Method for polishing substrate and polishing composition set

A multi-step polishing method using specific compositions and abrasive grain sizes addresses the challenge of achieving high flatness and reducing defects on substrates, enhancing efficiency and quality in substrate polishing.

JP7566062B2Active Publication Date: 2024-10-11FUJIMI INCORPORATED
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023018109
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-07-21
Filing Date
2023-02-09
Publication Date
2024-10-11
Estimated Expiration
2038-07-18

AI Technical Summary

Technical Problem

Existing substrate polishing methods face challenges in achieving high flatness and reducing defects while maintaining efficient polishing speed, particularly when using water-soluble polymers that slow down the process.

Method used

A method involving multiple preliminary polishing steps with specific compositions and abrasive grain sizes, including a first polishing liquid with low water-soluble polymer and large abrasive grains, a second liquid with higher polymer and moderate abrasive grains, and a third liquid with low or no abrasive grains and high polymer, applied sequentially to enhance flatness and reduce defects.

Benefits of technology

This approach efficiently achieves high flatness and reduces defects on substrates like silicon wafers by optimizing the polishing process, balancing speed and quality through the sequential use of polishing liquids with varying abrasive grain sizes and polymer contents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566062000001
    Figure 0007566062000001
  • Figure 0007566062000002
    Figure 0007566062000002
Patent Text Reader

Abstract

To provide a substrate polishing method capable of efficiently realizing a surface with high flatness and few defects. The pre-polishing process for a substrate includes a plurality of pre-polishing stages in which a first polishing liquid, a second polishing liquid, and a third polishing liquid are supplied in this order. P1 and the content COM of the water-soluble polymer P2 contained in the second polishing liquid. P2 and the content COM of the water-soluble polymer P3 contained in the third polishing liquid. P3 Relationship with COM P1 <COM P2 <COM P3 and the average primary particle diameter D of the abrasive grains A3 contained in the third polishing liquid A3 is the average primary particle diameter D of the abrasive grains A1 contained in the first polishing liquid. A1 and the average primary particle diameter D of the abrasive grains A2 contained in the second polishing liquid A2 or the third polishing liquid does not contain abrasive grains A3.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for polishing a substrate and a polishing composition set used for polishing a substrate. This application claims priority based on Japanese Patent Application No. 2017-141762 filed on July 21, 2017, the entire contents of which are incorporated herein by reference. [Background technology]

[0002] The surface of a substrate used in the manufacture of semiconductor products is generally finished to a high-quality mirror surface through a lapping process (rough polishing process) and a polishing process (precise polishing process). The polishing process typically includes a preliminary polishing process (preliminary polishing process) and a finish polishing process (finish polishing process). Patent documents 1 to 3 are cited as technical documents related to the polishing of semiconductor substrates such as silicon wafers. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 2003-257906 [Patent Document 2] Japanese Patent Application Publication No. 2014-103398 [Patent Document 3] Japanese Patent Application Publication No. 2001-239452 Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, semiconductor substrates such as silicon wafers and other substrates are required to have a high-quality surface with high flatness and few defects. Therefore, in the preliminary polishing process performed as a process before the final polishing process, it is required to have high flatness and few surface defects after polishing. In this regard, it has been considered to add a water-soluble polymer to the preliminary polishing composition in order to improve the flatness and surface defects of the substrate after polishing. However, when the preliminary polishing composition contains a water-soluble polymer, although the flatness and surface defects after polishing are improved, the polishing speed is decreased, so there is a problem that the time required for the polishing process (required polishing time) is extended. There is a demand for a polishing method that can efficiently realize a surface with high flatness and few defects after polishing.

[0005] Therefore, an object of the present invention is to provide a method for polishing a substrate that can efficiently produce a surface with high flatness and few defects. Another related object is to provide a polishing composition set that can be preferably used in such a polishing method. [Means for solving the problem]

[0006] According to this specification, a method for polishing a substrate is provided. The method includes a pre-polishing step of pre-polishing the substrate. The pre-polishing step includes a plurality of pre-polishing stages carried out on the same platen. The plurality of pre-polishing stages include, in this order, a first pre-polishing stage carried out by supplying a first polishing liquid to the substrate, a second pre-polishing stage carried out by supplying a second polishing liquid, and a third pre-polishing stage carried out by supplying a third polishing liquid. The content COM of water-soluble polymer P1 contained in the first polishing liquid P1 and the content COM of the water-soluble polymer P2 contained in the second polishing liquid. P2 and the content COM of the water-soluble polymer P3 contained in the third polishing liquid. P3 Relationship with COM P1 <COM P2 <COM P3 and the following condition is satisfied: (1) the average primary particle diameter D of the abrasive grains A3 contained in the third polishing liquid A3is the average primary particle diameter D of the abrasive grains A1 contained in the first polishing liquid A1 and the average primary particle diameter D of the abrasive grains A2 contained in the second polishing liquid A2 and (2) the third polishing liquid does not contain abrasive grains A3. According to the above polishing method, it is possible to efficiently realize a surface with high flatness and few defects after polishing.

[0007] In a preferred embodiment of the polishing method disclosed herein, the first polishing liquid does not contain the water-soluble polymer P1. By using the first polishing liquid, the polishing method disclosed herein can be preferably carried out.

[0008] The polishing method disclosed herein can be used in the pre-polishing process of various substrates. In particular, it can be preferably used in the pre-polishing process of silicon substrates. It is particularly suitable as a polishing method used in the pre-polishing of silicon wafers.

[0009] In a preferred embodiment of the polishing method disclosed herein, the second polishing liquid is a mixture of the first polishing liquid and the third polishing liquid. The second pre-polishing step is performed by simultaneously supplying the first polishing liquid and the third polishing liquid to the substrate. In this manner, the polishing method disclosed herein can be performed more simply and effectively by simultaneously supplying the first polishing liquid and the third polishing liquid to perform the second pre-polishing step.

[0010] The present invention also provides a polishing composition set for use in any of the polishing methods disclosed herein. The polishing composition set includes a first preliminary polishing composition which is the first polishing liquid or a concentrate thereof, and a third preliminary polishing composition which is the third polishing liquid or a concentrate thereof. The first preliminary polishing composition and the third preliminary polishing composition are stored separately from each other. In one embodiment, the polishing composition set further includes a second preliminary polishing composition which is the second polishing liquid or a concentrated liquid thereof, and the second preliminary polishing composition is stored separately from the first preliminary polishing composition and the third preliminary polishing composition. The polishing method disclosed herein can be suitably carried out using a polishing composition set having such a configuration. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Preferred embodiments of the present invention will be described below. Note that matters other than those specifically mentioned in this specification that are necessary for carrying out the present invention can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the relevant field.

[0012] The technology disclosed herein is preferably applied to polishing various substrates as the object to be polished. The material of the object to be polished may be, for example, metals or semimetals such as silicon, aluminum, nickel, tungsten, copper, tantalum, titanium, stainless steel, or alloys thereof; glassy materials such as quartz glass, aluminosilicate glass, and glassy carbon; ceramic materials such as alumina, silica, sapphire, silicon nitride, tantalum nitride, and titanium carbide; compound semiconductor substrate materials such as silicon carbide, gallium nitride, and gallium arsenide; and resin materials such as polyimide resin. The substrate may be made of a plurality of these materials.

[0013] The polishing method disclosed herein can be particularly preferably used for polishing a silicon substrate having a surface made of silicon, typically a silicon wafer. A typical example of the silicon wafer referred to here is a silicon single crystal wafer, for example, a silicon single crystal wafer obtained by slicing a silicon single crystal ingot. The surface to be polished in the technology disclosed herein is typically a surface made of silicon. Prior to the pre-polishing step disclosed herein, the silicon substrate may be subjected to a typical treatment that may be applied to a silicon substrate in a step upstream of the pre-polishing step, such as lapping or etching.

[0014] In the following description, the term "preliminary polishing liquid" may be used as a term that collectively refers to the polishing liquid used in the preliminary polishing step, regardless of which preliminary polishing step the polishing liquid is used in. In other words, the preliminary polishing liquid is a term that collectively refers to the first polishing liquid, the second polishing liquid, and the third polishing liquid described below. Similarly, the term "polishing liquid" may be used as a term that collectively refers to the polishing liquid used in the polishing step, regardless of which polishing step the polishing liquid is used in. In other words, the polishing liquid is a term that collectively refers to the polishing liquid used in the preliminary polishing step and the polishing liquid used in the finish polishing step.

[0015] <Preliminary polishing solution> The pre-polishing step in the polishing method disclosed herein is carried out in a manner in which a first pre-polishing stage in which a substrate to be polished is polished with a first polishing liquid, a second pre-polishing stage in which the substrate to be polished is polished with a second polishing liquid, and a third pre-polishing stage in which the substrate to be polished is polished with a third polishing liquid are carried out in this order on the same surface plate. That is, the first pre-polishing stage, the second pre-polishing stage, and the third pre-polishing stage are carried out without moving the substrate to another polishing device or another surface plate during the first pre-polishing stage, the second pre-polishing stage, and the third pre-polishing stage are carried out step by step on the same substrate to be polished. However, it is not prevented from simultaneously polishing a plurality of substrates in parallel in each pre-polishing stage, that is, performing batch-type polishing.

