Polyamic acid solution, transparent polyimide resin using same, and transparent substrate

A polyamic acid solution combining fluorinated and non-fluorinated aromatic diamines and dianhydrides enhances the transparency, mechanical strength, and thermal stability of polyimide resins, addressing the limitations of conventional polyimide resins for flexible display applications.

JP7564854B2Active Publication Date: 2024-10-09DOOSAN CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022177874
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-12-08
Filing Date
2022-11-07
Publication Date
2024-10-09
Estimated Expiration
2038-12-07

AI Technical Summary

Technical Problem

Conventional polyimide resins are colored and have low visible light transmittance, limiting their use in applications requiring transparency, and they lack sufficient thermal and mechanical properties for flexible display devices.

Method used

A polyamic acid solution is formulated using a mixture of fluorinated and non-fluorinated aromatic diamines and dianhydrides, along with an organic solvent, to produce a transparent polyimide resin with improved optical, mechanical, and thermal properties.

Benefits of technology

The solution results in a polyimide resin with high light transmittance, low yellowness, high elastic modulus, and excellent bending resistance, suitable for flexible display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564854000001
    Figure 0007564854000001
  • Figure 0007564854000002
    Figure 0007564854000002
  • Figure 0007564854000003
    Figure 0007564854000003
Patent Text Reader

Abstract

It has excellent optical and mechanical properties, making it suitable for use as a substrate for flexible display devices. To provide a transparent polyimide resin film and a transparent substrate. [Solution] (a) (a-1) a fluorinated aromatic diamine and (a-2) a non-fluorinated aromatic diamine (b) (b-1) a fluorinated aromatic dianhydride and (b- 2) a dianhydride mixture containing a non-fluorinated dianhydride containing an amide group; and (c) an organic solvent; and the content of the (b-1) fluorinated aromatic dianhydride is 50 to 95 mol % relative to 100 mol % of the (b) dianhydride mixture, The content of the (b-2) non-fluorinated dianhydride containing an amide group is 0.1 to 30 mol% of the polyamic acid solution relative to 100 mol% of the anhydride mixture. liquid.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention can be applied to cover windows, protective films or substrates for flexible display devices. Polyamic acid solution capable of being used for producing transparent polyimide resin film and transparent Regarding the substrate. [Background technology]

[0002] Generally, polyimide (PI) resin is a compound made of aromatic dianhydride and Solution polymerization of aromatic diamine or aromatic diisocyanate After this, the polyamic acid derivative is desorbed at high temperature. Refers to a highly heat-resistant resin produced through the imidazation process, which involves hydrocyclization. vinegar.

[0003] Such polyimide resin is an insoluble and infusible resin with extremely high heat resistance, and has excellent thermal oxidation resistance and heat resistance. It has excellent properties such as durability, radiation resistance, low temperature resistance, and chemical resistance, and is used in automotive materials, aviation and space applications. Heat-resistant advanced materials such as spacecraft materials, insulating coating materials, insulating films, semiconductors, L It is widely used in electronic materials applications such as electrode protection films for CDs.

[0004] However, polyimide resins tend to be colored brown or yellow due to the high density of aromatic rings. This results in low transmittance in the visible light range, making it difficult to use in areas where transparency is required. To solve this problem, a method was developed in which monomers and solvents were highly purified and then polymerized. However, the transmittance has not been significantly improved. Issue 480 discusses the use of aliphatic cyclic dianhydrides instead of aromatic dianhydrides. Although the method improves transparency and color, it is difficult to obtain a satisfactory level of high transmittance. Furthermore, there is a problem that the thermal and mechanical properties are deteriorated. Conventional polyimide resins have had limitations in their use in fields where transparency is required.

[0005] However, in order to use polyimide resin as a substrate or optical film, excellent In addition to excellent transparency, a low coefficient of thermal expansion is required to minimize warping and twisting. In addition, a plastic substrate made of polyimide resin was used instead of a glass substrate. Flat panels such as LCDs, LCD displays, and OLED displays To be applied to flat panel displays (FPD) It is necessary for the optical glass to have excellent optical properties and heat resistance, and excellent mechanical properties are also required.

[0006] Therefore, in order to be applicable as a display device material, it is necessary to provide a high transparency like a glass substrate. A polyamide resin is used to produce a transparent plastic substrate having good thermal and mechanical properties while maintaining the same thermal and mechanical properties. There is a need to develop a solution of carboxylic acids. Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention introduces a monomer having a rigid structure. By using a specific A diamine monomer having the structure and a dianhydride monomer containing an amide group are mixed. By combining these materials and adjusting their amounts, it is possible to maintain excellent optical properties while improving mechanical properties and The object of the present invention is to provide a polyamic acid solution having improved thermal properties.

