount of precipitation of the Nb-containing second phase before aging heat treatment is specified as a requirement. The reason for this is that it is effective to suppress the precipitation of the Nb-containing second phase as much as possible before use at high temperatures, and to effectively precipitate the Nb-containing second phase at the stage of use at high temperatures. This makes it possible to suppress the decrease in yield strength in the usage environment and the deterioration of high-temperature strength.
[0059] Here, the Nb-containing second phase refers to precipitates in which the amount of Nb in the precipitates is 20% by mass or more. Specifically, the Nb-containing second phase is a precipitate such as Nb carbonitride or a Laves phase containing Nb.
[0060] In the ferritic stainless steel sheet according to the present invention, the amount of precipitation of the Nb-containing second phase measured by extraction residue analysis is set to 0.15% or less by mass. While it is desirable to reduce the amount of precipitation of the Nb-containing second phase as much as possible before use, if an attempt is made to reduce it excessively, a higher temperature and longer annealing time is required in the annealing step after cold rolling. As a result, the crystal grains become coarse, which leads to rough surfaces during processing and reduced productivity. Therefore, the amount of precipitation of the Nb-containing second phase is set to the above range.
[0061] The amount of precipitated Nb-containing second phase may be measured by extraction residue analysis. Specifically, a sample of a given shape (20 mm x 30 mm x 1.2 mm) is cut out and the mass is measured. Then, an arbitrary amount of a solution containing 4 L of methanol, 500 g of maleic anhydride, and 400 ml of tetramethylammonium chloride is used to electrolyze 1 g of sample under electrolysis conditions of a constant potential of 100 mV. The solution after electrolysis is then filtered with a PTFE filter of φ0.2 mm, the precipitate is extracted as a residue, and the amount of precipitated Nb-containing second phase is measured.
[0062] 3. Nb-containing second phase after aging heat treatment In order to suppress deterioration of high-temperature strength, it is desirable that the Nb-containing second phase precipitates finely in a certain amount within the grains and does not easily grow coarsely in the usage environment. Therefore, in the ferritic stainless steel sheet according to the present invention, assuming a usage environment at high temperatures, the metal structure when aging heat treatment is performed, specifically, the Nb-containing second phase is specified.
[0063] 3-1. Amount of precipitation of Nb-containing second phase after aging heat treatment Assuming that the ferritic stainless steel sheet according to the present invention is used in a high-temperature environment, it is preferable that when the sheet is subjected to an aging heat treatment at 750°C for 100 hours, the amount of precipitation of a Nb-containing second phase as measured by extraction residue analysis is 0.20% by mass or more.
[0064] If the amount of precipitation of the Nb-containing second phase after the aging heat treatment is less than 0.20%, the Nb-containing second phase does not precipitate sufficiently, and precipitation strengthening, more specifically, particle dispersion strengthening, does not occur effectively. As a result, improvement of high-temperature strength cannot be expected. Therefore, the amount of precipitation of the Nb-containing second phase after the aging heat treatment under the above conditions is preferably 0.20% or more. The amount of precipitation of the Nb-containing second phase after the aging heat treatment is more preferably 0.25% or more, further preferably 0.28% or more, and extremely preferably 0.30% or more. Here, the upper limit of the amount of precipitation of the Nb-containing second phase after the aging heat treatment is not particularly set, but is usually about 0.7% or less. The amount of precipitation of the Nb-containing second phase after the aging heat treatment may also be measured by the same method as described above for the sample subjected to the aging heat treatment.
[0065] 3-2. Average particle size of Nb-containing second phase after aging heat treatment As described above, in order to suppress deterioration of high-temperature strength after aging heat treatment, it is desirable that a certain amount or more of fine Nb-containing second phase precipitates within the grains. Therefore, in the ferritic stainless steel sheet according to the present invention, when aging heat treatment is performed at 750°C for 100 hours, the average grain size of the Nb-containing second phase is preferably 200 nm or less.