[0016] The preliminary polishing liquid used in each preliminary polishing stage may typically contain abrasive grains, a water-soluble polymer, and water. Specifically, the first polishing liquid used in the first preliminary polishing stage may contain abrasive grains A1, a water-soluble polymer P1, and water. The second polishing liquid used in the second preliminary polishing stage may contain abrasive grains A2, a water-soluble polymer P2, and water. The third polishing liquid used in the third preliminary polishing stage may contain abrasive grains A3, a water-soluble polymer P3, and water.

[0017] The technology disclosed herein is a method for manufacturing a polishing liquid comprising the steps of: P1and the content COM of the water-soluble polymer P2 contained in the second polishing liquid. P2 and the content COM of the water-soluble polymer P3 contained in the third polishing liquid. P3 Relationship with COM P1 <COM P2 <COM P3 and the following conditions are met: (1) Average primary particle diameter D of abrasive grains A3 contained in the third polishing liquid A3 is the average primary particle diameter D of the abrasive grains A1 contained in the first polishing liquid. A1 and the average primary particle diameter D of the abrasive grains A2 contained in the second polishing liquid A2 is less than; and (2) The third polishing liquid does not contain abrasive grain A3; The present invention is implemented in a manner that satisfies either one of the above. According to this embodiment, it is possible to efficiently realize a surface with high flatness and few defects after polishing.

[0018] The reason why such an effect is exhibited is considered to be, for example, as follows. That is, the water-soluble polymer exhibits a substrate surface protection effect during polishing. Therefore, by using a preliminary polishing liquid containing the water-soluble polymer, the flatness after polishing can be increased and surface defects can be reduced, but the polishing rate tends to decrease. In addition, since abrasive grains with a large diameter have a stronger mechanical polishing force than abrasive grains with a small diameter, the surface of the substrate can be efficiently polished by using the large diameter abrasive grains, but the surface flatness after polishing tends to decrease and surface defects tend to increase. In the technology disclosed herein, the preliminary polishing liquid supplied to the object to be polished is sequentially switched from the first polishing liquid to the second polishing liquid and the third polishing liquid during polishing in the preliminary polishing step. The first polishing liquid contains a small amount of water-soluble polymer and contains large diameter abrasive grains, so it contributes to shortening the polishing time by largely polishing the surface of the substrate. The second polishing liquid contains a larger amount of water-soluble polymer and contains large diameter abrasive grains than the first polishing liquid, so it contributes to improving the surface flatness by moderately polishing and shaping the surface that has been largely polished by the polishing of the first polishing liquid. The third polishing liquid contains a larger amount of water-soluble polymer than the second polishing liquid and contains small-diameter abrasive grains or does not contain abrasive grains, so that the water-soluble polymer is appropriately adsorbed to the surface that has been polished with the second polishing liquid to protect the surface, thereby contributing to the reduction of surface defects. Therefore, by supplying the first polishing liquid, the second polishing liquid, and the third polishing liquid, which satisfy the above relationship, in this order, it is considered that the improvement of surface flatness and the reduction of surface defects can be achieved in a shorter required polishing time in the preliminary polishing process. In addition, by supplying these preliminary polishing liquids in a switching manner on the same platen, the preliminary polishing process using the above-mentioned multiple types of preliminary polishing liquids can be efficiently carried out while suppressing the complication of work and the complication of equipment. The composition of the preliminary polishing liquid will be described in more detail below.

[0019] (Water-soluble polymer) Each preliminary polishing liquid may contain a water-soluble polymer. The type of water-soluble polymer contained in the preliminary polishing liquid disclosed herein is not limited, and can be appropriately selected from water-soluble polymers known in the field of polishing liquids. The water-soluble polymer can be used alone or in combination of two or more.

[0020] The water-soluble polymer may have at least one functional group selected from cationic groups, anionic groups, and nonionic groups in the molecule. The water-soluble polymer may have, for example, a hydroxyl group, a carboxyl group, an acyloxy group, a sulfo group, a primary amide structure, a heterocyclic structure, a vinyl structure, a polyoxyalkylene structure, or the like in the molecule. From the viewpoint of reducing aggregates and improving washability, a nonionic polymer may be preferably used as the water-soluble polymer.

[0021] Examples of water-soluble polymers include cellulose derivatives, starch derivatives, polymers containing oxyalkylene units, polymers containing nitrogen atoms, polyvinyl alcohol, etc. Among them, cellulose derivatives, polymers containing nitrogen atoms, and polyvinyl alcohol are preferred, and cellulose derivatives are more preferred. By using these water-soluble polymers, surface flatness and surface defects after polishing can be improved.

[0022] The cellulose derivative is a polymer containing β-glucose units as the main repeating unit. Specific examples of the cellulose derivative include hydroxyethyl cellulose (HEC), hydroxypropyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, ethyl cellulose, ethyl hydroxyethyl cellulose, carboxymethyl cellulose, etc. Among them, HEC is preferable.

[0023] Starch derivatives are polymers that contain α-glucose units as the main repeating unit. Specific examples of starch derivatives include pregelatinized starch, pullulan, carboxymethyl starch, cyclodextrin, etc. Among these, pullulan is preferred.

[0024] Examples of polymers containing oxyalkylene units include polyethylene oxide (PEO), block copolymers of ethylene oxide (EO) and propylene oxide (PO) or butylene oxide (BO), and random copolymers of EO and PO or BO. Among these, block copolymers of EO and PO or random copolymers of EO and PO are preferred. The block copolymers of EO and PO may be diblock copolymers or triblock copolymers containing a PEO block and a polypropylene oxide (PPO) block. Examples of the triblock copolymers include PEO-PPO-PEO type triblock copolymers and PPO-PEO-PPO type triblock copolymers. Usually, PEO-PPO-PEO type triblock copolymers are more preferred. In a block or random copolymer of EO and PO, the molar ratio of EO to PO (EO / PO) constituting the copolymer is preferably greater than 1, more preferably 2 or more, and even more preferably 3 or more, for example, 5 or more, from the viewpoints of solubility in water, washability, etc.

[0025] As the polymer containing nitrogen atoms, both a polymer containing nitrogen atoms in the main chain and a polymer having nitrogen atoms in a side chain functional group (pendant group) can be used. Examples of the polymer containing nitrogen atoms in the main chain include homopolymers and copolymers of N-acylalkyleneimine type monomers. Specific examples of N-acylalkyleneimine type monomers include N-acetylethyleneimine, N-propionylethyleneimine, and the like. Examples of the polymer having nitrogen atoms in the pendant group include polymers containing N-vinyl type monomer units, and the like. For example, at least one of homopolymers and copolymers of N-vinylpyrrolidone (hereinafter also referred to as "PVP") in which N-vinylpyrrolidone is polymerized at a ratio of 50 mol % or more is preferably used.

[0026] When polyvinyl alcohol (PVA) is used as the water-soluble polymer, the saponification degree of the polyvinyl alcohol is not particularly limited. In one embodiment, polyvinyl alcohol having a saponification degree of 90 mol% or more, typically 95 mol% or more, for example, 98 mol% or more can be used.

[0027] In the technology disclosed herein, the molecular weight of the water-soluble polymer is not particularly limited. The weight average molecular weight (Mw) of the water-soluble polymer is, for example, 200×10 4 From the viewpoint of dispersion stability, the average particle size is usually 180×10 4 Below, typically 150×10 4 In order to improve the surface protection of the object to be polished after polishing, the Mw is usually 0.5×10 4 The above is appropriate, and 0.8×10 4 More preferably, 1×10 4 The above is even more preferable.

[0028] When a cellulose derivative is used as the water-soluble polymer, Mw is approximately 50×10 4 More than this is appropriate, and preferably 80×10 4 More preferably, 100×10 4 The above Mw is, for example, 200×10 4 Below 180x10, preferably 4 When a polymer containing nitrogen atoms is used as the water-soluble polymer, Mw is approximately 1×10 4 It is appropriate to set the concentration to 2×10 or more. 4 More preferably, 3×10 4 More preferably, 4×10 4 The Mw is preferably 20×10 4 Less than or equal to 10×10 4 Less than 6×10, more preferably 4 When polyvinyl alcohol is used as the water-soluble polymer, Mw is approximately 0.5 × 10 4 It is appropriate to set the value to 0.8×10 or more. 4More preferably, 1×10 4 The Mw is preferably 5×10 4 Less than or equal to 3×10 4 Less than 2×10, more preferably 4 The following is the result.

[0029] The relationship between the weight average molecular weight (Mw) and the number average molecular weight (Mn) of the water-soluble polymer is not particularly limited. From the viewpoint of preventing the generation of aggregates, for example, the molecular weight distribution (Mw / Mn) is preferably 10.0 or less, and more preferably 7.0 or less.

[0030] As the Mw and Mn of the water-soluble polymer, values ​​based on aqueous gel permeation chromatography (GPC) (aqueous, polyethylene oxide equivalent) can be used.

[0031] As described above, the technology disclosed herein is characterized in that the content COM of the water-soluble polymer P1 contained in the first polishing liquid P1 and the content COM of the water-soluble polymer P2 contained in the second polishing liquid. P2 and the content COM of the water-soluble polymer P3 contained in the third polishing liquid. P3 Relationship with COM P1 <COM P2 <COM P3 The present invention is carried out in a manner that satisfies the above.

