Polarizing plate with adhesive, image display device and method for manufacturing same

The use of a specialized adhesive sheet with an acrylic base polymer and ultraviolet absorbers addresses the issue of polarizer yellowing and discoloration in image display devices, ensuring durable and reliable bonding between the polarizer and cover window.

JP7565175B2Active Publication Date: 2024-10-10NITTO DENKO CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020125759
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-22
Publication Date
2024-10-10
Estimated Expiration
2040-07-22

AI Technical Summary

Technical Problem

Image display devices with a cover window bonded to a polarizer via an adhesive sheet are prone to polarizer yellowing and discoloration during weather and humidification tests, and adjusting the adhesive composition for durability compromises its reliability.

Method used

A pressure-sensitive adhesive sheet composed of an acrylic base polymer with specific monomer ratios and additives, including ultraviolet absorbers, is used to bond the polarizer and cover window, ensuring minimal light transmittance at 380 nm and incorporating a crosslinked structure for enhanced durability.

Benefits of technology

The adhesive sheet effectively suppresses polarizer discoloration and peeling, maintaining excellent adhesion reliability under various environmental conditions, including high temperatures and humidity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565175000002
    Figure 0007565175000002
  • Figure 0007565175000003
    Figure 0007565175000003
  • Figure 0007565175000004
    Figure 0007565175000004
Patent Text Reader

Abstract

To provide an adhesive sheet which is used to paste a polarizer and a cover window together and is disposed in contact with the polarizer.SOLUTION: An adhesive sheet (21) provided herein consists of an adhesive composition containing an acrylic base polymer and a UV absorbent. The adhesive sheet preferably has a light transmittance of 5% or less at a wavelength of 380 nm. A monomer component constituting the acrylic base polymer preferably contains less amounts of polar monomers such as hydroxy group-containing monomers, carboxy group-containing monomers, and nitrogen atom-containing monomers.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention is used in the formation of an image display device. Viscosity The present invention relates to a polarizing plate with an adhesive, an image display device, and a method for manufacturing the same. [Background technology]

[0002] Liquid crystal display devices and organic electroluminescence (EL) display devices are widely used as various image display devices such as mobile phones, smartphones, car navigation devices, PC monitors, and televisions. Due to the display principle of liquid crystal display devices, a polarizing plate is arranged on the viewing side surface of the liquid crystal cell. In self-luminous display devices such as organic EL, a circular polarizing plate (a laminate of a polarizing plate and a quarter-wave plate) is arranged on the viewing side surface of the cell to prevent external light from being reflected by the metal electrode (cathode) and being viewed as a mirror surface.

[0003] A front transparent plate (also called a "cover window") such as a transparent resin plate or a glass plate is provided on the viewing side surface of the image display device for the purpose of preventing damage to the image display panel due to impact from the outer surface, etc. The cover window is attached to the polarizing plate arranged on the viewing side surface of the image display panel via an adhesive sheet.

[0004] A polarizing plate generally has a laminated structure in which transparent protective films are bonded to both sides of a polarizer, but from the viewpoint of making image display devices thinner and more flexible, a structure in which the transparent protective films on one or both sides of the polarizer are omitted has been proposed. For example, Patent Document 1 discloses a structure in which a cover window is bonded to a polarizer via an adhesive sheet disposed in contact with the polarizer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2017 / 216886 Summary of the Invention [Problem to be solved by the invention]

[0006] It has been found that an image display device in which a cover window is bonded to a pressure-sensitive adhesive sheet provided in contact with the viewing side surface of a polarizer is prone to yellowing of the polarizer in a weather resistance test and discoloration of the polarizer in a humidification durability test, and thus has a problem with durability. Adjusting the composition of the pressure-sensitive adhesive placed in contact with the polarizer in order to increase durability tends to reduce adhesion reliability. In view of this problem, the present invention aims to provide a pressure-sensitive adhesive sheet that can contribute to a thinner image display device and is unlikely to cause discoloration of the polarizer or peeling between the polarizer and the cover window, and that can form an image display device with excellent durability. [Means for solving the problem]

[0007] One embodiment of the present invention is an adhesive sheet used for bonding a polarizer made of a polyvinyl alcohol-based film containing iodine to a cover window of an image display device. The adhesive sheet is made of an adhesive composition containing an acrylic-based polymer and an ultraviolet absorbing agent, and is arranged in contact with the polarizer. The optical transmittance of the adhesive sheet at a wavelength of 380 nm is preferably 5% or less.

[0008] The acrylic base polymer contained in the pressure-sensitive adhesive composition preferably contains 5 parts by weight or less of nitrogen-containing monomer, preferably 0.1 to 8 parts by weight of hydroxyl group-containing monomer, and preferably 1 part by weight or less of carboxyl group-containing monomer, relative to 100 parts by weight of the total of monomer components.

[0009] The acrylic base polymer may contain 20 to 75 parts by weight of a high Tg monomer that does not contain any of a hydroxy group, a carboxy group, and a nitrogen atom and has a homopolymer glass transition temperature of 10° C. or higher, relative to 100 parts by weight of the total of the monomer components. The high Tg monomer may be a (meth)acrylic acid ester having an alicyclic structure.

[0010] The acrylic base polymer may contain 20 to 79 parts by weight of a (meth)acrylic acid alkyl ester having a homopolymer glass transition temperature of −40° C. or lower, based on 100 parts by weight of the total of the monomer components.

[0011] The acrylic base polymer may have a crosslinked structure formed by a thermal crosslinking agent.

[0012] The adhesive composition constituting the adhesive sheet may contain a photopolymerizable polyfunctional compound having two or more photopolymerizable functional groups in one molecule, and a photopolymerization initiator.

[0013] One embodiment of the present invention is a polarizing plate with adhesive, which is made of a polyvinyl alcohol-based film containing iodine and has a first main surface and a second main surface, and the above-mentioned adhesive sheet is arranged on the first main surface of a polarizer having the first main surface and the second main surface. The polarizing plate with adhesive may further include an adhesive sheet on the second main surface side of the polarizer. The adhesive sheet arranged on the second main surface side of the polarizer may be in contact with the second main surface of the polarizer, or may be laminated on the second main surface of the polarizer via another layer.

[0014] One embodiment of the present invention is an image display device having, in this order, a second adhesive sheet, a polarizer made of a polyvinyl alcohol-based film containing iodine, a first adhesive sheet, and a cover window on the surface of an image display cell, wherein the first adhesive sheet is the above-mentioned adhesive sheet and is arranged in contact with the polarizer.

[0015] When the adhesive composition constituting the adhesive sheet contains a photopolymerizable multifunctional compound and a photopolymerization initiator, in forming an image display device, a polarizer and a cover window may be bonded together via a first adhesive sheet, and then active light may be irradiated from the cover window side to photocure the adhesive composition. Effect of the Invention

[0016] An image display device in which the pressure-sensitive adhesive sheet of an embodiment of the present invention is placed in contact with the viewing side surface of a polarizer suppresses discoloration and fading of the polarizer caused by external ultraviolet rays, heating, humidification, etc., and has excellent durability and interlayer adhesion reliability. [Brief description of the drawings]

[0017] [Figure 1] 1 is a cross-sectional view illustrating an embodiment of an image display device. [Diagram 2] FIG. 1 is a cross-sectional view showing one embodiment of a polarizing plate with a pressure-sensitive adhesive. [Diagram 3] FIG. 1 is a cross-sectional view illustrating one embodiment of a polarizing plate with a pressure-sensitive adhesive. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] One embodiment of the present invention is a pressure-sensitive adhesive sheet that is placed in contact with the viewing side surface of a polarizer in an image display device, and is used to bond the polarizer and a cover window.

[0019] 1 is a cross-sectional view showing one embodiment of an image display device having a cover window on the viewing side surface. The image display device 100 has a polarizing plate 10 attached to the surface of an image display cell 60 via an adhesive sheet 22, and a cover window 70 attached to the polarizing plate 10 via an adhesive sheet 21 of an embodiment of the present invention.

[0020] The polarizing plate 10 includes a polarizer 11 made of a polyvinyl alcohol-based film containing iodine. In the polyvinyl alcohol-based polarizer containing iodine, the polymer chain of polyvinyl alcohol and the polyiodine ion (I3 - and I5 - ) form a complex, and the polymer chains are oriented in a specific direction, which in turn aligns the polyiodine ions, thereby providing polarizing properties.

[0021] An appropriate optical layer 15 may be provided on the second main surface (surface on the image display cell 60 side) of the polarizer 11. The pressure-sensitive adhesive sheet 21 of the embodiment of the present invention is disposed on the first main surface (surface on the viewing side) of the polarizer 11 in contact with the polarizer 11. By disposing the pressure-sensitive adhesive sheet 21 on the viewing side of the polarizer 11 without any other optical layer therebetween, it is possible to make the image display device thinner and more flexible.

[0022] [Adhesive sheet] <Base polymer> The adhesive composition constituting the adhesive sheet 21 contains an acrylic-based polymer. The acrylic-based polymer contains a (meth)acrylic acid alkyl ester as a main constituent monomer component. In this specification, "(meth)acrylic" means acrylic and / or methacrylic.

