Semiconductor device manufacturing method and semiconductor manufacturing apparatus

By forming a 750 nm thick inorganic film on SiC wafers and using dummy and monitor wafers to stabilize the oxidation process, the method addresses variations in oxide film thickness, achieving uniformity and reducing deviations to 0.8 nm or less.

JP7565885B2Active Publication Date: 2024-10-11MITSUBISHI ELECTRIC CORP

Patent Information

Application Number
JP2021122358
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-07-27
Publication Date
2024-10-11
Estimated Expiration
2041-07-27

AI Technical Summary

Technical Problem

Conventional methods have not adequately addressed variations in the thickness of thermal oxide films among multiple silicon carbide (SiC) wafers during semiconductor manufacturing.

Method used

A method involving the formation of a first inorganic film on the lower surface of SiC wafers, followed by etching and thermal oxidation treatment, with the use of a SiC dummy wafer and a Si monitor wafer to control the oxidation process, ensuring the inorganic film remains at least 750 nm thick to stabilize the oxide film thickness.

Benefits of technology

This method effectively suppresses variations in oxide film thickness among SiC wafers, enhancing in-plane uniformity and reducing thickness deviations to 0.8 nm or less, thereby improving semiconductor device consistency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565885000001
    Figure 0007565885000001
  • Figure 0007565885000002
    Figure 0007565885000002
  • Figure 0007565885000003
    Figure 0007565885000003
Patent Text Reader

Abstract

To provide a manufacturing method of semiconductor devices capable of suppressing variations in thickness of oxide films among multiple SiC wafers.SOLUTION: The manufacturing method of semiconductor devices includes steps of: performing etching on multiple silicon carbide wafers so that the thickness of a first inorganic film remains at least 750nm after forming the first inorganic film on the underside of the multiple silicon carbide wafers; and forming an oxide film on the upper surface of the multiple silicon carbide wafers by performing thermal oxidation treatment after the etching. The thermal oxidation treatment is performed in a state where at least one wafer including at least one of a dummy wafer or a monitor wafer and the multiple silicon carbide wafers are arranged along one direction with the upper surfaces of the multiple silicon carbide wafers are directed in the one direction. In the state of thermal oxidation treatment, a first silicon carbide wafer out of the multiple silicon carbide wafers is positioned directly under at least one of the wafers and a second silicon carbide wafer out of the multiple silicon carbide wafers is arranged directly under a third silicon carbide wafer out of the multiple silicon carbide wafers.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing a semiconductor device and a semiconductor manufacturing apparatus. [Background technology]

[0002] Patent Documents 1 and 2 disclose methods for suppressing variations in thickness of oxide films among a plurality of silicon carbide (hereinafter also referred to as SiC) wafers when oxide films are formed on the plurality of SiC wafers. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-165348 A [Patent Document 2] Patent No. 6141130 Summary of the Invention [Problem to be solved by the invention]

[0004] The techniques in the prior art were not necessarily sufficient for suppressing the variation in thickness of the thermal oxide film among a plurality of SiC wafers.

[0005] The present disclosure is made to solve the above problems, and has an object to provide a method for manufacturing a semiconductor device that can suppress variations in oxide film thickness among multiple SiC wafers. [Means for solving the problem]

[0006] The present disclosure OneA method for manufacturing a semiconductor device includes forming a first inorganic film on lower surfaces of a plurality of silicon carbide wafers, etching the plurality of silicon carbide wafers after the formation of the first inorganic film, performing the etching such that a thickness of the first inorganic film of the plurality of silicon carbide wafers remains at 750 nm or more after the etching, performing a thermal oxidation process using a semiconductor manufacturing apparatus after the etching to form an oxide film on upper surfaces of the plurality of silicon carbide wafers, and performing the thermal oxidation process in a state in which at least one wafer including at least one of a dummy wafer or a monitor wafer, the at least one wafer being different from the plurality of silicon carbide wafers, and the plurality of silicon carbide wafers are arranged along one direction and with upper surfaces of the plurality of silicon carbide wafers facing in one direction, and in a state in which a first silicon carbide wafer of the plurality of silicon carbide wafers is arranged directly below any one of the at least one wafers, and a second silicon carbide wafer of the plurality of silicon carbide wafers is arranged directly below a third silicon carbide wafer of the plurality of silicon carbide wafers. In each of the silicon carbide wafers, the upper surface is a Si surface and the lower surface is a C surface, and etching is performed by wet etching using a dip method. The present invention relates to a method for manufacturing a semiconductor device. Effect of the Invention

[0007] The present disclosure provides a method for manufacturing a semiconductor device that can suppress variations in thickness of oxide films among a plurality of SiC wafers. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a diagram showing a vertical batch-type diffusion furnace according to a first embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing a state near a SiC wafer during thermal oxidation treatment. [Diagram 3] FIG. 2 is a diagram showing a schematic diagram of a crystal structure of a SiC wafer. [Figure 4] 2 is a diagram showing the inside of a cell of the semiconductor device of the first embodiment; FIG. [Diagram 5] 2 is a diagram showing a cell periphery of the semiconductor device of the first embodiment. FIG. [Figure 6] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device of the first embodiment. [Figure 7]1 is a cross-sectional view showing a state during the manufacture of the semiconductor device of the first embodiment. [Figure 8] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device of the first embodiment. [Figure 9] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device of the first embodiment. [Figure 10] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device of the first embodiment. [Figure 11] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device of the first embodiment. [Figure 12] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device of the first embodiment. [Figure 13] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device of the first embodiment. [Figure 14] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device of the first embodiment. [Figure 15] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device of the first embodiment. [Figure 16] 1 is a cross-sectional view showing a state during the manufacture of the semiconductor device of the first embodiment. [Figure 17] 3 is a flowchart of a method for manufacturing the semiconductor device according to the first embodiment. [Figure 18] FIG. 13 is a diagram showing the relationship between the thickness of an interlayer insulating film formed on a C-face of a SiC wafer and the variation in thickness of a gate oxide film between SiC wafers. [Figure 19] FIG. 11 is a diagram showing an arrangement of wafers in the second embodiment. [Figure 20] FIG. 11 is a diagram showing a vertical batch-type diffusion furnace according to a third embodiment. [Figure 21] FIG. 13 is a diagram showing a vertical batch-type diffusion furnace according to a fourth embodiment. [Figure 22] FIG. 13 is a diagram showing an example of a vertical batch-type diffusion furnace according to a fifth embodiment. [Figure 23] FIG. 13 is a diagram showing an example of a vertical batch-type diffusion furnace according to a fifth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] <Prerequisite technology> 1 is a diagram showing the configuration of a vertical batch-type diffusion furnace 80, which is an example of a vertical batch-type diffusion furnace used in each embodiment. In each embodiment described later, an oxide film is formed on a SiC wafer 50 that becomes a silicon carbide semiconductor device by using, for example, the vertical batch-type diffusion furnace 80 shown in FIG.

[0010] The vertical batch-type diffusion furnace 80 includes a tube 81, a boat 82, and a gas introduction line 83. The boat 82 includes a plurality of support parts 82a for supporting wafers. The tube 81 is a container for performing thermal oxidation treatment. The vertical batch-type diffusion furnace 80 supports a plurality of wafers by the plurality of support parts 82a in one direction with the main surfaces of the wafers aligned in one direction.

