Coated Tools

The coated tool with a Ti(C x N 1-x) coating layer and controlled carbon content and KAM values addresses peeling and chipping issues, enhancing adhesion and wear resistance under heavy cutting conditions.

JP7566153B2Active Publication Date: 2024-10-11KYOCERA CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023531352
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-07-02
Filing Date
2022-01-25
Publication Date
2024-10-11
Estimated Expiration
2042-01-25

AI Technical Summary

Technical Problem

Conventional coated tools face issues with peeling and chipping of the coating layer due to large impacts during heavy interrupted cutting, necessitating improved wear resistance and adhesion between the cemented carbide base and the coating layer.

Method used

A coated tool with a substrate made of cemented carbide and a coating layer comprising a first layer of Ti(C x N 1-x) (0≦x≦1) is designed, where the carbon content in regions near the surface is higher than in deeper regions, and the average Kernel Average Misorientation (KAM) values are controlled to less than 0.4°, enhancing adhesion and reducing strain.

Benefits of technology

The design significantly improves the adhesion between the base and the coating layer, preventing peeling and chipping, even under severe cutting conditions, with enhanced wear resistance and fracture resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566153000004
    Figure 0007566153000004
  • Figure 0007566153000005
    Figure 0007566153000005
  • Figure 0007566153000001
    Figure 0007566153000001
Patent Text Reader

Abstract

A coated tool according to a nonlimiting aspect of the present disclosure comprises a base body made of a cemented carbide alloy, and a coating layer positioned on the surface of the base body. The coating layer includes a first layer in contact with the base body. The first layer contains Ti (CxN1-x) (0 ≤ x ≤ 1). The base body contains a plurality of WC particles. A region from the surface of the base body to 5 µm in depth is defined as a first region, and a region between 100 µm and 200 µm in depth, both inclusive, from the surface of the base body is defined as a second region. The maximum value of the carbon content of the first region is defined as a first carbon content, and the maximum value of the carbon content of the second region is defined as a second carbon content. The first carbon content is greater than the second carbon content. An average value of the KAM value of the first region is less than 0.4°.
Need to check novelty before this filing date? Find Prior Art

Description

CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims priority to Japanese Patent Application No. 2021-110444, filed on July 2, 2021, the entire disclosure of which is incorporated herein by reference. [Technical field]

[0002] The present disclosure relates to a coated tool having a coating layer on a surface of a substrate. [Background technology]

[0003] 2. Description of the Related Art Conventionally, coated tools have been known in which one or more layers such as a titanium carbide layer, a titanium nitride layer, a titanium carbonitride layer, an aluminum oxide layer, and a titanium aluminum nitride layer are formed on the surface of a substrate made of cemented carbide.

[0004] Coated tools are required to have high wear resistance and chipping resistance, and for example, cutting tools are increasingly being used for heavy interrupted cutting, where a large impact is applied to the cutting edge, as cutting processes become more efficient. Under such severe cutting conditions, it is necessary to suppress peeling and chipping of the coating layer due to the large impact applied to the coating layer.

[0005] JP 2011-152602 A (Patent Document 1) discloses a cutting tool in which a titanium nitride layer is formed as a coating layer on the surface of a base by physical vapor deposition. It also discloses that the crystal orientation of titanium nitride crystal grains on the surface of the coating layer, which is measured by an electron backscatter diffraction (EBSD) device, is within a predetermined range.

[0006] Coated tools are required to be able to be used under more severe machining conditions in order to improve machining efficiency, and there is a demand for improving the adhesion between the cemented carbide substrate and the coating layer to suppress peeling and chipping of the coating layer. Summary of the Invention