[0032] Content of water-soluble polymer P1 in the first polishing liquid COM P1 is the content of the water-soluble polymer P2 contained in the second polishing liquid. P2 There is no particular limitation as long as it is smaller than the value. P1 In terms of polishing efficiency, the COM P1 is preferably 0.01% by weight or less, more preferably 0.005% by weight or less, further preferably 0.001% by weight or less, and particularly preferably 0.0001% by weight or less. P1may be, for example, less than 0.00001% by weight, and typically 0.000005% by weight or less. The technology disclosed herein may also be practiced in an embodiment in which the first polishing liquid is substantially free of the water-soluble polymer P1.

[0033] Content of water-soluble polymer P2 in the second polishing liquid COM P2 The above COM P1 and the content COM of the water-soluble polymer P3 contained in the third polishing liquid P3 There is no particular limitation as long as it is smaller than the value. P2 Typically, the content of COM is 0.00001% by weight or more. From the viewpoint of obtaining a surface with a higher flatness, etc. P2 is preferably 0.00005% by weight or more, more preferably 0.0001% by weight or more, and even more preferably 0.0003% by weight or more. P2 In terms of shortening the required polishing time, the COM P2 is preferably 0.5 wt % or less, more preferably 0.1 wt % or less, further preferably 0.005 wt % or less, and particularly preferably 0.003 wt % or less. P2 This can be preferably carried out in an embodiment in which the amount of the water is 0.0003% by weight or more and 0.002% by weight or less.

[0034] In one embodiment of the technology disclosed herein, the COM of the water-soluble polymer P2 P2 Com of water-soluble polymer P1 from P1 The value obtained by subtracting the above is preferably 0.00005% by weight or more, more preferably 0.0001% by weight or more, and even more preferably 0.0003% by weight or more. P2 Com of water-soluble polymer P1 from P1 is preferably 0.5 wt % or less, more preferably 0.1 wt % or less, further preferably 0.005 wt % or less, and particularly preferably 0.003 wt % or less. According to this embodiment, both improvement in polishing efficiency and improvement in surface flatness can be suitably achieved.

[0035] Content of water-soluble polymer P3 in the third polishing solution COM P3 The above COM P2 There is no particular limitation as long as it is larger than COM P3 Typically, the content of COM is 0.0001% by weight or more. From the viewpoint of obtaining a higher quality surface, P3 is preferably 0.0005% by weight or more, more preferably 0.001% by weight or more, and even more preferably 0.003% by weight or more. P3 In terms of shortening the required polishing time, COM P3 is preferably 1 wt % or less, more preferably 0.5 wt % or less, further preferably 0.05 wt % or less, and particularly preferably 0.03 wt % or less. P3 This can be preferably carried out in an embodiment in which the amount is 0.003% by weight or more and 0.02% by weight or less.

[0036] COM of water-soluble polymer P2 P2 COM of water-soluble polymer P3 against P3 The magnification of COM P2 COM for P3 Ratio of COM P3 / COM P2 ) is not particularly limited as long as it is greater than 1. The magnification is usually appropriate to be 2 times or more, preferably 3 times or more, more preferably 5 times or more, and even more preferably 8 times or more. The magnification is usually appropriate to be 40 times or less, preferably 30 times or less, and more preferably 25 times or less. The technology disclosed herein can be preferably implemented in an embodiment in which the magnification is 5 times or more and 25 times or less. By making the magnification not too large and not too small, it is possible to suitably achieve both improvement in surface flatness and reduction in surface defects.

[0037] In one embodiment of the technology disclosed herein, the COM of the water-soluble polymer P3 P3 Com of water-soluble polymer P2 from P2The value obtained by subtracting the above is preferably 0.0005% by weight or more, more preferably 0.001% by weight or more, and even more preferably 0.003% by weight or more. P3 Com of water-soluble polymer P2 from P2 is preferably 0.5 wt % or less, more preferably 0.1 wt % or less, further preferably 0.05 wt % or less, and particularly preferably 0.03 wt % or less. According to this embodiment, it is possible to appropriately achieve both improvement in surface flatness and reduction in surface defects.

[0038] (Abrasive grain) The material and properties of the abrasive grains contained in the preliminary polishing liquid used in the technology disclosed herein are not particularly limited and can be appropriately selected according to the purpose and mode of use. The abrasive grains may be used alone or in combination of two or more types. Examples of the abrasive grains include inorganic particles, organic particles, and organic-inorganic composite particles. Specific examples of the inorganic particles include silicon compound particles such as silica particles, silicon nitride particles, and silicon carbide particles, and diamond particles. Specific examples of the organic particles include polymethylmethacrylate (PMMA) particles and polyacrylonitrile particles. Among them, inorganic particles are preferred.

[0039] In the technology disclosed herein, particularly preferred abrasive grains include silica grains. The technology disclosed herein can be preferably implemented, for example, in an embodiment in which the abrasive grains are substantially composed of silica grains. Here, "substantially" means that 95% by weight or more of the grains constituting the abrasive grains are silica grains. Preferably, 98% by weight or more, more preferably 99% by weight, for example 100% by weight of the grains constituting the abrasive grains may be silica grains.

[0040] Specific examples of silica particles include colloidal silica, fumed silica, precipitated silica, etc. The silica particles can be used alone or in combination of two or more. Colloidal silica is particularly preferred because it is less likely to cause scratches on the surface of the object to be polished and can exhibit good polishing performance. As colloidal silica, for example, colloidal silica produced by an ion exchange method using water glass (sodium silicate) as a raw material, or alkoxide-method colloidal silica produced by a hydrolysis and condensation reaction of alkoxysilane can be preferably used. The colloidal silica can be used alone or in combination of two or more.

[0041] The true specific gravity of the silica constituting the silica particles is preferably 1.5 or more, more preferably 1.6 or more, and even more preferably 1.7 or more. The polishing rate tends to increase as the true specific gravity of silica increases. From this viewpoint, silica particles having a true specific gravity of 2.0 or more, for example, 2.1 or more, are particularly preferred. The upper limit of the true specific gravity of silica is not particularly limited, but is typically 2.3 or less, for example, 2.2 or less. The true specific gravity of silica can be measured by a liquid substitution method using ethanol as a substitution liquid.

[0042] When the third polishing liquid contains abrasive grains A3, the average primary particle diameter D of the abrasive grains A3 contained in the third polishing liquid A3 is the average primary particle diameter D of the abrasive grains A1 contained in the first polishing liquid A1 and the average primary particle diameter D of the abrasive grains A2 contained in the second polishing liquid A2 (i.e., D A3 <D A1 And D A3 <D A2 By sequentially using the first polishing liquid, the second polishing liquid, and the third polishing liquid, each of which contains abrasive grains that satisfy this relationship in average primary particle size, it is possible to efficiently achieve both improved surface flatness and a reduction in surface defects in the preliminary polishing step.

[0043] Average primary particle diameter D of abrasive grains A1 contained in the first polishing liquid A1 D of abrasive grain A3 A3As long as it is larger than D A1 It is appropriate to set the D of the abrasive grain A1 to about 20 nm or more, and from the viewpoint of polishing efficiency, etc., it is preferably 30 nm or more, more preferably 40 nm or more, and particularly preferably 50 nm or more. A1 is preferably 100 nm or less, more preferably 80 nm or less, and even more preferably 70 nm or less. A1 may be 65 nm or less, for example 60 nm or less.

[0044] Although not particularly limited, when the third polishing liquid contains abrasive grains A3, D A1 and D A3 Relationship with 1 <D A1 / D A3 It is preferable that the above-mentioned ratio satisfies the above-mentioned range. A1 and D A3 The relationship is 1.2≦D A1 / D A3 ≦2.5, more preferably 1.4≦D A1 / D A3 ≦2, more preferably 1.5≦D A1 / D A3 It is preferable to implement the embodiment in which the ratio is ≦1.8. A1 D A3 It is preferably 5 nm or more larger, more preferably 10 nm or more larger, and even more preferably 15 nm or more larger. A1 From D A3 (i.e., D A1 -D A3 ) is preferably 30 nm or less, more preferably 25 nm or less, and further preferably 22 nm or less.

[0045] Average primary particle diameter D of abrasive grains A2 contained in the second polishing liquid A2 D of abrasive grain A3 A3 As long as it is larger than D A2It is appropriate to set the D of the abrasive grain A2 to about 15 nm or more, and from the viewpoint of polishing efficiency, etc., it is preferably 25 nm or more, more preferably 35 nm or more, and particularly preferably 45 nm or more. A2 is preferably 95 nm or less, more preferably 75 nm or less, and even more preferably 65 nm or less. A2 The D of the abrasive grain A2 may be 60 nm or less, for example, 55 nm or less. A2 is the D of grain A1 A1 may be the same as or different from, but D A1 It is preferable that it is smaller than .

[0046] Average primary particle diameter D of abrasive grains A3 contained in the third polishing liquid A3 D A1 and D. A2 There is no particular limitation as long as the above relationship is satisfied. For example, A3 It is appropriate to set the D of the abrasive grain A3 to about 5 nm or more, and from the viewpoint of polishing efficiency, etc., it is preferably 10 nm or more, more preferably 20 nm or more, and particularly preferably 30 nm or more. A3 is preferably 70 nm or less, more preferably 60 nm or less, and even more preferably 50 nm or less. A3 may be 45 nm or less, for example 40 nm or less.

