Temperature-responsive material and light-shielding material using same
A temperature-responsive material with a polymer and nanopolysaccharide ensures uniform transparency changes, addressing the non-uniformity issue in conventional materials, providing effective light and heat control.
Patent Information
- Application Number
- JP2020083233
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-11
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-05-11
AI Technical Summary
Conventional temperature-sensitive light-shielding materials using temperature-responsive polymers do not uniformly change transparency in response to temperature changes, leading to issues with uniform light and heat control.
A temperature-responsive material comprising a temperature-responsive polymer with a lower critical solution temperature (LCST) and a nanopolysaccharide with water-retentive properties, optionally including a near-infrared absorbing material, is disposed between transparent plates to ensure uniform transparency changes based on temperature.
The material achieves uniform transparency transitions, effectively blocking light and heat by becoming cloudy or transparent at specific temperatures, enhancing light and heat management without cracking.
Smart Images

Figure 0007565512000003 
Figure 0007565512000004 
Figure 0007565512000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a temperature responsive material whose transparency changes depending on temperature, and a light-shielding material using this temperature responsive material. [Background technology]
[0002] In recent years, instead of mechanical methods, light-controlling glass has been proposed that uses composite glass incorporating functional materials to reversibly control light physicochemically. For example, liquid crystal, electrochromic, fine particle polarization orientation, photochromic, thermochromic, and other methods are available. In addition, in recent years, windows have been upgraded from the use of simple single-pane glass to the use of functional glass that has been processed with glass composition, surface treatment, multilayering, and other processes. For example, tempered glass and laminated glass that are difficult to break, double-insulating glass with thermal insulation properties, heat-absorbing glass and heat-reflecting glass that prevent solar energy from entering living spaces, and the like are used in windows. However, while heat-absorbing glass and heat-reflecting glass do indeed prevent solar energy from entering living spaces, they have the disadvantage of leaving coloration and glare on the surface, reducing the inherent colorless transparency of glass, and furthermore, from the perspective of energy saving, the control of visible light, which has about half the energy of solar light, is still insufficient.
[0003] Therefore, a thermosensitive light-shielding material has been proposed that utilizes the characteristics of a temperature-responsive polymer having a lower critical solution temperature (LCST) (see, for example, Patent Document 1). When a temperature-responsive polymer such as N-isopropylacrylamide (NIPAM) is allowed to coexist with water, it becomes hydrophilic at a temperature lower than the LCST and dissolves in water, making the thermosensitive light-shielding material transparent. In addition, when a temperature-responsive polymer is allowed to coexist with water, it becomes hydrophobic at a temperature equal to or higher than the LCST and does not dissolve in water, making the thermosensitive light-shielding material opaque and cloudy, thereby preventing the transmission of light. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 61-7948 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the thermosensitive light-shielding materials described in the above-mentioned patent documents, the temperature-responsive polymer may not become transparent or opaque uniformly in response to temperature changes.
[0006] The present invention has been proposed in view of the above-mentioned problems associated with the conventional technology, and aims to provide a temperature-responsive material that improves the uniformity of the change in transparency with temperature. [Means for solving the problem]
[0007] In order to overcome the above problems and achieve the intended object, the temperature responsive material according to the present invention comprises: a temperature-responsive polymer having a lower critical solution temperature for water; A nanopolysaccharide having water retention properties; and water.
[0008] In order to overcome the above problems and achieve the intended object, the light-shielding material according to the present invention comprises: The gist of the present invention is that the temperature responsive material according to the present invention is disposed between opposing transparent plates. Effect of the Invention
[0009] According to the temperature responsive material of the present invention, it is possible to improve the uniformity of the change in transparency in response to temperature. According to the light-shielding material of the present invention, the transparency of the temperature-responsive material changes uniformly in response to temperature, so that light and heat can be appropriately shielded. [Brief description of the drawings]
[0010] [Figure 1]1 is an image showing the change in poly(N-isopropylacrylamide) (PNIPAM) dispersed in water, (a) below the LCST and (b) above the LCST. [Diagram 2] FIG. 2 is a graph showing the relationship between drying time and water evaporation rate when a 2 wt % aqueous dispersion of nanopolysaccharide is dried at 105° C. [Diagram 3] 1 is a structural formula showing carboxymethyl cellulose nanofiber. [Figure 4] (a) is a structural formula showing chitin nanofibers, and (b) is a structural formula showing chitosan formed on the surface of (a). [Diagram 5] FIG. 2 is an explanatory diagram showing a light-blocking material using a temperature-responsive material, where (a) is at a temperature below the LCST and (b) is at a temperature above the LCST. [Figure 6] FIG. 2 is a schematic diagram showing polymerization of a temperature-responsive polymer in Example 1. [Figure 7] FIG. 2 is a schematic diagram showing polymerization of a temperature-responsive polymer in Example 2. [Figure 8] FIG. 4 is a schematic diagram showing polymerization of a temperature-responsive polymer in Example 3. [Figure 9] FIG. 1 is a graph showing the results of transmittance measurement and particle size measurement of the temperature responsive material of Example 4 and the temperature responsive material of Comparative Example 1. [Figure 10] FIG. 1 is a graph showing the results of a water retention test. [Figure 11] FIG. 13 is a graph showing the results of transmittance measurement and particle size measurement of the temperature responsive material of Example 5 and the temperature responsive material of Comparative Example 1. [Figure 12] FIG. 13 is a graph showing the results of transmittance measurement and particle size measurement of the temperature responsive material of Example 6 and the temperature responsive material of Comparative Example 2. [Figure 13] FIG. 13 is a graph showing the results of transmittance measurement and particle size measurement of the temperature responsive material of Example 7 and the temperature responsive material of Comparative Example 3. [Figure 14] FIG. 13 is a graph showing the results of transmittance measurement and particle size measurement of the temperature responsive material of Example 8 and the temperature responsive material of Comparative Example 1. [Figure 15] FIG. 2 is an explanatory diagram showing a light-shielding material. [Figure 16] FIG. 2 is an explanatory diagram showing a temperature suppression effect measuring device. [Figure 17] FIG. 13 is a graph showing the measurement results of the temperature suppression effect of the light-shielding material of Example 5. [Figure 18] FIG. 13 is a graph showing the measurement results of the temperature suppression effect of the light-shielding material of Example 6. [Figure 19] FIG. 13 is a graph showing the measurement results of the temperature suppression effect of the light-shielding material of Example 7. [Figure 20] FIG. 13 is a graph showing the measurement results of the temperature suppression effect of the light-shielding materials of Examples 9 and 12. [Figure 21] FIG. 13 is a graph showing the measurement results of the temperature suppression effect of the light-shielding materials of Examples 10 and 13. [Figure 22] FIG. 13 is a graph showing the measurement results of the temperature suppression effect of the light-shielding materials of Examples 11 and 14. [Diagram 23] 1 is a photograph showing the clouding of the light-shielding material of Example 13. [Figure 24] 13 is a photograph showing the clouding of the light-shielding material of Comparative Example 1. [Diagram 25] 1 is a photograph showing the clouding of the light-shielding material of Example 14. [Figure 26] 13 is a photograph showing the clouding of the light-shielding material of Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] (overview) The temperature-responsive material according to the present disclosure includes a temperature-responsive polymer having an LCST with respect to water, a nanopolysaccharide having water retention, and water. The temperature-responsive material may also include a near-infrared absorbing material in addition to the temperature-responsive polymer, the nanopolysaccharide, and water. When the temperature-responsive material is equal to or higher than the LCST, the transparency of the material decreases due to clouding, etc., compared to when the temperature is below the LCST. For example, if the temperature-responsive material is used for light-shielding purposes (such as light-shielding glass) by clouding the material due to the temperature-responsive polymer in response to an increase in temperature, the material may be transparent at temperatures below the LCST and opaque when the temperature exceeds the LCST. In this way, the transparency (light transmittance) of the temperature-responsive material changes at the LCST.