[0023] As the (meth)acrylic acid alkyl ester, a (meth)acrylic acid alkyl ester having an alkyl group with a carbon number of 1 to 20 is preferably used. The (meth)acrylic acid alkyl ester may have an alkyl group that is branched, or may have a cyclic alkyl group (alicyclic alkyl group).

[0024] Specific examples of (meth)acrylic acid alkyl esters having a chain alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, and butyl (meth)acrylate. ) nonyl acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, isododecyl (meth)acrylate, tetradecyl (meth)acrylate, isotetradecyl (meth)acrylate, pentadecyl (meth)acrylate, cetyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isooctadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.

[0025] Specific examples of the (meth)acrylic acid alkyl ester having an alicyclic alkyl group include (meth)acrylic acid cycloalkyl esters such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, and cyclooctyl (meth)acrylate; (meth)acrylic acid esters having a bicyclic aliphatic hydrocarbon ring such as isobornyl (meth)acrylate; and (meth)acrylic acid esters having a tricyclic or higher aliphatic hydrocarbon ring such as dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, tricyclopentanyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, and 2-ethyl-2-adamantyl (meth)acrylate. The (meth)acrylic acid alkyl ester having an alicyclic alkyl group may have a substituent on the ring such as 3,3,5-trimethylcyclohexyl (meth)acrylate. The (meth)acrylic acid alkyl ester having an alicyclic alkyl group may be a (meth)acrylic acid ester containing a condensed ring of an alicyclic structure and a ring structure having an unsaturated bond, such as dicyclopentenyl (meth)acrylate.

[0026] The amount of the (meth)acrylic acid alkyl ester relative to 100 parts by weight of the total amount of the monomer components constituting the acrylic base polymer is preferably 60 parts by weight or more, more preferably 70 parts by weight or more, even more preferably 80 parts by weight or more, and may be 85 parts by weight or more, 90 parts by weight or more, or 92 parts by weight or more.

[0027] The acrylic base polymer preferably contains an acrylic monomer having a crosslinkable functional group as a copolymerization monomer component. By having the crosslinkable functional group in the base polymer, the base polymer can be reacted with a crosslinking agent to increase the cohesive strength of the pressure-sensitive adhesive and improve the adhesion reliability.

[0028] Examples of acrylic monomers having crosslinkable functional groups include hydroxyl group-containing monomers and carboxyl group-containing monomers. For example, when an isocyanate-based crosslinking agent is used, a crosslinking structure is introduced by the reaction between a hydroxyl group and an isocyanate group. When an epoxy-based crosslinking agent is used, a crosslinking structure is introduced by the reaction between a carboxyl group and an epoxy group. As described below, from the viewpoint of making the adhesive acid-free, it is preferable to use a hydroxyl group-containing monomer as a copolymerization component of the base polymer and introduce a crosslinking structure by an isocyanate-based crosslinking agent. When the base polymer contains a hydroxyl group-containing monomer as a monomer component, the crosslinking property of the base polymer is enhanced and the opacity of the adhesive in a high temperature and high humidity environment tends to be suppressed, resulting in a highly transparent adhesive.

[0029] Examples of hydroxyl group-containing monomers include (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methyl acrylate. Among these, 2-hydroxyethyl acrylate (Tg of homopolymer: -15°C) and 4-hydroxybutyl acrylate (Tg of homopolymer: -32°C) are preferred because they contribute greatly to improving adhesive strength and can suppress clouding of the pressure-sensitive adhesive sheet in a high humidity environment.

[0030] The amount of the hydroxyl group-containing monomer relative to 100 parts by weight of the total amount of the monomer components constituting the acrylic base polymer is preferably 0.1 parts by weight or more, more preferably 0.5 parts by weight or more, and even more preferably 0.8 parts by weight or more, and may be 1 part by weight or more, 1.5 parts by weight or more, or 2 parts by weight or more. By increasing the amount of the hydroxyl group-containing monomer, the unreacted functional groups of the crosslinking agent are reduced, so that the degree of crosslinking can be increased with a small amount of crosslinking agent, and the adhesion reliability can be improved.

[0031] On the other hand, if the amount of the hydroxyl group-containing monomer in the base polymer is excessively large, the hydrophilicity and moisture permeability of the adhesive sheet increases with an increase in the polarity of the polymer, and the polarizer 11 arranged in contact with the adhesive sheet 21 is likely to fade under high temperature and high humidity conditions. If the adhesive sheet has high hydrophilicity and moisture permeability, moisture from the external environment is likely to reach the polarizer, and the orientation of the polymer chains constituting the polarizer is disturbed by moisture, and polyiodine ions are detached from the polymer chains, which is thought to be one of the causes of the fading of the polarizer. The amount of the hydroxyl group-containing monomer relative to 100 parts by weight of the total amount of the monomer components constituting the acrylic base polymer is preferably 8 parts by weight or less, more preferably 7 parts by weight or less, and may be 6 parts by weight or less or 5 parts by weight or less.

[0032] The acrylic base polymer may contain monomer components other than those described above. The acrylic base polymer may contain, as monomer components, for example, vinyl ester monomers, aromatic vinyl monomers, epoxy group-containing monomers, vinyl ether monomers, and the like.

[0033] The acrylic base polymer may contain a nitrogen-containing monomer as a monomer component, such as N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, (meth)acryloylmorpholine, N-vinylcarboxylic acid amides, N-vinylcaprolactam, acrylonitrile, and methacrylonitrile.

[0034] The acrylic base polymer contains a nitrogen-containing monomer as a monomer component, which tends to improve the cohesive force and enhance the adhesion reliability. On the other hand, as the amount of the nitrogen-containing monomer in the base polymer contained in the adhesive increases, the polarizer 11 arranged in contact with the adhesive sheet 21 is more likely to fade. Since nitrogen atoms are easily coordinated to iodine, when the amount of nitrogen atoms contained in the base polymer of the adhesive sheet increases, it is considered that one of the causes of the fading of the polarizer is that iodine fixed to the polymer chain of the polarizer is detached from the polymer chain by coordinating with the nitrogen atom of the adhesive. The amount of the nitrogen-containing monomer relative to 100 parts by weight of the total amount of the monomer components constituting the acrylic base polymer is preferably 5 parts by weight or less, more preferably 3 parts by weight or less, and may be 1 part by weight or less, 0.5 parts by weight or less, 0.1 parts by weight or less, or 0.05 parts by weight or less. The acrylic base polymer may not contain a nitrogen-containing monomer as a monomer component.

[0035] If the acid component contained in the adhesive sheet migrates to the polarizer, it may promote hydrolysis of polyvinyl alcohol, which may cause the polarizer to deteriorate. Therefore, the adhesive sheet 21 preferably has a low content of organic acid monomers (free organic acids) such as (meth)acrylic acid. In a thermosetting or photosetting polymer, the presence of unreacted residual monomers is inevitable. Therefore, in order to reduce the content of acid monomers in the adhesive sheet, it is preferable to reduce the amount of organic acid monomer components such as (meth)acrylic acid in the monomer components constituting the base polymer. The content of the carboxyl group-containing monomer relative to the total amount of 100 parts by weight of the constituent monomer components of the acrylic base polymer is preferably 1 part by weight or less, more preferably 0.5 parts by weight or less, and even more preferably 0.1 parts by weight or less. It is preferable that the acrylic base polymer does not contain a carboxyl group-containing monomer as a monomer component.

[0036] From the viewpoint of suppressing fading of the polarizer 11 in a high-temperature and high-humidity environment, the base polymer constituting the adhesive sheet 21 arranged in contact with the polarizer 11 preferably has low polarity. In order to reduce the polarity of the base polymer, it is preferable that the content of polar monomers such as nitrogen-containing monomers, hydroxyl group-containing monomers, and carboxyl group-containing monomers as constituent monomer components is small. The content of the polar monomer relative to 100 parts by weight of the total amount of the constituent monomer components of the acrylic base polymer is preferably 12 parts by weight or less, more preferably 10 parts by weight or less, even more preferably 8 parts by weight or less, and may be 6 parts by weight or less, or 5 parts by weight or less.

[0037] The acrylic base polymer may not contain a polar monomer as a constituent monomer component. However, from the viewpoint of introducing a crosslinking structure by a thermal crosslinking agent such as an isocyanate-based crosslinking agent into the base polymer, it is preferable that the polar monomer such as a hydroxyl group-containing monomer is contained in an amount of 0.1 parts by weight or more. The content of the polar monomer relative to 100 parts by weight of the total amount of the constituent monomer components of the acrylic base polymer is more preferably 0.5 parts by weight or more, further preferably 0.8 parts by weight or more, and may be 1 part by weight or more, 1.5 parts by weight or more, or 2 parts by weight or more.

[0038] From the viewpoint of increasing the cohesive strength of an acrylic base polymer having a small content of polar monomer components and improving adhesion reliability, it is preferable that the acrylic base polymer contains, as a constituent monomer component, a high Tg monomer that does not contain any of a hydroxy group, a carboxy group, and a nitrogen atom and whose homopolymer has a glass transition temperature of 10°C or higher.