[0047] When the third polishing liquid does not contain the abrasive grains A3, the average primary particle diameter of the abrasive grains A1 and A2 is not particularly limited. For example, from the viewpoint of polishing efficiency, the average primary particle diameter of the abrasive grains A1 and A2 is preferably 10 nm or more, more preferably 20 nm or more, and particularly preferably 30 nm or more. In addition, from the viewpoint of easily obtaining a surface with a higher flatness, the average primary particle diameter of the abrasive grains A1 and A2 is preferably 100 nm or less, more preferably 80 nm or less, and even more preferably 70 nm or less. In one embodiment, the average primary particle diameter of the abrasive grains A1 and A2 may be 65 nm or less, for example 60 nm or less.

[0048] The average primary particle size of the abrasive grains is calculated from the specific surface area (BET value) measured by the BET method as follows: Average primary particle size (nm) = 6000 / (true density (g / cm 3 ) × BET value (m 2 For example, in the case of silica particles, the average primary particle size (nm) = 2727 / BET value (m 2 The average primary particle size can be calculated from the specific surface area (g / g). The specific surface area can be measured using, for example, a surface area measuring device manufactured by Micromeritics, Inc., under the trade name "Flow Sorb II 2300".

[0049] The shape (outer shape) of the abrasive grains may be spherical or non-spherical. Specific examples of non-spherical grains include peanut-shaped, i.e., peanut shell-shaped, cocoon-shaped, confetti-shaped, rugby ball-shaped, etc. For example, abrasive grains in which most of the grains are peanut-shaped can be preferably used.

[0050] The content of the abrasive grains in each preliminary polishing liquid is not particularly limited. In one embodiment, the content is preferably 0.01% by weight or more, more preferably 0.05% by weight or more, and even more preferably 0.1% by weight or more. The content of the abrasive grains may be, for example, 0.5% by weight or more, typically 1% by weight or more. By increasing the content of the abrasive grains, a higher polishing rate can be realized. In addition, from the viewpoint of removability from the object to be polished, the content is usually 10% by weight or less, preferably 7% by weight or less, more preferably 5% by weight or less, and even more preferably 3% by weight or less, for example 2% by weight or less.

[0051] The technology disclosed herein is a method for determining the content COM of abrasive grains A1 contained in the first polishing liquid. A1 and the content COM of abrasive grains A2 contained in the second polishing liquid A2 and the content of abrasive grains A3 in the third polishing liquid, COM A3 Relationship with COM A3 <COM A2 ≦COM A1 It can be preferably implemented in a mode that satisfies the following: COMA3 <COM A2 <COM A1 It is more preferable that the relationship be satisfied. By sequentially using the first polishing liquid, the second polishing liquid, and the third polishing liquid that satisfy this relationship in the content of abrasive grains, it is possible to efficiently achieve improvement in surface flatness and reduction in surface defects in the preliminary polishing step.

[0052] In a preferred embodiment, the content COM of abrasive grains A1 contained in the first polishing liquid A1 may be 0.1% by weight or more. A1 is preferably 0.3% by weight or more, more preferably 0.5% by weight or more, and further preferably 1% by weight or more. A1 is usually suitably 10% by weight or less, preferably 7% by weight or less, more preferably 5% by weight or less, further preferably 3% by weight or less, for example 2% by weight or less.

[0053] In a preferred embodiment, the content COM of abrasive grains A2 contained in the second polishing liquid A2 may be 0.05% by weight or more. A2 is preferably 0.2% by weight or more, more preferably 0.4% by weight or more, and further preferably 0.8% by weight or more. A2 is usually suitably 8% by weight or less, preferably 6% by weight or less, more preferably 5% by weight or less, further preferably 3% by weight or less, for example 1.5% by weight or less.

[0054] In a preferred embodiment, the content COM of abrasive grains A3 contained in the third polishing liquid A3 may be, for example, 0.01% by weight or more. A3 may be, for example, 0.05% by weight or more, typically 0.1% by weight or more, for example, 0.2% by weight or more. A3 is usually 5% by weight or less, preferably 3% by weight or less, more preferably 1% by weight or less, and further preferably 0.8% by weight or less. A3may be, for example, 0.5 wt % or less, typically 0.03 wt % or less. In one embodiment, the third polishing liquid does not contain abrasive grains A3. The technology disclosed herein may also be preferably implemented in an embodiment in which the third polishing liquid does not substantially contain abrasive grains A3.

[0055] (water) The preliminary polishing liquid typically contains water. As the water, ion-exchanged water (deionized water), pure water, ultrapure water, distilled water, etc. can be preferably used. In order to avoid as much as possible the inhibition of the action of other components contained in the preliminary polishing liquid, it is preferable that the water used has a total transition metal ion content of, for example, 100 ppb or less. For example, the purity of the water can be increased by removing impurity ions using an ion exchange resin, removing foreign matter using a filter, distillation, or other operations.

[0056] (Basic compounds) The preliminary polishing liquid preferably contains a basic compound. In this specification, the basic compound refers to a compound that dissolves in water and has the function of increasing the pH of the aqueous solution. As the basic compound, an organic or inorganic basic compound containing nitrogen, an alkali metal hydroxide, an alkaline earth metal hydroxide, various carbonates and hydrogen carbonates, etc. can be used. Examples of the basic compound containing nitrogen include quaternary ammonium compounds, ammonia, amines, etc. The amine is preferably a water-soluble amine. Such basic compounds can be used alone or in combination of two or more.

[0057] Specific examples of hydroxides of alkali metals include potassium hydroxide and sodium hydroxide. Specific examples of carbonates or hydrogen carbonates include ammonium hydrogen carbonate, ammonium carbonate, potassium hydrogen carbonate, potassium carbonate, sodium hydrogen carbonate, and sodium carbonate. Specific examples of amines include methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, monoethanolamine, N-(β-aminoethyl)ethanolamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, anhydrous piperazine, piperazine hexahydrate, 1-(2-aminoethyl)piperazine, N-methylpiperazine, guanidine, azoles such as imidazole and triazole, and the like. Specific examples of quaternary phosphonium compounds include quaternary phosphonium hydroxides such as tetramethylphosphonium hydroxide and tetraethylphosphonium hydroxide.

[0058] As the quaternary ammonium compound, quaternary ammonium salts such as tetraalkylammonium salts and hydroxyalkyltrialkylammonium salts can be preferably used. The anion component in such a quaternary ammonium salt is, for example, OH - , F - , Cl - , Br - , I - , ClO4 - , BH4 - etc. In particular, a preferred example is one in which the anion is OH -Examples of quaternary ammonium hydroxides include quaternary ammonium salts having the formula: quaternary ammonium hydroxide, i.e., quaternary ammonium hydroxide. Specific examples of quaternary ammonium hydroxides include tetraalkylammonium hydroxides such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, tetrapentylammonium hydroxide, and tetrahexylammonium hydroxide; and hydroxyalkyltrialkylammonium hydroxides such as 2-hydroxyethyltrimethylammonium hydroxide (also called choline). Among these, tetraalkylammonium hydroxides are preferred, and tetramethylammonium hydroxide (TMAH) is particularly preferred.

[0059] The preliminary polishing liquid may contain a combination of the above-mentioned quaternary ammonium compound and a weak acid salt. As the weak acid salt, one that can be used in polishing using silica particles and can exert a desired buffering effect in combination with the quaternary ammonium compound can be appropriately selected. The weak acid salt can be used alone or in combination of two or more. Specific examples of the weak acid salt include sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, sodium orthosilicate, potassium orthosilicate, sodium acetate, potassium acetate, sodium propionate, potassium propionate, calcium carbonate, calcium bicarbonate, calcium acetate, calcium propionate, magnesium acetate, magnesium propionate, zinc propionate, manganese acetate, and cobalt acetate. Weak acid salts whose anion component is carbonate ion or bicarbonate ion are preferred, and weak acid salts whose anion component is carbonate ion are particularly preferred. In addition, alkali metal ions such as potassium and sodium are suitable as the cationic component. Particularly preferred weak acid salts include sodium carbonate, potassium carbonate, sodium bicarbonate, and potassium bicarbonate. Among them, potassium carbonate (K2CO3) is preferred.

[0060] The concentration of the basic compound in the preliminary polishing liquid is not particularly limited. From the viewpoint of improving the polishing rate, the concentration is usually preferably 0.00001% by weight or more of the polishing liquid, more preferably 0.00005% by weight or more, for example 0.0001% by weight or more, typically 0.0002% by weight or more. From the viewpoint of reducing haze, the concentration is suitably 1% by weight or less, preferably 0.5% by weight or less, more preferably 0.3% by weight or less.

