Solid oxide battery chip having dual electrolyte structure and its manufacturing method

The dual electrolyte structure in the solid oxide battery chip addresses gas transport and structural strength issues, enhancing efficiency and reducing costs by optimizing gas flow and heat management.

JP7565651B2Active Publication Date: 2024-10-11ZHEJIANG ZHENTAI ENERGY TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023551961
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-25
Filing Date
2021-03-18
Publication Date
2024-10-11
Estimated Expiration
2041-03-18

AI Technical Summary

Technical Problem

Existing solid oxide batteries face challenges in balancing gas transport resistance and structural strength, leading to inefficiencies in gas diffusion, reduced power output, and high manufacturing costs due to complex assembly and sealing issues.

Method used

A solid oxide battery chip with a dual electrolyte structure featuring internal electrodes sandwiched between two electrolyte layers, embedded micro gas channels, and a multi-layered sealing system, along with a tapered design to optimize gas flow and reduce heat loss.

Benefits of technology

The dual electrolyte structure enhances gas transport efficiency, improves structural integrity, reduces manufacturing complexity, and increases power output by up to 10% compared to rectangular designs, while lowering production costs and improving yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565651000001
    Figure 0007565651000001
  • Figure 0007565651000002
    Figure 0007565651000002
  • Figure 0007565651000003
    Figure 0007565651000003
Patent Text Reader

Abstract

The present invention provides a solid oxide battery chip with a dual electrolyte structure and a manufacturing method thereof, which belongs to the technical field of electrochemistry. The solid oxide battery chip with a dual electrolyte structure includes two electrolyte layers, separated by an internal electrode sandwiched therebetween, with regularly arranged gas flow paths formed inside the internal electrode, and at least two sides of the internal electrode are covered with a side seal member. An outer surface member is provided on the outer surface of the electrolyte, and the outer surface member includes an intermediate layer, an external electrode, an internal electrode plate, and an external electrode plate, with the internal electrode connected to the internal electrode plate, and the external electrode connected to the external electrode plate. The side seal layer is provided as a multi-layer structure, with an inner sub-layer that can increase the leakage resistance of gas flowing through the internal electrode, and the material of the outer sub-layer has a different composition and structure from the material of the inner sub-layer, thereby achieving better sealing against gas leakage after decompression and maintaining better structural strength.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solid oxide battery chip and a manufacturing method thereof, and more particularly to a solid oxide battery chip having a double-electrolyte structure and a manufacturing method thereof. [Background technology]

[0002] 1. Operating principle of Solid Oxide Cell (SOC)

[0003] A solid oxide cell (SOC) is a ceramic electrochemical device that uses a solid oxide as an electrolyte. It is composed of at least one electrolyte layer and at least two electrodes. The electrodes provide the overall strength of the battery in an electrode-supported solid oxide cell, while the electrolyte provides the overall strength of the battery in an electrolyte-supported solid oxide cell. The electrolyte material is usually doped stabilized zirconium oxide, such as yttria-stabilized zirconia (YSZ), scandia-stabilized zirconia (ScSZ), scandia and yttria stabilized zirconia (ScYSZ), scandia and cerium stabilized zirconia (ScCeSZ) or calcium oxide stabilized zirconia (CaO) (CSZ), of which 8 mol% yttrium stabilized zirconia (8YSZ) is the most widely used. The electrolyte can also be other oxides with fluorite structure, such as cerium oxide stabilized by doping with gadolinium oxide or samarium oxide, i.e., GDC (gadolinia doped ceria) or SDC (samaria doped ceria), or oxides with perovskite structure, such as LaSrGaMgO (LSGM), which are well known to those skilled in the art [VVKharton, et al., Transport properties of solid oxide electrolyte ceramics: a brief review, Solid State Ionics, 174:135-149 (2004)].The material composition of the electrode can be an oxide with a perovskite structure, such as LaSrMnO (LSM) or LaSrCoFeO (LSCF), or an oxide with a fluorite structure, such as SDC or GDC, or a composite, such as a composite of LSM and YSZ / CGO, or a noble metal, such as Pt, or a composite containing a noble metal, such as a composite of Pt and YSZ, which are well known to those skilled in the art [EVT sipis, et al., Electrode materials and reaction mechanisms in solid oxide fuel cells: a brief review, J. Solid State Electrochem., 12: 1367-1391 (2008)].

[0004] When a solid oxide battery (SOC) operates, there is a difference of 10 times or several orders of magnitude in the oxygen concentration near at least two electrodes, and in the following, the gas with a relatively high oxygen concentration is referred to as an "oxygen-rich gas", and the electrode operating in the oxygen-rich gas is referred to as an "oxygen-rich electrode". The gas with a relatively low oxygen concentration is referred to as an "oxygen-deficient gas", and the corresponding electrode is referred to as an "oxygen-deficient electrode". The components of the oxygen-rich gas can include oxygen gas, nitrogen gas, argon gas, and helium gas, but the most commonly used and most typical oxygen-rich gas is air, and the corresponding electrode is referred to as the "air electrode". The oxygen-deficient gas can include multiple types of gas components with fuel properties or reducing properties, such as carbon monoxide, methane, methanol, and hydrogen gas. Typical oxygen-deficient atmospheres can be, for example, hydrogen / water mixed gas, hydrogen / carbon monoxide / water vapor mixed gas, carbon monoxide / carbon dioxide mixed gas, and nitrogen oxide (NOx) / nitrogen gas mixed gas, and the corresponding electrode is referred to as the "fuel electrode". The oxygen-deficient electrode and the oxygen-rich electrode are separated by an electrolyte, which should be as dense as possible and gas-tight, and its conductivity should be realized by the movement of ions, not the movement of electrons, as much as possible. If electronic conduction exists in the electrolyte, a short circuit current will occur inside the battery, greatly reducing the overall efficiency of the battery. The charge transport of SOC electrolytes is usually carried by oxygen ions, i.e., it is conducted by oxygen ions.

[0005] Solid oxide cells (SOCs) operate in the temperature range of 500-1000°C and have two operating modes. These are the Solid Oxide Fuel Cell (SOFC) mode in power generation mode and the Solid Oxide Electrolysis Cell (SOEC) mode in electrolysis mode. When an SOC operates in power generation mode, i.e., SOFC mode, oxygen molecules in the oxygen-enriched electrode undergo a reduction reaction to produce oxygen ions (O 2-), and oxygen ions move from the oxygen-rich electrode side to the oxygen-deficient electrode side by diffusing through the electrolyte, and if there are fuel gas molecules in the oxygen-deficient electrode, the oxygen ions react chemically with the fuel gas molecules in the oxygen-deficient electrode. Typically, if the gas components in the oxygen-deficient electrode include hydrogen (H2) and carbon monoxide (CO), the chemical reactions that occur in the oxygen-deficient electrode include:

[0006] H2+O 2- →H2O+2e-

[0007] CO+O 2- -→CO2+2e-

[0008] Macroscopically, the whole process is as follows: oxygen molecules move from the oxygen-rich gas side to the oxygen-deficient gas side through the electrolyte, and the oxygen concentration difference between the oxygen-rich gas and the oxygen-deficient gas decreases accordingly. In power generation mode, the SOC converts the chemical energy of the oxygen-deficient gas into electrical energy and outputs it to the outside. Taking the hydrogen electrode and the oxygen electrode as an example, the electrode reaction and the overall electrochemical reaction in SOFC mode can be expressed as follows:

[0009] Anode (oxygen-deficient electrode): H2+O 2- →H2O+2e-

[0010] Cathode (oxygen-enriched electrode): 1 / 2O2+2e-→O 2-

[0011] Overall reaction: H2+1 / 2O2→H2O

[0012] If the electrode reaction products cannot be removed quickly, the oxygen concentration difference between the oxygen-rich and oxygen-deficient gases will decrease as the reaction proceeds.

[0013] When a solid oxide cell (SOC) operates in electrolysis mode, i.e., SOEC mode, gases in the oxygen-deficient electrode, such as oxygen (O2), water vapor (HO), carbon dioxide (CO2), nitrogen oxides (NO x ) are converted to oxygen ions (O 2-) and migrate to the oxygen-rich electrode through the electrolyte, where the oxygen-rich electrode undergoes an oxidation reaction to become oxygen molecules. Macroscopically, the entire process is as follows: under the action of an external electric field, oxygen molecules migrate from the oxygen-deficient gas side, where the oxygen concentration is relatively low, through the electrolyte to the oxygen-rich gas side, where the oxygen concentration is relatively high. The oxygen concentration difference between the oxygen-rich gas and the oxygen-deficient gas increases accordingly. In the electrolysis mode, the SOC absorbs the electrical energy input from the outside and converts it into the chemical energy of the oxygen-deficient gas. Taking the hydrogen electrode and the oxygen electrode as an example, the electrode reaction and the overall electrochemical reaction in the SOEC mode can be expressed as follows:

[0014] Anode (oxygen-enriched electrode): O 2- →1 / 2O2+2e-

[0015] Cathode (oxygen-deficient electrode): H2O+2e-→H2+O 2-

[0016] Overall reaction: H2O→H2+1 / 2O2

[0017] When SOC works by switching between the two modes, it can realize the interconversion between electrical energy and chemical energy, and this process may involve the release or absorption of heat. Whether SOC works in power generation (SOFC) mode or electrolysis (SOEC) mode, it may accept the input of thermal energy from the outside or release thermal energy to the outside, so that SOC technology can be used to realize the interconversion between electrical energy, thermal energy, and chemical energy. When SOC works in electrolysis mode (SOEC), it converts electrical energy into chemical energy and stores it, and when it works in power generation mode (SOFC), it directly converts the chemical energy of oxygen-deficient gas into electrical energy. This avoids the limitations on the power generation efficiency of the heat engine process caused by the Carnot cycle and realizes efficient utilization of chemical energy.