[0066] If the average particle size of the Nb-containing second phase exceeds 200 nm, the coarsely grown Nb-containing second phase does not contribute to particle dispersion strengthening, so the average particle size of the Nb-containing second phase is preferably 200 nm or less, more preferably 100 nm or less.
[0067] The average particle size of the Nb-containing second phase may be measured by the following procedure. Specifically, a double-sided jet electrolytic polishing method is used to prepare an observation sample that allows observation of the 1 / 4t portion of the steel sheet in the same manner as described above. The obtained sample is then observed for precipitates of the second phase using a transmission electron microscope. The observation magnification is set to 50,000 times, which allows the Nb-containing second phase to be observed almost uniformly, and 10 arbitrary locations (10 fields of view) are observed. The Fe, C, Si, Nb, and Cr of the precipitates are quantified using an EDS attached to the transmission electron microscope, and precipitates with an Nb content of 20 mass% or more are identified as the Nb-containing second phase. In addition, the Nb-containing precipitate phase is colored and image-processed, and then the area of each particle is calculated using the image analysis software "ImageJ" manufactured by NIH, and the particle size of the Nb-containing second phase is measured by converting the area into a circle equivalent diameter, and the average value is taken as the average particle size.
[0068] As a transmission electron microscope used for observation, for example, a 200 kV field emission transmission electron microscope JEM2100F manufactured by JEOL Ltd. may be used, and as an EDS device, for example, a 200 kV field emission transmission electron microscope JEM2100F manufactured by JEOL Ltd. may be used.
[0069] 3-3. Ratio of M6C type carbides It is preferable that the second phase has a crystal structure that is difficult to grow coarsely, regardless of whether or not Nb is contained. Therefore, in the ferritic stainless steel sheet according to the present invention, the ratio of M6C carbides, which are difficult to grow, to the entire second phase is preferably set to the following range.
[0070] That is, the ratio of M6C carbides to the entire second phase is preferably 50% or more by mass. If the ratio of M6C carbides to the entire second phase is less than 50% by mass, the second phase grows too coarsely and particle dispersion strengthening does not occur effectively. As a result, it becomes difficult to suppress deterioration of high-temperature strength. For this reason, the ratio of M6C carbides to the entire mass of the second phase is preferably 50% or more by mass, and more preferably 60% or more. There is no particular upper limit for the ratio of M6C carbides, but it is generally considered to be 80% or less.
[0071] Here, the M6C type carbide is a carbide consisting of Fe, Si, Nb, Cr, etc., excluding C. M means an element constituting the carbide as described above. An example of the M6C type carbide is Fe3Nb3C.
[0072] The measurement can be performed according to the following procedure. The ratio of M6C carbides to the entire second phase can be determined by collecting the extraction residue as described above, performing a qualitative analysis using an X-ray diffraction device, and identifying various second phases. After that, the ratio of M6C carbides to all the second phases can be calculated as a percentage using the RIR method.
[0073] As an X-ray diffraction apparatus used for identifying the second phase by X-ray diffraction method, for example, Rigaku's RINT-2500H may be used, and as a quantitative analysis software by the RIR method, for example, Rigaku's PDXL may be used.
[0074] 4.Applications The ferritic stainless steel sheet according to the present invention is suitable for use in exhaust parts of automobiles and motorcycles. Examples of exhaust parts include exhaust manifolds, catalytic converter cases, EGR cooler cases, exhaust heat recovery devices, center pipes, mufflers, and turbocharger parts. In addition, the ferritic stainless steel sheet may be used in parts related to the insulation of exhaust pipes.
[0075] 5. Manufacturing method The method for producing a ferritic stainless steel sheet according to the present invention will now be described. The method for producing a steel sheet according to the present invention comprises, for example, the steps of steelmaking-hot rolling-annealing-pickling-cold rolling-annealing and pickling.