[0061] (chelating agent) The preliminary polishing liquid may contain a chelating agent as an optional component. The chelating agent forms a complex ion with metal impurities that may be contained in the preliminary polishing liquid and captures the complex ion, thereby suppressing contamination of the polishing object by metal impurities. Examples of the chelating agent include aminocarboxylic acid-based chelating agents and organic phosphonic acid-based chelating agents. Examples of the aminocarboxylic acid-based chelating agents include ethylenediaminetetraacetic acid, sodium ethylenediaminetetraacetate, nitrilotriacetic acid, sodium nitrilotriacetate, ammonium nitrilotriacetate, hydroxyethylethylenediaminetriacetic acid, sodium hydroxyethylethylenediaminetriacetate, diethylenetriaminepentaacetic acid, sodium diethylenetriaminepentaacetate, triethylenetetraminehexaacetic acid, and sodium triethylenetetraminehexaacetate. Examples of organic phosphonic acid chelating agents include 2-aminoethylphosphonic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, aminotri(methylenephosphonic acid), ethylenediaminetetrakis(methylenephosphonic acid), diethylenetriaminepenta(methylenephosphonic acid), ethane-1,1-diphosphonic acid, ethane-1,1,2-triphosphonic acid, ethane-1-hydroxy-1,1-diphosphonic acid, ethane-1-hydroxy-1,1,2-triphosphonic acid, ethane-1,2-dicarboxy-1,2-diphosphonic acid, methanehydroxyphosphonic acid, 2-phosphonobutane-1,2-dicarboxylic acid, 1-phosphonobutane-2,3,4-tricarboxylic acid and α-methylphosphonosuccinic acid.Of these, organic phosphonic acid chelating agents are more preferred. Among them, preferred are ethylenediaminetetrakis(methylenephosphonic acid), diethylenetriaminepenta(methylenephosphonic acid) and diethylenetriaminepentaacetic acid. Particularly preferred are ethylenediaminetetrakis(methylenephosphonic acid) and diethylenetriaminepenta(methylenephosphonic acid). The chelating agent can be used alone or in combination of two or more.

[0062] (Other Ingredients) The preliminary polishing liquid may further contain, as necessary, known additives that can be used in polishing liquids, such as water-soluble polymers, surfactants, organic acids, organic acid salts, inorganic acids, inorganic acid salts, preservatives, and antifungal agents, within the scope that does not significantly impair the effects of the present invention.

[0063] It is preferable that the preliminary polishing liquid does not substantially contain an oxidizing agent. If the preliminary polishing liquid contains an oxidizing agent, the surface of the object to be polished may be oxidized by supplying the preliminary polishing liquid to the object to be polished, resulting in an oxide film, which may result in a decrease in the polishing rate. The object to be polished may be, for example, a silicon substrate. Specific examples of the oxidizing agent referred to here include hydrogen peroxide (H2O2), sodium persulfate, ammonium persulfate, sodium dichloroisocyanurate, etc. Note that the preliminary polishing liquid being substantially free of an oxidizing agent means that the oxidizing agent is not intentionally contained at least.

[0064] (pH) The pH of the preliminary polishing liquid is typically 8.0 or more, preferably 8.5 or more, more preferably 9.0 or more, even more preferably 9.5 or more, for example 10.0 or more. When the pH of the preliminary polishing liquid is high, the polishing rate and the ability to eliminate bumps tend to improve. On the other hand, from the viewpoint of preventing dissolution of the abrasive grains and suppressing the deterioration of the mechanical polishing action of the abrasive grains, the pH of the preliminary polishing liquid is suitably 12.0 or less, preferably 11.8 or less, more preferably 11.5 or less, and even more preferably 11.0 or less. The same pH can also be preferably adopted in the finish polishing liquid described later.

[0065] In the technology disclosed herein, the pH of a liquid composition can be determined by performing three-point calibration using a pH meter, placing a glass electrode in the composition to be measured, and measuring the value after 2 minutes or more have elapsed and the value has stabilized. The liquid composition can be a polishing liquid, a concentrated solution thereof, a rinse liquid described below, etc. Examples of standard buffer solutions include phthalate pH buffer solution: pH 4.01 (25°C), neutral phosphate pH buffer solution: pH 6.86 (25°C), and carbonate pH buffer solution: pH 10.01 (25°C).

[0066] <Preliminary polishing process> The preliminary polishing process disclosed herein is carried out in the above-mentioned manner by carrying out a first preliminary polishing stage in which the object to be polished is polished with a first polishing liquid, a second preliminary polishing stage in which the object to be polished is polished with a second polishing liquid, and a third preliminary polishing stage in which the object to be polished is polished with a third polishing liquid in this order. The object to be polished can also be generally understood as a workpiece. When starting and ending the supply of each polishing liquid, the supply amount may be changed gradually or stepwise, or may be changed all at once.

[0067] In a preferred embodiment, in the preliminary polishing step, a first polishing liquid, a second polishing liquid, and a third polishing liquid are prepared, and the first polishing liquid is supplied to the substrate to be polished to start the first preliminary polishing stage. After a predetermined time has elapsed from the start of the first preliminary polishing stage, the polishing liquid supplied is changed from the first polishing liquid to the second polishing liquid to start the second preliminary polishing stage. After a predetermined time has elapsed from the start of the second preliminary polishing stage, the polishing liquid supplied is changed from the second polishing liquid to the third polishing liquid to start the third preliminary polishing stage. This allows multiple preliminary polishing stages to be suitably performed on the same platen.

[0068] In another preferred embodiment, the second polishing liquid is a mixture of the first polishing liquid and the third polishing liquid. The second pre-polishing stage is performed by simultaneously supplying the first polishing liquid and the third polishing liquid to the substrate to be polished. In one embodiment, the supply time of the first polishing liquid and the supply time of the third polishing liquid are partially overlapped, and the second pre-polishing stage is performed in the overlapping portion. Typically, in the pre-polishing step, the first polishing liquid and the third polishing liquid are prepared, and the first polishing liquid is supplied to the substrate to be polished to start the first pre-polishing stage. After a predetermined time has elapsed from the start of the first pre-polishing stage, the third polishing liquid is supplied while continuing the supply of the first polishing liquid to start the second pre-polishing stage. After a predetermined time has elapsed from the start of the second pre-polishing stage, the supply of the first polishing liquid is stopped while continuing the supply of the third polishing liquid to start the third pre-polishing stage. In this way, the first polishing liquid and the third polishing liquid are supplied simultaneously to perform the second pre-polishing stage, so that the polishing method disclosed herein can be performed more simply and effectively.

[0069] The ratio of the supply rate of the first polishing liquid to the supply rate of the third polishing liquid in the second preliminary polishing stage (first polishing liquid / third polishing liquid) is not particularly limited. From the viewpoint of polishing efficiency, etc., the supply rate ratio is usually appropriate to be 2 or more, preferably 3 or more, more preferably 5 or more, and even more preferably 8 or more. From the viewpoint of obtaining a flatter surface, etc., the supply rate ratio is usually appropriate to be 50 or less, preferably 40 or less, more preferably 30 or less, and even more preferably 25 or less.

[0070] In another embodiment, the second polishing liquid is a mixture of the first polishing liquid and the fourth polishing liquid. The fourth polishing liquid may contain one or more of the abrasive grains and water-soluble polymers exemplified as those usable in the preliminary polishing liquid. The second preliminary polishing stage is performed by simultaneously supplying the first polishing liquid and the fourth polishing liquid to the substrate to be polished. Typically, in the preliminary polishing step, the first polishing liquid, the third polishing liquid, and the fourth polishing liquid are prepared, and the first polishing liquid is supplied to the substrate to be polished to start the first preliminary polishing stage. After a predetermined time has elapsed from the start of the first preliminary polishing stage, the fourth polishing liquid is supplied while continuing to supply the first polishing liquid to start the second preliminary polishing stage. After a predetermined time has elapsed from the start of the second preliminary polishing stage, the polishing liquid to be supplied is changed from the first polishing liquid and the fourth polishing liquid to the third polishing liquid to start the third preliminary polishing stage. The technology disclosed herein may also be implemented in an embodiment in which the first polishing liquid and the fourth polishing liquid are supplied simultaneously in this way to perform the second preliminary polishing stage.

[0071] The polishing time T1 in the first preliminary polishing stage is not particularly limited, but it is preferable that the relationship with the polishing time T3 in the third preliminary polishing stage satisfies T3 < T1. For example, the magnification of the polishing time T1 in the first preliminary polishing stage with respect to the polishing time T3 in the third preliminary polishing stage, that is, the ratio T1 / T3 of T1 to T3, is usually suitably set to 2 times or more. From the viewpoint of shortening the required polishing time and the like, the magnification T1 / T3 is preferably 3 times or more, more preferably 4 times or more, and even more preferably 5 times or more. Also, the magnification T1 / T3 is usually suitably 15 times or less, preferably 10 times or less, and more preferably 8 times or less. By performing the first preliminary polishing stage and the third preliminary polishing stage with such a ratio of polishing times, shortening of the required polishing time and reduction of surface defects can be preferably achieved simultaneously. The polishing time T1 in the first preliminary polishing stage can be set, for example, to 10 minutes to 30 minutes, typically 15 minutes to 25 minutes.

[0072] The polishing time T2 in the second preliminary polishing stage is not particularly limited, but it is preferable that the relationship with the polishing time T1 in the first preliminary polishing stage satisfies T2 < T1. For example, the magnification of the polishing time T1 in the first preliminary polishing stage with respect to the polishing time T2 in the second preliminary polishing stage, that is, the ratio T1 / T2 of T1 to T2, is usually suitably set to 2 times or more. From the viewpoint of shortening the required polishing time and the like, the magnification T1 / T2 is preferably 3 times or more, more preferably 4 times or more, and even more preferably 5 times or more. Also, the magnification T1 / T2 is usually suitably 15 times or less, preferably 10 times or less, and more preferably 8 times or less. By performing the first preliminary polishing stage and the second preliminary polishing stage with such a ratio of polishing times, shortening of the required polishing time and improvement of surface flatness can be preferably achieved simultaneously. The polishing time T2 in the second preliminary polishing stage can be set, for example, to 0.3 minutes to 8 minutes, typically 0.5 minutes to 3 minutes.

