Alkaline dry cell gasket
Through the composition of polyamide 610 resin and polyethylene resin, the structure and composition of the resin are optimized, and the problems of large differences in cracking strength, insufficient heat resistance and transparency during absolute drying and water absorption are solved, and the problem of insufficient cracking strength of alkaline drying battery sealing gaskets is realized. Improved stability and detection accuracy.
Patent Information
- Application Number
- CN202180017291.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-19
- Filing Date
- 2021-02-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-02-25
AI Technical Summary
The existing alkaline dry battery seals have large differences in the cracking strength between absolute dryness and water absorption, and insufficient heat resistance and transparency, resulting in unstable working pressure of the safety valve and low foreign object detection accuracy.
The polyamide 610 resin and polyethylene resin are used to ensure that the polyamide 610 resin forms a continuous phase by transmittance electron tomography, and the polyethylene resin forms a dispersed phase. The average dispersion diameter of the dispersed phase is above 1 nm and below 1000 nm, and the acid is combined with Mixing of modified and unmodified polyethylene resins optimizes viscosity and terminal amino concentrations for improved compatibility and transparency.
It realizes the small difference between the cracking strength between absolute dryness and water absorption, excellent alkali resistance and heat resistance, and improves the transparency of the sealing gasket, ensures the stable operation of the safety valve and the leakage prevention of electrolyte, and enhances the accuracy of foreign matter detection .
Smart Images

Figure BDA0003817723060000131 
Figure BDA0003817723060000141
Abstract
Description
Technical Field
[0001] The present invention relates to an alkaline dry cell gasket formed of a polyamide resin composition containing polyamide resin 610 and polyethylene resin. Background Art
[0002] Alkaline dry batteries are a type of battery that works by the redox reaction of zinc and manganese dioxide, and are manufactured in the form of cylinders, buttons, etc. For example, in an alkaline dry battery that takes a cylindrical form, a power generation element is housed in a bottom cylindrical positive electrode casing that serves as both a positive terminal and a positive electrode collector. The opening of such a positive electrode casing needs to be sealed with a gasket between it and the negative terminal plate to prevent leakage of the electrolyte.
[0003] In addition, alkaline dry batteries need to have a function (safety valve) to prevent explosions caused by short circuits, etc., and require a gasket with a thin wall portion that can be broken at a certain pressure or above. The pressure at which the gasket breaks is called burst strength.
[0004] In the past, gaskets used polyamide resins that are easy to mold as raw materials, but polyamide resins have a difference in burst strength when they are absolutely dry and when they absorb water due to their hygroscopicity. Such a difference in strength means a deviation in the working pressure of the safety valve under the use environment, so in recent years, it is hoped that the strength change will be suppressed. In addition, for gaskets that can be used as safety valves (which are safety components), since there is a process for checking foreign matter and bubbles, if the transparency is low in this process, the detection accuracy of foreign matter deteriorates, so high transparency is required.
[0005] To address these problems, various technical improvements have been attempted, for example, in polyamide 610 resin (Patent Documents 1 and 2), polyolefin resin (Patent Document 3), and composite resins of polyamide 610 resin and polyolefin resin (Patent Documents 3 and 4).
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2015-26477
[0009] Patent Document 2: Japanese Patent Application Publication No. 2018-181825
[0010] Patent Document 3: Japanese Patent Application Publication No. 2001-202935
[0011] Patent Document 4: Japanese Patent Application Publication No. 2008-103221 Summary of the invention
[0012] Problems to be solved by the invention
[0013] However, in gaskets containing polyamide 610 resin having low water absorption as a main component as disclosed in Patent Documents 1 and 2, the difference in burst strength between when absolutely dry and when water absorbed tends to decrease, but this is still insufficient.
[0014] Furthermore, the gasket using a polyolefin resin disclosed in Patent Document 3 has a problem that it has lower heat resistance than a gasket using a polyamide resin and deforms due to heat generated by a short circuit, causing leakage of electrolyte of the dry cell.
[0015] In addition, a composite resin obtained by dispersing a polyolefin resin in a polyamide 610 resin as in Patent Documents 3 and 4 has a problem that the transparency is inferior to that of a gasket composed of a single component of polyamide resin.