[0018] For a typical oxygen-deficient gas, such as a mixture of H2 and H2O, the overall reaction of SOC under power generation mode (SOFC) is: H2+1 / 2O2→H2O. Under electrolysis mode (SOEC), the overall reaction of SOC is: H2O→H2+1 / 2O2. For a typical oxygen-deficient gas, such as a mixture of CO2, H2O, CO, and H2, the overall reaction of SOC under power generation mode is: H2+1 / 2O2→H2O, 2CO+O2→2CO2. Under the electrolysis mode (SOEC), the overall reaction of SOC is H2O→H2+1 / 2O2, 2CO2→2CO+O2, and the electrolysis products containing CO and H2 are also called synthesis gases, which can be further converted into a series of hydrocarbon compounds, such as methanol, ethanol, natural gas, gasoline, diesel oil, and other mature and widely used fuels or industrial raw materials, through the mature Fischer-Tropsch synthesis process. The gas components containing oxygen element are converted into nitrogen oxides NO x , sulfur oxides SO x For typical environmental pollutants such as those listed above, SOC's electrolysis technology can be used to remove these pollutants, and the chemical process can be expressed as follows:

[0019] NO x →N2+O2(x=1or2)orSO x →S+O2(x=1 or 2);

[0020] 2. Electrode reaction process of solid oxide batteries (SOC)

[0021] In the electrode reaction process of SOC, at least three phases of material are involved in the reaction: oxygen ions (O 2- ), electron (e -), and gaseous substances, such as oxygen molecules (O2), water (H2O), hydrogen (H2), carbon monoxide (CO), etc. In order for the electrode reaction process to proceed continuously and rapidly, all substances involved in the reaction need passages (channels) to enter and exit quickly, for example, the electrons and oxygen ions required for the reaction process need smooth transport channels, in other words, the electrode needs to contain a material with high electronic conductivity and high oxygen ion conductivity, and at the same time, it needs to have a certain porosity, which can help the gaseous reactants to enter the electrode and the gaseous products of the electrode reaction to exit the electrode under high temperature. Known electronic conductive materials for oxygen-deficient electrodes include metallic nickel (Ni), gold (Au), platinum (Pt), palladium (Pd), rhodium (Rh), etc., and oxygen ion conductors include yttria-stabilized zirconia (YSZ), scandia and yttria stabilized zirconia (ScYSZ), scandia and cerium stabilized zirconia (ScCeSZ), or cerium stabilized with samarium oxide (Sm2O3), gadolinium oxide (Gd2O3), etc., such as SDC, GDC, etc. Some known oxygen ion conductor materials, such as cerium stabilized by doping, such as SDC, GDC, etc., also have a certain degree of electronic conductivity and are called mixed conductors. The electron conductor material of the known oxygen-enriched electrode can include oxides such as LaSrMnO, LaSrCoO, and LaSrCoFeO that can maintain stable properties in a high-temperature oxidizing atmosphere and whose specific component composition can vary within a certain range, or can be high-temperature oxidation-resistant precious metals such as silver (Ag), gold (Au), platinum (Pt), palladium (Pd), and rhodium (Rh). These high-temperature oxidation-resistant precious metals also act as catalysts to promote the reaction of the electrode.The oxygen ion conductor of the oxygen-enriched electrode is a material such as zirconium oxide stabilized by adding yttrium oxide (YSZ), or cerium oxide stabilized by adding samarium oxide (Sm2O3) or gadolinium oxide (Gd2O3), such as SDC and GDC. At the same time, the electronic conductor material in the oxygen-enriched electrode, such as oxides such as LaSrCoO and LaSrCoFeO, may also have a certain oxygen ion conductivity, and are also called mixed conductors in the industry. These are well known in the industry [EVTsipis, et al., Electrode materials and reaction mechanisms in solid oxide fuel cells: a brief review, J. Solid State Electrochem., 12: 1367-1391 (2008)].

[0022] Commonly used solid oxide batteries are electrode-supported, and by arranging gas channels in the electrodes, part of the electrode structure becomes hollow, which significantly reduces the structural strength of the battery. The larger the volume of the gas channels, the higher the occupation ratio, and the more non-uniform the size, the greater the reduction in battery strength. Therefore, in conventional solid oxide battery (SOC) technology, the size of the gas channels in the electrodes is small, less than 1 μm, and exhibits an irregular point-like distribution [MB Mogensen, et al., Reversible solid-oxide cells for clean and sustainable energy, Clean Energy, 1-27 (2019).]

[0023] The method of forming gas flow channels in these electrodes is usually to add a certain content of pore formers (such as graphite or starch) in the precursor powder slurry for electrode production. These pore formers and some solvents (such as alcohol, toluene and isopropanol) are volatilized by high-temperature pyrolysis during the high-temperature sintering manufacturing process of the battery and escape from the electrode, or are oxidized by oxygen in the air to produce gas oxides, such as carbon dioxide (CO2), which escape from the electrode, leaving gas flow channels in the electrode. These are well-known methods in the industry [M. Chen, et al., Microstructural degradation of Ni / YSZ electrodes in solid oxide electrolysis cells under high current. J. Electrochem. Soc., 160: F883-F891 (2013)].

[0024] The fine gas pores constructed in this way cannot form a channel that can rapidly transport gas within the entire electrode, so that the gas cannot be supplied sufficiently to the entire battery or the gas products cannot be rapidly discharged. The usual solution to this problem is to construct an external gas flow path outside the electrode, and the oxygen-rich gas and the oxygen-deficient gas flow within the external gas flow path, respectively, i.e., the oxygen-rich flow path and the oxygen-deficient flow path, which are formed surrounded by the interconnect, the battery, and the sealing glass, which are introduced in the open literature [MB Mogensen, et al., Reversible solid-oxide cells for clean and sustainable energy, Clean Energy, 1-27 (2019).]. Figure 1 shows a schematic structure of a cross section of one battery chip of a typical solid oxide battery (SOC) technology available in the open literature. It can be seen that in these typical structures, the diffusion flow rate of gas, especially oxygen-deficient gas, inside the electrode is very low, so the gas flow rate leaking from the side edge of the battery is very small, so there is no need to seal the side edge of the electrode, and a high-temperature sealing material, such as glass, can be used to seal the gap between the interconnect and the electrode. In these configurations, the main gas is located outside the battery and flows in a gas flow path with a regular outline, the geometry and cross-sectional shape of the gas flow path can be designed and manufactured according to requirements, the gas raw material as reactant first diffuses from the external gas flow path into the electrochemical reaction zone at the electrode-electrolyte interface, and after the electrode reaction, the gas product as product diffuses again from the relatively dense electrode into the external gas flow path and is removed.

[0025] In such a design, the gas flow paths in the electrode should not be too many or too large due to the need for structural strength. Therefore, the gas transport rate in the electrode is too low, which is one of the main factors limiting the electrode reaction rate. To alleviate this problem, the electrodes in solid oxide batteries are usually made very thin, typically 0.05-0.5 mm thick. This reduces the amount of gas components that diffuse into and out of the electrode, i.e., reduces the distance from the gas flow paths to the electrode and electrolyte interface. Although an electrode that is too thin contributes to reducing the resistance of gases that diffuse into and out of the electrode, it can significantly reduce the structural strength of the battery. Batteries designed and manufactured in this way are prone to bursting during the assembly and use of the stack (cell group), and even the entire stack will expire and become unusable. This is one of the main factors limiting the large-scale use of high-temperature solid oxide battery technology in commercialization.

