Metal recovery from lead-containing electrolytes

The use of an electropolishing reactor with a high surface area cathode and controlled current density enables selective recovery of copper and silver from lead electrolytes, enhancing lead purity to 99.9999% and facilitating continuous production.

JP7565338B2Active Publication Date: 2024-10-10AQUA METALS INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022506755
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-01
Filing Date
2020-07-28
Publication Date
2024-10-10
Estimated Expiration
2040-07-28

AI Technical Summary

Technical Problem

Existing methods for recovering lead from electrolytes, particularly from lead acid batteries, face challenges in achieving high purity due to the presence of copper and silver, which co-deposit with lead, and are environmentally harmful, with low concentrations of these metals complicating selective recovery.

Method used

A method involving an electropolishing reactor with a high surface area cathode and controlled current density to preferentially deposit copper and silver on the cathode, followed by electrochemical production of high-purity metallic lead.

Benefits of technology

This approach achieves lead purity of at least 99.9999% by selectively removing copper and silver, allowing for continuous production and recovery of valuable metals from lead-enriched electrolytes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000009_0000
    Figure 00000009_0000
  • Figure 00000009_0001
    Figure 00000009_0001
  • Figure 00000009_0002
    Figure 00000009_0002
Patent Text Reader

Abstract

Valuable metals, particularly copper and silver, are recovered from lead-bearing electrolyte in a process in which the electrolyte is fed to an electropolishing reactor having a high surface area cathode where the electrode potential is controlled, thus preferentially reducing the copper and silver and forming a pre-treated lead-enriched electrolyte that can subsequently undergo electrochemical lead recovery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority to co-pending U.S. Provisional Application No. 62 / 881,743, filed Aug. 1, 2019, which is incorporated herein by reference.

[0002] FIELD OF THEINVENTION The present disclosure relates to compositions, methods, and apparatus for recovering various metals from electrolytes, particularly as it relates to the removal and / or recovery of copper and silver from lead ion-containing electrolytes. [Background technology]

[0003] 2. Background of the Invention The background discussion includes information that may be useful in understanding the present disclosure. This is not an admission that any of the information provided herein is prior art or relevant to the claimed invention, or that any publication specifically or implicitly referenced is prior art.

[0004] All publications and patent applications herein are incorporated by reference to the same extent as if each individual publication or patent application was specifically and individually indicated to be incorporated by reference. In the event that a definition or use of a term in an incorporated reference is inconsistent with or contrary to the definition of that term provided herein, the definition of that term provided herein applies and the definition of that term in the reference does not apply.

[0005] Various efforts have been made to move away from smelting operations and to use more environmentally friendly solutions in the recovery and refining of lead from lead-acid batteries. For example, U.S. Patent No. 4,927,510 (to Olper and Fracchia) teaches the recovery of substantially all of the lead in pure metallic form from battery sludge after a desulfurization process. Unfortunately, such methods require the use of environmentally problematic fluorine-containing electrolytes. To overcome some of the difficulties associated with fluorine-containing electrolytes, desulfurized lead active material was dissolved in methanesulfonic acid, as described in U.S. Patent No. 5,262,020 (to Masanté and Serracane) and U.S. Patent No. 5,520,794 (to Gernon). However, because lead sulfate is fairly insoluble in methanesulfonic acid, upstream desulfurization is necessary, and residual insoluble material typically reduces the overall yield to an economically unattractive process. To improve at least some of the aspects related to lead sulfate, oxygen and / or ferric methanesulfonate can be added as described in International Patent Application Publication No. 2014 / 076544 (to Fassbender et al.), or mixed oxides can be produced as taught in International Patent Application Publication No. 2014 / 076547 (to Fassbender et al.). However, despite the improved yields, some drawbacks still remain. Notably, recycling of the solvent in these processes often requires additional effort, and residual sulfate is still lost as waste. Furthermore, during process upsets or power outages (not uncommon in electrolytic lead recovery), in conventional electrolytic recovery operations, unless the cathode is removed and the lead stripped, the plated metallic lead will dissolve back into the electrolyte, making batch operations problematic at best.