[0076] 5-1.Steelmaking process A method in which steel having the above-mentioned chemical composition is melted in a converter and then subjected to secondary refining is suitable. The molten steel is formed into a slab by a known casting method (continuous casting).
[0077] 5-2.Hot rolling process The slab is heated, for example, in the range of 1100 to 1300°C, and hot-rolled by continuous rolling to become a hot-rolled sheet. Hot rolling is performed in a hot rolling mill consisting of multiple stands, and the obtained hot-rolled sheet is coiled to become a hot-rolled coil. The coiling temperature is 400 to 750°C from the viewpoint of the toughness of the hot-rolled sheet. If the coiling temperature is less than 400°C, rapid cooling is required, which increases the manufacturing cost. For this reason, the coiling temperature is set to 400°C or higher. On the other hand, if the coiling temperature exceeds 750°C, the amount of precipitates that deteriorate the toughness increases significantly, which reduces the toughness of the hot-rolled sheet and reduces manufacturability. For this reason, the coiling temperature is set to 750°C or lower. After hot rolling and coiling, annealing is performed as necessary. Then, pickling is performed.
[0078] 5-3.Cold rolling process Next, the hot-rolled sheet is cold-rolled to a final thickness to obtain a cold-rolled sheet. The rolling reduction during cold rolling is not particularly limited. The rolling reduction may be adjusted as appropriate according to the thickness. In cold rolling, either a tandem rolling mill or a Sendzimir rolling mill may be used.
[0079] 5-4. Cold-rolled sheet annealing The cold-rolled sheet is then annealed. When annealing the cold-rolled sheet, it is heated to a temperature range of 1100 to 1200°C, and then allowed to remain in that temperature range for 30 seconds to 3 minutes, and then cooled. During cooling, the cooling rate in the temperature range of 1100 to 600°C is controlled to 5 to 20°C / sec.
[0080] If the heating temperature during annealing is less than 1100 ° C, a large amount of coarse Laves phase precipitates, and high-temperature strength decreases. Therefore, the heating temperature during annealing is set to 1100 ° C or higher. On the other hand, if the heating temperature during annealing exceeds 1200 ° C, the crystal grains become excessively coarse, and there is a risk of roughness called orange peel occurring in the product sheet. Therefore, the heating temperature during annealing is set to 1200 ° C or lower. From the viewpoint of productivity, the heating temperature during annealing is preferably set to 1180 ° C or lower, and more preferably set to 1150 ° C or lower.
[0081] In addition, if the residence time in the heating temperature range during annealing is less than 30 seconds, the crystal grains do not grow sufficiently, and the Nb-containing second phase is difficult to precipitate within the grains. As a result, the deterioration of high-temperature strength cannot be suppressed. For this reason, the residence time in the heating temperature range is set to 30 seconds or more. On the other hand, if the residence time in the heating temperature range exceeds 3 minutes, the crystal grains become excessively coarse. In addition, productivity is significantly reduced. For this reason, the residence time in the heating temperature range is set to 3 minutes or less.
[0082] After heating and retention, cooling is performed. During cooling, the cooling rate in the temperature range of 1100 to 600°C is controlled to 5 to 20°C / sec. If the cooling rate in the above temperature range is less than 5°C / sec, the Nb-containing second phase precipitates during cooling, making it difficult to secure the Nb-containing second phase in the usage environment. As a result, high-temperature strength may deteriorate. In addition, the strength of the product plate may increase, and press formability may decrease. For this reason, the cooling rate in the above temperature range is preferably 5°C / sec or more.
[0083] On the other hand, if the cooling rate in the above temperature range exceeds 20°C / sec, it becomes difficult to uniformly cool the entire steel sheet, and the product quality may become unstable. Therefore, the cooling rate in the above temperature range is preferably 20°C / sec or less. From the viewpoint of stable product quality, the cooling rate in the above temperature range is more preferably 15°C / sec or less, and even more preferably 10°C / sec or less. The annealing atmosphere may be appropriately selected as necessary.