[0007] A coated tool according to one non-limiting aspect of the present disclosure has a substrate made of cemented carbide and a coating layer located on the surface of the substrate. The coating layer has a first layer in contact with the substrate. The first layer is made of Ti(C x N 1-x ) (0≦x≦1). The substrate contains a plurality of WC particles. A region from the surface of the substrate to a depth of 5 μm is defined as a first region, and a region from the surface of the substrate to a depth of 100 μm or more and 200 μm or less is defined as a second region. The maximum carbon amount in the first region is defined as a first carbon amount, and the maximum carbon amount in the second region is defined as a second carbon amount. The KAM value is a value obtained by measuring the WC particles by an electron backscatter diffraction (EBSD) method using a scanning electron microscope equipped with an electron backscatter diffraction image system under the conditions that the distance (step size) between adjacent pixels is 0.1 μm, and the orientation difference between adjacent pixels is 5° or more, and is regarded as a grain boundary. The first carbon amount is greater than the second carbon amount. The average value of the KAM value in the first region is less than 0.4°. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a perspective view of a non-limiting one-sided coated tool (cutting tool) of the present disclosure. [Diagram 2] FIG. 2 is a cross-sectional view of the coated tool shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] <Coated tools> Hereinafter, a non-limiting one-sided coated tool 1 (hereinafter, sometimes referred to as "tool 1") of the present disclosure will be described in detail with reference to the drawings. However, for the sake of convenience, each of the drawings referred to below shows a simplified view of only the main components necessary for explaining the embodiment. Therefore, the tool 1 may include any component not shown in each of the drawings referred to. Furthermore, the dimensions of the components in each drawing do not faithfully represent the actual dimensions of the component components and the dimensional ratios of each component.

[0010] 1 and 2, a cutting tool (cutting insert) is shown as an example of the tool 1. Note that the tool 1 is not limited to a cutting tool. The tool 1 may be, for example, an excavation tool or a cutting tool.

[0011] As shown in FIG. 1 as an example, the tool 1 may have a first surface 2 (top surface in FIG. 1), a second surface 3 (side surface in FIG. 1), and a cutting edge 4 located at the intersection of the first surface 2 and the second surface 3. At least a part of the first surface 2 can function as a rake surface. At least a part of the second surface 3 can function as a flank surface. The cutting edge 4 can be used to cut a workpiece. In other words, the tool 1 can cut the workpiece by bringing the cutting edge 4 into contact with the workpiece. The cutting edge 4 may be located at the entire intersection of the first surface 2 and the second surface 3, or may be located at only a part of the intersection of the first surface 2 and the second surface 3.

[0012] The tool 1 may have a substrate 5 and a coating layer 6 located on the surface of the substrate 5, as in an example shown in FIG.

[0013] The substrate 5 may be made of a cemented carbide. Examples of the composition of the cemented carbide include WC-Co, WC-TiC-Co, and WC-TiC-TaC-Co. Here, WC (tungsten carbide), TiC (titanium carbide), and TaC (tantalum carbide) are hard particles, and Co (cobalt) is a binder phase. The above composition is an example, and the substrate 5 may have another composition having, for example, WC particles, at least one hard phase selected from the group of carbides, nitrides, and carbonitrides of metals in Groups 4, 5, and 6 of the periodic table, and a binder phase made of Co.

[0014] The coating layer 6 may have a first layer 7 in contact with the substrate 5. The first layer 7 is made of Ti(C x N 1-x ) (0≦x≦1).

[0015] The substrate 5 may contain a plurality of WC particles. Here, a region from the surface of the substrate 5 to a depth of 5 μm is defined as the first region 8, and a region from the surface of the substrate 5 to a depth of 100 μm or more and 200 μm or less is defined as the second region 9. The maximum carbon amount in the first region 8 is defined as the first carbon amount, and the maximum carbon amount in the second region 9 is defined as the second carbon amount. Furthermore, under the condition that the distance (step size) between adjacent pixels is 0.1 μm and the orientation difference between adjacent pixels is 5° or more, the WC particles are measured by the electron backscatter diffraction (EBSD) method using a scanning electron microscope (SEM) equipped with an electron backscatter diffraction image system, and the KAM value is defined as the value. The first carbon amount may be greater than the second carbon amount. The average value of the KAM value in the first region 8 may be less than 0.4°.

