Wear-resistant steel material with excellent resistance to cutting cracks and its manufacturing method
A wear-resistant steel with a specific alloy composition and controlled microstructure, combined with a precise manufacturing process, addresses cutting crack issues by achieving high hardness and crack resistance, especially in thick materials.
Patent Information
- Application Number
- JP2022537685
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-19
- Filing Date
- 2020-12-16
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-12-16
AI Technical Summary
Existing wear-resistant steel materials suffer from cutting cracks due to hydrogen penetration during cutting, and conventional methods to prevent this, such as preheating and post-heating, are time-consuming and inefficient.
A wear-resistant steel composition with specific alloy elements (C, Si, Mn, P, S, Al, Cr, Mo, Nb, V, B, Ti, Ni, Cu, Ca) and a controlled microstructure of 90% tempered martensite, 10% bainite, and 2% martensite, along with a manufacturing process involving controlled heating, rolling, and rapid cooling followed by heat treatment, to achieve high hardness and resistance to cutting cracks.
The steel material exhibits high hardness and excellent resistance to cutting cracks, particularly in thick materials, ensuring no cracking occurs even after cutting, with a Brinell hardness of 360 to 440 HB.
Smart Images

Figure 0007564873000001 
Figure 0007564873000002 
Figure 0007564873000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an abrasion-resistant steel material having excellent resistance to cracking during cutting and a manufacturing method thereof, and more particularly to an abrasion-resistant steel material which does not crack even after being cut by a method such as gas, and a manufacturing method thereof. [Background technology]
[0002] Construction and industrial machinery used in many industrial fields, including construction, civil engineering, mining, and the cement industry, is subject to severe wear due to friction during operation, and so materials that exhibit wear-resistant properties must be used. Generally, the wear resistance and hardness of thick steel plates are correlated, so thick steel plates that are prone to wear must have high hardness, and such thick steel plates are usually called wear-resistant steels.
[0003] Wear-resistant steels with high hardness are generally manufactured by hot rolling, reheating to a temperature of Ac3 or higher, and then quenching. Wear-resistant steels manufactured through this process have a fine structure called martensite, which is a characteristic unique to steel obtained through phase transformation. Wear-resistant steels having martensite as the main structure contain a large amount of carbon and alloy elements inside, and in practice, there is a problem that cracks are likely to occur after the material is cut to a desired size and shape.
[0004] Cracks that occur after cutting are caused by hydrogen that penetrates into the material when it is cut, and the reliability of the material can only be ensured if the resistance to hydrogen embrittlement is improved. To do this, it is usually necessary to preheat the material to 100°C or higher, although this varies depending on the thickness before cutting. However, preheating the material in this way takes a considerable amount of time, and it is very difficult to ensure and maintain a uniform temperature. In addition, in order to prevent cutting cracks, post-heating is sometimes performed on the cut surface in the same way as preheating, but this is not efficient in terms of workability. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Korean Patent Publication No. 10-2015-0179009 Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a wear-resistant steel material having high hardness and excellent resistance to cutting cracking, and a method for producing the same.
[0007] The object of the present invention is not limited to the above. Anyone having ordinary knowledge in the technical field to which the present invention pertains will have no difficulty in understanding further object of the present invention from the entire contents of the specification of the present invention. [Means for solving the problem]
[0008] The wear-resistant steel material of the present invention contains, by weight, carbon (C): 0.25 to 0.50%, silicon (Si): 0.15 to 0.5%, manganese (Mn): 0.6 to 1.6%, phosphorus (P): 0.05% or less (excluding 0), sulfur (S): 0.02% or less (excluding 0), aluminum (Al): 0.07% or less (excluding 0), chromium (Cr): 0.1 to 1.5%, molybdenum (Mo): 0.1 to 0.8%, niobium (Nb): 0.08% or less (excluding 0), vanadium (V): 0.05 to 0.5%, and boron (B): 50 ppm or less (excluding 0). and additionally containing at least one selected from the group consisting of titanium (Ti): 0.02% or less (excluding 0), nickel (Ni): 0.5% or less (excluding 0), copper (Cu): 0.5% or less (excluding 0), and calcium (Ca): 2 to 100 ppm, with the remainder consisting of Fe and other unavoidable impurities, satisfying the following relational formula 1, and characterized in that the microstructure contains, in terms of area fraction, 90% or more tempered martensite, 10% or less bainite, and 2% or less martensite, and has a Brinell hardness in the range of 360 to 440 HB.
[0009] [Equation 1] ([V]×[Nb]) / [Mo]≧6×10 -3 (In the above Relational Formula 1, the [V] indicates the average weight percent content of V in the steel material, the [Nb] indicates the average weight percent content of Nb in the steel material, and the [Mo] indicates the average weight percent content of Mo in the steel material.)