[0084] After annealing the cold-rolled sheet, it may be appropriately and optionally subjected to temper rolling or tension leveling. It may also be pickled. The pickling method may be a conventional method. Through these steps, the structure of the ferritic stainless steel sheet is obtained. The steel sheet obtained by the above procedure may be processed to produce an exhaust part.
[0085] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. EXAMPLES
[0086] Steels having the chemical compositions shown in Tables 1 and 2 were melted and cast into slabs, which were then heated to a temperature range of 1100 to 1300°C, hot-rolled, and coiled at a temperature of 400 to 800°C as shown in Tables 3 and 4 to form hot-rolled coils with a thickness of 5 mm. The toughness of the hot-rolled coils thus obtained was evaluated by the method described below.
[0087] The coil was then cold rolled to a thickness of 1.2 mm, and annealed and pickled to obtain a product sheet. In the annealing after the above cold rolling, the heating temperature was changed between 1100 and 1210°C as shown in Tables 3 and 4, and the sheet was held at the temperature for 30 to 170 seconds, after which it was cooled. In the cooling, the cooling rate in the temperature range of 1100 to 600°C was 6 to 24°C / sec, and a ferritic stainless steel sheet was obtained.
[0088] [Table 1]
[0089] [Table 2]
[0090] (Measurement of the average crystal grain size of the parent phase) The average crystal grain size of the parent phase was measured for the obtained steel sheets. Specifically, the 1 / 4t portion of the L cross section of the steel sheets was observed using an optical microscope. The observation magnification was 50x, and observation was performed in five fields of view. Based on the observation results, the crystal grain size of each crystal grain was measured, and the average value was taken as the average crystal grain size. The measurement of the average crystal grain size was in accordance with JIS G 0551:2013, and the crystal grain size was calculated by rounding off decimal points.
[0091] (Amount of Nb-containing second phase precipitated) The amount of precipitation of the Nb-containing second phase was calculated for the obtained steel sheet. Similarly, after performing aging heat treatment at 750°C for 100 hours, the amount of precipitation of the Nb-containing second phase was calculated by extraction residue analysis. The amount of precipitation of each Nb-containing second phase was measured by the following procedure.
[0092] Specifically, a sample was cut to 20 mm x 30 mm x 1.2 mm, and the mass was measured. Then, an arbitrary amount of a solution containing 4 L of methanol, 500 g of maleic anhydride, and 400 ml of tetramethylammonium chloride was used to electrolyze 1 g of the sample under electrolysis conditions of a constant potential of 100 mV. The electrolytic solution was then filtered with a PTFE filter of φ0.2 mm, and the precipitate was extracted as a residue, and the amount of precipitate of the Nb-containing second phase was measured.
[0093] (Average particle size of Nb-containing second phase and proportion of M6C type carbides) The average particle size of the Nb-containing second phase was measured for the steel sheet after aging heat treatment at 750°C for 100 hours. Specifically, an observation sample was prepared by double-sided jet electrolytic polishing so that 1 / 4t of the steel sheet could be observed. The obtained sample was then observed for precipitates of the second phase using a transmission electron microscope. The observation magnification was set to 50,000 times, which allows the Nb-containing second phase to be observed almost uniformly, and 10 fields of view were observed.
[0094] The Fe, C, Si, Nb, and Cr of the precipitates were quantified using an EDS attached to a transmission electron microscope, and precipitates with an Nb content of 20 mass% or more were identified as Nb-containing second phases. In addition, the Nb-containing precipitates were colored and image-processed, and the area of each particle was calculated using NIH's image analysis software "ImageJ." The particle diameter of the Nb-containing second phase was measured by converting the area into a circle equivalent diameter, and the average value was used as the average particle diameter.
[0095] As for the ratio (mass%) of M6C carbides to the entire second phase, as described above, the extraction residue was collected and subjected to qualitative analysis using an X-ray diffraction device to identify various second phases.Then, the ratio of M6C carbides to all the second phases was calculated as a percentage by the RIR method.
