Anode active material for aqueous secondary battery, cathode for aqueous secondary battery and aqueous secondary battery

Graphite with C-F bonding groups and controlled surface area enhances the discharge current density in water-based secondary batteries by suppressing electrolyte decomposition and optimizing lithium release, addressing the inefficiencies in conventional water-based batteries.

JP7565501B2Active Publication Date: 2024-10-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021574491
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-30
Filing Date
2020-12-01
Publication Date
2024-10-11
Estimated Expiration
2040-12-01

AI Technical Summary

Technical Problem

Conventional water-based secondary batteries suffer from low charge/discharge efficiency and low current density due to the reductive decomposition of the aqueous electrolyte on the carbon material used as the negative electrode active material, leading to insufficient rapid charging and discharging characteristics.

Method used

The use of graphite with C-F bonding groups on its surface and a specific BET surface area range, optimized to suppress the reductive decomposition of the aqueous electrolyte, thereby enhancing the discharge current density by forming a dense film and controlling irreversible lithium release sites.

Benefits of technology

This approach improves the discharge current density by inhibiting the reductive decomposition of the aqueous electrolyte and promoting efficient charge/discharge reactions, while maintaining safety with a non-flammable electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565501000003
    Figure 0007565501000003
  • Figure 0007565501000001
    Figure 0007565501000001
  • Figure 0007565501000002
    Figure 0007565501000002
Patent Text Reader

Abstract

A negative electrode active material for aqueous secondary batteries, said negative electrode active material being applied to an aqueous secondary battery that uses an aqueous electrolyte solution containing water and a lithium salt, wherein: the negative electrode active material contains graphite; the graphite has a C-F bond group on the surface; if I688eV is the peak intensity at around 688 eV ascribed to a C-F bond and I284eV is the peak intensity at around 284 eV ascribed to a C-C bond in the XPS spectrum of the graphite as obtained by X-ray photoelectron spectroscopy, the ratio of the peak intensity I688eV to the peak intensity I284eV (namely, the value of I688eV / I284eV) is from 0.1 to 7; and the BET specific surface area is from 0.5 m2 / g to 3.9 m2 / g.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a negative electrode active material for an aqueous secondary battery, a negative electrode for an aqueous secondary battery, and an aqueous secondary battery. [Background technology]

[0002] As a secondary battery with high output and high energy density, a lithium ion secondary battery is widely used, which includes a positive electrode, a negative electrode, and an electrolyte, and charges and discharges by transferring lithium ions between the positive electrode and the negative electrode. Conventional secondary batteries use an organic solvent-based electrolyte to achieve a high energy density.

[0003] However, organic solvents are generally flammable, making safety an important issue, and the ionic conductivity of organic solvents is lower than that of aqueous solutions, making rapid charge / discharge characteristics insufficient.

[0004] In view of such problems, secondary batteries using an electrolyte solution containing water (hereinafter, sometimes referred to as an aqueous electrolyte solution) have been studied. For example, Patent Documents 1 and 2 propose the use of an aqueous solution containing a high concentration of alkaline salt as the aqueous electrolyte solution of a secondary battery, and Patent Document 3 proposes the use of an aqueous electrolyte solution in which an organic carbonate is added to an aqueous solution containing a high concentration of alkaline salt. Patent Document 4 proposes a secondary battery having a negative electrode, a positive electrode, and an aqueous electrolyte solution, and the negative electrode has a composite of a negative electrode active material and polytetrafluoroethylene. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6423453 [Patent Document 2] International Publication No. 2017 / 122597 [Patent Document 3] JP 2018-73819 A [Patent Document 4] JP 2019-57359 A Summary of the Invention

[0006] Conventional aqueous secondary batteries have problems such as low charge / discharge efficiency and only very low current density due to Li+ release.

[0007] One aspect of the present disclosure is a negative electrode active material that is applied to an aqueous secondary battery that uses an aqueous electrolyte solution containing water and a lithium salt, the negative electrode active material including graphite, the graphite having a C—F bond group on a surface thereof, and the graphite having a peak intensity of I at about 688 eV derived from a C—F bond in an XPS spectrum obtained by X-ray photoelectron spectroscopy measurement. 688eV The peak intensity at around 284 eV due to the C-C bond is I 284eV When the peak intensity I 284eV The peak intensity I 688eV The ratio (I 688eV / I 284eV value) is 0.1 to 7, and the BET specific surface area is 0.5m 2 / g or more 3.9m 2 / g or less.

[0008] Another aspect of the present disclosure is a negative electrode for an aqueous secondary battery, comprising the above-mentioned negative electrode active material for an aqueous secondary battery.

[0009] Another aspect of the present disclosure is an aqueous secondary battery having the above-mentioned aqueous secondary battery negative electrode, a positive electrode, and an aqueous electrolyte solution containing water and a lithium salt.

[0010] According to the present disclosure, it is possible to improve the current density (discharge current density) resulting from the release of Li+ from a water-based secondary battery. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a water-based secondary battery according to this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] In general, in an aqueous secondary battery using an aqueous electrolyte solution containing water and a lithium salt, when a carbon material is used as the negative electrode active material, the aqueous electrolyte solution is actively reductively decomposed on the carbon material, and the progress of the charging reaction of the negative electrode active material is inhibited. However, as a result of intensive research, the present inventors have found that by using graphite having a C-F bond group formed on its surface as the negative electrode active material, and optimizing the absolute amount of the C-F bond group on the graphite surface and the BET specific surface area of ​​the graphite, the reductive decomposition of the aqueous electrolyte solution can be suppressed to advance the charging and discharging reaction of the negative electrode active material, thereby improving the current density (discharge current density) caused by the release of Li+ from the aqueous secondary battery. Hereinafter, one embodiment of the present disclosure will be described.

[0013] The negative electrode active material for an aqueous secondary battery according to one embodiment of the present disclosure includes graphite, the graphite having a C—F bond group on its surface, and the graphite has a peak intensity of I at about 688 eV derived from a C—F bond in an XPS spectrum obtained by X-ray photoelectron spectroscopy. 688eV The peak intensity at around 284 eV due to the C-C bond is I 284eV When the peak intensity I 284eV The peak intensity I 688eV The ratio (I 688eV / I 284eV value) is 0.1 to 7, and the BET specific surface area is 0.5m 2 / g or more 3.9m 2 / g or less. By using the negative electrode active material for aqueous secondary batteries according to one embodiment of the present disclosure, the current density (discharge current density) resulting from the release of Li+ from the secondary battery can be improved. The mechanism by which this effect is achieved is not fully clear, but the following is presumed.