[0006] Most of the above problems are overcome in an integrated process of desulfurizing the lead paste and reducing the lead dioxide before or after desulfurization to produce lead ion species soluble in alkanesulfonic acid electrolytes, as described in WO 2016081030 and WO 2016183428. Advantageously, such a process allows for the continuous production of relatively high purity lead on a moving cathode. However, metals more noble than lead (e.g., copper, silver) are typically present in the electrolytes of such processes, and co-plating of these metals limits the purity that can be achieved with such processes. Unfortunately, selective recovery of metals more noble than lead is often problematic, as these metals are usually present in very low concentrations compared to lead. For example, typically, a lead electrolyte may have a lead ion concentration of 20-200 g / l, while silver and copper ions are present at about 5 mg / l and 8 mg / l, respectively.

[0007] Thus, while systems and methods for recovering lead from electrolytes are known, small amounts of more noble metals such as silver and / or copper may reduce the purity of the electrochemically produced metallic lead. Thus, a need remains for improved systems for increasing lead purity and / or recovering low concentrations of valuable metals from process electrolytes. Summary of the Invention

[0008] The inventors have discovered various devices, systems, and methods that allow for the removal and / or recovery of valuable metals, particularly copper and silver, from electrolytes that contain significant amounts of lead ions.

[0009] In one aspect of the inventive subject matter, the inventors contemplate a method of treating a lead-enriched electrolyte, comprising feeding the lead-enriched electrolyte to an electropolishing reactor having an anode and a high surface area cathode. In the contemplated method, the lead-enriched electrolyte contains at least one other metal ion (e.g., copper and / or silver) that has an electrode potential higher than that of lead. In another step, a low current is applied to the high surface area cathode to reduce the other metal ion on the high surface area cathode, thus producing a pretreated lead-enriched electrolyte.

[0010] Most typically, the lead ions in the pretreated lead-enriched electrolyte may then be reduced in an electrochemical production reactor to produce metallic lead. In some embodiments, the lead-enriched electrolyte has a lead ion concentration of at least 20 g / L, or at least 50 g / L, or at least 100 g / L, while the lead-enriched electrolyte has a metal ion concentration of copper and / or silver of less than 10 mg / L.

[0011] With respect to the electrodes, it is contemplated that the high surface area cathode comprises carbon felt, expanded vitreous carbon, carbon cloth, expanded graphite, carbon nanotubes, or graphene. Preferably, the high surface area cathode is configured as a flow-through cathode. Most typically, the anode comprises titanium or other suitable material. Most typically, the anode comprises a 100 cm 2 For a cell, low current is a current of less than 400 mA, or less than 300 mA, or less than 200 mA, but in a preferred embodiment, low current is less than 4 mA / cm 2 or less than 3mA / cm 2 or less than 2mA / cm 2 This produces a current density of: From a different perspective, control of the electrode potential is used to preferentially reduce selected more noble metal ions in the presence of relatively high concentrations of less noble metals.

[0012] In further aspects, the concentration of at least one other metal ion in the pretreated lead-enriched electrolyte is 10 ppb or less, or 5 ppb or less, or 1 ppb or less. Additionally, it is contemplated that the step of feeding the lead-enriched electrolyte to the electropolishing reactor may be performed simultaneously with the step of reducing lead ions in the pretreated lead-enriched electrolyte in the electrochemical production reactor, thus continuously producing metallic lead. Most typically, the electrochemically produced lead from the pretreated lead-enriched electrolyte has a purity of at least 99.99%, or at least 99.999%, or at least 99.9999%, or at least 99.99999%.