[0026] 3. Solid Oxide Battery (SOC) Stack Assembly Design

[0027] The most common SOC configuration for solid oxide batteries is the flat plate type. The stack structure of the flat plate type SOC is realized by sequentially connecting the SOC elements, sealing rings, interconnects, etc., and the entire stack is placed in a high-temperature environment, which has been introduced in the open literature [NQMinh, System design and application, in High-Temperature Solid Oxide Fuel Cells for the 21st Century]. st Century (2 ndEd.ISBN:978-0-12-410453-2),2015.]. The sealing ring is usually made of glass or metal (e.g. gold, silver, etc.), and the material of the interconnector is usually a high-temperature resistant alloy. The alloy interconnector is usually spray-coated with a conductive anti-oxidation coating on the surface that contacts the battery, which improves the anti-oxidation ability under high-temperature conditions and reduces the electrical resistance loss of the stack connection. In many cases, there is an additional layer or layers of relatively soft metal or ceramic pads between the electrodes on both sides of the solid oxide battery (SOC) and the alloy interconnector, which ensures good electrical contact between the battery (SOC) and the interconnector. Typically, a mesh made of a metal that is resistant to high-temperature oxidation, such as gold (Au) or silver (Ag), is used to ensure good electrical contact. In one sheet-type SOC stack, the airflow (oxygen-deficient gas and oxygen-rich gas) flows within the isolated space formed by the interconnector, the battery (SOC), and the sealing ring, preventing leakage outside the stack. Each element that makes up a sheet-type SOC stack includes the battery (SOC), sealing ring, interconnector, etc., and each of these must be manufactured separately before finally being assembled into a stack. Sheet-type SOC stacks have regular electrode shapes, short current paths, relatively high power density, and are easy to assemble. However, it is difficult to put sheet-type SOC stacks into practical use for the following reasons:

[0028] 1) The reliability of the sealing ring is low. The sealing ring must simultaneously meet the requirements of airtightness, heat cycle resistance, high temperature reduction resistance, and high temperature oxidation resistance, and must also have certain mechanical strength and toughness. Furthermore, the thermal expansion coefficients of the alloy interconnector and the SOC battery sheet must be close, i.e., the thermal expansion must be matched. That is, the dimensional changes of the sealing ring and the sealing member must be almost the same under temperature changes. Whether the sealing ring is made of glass or metal, it is difficult to simultaneously achieve these performance requirements. For example, glass sealing rings are usually fragile and are very easily broken or lost during the assembly of SOC stacks and the operation of thermal cycles. Even if the sealing between ceramics and metal is barely achieved using glass, the temperature change rate that it can withstand must be very small to avoid the sealing ring being overstrained by excessive stress, and as a result, the start-up and shutdown times of stacks using ordinary solid oxide battery technology are very long, usually more than 10 hours, and sometimes even more than 20 hours.

[0029] 2) Each stack element must be manufactured individually, which is technically demanding. The requirements for flatness, strength, toughness, oxidation resistance, and thermal expansion matching of each element are all relatively high, so the cost of sheet-type SOC stacks is generally high, limiting their practical applications.

[0030] 3) The degree of freedom of stack assembly is low. The connection method of each unit cell of a sheet-type SOC stack is series connection, and the sealing ring is a disposable element. After a sheet-type SOC stack is heat-treated, that is, after the sealing ring and the sealing member are fused at a high temperature, for example, 850°C, to achieve sealing, each stack element including each unit cell and interconnector cannot be replaced, so that the failure of any element in the entire stack will result in the failure of the entire stack, which greatly increases the risk of using the sheet-type SOC stack and significantly increases the usage cost.

[0031] The existing patent [CN108336386B] discloses a flat tubular type solid oxide electrochemical device and its manufacturing method, [CN108321408B] discloses a flat tubular type solid oxide electrochemical device including multiple pairs of electrodes and its manufacturing method, and [CN108336376B] discloses a flat tubular type solid oxide battery structure and its manufacturing method for improving the yield and power of a single cell, providing a solution to the above technical problems. This solution employs a flat tubular type solid oxide battery, and such a battery can use electrolyte support. When operating, the battery using this technology spans a high and low temperature range, and the battery performs electrochemical reactions at the high temperature end and realizes sealing and external connection at the low temperature end. The structural features of the battery using this technology are as follows: 1) The gas flow isolation structure required for the operation of the battery, i.e., the gas flow path, is formed by being surrounded by an electrolyte, two gas flow path walls, and a single layer of separator; 2) The electrolyte, the gas flow path wall, and the separator are made of the same material or materials with similar compositions; 3) The outer surface of the inlet and outlet of the non-gas flow path of the battery has a gas flow path wall, and the gas flow path wall must have a certain width to ensure the reliability of the seal. In this structure, the gas flow path is sealed by the gas flow path wall, not by high-temperature sealing materials, such as glass, that are commonly used in conventional technology. The remaining gas flow path wall reduces the effective power generation area of ​​the battery, but the composition and properties of the gas flow path material are similar to those of the electrolyte, which solves or greatly alleviates the problems commonly seen in sheet-type stack technology, such as the thermal expansion characteristics of each stack element not matching, which causes the components to burst and fail during the thermal cycle of the stack, or the stack components react with each other due to chemical incompatibility during long-term high-temperature operation, which causes the stack performance to weaken and fail.

[0032] The problem in the practical application of the flat tube battery structure is that it is difficult to balance the yield and electrical performance of the battery. The realization of the gas flow passage enclosing structure in the flat tube structure includes at least one electrolyte layer. The electrolyte is an essential functional component for the electrochemical reaction to occur during the operation of the solid oxide battery. The thinner the electrolyte, the lower the resistance to the transport of oxygen ions, and the better the electrical performance of the battery. However, the thinner the electrolyte, the lower the strength, and the electrolyte part constituting the gas flow passage is easy to burst during the manufacturing process of the battery or when a large amount of air flows through it during the operation of the battery, which reduces the yield and reliability of the flat tube battery and increases the cost of using the technology. Typically, in order to provide sufficient strength to the gas chamber of the flat tube battery, the thickness of the electrolyte generally needs to be more than 0.5 mm, but by making the thickness of the electrolyte 0.5 mm, the output power density of the battery can be reduced to 100 mW / cm. 2 This makes the battery output power density 300mW / cm 2 To achieve the above, it is desirable that the thickness of the electrolyte does not exceed 0.1 mm. However, such a thickness makes the electrolyte easily burst at the gas tank, so that such a technology is difficult to achieve both yield and electrical performance. In addition, the side of the non-gas flow inlet and outlet of the battery needs to be a gas flow wall, so that when manufacturing the battery, the gas flow wall at the edge of the battery needs to be precisely printed or attached at a specified position of the corresponding slurry or gas flow wall film, which requires an additional manufacturing process step to be added, which increases the requirements for the manufacturing process of the battery, increases the cost, and reduces the production efficiency of the battery.

[0033] The batteries disclosed in the above-mentioned existing patents can also use an electrode-supported technical configuration, and the operation of the battery spans the same high and low temperature range, with the battery performing electrochemical reactions at the high temperature end and sealing and external connection at the low temperature end. However, the electrolyte that surrounds and forms the gas flow path is replaced by an internal electrode, so that the gas flow path is realized entirely by the electrode material, and the strength of the gas flow path wall and the battery can be realized by moderately increasing the thickness of the internal electrode, while keeping the thickness of the electrolyte relatively thin contributes to the battery having a relatively large power. In such a configuration, the gas flow path wall is also present on the outer surface of the non-gas flow path inlet and outlet of the battery, and the sealing of the high temperature area during the operation of the battery is realized by the gas flow path wall, not by high temperature sealing materials commonly used in conventional technology, such as glass. The width of the gas flow path wall that must be left in advance reduces the power generation area of ​​the battery, and at the same time, the side of the non-gas flow path inlet and outlet of the battery must be a gas flow path wall, so when manufacturing the battery, the gas flow path wall at the edge of the battery needs to be precisely printed or pasted with a corresponding slurry or film piece at a specified position, which requires an additional manufacturing process step to be added, which increases the requirements for the battery manufacturing process, increases the cost, and reduces the production efficiency of the battery. In addition, although such a configuration is effective in improving the performance and yield of the battery, the extent is limited, the gas diffusion speed in the internal electrode with a relatively low porosity is limited, excessive increase in the thickness of the electrode leads to insufficient gas supply for the electrode reaction, and the relatively thin internal electrode leads to insufficient strength of the gas flow path, making it impossible to achieve a high manufacturing yield of the battery.

[0034] In the above-mentioned existing patent, the internal electrode current transport region is between the central battery operating high temperature region (high temperature end) and the low temperature region (low temperature end) plate that performs external connection and sealing functions, and the current carrier, i.e., the conductive material, is a high temperature resistant metal such as platinum (Pt) or nickel (Ni), and the current collection resistance of the circuit is relatively large. For example, the conductivity of precious metals such as Pt is about 9×10 4Because precious metals are expensive, they can only be used in thin layers, typically about 50 μm thick, and the electrical resistance of the current collector of a Pt coating layer is about 20 mOhm (for an example of a width of 1 cm and a length of 10 cm). The electrical conductivity of nickel is about 1×10 5 S / cm, but due to the needs of forming in the electrode, its content is generally less than 60%, and the conductivity of the entire internal electrode is usually only 200-250S / cm. Therefore, the current collection resistance of the nickel electrode is about 400mOhm (for example, width 1cm, thickness 1mm, length 10cm), and the circuit current collection resistance of the internal electrode is relatively large.