[0016] In the above case, the amount of deformation of the WC particles present on the surface of the substrate 5 is reduced, and the residual stress between the substrate 5 and the first layer 7 is reduced. This improves the adhesion between the substrate 5 and the coating layer 6, and prevents peeling and chipping of the coating layer 6. When the average KAM value of the first region 8 is less than 0.3°, the adhesion between the substrate 5 and the coating layer 6 can be further improved.

[0017] KAM (Kernel Average Misorientation) represents the local misorientation, which is the difference in crystal orientation between adjacent measurement points measured by the EBSD method, and the KAM value is a value that correlates with the magnitude of plastic strain, etc. In addition, since KAM reflects local deformation and dislocation density at the microscopic level, local plastic deformation at the microscopic level can be confirmed by measuring the KAM value. The average KAM value is calculated by averaging the KAM values ​​measured at each position in the observation area.

[0018] In the conventional process of forming a coating layer, distortion may occur between the substrate made of cemented carbide and the coating layer in contact with it. This is thought to be due to the fact that the carbon content is reduced in the region near the substrate surface compared to the inside of the substrate, and the substrate surface is altered in the process of forming the coating layer. The alteration of the substrate surface tends to leave minute plastic distortions in some of the WC particles present on the substrate surface, which may cause the coating layer to peel off from the substrate when the coated tool is subjected to an impact.

[0019] In the tool 1, the carbon content ratio in the region near the surface of the substrate 5 relative to the inside of the substrate 5 is increased to reduce the strain between the substrate 5 and the coating layer 6, and as a result, the average KAM value in the region near the surface of the substrate 5 is less than 0.4°. Therefore, in the tool 1, minute plastic strains occurring in the WC particles near the surface of the substrate 5 are suppressed, so that the strain between the substrate 5 and the coating layer 6 is small. As a result, even when the tool 1 is subjected to a large impact, the coating layer 6 is unlikely to peel off from the substrate 5.

[0020] The lower limit of the average value of the KAM value in the first region 8 may be 0.1° or more. The substrate 5 may have a thickness of 1 mm or more. The average particle size of the WC particles may be 0.01 to 20.0 μm. The average particle size of the WC particles may be measured by image analysis. In this case, the circle equivalent diameter may be the average particle size of the WC particles. The average particle size of the WC particles may be measured by the following procedure. First, a cross section of the substrate 5 may be observed at a magnification of 3000 to 5000 times using an SEM to obtain an SEM image. At least 50 or more WC particles may be identified and extracted from this SEM image. Then, the circle equivalent diameter may be calculated using image analysis software ImageJ (1.52) to obtain the average particle size of the WC particles.

[0021] The first carbon amount may be 1.10 times or more larger than the second carbon amount. In other words, the ratio of the first carbon amount to the second carbon amount (first carbon amount / second carbon amount) may be 1.10 or more. In this case, the adhesion between the substrate 5 and the coating layer 6 is further improved. The upper limit of the above ratio may be less than 1.40. When the ratio of the first carbon amounts (first carbon amount / second carbon amount) is 1.40 or more, the adhesion between the substrate 5 and the first layer 7 may decrease, and the coating layer 6 may easily peel off from the substrate 5. The carbon amount can be measured by Auger electron spectroscopy (AES analysis). The first carbon amount and the second carbon amount are not limited to specific values. For example, the first carbon amount may be set to 20 atomic % to 75 atomic %, and the second carbon amount may be set to 15 atomic % to 70 atomic %.

[0022] When the carbon amount at the center in the thickness direction of the first layer 7 is defined as the third carbon amount, the third carbon amount may be greater than the second carbon amount. Specifically, the ratio of the third carbon amount to the second carbon amount (third carbon amount / second carbon amount) may be 1.70 or more. In this case, the adhesion between the substrate 5 and the coating layer 6 is further improved. The above ratio may be 1.50 or more. The upper limit of the above ratio may be 2.50 or less. The third carbon amount is not limited to a specific value. For example, the third carbon amount may be set to 15 atomic % to 75 atomic %.

[0023] The first layer 7 may have a thickness of 1 μm or more. In this case, the orientation of the crystal grains in the region of the first layer 7 ranging from the surface of the substrate 5 to 0.3 μm may be different from the orientation of the crystal grains in the center of the thickness direction of the first layer 7. In this case, the chipping resistance is high. The orientation of the crystal grains can be measured by the EBSD method.

