Method for restoring non-aqueous electrolyte secondary battery and method for manufacturing non-aqueous electrolyte secondary battery
A novel recovery method for non-aqueous electrolyte secondary batteries using an aromatic hydrocarbon compound and metal ions addresses the complexity of third electrode methods, achieving improved capacity and cycle capacity retention through controlled voltage application.
Patent Information
- Application Number
- JP2021040458
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-12
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2041-03-12
AI Technical Summary
Existing methods for restoring the capacity of non-aqueous electrolyte secondary batteries, such as incorporating a third electrode, complicate the battery structure and require a novel recovery method without a third electrode.
A recovery method for non-aqueous electrolyte secondary batteries using a solution containing an aromatic hydrocarbon compound in a reduced state and metal ions of the same type as the carrier ions, injected with a constant voltage application to maintain a predetermined voltage lower than the fully charged voltage, facilitating capacity recovery.
The method effectively recovers battery capacity and improves the cycle capacity retention rate by maintaining a high potential difference for the recovery reaction, suppressing residual aromatic hydrocarbon compounds, and enhancing the battery's performance.
Smart Images

Figure 0007564740000007 
Figure 0007564740000008 
Figure 0007564740000009
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for restoring a nonaqueous electrolyte secondary battery and a method for manufacturing a nonaqueous electrolyte secondary battery. [Background technology]
[0002] Conventionally, as a method for restoring the capacity of a nonaqueous electrolyte secondary battery whose capacity has deteriorated due to long-term storage or charge-discharge cycles, a method has been proposed in which a third electrode is provided in addition to a positive electrode and a negative electrode, the third electrode and the positive electrode are externally short-circuited, and carrier ions are supplied from the third electrode to the positive electrode (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-076358 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in Patent Document 1, there is a problem that the structure of the battery becomes complicated by incorporating a third electrode. For this reason, a new recovery method for a nonaqueous electrolyte secondary battery that can recover the capacity without using a third electrode has been desired.
[0005] The present disclosure has been made to solve such problems, and has as its main object to provide a novel method for restoring a non-aqueous electrolyte secondary battery. [Means for solving the problem]
[0006] As a result of intensive research to achieve the above-mentioned object, the present inventors have found that the capacity of a non-aqueous electrolyte secondary battery is restored by injecting a solution containing an aromatic hydrocarbon compound in a reduced state and the same type of metal ion as the carrier ion of the non-aqueous electrolyte secondary battery into the battery. In particular, the present inventors have found that the capacity and cycle capacity retention rate of the battery after recovery are further improved by injecting the above-mentioned recovery agent into the non-aqueous electrolyte secondary battery and maintaining a predetermined voltage lower than the full charge voltage by applying a constant voltage, and have thus completed the present disclosure.
[0007] That is, the method for recovering a nonaqueous electrolyte secondary battery disclosed in the present specification includes the steps of: A method for recovering the capacity of a non-aqueous electrolyte secondary battery that uses metal ions as carrier ions, comprising the steps of: a recovery step of injecting a recovery agent, which is a solution containing a reduced aromatic hydrocarbon compound and the same type of metal ions as the carrier ions, into the nonaqueous electrolyte secondary battery, and maintaining a predetermined voltage lower than a full charge voltage by applying a constant voltage, thereby recovering the capacity of the nonaqueous electrolyte secondary battery; It includes.
[0008] The method for producing a nonaqueous electrolyte secondary battery disclosed in the present specification further comprises the steps of: a battery preparation step of preparing a capacity-degraded nonaqueous electrolyte secondary battery having metal ions as carrier ions; a recovery step of recovering the capacity of the nonaqueous electrolyte secondary battery in the above-mentioned recovery method for the nonaqueous electrolyte secondary battery; It includes. Effect of the Invention
[0009] This method for recovering a non-aqueous electrolyte secondary battery can provide a novel method for recovering a non-aqueous electrolyte secondary battery. The reason why such an effect is obtained is presumed to be as follows. For example, a recovery agent containing an aromatic hydrocarbon compound in a reduced state and a metal ion acts directly on the positive electrode by simply injecting it into a non-aqueous electrolyte secondary battery, causing a recovery reaction that supplies electrons and metal ions to the positive electrode. It is considered that the driving force of this recovery reaction is the potential difference between the positive electrode and the recovery agent. When the recovery agent is only injected and a constant voltage is not applied, the potential of the positive electrode decreases as electrons and metal ions are supplied to the positive electrode, and the potential difference between the positive electrode and the recovery agent becomes smaller. On the other hand, when the recovery agent is injected and a predetermined voltage is maintained by applying a constant voltage, the potential of the positive electrode is kept high even if electrons and metal ions are supplied to the positive electrode, and the potential difference between the positive electrode and the recovery agent is kept high. As a result, the driving force of the recovery reaction is kept high, so that more metal ions can be supplied to the battery, and the residual aromatic hydrocarbon compound in a reduced state that may hinder the charge / discharge cycle can be suppressed. As a result, it is considered that the capacity and cycle capacity retention rate of the battery after recovery are further improved. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic diagram showing an example of a nonaqueous electrolyte secondary battery 20. FIG. [Diagram 2] FIG. 2 is an explanatory diagram showing an example of a recovery reaction scheme. [Diagram 3] 1 is an estimated diagram conceptually showing the change in the potential difference ΔErec between the positive electrode and the recovery agent when the recovery agent is left in an open circuit state after injection. [Figure 4] 1 is an estimated diagram conceptually showing a change in the potential difference ΔErec between the positive electrode and the recovery agent when a predetermined voltage is maintained by applying a constant voltage while injecting the recovery agent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The recovery method of the non-aqueous electrolyte secondary battery disclosed in this specification is a recovery method for recovering the capacity of the non-aqueous electrolyte secondary battery, and includes a recovery step of recovering the capacity of the non-aqueous electrolyte secondary battery using a recovery agent. The non-aqueous electrolyte secondary battery is not particularly limited as long as it is a non-aqueous electrolyte secondary battery using metal ions as carrier ions. For example, it may be one using Group 1 ions such as lithium, sodium, and potassium, or Group 2 ions such as magnesium, calcium, and strontium as carrier ions. Further, the non-aqueous electrolyte secondary battery may be an ion secondary battery such as a lithium-ion secondary battery, or a metal secondary battery such as a lithium metal secondary battery. Hereinafter, as an example, the case where the non-aqueous electrolyte secondary battery is a lithium-ion secondary battery will be mainly described.
