Positive electrode active material precursor and method for producing same

A novel positive electrode active material precursor with a nickel-cobalt-manganese structure addresses thermal and structural instability issues in lithium nickel-based oxides, enhancing battery performance for energy storage applications.

JP7566402B2Active Publication Date: 2024-10-15LG CHEM LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023501527
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-24
Filing Date
2021-07-26
Publication Date
2024-10-15
Estimated Expiration
2041-07-26

AI Technical Summary

Technical Problem

Existing lithium nickel-based oxides used in positive electrode active materials for secondary batteries suffer from poor thermal stability and structural instability due to high nickel content, leading to potential battery explosions and reduced long-term life, limiting their use in applications like electric vehicles.

Method used

A positive electrode active material precursor is developed with a novel structure comprising a nickel-cobalt-based composite metal hydroxide or oxyhydroxide core and a manganese-based metal hydroxide or oxyhydroxide layer, formed through a controlled precipitation process, ensuring non-uniform distribution of nickel, cobalt, and manganese, enhancing thermal stability and capacity characteristics.

Benefits of technology

The precursor produces a positive electrode active material with improved thermal stability, high capacity, and prolonged life, suitable for high-energy density batteries used in devices such as mobile phones, digital cameras, and electric vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566402000004
    Figure 0007566402000004
  • Figure 0007566402000005
    Figure 0007566402000005
  • Figure 0007566402000006
    Figure 0007566402000006
Patent Text Reader

Abstract

The present invention relates to a positive electrode active material precursor including a first region formed in the center of a particle of the positive electrode active material precursor and having a composition represented by Chemical Formula 1 or Chemical Formula 2, and a second region formed on top of the first region and having a composition represented by Chemical Formula 3 or Chemical Formula 4, and a method for producing the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0092347, filed on July 24, 2020, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a positive electrode active material precursor having a novel structure and a method for producing the same. [Background technology]

[0003] With the technological development and increasing demand for mobile devices and electric vehicles, the demand for secondary batteries as energy sources is rapidly increasing. Among secondary batteries, lithium secondary batteries, which have high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used.

[0004] Lithium transition metal composite oxides are used as the positive electrode active material of lithium secondary batteries, and among them, lithium cobalt composite metal oxides such as LiCoO2, which have high working voltage and excellent capacity characteristics, are mainly used. However, LiCoO2 has very poor thermal characteristics due to the instability of the crystal structure caused by delithiation. In addition, the LiCoO2 is expensive, so there is a limit to its mass use as a power source in fields such as electric vehicles.

[0005] Therefore, lithium manganese oxides (LiMnO2 or LiMn2O4, etc.), lithium iron phosphate compounds (LiFePO4, etc.), or lithium nickel oxides (LiNiO2, etc.) have been developed as materials to be used instead of LiCoO2. Among them, research and development of lithium nickel oxides, which have a high reversible capacity of about 200 mAh / g and can easily realize large-capacity batteries, has been actively carried out. However, LiNiO2 has inferior thermal stability compared to LiCoO2, and if an internal short circuit occurs due to external pressure in a charged state, the positive electrode active material itself decomposes, causing the battery to explode and catch fire. Therefore, as a method for improving the low thermal stability while maintaining the excellent reversible capacity of LiNiO2, lithium composite transition metal oxides in which part of the nickel is replaced with cobalt, manganese and / or aluminum have been developed.

[0006] Meanwhile, in response to the recent increase in demand for secondary batteries with high energy density, high-nickel-lithium composite transition metal oxides with a high nickel content have been developed to increase the capacity of the positive electrode active material. High-nickel-lithium composite transition metal oxides have the advantage of exhibiting high capacity, but the high nickel content increases the amount of nickel oxidation at the same voltage range, resulting in an increase in the amount of lithium ion migration, which reduces the structural stability of the positive electrode active material and reduces the long-term life and thermal stability.

[0007] Therefore, there is a demand for the development of a positive electrode active material that has high capacity characteristics as well as excellent physical properties such as life characteristics and thermal stability. Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made to solve the above-mentioned problems, and has an object to provide a positive electrode active material precursor having a novel structure capable of realizing excellent capacity characteristics, and a method for producing the same. [Means for solving the problem]

[0009] The present invention provides a positive electrode active material precursor, comprising: a first region formed in a center of a particle of the positive electrode active material precursor and having a composition represented by Chemical Formula 1 or 2 below; and a second region formed on an upper portion of the first region and having a composition represented by Chemical Formula 3 or 4 below. [Chemical formula 1] [Ni a Co b M 1 c ](OH)2 [Chemical formula 2] [Ni a Co b M 1 c ]O·OH In the above Chemical Formula 1 and Chemical Formula 2, the M 1 is one or more selected from the group consisting of B, Mg, Ca, Al, Ti, V, Cr, Fe, Zn, Ga, Y, Zr, Nb, Mo, Ta and W, and 0 <a<1、0<b<1、0≦c<0.5、a+b+c=1であり、 [Chemical formula 3] [Mn d M 2 e ](OH)2 [Chemical formula 4] [Mn d M 2 e ]O·OH In the above Chemical Formula 3 and Chemical Formula 4, the M 2 is one or more selected from the group consisting of B, Mg, Ca, Al, Ti, V, Cr, Fe, Zn, Ga, Y, Zr, Nb, Mo, Ta and W, and 0.5 <d≦1、0≦e<0.5、d+e=1である。

[0010] The present invention also provides a method for producing a cathode active material precursor according to the present invention, comprising: a first step of mixing a first metal solution containing nickel and cobalt, an ammonium cation complex former, and a basic compound to form nickel-cobalt-based composite metal hydroxide or oxyhydroxide particles by a precipitation reaction; and a second step of mixing a second metal solution containing manganese, an ammonium cation complex former, and a basic compound with the solution containing the nickel-cobalt-based composite metal hydroxide or oxyhydroxide particles to form manganese-based metal hydroxide or oxyhydroxide on top of the nickel-cobalt-based composite metal hydroxide or oxyhydroxide particles by a precipitation reaction.