[0016] Therefore, in view of the problems of the prior art, the present invention aims to provide an alkaline dry cell gasket made of a polyamide resin composition, which has a small difference in bursting strength between when absolutely dry and when water-absorbed, is excellent in alkali resistance, heat resistance, and lightness, and has a transparency level that allows foreign matter inspection.
[0017] Means for solving problems
[0018] That is, the present invention mainly has the following configurations.
[0019] An alkaline dry cell sealing gasket is made of a resin composition, wherein the total amount of polyamide 610 resin (A) and polyethylene resin (B) is 100 parts by weight, and 50 to 95 parts by weight of polyamide 610 resin (A) and 5 to 50 parts by weight of polyethylene resin (B) are mixed. In the morphology obtained by observing the resin composition by transmission electron tomography, the polyamide 610 resin (A) forms a continuous phase, the polyethylene resin (B) forms a dispersed phase, and the average dispersion diameter of the dispersed phase is greater than 1 nm and less than 1000 nm.
[0020] Effects of the Invention
[0021] The present invention provides an alkaline dry cell gasket made of a polyamide resin composition, which has a small difference in burst strength between when absolutely dry and when water-absorbed, is excellent in alkali resistance, heat resistance, and lightness, and has a transparency level that allows foreign matter inspection.
[0022] Such an alkaline dry cell gasket can be stored for a long time and can operate the explosion-proof safety valve with stable accuracy regardless of the surrounding usage environment. In addition, foreign matter can be easily detected during the production process, so that the risk of electrolyte leakage when assembled into a dry cell can be suppressed, and the undesirable situation that the safety valve operates outside the assumed pressure range can be prevented. DETAILED DESCRIPTION
[0023] Hereinafter, the present invention will be described in detail.
[0024] The polyamide resin composition for forming the alkaline dry battery gasket of the present invention is composed of a polyamide 610 resin (A) and a polyethylene resin (B).
[0025] The polyamide 610 resin (A) of the present invention refers to a polymer having a chain skeleton obtained by polymerizing hexamethylenediamine as a diamine and sebacic acid as a dicarboxylic acid as polymerization monomers. By using such (A), lightness, transparency, alkali resistance and heat resistance can be imparted. In addition, by utilizing low water absorption, the difference in burst strength between when absolutely dry and when absorbing water can be reduced.
[0026] The viscosity of the polyamide 610 resin (A) in the present invention is not particularly limited, but the viscosity measured in accordance with JIS K 6933 (2013) based on ISO307 is preferably in the range of 70 ml / g or more and less than 120 ml / g. When the viscosity is 70 ml / g or more, the compatibility with the polyethylene resin (B) is good, the transparency and appearance of the molded product are excellent, and a certain alkali resistance can be maintained, so it is preferred. When the viscosity is less than 120 ml / g, the difference in burst strength between the absolute dry state and the water absorption state can be reduced, so it is preferred.
[0027] The terminal amino group concentration of the polyamide 610 resin (A) in the present invention is not particularly limited, but from the viewpoint of reactivity with the polyethylene resin (B), the terminal amino group concentration is 1.0×10 -5 The polyamide 610 resin (A) having a concentration of 1 mol / g or more is preferred. The terminal amino group concentration can be measured by dissolving the polyamide resin in 85% phenol-ethanol solution, using thymol blue as an indicator, and titrating with a hydrochloric acid aqueous solution.
[0028] There is no limitation on the terminal carboxyl concentration of the polyamide 610 resin (A) in the present invention, but the terminal carboxyl concentration is 10.0×10 -5 The polyamide 610 resin (A) with a molecular weight of 1 mol / g or less is preferred because of its excellent alkali resistance. The terminal carboxyl group concentration can be measured by heating and dissolving in benzyl alcohol and titrating with a potassium hydroxide aqueous solution having a normality of 0.02N using a phenolphthalein indicator.
[0029] The polyethylene resin (B) of the present invention refers to a homopolymer having a chain skeleton derived from ethylene. Copolymers with propylene or other olefins and synthetic rubber resins are not included. By using such (B), lightness and alkali resistance can be imparted, and the difference in burst strength between when absolutely dry and when absorbing water can be reduced.