[0013] Various objects, features, aspects and advantages will become more apparent from the following detailed description of preferred embodiments, taken in conjunction with the accompanying drawings, in which like reference numerals represent like elements and in which: [Brief description of the drawings]

[0014] [Figure 1] 1 shows a schematic of the half-cell potentials of selected ions for reactions occurring at the cathode. [Diagram 2] 1 illustrates generally an exemplary lab-scale configuration of an electrolytic cell in accordance with the inventive subject matter. [Diagram 3] 1 is a photograph of an exemplary lab-scale configuration of an electrolytic cell in accordance with the subject invention. [Figure 4] 1 is a graph showing exemplary results of Ag / Cu concentration versus current in an electrolytic cell in accordance with the subject invention. [Diagram 5] 1 is a graph showing exemplary results of Ag / Cu recovery using an electrolytic cell in accordance with the subject matter. [Figure 6] Various calculations related to the methods presented herein are provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Detailed Description The inventors have now discovered that lead ion-containing electrolytes can be pretreated to reduce the metal ion content of metals more noble than lead (i.e., metals having a more positive electrode potential in a given electrolyte) in a given electrolyte. Such pretreated electrolytes would thus be capable of electrochemical production of metallic lead of very high purity. Furthermore, removal of metals more noble than lead would also enable recovery of values, particularly copper and silver. Figure 1 illustratively shows the half-cell potentials of selected ions for their reactions occurring at the cathode.

[0016] For example, in one preferred embodiment of the inventive subject matter, the lead-enriched electrolyte comprises an alkane sulfonic acid (preferably methane sulfonic acid) and lead ions are present in the electrolyte at a concentration of about 20-200 g / L. Most typically, the lead-enriched electrolyte will further comprise copper ions at a concentration of about 5-10 mg / L, and silver ions at a concentration of about 3-8 mg / L. The lead-enriched electrolyte is then fed to an electropolishing reactor containing an anode and a high surface area cathode configured as a flow-through electrode, where the copper and silver are electrolytically polished at a low current density (e.g., 5 mA / cm 2 The copper and silver are plated onto the high surface area cathode using low currents (e.g., less than 500 mA) of less than 1000 mA. Of course, it should be understood that the copper and silver may be plated separately or together, as described in more detail below.

[0017] With respect to a suitable electropolishing reactor, it is contemplated that the reactor will typically be configured to allow for continuous processing of the lead-enriched electrolyte. Thus, a suitable electropolishing reactor may be configured as a single flow-through reactor, or a flow-through reactor including a surge tank from which the lead-enriched electrolyte is recirculated. In a less preferred embodiment, the electropolishing reactor may also be configured to operate in batch mode to pretreat the lead-enriched electrolyte. Regardless of the particular configuration, typically the cathode of the electropolishing reactor will have a high surface area (e.g., 0.2-0.8 m 2Preferably, the high surface area cathode comprises a cathode having a surface area of ​​at least 0.1 m / g. In most cases, such high surface area cathodes will comprise (active) carbon felt, graphite felt, expanded vitreous carbon, expanded graphite, carbon nanotubes, and / or graphene, and will have a porosity that allows for the flow of lead-rich electrolyte through the cathode (most typically across the thickness of the cathode). Thus, contemplated high surface area cathodes will have a surface area of ​​at least 0.1 m. 2 / g, or at least 1.0m 2 / g, or at least 10m 2 / g, or at least 50m 2 / g, or at least 100m 2 / g, or at least 200m 2 / g, at least 500m 2 / g, at least 1,000m 2 / g, or even higher. For example, suitable high surface area cathodes will have a minimum length through-path (measured between electrolyte inflow and exit) of at least 1 mm, or at least 2 mm, or at least 3 mm, or at least 5 mm, or at least 10 mm, or at least 25 mm, or at least 50 mm, or even greater. It is generally more preferred that the high surface area cathode has a height and / or width at least 10 times, or at least 20 times, or at least 40 times, or at least 100 times the thickness of the high surface area cathode. Thus, viewed from a different perspective, contemplated high surface area cathodes will generally be configured as thick sheets, with electrolyte flow across the thickness of the high surface area cathode.

[0018] As will be readily understood, the carbon felt or other high surface area material may be bonded to a conductive carrier such as stainless steel mesh. Figure 2 shows an exemplary schematic diagram of an electropolishing reactor having two end plates with an inlet and an outlet disposed therebetween, a vent, and a stainless steel mesh to which the graphite felt is conductively attached. The outlet plate may further include an iridium-coated titanium mesh anode. Figure 3 is a photograph of a pilot cell according to Figure 2, which was used in the experiments described in more detail further below.