[0008] The present invention also provides a method for producing a polyamic acid solution having low yellowness and high light transmittance. Polyimide resin film with improved mechanical properties and LCD and OLED frames Transparent plastic substrates for flexible display devices, TFT substrates, flexible printed circuit boards, We provide transparent substrates that can be used for flexible OLED surface lighting substrates, electronic paper substrate materials, etc. The purpose is to provide [Means for solving the problem]

[0009] In order to achieve the above object, the present invention provides a method for producing a fluorinated aromatic diamine comprising the steps of: (a) (a-1) a fluorinated aromatic diamine and ( (a-2) a non-fluorinated aromatic diamine mixture; (b) (b-1 ) Fluorinated aromatic dianhydrides and (b-2) Non-fluorinated dianhydrides containing amide groups (c) a dianhydride mixture containing a polyamic acid solution containing an organic solvent; Provide the liquid.

[0010] The present invention also relates to a transparent polyimide resin produced by imidizing the polyamic acid solution. Provides a greasy film.

[0011] The present invention further provides a transparent substrate comprising the transparent polyimide resin film. Effect of the Invention

[0012] According to the present invention, fluorinated aromatic diamines, non-fluorinated aromatic diamines, fluorinated aromatic The monomers used were aromatic dianhydrides and non-fluorinated dianhydrides containing amide groups. By synthesizing polyimide resin using this material, it is possible to obtain high light transmittance, low yellowing, high elasticity, and strength. It is possible to provide a polyamic acid composition that can exhibit high yield strain and flex resistance.

[0013] According to the present invention, the polyamide resin has high light transmittance and a high glass transition temperature. By applying the acid composition to the substrate, it is possible to develop a flexible substrate that exhibits excellent physical properties and product reliability. It is possible to provide a substrate for a blue display device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention will be described in detail below. However, the examples described below are merely illustrative, and the present invention is not limited to these examples. The present invention is not limited thereby, but is instead indicated by the scope of the claims that follow.

[0015] <Polyamic acid solution> The polyamic acid solution according to the present invention has high transparency and excellent optical properties while being functional. The purpose of the present invention is to produce a polyimide resin film having improved mechanical and thermal properties. (a) (a-1) a fluorinated aromatic diamine and (a-2) a non-fluorinated aromatic diamine (b) (b-1) Aromatic diamine mixture containing a fluorinated aromatic dianhydride and ( b-2) A mixture of non-fluorinated dianhydrides containing an amide group and a dianhydride containing and (c) an organic solvent.

[0016] (a) Aromatic diamine mixture The polyamic acid solution according to the present invention contains, as an aromatic diamine component, (a-1) a fluorinated The diamines include both aromatic diamines and (a-2) non-fluorinated aromatic diamines.

[0017] The polyamic acid solution contains a fluorinated aromatic diamine having a fluorine substituent introduced therein. In this case, the charge transfer effect occurs due to the fluorine substituent in the monomer. This reduces the ion exchange effect and allows the production of polyimide resin with excellent optical properties. do.

[0018] The fluorinated aromatic diamine may be mixed with a non-fluorinated aromatic diamine to produce a desired product. In this case, the reactivity of non-fluorinated aromatic diamines with dianhydrides containing amide groups is examined. Easily adjust the viscosity of polyamic acid solution to the range of 1,000~50,000cps. In addition, compared to when only a non-fluorinated aromatic diamine is used, It is possible to produce polyimide resins with improved optical and mechanical properties. .

[0019] The fluorinated aromatic diamine (a-1) used in the present invention is an aromatic diamine containing fluorine. There is no particular limitation as long as it is an aromatic diamine. However, among fluorinated aromatic diamines, fluorinated aromatic diamines are preferred. The diamine containing a halogenated biphenyl structure adjusts the reactivity with the dianhydride and Improve the thermal properties of polyimide resins by achieving high glass transition temperature and low thermal expansion. It is possible.

[0020] The fluorinated aromatic diamines include 2,2'-bis(trifluoromethyl)-4, 4'-Diaminobiphenyl (2,2'-Bis(trifluoromethyl)-4 ,4'-diaminobiphenyl, 2,2'-TFDB), bisaminohydroxy Bis aminohydroxy phenyl hexafluoropropane hexafluoropropane, DBOH), bisaminophenoxyphenyl Bisaminophenoxy phenyl hexafluoropropane luoropropane, 4BDAF), 2,2'-bis(trifluoromethyl)-4 ,3'-Diaminobiphenyl(2,2'-Bis(trifluoromethyl)- 4,3'-diaminobiphenyl), 2,2'-bis(trifluoromethyl) -5,5'-diaminobiphenyl (2,2'-Bis(trifluoromethyl )-5,5'-diaminobiphenyl), etc. In addition, when 2,2'-TFDB is used, The objective of the present invention is to increase the transparency and glass transition temperature of polyimide resin and to reduce the thermal expansion coefficient. can be done.

[0021] The content of such a fluorinated aromatic diamine is not particularly limited, but The amount of the mixture may be 50 to 99.9 mol % based on 100 mol % of the mixture, and preferably 70 In the case where a fluorinated diamine is contained within the above range, the fluorine in the monomer is The substituents reduce the electromigration effect and improve the optical properties of the polyimide resin.

[0022] The non-fluorinated aromatic diamine (a-2) used in the present invention does not contain fluorine. However, the non-fluorinated aromatic diamine is not particularly limited as long as it has a high In order to realize high mechanical strength and excellent optical properties, a monomer with a rigid structure is used. Such non-fluorinated aromatic diamines include phenyl, biphenyl, It can be a monomer containing a sulfone group (SO2), a silane group (Si), or the like.