[0010] The manufacturing method of the wear-resistant steel material of the present invention includes the steps of heating a steel slab having the above-mentioned alloy composition in a temperature range of 1050 to 1250 ° C., rough rolling the reheated steel slab in a temperature range of 950 to 1050 ° C. to obtain a rough rolled bar, hot rolling the rough rolled bar in a temperature range of 850 to 950 ° C. to obtain a hot-rolled steel plate, cooling the hot-rolled steel plate to a cooling end temperature of Ms-50 ° C. or less at an average cooling rate of 3 ° C. / s or more, and heat treating the cooled steel plate at a temperature of 450 to 650 ° C. for 15 minutes or more. Effect of the Invention
[0011] According to the present invention, it is possible to provide a wear-resistant steel material having high hardness and excellent resistance to cutting cracks, and a manufacturing method thereof. In particular, according to the present invention, it is possible to provide a wear-resistant steel material having high hardness and excellent resistance to cutting cracks, even for thick steel materials having a thickness of 60 mm or more, and a manufacturing method thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The wear-resistant steel material according to one aspect of the present invention contains, by weight, 0.25 to 0.50% carbon (C), 0.15 to 0.5% silicon (Si), 0.6 to 1.6% manganese (Mn), 0.05% or less (excluding 0) phosphorus (P), 0.02% or less (excluding 0) sulfur (S), 0.07% or less (excluding 0) aluminum (Al), 0.1 to 1.5% chromium (Cr), 0.1 to 0.8% molybdenum (Mo), 0.08% or less (excluding 0) niobium (Nb), 0.05 to 0.5% vanadium (V), and 50 ppm or less boron (B). and additionally containing at least one selected from the group consisting of titanium (Ti): 0.02% or less (excluding 0), nickel (Ni): 0.5% or less (excluding 0), copper (Cu): 0.5% or less (excluding 0), and calcium (Ca): 2 to 100 ppm, with the balance being Fe and other unavoidable impurities, satisfying the following relational formula 1, and the microstructure containing, by area fraction, 90% or more tempered martensite, 10% or less bainite, and 2% or less martensite, and having a Brinell hardness in the range of 360 to 440 HB.
[0013] [Equation 1] (V×Nb) / Mo≧6×10 -3 (In the relational formula 1, [V] represents the average weight percent content of V in the steel, [Nb] represents the average weight percent content of Nb in the steel, and [Mo] represents the average weight percent content of Mo in the steel.)
[0014] The reasons for limiting the alloy composition of the wear-resistant steel material having excellent cutting crack resistance provided by the present invention as described above will be explained in detail below. In the present invention, the content of each element is based on weight percent unless otherwise specified.
[0015] Carbon (C): 0.25~0.50% Carbon (C) is an element that is effective in increasing hardness and improving hardenability in steels mainly composed of martensite. In order to fully secure the above-mentioned effects, it is preferable to add 0.25% or more, and if the content exceeds 0.50%, the risk of fracture in the slab heating furnace at the reheating stage of the thick plate manufacturing process increases. Therefore, in the present invention, it is preferable to control the C content to 0.25 to 0.50%. On the other hand, the lower limit of the C content is more preferably 0.26%, further preferably 0.28%, and most preferably 0.29%. The upper limit of the C content is more preferably 0.49%, further preferably 0.48%, and most preferably 0.47%.
[0016] Silicon (Si): 0.15-0.5% Silicon (Si) is an element effective in improving strength through deoxidation and solid solution strengthening. In order to effectively obtain the above-mentioned effects, it is preferable to add 0.15% or more. However, if the content exceeds 0.5%, excessive scale may be generated during hot rolling, which is not preferable. Therefore, in the present invention, it is preferable to control the Si content to 0.15 to 0.5%. The lower limit of the Si content is more preferably 0.16%, further preferably 0.18%, and most preferably 0.20%. The upper limit of the Si content is more preferably 0.48%, further preferably 0.46%, and most preferably 0.45%.
[0017] Manganese (Mn): 0.6-1.6% Manganese (Mn) is an element that suppresses the formation of ferrite and lowers the Ar3 temperature, thereby effectively increasing the hardenability and improving the strength and toughness of steel. In order to effectively obtain the above-mentioned effects, it is preferable to add 0.6% or more. However, if the Mn content exceeds 1.6%, there is a problem that a MnS segregation band is likely to occur in the thickness center, which makes it easy for cracks to occur. Therefore, in the present invention, it is preferable to control the Mn content to 1.6% or less. The lower limit of the Mn content is more preferably 0.63%, even more preferably 0.65%, and most preferably 0.70%. The upper limit of the Mn content is more preferably 1.58%, even more preferably 1.55%, and most preferably 1.50%.