[0019] Most typically, the polishing reactor will be configured so that at least 60%, or at least 70%, or at least 80%, or at least 90%, or at least 95%, or at least 98% of the copper and / or silver in the lead-enriched electrolyte is deposited on the flow-through cathode at a flow rate that allows continuous lead recovery at the cathode downstream of the lead reduction reactor. Thus, the polishing reactor may have multiple electrolytic cells (typically operating in parallel). However, in other embodiments, one or more polishing reactors may also be operated in batch mode to accommodate flow rates different from those required to feed the lead reduction reactor(s).

[0020] During operation, more noble metals such as copper and silver will deposit on and into the high surface area cathode, especially when relatively low currents are used with correspondingly low current densities. Thus, depending on the particular operating conditions, the metals may be (preferentially) deposited by controlling the current or may codeposit, and the particular electrode potential with the particular metal and electrolyte system will determine the type of deposition. However, as will be readily understood, the more noble metal will typically codeposit with metallic lead if the lead concentration is significantly higher than the more noble metal. For example, when copper and silver ions are reduced to metallic copper and metallic silver, lead will also codeposit, especially when lead ions are present at concentrations greater than 20 g / L, or greater than 50 g / L, or greater than 100 g / L.

[0021] Of course, it should be understood that the nature of the electrolyte may vary considerably, and all known electrolytes, including those containing alkanesulfonic acid, sulfuric acid, fluoroboric acid, or strong bases (e.g., KOH, NaOH, etc.), are considered suitable for use herein. Additionally, suitable electrolytes may contain a variety of other ionic species, most typically metal ions found in lead acid battery recycling. As a result, it is contemplated that electrolyte pretreatment may be implemented with any electrolytic process that recovers lead from lead acid battery recycling. Lead ions will generally be present in the electrolyte at concentrations of 10-20 g / L, or 20-50 g / L, or 50-100 g / L, or 100-200 g / L, or even higher. On the other hand, the more noble metals will generally be present in individual concentrations of 1 g / L or less, or 500 mg / L or less, or 200 mg / L or less, or 100 mg / L or less, or 50 mg / L or less, or 25 mg / L or less, or 10 mg / L or less.

[0022] With respect to the electropolishing reactor, it is contemplated that the specific dimensions will typically be determined by the volume of electrolyte being processed and / or the type of operation (e.g., single-flow, recirculation, batch processing, etc.). For example, the polishing reactor may be configured to have electrolyte flow rates of about 50-200 mL / min, or about 200-500 mL / min, or about 500-5,000 mL / min, or about 5-50 L / min, and even higher. As a result, the cathode working area may be 50-200 cm 2 , or 200~2,000cm 2 , or 2,000 to 20,000 cm 2 , and even higher. Additionally, it should be noted that the electropolishing reactor may have two or more high surface area cathodes, which may be arranged in series (to provide a first pretreatment electrolyte to a second cathode) or in parallel. The use of multiple cathodes is particularly advantageous when continuous operation requires the removal of one cathode while diverting the electrolyte flow to another cathode.

[0023] Most typically, operation of the electropolishing reactor is a continuous process, or at least to the point where backpressure due to metal accumulation in the cathode reaches a predetermined level (or where the high surface area is reduced to a predetermined extent). Most typically, depending on the particular more noble metal, the current and current density will vary at least to some extent. However, it is generally preferred that the current and current density be as low as practicable so that the more noble metal deposits preferentially and lead formation on the cathode is reduced. Thus, preferred currents are often 500 mA or less, or 400 mA or less, or 350 mA or less, or 300 mA or less, or 250 mA or less, or 200 mA or less, or 150 mA or less, and may even be lower. As a result, current densities for high surface area cathodes are typically less than 5 mA / cm. 2 Below, 4mA / cm 2 Below, 3.5mA / cm 2 Below, 3mA / cm 2 Below, 2.5mA / cm 2 Below, 2mA / cm 2 or even lower (mA / cm 2 (Density at was calculated using the outer dimensions of the high surface material rather than the actual electrode surface). Most typically, the residual amount of non-lead metals in the lead-containing electrolyte may be less than 500 ppb, or less than 300 ppb, or less than 200 ppb, or less than 100 ppb, or less than 50 ppb, or less than 25 ppb, or less than 10 ppb, or even below the detection limit using standard detection methods known in the art. Thus, the electrolyte may be substantially depleted (e.g., less than 100 ppb or less than 25 ppb) of one or more of the non-lead metals in the electrolyte.