[0012] (Non-aqueous electrolyte secondary battery) The non-aqueous electrolyte secondary battery includes a positive electrode, a negative electrode, and a non-aqueous electrolyte. The positive electrode may have a positive electrode active material capable of occluding and releasing lithium ions. The negative electrode may have a negative electrode active material capable of occluding and releasing lithium ions. The non-aqueous electrolyte may be interposed between the positive electrode and the negative electrode and conduct lithium ions.
[0013] For example, the positive electrode may be formed by mixing a positive electrode active material, a conductive material, and a binder, adding an appropriate solvent to form a paste-like positive electrode mixture, applying and drying it on the surface of a current collector, and compressing it as necessary to increase the electrode density. As the positive electrode active material, sulfides containing transition metal elements, oxides containing lithium and transition metal elements, etc. can be used. Specifically, transition metal sulfides such as TiS2, TiS3, MoS3, and FeS2, lithium manganese composite oxides with a basic composition formula of Li (1-x) MnO2 (0 < x < 1, etc., the same below), Li (1-x) Mn2O4, etc., lithium cobalt composite oxides with a basic composition formula of Li (1-x) CoO2, etc., lithium nickel composite oxides with a basic composition formula of Li (1-x) NiO2, etc., and lithium nickel cobalt manganese composite oxides with a basic composition formula of Li (1-x) Ni a Co b Mn cLithium nickel cobalt manganese composite oxides having a basic composition formula of LiV2O2(a+b+c=1), lithium vanadium composite oxides having a basic composition formula of LiV2O3, transition metal oxides having a basic composition formula of V2O5, etc. can be used. Among these, lithium transition metal composite oxides, such as LiCoO2, LiNiO2, LiMnO2, LiV2O3, etc., are preferred. The term "basic composition formula" means that other elements may be included. The positive electrode active material may have an oxidation-reduction potential of 3.5V or more, 4.0V or more, or 4.5V or more based on Li metal.
[0014] In the positive electrode, the conductive material may be, for example, one or more of graphite such as natural graphite (scale graphite, flake graphite) or artificial graphite, acetylene black, carbon black, Ketjen black, carbon whisker, needle coke, carbon fiber, metal (copper, nickel, aluminum, silver, gold, etc.), etc. Among these, from the viewpoint of electronic conductivity and coating property, carbon black and acetylene black are preferable as the conductive material. The binder plays a role of binding the active material particles and the conductive material particles, and may be, for example, fluorine-containing resin such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine rubber, etc., or thermoplastic resin such as polypropylene and polyethylene, ethylene propylene diene monomer (EPDM) rubber, sulfonated EPDM rubber, natural butyl rubber (NBR), etc., used alone or as a mixture of two or more kinds. In addition, aqueous binders such as cellulose-based carboxymethylcellulose (CMC), styrene butadiene copolymer (SBR), and aqueous dispersions of polyvinyl alcohol can also be used. As a solvent for dispersing the positive electrode active material, conductive material, and binder, for example, organic solvents such as N-methylpyrrolidone, dimethylformamide, dimethylacetamide, methyl ethyl ketone, cyclohexanone, methyl acetate, methyl acrylate, diethylenetriamine, N,N-dimethylaminopropylamine, ethylene oxide, and tetrahydrofuran can be used. In addition, a dispersant, a thickener, and the like can be added to water, and the active material can be slurried with latex such as SBR. As a thickener, for example, polysaccharides such as carboxymethylcellulose and methylcellulose can be used alone or as a mixture of two or more kinds. Examples of application methods include roller coating such as an applicator roll, screen coating, doctor blade method, spin coating, and bar coater, and any thickness and shape can be obtained by using any of these. The basis weight of the positive electrode mixture is not particularly limited, but for example, 5 mg / cm 2 May exceed 6mg / cm 2 or more, 7 mg / cm 2The weight of the positive electrode mixture may be, for example, 20 mg / cm 2 The following may be used. As the current collector, in addition to aluminum, titanium, stainless steel, nickel, iron, baked carbon, conductive polymer, conductive glass, etc., aluminum or copper whose surface is treated with carbon, nickel, titanium, silver, etc. for the purpose of improving adhesion, conductivity, and oxidation resistance can be used. The surface of these can also be subjected to oxidation treatment. The shape of the current collector can be a foil, film, sheet, net, punched or expanded one, lath, porous body, foam, fiber group formation, etc. The thickness of the current collector used is, for example, 1 to 500 μm.