[0014] The C-F bond group on the graphite surface is a surface modification group in which fluorine is bonded to a functional group present on the graphite or on the graphite surface, and is formed by subjecting the graphite to a fluorine treatment described later. The formation of the C-F bond group on the graphite surface can suppress the electrochemical reduction catalytic activity at the defective sites (electrochemically active sites) on the graphite surface. As a result, the growth rate of the film formed on the graphite surface by the reduction and decomposition of the aqueous electrolyte can be suppressed, and the denseness of the film can be improved. In addition, the water repellency of the C-F bond group can be expected to have the effect of keeping water molecules in the aqueous electrolyte away from the graphite surface. However, since the C-F bond group on the graphite surface can also become an irreversible site that traps lithium ions, if the absolute amount of the C-F bond group is too large, the amount of lithium released from the negative electrode active material during discharge decreases. Therefore, by optimizing the absolute amount of C—F bond groups on the graphite surface, a dense film can be formed and the decrease in the amount of lithium released due to the increase in irreversible sites can be suppressed, so that the charge / discharge reaction of the negative electrode active material can be promoted and the current density (discharge current density) caused by the release of Li+ from the secondary battery can be improved. Specifically, as described above, the peak intensity I 284eV Peak intensity I 688eV The ratio (I 688eV / I 284eV value) is 0.1 to 7, and the BET specific surface area is 0.5m 2 / g or more 3.9m 2 / g or less, the amount of C—F bond groups present on the graphite surface is appropriate from the viewpoint of achieving the above-mentioned effect. 284eV Peak intensity I 688eV The ratio (I 688eV / I 284eV Even if the BET specific surface area is 0.5m or less, the 2 When the carbon black is less than 1.0 m / g, the absolute amount of C—F bond groups on the graphite surface is small, so a dense film is not formed and the BET specific surface area is 3.9 m 2 When the BET specific surface area is more than 0.5 m / g, the absolute amount of C—F bond groups on the graphite surface is large, so the amount of lithium released due to the increase in irreversible sites decreases. 2 / g or more 3.9m 2 / g or less, the peak intensity I 284eVPeak intensity I 688eV The ratio (I 688eV / I 284eV When the value is less than 0.1, the absolute amount of C—F bond groups on the graphite surface is small, so a dense film is not formed and the peak intensity I 284eV Peak intensity I 688eV The ratio (I 688eV / I 284eV When the value exceeds 7, the absolute amount of C—F bonding groups on the graphite surface is large, so that the amount of lithium released due to the increase in irreversible sites decreases.

[0015] Hereinafter, an embodiment of the aqueous secondary battery according to the present disclosure will be described in detail.

[0016] The shape of the aqueous secondary battery of this embodiment is not particularly limited, and examples thereof include a coin type, a button type, a sheet type, a laminated type, a cylindrical type, a flat type, and a square type. FIG. 1 is a schematic cross-sectional view showing an example of the aqueous secondary battery of this embodiment. The aqueous secondary battery 20 shown in FIG. 1 includes a cup-shaped battery case 21, a positive electrode 22 provided on the upper part of the battery case 21, a negative electrode 23 provided at a position facing the positive electrode 22 with a separator 24 interposed therebetween, a gasket 25 formed of an insulating material, and a sealing plate 26 disposed at an opening of the battery case 21 and sealing the battery case 21 with the gasket 25. In the aqueous secondary battery 20 shown in FIG. 1, the space between the positive electrode 22 and the negative electrode 23 is filled with an electrolyte 27. The electrolyte 27, the positive electrode 22, the negative electrode 23, and the separator 24 will be described in detail below.

[0017] The electrolyte 27 is an aqueous electrolyte containing a solvent containing water and a lithium salt. Since the aqueous electrolyte contains water that is not flammable, it is possible to improve the safety of the aqueous secondary battery 20. The solvent may be water alone, but the content of water relative to the total amount of the solvents contained in the electrolyte 27 is preferably 10% or more and less than 100%, and more preferably 10% or more and less than 50%, by volume.

[0018] Furthermore, the amount of water relative to the lithium salt contained in the electrolyte 27 is preferably 1:4 or less, more preferably in the range of 1:0.4 to 1:4, and even more preferably in the range of 1:0.4 to 1:3, in terms of the molar ratio of lithium salt:water. When the amount of water relative to the lithium salt contained in the electrolyte 27 is within the above range, for example, the potential window of the electrolyte 27 is expanded, and the voltage applied to the aqueous secondary battery 20 may be increased, compared to when the amount is outside the above range.

[0019] The electrolytic solution 27 may contain a solvent other than water. Examples of the solvent other than water include organic solvents such as esters, ethers, nitriles, alcohols, ketones, amines, amides, sulfur compounds, and hydrocarbons. In addition, the solvent may be a halogen-substituted solvent in which at least a part of the hydrogen of these solvents is replaced with a halogen atom such as fluorine. Specifically, in terms of improving the battery characteristics of the aqueous secondary battery, organic carbonates such as cyclic organic carbonates such as ethylene carbonate, propylene carbonate, vinylidene carbonate, and butylene carbonate, chain organic carbonates such as dimethyl carbonate, methyl ethyl carbonate, and diethyl carbonate, and fluorinated organic carbonates containing fluorine as a constituent element such as fluoroethylene carbonate, fluorodimethyl carbonate, and methyl fluoropropionate are preferred. Among the above-mentioned examples, cyclic organic carbonates and fluorinated organic carbonates containing fluorine as a constituent element are particularly preferred in terms of suppressing the self-discharge of the battery. Among the above-listed fluorinated organic carbonates, fluoroethylene carbonate is preferred. These organic solvents may be used alone or in combination of two or more.

[0020] The amount of organic carbonate relative to the lithium salt contained in the electrolytic solution 27, in terms of the molar ratio of lithium salt:organic carbonate, is preferably in the range of 1:0.01 to 1:5, and more preferably in the range of 1:0.05 to 1:2. When the amount of organic carbonate relative to the lithium salt contained in the electrolytic solution 27 is within the above range, the battery characteristics of the aqueous secondary battery may be improved in some cases, compared to when it is outside the above range.

[0021] Any lithium salt can be used as long as it dissolves in a solvent containing water and dissociates to cause lithium ions to exist in the electrolyte solution 27. It is preferable that the lithium salt does not cause deterioration of battery characteristics due to reaction with materials constituting the positive and negative electrodes. Examples of such lithium salts include salts with inorganic acids such as perchloric acid, sulfuric acid, and nitric acid, salts with halide ions such as chloride ions and bromide ions, and salts with organic anions containing carbon atoms in their structures.

[0022] Examples of the organic anion constituting the lithium salt include anions represented by the following general formulas (i) to (vi). (R 1 SO2)(R 2 SO2)N - (i) (R 1 , R 2 are each independently selected from an alkyl group or a halogen-substituted alkyl group. 1 and R 2 may be bonded to each other to form a ring. R 3 SO3 - (ii) (R 3 is selected from an alkyl group or a halogen-substituted alkyl group. R 4 CO2 - (iii) (R 4 is selected from an alkyl group or a halogen-substituted alkyl group. (R 5 SO2)3C - (iv) (R 5 is selected from an alkyl group or a halogen-substituted alkyl group. [(R 6 SO2)N(SO2)N(R 7 SO2)] 2- (v) (R 6 , R 7 is selected from an alkyl group or a halogen-substituted alkyl group. [(R 8 SO2)N(CO)N(R 9 SO2)] 2- (vi) (R 8 , R 9 is selected from an alkyl group or a halogen-substituted alkyl group. In the above general formulas (i) to (vi), the number of carbon atoms in the alkyl group or the halogen-substituted alkyl group is preferably 1 to 6, more preferably 1 to 3, and further preferably 1 to 2. The halogen in the halogen-substituted alkyl group is preferably fluorine. The number of halogen substitutions in the halogen-substituted alkyl group is equal to or less than the number of hydrogen atoms in the original alkyl group.