[0035] The batteries of the above-mentioned existing patents need to span a temperature range between high and low temperatures in order to operate. That is, the electrodes of the battery undergo electrochemical reaction in the high temperature area (high temperature area), and the battery is sealed and connected to the outside in the low temperature area (low temperature area). Therefore, the entire battery inevitably transfers heat from the high temperature area to the low temperature area during operation, resulting in heat outflow and reducing the system efficiency. The manufacturing process of the battery using such a technical configuration is complicated, and in practice, only batteries with a relatively simple shape, such as a rectangular or square shape, can be manufactured. In such a shape design, the path through which heat moves from the high temperature area to the low temperature area has the same dimensions and cross-sectional area, and the heat loss is relatively large. If a gradually narrowing structure, i.e., a structure in which the battery gradually reduces in size from the high temperature operating area to the low temperature sealing area, could be used, the path through which heat flows from high temperature to low temperature could be gradually narrowed, which is advantageous for reducing the heat outflow rate of the battery, but in the known technical configuration, it is difficult to realize due to the complicated process.

[0036] Summary of the Invention

[0037] In view of the above problems in the prior art, the object of the present invention is to propose a solid oxide battery chip, and the technical problem to be solved by the present invention is how to establish a low resistance gas transport path for rapid electrode reactions while at the same time ensuring sufficient structural strength for the battery. The solid oxide battery chip described in the present invention is referred to herein as a "cell chip" or simply as a "cell".

[0038] The object of the present invention can be realized by the following technical configuration: A solid oxide battery chip having a dual electrolyte structure, characterized in that the two electrolyte layers are separated by an internal electrode sandwiched therebetween, the internal electrode is provided with a plurality of regularly arranged gas flow paths, and at least two sides of the internal electrode are covered with a side seal member, and an outer surface component is provided on the outer surface of the electrolyte, the outer surface component includes an intermediate layer, an external electrode, an internal electrode plate, and an external electrode plate, the internal electrode is connected to the internal electrode plate, and the external electrode is connected to the external electrode plate.

[0039] There is an oxygen partial pressure difference between the inner and outer electrodes, i.e., the outer electrode can be designed as an oxygen-rich electrode and the inner electrode as an oxygen-deficient electrode, or the outer electrode can be designed as an oxygen-deficient electrode and the inner electrode as an oxygen-rich electrode according to operation needs.

[0040] In the solid oxide battery chip having the dual electrolyte structure, the equivalent diameter of a cross section of a single gas flow path among the multiple gas flow paths regularly arranged in the internal electrode is within a range of 20 to 200 μm.

[0041] In the solid oxide battery chip having the dual electrolyte structure, the side seal member includes a plurality of sublayers, at least one of which is dense and non-permeable, and at least one highly rough and permeable sublayer is provided between the dense and non-permeable sublayer and the side surface of the battery chip.

[0042] In the solid oxide battery chip having the dual electrolyte structure, the external member further includes a plurality of external current collectors covering the outer surfaces of the external electrodes, and the electrical conductivity of the external current collectors is not lower than that of the external electrodes.

[0043] In the solid oxide battery chip having the dual electrolyte structure, the outer surface member further includes a protective layer, and the protective layer covers at least one of the outer surface members.

[0044] In the solid oxide battery chip having the dual electrolyte structure, the internal electrodes and the plates of the internal electrodes are connected by internal bus bars, and the conductivity of the internal bus bars is not lower than that of the internal electrodes.

[0045] In the solid oxide battery chip having the dual electrolyte structure, the internal bus bar is located between a side seal member and a side surface of the battery chip.

[0046] In the solid oxide battery chip having the dual electrolyte structure, the main body of the internal busbar is disposed on the outer surface of the electrolyte and is connected to the internal electrode through the electrolyte.

[0047] In the solid oxide battery chip with the dual electrolyte structure, the internal bus bars penetrate the electrolyte and are individually sealed with a sealing material to prevent gas leakage.

[0048] In the solid oxide battery chip having the dual electrolyte structure, the battery chip is in the form of a long sheet, and the outer shape of the battery chip gradually narrows from the external electrode region in the center of the battery chip toward the end face of the gas flow path inlet / outlet.

[0049] The object of the present invention can be further achieved by the following technical configurations: A method for manufacturing a high temperature solid oxide battery chip, the method comprising the steps of:

[0050] (1) Production of substrate sheets: After adding appropriate auxiliary agents and solvents to the components constituting the internal electrodes and electrolyte according to the appropriate ratio, thin substrate sheets are produced by a casting operation, and gas flow path precursors are produced on a portion of the substrate sheets according to needs.

[0051] (2) Lamination of base sheets: An electrolyte base sheet, an internal electrode base sheet including a gas flow path, and an internal electrode base sheet not including a gas flow path are aligned and stacked in a specific order, then placed in a vacuum bag, evacuated and sealed, and the base sheet assembly placed in the vacuum bag is placed in a press machine and fused by high-temperature compression to form a laminate.

[0052] (3) Cutting: The laminate is placed in a die-cutting device and cut into battery chip blanks (green bodies) having the specified design shape.

[0053] (4) Sintering: The battery chip blank is placed in a high-temperature furnace and sintered with a suitable heat treatment schedule, after which the battery chip blank becomes a battery chip with relatively high strength. At the same time, during the heat treatment schedule, the gas flow path precursor gasifies and escapes, leaving regular and uniform embedded gas flow paths in the internal electrodes of the battery chip.

[0054] (5) Firing of the intermediate layer: After firing, an intermediate layer is formed on the electrolyte on both sides of the battery chip by high-temperature heat treatment.

[0055] (6) Reduction: The battery chip with the fired intermediate layer is placed in a reduction furnace for reduction, and the nickel oxide in the internal electrode is reduced to metallic nickel. The reduction operation of the battery chip can be completed before the battery chip is used and assembled into a stack, other than the case shown here, or can be achieved by reducing the entire stack after the battery chip is assembled into a stack.

[0056] (7) Manufacturing of external surface members: The external surface members of the battery chip are printed on the external surface of the battery chip after reduction. These external surface members include an external current collector, an external electrode, an external electrode plate, an internal electrode plate, an external electrode bus bar, an internal electrode bus bar, and a protective layer, etc., and these members can be printed entirely on the intermediate layer, or partially or entirely on the surface of the electrolyte. The various slurries used can use a mixture of ethanol and terpineol as a solvent, and further contain about 0-10% graphite as a pore former.

[0057] (8) Manufacturing of side seal member: A side seal member is manufactured for the battery chip that has completed the above steps. The side seal member can include a sub-structure of two layers, an inner layer and an outer layer. The inner layer of the side seal is applied first, and the preferred material is graphite (C) or magnesium silicate talc material (Mg6)[Si8]O20(OH)4). After the inner layer of the side seal is dried, the outer layer of the side seal is applied on top of it. The preferred material is potash-lime glass, and the composition is 12-18% K2O, 5-12% CaO, and 60-75% SiO2.

[0058] (9) Heat treatment: The battery chips on which the outer surface components are printed and the side seal components are applied are heat treated, and after the heat treatment, the outer surface components and their attachments form a strong connection, and the side seal components have at least one layer of densified structure. The preferred heat treatment schedule is 850°C for 1 hour, the atmosphere is a reducing protective atmosphere, the hydrogen content is 5-60%, and the balance gas is nitrogen.

[0059] (10) Electrode strengthening. The heat-treated battery chip can be used in practical applications, and the electrode can be strengthened to further improve the electrical properties of the battery chip and reduce the internal resistance. A typical electrode strengthening method is, for example, impregnation.

[0060] In addition to the characteristics of the solid oxide battery chip manufactured by the present invention being able to operate at the same high temperature end and having external connections and sealing at the low temperature end, the battery chip of the present invention further has the following characteristics:

[0061] 1) The dual electrolyte is separated by a sandwiched inner electrode, in which are embedded micro gas channels arranged in a regular pattern. The sides of the non-gas inlet / outlet end faces of the battery chip can also include the outlets of these gas channels, which can significantly reduce the process steps in the manufacture of the battery chip, improve the production efficiency of the battery chip, and reduce the production cost of the battery chip.

[0062] 2) The internal electrode may have multiple layers, for example, an active internal electrode and a supporting internal electrode, of which the active internal electrode is responsible for promoting the electrochemical reaction in terms of composition, and the supporting internal electrode is responsible for improving the overall strength and / or conductivity of the battery chip in terms of composition.

[0063] 3) Regularly arranged micro gas channels are embedded, and the number and position of the gas channels can be adjusted as needed. The internal electrodes can be arranged in a uniform manner and can be in close proximity to the electrolyte, and the supply rate of the raw material gas required for the electrode reaction or the exhaust rate of the product gas does not decrease with an increase in the thickness of the internal electrodes, but rather increases with an increase in the thickness of the internal electrodes. At the same time, the increase in the thickness of the internal electrodes improves the electrical conductivity of the entire internal electrodes and the strength of the battery chip.

[0064] 4) The internal gas flow passages are regularly arranged, and the equivalent diameter of the cross section of a single gas flow passage is within the range of 20-200 μm, preferably within the range of 30-60 μm. If the cross section of the gas flow passage is too large, it will reduce the strength of the battery chip, making the battery chip more fragile and significantly reducing the yield of the battery chip. If the gas flow passage is too small, it will cause an excessive air pressure drop during the operation of the battery chip. According to the actual test results, the equivalent diameter of a single gas flow passage should be controlled within the range of 30-60 μm. At the same time, the number of gas flow passages included in a single battery chip is 6 or more, which ensures that the battery chip has a certain ventilation capacity and ensures that the single battery chip has sufficient power.