[0015] The negative electrode may be formed by bonding a negative electrode active material and a current collector, or may be formed by mixing a negative electrode active material, a conductive material, and a binder, adding an appropriate solvent to form a paste-like negative electrode composite, applying it to the surface of a current collector, drying it, and compressing it to increase the electrode density as necessary. Examples of the negative electrode active material include inorganic compounds such as lithium, lithium alloys, and tin compounds, carbonaceous materials capable of absorbing and releasing lithium ions, composite oxides containing multiple elements, and conductive polymers. Examples of the carbonaceous material include cokes, glassy carbons, graphites, non-graphitizable carbons, pyrolytic carbons, and carbon fibers. Among these, graphites such as artificial graphite and natural graphite are preferred because they have an operating potential close to that of metallic lithium, can be charged and discharged at a high operating voltage, and can suppress self-discharge when a lithium salt is used as a supporting salt, and can reduce irreversible capacity during charging. Examples of the composite oxide include lithium titanium composite oxide and lithium vanadium composite oxide. Of these, carbonaceous materials are preferred as the negative electrode active material from the viewpoint of safety. The conductive material, binder, solvent, etc. used in the negative electrode can be the same as those exemplified for the positive electrode. The negative electrode active material may have an oxidation-reduction potential of 1.0 V or less, 0.5 V or less, or 0.3 V or less, based on Li metal. The weight of the negative electrode composite material is, for example, 3 mg / cm. 2 May exceed 4mg / cm 2The weight of the negative electrode mixture may be, for example, 15 mg / cm. 2 The negative electrode current collector may be made of copper, nickel, stainless steel, titanium, aluminum, baked carbon, conductive polymer, conductive glass, Al-Cd alloy, etc., or may be made of copper or the like whose surface has been treated with carbon, nickel, titanium, silver, etc., for the purpose of improving adhesion, conductivity, and reduction resistance. The surface of these materials may also be oxidized. The shape of the current collector may be the same as that of the positive electrode.
[0016] The non-aqueous electrolyte may contain a supporting salt and an organic solvent. Examples of the supporting salt include inorganic salts such as LiPF6, LiClO4, LiAsF6, and LiBF4, and organic salts such as LiN(FSO2)2, LiN(CF3SO2)2, and LiN(C2F5SO2)2. These supporting salts may be used alone or in combination. The concentration of the supporting salt is preferably 0.1 to 2.0 M, and more preferably 0.8 to 1.2 M. Examples of the organic solvent that can be used include aprotic organic solvents. Examples of such organic solvents include cyclic carbonates, chain carbonates, cyclic esters, cyclic ethers, and chain ethers. Examples of the cyclic carbonates include ethylene carbonate, propylene carbonate, butylene carbonate, and vinylene carbonate. Examples of the chain carbonates include dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate. Examples of cyclic esters include gamma butyrolactone and gamma valerolactone. Examples of cyclic ethers include tetrahydrofuran and 2-methyltetrahydrofuran. Examples of chain ethers include dimethoxyethane and ethylene glycol dimethyl ether. These may be used alone or in combination. In addition, the non-aqueous electrolyte may include nitrile solvents such as acetonitrile and propylnitrile, ionic liquids, gel electrolytes, etc. The non-aqueous electrolyte may contain additives such as a film-forming agent and a flame retardant.
[0017] The non-aqueous electrolyte secondary battery may have a separator between the positive electrode and the negative electrode. The separator is not particularly limited as long as it has a composition that can withstand the range of use of the non-aqueous electrolyte secondary battery, and examples thereof include polymer non-woven fabrics such as polypropylene non-woven fabrics and polyphenylene sulfide non-woven fabrics, and thin microporous films of olefin resins such as polyethylene and polypropylene. These may be used alone or in combination.
[0018] The nonaqueous electrolyte secondary battery may have an openable / closable electrolyte inlet in a battery case that houses the positive electrode, the negative electrode, and the nonaqueous electrolyte, allowing the recovery agent to be easily injected through the electrolyte inlet.
[0019] The shape of the nonaqueous electrolyte secondary battery is not particularly limited, and examples thereof include coin type, button type, sheet type, laminated type, cylindrical type, flat type, and square type. The nonaqueous electrolyte secondary battery may also be applied to large batteries used in electric vehicles and the like. FIG. 1 is a schematic diagram showing an example of a nonaqueous electrolyte secondary battery 20. The nonaqueous electrolyte secondary battery 20 includes a cup-shaped battery case 21, a positive electrode 22 having a positive electrode active material and provided at the bottom of the battery case 21, a negative electrode 23 having a negative electrode active material and provided at a position facing the positive electrode 22 via a separator 24, a gasket 25 formed of an insulating material, and a sealing plate 26 disposed at the opening of the battery case 21 and sealing the battery case 21 via the gasket 25. In the nonaqueous electrolyte secondary battery 20, a nonaqueous electrolyte 27 is filled in the space between the positive electrode 22 and the negative electrode 23.
[0020] A non-aqueous electrolyte secondary battery has an internal resistance of 5 Ωcm when the capacity of the battery is not degraded (also called a pre-degraded battery). 2 It may be in excess of 7 Ωcm 2 It may be 10 Ωcm or more. 2In non-aqueous electrolyte secondary batteries, such as batteries for electric vehicles, in which the thickness or weight of the electrode composite is large and the internal resistance is relatively high, the capacity and cycle capacity retention rate of the battery after recovery are often low simply by injecting a recovery agent, so it is highly meaningful to apply the recovery method for non-aqueous electrolyte secondary batteries of the present disclosure. Note that the internal resistance of the battery before deterioration is 50 Ω cm 2 It may be the following:
[0021] (Recovery Agent) The recovery agent is a solution containing an aromatic hydrocarbon compound in a reduced state and metal ions of the same type as the carrier ions of the nonaqueous electrolyte secondary battery. The recovery agent may be a recovery agent prepared in advance, or may be prepared in a preparation step for preparing the recovery agent. In the recovery agent, the aromatic hydrocarbon compound in a reduced state and the metal ions may be dissociated or associated. The recovery agent may contain an electrolyte in addition to a recovery agent stock solution containing an aromatic hydrocarbon compound in a reduced state and metal ions of the same type as the carrier ions of the nonaqueous electrolyte secondary battery. The recovery agent may be a recovery agent stock solution without containing an electrolyte.