[0012] (Temperature-responsive polymers) Temperature-responsive polymers have the property that they dissolve in water at temperatures lower than the LCST, but are insoluble in water above the LCST. For example, in the case of poly(N-isopropylacrylamide) (PNIPAM), a representative temperature-responsive polymer, at temperatures below the LCST, the polymer chains are hydrated and stretched due to hydrogen bonds between the amide groups and water, forming a random coil shape as shown in Figure 1(a). At temperatures above the LCST, the hydrogen bonds between the amide groups and water become unstable, causing dehydration of the hydrophobic parts. This hydrophobic effect causes the polymer chains to aggregate into a globular state, as shown in Figure 1(b).
[0013] The temperature-responsive polymer may be a non-ionic hydrophilic (water-soluble) polymer. Specifically, for example, poly(meth)acrylamide derivatives, polyvinylamide derivatives, polyvinyl methyl ether, cellulose derivatives, etc. may be used. Other examples include polyoxazolidones, polyalkylene oxides, polyvinyl alcohols, polymethacrylic acid, and derivatives thereof. Furthermore, the temperature-responsive polymer may be a polyethylene glycol / polypropylene glycol block copolymer. For example, polyvinyl alcohol derivatives may be partial acetoacetal compounds, partial formal compounds, partial butyral compounds, etc. of polyvinyl alcohol.
[0014] (Poly(meth)acrylamide derivatives) Examples of poly(meth)acrylamide derivatives include poly N-substituted (meth)acrylamide derivatives. Examples of N-substituted (meth)acrylamide include polymers obtained by polymerizing N-cyclopropyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, Nn-propyl(meth)acrylamide, N-methyl-N-ethylacrylamide, N-methyl-N-isopropylacrylamide, N-methyl-Nn-propylacrylamide, N,N-diethylacrylamide, N-acryloylpiperidine, N-acryloylpyrrolidine, and N-tetrahydrofuryl acrylamide. Examples of poly(meth)acrylamide derivatives include poly(meth)acrylamide copolymers obtained by copolymerizing multiple types of (meth)acrylamides or (meth)acrylamide with other monomers.
[0015] (Polyvinylamide derivatives) Examples of polyvinylamide derivatives include polymers obtained by polymerizing N-vinylformamide, N-vinylacetamide, N-vinyl-N-methylacetamide, N-vinyl-N-methylformamide, N-vinylpropionamide, etc. Preferred are N-vinylacetamide and N-vinyl-N-methylacetamide. In addition, the polyvinylamide derivative may be a polyvinylamide copolymer obtained by copolymerizing multiple types of vinylamide monomers or a vinylamide monomer with another monomer.
[0016] (Cellulose derivatives) As the cellulose derivative, for example, alkyl-substituted cellulose derivatives such as methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, and hydroxyethyl methyl cellulose can be used.
[0017] Each temperature-responsive polymer has its own LCST. If the temperature-responsive material is used for light-shielding purposes (light-shielding glass) by making the material opaque (opaque) with the temperature-responsive polymer in response to an increase in temperature, a temperature-responsive polymer having an LCST between 25°C and 45°C may be used. In this way, a temperature-responsive polymer having a required LCST may be selected as the temperature-responsive material depending on the application and the required function. For example, examples of temperature-responsive polymers having an LCST between 30°C and 40°C include derivatives (copolymers) obtained from N-isopropyl(meth)acrylamide, N-cyclopropyl(meth)acrylamide, N-ethylacrylamide, N-methyl-N-ethylacrylamide, N,N-diethylacrylamide, N-acryloylpyrrolidine, etc., and polyvinyl methyl ether.
[0018] (Size of temperature-responsive polymer) The particle size of the temperature-responsive polymer is preferably in the range of 1 nm to 1000 nm, more preferably 20 nm to 500 nm. When the particle size of the temperature-responsive polymer is in the above-mentioned range at or below the LCST, it is preferable because it shows appropriate temperature responsiveness and can ensure transparency by suppressing turbidity. Furthermore, the particle size of the temperature-responsive polymer is preferably in the range of 200 nm to 50 μm at a temperature above the LCST, more preferably 300 nm to 35 μm. When the particle size of the temperature-responsive polymer is in the above-mentioned range at a temperature above the LCST, it is preferable because it can ensure suitable light-shielding properties such that the light transmittance at a wavelength of 700 nm is 60% or less, and turbidity progresses uniformly, preventing cracks in the temperature-responsive material.
[0019] (LCST control) The LCST of a temperature-responsive polymer capable of producing a copolymer such as a poly(meth)acrylamide derivative or a polyvinylamide derivative can be controlled by the monomer unit introduced into poly(meth)acrylamide or polyvinylamide. For example, when a hydrophobic monomer unit is introduced into poly(meth)acrylamide to produce a copolymer, the LCST is lowered if the polarity of the resulting temperature-responsive polymer is made more hydrophobic than that of poly(meth)acrylamide. When a hydrophilic monomer unit is introduced into poly(meth)acrylamide to produce a copolymer, the LCST is raised if the polarity of the resulting temperature-responsive polymer is made more hydrophilic than that of poly(meth)acrylamide. This effect is the same as that of a poly(meth)acrylamide polymer even in the case of a polyvinylamide copolymer.
[0020] (Amount of temperature-responsive polymer) In the temperature-responsive material, the concentration of the temperature-responsive polymer is preferably in the range of 0.05 wt% to 10 wt%, more preferably 0.1 wt% to 1.0 wt%. When the concentration of the temperature-responsive polymer in the temperature-responsive material is in the above-mentioned range, when the material becomes cloudy at a temperature above the LCST, the light transmittance at a wavelength of 700 nm becomes less than 60%, and a suitable light-shielding effect can be obtained. In addition, when the concentration of the temperature-responsive polymer in the temperature-responsive material is in the above-mentioned range, the viscosity of the temperature-responsive material can be made appropriate, making it easier to form a film of the temperature-responsive material.