[0039] Examples of high Tg monomers not containing polar groups include styrene (Tg: 80°C), methyl methacrylate (Tg: 105°C), cyclohexyl acrylate (Tg: 15°C), cyclohexyl methacrylate (Tg: 66°C), 3,3,5-trimethylcyclohexyl acrylate (Tg: 52°C), dicyclopentanyl methacrylate (Tg: 175°C), dicyclopentanyl acrylate (Tg: 120°C), dicyclopentenyl acrylate (Tg: 120°C), isobornyl methacrylate (Tg: 173°C), isobornyl acrylate (Tg: 97°C), 1-adamantyl methacrylate (Tg: 250°C), and 1-adamantyl acrylate (Tg: 153°C). Among these high Tg monomers, acrylic acid esters are preferred because they have excellent copolymerizability with the low Tg monomers (lower alkyl acrylic esters) described below. In addition, since both acrylic acid esters and methacrylic acid esters can exhibit high Tg, (meth)acrylic acid esters having an alicyclic structure are preferred as high Tg monomers, and among them, acrylic acid esters having an alicyclic structure such as cyclohexyl acrylate, dicyclopentanyl acrylate, dicyclopentenyl acrylate, isobornyl acrylate, and 1-adamantyl acrylate are preferred. The high Tg monomer may have a glass transition temperature of 13°C or higher or 15°C or higher as a homopolymer.

[0040] From the viewpoint of improving the adhesive reliability of the pressure-sensitive adhesive sheet, the content of the high Tg monomer not containing a polar group relative to the total amount of 100 parts by weight of the constituent monomer components of the acrylic base polymer is preferably 20 parts by weight or more, more preferably 25 parts by weight or more, and even more preferably 30 parts by weight or more. On the other hand, if the content of the high Tg monomer is excessively large, the glass transition temperature of the base polymer increases, and the adhesiveness and impact resistance at low temperatures may decrease. Therefore, the content of the high Tg monomer not containing a polar group relative to the total amount of 100 parts by weight of the constituent monomer components of the acrylic base polymer is preferably 75 parts by weight or less, more preferably 70 parts by weight or less, and may be 65 parts by weight or less, 60 parts by weight or less, 55 parts by weight or less, or 50 parts by weight or less.

[0041] From the viewpoint of achieving both the adhesive reliability of the pressure-sensitive adhesive sheet and the adhesiveness and impact resistance at low temperatures, the glass transition temperature of the acrylic base polymer is preferably −50 to 10° C., more preferably −45 to 5° C., and even more preferably −40 to 0° C. The glass transition temperature of the acrylic base polymer may be calculated based on the theoretical Tg. The theoretical Tg is the glass transition temperature Tg of a homopolymer of the constituent monomer components of the base polymer. i and the weight fraction W of each monomer component i It is calculated using the following Fox formula: 1 / Tg=Σ(W i / Tg i )

[0042] Tg is the glass transition temperature of the base polymer (unit: K), W i is the weight fraction of monomer component i constituting the base polymer (copolymerization ratio by weight), Tg i is the glass transition temperature (unit: K) of the homopolymer of monomer component i. The glass transition temperature of the homopolymer can be the value described in Polymer Handbook, 3rd Edition (John Wiley & Sons, Inc., 1989). For the Tg of the homopolymer of a monomer not described in the above literature, the peak top temperature of the loss tangent (tan δ) measured by dynamic viscoelasticity measurement can be used.

[0043] In order to set the glass transition temperature of the acrylic base polymer containing 20 parts by weight or more of a high Tg monomer as a monomer component within the above range, the acrylic base polymer preferably contains a low Tg monomer having a homopolymer glass transition temperature of -40°C or less as a monomer component. Examples of the low Tg monomer include acrylic acid chain alkyl esters such as 2-ethylhexyl acrylate (Tg: -70°C), n-hexyl acrylate (Tg: -65°C), n-octyl acrylate (Tg: -65°C), isononyl acrylate (Tg: -60°C), n-nonyl acrylate (Tg: -58°C), isooctyl acrylate (Tg: -58°C), and butyl acrylate (Tg: -55°C). Among these, butyl acrylate and 2-ethylhexyl acrylate are particularly preferred.

[0044] The content of the (meth)acrylic acid alkyl ester having a homopolymer glass transition temperature of -40°C or lower relative to 100 parts by weight of the total amount of the constituent monomer components of the acrylic base polymer is preferably 20 to 79 parts by weight, more preferably 25 to 70 parts by weight, and may be 30 to 65 parts by weight.

[0045] The monomer components are polymerized by various known methods such as solution polymerization, emulsion polymerization, and bulk polymerization to obtain an acrylic base polymer. From the viewpoint of the balance of properties such as adhesive strength and holding power of the adhesive, and the cost, the solution polymerization method is preferable. As a solvent for solution polymerization, ethyl acetate, toluene, etc. are generally used. The solution concentration is usually about 20 to 80% by weight. As a polymerization initiator, a thermal polymerization initiator such as an azo initiator, a peroxide initiator, or a redox initiator combining a peroxide and a reducing agent (for example, a combination of a persulfate and sodium hydrogen sulfite, or a combination of a peroxide and sodium ascorbate) is preferably used. The amount of the polymerization initiator is not particularly limited, but for example, it is preferably about 0.005 to 5 parts by weight, more preferably about 0.02 to 3 parts by weight, based on 100 parts by weight of the total amount of the monomer components forming the base polymer.

[0046] A chain transfer agent may be used to adjust the molecular weight of the base polymer. The chain transfer agent receives radicals from the growing polymer chain to stop the elongation of the polymer, and the chain transfer agent that has received the radicals attacks the monomer to restart polymerization. Therefore, by using a chain transfer agent, it is possible to suppress an increase in the molecular weight of the base polymer without decreasing the radical concentration in the reaction system. As the chain transfer agent, for example, thiols such as α-thioglycerol, lauryl mercaptan, glycidyl mercaptan, mercaptoacetic acid, 2-mercaptoethanol, thioglycolic acid, 2-ethylhexyl thioglycolate, and 2,3-dimercapto-1-propanol are preferably used.

[0047] The amount of chain transfer agent used is not particularly limited, but if the amount of chain transfer agent used is too large, the molecular weight of base polymer decreases, and the processability and processing dimensional stability of the adhesive sheet before photocuring may decrease.Therefore, the amount of chain transfer agent used is preferably 1 part by weight or less, more preferably 0.3 parts by weight or less, even more preferably 0.15 parts by weight or less, and particularly preferably 0.1 parts by weight or less, based on 100 parts by weight of the total amount of the monomer components constituting the base polymer.

[0048] The weight average molecular weight of the acrylic base polymer is preferably 100,000 to 3,000,000, more preferably 250,000 to 2,000,000, and even more preferably 500,000 to 1,500,000. When a crosslinked structure is introduced into the acrylic base polymer, the molecular weight of the base polymer refers to the molecular weight before the introduction of the crosslinked structure.

[0049] <Cross-linked structure of base polymer> The acrylic base polymer preferably has a crosslinked structure. Methods for introducing a crosslinked structure into a base polymer generally include (1) a method in which a base polymer having a functional group capable of reacting with a crosslinking agent is polymerized, and then a crosslinking agent is added to react the base polymer with the crosslinking agent; and (2) a method in which a photopolymerizable multifunctional compound is included in the polymerization components of the base polymer to introduce a branched structure (crosslinked structure) into the polymer chain.

[0050] In the adhesive composition constituting the adhesive sheet 21 arranged in contact with the polarizer 11, the acrylic base polymer preferably has a crosslinked structure introduced by the above method (1). The adhesive composition constituting the adhesive sheet 21 may contain a photopolymerizable multifunctional compound and a photopolymerization initiator, and may be one in which the crosslinked structure of the above method (2) is introduced by photocuring after bonding the adhesive sheet 21 and the cover window 70 together. That is, the adhesive composition constituting the adhesive sheet 21 preferably has a base polymer with a crosslinked structure caused by a (thermal) crosslinking agent such as an isocyanate-based crosslinking agent, and may further be one in which a crosslinked structure caused by a photopolymerizable multifunctional compound (photocrosslinking agent) can be introduced by photocuring.

[0051] <Adhesive composition> A pressure-sensitive adhesive composition is prepared by mixing an acrylic base polymer with a crosslinking agent, a photopolymerizable multifunctional compound, a photopolymerization initiator, and, if necessary, an oligomer or various additives. The pressure-sensitive adhesive composition preferably has a viscosity (for example, about 0.5 to 20 Pa·s) suitable for application onto a substrate. The viscosity of the pressure-sensitive adhesive composition can be adjusted to an appropriate range by adjusting the molecular weight of the base polymer, the amount of the photopolymerizable multifunctional compound added, and the composition, molecular weight, and amount added of other components (for example, oligomers). A thickening additive or the like may be used for the purpose of viscosity adjustment or the like.