[0030] The polyethylene resin (B) of the present invention is preferably a mixture of an acid-modified polyethylene resin (B1) and an unmodified polyethylene resin (B2). The use of (B) as a mixture of (B1) and (B2) is preferred because the reactivity with the polyamide 610 resin (A) is improved and the transparency is increased.
[0031] The acid-modified polyethylene resin (B1) refers to a polyethylene resin modified with maleic anhydride or carboxylic acid. The density of the acid-modified polyethylene resin (B1) is not particularly limited, but is preferably 940 kg / m 2 which is classified as a high-density polyethylene resin from the viewpoint of improving transparency when mixed with the polyamide 610 resin (A). 3 In addition, the molecular weight of (B1) is not particularly limited. In addition, the density of the acid-modified polyethylene resin is preferably 980 kg / m 3 the following.
[0032] The acid modification amount of the acid-modified polyethylene resin (B1) is not particularly limited, but the acid value measured using xylene as a solvent in accordance with JIS K 0070 (1992) is preferably 3.0 to 10.0 mgKOH / g.
[0033] The unmodified polyethylene resin (B2) is a polyethylene resin that has not been subjected to acid modification or the like. The density of the unmodified polyethylene resin is not particularly limited, but is preferably 940 kg / m 2 which is classified as a high-density polyethylene resin from the viewpoint of improving transparency when mixed with the polyamide 610 resin. 3 In addition, the density of the unmodified polyethylene resin is preferably 980 kg / m 3 the following.
[0034] In the polyamide resin composition forming the alkaline dry battery gasket of the present invention, when the total amount of polyamide 610 resin (A) and polyethylene resin (B) is recorded as 100 parts by weight, the amount of polyamide 610 resin (A) is 50 to 95 parts by weight, and the amount of polyethylene resin (B) is 5 to 50 parts by weight. When the polyamide 610 resin (A) is less than 50 parts by weight, the compatibility of polyamide 610 resin (A) and polyethylene resin (B) deteriorates, and the gasket is prone to poor appearance such as reduced transparency and whitening caused by the separation of the polyamide phase and the polyethylene phase, so it is not preferred. On the other hand, when the polyamide 610 resin (A) is more than 95 parts by weight, the water absorption rate when molded into a gasket cannot be fully reduced, and the difference between the bursting strength when absolutely dry and when absorbing water becomes large, so it is not preferred.
[0035] From the viewpoint of improving the reactivity with the polyamide 610 resin (A), improving the transparency, and improving the appearance of the gasket, the blending ratio of the acid-modified polyethylene resin (B1) in the present invention is preferably 10 to 95 parts by weight, more preferably 20 to 70 parts by weight, based on 100 parts by weight of the total amount of the polyethylene resin (B). In addition, the blending ratio of the unmodified polyethylene resin (B2) in the present invention is preferably 5 to 90 parts by weight, more preferably 30 to 80 parts by weight, based on 100 parts by weight of the total amount of the polyethylene resin (B).
[0036] The morphology of the polyamide resin composition forming the alkaline dry cell gasket in the present invention can be observed by transmission electron tomography (hereinafter, sometimes referred to as TEM), and the polyamide 610 resin (A) forms a continuous phase, and the polyethylene resin (B) forms a dispersed phase. Furthermore, the average dispersion diameter of the dispersed phase of the polyethylene resin (B) is greater than 1nm and less than 1000nm. When the average dispersion diameter of the dispersed phase is greater than 1000nm, the transparency of the gasket is reduced and the appearance of the whitening caused by phase peeling is poor. In addition, due to the uneven composition of the gasket, the bursting strength of the gasket is biased. In addition, when the average dispersion diameter of the dispersed phase is less than 1nm, the heat resistance of the gasket is reduced, so it is not preferred. Here, the following content is applicable to the morphological observation by TEM. In general, regarding the morphology in the thermoplastic resin composition, since the morphology can be maintained even after melt molding, in the present invention, the molded body formed by injection molding the polyamide resin composition is used to observe the morphology. That is, the cross-sectional center of the ASTM No. 4 tensile test piece obtained by injection molding at a barrel temperature of the melting point of the polyamide resin + 50°C was cut into 1-2 mm squares, and the polyamide resin was dyed with phosphotungstic acid and osmium, and then cut into ultrathin sections of 0.1 μm or less (about 80 nm) at -196°C using an ultrathin slicer, and observed by magnifying it to 5000 times using a Hitachi transmission electron microscope (model: H-7100). The obtained image was analyzed using the analysis software "Image-Pro" made by Japan Roper. The white area was taken as the polyethylene phase, and the "area length" was taken as the average dispersion diameter of the dispersed phase.