[0021] (polysaccharide) The polysaccharides used are those having water retention properties. In addition, the polysaccharides are preferably poorly water-soluble, i.e., hardly soluble in water or insoluble in water. Examples of the polysaccharides having water retention properties include cellulose, chitin, chitosan, glucomannan, pullulan, starch, agarose, dextran, and sacran, and may be salts or derivatives of these polysaccharides. Furthermore, when the temperature-responsive material is used for light-shielding purposes, the polysaccharides are preferably those having high transparency when dispersed in water, and examples of such polysaccharides having high transparency include chitin, chitin deacetylation products, carboxymethylcellulose, TEMPO oxidized cellulose, sulfated cellulose, and phosphorylated cellulose.
[0022] (Polysaccharide size) The polysaccharides used are so-called nanopolysaccharides, which are nano-sized with an average fiber width in the range of 1 nm to 999 nm. Nanopolysaccharides have excellent water retention properties, so when used in a temperature-responsive material, they can supply sufficient water to the temperature-responsive polymer. Among these, it is preferable to use polysaccharide nanofibers with an average fiber width in the range of 4 nm to 100 nm and an average fiber length of 5 μm or more, or polysaccharide nanocrystals with an average fiber width in the range of 4 nm to 50 nm and an average fiber length in the range of 100 nm to 400 nm.
[0023] (Water retention of polysaccharides) Nanopolysaccharides have been shown to have higher water retention than non-fibrillated polysaccharides (Reference: Kota Ogura, "Development of high-value-added composite materials by adding cellulose nanofibers", Defibration of cellulose nanofibers, improvement of dispersibility in resin and development of composite materials, Technical Information Association, November 14, 2019, p.1-41). For example, when a 2 wt% aqueous dispersion of nanopolysaccharides and non-fibrillated polysaccharides is dried at 105°C, the residual mass rate of non-fibrillated polysaccharides is 5 wt% after about 57 minutes of heating, while the residual mass rate of highly defibrated nanopolysaccharides is 5 wt% after 70 minutes of heating. Nanopolysaccharides have a larger specific surface area and an increased amount of hydroxyl groups in contact with water, which improves water retention through hydrogen bonding. In addition, the shorter the fiber length of nanopolysaccharides, the larger the specific surface area and the higher the water absorption.
[0024] FIG. 2 shows the relationship between the drying time and the water evaporation rate when a 2 wt% aqueous dispersion of nanopolysaccharides and unfibrillated polysaccharides is dried at 105°C. Circle 1 is chitin nanofiber, circle 2 is carboxymethylcellulose nanofiber, circle 3 is cellulose nanofiber, circle 4 is chitosan nanofiber, and circle 5 is cellulose (unfibrillated). As shown in FIG. 2, among nanopolysaccharides, chitin nanofibers and carboxymethylcellulose nanofibers have high water retention. For this reason, chitin nanofibers and carboxymethylcellulose nanofibers are preferred as polysaccharides to be used in temperature-responsive materials because of their high water retention and high dispersion transparency.
[0025] In order to perform reversible switching from transparent to opaque at the LCST of the temperature-responsive polymer, the nanopolysaccharide must be transparent. Examples of nanopolysaccharides that have been modified with cellulose nanofibers to increase hydrophilicity and improve transparency include carboxymethylcellulose, TEMPO-oxidized cellulose, sulfated cellulose, and phosphorylated cellulose, which are compatible with temperature-responsive polymers in light- and heat-shielding applications.
[0026] As shown in Figure 3, the hydroxyl group at the C6 position of carboxymethyl cellulose nanofibers has a negative charge in water, so that the osmotic pressure effect causes nano-dispersion down to the microfibril unit, and in that state the nano-dispersed state can be stably maintained in water due to the charge repulsion between the microfibrils.
[0027] Since the chitin shown in Figure 4(a) is white, it is preferable to deacetylate the surface of the chitin to make it chitosan (see Figure 4(b)). In the case of deacetylated chitin nanofibers with such a surface converted to chitosan, adding lactic acid and making the pH acidic makes the amino groups of the chitosan on the surface cationic, dispersing due to charge repulsion and making it translucent. In addition, the charge repulsion can suppress hydrogen bonding between chitin amides and promote hydrogen bonding with water.
[0028] (Polysaccharide content) The polysaccharide concentration in the temperature-responsive material is preferably in the range of 0.02 wt% to 10 wt%, more preferably in the range of 0.1 wt% to 1.0 wt%. When the polysaccharide concentration in the temperature-responsive material is in this range, water can be appropriately retained and the temperature-responsive material can have an appropriate viscosity of more than 3.0 mPa s, making it easy to form a film. Furthermore, when the polysaccharide concentration in the temperature-responsive material is in this range, the appropriate viscosity can be achieved and the reversible cloudiness of the temperature-responsive polymer can be appropriately expressed.
[0029] (Near infrared absorbing material) The temperature-responsive material may contain one or more near-infrared absorbing materials that absorb infrared rays. As the near-infrared absorbing material, one that has excellent near-infrared absorbing properties is preferable. As the near-infrared absorbing material, for example, thiophene and its derivatives, conductive polymers doped with polyanions, and semiconductor materials can be mentioned. Among these, thiophene and its derivatives, and conductive polymers doped with polyanions are more preferable than semiconductor materials, taking into consideration environmental loads and costs. In addition, as the semiconductor material, for example, indium tin oxide (ITO), antimony tin oxide (ATO), lanthanum hexaboride (LaB6), cesium tungsten oxide (CWO), etc. can be used.