[0011] As shown in Fig. 1, in the thermal oxidation process, a plurality of SiC wafers 50 are supported by supports 82a and placed in a tube 81 with a gap between them. Hereinafter, a group of a plurality of SiC wafers 50 simultaneously processed in the vertical batch-type diffusion furnace 80 is called a batch. The gas introduction line 83 is a line for introducing an oxidizing gas into the tube 81. The gas introduction line 83 is provided with an opening 830, and the oxidizing gas is introduced into the tube 81 through the opening 830. The oxidizing gas is a gas used in the thermal oxidation process, such as oxygen (O2) gas or ozone (O3) gas.

[0012] In the SiC wafer 50, for example, one main surface is a carbon (C) surface and the other main surface is a silicon (Si) surface.

[0013] FIG. 1 shows an example of the arrangement of a SiC wafer 50 when a thermal oxidation process is performed.

[0014] The SiC wafers 50 are held in the boat 82 with their carbon (C) surfaces facing downward and their silicon (Si) surfaces facing upward. The SiC wafers 50 are stacked with gaps between them in a direction intersecting the principal surfaces of the SiC wafers 50, for example, in a direction perpendicular to the principal surfaces of the SiC wafers 50.

[0015] Before the thermal oxidation treatment, an inorganic film 90 (see FIGS. 2 and 3) is formed on the C-face 12, which is the lower surface of each SiC wafer 50.

[0016] A SiC dummy wafer 51 is placed on the topmost SiC wafer 50 among the SiC wafers 50 with a gap therebetween. A Si monitor wafer 52 is placed on the SiC dummy wafer 51 with a gap therebetween.

[0017] An inorganic film 90 is formed on the lower surface of the SiC dummy wafer 51, similarly to the lower surface of the SiC wafer 50 in Fig. 2. The reason for providing the SiC dummy wafer 51 will be described later.

[0018] After the thermal oxidation process is completed, the thickness of the oxide film on the Si monitor wafer 52 is measured to check whether there is a problem with the oxide film formed on each SiC wafer 50.

[0019] When O2 gas is used as the oxidizing gas, the thermal oxidation reaction in the SiC wafer 50 is estimated to be as shown in the following formula (1). In each formula shown below, "(↑)" means that gas is generated.

[0020] SiC+2O2=SiO2+CO2(↑) …(1) As shown in formula (1), in the thermal oxidation reaction in the SiC wafer 50, a silicon dioxide (SiO2) film is formed and carbon dioxide (CO2) gas is generated. It is presumed that the generated CO2 gas is reversibly decomposed in the high temperature environment in the tube 81 and undergoes the reaction shown in formula (2) below, whereby carbon monoxide (CO) gas is discharged and O2 gas is generated again.

[0021] 2CO2=2CO(↑)+O2(↑) …(2) Fig. 2 is a cross-sectional view showing a state near the SiC wafer 50 during thermal oxidation treatment. Fig. 3 is a diagram showing a schematic crystal structure of the SiC wafer 50.

[0022] 3, the crystal structure of a SiC wafer 50 is composed of silicon (Si) atoms 45 and carbon (C) atoms 46. One main surface of the SiC wafer 50 is a C-face 12 where the C atoms 46 are exposed, and the other main surface is a Si-face 13 where the Si atoms 45 are exposed.

[0023] As shown in Fig. 2, when O2 gas is supplied to a SiC wafer 50 to form an oxide film 5a, CO2 gas is generated by the reaction of formula (1). As shown in Fig. 3, there are more C atoms 46 on the C-face 12 side of the SiC wafer 50 than on the Si-face 13 side. Therefore, it is considered that the C-face 12 generates more CO2 gas than the Si-face 13.

[0024] As described above, an inorganic film 90 is formed on the C-face 12 of the SiC wafer 50. The inorganic film 90 provided on the C-face 12 of the SiC wafer 50 has the effect of suppressing the reaction (1) on the C-face 12 of the SiC wafer 50. When the inorganic film 90 is thin, the effect of suppressing the reaction of the above-mentioned formula (1) is small, and therefore the degree to which the reaction of formula (2) is suppressed is small, and the effect of increasing the oxygen concentration due to the reaction of formula (2) directly below the C-face 12 of the SiC wafer 50 is large. Therefore, when the C-face 12 of the SiC wafer 50 faces the Si-face 13 of the adjacent SiC wafer 50 as shown in FIG. 2, it is considered that the oxide film 5a formed by the thermal oxidation process becomes thick on the Si-face 13 of the SiC wafer 50 arranged directly below the SiC wafer 50. In addition, since the effect of the oxygen generated by reaction (2) varies depending on the position on the wafer surface, the degree to which the oxidation reaction occurs becomes non-uniform within the surface, and it is considered that in the SiC wafer 50 disposed directly below the SiC wafer 50, the thickness of the oxide film 5a formed by the thermal oxidation process varies depending on the position on the surface.

[0025] In the arrangement of FIG. 1, consider a case where the inorganic film 90 formed on the C-face 12 of the SiC wafer 50 is thin and the SiC dummy wafer 51 is not placed between the Si monitor wafer 52 and the SiC wafer 50. That is, consider a case where the SiC wafer 50 is also placed at the position of the SiC dummy wafer 51 in FIG. 1. Since the reaction of formula (1) does not occur in the Si monitor wafer 52, the reaction of formula (2) does not occur due to the presence of the Si monitor wafer 52, and O2 gas is not generated. In this case, the oxide film 5a formed by the thermal oxidation process is thinner in the SiC wafer 50 immediately below the Si monitor wafer 52 than in the SiC wafer 50 immediately below the SiC wafer 50. In this way, the thickness of the oxide film 5a formed on the upper surface of the SiC wafer 50 becomes non-uniform among the SiC wafers 50 in the batch.

[0026] As shown in FIG. 1, by placing a SiC dummy wafer 51 having an inorganic film 90 formed on its C-face 12 between a Si monitor wafer 52 and a SiC wafer 50, it is possible to prevent the thickness of the oxide film 5a formed by the thermal oxidation process from becoming non-uniform among the SiC wafers 50 in a batch.

[0027] An inorganic film 90 is formed on the C-face 12 of the SiC dummy wafer 51. The inorganic film 90 on the C-face 12 of the SiC dummy wafer 51 has the same thickness as the inorganic film 90 on the C-face 12 of the SiC wafer 50, for example. In this case, the same amount of CO2 gas as that generated from the C-face 12 of the SiC wafer 50 is generated from the C-face 12 of the SiC dummy wafer 51, so that it is possible to suppress the thickness of the oxide film 5a formed by the thermal oxidation process from being non-uniform among the SiC wafers 50 in the batch.

[0028] However, by repeatedly using the SiC dummy wafer 51, a thick thermal oxide film is formed on the C surface 12 of the SiC dummy wafer 51, and the inorganic film 90 becomes thicker. For this reason, the amount of O2 gas generated on the C surface 12 of the SiC dummy wafer 51 is less than that on the C surface 12 of the SiC wafer 50. The oxide film 5a formed by thermal oxidation on the upper surface of the SiC wafer 50 directly below the SiC dummy wafer 51 becomes thinner than the oxide film 5a formed by thermal oxidation on the upper surface of the SiC wafer 50 directly below the SiC wafer 50. As a result, the thickness of the oxide film 5a formed by thermal oxidation becomes non-uniform among the SiC wafers 50 within the batch.