[0023] R 1 ~R 9 Each of the above is, for example, a group represented by the following general formula (vii):

[0024] C n H a F b Cl c Br d I e (vii) (n is an integer greater than or equal to 1, a, b, c, d, and e are integers greater than or equal to 0, and 2n+1=a+b+c+d+e is satisfied.) Specific examples of the organic anion represented by the above general formula (i) include bis(trifluoromethanesulfonyl)imide (TFSI; [N(CF3SO2)2] - ), bis(perfluoroethanesulfonyl)imide (BETI; [N(C2F5SO2)2] - ), (perfluoroethanesulfonyl)(trifluoromethanesulfonyl)imide ([N(C2F5SO2)(CF3SO2)] - ) and the like. Specific examples of the organic anion represented by the above general formula (ii) include, for example, CF3SO3 - , C2F5SO3 - Specific examples of the organic anion represented by the general formula (iii) include, for example, CF3CO2 - , C2F5CO2 -Specific examples of the organic anion represented by the general formula (iv) include tris(trifluoromethanesulfonyl)carbonate ([(CF3SO2)3C] - ), tris(perfluoroethanesulfonyl)carbonic acid ([(C2F5SO2)3C] - ) and the like. Specific examples of the organic anion represented by the above general formula (V) include sulfonylbis(trifluoromethanesulfonyl)imide ([(CF3SO2)N(SO2)N(CF3SO2)] 2- ), sulfonylbis(perfluoroethanesulfonyl)imide ([(C2F5SO2)N(SO2)N(C2F5SO2)] 2- ), sulfonyl(perfluoroethanesulfonyl)(trifluoromethanesulfonyl)imide ([(C2F5SO2)N(SO2)N(CF3SO2)] 2- ) and the like. Specific examples of the organic anion represented by the above general formula (vi) include, for example, carbonylbis(trifluoromethanesulfonyl)imide ([(CF3SO2)N(CO)N(CF3SO2)] 2- ), carbonylbis(perfluoroethanesulfonyl)imide ([(C2F5SO2)N(CO)N(C2F5SO2)] 2- ), carbonyl(perfluoroethanesulfonyl)(trifluoromethanesulfonyl)imide ([(C2F5SO2)N(CO)N(CF3SO2)] 2- ) etc.

[0025] Examples of organic anions other than those represented by the above general formulas (i) to (vi) include anions such as bis(1,2-benzenediolate(2-)-O,O') borate, bis(2,3-naphthalenediolate(2-)-O,O') borate, bis(2,2'-biphenyldiolate(2-)-O,O') borate, and bis(5-fluoro-2-oleate-1-benzenesulfonic acid-O,O') borate.

[0026] The anion constituting the lithium salt is preferably an imide anion. Specific examples of suitable imide anions include the imide anions exemplified as the organic anion represented by the general formula (i) above, as well as bis(fluorosulfonyl)imide (FSI; [N(FSO2)2] - ), (fluorosulfonyl)(trifluoromethanesulfonyl)imide (FTI; [N(FSO2)(CF3SO2)] - ) etc.

[0027] The lithium salt having a lithium ion and an imide anion is preferably, for example, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(perfluoroethanesulfonyl)imide (LiBETI), lithium (perfluoroethanesulfonyl)(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide (LiFSI), or lithium (fluorosulfonyl)(trifluoromethanesulfonyl)imide (LiFTI), in terms of being able to effectively suppress self-discharge of the battery, and more preferably lithium bis(trifluoromethanesulfonyl)imide (LiTFSI). These may be used alone or in combination of two or more kinds.

[0028] Specific examples of other lithium salts include CF3SO3Li, C2F5SO3Li, CF3CO2Li, C2F5CO2Li, (CF3SO2)3CLi, (C2F5SO2)3CLi, (C2F5SO2)2(CF3SO2)CLi, (C2F5SO2)(CF3SO2)2CLi, [(CF3SO2)N(SO2)N(CF3SO2)]Li2, [(C2F5SO2)N(SO2)N(C2F5SO2)]Li2, [(C2F5SO2)N(SO2)N(CF3SO2)]Li2, [(CF3SO2)N(CO)N(CF3SO2)]Li2, [(C2F5SO2)N (CO)N(CF3SO2)]Li2, lithium bis(1,2-benzenedioleate(2-)-O,O')borate, lithium bis(2,3-naphthalenediolate(2-)-O,O')borate, lithium bis(2,2'-biphenyldioleate(2-)-O,O')borate, lithium bis(5-fluoro-2-oleate-1-benzenesulfonic acid-O,O')borate, lithium perchlorate (LiClO4), lithium chloride (LiCl), lithium bromide (LiBr), lithium hydroxide (LiOH), lithium nitrate (LiNO3), lithium sulfate (Li2SO4), lithium sulfide (Li2S), lithium hydroxide (LiOH), etc. These may be used alone or in combination of two or more.

[0029] The electrolyte 27 preferably contains an additive. The additive is added, for example, to improve the battery performance, and any additive known in the art can be used. In particular, a dicarbonyl group-containing compound is preferred in that it can form an electrochemically stable film on the negative electrode by the reduction reaction of the electrolyte 27 and effectively suppress the reduction decomposition reaction of the electrolyte 27.

[0030] Examples of the dicarbonyl group-containing compound include succinic acid, glutaric acid, phthalic acid, maleic acid, citraconic acid, glutaconic acid, itaconic acid, and diglycolic acid. The dicarbonyl group-containing compound may be an anhydride, and examples thereof include succinic anhydride, glutaric anhydride, phthalic anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, and diglycolic anhydride. Among the above, succinic acid, succinic anhydride, maleic acid, maleic anhydride, diglycolic acid, and glutaric acid are preferred in that they form an electrochemically stable film on the negative electrode and can more effectively suppress the reductive decomposition reaction of the electrolyte 27. Among these, succinic acid and maleic anhydride are preferred. These may be used alone or in combination of two or more.

[0031] The content of the additive is, for example, preferably 0.1% by mass to 5.0% by mass, and more preferably 0.5% by mass to 3.0% by mass, relative to the total amount of the electrolytic solution 27. By setting the content within the above range, the reductive decomposition reaction of the electrolytic solution 27 may be more effectively suppressed than when the content is outside the above range.

[0032] The positive electrode 22 includes, for example, a positive electrode current collector and a positive electrode composite layer formed on the positive electrode current collector. As the positive electrode current collector, a foil of a metal that is electrochemically and chemically stable in the potential range of the positive electrode, a film having the metal disposed on the surface layer, or the like can be used. The form of the positive electrode current collector is not particularly limited, and for example, a mesh body of the metal, a punching sheet, an expanded metal, or other porous body may be used. As the material of the positive electrode current collector, a known metal that can be used in a secondary battery using an aqueous electrolyte can be used. Examples of such metals include stainless steel, Al, aluminum alloy, and Ti. The thickness of the positive electrode current collector is preferably, for example, 3 μm or more and 50 μm or less from the viewpoint of current collecting properties, mechanical strength, and the like.

[0033] The positive electrode mixture layer contains a positive electrode active material. The positive electrode mixture layer may also contain a binder, a conductive material, etc. The positive electrode 22 can be manufactured, for example, by applying a positive electrode mixture slurry containing a positive electrode active material, a binder, a conductive material, etc., onto a positive electrode current collector, drying and rolling the coating, and forming a positive electrode mixture layer on the positive electrode current collector.