[0024] The thickness of the first layer 7 is not limited to a specific one. For example, the thickness of the first layer 7 may be set to 6 to 15 μm. When the thickness of the first layer 7 is 6 μm or more, particularly 10 μm or more, the wear resistance is high. Furthermore, when the thickness of the first layer 7 is 15 μm or less, particularly 13 μm or less, the chipping resistance is high.

[0025] Ti(C x N 1-x )(0 ≦ x ≦ 1) contained in the first layer 7 may be composed of a single layer or may have a structure in which a plurality of layers (layered portions) are laminated. For example, as shown in an example in FIG. 2, the first layer 7 may have a layered first portion 10 in contact with the substrate 5 and a layered second portion 11 located above the first portion 10.

[0026] The carbon contained in the first portion 10 may be less than the carbon contained in the second portion 11. Specifically, the first portion 10 may have titanium nitride (TiN) as the main component. Also, the second portion 11 may have titanium carbonitride (Ti(C x N 1-x )(0 < x < 1)) as the main component. When the first layer 7 has the above structure, the adhesion between the substrate 5 and the first layer 7 is further enhanced. In particular, when the first portion 10 in the first layer 7 is composed of TiN, the diffusion of the cemented carbide components from the substrate 5 to the coating layer 6 is suppressed, so that the alteration of the surface of the substrate 5 can be suppressed. Note that the above "main component" refers to the component with the largest mass% value compared to other components.

[0027] The first portion 10 may be composed of titanium nitride particles having an average particle size of 0.05 to 0.5 μm. The titanium nitride particles may be columnar crystals extending in a direction perpendicular to the surface of the substrate 5.

[0028] In the tool 1, there may be a location where epitaxial growth occurs between the WC particles located on the surface of the substrate 5 and the titanium nitride particles located on the substrate 5 side in the first portion 10. Also, Co may diffuse into the first portion 10 at a ratio of 0.2 to 3 mass%. When Co diffuses in this way, the adhesion between the substrate 5 and the coating layer 6 can be further enhanced.

[0029] The second portion 11 may be composed of a layer-like third portion 12 mainly composed of so-called MT (Moderate Temperature)-titanium carbonitride, and a layer-like fourth portion 13 mainly composed of HT (High Temperature)-titanium carbonitride located on this third portion 12.

[0030] The third portion 12 may be composed of columnar crystals containing acetonitrile (CH3CN) gas as a raw material and formed at a relatively low film formation temperature of 780 to 900° C. In this case, the columnar crystals may have a width of 0.4 μm or less in a direction parallel to the surface of the base 5. When the columnar crystals have the above configuration, the adhesion between the first portion 10 and the fourth portion 13 is further improved.

[0031] The fourth portion 13 may be composed of granular crystals formed at a relatively high film formation temperature of 900 to 1100° C. Furthermore, protrusions that are triangular in cross section and tapered upward may be formed on the surface of the fourth portion 13. When the fourth portion 13 has such protrusions, the fourth portion 13 has high adhesion to the second layer 14 described below, and peeling and chipping of the coating layer 6 can be suppressed.

[0032] The first region 10 and the second region 11 are not limited to a specific thickness. For example, the thickness of the first region 10 may be set to 0.5 to 3 μm. The thickness of the second region 11 may be set to 5.5 to 14.5 μm. When the thickness of the first region 10 is 0.5 to 3 μm, particularly 0.5 to 2.0 μm, and the thickness of the second region 11 is 5.5 to 14.5 μm, particularly 8.0 to 12.5 μm, the coating layer 6 has high adhesion to the substrate 5 and also has high abrasion resistance.

[0033] The covering layer 6 may further include a second layer 14 and a third layer 15 in addition to the first layer 7. The second layer 14 may be located on the first layer 7 (fourth portion 13). The third layer 15 may be located on the second layer 14.