[0011] The present invention also provides a positive electrode active material, which is a sintered product of the positive electrode active material precursor according to the present invention and a lithium source material. Effect of the Invention

[0012] The positive electrode active material precursor of the present invention has high capacity characteristics, in which nickel, cobalt, and manganese are not uniformly distributed in the positive electrode active material precursor, and includes a first region containing a nickel-cobalt-based composite metal hydroxide or oxyhydroxide, and a second region formed on an upper portion of the first region and containing a manganese-based metal hydroxide or oxyhydroxide.

[0013] According to the production method of the present invention, nickel and cobalt, which have similar precipitation reaction conditions, are first mixed and precipitated, and manganese, which has the most different precipitation reaction conditions, is separated and precipitated, thereby improving the reaction efficiency.

[0014] In addition, according to the manufacturing method of the present invention, the transition metal composition of a first region formed in the center of a positive electrode active material precursor particle and a second region formed on an upper portion of the first region can be easily adjusted, and a positive electrode active material precursor optimized to obtain desired physical properties can be manufactured. [Brief description of the drawings]

[0015] [Figure 1]1 is a diagram illustrating an embodiment of a positive electrode active material precursor according to the present invention; [Diagram 2] 1(a) is a scanning electron microscope (SEM) image of a particle having a Ni0.95Co0.05(OH)2 composition in Example 1, and FIG. 1(b) is an SEM image of a positive electrode active material precursor in which a second region having a Mn(OH)2 composition in Example 1 is formed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of ​​the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.

[0017] In this specification, the terms "comprise", "comprise", "have" and the like are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, but are not intended to preclude the presence or additional possibility of one or more different features, numbers, steps, components, or combinations thereof.

[0018] In this specification, D 50 and D can be defined as the particle size that corresponds to 50% of the cumulative volume in the particle size distribution curve (graph curve of particle size distribution degree). 50 can be measured by using, for example, a laser diffraction method. The laser diffraction method generally allows measurement of particle sizes from the submicron range to several mm, and can provide results with high reproducibility and high resolution.

[0019] As used herein, the term "on" is meant to include not only cases where one structure is formed immediately on top of another structure, but also cases where a third structure is interposed between the structures.

[0020] In this specification, the crystal grain size on a specific crystal plane of a positive electrode active material precursor particle is a value obtained by measuring an XRD pattern of the precursor using an X-ray diffraction analyzer (manufactured by Rikaku Corporation), obtaining a half-width at a peak on a specific crystal plane from the measured XRD pattern, and calculating the half-width at the peak using ellipsoid modelling and the Scherrer equation.

[0021] The present invention will now be described in more detail.

[0022] Positive electrode active material precursor First, the positive electrode active material precursor according to the present invention will be described.

[0023] The present invention provides a positive electrode active material precursor, comprising: a first region formed in a center of a particle of the positive electrode active material precursor and having a composition represented by Chemical Formula 1 or 2 below; and a second region formed on an upper portion of the first region and having a composition represented by Chemical Formula 3 or 4 below. [Chemical formula 1] [Ni a Co b M 1 c ](OH)2 [Chemical formula 2] [Ni a Co b M 1 c ]O·OH In the above Chemical Formula 1 and Chemical Formula 2, the M 1 is one or more selected from the group consisting of B, Mg, Ca, Al, Ti, V, Cr, Fe, Zn, Ga, Y, Zr, Nb, Mo, Ta and W, and 0 <a<1、0<b<1、0≦c<0.5、a+b+c=1であり、 [Chemical formula 3] [Mn d M 2 e ](OH)2 [Chemical formula 4] [Mn d M 2 eO·OH In Chemical Formula 3 and Chemical Formula 4, the M 2 is one or more selected from the group consisting of B, Mg, Ca, Al, Ti, V, Cr, Fe, Zn, Ga, Y, Zr, Nb, Mo, Ta, and W, and 0.5 < d ≦ 1, 0 ≦ e < 0.5, and d + e = 1.

[0024] That is, the present invention provides a positive electrode active material precursor in which a first region containing a nickel-cobalt-based composite metal hydroxide or oxyhydroxide is formed in the central portion of the particles of the positive electrode active material precursor, and a second region containing a manganese-based metal hydroxide or oxyhydroxide is formed above the first region.

[0025] FIG. 1 shows an embodiment of the positive electrode active material precursor according to the present invention. Hereinafter, the positive electrode active material precursor according to the present invention will be described with reference to the drawings.

[0026] As shown in FIG. 1, the positive electrode active material precursor according to the present invention includes a first region 10 formed in the central portion of the precursor particles and a second region 20 formed above the first region. The first region contains nickel and cobalt, and the second region contains manganese as a main component.

[0027] The positive electrode active material precursor of the present invention includes a manganese-based metal hydroxide or oxyhydroxide region containing manganese as a main component formed on the upper part of the particles, and an effect of further improving the high-temperature life characteristics can be obtained. This is because manganese has excellent thermal stability characteristics.

[0028] According to the present invention, the a, b, and c are within nickel-cobalt-based composite metal hydroxide or oxyhydroxide particles (particles having a composition represented by Chemical Formula 1 or Chemical Formula 2), and represent the molar ratios of Ni, Co, and M 1 respectively. Specifically, the a, b, and c can be 0.6 ≦ a < 1, 0 < b < 0.4, and 0 ≦ c < 0.4, and more specifically, can be 0.75 ≦ a < 1, 0 < b < 0.25, and 0 ≦ c < 0.25.

[0029] According to the present invention, said d and e represent the molar ratios of Mn and M within manganese-based composite metal hydroxide or oxyhydroxide particles (particles having a composition represented by Chemical Formula 3 or Chemical Formula 4). 2 Specifically, said d and e can satisfy 0.8 < d ≤ 1 and 0 ≤ e < 0.2, and more specifically, can satisfy 0.9 < d ≤ 1 and 0 ≤ e < 0.1.

[0030] According to the present invention, the cathode active material precursor can contain 60 mol% to 98 mol% of Ni, 1 mol% to 20 mol% of Co, and 1 mol% to 20 mol% of Mn among all transition metals. Specifically, the cathode active material precursor can contain 60 mol% to 90 mol% of Ni, 3 mol% to 20 mol% of Co, and 3 mol% to 20 mol% of Mn among all transition metals. In this case, since nickel, which is cheaper than cobalt and occupies more than half, has a high charge capacity, there are advantages such as low production cost and environmental friendliness.