[0052] (UV absorber) The adhesive sheet 21 preferably has ultraviolet absorbing properties. In a polarizing plate in which a transparent protective film is provided on the viewing side surface of the polarizer, the transparent protective film generally has ultraviolet absorbing properties to suppress deterioration of the polarizer due to ultraviolet rays incident from outside the display device. On the other hand, in a configuration in which the adhesive sheet 21 is disposed in contact with the viewing side surface of the polarizer 11, since no transparent protective film is provided on the viewing side of the polarizer, the adhesive sheet 21 is provided with ultraviolet absorbing properties to suppress photodeterioration of the polarizer 11 caused by ultraviolet rays (for example, structural changes in polyiodine ions (I5 - From I3 - It is preferable to prevent color change of the polarizer due to the change to a transparent state or the like.

[0053] In order to impart ultraviolet absorbing properties to the adhesive sheet 21, the adhesive composition preferably contains an ultraviolet absorbing agent. Examples of ultraviolet absorbing agents include benzotriazole-based ultraviolet absorbing agents, benzophenone-based ultraviolet absorbing agents, triazine-based ultraviolet absorbing agents, salicylate-based ultraviolet absorbing agents, and cyanoacrylate-based ultraviolet absorbing agents. Triazine-based ultraviolet absorbing agents and benzotriazole-based ultraviolet absorbing agents are preferred because they have high ultraviolet absorbing properties, are highly compatible with acrylic polymers, and are easy to use to obtain highly transparent acrylic adhesives. Among these, triazine-based ultraviolet absorbing agents containing a hydroxyl group and benzotriazole-based ultraviolet absorbing agents having one benzotriazole skeleton in one molecule are preferred.

[0054] Commercially available products may be used as the ultraviolet absorber. Commercially available triazine-based ultraviolet absorbers include the reaction product of 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl)-5-hydroxyphenyl and [(alkyloxy)methyl]oxirane (BASF's "TINUVIN 400"), the reaction product of 2-(2,4-dihydroxyphenyl)-4,6-bis-(2,4-dimethylphenyl)-1,3,5-triazine and (2-ethylhexyl)-glycidic acid ester (BASF's "TINUVIN 405"), (2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine (BASF's "TINUVIN 460"), 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol (BASF "TINUVIN 577"), 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (BASF "TINUVIN 479"), 5,5'-bis(2-ethylhexyloxy)-2,2'-[6-(4-methoxyphenyl)-1,3,5-triazine-2,4-diyl]diphenol (BASF "Tinosorb S"), 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]-phenol (ADEKA "ADK STAB LA-46" and others.

[0055] Commercially available benzotriazole UV absorbers include 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (BASF's "TINUVIN 928"), 2-(2-hydroxy-5-tert-butylphenyl)-2H-benzotriazole (BASF's "TINUVIN PS"), 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (BASF's "TINUVIN 900"), and 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (BASF's "TINUVIN 928"), 2-(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol (BASF "TINUVIN 571"), 2-(2H-benzotriazol-2-yl)-p-cresol (BASF "TINUVIN P"), 2-(2H-benzotriazol-2-yl)-4-6-bis(1-methyl-1-phenylethyl)phenol (BASF "TINUVIN 234"), 2-[5-chloro(2H)-benzotriazol-2-yl]-4-methyl-6-(tert-butyl)phenol (BASF "TINUVIN 326"), 2-(2H-benzotriazol-2-yl)-4,6-di-tert-pentylphenol (BASF "TINUVIN 328"), 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (BASF "TINUVIN 329"), benzenepropanoic acid and 3-(2H-benzotriazol-2-yl)-5-(1,Examples of such compounds include esters of 1-dimethylethyl)-4-hydroxy (C7-9 side chain and linear alkyl) (BASF's "TINUVIN 384-2"), reaction products of methyl-3-(3-(2H-benzotriazol-2-yl)-5-t-butyl-4-hydroxyphenyl)propionate and polyethylene glycol (BASF's "TINUVIN 1 130"), reaction products of methyl 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate and polyethylene glycol 300 (BASF's "TINUVIN 213"), and 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimido-methyl)-5-methylphenyl]benzotriazole (Sumitomo Chemical's "Sumisorb 250"), etc.

[0056] When the pressure-sensitive adhesive composition contains an ultraviolet absorbing agent, the content of the ultraviolet absorbing agent relative to 100 parts by weight of the acrylic base polymer is about 0.05 to 10 parts by weight, preferably 0.1 to 5 parts by weight, and more preferably 0.3 to 3 parts by weight. By setting the content of the ultraviolet absorbing agent within the above range, it is possible to impart ultraviolet shielding properties to the pressure-sensitive adhesive sheet 21 while suppressing a decrease in transparency due to bleeding out of the ultraviolet absorbing agent, and to suppress photodegradation of the polarizer caused by ultraviolet rays from the outside.

[0057] (Crosslinking agent) As described above, the acrylic base polymer preferably has a crosslinked structure. The crosslinked structure is introduced into the base polymer by adding a crosslinking agent to the adhesive composition and heating it as necessary. In order to distinguish it from the crosslinked structure introduced by the photopolymerizable multifunctional compound, the crosslinking by the isocyanate crosslinking agent or the like may be described as "thermal crosslinking", but the introduction of the crosslinked structure by the crosslinking agent may not be accompanied by heating. By introducing a thermal crosslinked structure into the acrylic base polymer, the cohesiveness of the adhesive sheet is increased, and the adhesiveness tends to be improved.

[0058] Examples of the crosslinking agent include compounds that react with functional groups such as hydroxyl groups contained in the base polymer. Specific examples of the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, carbodiimide-based crosslinking agents, and metal chelate-based crosslinking agents. Among these, isocyanate-based crosslinking agents are preferred because they have high reactivity with the hydroxyl groups of the base polymer and are easy to introduce a crosslinked structure.

[0059] As the isocyanate crosslinking agent, a polyisocyanate having two or more isocyanate groups in one molecule is used. Examples of the isocyanate crosslinking agent include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate, and isophorone diisocyanate; aromatic isocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and xylylene diisocyanate; trimethylolpropane / Examples of isocyanate adducts include tolylene diisocyanate trimer adducts (e.g., "Coronate L" manufactured by Tosoh), trimethylolpropane / hexamethylene diisocyanate trimer adducts (e.g., "Coronate HL" manufactured by Tosoh), trimethylolpropane adducts of xylylene diisocyanate (e.g., "Takenate D110N" manufactured by Mitsui Chemicals, and isocyanurate of hexamethylene diisocyanate (e.g., "Coronate HX" manufactured by Tosoh).

[0060] The cohesive strength and adhesive strength of the pressure-sensitive adhesive can be adjusted by adjusting the amount of the crosslinking agent added. The amount of the crosslinking agent added is preferably 0.01 to 1 part by weight, more preferably 0.05 to 0.7 parts by weight, and even more preferably 0.1 to 0.5 parts by weight, relative to 100 parts by weight of the base polymer.

[0061] (Photopolymerizable polyfunctional compound) In order to impart photocurability to the adhesive sheet, the adhesive composition preferably contains a photopolymerizable multifunctional compound. The photopolymerizable multifunctional compound has two or more photopolymerizable functional groups in one molecule. The photopolymerizable functional group may be any of radical polymerizable, cationic polymerizable, and anionic polymerizable, but a radical polymerizable functional group having an unsaturated double bond (ethylenically unsaturated group) is preferable because of its excellent reactivity. As the photopolymerizable multifunctional compound, a multifunctional (meth)acrylate is preferable because of its high compatibility with an acrylic-based polymer, and a multifunctional acrylate is particularly preferable because of its high photoradical reactivity.

[0062] Examples of polyfunctional (meth)acrylates include hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, bisphenol A ethylene oxide modified di(meth)acrylate, bisphenol A propylene oxide modified di(meth)acrylate, alkanediol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, pentaerythritol di(meth)acrylate, neopentyl glycol di(meth)acrylate, and glycerin di(meth)acrylate. trifunctional (meth)acrylic acid esters such as pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, and ethoxylated isocyanuric acid tri(meth)acrylate; tetrafunctional (meth)acrylic acid esters such as ditrimethylolpropane tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, and pentaerythritol tetra(meth)acrylate; and penta- or higher functional (meth)acrylic acid esters such as dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate.

[0063] From the viewpoint of improving the adhesive reliability of the pressure-sensitive adhesive sheet after photocuring, the molecular weight of the photopolymerizable multifunctional compound is preferably 1500 or less, and more preferably 1000 or less. The functional group equivalent (g / eq) of the multifunctional compound is preferably 50 to 500, more preferably 70 to 300, and even more preferably 80 to 200. In order to exhibit appropriate compatibility with the base polymer, the photopolymerizable multifunctional compound is preferably a liquid at room temperature.