[0018] Phosphorus (P): 0.05% or less (excluding 0) Phosphorus (P) is an element that is inevitably contained in steel and that impairs the toughness of steel. Therefore, it is preferable to control the P content as low as possible to 0.05% or less, and more preferably, the upper limit of the P content may be 0.03%, and most preferably, 0.015%. However, taking into consideration the level of unavoidable inclusion, the P content may exclude 0%, or the lower limit of the P content may be set to 0.001%.
[0019] Sulfur (S): 0.02% or less (excluding 0) Sulfur (S) is an element that forms MnS inclusions in steel and impairs the toughness of the steel. Therefore, it is preferable to control the S content as low as possible to 0.02% or less, and more preferably, the upper limit of the S content may be 0.009%. However, taking into consideration the level of unavoidable inclusion, the S content may be excluded from 0%, or the lower limit of the S content may be set to 0.0005%.
[0020] Aluminum (Al): 0.07% or less (excluding 0) Aluminum (Al) is an element that is effective as a deoxidizer for steel to reduce the oxygen content in molten steel. However, if the Al content exceeds 0.07%, it is not preferable because it impairs the cleanliness of the steel. Therefore, in the present invention, it is preferable to control the Al content to 0.07% or less, and more preferably, the upper limit of the Al content may be 0.06%, even more preferably, the upper limit of the Al content may be 0.05%, and most preferably, the upper limit of the Al content may be 0.04%. However, taking into consideration the load during the steelmaking process, the increase in manufacturing costs, etc., the Al content may be excluded from 0%, or the lower limit of the Al content may be 0.005%.
[0021] Chromium (Cr): 0.1-1.5% Chromium (Cr) is an element that increases the hardenability and strength of steel, and is also advantageous in ensuring hardness. In order to obtain the above-mentioned effects, it is preferable to add Cr at 0.1% or more. However, if the content exceeds 1.5%, the hardening ability becomes excessively large, and the probability of cracks occurring on the surface of the slab during continuous casting increases. Therefore, in the present invention, it is preferable to control the Cr content to 0.1 to 1.5%. The lower limit of the Cr content is more preferably 0.12%, even more preferably 0.15%, and most preferably 0.20%. The upper limit of the Cr content is more preferably 1.4%, even more preferably 1.3%, and most preferably 1.2%.
[0022] Molybdenum (Mo): 0.1-0.8% Molybdenum (Mo) is a very useful element for increasing the hardenability of steel and for ensuring strength at high temperatures of 500°C or higher by forming fine carbides (Mo2C) at high temperatures. In order to fully obtain the above-mentioned effects, it is preferable to add Mo in an amount of 0.1% or more. However, Mo is a somewhat expensive element, and if its content exceeds 0.8%, there is a problem that the manufacturing cost increases. Therefore, in the present invention, it is preferable to control the Mo content to 0.1 to 0.8%. Alternatively, the Mo content may be more preferably 0.2% or more, and more preferably 0.3%. Moreover, the Mo content may be more preferably 0.7% or less, and more preferably 0.63%.
[0023] Niobium (Nb): 0.08% or less (excluding 0) Niobium (Nb) dissolves in austenite to increase the hardening ability of austenite, forms carbonitrides such as Nb(C,N) at high temperatures to increase the strength of steel, and inhibits the growth of austenite grains. However, if the Nb content exceeds 0.08%, there is a problem that coarse precipitates are formed, which become the starting point of brittle fracture and impair toughness. Therefore, in the present invention, it is preferable to control the Nb content to 0.08% or less. Alternatively, the Nb content may be more preferably 0.07% or less, even more preferably 0.06% or less, and most preferably 0.05% or less.
[0024] On the other hand, in the present invention, since the above-mentioned effects can be ensured by adding Nb, the Nb content can be excluded from 0% (i.e., exceeds 0%). However, more preferably, the Nb content may be 0.001% or more, even more preferably, 0.005% or more, and most preferably, 0.01% or more.
[0025] Vanadium (V): 0.05 to 0.5% Vanadium (V) is an element advantageous in suppressing the growth of austenite grains by forming VC carbides during reheating after hot rolling, improving the hardenability of steel, and ensuring strength. In order to fully obtain the above-mentioned results, it is preferable to add V at 0.05% or more. However, V is a somewhat expensive element, and if its content exceeds 0.5%, there is a problem that the manufacturing cost increases. Therefore, in the present invention, when V is added, it is preferable to control its content to 0.5% or less. On the other hand, the lower limit of the Mo content is more preferably 0.06%, further preferably 0.07%, and most preferably 0.08%. The upper limit of the V content is more preferably 0.4% or less, further preferably 0.35% or less, and most preferably 0.3% or less.