[0031] According to the present invention, the average particle size (D 50 ) of the cathode active material precursor can be 3 μm to 20 μm. Specifically, the average particle size (D 50 ) of the cathode active material precursor can be 3 μm to 15 μm, and more specifically, 4 μm to 12 μm. When the average particle size of the cathode active material precursor is within the above range, the dispersibility does not decrease, and the mechanical strength and specific surface area of the cathode active material can be maintained at a certain level, improving the output characteristics.

[0032] According to the present invention, the BET specific surface area of the cathode active material precursor can be 2 m 2 / g to 20 m 2 / g. Specifically, the BET specific surface area of the cathode active material precursor can be 2 m 2 / g to 15 m 2 / g, and more specifically, 2 m 2 / g to 10 m 2The BET specific surface area can be measured using a BELSORP-mini II device manufactured by BEL Japan, and when the BET specific surface area of ​​the positive electrode active material precursor is within the above range, the capacity and life of a battery using a positive electrode active material produced from the positive electrode active material precursor can be excellent.

[0033] According to the present invention, the positive electrode active material precursor may have a tap density of 1.0 g / cc to 3.0 g / cc. The tap density of the positive electrode active material precursor may be specifically 1.5 g / cc to 2.5 g / cc, more specifically 1.5 g / cc to 2.0 g / cc. When the tap density of the positive electrode active material precursor is within the above range, a positive electrode having excellent energy density can be produced.

[0034] The tap density is the mass per volume of a powder made of particles, and means the density when the voids between the particles are filled by constant tapping or vibration. Factors that affect the tap density include particle size distribution, moisture content, particle shape, and cohesiveness. The tap density can predict the fluidity and compressibility of a material. The tap density can be measured according to ASTM D4781, and can be calculated using the formula TD=W / V (TD: tap density, W: weight of sample (g), V: volume of sample after tapping).

[0035] According to the present invention, the second region may have a thickness of 30 nm to 500 nm. Specifically, the thickness of the second region may be 30 nm to 400 nm, more specifically, 50 nm to 350 nm. The thickness of the second region is determined by dividing Mn and M 2 When the thickness of the second region is within the above range, excellent capacity and life can be achieved.

[0036] According to the present invention, the positive electrode active material precursor can satisfy the following formula 1.

[0037] [Formula 1] 3.0≦C (100) / C (001) <= 5.0

[0038] In the above formula 1, C (100) is the grain size on the (100) plane, and C (001) is the grain size on the (001) plane.

[0039] Specifically, the positive electrode active material precursor has a C (100) / C (001) ≦4.5, and more specifically, 3.0≦C (100) / C (001) In this case, the positive electrode active material precursor has a minimized (001) crystal size and a predominant (100) crystal size that can act as a lithium passage, and the calcination temperature after mixing with the lithium source material can be reduced, and a positive electrode active material having higher energy density and excellent cycle characteristics can be provided.

[0040] According to the present invention, the positive electrode active material precursor may have a crystal grain size of 35 nm to 100 nm on the (100) plane. Specifically, the crystal grain size of the positive electrode active material precursor on the (100) plane may be 35 nm to 50 nm. In this case, the size of the (100) crystals that can act as lithium passages is predominant, and a positive electrode active material having excellent cycle characteristics can be provided.

[0041] Method for producing a positive electrode active material precursor Next, a method for producing the positive electrode active material precursor according to the present invention will be described.

[0042] The method for producing a positive electrode active material precursor according to the present invention includes a first step of mixing a first metal solution containing nickel and cobalt, an ammonium cation complex-forming agent, and a basic compound, and forming nickel-cobalt-based composite metal hydroxide or oxyhydroxide particles by a precipitation reaction, and a second step of mixing a second metal solution containing manganese, an ammonium cation complex-forming agent, and a basic compound with the solution containing the nickel-cobalt-based composite metal hydroxide or oxyhydroxide particles, and forming manganese-based metal hydroxide or oxyhydroxide on top of the nickel-cobalt-based composite metal hydroxide or oxyhydroxide particles by a precipitation reaction.

[0043] The method for producing a positive electrode active material precursor according to the present invention is a method for producing a positive electrode active material precursor having a first region formed in the center of a particle of the positive electrode active material precursor and containing a nickel-cobalt-based composite metal hydroxide or oxyhydroxide, and a second region formed on an upper portion of the first region and containing a manganese-based metal hydroxide or oxyhydroxide.

[0044] Each step of the present invention will now be described in detail.

[0045] (1) First step The first metal solution containing nickel and cobalt may be prepared by dissolving a nickel-containing source material and a cobalt-containing source material in a solvent such as water.

[0046] In this case, the nickel-containing raw material may be an acetate, carbonate, nitrate, sulfate, halide, sulfide, or oxide of nickel, and the cobalt-containing raw material may be an acetate, carbonate, nitrate, sulfate, halide, sulfide, or oxide of cobalt metal.

[0047] The nickel-containing source material can be, for example, but is not limited to, NiO, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, nickel halides, or combinations thereof.

[0048] The cobalt-containing source material may be, for example, CoSO4, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, CoSO4·7H2O, or a combination thereof, but is not limited thereto.

[0049] According to the present invention, the first metal solution is 1 It may further contain a metal. 1 The metal may be one or more selected from the group consisting of B, Mg, Ca, Al, Ti, V, Cr, Fe, Zn, Ga, Y, Zr, Nb, Mo, Ta and W, and may specifically be Al.

[0050] M 1 Metal solutions that further contain metals are prepared by adding M 1 It may be prepared by dissolving a metal-containing source material together with a nickel-containing source material and a cobalt-containing source material.

[0051] At this time, the M 1 The metal-containing raw material is M 1 The M may be a metal acetate, carbonate, nitrate, sulfate, halide, sulfide, or oxide, etc. 1 The metal may be included in an amount of 10 mol % or less, for example, 0.01 mol % to 10 mol %, 0.05 mol % to 10 mol %, or 1 mol % to 5 mol %, of the total metals in the first metal solution.