[0034] Examples of the positive electrode active material include lithium transition metal oxides containing lithium (Li) and transition metal elements such as cobalt (Co), manganese (Mn) and nickel (Ni). Other examples of the positive electrode active material include transition metal sulfides, metal oxides, lithium-containing polyanion compounds containing one or more transition metals such as lithium iron phosphate (LiFePO4) and lithium iron pyrophosphate (Li2FeP2O7), sulfur-based compounds (Li2S), oxygen-containing metal salts such as oxygen and lithium oxide, and the like. The positive electrode active material is preferably a lithium-containing transition metal oxide, and preferably contains at least one of Co, Mn and Ni as the transition metal element.

[0035] The lithium transition metal oxide may contain additional elements other than Co, Mn, and Ni, such as aluminum (Al), zirconium (Zr), boron (B), magnesium (Mg), scandium (Sc), yttrium (Y), titanium (Ti), iron (Fe), copper (Cu), zinc (Zn), chromium (Cr), lead (Pb), tin (Sn), sodium (Na), potassium (K), barium (Ba), strontium (Sr), calcium (Ca), tungsten (W), molybdenum (Mo), niobium (Nb), and silicon (Si).

[0036] Specific examples of lithium transition metal oxides include Li x CoO2, Li x NiO2, Li x MnO2, Li x Co y Ni 1-y O2, Li x Co y M 1-y O z , Li x Ni1-y M y O z 、 Li x Mn2O4, Li x Mn 2-y M y O4, LiMPO4, Li2MPO4F (in each chemical formula, M is at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B, 0 < x ≤ 1.2, 0 < y ≤ 0.9, 2.0 ≤ z ≤ 2.3). The lithium transition metal oxide may be used alone or in combination of multiple types. From the perspective of increasing the capacity, it is preferable that the lithium transition metal oxide contains 80 mol% or more of Ni with respect to the total amount of transition metals other than lithium. Also, from the perspective of the stability of the crystal structure, the lithium transition metal oxide is Li a Ni b Co c Al d O2 (0 < a ≤ 1.2, 0.8 ≤ b < 1, 0 < c < 0.2, 0 < d ≤ 0.1, b + c + d = 1) is more preferable.

[0037] As the conductive material, a known conductive material that enhances the electrical conductivity of the positive electrode composite layer can be used. For example, carbon materials such as carbon black, acetylene black, ketjen black, graphite, carbon nanofiber, carbon nanotube, and graphene can be mentioned. As the binder, a known binder that maintains a good contact state between the positive electrode active material and the conductive material and enhances the binding property of the positive electrode active material and the like to the surface of the positive electrode current collector can be used. For example, fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin, carboxymethyl cellulose (CMC) or its salt, styrene-butadiene rubber (SBR), polyethylene oxide (PEO), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), etc. can be mentioned.

[0038] The negative electrode 23 includes, for example, a negative electrode current collector and a negative electrode composite layer formed on the negative electrode current collector. As the negative electrode current collector, a foil of a metal that is electrochemically and chemically stable in the potential range of the negative electrode, a film having the metal disposed on the surface layer, or the like can be used. The form of the negative electrode current collector is not particularly limited, and for example, a porous body such as a mesh body, a punching sheet, or an expanded metal of the metal can be used. As the material of the negative electrode current collector, a known metal that can be used in an aqueous secondary battery can be used. Examples of such metals include Al, Ti, Mg, Zn, Pb, Sn, Zr, In, and the like. These may be used alone or may be alloys of two or more kinds, and may be composed of a material having at least one of them as a main component. In addition, when two or more elements are included, it is not necessarily necessary to alloy them. The thickness of the negative electrode current collector is preferably, for example, 3 μm or more and 50 μm or less from the viewpoint of current collecting properties, mechanical strength, and the like.

[0039] The negative electrode mixture layer contains a negative electrode active material. The negative electrode mixture layer may also contain a binder, a conductive material, and the like. The conductive material and binder can be the same as those on the positive electrode side. The negative electrode 23 can be manufactured, for example, by applying a negative electrode mixture slurry containing a negative electrode active material, a binder, a conductive material, and the like onto a negative electrode current collector, drying and rolling the coating, and forming a negative electrode mixture layer on the negative electrode current collector.

[0040] The negative electrode active material includes graphite having a C—F bond group on the surface. Hereinafter, such graphite may be referred to as surface-modified graphite. Surface-modified graphite is a graphite that has a peak intensity of about 688 eV (for example, in the range of 686.5 eV to 689.5 eV) derived from C—F bonds in an XPS spectrum obtained by X-ray photoelectron spectroscopy measurement, and is therefore characterized by being improved in current density (discharge current density) resulting from Li+ release from an aqueous secondary battery. 688eV The peak intensity around 284 eV (for example, in the range of 282.5 eV to 285.5 eV) derived from the C-C bond is defined as I 284eV When the peak intensity I 284eV Peak intensity I 688eV (hereinafter, the peak intensity I 688eV / Peak Intensity I 284eVThe BET specific surface area of ​​the surface-modified graphite is preferably 0.5 to 4, and more preferably 1.2 to 3. In order to improve the current density resulting from the release of Li+ from an aqueous secondary battery, the surface-modified graphite should have a BET specific surface area of ​​0.5 m 2 / g or more 3.9m 2 / g or less is acceptable, but 1m 2 / g or more 2m 2 / g or less, and 1.2m 2 / g or more 1.8m 2 It is more preferable that the molecular weight is not more than 1 / g.

[0041] Peak Intensities from XPS Spectra Measured by X-ray Photoelectron Spectroscopy I 688eV and peak intensity I 284eV is obtained under the following conditions:

[0042] Measurement equipment: PHI Quantera SXM, manufactured by ULVAC-PHI X-ray source used: Al-mono (1486.6eV), 20kV / 100W Analysis area: 100μmφ Photoelectron take-off angle: 45° Neutralization conditions: Electron + floating ion neutralization Measurement range (eV): 1300~0 Step (eV): 1.0 Pass E(eV):280.0 Measurement time (msec / step): 60 The BET specific surface area is obtained under the following measurement conditions.

[0043] Measurement equipment: Quantachrome, Autosorb iQ-MP Pre-drying (degassing conditions): in vacuum, 100℃, 1 hour Adsorption gas: N2 Surface-modified graphite is obtained by subjecting graphite to a fluorine treatment. The fluorine treatment of graphite can be performed, for example, by a dry method or a wet method. In the dry method, a gaseous fluorinating agent is used to subject graphite to a fluorine treatment in a gas phase. In the wet method, a liquid fluorinating agent is used to subject graphite to a fluorine treatment in a liquid phase. Among these methods, the dry method is preferred from the viewpoints of ease of operation, ease of forming C—F bond groups on the graphite surface, and difficulty in doping F into the inside of the graphite.

[0044] Examples of the fluorinating agent include fluorine (F2), nitrogen trifluoride, chlorine trifluoride, etc., and among the fluorinating agents, fluorine (F2) is preferred from the viewpoint of ease of handling. In addition, when the fluorination treatment is performed by a dry method, the fluorinating agent may be diluted with a diluent gas such as an inert gas, such as nitrogen gas, helium gas, neon gas, argon gas, or xenon gas.

[0045] In the following, a case where the fluorine treatment is performed on graphite by a dry method will be described.