[0029] As will be described later, in the manufacturing methods of the semiconductor devices according to Embodiments 1 to 5, when performing the thermal oxidation treatment, since a thick inorganic film 90 is formed on the C surface 12 of the SiC wafer 50, the non-uniformity of the thickness of the oxide film 5a formed by the thermal oxidation treatment among the SiC wafers 50 within the batch is suppressed.

[0030] In the above description, the explanation was made based on the presumption that the reactions of Formula (1) and Formula (2) occur, but the effects of the manufacturing methods of the semiconductor devices according to Embodiments 1 to 5 are not limited to suppressing the influence by the reactions of Formula (1) and Formula (2). The atmosphere above a certain SiC wafer 50 can vary depending on whether the wafer above the SiC wafer 50 is a Si monitor wafer 52, a SiC dummy wafer 51, or a SiC wafer 50. In the manufacturing methods of the semiconductor devices according to Embodiments 1 to 5, the non-uniformity of the thickness of the oxide film 5a formed by the thermal oxidation treatment among the SiC wafers 50 within the batch can be suppressed due to such a change in the atmosphere.

[0031] <A. Embodiment 1> <A-1. Configuration> By the method for manufacturing a silicon carbide semiconductor device according to the present embodiment, for example, a MOSFET, a pn diode, a Schottky Barrier diode (SBD), a Bipolar Junction Transistor (BJT), a Junction FET (JFET), or an Insulated Gate Bipolar Transistor (IGBT) is manufactured.

[0032] In the following description, it is assumed that a semiconductor device manufactured by the method for manufacturing a silicon carbide semiconductor device according to the present embodiment is MOSFET 100 shown in Figures 4 and 5. Figure 4 shows the inside of a cell of MOSFET 100. Figure 5 shows the outer periphery of a cell of MOSFET 100. In the following description, the conductivity types of the semiconductor layers may be interchanged.

[0033] As shown in FIGS. 4 and 5, MOSFET 100 includes a SiC substrate 1, a SiC drift layer 2, a base region 3, a source region 4, a gate oxide film 5, a gate wiring 6, a source electrode 7, a drain electrode 8, an interlayer insulating film 9, and a gate electrode 10.

[0034] The upper surface of the SiC substrate 1 is a Si surface. The SiC substrate 1 is a single-crystal n-type substrate having a 4H crystal structure.

[0035] The SiC drift layer 2 is formed on the upper surface of the SiC substrate 1.

[0036] The base region 3 is selectively formed in a surface layer portion of the upper surface of the SiC drift layer 2. The base region 3 is a p-type semiconductor layer, and contains, for example, aluminum (Al) as a p-type impurity.

[0037] The source region 4 is selectively formed inside the cell in a surface portion of the upper surface of the base region 3. The source region 4 is an n-type semiconductor layer. The source region 4 contains, for example, nitrogen (N) as an n-type impurity.

[0038] The gate oxide film 5 is formed across the region 2a sandwiched between two adjacent source regions 4 among the source region 4, the base region 3, and the SiC drift layer 2. A gate wiring 6 is formed on the gate oxide film 5. Also, a drain electrode 8 is formed on the C surface which is the lower surface of the SiC substrate 1. The gate wiring 6 and the source electrode 7 are separated by an interlayer insulating film 9. The gate wiring 6 is routed from inside the cell to the cell outer periphery and is connected to the gate electrode 10 at the cell outer periphery.

[0039] In FIG. 4, the MOSFET 100 is shown as a planar gate structure, but the MOSFET 100 may be of a trench gate type.

[0040] <A-2. Manufacturing method> FIG. 17 is a flowchart of the manufacturing method of the semiconductor device of the present embodiment.

[0041] FIGS. 6 to 11 are cross-sectional views showing the states during the manufacturing of the MOSFET 100. Hereinafter, the manufacturing process of the MOSFET will be described along FIGS. 6 to 11. FIG. 6 is a view corresponding to both the inside and the outer periphery of the cell. FIGS. 7 to 9, 11, 13, and 15 are views corresponding to the inside of the cell. FIGS. 10, 12, 14, and 16 are views corresponding to the outer periphery of the cell.

[0042] First, in step S1, a silicon carbide substrate 1 is prepared.

[0043] Next, in step S2, an SiC drift layer 2 is epitaxially grown on the upper surface of the silicon carbide substrate 1 by CVD method (see FIG. 6). The n-type impurity concentration of the SiC drift layer 2 is 1×10 15 cm -3 ~1×10 17 cm -3 , and the thickness is 5 to 50 μm.

[0044] Next, in step S3, a mask 41 is formed on the upper surface of the SiC drift layer 2, and Al, which is a p-type impurity, is ion-implanted into the SiC drift layer 2 using the mask 41 (see FIG. 7). At this time, the depth of the Al ion implantation is about 0.5 to 3 μm, which does not exceed the thickness of the SiC drift layer 2. The impurity concentration of the implanted Al is 1×10 17 cm -3 ~1×10 19 cm -3 and is higher than the n-type impurity concentration of SiC drift layer 2. The region of SiC drift layer 2 into which Al ions have been implanted and which becomes p-type becomes base region 3. After the Al ion implantation, mask 41 is removed.

[0045] Furthermore, in step S3, after removing the mask 41, a mask 42 is formed on the upper surface of the SiC drift layer 2, and N, which is an n-type impurity, is ion-implanted into the surface layer portion of the SiC drift layer 2 using the mask 42 (see FIG. 8). In step S3, the region of the SiC drift layer 2 into which Al ions have been previously implanted in step S3 is also referred to as the SiC drift layer 2. The depth to which N is ion-implanted is shallower than the thickness of the base region 3. The impurity concentration of N to be ion-implanted is 1×10 18 cm -3 ~1×10 21 cm -3 The N ion implantation is performed so that the p-type impurity concentration exceeds that of the base region 3 within the range. Of the regions in the SiC drift layer 2 into which N has been implanted, the region exhibiting n-type becomes the source region 4. After the N ion implantation, the mask 42 is removed.

[0046] Next, in step S4, annealing is performed in a heat treatment device in an atmosphere of an inert gas such as argon (Ar) gas at 1300 to 1900° C. for 30 seconds to 1 hour to activate the N and Al ions implanted in step S3.

[0047] Next, in step S5, an interlayer insulating film forming process is performed in which an interlayer insulating film 9 is formed by a CVD method (see FIG. 9 and FIG. 10). When a gate wiring 6 formed in a later process is routed to the outer periphery of the cell and connected to a gate electrode 10, the interlayer insulating film 9 insulates the SiC drift layer 2, the base region 3, and the source region 4 from the gate wiring 6. The thickness of the interlayer insulating film 9 is preferably 1 to 3 μm, which does not affect the gate capacitance and makes the interlayer insulating film 9 less likely to be broken by switching, surges, etc. The material of the interlayer insulating film 9, which is an inorganic film, is BPSG (Boro-Phospho Silicate Glass), PSG (Phospho Silicate Glass), TEOS (Tetraethyl orthosilicate), etc. The configuration consisting of the SiC substrate 1, the SiC drift layer 2, the base region 3, and the source region 4 shown in FIG. 8 corresponds to the SiC wafer 50 in FIG. 1. 2. The interlayer insulating film 9 corresponds to the inorganic film 90 in FIG.