[0052] Once the first metal solution is prepared, the first metal solution, the ammonium cation complexing agent, and the basic compound are mixed together to form nickel-cobalt based composite metal hydroxide or oxyhydroxide particles through a precipitation reaction.

[0053] In this case, the ammonium cation complexing agent may be at least one selected from the group consisting of NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, and (NH4)2CO3, and may be added to the reactor in the form of a solution in which the compound is dissolved in a solvent. In this case, the solvent may be water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that is uniformly miscible with water.

[0054] The basic compound may be at least one selected from the group consisting of NaOH, KOH, and Ca(OH)2, and may be added to the reactor in the form of a solution in which the basic compound is dissolved in a solvent, which may be water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that is uniformly miscible with water.

[0055] The ammonium cation complexing agent and the basic compound are added in amounts such that the pH of the reaction solution falls within the desired range.

[0056] According to the present invention, the first step is to mix a first metal solution containing nickel and cobalt, an ammonium cation complexing agent and a basic compound, form nickel-cobalt composite metal hydroxide or oxyhydroxide particle nuclei by precipitation reaction at pH 11.5 to pH 12.5, specifically pH 11.8 to pH 12.3, and then form nickel-cobalt composite metal hydroxide or oxyhydroxide particles by precipitation reaction at pH 11.0 to pH 12.0, specifically pH 11.2 to pH 11.6. Meanwhile, the pH condition of the particle forming step can be lower than that of the particle nuclei forming step. When the precipitation reaction is carried out under the above pH ranges during the nucleation and particle formation, there is an advantageous effect on the nucleation and precursor growth (particle formation). Specifically, when the pH range is adjusted within the above range, particle growth by oriented attachment rather than by Ostwald ripening acts as the main mechanism, and a precursor grown in the preferred crystal direction ((100) or (101) direction) can be obtained. On the other hand, when the size of the (001) crystal is minimized and the sizes of the (100) and (101) crystals that can act as lithium passages predominate, the temperature of the subsequent calcination can be reduced, and furthermore, a cathode active material with higher energy density and excellent cycle characteristics can be provided.

[0057] That is, in the case of the positive electrode active material precursor produced by the method of the present invention, the growth of (001) crystals is suppressed, and the formation of (100) crystal size is relatively dominant, thereby satisfying the above-mentioned formula 1.

[0058] (2) Second step When nickel-cobalt-based composite metal hydroxide or oxyhydroxide particles are sufficiently formed in the first step, the supply of the first metal solution is interrupted, and a second metal solution containing manganese, an ammonium cation complex forming agent and a basic compound are added and mixed into the solution containing the nickel-cobalt-based composite metal hydroxide or oxyhydroxide particles, and a second region having a manganese-based metal hydroxide or oxyhydroxide composition is formed on the nickel-cobalt-based composite metal hydroxide or oxyhydroxide particles by a precipitation reaction.

[0059] The manganese-containing second metal solution may be prepared by dissolving a manganese-containing raw material in a solvent such as water.

[0060] In this case, the manganese-containing raw material may be manganese acetate, carbonate, nitrate, sulfate, halide, sulfide, or oxide.

[0061] The manganese-containing source material may be, for example, but is not limited to, Mn2O3, MnO2, Mn3O4, MnCO3, Mn(NO3)2, MnSO4, manganese acetate, manganese halide, or a combination thereof.

[0062] According to the present invention, the second metal solution is 2 It may further contain a metal. 2 The metal may be one or more selected from the group consisting of B, Mg, Ca, Al, Ti, V, Cr, Fe, Zn, Ga, Y, Zr, Nb, Mo, Ta and W, and may specifically be Al.

[0063] M 2 Metal solutions that further contain metals are prepared by adding M 2 It may be prepared by dissolving a metal-containing source material together with a nickel-containing source material and a cobalt-containing source material.

[0064] At this time, the M 2 The metal-containing raw material is M 2The M may be a metal acetate, carbonate, nitrate, sulfate, halide, sulfide, or oxide, etc. 2 The metal may be included in an amount of 10 mol % or less, for example, 0.01 mol % to 10 mol %, 0.05 mol % to 10 mol %, or 1 mol % to 5 mol %, of the total metals in the second metal solution.

[0065] The ammonium cation complexing agent and the basic compound may be the same as those described above, and the ammonium cation complexing agent and the basic compound are added in amounts that allow the pH of the reaction solution to fall within a desired range.

[0066] According to the present invention, the second step may be carried out at pH 10.5 to pH 11.5. Specifically, the second step may be carried out at pH 10.7 to pH 11.2. When the pH is adjusted within the above range, there is an advantageous effect in terms of controlling the precipitation reaction and the derivative of the second step.

[0067] By the above-mentioned method, it is possible to prepare a novel cathode active material precursor of the present invention having a structure including nickel-cobalt-based composite metal hydroxide or oxyhydroxide particles and a second region having a manganese-based metal hydroxide or oxyhydroxide composition formed on the upper part of the particles.

[0068] positive electrode active material Next, the positive electrode active material according to the present invention will be described.

[0069] The positive electrode active material according to the present invention is a product obtained by sintering the positive electrode active material precursor according to the present invention and a lithium source material.

[0070] The positive electrode active material can be prepared by mixing the positive electrode active material precursor of the present invention with a lithium source material and then calcining the mixture.

[0071] Examples of the lithium source material include lithium-containing carbonates (e.g., lithium carbonate, etc.), hydrates (e.g., lithium hydroxide hydrate (LiOH·H2O), etc.), hydroxides (e.g., lithium hydroxide, etc.), nitrates (e.g., lithium nitrate (LiNO3), etc.), chlorides (e.g., lithium chloride (LiCl), etc.), and any one of these may be used alone or in combination of two or more.

[0072] Meanwhile, the positive electrode active material precursor and the lithium source material may be mixed by solid-phase mixing, and the mixing ratio of the positive electrode active material precursor and the lithium source material may be determined to be within a range that satisfies the atomic fraction of each component in the finally prepared positive electrode active material. For example, the positive electrode active material precursor and the lithium source material may be mixed in an amount such that the molar ratio of transition metal:Li is 1:0.9 to 1:1.2, specifically 1:0.98 to 1:1.1. When the precursor and the lithium source material are mixed within the above range, a positive electrode active material exhibiting excellent capacity characteristics may be prepared.