[0064] The content of the photopolymerizable multifunctional compound in the adhesive composition is preferably 0.3 to 15 parts by weight, more preferably 0.5 to 10 parts by weight, and even more preferably 1 to 5 parts by weight, based on 100 parts by weight of the acrylic base polymer. When the content of the photopolymerizable multifunctional compound is low, the adhesive reliability of the adhesive sheet after photocuring tends to be insufficient. On the other hand, when the content of the photocurable multifunctional compound is excessively large, the ratio of the base polymer in the adhesive sheet (adhesive composition) before photocuring becomes small, and the processability and processing dimensional stability of the adhesive sheet may decrease. In addition, when the content of the photocurable multifunctional compound is excessively large, the adhesive sheet after photocuring becomes hard, and the adhesive strength and impact resistance of the adhesive sheet 21 at low temperatures may become insufficient.

[0065] (Photopolymerization initiator) The photocurable adhesive composition containing the photopolymerizable polyfunctional compound preferably contains a photopolymerization initiator. Examples of the photopolymerization initiator include benzoin ether-based photopolymerization initiators, acetophenone-based photopolymerization initiators, α-ketol-based photopolymerization initiators, aromatic sulfonyl chloride-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzyl-based photopolymerization initiators, benzophenone-based photopolymerization initiators, ketal-based photopolymerization initiators, thioxanthone-based photopolymerization initiators, and acylphosphine oxide-based photopolymerization initiators. The content of the photopolymerization initiator in the adhesive composition is preferably 0.01 to 5 parts by weight, more preferably 0.05 to 3 parts by weight, based on 100 parts by weight of the base polymer.

[0066] (Oligomer) The pressure-sensitive adhesive composition may contain various oligomers for the purpose of adjusting the adhesive strength and viscosity of the pressure-sensitive adhesive sheet, etc. As the oligomer, for example, one having a weight average molecular weight of about 1000 to 30000 is used. As the oligomer, an acrylic oligomer is preferable because it has excellent compatibility with the acrylic base polymer.

[0067] The acrylic oligomer contains an alkyl (meth)acrylate ester as a main constituent monomer component. Among them, it is preferable to use an alkyl (meth)acrylate ester having a chain alkyl group (chain alkyl (meth)acrylate) and an alkyl (meth)acrylate ester having an alicyclic alkyl group (alicyclic alkyl (meth)acrylate) as the constituent monomer component. Specific examples of the chain alkyl (meth)acrylate and the alicyclic alkyl (meth)acrylate are as exemplified above as the constituent monomers of the acrylic base polymer.

[0068] The glass transition temperature of the acrylic oligomer is preferably 20°C or higher, more preferably 50°C or higher, even more preferably 80°C or higher, and particularly preferably 100°C or higher. The adhesive strength of the pressure-sensitive adhesive sheet tends to be improved by using a low Tg base polymer with a crosslinked structure introduced and a high Tg acrylic oligomer in combination. The upper limit of the glass transition temperature of the acrylic oligomer is not particularly limited, but is generally 200°C or lower, preferably 180°C or lower, and more preferably 160°C or lower. The glass transition temperature of the acrylic oligomer is calculated by the above-mentioned Fox formula.

[0069] Among the exemplified (meth)acrylic acid alkyl esters, methyl methacrylate is preferred as the chain alkyl (meth)acrylate because it has a high glass transition temperature and excellent compatibility with the base polymer. As the alicyclic alkyl (meth)acrylate, dicyclopentanyl acrylate, dicyclopentanyl methacrylate, cyclohexyl acrylate, and cyclohexyl methacrylate are preferred. That is, the acrylic oligomer preferably contains, as a constituent monomer component, one or more selected from the group consisting of dicyclopentanyl acrylate, dicyclopentanyl methacrylate, cyclohexyl acrylate, and cyclohexyl methacrylate, and methyl methacrylate.

[0070] The amount of the alicyclic alkyl (meth)acrylate relative to the total amount of the monomer components constituting the acrylic oligomer is preferably 10 to 90% by weight, more preferably 20 to 80% by weight, and even more preferably 30 to 70% by weight. The amount of the chain alkyl (meth)acrylate relative to the total amount of the monomer components constituting the acrylic oligomer is preferably 10 to 90% by weight, more preferably 20 to 80% by weight, and even more preferably 30 to 70% by weight.

[0071] The weight average molecular weight of the acrylic oligomer is preferably from 1000 to 30000, more preferably from 1500 to 10000, and even more preferably from 2000 to 8000. By using an acrylic oligomer having a molecular weight within this range, the adhesive strength and adhesive retention of the pressure-sensitive adhesive sheet tend to be improved.

[0072] The acrylic oligomer can be obtained by polymerizing the above-mentioned monomer components by various polymerization methods. Various polymerization initiators may be used in the polymerization of the acrylic oligomer. In addition, a chain transfer agent may be used for the purpose of adjusting the molecular weight.

[0073] When the pressure-sensitive adhesive composition contains an oligomer component such as an acrylic oligomer, the content is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, relative to 100 parts by weight of the base polymer. When the content of the oligomer in the pressure-sensitive adhesive composition is within the above range, improvement in adhesion can be expected.

[0074] (Silane coupling agent) A silane coupling agent may be added to the pressure-sensitive adhesive composition for the purpose of adjusting adhesive strength, etc. When a silane coupling agent is added to the pressure-sensitive adhesive composition, the amount added is usually about 0.01 to 5.0 parts by weight, and preferably about 0.03 to 2.0 parts by weight, per 100 parts by weight of the base polymer.

[0075] (Antioxidants) The pressure-sensitive adhesive composition may contain an antioxidant. By containing an antioxidant, it is possible to suppress the reaction or deterioration of the curable component caused by heat or light in the storage environment or use environment of the pressure-sensitive adhesive composition or the pressure-sensitive adhesive sheet. Examples of the antioxidant include amine-based antioxidants, sulfur-based antioxidants, phosphorus-based antioxidants, and phenol-based antioxidants. Among them, those that act as radical chain inhibitors such as amine-based antioxidants and phenol-based antioxidants are preferred, and phenol-based antioxidants having a hindered phenol structure are particularly preferred.

[0076] Antioxidants having a hindered phenol structure have a group with large steric hindrance, such as a tert-butyl group, bonded to at least one of the carbon atoms adjacent to the carbon atom on the aromatic ring to which the OH group of phenol is bonded. Examples of antioxidants having a hindered phenol structure include dibutylhydroxytoluene (BHT), pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (BASF's "Irganox 1010"), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (BASF's "Irganox 1076"), 3,3',3",5,5',5"-hexa-tert-butyl-a,a',a"-(mesitylene-2,4,6-triyl)tri-p-cresol (BASF's "Irganox 1076"). 1330"), 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (BASF "Irganox 3114"), tris[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxyethyl]isocyanurate (BASF "Irganox 3125"), pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (ADEKA "ADEKA STAB AO-60"), 3,9-bis{2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane (ADEKA "ADEKA STAB AO-80"), 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate (Sumitomo Chemical "Sumilizer GS"), 2-tert-butyl-4-methyl-6-(2-hydroxy-3-tert-butyl-5-methylbenzyl)phenyl acrylate (Sumitomo Chemical "Sumilizer GM"), 2,2'-dimethyl-2,2'-(2,4,8,10-tetraoxaspiro[5.5]undecane-3,9-diyl)dipropane-1,1'-diyl=bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propanoate] (Sumitomo Chemical's "Sumilizer GA-80"), 1,3,5-tris(3-hydroxy-4-tert-butyl-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (Cyanox 1790) and the like.

[0077] When the adhesive composition contains an antioxidant, the content of the antioxidant is preferably 0.01 parts by weight or more, more preferably 0.05 parts by weight or more, even more preferably 0.1 parts by weight or more, and may be 0.3 parts by weight or more or 0.5 parts by weight or more, based on 100 parts by weight of the acrylic base polymer, from the viewpoint of suppressing undesired curing reaction or deterioration. On the other hand, if the content of the antioxidant is excessively high, it may cause curing inhibition when the adhesive sheet is photocured. Therefore, the content of the antioxidant is preferably 10 parts by weight or less, more preferably 5 parts by weight or less, and even more preferably 3 parts by weight or less, based on 100 parts by weight of the acrylic base polymer.

[0078] (Other additives) In addition to the above-exemplified components, the pressure-sensitive adhesive composition may contain additives such as a chain transfer agent, a tackifier, a plasticizer, a softener, an antidegradant, a filler, a colorant, a surfactant, and an antistatic agent.

[0079] [Adhesive sheet] The adhesive composition is applied onto a substrate, and the solvent is dried and removed as necessary to form an adhesive sheet on the substrate. Any suitable substrate is used for forming the adhesive sheet. The substrate may be a release film having a release layer on the surface of a resin film.

[0080] Examples of the resin material of the release film include polyester resins such as polyethylene terephthalate and polyethylene naphthalate, acetate resins, polyethersulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, polyvinyl chloride resins, polyvinylidene chloride resins, polystyrene resins, polyvinyl alcohol resins, polyarylate resins, and polyphenylene sulfide resins. Among these, polyester resins such as polyethylene terephthalate are particularly preferred. The thickness of the release film is preferably 10 to 200 μm, and more preferably 25 to 150 μm. Examples of the material of the release layer include silicone-based release agents, fluorine-based release agents, long-chain alkyl-based release agents, and fatty acid amide-based release agents. The thickness of the release layer is generally about 10 to 2000 nm.