[0034] The second layer 14 may contain titanium and oxygen, and may be composed of, for example, TiCO, TiNO, TiCNO, TiAlCO, TiAlCNO, etc. Specifically, the second layer 14 may contain Ti(C x N 1-x-y O y )(0 < x < 1, 0 < y < 1). Further, the third layer 15 may contain aluminum oxide.

[0035] When the coating layer 6 has the above third layer 15, the wear resistance of the coating layer 6 can be further enhanced. When the second layer 14 is located between the first layer 7 and the third layer 15, the adhesion between the first layer 7 and the third layer 15 can be enhanced.

[0036] Also, when the second layer 14 contains the above components, the aluminum oxide particles constituting the third layer 15 have an α-type crystal structure. The third layer 15 composed of aluminum oxide with an α-type crystal structure has high hardness. Therefore, the wear resistance of the coating layer 6 can be enhanced.

[0037] When the second layer 14 contains Ti(C x N 1-x-y O y ), when x + y = 1, Ti(C x N 1-x-y O y ) in the second layer 14 becomes acicular and has a crystal structure extending in a direction perpendicular to the surface of the substrate 5 at a height of 0.05 to 0.5 μm. With this structure, the adhesion between the second part 11 and the third layer 15 can be enhanced.

[0038] Also, when the third layer 15 is composed of aluminum oxide with an α-type crystal structure, the hardness of the third layer 15 is increased, and the wear resistance of the coating layer 6 can be improved. At this time, in the peaks detected by X-ray diffraction measurement from the surface side of the third layer 15, when I(116) and I(104) are the strongest first and second, the wear of the coating layer 6 tends to be suppressed.

[0039] There is no particular limitation to the thickness of the second layer 14 and the third layer 15. For example, the thickness of the second layer 14 may be set to 0.05 to 5.0 μm. The thickness of the third layer 15 may be set to 1.0 to 15 μm.

[0040] The coating layer 6 may further include a fourth layer 16 in addition to the first layer 7, the second layer 14, and the third layer 15. The fourth layer 16 may be located on the third layer 15. The fourth layer 16 may include Ti(C x N 1-x-y O y ) (0≦x≦1, 0≦y<1). The fourth layer 16 may be made of other materials such as chromium nitride. The fourth layer 16 is not limited to a particular thickness. For example, the thickness of the fourth layer 16 may be set to 0.1 to 3 μm.

[0041] The coating layer 6 may be configured by laminating, in order from the substrate 5 side, a first portion 10 consisting of a titanium nitride layer, a second portion 11 consisting of a titanium carbonitride layer, a second layer 14, a third layer 15, and a fourth layer 16.

[0042] The thickness of each layer and the morphology of the crystals constituting each layer can be measured by observing electron microscope photographs (SEM photographs or transmission electron microscope (TEM) photographs) of the cross section of the tool 1. The crystals constituting each layer of the coating layer 6 being columnar in morphology means that the ratio of the average crystal width to the length of each crystal in the thickness direction of the coating layer 6 is 0.3 or less on average. On the other hand, when the ratio of the average crystal width to the length of each crystal in the thickness direction of the coating layer 6 exceeds 0.3 on average, the crystal morphology is defined as granular.

[0043] <Method of manufacturing coated tools> Next, a non-limiting method for manufacturing a one-sided coated tool according to the present disclosure will be described using the case of manufacturing the tool 1 as an example.

[0044] First, a metal powder, a carbon powder, etc. are appropriately added to an inorganic powder such as a metal carbide, nitride, carbonitride, or oxide that can be formed into the cemented carbide that becomes the base 5 by firing, and mixed to obtain a mixed powder. Next, this mixed powder is molded into a predetermined tool shape by a known molding method such as press molding, casting molding, extrusion molding, or cold isostatic pressing to obtain a molded body. Thereafter, the obtained molded body is fired in a vacuum or a non-oxidizing atmosphere to obtain the base 5 made of the above-mentioned cemented carbide. The surface of the base 5 may be polished or honed.

[0045] Next, a coating layer 6 is formed on the surface of the obtained substrate 5 by a chemical vapor deposition (CVD) method, and the tool 1 is obtained.