[0065] 5) The side of the non-gas flow passage wall of the battery chip has a dedicated sealing structure, and one sealing structure may include multiple sub-layers, with different materials and microstructures. Different sub-structures can have different functions, for example, the sub-structure of the innermost layer is mainly used to strengthen the contact with the sealing bottom surface and has low requirements for airtightness. The structure of the outermost layer is used for sealing that requires high airtightness, and more sub-structures can be embedded in the sub-structures of the outermost layer and the innermost layer according to the functions. In any case, at least one sub-layer of the side seal member is dense and non-breathable.

[0066] 6) The current collecting structure of the internal electrode may include a layer, the conductivity of which is relatively high, and reduces the current collecting resistance of the internal electrode. The current collecting structure of the internal electrode may be disposed in the sealing layer, attached to the side of the internal electrode, or disposed in another position, for example, on the surface of the battery chip. The preferred material of the current collecting structure of the internal electrode is a silver (Ag) or nickel (Ni)-based coating layer. The material cost of silver and nickel is cheaper than precious metals such as Pt, and they have high conductivity. They are only used to apply to one side or side of the battery chip, and there is no structural requirement, so there is a relatively large adjustment room for the material composition. The conductivity of the current collecting structure of the internal electrode can be much higher than the conductivity of the commonly used nickel electrode material. For example, the conductivity of the nickel electrode is about 250 S / cm, but the current collecting coating layers of silver and nickel are 6×10 5 S / cm and 1×10 5 A conductivity of 1000 S / cm can be achieved. Under the same conditions, the wiring resistance of the side current collector coating layer made of silver (Ag) material is about 17 mOhm, and the wiring resistance of the side current collector coating layer made of nickel (Ni) material is about 100 mOhm (for an example with a width of 1 cm, a thickness of 1 mm, and a length of 10 cm). Both are significantly smaller than the current collection resistance of the nickel electrode, which is about 400 mOhm. As is clear, by using such an internal electrode current collection structure, it is believed that the current collection resistance of the internal electrodes of the battery chip can be significantly reduced at a relatively low cost.

[0067] 7) The battery chip may adopt a tapered shape design, that is, the working surface of the battery chip in the high temperature region is wider, but the width of the battery chip is gradually narrowed toward the low temperature region of the battery chip along the airflow direction of the internal electrode. Such a tapered design allows the battery chip to maximize the working area in the high temperature region, and the heat conduction cross-sectional area of ​​the battery chip is gradually reduced in the transition region from high temperature to low temperature. The heat loss caused by the heat conduction of the battery chip is also mitigated, so that the power output of the battery chip can be effectively improved. Test results show that the output power of a single cell adopting a tapered design is up to about 10% higher than that of a single cell adopting a rectangular equal width design. However, the tapered battery chip design leads to an increase in the airflow resistance of the internal electrode, that is, the pressure drop when the gas of the internal electrode flows through the battery chip is increased. Actual tests and fluid dynamics simulation calculations have shown that when the angle α between the hypotenuse of the tapered shape of the battery chip and the straight side of the high-temperature region is in the range of 5° to 60°, and preferably in the range of 10° to 30°, the voltage drop of the internal current flowing within the battery chip is relatively small.

[0068] According to different functions, the battery chip of the present invention should include the following components, among which, the structural members located outside the battery chip and directly or indirectly attached on the electrolyte other than the intermediate layer are called the outer surface members of the battery chip, and the functions and material compositions of each member are as follows:

[0069] 1) Internal electrode plates and external electrode plates: These are connection members for realizing electrical connection between the internal and external electrodes of the battery chip and external devices, and are preferably made of a material having relatively high electrical conductivity and anti-oxidation properties, such as silver (Ag), nickel (Ni), gold (Au), platinum (Pt), rhodium (Ph), palladium (Pd), chromium (Cr), tungsten (W), etc.

[0070] 2) Internal electrode: The gas flowing through the internal electrode electrochemically reacts to provide a place for the electrochemical process of the internal electrode to occur, provide the structural strength of the entire battery chip, and at least partially provide a current transport path for the internal electrode. The internal electrode may include different sub-layers, which respectively realize three functions of electrochemical reaction, strength support, and current transport. The different internal electrode sub-layers are composed of materials with similar compositions, and preferably the internal electrode includes two sub-layers, an active internal electrode and a supporting internal electrode. The components of the active internal electrode are designed to be favorable for electrochemical reaction, for example, 50-60% 8YSZ and 40-50% metallic nickel (Ni), and the components of the supporting internal electrode are designed to be favorable for electron transport and strength support of the battery chip, for example, 30-50% 3YSZ and 50-70% Ni are used. The inner electrode is based on the basic composition of Ni and YSZ, and may contain small amounts of other additives, such as platinum, cerium oxide, aluminum oxide, magnesium oxide, lanthanum oxide, strontium titanate, or composites based on these additives. The content of these additives is usually less than 5%, but they can provide the inner electrode with better electrochemical activity and better high temperature stability.

[0071] 3) Gas flow path: Provides the internal electrode with a passage for supplying raw materials and removing products required for the electrode process. The gas flow paths are distributed throughout the internal electrode and extend to the edge of the battery chip. The equivalent diameter of a single gas flow path is in the range of 20-200 μm, preferably in the range of 30-60 μm. In this way, even if a gas flow path is provided throughout the internal electrode, it is ensured that the strength of the internal electrode is not significantly reduced. The thicker the internal electrode in which such regular micro gas flow paths are arranged, the more gas flow paths it contains, and the greater the gas supply amount and strength of the battery chip.

[0072] 4) Electrolyte: A separator between the internal and external electrodes that provides the ion passages necessary for the electrode reaction to continue. The smaller the electronic conductivity of the electrolyte, the better, and the higher the airtightness, the better. The electrolyte is preferably based on doped stabilized zirconia, and in particular, yttrium oxide stabilized zirconium oxide (YSZ).

[0073] 5) Internal current collector: A member that is bonded to the internal electrode or is itself a part of the internal electrode, and provides a high-speed electron transport path required for the electrode reaction of the internal electrode. The internal current collector, which is made of an appropriate material and arranged at an appropriate position, can effectively increase the overall electrical conductivity of the internal electrode, thereby reducing the internal resistance of the battery chip, especially the internal resistance of the current collector. Preferably, the internal current collector is made of a high-temperature oxidation-resistant metal material or alloy that has a higher electronic conductivity than the internal electrode, such as silver (Ag), nickel (Ni), gold (Au), platinum (Pt), rhodium (Ph), palladium (Pd), chromium (Cr), tungsten (W), or an oxide that has high-temperature electrical conductivity under a reducing atmosphere, such as strontium titanate. Preferably, the internal current collector is arranged on the side of the battery chip, not on the end surface where gas enters and leaves the battery chip, or can be arranged in other parts of the battery chip, such as the battery chip surface where the external electrode is located. The internal current collector can be a dedicated battery chip component, or the internal electrode itself can carry this function.

[0074] 6) Internal busbar: An electron transport passage that connects the internal collector and the plate of the internal electrode. Since the internal electrode needs to pass current, the internal busbar generally has a relatively large cross-sectional area and a relatively high electrical conductivity, thereby ensuring a relatively small electrical resistance during electron transport. Preferably, the internal busbar has a higher electronic conductivity than the internal electrode, and the material composition is a high-temperature oxidation-resistant metal, such as silver (Ag), nickel (Ni), gold (Au), platinum (Pt), rhodium (Ph), palladium (Pd), chromium (Cr), tungsten (W), copper (Cu), and alloys thereof, and a composite of these metal materials and oxides having high temperature conductivity, such as strontium titanate, doped stabilized cerium oxide, doped stabilized zirconia oxide, and other high-temperature conductive oxide materials.

[0075] 7) Intermediate layer: A member that promotes contact between the outer surface members of the battery chip and the electrolyte, and reduces or avoids the reaction between these outer surface members and the electrolyte at high temperatures. Due to the high temperature sintering of the battery chip, the electrolyte is usually relatively dense and smooth, which is disadvantageous in realizing and maintaining good contact between the outer surface members of the battery chip and the electrolyte. In addition, the temperature is relatively high during the manufacturing process and use process of the battery chip. For example, during the manufacturing process of the battery chip, the maximum temperature can reach 1500°C, and the long-term use of the battery can be maintained at a high temperature range of 500 to 1000°C. Under such conditions, the outer surface members of the battery chip are likely to react with the electrolyte, resulting in a decrease in the performance of the battery chip. Therefore, by introducing one layer of intermediate layer, these problems can be avoided or alleviated. The intermediate layer not only maintains chemical stability with respect to the electrolyte and each outer surface member of the battery chip at high temperatures, but also has a relatively rough surface after manufacturing to realize good contact with each outer surface member. The intermediate layer can be fabricated not only between the external electrode and the electrolyte, but also between all battery chip outer surface components and the electrolyte, which can include the following: external electrodes, inner / outer electrode plates, inner / outer bus bars, inner / outer fluid collectors, protective layers, sealing structures, etc. Preferably, the material of the intermediate layer is made of doped stabilized cerium oxide (e.g., SDC or GDC) or a composite material of doped stabilized cerium oxide (e.g., SDC or GDC) and doped stabilized zirconium oxide (e.g., YSZ or ScYSZ).