[0022] In the recovery agent, the aromatic hydrocarbon compound is preferably polyacene or polyphenyl. Polyacene is a compound having a structure in which a plurality of benzene rings are condensed, and examples thereof include naphthalene, anthracene, tetracene, and pentacene. Polyphenyl is a compound having a structure in which a plurality of phenyl groups are linked by single bonds, and examples thereof include biphenyl, ortho-terphenyl, meta-terphenyl, para-terphenyl, para-quaterphenyl, and para-quinquiphenyl. Polyacene and polyphenyl may have a substituent on the aromatic ring, or may contain a heteroatom in the aromatic ring. Examples of the substituent include a halogen atom, an alkyl group, an aryl group, an alkenyl group, an alkoxy group, an aryloxy group, a sulfonyl group, an amino group, a cyano group, a carbonyl group, an acyl group, an amide group, and a hydroxyl group. Examples of the heteroatom include nitrogen, oxygen, and sulfur. Examples of polyacene containing a heteroatom in an aromatic ring include quinoline, chromene, and acridine. Examples of polyphenyl containing a heteroatom in an aromatic ring include bipyridine. The aromatic hydrocarbon compound is preferably one or more of naphthalene, biphenyl, anthracene, ortho-terphenyl, and para-terphenyl among the above-mentioned compounds, and more preferably one or more of naphthalene and biphenyl. The aromatic hydrocarbon compound may be, for example, one or more of formula (1) and formula (2). The aromatic hydrocarbon compound in a reduced state is, for example, the above-mentioned aromatic hydrocarbon compound in a reduced state (also called a reduced form), for example, a radical anion. The aromatic hydrocarbon compound in a reduced state may be, for example, one or more of the reduced form of the compound of formula (1) and the reduced form of the compound of formula (2).
[0023] [ka]
[0024] In the recovery agent, the metal ions may be of the same type as the carrier ions in the nonaqueous electrolyte secondary battery, but are preferably one or more of alkali metal ions such as lithium ions, sodium ions, and potassium ions.
[0025] The restoring agent may include one or more compounds of formula (3) and formula (4). In the compounds of formula (3) and formula (4), the radical anion portion is the above-mentioned aromatic hydrocarbon compound in a reduced state, and the metal cation portion is the above-mentioned metal ion.
[0026] [ka]
[0027] The recovery agent may contain a solvent or an organic solvent. The organic solvent is preferably a solvent having an ether skeleton, and may be a cyclic ether or a chain ether. The recovery agent may contain one or more solvents selected from tetrahydrofuran (THF), dimethoxyethane (DME), diethoxyethane (DEE), dioxolane (DOL), and dioxane (DOX). The recovery agent preferably contains one or more solvents selected from tetrahydrofuran and dimethoxyethane.
[0028] The recovery agent may be obtained by adding an aromatic hydrocarbon compound and a metal in a metallic state, not an ion state, to a solvent. For example, the recovery agent may be obtained by one or more of formulas (5) and (6). More specifically, the recovery agent may be obtained by reacting naphthalene, diphenyl, or terphenyl with Li metal in a THF solvent, as shown in formulas (7) to (9). Also, the recovery agent may be obtained by reacting naphthalene, diphenyl, or terphenyl with Li metal in a DME solvent, according to formulas (7) to (9). In this way, a recovery agent containing an aromatic hydrocarbon compound in a reduced state and a metal ion can be easily prepared. The recovery agent may be prepared by adding a metal to a precursor obtained by adding an aromatic hydrocarbon compound to a solvent. The recovery agent may be prepared under an inert atmosphere such as an argon atmosphere. The recovery agent may be prepared under a low dew point environment, such as a dew point of -20°C or less, -40°C or less, or -60°C or less. The recovery agent may be prepared by stirring a solvent, an aromatic hydrocarbon compound, and a metal, and a stirrer or the like may be used in this case.
[0029] [ka]
[0030] [ka]
[0031] The above-described restoring agent is also referred to as a restoring agent stock solution. In the restoring agent stock solution, the concentrations of the aromatic hydrocarbon compound in a reduced state and the metal ion may be 0.05 mol / L or more and 1.1 mol / L or less, 0.1 mol / L or more and 1.1 mol / L or less, or 0.5 mol / L or more and 1.0 mol / L or less, respectively. Moreover, these concentrations may be equal to or less than the solubility. Moreover, the number of moles M of the aromatic hydrocarbon compound in a reduced state contained in the restoring agent is A (mol) and the number of moles of metal ion M B (mol) M A / M B is preferably 1 / 1, but may be 1.1 / 1.0 to 1.0 / 1.1, or may be 1.2 / 1.0 to 1.0 / 1.2.
[0032] When the recovery agent contains an electrolyte in addition to the recovery agent stock solution, the electrolyte may be, for example, a nonaqueous electrolyte exemplified in the nonaqueous electrolyte of the nonaqueous electrolyte secondary battery, or may contain an organic solvent exemplified in the nonaqueous electrolyte and a supporting salt exemplified in the nonaqueous electrolyte. The solvent of the electrolyte may be different from the solvent of the recovery agent stock solution, but is preferably one or more of cyclic carbonate, chain carbonate, and cyclic ester, and more preferably one or more of cyclic carbonate and chain carbonate. The solvent of the electrolyte may be one or more of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate. The supporting salt of the electrolyte may be different from the solute of the recovery agent stock solution, but may be an inorganic salt such as LiPF6. The electrolyte may contain additives such as a film-forming agent and a flame retardant. The composition of the electrolyte may be the same as the nonaqueous electrolyte of the nonaqueous electrolyte secondary battery to be recovered. When the recovery agent contains an electrolyte solution, the content of the electrolyte solution may be 30% by volume to 70% by volume, 30% by volume to 60% by volume, or 30% by volume to 50% by volume. When preparing a recovery agent containing an electrolyte solution, the recovery agent stock solution and the electrolyte solution may be mixed, and the recovery agent stock solution and the electrolyte solution may be stirred, or may be stirred using a stirrer or the like.
[0033] The redox potential of the recovery agent may be higher than that of the negative electrode and lower than that of the positive electrode. The redox potential of the recovery agent may be, for example, 0.5 V to 2.5 V, 1.0 V to 2.0 V, or 1.2 V to 1.9 V, based on Li metal.