[0081] As a method for applying the pressure-sensitive adhesive composition onto a substrate, various methods such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brush, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coater can be used.

[0082] When the pressure-sensitive adhesive composition contains a solvent, it is preferable to dry the solvent after applying the pressure-sensitive adhesive composition onto the substrate. As the drying method, a suitable method can be adopted depending on the purpose. The heating and drying temperature is preferably 40°C to 200°C, more preferably 50°C to 180°C, and particularly preferably 70°C to 170°C. As the drying time, a suitable time can be adopted. The drying time is preferably 5 seconds to 20 minutes, more preferably 5 seconds to 15 minutes, and particularly preferably 10 seconds to 10 minutes.

[0083] After drying the solvent, it is preferable to attach a cover sheet to protect the surface of the pressure-sensitive adhesive sheet. As the cover sheet, it is preferable to use a release film having a release layer on the surface that comes into contact with the pressure-sensitive adhesive sheet, similar to the base film.

[0084] After the adhesive composition is applied onto the substrate, it is heated as necessary to introduce a crosslinked structure into the base polymer. The heating temperature and heating time may be appropriately set depending on the type of crosslinking agent used, and are usually in the range of 20°C to 160°C and about 1 minute to 7 days. The heating for drying the solvent may also serve as the heating for crosslinking. As mentioned above, the introduction of a crosslinked structure does not necessarily have to be accompanied by heating.

[0085] A crosslinking catalyst may be used to promote the formation of a crosslinked structure. For example, the crosslinking catalyst for the isocyanate-based crosslinking agent may be a metal-based crosslinking catalyst (especially a tin-based crosslinking catalyst) such as tetra-n-butyl titanate, tetraisopropyl titanate, nursem ferric, butyltin oxide, dioctyltin dilaurate, or dibutyltin dilaurate.

[0086] By laminating a release film on the surface of the adhesive sheet, an adhesive sheet having release films temporarily attached to both sides is obtained. The substrate or cover sheet used in forming the adhesive sheet may be used as the release film.

[0087] When release films are provided on both sides of the pressure-sensitive adhesive sheet, the thickness of one release film and the thickness of the other release film may be the same or different. The peeling force when peeling the release film temporarily attached to one side from the pressure-sensitive adhesive sheet and the peeling force when peeling the release film temporarily attached to the other side from the pressure-sensitive adhesive sheet may be the same or different.

[0088] The thickness of the adhesive sheet 21 used to attach the polarizer 11 and the cover window 70 is preferably 30 μm or more, more preferably 40 μm or more, and even more preferably 50 μm or more. By increasing the thickness of the adhesive sheet 21, impact resistance tends to increase. Furthermore, when the cover window 70 has a printing step due to decorative printing, the adhesive sheet 21 can be made to have step absorption properties. There is no particular upper limit on the thickness of the adhesive sheet 21, but from the viewpoint of the productivity of the adhesive sheet, etc., it is preferably 500 μm or less, more preferably 300 μm or less, and even more preferably 250 μm or less.

[0089] The total light transmittance of the pressure-sensitive adhesive sheet 21 is preferably 85% or more, and more preferably 90% or more. The haze of the pressure-sensitive adhesive sheet is preferably 1.5% or less, and more preferably 1% or less.

[0090] The optical transmittance of the adhesive sheet 21 at a wavelength of 380 nm is preferably 5% or less, more preferably 4% or less, and may be 3% or less. By increasing the ultraviolet shielding property of the adhesive sheet 21, it is possible to suppress photodegradation such as yellowing of the polarizer 11 caused by ultraviolet light incident from the outside. As described above, by including an ultraviolet absorbing agent in the adhesive composition, it is possible to impart ultraviolet absorbing properties to the adhesive sheet 21 while maintaining the transparency of visible light.

[0091] [Polarizing plate] <Polarizer> The polarizing plate 10 includes a polarizer 11. The polarizer 11 is a polyvinyl alcohol-based film containing iodine. As a material for the polyvinyl alcohol-based film applied to the polarizer, polyvinyl alcohol or a derivative thereof is used. Examples of the polyvinyl alcohol derivative include polyvinyl formal, polyvinyl acetal, etc., as well as derivatives modified with olefins such as ethylene and propylene, unsaturated carboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid, their alkyl esters, acrylamide, etc. Polyvinyl alcohol having a degree of polymerization of about 1000 to 10000 and a degree of saponification of about 80 to 100 mol % is generally used.

[0092] A polarizer is obtained by subjecting a polyvinyl alcohol-based film to iodine dyeing and stretching treatment. The thickness of the polarizer is preferably about 1 to 50 μm. A thin polarizer having a thickness of 10 μm or less can also be used as the polarizer. Examples of the thin polarizer include polarizers described in JP-A-51-069644, JP-A-2000-338329, WO2010 / 100917, Japanese Patent No. 4691205, Japanese Patent No. 4751481, etc. Such a thin polarizer can be obtained, for example, by a manufacturing method including a step of stretching a polyvinyl alcohol-based resin layer and a resin substrate for stretching in a laminate state, and a step of dyeing with iodine.

[0093] <Optical layer> No optical layer is provided on the first main surface (the surface on the viewing side) of the polarizer 11, and as described above, the adhesive sheet 21 is provided in contact with the polarizer 11. The polarizing plate 10 may be composed of only the polarizer 11, or an appropriate optical layer 15 may be disposed on the second main surface (the surface on the image display cell 60 side) of the polarizer 11.

[0094] The optical layer 15 may be a transparent protective film for protecting the polarizer 11, or may have a function such as an optical compensation layer for the purpose of widening the viewing angle, or a quarter-wave plate for constituting a circular polarizing plate together with the polarizer 11. The optical layer 15 may have both a function as a transparent protective film and a function as a retardation plate.

[0095] Examples of materials constituting the optical layer 15 include resin materials having excellent transparency, mechanical strength, and thermal stability. Specific examples of such resin materials include cellulose-based resins such as triacetyl cellulose, polyester-based resins, polyethersulfone-based resins, polysulfone-based resins, polycarbonate-based resins, polyamide-based resins, polyimide-based resins, polyolefin-based resins, (meth)acrylic-based resins, cyclic polyolefin-based resins (norbornene-based resins), polyarylate-based resins, polystyrene-based resins, polyvinyl alcohol-based resins, and mixtures thereof. The optical layer 15 may be a liquid crystal material. For example, the optical layer 15 may be a liquid crystal layer in which liquid crystal molecules are aligned in a predetermined direction.

[0096] The optical layer 15 may be in direct contact with the second main surface of the polarizer 11, or may be attached via an appropriate adhesive layer. The optical layer 15 may be a laminate of two or more layers. For example, the optical layer 15 may be a laminate of two or more films, a laminate in which a liquid crystal layer is provided on a film substrate, or a laminate in which two or more liquid crystal layers are laminated. The optical layer 15 may include an alignment film for aligning liquid crystal molecules in a predetermined direction.

[0097] [Polarizing plate with adhesive] The adhesive sheet 21 may be provided as an adhesive-attached polarizing plate 81 integrally laminated with the polarizing plate 10, as shown in Fig. 2. In the adhesive-attached polarizing plate, the adhesive sheet 21 is disposed in contact with a first main surface of the polarizer 11. In Fig. 2, an optical layer 15 is provided on the second main surface of the polarizer 11, but as described above, the polarizing plate 10 does not need to have an optical layer on the second main surface of the polarizer.

[0098] There is no particular limitation on the method for attaching the adhesive sheet 21 onto the first main surface of the polarizer 11. The adhesive sheet 21, which has been prepared in advance on a base material, may be attached onto the polarizer 11, or the adhesive sheet 21 may be formed using the polarizer 11 as a base material.

[0099] In the polarizing plate 81 with adhesive, a release film 41 is preferably removably attached onto the adhesive sheet 21. The release film has a function of protecting the exposed surface of the adhesive sheet 21 until the adhesive sheet 21 is attached to the cover window 70. The base material used in forming (applying) the adhesive sheet may be used as it is as the release film 41 on the adhesive sheet 21.

[0100] 3, the polarizing plate with adhesive may be a double-sided adhesive polarizing plate having an adhesive sheet 21 in contact with the polarizer 11 on the viewing side surface of the polarizing plate 10, and another adhesive sheet 22 on the other side of the polarizing plate. It is preferable that a release film 42 is removably attached on the adhesive sheet 22.

[0101] 3, a polarizing plate 10 has an optical layer 15 on the second main surface of a polarizer 11, and an adhesive sheet 22 is disposed on the optical layer 15. The adhesive sheet 22 may be laminated on the second main surface of the polarizer 11 in contact with the polarizer 11 without any other layer therebetween.

[0102] In this way, by using a double-sided adhesive polarizing plate in which an adhesive layer has already been applied to both sides of the polarizing plate 10, the process of attaching a separate adhesive sheet to the polarizing plate after bonding the polarizing plate to the surface of the image display cell can be omitted, and the manufacturing process of the image display device can be simplified.