[0073] The firing may be performed at 600°C to 1000°C, specifically 700°C to 900°C, and the firing time may be 5 hours to 30 hours, specifically 8 hours to 15 hours, but is not limited thereto.

[0074] positive electrode Next, a positive electrode containing the above-mentioned positive electrode active material of the present invention will be described.

[0075] The positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, and the positive electrode active material layer includes the positive electrode active material according to the present invention.

[0076] Since the positive electrode active material has been described above, a detailed description thereof will be omitted, and only the remaining components will be described in detail below.

[0077] The positive electrode current collector may contain a metal having high conductivity, and is not particularly limited as long as the positive electrode active material layer is easily attached and is non-reactive in the voltage range of the battery. The positive electrode current collector may be, for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. In addition, the positive electrode current collector may usually have a thickness of 3 μm to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the adhesive force of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0078] The positive electrode active material layer may optionally contain a conductive material and a binder, in addition to the positive electrode active material, as necessary.

[0079] In this case, the positive electrode active material may be included in an amount of 80 wt% to 99 wt%, more specifically, 85 wt% to 98.5 wt%, based on the total weight of the positive electrode active material layer, and excellent capacity characteristics may be exhibited when included in the above content range.

[0080] The conductive material is used to give the electrode conductivity, and can be used without any particular limitation as long as it does not cause a chemical change in the battery and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive tubes such as carbon nanotubes; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and one or more of these can be used alone or in combination. The conductive material can be contained in an amount of 0.1 to 15% by weight based on the total weight of the positive electrode active material layer.

[0081] The binder serves to improve adhesion between the positive electrode active material particles and adhesion between the positive electrode active material and the current collector.Specific examples of the binder include polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, polymethyl methacrylate, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, polymers in which hydrogen is replaced by Li, Na, or Ca, or various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be contained in an amount of 0.1 to 15% by weight based on the total weight of the positive electrode active material layer.

[0082] The positive electrode can be manufactured by a normal method for manufacturing a positive electrode, except for using the positive electrode active material. Specifically, the positive electrode can be manufactured by applying a composition for forming a positive electrode active material layer, which is prepared by dissolving or dispersing the positive electrode active material and, if necessary, a binder, a conductive material, and a dispersant selectively in a solvent, onto a positive electrode current collector, followed by drying and rolling.

[0083] The solvent may be a solvent commonly used in the art, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), dimethyl formamide (DMF), acetone, water, etc., and one or more of these may be used alone or in combination. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, binder, and dispersant in consideration of the coating thickness of the slurry and the manufacturing yield, and to have a viscosity that can show excellent thickness uniformity when applied to manufacture a positive electrode.

[0084] As another method, the positive electrode can also be produced by casting the composition for forming a positive electrode active material layer on another support, peeling the composition from the support, and laminating the resulting film on a positive electrode current collector.

[0085] Electrochemical Devices Next, an electrochemical device including the above-mentioned positive electrode will be described.

[0086] The electrochemical device may be, specifically, a battery, a capacitor, or the like, and more specifically, a lithium secondary battery.

[0087] Specifically, the lithium secondary battery includes a positive electrode, a negative electrode facing the positive electrode, and a separator and an electrolyte interposed between the positive electrode and the negative electrode. Since the positive electrode is as described above, a detailed description thereof will be omitted, and only the remaining components will be described in detail below.

[0088] Also, the lithium secondary battery may optionally further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0089] In the lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0090] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may have a thickness of typically 3 μm to 500 μm, and like the positive electrode current collector, the surface of the current collector may be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, or nonwoven fabric.

[0091] The negative electrode active material layer includes a negative electrode active material and, optionally, a binder and a conductive material.

[0092] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β(0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. Also, a thin film of metallic lithium may be used as the negative electrode active material. Also, the carbon material may be either low crystalline carbon or high crystalline carbon. Representative examples of low crystalline carbon include soft carbon and hard carbon, and representative examples of high crystalline carbon include amorphous, plate-like, flake-like, spherical or fibrous natural or artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes.

[0093] The negative electrode active material may be included in an amount of 80% by weight to 99% by weight based on the total weight of the negative electrode active material layer.

[0094] The binder is a component that facilitates bonding between the conductive material, the active material, and the current collector, and is usually added in an amount of 0.1% by weight to 10% by weight based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.

[0095] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10% by weight or less, specifically 5% by weight or less, based on the total weight of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of such conductive materials include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0096] The negative electrode active material layer can be produced by applying a composition for forming a negative electrode active material layer, which is prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent, onto a negative electrode current collector and drying the composition. Alternatively, the negative electrode active material layer can be produced by casting the composition for forming a negative electrode active material layer onto a separate support, peeling it off from the support, and laminating the resulting film onto the negative electrode current collector.

[0097] For example, the negative electrode active material layer may be prepared by coating a composition for forming a negative electrode active material layer, which is prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent, on a negative electrode current collector and drying the composition; or by casting the composition for forming a negative electrode active material layer on a separate support, peeling the composition from the support, and laminating the resulting film on the negative electrode current collector.

[0098] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent electrolyte moisture-absorbing ability is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high-melting point glass fiber, a polyethylene terephthalate fiber, etc. can be used. In addition, a coated separator containing a ceramic component or a polymeric material can be used to ensure heat resistance or mechanical strength, and can be selectively used in a single-layer or multi-layer structure.

[0099] Examples of the electrolyte include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.

[0100] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0101] The organic solvent can be used without any particular limitation as long as it can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, ε-caprolactone, etc.; an ether solvent such as dibutyl ether or tetrahydrofuran, etc.; a ketone solvent such as cyclohexanone, etc.; an aromatic hydrocarbon solvent such as benzene or fluorobenzene, etc.; dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), propylene carbonate (propylene carbonate), etc. Examples of the solvents that can be used include carbonate-based solvents such as ethylene carbonate (PC), alcohol-based solvents such as ethanol and isopropyl alcohol, nitriles such as R-CN (R is a straight-chain, branched or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can enhance the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is more preferred. In this case, the cyclic carbonate and the linear carbonate are mixed in a volume ratio of about 1:1 to about 1:9 to provide an excellent electrolyte performance.