[0034] (Recovery process) In this process, a recovery agent is injected into the nonaqueous electrolyte secondary battery, and a predetermined voltage lower than the full charge voltage is maintained by applying a constant voltage to recover the capacity of the nonaqueous electrolyte secondary battery. The nonaqueous electrolyte secondary battery to be recovered is a battery in a state of capacity degradation (also called a deteriorated battery), and may be, for example, a battery in a state of capacity degradation relative to the rated capacity of the nonaqueous electrolyte secondary battery. The nonaqueous electrolyte secondary battery to be recovered may be an unused product or a used product. Even if it is an unused product, the capacity may be deteriorated due to long-term storage or the like. The predetermined voltage may be a voltage lower than the full charge voltage, but is preferably a voltage at which the potential of the positive electrode is higher than the potential of the recovery agent. The full charge voltage may be the upper limit charging voltage set for the nonaqueous electrolyte secondary battery (battery before deterioration). The predetermined voltage may be appropriately determined according to the configuration of the battery to be recovered, and may be, for example, 3.0V or more and less than 4.1V, 3.5V or more and 4.0V or less, or 3.7V or more and 4.0V or less.
[0035] In this step, prior to injecting the recovery agent, the voltage of the nonaqueous electrolyte secondary battery may be adjusted to the above-mentioned predetermined voltage. In this case, for example, the nonaqueous electrolyte secondary battery may be charged by constant current charging (CC charging) or constant current constant voltage charging (CCCV charging) to adjust the voltage of the nonaqueous electrolyte secondary battery. This voltage adjustment is not necessary, but it is preferable that the voltage of the nonaqueous electrolyte secondary battery to be recovered is the above-mentioned predetermined voltage.
[0036] In this step, when injecting the recovery agent, the nonaqueous electrolyte secondary battery may be opened and the recovery agent may be injected to seal the opening, or the recovery agent may be injected into the nonaqueous electrolyte secondary battery by injection or the like to seal the perforation. When injecting the recovery agent, it may be injected under an inert atmosphere such as an argon atmosphere. The recovery agent may be injected so as to contact at least the positive electrode, but may also be mixed with the nonaqueous electrolyte. The injection amount of the recovery agent may be appropriately determined depending on the configuration of the nonaqueous electrolyte secondary battery, the degree of deterioration, and the like. The injection amount of the recovery agent may be, for example, 1% or more and 100% or less, 10% or more and 75% or less, or 25% or more and 50% or less with respect to the volume [mL] of the nonaqueous electrolyte contained in the nonaqueous electrolyte secondary battery. The constant voltage application may be continued before or during the injection of the recovery agent, or may be started after the injection of the recovery agent while the voltage drop of the nonaqueous electrolyte secondary battery due to the supply of metal ions to the positive electrode is negligibly small (for example, within 5 minutes, preferably within 3 minutes, more preferably within 1 minute). The constant voltage application time can be appropriately determined according to the configuration of the nonaqueous electrolyte secondary battery, the degree of deterioration, the injection amount of the recovery agent, etc. For example, the injection amount of the recovery agent may be constant, and the constant voltage application time may be adjusted according to the configuration and degree of deterioration of the nonaqueous electrolyte secondary battery. The constant voltage application time may be, for example, 1 hour or more and 48 hours or less, 6 hours or more and 36 hours or less, or 12 hours or more and 24 hours or less. In addition, when the constant voltage application is started before the completion of the injection of the recovery agent, the constant voltage application time is the constant voltage application time after the completion of the injection of the recovery agent.
[0037] In this step, when the recovery agent is injected, a recovery reaction such as that shown in FIG. 2 is thought to occur. FIG. 2 is an explanatory diagram showing an example of a recovery reaction scheme, and is an explanatory diagram showing a scheme in which the positive electrode active material is a lithium transition metal composite oxide. As shown in FIG. 2, the recovery agent reacts with the radical anion of an aromatic hydrocarbon compound (Are·- in FIG. 2) and a metal ion (Li + ) functions as a reducing agent that donates electrons, and reduces the amount of depleted positive electrode (Li in Figure 2). n-yBy applying the reducing agent to MeO2), electrons and metal ions are donated from the reducing agent to the positive electrode, and the capacity can be restored. If the recovery agent is simply injected and left in an open circuit state without applying a constant voltage, as shown in Figure 3, the positive electrode potential decreases as the recovery reaction progresses, and the potential difference △E between the positive electrode and the recovery agent, which is the driving force for the reaction, rec However, as the recovery reaction progresses, △E rec.1 >△E rec.2 >△E rec.3 Therefore, it is considered that the effect of the recovery agent gradually weakens. On the other hand, when the recovery agent is injected and a certain voltage is maintained by applying a constant voltage, as shown in Figure 4, the decrease in the positive electrode potential is suppressed by keeping the battery voltage constant, so that the potential difference ΔE between the positive electrode and the recovery agent, which is the driving force of the reaction, rec However, even if the recovery reaction proceeds, △E rec.1 ≒△E rec.2 ≒△E rec.3 It is considered that the charge is kept substantially constant. At this time, the electrons donated from the recovery agent to the positive electrode are immediately sent to the negative electrode by the application of a constant voltage, and the metal ions supplied to the positive electrode also move to the negative electrode, so that the positive electrode has an empty orbital that can accept metal ions and electrons while maintaining a high potential. As a result, even when an electrode with a relatively high resistance is used, it is considered that the reaction driving force can be kept high while recovering the battery capacity (while increasing the amount of metal ions in the battery). Therefore, it is considered that the recovery agent can be effectively used, and the capacity of the battery after recovery is further improved. In addition, it is considered that the activity of the radical anions of the aromatic hydrocarbon compound is appropriately suppressed by the application of a constant voltage, and the residual radical anions of the aromatic hydrocarbon compound are suppressed by the effective use of the recovery agent, so that the cycle capacity retention rate of the battery after recovery is also improved. In this way, the capacity of the nonaqueous electrolyte secondary battery is restored, and a nonaqueous electrolyte secondary battery with restored capacity (also called a restored battery) is obtained.