[0076] 8) External electrode: The gas flowing outside the battery chip undergoes an electrochemical reaction, providing a reaction site for the electrode process of the external electrode. Preferably, the external electrode material can be a composite material composed of cerium oxide stabilized by doping and an antioxidant metal such as Ag, Pt, Pd, or a known electrode material of solid oxide battery technology, such as an oxide or a composite material based on the oxide, such as LaSrMnO, LaSrCoFeO, LaNiFeO, etc. In addition, the manufacturing process of the external electrode can include various known electrode strengthening processes, such as impregnation with active oxides.

[0077] 9) External current collector: A member that is attached to the external electrode or is itself a part of the external electrode, and provides a high-speed electron transport path required for the electrode reaction with the external electrode. Preferably, the external current collector is made of a composite of a high-temperature oxidation-resistant metal, such as silver (Ag), nickel (Ni), gold (Au), platinum (Pt), rhodium (Ph), palladium (Pd), chromium (Cr), tungsten (W), etc. and alloys thereof, and an oxide having high-temperature conductivity, such as strontium titanate, doped stabilized cerium oxide, doped stabilized zirconia oxide, etc., having high-temperature conductivity. Preferably, the external current collector is disposed on the outer surface of the external electrode, or it can be located on the inner surface, i.e., between the external electrode and the electrolyte, or between the external electrode and the intermediate layer. Preferably, the external current collector is in the form of a grid to enhance the current collection effect.

[0078] 10) Protective layer: a structure that directly or indirectly covers each external member including the external electrode to provide protection therefor. External members that may be covered by the protective layer include external electrodes, electrode plates of internal / external electrodes, internal / external current busbars, internal / external current collectors, protective layers, side seal members, and sealing structures. The protective layer can enhance the high-temperature stability of each external member of the battery chip including the external electrode by suppressing the volatilization and outflow of active ingredients, or enhance the resistance of each external member to external gas impurities (e.g., dust or water vapor) or gas impurities (e.g., aromatic hydrocarbons, silane, CO, etc.) that are likely to poison and deactivate other battery chip external members by physical filtration or chemical absorption methods, thereby improving the stability of the operation of the battery chip and effectively extending the service life of the battery chip. Preferably, the protective layer can be made of oxide and / or metal materials that can maintain stable properties under high-temperature conditions, such as aluminum oxide, zirconium oxide, cerium oxide, silicon oxide, platinum, palladium, and rhodium.

[0079] 11) External busbar: An electron transport passage that connects the external current collector and the plate of the external electrode. Since it is necessary to pass the external electrode current, the external busbar generally has a relatively large cross-sectional area and a relatively high electrical conductivity, which ensures that the resistance during electron transport is relatively small. Preferably, the external busbar is made of a composite of a metal or alloy thereof having a higher electronic conductivity than the external electrode material, such as silver (Ag), nickel (Ni), gold (Au), platinum (Pt), rhodium (Ph), palladium (Pd), chromium (Cr), tungsten (W), copper (Cu), etc., and an oxide material having high temperature electrical conductivity, such as strontium titanate, doped stabilized cerium oxide, doped stabilized zirconia oxide, etc.

[0080] 12) Side seal member: a structure for isolating and sealing the non-gas inlet / outlet end surface of the battery chip, which may include a multiple sub-layer structure. Preferably, it includes two side seal sub-layers, an inner one and an outer one, and the inner side seal layer covers the side surface of the internal electrode of the battery chip and is located between the internal electrode and the outer side seal layer, increasing the resistance of the airflow of the internal electrode leaking from the side edge of the battery chip, realizing excellent contact with the outer side seal layer, and further maintaining chemical stability with the outer side seal layer, so that the structures of both are not destroyed by chemical reaction even at high temperatures. Preferably, the material of the inner side seal layer is graphite (C) or magnesium silicate talc material, such as (Mg6)[Si8]O 20 (OH)4, etc. can be used. The side seal outer layer is the outermost layer of the battery chip side seal member, and is a dense sealing structure that prevents gas flowing through the gas flow path of the internal electrode from leaking outside the battery chip. Preferably, the side seal outer layer is made of a material based on graphite or potash-lime glass. For example, when using potash-lime glass, the preferred range of the compounding ratio of the components is: K2O 12-18%, CaO 5-12%, SiO2 60-75%.

[0081] It should be noted here that the components are defined by their different functions and are not differentiated by their different positions or material compositions. In the course of implementation, the different functional components are manufactured from similar, even the same, materials and by the same manufacturing process. In such cases, the different components may also have the same or similar structural features, so that they are indistinguishable in terms of their microstructural features. For example, the external electrodes, the external current collectors, and the external busbars may be manufactured from the same material, e.g., the same type of material, e.g., a composite material consisting of 70% Ag and 30% SDC, and by the same manufacturing process, e.g., the same operational steps, e.g., screen printing, even though they perform different functions.

[0082] Compared with the prior art, the present invention has the following advantages:

[0083] 1. The regular microchannels embedded in the internal electrode significantly reduce the air flow resistance of the gas flowing through the internal electrode, and the regular microchannels distributed in the internal electrode contribute to the gas flowing through the internal electrode being uniformly distributed over the entire electrolyte and electrode interface area, which makes the electrode reaction more efficient and increases the electrical efficiency of the battery chip.

[0084] 2. The internal electrode may include multiple sub-layers, e.g., an active internal electrode and a supporting internal electrode, of which the active internal electrode is advantageous in terms of composition for electrical and chemical reactions, and the supporting internal electrode is advantageous in terms of composition for improving the overall strength and / or conductivity of the battery.

[0085] 3. The internal electrode can also serve as a support between the two layers of electrolyte, ensuring a relatively high yield even if the thickness of the electrolyte is relatively thin.

[0086] 4. The side seal layer has a multi-layer structure, and the inner sub-layer can increase the leakage resistance of the gas flowing through the internal electrode. The material of the outer sub-layer has a different composition and structure from the material of the inner sub-layer, which can achieve better sealing against leaking gas after decompression and better maintain the structural strength. [Brief description of the drawings]

[0087] [Figure 1] FIG. 1 is a schematic cross-sectional view of one stack unit of a known typical solid oxide battery.

[0088] [Diagram 2] FIG. 2 is a plan view of the structure according to the first embodiment of the present invention.

[0089] [Diagram 3] FIG. 3 is a structural diagram of an end portion of the first embodiment of the present invention as seen from a side.

[0090] [Figure 4] FIG. 4 is a schematic cross-sectional view of the first embodiment of the present invention.

[0091] [Diagram 5] FIG. 5 is a plan view of the structure according to the second embodiment of the present invention.

[0092] [Figure 6] FIG. 6 is an exploded view of the second embodiment of the present invention.

[0093] [Figure 7] FIG. 7 is a plan view of the structure according to the third embodiment of the present invention.

[0094] [Figure 8] FIG. 8 is a plan view of the fourth embodiment of the present invention.

[0095] In the figure, 1 is an electrolyte, 2 is an inner electrode, 201 is a supporting inner electrode, 202 is an active inner electrode, 3 is an outer electrode, 4 is a side seal member, 401 is a side seal inner layer, 402 is a side seal outer layer, 5 is an intermediate layer, 6 is an inner electrode plate, 7 is an outer electrode plate, 8 is an inner bus bar, 9 is an outer bus bar, 10 is a sealing structure, 11 is a gas flow path, 12 is an outer current collector, 13 is a protective layer, 14 is an inner current collector, and 15 is a connecting piece. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0096] The following are specific examples of the present invention, and the technical configurations of the present invention will be further described with reference to the drawings. However, the present invention is not limited to these examples.

[0097] EXAMPLES

[0098] 2 and 3, the present embodiment 1 is a solid oxide battery chip, and the battery chip uses a rectangular long sheet structure to include two layers of electrolyte 1 separated from each other in the thickness direction. An internal electrode 2 is disposed between the two layers of electrolyte 1, and both sides of the internal electrode 2 are covered with side seal members 4, and an external member is provided on the outer surface of the electrolyte 1. The external member includes an intermediate layer 5, an external electrode 3, an internal electrode plate 6, and an external electrode plate 7, and the internal electrode 2 is connected to the internal electrode plate 6, and the external electrode 3 is connected to the external electrode plate 7.