[0024] In further contemplated embodiments, one or more of the more noble metals may also be recovered using an ion exchange process. For example, if removal of copper by ion exchange is desired, a copper-selective chelating resin may be used (e.g., DOWEX™ M4195). The use of such a resin is typically upstream of the electropolishing reactor. Similarly, silver ions may be removed using a silver-selective ion exchange resin (e.g., Chelex-100). Such adsorptive methods would typically be implemented online so that the lead-enriched electrolyte can flow continuously into the electropolishing reactor after passing through the resin. On the other hand, an ion exchange resin may also be placed downstream of the polishing reactor to reduce copper and / or silver breakthrough when reduction at the flow-through cathode is terminated or interrupted.

[0025] Regardless of the particular method of non-lead ion removal, it is generally preferred that the metals be recovered as a product of value. Most typically, the product of value can be further refined since lead, due to its overwhelming presence in the lead-rich electrolyte, will be the major component of the metals recovered. Because lead has a very low melting point compared to other metals, it can be removed from the other metals by any thermal method. Alternatively, lead can also be (electro)chemically dissolved from the cathode material into a suitable electrolyte (e.g., sulfuric acid, fluoroboric acid, or methanesulfonic acid).

[0026] In further contemplated aspects, it should be particularly recognized that the processes presented herein are particularly suitable for solvent / electrolyte-based recycling processes of lead materials, particularly lead-acid battery recycling processes. Such recycling processes may have various components, such as upstream desulfurization of the lead paste, treatment of the lead paste (desulfurized or not) to remove or convert lead dioxide, heat treatment of the lead paste, and washing and / or drying steps. Exemplary processes suitable for integration with electrolyte pretreatment include those described in WO 2015 / 077227, WO 2016 / 081030, WO 2016 / 183428, and US 62 / 860,928, all of which are incorporated herein by reference. Thus, the inventors specifically contemplate one or more polishing reactors as presented herein fluidly and upstream coupled to one or more lead reduction reactors, where the polishing reactor(s) and the lead reduction reactor(s) may operate simultaneously such that electrolyte can flow from the polishing reactor(s) to the lead reduction reactor(s).

[0027] Furthermore, while the above description has focused primarily on the removal / recovery of silver and / or copper from lead ion-containing electrolytes, it should be understood that the apparatus and methods presented herein may be more broadly applied to any situation in which the electrolyte contains a more noble (positive potential) metal at a lower (often substantially lower) concentration than that of another less noble metal. In these cases, it should be understood that the combination of controlling the electrode potential and using a high surface cathode (preferably a flow-through cathode) advantageously allows for preferential reduction of the more noble metal at the cathode in the presence of the less noble metal. Thus, from a different perspective, selected non-lead metals (e.g., silver) can be removed and reduced from the lead-containing electrolyte, while other non-lead metals (e.g., copper) remain in the lead-containing electrolyte.

[0028] Working Example The following examples are provided to illustrate aspects of the inventive subject matter and should not be construed as limiting the invention in any way. Unless otherwise noted, the lead-enriched electrolyte was obtained from dissolving desulfurized lead paste in methanesulfonic acid. In most cases, the lead ion concentration was 20-200 mg / L, and contained about 5.2 mg / L silver, and about 8 mg / L copper.