[0030] As the conductive polymer, a π-conjugated conductive polymer that is unsubstituted or has a functional group such as an alkyl group, a carboxy group, a sulfo group, an alkoxyl group, a hydroxyl group, or a cyano group introduced therein can be used. Examples of the conductive polymer include polypyrrole, poly(N-methylpyrrole), poly(3-methylpyrrole), poly(3-ethylpyrrole), poly(3-n-propylpyrrole), poly(3-butylpyrrole), poly(3-octylpyrrole), poly(3-decylpyrrole), poly(3-dodecylpyrrole), poly(3,4-dimethylpyrrole), poly(3,4-dibutylpyrrole), poly(3-carboxypyrrole), poly(3-methyl-4 ... Poly(ethylpyrrole), poly(3-methyl-4-carboxybutylpyrrole), poly(3-hydroxypyrrole), poly(3-methoxypyrrole), poly(3-ethoxypyrrole), poly(3-butoxypyrrole), poly(3-hexyloxypyrrole), poly(3-methyl-4-hexyloxypyrrole), poly(3-methyl-4-hexyloxypyrrole), poly(thiophene), poly(3-methylthiophene), poly(3-ethylthiophene), poly(3-propylthiophene), poly(3-butylthiophene), thiophene), poly(3-hexylthiophene), poly(3-heptylthiophene), poly(3-octylthiophene), poly(3-decylthiophene), poly(3-dodecylthiophene), poly(3-octadecylthiophene), poly(3-bromothiophene), poly(3-chlorothiophene), poly(3-iodothiophene), poly(3-cyanothiophene), poly(3-phenylthiophene), poly(3,4-dimethylthiophene), poly(3,4-dibutylthiophene), poly(3-hydroxythiophene), ), poly(3-methoxythiophene), poly(3-ethoxythiophene), poly(3-butoxythiophene), poly(3-hexyloxythiophene), poly(3-heptyloxythiophene), poly(3-octyloxythiophene), poly(3-decyloxythiophene), poly(3-dodecyloxythiophene), poly(3-octadecyloxythiophene), poly(3,4-dihydroxythiophene), poly(3,4-dimethoxythiophene), poly(3,4-diethoxythiophene), poly(3,4-dipropoxythiophene), poly(3,4-dibutoxythiophene), poly(3,4-dihexyloxythiophene), poly(3,4-diheptyloxythiophene), poly(3,4-dioctyloxythiophene), poly(3,4-didecyloxythiophene), poly(3,4-didodecyloxythiophene), poly(3,4-ethylenedioxythiophene), poly(3,4-propylenedioxythiophene), poly(3,4-butenedioxythiophene), poly Examples of the poly(3-methyl-4-methoxythiophene), poly(3-methyl-4-ethoxythiophene), poly(3-carboxythiophene), poly(3-methyl-4-carboxythiophene), poly(3-methyl-4-carboxyethylthiophene), poly(3-methyl-4-carboxybutylthiophene), polyaniline, poly(2-methylaniline), poly(3-isobutylaniline), poly(2-anilinesulfonic acid), poly(3-anilinesulfonic acid), etc. Among them, polypyrrole, polythiophene, poly(N-methylpyrrole), poly(3-methylthiophene), poly(3-methoxythiophene), poly(3,4-ethylenedioxythiophene), and (co)polymers consisting of one or more of these can be used.
[0031] As the polyanion to be doped into the conductive polymer, any anionic compound can be used without any particular restrictions. The anionic compound is a compound having an anionic group in the molecule that can cause chemical oxidation doping into the π-conjugated conductive polymer. As the anionic group, from the viewpoints of ease of production and high stability, a phosphate group, a carboxy group, a sulfonic acid group, and the like are preferred. Among these anionic groups, a sulfonic acid group or a carboxy group is more preferred because of its excellent doping effect on the π-conjugated conductive polymer.
[0032] As the near infrared absorbing material, polythiophene or polythiophene derivative doped with polyanion is preferable. For example, there is PEDOT / PSS in which polystyrene sulfonic acid (PSS) is doped into poly(3,4-ethylenedioxythiophene) (PEDOT). In addition, there may be PT / CS in which polythiophene or polythiophene derivative (hereinafter referred to as PT) is doped with sulfated cellulose nanofiber (CS) or sulfated cellulose nanocrystal (CS). For example, there is PEDOT / CS in which PEDOT is doped with CS.
[0033] (PT / CS) PT / CS contains sulfated cellulose nanofibers or sulfated cellulose nanocrystals and polythiophene doped with the sulfated cellulose nanofibers or sulfated cellulose nanocrystals. The sulfated cellulose nanofibers or sulfated cellulose nanocrystals of PT / CS are expressed as the following chemical formula 1. PT / CS is composed of sulfated cellulose nanofibers or sulfated cellulose nanocrystals as a skeleton, and polythiophene is oriented on the surface of the sulfated cellulose nanofibers or sulfated cellulose nanocrystals. PT / CS has low visible light absorption, high near-infrared absorption, and transparency, and has the properties required for a near-infrared absorbing material. PT / CS is hydrophilic and can be dispersed in water. PT / CS is easy to coat and can be given high conductivity. PT / CS does not contain environmentally unfriendly substances such as antimony and cesium, so it has a low burden on the environment, and does not use rare metals such as indium, so it can be obtained at low cost.
[0034] [ka] R shown in Chemical Formula 1 1 ~R 6each independently represents a hydrogen atom, a sulfonic acid group, or an alkylsulfonic acid group having a carbon chain number of 1 to 6, and R 1 ~R 6 At least one of the groups is a sulfonic acid group or an alkylsulfonic acid group having a carbon chain number of 1 to 6. Furthermore, n in Chemical Formula 1 indicates the repetition in the parentheses.
[0035] PT / CS is, for example, R 1 , R 2 , R 4 and R 5 is a hydrogen atom and R 3 and R 6 A specific example is a composite (PEDOT / CS) of sulfated cellulose nanofiber (CS) or sulfated cellulose nanocrystal (CS), which has sulfonic acid groups, and poly(3,4-ethylenedioxythiophene), also abbreviated as PEDOT.
[0036] (Size of near infrared absorbing material) The particle size of the near-infrared absorbing material is preferably in the range of 5 nm to 1000 nm, more preferably 20 nm to 400 nm. When the particle size of the near-infrared absorbing material is in the above range, it is preferable because a heat conduction path can be properly formed in the temperature responsive material, and the heat ray absorption performance can be improved. In addition, when the particle size of the near-infrared absorbing material is in the above range, it can be properly dispersed in water to suppress aggregation, and the temperature responsive material can be easily applied.
[0037] (Near infrared absorbing material blend amount) The concentration of the near-infrared absorbing material in the temperature-responsive material is preferably in the range of 0.001wt% to 2wt%, more preferably in the range of 0.01wt% to 0.5wt%. When the concentration of the near-infrared absorbing material in the temperature-responsive material is in the above range, a moderate heat ray absorption rate is generated, and the performance as a heat ray absorbing material can be exhibited. In addition, when the concentration of the near-infrared absorbing material in the temperature-responsive material is in the above range, coloring due to the near-infrared absorbing material can be suppressed, and transparency can be ensured at temperatures below the LCST.
[0038] (Relationship between temperature-responsive polymers and polysaccharides) The weight ratio of the temperature-responsive polymer to the polysaccharide (temperature-responsive polymer:polysaccharide) to be incorporated in the temperature-responsive material is preferably in the range of 0.5:99.5 to 99.5:0.5, more preferably in the range of 20:80 to 80:20. When in this range, the light transmittance at a wavelength of 700 nm at a temperature above the LCST becomes 50% or less, and a suitable light-shielding effect can be obtained. Furthermore, when the weight ratio of the temperature-responsive polymer to the polysaccharide to be incorporated in the temperature-responsive material is in the above range, the polysaccharide can appropriately retain water.