[0099] Referring to FIG. 4, the internal electrode 2 is provided with regularly arranged micro gas flow channels 11, and the side seal member 4 includes two sub-layers, namely, a side seal inner layer 401 and a side seal outer layer 402, and the materials of the side seal inner layer 401 and the side seal outer layer 402 are different from the materials of the electrolyte 1 and the internal electrode 2, and the side seal outer layer 402 is dense and non-permeable, and the side seal inner layer 401 is rough (porous) and permeable. The internal electrode and the external electrode each have their own plate, which is for connecting the battery chip to the outside, and the plate 7 of the outer electrode and the external electrode 3 are connected by an external bus bar 9. The internal electrode 2 includes a supporting internal electrode 201 and an active internal electrode 202, and the connection between the internal electrode 2 and the plate 6 of the internal electrode is connected by an internal bus bar 8, and an external collector 12 is provided on the outer surface of the external electrode 3, and a protective layer 13 is provided on the outer surface of the external electrode 3, and the external collector 12 and the external electrode 3 are covered with a protective layer 13. The internal electrode plate 6, the external electrode plate 7, the external electrode 3, the external bus bar 9, etc. are all provided on the intermediate layer 5 and do not directly contact the electrolyte 1. The internal electrode plate 6 and the external electrode plate 7 in this Example 1 are provided at the same end of the battery chip, and the internal current collector 14 is embedded in the side seal member 4.

[0100] The manufacturing process of the battery chip of this Example 1 is as follows.

[0101] 1) Preparation of the substrate sheet. The substrate sheet can be divided into three types: supporting inner electrode substrate sheet, active inner electrode substrate sheet and electrolyte substrate sheet. The preparation process of each substrate sheet is as follows:

[0102] (a) Preparation of slurry. Ceramic fine powder, such as oxide fine powder of 8YSZ, NiO and GDC, is added with an appropriate amount of organic auxiliary and solvent, such as PVB, triethanolamine, ethanol, etc., and mixed by ball milling, and then these ceramic fine powders are uniformly dispersed and prepared into a stable slurry. In a typical active inner electrode slurry, the content of solid active components is 8YSZ:NiO:GDC=5:4:1 (weight ratio), and has a variation range of about 20%. In a typical supporting inner electrode slurry, the content of solid active components is 8YSZ:NiO:Al2O3=3.5:5.5:1 (weight ratio), and has a variation range of about 20%. The content of nickel oxide (NiO) in the supporting inner electrode is slightly higher, which makes the inner electrode have a higher conductivity after reduction. In a typical electrolyte slurry, the solid active component is 8YSZ or ScYSZ.

[0103] (b) Production of substrate sheet. The slurry in (a) is produced into a thin film of electrolyte and internal electrode in a casting device, the typical thickness of the electrolyte thin film is 5-40 μm, and the typical thickness of the internal electrode thin film is 100-200 μm. After drying the thin film at 60° C. for 2 hours, it is cut into a piece of a predetermined size, for example, 270×220 mm, which is called a substrate sheet. Correspondingly, the substrate sheet produced from the active internal electrode slurry is called the active internal electrode substrate sheet, the substrate sheet produced from the supporting internal electrode slurry is called the supporting internal electrode substrate sheet, and the substrate sheet produced from the electrolyte slurry is called the electrolyte substrate sheet.

[0104] (c) Preparation of gas flow channel precursor. The gas flow channel precursor of the battery chip is fabricated on one supporting internal electrode substrate sheet. A typical gas flow channel precursor is a slurry containing fine powder of graphite, starch, or other polymeric materials such as PTFE, PVC, etc. In these slurries, the content of solid powder such as graphite, starch, PTFE, PVC, etc. is preferably in the range of 5-30%, and the solvent is terpineol. Methods for fabricating the precursor slurry on the internal electrode substrate sheet include methods known in the industry such as screen printing and high temperature pressing.

[0105] 2) Lamination of the substrate sheets. The electrolyte substrate sheet, the active internal electrode substrate sheet, the supporting internal electrode substrate sheet containing the gas flow path precursor, and the supporting internal electrode substrate sheet not containing the gas flow path are aligned and stacked in the order shown in FIG. 4, and then placed in a vacuum bag for evacuation and sealing. The sealed vacuum bag containing the substrate sheet assembly is then placed in an isostatic press and subjected to a pressure of 20 MPa in a water bath at 75° C. for 5 minutes, and then removed. After the isostatic press process, the substrate sheets in the assembly are fused to each other to form a laminate. The thickness of the laminate is about 2 mm, and each constituent layer is partially or completely separated and cannot be made into a single substrate sheet.

[0106] 3) Cutting: The laminate produced in the above steps is set in a punching machine, and cut into battery chip blanks of a specified design shape by a punching die. Typically, one laminate is cut into three battery chip blanks with an outer shape of 65 x 260 mm.

[0107] 4) Sintering. The battery chip blank is placed in a high-temperature furnace and a suitable heat treatment schedule is selected to perform high-temperature sintering. By high-temperature sintering, for example, when sintered at 1400°C for 2 hours, the dimensions of the blank shrink by 20-30%, resulting in a battery chip with relatively high strength. At the same time, the gas flow channel precursor gas is lost during the heat treatment schedule, leaving regular and uniform micro gas flow channels embedded in the battery chip.

[0108] 5) Firing the intermediate layer. An intermediate layer is printed on the electrolyte on both sides of the fired battery chip. A typical intermediate layer material is doped cerium oxide, such as GDC or SDC, and the printing method can use a screen printing process well known in the industry. The battery chip with the printed intermediate layer is dried at 90°C for 1 hour and then placed in a high-temperature furnace, and then the furnace temperature is increased to 1300°C and fired for 2 hours, after which the furnace temperature is reduced and the cooling rate is not more than 5°C / min. When the temperature in the furnace is reduced to room temperature, the battery chip is taken out, at which time the intermediate layers on both sides are firmly fired on the outer surface of the electrolyte of the battery chip.

[0109] 6) Reduction. The battery chip with the fired intermediate layer is placed in a reduction furnace and reduced. The reducing atmosphere is a mixture of hydrogen and nitrogen gas, with a hydrogen content of 70-100% and a nitrogen content of 0-30%, and the reduction conditions are 680°C and 6 hours. After the reduction operation, the nickel oxide in the internal electrode of the battery chip is reduced to metallic nickel, which not only forms an extra gas flow path in the internal electrode, but also, since the metallic nickel formed is an electronic conductor, the reduced internal electrode has electrical conductivity and can form an electron transport path connecting the high-temperature region of the battery chip that performs the electrochemical reaction and the electrode plate of the internal electrode that is responsible for connecting with the outside.

[0110] 7) Manufacturing of external components. Print the external components of the cell on the external surface of the reduced battery chip, and these external components include an external current collector, an external electrode, an external electrode plate, an internal electrode plate, an external electrode bus bar, an internal electrode bus bar, and a protective layer, and these components can all be printed on the intermediate layer, or printed partially or entirely on the electrolyte surface. Since the battery chip has two electrolytes arranged opposite each other, the external part of one side of the battery chip can be manufactured sequentially after the external part of the other side is manufactured.

[0111] In the outer surface members of the battery chip, the components of the external current collector, the external electrode plate, the internal electrode plate, the external electrode bus bar, and the internal electrode bus bar are the same or similar, for example, the content of doped stabilized cerium oxide (SDC or GDC) is 5-20%, the content of silver is 80-95%, and they can be printed in the same screen and in the same step. The components of the external electrode are the content of doped stabilized cerium oxide (SDC or GDC) is 30-55%, the content of silver is 45-70%, and the printing can be performed before or after printing the external current collector, with a drying process between the two, and the drying conditions are hot air drying at 90°C for 1 hour. The components of the protective layer are aluminum oxide, zirconium oxide, silicon dioxide, or various composite materials based on oxides, with the preferred component being aluminum oxide, and the slurry made from these oxides is printed or spray-coated on other outer surface members after drying. The various slurries used in this step can use a mixture of ethanol and terpineol as the solvent and further contain about 0-10% graphite as a pore former.

[0112] 8) Manufacturing of internal collector. Internal collector is manufactured for battery chips on which external electrodes and other components are printed. First, internal collector slurry is applied to the side of the battery chip. The basic components are 5-20% stabilized cerium oxide (SDC or GDC) content by doping and 80-95% silver content. The electric cell with the internal collector applied is dried with hot air at 90°C for 1 hour to harden the slurry.

[0113] 9) Manufacture of side seal members. The side seal inner layer is applied to the battery chip after the above process. The side seal inner layer can be applied on the inner current collector coating layer, and its basic components are graphite or magnesium silicate talc material ((Mg6)[Si8]O 20(OH)4. The side seal inner layer is dried with hot air at 90℃ for 1 hour, and then the side seal outer layer is applied on top of the side seal inner layer. The basic material is graphite or potassium lime glass, with the composition being 12-18% K2O, 5-12% CaO, and 60-75% SiO2.

[0114] 10) Heat treatment. The battery chips on which the printing of the outer surface members and the application of the side seal members are completed are heat treated. After the heat treatment, each outer surface member and its attachment form a strong connection, and at least the outermost layer of the side seal member is densified. The preferred heat treatment schedule is 850°C for 1 hour, the atmosphere is a reducing protective atmosphere, the hydrogen content is 5-60%, and the balance gas is nitrogen.