[0026] Boron (B): 50ppm or less (excluding 0) Boron (B) is an element that effectively increases the hardenability of steel and improves strength even when added in small amounts. Since B exerts the above-mentioned effects even when added in small amounts, the B content can be excluded from 0% (i.e., exceeds 0%), and more preferably, the lower limit of the B content can be set to 0.0005%. However, since an excessive B content rather impairs the toughness and weldability of the steel, it is preferable to control the content to 50 ppm or less (0.005% or less). Therefore, the B content is preferably 50 ppm or less (excluding 0). The B content is more preferably 40 ppm or less, even more preferably 35 ppm or less, and most preferably 30 ppm or less.
[0027] Meanwhile, the wear-resistant steel material according to one aspect of the present invention may further include at least one additional element selected from the following elements in addition to the above-mentioned elements.
[0028] Titanium (Ti): 0.02% or less (excluding 0) Titanium (Ti) is an element that maximizes the effect of B, which is an element effective in improving the hardenability of steel. Specifically, Ti combines with nitrogen (N) to form TiN precipitates, suppressing the formation of BN, thereby increasing the amount of solute B and maximizing the improvement of hardenability. In order to ensure the above-mentioned effects, the Ti content may be excluded from 0%, and more preferably, the lower limit of the Ti content may be 0.005%. However, if the Ti content exceeds 0.02%, there is a problem that coarse TiN precipitates are formed and the toughness of the steel is deteriorated. Therefore, in the present invention, it is preferable to control the Ti content to 0.02% or less. Alternatively, more preferably, the Ti content may be 0.017% or less, even more preferably, 0.015%, and most preferably, 0.012%.
[0029] Nickel (Ni): 0.5% or less (excluding 0) Nickel (Ni) is generally an effective element for improving the toughness as well as the strength of steel. Therefore, in order to ensure the above-mentioned effects, the Ni content can be excluded from 0%, and more preferably, the lower limit of the Ni content can be set to 0.01%. However, Ni is an expensive element, and if the Ni content exceeds 0.5%, it causes an increase in manufacturing costs. Therefore, in the present invention, it is preferable to control the upper limit of Ni to 0.5%, and more preferably, the Ni content may be 0.47% or less, even more preferably, 0.45% or less, and most preferably, 0.42% or less.
[0030] Copper (Cu): 0.5% or less (excluding 0) Copper (Cu) is an element that improves the strength and hardness of steel by solid solution strengthening. It is also an effective element for improving toughness together with Ni. In order to ensure the above-mentioned effects, the Cu content can be excluded from 0%, and more preferably, the lower limit of the Cu content can be set to 0.01%. However, if the Cu content exceeds 0.5%, there is a problem that surface defects are generated in the slab during high-temperature heating before hot rolling, and hot workability is impaired, so when Cu is added, it is preferable to add it at 0.5% or less. Alternatively, the upper limit of the Cu content may be more preferably 0.4%, even more preferably 0.35%, and most preferably 0.3%.
[0031] Calcium (Ca): 2-100 ppm Calcium (Ca) has excellent bonding strength with S, and by forming CaS, it has the effect of suppressing the formation of MnS that segregates in the thickness center of the steel material. As a result, the addition of Ca plays a role in reducing the mechanical anisotropy of the material. In order to obtain the above-mentioned effect, it is preferable to add Ca at 2 ppm or more, but if the content exceeds 100 ppm, there is a problem that nozzle clogging and the like is induced during steelmaking operations. Therefore, in the present invention, it is preferable to control the Ca content to 2 to 100 ppm (i.e., 0.0002 to 0.01%). The lower limit of the Ca content is more preferably 2.5 ppm, even more preferably 3 ppm, and most preferably 3.5 ppm. The upper limit of the Ca content is more preferably 80 ppm, even more preferably 60 ppm, and most preferably 40 ppm.
[0032] The remaining component of the present invention is iron (Fe). However, in a normal manufacturing process, unintended impurities may be inevitably mixed in from the raw materials or the surrounding environment, and it is not possible to exclude them. These impurities are known to any technician in a normal manufacturing process, so the entire contents of them will not be mentioned in this specification.
[0033] According to one aspect of the present invention, the steel satisfies the following relational expression 1. The steel according to the present invention contains V, Nb, and Mo as essential components, and if the steel does not contain any of these components, the intended effect of the present invention cannot be obtained. Furthermore, when the composition of the steel according to the present invention satisfies the following relational expression 1, the intended effect of the present invention in terms of excellent cutting crack resistance can be achieved.