[0039] (Relationship between near-infrared absorbing materials and temperature-responsive polymers) The weight ratio of the near-infrared absorbing material and the temperature-responsive polymer (near-infrared absorbing material: temperature-responsive polymer) to be mixed in the temperature-responsive material is preferably in the range of 0.1:99.9 to 99.9:0.1, more preferably in the range of 0.5:99.5 to 99.5:0.5. When the weight ratio of the near-infrared absorbing material and the temperature-responsive polymer to be mixed in the temperature-responsive material is in the above range, a moderate heat ray absorption rate is generated, and the performance as a heat ray absorbing material can be exhibited. In addition, when the concentration of the near-infrared absorbing material in the temperature-responsive material is in the above range, the light transmittance at a wavelength of 700 nm at a temperature below the LCST exceeds 50%, and transparency can be ensured.
[0040] (Relationship between near-infrared absorbing materials and polysaccharides) The ratio of the near-infrared absorbing material to the mixture of the temperature-responsive polymer and the nanopolysaccharide (temperature-responsive polymer + nanopolysaccharide: near-infrared absorbing material (weight ratio)) is preferably in the range of 0.1:99.9 to 99.9:0.1, more preferably in the range of 0.5:99.5 to 99.5:0.5. When the ratio of the near-infrared absorbing material to the mixture of the temperature-responsive polymer and the nanopolysaccharide is in the above range, a moderate heat ray absorption rate is generated, and the performance as a heat ray absorbing material can be exhibited. In addition, when the ratio of the near-infrared absorbing material to the mixture of the temperature-responsive polymer and the nanopolysaccharide is in the above range, the light transmittance at a wavelength of 700 nm at a temperature below the LCST exceeds 50%, and transparency can be ensured.
[0041] Among temperature-responsive polymers, PNIPAM or NIPAM-acrylamide derivative copolymers become cloudy in a narrow temperature range at LCST when the temperature is increased from room temperature. Combining them with near-infrared absorbing materials, PEDOT / PSS or PEDOT / CS, accelerates the rate of clouding, making them the most preferable temperature-responsive materials. PEDOT / PSS and PEDOT / CS are dispersed in water in a colloidal state and can be easily mixed with an aqueous solution of NIPAM or NIPAM copolymer.
[0042] A combination of carboxymethylcellulose, TEMPO oxidized cellulose, cellulose sulfate, cellulose phosphorylated, and chitin deacetylated products as nanopolysaccharides with high water retention and PEDOT / PSS or PEDOT / CS as near-infrared absorbing materials is preferred. The nanopolysaccharides carboxymethylcellulose, TEMPO oxidized cellulose, cellulose sulfate, cellulose phosphorylated, and chitin deacetylated products are highly transparent, and maintain their transparency even when mixed with the near-infrared absorbing materials PEDOT / PSS or PEDOT / CS.
[0043] (Method of manufacturing temperature-responsive material) The aqueous solution of the temperature-responsive polymer can be prepared by preparing an aqueous solution of the temperature-responsive monomer, adding a polymerization initiator while bubbling nitrogen, carrying out a polymerization reaction, and then purifying the solution. The polymerization method may be any method that can polymerize the polymer, such as redox polymerization, gamma-ray polymerization, thermal polymerization, solution polymerization, emulsion polymerization, suspension polymerization, etc., and is not particularly limited. The purification method may be any method that can purify the polymer, such as dialysis, precipitation, etc., and is not particularly limited.
[0044] The temperature-responsive material is prepared by mixing a temperature-responsive polymer, a nanopolysaccharide, and, if necessary, a near-infrared absorbing material. The mixing of the solutions can be carried out regardless of the temperature condition, whether below or above the LCST of the temperature-responsive polymer.
[0045] (Effects of temperature-responsive materials) When the temperature of the temperature-responsive material is below the LCST, the polysaccharides, which have water retention properties, hold the water in which the temperature-responsive polymer is dissolved, preventing the evaporation of water. When the temperature of the temperature-responsive material rises above the LCST, the water in which the temperature-responsive polymer is dissolved is held by the polysaccharides, making it easier for the temperature-responsive polymer to separate from the water and inducing the insolubilization of the temperature-responsive polymer. This causes the temperature-responsive material to become uniformly cloudy. When the temperature of the temperature-responsive material is above the LCST, the polysaccharides hold the water, preventing the evaporation of water. When the temperature of the temperature-responsive material falls below the LCST, the temperature-responsive polymer dissolves in the water held by the polysaccharides, inducing the temperature-responsive polymer to become water-soluble. This causes the temperature-responsive material to become uniformly transparent.
[0046] In this way, the temperature-responsive material retains water due to the water-retentive polysaccharides, so the amount of water does not change, and water can be supplied sufficiently during the dissolution and precipitation of the temperature-responsive polymer according to the LCST. Therefore, the temperature-responsive material becomes transparent or opaque uniformly with good response speed. Furthermore, defects such as the temperature-responsive material appearing to be cracked can be avoided.
[0047] (shading material) A light-shielding material can be constructed by applying a temperature-responsive material onto a transparent material such as a glass plate, a resin plate, or a transparent film, and arranging two transparent materials facing each other with the temperature-responsive material between them. For example, as shown in FIG. 5, a light-shielding material 10 includes two transparent materials 12, 12 arranged facing each other, and a temperature-responsive material 14 arranged between the two transparent materials 12, 12. In addition, the light-shielding material 10 includes a spacer 16 arranged between the two transparent materials 12, 12 so as to surround the temperature-responsive material 14. In this way, the light-shielding material 10 includes a temperature-responsive material 14 formed in a thin film shape arranged in a closed space surrounded by the transparent materials 12 and the spacer 16.
[0048] In the light-shielding material 10, the temperature-responsive polymer dissolves in water at a temperature equal to or lower than the LCST, so that the temperature-responsive material 14 becomes transparent and allows light to pass through. As a result, the light-shielding material 10 can moderately transmit light to ensure brightness and increase temperature at low temperatures equal to or lower than the LCST. In contrast, the light-shielding material 10 can moderately restrict light transmission at temperatures higher than the LCST, so that the temperature-responsive material 14 becomes opaque and restricts light transmission. As a result, the light-shielding material 10 can moderately restrict light transmission at high temperatures higher than the LCST, so that it can block temperature increases and reduce glare. In the light-shielding material 10, the temperature-responsive material 14 becomes transparent or opaque uniformly with a good response speed, so that the light-transmitting state and the light-shielding state can be switched quickly and uniformly. In addition, the light-shielding material 10 can avoid defects in which the temperature-responsive material 14 appears to be cracked.
[0049] Next, the temperature responsive material and the light shielding material according to the present invention will be described below with reference to preferred examples. EXAMPLES
[0050] (LCST control) In a three-neck flask, 15.0 g (0.133 mol) of NIPAM was dissolved in 100 ml of water while stirring. 1.9 ml (14.7 mmol) of TMED was added as a polymerization promoter, and nitrogen replacement was performed in an ice bath (5°C). 303 mg (1.33 mmol) of APS dissolved in 20 ml of water was added as a polymerization initiator, and the reaction was performed for 3 hours in an ice bath. As a result, a transparent reaction solution with high viscosity was obtained, so the reaction solution was diluted with ion-exchanged water and dialyzed with a 12-14 kDa dialysis membrane for 3 days. As shown in FIG. 6, NIPAM was polymerized to obtain PNIPAM (temperature-responsive polymer of Example 1).