[0048] The interlayer insulating film 9 is formed on the Si surface 13 (i.e., the main surface on the source region 4 side) which is the upper surface of the SiC wafer 50, and on the C surface 12 (i.e., the main surface on the lower surface side of the SiC substrate 1) which is the lower surface. The interlayer insulating film 9 on the C surface 12 is an example of a first inorganic film, and the interlayer insulating film 9 on the Si surface 13 is an example of a second inorganic film.

[0049] Next, in step S6, an etching process is performed. In the etching process of step S6, the interlayer insulating film 9 on the Si surface 13 side inside the cell is removed by patterning, dry etching, and wet etching, and the interlayer insulating film 9 on the Si surface 13 side at a desired position on the cell periphery is also removed (see FIGS. 9 and 10).

[0050] In step S6, the interlayer insulating film 9 on the Si surface 13 side is etched. Depending on the etching method, the interlayer insulating film 9 on the C surface 12 side of the SiC wafer 50 may also be etched, and the interlayer insulating film 9 on the C surface 12 side of the SiC wafer 50 may become thinner. In a later step, it is preferable that the interlayer insulating film 9 on the C surface side of the SiC wafer 50 has a thickness of 0.75 μm, that is, 750 nm or more. Therefore, in this embodiment, the etching process of step S6 is performed so that the interlayer insulating film 9 on the C surface 12 side of the SiC wafer 50 remains at a thickness of 0.75 μm or more after the etching of step S6 is performed. The reason why it is preferable that the interlayer insulating film 9 on the C surface 12 side of the SiC wafer 50 remains at a thickness of 0.75 μm or more after the etching of step S6 is performed will be described later. The thickness of the interlayer insulating film 9 remaining on the C surface 12 side of the SiC wafer 50 after the etching of step S6 may be 1.2 μm or more, or may be 1.6 μm or more.

[0051] In step S6, for example, the interlayer insulating film 9 on the C-face side of the SiC wafer 50 is left with a thickness of 0.75 μm or more at the center in a plan view of the SiC wafer 50. Also, in step S6, for example, the interlayer insulating film 9 is left with a thickness of 0.75 μm or more over the entire C-face side of the SiC wafer 50. Also, in step S6, for example, the interlayer insulating film 9 is left with an average thickness of 0.75 μm or more on the C-face side of the SiC wafer 50. Here, the average thickness of the interlayer insulating film 9 refers to the average of thicknesses measured at a large number of evenly arranged points, for example, 100 or more points, within the surface of the SiC wafer 50.

[0052] For example, as a method for leaving 0.75 μm or more of the interlayer insulating film 9 on the C-face 12 side of the SiC wafer 50 after the etching in step S6, for example, the interlayer insulating film 9 on the C-face 12 side of the SiC wafer 50 may be formed thicker in advance, or a protective film may be formed on the interlayer insulating film 9 on the C-face 12 side of the SiC wafer 50 when performing the process in step S6 so that the interlayer insulating film 9 on the C-face 12 side of the SiC wafer 50 is not easily etched in step S6. For example, if the dip-type wet etching is performed without forming a protective film in step S6, not only the interlayer insulating film 9 on the Si-face 13 side but also the interlayer insulating film 9 on the C-face 12 side is etched. By forming a protective film on the interlayer insulating film 9 on the C-face 12 side of the SiC wafer 50 before performing the dip-type wet etching, it is possible to reduce costs and leave, for example, 0.75 μm or more of the interlayer insulating film 9 on the C-face 12 side of the SiC wafer 50.

[0053] Next, in step S7, as shown in Figs. 11 and 12, a gate oxide film 5, which is a thermal oxide film, is formed by thermal oxidation in an area of ​​the upper surface side of the SiC wafer 50 where the interlayer insulating film 9 is not formed. In the thermal oxidation, as described above, an oxidizing gas, for example, O2 gas or O3 gas, is used. The gate oxide film 5 corresponds to the oxide film 5a in Fig. 2. In Fig. 2, the inorganic film 90 is shown on the lower surface of the SiC wafer 50, and the oxide film 5a is shown on the upper surface of the SiC wafer 50, but in step S7 of this embodiment, the interlayer insulating film 9 may also be formed on a part of the upper surface of the SiC wafer 50.

[0054] Step S7 will be described in detail below. In step S7, the gate oxide film 5 is formed by subjecting the SiC wafer 50 to a thermal oxidation treatment in a vertical batch-type diffusion furnace 80 shown in FIG.

[0055] In step S7, first, the SiC wafer 50 having the interlayer insulating film 9 remaining on the C-face 12 by 0.75 μm or more is placed in a vertical batch-type diffusion furnace 80 as shown in Fig. 1. The SiC wafer 50 and the SiC dummy wafer 51 are placed so that the C-face 12 faces downward. Note that the interlayer insulating film 9 is not shown in Fig. 1.

[0056] Next, the Si surface 13 of the SiC wafer 50 is thermally oxidized at 1200°C or more and 1300°C or less to form a thermal oxide film on the Si surface 13 of the SiC wafer 50. At this time, a gate oxide film 5, which is a thermal oxide film, is formed in a region of the Si surface 13 of the SiC wafer 50 where the interlayer insulating film 9 is not formed (i.e., a region where the interlayer insulating film 9 has been removed in step S6). The thicker the interlayer insulating film 9 left on the C surface 12 side of the SiC wafer 50 is, the more difficult it is for the O2 gas to reach the C surface 12 because it is blocked by the interlayer insulating film 9. For this reason, the amount of O2 gas generated from the C surface 12 by the reactions of the above formulas (1) and (2) is reduced, and the oxidation reaction by the O2 gas is less likely to occur in the SiC wafer 50 directly below the SiC wafer 50.

[0057] The thickness of the gate oxide film 5 formed in step S7 will be described in detail with reference to FIG. 18. FIG. 18 is a diagram showing the relationship between the thickness of the interlayer insulating film 9 formed on the C-face 12 of the SiC wafer 50 and the variation in the thickness of the gate oxide film 5 between the SiC wafers 50. The horizontal axis of FIG. 18 is the average thickness of the interlayer insulating film 9 formed on the C-face 12 of a certain SiC wafer 50. The horizontal axis of FIG. 18 is the thickness of the interlayer insulating film 9 formed on the C-face 12 of a representative SiC wafer 50, but the interlayer insulating film 9 of approximately the same thickness is formed on the C-face 12 of each SiC wafer 50 in the batch. The vertical axis of FIG. 18 is the difference between the maximum and minimum thicknesses of the gate oxide film 5 formed on the Si-face 13 of each SiC wafer 50 in the batch when the thermal oxidation treatment in step S7 is performed. In FIG. 18, the values ​​marked as "measured value" are the results of measurements made by actually performing the thermal oxidation treatment, and the values ​​marked as "calculated value" are the results obtained by performing a numerical simulation. Among the SiC wafers 50 in the batch, the SiC wafer 50 immediately below the SiC dummy wafer 51 had the thinnest gate oxide film 5 formed on the Si surface 13 .

[0058] The results shown in FIG. 18 were obtained when a thermal oxidation process was performed using the vertical batch-type diffusion furnace 80 shown in FIG. 1. In the thermal oxidation process, a gate oxide film 5 of about 45 to 50 nm was formed on the upper surface of a SiC wafer 50 having a diameter of 4 inches. Before the thermal oxidation process, an interlayer insulating film 9 having a sufficient thickness that it is considered that there is no O2 gas generated by the formulas (1) and (2) is formed on the C surface 12 of the SiC dummy wafer 51. On the C surface 12 of the SiC dummy wafer 51, the interlayer insulating film 9, which is an inorganic film, is formed to a thickness greater than the interlayer insulating film 9 formed on the C surface 12 of each SiC wafer 50 in the batch.