[0038] In the method for restoring a non-aqueous electrolyte secondary battery described above, the capacity of the non-aqueous electrolyte secondary battery can be restored by injecting a specific restoring agent. This is a novel method for restoring a non-aqueous electrolyte secondary battery that does not require a third electrode. In addition, in the method for restoring a non-aqueous electrolyte secondary battery, the capacity and cycle capacity retention rate of the battery after recovery can be further improved by injecting the restoring agent and maintaining a specific voltage by applying a constant voltage.
[0039] It goes without saying that the present disclosure is in no way limited to the above-described embodiment, and can be embodied in various forms as long as it falls within the technical scope of the present disclosure.
[0040] For example, in the above-mentioned embodiment, the method for recovering a nonaqueous electrolyte secondary battery has been described, but in this method for recovering a nonaqueous electrolyte secondary battery, a new nonaqueous electrolyte secondary battery with recovered capacity can be manufactured using a nonaqueous electrolyte secondary battery with deteriorated capacity. Therefore, the method for recovering a nonaqueous electrolyte secondary battery can also be said to be a method for manufacturing a nonaqueous electrolyte secondary battery. A nonaqueous electrolyte secondary battery may be manufactured using the above-mentioned method for recovering a nonaqueous electrolyte secondary battery. The method for manufacturing a nonaqueous electrolyte secondary battery may include a battery preparation step of preparing a capacity-deteriorated nonaqueous electrolyte secondary battery using a metal ion as a carrier ion, and a recovery step of recovering the capacity of the nonaqueous electrolyte secondary battery using the above-mentioned method for recovering a nonaqueous electrolyte secondary battery. The nonaqueous electrolyte secondary battery prepared in the battery preparation step may be the same as the deteriorated battery described in the above-mentioned embodiment. EXAMPLES
[0041] Hereinafter, examples of recovering a lithium ion battery using the method for recovering a non-aqueous electrolyte secondary battery of the present disclosure will be described as examples. Note that Experimental Examples 1 to 3 and 5 correspond to working examples, Experimental Examples 4 and 6 correspond to comparative examples, and Experimental Examples 7 to 14 correspond to reference examples. It goes without saying that the present disclosure is not limited to the following examples, and can be implemented in various forms as long as it falls within the technical scope of the present disclosure.
[0042] [Experimental Example 1] (Non-aqueous electrolyte secondary battery (battery before deterioration)) The positive electrode is LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 A positive electrode composite material containing 92 wt% O2 (NCM, Toda Kogyo Co., Ltd.), 5 wt% acetylene black (Denka Co., Ltd.), and 3 wt% polyvinylidene fluoride (Kureha Co., Ltd.) was used with a weight of 7 mg / cm. 2 The negative electrode was made of a negative electrode composite material containing 98 wt% graphite (OMAC1.5s, Osaka Gas Chemicals), 1 wt% carboxymethyl cellulose (Daicel), and 1 wt% styrene butadiene rubber (JSR), with a weight of 4 mg / cm. 2 The electrolyte was prepared by dissolving LiPF6 at a concentration of 1.1M in a mixed solvent containing 30 vol% ethylene carbonate, 40 vol% dimethyl carbonate, and 30 vol% ethyl methyl carbonate. A polypropylene separator impregnated with 1 mL of electrolyte was sandwiched between the positive and negative electrodes to prepare a laminate cell. This was used as the pre-degradation battery. The electrode area of the cell was 10 cm2 for both the positive and negative electrodes. 2 When the resistance of the battery before deterioration was measured with a digital multimeter, the cell resistance was 10 Ω cm 2 In this nonaqueous electrolyte secondary battery, the lower limit discharge voltage was 3.0V and the upper limit charge voltage was 4.1V, which are determined according to the battery configuration.
[0043] (Deteriorated battery) The laminated cell thus produced was charged to a capacity (SOC=50%) equivalent to 50% of the electric capacity of the cell in the voltage range of 3.0V to 4.1V, and Li was extracted from the positive electrode to obtain a positive electrode with a simulated reduced capacity (also called a degraded positive electrode). The cell was then disassembled, and the degraded positive electrode was removed. A laminated cell was produced in the same manner as the pre-degraded battery, except that the degraded positive electrode was used as the positive electrode. This was used as a degraded battery. The degraded battery was CC-charged at 0.9 mA to 4.1V, and then CC-discharged at 0.9 mA to 3.0V, and the discharge capacity was measured.
[0044] (Recovery Agent) In an inert atmosphere, naphthalene was dissolved in tetrahydrofuran (THF) solvent to a concentration of 1.0 mol / L, and then 1.0 mol / L of lithium metal was added and stirred to prepare a dark green radical anion liquid composition (lithium naphthalenide + THF) as a recovery agent stock solution by the reaction shown in the above formula (7).Then, the recovery agent stock solution and the above electrolyte were mixed in a volume ratio of 5:5 to prepare a recovery agent.
[0045] (Recovery of degraded batteries) The deteriorated battery was CC-charged at 0.9 mA to adjust the cell voltage to 3.7 V (adjustment process), a part of the deteriorated battery was opened under an argon atmosphere, 0.5 mL of the recovery agent was injected with a pipette, the opened part was sealed, and immediately after (within 3 minutes of injecting the recovery agent in the experimental example), a constant voltage of 3.7 V was applied to the deteriorated battery, and the constant voltage application was continued for 24 hours (recovery process). In this way, the deteriorated battery was restored, and a restored battery was obtained.