[0046] When graphite is fluorinated by a dry method, the graphite can be fluorinated by contacting it with a fluorinating agent gas. Examples of the method for contacting graphite with a fluorinating agent gas include a method in which graphite is placed in a closed atmosphere of a fluorinating agent gas and the graphite is contacted with the fluorinating agent gas (called a batch method), and a method in which the fluorinating agent gas is supplied to the graphite and the graphite is contacted with the fluorinating agent gas (flow method).

[0047] When the graphite is brought into contact with the fluorinating agent gas, it is preferable to heat the graphite in order to increase the efficiency of the fluorination treatment, etc. The heating temperature is, for example, preferably 200° C. or more and 500° C. or less, and more preferably 300° C. or more and 400° C. or less.

[0048] The longer the graphite is exposed to the fluorinating agent gas, the greater the peak intensity I 688eV Therefore, the time for which the graphite is in contact with the fluorinating gas increases with the peak intensity I688eV / Peak Intensity I 284eV The time for which the graphite is in contact with the fluorinating gas must be set so that the BET specific surface area is within the range of 0.1 to 7. In addition, the longer the time for which the graphite is in contact with the fluorinating gas, the larger the BET specific surface area of ​​the fluorinated surface-modified graphite. Therefore, the time for which the graphite is in contact with the fluorinating gas must be set so that the BET specific surface area is 0.5 m 2 / g or more 3.9m 2 It is also necessary to keep the time within the range of 0.5 m / g or less. Note that the BET specific surface area of ​​the surface-modified graphite increases due to the fluorination treatment of graphite, so the BET specific surface area of ​​the graphite before the fluorination treatment is 0.5 m 2 / g or less.

[0049] In the XPS spectrum obtained by X-ray photoelectron spectroscopy, it is preferable that the surface-modified graphite does not have a peak at about 685 eV (for example, in the range of 683.5 eV to 686.5 eV) derived from the Me-F bond (Me: alkali metal, alkaline earth metal). However, the peak derived from the Me-F bond in the XPS spectrum measured by X-ray photoelectron spectroscopy is confirmed for the surface-modified graphite before charging and discharging the secondary battery. This is because a film having an Me-F bond such as LiF may be formed on the surface of the surface-modified graphite after charging and discharging the secondary battery. By using surface-modified graphite that does not have a Me-F bond group on the surface, for example, since there is no insulator such as LiF on the surface of the surface-modified graphite during initial charging, local non-uniformity of the current density during charging can be suppressed, and a thinner and denser film can be formed. Therefore, the contact resistance between the surface-modified non-graphitizable carbons can be suppressed, and the battery characteristics such as output characteristics can be improved in some cases.

[0050] The conditions for measuring the peaks derived from Me-F bonds in the XPS spectrum measured by X-ray photoelectron spectroscopy are as follows.

[0051] Measurement equipment: PHI Quantera SXM, manufactured by ULVAC-PHI X-ray source used: Al-mono (1486.6eV), 20kV / 100W Analysis area: 100μmφ Photoelectron take-off angle: 45° Neutralization conditions: Electron + floating ion neutralization Measuring element: F1s Measurement range (eV): 695-675 Step (eV): 0.05 Path E(eV):55 Measurement time (msec / step): 60 Surface-modified graphite has a peak intensity of I near the diffraction angle 2θ = 41° (for example, 40° to 42°) in the X-ray diffraction pattern obtained by X-ray diffraction measurement. 41° The peak intensity at the diffraction angle 2θ = 26.5° (for example, 25.5° to 27.5°; if a shoulder peak exists, the main peak intensity is used) is defined as I 26.5° When the peak intensity I 26.5° Peak intensity I 41° (hereinafter, peak intensity I 41° / Peak Intensity I 26.5° The peak at the diffraction angle 2θ of about 41° is due to graphite fluoride (CF n ), and the peak at a diffraction angle of 2θ = 26.5° is a peak derived from the (002) plane of graphite. 41° / Peak Intensity I 26.5° The smaller the value, the less fluorine atoms there are inside the graphite. 41° / Peak Intensity I 26.5° Surface-modified graphite with a value of 0.01 or less has C—F bond groups on the surface but has few or no fluorine atoms inside, which may prevent irreversible sites that trap lithium ions from being formed inside the graphite, improving the current density (discharge current density) resulting from the release of Li+ from a secondary battery. In order to arrange many fluorine atoms on the surface of the surface-modified graphite, it is preferable to carry out fluorine treatment by the above-mentioned dry method.

[0052] Surface-modified graphite is characterized by a peak intensity at a diffraction angle of 2θ = 26.5° (e.g., 25.5° to 27.5°; if a shoulder peak exists, the main peak intensity is used) in the X-ray diffraction pattern obtained by X-ray diffraction measurement. 26.5° The peak intensity at the diffraction angle 2θ = 77.5° (for example, 76.5° to 78.5°; if a shoulder peak exists, the main peak intensity is used) is defined as I 77.5° When the peak intensity I 77.5° Peak intensity I 26.5° (hereinafter, peak intensity I 26.5° / I 77.5° The value of the diffraction angle I is preferably 30 or more and 100 or less, and more preferably 40 or more and 80 or less. The peak intensity at a diffraction angle 2θ of 26.5° is a peak derived from the (002) plane of graphite, and the peak intensity at a diffraction angle 2θ of 77.5° is a peak derived from the (110) plane of graphite. 26.5° / I 77.5° The peak intensity I is an index of the crystal orientation of graphite. 26.5° / I 77.5° When the value satisfies the above range, the hardness of the surface-modified graphite can be increased, and as a result, for example, when the negative electrode active material layer is compressed to a predetermined packing density, the shape change of the graphite is suppressed, and the generation of new surfaces that are not fluorine-treated is suppressed, so that the effect of the fluorine treatment can be more effectively obtained.

[0053] Surface-modified graphite has a peak intensity of I near the diffraction angle 2θ = 44.5° (for example, 43.5° to 46.0°) in the X-ray diffraction pattern obtained by X-ray diffraction measurement. 44.5° The peak intensity at the diffraction angle 2θ = 42.5° (for example, 41.5° to 43.5°) is defined as I 42.5° When the peak intensity I 42.5° Peak intensity I 44.5° (hereinafter, peak intensity I 44.5° / I 42.5°It is preferable that the peak intensity I is 1 or more and 2 or less. The peak at a diffraction angle 2θ of 42.5° is a peak derived from the (100) plane of graphite, and the peak at a diffraction angle 2θ of 44.5° is a peak derived from the (101) plane of graphite. 44.5° / I 42.5° The value is an index of the degree of graphitization of graphite. 44.5° / I 42.5° By satisfying the above range, moderately unstable sites (e.g., dangling bonds) are formed on the graphite surface, and C—F bond groups can be formed on the graphite surface under milder fluorine treatment conditions. As a result, for example, the increase in the BET specific surface area of ​​graphite due to fluorine treatment can be suppressed, and the increase in irreversible sites that trap lithium ions can be suppressed in some cases.

[0054] The surface-modified graphite preferably has an average lattice spacing (d002) of the (002) plane obtained by X-ray diffraction measurement in the range of 0.3354 nm or more and 0.3380 nm or less, a lattice constant a of the (002) plane in the range of 0.2459 nm or more and 0.2464 nm or less, and a lattice constant c of the (002) plane in the range of 0.6713 nm or more and 0.6730 nm or less.