[0034] [Equation 1] ([V]×[Nb]) / [Mo]≧6×10 -3 (In the relational formula 1, [V] represents the average weight percent content of V in the steel, [Nb] represents the average weight percent content of Nb in the steel, and [Mo] represents the average weight percent content of Mo in the steel.)
[0035] On the other hand, according to one aspect of the present invention, from the viewpoint of further improving the above-mentioned cutting crack resistance, the value of ([V] × [Nb]) / [Mo] defined in the following relational expression 1 may be more preferably 0.008 or more and 0.025 or less. In this case, since the following relational expression 1 is an empirically obtained value, it is not necessary to separately define a unit, and it is sufficient that each unit of [V], [Nb] and [Mo] (i.e., weight %) below is satisfied in this specification.
[0036] According to one embodiment of the present invention, the microstructure of the steel material preferably contains tempered martensite as the main structure (i.e., in terms of area %, tempered martensite is contained in 50% or more, more preferably 90% or more). As a result, the steel material of the present invention can ensure high hardness and at the same time ensure cutting crack resistance such that no cracks occur after cutting by a method such as gas, and can ensure high hardness and excellent cutting crack resistance even in thick steel materials of 60 mm or more.
[0037] That is, the probability of cutting cracks occurring is relatively low in thin wear-resistant steels, and thus tempering was not performed in the past. However, when the thickness of such wear-resistant steels is 60 mm or more, cutting cracks are more likely to occur, but in the past, there was no way to achieve both excellent hardness and cutting crack resistance without preheating or post-heating in thick steel materials with a thickness of 60 mm or more. As a result of intensive research, the inventors found that by satisfying the above-mentioned alloy composition and controlling the microstructure, it is possible to ensure excellent hardness and cutting crack resistance even in thick steel materials, and thus completed the present invention.
[0038] According to one embodiment of the present invention, the upper limit of the fraction of tempered martensite is controlled to 10% because bainite may be unavoidably formed in some regions during rapid cooling depending on the thickness of the material in manufacturing operations. That is, the microstructure of the present invention preferably contains, in terms of area fraction, 90% or more tempered martensite, 10% or less bainite, and 2% or less martensite.
[0039] If the tempered martensite fraction is less than 90% by area, there is a problem that it is difficult to ensure sufficient crack resistance after gas cutting, so the lower limit of the tempered martensite fraction is more preferably 92% by area or more, and even more preferably 95% by area or more. Also, the bainite fraction is more preferably 8% by area or less, and even more preferably 5% by area or less.
[0040] On the other hand, according to one aspect of the present invention, the area fraction of the tempered martensite structure is more preferably 90% or more and 98% or less, and the area fraction of the bainite structure is preferably 2% or more and 10% or less.
[0041] Also, according to one aspect of the present invention, the steel material contains, in terms of area percentage, 90% or more of tempered martensite and 10% or less of bainite as a microstructure, and may further contain the balance of martensite as other phases.
[0042] Therefore, according to one aspect of the present invention, the steel material can contain, in terms of area percentage, as a microstructure, 90% or more and 98% or less of tempered martensite, 2% or more and 10% or less of bainite, and 2% or less (including 0%) of martensite.
[0043] Meanwhile, according to one aspect of the present invention, the steel material of the present invention may contain fine carbides, which can simultaneously improve the strength of the steel and the resistance to hydrogen embrittlement. That is, hydrogen that has flowed into the inside of a material by gas cutting usually causes delayed fracture that requires a certain incubation period of 24 to 48 hours, but the fine carbides enhance the resistance to such delayed fracture.
[0044] More specifically, fine carbides directly or indirectly act as hydrogen trapping sites, and carbides of Nb, Ti, V, Mo, etc. are effective in increasing hydrogen embrittlement resistance in steel materials having tempered martensite as a matrix structure. Incidentally, the size of the above-mentioned fine carbides is several to several tens of nm, and the size varies somewhat depending on the added elements.
[0045] According to one aspect of the present invention, the fine carbides preferably include Nb, V series fine carbides.
[0046] According to one aspect of the present invention, the Brinell hardness of the wear-resistant steel material is a grade of about 360 to 440HB. By satisfying the Brinell hardness range of 360 to 440HB, which is the target hardness range for wear-resistant steel material, it is possible to obtain a steel material that exhibits both the excellent hardness and crack resistance effects intended by the present invention.