[0096] (Toughness of hot-rolled sheet) Manufacturability was evaluated based on the toughness of the hot-rolled sheet. If the toughness of the hot-rolled sheet is low, for example, cracks may occur during manufacturing, resulting in reduced manufacturability. After coiling, the cooled hot-rolled sheet was subjected to a Charpy impact test to evaluate toughness. Test pieces were prepared as C-direction Charpy impact test pieces (V notch) of the hot-rolled sheet, and tests were conducted. The test pieces were sub-sized, and the average impact value of three tests was 10 J / cm. 2 When the average impact value of the three tests was 10 J / cm or more, it was marked as ○ in the table. 2 If the result was below this, it was marked as "X" in the table.
[0097] (Evaluation of high temperature strength) From the obtained steel sheet, a high-temperature tensile test piece was taken so that the rolling direction was the tensile direction, and a high-temperature tensile test was carried out at 750°C to measure the 0.2% proof stress. The high-temperature tensile test was carried out in accordance with JIS G 0567:2012, and the measured values were calculated by rounding off to the nearest few points.
[0098] In addition, to simulate a case where the material was used for a long time in a high-temperature environment, a high-temperature tensile test was performed at 750°C to measure the 0.2% yield strength after aging heat treatment at 750°C for 100 hours, as described above. If the 0.2% yield strength at 750°C is 60MPa or more and the 0.2% yield strength at 750°C after aging heat treatment at 750°C for 100 hours is 25MPa or more, the material can be applied to general exhaust parts. Therefore, in the table, if the 0.2% yield strength at 750°C is 60MPa or more, and the 0.2% yield strength after aging heat treatment at 750°C for 100 hours is 25MPa or more, the characteristics are judged to be good, and are marked with ◯. The rest are marked with ×.
[0099] (Evaluation of rough skin) In addition, to check whether or not the obtained steel sheet had rough surfaces, a cylindrical squeeze test piece with a diameter of 80 mm was prepared from the steel sheet, and a cylindrical squeeze test was performed at room temperature. The test conditions were punch diameter 40 mm, rp 4 mm, die diameter 42 mm, rp 4 mm, cushion pressure 10 kN, forming speed 20 mm / min, and lubrication with Johnson wax #122. The cup corners after the test were visually observed to check whether or not rough surfaces had occurred, and if no rough surfaces had occurred, they were marked with ◯ in the table, and if rough surfaces had occurred, they were marked with ×. The results are summarized in Tables 3 and 4 below.
[0100] [Table 3]
[0101] [Table 4]
[0102] In Test Nos. 1 to 32, which satisfied the requirements of the present invention, the deterioration of high-temperature strength was suppressed, whereas in Test Nos. 33 to 45, which did not satisfy the requirements of the present invention, at least one of the high-temperature strength and manufacturability was deteriorated.
[0103] In Nos. 33 and 34, the C and N contents were outside the upper limits stipulated in the present invention, so the matrix hardened and the hot-rolled sheet toughness was poor. In No. 35, the Si content was outside the lower limit, so refined precipitates effective for strengthening did not precipitate, and the yield strength was low before and after aging heat treatment at 750°C. In No. 36, the Si content was outside the upper limit, so the matrix hardened and the hot-rolled sheet toughness was poor. In No. 37, the Mn content was outside the upper limit, so MnS crystallized during the steelmaking stage, and the hot-rolled sheet toughness was poor.
[0104] In Nos. 38 and 39, the P and S contents were outside the upper limit, respectively, and in both cases the toughness of the steel plate was poor. In No. 40, the Cr content was outside the lower limit, which reduced the high-temperature strength and resulted in poor yield strength before and after aging heat treatment at 750°C. In Nos. 41, 42, and 43, the Cr content, Ti content, and Nb content were outside the upper limit, respectively, which caused the base metal to harden and resulted in poor hot-rolled sheet toughness.