[0046] (Recovery battery evaluation) The discharge capacity of the recovered battery was measured in the same manner as the deteriorated battery, and the ratio of the discharge capacity of the recovered battery to the discharge capacity of the deteriorated battery (capacity ratio) was calculated. In addition, the recovered battery was subjected to 20 charge / discharge cycles at 1.8 mA in the voltage range of 3.0 V to 4.1 V, and the capacity retention rate at the 20th cycle relative to the capacity at the 1st cycle was calculated.
[0047] [Experimental Examples 2-4] Experimental Example 2 was the same as Experimental Example 1 except that the cell voltage and applied voltage in the adjustment process and recovery process were 3.9 V. Experimental Example 3 was the same as Experimental Example 1 except that the cell voltage and applied voltage in the adjustment process and recovery process were 4.0 V. Experimental Example 4 was the same as Experimental Example 1 except that the cell voltage and applied voltage in the adjustment process and recovery process were 4.1 V.
[0048] [Experimental Examples 5-6] Experimental Example 5 was the same as Experimental Example 3, except that the solvent of the recovery agent concentrate was dimethoxyethane (DME). Experimental Example 6 was the same as Experimental Example 4, except that the solvent of the recovery agent concentrate was dimethoxyethane (DME).
[0049] [Experimental Example 7] Experimental Example 7 was the same as Experimental Example 1, except that the following pre-degraded battery was used as the pre-degraded battery, the electrolyte-free recovery agent stock solution was used as is as the recovery agent, the degraded battery was CC-charged at 0.9 mA to adjust the cell voltage to 3.6 V, and then the recovery agent was injected in an open circuit state, and the open circuit state was maintained for 24 hours without applying a constant voltage.
[0050] (Battery before deterioration) The positive electrode is LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 A positive electrode composite material containing 85 wt% O2 (NCM, Toda Kogyo Co., Ltd.), 10 wt% acetylene black (Denka Co., Ltd.), and 5 wt% polyvinylidene fluoride (Kureha Co., Ltd.) was applied to the electrode with a weight of 5 mg / cm. 2 The negative electrode was made of a negative electrode composite material containing 98 wt% graphite (OMAC1.5s, Osaka Gas Chemicals), 1 wt% carboxymethyl cellulose (Daicel), and 1 wt% styrene butadiene rubber (JSR), with a basis weight of 3 mg / cm. 2 The electrolyte was prepared by dissolving LiPF6 at a concentration of 1.1M in a mixed solvent containing 30 vol% ethylene carbonate, 40 vol% dimethyl carbonate, and 30 vol% ethyl methyl carbonate. A polypropylene separator impregnated with 1 mL of electrolyte was sandwiched between the positive and negative electrodes to prepare a laminate cell. This was used as the pre-deterioration battery of Experimental Example 7. The electrode area of the cell was 10 cm2 for both the positive and negative electrodes. 2 When the resistance of the battery before deterioration was measured with a digital multimeter, the cell resistance was 5 Ω cm 2 In this nonaqueous electrolyte secondary battery, the lower limit discharge voltage was 3.0V and the upper limit charge voltage was 4.1V, which are determined according to the battery configuration.
[0051] [Experimental Example 8] Experimental Example 8 was the same as Experimental Example 7, except that the recovery agent used was a mixture of the recovery agent stock solution and the above-mentioned electrolyte solution in a volume ratio of 5:5.
[0052] [Experimental Examples 9-10] Experimental Example 9 was the same as Experimental Example 7, except that the solvent of the undiluted recovery agent solution was dimethoxyethane (DME). Experimental Example 10 was the same as Experimental Example 8, except that the solvent of the undiluted recovery agent solution was dimethoxyethane (DME).
[0053] [Experimental Examples 11-14] Experimental Example 11 was the same as Experimental Example 1 except that the recovery process was performed in an open circuit state. Experimental Example 12 was the same as Experimental Example 2 except that the recovery process was performed in an open circuit state. Experimental Example 13 was the same as Experimental Example 3 except that the recovery process was performed in an open circuit state. Experimental Example 14 was the same as Experimental Example 4 except that the recovery process was performed in an open circuit state.
[0054] [Results and Discussion] The results of Experimental Examples 1 to 14 are summarized in Table 1. First, the addition of an electrolyte to the recovery agent stock solution was examined. In Experimental Examples 7 and 9, in which an electrolyte was not added to the recovery agent stock solution, the capacity ratio and cycle capacity retention rate of the recovered battery relative to the degraded battery were lower than those in Experimental Examples 8 and 10, in which an electrolyte was added to the recovery agent stock solution. The reason for this is presumed to be as follows. For example, a lithium naphthalenide liquid composition prepared using a THF solvent exhibits a high reducing power of 0.64 V based on Li metal (Reference: Electrochimica Acta 180 (2015) 629-635). When the lithium naphthalenide liquid composition and the electrolyte were mixed at a ratio of 5:5, the reducing power was 1.2 V to 1.9 V based on Li metal, and the reducing power was mitigated. In Experimental Examples 7 and 9, in which an electrolyte was not added to the recovery agent stock solution, it was presumed that a reaction that inhibited capacity recovery occurred because the lithium naphthalenide liquid composition was injected in a state of strong reducing power. On the other hand, in Experimental Examples 8 and 10, in which an electrolyte was added to the recovery agent stock solution, the reducing power of the lithium naphthalenide liquid composition was alleviated by the electrolyte, and the reaction that inhibits the capacity recovery and the capacity maintenance after recovery was suppressed, so that it was presumed that the capacity recovery effect and the capacity maintenance effect after recovery were sufficiently obtained. Note that, in Experimental Examples 8 to 11, the recovery agent was injected in an open circuit state, but when the recovery agent was injected in a constant voltage state, it was presumed that the reducing power of the lithium naphthalenide liquid composition was suppressed to a certain extent by applying a constant voltage, even if an electrolyte was not added to the recovery agent stock solution.