[0023] The non-fluorinated aromatic diamines include oxydianiline. e, ODA), 4,4'-diamino-2,2'-dimethylbiphenyl (4,4'-Dia mino-2,2'-dimethylbiphenyl, m-Tolidine), Paraphenylenediamine (p-PDA), Meta phenylenediamine (m-PDA) , Bis aminophenoxy phenylpropane nylpropane, 6HMDA), bisaminophenoxydiphenylsulfone (Bi s aminophenoxy diphenylsulfone, DBSDA), 4, 4'-Diaminodiphenyl sulfone lfone, 4,4'-DDS), 3,3'-diaminodiphenylsulfone (3,3'- Diaminodiphenyl sulfone, 3,3'-DDS, bis(carbocyanide) Bis(carboxyphenyl)dimethylsilane These may be used alone or in combination of two or more. In addition, p-PDA, m-PDA or m-Tolidine can be used. In this case, the optical properties of the polyimide resin are improved without deteriorating the thermal properties.

[0024] The content of such non-fluorinated aromatic diamine is not particularly limited. The amount of the fluorine-containing compound may be 0.01 to 50 mol % based on 100 mol % of the mixture, and preferably 0. When the non-fluorinated aromatic diamine is contained within the above range, the poly The optical properties (light transmittance and yellowness index) of the imide resin are improved.

[0025] The aromatic diamine (a) according to the present invention is capable of providing a polyimide resin with high transparency and a high glass transition temperature. In consideration of low yellowness, (a-1) 2,2'-TFDB as a fluorinated aromatic diamine (a-2) m-Tolidine, p It is preferable to use a mixture of poly-PDA and m-PDA. The polymer of the polyimide resin can be induced to have a linear shape.

[0026] (b) Dianhydride mixture The polyamic acid solution according to the present invention contains, as a dianhydride component, (b-1) a fluorinated Aromatic dianhydrides and (b-2) non-fluorinated compounds containing amide groups and dianhydrides.

[0027] In the polyamic acid solution, a fluorinated aromatic dianhydride and an amide group-containing When used in combination with a non-fluorinated dianhydride, the optical properties and The thermal properties are improved at the same time. This makes it possible to produce polyimide resins with excellent optical properties. The rigid amide group of the non-fluorinated dianhydride provides excellent thermal properties. This makes it possible to produce polyimide resins with high molecular weight.

[0028] The fluorinated aromatic dianhydride (b-1) used in the present invention contains fluorine. There are no particular limitations on the aromatic dianhydride as long as it satisfies the above requirements.

[0029] The fluorinated aromatic dianhydride may be 2,2-bis(3,4-dicarboxyfluoride). 2,2-Bisphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride (3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafl uoropropane dianhydride, 6FDA), 4-(trifluoromethyl 4-(trifluoromethyl)pyromellitic dianhydride llitic dianhydride, 4-TFPPMDA), 9,9-bis(trifluoroethylene) (fluoromethyl)-9H-xanthene-2,3,6,7-tetracarboxylic acid dianhydride (9 ,9'-Bis(trifluoromethyl)-9H-xanthene-2,3 ,6,7-tetracarboxylic dianhydride, 6FCDA) These can be used alone or in combination of two or more. When 6FDA is used, inter- and intrachain charge transfer complexes By controlling the formation of CTC (Constant Complex), the The optical properties are improved.

[0030] The content of such a fluorinated aromatic dianhydride is not particularly limited, but may be, for example, The amount of the fluoride may be 10 to 95 mol % based on 100 mol % of the fluoride mixture, and preferably 5 The content is 0 to 90 mol %.

[0031] (b-2) Non-fluorinated dianhydride containing an amide group used in the present invention The amide group [-C(=O)-NH-] is introduced to form aromatic or is not particularly limited as long as it is a non-aromatic dianhydride. (moiety) is a non-fluorinated aromatic diamine component (a-2). The structure of the aromatic diamine may be the same as or different from that of the aromatic diamine. The amide group-containing moiety in the fluorinated dianhydride is a non-fluorinated aromatic diamine. If the structure is the same or similar, hydrogen bonds between the polymer main chains are induced. It is expected that the heat resistance and mechanical properties of the polymer will be improved. do.

[0032] The non-fluorinated dianhydride containing an amide group is a compound represented by the following formula 1. There can be.

[0033] [ka] (Wherein, A is C6 to C 40 is an arylene group or a sulfone group (-S(=O)-) of A's are the same or different, m is an integer of 1 to 3, and B is an aromatic ring or or an aliphatic ring, X1 and X2 are the same or different and each independently represent a hydrogen atom. , halogen, and C1 to C6 alkyl groups, 40 Ants The olefin group can be substituted with a C1 to C6 alkyl group.