[0037] There are no particular restrictions on the means for making the average dispersion diameter of the polyethylene resin (B) be greater than 1 nm and less than 1000 nm. For example, the following methods can be used: when the total amount of the polyamide 610 resin (A) and the polyethylene resin (B) is 100 parts by weight, the amount of the polyamide 610 resin (A) is 50 to 95 parts by weight, and the amount of the polyethylene resin (B) is 5 to 50 parts by weight, and the polyethylene resin (B) is a mixture of an acid-modified polyethylene resin (B1) and an unmodified polyethylene resin (B2), and the mixing ratio of the acid-modified polyethylene resin (B1) is 10 to 95 parts by weight when the total amount of the polyethylene resin (B) is 100 parts by weight.
[0038] The resin composition forming the alkaline dry cell gasket of the present invention may contain other components in addition to the polyamide 610 resin (A) and the polyethylene resin (B) within a range that does not impair its characteristics. For example, as other components, a thermoplastic resin other than the components (A) and (B) may be contained. As the thermoplastic resin, polyamide resins other than the polyamide 610 resin (A), polyester resins, polyphenylene sulfide resins, polyphenylene ether resins, polycarbonate resins, polylactic acid resins, polyacetal resins, polysulfone resins, tetrafluoroethylene resins, polyetherimide resins, polyamideimide resins, polyimide resins, polyethersulfone resins, polyetherketone resins, polysulfideetherketone resins, polyetheretherketone resins, polystyrene resins, ABS resins and other styrene resins, polyalkylene oxide resins, etc. may be cited.
[0039] When the thermoplastic resin is used, the content thereof is not limited, but is preferably 0.1 parts by weight or more and less than 10 parts by weight based on 100 parts by weight of the total of the polyamide 610 resin (A) and the polyethylene resin (B).
[0040] Furthermore, as other components, one or more common additives such as ultraviolet absorbers, crystal nucleating agents, anti-coloring agents, weathering agents, mold release agents, lubricants, and antistatic agents may be added within a range that does not impair the purpose of the present invention.
[0041] As the additives, for example, ultraviolet absorbers such as benzotriazole, phenol, and phosphorus, organic nucleating agents such as metal salts of aromatic carboxylic acids, sorbitol derivatives, organic phosphates, and aromatic amide compounds, nucleating agents of inorganic nucleating agents such as talc, boron nitride, and other metal silicates, weathering agents such as resorcinol, salicylate, benzotriazole, benzophenone, and hindered amine, mold release agents such as stearic acid metal salts, aliphatic alcohols, aliphatic amides, aliphatic bisamides, ethylenebisstearamide, and higher fatty acid esters, lubricants such as octyl paraben and wax, alkyl sulfate type anionic systems, quaternary ammonium salt type cationic systems, nonionic systems such as polyoxyethylene sorbitan monostearate, and betaine-based amphoteric antistatic agents, etc. Among them, nucleating agents and mold release agents are preferred from the viewpoint of molding processability. The content of the crystal nucleating agent is preferably 0.01 parts by weight or more and less than 5 parts by weight, based on 100 parts by weight of the total amount of the polyamide 610 resin (A) and the polyethylene resin (B). In addition, the content of the release agent is preferably 0.1 parts by weight or more and less than 3 parts by weight.
[0042] The ultraviolet absorber, crystal nucleating agent, anti-coloring agent, weathering agent, release agent, lubricant, antistatic agent and other additives may be used in two or more kinds. The content thereof is not particularly limited, but is preferably 0.01 parts by weight or more and less than 5 parts by weight relative to 100 parts by weight of the polyamide 610 resin (A).
[0043] From the viewpoint of lightness, the density of the alkaline dry battery gasket made of the polyamide resin composition of the present invention is preferably 1000 kg / m 3 Above and 1070kg / m 3 In addition, in order to prevent the electrolyte of the alkaline dry battery from leaking out due to the heat generated by the short circuit, the melting point of the alkaline dry battery gasket made of the polyamide resin composition of the present invention is preferably 210°C or more and 280°C or less. Furthermore, in order to improve the detection accuracy of foreign matter in the process of inspecting foreign matter and bubbles in the gasket, the haze of the ASTM No. 4 tensile test piece made of the polyamide resin composition of the present invention is preferably less than 90%, and particularly preferably less than 80%. The lower limit is not particularly limited, and is defined as 0%.