[0073] The polishing time T3 in the third preliminary polishing stage is not particularly limited. The polishing time T3 in the third preliminary polishing stage may be shorter or longer than the polishing time T2 in the second preliminary polishing stage, but is more preferably longer. For example, the ratio of the polishing time T3 in the third preliminary polishing stage to the polishing time T2 in the second preliminary polishing stage, that is, the ratio T3 / T2 of T3 to T2, is usually 0.5 to 3 times, preferably 0.8 to 2.5 times, more preferably 0.9 to 2 times, and even more preferably 1 to 2 times, for example 1.1 to 1.5 times. By carrying out the second preliminary polishing stage and the third preliminary polishing stage at such a polishing time ratio, it is possible to suitably achieve both improvement of surface flatness and reduction of surface defects. The polishing time T3 in the third preliminary polishing stage can be set, for example, to 0.5 to 10 minutes, typically 1 to 5 minutes.

[0074] The preliminary polishing process disclosed herein may include a preliminary polishing stage Ei, which is performed before a first preliminary polishing stage in which the object to be polished is polished with a first polishing liquid, by supplying a polishing liquid Ei to the object to be polished on the same platen as the first preliminary polishing stage. Such a preliminary polishing stage may be preferably performed in a manner in which the polishing liquid supplied to the object to be polished is switched from the polishing liquid Ei to the first polishing liquid during the polishing of the object to be polished. In addition, the preliminary polishing process disclosed herein may include a preliminary polishing stage Fi, which is performed after a third preliminary polishing stage in which the object to be polished is polished with a third polishing liquid, by supplying a polishing liquid Fi to the object to be polished on the same platen as the third preliminary polishing stage. Such a preliminary polishing process may be preferably performed in a manner in which the polishing liquid supplied to the object to be polished is switched from the third polishing liquid to the polishing liquid Fi during the polishing of the object to be polished. Each of the preliminary polishing stages Ei and Fi may include two or more polishing stages.

[0075] In the technology disclosed herein, the number of the multiple pre-polishing steps performed on the same platen, i.e., the multiple pre-polishing steps including at least the first pre-polishing step, the second pre-polishing step, and the third pre-polishing step, may be three or four or more. From the viewpoint of avoiding the pre-polishing process becoming excessively complicated, it is usually appropriate to set the number of the pre-polishing steps to six or less. A pre-polishing process including four or more pre-polishing steps can be preferably carried out in an embodiment in which the first step, the second step, and the third step are the first three steps or the last three steps.

[0076] The pre-polishing step may further include one or more pre-polishing steps performed on a separate platen in addition to the multiple pre-polishing steps performed on the same platen. The separate platen may be, for example, a separate platen of the same polishing apparatus or a separate platen of a polishing apparatus.

[0077] <Finishing polishing liquid> The object to be polished that has finished the preliminary polishing step is typically further subjected to a final polishing step.Therefore, the subject matter disclosed in this specification includes a method for polishing a substrate, which comprises a preliminary polishing step in any of the polishing methods disclosed herein and a final polishing step carried out after the preliminary polishing step, a method for producing a polished object characterized by applying the polishing method, and a polishing composition set that can be preferably used in the above-mentioned polishing method or production method.

[0078] The final polishing step is usually performed by using a polishing machine different from that used in the preliminary polishing step, supplying a final polishing liquid to the object to be polished. The final polishing step may include a plurality of final polishing steps performed on the same or different polishing plates.

[0079] The final polishing liquid used in the final polishing step typically contains abrasive grains and water. The water may be the same as that used in the preliminary polishing liquid.

[0080] (Abrasive grain) As the abrasive grains for the finish polishing liquid, silica particles can be preferably used, as in the preliminary polishing liquid. As the silica particles, colloidal silica is particularly preferable, and for example, colloidal silica produced by an ion exchange method using water glass (sodium silicate) as a raw material can be preferably used. The colloidal silica can be used alone or in combination of two or more types. The preferred true specific gravity, outer shape and average aspect ratio of the abrasive grains of the silica particles are the same as those of the abrasive grains of the preliminary polishing liquid, so that the overlapping descriptions will be omitted.

[0081] The average primary particle size of the abrasive grains contained in the finishing polishing liquid is not particularly limited. From the viewpoint of polishing efficiency, the average primary particle size is preferably 5 nm or more, more preferably 10 nm or more. From the viewpoint of obtaining a higher polishing effect, such as reducing haze and removing defects, the average primary particle size is preferably 15 nm or more, more preferably 20 nm or more, for example, more than 20 nm. In addition, from the viewpoint of easily obtaining a surface with higher smoothness, the average primary particle size of the abrasive grains is preferably 100 nm or less, more preferably 50 nm or less, and even more preferably 40 nm or less. From the viewpoint of easily obtaining a higher quality surface, abrasive grains having an average primary particle size of 35 nm or less, typically less than 35 nm, preferably less than 32 nm, for example less than 30 nm may be used.

[0082] The content of abrasive grains in the final polishing liquid is not particularly limited. In one embodiment, the content is preferably 0.01% by weight or more, more preferably 0.03% by weight or more, even more preferably 0.05% by weight or more, for example 0.08% by weight or more. By increasing the content of abrasive grains, a higher polishing effect can be realized. In addition, from the viewpoint of removability from the polishing object, the content of abrasive grains in the final polishing liquid is usually 7% by weight or less, preferably 5% by weight or less, more preferably 3% by weight or less, even more preferably 2% by weight or less, for example 1% by weight or less.

[0083] (Water-soluble polymer) The finish polishing liquid preferably contains a water-soluble polymer, which may be one or more of the water-soluble polymers exemplified as those usable in the preliminary polishing liquid.

[0084] (Basic compounds) The finish polishing liquid preferably contains a basic compound. As the basic compound, one or more of the basic compounds exemplified as the basic compounds that can be used in the preliminary polishing liquid can be used.

[0085] (Surfactant) In a preferred embodiment, the finish polishing liquid may contain a surfactant. The surfactant may contribute to improving the dispersion stability of the polishing liquid or its concentrate. Anionic or nonionic surfactants may be preferably used as the surfactant. From the viewpoint of low foaming and ease of pH adjustment, nonionic surfactants are more preferable. Examples of nonionic surfactants include oxyalkylene polymers such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; polyoxyalkylene adducts such as polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene alkylamines, polyoxyethylene fatty acid esters, polyoxyethylene glyceryl ether fatty acid esters, and polyoxyethylene sorbitan fatty acid esters; and copolymers of multiple oxyalkylenes. Examples of copolymers of multiple oxyalkylenes include diblock copolymers, triblock copolymers, random copolymers, and alternating copolymers. The surfactants may be used alone or in combination of two or more.

[0086] The Mw of the surfactant is typically 1×10 4It is less than 9500, and preferably 9500 or less from the viewpoint of filterability of the polishing liquid and washability of the object to be polished. The Mw of the surfactant is typically 200 or more, and preferably 250 or more from the viewpoint of haze reduction effect, and more preferably 300 or more, for example, 500 or more. The Mw of the surfactant can be a value determined by GPC (water-based, polyethylene glycol equivalent) or a value calculated from a chemical formula. The technology disclosed herein can be implemented in an embodiment using a finish polishing liquid that does not substantially contain a surfactant as described above.

[0087] (Other Ingredients) The final polishing liquid may further contain known additives that can be used in polishing liquids, such as chelating agents, organic acids, organic acid salts, inorganic acids, inorganic acid salts, preservatives, and antifungal agents, as necessary, within the scope that does not significantly impair the effects of the present invention. As the chelating agent, the same chelating agent that can be used in the preliminary polishing liquid may be used. The technology disclosed herein may be implemented in an embodiment that uses a final polishing liquid that does not substantially contain a chelating agent.

[0088] It is preferable that the finish polishing liquid does not substantially contain an oxidizing agent, like the preliminary polishing liquid.

[0089] <Polishing> The polishing in the preliminary polishing step and the finish polishing step can be carried out, for example, in a manner including the following operations. That is, the polishing liquid used in each polishing step or each polishing stage is prepared. Then, the polishing liquid (e.g., working slurry) is supplied to the object to be polished, and polished by a conventional method. For example, the object to be polished is set in a polishing device, and the polishing liquid is supplied to the surface of the object to be polished (the surface to be polished) through a polishing pad fixed to the platen (polishing platen) of the polishing device. Typically, the polishing pad is pressed against the surface of the object to be polished, and the two are moved relatively (e.g., rotated) while the polishing liquid is continuously supplied.

[0090] Each polishing liquid may be in a concentrated form before being supplied to the object to be polished. The concentrated form is the form of a concentrated polishing liquid, and may also be understood as the stock liquid of the polishing liquid. Such a concentrated polishing liquid is advantageous from the viewpoint of convenience and cost reduction during production, distribution, storage, etc. The concentration ratio is not particularly limited, and can be, for example, about 2 to 100 times in volume conversion, and is usually about 5 to 50 times, for example, about 10 to 40 times.