[0034] In the compound represented by Chemical Formula 1, A is one or more C6-C 40 of An arylene group, a sulfone group, or a form in which an arylene group and a sulfone group are linked (e.g. For example, C6~C 40 Arylene-sulfonic acid group, C6-C 40 Arylene-sulfone group -C6~C 40 Specifically, m is 1. A is an arylene group or a sulfone group, and m is 2 or 3. In the case where A is a substituted or unsubstituted aryl group, A represents a linkage between one or more arylene groups and one or more sulfone groups. That is, a plurality of A's may be the same or different, and each independently represents C6 to C 40 No.A An arylene group or a sulfone group. Here, "arylene" means a group having 6 to 40 carbon atoms. It refers to a divalent substituent derived from an aromatic hydrocarbon. Specific examples of such arylene include , phenylene, biphenylene, triphenylene, sulfondiphenylene, etc. .

[0035] In particular, A is preferably selected from the group of substituents represented by the following chemical formula: It is nice.

[0036] [ka] In the formula, * is a site connected to the formula 1. R1 to R3 are each the same or Each of R1 is independently hydrogen or a C1 to C6 alkyl group. Each of R3 can independently be hydrogen or methyl.

[0037] B is an aromatic or aliphatic ring as known in the art, and may be a 6-membered aromatic ring or a 6-membered aliphatic ring. When B is a 6-membered aromatic ring, the diam- The dianhydride is an aromatic dianhydride containing an amide group, and when B is a six-membered aliphatic ring, In this case, the dianhydride in formula 1 is a non-aromatic dianhydride containing an amide group. It is possible.

[0038] According to one embodiment of the present invention, the compound represented by Chemical Formula 1 can be prepared by the synthesis of diazonium chloride, as shown in the following synthesis formula 1: A with an amine group and trimellitic anhydride chloride Aromatic diamines obtained by reacting with triamine hydrochloride (TAC) or, as shown in the synthesis scheme 2 below, A is linked to a diamine group, and 1,2 ,4-Cyclohexanetricarboxylic acid-1,2-anhydride-4-chloride (1,2,4-C yclohexanetricarboxy acid-1,2-anhydride- 4-chloride, HTAC) to obtain a non-aromatic dianhydride monomer. It can be a body.

[0039] [Synthesis formula 1] [ka]

[0040] [Synthesis formula 2] [ka] In the formula, A and m are defined as in Chemical Formula 1 above.

[0041] The compound represented by Chemical Formula 1 has an acyclic aryl group having a rigid structure between the dianhydrides. The introduction of rylene groups and / or sulfone groups allows the compound to be decomposed by heat or light. Since it is stable against external shocks, the polyimide resin produced using this product has excellent optical properties. The chemical properties, thermal properties, and mechanical properties (strength, bending resistance) are significantly improved. The compound represented by 1 is a dianhydride with an amide group, which is a good hydride. It reacts with the oxygen atom in the anhydride monomer to form a hydrogen bond, which then attaches it to the main chain of the polymer. This creates a certain degree of bonding strength, which significantly improves the mechanical and heat resistance properties of the polyimide resin. It will be improved.

[0042] The compound represented by Chemical Formula 1 is a metaphenylenediamine, as shown in the following chemical formula group: bis( Trimellitic anhydride ) (Methaphenylenediamine bis( Trimeric anhydride ) , MPTA), paraphenylene Diamine bis( Trimellitic anhydride ) (Paraphenylenediamine bis( Trimeric anhydride ) , PPTA), Bis(octahydro-1,3-dioxo-5-isobenzofuran carboxylic acid) 1,4-phenylenediamide (PPHT), Bis(octahydro-1,3-dioxo-5-isobenzofuran carboxylic acid) 4,4'-sulfonyl dianilide (PSHT), etc., which can be used alone or in combination of two or more.

[0043] [ka]

[0044] The content of such fluorinated dianhydride containing an amide group is not particularly limited. may be 0.1 to 50 mol % based on 100 mol % of the dianhydride mixture; The content is preferably 0.5 to 30 mol %. When an anhydride is contained, the high transmittance and low yellowness of the polyimide resin are maintained, while the polyimide resin is The heat resistance of the polyimide resin is improved.

[0045] The polyamic acid solution according to the present invention further comprises, as a dianhydride component, (b-3) a lipid It may further comprise a cyclic dianhydride.

[0046] The alicyclic dianhydride may be pyromellitic dianhydride. ic dianhydride PMDA), cyclobutane-1,2,3,4-tetracarboxylic acid Cyclobutane-1,2,3,4-tetracarboxylic acid dianhydride ylic dianhydride (CBDA), 1,2,3,4-cyclopentanetetraacetate Cyclopentane tetracarboxylic dianhydride (1,2,3,4-Cyclopentane tetracarboxamide boxylic dianhydride, CPDA), 3,3',4,4'-biphenyl 3,3',4,4'-Biphenyltetracarboxylic dianhydride boxylic dianhydride, BPDA, etc. or a mixture of two or more of them can be used.

[0047] The content of such alicyclic dianhydrides is not particularly limited, but the dianhydride mixture may be The amount of the aryl group may be 0.1 to 30 mol % relative to 100 mol % of the mixture, and preferably 5 to 25 It is in mole percent.