[0044] There is no particular restriction on the method for producing the resin composition for forming the alkaline dry cell gasket of the present invention, as long as the polyamide 610 resin (A) and the polyethylene resin (B) can be melt-mixed. As a production method, melt-mixing using a twin-screw extruder is generally preferred from the perspective of productivity and mixability. As a melt-mixing method using a twin-screw extruder, for example, the following method can be cited: premixing the polyamide 610 resin (A), the polyethylene resin (B) and the components other than (A) and (B) used as required, supplying them to a twin-screw extruder whose barrel temperature is set to 230°C to 300°C, and melt-mixing them. There is no particular restriction on the mixing order of the raw materials, and any of the following methods can be used: a method of melt-mixing all the raw materials using the above method; a method of melt-mixing a part of the raw materials using the above method and further melt-mixing the remaining raw materials; or a method of using a side feeder to mix the remaining raw materials during the process of melt-mixing a part of the raw materials; and the like. As a screw structure, it is preferred to have 1 to 5 kneading areas, and when the ratio (%) of the total length of the kneading areas to the total length of the screw is expressed as (total length of the kneading areas) ÷ (total length of the screw) × 100, it is preferably 5 to 40%. It is also preferred to adopt a method of exposing the extruder to a vacuum state in the middle of the extruder to remove the generated gas. The resin composition extruded after melt kneading is usually pulled out in a strand shape and processed into a pellet shape by a pelletizer.
[0045] The method for producing the alkaline dry battery gasket of the present invention is not particularly limited as long as it is a common thermoplastic resin processing method, but generally, it is preferable to use an injection molding method which has high dimensional accuracy of the product and excellent productivity.
[0046] Example
[0047] The present invention is specifically described below with reference to the following examples. It should be noted that the present invention is not limited to the following examples. The evaluation methods of various properties in the examples are as follows.
[0048] (1) Density of gasket
[0049] Using an alkaline dry cell gasket obtained by injection molding at a cylinder temperature of the melting point of the polyamide resin + 50°C, the measurement was performed by a density gradient tube method using a specific gravity liquid prepared from carbon tetrachloride and toluene.
[0050] (2) Melting point of gasket
[0051] The measurement was performed using a differential scanning calorimeter (product number: DSC8000) manufactured by Parkin Elmer Inc. using an alkaline dry battery gasket obtained by injection molding at a cylinder temperature of the melting point of the polyamide resin + 50°C.
[0052] (3) Average dispersion diameter of the dispersed phase
[0053] The cross-sectional center of an ASTM No. 4 tensile test piece (gasket test piece) obtained by injection molding at a cylinder temperature of the melting point of the polyamide resin + 50°C was cut into 1-2 mm squares, and the polyamide resin was stained with phosphotungstic acid and osmium, and then cut into ultrathin sections of less than 0.1 μm (about 80 nm) at -196°C using an ultrathin slicer, and observed using a Hitachi transmission electron microscope (model: H-7100) magnified to 5000 times. The obtained image was analyzed using the analysis software "Image-Pro" manufactured by Japan Roper, and the white area was regarded as the polyethylene phase, and the "area length" was regarded as the average dispersion diameter of the dispersed phase.
[0054] (4) Transparency
[0055] The haze (turbidity) of ASTM No. 4 tensile test pieces obtained by injection molding at a cylinder temperature of the melting point of the polyamide resin + 50°C was measured using a direct-reading haze meter manufactured by Toyo Seiki Seisaku-sho. When the haze was less than 80%, the transparency was judged to be very good (indicated by ◎ in the table), when the haze was 80% or more and less than 90%, the transparency was judged to be good (indicated by ○ in the table), and when the haze was 90% or more, the transparency was judged to be poor (indicated by × in the table).
[0056] (5) Appearance of molded products
[0057] The alkaline dry battery gasket obtained by injection molding at a cylinder temperature of the melting point of the polyamide resin + 50° C. was visually checked and evaluated based on the presence or absence of whitening due to peeling.