[0102] The lithium salt can be used without any particular limitation as long as it is a compound that can provide lithium ions used in lithium secondary batteries. Specifically, the anion of the lithium salt is F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - The lithium salt may be at least one selected from the group consisting of: LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The lithium salt is preferably used at a concentration within the range of 0.1M to 2.0M. When the lithium salt concentration is within the above range, the electrolyte has appropriate conductivity and viscosity, and therefore excellent electrolyte performance can be exhibited, and lithium ions can be effectively transferred.

[0103] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazole lisinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing the decrease in battery capacity, improving the discharge capacity of the battery, etc. In this case, the additives may be contained in an amount of 0.1 to 5 wt % based on the total weight of the electrolyte.

[0104] As described above, the lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics and life characteristics, and is therefore useful in portable devices such as mobile phones, notebook computers and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0105] As a result, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same can be provided.

[0106] The battery module or battery pack may be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0107] The shape of the lithium secondary battery is not particularly limited, but may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.

[0108] The lithium secondary battery can be used not only as a battery cell used as a power source for a small device, but also as a unit battery in a medium- to large-sized battery module including a large number of battery cells.

[0109] Examples of the medium to large devices include, but are not limited to, electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems.

[0110] The present invention will now be described in more detail with reference to specific examples.

[0111] Examples and Comparative Examples Example 1 NiSO4 and CoSO4 were added to distilled water in amounts such that the nickel:cobalt molar ratio was 95:5 to prepare a first metal solution with a concentration of 2.4 M. MnSO4 was added to distilled water to prepare a second metal solution with a concentration of 2.4 M. In addition, an 8.0 M NaOH solution and a 5.1 M NH4OH solution were prepared.

[0112] 13 L of deionized water, 0.013 L of the NaOH aqueous solution, and 0.64 L of the NHOH aqueous solution were charged into a batch reactor equipped with a filter and a pump set at 50° C., and then nitrogen gas was purged into the reactor to remove dissolved oxygen in the water and create a non-oxidizing atmosphere inside the reactor.

[0113] The first metal solution was added at a rate of 3.8 L / hr, the NaOH aqueous solution at a rate of 2.3 L / hr, and the NH4OH aqueous solution at a rate of 0.54 L / hr, while stirring at a rate of 900 rpm, and a precipitation reaction was carried out for 10 minutes at pH 11.9 to form nickel-cobalt composite metal hydroxide particle nuclei. Next, the stirring speed was gradually decreased, NaOH was added using a pH sensor to adjust the pH of the reaction solution to pH 11.2 to pH 11.6, and then the first metal solution was added at a rate of 3.8 L / hr, the NaOH aqueous solution at a rate of 2.3 L / hr, and the NH4OH aqueous solution at a rate of 0.54 L / hr, while a precipitation reaction was carried out for 48 hours to form Ni0.95 Co 0.05 Particles were produced having the composition (OH)2.

[0114] Next, the supply of the first metal solution was stopped, and NaOH was supplied in a pH sensor-linked manner to adjust the pH of the reaction solution to pH 10.7 to pH 11.2. The second metal solution was then supplied at a rate of 3.8 L / hr, the NaOH aqueous solution at a rate of 2.3 L / hr, and the NH4OH aqueous solution at a rate of 0.54 L / hr, while stirring at a rate of 150 rpm, and the precipitation reaction was carried out for 4 hours. 0.95 Co 0.05 A positive electrode active material precursor was prepared in which a second region having a Mn(OH)2 composition was formed on top of a first region having a (OH)2 composition.

[0115] In this case, Ni was 88 mol %, Co was 5 mol %, and Mn was 7 mol % of the total transition metals, the thickness of the second region was 120 nm, and the average particle size (D 50 ) is 10μm, and the BET specific surface area is 9.48m 2 The viscosity was 1.08 g / g and the tap density was 1.89 g / cc.

[0116] Example 2 NiSO4 and CoSO4 were added to distilled water in amounts such that the molar ratio of nickel:cobalt was 75:25 to prepare a first metal solution with a concentration of 2.4 M. The second metal solution was added at a rate of 3.8 L / hr, the NaOH aqueous solution at 2.3 L / hr, and the NH4OH aqueous solution at 0.54 L / hr, while stirring at a speed of 150 rpm for 10 hours to cause a precipitation reaction. 0.75 Co 0.25 The precursor was prepared in the same manner as in Example 1, except that a cathode active material precursor was prepared in which a second region having a Mn(OH)2 composition was formed on top of a first region having a (OH)2 composition. In this case, Ni was 60 mol%, Co was 20 mol%, and Mn was 20 mol% of the total transition metals, the thickness of the second region was 350 nm, and the average particle size (D 50 ) was 10 μm.

[0117] Example 3 NiSO4 and CoSO4 were added to distilled water in amounts such that the nickel:cobalt molar ratio was 94:6 to prepare a first metal solution with a concentration of 2.4 M. MnSO4 was added to distilled water to prepare a second metal solution with a concentration of 2.4 M. In addition, an 8.0 M NaOH solution and a 5.1 M NH4OH solution were prepared.

[0118] 13 L of deionized water, 0.066 L of the NaOH aqueous solution, and 0.51 L of the NHOH aqueous solution were charged into a batch reactor equipped with a filter and a pump set at 50° C., and then nitrogen gas was purged into the reactor to remove dissolved oxygen in the water and create a non-oxidizing atmosphere inside the reactor.

[0119] The first metal solution was added at a rate of 3.8 L / hr, the NaOH aqueous solution at a rate of 2.3 L / hr, and the NH4OH aqueous solution at a rate of 0.54 L / hr, while stirring at a speed of 900 rpm, and a precipitation reaction was carried out for 10 minutes at pH 12.2 to form nickel-cobalt composite metal hydroxide particle nuclei. Next, the stirring speed was gradually decreased, NaOH was added using a pH sensor to adjust the pH of the reaction solution to pH 11.4 to pH 11.8, and then the first metal solution was added at a rate of 3.8 L / hr, the NaOH aqueous solution at a rate of 2.3 L / hr, and the NH4OH aqueous solution at a rate of 0.54 L / hr, while a precipitation reaction was carried out for 21 hours, and Ni 0.94 Co 0.06 Particles were produced having the composition (OH)2.