[0105] In No. 44, the finishing temperature of the cold rolling was low, the grain size was too small, and precipitation at the grain boundaries was promoted, resulting in poor yield strength after aging heat treatment at 750°C. In No. 45, the coiling temperature and annealing temperature after hot rolling were high, which caused coarse precipitates that reduce toughness, resulting in poor hot-rolled sheet toughness. In addition, the grain size increased, resulting in rough surfaces.
Claims
1. The chemical composition, in mass%, is C: 0.001-0.030%, N: 0.001-0.030%, Si: 2.00-4.00%, Mn: 0.01 to 2.00%, P: 0.010-0.050%, S: 0.0001-0.010%, Cr: 10.0-30.0%, Nb: 0.01 to 0.80%, Ti: 0 to 0.50%, B: 0 to 0.0009%, Al: 0-2.5%, Cu: 0-3.0%, Mo: 0-3.0%, W: 0-0.50%, V: 0 to 1.0%, Sn: 0 to 0.50%, Ni: 0-1.0%, Mg: 0 to 0.01%, Sb: 0 to 0.50%, Zr: 0 to 0.30%, Ta: 0-0.30%, Hf: 0-0.30%, Co: 0 to 0.30%, Ca: 0-0.01%, REM: 0-0.20%, Ga: 0-0.30%, The balance is Fe and impurities. In metal structure, The average crystal grain size of the matrix is 100 to 200 μm, When the second phase containing Nb is referred to as the Nb-containing second phase, The amount of precipitation of the Nb-containing second phase measured by extraction residue analysis is 0.15% or less by mass%, When aging heat treatment was performed at 750°C for 100 hours, The amount of precipitation of the Nb-containing second phase measured by extraction residue analysis is 0.20% or more by mass%, The average particle size of the Nb-containing second phase is 200 nm or less; A ferritic stainless steel plate having a ratio of M6C type carbides to the entire second phase of 50% or more, in mass percent.
2. The chemical composition, in mass%, Ti: 0.01 to 0.50%, B: 0.0001 to 0.0009%, Al: 0.01-2.5%, Cu: 0.01 to 3.0%, Mo: 0.01-3.0%, W: 0.01-0.50%, V: 0.05-1.0%, Sn: 0.003 to 0.50%, Ni: 0.05-1.0%, Mg: 0.0002-0.01%, Sb: 0.0001 to 0.50%, Zr: 0.001 to 0.30%, Ta: 0.001 to 0.30%, Hf: 0.001-0.30%, Co: 0.01 to 0.30%, Ca: 0.0002-0.01%, REM: 0.001 to 0.20%, and Ga: 0.0002-0.30%, The ferritic stainless steel sheet according to claim 1, comprising one or more selected from the following:
3. A method for producing a ferritic stainless steel sheet according to claim 1 or 2, (a) hot rolling a steel having the chemical composition according to claim 1 or 2 to obtain a hot rolled sheet; (b) coiling the hot-rolled sheet in a temperature range of 400 to 750 ° C.; (c) cold rolling the coiled hot-rolled sheet to obtain a cold-rolled sheet; (d) heating the cold-rolled sheet to a temperature range of 1100 to 1200°C, and then performing an annealing treatment in which the cold-rolled sheet is retained in the temperature range for 30 seconds to 3 minutes.
4. An exhaust part using the ferritic stainless steel sheet according to claim 1 or 2.
Citation Information
Patent Citations
Ferritic precipitation hardening stainless steel
JP1990115347A
Manufacture of high temperature high strength and high workability ferritic stainless steel
JP1993331551A
FERRITIC Cr-CONTAINING STEEL AND ITS PRODUCTION METHOD
JP2005206944A
Ferritic stainless steel for exhaust gas passage member
JP2008189974A
Ferritic stainless steel material for automotive member of exhaust gas path
JP2009120893A