[0047] Another embodiment of the present invention provides a method for producing a wear-resistant steel material, comprising the steps of heating a steel slab having the above-mentioned alloy composition in a temperature range of 1050 to 1250 ° C, rough rolling the reheated steel slab in a temperature range of 950 to 1050 ° C to obtain a rough rolled bar, hot rolling the rough rolled bar in a temperature range of 850 to 950 ° C to obtain a hot-rolled steel plate, cooling the hot-rolled steel plate to Ms-50 ° C or less at an average cooling rate of 3 ° C / s or more, and heat treating the cooled steel plate at a temperature of 450 to 650 ° C for 15 minutes or more.
[0048] The method for producing a high-hardness, wear-resistant steel material having excellent resistance to cutting cracks according to the present invention will now be described in detail.
[0049] First, a steel slab satisfying the above-mentioned alloy composition is heated in a temperature range of 1050 to 1250°C. If the slab heating temperature is less than 1050°C, re-dissolution of Nb and the like is insufficient, while if it exceeds 1250°C, the austenite grains may become coarse and a non-uniform structure may be formed. Therefore, in the present invention, the heating temperature of the steel slab is preferably in the range of 1050 to 1250°C. The lower limit of the heating temperature of the steel slab is more preferably 1065°C, further preferably 1080°C, and most preferably 1100°C. The upper limit of the heating temperature of the steel slab is more preferably 1220°C, further preferably 1200°C, and most preferably 1180°C.
[0050] The reheated steel slab is roughly rolled in a temperature range of 950 to 1050 ° C to obtain a roughly rolled bar. If the temperature during rough rolling is less than 950 ° C, the rolling load increases and the rolling is relatively weak, so that the deformation is not sufficiently transmitted to the center of the thickness direction of the slab, and defects such as voids may not be removed. On the other hand, if the temperature exceeds 1050 ° C, the particles grow after recrystallization occurs simultaneously with rolling, and the initial austenite particles may become excessively coarse. Therefore, in the present invention, the rough rolling temperature is preferably 950 to 1050 ° C. The lower limit of the rough rolling temperature is more preferably 960 ° C, more preferably 970 ° C, and most preferably 980 ° C. The upper limit of the rough rolling temperature is more preferably 1045 ° C, more preferably 1040 ° C, and most preferably 1035 ° C.
[0051] The rough rolled bar is hot rolled in a temperature range of 850 to 950 ° C to obtain a hot rolled steel sheet. If the hot rolling temperature is less than 850 ° C, it may be two-phase rolling and ferrite may be generated in the microstructure, while if the hot rolling temperature exceeds 950 ° C, bainite may be excessively generated during air cooling due to the relatively fast cooling rate. Therefore, in the present invention, the hot rolling temperature is preferably 850 to 950 ° C. On the other hand, the lower limit of the hot rolling temperature is more preferably 860 ° C, further preferably 870 ° C, and most preferably 880 ° C. The upper limit of the hot rolling temperature is more preferably 940 ° C, further preferably 930 ° C, and most preferably 920 ° C.
[0052] According to one aspect of the present invention, the method may further include a step of air-cooling the hot-rolled steel sheet obtained by hot rolling. Then, the method may include a step of reheating the hot-rolled steel sheet to a temperature of Ac+30°C or higher (more preferably, in the range of 890 to 920°C) based on the surface temperature of the hot-rolled steel sheet. In this case, the reheating furnace time may be in the range of 100 to 160 minutes (more preferably, 106 to 151 minutes).
[0053] Thereafter, the steel sheet is cooled at an average cooling rate of 3°C / s or more (preferably 3 to 20°C / s, more preferably 3.2 to 10.1°C / s) to a cooling end temperature of Ms-50°C or less (from a cooling start temperature of Ac3+30°C or more) based on the surface temperature of the hot-rolled steel sheet. In this case, the cooling is preferably rapid cooling using water at 30°C or less.
[0054] If the average cooling rate is less than 3°C / s or the cooling end temperature exceeds Ms-50°C, there is a risk that ferrite phases will be formed during cooling or bainite phases will be excessively formed. Therefore, it is preferable to cool to Ms-50°C or lower at an average cooling rate of 3°C / s or more. The faster the cooling rate, the more advantageous it is for the formation of the microstructure that is to be obtained in the present invention, but when the thickness is 60 mm or more, the cooling rate inside the material will physically decrease. On the other hand, the present invention does not particularly limit the upper limit of the cooling rate, and any ordinary engineer can set it appropriately taking into account the limitations of the equipment.
[0055] Although not particularly limited, according to one aspect of the present invention, during cooling, the end temperature of cooling may more preferably be Ms-80°C or less (even more preferably Ms-100°C or less, and most preferably Ms-150°C or less).