[0120] Next, the addition of the first metal solution was stopped, and NaOH was added using a pH sensor to adjust the pH of the reaction solution to pH 10.7 to pH 11.2. The second metal solution was added at a rate of 3.8 L / hr, the NaOH aqueous solution at a rate of 2.3 L / hr, and the NH4OH aqueous solution at a rate of 0.54 L / hr, while stirring at a rate of 150 rpm, and the precipitation reaction was carried out for 3 hours. The Ni 0.94 Co 0.06A positive electrode active material precursor was prepared in which a second region having a Mn(OH)2 composition was formed on top of a first region having a (OH)2 composition.

[0121] In this case, Ni was 83 mol %, Co was 5 mol %, and Mn was 12 mol % of the total transition metals, the thickness of the second region was 100 nm, and the average particle size (D 50 ) is 4.8μm, and the BET specific surface area is 2.50m 2 / g and tap density was 1.64 g / cc.

[0122] Comparative Example 1 NiSO4, CoSO4, and MnSO4 were mixed in distilled water in amounts such that the molar ratio of nickel:cobalt:manganese was 88:5:7 to prepare a metal solution with a concentration of 2.4 M. In addition, an 8.0 M NaOH solution and a 5.1 M NH4OH solution were prepared.

[0123] 13 L of deionized water, 0.013 L of the NaOH aqueous solution, and 0.64 L of the NHOH aqueous solution were charged into a batch reactor equipped with a filter and a pump set at 50° C., and then nitrogen gas was purged into the reactor to remove dissolved oxygen in the water and create a non-oxidizing atmosphere inside the reactor.

[0124] The metal solution was added at a rate of 3.8 L / hr, the NaOH aqueous solution at a rate of 2.3 L / hr, and the NH4OH aqueous solution at a rate of 0.54 L / hr, while stirring at a speed of 900 rpm, and a precipitation reaction was carried out for 10 minutes at pH 11.9 to form nickel manganese cobalt composite metal hydroxide particle nuclei. Next, the stirring speed was gradually decreased, NaOH was added using a pH sensor to adjust the pH of the reaction solution to pH 11.2 to pH 11.6, and then the metal solution was added at a rate of 3.8 L / hr, the NaOH aqueous solution at a rate of 2.3 L / hr, and the NH4OH aqueous solution at a rate of 0.54 L / hr, while a precipitation reaction was carried out for 48 hours, and Ni 0.88 Co 0.05 Mn 0.07 A positive electrode active material precursor having an (OH)2 composition (a uniform composition throughout the positive electrode active material precursor) was prepared.

[0125] At this time, among the total transition metals, Ni is 88 mol%, Co is 5 mol%, and Mn is 7 mol%. The average particle size (D 50 ) is 10 μm, the BET specific surface area is 5.17 m 2 / g, and the tap density is 1.98 g / cc.

[0126] Experimental Example Experimental Example 1: Precursor Analysis <SEM / EDS Analysis> In Example 1, the SEM image of the particles having the Ni 0.95 Co 0.05 (OH)2 composition was measured and shown in Fig. 2(a), and the SEM image of the positive electrode active material precursor in which the second region having the Mn(OH)2 composition was formed is shown in Fig. 2(b).

[0127] In addition, in order to confirm the metal element distribution inside and on the surface of the positive electrode active material precursors of Examples 1, 2, and Comparative Example 1, SEM / EDS analysis was performed, and the results are shown in Table 1 below.

[0128] [Table 1]

[0129] Referring to Fig. 2, it can be confirmed that the positive electrode active material precursor according to the present invention includes a second region having a Mn(OH)2 composition formed on particles (first region) having a Ni 0.95 Co 0.05 (OH)2 composition.

[0130] Referring to Table 1, it can be seen that for the precursors of Examples 1 and 2 which are the positive electrode active material precursors according to the present invention, Mn is distributed only on the particle surface, while for the precursor of Comparative Example 1, Mn is included not only inside the particles but also in the same composition as the surface.

[0131] <XRD Analysis> The crystal grain sizes of the positive electrode active material precursor particles produced in Examples 1, 3, and Comparative Example 1 were obtained by the following method.

[0132] Specifically, the XRD pattern of the precursor was measured using an X-ray diffraction analyzer (Rikaku). After obtaining the half-width of the peak for each crystal plane from the measured XRD pattern, the crystal grain size (C (100) ) and the grain size on the (001) plane (C (001) ) was calculated using the Scherrer formula, and C (100) , C (001) , C (100) / C (001) The values ​​are shown in Table 2 below.

[0133] [Table 2]

[0134] As shown in Table 2, the positive electrode active material precursors prepared in Examples 1 and 3 were found to have more (100) crystal faces than the positive electrode active material precursor prepared in Comparative Example 1.

[0135] Experimental Example 2: Evaluation of Battery Performance The positive electrode active material precursor of Example 1 and LiOH·H2O were mixed so that the molar ratio of Li:transition metal was 1.05:1, and calcined at 805°C for 13 hours in an oxygen atmosphere to produce a positive electrode active material from the positive electrode active material precursor of Example 1.

[0136] A positive electrode active material was produced from the positive electrode active material precursor of Comparative Example 1 in the same manner as described above, except that the firing temperature was 765°C.

[0137] The positive electrode active materials, conductive material (carbon black), and binder (PVdF) prepared as above were mixed in a weight ratio of 97.5:1:1.5 in N-methyl-2-pyrrolidone (NMP) solvent to prepare positive electrode slurry. The positive electrode slurry was applied to one side of an aluminum current collector, dried at 130°C, and rolled to a porosity of 24% to prepare positive electrodes.

[0138] A 2032-standard coin cell type lithium secondary battery was manufactured using each of the manufactured positive electrodes, and the performance of each lithium secondary battery was evaluated. In this case, a lithium metal disk was used as the negative electrode, and a separator was interposed between the positive electrode and the negative electrode to manufacture an electrode assembly, which was then placed inside a battery case, and an electrolyte was injected into the case to manufacture a lithium secondary battery. In this case, the electrolyte used was an organic solvent in which ethylene carbonate: ethyl methyl carbonate: diethyl carbonate were mixed in a volume ratio of 3: 3: 4, and 1M LiPF6 was dissolved therein.