[0055] The solvent used to prepare the recovery agent stock solution was examined. In Experimental Example 10, in which DME was used to prepare the recovery agent stock solution, the capacity ratio to the deteriorated battery in the recovered battery was slightly lower than in Experimental Example 8, in which THF was used, but the cycle capacity retention rate was high, and the balance between the two was good. From this, it was inferred that DME is more suitable as the solvent to use in preparing the recovery agent stock solution.
[0056] The influence of the internal resistance of the pre-degraded battery was examined. In Experimental Example 10, in which the internal resistance of the non-aqueous electrolyte secondary battery was relatively small, the restored battery had a high capacity ratio and cycle capacity retention rate relative to the degraded battery even in an open circuit state. On the other hand, in Experimental Examples 11 to 14, in which the internal resistance of the pre-degraded battery was relatively large, the capacity ratio and cycle capacity retention rate relative to the degraded battery were lower than those of Experimental Example 10 in an open circuit state. From the above, it was found that the higher the internal resistance of the pre-degraded battery, the more difficult it is to obtain the effect of capacity recovery and the effect of maintaining cycle capacity after recovery. This is presumably because the higher the internal resistance, the higher the overvoltage (E=RI) caused by the internal resistance (R), and therefore the potential difference between the recovery agent and the positive electrode, which is the driving force of the recovery reaction, is reduced, and the reaction driving force is likely to decrease as shown in FIG. 3.
[0057] A study was conducted on the case where a predetermined voltage was maintained by applying a constant voltage. In Experimental Examples 1 to 3 and 5, in which a predetermined voltage lower than the cell voltage (4.1 V) in a fully charged state was maintained by applying a constant voltage, the capacity ratio of the restored battery was larger and the cycle capacity retention rate was also larger than in Experimental Examples 11 to 14, in which an open circuit state was established. This is presumed to be because, in Experimental Examples 1 to 3 and 5, the reaction driving force in the recovery reaction was maintained at a high state by maintaining a constant voltage. In particular, in Experimental Example 5, in which DME was used to prepare the recovery agent stock solution, the capacity ratio to the deteriorated battery and the cycle capacity retention rate were higher than in Experimental Example 3, which was the same except that THF was used. It was predicted from Experimental Examples 7 to 10 that the cycle capacity retention rate would be significantly reduced if THF was used to prepare the recovery agent stock solution, but the cycle capacity retention rate was also good in Experimental Examples 1 to 3, in which a predetermined voltage was maintained by applying a constant voltage. On the other hand, in the restored batteries of Experimental Examples 4 and 6, in which the same voltage as the cell voltage in the fully charged state (4.1 V) was maintained by applying a constant voltage, the capacity was lower than that of the degraded battery, and the cycle capacity retention rate was also lower. In particular, in Experimental Example 6, the battery stopped working immediately after the recovery agent was injected. This was presumably because at the fully charged voltage, substantially all of the metal ions were supplied to the negative electrode, and did not contribute to the capacity recovery of the positive electrode. From the above, it was found that the capacity and cycle capacity retention rate of the restored battery can be increased compared to the degraded battery by injecting the recovery agent and maintaining a predetermined voltage lower than the cell voltage in the fully charged state by applying a constant voltage.
[0058] [Table 1] [Explanation of symbols]
[0059] 20 nonaqueous electrolyte secondary battery, 21 battery case, 22 positive electrode, 23 negative electrode, 24 separator, 25 gasket, 26 sealing plate, 27 nonaqueous electrolyte.
Claims
1. A method for recovering the capacity of a non-aqueous electrolyte secondary battery that uses metal ions as carrier ions, comprising the steps of: a recovery step of injecting a recovery agent, which is a solution containing an aromatic hydrocarbon compound in a reduced state and the same type of metal ion as the carrier ion, into the nonaqueous electrolyte secondary battery, and maintaining a predetermined voltage lower than a full charge voltage by applying a constant voltage, thereby recovering the capacity of the nonaqueous electrolyte secondary battery. A method for recovering a non-aqueous electrolyte secondary battery.
2. In the recovery step, the recovery agent containing at least one of a reduced form of a compound of formula (1) and a reduced form of a compound of formula (2) is used as the aromatic hydrocarbon compound in a reduced state. The method for restoring a nonaqueous electrolyte secondary battery according to claim 1 . 【Chemistry 1】
3. In the recovery process, the predetermined voltage is set to 3.0 V or more and 4.0 V or less. The method for restoring a nonaqueous electrolyte secondary battery according to claim 1 or 2.
4. In the recovery step, the recovery agent is used, the recovery agent including the aromatic hydrocarbon compound in a reduced state, metal ions of the same kind as the carrier ions, and one or more solvents selected from tetrahydrofuran and dimethoxyethane. The method for restoring a nonaqueous electrolyte secondary battery according to any one of claims 1 to 3.
5. In the recovery step, the recovery agent is used, the recovery agent including a recovery agent stock solution including the aromatic hydrocarbon compound in a reduced state and the same metal ion as the carrier ion, and an electrolyte. The method for restoring a non-aqueous electrolyte secondary battery according to any one of claims 1 to 4.
6. a battery preparation step of preparing a capacity-degraded nonaqueous electrolyte secondary battery having metal ions as carrier ions; The method for recovering a capacity of a nonaqueous electrolyte secondary battery according to any one of claims 1 to 5, comprising: The method for producing a non-aqueous electrolyte secondary battery includes the steps of:
Citation Information
Patent Citations
Liquid composition and manufacturing method thereof, non-aqueous electrolyte secondary battery and capacity recovery method thereof
CN112490506A
Nonaqueous electrolyte secondary battery apparatus, and method for charging anode of the same
JP2011165343A
Nonaqueous electrolytic secondary battery
JP2013069659A
Lithium ion secondary battery and battery system
JP2016076358A
Lithium ion secondary battery and method for manufacturing the same
JP2018147669A