[0103] The adhesive sheet 22 is used to bond the polarizing plate 10 and the image display cell 60 together. The thickness of the adhesive sheet 22 is preferably 3 μm to 30 μm, more preferably 5 μm to 27 μm, and even more preferably 10 μm to 25 μm. As the adhesive sheet 22, various adhesives used to bond a polarizing plate and an image display cell can be used. As the adhesive constituting the adhesive sheet 22, an acrylic adhesive is preferably used.

[0104] [Image display device] 1, the image display device 100 includes a cover window 70 attached to the viewing side of a polarizing plate 10 via an adhesive sheet 21. An image display cell 60 such as a liquid crystal cell or an organic EL cell is attached to the other surface of the polarizing plate 10 via an adhesive sheet 22. The image display cell 60 may be foldable.

[0105] A transparent plate having appropriate mechanical strength and thickness is used as the cover window 70. For example, a transparent resin plate such as an acrylic resin or a polycarbonate resin, or a glass plate is used as such a transparent plate. When the image display cell 60 is foldable, the cover window 70 may also be foldable. The cover window may be a laminate of a plurality of transparent films with an adhesive or a bonding agent interposed therebetween, and may include a touch panel sensor. As the touch panel sensor, any type of touch panel such as a resistive film type, a capacitive type, an optical type, or an ultrasonic type is used.

[0106] There is no particular limitation on the order of bonding the polarizing plate 10 and the cover window 70 with the adhesive sheet 21 and bonding the adhesive sheet 22 and the image display cell 60. As described above, an adhesive-attached polarizing plate in which an adhesive sheet is attached in advance to the surface of the polarizing plate may be used.

[0107] After the polarizing plate 10 and the cover window 70 are bonded together via the adhesive sheet 21, degassing may be performed to remove air bubbles at the bonding interface and near the printing step. As a degassing method, a suitable method such as heating, pressurization, or decompression may be used. For example, bonding may be performed under reduced pressure and heating while suppressing the inclusion of air bubbles, and then heating and pressurization may be performed simultaneously by autoclaving or the like in order to suppress delay bubbles, etc.

[0108] When the adhesive sheet 21 is made of a photocurable adhesive composition, the adhesive composition is photocured after bonding the polarizing plate 10 and the cover window 70. The light irradiation causes a polymerization reaction of the photopolymerizable multifunctional compound, which increases the adhesion reliability of the adhesive sheet.

[0109] The amount of light irradiated during photocuring is not particularly limited as long as the adhesive sheet can be photocured, and for example, the cumulative light amount is 50 to 10,000 mJ / cm 2 The adhesive sheet 21 may be irradiated with light from either the polarizing plate 10 side or the cover window 60 side, but from the viewpoint of preventing deterioration of the polarizer 11 due to ultraviolet rays, it is preferable to irradiate the ultraviolet rays from the cover window 10 side. If the adhesive sheet 21 has ultraviolet shielding properties, even when ultraviolet rays are irradiated to photo-cure the adhesive sheet 21, most of the ultraviolet rays are absorbed by the adhesive sheet 21, so that the amount of ultraviolet rays irradiated to the polarizer can be reduced.

[0110] In the image display device 100, the adhesive sheet 21 arranged in contact with the viewing side of the polarizer 11 has the composition as described above. Therefore, even when the image display device is exposed to a high-temperature and high-humidity environment or exposed to external light for a long period of time, deterioration such as fading and yellowing of the polarizer is suppressed, and the adhesive reliability between the polarizing plate 10 and the cover window 70 is excellent. EXAMPLES

[0111] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0112] [Preparation of adhesive sheets 1 to 14] <Polymerization of base polymer> In a reaction vessel equipped with a thermometer, a stirrer, a cooler, and a nitrogen gas inlet tube, the monomer components (total 100 parts by weight) in the ratio shown in Table 1 and azobisisobutyronitrile (AIBN) as a thermal polymerization initiator were charged together with 233 parts by weight of ethyl acetate, and the mixture was stirred for 1 hour in a nitrogen atmosphere at 23°C, followed by nitrogen substitution. The mixture was then reacted at 56°C for 5 hours, and then at 70°C for 3 hours to prepare an acrylic-based polymer solution.

[0113] In Table 1, the monomers are described by the following abbreviations. BA: Butyl acrylate CHA: Cyclohexyl acrylate IBXA: Isobornyl acrylate DCPA: dicyclopentenyl acrylate 4HBA: 4-hydroxybutyl acrylate NVP: N-vinyl-2-pyrrolidone AM: Acrylamide HEAA: Hydroxyethylacrylamide

[0114] <Preparation of Photocurable Pressure-Sensitive Adhesive Composition> The following post-added components were added to the acrylic base polymer solution obtained above in the amounts shown in Table 1 per 100 parts by weight of the base polymer, and then mixed uniformly to prepare a photocurable pressure-sensitive adhesive composition. Isocyanate-based crosslinking agent: Trimethylolpropane adduct of xylylene diisocyanate ("Takenate D110N" manufactured by Mitsui Chemicals) Multifunctional acrylate: Dipentaerythritol hexaacrylate (DPHA) Silane coupling agent: 3-glycidoxypropyltrimethoxysilane ("KBM-403" manufactured by Shin-Etsu Chemical Co., Ltd.) Antioxidant: Pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (BASF "Irganox 1010" Photoinitiator: 2,2-dimethoxy-2-phenylacetophenone ("Omnirad 651" manufactured by IGM Resins): 0.2 parts by weight; and UV absorber: 5,5'-bis(2-ethylhexyloxy)-2,2'-[6-(4-methoxyphenyl)-1,3,5-triazine-2,4-diyl]diphenol (BASF "Tinosorb S")

[0115] <Preparation of adhesive sheet> The above photocurable adhesive composition was applied onto a release film (a polyethylene terephthalate film with a silicone-based release layer on one side), heated at 100°C for 3 minutes to remove the solvent, and then another release film was attached to the surface. This laminate was aged in an atmosphere of 25°C for 3 days to promote crosslinking, and an adhesive sheet with release films temporarily attached to both sides was obtained.

[0116] [Adhesive sheet A] In a reaction vessel equipped with a thermometer, a stirrer, a cooler, and a nitrogen gas inlet tube, 99 parts by weight of butyl acrylate and 1 part by weight of 4-hydroxybutyl acrylate as monomer components, and 0.2 parts by weight of AIBN as a thermal polymerization initiator were added together with 233 parts by weight of ethyl acetate, and the mixture was stirred for 1 hour under a nitrogen atmosphere at 23°C to perform nitrogen substitution. After that, the mixture was reacted for 5 hours at 60°C to obtain a solution of an acrylic base polymer having a weight average molecular weight (Mw) of 1.1 million. To this base polymer solution, 0.8 parts by weight of trimethylolpropane tolylene diisocyanate ("Coronate L" manufactured by Nippon Polyurethane Industry Co., Ltd.) as an isocyanate crosslinking agent and 0.1 parts by weight of a silane coupling agent ("KBM403" manufactured by Shin-Etsu Chemical Co., Ltd.) were added, and the mixture was mixed uniformly to prepare a pressure-sensitive adhesive composition solution.

[0117] The above pressure-sensitive adhesive composition was applied onto a release film so that the thickness after drying would be 20 μm, and after drying for 3 minutes at 100° C. to remove the solvent, another release film was attached to the surface. This laminate was aged in an atmosphere at 50° C. for 2 days to promote crosslinking, and a pressure-sensitive adhesive sheet A with release films temporarily attached to both sides was obtained.

[0118] [Evaluation of Adhesive Sheets 1-14] <UV transmittance> One release film was peeled off from the surface of the pressure-sensitive adhesive sheet, and the sheet was attached to a non-alkali glass plate, after which the other release film was peeled off to prepare a measurement sample. The transmittance spectrum was measured using a visible-ultraviolet spectrophotometer, and the transmittance at a wavelength of 380 nm was read.

[0119] <Adhesion reliability> A polarizer made of a stretched polyvinyl alcohol film with a thickness of 25 μm impregnated with iodine was attached to a non-alkali glass plate via adhesive sheets 1 to 14. Aluminum foil was then attached onto the polarizer via adhesive sheet A, and a metal halide lamp (300 mW / cm 2 ) with an accumulated light output of 3000mJ / cm 2 The adhesive was cured by irradiation with ultraviolet light of 1000 nm to prepare a sample for evaluation.

[0120] The evaluation sample was placed in a thermo-hygrostat at 85°C and 85% relative humidity for 100 hours to carry out a humidity and moisture resistance test. After the test, a 10cm x 10cm area of ​​the sample was observed with a digital microscope at 20x magnification to check for the presence of bubbles. Samples with no bubbles of 20μm or more in diameter were rated as OK, and samples with one or more bubbles of 20μm or more in diameter were rated as NG.