[0055] The conditions for the X-ray diffraction measurement are as follows.

[0056] Measurement device: PANalytical, X'PertPRO Target / monochrome: Cu / C Sample state: Powder Tube voltage / current: 45kV / 40mA Scanning mode: Continuous Step width: 0.01° Scanning speed: 5s / step Slit width (DS / SS / RS): 0.5° / None / 0.1mm Measurement range: 10°~120° Measurement temperature: room temperature Analysis software: PANalytical, HighScore Plus Lattice constant calculation method: Calculated using regression analysis from peak positions and plane indices calculated by local profile fitting analysis The surface-modified graphite preferably has a work function in the range of 5.0 eV to 6.0 eV obtained by an atmospheric photoelectron yield spectrometer. When the work function is less than 5.0 eV, the electrochemical reduction catalytic activity at the defect sites (electrochemically active sites) on the graphite surface is not sufficiently suppressed. As a result, the growth rate of the film formed on the graphite surface by the reductive decomposition of the aqueous electrolyte cannot be sufficiently suppressed, and the denseness of the film formed on the surface may decrease. Therefore, compared with the case where the work function satisfies the above range, the current density (discharge current density) caused by Li+ release from the secondary battery may decrease. In addition, when the work function exceeds 6.0 eV, the Li+ absorption reaction between the graphite layers becomes difficult to proceed, and the Li+ absorption and release reaction may be inhibited. Therefore, compared with the case where the work function satisfies the above range, the current density (discharge current density) caused by Li+ release from the secondary battery may decrease.

[0057] The conditions for measuring the work function using an atmospheric photoelectron yield spectrometer are as follows.

[0058] Measurement equipment: Riken Keiki Co., Ltd., AC-5 Sample state: Powder Light output: 100nW Photoelectron measurement energy scan range: 4.2~6.2eV Actinometer energy scanning range: 4.2~6.2eV Step width: 0.1 eV Measurement atmosphere: Air Measurement temperature: room temperature When the percentage of fluorine present on the surface of the surface-modified graphite is X atomic %, and the percentage of fluorine present in the entire surface-modified graphite is Y atomic %, the ratio of X atomic % / Y atomic % is preferably 3 to 40. When the ratio of X atomic % / Y atomic % is less than 3, the absolute amount of C—F bond groups on the surface of the surface-modified graphite is small, and the denseness of the film formed on the surface may decrease, or there may be many F atoms inside the surface-modified graphite, and there may be an increase in irreversible sites that trap lithium ions inside. Therefore, compared to when the ratio of X atomic % / Y atomic % is in the above range, the current density (discharge current density) due to Li+ release from the secondary battery may be lower. When the ratio of X atomic % / Y atomic % is more than 40, the absolute amount of C—F bond groups on the surface of the surface-modified graphite is large, and there may be an increase in irreversible sites that trap lithium ions on the surface. Therefore, compared to when the ratio of X atomic % / Y atomic % is in the above range, the current density (discharge current density) due to Li+ release from the secondary battery may be lower. In order to increase the amount of fluorine present on the surface of the surface-modified graphite, it is preferable to carry out fluorine treatment by the above-mentioned dry method.

[0059] The fluorine percentage (A atomic %) of the surface-modified non-graphitizable carbon is a value calculated by X-ray photoelectron spectroscopy. Specifically, the fluorine amount (atomic %), carbon amount (atomic %), and oxygen amount (atomic %) are determined by X-ray photoelectron spectroscopy, and the fluorine percentage is calculated by setting the total amount of these to 100, and this value is the fluorine percentage (A atomic %) of the surface-modified non-graphitizable carbon. The fluorine percentage (B atomic %) of the entire surface-modified non-graphitizable carbon is a value calculated using the following elemental analyzer. The fluorine percentage (weight %) of the entire surface-modified non-graphitizable carbon is determined by an organic elemental analysis system (XS-2100H, manufactured by Mitsubishi Chemical Analytical Co., Ltd.), and then the carbon percentage (weight %) of the entire surface-modified non-graphitizable carbon is determined by an elemental analyzer (JM11, manufactured by J Science Lab Co., Ltd.). The total of the fluorine amount (weight %), carbon amount (weight %) and oxygen amount (weight %) of the entire surface-modified non-graphitizable carbon is taken as 100, and the above-mentioned fluorine percentage (weight %) and carbon percentage (weight %) are subtracted to determine the oxygen percentage (weight %) of the entire surface-modified non-graphitizable carbon. The fluorine percentage (weight %) is then converted to a fluorine percentage (atomic %), and this value is taken as the fluorine percentage (B atomic %) of the entire surface-modified non-graphitizable carbon.

[0060] The average particle diameter (D50) of the surface-modified graphite is preferably, for example, 5 μm or more and 30 μm or less. When the average particle diameter (D50) of the surface-modified graphite satisfies the above range, the packing density of the negative electrode is improved and good battery characteristics may be obtained, compared with the case where the average particle diameter (D50) does not satisfy the above range. The average particle diameter (D50) means the volume average particle diameter at which the volume integrated value is 50% in the particle size distribution obtained by the laser diffraction scattering method.

[0061] Examples of graphite to be subjected to the fluorination treatment include natural graphite such as flake graphite, lump graphite, and earthy graphite, and artificial graphite such as lump artificial graphite (MAG) and spherulitic graphitized mesophase microspheres (MCMB). Among these, spherulitic graphitized mesophase microspheres are preferred because they are spherulitic graphite with edge faces oriented on the surface, and therefore have high particle hardness and have moderately unstable sites on the graphite surface. These may be used alone or in combination of two or more.

[0062] In addition to the surface-modified graphite, the negative electrode active material may contain a material that can be used as a negative electrode active material in a conventional lithium-ion secondary battery, as long as the effect of the present disclosure is not impaired. For example, alloys containing lithium element, metal oxides, metal sulfides, metal nitrides, and other metal compounds, silicon, and the like can be cited. For example, alloys containing lithium element include lithium aluminum alloys, lithium tin alloys, lithium lead alloys, and lithium silicon alloys. Furthermore, metal oxides containing lithium element include lithium titanate (Li4Ti5O 12 Examples of metal nitrides containing lithium include lithium cobalt nitride, lithium iron nitride, and lithium manganese nitride. Examples of sulfur-based compounds are also included.

[0063] The separator 24 is not particularly limited as long as it is permeable to lithium ions and has the function of electrically separating the positive electrode and the negative electrode, and for example, a porous sheet composed of a resin or an inorganic material is used. Specific examples of the porous sheet include a microporous thin film, a woven fabric, a nonwoven fabric, and the like. Examples of the material of the separator 24 include olefin resins such as polyethylene and polypropylene, polyamide, polyamideimide, cellulose, and the like. Examples of the inorganic material constituting the separator 24 include glass and ceramics such as borosilicate glass, silica, alumina, and titania. The separator 24 may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. The separator 24 may also be a multilayer separator including a polyethylene layer and a polypropylene layer, and a separator having a material such as an aramid resin or ceramic applied to the surface of the separator may also be used.

[0064] <Example> The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.