[0091] Such a concentrated solution can be used in such a manner that the polishing solution is prepared by diluting it at a desired timing, and the polishing solution is then supplied to the object to be polished. The dilution can be performed, for example, by adding water to the concentrated solution and mixing it.

[0092] The content of the abrasive grains in the concentrated liquid can be, for example, 50% by weight or less. In view of the handling property of the concentrated liquid, for example, the dispersion stability of the abrasive grains and filterability, the content of the abrasive grains in the concentrated liquid is usually preferably 45% by weight or less, more preferably 40% by weight or less. In view of convenience and cost reduction during production, distribution, storage, etc., the content of the abrasive grains can be, for example, 0.5% by weight or more, preferably 1% by weight or more, more preferably 3% by weight or more, for example 4% by weight or more. In a preferred embodiment, the content of the abrasive grains may be 5% by weight or more, 10% by weight or more, for example 15% by weight or more, or 20% by weight or more, or 30% by weight or more.

[0093] The polishing liquid or its concentrate used in the technology disclosed herein may be a one-component type or a multi-component type such as a two-component type. For example, the polishing liquid may be prepared by mixing at least part A containing abrasive grains and part B containing the remaining components of the polishing liquid, and diluting the mixture at an appropriate time as necessary.

[0094] The method for preparing the polishing liquid or its concentrate is not particularly limited. For example, the components contained in the polishing liquid or its concentrate may be mixed using a known mixing device such as a blade stirrer, an ultrasonic disperser, or a homomixer. The manner in which these components are mixed is not particularly limited, and for example, all the components may be mixed at once, or may be mixed in an appropriately set order.

[0095] In each polishing step or each polishing stage, the polishing liquid may be used in a manner that it is used once for polishing and then discarded (so-called "run-through"), or may be recycled and reused. One example of a method for recycling the polishing liquid is a method in which the used polishing liquid discharged from the polishing apparatus is collected in a tank and the collected polishing liquid is supplied again to the polishing apparatus.

[0096] The polishing pad used in each platen is not particularly limited. For example, a polishing pad of a polyurethane foam type, a nonwoven fabric type, a suede type, etc. can be used. Each polishing pad may or may not contain abrasive grains.

[0097] The polishing device may be a double-sided polishing device that simultaneously polishes both sides of the object to be polished, or a single-sided polishing device that polishes only one side of the object to be polished. Although not particularly limited, for example, a double-sided polishing device, such as a batch-type double-sided polishing device, may be preferably used in the preliminary polishing step. Also, a single-sided polishing device may be preferably used in the finish polishing step. The number of platens provided in each polishing device may be one or two or more. Each polishing device may be a single-wafer type polishing device configured to polish one object to be polished at a time, or a batch-type polishing device that can polish multiple objects to be polished simultaneously on the same platen.

[0098] Although not particularly limited, in a plurality of preliminary polishing steps carried out on the same platen, the supply rate of the polishing liquid to the platen is usually appropriate to be 0.3 L / min or more, preferably 0.5 L / min or more, more preferably 1 L / min or more, for example 2 L / min or more, from the viewpoint of polishing efficiency, etc. Also, the supply rate of the polishing liquid to the platen is usually appropriate to be 15 L / min or less, more preferably 10 L / min or less, for example 7 L / min or less, from the viewpoint of economic efficiency and reduction of environmental load, etc. In one embodiment, the total area of ​​the surface to be polished is about 0.71 m 2 The above supply rate can be preferably applied as the supply rate of the polishing liquid per 1000 mm of the total surface area of ​​the polishing target surface. 2 The supply rate of the polishing liquid per total area can be appropriately increased or decreased depending on the total area of ​​the surface to be polished, so that the supply rate per total area is maintained at approximately the same level.

[0099] The object to be polished after the preliminary polishing step is typically washed before the finish polishing step is started. This washing can be performed using an appropriate washing liquid. The washing liquid to be used is not particularly limited, and for example, SC-1 washing liquid, SC-2 washing liquid, etc., which are common in the field of semiconductors, etc., can be used. For example, the SC-1 washing liquid is a mixture of ammonium hydroxide (NH4OH), hydrogen peroxide (H2O2), and water (H2O). For example, the SC-2 washing liquid is a mixture of hydrogen chloride (HCl), H2O2, and H2O. The temperature of the washing liquid can be, for example, room temperature, typically about 15°C to 25°C or higher, up to about 90°C. From the viewpoint of improving the washing effect, a washing liquid of about 50°C to 85°C can be preferably used. The object to be polished after the finish polishing step can also be washed in the same manner. The washing is typically performed outside the polishing device used in the preliminary polishing step, that is, after the object to be polished is removed from the polishing device.

[0100] According to the polishing method disclosed herein, polishing of the object to be polished is completed through the above-mentioned preliminary polishing step and the subsequent finish polishing step. Therefore, as another aspect of the technology disclosed herein, there is provided a method for producing a polished object, characterized in that the above-mentioned object to be polished is polished by applying any one of the polishing methods disclosed herein.

[0101] <Polishing composition set> According to this specification, a polishing composition set that can be preferably used in the polishing method disclosed herein is provided. The polishing composition set includes at least a first preliminary polishing composition and a third preliminary polishing composition that are stored separately from each other. The first preliminary polishing composition can be the first polishing liquid or a concentrated solution thereof. The third preliminary polishing composition can be the third polishing liquid or a concentrated solution thereof. In one embodiment, the polishing liquid further includes a second preliminary polishing composition which is the second polishing liquid or a concentrated liquid thereof. The second preliminary polishing composition is stored separately from the first preliminary polishing composition and the third preliminary polishing composition. The polishing method disclosed herein can be suitably carried out using such a polishing composition set. Therefore, the above-mentioned polishing composition set can be suitably used in the polishing method disclosed herein and the polished product manufacturing method including carrying out the polishing method. Each of the polishing compositions constituting the polishing composition set may be a single-component type, or may be a multi-component type including a two-component type. The multi-component type polishing composition can be stored, for example, in a part A containing at least abrasive grains among the components of each polishing composition and a part B containing the remaining components, and the polishing composition or polishing liquid can be prepared by mixing the above-mentioned part A and the above-mentioned part B and diluting them at an appropriate timing as necessary. EXAMPLES

[0102] Some examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in these examples. In the following description, "%" is based on weight unless otherwise specified.

[0103] 1. Preparation of Polishing Solution (Composition A) Colloidal silica, tetramethylammonium hydroxide (TMAH), potassium carbonate, and ion-exchanged water were mixed to prepare a composition A containing 1.2% by weight of colloidal silica, 0.086% by weight of TMAH, and 0.037% by weight of K2CO3.

[0104] (Composition B) Colloidal silica, ammonia, hydroxyethyl cellulose (HEC: Mw 1200000) and ion-exchanged water were mixed to prepare composition B containing 0.5 wt % colloidal silica, 0.01 wt % ammonia and 0.012 wt % HEC.

[0105] (Composition C) Colloidal silica, TMAH, potassium carbonate, PVP (Mw 45000) and ion-exchanged water were mixed to prepare composition C containing 1.2 wt% colloidal silica, 0.086 wt% TMAH, 0.037 wt% potassium carbonate and 0.0012 wt% PVP.

[0106] (Composition D) Composition D containing PVP at a content of 0.0121% by weight was prepared by mixing PVP (Mw 45000) and ion-exchanged water.

[0107] (Composition E) Polyvinyl alcohol (PVA: Mw 13000) and ion-exchanged water were mixed to prepare composition E containing PVA at a content of 0.00403% by weight.

[0108] (Composition F) Ammonia, HEC and ion-exchanged water were mixed to prepare composition F containing 0.00037% by weight of ammonia and 0.012% by weight of HEC.

[0109] (Composition G) Colloidal silica, ammonia, hydroxyethyl cellulose (HEC: Mw 1200000) and ion-exchanged water were mixed to prepare composition G containing 0.5 wt % colloidal silica, 0.01 wt % ammonia and 0.006 wt % HEC.

[0110] (Composition H) Colloidal silica, TMAH, potassium carbonate, PVP (Mw 45000) and ion-exchanged water were mixed to prepare composition H containing 1.2 wt% colloidal silica, 0.086 wt% TMAH, 0.037 wt% potassium carbonate and 0.012 wt% PVP.

[0111] The pH of each of Compositions A to H was adjusted to be 10 or more and 11 or less. The average primary particle size and content of the abrasive grains, the content of the basic compound, and the content of the water-soluble polymer used in each composition are shown in Table 1. The average primary particle size of the abrasive grains was determined using a surface area measuring device manufactured by Micromeritics, product name "Flow Sorb II 2300."

[0112] [Table 1]

[0113] 2.Silicon wafer polishing <Examples 1 to 8> A pre-polishing process consisting of the pre-polishing steps shown in Table 2 was carried out using a polishing solution in which each of the compositions A to H was mixed alone or in combination. The object to be polished (test piece) was a commercially available silicon single crystal wafer (thickness: 785 μm, conductivity type: P type, crystal orientation: <100> , resistivity: 1 Ω·cm or more and less than 100 Ω·cm) was used.