[0058] (6) Breaking strength
[0059] For an alkaline dry cell gasket having a thin wall thickness of 0.25 mm obtained by injection molding at a cylinder temperature of the melting point of the polyamide resin + 50°C, an internal pressure was applied to the gasket using compressed air using a dedicated breaking pressure measuring instrument, and the pressure gauge display value at the time when the thin wall portion of the gasket was at its highest just before it broke was recorded as the bursting strength. The value measured within 1 hour after molding the gasket was taken as the absolute dry bursting strength (a), and the value measured after immersing the gasket in hot water at 80°C for 1 hour to absorb water and then naturally drying it in the air for 1 hour was taken as the bursting strength after water absorption (b). The absolute dry / water absorption strength difference was calculated by (a)-(b), and the strength reduction rate due to water absorption was calculated by the formula {(a)-(b)} / (a)×100(%).
[0060] (7) Alkali resistance
[0061] For ASTM No. 4 tensile test pieces (gasket test pieces) obtained by injection molding at a cylinder temperature of the melting point of the polyamide resin + 50°C, tensile tests were carried out before and after immersion treatment in a 25% KOH aqueous solution at 70°C × 10 weeks. If the tensile strength after immersion is 75% or more compared with that before immersion, it is recorded as good (indicated by 0 in the table), and if it is less than 75%, it is recorded as poor (indicated by × in the table).
[0062] In addition, each raw material of the resin composition used in Examples and Comparative Examples is as follows.
[0063] (A-1) A polyamide 610 resin having a melting point of 221° C. and a viscosity of 112 ml / g as measured in accordance with JIS K 6933 (2013).
[0064] (A-2) A polyamide 610 resin having a melting point of 221° C. and a viscosity of 98 ml / g as measured in accordance with JIS K 6933 (2013).
[0065] (A-3) A polyamide 610 resin having a melting point of 221° C. and a viscosity of 78 ml / g as measured in accordance with JIS K 6933 (2013).
[0066] (A-4) A polyamide 610 resin having a melting point of 221° C. and a viscosity of 132 ml / g as measured in accordance with JIS K 6933 (2013).
[0067] (B1-1) density is 960kg / m 3 , an acid-modified polyethylene resin "Admer HE810" (manufactured by Mitsui Chemicals, Inc.) having an acid value of 7.4 mgKOH / g.
[0068] (B2-1) Density: 960kg / m 3 The high-density polyethylene resin "Hakusui" 1300J (manufactured by Huraman Co., Ltd.).
[0069] (B2-2) density is 910kg / m 3 Linear low-density polyethylene resin ""Eroman" SP1071" (manufactured by Boroman Co., Ltd.).
[0070] (B2-3) Density: 920kg / m 3 Low-density polyethylene resin "UBE J-1019" (manufactured by Ube Industries, Ltd.).
[0071] (C-1) A polyamide 612 resin having a melting point of 215° C. and a viscosity of 88 ml / g as measured in accordance with JIS K 6933 (2013).
[0072] (C-2) A polyamide 66 resin having a melting point of 262° C. and a viscosity of 112 ml / g as measured in accordance with JIS K 6933 (2013).
[0073] (C-3) A polyamide 11 resin having a melting point of 189° C. and a viscosity of 110 ml / g as measured in accordance with JIS K 6933 (2013).
[0074] (D-1) Block copolymer resin of propylene and ethylene ""Huraman E702MG" (manufactured by Harman Co., Ltd.).
[0075] (D-2) Polypropylene resin ""Hurler E111G" (manufactured by Handler Co., Ltd.).
[0076] (E-1) Crystal nucleating agent: Talc "Microtech #7000" (manufactured by Hayashi Kasei Co., Ltd.).