[0048] As described above, in one embodiment of the present invention, the aromatic diamine component is (a-1) fluorine (a-1) a fluorinated aromatic diamine and (a-2) a non-fluorinated aromatic diamine are used as dianhydride components. (b-1) fluorinated aromatic dianhydrides and (b-2) non-fluorinated dianhydrides containing amide groups In this case, (a) an aromatic diamine mixture and (b) an aromatic dianhydride are mixed and used. b) The dianhydride mixture is used to improve the yellowness and yield strain of polyimide resin. They can be mixed in a weight ratio of (a):(b)=1:0.1-10.

[0049] (c) Organic Solvent The organic solvent according to the present invention is not particularly limited as long as it is known in the art. The solvents used were m-cresol, N-methyl-2-pyrrolidone (NMP), N,N-dimethyl Dimethylformamide (DMF), dimethylacetamide (DMAc), dimethylsulfoxide Polar solvents such as diethyl ether (DMSO), acetone, and diethyl acetate; THF), low boiling point solvents such as chloroform; low absorption solvents such as γ-butyrolactone, etc. These can be used alone or in combination of two or more.

[0050] In the polyamic acid solution according to the present invention as described above, the aromatic diamine mixture, The content of the anhydride mixture and the organic solvent is not particularly limited, but the polyamic acid solution (a) 6 to 10% by weight of the aromatic diamine mixture, (b) diamine The hydride mixture may be 6 to 10% by weight, and the remainder may be the organic solvent. When the content of each component in the triamic acid solution is less than the above range, the polyamide If the viscosity of the polyamic acid solution becomes too low and exceeds the above range, the polyamic acid solution may be deformed. The viscosity of the acid solution may become excessively high. If the content of each component in the polyamic acid solution is adjusted to be within the above-mentioned range, Approximately 1,000 to 50,000 cps (preferably, approximately 2,000 to 35,000 cps) In addition, it is possible for the viscosity of the polyamic acid solution to be within the above range. If the thickness is adjusted, it is easy to adjust the thickness of the polyamic acid solution. The surface of the coated film is then uniform.

[0051] On the other hand, the polyamic acid solution according to the present invention may be modified as necessary without impairing the objects and effects of the present invention. Plasticizers, antioxidants, flame retardants, dispersants, viscosity adjusters, leveling agents, etc., within the limits of their usefulness. It may contain small amounts of any of the additives.

[0052] By carrying out the solution polymerization reaction of the polyamic acid solution according to the present invention as described above, polyamic acid Specifically, a fluorinated aromatic diamine and a non-fluorinated aromatic diamine are mixed to obtain a fluorinated acid solution. is put into an organic solvent and dissolved, and then a fluorinated aromatic dianhydride and an amide group are added thereto. A non-fluorinated dianhydride containing In this case, the reaction conditions are not particularly limited, and the reaction is carried out at -20 to 80°C for 1 to 12 hours. The reaction can be carried out for a period of time (preferably 1 to 5 hours).

[0053] <Transparent polyimide resin film> The present invention relates to a transparent polyimide film produced by imidizing the above-mentioned polyamic acid solution. Provides a program.

[0054] Polyimide resin is a random copolymer. or in the form of a block copolymer.

[0055] The transparent polyimide resin film according to the present invention is produced using the polyamic acid solution. This results in improved mechanical properties (elastic modulus, strength) as well as optical properties (transparency and yellowness). Excellent thermal properties (thermal expansion coefficient and glass transition Specifically, the transparent polyimide resin film according to the present invention has Because of its rigid chemical structure, when the film is 20 μm thick, the wavelength is 550 The light transmittance at wavelength 550 nm is 89% or more, and the yellowness at wavelength 550 nm is 1.06% or more. The modulus of elasticity (Modul us) is 5.5 GPa or more (preferably, 6.0 GPa or more), and the mechanical strength (St strength) is 155 MPa or more (preferably 160 MPa or more), (Yield strain) is 5% or more (preferably 5.5% or more), and bending resistance is The resistance (times / R@1.0mm) is more than 200,000 times, and the glass transition temperature is 350 to The temperature is 450°C.

[0056] In addition, the transparent polyimide resin film according to the present invention has heat resistance because it contains imide groups. It has excellent chemical resistance, abrasion resistance and electrical properties.

[0057] The method for producing such a transparent polyimide resin film is not particularly limited, but for example, For example, the polyamic acid solution is coated (cast) on a glass substrate, and then, The temperature is gradually increased from 30 to 350°C, and the imidization reaction is continued for 0.5 to 8 hours. ation), a polyimide resin film can be produced.

[0058] The coating method is not particularly limited as long as it is a method well known in the art. For example, spin coating, dip coating, etc. oating, Solvent casting, Slot die casting Slot die coating, Spray coat method ting) etc.

[0059] The thickness of the transparent polyimide resin film is not particularly limited, but is preferably from several hundred nm to several tens of μm. The thickness of the polyamic acid solution is adjusted by coating the solution once or more. This can be done.