[0059] 18, the thicker the interlayer insulating film 9 formed on the C-face 12 of the SiC wafer 50, the smaller the variation in thickness of the gate oxide film 5 formed in step S7 among the SiC wafers 50 in a batch. This is believed to be because the thicker the interlayer insulating film 9 formed on the C-face 12 of the SiC wafer 50, the more the generation of O2 gas from the C-face 12 of the SiC wafer 50 due to the reactions represented by formulas (1) and (2) can be suppressed.

[0060] When performing step S7, the interlayer insulating film 9 is formed on the SiC dummy wafer 51 with a sufficient thickness such that it is considered that there is no O2 gas generated by the formulas (1) and (2). Therefore, even if the SiC dummy wafer 51 is not placed and the Si monitor wafer 52 is directly above the SiC wafer 50, the same result as that shown in FIG. 18 can be obtained. That is, by making the thickness of the interlayer insulating film 9 on the C surface 12 of the SiC wafer 50 0.75 μm or more, the variation in the thickness of the gate oxide film 5 between the SiC wafers 50 in the batch is suppressed even if the SiC dummy wafer 51 is eliminated. Therefore, if the thickness of the interlayer insulating film 9 on the C surface 12 of the SiC wafer 50 is made 0.75 μm or more, the SiC wafer 50 may be placed at the position where the SiC dummy wafer 51 is placed in FIG. 1.

[0061] As described above, as a result of extensive research, it has been newly discovered that if the thickness of the interlayer insulating film 9 left on the underside of the SiC wafer 50 in step S6 is set to 0.75 μm or more, the difference in thickness of the gate oxide film 5 formed in step S7 between SiC wafers 50 in a batch can be suppressed to 0.8 nm or less.

[0062] Furthermore, if the interlayer insulating film 9 on the C-face 12 of the SiC wafer 50 is thin, the thickness of the interlayer insulating film 9 on the C-face 12 of the SiC wafer 50 is not uniform in the plane, which causes a large deviation in the amount of O2 generated depending on the in-plane position, and the in-plane uniformity of the gate oxide film 5 of the SiC wafer 50 directly below the SiC wafer 50 deteriorates. If the interlayer insulating film 9 of the SiC wafer 50 is left at a thickness of 0.75 μm or more, the generation of O2 gas can be suppressed, and the in-plane uniformity of the gate oxide film 5 formed on the Si-face 13 of the SiC wafer 50 directly below the SiC wafer 50 improves.

[0063] When the thickness of the interlayer insulating film 9 on the C-face 12 of the SiC wafer 50 is set to 1.2 μm or more, the difference in thickness of the gate oxide film 5 between the SiC wafers 50 in a batch can be suppressed to 0.3 nm or less. When the thickness of the interlayer insulating film 9 on the C-face 12 of the SiC wafer 50 is set to 1.6 μm or more, the difference in thickness of the gate oxide film 5 between the SiC wafers 50 in a batch can be suppressed to 0.1 nm or less. Therefore, it is more preferable to leave 1.2 μm of the interlayer insulating film 9 in step S6, and it is even more preferable to leave 1.6 μm of the interlayer insulating film 9 in step S6.

[0064] In step S7, after forming a thermal oxide film, post-annealing to reduce the interface state at the interface between SiO2 and SiC is performed with the wafer positioned as in Fig. 1. The post-annealing is performed in an oxidizing gas atmosphere such as a WET atmosphere, a nitrogen oxide (NO or N2O) atmosphere, or a POCl3 atmosphere, or a reducing gas atmosphere such as H2 gas or NH3 gas.

[0065] Thereafter, in step S8, a gate wiring 6 is formed on the gate oxide film 5. The gate wiring 6 is formed by forming a conductive polycrystalline silicon film by low pressure CVD and then patterning the polycrystalline silicon film. Thereafter, an interlayer insulating film 9 having a thickness of about 1.0 to 3.0 μm is additionally formed in a CVD apparatus to cover the gate wiring 6.

[0066] Thereafter, in step S9, the interlayer insulating film 9 and the polycrystalline silicon film on the lower surface of the SiC wafer 50 are removed by wet etching or dry etching, thereby obtaining the state shown in FIGS.

[0067] Next, in step S10, the source electrode 7 and the gate electrode 10 are formed.

[0068] In step S10, first, the interlayer insulating film 9 in the region where the source electrode 7 is to be formed is removed by patterning and dry etching. Furthermore, after a silicide layer is formed in the region where the source electrode 7 is to be formed, the interlayer insulating film 9 in the region that makes contact with the gate wiring 6 is removed by patterning and dry etching (see FIGS. 15 and 16). Next, the source electrode 7 that is electrically connected to the source region 4 and the gate electrode 10 that is electrically connected to the gate wiring 6 are formed. The source electrode 7 and the gate electrode 10 are formed by forming a film of an Al alloy or the like over the entire upper surface of the SiC wafer 50 by sputtering, and then patterning and wet etching the film. plastic surgery It is formed by

[0069] Next, in step S11, the drain electrode 8 is formed on the lower surface side of the SiC wafer 50. The material of the drain electrode 8 is, for example, an Al alloy.

[0070] Through the above steps, the vertical MOSFET 100 shown in FIGS. 4 and 5 is completed.

[0071] Summarizing the manufacturing method of the silicon carbide semiconductor device of Embodiment 1 described above, it is as follows. Prepare a plurality of SiC wafers 50, form an interlayer insulating film 9, which is a first inorganic film, on the lower surfaces of the plurality of SiC wafers 50, and perform etching on the plurality of SiC wafers 50 after the formation of the first inorganic film. The etching is performed so that the thickness of the first inorganic film of the plurality of SiC wafers 50 remains 0.75 μm or more after the etching. Next, in step S7, a thermal oxidation treatment is performed using a vertical batch diffusion furnace 80 to form a gate oxide film 5 on the upper surfaces of the plurality of SiC wafers 50. The thermal oxidation treatment is performed on at least one wafer including at least one of a Si monitor wafer 52 or a SiC dummy wafer 51, which is different from the plurality of SiC wafers 50, and the plurality of SiC wafers 50 are arranged along one direction and with the upper surfaces of the plurality of SiC wafers 50 facing one direction. In the state of the thermal oxidation treatment, the first SiC wafer 50 among the plurality of SiC wafers 50 is disposed immediately below any one of at least one wafer including at least one of a Si monitor wafer 52 or a SiC dummy wafer 51, and the second SiC wafer 50 among the plurality of SiC wafers 50 is disposed immediately below the third SiC wafer 50 among the plurality of SiC wafers 50.

[0072] In step S7, since the thickness of the interlayer insulating film 9 on the C-plane 12 side of the SiC wafer 50 is 0.75 μm or more, the gas generated from the C-plane 12 of the SiC wafer 50 is suppressed, so that the thickness of the gate oxide film 5 is made uniform among the SiC wafers 50 in the batch. Further, since the gas generated from the C-plane 12 of the SiC wafer 50 is suppressed, the SiC dummy wafer 51 can also be eliminated.