[0046] First, the substrate 5 made of cemented carbide may be pretreated by adjusting a mixed gas consisting of 2 to 10 volume % titanium tetrachloride (TiCl4) gas and the remainder hydrogen (H2) gas and introducing it into a chamber (furnace), setting the film formation temperature (furnace temperature) to 800 to 940°C, the pressure to 8 to 50 kPa, and the time to 1 to 10 minutes. In this case, the carbon content in the region near the surface of the substrate 5 is likely to be high. Therefore, when the first layer 7 is next formed, the carbon component near the surface of the substrate 5 is prevented from diffusing and moving to the first layer 7 side, and the WC particles near the surface of the substrate 5 are prevented from being significantly distorted. Therefore, when the substrate 5 is pretreated, the first carbon amount is likely to be greater than the second carbon amount, and the average KAM value of the first region 8 is likely to be less than 0.4°.

[0047] Next, the first portion 10, which is mainly composed of titanium nitride (TiN) in the first layer 7, is formed. The film forming conditions for the first portion 10 include adjusting the reactive gas composition to a mixed gas consisting of 0.5 to 10 volume % titanium tetrachloride (TiCl4) gas, 10 to 60 volume % nitrogen (N2) gas, and the remainder hydrogen (H2) gas, and introducing the gas into the chamber, setting the film forming temperature to 800 to 940°C, and the pressure to 8 to 50 kPa. Under these film forming conditions, the film forming start temperature may be set to a temperature 10 to 50°C lower than the film forming end temperature, and the temperature may be increased during film forming. In this case, the diffusion of W and Co elements in the vicinity of the surface of the substrate 5 can be suppressed, and the occurrence of large distortion in the WC grains in the vicinity of the surface of the substrate 5 can be suppressed.

[0048] Next, the second portion 11 of the first layer 7 is formed. First, the third portion 12, which is mainly composed of MT-titanium carbonitride, is formed in the second portion 11. The conditions for forming the third portion 12 include adjusting the reactive gas composition to a mixed gas consisting of 0.5 to 10 volume % titanium tetrachloride (TiCl4) gas, 0.1 to 3.0 volume % acetonitrile (CH3CN) gas, and the remainder hydrogen (H2) gas, and introducing the mixed gas into the chamber, setting the film formation temperature to 780 to 900°C, and the pressure to 5 to 25 kPa. Under these film formation conditions, the content ratio of acetonitrile (CH3CN) gas may be increased in the later film formation stage compared to the early film formation stage. In this case, the average crystal width of the columnar crystals of titanium carbonitride constituting the third portion 12 can be configured to be larger on the surface side than on the substrate 5 side.

[0049] Next, a fourth portion 13 is formed, the main component of which is HT-titanium carbonitride in the second portion 11. The conditions for forming the fourth portion 13 include adjusting a mixed gas containing 1 to 10 volume % titanium tetrachloride (TiCl4) gas, 5 to 30 volume % nitrogen (N2) gas, 0.1 to 10 volume % methane (CH4) gas, and the remainder hydrogen (H2) gas as a reactive gas composition and introducing the adjusted mixed gas into the chamber, setting the film formation temperature to 900 to 1100°C, and the pressure to 5 to 40 kPa.

[0050] Next, the second layer 14 is formed. The film forming conditions for the second layer 14 include adjusting the reactive gas composition to 3 to 15 volume % of titanium tetrachloride (TiCl4) gas, 3 to 10 volume % of methane (CH4) gas, 0.5 to 2.0 volume % of carbon monoxide (CO) gas, and the remainder being hydrogen (H2) gas, and introducing the adjusted gas into the chamber, setting the film forming temperature to 900 to 1050°C, and the pressure to 5 to 40 kPa. Note that the reactive gas composition may include 10 to 25 volume % of nitrogen (N2) gas. The nitrogen (N2) gas may be replaced with argon (Ar) gas. Under the above film forming conditions, needle-shaped crystals extending in a direction perpendicular to the surface of the substrate 5 are generated in the second layer 14, and the adhesion with the third layer 15 to be formed next can be improved.