[0051] In a three-neck flask, 14.25 g (0.126 mol) of NIPAM was dissolved in 100 ml of water while stirring. 0.75 g (5.90 mmol) of DEAA was further added and stirred. 1.9 ml (14.7 mmol) of TMED was added as a polymerization promoter, and nitrogen substitution was performed under an ice bath (5°C). 303 mg (1.33 mmol) of APS dissolved in 20 ml of water was added as a polymerization initiator, and the reaction was performed for 3 hours under an ice bath. As a result, a transparent and highly viscous reaction solution was obtained, so the reaction solution was diluted with ion-exchanged water and dialyzed with a 12-14 kDa dialysis membrane for 3 days. As shown in FIG. 7, NIPAM and DEAA were copolymerized to obtain a Poly(NIPAM-co-DEAA) polymer (temperature-responsive polymer of Example 2).
[0052] In a three-neck flask, 14.25 g (0.126 mol) of NIPAM was dissolved in 100 ml of water while stirring. Furthermore, 0.75 g (6.51 mmol) of HEAA was added and stirred. 1.9 ml (14.7 mmol) of TMED was added as a polymerization promoter, and nitrogen substitution was performed under an ice bath (5°C). 303 mg (1.33 mmol) of APS dissolved in 20 ml of water was added as a polymerization initiator, and the reaction was performed for 3 hours under an ice bath. As a result, a transparent and highly viscous reaction solution was obtained, so the reaction solution was diluted with ion-exchanged water and dialyzed with a 12-14 kDa dialysis membrane for 3 days. As shown in FIG. 8, NIPAM and HEAA were copolymerized to obtain a Poly(NIPAM-co-HEAA) polymer (temperature-responsive polymer of Example 3).
[0053] In the examples, the following reagents are used. N-isopropylacrylamide (NIPAM): KJ Chemicals Co., Ltd. Trimethylethylenediamine (TMED): manufactured by Tokyo Chemical Industry Co., Ltd. Ammonium peroxodisulfate (APS): Wako Pure Chemical Industries, Ltd. Diethylacrylamide (DEAA): KJ Chemicals Co., Ltd. Hydroxyethylacrylamide (HEAA): KJ Chemicals Co., Ltd. Lithium bromide: Nacalai Tesque, Inc. Carboxymethyl cellulose (CM-CNF or CMC): manufactured by Sugino Machine Co., Ltd. Chitin / chitosan nanofiber (chitin deacetylated nanofiber): manufactured by Marine Nanofiber Co., Ltd.
[0054] (composite with polysaccharides) In a three-neck flask, NIPAM (2.1 g) and CM-CNF (105.0 g) were dissolved in 172.9 ml of water, TMED (0.266 ml) was added as a polymerization accelerator, and nitrogen replacement was performed under an ice bath (5 ° C). APS (0.126 mg) dissolved in 20 ml of water was added as a polymerization initiator, and the reaction was performed for 3 hours under an ice bath. As a result, a transparent and highly viscous reaction solution was obtained, so the reaction solution was diluted with ion-exchanged water and dialyzed with a 12-14 kDa dialysis membrane for 3 days. In this way, NIPAM was polymerized in the presence of polysaccharides to polymerize PNIPAM, and the temperature-responsive material of Example 4 was obtained.
[0055] (Temperature-responsive materials of Examples 5 to 7) The temperature-responsive polymer of Example 1 (0.5 g), CM-CNF (0.5 g), and water (99 ml) were mixed to prepare the temperature-responsive material of Example 5. The temperature-responsive polymer of Example 2 (0.5 g), CM-CNF (0.5 g), and water (99 ml) were mixed to prepare the temperature-responsive material of Example 6. The temperature-responsive polymer of Example 3 (0.5 g), CM-CNF (0.5 g), and water (99 ml) were mixed to prepare the temperature-responsive material of Example 7.
[0056] (Temperature-responsive materials of Comparative Examples 1 to 3) The temperature-responsive polymer of Example 1 (0.5 g) and water (99.5 ml) were mixed to prepare a temperature-responsive material of Comparative Example 1. The temperature responsive polymer of Example 2 (0.5 g) and water (99.5 ml) were mixed to prepare a temperature responsive material of Comparative Example 2. The temperature responsive polymer of Example 3 (0.5 g) and water (99.5 ml) were mixed to prepare a temperature responsive material of Comparative Example 3.
[0057] The temperature-responsive material of Example 4 and the temperature-responsive material of Comparative Example 1 (temperature-responsive polymer of Example 1) were measured for light transmittance using an ultraviolet-visible spectrophotometer (V-670, Spectrophotometer, manufactured by JASCO), and particle size was measured by dynamic light scattering (DLS) using a dynamic light scattering meter (Malvern, Zetasizer Nano ZS) to confirm the LCST. The temperature was raised from 20°C to 40°C in increments of 2°C for each measurement. For the light transmittance measurement, the transmittance at 700nm was plotted to see the turbidity at a certain wavelength. The results are shown in FIG. 9. As a result, in the light transmittance measurement, the transmittance at a wavelength of 700nm decreased from 92.1% to 30.8% from 32°C to 34°C. On the other hand, the results of DLS showed that the particle size increased from 303nm to 4320nm from 32°C to 34°C, and therefore it was found that the LCST of Example 4 was 34°C. In addition, since the transmittance at a wavelength of 700 nm did not decrease significantly compared to Comparative Example 1, it is believed that the aggregation of PNIPAM can be suppressed by forming a composite.
[0058] For Example 7 and Comparative Example 3, the water retention was compared based on the relationship between drying time and water evaporation rate when dried at 105°C. The results are shown in Figure 10. It can be seen that the water retention is higher in Example 7 than in the corresponding Comparative Example 3. In addition, CM-CNF has three hydroxyl groups per glucose unit, and therefore exhibits high water retention. This is thought to be because HEAA has hydroxyl groups, and at temperatures above the LCST, it gathers like micelles due to the hydrophobic effect of the hydrophobic part of Poly(NIPAM-co-HEAA), the temperature-responsive polymer of Example 3, and the hydrophilic part becomes exposed, making it easier to release water.
[0059] For the temperature-responsive materials of Examples 5 to 7 and Comparative Examples 1 to 3, the light transmittance was measured using an ultraviolet-visible spectrophotometer (V-670, Spectrophotometer, manufactured by JASCO), and the particle size was measured by dynamic light scattering (DLS) using a dynamic light scattering meter (Malvern, Zetasizer Nano ZS) to confirm the LCST. The temperature was raised from 20°C to 40°C in increments of 2°C for each measurement. For the light transmittance measurement, the transmittance at 700 nm was plotted to see the turbidity at a certain wavelength.