[0073] A configuration similar to step S7 of the manufacturing method of the present embodiment can also be applied to other processes for performing heat treatment in a batch-type apparatus, such as a heat treatment process of a metal electrode. Further, a configuration similar to step S7 can also be applied to a process of forming an oxide film other than the gate oxide film 5.

[0074] <B. Embodiment 2> FIG. 19 is a diagram showing how wafers are arranged in the vertical batch diffusion furnace 80 in step S7 (see FIG. 17) of the method for manufacturing a semiconductor device according to Embodiment 2. In step S7 of the present embodiment, SiC wafers 50 and Si dummy wafers 51a are alternately arranged on a boat 82. The method for manufacturing a semiconductor device of the present embodiment is the same as the method for manufacturing a semiconductor device of Embodiment 1 in other respects.

[0075] By arranging the wafers as shown in FIG. 19, the diffusion of O2 gas generated from the C surface 12 of the SiC wafer 50 is blocked by the Si dummy wafer 51a installed directly below it. The amount of O2 gas reaching other SiC wafers 50 due to diffusion decreases. Therefore, oxidation by O2 gas generated from the C surface 12 of other SiC wafers 50 hardly occurs in the SiC wafer 50 directly below the Si dummy wafer 51a, and variations in the thickness of the gate oxide film 5 among the SiC wafers 50 in the batch are suppressed.

[0076] Furthermore, since the generation of O2 gas can be suppressed, the in-plane uniformity of the thickness of the gate oxide film 5 formed on the Si surface 13 of each SiC wafer 50 in the batch in step S7 is improved. Instead of the Si dummy wafer 51a, other dummy wafers that hardly generate O2 gas on the lower surface and hardly cause a non-uniform oxidation reaction to the SiC wafer 50 directly below it may be used. The other dummy wafer is, for example, a SiC dummy wafer 51 having an inorganic film with a thickness of 0.75 μm or more formed on the lower surface.

[0077] If an interlayer insulating film 9 of 0.75 μm or more remains on the lower surface of the SiC wafer 50, the amount of O2 gas generated from the lower surface of the SiC wafer 50 in step S7 decreases. Therefore, the amount of O2 gas that diffuses around the Si dummy wafer 51a to other SiC wafers 50 also decreases, and variations in the thickness of the gate oxide film 5 among the SiC wafers 50 in the batch can be suppressed with higher precision.

[0078] <C. Embodiment 3> Fig. 20 is a diagram showing the configuration of a vertical batch-type diffusion furnace 80c used in this embodiment. The manufacturing method of the semiconductor device of this embodiment is different from the manufacturing method of the semiconductor device of the first embodiment in that a vertical batch-type diffusion furnace 80c is used instead of the vertical batch-type diffusion furnace 80 in step S7 (see Fig. 17). Although Fig. 20 shows a case where a SiC dummy wafer 51 is not used, the SiC dummy wafer 51 may be disposed between the Si monitor wafer 52 and the SiC wafer 50 in this embodiment as in the first embodiment. The manufacturing method of the semiconductor device of this embodiment is otherwise similar to the manufacturing method of the semiconductor device of the first embodiment.

[0079] Compared with the vertical batch-type diffusion furnace 80 used in the first and second embodiments, the vertical batch-type diffusion furnace 80c of the present embodiment has a support part 82b instead of the support part 82a. The vertical batch-type diffusion furnace 80c is similar to the vertical batch-type diffusion furnace 80 in other respects.

[0080] In the vertical batch-type diffusion furnace 80 of the embodiment 1, the support portion 82a of the boat 82 is claw-shaped, and only the edge portion of the wafer is in contact with the support portion 82a, and the wafer is supported by the support portion 82a in a state where the center portion of the wafer does not overlap with the support portion 82a in a planar view.

[0081] On the other hand, in the vertical batch-type diffusion furnace 80c of the present embodiment, the support portion 82b is plate-shaped. The SiC wafer 50 is placed on the plate-shaped support portion 82b with the C-face 12 facing downward. The SiC wafer 50 is placed on the plate-shaped support portion 82b so that, for example, the entire SiC wafer 50 overlaps with the plate-shaped support portion 82b in a plan view. The SiC wafer 50 is placed on the plate-shaped support portion 82b so that, for example, a part of the SiC wafer 50 including the center in a plan view or the entire SiC wafer 50 in a plan view is in contact with the support portion 82b.

[0082] In the vertical batch diffusion furnace 80c, a plate-shaped support portion 82b partitions between a certain SiC wafer 50 and the SiC wafer 50 directly below the certain SiC wafer 50. Therefore, diffusion of O2 gas generated from the C surface 12 of the certain SiC wafer 50 to the SiC wafer 50 directly below it due to the reactions of formulas (1) and (2) is suppressed, and it is possible to suppress an excessive oxidation reaction by O2 gas from occurring in the SiC wafer 50 directly below the certain SiC wafer 50. In the vertical batch diffusion furnace 80c, for example, the spaces between adjacent SiC wafers 50 are each partitioned by a plate-shaped support portion 82b.

[0083] In this way, by using the vertical batch diffusion furnace 80c, it is possible to suppress variations in the thickness of the gate oxide film 5 among the SiC wafers 50 within a batch. Furthermore, since the influence of the O2 gas generated by the reactions of formulas (1) and (2) can be suppressed, the in-plane uniformity of the thickness of the gate oxide film 5 formed on the Si surface 13 of each SiC wafer 50 within a batch is improved.

[0084] If an interlayer insulating film 9 remains at 0.75 μm or more on the lower surface of the SiC wafer 50 in step S6 (see FIG. 17), the amount of O2 gas generated from the lower surface of the SiC wafer 50 in step S7 (see FIG. 17) decreases. Therefore, the O2 gas that diffuses around the plate-shaped support portion 82b decreases, and variations in the thickness of the gate oxide film 5 among the SiC wafers 50 within a batch can be suppressed with higher precision.

[0085] <D. Embodiment 4> Fig. 21 is a diagram showing the configuration of a vertical batch-type diffusion furnace 80d used in this embodiment. The manufacturing method of a semiconductor device in this embodiment is different from the manufacturing method of a semiconductor device in the first embodiment in that a vertical batch-type diffusion furnace 80d is used instead of the vertical batch-type diffusion furnace 80 in step S7 (see Fig. 17). Although Fig. 21 shows a case where a SiC dummy wafer 51 is not used, the SiC dummy wafer 51 may be disposed between the Si monitor wafer 52 and the SiC wafer 50 in this embodiment as in the first embodiment. The manufacturing method of a semiconductor device in this embodiment is otherwise similar to the manufacturing method of a semiconductor device in the first embodiment.

[0086] Compared with the vertical batch-type diffusion furnace 80 used in the first and second embodiments, the vertical batch-type diffusion furnace 80d of the present embodiment is different in that it further includes a partition 84. The vertical batch-type diffusion furnace 80d is similar to the vertical batch-type diffusion furnace 80 in other respects.

[0087] In the vertical batch-type diffusion furnace 80d, a wafer supported by a support portion 82a is separated from a wafer supported by a support portion 82a of an adjacent stage by a partition 84. In the vertical batch-type diffusion furnace 80d, for example, adjacent SiC wafers 50 are separated by partitions 84, respectively.