[0115] 11) Electrode strengthening. The heat-treated battery chip can be used in practical applications, and the electrode can be strengthened to further improve the electrical properties of the battery chip and reduce the internal resistance. A typical electrode strengthening method is impregnation. Take the impregnation of SDC (samaria doped ceria) as an example, firstly, Sm(NO3)2 and Ce(NO3)4 are dissolved in an aqueous solution (or diluted nitric acid with a pH of about 5) according to a certain Sm2O3:CeO2 (e.g., Sm2O3:CeO2 with a molar ratio of 20:80), and then the solution is applied onto the internal and external electrodes and subjected to a heat treatment at elevated temperature (e.g., heat treatment at 500°C or 300°C for 20 minutes). Sm(NO3)2, Ce(NO3)4 decompose to form a doped and stabilized compound SDC with a certain ratio of Sm2O3:CeO2. This process can be repeated 3-5 times to increase the impregnation amount of SDC. SDC is a known oxide with excellent catalytic activity and mixed ionic / electronic conductivity. After impregnation, SDC can be dispersed in the electrode with very small nanometer scale, e.g., less than 100 nanometers, and the reaction area of ​​the electrode process, i.e., the triple phase boundary (TPB), i.e., the gas-solid electrochemical site, can be greatly enlarged, which significantly reduces the resistance of the electrode process and reduces the internal resistance of the battery chip. This is a well-known technique in the industry.

[0116] EXAMPLES

[0117] 5 and 6, the structure of the present embodiment 2 is basically the same as that of the embodiment 1, with the following differences: the intermediate layer 5 can be coated on the entire outer wall surface of the electrolyte 1, or can be partially coated on the electrolyte 1. The internal electrode plate 6 connected to the internal electrode 2 and the external electrode plate 7 connected to the external electrode 3 are respectively disposed on both ends of the battery chip, and the internal bus bar 8 is located on the end face of the battery chip.

[0118] EXAMPLES

[0119] Referring to FIG. 7, the structure of the present embodiment 3 is basically the same as that of the embodiment 2, with the following differences: the battery chip of the embodiment 3 adopts a tapered design at both ends, and the included angle α between the oblique side of the tapered shape and the straight side of the high temperature region is in the range of 5°-60°, preferably in the range of 10°-30°. When the battery chip is operated, the temperature of the gas inlet and outlet of the internal electrode 2 is at least 200°C different from the temperature of the center of the external electrode, and the above design can better meet the above operating conditions. The external current collector 12 of the present embodiment 3 is located on the outer surface of the external electrode 3, and a connecting piece 15 for external connection is welded onto the electrode plate 7 of the external electrode. Preferably, the connecting piece 15 is made of copper, nickel, gold, or silver.

[0120] EXAMPLES

[0121] Referring to FIG. 8, the structure of the present embodiment 4 is basically the same as that of the embodiment 3, with the difference being that the internal busbar 8 of the embodiment 4 is provided on the surface of the battery chip, and its high-temperature area penetrates the opening on the surface of the electrolyte 1 to connect with the internal electrode 2, and the surface of the opening of the electrolyte 1 is further covered with a layer of the sealing structure 10, which penetrates into the electrolyte 1 and completely covers the opening of the electrolyte 1, and completely covers the joining and connecting point of the internal busbar 8 and the internal electrode 2, thereby ensuring that the gas flowing through the internal electrode does not leak out of the battery chip through this opening.

[0122] The specific embodiments described in this specification are merely illustrative of the spirit of the present invention. Those skilled in the art to which the present invention pertains may make various modifications or additions to the specific embodiments described, or replace them with similar methods, without departing from the spirit of the present invention or beyond the scope defined in the appended claims.

Claims

1. A solid oxide cell chip having a dual electrolyte structure with two operation modes, a solid oxide fuel cell and a solid oxide electrolysis cell, two electrolyte layers, the two electrolyte layers being separated by an internal electrode sandwiched therebetween; A plurality of gas flow paths are provided inside the internal electrode and are regularly arranged, and at least two side surfaces of the non-gas flow path inlet / outlet of the internal electrode are covered with a side seal member; an outer surface member is provided on an outer surface of the electrolyte layer, the outer surface member including an intermediate layer, an outer electrode, an inner electrode plate, and an outer electrode plate; The outer surface is a surface of the electrolyte layer not adjacent to the internal electrode, the intermediate layer is provided so as to cover all or at least a part of the outer surface of the electrolyte layer; the internal electrode is connected to a plate of the internal electrode, and the external electrode is connected to a plate of the external electrode; the external electrode and the electrolyte layer are separated by the intermediate layer; The side seal member includes at least a side seal outer layer which is a single dense, non-breathable sub-layer; and a side seal inner layer, which is a single breathable sub-layer; the side seal inner layer covers a side surface of the internal electrode, The side seal inner layer is located between the internal electrode and the side seal outer layer.

4. A solid oxide cell chip having the dual electrolyte structure.

2. The solid oxide cell chip having a dual electrolyte structure according to claim 1, characterized in that the equivalent diameter of a cross section of a single gas flow path in the plurality of gas flow paths regularly arranged inside the internal electrode is within a range of 20 to 200 μm.

3. 2. The solid oxide cell chip having a dual electrolyte structure according to claim 1, wherein the external member further comprises a plurality of external current collectors covering the outer surfaces of the external electrodes, and the electrical conductivity of the external current collectors is not lower than the electrical conductivity of the external electrodes.

4. The outer surface member further includes a protective layer.

2. The solid oxide cell chip having a dual electrolyte structure according to claim 1, wherein said protective layer covers at least one of the outer surface members.

5. The internal electrodes and the plates of the internal electrodes are connected by internal bus bars, The electrical conductivity of the internal busbar is not lower than the electrical conductivity of the internal electrodes.

2. A solid oxide cell chip having the dual electrolyte structure according to claim 1.

6. 6. The solid oxide cell chip having a dual electrolyte structure according to claim 5, wherein the internal bus bar is located between a side seal member and a side surface of the cell chip.

7. the internal busbar is at least partially disposed on one surface of the electrolyte where the external electrodes are located, and is connected to the internal electrodes through openings in the electrolyte; 6. The solid oxide cell chip having a dual electrolyte structure according to claim 5, wherein a surface of the opening of the electrolyte is covered with a single-layer sealing structure, completely covering and sealing a joining connection point of the internal bus bar and the internal electrode at the opening of the electrolyte.

8. The cell chip has a long sheet shape, 2. The solid oxide cell chip with a dual electrolyte structure according to claim 1, wherein the outer shape of the cell chip gradually narrows from the external electrode region in the center of the cell chip toward the end face having the gas flow path inlet and outlet, and the angle between the oblique side of the tapered shape and the straight side of the external electrode region in the center of the cell chip is within the range of 5° to 60°.

9. Step (1) Preparation of a substrate sheet: Adding appropriate auxiliary agents and solvents to the components constituting the internal electrodes and electrolytes according to the ratio, and then preparing a thin substrate sheet by casting; Step (2) Lamination of substrate sheets: After stacking the electrolyte substrate sheet, the internal electrode substrate sheet including the gas flow path, and the internal electrode substrate sheet not including the gas flow path in a certain order, placing the assembly in a vacuum bag, drawing a vacuum and sealing the bag, and fusing the assembly of base sheets placed in the vacuum bag by high-temperature compression to form a laminate; Step (3) Cutting: placing the laminate in a punching device and cutting it into cell chip blanks having a specified design shape; Step (4) sintering: placing the cell chip blank in a high-temperature furnace and sintering it according to a suitable heat treatment schedule, after sintering, the cell chip blank shrinks in size and becomes a cell chip with relatively high strength, and the gas flow path precursor is vaporized and escaped during the heat treatment schedule, leaving regular and uniform embedded gas flow paths in the internal electrodes of the cell chip; Step (5) sintering the intermediate layer: fabricating an intermediate layer on the electrolyte on both sides of the sintered cell chip by high-temperature heat treatment; Step (6) reduction: placing the cell chip with the fired intermediate layer in a reduction furnace and reducing the nickel oxide in the internal electrodes to metallic nickel; Step (7) Manufacturing an external member: printing an external member on the external surface of the reduced cell chip; Step (8) Manufacturing side seal members: manufacturing side seal members for the cell chips that have completed the above steps, first manufacturing a rough and air-permeable side seal inner layer, and then manufacturing a dense and air-impermeable side seal outer layer on top of the side seal inner layer after the side seal inner layer is dried; Step (9) heat treatment: heat treatment is performed on the cell chip after the printing of the outer surface member and the manufacturing of the side seal member. After the heat treatment, each outer surface member and its attachment form a strong connection, and the side seal member has at least one layer of densified structure; A method for manufacturing a solid oxide cell chip having a dual electrolyte structure according to any one of claims 1 to 8, comprising the steps of: (10) strengthening the electrodes;

Citation Information

Patent Citations

  • Solid oxide fuel cell

    JP2006277969A

  • Method of manufacturing solid-oxide fuel cell, and method of manufacturing molded body of divided body of the same cell

    JP2011134537A

  • Method of manufacturing solid oxide fuel cell

    JP2014007061A