[0056] The hot-rolled steel sheet that has been subjected to the rapid cooling heat treatment is subjected to a subsequent heat treatment at 450 to 650° C. in order to ensure the final target hardness and cutting crack resistance. That is, the target hardness of 360 to 440HB can be ensured by the subsequent heat treatment, which is usually called tempering.
[0057] Specifically, hot-rolled steel sheets that are rapidly cooled before the subsequent heat treatment exceed the upper limit of hardness of 440HB, which is the target hardness of the present invention, due to the high carbon content, and the cut crack resistance cannot be ensured. Therefore, in the present invention, the hardness is adjusted downward by reducing the dislocation density inside the material through tempering heat treatment, and further, fine carbides of alloy elements such as Nb and V that are added in small amounts are precipitated, thereby making it possible to ensure the cut crack resistance.
[0058] Therefore, the subsequent heat treatment is preferably carried out at 450 to 650° C. For the precipitation of fine carbides, the subsequent heat treatment temperature is more preferably 460° C. or higher, further preferably 480° C. or higher, and most preferably 489° C. or higher.
[0059] Moreover, the subsequent heat treatment temperature is more preferably 640° C. or less, further preferably 620° C. or less, and most preferably 600° C. or less.
[0060] According to one aspect of the present invention, the soaking time during the subsequent heat treatment is preferably 15 minutes or more. If the soaking time is less than 15 minutes, the temperature does not rise sufficiently to the center when the thickness of the material is taken into consideration, and the effect of reducing dislocation density and precipitating fine carbides is insufficient. If the soaking time exceeds 50 minutes, the hardness is significantly reduced and the target level cannot be met.
[0061] Therefore, the residence time in the furnace for the subsequent heat treatment is preferably 15 to 50 minutes. On the other hand, the residence time is more preferably 16 minutes or more, even more preferably 17 minutes or more, and most preferably 19 minutes or more. Also, the residence time is more preferably 48 minutes or less, even more preferably 45 minutes or less, and most preferably 41 minutes or less.
[0062] The present invention will be described in more detail with reference to the following examples. However, it should be noted that the following examples are intended to illustrate and explain the present invention in more detail, and are not intended to limit the scope of the present invention. The scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred therefrom.
[0063] [Example] Steel slabs having the alloy compositions shown in Tables 1 and 2 below were prepared, and then the steel slabs were subjected to the following steps of steel slab heating-rough rolling-hot rolling-cooling (room temperature; air cooling)-reheating-cooling-subsequent heat treatment under the conditions shown in Table 3 below to produce hot-rolled steel sheets. The microstructures and mechanical properties of the hot-rolled steel sheets were measured and are shown in Table 4 below.
[0064] In this case, the microstructure was observed at the 1 / 2t position, which is the center of the thickness, using an optical microscope and an electron scanning microscope after cutting the test piece to an arbitrary size to prepare a mirror surface and etching it with a nital etching solution.
[0065] The hardness was measured using a Brinell hardness tester (load 3000 kgf, 10 mm tungsten inlet). The surface of the plate was milled in the thickness direction by 2 mm to thoroughly remove the decarburized layer, and the average value of three measurements was used.
[0066] On the other hand, the occurrence of cutting cracks was evaluated by preparing hot-rolled steel sheets having the alloy compositions shown in Tables 1 and 2 below and the thicknesses shown in Table 3 below, and then performing normal gas cutting using oxygen gas without preheating (no preheating), and leaving the cut material at room temperature for 48 hours. This was to check the occurrence of delayed fracture, which is not observed immediately after cutting, due to hydrogen that flowed into the cut part during cutting. The occurrence of cutting cracks was evaluated by first visually checking the cut surface, and then rechecking for fine cracks using an optical microscope, and the results are shown in Table 4.
[0067] [Table 1]
[0068] [Table 2]
[0069] [Table 3] * Ac 3= 910-203×C1 / 2 -15.2×Ni+44.7×Si+104×V+31.5×Mo+13.1× W *Ms=539-423×C-30.4×Mn-17.7×Ni-12.1×Cr-7.5×Mo Here, C, Ni, Si, V, Mo, W, Mn, and Cr are the weight percentages of each element.