[0139] Each of the prepared lithium secondary batteries was charged in CC / CV mode at a constant current of 0.1C at 25°C up to 4.25V (CV 0.05C) and then discharged in CC mode up to 3V to measure the initial charge capacity and discharge capacity. The results are shown in Table 3 below.

[0140] [Table 3]

[0141] Referring to Table 3, it can be seen that the lithium secondary battery including the positive electrode active material prepared from the positive electrode active material precursor according to the present invention has improved charge capacity and discharge capacity. [Explanation of symbols]

[0142] 10 First area 20 Second area

Claims

1. A first region formed in the center of a particle of a positive electrode active material precursor and having a composition represented by the following Chemical Formula 1 or the following Chemical Formula 2; a second region formed on the first region and having a composition represented by the following Formula 3 or Formula 4: The positive electrode active material precursor satisfies the following formula 1: [Chemical formula 1] [Ni a Co b M 1 c ](OH) 2 [Chemical formula 2] [Ni a Co b M 1 c ]O.H.O. In the above Chemical Formula 1 and Chemical Formula 2, M 1 is one or more selected from the group consisting of B, Mg, Ca, Al, Ti, V, Cr, Fe, Zn, Ga, Y, Zr, Nb, Mo, Ta, and W, 0<a<1, 0<b<1, 0≦c<0.5, a+b+c=1, [Chemical formula 3] [Mn d M 2 e ](OH) 2 [Chemical formula 4] [Mn d M 2 e ]O.H.O. In the above Chemical Formula 3 and Chemical Formula 4, M 2 is one or more selected from the group consisting of B, Mg, Ca, Al, Ti, V, Cr, Fe, Zn, Ga, Y, Zr, Nb, Mo, Ta, and W, 0.5<d≦1, 0≦e<0.5, and d+e=1; [Formula 1] 3.0≦C (100) / C (001) ≦5.0 In the above formula 1, C (100) is the size of a crystal grain on the (100) plane, and C (001) is the size of a crystal grain on the (001) plane.

2. In the formulas 1 and 2, 0.6≦a<1, 0<b<0.4, and 0≦c<0.4; 2. The positive electrode active material precursor according to claim 1, wherein in Chemical Formula 3 and Chemical Formula 4, 0.8<d≦1 and 0≦e<0.

2.

3. In the formulas 1 and 2, 0.75≦a<1, 0<b<0.25, and 0≦c<0.25; 3. The positive electrode active material precursor according to claim 1, wherein in Chemical Formula 3 and Chemical Formula 4, 0.9<d≦1 and 0≦e<0.

1.

4. 4. The positive electrode active material precursor according to claim 1, wherein the positive electrode active material precursor contains, among all transition metals, 60 mol % to 98 mol % of Ni, 1 mol % to 20 mol % of Co, and 1 mol % to 20 mol % of Mn.

5. The positive electrode active material precursor has an average particle size (D 50 5. The positive electrode active material precursor according to claim 1, wherein the average particle diameter is 3 μm to 20 μm.

6. 6. The positive electrode active material precursor according to claim 1, wherein the second region has a thickness of 30 nm to 500 nm.

7. The positive electrode active material precursor has a BET specific surface area of ​​2 m 2 / g to 20m 2 The positive electrode active material precursor according to claim 1 , wherein the molecular weight of the positive electrode active material precursor is 1 / g.

8. The positive electrode active material precursor according to any one of claims 1 to 7, wherein the positive electrode active material precursor has a tap density of 1.0 g / cc to 3.0 g / cc.

9. The positive electrode active material precursor according to claim 1 , wherein the positive electrode active material precursor has a crystal grain size on a (100) plane of 35 nm or more and 100 nm or less.

10. A method for producing the positive electrode active material precursor of claim 1, comprising: A first step of mixing a first metal solution containing nickel and cobalt, an ammonium cation complexing agent and a basic compound to form nickel-cobalt based composite metal hydroxide or oxyhydroxide particles through a precipitation reaction; and a second step of mixing the solution containing the nickel-cobalt-based composite metal hydroxide or oxyhydroxide particles with a second metal solution containing manganese, an ammonium cation complex-forming agent and a basic compound to form a manganese-based metal hydroxide or oxyhydroxide on the top of the nickel-cobalt-based composite metal hydroxide or oxyhydroxide particles through a precipitation reaction.

11. 11. The method according to claim 10, wherein the first step comprises mixing a first metal solution containing nickel and cobalt, an ammonium cation complex-forming agent and a basic compound to form nickel-cobalt-based composite metal hydroxide or oxyhydroxide particle nuclei through a precipitation reaction at a pH of 11.5 to 12.5, and then growing the nickel-cobalt-based composite metal hydroxide or oxyhydroxide particles through a precipitation reaction at a pH of 11.0 to 12.

0.

12. The method according to claim 10, wherein the second step is carried out at a pH of 10.5 to 11.

5.

13. The first metal solution is M 1 Further containing a metal, Said M 1 11. The method of claim 10, wherein the metal is one or more selected from the group consisting of B, Mg, Ca, Al, Ti, V, Cr, Fe, Zn, Ga, Y, Zr, Nb, Mo, Ta and W.

14. The second metal solution is M 2 Further containing a metal, Said M 2 11. The method of claim 10, wherein the metal is one or more selected from the group consisting of B, Mg, Ca, Al, Ti, V, Cr, Fe, Zn, Ga, Y, Zr, Nb, Mo, Ta and W.

15. A positive electrode active material, which is a sintered product of the positive electrode active material precursor according to any one of claims 1 to 9 and a lithium source material.

Citation Information

Patent Citations

  • Cathode material precursor, preparation method thereof, cathode material and lithium battery

    CN102456877A

  • Li-Ni SYSTEM COMPOSITE OXIDE PARTICLE POWDER FOR NONAQUEOUS ELECTROLYTE SECONDARY BATTERY, METHOD FOR MANUFACTURING THE SAME, AND NONAQUEOUS ELECTROLYTE SECONDARY BATTERY

    JP2010114088A