[0065] <Example 1> [Negative electrode] Surface-modified graphite was produced by subjecting graphite A to a fluorine treatment. Specifically, first, a Ni crucible containing graphite A was placed in a heating furnace, and N2 gas (flow rate: 2.7 L / min) was supplied into the heating furnace for 1.5 hours. Then, while continuing to supply N2 gas, the temperature inside the heating furnace was raised to 300°C over 3.5 hours. Next, the temperature inside the heating furnace was maintained at 300°C, and a mixed gas of N2 gas (flow rate: 2.0 L / min) and F2 gas (1.9 mol / h) was supplied into the heating furnace for 2 minutes. Then, the heating inside the heating furnace was stopped, and N2 gas (flow rate: 2.7 L / min) was supplied into the heating furnace, and the furnace was allowed to cool, obtaining surface-modified graphite. The physical properties of the obtained surface-modified graphite were measured, and the results are summarized in Table 1.

[0066] The surface-modified graphite (negative electrode active material) and PVDF as a binder were mixed in N-methyl-2-pyrrolidone (NMP) at a solid content mass ratio of 96:4 to prepare a negative electrode composite slurry. Next, the negative electrode composite slurry was applied onto a negative electrode current collector made of copper foil, and the coating was dried and then rolled with a rolling roller. Then, the negative electrode was obtained by cutting into a predetermined electrode size. The application amount of the negative electrode composite slurry and the packing density of the negative electrode active material layer were 32.3 g / m, respectively. 2 , 1.0gcm -3 It was.

[0067] [Positive electrode] A positive electrode composite slurry was prepared by mixing LiCoO2 as a positive electrode active material, carbon black as a conductive material, and PVdF as a binder in a mass ratio of 94:3:3 in NMP. The positive electrode composite slurry was then applied onto a positive electrode current collector made of Ti foil, the coating was dried, and then rolled with a rolling roller. The positive electrode was then cut into a predetermined electrode size to obtain a positive electrode. The amount of application of the positive electrode composite slurry and the packing density of the positive electrode active material layer were 65.0 g / cm. 2 , 2.8gcm -3 It was.

[0068] [Aqueous electrolyte] LITFSI, LIBETI, water, and fluoroethylene carbonate (FEC) were mixed in a molar ratio of 1.0:0.42:1.23:2.60 to prepare an aqueous electrolyte solution with a water volume ratio of 10% in the solvent.

[0069] [Test cell] A three-electrode cell (test cell) containing the above electrolyte was constructed, with the above negative electrode as a working electrode, the above positive electrode as a counter electrode, and Ag / AgCl (3M NaCl) as a reference electrode.

[0070] <Example 2> Surface-modified graphite was prepared in the same manner as in Example 1, except that a mixed gas of N2 gas and F2 gas was supplied into the heating furnace for 10 minutes in the preparation of the surface-modified graphite. The physical properties of the obtained surface-modified graphite were measured, and the results are summarized in Table 1. Then, a test cell was constructed in the same manner as in Example 1, except that this surface-modified graphite was used as the negative electrode active material.

[0071] <Example 3> Surface-modified graphite was prepared in the same manner as in Example 1, except that the temperature inside the heating furnace was raised to 400°C over 4.5 hours, the temperature inside the heating furnace was maintained at 400°C, and a mixed gas of N2 gas and F2 gas was supplied into the heating furnace for 2 minutes. The physical properties of the obtained surface-modified graphite were measured, and the results are summarized in Table 1. Then, a test cell was constructed in the same manner as in Example 1, except that this surface-modified graphite was used as the negative electrode active material.

[0072] <Example 4> Surface-modified graphite was prepared in the same manner as in Example 3, except that a mixed gas of N2 gas and F2 gas was supplied into the heating furnace for 10 minutes in the preparation of the surface-modified graphite. The physical properties of the obtained surface-modified graphite were measured, and the results are summarized in Table 1. Then, a test cell was constructed in the same manner as in Example 1, except that this surface-modified graphite was used as the negative electrode active material.

[0073] <Comparative Example 1> Graphite A that was not subjected to fluorination treatment was used as the negative electrode active material. The physical properties of graphite A were measured, and the results are summarized in Table 1. A test cell was constructed in the same manner as in Example 1 using this graphite A as the negative electrode active material.

[0074] <Comparative Example 2> Surface-modified graphite was prepared in the same manner as in Example 1, except that graphite B was used in the preparation of the surface-modified graphite. The physical properties of the obtained surface-modified graphite were measured, and the results are summarized in Table 1. Then, a test cell was constructed in the same manner as in Example 1, except that this surface-modified graphite was used as the negative electrode active material.

[0075] <Comparative Example 3> Surface-modified graphite was prepared in the same manner as in Example 2, except that graphite B was used in the preparation of the surface-modified graphite. The physical properties of the obtained surface-modified graphite were measured, and the results are summarized in Table 1. Then, a test cell was constructed in the same manner as in Example 1, except that this surface-modified graphite was used as the negative electrode active material.

[0076] <Comparative Example 4> Surface-modified graphite was prepared in the same manner as in Example 3, except that graphite B was used in the preparation of the surface-modified graphite. The physical properties of the obtained surface-modified graphite were measured, and the results are summarized in Table 1. Then, a test cell was constructed in the same manner as in Example 1, except that this surface-modified graphite was used as the negative electrode active material.

[0077] <Comparative Example 5> Surface-modified graphite was prepared in the same manner as in Example 4, except that graphite B was used in the preparation of the surface-modified graphite. The physical properties of the obtained surface-modified graphite were measured, and the results are summarized in Table 1. Then, a test cell was constructed in the same manner as in Example 1, except that this surface-modified graphite was used as the negative electrode active material.

[0078] <Comparative Example 6> Graphite B that was not subjected to fluorination treatment was used as the negative electrode active material. The physical properties of graphite B were measured, and the results are summarized in Table 1. A test cell was constructed in the same manner as in Example 1 using this graphite B as the negative electrode active material.

[0079] Cyclic voltammetry measurements were carried out using the test cells of Examples 1 to 4 and Comparative Examples 1 to 6, and the current density of the oxidation peak in the second cycle was evaluated. The measurement conditions are shown below.

[0080] Starting potential: OCV First folding potential: -2.950V vs. Ag / AgCl (3M NaCl) (0.288V based on Li) Second folding potential: -0.238V vs. Ag / AgCl (3M NaCl) (3V based on Li) Number of cycles: 2 cycles Sweep speed: 0.5mV / sec Measurement temperature: 25℃ Table 1 summarizes the increase in the current density of the oxidation peak at the second cycle for each of Examples 1 to 4 relative to the current density of the oxidation peak at the second cycle for Comparative Example 1, in which graphite A was not fluorine-treated, and also summarizes the increase in the current density of the oxidation peak at the second cycle for each of Comparative Examples 2 to 5 relative to the current density of the oxidation peak at the second cycle for Comparative Example 6, in which graphite B was not fluorine-treated. In Table 1, the level at which no oxidation peak appeared is indicated by -.

[0081] [Table 1]

[0082] As can be seen from Table 1, I 688eV / I 284eV The value is 0.1 to 7, and the BET specific surface area is 0.5 m 2 / g or more 3.9m 2 In Examples 1 to 4, surface-modified graphite satisfying the range of I 688eV / I 284eVThe current density of the oxidation peak increased compared to Comparative Example 1 which did not satisfy at least one of the value and the BET specific surface area. Note that in Comparative Examples 1 to 6, no clear oxidation peak was confirmed.