[0060] (LCST and particle size of the temperature-responsive material of Comparative Example 1 (temperature-responsive polymer of Example 1)) 11, in the temperature-responsive material of Comparative Example 1, the light transmittance measurement showed that the transmittance at a wavelength of 700 nm decreased from 93.0% to 7.65% at a temperature ranging from 32° C. to 34° C. Similarly, the DLS results showed that the particle size increased from 47.3 nm to 347 nm at a temperature ranging from 32° C. to 34° C., indicating that the LCST of the temperature-responsive polymer of Example 1 was 34° C.
[0061] (LCST and particle size of the temperature-responsive material of Comparative Example 2 (temperature-responsive polymer of Example 2) As shown in FIG. 12, in the light transmittance measurement of the temperature-responsive material of Comparative Example 2, the transmittance at a wavelength of 700 nm decreased from 92.6% to 7.65% from 30°C to 32°C. Similarly, the DLS results showed that the particle size increased from 46.8 nm to 330 nm from 30°C to 32°C, indicating that the LCST of the temperature-responsive polymer of Example 2 was 32°C. In Comparative Example 2, the particle size was approximately 30,000 nm at temperatures above 36°C. Thus, in Comparative Example 2, the particle size gradually increased, suggesting that it may be a random copolymer.
[0062] (LCST and particle size of the temperature-responsive material of Comparative Example 3 (temperature-responsive polymer of Example 2) 13, in the light transmittance measurement of the temperature-responsive material of Comparative Example 3, the transmittance at a wavelength of 700 nm decreased from 92.8% to 2.89% from 36° C. to 38° C. Similarly, the DLS results showed that the particle size increased from 5.36 nm to 13,500 nm from 36° C. to 38° C., indicating that the LCST of the temperature-responsive polymer of Example 3 was 38° C. In Comparative Example 3, the particle size of the temperature-responsive polymer suddenly increased from 36° C. to 38° C., which suggests that it may have become a block copolymer.
[0063] In this way, the LCST can be controlled to be lower by introducing a monomer (DEAA) that is less polar than NIPAM. Also, the LCST can be controlled to be higher by introducing a monomer (HEAA) that is more polar than NIPAM. In other words, by introducing a hydrophobic monomer unit into the main monomer and making the polarity of the resulting temperature-responsive polymer more hydrophobic than the main monomer, the LCST decreases. By introducing a hydrophilic monomer unit into the main monomer and making the polarity of the resulting temperature-responsive polymer more hydrophilic, the LCST increases.
[0064] As shown in FIG. 11, the particle size at a temperature above the LCST in Comparative Example 1 was 300 nm, but when CM-CNF was mixed in as in Example 5, it increased to 10,000 nm. This is thought to be due to aggregation while incorporating CM-CNF in Example 5. On the other hand, the transmittance showed similar changes in the graphs for both. Therefore, blending CM-CNF did not cause a change in the LCST.
[0065] As shown in FIG. 12, the particle size at a temperature above the LCST in Comparative Example 2 was 31,000 nm, but when CM-CNF was mixed in as in Example 6, it became smaller at 10,000 nm. This is thought to be due to the fact that CM-CNF inhibited the aggregation of the copolymer, forming heterogeneous giant aggregates on the glass, and causing phase separation between the aggregates. On the other hand, the transmittance showed similar changes in the graph for both. Therefore, blending CM-CNF did not cause a change in the LCST.
[0066] As shown in FIG. 13, the particle size at a temperature above the LCST in Comparative Example 3 was 14,000 nm, but when CM-CNF was mixed in as in Example 7, it became smaller at 10,000 nm. This is thought to be due to the fact that CM-CNF inhibited the aggregation of the copolymer, forming heterogeneous giant aggregates on the glass, and causing phase separation between the aggregates. On the other hand, the transmittance showed similar changes in the graph for both. Therefore, blending CM-CNF did not cause a change in the LCST.
[0067] The temperature-responsive polymer (0.5 g) of Example 1, chitin / chitosan nanofiber (0.5 g), and water (99 ml) were mixed to prepare the temperature-responsive material of Example 8. The temperature-responsive materials of Example 8 and Comparative Example 1 were subjected to light transmittance measurement using a UV-Visible Spectrophotometer V-670 (Spectrophotometer, manufactured by JASCO) and particle size measurement using dynamic light scattering (DLS) using a dynamic light scattering meter (Malvern, Zetasizer Nano ZS) to confirm the LCST. The temperature was raised from 20°C to 40°C in increments of 2°C. The results are shown in FIG. 14. For the light transmittance measurement, the transmittance at 700 nm was plotted to see the turbidity at a certain wavelength.
[0068] Light-shielding materials were produced using the temperature-responsive materials of Examples 5 to 7 and Comparative Examples 1 to 3. As shown in Fig. 15, a silicon sheet (thickness: 1 mm) was used as a spacer frame between two glass plates (thickness: 3 mm). First, the spacer frame was placed on one piece of glass, and the temperature-responsive materials of Examples 5 to 7 and Comparative Examples 1 to 3 were poured into the frame, which was then sandwiched between another piece of glass, and the edges of the glass were fixed with clips to produce the light-shielding materials of Examples 5 to 7 and Comparative Examples 1 to 3.
[0069] The heat shielding properties were measured using the light shielding materials of Examples 5 to 7 and Comparative Examples 1 to 3 as follows. As shown in Fig. 16, a temperature recorder was installed inside an insulating box, and the light shielding material was placed so as to cover an opening in the ceiling of the insulating box. In Fig. 16, the light shielding material is written as heat shielding laminated glass. Then, light was irradiated from a simulated solar light irradiator (light source) installed above the insulating box toward the opening of the insulating box, and the temperature was recorded every second by the temperature recorder. The results are shown in Figs. 17 to 19.
[0070] As shown in Figs. 17 to 19, the light-shielding materials of Examples 5 to 7 were able to suppress the temperature rise by about 8°C to 9°C after 30 minutes compared to the reference example in which only the glass plate was used. This is thought to be due to the temperature-responsive material being inserted in the middle of the light-shielding material, which used energy for molecular vibration, and the temperature-responsive material becoming cloudy, which absorbed heat rays. There was not much difference in the temperature rise suppression effect between Example 5 and Comparative Example 1 (see Fig. 17). On the other hand, as shown by the relationship between Example 6 and Comparative Example 2 and the relationship between Example 7 and Comparative Example 3, the presence of polysaccharides increases the temperature rise suppression effect (see Figs. 18 and 19).