[0051] Next, the third layer 15 is formed. The film forming conditions for the third layer 15 are as follows: mixed gas containing 0.5-5.0 volume % aluminum trichloride (AlCl3) gas, 0.5-5.0 volume % hydrogen chloride (HCl) gas, 0.5-5.0 volume % carbon dioxide (CO2) gas, 0-1.0 volume % hydrogen sulfide (H2S) gas, and the remainder hydrogen (H2) gas is used as the reaction gas composition, and the film forming temperature is changed to 950-1100°C and the pressure is changed to 5-20 kPa. The growth state of the aluminum oxide crystals is adjusted according to these film forming conditions to control the orientation of the aluminum oxide crystals. The film forming conditions for the third layer 15 are not limited to one film forming process. The third layer 15 may be formed by a film forming process consisting of multiple stages.

[0052] Next, the fourth layer 16 is formed. For example, the film forming conditions when the fourth layer 16 is made of TiN are as follows: a mixed gas containing 0.1 to 10 volume % titanium tetrachloride (TiCl4) gas, 10 to 60 volume % nitrogen (N2) gas, and the remainder hydrogen (H2) gas is adjusted and introduced into the chamber as the reaction gas composition, the film forming temperature is 960 to 1100°C, and the pressure is 10 to 85 kPa.

[0053] In the obtained tool 1, at least a portion of the surface of the coating layer 6 where the cutting edge 4 is located may be polished. This makes the cutting edge 4 smooth, suppresses adhesion of the workpiece, and provides the tool 1 with excellent chipping resistance.

[0054] The present disclosure will be described in detail below with reference to examples, but the present disclosure is not limited to the following examples. EXAMPLES

[0055] [Samples No. 1-4] <Preparation of coated tools> First, a substrate was prepared. Specifically, 6% by mass of metal cobalt powder having an average particle size of 1.2 μm, 0.5% by mass of titanium carbide powder having an average particle size of 2.0 μm, 5% by mass of niobium carbide powder having an average particle size of 2.0 μm, and the remainder of the mixture was mixed and pressed to form a cutting tool shape (CNMG120408) to obtain a molded body. The obtained molded body was subjected to a binder removal treatment and sintered in a vacuum or a non-oxidizing atmosphere to produce a substrate made of cemented carbide. Thereafter, the substrate was brushed, and the portion to be the cutting edge was subjected to R-honing. The average particle size of the WC particles contained in the substrate was measured by the above-mentioned image analysis, and was found to be 1.0 μm.

[0056] Next, a coating layer was formed on the obtained substrate by a CVD method. A reaction gas having the composition shown in Table 1 was used for the film formation. The coating layer was formed under the film formation conditions shown in Table 2. In Tables 1 and 2, each compound is represented by its chemical symbol. The numbers in parentheses in Table 2 indicate the thickness of each layer. The thickness of the coating layer shown in Table 2 is the value obtained by cross-sectional measurement using an SEM. Samples No. 1 to 4 were subjected to different pretreatment times. The pretreatment time for sample No. 1 was 0 minutes. In other words, sample No. 1 was not subjected to pretreatment.

[0057] <Evaluation> (Measuring the average KAM value in the first area) The KAM was measured by EBSD for the first region of the obtained coated tool as follows. The cross section of the coated tool was buffed using colloidal silica, and then the measurement area was divided into square regions (pixels) using an Oxford EBSD (model number JSM7000F). For each divided region, a Kikuchi pattern was obtained from the reflected electrons of an electron beam incident on the sample surface, and the pixel orientation was measured. The measured orientation data was analyzed using the system's analysis software, and various parameters were calculated.

[0058] The observation conditions were an acceleration voltage of 15 kV, a measurement area of ​​50 μm wide x 2 μm deep on the surface of the cemented carbide substrate, and a distance (step size) between adjacent pixels of 0.1 μm. An orientation difference of 5° or more between adjacent pixels was considered to be a grain boundary. KAM was calculated by averaging the orientation difference between a pixel within a grain and an adjacent pixel that does not cross the grain boundary, and the average KAM value was measured as the average value for all pixels constituting the entire measurement area. The average KAM value was measured for three arbitrary fields of view in the first region, and the average was used for evaluation. The results are shown in Table 3.