[0029] The electropolishing reactor was configured as a bench-scale flow-through electrolysis apparatus, as exemplarily shown in Figures 2 and 3. The anode material was iridium-coated titanium mesh and the cathode was stainless steel mesh conductively bonded to graphite felt. The graphite felt was a 100 cm2 tube used as a flow-through cathode as shown in Figure 2, with a flow rate of 100 mL / min. 2 The lead-enriched electrolyte was pumped through the cell in a single pass closed system for approximately 6-8 hours / day until back pressure due to metal accumulation at the electrodes limited the flow. The feed and outlet solutions were tested for copper and silver concentrations. Electrolytic recovery of metals was performed at suitable currents using considerations / parameters for reduction of ions to the corresponding metals as shown in Table 1. More specifically, Table 1 shows exemplary electrode potentials for reactions at the cathode and Table 2 shows exemplary electrode potentials for reactions at the anode. Table 3 shows the cell potentials used for exemplary pretreatment reactions. [Table 1] [Table 2] [Table 3]

[0030] As can be seen from the results in Figure 4, silver has a current of 200 mA (and a current of approximately 2.0 mA / cm 2 ) and the copper is selectively plated at a current of about 350 mA (and a current density of about 3.5 mA / cm 21000 ppb) of silver ions and 8000 ppb of copper ions in the presence of about 200 g / L of lead ions. Looking at the time course or recovery, the copper and silver levels were below the detection limit for the first 53 hours of run time using a solution containing about 5200 ppb of silver ions and about 8000 ppb of copper ions in the presence of about 200 g / L of lead ions. As can be seen from FIG. 5, after 55 hours of run time, the copper concentration in the effluent increased significantly, while the silver concentration remained below the feed concentration. When analyzing the metals in the cathode, a co-deposition of lead, copper, and silver was observed, with about 80% of the metal being lead, 12% of the metal being copper, and 8% of the metal being silver. FIG. 6 provides further equations and calculations used herein. Finally, it should be noted that the process herein is suitable for all processes in primary lead production and lead plating, not just lead acid battery recycling.

[0031] The recitation of ranges of values ​​herein is merely intended to serve as a shorthand method of individually referring to each separate value within the range. Unless otherwise indicated herein, each separate value is incorporated into the specification as if it were individually recited herein. All methods described herein may be performed in any suitable order unless otherwise indicated herein or clearly contradicted by context. Any examples provided with respect to specific embodiments herein, or the use of exemplary language (e.g., "etc.") is intended merely to better illuminate the full scope of the disclosure and does not impose limitations on the scope of the invention as otherwise claimed. No language in the specification should be construed as indicating any non-claimed element essential to the practice of the claimed invention.

[0032] It will be apparent to those skilled in the art that many more modifications beyond those already described are possible without departing from the full scope of the concepts disclosed herein. Thus, the disclosed subject matter should not be limited except as by the appended claims. Moreover, in interpreting both the specification and the claims, all terms should be interpreted in the broadest possible manner consistent with the context. In particular, the terms "comprises" and "comprising" should be interpreted as referring to elements, components, or steps in an open-ended manner, indicating that the mentioned element, component, or step may be present or utilized or may be combined with other elements, components, or steps not expressly mentioned. When the specification and claims refer to at least one selected from the group consisting of A, B, C... and N, the sentence should be interpreted as requiring only one element from the group, not A+N or B+N, etc.

Claims

1. 1. A method for treating an electrolyte, comprising the steps of: The electrolyte is applied to an anode and at least 0.1 m 2 / g of surface area of ​​a high surface area cathode; the electrolyte comprises a first metal ion and a second metal ion, the first metal being more noble than the second metal, the first metal ion being present in the electrolyte at a lower concentration than the second metal ion, the concentration of the first metal in the electrolyte is 10 mg / L or less, the concentration of the second metal in the electrolyte is at least 20 g / L, the second metal ion is a lead ion, and the electrolyte comprises an alkane sulfonic acid; controlling an electrode potential of said high surface area cathode to preferentially reduce said first metal ions in the presence of said second metal ions, thus producing a pretreatment electrolyte containing said second metal and substantially depleted of said first metal; A method comprising:

2. The method of claim 1 , wherein the high surface area cathode is configured as a flow-through cathode.

3. The method of any one of claims 1 to 2, wherein the high surface area cathode comprises carbon felt, woven or non-woven carbon cloth, foamed vitreous carbon, expanded graphite, carbon nanotubes, or graphene.