[0088] The partition 84 prevents the O2 gas generated from the underside of the SiC wafer 50 in step S7 from diffusing to the SiC wafer 50 directly below the SiC wafer 50, thereby suppressing the oxidation reaction caused by the O2 gas in the SiC wafer 50 directly below the SiC wafer 50. This makes it possible to suppress the variation in thickness of the gate oxide film 5 between the SiC wafers 50 in the batch. Furthermore, since the diffusion of O2 gas can be suppressed, the in-plane uniformity of the thickness of the gate oxide film 5 on the Si surface 13 of each SiC wafer 50 in the batch is improved.

[0089] In step S6 (see FIG. 17), if the interlayer insulating film 9 remains on the lower surface of the SiC wafer 50 at 0.75 μm or more, the amount of O2 gas generated from the lower surface of the SiC wafer 50 decreases in step S7 (see FIG. 17). Therefore, the O2 gas that circulates and diffuses around the partition 84 decreases, and the variation in the thickness of the gate oxide film 5 between the SiC wafers 50 in the batch can be suppressed with higher precision.

[0090] In order to prevent the gas generated from the SiC wafer 50 from circulating and diffusing around the partition 84, it is desirable that the size of the partition 84 is equal to or larger than the size of the wafer. For example, in step S7 (see FIG. 17), the SiC wafer 50 is supported by the support portion 82a in such an arrangement that the entire SiC wafer 50 overlaps the partition 84 in plan view.

[0091] The partition 84 may be integral with the boat 82 or may be removable from the boat 82.

[0092] If the partition 84 can be removed from the boat 82, the handling of the boat 82 is improved, and the installation and maintenance of the vertical batch diffusion furnace 80d become easy.

[0093] <E. Embodiment 5> FIG. 22 is a diagram showing the configuration of the vertical batch diffusion furnace 80e used in the present embodiment and the arrangement of the wafers in step S7 (see FIG. 17). The method for manufacturing a semiconductor device according to the present embodiment is different from the method for manufacturing a semiconductor device according to Embodiment 1 in that the vertical batch diffusion furnace 80e is used instead of the vertical batch diffusion furnace 80 in step S7. FIG. 22 shows a case where the SiC dummy wafer 51 is not used. The method for manufacturing a semiconductor device according to the present embodiment is the same as the method for manufacturing a semiconductor device according to Embodiment 1 in other respects.

[0094] The vertical batch-type diffusion furnace 80e differs from the vertical batch-type diffusion furnace 80 used in the first and second embodiments in that it includes a gas introduction line 83a in addition to the gas introduction line 83. The vertical batch-type diffusion furnace 80e can supply more O2 gas or O3 gas to a region between a pair of supporting parts 82a adjacent in the direction in which the wafers are stacked, by the gas introduction line 83a, than to a region between another pair of supporting parts 82a adjacent in the direction in which the wafers are stacked.

[0095] In the manufacturing method of the semiconductor device of the present embodiment, in step S7 (see FIG. 17), in addition to supplying oxygen through the gas introduction line 83, O2 gas or O3 gas is selectively supplied between the Si monitor wafer 52 and the SiC wafer 50 through the gas introduction line 83a. As a result, more O2 gas or O3 gas is supplied to the region between the Si monitor wafer 52 and the SiC wafer 50 than to the region between the SiC wafers 50. When a dummy wafer is used in step S7 (see FIG. 17), O2 gas or O3 gas is supplied to the region between the dummy wafer and the SiC wafer 50 through the gas introduction line 83a. As a result, more O2 gas or O3 gas is supplied to the region between the dummy wafer and the SiC wafer 50 than to the region between the SiC wafers 50.

[0096] As described above, in the results shown in FIG. 18 of the first embodiment, the gate oxide film 5 formed on the SiC wafer 50 placed directly below the monitor wafer or dummy wafer in step S7 (see FIG. 17) was thinner than the gate oxide film 5 formed on the SiC wafer 50 placed directly below the SiC wafer 50 in step S7 (see FIG. 17).

[0097] In the manufacturing method of the semiconductor device of the present embodiment, O2 gas or O3 gas is preferentially supplied from the gas introduction line 83a to the upper surface of the SiC wafer 50 arranged immediately below the monitor wafer or dummy wafer, and the oxidation reaction by the O2 gas or O3 gas is likely to occur on the upper surface of the SiC wafer 50 arranged immediately below the monitor wafer or dummy wafer. Therefore, the variation in thickness of the gate oxide film 5 between the SiC wafers 50 in the batch can be suppressed.

[0098] The vertical batch-type diffusion furnace 80e may not be provided with the gas introduction line 83a. In that case, as shown in Fig. 23, the gas introduction line 83 has an opening 831 on the side in addition to the opening 830 in the tube 81. O2 gas or O3 gas is preferentially supplied from the opening 831 to the region between the monitor wafer or dummy wafer and the SiC wafer 50 arranged directly below the monitor wafer or dummy wafer, thereby suppressing the variation in thickness of the gate oxide film 5 between the SiC wafers 50 in the batch.

[0099] As described in the first embodiment, if the interlayer insulating film 9 is left on the lower surface of the SiC wafer 50 by 0.75 μm or more in step S6 (see FIG. 17), the difference in thickness of the gate oxide film 5 between the SiC wafers 50 in the batch can be suppressed to 0.8 nm or less in step S7. By using the fifth embodiment in combination, the variation in thickness of the gate oxide film 5 between the SiC wafers 50 in the batch can be suppressed with higher accuracy. In this case, in step S7 (see FIG. 17), the amount of oxidizing gas supplied from the gas introduction line 83a is adjusted according to the thickness of the interlayer insulating film 9 formed on the lower surface of the SiC wafer 50. In addition, when the SiC dummy wafer 51 is disposed between the SiC wafer 50 and the Si monitor wafer 52, the amount of oxidizing gas supplied from the gas introduction line 83a is adjusted according to the thickness of the interlayer insulating film 9 formed on the lower surface of the SiC wafer 50 and the thickness of the interlayer insulating film 9 formed on the lower surface of the SiC dummy wafer 51 in step S7 (see FIG. 17).

[0100] It should be noted that the embodiments can be freely combined, and each embodiment can be modified or omitted as appropriate. [Explanation of symbols]

[0101] 1 SiC substrate, 2 SiC drift layer, 3 base region, 4 source region, 5 gate oxide film, 5a oxide film, 6 gate wiring, 7 source electrode, 8 drain electrode, 9 interlayer insulating film, 10 gate electrode, 12 C surface, 13 Si surface, 41, 42 mask, 45 Si atom, 46 C atom, 50 SiC wafer, 51 SiC dummy wafer, 51a Si dummy wafer, 52 Si monitor wafer, 80, 80c, 80d, 80e vertical batch type diffusion furnace, 81 tube, 82 boat, 82a, 82b support, 83, 83a gas introduction line, 84 partition, 90 inorganic film, 830, 831 opening.