[0077] (E-2) Crystal nucleating agent: magnesium silicate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0078] (F-1) Release agent: "Loxiol G78" (manufactured by Emirac)
[0079] (F-2) Mold release agent: magnesium stearate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0080] (G-1) Maleic anhydride "M0005" (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0081] (G-2) Free radical generator "Sanperox TY-1.3-8" (manufactured by Sanken Chemical Industry)
[0082] (Examples 1 to 9, Comparative Examples 1 to 4, 7 to 12)
[0083] The raw materials were added from the raw material supply port upstream of the twin-screw extruder according to the composition shown in Tables 1 and 2, melt-kneaded, and the extruded strands were granulated to obtain a granular resin composition. The twin-screw extruder used TEX30α manufactured by Japan Steel Works, Ltd., and melt-kneaded under the conditions of a barrel temperature of 260°C, a screw speed of 200 rpm, and a discharge rate of 40 kg / hr. After the pellets of the obtained resin composition were vacuum dried at 80°C for more than 12 hours, they were injection molded under the conditions of a barrel temperature: melting point + 50°C, and a mold temperature: 80°C to obtain an alkaline dry cell gasket. In addition, under the same conditions, another mold was used to obtain an ASTM No. 4 tensile test piece. Using the obtained gasket, density measurement, melting point measurement, molded product appearance confirmation, and burst strength measurement were carried out. Using the ASTM No. 4 tensile test piece, the average dispersion diameter measurement, transparency measurement, and alkali resistance evaluation using transmission electron tomography were implemented.
[0084] (Comparative Example 5)
[0085] Melt kneading, injection molding and evaluation were carried out in the same manner as in Example 1 except that the cylinder temperature was set at 280°C for melt kneading.
[0086] (Comparative Example 6)
[0087] Melt kneading, injection molding and evaluation were carried out in the same manner as in Example 1 except that the cylinder temperature was set at 230°C for melt kneading.
[0088] In Examples 1 to 9, gaskets with excellent lightness, good dispersion of polyethylene resin in polyamide 610 resin, and excellent transparency and molded product appearance were obtained. In addition, the obtained gaskets had little change in burst strength between absolute dryness and water absorption, and excellent alkali resistance.
[0089] It is found that the gasket of Comparative Example 1 has a large change in burst strength due to water absorption, and the stability of the operating pressure of the safety valve is inferior to that of the example.
[0090] The polyethylenes in Comparative Examples 2 to 4 had large average dispersion diameters, and their transparency was deteriorated compared to that in the Examples, and poor appearance due to phase separation occurred on the surface of the obtained gaskets.
[0091] Comparative Example 5 was inferior in transparency and alkali resistance compared with Example 2, and Comparative Example 6 was also inferior in heat resistance and transparency compared with Example 2. Comparative Example 7 was inferior in the reduction rate of chipping strength due to water absorption.
[0092] Comparative Example 8 had a large change in burst strength due to water absorption, and the polypropylenes of Comparative Examples 9 and 10 had large dispersion diameters, and the transparency and appearance of the molded products were deteriorated compared to the Examples.
[0093] It is found that the transparency of Comparative Examples 11 and 12 is deteriorated compared with that of the Example.
[0094] As described above, it can be seen that the gaskets obtained from the resin compositions of Examples 1 to 9 are excellent in lightness, transparency and appearance of the molded products, and are also excellent in alkali resistance and heat resistance. In addition, it can be seen that the difference in burst strength between the absolute dry state and the state of water absorption is small, and when the alkaline dry cell is prepared, the stability of the operating pressure of the safety valve is high.
[0095] [Table 1]
[0096]
[0097] [Table 2]
[0098]
Claims
1. An alkaline dry cell gasket, comprising a resin composition, wherein the total amount of polyamide 610 resin (A) and polyethylene resin (B) is 100 parts by weight, and the polyamide 610 resin (A) is 70 to 95 parts by weight and the polyethylene resin (B) is 5 to 30 parts by weight. The resin composition is observed by transmission electron tomography, wherein the polyamide 610 resin (A) forms a continuous phase, the polyethylene resin (B) forms a dispersed phase, and the average dispersion diameter of the dispersed phase is 1 nm or more and 1000 nm or less. The polyethylene resin (B) is a mixture of an acid-modified polyethylene resin (B1) and an unmodified polyethylene resin (B2), The density of the acid-modified polyethylene resin (B1) and the unmodified polyethylene resin (B2) is 940 kg / m 3 Above and 980kg / m 3 the following. 2 . The alkaline dry battery gasket according to claim 1 , wherein the viscosity of the polyamide 610 resin (A) measured in accordance with JIS K 6933 (2013) is in the range of 70 ml / g or more and less than 120 ml / g.