[0060] Such a transparent polyimide resin film can be used in various fields, and in particular, Displays and liquid crystal devices for organic electroluminescent devices (OLEDs) that require brightness and heat resistance For displays, TFT substrates, flexible printed circuit boards, flexible OLED surface lighting Substrates for flexible displays such as substrates, substrate materials for electronic paper, and protective films This can be applied.

[0061] <Transparent substrate> The present invention provides a transparent substrate using the above-mentioned polyamic acid solution.

[0062] The transparent substrate is a transparent polyimide resin produced by imidizing the polyamic acid solution. The transparent substrate can be formed by laminating one or more layers of a resin film. The thin film substrate can exhibit high transparency like a glass substrate and also have improved mechanical strength.

[0063] Therefore, the transparent substrate according to the present invention can be applied in various fields, and in particular, has high transparency and Heat resistance is required for flexible displays such as OLED displays and LCD displays. It can be used as a substrate for a blue display device. EXAMPLES

[0064] The present invention will be described in detail below based on examples and comparative examples. The comparative examples are not intended to be limiting in any way.

[0065] [Example 1] Preparation of transparent polyimide film 1-1. Preparation of polyamic acid solution In a 100-mL three-neck round-bottom flask, add 9 mL of N,N'-dimethylacetamide (DMAc). After adding 8.8 g, the temperature of the flask was raised to 50° C. Next, 2,2' 10.0 g of TFDB was added, and 30 minutes later, 0.8 g of m-PDA was added. This was stirred for 1 hour. The flask was then stirred to completely dissolve 2,2'-TFDB and m-PDA. 3.6 g of TA and 13.8 g of 6FDA were added in turn and dissolved at 50° C. The solid content was 20%. The mixture was then stirred for 3 hours to react. After the reaction between the monomers was completed, After natural cooling, the polyamic acid solution (solution viscosity at 25°C: 96 poise (9,600 CPs) were produced.

[0066] 1-2. Manufacturing of transparent polyimide film The polyamic acid solution obtained in Example 1-1 was spin-coated onto LCD glass. After that, it was heated in a convection oven at 80°C for 30 minutes and at 150°C for 30 minutes under a nitrogen atmosphere. The temperature was gradually increased to 100°C for 1 hour, 200°C for 1 hour, and 300°C for 30 minutes, and then the film was dried and imidized. As a result, a transparent polyimide film with a thickness of 20 μm was obtained. Imide resin film (imidization rate: 85% or more) was produced. The film was peeled off to obtain a transparent polyimide resin film.

[0067] [Example 2] Preparation of transparent polyimide film 0.8 g of p-PDA instead of m-PDA, and 3.6 g of PPTA instead of MPTA A polyamic acid solution (solution viscosity at 25°C: 91 poise (9,100 CPs) was produced.

[0068] The polyamic acid solution was used to prepare a transparent polyimide resin film in the same manner as in Example 1-2. The imidization rate was 85% or more.

[0073] [Example 5] Preparation of transparent polyimide film DMAc 99.1g, 2,2'-TFDB 11.7g, p- Except for the use of 0.4 g of PDA, 5.5 g of MPTA, and 12.6 g of 6FDA, In the same manner as in Example 1-1, a polyamic acid solution (solution viscosity at 25°C: 97.5 poise) was prepared. (9,750CPs) was produced.

[0074] The polyamic acid solution was used to prepare a transparent polyimide resin film in the same manner as in Example 1-2. The imidization rate was 85% or more.

[0075] [Example 6] Preparation of transparent polyimide film DMAc 99.1g, 2,2'-TFDB 11.7g, p- 0.4g of PDA, 5.6g of PPTA instead of MPTA, and 12.6g of 6FDA were used. A polyamic acid solution (solution viscosity at 25° C.: 10 1 poise (10,100 CPs) was produced.

[0076] The polyamic acid solution was used to prepare a transparent polyimide resin film in the same manner as in Example 1-2. The imidization rate was 85% or more.

[0077] [Example 7] Preparation of transparent polyimide film DMAc 99.1g, 4,4'-DDS 0.8g instead of m-PDA, MPTA and 1.6 g of MPTA, 1.6 g of PPTA, and 12 g of 6FDA instead of 6FDA. The same procedure as in Example 1-1 was repeated except that 0.3 g of polyamic acid solution (solution at 25° C.) was used. Viscosity: 80 poise (8,000 CPs) was produced.

[0078] The polyamic acid solution was used to prepare a transparent polyimide resin film in the same manner as in Example 1-2. The imidization rate was 85% or more.

[0083] [Example 10] Preparation of transparent polyimide film DMAc 101.9g, MPTA 1.7g instead of MPTA and 6FDA, CB The same procedure as in Example 1-1 was repeated except that 0.7 g of DA and 13.8 g of 6FDA were used. Prepare a polyamic acid solution (solution viscosity at 25°C: 95 poise (9,500 CPs)). It was created.

[0084] The polyamic acid solution was used to prepare a transparent polyimide resin film in the same manner as in Example 1-2. The imidization rate was 85% or more.