[0071] NIPAM and a specified monomer shown in Table 1 were dissolved in water with stirring. TMED was added as a polymerization accelerator, and nitrogen replacement was performed in an ice bath (5 ° C.). APS aqueous solution was added as a polymerization initiator, and the reaction was allowed to proceed for 3 hours in an ice bath. As a result, a transparent and highly viscous reaction solution was obtained, so the reaction solution was diluted with ion-exchanged water and dialyzed with a 12-14 kDa dialysis membrane for 3 days to obtain a temperature-responsive polymer. The amount of each raw material is as shown in Table 1. 49.5 ml of a 1 wt% aqueous solution of the obtained temperature-responsive polymer and a 1 wt% aqueous solution of carboxymethyl cellulose nanofiber were mixed together. 1 ml of a 1 wt% aqueous solution of PEDOT / CS was further added to prepare a total of 100 ml of the temperature-responsive materials of Examples 9 to 11.
[0072] [Table 1]
[0073] (Near infrared absorbing material) As shown in FIG. 15, a silicon sheet (thickness: 1 mm) was used as a spacer frame between two glass plates (thickness: 3 mm). First, the spacer frame was placed on one piece of glass, and the temperature-responsive material of Examples 9 to 11 was poured into the frame, sandwiched between another piece of glass, and the edges of the glass were fixed with clips to produce the light-shielding materials of Examples 9 to 11. In addition, a light-shielding material of Example 12, which is the same as Example 9 except that no near-infrared absorbing material is blended, a light-shielding material of Example 13, which is the same as Example 10 except that no near-infrared absorbing material is blended, and a light-shielding material of Example 14, which is the same as Example 11 except that no near-infrared absorbing material is blended, were each produced.
[0074] The heat shielding properties were measured using the light shielding materials of Examples 9 to 14 as follows. As shown in Fig. 16, a temperature recorder was installed inside an insulating box, and the light shielding material was placed so as to cover an opening in the ceiling of the insulating box. In Fig. 16, the light shielding material is referred to as heat shielding laminated glass.
[0075] For the light-shielding material of Example 9 and the light-shielding material of Example 12, light was irradiated from a pseudo-sunlight irradiator (light source) installed above the insulating box toward the opening of the insulating box, and the temperature was recorded every second by a temperature recorder. The results are shown in FIG. 20. The light-shielding material of Example 9 started to become cloudy in 3.06 minutes and took 10 minutes for the entire surface to become cloudy, while the light-shielding glass of Example 12, which does not contain a near-infrared absorbing material, started to become cloudy in 3.21 minutes and took 10.5 minutes for the entire surface to become cloudy. In addition, when the temperature of the insulating box after 30 minutes of irradiation with pseudo-sunlight was compared, the light-shielding material of Example 9 was 36.5°C, while the heat-shielding laminated glass of Example 12, which does not contain an infrared absorbing material, was 37.3°C. Thus, it can be seen that the light-shielding material of Example 9 becomes cloudy earlier than the light-shielding material of Example 12, which does not contain a near-infrared absorbing material, and has a higher temperature suppression effect.
[0076] For the light-shielding material of Example 10 and the light-shielding material of Example 13, light was irradiated from a pseudo-sunlight irradiator (light source) installed above the insulating box toward the opening of the insulating box, and the temperature was recorded every second by a temperature recorder. The results are shown in FIG. 21. The light-shielding material of Example 10 started to become cloudy in 1.50 minutes and took 7.72 minutes for the entire surface to become cloudy, while the light-shielding glass of Example 13, which does not contain a near-infrared absorbing material, started to become cloudy in 2.07 minutes and took 8.73 minutes for the entire surface to become cloudy. In addition, when the temperature of the insulating box after 30 minutes of irradiation with pseudo-sunlight was compared, the light-shielding material of Example 10 was 35.5°C, while the heat-shielding laminated glass of Example 13, which does not contain an infrared absorbing material, was 36.8°C. Thus, it can be seen that the light-shielding material of Example 10 becomes cloudy earlier than the light-shielding material of Example 13, which does not contain a near-infrared absorbing material, and has a higher temperature suppression effect.
[0077] For the light-shielding material of Example 11 and the light-shielding material of Example 14, light was irradiated from a pseudo-sunlight irradiator (light source) installed above the insulating box toward the opening of the insulating box, and the temperature was recorded every second by a temperature recorder. The results are shown in FIG. 22. The light-shielding material of Example 11 started to become cloudy in 5.17 minutes and took 12.6 minutes until the entire surface became cloudy, while the light-shielding glass of Example 14, which does not contain a near-infrared absorbing material, started to become cloudy in 6.48 minutes and took 16.0 minutes until the entire surface became cloudy. In addition, when the temperature of the insulating box after irradiating with pseudo-sunlight for 30 minutes was compared, the temperature was 35.5°C for the light-shielding material of Example 11, while it was 37.1°C for the heat-shielding laminated glass of Example 14, which does not contain an infrared absorbing material. Thus, it can be seen that the light-shielding material of Example 11 becomes cloudy earlier than the light-shielding material of Example 14, which does not contain a near-infrared absorbing material, and has a higher temperature suppression effect.
[0078] The light-shielding materials of the above-mentioned Examples 13 and 14 were observed when they became cloudy. In addition, a light-shielding material of Comparative Example 1, which is the same as Example 13 except that no polysaccharide is blended, and a light-shielding material of Comparative Example 2, which is the same as Example 14 except that no polysaccharide is blended, were prepared, and the state of these materials when they became cloudy was also observed. As shown in Figs. 23 and 25, it can be seen that the example using the temperature-responsive material containing polysaccharide is uniformly cloudy. In contrast, as shown in Figs. 24 and 26, the comparative example using the temperature-responsive material not containing polysaccharide cracks when it becomes cloudy. In this way, the temperature-responsive material of the examples can change its transparency uniformly when the temperature exceeds the LCST by blending polysaccharide. [Explanation of symbols]
[0079] 10 Light-shielding materials, 12 Transparent materials, 14 Temperature-responsive materials
Claims
1. a temperature-responsive polymer having a lower critical solution temperature for water; A nanopolysaccharide having water retention properties; Water, a near infrared absorbing material; The nanopolysaccharide is carboxymethylcellulose, chitin deacetylation product, TEMPO oxidized cellulose or sulfated cellulose; The near-infrared absorbing material is a polythiophene or a polythiophene derivative doped with sulfated cellulose nanofibers or sulfated cellulose nanocrystals. A temperature responsive material characterized by:
2. The temperature-responsive material according to claim 1 , wherein the nanopolysaccharide is a nanofiber or a nanocrystal.
3. 3. The temperature responsive material according to claim 1, wherein the temperature responsive polymer is a poly(meth)acrylamide derivative or a poly(meth)acrylamide copolymer composed of a plurality of monomers including at least a (meth)acrylamide monomer.
4. A light-shielding material comprising the temperature-responsive material according to any one of claims 1 to 3 disposed between opposing transparent plates.
Citation Information
Patent Citations
Multiprocessor of same program
JP1986007948A
Laminated body, its production and window using that
JP1996082809A
Light-controlling panel
JP2012189746A
Stimulation responsive gel and actuator using the same
JP2014005469A
Slurry for forming electrode active material layer of battery
JP2020013763A