[0070] [Table 4]
[0071] As shown in Tables 1 to 4 above, in the case of Comparative Examples 1 to 15, which do not satisfy any of the alloy composition and manufacturing conditions specified in the present invention, the surface hardness is outside the Brinell hardness range of 360 to 440HB, which is the range targeted by the present invention, and a steel material having the hardness of the grade intended by the present invention cannot be obtained, and / or cutting cracks occurred. In contrast, in the case of Invention Examples 1 to 9, which satisfy all of the alloy composition and manufacturing conditions specified in the present invention, all satisfy the Brinell hardness range of 360 to 440HB, which is the hardness range targeted by the present invention, and no cutting cracks occurred. Therefore, it was confirmed that when all of the alloy composition and manufacturing conditions specified in the present invention are satisfied, even in thick steel materials having a thickness of 60 mm or more, the targeted excellent hardness characteristics can be achieved at the same time as excellent cutting crack resistance characteristics.
Claims
1. In weight percent, carbon (C): 0.25-0.50%, silicon (Si): 0.15-0.5%, manganese (Mn): 0.6-1.6%, phosphorus (P): 0.05% or less (excluding 0), sulfur (S): 0.02% or less (excluding 0), aluminum (Al): 0.07% or less (excluding 0), chromium (Cr): 0.1-1.5%, molybdenum (Mo): 0.1-0.8%, niobium (Nb): 0.08% or less (excluding 0). 0.05 to 0.5% vanadium (V) and 50 ppm or less (excluding 0) boron (B), and further including at least one selected from the group consisting of 0.02% or less titanium (Ti) and 0.5% or less (excluding 0), 0.5% or less nickel (Ni) and 0.5% or less copper (Cu) and 2 to 100 ppm calcium (Ca), with the remainder being Fe and other inevitable impurities; A wear-resistant steel material characterized in that it satisfies the following Relational Expression 1, its microstructure contains, in terms of area fraction, 90% or more of tempered martensite, 10% or less of bainite, and 2% or less of martensite, and its Brinell hardness is in the range of 360 to 440 HB. [Relationship 1] ([V]×[Nb]) / [Mo]≧6×10 -3 (In the above Relational Formula 1, the [V] indicates the average weight percent content of V in the steel material, the [Nb] indicates the average weight percent content of Nb in the steel material, and the [Mo] indicates the average weight percent content of Mo in the steel material.)
2. The wear-resistant steel material according to claim 1, characterized in that the steel material contains, as a microstructure, in area percentages, 90% to 98% tempered martensite, 2% to 10% bainite, and 2% or less (including 0%) martensite.
3. 2. The wear-resistant steel material according to claim 1, characterized in that the steel material has a thickness of 60 mm or more.
4. A method for producing a wear-resistant steel material, comprising the steps of: In weight percent, carbon (C): 0.25-0.50%, silicon (Si): 0.15-0.5%, manganese (Mn): 0.6-1.6%, phosphorus (P): 0.05% or less (excluding 0), sulfur (S): 0.02% or less (excluding 0), aluminum (Al): 0.07% or less (excluding 0), chromium (Cr): 0.1-1.5%, molybdenum (Mo): 0.1-0.8%, niobium (Nb): 0.08% or less (excluding 0). 0.05 to 0.5% vanadium (V) and 50 ppm or less (excluding 0) boron (B), and further including at least one selected from the group consisting of 0.02% or less titanium (Ti) and 0.5% or less (excluding 0), 0.5% or less nickel (Ni) and 0.5% or less copper (Cu) and 2 to 100 ppm calcium (Ca), with the remainder being Fe and other inevitable impurities; Heating a steel slab having an alloy composition satisfying the following Relation 1 in a temperature range of 1050 to 1250 ° C.; Rough rolling the heated steel slab at a temperature range of 950 to 1050° C. to obtain a rough rolled bar; hot rolling the rough rolled bar at a temperature range of 850 to 950° C. to obtain a hot rolled steel sheet; cooling the hot-rolled steel sheet to a cooling end temperature of Ms-50°C or less at an average cooling rate of 3°C / s or more; and heat treating the cooled steel plate at a temperature of 450 to 650° C. for 15 minutes or more. The microstructure of the wear-resistant steel material contains, by area fraction, 90% or more of tempered martensite, 10% or less of bainite, and 2% or less of martensite, and has a Brinell hardness in the range of 360 to 440 HB. [Relationship 1] (V×Nb) / Mo≧6×10 -3
5. 5. The method of claim 4, wherein the heat treatment is performed for 15 minutes to 50 minutes.
6. 5. The method of claim 4, wherein the heat treatment is performed at a temperature of 489 to 600.degree.
Citation Information
Patent Citations
Production of high hardness wear resistant steel excellent in low temperature toughness
JP1996041535A
Wear resistant steel plate excellent in stress corrosion cracking resistance and method for manufacturing the same
JP2012214890A
High-hardness low-alloy wear-resistant steel plate and its manufacturing method
JP2016505094A
High-hardness hot-rolled steel product and its manufacturing method
JP2016534230A
KR10-2015-0179009