[0085] [Example 11] Preparation of transparent polyimide film DMAc 101.9g, PPTA 1.7g instead of MPTA and 6FDA, CB The same procedure as in Example 1-1 was repeated except that 0.7 g of DA and 13.8 g of 6FDA were used. Polyamic acid solution (solution viscosity at 25°C: 88.3 poise (8,830 CPs)) was manufactured.

[0086] The polyamic acid solution was used to prepare a transparent polyimide resin film in the same manner as in Example 1-2. The imidization rate was 85% or more.

[0087] [Comparative Example 1] Production of transparent polyimide film DMAc (98.1 g), 2,2'-TFDB (8.7 g), and m-PDA (0.7 g) were used. The same procedure as in Example 1-1 was repeated except that 15.1 g of 6FDA was used instead of MPTA. A polyamic acid solution (solution viscosity at 25°C: 69 poise (6,900 CPs)) was Manufactured.

[0088] The polyamic acid solution was used to prepare a transparent polyimide resin film in the same manner as in Example 1-2. The imidization rate was 85% or more.

[0089] [Comparative Example 2] Preparation of transparent polyimide film DMAc 98.1g, 2,2'-TFDB 8.7g, pP instead of m-PDA Except for using 0.7 g of DA and 15.1 g of 6FDA without MPTA, In the same manner as in Example 1-1, a polyamic acid solution (solution viscosity at 25° C.: 67 poise (6 ,700CPs) were produced.

[0090] The polyamic acid solution was used to prepare a transparent polyimide resin film in the same manner as in Example 1-2. The imidization rate was 85% or more.

[0091] [Comparative Example 3] Preparation of transparent polyimide film DMAc 99.1g, 2,2'-TFDB 9.6g, 4,4 instead of m-PDA '-DDS 1.8g, PMDA 1.6g instead of MPTA, 6FDA 13.3g A polyamic acid solution (solution viscosity at 25°C: 76 poise (7,600 CPs) was produced.

[0092] The polyamic acid solution was used to prepare a transparent polyimide resin film in the same manner as in Example 1-2. The imidization rate was 85% or more.

[0093] [Comparative Example 4] Preparation of transparent polyimide film DMAc 99.5g, 2,2'-TFDB 8.5g, 4,4 instead of m-PDA '-DDS 1.6g, except for using 6FDA 14.7g without MPTA In the same manner as in Example 1-1, a polyamic acid solution (solution viscosity at 25°C: 61 pois e (6,100 CPs) was produced.

[0094] The polyamic acid solution was used to prepare a transparent polyimide resin film in the same manner as in Example 1-2. The imidization rate was 85% or more.

[0095] [Comparative Example 5] Preparation of transparent polyimide film DMAc was used in the same manner as in Example 1. 1.6g of 4'-DDS, 1.6g of PMDA instead of MPTA, 13.6g of 6FDA The same procedure as in Example 1-1 was repeated except that a polyamic acid solution (solution viscosity at 25° C.) was used. :84 poise (8,400 CPs) was produced.

[0096] The polyamic acid solution was used to prepare a transparent polyimide resin film in the same manner as in Example 1-2. The imidization rate was 85% or more.

[0097] The above-mentioned embodiment 1, 2, 5-7, 10, and 11, and The amounts of (a) the aromatic diamine mixture and (b) the dianhydride mixture used in Comparative Examples 1 to 5 are shown in Table 1 below (unit: mol %).

[0098] [Table 1]

[0099] [Experimental Example 1] Evaluation of the physical properties of transparent polyimide resin films 1, 2, 5-7, 10, and 11, and The physical properties of the transparent polyimide resin films obtained in Comparative Examples 1 to 5 were evaluated by the following methods. The results are shown in Table 2.

[0100] 1. Measurement of light transmittance and yellowness index (YI) A UV spectrometer (Konica Minolta, CM-3700d) was used at a wavelength of 550 nm. Light transmission and yellowness were measured according to ASTM E313.

[0101] YI is a transparent polyimide resin film that was exposed to a UB-B lamp for 72 hours and then It is a value that measures the color change before and after dew. That is, YI is calculated from the following formula 1. do.

[0102] [Formula 1] △YI=YI (after 71 hours exposure) - YI (before 72 hours exposure)

[0103] 2. Mechanical Property Measurement Instron(Model 3345 Electromechanical Sy Using the tensile modulus (Modulus) and mechanical properties according to ASTM D882 The mechanical strength and yield strain were measured.

[0104] 3. Flex resistance measurement Using MIT (Folding Endurance Tester, D-2), The bending resistance (times / R@ 1 mm) was measured by STM D2176.

[0105] 4. Thickness measurement A silicon wafer is coated with polyamic acid resin to a thickness of 20 μm or less. After coating, the material is dried and subjected to an imidization reaction to synthesize a transparent polyimide resin. A refractive index measurement device (Ellipso Technology, Elli-RP) was used. The film thickness was measured at a wavelength of 550 nm.

[0106] 5. Measurement of Glass Transition Temperature Dynamic Mechanical Analysis(TA Instrument The glass transition temperature was measured using a PTFE-based thermocouple (Q800, manufactured by NTS).