4. The method according to any one of claims 1 to 3, wherein the first metal is silver or copper.

5. The method of any one of claims 1 to 4, further comprising reducing the second metal ions in the pretreatment electrolyte in an electrochemical generation reactor.

6. 3. The method of claim 1 or claim 2, wherein the high surface area cathode comprises carbon felt, woven or non-woven carbon cloth, foamed vitreous carbon, expanded graphite, carbon nanotubes, or graphene.

7. The method of claim 1 , wherein the first metal is silver or copper and the second metal is lead.

8. 10. The method of claim 1 further comprising reducing the second metal ions in the pretreatment electrolyte in an electrochemical generation reactor.

9. 1. A method for treating a lead-rich electrolyte comprising the steps of: providing the lead-enriched electrolyte to an electropolishing reactor having an anode and a high surface area cathode configured as a flow-through cathode, the high surface area cathode having an area of ​​at least 0.1 m 2 providing a crystalline silica having a surface area of ​​1 / g; the lead-enriched electrolyte comprises an alkane sulfonic acid and at least one other metal ion having an electrode potential higher than that of lead, the lead-enriched electrolyte having a lead ion concentration of at least 20 g / L, the lead-enriched electrolyte having the other metal ion at a concentration of less than 10 mg / L; applying a low current of 500 mA or less to said high surface area cathode or controlling its electrode potential to preferentially reduce said other metal ions on said high surface area cathode, thus producing a pretreated lead-enriched electrolyte and a cathode plated with said other metal; A method comprising:

10. 10. The method of claim 9, further comprising reducing lead ions in the pretreated lead-enriched electrolyte in an electrochemical production reactor to produce metallic lead.

11. 10. The method of claim 9, wherein the lead-enriched electrolyte has a lead ion concentration of at least 50 g / L, and the lead-enriched electrolyte has the other metal ions at a concentration of less than 10 mg / L.

12. 10. The method of claim 9, wherein the lead-enriched electrolyte has a lead ion concentration of at least 100 g / L, and the lead-enriched electrolyte has the other metal ions at a concentration of less than 10 mg / L.

13. 10. The method of claim 9, wherein the high surface area cathode comprises carbon felt, woven or non-woven carbon cloth, expanded vitreous carbon, expanded graphite, carbon nanotubes, or graphene.

14. The anode is made of RuO 2 or IrO 2 The method of claim 9, comprising coating titanium with

15. The method of claim 9 , wherein the at least one other metal ion is a copper ion or a silver ion.

16. The low current is 4mA / cm 2 10. The method of claim 9, producing a current density of:

17. The low current is 3 mA / cm 2 10. The method of claim 9, producing a current density of:

18. The low current is 2 mA / cm 2 10. The method of claim 9, producing a current density of:

19. 10. The method of claim 9, wherein the concentration of the at least one other metal ion in the pretreated lead-enriched electrolyte is less than or equal to 10 ppb.

20. 10. The method of claim 9, wherein the concentration of the at least one other metal ion in the pretreated lead-enriched electrolyte is less than or equal to 5 ppb.

21. 10. The method of claim 9, wherein the step of supplying the lead-enriched electrolyte to the electropolishing reactor occurs simultaneously with the step of reducing lead ions in the pretreated lead-enriched electrolyte in an electrochemical production reactor to produce metallic lead.

22. 22. The method of claim 21, wherein the electrochemically produced lead from the pretreated lead-enriched electrolyte has a purity of at least 99.99%.

Citation Information

Patent Citations

  • Process and device of recovering electroplating gold-containing wastewater

    CN109055983A

  • Electrolytic extraction of metals

    GB2368349A

  • Ribaashibururyomenamiji no henseihoho

    JP1976026364A

  • Kihakudenkaishitsuyoekino denkaikangenho

    JP1976067267A

  • Electrochemical recovering method of copper

    JP1977053719A