[0083] Among Examples 1 to 4, Examples 2 and 4, which used surface-modified graphite with an (I688eV / I284eV) / (BET specific surface area) ratio in the range of 1.15 to 1.8, were particularly preferable in terms of increasing the current density of the oxidation peak.

[0084] <Example 5> A test cell was constructed in the same manner as in Example 2, except that in the preparation of the aqueous electrolyte solution, LITFSI, LIBETI, and water were mixed in a molar ratio of 0.7:0.3:2.0 to prepare an aqueous electrolyte solution in which the volume ratio of water in the solvent was 100%.

[0085] <Example 6> A test cell was constructed in the same manner as in Example 4, except that the aqueous electrolyte solution of Example 5 was used.

[0086] <Comparative Example 7> A test cell was constructed in the same manner as in Comparative Example 1, except that the aqueous electrolyte solution of Example 5 was used.

[0087] <Comparative Example 8> A test cell was constructed in the same manner as in Comparative Example 3, except that the aqueous electrolyte solution of Example 5 was used.

[0088] <Comparative Example 9> A test cell was constructed in the same manner as in Comparative Example 5, except that the aqueous electrolyte solution of Example 5 was used.

[0089] <Comparative Example 10> A test cell was constructed in the same manner as in Comparative Example 6, except that the aqueous electrolyte solution of Example 5 was used.

[0090] Using the test cells of Examples 5 to 6 and Comparative Examples 7 to 10, cyclic voltammetry measurements were performed in the same manner as above to evaluate the current density of the oxidation peak in the first cycle. Table 2 summarizes the increase in the current density of the oxidation peak in the first cycle for each of Examples 5 to 6 relative to the current density of the oxidation peak in the first cycle for Comparative Example 7, in which graphite A was not fluorinated, and also summarizes the increase in the current density of the oxidation peak in the first cycle for each of Comparative Examples 8 to 9 relative to the current density of the oxidation peak in the first cycle for Comparative Example 10, in which graphite B was not fluorinated. The level at which no oxidation peak appeared is indicated as -.

[0091] [Table 2]

[0092] As can be seen from Table 2, in Examples 5 and 6, the current density of the oxidation peak increased compared to Comparative Example 7, even though an aqueous electrolyte in which the volume ratio of water in the solvent was 100% was used. [Explanation of symbols]

[0093] 20 Secondary battery 21 Battery case 22 Positive electrode 23 Negative electrode 24 Separator 25 Gasket 26 Sealing plate 27 Electrolyte

Claims

1. A negative electrode active material for use in an aqueous secondary battery using an aqueous electrolyte solution containing water and a lithium salt, The negative electrode active material includes graphite, The graphite has a C—F bond group on its surface, The graphite has a peak intensity of I near 688 eV due to a C—F bond in an XPS spectrum obtained by X-ray photoelectron spectroscopy. 688eV The peak intensity at around 284 eV due to the C-C bond is I 284eV When the peak intensity I 284eV The peak intensity I 688eV The ratio (I 688eV / I 284eV value) is 0.1 to 7, and the BET specific surface area is 0.5 m 2 / g or more 3.9m 2 / g or less.

2. The graphite has a peak intensity of I near a diffraction angle 2θ=41° in an X-ray diffraction pattern obtained by X-ray diffraction measurement. 41° The peak intensity at the diffraction angle 2θ = 26.5° is I 26.5° When the peak intensity I 26.5° The peak intensity I 41° The ratio (I 41° / I 26.5° 2. The negative electrode active material for an aqueous secondary battery according to claim 1, wherein the value of α is 0.01 or less.

3. 3. The negative electrode active material for an aqueous secondary battery according to claim 1, wherein, when a fluorine percentage present on a graphite surface is X atomic % and a fluorine percentage present on the entire graphite is Y atomic %, the ratio of X atomic % / Y atomic % is 3 or more and 40 or less.

4. 4. The negative electrode active material for a water-based secondary battery according to claim 1, wherein the graphite has an average particle size (D50) of 5 μm or more and 30 μm or less.

5. In the X-ray diffraction pattern obtained by X-ray diffraction measurement, the graphite has a peak intensity of I 26.5° The peak intensity at the diffraction angle 2θ = 77.5° is I 77.5° When the peak intensity I 77.5° The peak intensity I 26.5° The ratio (I 26.5° / I 77.5° 5. The negative electrode active material for an aqueous secondary battery according to claim 1, wherein the value of β-

6. In the X-ray diffraction pattern obtained by X-ray diffraction measurement, the graphite has a peak intensity of I 44.5° The peak intensity at the diffraction angle 2θ = 42.5° is I 42.5° When the peak intensity I 42.5° The peak intensity I 44.5° The ratio (I 44.5° / I 42.5° 6. The negative electrode active material for an aqueous secondary battery according to claim 1, wherein the value of (a) is 1 or more and 2 or less.

7. The negative electrode active material for aqueous secondary batteries according to any one of claims 1 to 6, wherein the graphite is a spherulitic graphitized product of mesophase microspheres.

8. A negative electrode for use in an aqueous secondary battery using an aqueous electrolyte solution containing water and a lithium salt, The negative electrode comprises the negative electrode active material for an aqueous secondary battery according to any one of claims 1 to 7.

9. 9. An aqueous secondary battery comprising a negative electrode, a positive electrode, and an aqueous electrolyte solution containing water and a lithium salt, the negative electrode being the aqueous secondary battery negative electrode according to claim 8.

10. 10. The aqueous secondary battery of claim 9, wherein the lithium salt comprises a salt having a lithium ion and an imide anion.

11. 11. The aqueous secondary battery of claim 10, wherein the lithium salt comprises lithium bis(trifluoromethanesulfonyl)imide.

12. 12. The aqueous secondary battery according to claim 9, wherein the content of the water relative to the lithium salt contained in the aqueous electrolyte is 1:4 or less in terms of a molar ratio of the lithium salt:water.

13. The aqueous secondary battery according to any one of claims 9 to 12, wherein the aqueous electrolyte solution contains an organic carbonate.

14. The aqueous secondary battery according to claim 13, wherein a content of the organic carbonate relative to the lithium salt contained in the aqueous electrolyte solution is in a range of 1:0.01 to 1:5 in terms of a molar ratio of the lithium salt:the organic carbonate, and a content of the water relative to the lithium salt contained in the aqueous electrolyte solution is in a range of 1:0.4 to 1:4 in terms of a molar ratio of the lithium salt:the water.

15. 15. The aqueous secondary battery of claim 13 or 14, wherein the organic carbonate comprises a cyclic organic carbonate.

16. The aqueous secondary battery according to claim 15 , wherein the cyclic organic carbonate contains fluorine as a constituent element.

17. 17. The aqueous secondary battery of claim 16, wherein the cyclic organic carbonate comprises fluoroethylene carbonate.

Citation Information

Patent Citations

  • Aqueous battery using carbon fluoride as anode

    CN102903921A

  • Method for preparing graphite fluoride at low temperature

    CN103043641A

  • Rotation controller for rotary head

    JP1989023453A

  • Activating agent for lead storage battery and lead storage battery using same

    JP2003059527A

  • Aqueous electrolyte having carbonate and battery arranged by use thereof

    JP2018073819A