[0121] <Fading and weather resistance> A polarizer made of a stretched polyvinyl alcohol film with a thickness of 25 μm impregnated with iodine was attached to a first non-alkali glass plate via an adhesive sheet A. A second non-alkali glass plate was then attached thereon via adhesive sheets 1 to X, and a metal halide lamp (300 mW / cm 2 ) with an accumulated light output of 3000mJ / cm 2 The adhesive was cured by irradiation with ultraviolet light of 1000 nm to prepare a sample for evaluation.

[0122] (Moisture and heat resistance) The evaluation sample was subjected to a humidity and moisture resistance test by keeping it in a thermo-hygrostat at a temperature of 85°C and a relative humidity of 85% for 100 hours. The difference ΔT=T1-T0 between the light transmittance T0 at a wavelength of 550 nm before the test and the light transmittance T1 at a wavelength of 550 nm after the test was calculated.

[0123] (weather resistance) The evaluation sample was attached to a fixture so that no light was incident on the first non-alkali glass plate side, and measured with an ultraviolet fade meter (U48AU, manufactured by Suga Test Instruments) at a temperature of 40°C and a relative humidity of 20% with a radiation intensity (300-700 nm integrated illuminance) of 500±50 W / m 2 The weather fade test was carried out by irradiating the second non-alkali glass plate with carbon arc lamp light for 100 hours under the conditions of * 0 and the b of the transmitted light of the sample after the test * Difference from 1 Δb * =b * 1-b * 0 was obtained. Note that b * is the chromaticity index b of the CIE1976 color space * The measurement was performed by placing a sample on a backlight.

[0124] The adhesive composition of each adhesive sheet and the evaluation results are shown in Table 1.

[0125] [Table 1]

[0126] In the example using composition 3 that does not contain an ultraviolet absorber, Δb * The increase in the temperature was large, and the polarizer yellowed. Comparing Composition 2 and Composition 3 shows that the inclusion of an ultraviolet absorber in the pressure-sensitive adhesive sheet improves weather resistance and inhibits yellowing of the polarizer.

[0127] In the sample using composition 7 containing 8 parts by weight of NVP out of 100 parts by weight of the monomer components constituting the base polymer, the change in transmittance ΔT before and after the moist heat resistance test was large, and the moist heat resistance was insufficient. The same was true for composition 8 containing 8 parts by weight of AM and composition 9 containing 8 parts by weight of HEAA. Comparing compositions 2, 6, and 7, there was a tendency for ΔT to be smaller as the amount of NVP was smaller. From these results, it can be seen that by reducing the amount of nitrogen atom-containing monomer in the monomer components constituting the base polymer, the moist heat resistance can be improved and the fading of the polarizer can be suppressed.

[0128] A comparison of compositions 2, 10, 11, and 12, which have different amounts of 4HBA in the monomer components that make up the base polymer, shows a tendency for ΔT to decrease as the amount of 4HBA decreases. These results show that by reducing the amount of hydroxyl group-containing monomer in the monomer components that make up the base polymer, it is possible to improve moist heat resistance and suppress fading of the polarizer.

[0129] The sample using composition 1, in which the amount of CHA in the monomer components constituting the base polymer is 15 parts by weight, had insufficient adhesive reliability compared to the sample using composition 2, in which the amount of CHA is 30 parts by weight. Samples using compositions 13 and 14, in which the proportion of CHA was increased, showed sufficient adhesive reliability. Furthermore, Example 4, in which IBXA was used instead of CHA, and Example 5, in which DCPA was used, also showed sufficient adhesive reliability. From these results, it can be seen that by increasing the proportion of high Tg monomers in the constituent monomer components of the base polymer, the pressure-sensitive adhesive sheet shows excellent adhesive reliability even when the proportion of nitrogen atom-containing monomers or hydroxyl group-containing monomers is small. [Explanation of symbols]

[0130] 10 Polarizing plate 11 Polarizer 15 Optical layer 21,22 Adhesive sheet 81,82 Adhesive polarizing plate 60 Image display cells 70 Cover Window 100 Image display device

Claims

1. A polarizing plate with a pressure-sensitive adhesive comprising: a polarizer made of a polyvinyl alcohol-based film containing iodine, the polarizer having a first main surface and a second main surface; and a first pressure-sensitive adhesive sheet disposed in contact with the first main surface of the polarizer, the first pressure-sensitive adhesive sheet is made of a pressure-sensitive adhesive composition containing an acrylic base polymer and an ultraviolet absorber, The acrylic base polymer is, relative to 100 parts by weight of the total of the monomer components, the amount of nitrogen-containing monomer is 5 parts by weight or less; Contains 20 to 75 parts by weight of a high Tg monomer which does not contain any of a hydroxy group, a carboxy group, and a nitrogen atom and has a glass transition temperature of 10°C or higher as a homopolymer. Polarizing plate with adhesive.

2. An adhesive polarizing plate as described in claim 1, wherein the first adhesive sheet has a light transmittance of 5% or less at a wavelength of 380 nm.

3. 3. The polarizing plate with a pressure-sensitive adhesive according to claim 1, wherein the acrylic base polymer contains 0.1 to 8 parts by weight of a hydroxyl group-containing monomer relative to 100 parts by weight of the total of monomer components.

4. 4. The polarizing plate with a pressure-sensitive adhesive according to claim 1, wherein the acrylic base polymer contains 1 part by weight or less of a carboxyl group-containing monomer per 100 parts by weight of the total of monomer components.

5. 5. The polarizing plate with adhesive according to claim 1, wherein the high Tg monomer is a (meth)acrylic acid ester having an alicyclic structure.

6. The acrylic base polymer contains 20 to 79 parts by weight of a (meth)acrylic acid alkyl ester having a homopolymer glass transition temperature of −40° C. or lower per 100 parts by weight of the total of the monomer components. The polarizing plate with adhesive according to any one of claims 1 to 5.

7. 7. The polarizing plate with adhesive according to claim 1, wherein the acrylic base polymer has a crosslinked structure formed by a thermal crosslinking agent.

8. The pressure-sensitive adhesive polarizing plate according to any one of claims 1 to 7, wherein the pressure-sensitive adhesive composition comprises a photopolymerizable polyfunctional compound having two or more photopolymerizable functional groups in one molecule, and a photopolymerization initiator.

9. The polarizing plate with adhesive according to any one of claims 1 to 8, further comprising a second adhesive sheet on a second main surface side of the polarizer.

10. The polarizing plate with adhesive according to claim 9 , wherein the second adhesive sheet is laminated in contact with a second main surface of the polarizer.

11. The polarizing plate with adhesive according to claim 9 , wherein the second adhesive sheet is laminated on a second main surface of the polarizer via another layer.

12. An image display device comprising a second adhesive sheet, a polarizer made of a polyvinyl alcohol-based film containing iodine, a first adhesive sheet, and a cover window, in this order, on a surface of an image display cell, the first pressure-sensitive adhesive sheet is made of a pressure-sensitive adhesive composition containing an acrylic base polymer and an ultraviolet absorber, The acrylic base polymer is, relative to 100 parts by weight of the total of the monomer components, the amount of nitrogen-containing monomer is 5 parts by weight or less; containing 20 to 75 parts by weight of a high Tg monomer which does not contain any of a hydroxy group, a carboxy group, and a nitrogen atom and has a glass transition temperature of 10° C. or higher as a homopolymer; The image display device, wherein the first adhesive sheet is disposed in contact with the polarizer.

13. A method for manufacturing an image display device, comprising the steps of: the image display device includes a second adhesive sheet, a polarizer made of a polyvinyl alcohol-based film containing iodine, a first adhesive sheet in contact with the polarizer, and a cover window, which are arranged in this order on a surface of an image display cell; the first pressure-sensitive adhesive sheet is made of a pressure-sensitive adhesive composition including an acrylic base polymer, a photopolymerizable multifunctional compound having two or more photopolymerizable functional groups in one molecule, a photopolymerization initiator, and an ultraviolet absorber; The acrylic base polymer is, relative to 100 parts by weight of the total of the monomer components, the amount of nitrogen-containing monomer is 5 parts by weight or less; containing 20 to 75 parts by weight of a high Tg monomer which does not contain any of a hydroxy group, a carboxy group, and a nitrogen atom and has a glass transition temperature of 10° C. or higher as a homopolymer; the polarizer and the cover window are bonded to each other via the first pressure-sensitive adhesive sheet, and then actinic rays are irradiated from the cover window side to photocure the pressure-sensitive adhesive composition. A method for manufacturing an image display device.

Citation Information

Patent Citations

  • Pressure-sensitive adhesive composition, pressure-sensitive adhesive layer, method for producing the layer, and optical member with pressure-sensitive adhesive

    JP2007138147A

  • Adhesive sheet

    JP2013075978A

  • Ultraviolet-curable acrylic adhesive composition, ultraviolet-curable acrylic adhesive layer, polarization film with adhesive layer, method for producing ultraviolet-curable acrylic adhesive layer and image display device

    JP2016155981A

  • Optical film with adhesive layer and liquid crystal display

    JP2016194694A

  • Polarization film with adhesive layers on both sides, and image display unit

    JP2016224307A