[0114] Specifically, the preliminary polishing step was carried out as follows: Five test pieces (total surface area of ​​surfaces to be polished: approximately 0.71 m2) were placed in a double-sided polishing machine shown below. 2) was set, and the first polishing liquid was supplied to start the first preliminary polishing stage. 18 minutes after the start of the first preliminary polishing stage, the polishing liquid supplied was changed to the second polishing liquid and the second preliminary polishing stage was started. 2.3 minutes after the start of the second preliminary polishing stage, the polishing liquid supplied was changed to the third polishing liquid and the third preliminary polishing stage was started. 3 minutes after the start of the third preliminary polishing stage, the supply of the third polishing liquid and the operation of the double-sided polisher were stopped.

[0115] [Pre-polishing conditions] Polishing equipment: SpeedFam double-sided polishing equipment, model number "DSM20B-5P-4D" Polishing load: 150g / cm 2 Upper plate relative rotation speed: 20 rpm Lower surface plate relative rotation speed: -20 rpm Polishing pad: Nitta Haas, product name "MH S-15A" Processing carrier: Double-sided DLC coated carrier, average thickness 776 microns Polishing environment temperature: 23℃

[0116] (Washing) The test piece after pre-polishing was removed from the polishing machine and washed with a cleaning solution of NH4OH (29%):H2O2 (31%):deionized water (DIW) = 1:3:30 (volume ratio) (SC-1 cleaning). More specifically, two cleaning tanks equipped with ultrasonic oscillators with a frequency of 950 kHz were prepared, the first and second cleaning tanks were each filled with the above cleaning solution and kept at 60°C, and the test piece after pre-polishing was immersed in the first cleaning tank for 6 minutes, then in a rinse tank using ultrapure water and ultrasonic waves, and then in the second cleaning tank for 6 minutes, with the ultrasonic oscillators operating.

[0117] <Comparative Examples 1 to 8> In this example, a pre-polishing process consisting of two pre-polishing stages shown in Table 2 was carried out using a polishing liquid in which each of the compositions A to H was mixed alone or in combination. That is, the first pre-polishing stage was started by supplying the first polishing liquid. After a predetermined time has elapsed from the start of the first pre-polishing stage, the polishing liquid to be supplied was changed to the second polishing liquid to start the second pre-polishing stage. After a predetermined time has elapsed from the start of the second pre-polishing stage, the supply of the second polishing liquid and the operation of the double-side polishing machine were stopped. In other respects, the pre-polishing process for silicon wafers was carried out in the same manner as in Examples 1 to 8.

[0118] 3. Evaluation <Calculation of required polishing time> The average thickness of the test pieces before and after polishing under the above conditions was measured using a flatness measuring device "Nano Metro 300TT" manufactured by Kuroda Precision Industries, Ltd., and the thickness reduction due to polishing (polishing allowance) was calculated. When the polishing removal amount was not 10 μm, the polishing time was changed from the above polishing conditions to find the polishing time at which the polishing removal amount was 10 μm, and this was recorded as the required polishing time [min]. Here, the required polishing time was calculated as the sum of the polishing time in the first preliminary polishing stage, the polishing time in the second preliminary polishing stage, and the polishing time in the third preliminary polishing stage.

[0119] <Number of defects> The silicon wafers obtained in each example (test pieces that had been subjected to the preliminary polishing process and subsequent cleaning) were analyzed using a SURFSCAN SP2 manufactured by KLA Tencor. XP The entire surface of the wafer was inspected using a "Test Tool" and the number of defects larger than 0.2 microns was counted. The number of defects obtained was evaluated on a four-point scale as follows. The results are shown in the "Number of Defects" column in Table 2. 4: 10 pieces or less 3: More than 10 and less than 20 2: More than 20 and less than 30 Over 1:30 pieces

[0120] <Flatness (GBIR)> GBIR (edge ​​exclusion area 2 mm) was measured in accordance with SEMI standards using a flatness measuring device "Nano Metro 300TT" manufactured by Kuroda Precision Industries Co., Ltd. The measured values ​​were evaluated on the following three-point scale. 3:200nm or less 2: Over 200nm and 300nm or less More than 1:300nm

[0121] The evaluation results of the required polishing time, the number of defects, and the flatness are shown in Table 2. Table 2 also shows the composition used in each pre-polishing step, the flow rate, the polishing time, and the content of the water-soluble polymer in the second pre-polishing step.

[0122] [Table 2]

[0123] As shown in Tables 1 and 2, in Examples 1 to 4, 7, and 8, the content COM of the water-soluble polymer contained in the first polishing liquid was P1 and the content COM of the water-soluble polymer P2 contained in the second polishing liquid. P2 and the content COM of the water-soluble polymer P3 contained in the third polishing liquid. P3 Relationship with COM P1 <COM P2 <COM P3 and the third polishing liquid does not contain abrasive grains. P1 <COM P2 <COM P3 and the average primary particle diameter D of the abrasive grains A3 contained in the third polishing liquid A3 is the average primary particle diameter D of the abrasive grains A1 contained in the first polishing liquid. A1 and the average primary particle diameter D of the abrasive grains A2 contained in the second polishing liquid A2is smaller than . According to Examples 1 to 8, in which a preliminary polishing process consisting of such three preliminary polishing stages was carried out, the required polishing time was short, and a high-quality surface with high flatness and few defects was efficiently obtained. In contrast, it was confirmed that all of Comparative Examples 1 to 4, in which a preliminary polishing process consisting of two preliminary polishing stages was carried out, lacked a balance between improved flatness, reduced surface defects, and shortened required polishing time. Moreover, in Comparative Examples 5 and 6, the content COM of the water-soluble polymer contained in the first polishing liquid was 0.01 to 0.01. P1 and the content COM of the water-soluble polymer P2 contained in the second polishing liquid. P2 and the content COM of the water-soluble polymer P3 contained in the third polishing liquid. P3 Relationship with COM P1 <COM P2 <COM P3 In Comparative Example 7, the average primary particle diameter D A3 is the average primary particle diameter D of the abrasive grains A1 contained in the first polishing liquid. A1 and the average primary particle diameter D of the abrasive grains A2 contained in the second polishing liquid A2 The content of the water-soluble polymer and the average primary particle size of the abrasive grains in Comparative Example 8 do not satisfy the above-mentioned preferable conditions. It was confirmed that each of Comparative Examples 5 to 8 lacks a balance between the improvement of flatness, the reduction of surface defects, and the shortening of the required polishing time.

[0124] Although specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above.

Claims

1. 1. A method of polishing a substrate, comprising: a preliminary polishing step of pre-polishing the substrate by using a double-sided polishing machine and supplying a preliminary polishing liquid thereto; and a finish polishing step of finish-polishing the substrate by using a single-sided polishing machine and supplying a finish polishing liquid thereto after the preliminary polishing step, The pre-polishing process includes multiple pre-polishing stages carried out on the same platen, the plurality of pre-polishing steps include, in this order, a first pre-polishing step performed by supplying a first polishing liquid as the preliminary polishing liquid to the substrate, a second pre-polishing step performed by supplying a second polishing liquid as the preliminary polishing liquid, and a third pre-polishing step performed by supplying a third polishing liquid as the preliminary polishing liquid; The water-soluble polymer P contained in the first polishing liquid 1 Content of COM P1 and the water-soluble polymer P contained in the second polishing liquid. 2 Content of COM P2 and the water-soluble polymer P contained in the third polishing liquid. 3 Content of COM P3 The relationship with COM P1 <COM P2 <COM P3 Fulfilling The second polishing liquid contains abrasive grains A 2 Including, And the following conditions: (1) Abrasive grains A contained in the third polishing liquid 3 Average primary particle diameter D A3 is abrasive grain A contained in the first polishing liquid 1 Average primary particle diameter D A1 and abrasive grains A contained in the second polishing liquid 2 Average primary particle diameter D A2 is less than; and (2) The third polishing liquid contains abrasive grain A 3 Does not contain; A polishing method that satisfies either one of the above.

2. Abrasive grains A contained in the first polishing liquid 1 Content of COM A1 and the content COM of abrasive grains A2 contained in the second polishing liquid. A2 and the content COM of abrasive grains A3 contained in the third polishing liquid. A3 The relationship with COM A3 <COM A2 <<COM A1 The polishing method according to claim 1 , wherein the above formula (1) is satisfied.

3. A polishing composition set for use in the polishing method according to claim 1 or 2, a first preliminary polishing composition which is the first polishing liquid or a concentrated solution thereof; a second preliminary polishing composition which is the second polishing liquid or a concentrated solution thereof; and a third preliminary polishing composition which is the third polishing liquid or a concentrated solution thereof, The polishing composition set, wherein the first preliminary polishing composition and the third preliminary polishing composition are stored separately from each other.

4. The polishing composition set described in claim 3, wherein the second preliminary polishing composition is stored separately from the first preliminary polishing composition and the third preliminary polishing composition.

Citation Information

Patent Citations

  • Finish polishing method for semiconductor wafer

    JP2001239452A

  • Method for polishing semiconductor wafer

    JP2003257906A

  • Semiconductor wafer and manufacturing method thereof

    JP2010021487A

  • Process for polishing semiconductor wafer

    JP2014103398A

  • Method of continuously manufacturing semiconductor substrate

    JP2015159259A