[0107] [Table 2]

[0108] As shown in Table 2, in Example 1, 2, 5-7, 10, and 11 It was confirmed that the transparent polyimide resin film obtained in the above step 1 had improved mechanical and thermal properties while maintaining the optical properties.

[0109] Specifically, in the embodiment 1, 2, 5-7, 10, and 11 The transparent polyimide resin film obtained in Example 1 has a transmittance of 89% or more, a yellowness index of 2.5 or less, a bending resistance of 200,000 times or more, an elastic modulus of 5.5 GPa or more, a strength of 160 MPa or more, a yield strain of 2% or more, and a glass transition temperature of 350 to 450°C. Compared with the transparent polyimide resin films obtained in Comparative Examples 1 to 5, the transparent polyimide resin film has a lower yellowness change rate and is excellent in mechanical properties and thermal properties, and therefore meets the conditions for application as a material for flexible display devices.

[0110] As described above, the transparent polyimide resin produced using the polyamic acid solution according to the present invention The oil film has high light transmittance, low yellowing, and excellent mechanical and thermal properties. Therefore, it has been confirmed that the film can be used as a material, substrate, or protective film for flexible display devices. It was.

Claims

1. (a) an aromatic diamine mixture containing (a-1) a fluorinated aromatic diamine and (a-2) a non-fluorinated aromatic diamine; (b) a dianhydride mixture containing (b-1) a fluorinated aromatic dianhydride and (b-2) a non-fluorinated dianhydride containing an amide group; and (c) an organic solvent; Including, The content of the (b-1) fluorinated aromatic dianhydride is 50 to 95 mol % relative to 100 mol % of the (b) dianhydride mixture; the content of the (b-2) non-fluorinated dianhydride containing an amide group is 0.1 to 30 mol % relative to 100 mol % of the (b) dianhydride mixture; The (b-1) fluorinated aromatic dianhydride is at least one selected from the group consisting of 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride (6FDA), 3-(trifluoromethyl)pyromellitic dianhydride (3-TFPPMDA), and 9,9-bis(trifluoromethyl)-9H-xanthene-2,3,6,7-tetracarboxylic dianhydride (6FCDA); The (b-2) non-fluorinated dianhydride containing an amide group is at least one selected from the group consisting of metaphenylenediamine bis(trimellitic anhydride) (MPTA) and paraphenylenediamine bis(trimellitic anhydride) (PPTA).

2. The (a-1) fluorinated aromatic diamine is at least one selected from the group consisting of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (2,2'-TFDB), bisaminohydroxyphenylhexafluoropropane (DBOH), bisaminophenoxyphenylhexafluoropropane (4BDFA), 2,2'-bis(trifluoromethyl)-4,3'-diaminobiphenyl, and 2,2'-bis(trifluoromethyl)-5,5'-diaminobiphenyl; 2. The polyamic acid solution according to claim 1, wherein the (a-2) non-fluorinated aromatic diamine is at least one selected from the group consisting of oxydianiline (ODA), 4,4'-diamino-2,2'-dimethylbiphenyl (m-Tolidine), paraphenylenediamine (p-PDA), metaphenylenediamine (m-PDA), bisaminophenoxyphenylpropane (6HMDA), bisaminophenoxydiphenylsulfone (DBSDA), 4,4'-diaminodiphenylsulfone (4,4'-DDS), and 3,3'-diaminodiphenylsulfone (3,3'-DDS).

3. the content of the (a-1) fluorinated aromatic diamine is 50 to 99.9 mol % relative to 100 mol % of the (a) aromatic diamine mixture, 2. The polyamic acid solution according to claim 1, wherein a content of the (a-2) non-fluorinated aromatic diamine is 0.1 to 50 mol % relative to 100 mol % of the (a) aromatic diamine mixture.

4. 2. The polyamic acid solution according to claim 1, wherein the (b) dianhydride mixture further contains (b-3) an alicyclic dianhydride.

5. 2. The polyamic acid solution according to claim 1, wherein the weight ratio of the aromatic diamine mixture (a) to the dianhydride mixture (b) is (a):(b)=1:0.1-10.

6. 2. The polyamic acid solution according to claim 1, having a viscosity of 1,000 to 50,000 cps.

7. A transparent polyimide resin film produced by imidizing the polyamic acid solution according to claim 1 .

8. The transparent polyimide resin film according to claim 7, which satisfies the following physical property conditions (i) to (v): (i) In a film thickness of 5 to 60 μm, the light transmittance at a wavelength of 550 nm is 89% or more; (ii) a yellowness index according to ASTM E313 of 2.5 or less; (iii) an elastic modulus according to ASTM D882 of 5.5 GPa or more, a mechanical strength of 155 MPa or more, and a yield strain of 5.5% or more; (iv) flex resistance according to ASTM D2176 is 200,000 times or more; (v) The glass transition temperature is 350 to 400°C.

9. A transparent substrate comprising the transparent polyimide resin film according to claim 7 or 8.

Citation Information

Patent Citations

  • Liquid crystal aligning agent and liquid crystal display element

    JP2010097188A

  • Radiation-sensitive polymer composition, insulation film, and organic el element

    JP2014074772A