Claims

1. forming a first inorganic film on lower surfaces of a plurality of silicon carbide wafers; etching the plurality of silicon carbide wafers after the formation of the first inorganic film; the etching is performed such that a thickness of the first inorganic film of the plurality of silicon carbide wafers remains at 750 nm or more after the etching; After the etching, a thermal oxidation process is performed using a semiconductor manufacturing device to form an oxide film on the upper surfaces of the silicon carbide wafers; performing the thermal oxidation treatment on at least one wafer including at least one of a dummy wafer or a monitor wafer, the at least one wafer being different from the plurality of silicon carbide wafers, and the plurality of silicon carbide wafers, in a state in which the plurality of silicon carbide wafers are arranged along one direction with upper surfaces of the plurality of silicon carbide wafers facing the one direction; In the state of the thermal oxidation treatment, a first silicon carbide wafer of the plurality of silicon carbide wafers is disposed directly below any one of the at least one wafer, and a second silicon carbide wafer of the plurality of silicon carbide wafers is disposed directly below a third silicon carbide wafer of the plurality of silicon carbide wafers; In each of the plurality of silicon carbide wafers, the upper surface is a Si-plane and the lower surface is a C-plane; The etching is performed by dip-type wet etching. A method for manufacturing a semiconductor device.

2. 2. The method of manufacturing a semiconductor device according to claim 1, forming a second inorganic film on an upper surface of the plurality of silicon carbide wafers; In the etching, the second inorganic film on the upper surfaces of the plurality of silicon carbide wafers is etched. A method for manufacturing a semiconductor device.

3. 3. The method for manufacturing a semiconductor device according to claim 1, further comprising the steps of: The oxide film is a gate oxide film. A method for manufacturing a semiconductor device.

4. 4. A method for manufacturing a semiconductor device according to claim 1, comprising the steps of: The thermal oxidation treatment is carried out using oxygen gas or ozone gas. A method for manufacturing a semiconductor device.

5. A method of forming a first inorganic film on the underside of a plurality of silicon carbide wafers, etching the plurality of silicon carbide wafers after the formation of the first inorganic film; the etching is performed such that a thickness of the first inorganic film of the plurality of silicon carbide wafers remains at 750 nm or more after the etching; After the etching, a thermal oxidation process is performed using a semiconductor manufacturing device to form an oxide film on the upper surfaces of the silicon carbide wafers; performing the thermal oxidation treatment on at least one wafer including at least one of a dummy wafer or a monitor wafer, the at least one wafer being different from the plurality of silicon carbide wafers, and the plurality of silicon carbide wafers, in a state in which the plurality of silicon carbide wafers are arranged along one direction with upper surfaces of the plurality of silicon carbide wafers facing the one direction; In the state of the thermal oxidation treatment, a first silicon carbide wafer of the plurality of silicon carbide wafers is disposed directly below any one of the at least one wafer, and a second silicon carbide wafer of the plurality of silicon carbide wafers is disposed directly below a third silicon carbide wafer of the plurality of silicon carbide wafers; In each of the plurality of silicon carbide wafers, the upper surface is a Si-plane and the lower surface is a C-plane; In the thermal oxidation treatment, a larger amount of oxygen gas or ozone gas is supplied to a region between any one of the at least one wafer and a first silicon carbide wafer than to a region between the second silicon carbide wafer and the third silicon carbide wafer. A method for manufacturing a semiconductor device.

6. 6. The method for manufacturing a semiconductor device according to claim 5, the semiconductor manufacturing apparatus includes a vessel for performing the thermal oxidation treatment, and a first introduction line and a second introduction line for introducing oxygen gas or ozone gas into the vessel; In the thermal oxidation treatment, the second introduction line selectively supplies oxygen gas or ozone gas to a region between the any one of the at least one wafer and the first silicon carbide wafer. A method for manufacturing a semiconductor device.

7. 6. The method for manufacturing a semiconductor device according to claim 5, the semiconductor manufacturing equipment includes a vessel for performing the thermal oxidation treatment, and an introduction line for introducing oxygen gas or ozone gas into the vessel, The introduction line has an opening on a side surface of the introduction line within the container, In the thermal oxidation treatment, the opening is located between the any one of the at least one wafer and the first silicon carbide wafer in the one direction, and oxygen gas or ozone gas is supplied into the container through the opening. A method for manufacturing a semiconductor device.

8. A method of forming a first inorganic film on the underside of a plurality of silicon carbide wafers, etching the plurality of silicon carbide wafers after the formation of the first inorganic film; the etching is performed such that a thickness of the first inorganic film of the plurality of silicon carbide wafers remains at 750 nm or more after the etching; After the etching, a thermal oxidation process is performed using a semiconductor manufacturing device to form an oxide film on the upper surfaces of the silicon carbide wafers; performing the thermal oxidation treatment on at least one wafer including at least one of a dummy wafer or a monitor wafer, the at least one wafer being different from the plurality of silicon carbide wafers, and the plurality of silicon carbide wafers, in a state in which the plurality of silicon carbide wafers are arranged along one direction with upper surfaces of the plurality of silicon carbide wafers facing the one direction; In the state of the thermal oxidation treatment, a first silicon carbide wafer of the plurality of silicon carbide wafers is disposed directly below any one of the at least one wafer, and a second silicon carbide wafer of the plurality of silicon carbide wafers is disposed directly below a third silicon carbide wafer of the plurality of silicon carbide wafers; In each of the plurality of silicon carbide wafers, the upper surface is a Si-plane and the lower surface is a C-plane; the at least one wafer is a plurality of wafers; In the state during the thermal oxidation treatment, the plurality of wafers and the plurality of silicon carbide wafers are alternately arranged in the one direction. A method for manufacturing a semiconductor device.

9. A method of forming a first inorganic film on the underside of a plurality of silicon carbide wafers, etching the plurality of silicon carbide wafers after the formation of the first inorganic film; the etching is performed such that a thickness of the first inorganic film of the plurality of silicon carbide wafers remains at 750 nm or more after the etching; After the etching, a thermal oxidation process is performed using a semiconductor manufacturing device to form an oxide film on the upper surfaces of the silicon carbide wafers; performing the thermal oxidation treatment on at least one wafer including at least one of a dummy wafer or a monitor wafer, the at least one wafer being different from the plurality of silicon carbide wafers, and the plurality of silicon carbide wafers, in a state in which the plurality of silicon carbide wafers are arranged along one direction with upper surfaces of the plurality of silicon carbide wafers facing the one direction; In the state of the thermal oxidation treatment, a first silicon carbide wafer of the plurality of silicon carbide wafers is disposed directly below any one of the at least one wafer, and a second silicon carbide wafer of the plurality of silicon carbide wafers is disposed directly below a third silicon carbide wafer of the plurality of silicon carbide wafers; In each of the plurality of silicon carbide wafers, the upper surface is a Si-plane and the lower surface is a C-plane; In the state during the thermal oxidation treatment, the second silicon carbide wafer and the third silicon carbide wafer are separated by a partition overlapping a central portion of the second silicon carbide wafer in a plan view. A method for manufacturing a semiconductor device.

10. 10. The method of manufacturing a semiconductor device according to claim 9, The partition is a support portion that supports the second silicon carbide wafer. A method for manufacturing a semiconductor device.

11. 10. The method of manufacturing a semiconductor device according to claim 9, The partition is a partition that is different from the support portion that supports the second silicon carbide wafer. A method for manufacturing a semiconductor device.

Citation Information

Patent Citations

  • Optical switch

    JP1986041130A

  • Processing tube

    JP2006303516A

  • Method for manufacturing semiconductor device, substrate treatment method and substrate treatment apparatus

    JP2012015536A

  • Heat treatment device

    JP2013185760A

  • Semiconductor device manufacturing method

    JP2014165348A

Cited By

  • Method of manufacturing semiconductor device and semiconductor manufacturing apparatus

    US12451355B2

  • Method of manufacturing semiconductor device and semiconductor manufacturing apparatus