[0059] (Measurement of the amount of carbon 1 to 3) The amounts of the first to third carbons were measured by AES analysis, and the ratio (amount of the first carbon / amount of the second carbon) and the ratio (amount of the third carbon / amount of the second carbon) were calculated. The AES analysis conditions are shown below, and the results are shown in Table 3. Equipment: PHI "Model 680" Accelerating voltage: 10 kV Specimen current: 10nA Electron probe diameter: 0.1 μm or less

[0060] (Cutting test) The coated tools thus obtained were used in an intermittent cutting test to evaluate their fracture resistance. The intermittent cutting conditions are shown below, and the results are shown in Table 3. Workpiece: General structural rolled steel, 8 grooved steel (SS400) Tool shape: CNMG120408 Cutting speed: 300m / min Feed rate: 0.30mm / rev Cutting depth: 1.0mm Other: Water-soluble cutting fluid used Evaluation item: Measure the number of impacts that lead to breakage

[0061] [Table 1]

[0062] [Table 2]

[0063] [Table 3]

[0064] As shown in Table 3, the pretreated samples Nos. 2 to 4 had a longer life than sample No. 1. The measurement results showed that the first carbon amount in samples Nos. 2 to 4 was greater than the second carbon amount, and the average KAM value of the first region was less than 0.4°. [Explanation of symbols]

[0065] 1. Coated tools (cutting tools) 2...Front page 3...Second side 4. Cutting edge 5...Base 6...Covering layer 7...1st layer 8...1st area 9...Second area 10...1st part 11...Second part 12...3rd part 13...4th part 14...2nd layer 15...Third layer 16...4th layer

Claims

1. A substrate made of a cemented carbide; a coating layer located on a surface of the substrate; The coating layer has a first layer in contact with the substrate, The first layer is Ti(C x N 1-x ) (0≦x≦1), the substrate contains a plurality of WC grains; A region having a depth of 5 μm from the surface of the substrate is defined as a first region, A region having a depth of 100 μm or more and 200 μm or less from the surface of the substrate is defined as a second region, a maximum carbon amount (atomic %) in the first region measured by Auger electron spectroscopy under conditions of an acceleration voltage of 10 kV, a sample current of 10 nA, and an electron probe diameter of 0.1 μm or less is defined as a first carbon amount, and a maximum carbon amount (atomic %) in the second region is defined as a second carbon amount; The distance (step size) between adjacent pixels is 0.1 μm, and the orientation difference between adjacent pixels is 5° or more, and the WC grains are measured by an electron backscatter diffraction (EBSD) method using a scanning electron microscope equipped with an electron backscatter diffraction image system under the conditions that the grain boundary is considered to exist. The KAM value is: the first carbon amount is greater than the second carbon amount; The coated tool, wherein the average KAM value of the first region is less than 0.4°.

2. 2. The coated tool according to claim 1, wherein the first carbon amount is at least 1.10 times and less than 1.40 times the second carbon amount.

3. The coated tool according to claim 1 or 2, wherein the average KAM value is less than 0.3°.

4. The first layer has a thickness of 1 μm or more, an orientation of crystal grains in a region of the first layer ranging from the surface of the substrate to a depth of 0.3 μm; The coated tool according to any one of claims 1 to 3, wherein the orientation of crystal grains at the center in the thickness direction of the first layer is different from that at the center in the thickness direction of the first layer.

Citation Information

Patent Citations

  • Surface-coated cutting tool provided with hard coated layer demonstrating superior chipping resistance

    JP2011152602A

  • Surface-coated cemented carbide cutting tool

    JP2014184521A

  • Coated cutting tool

    JP2019195872A

  • Member coated with hard film, process for producing same, and bit-exchangeable rotary tool equipped therewith

    WO2012133461A1

  • Hard film coating tool and method for manufacturing said tool

    WO2014054591A1