Method for manufacturing hollow core fiber and method for manufacturing preform for hollow core fiber

By forming anti-resonant elements through pressure and heat deformation within the cladding tube, the method addresses the precision and reproducibility issues in manufacturing anti-resonant hollow core fibers, achieving low optical attenuation and wide transmission spectra.

JP7566793B2Active Publication Date: 2024-10-15HERAEUS QUARZGLAS GMBH & CO KG +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021571732
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-01
Filing Date
2020-07-15
Publication Date
2024-10-15
Estimated Expiration
2040-07-15

AI Technical Summary

Technical Problem

Conventional methods for manufacturing anti-resonant hollow core fibers face challenges in achieving precise and reproducible positioning of anti-resonant elements due to complex internal geometries and stringent dimensional tolerances, leading to difficulties in producing fibers with low optical attenuation and wide transmission spectra.

Method used

A method involving the formation of elongated pressure chambers within the cladding tube to deform the glass wall and create anti-resonant elements by applying pressure and heat, eliminating the need for precise positioning of prefabricated elements, and allowing for the formation of nested structural elements with controlled dimensions.

Benefits of technology

This approach enables the precise and reproducible manufacturing of anti-resonant hollow core fibers with reduced optical attenuation and wide transmission spectra, ensuring accurate positioning and structural integrity of anti-resonant elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566793000004
    Figure 0007566793000004
  • Figure 0007566793000005
    Figure 0007566793000005
  • Figure 0007566793000006
    Figure 0007566793000006
Patent Text Reader

Abstract

A method for manufacturing an anti-resonant hollow-core fiber having a hollow core extending along a longitudinal axis of the fiber and an inner cladding region including a plurality of anti-resonant elements and surrounding the hollow core is known. The known method includes the steps of providing a cladding tube having an inner bore and a longitudinal axis, the cladding tube wall extending along the longitudinal axis and defined by an inner and outer surface, forming a plurality of pre-anti-resonant elements at targeted locations on the cladding tube wall, and drawing the primary preform into a hollow-core fiber or further processing the primary preform into a secondary preform from which the hollow-core fiber is drawn. Starting from this, in order to achieve high precision and accurate positioning of the antiresonant element in a sufficiently stable and reproducible manner, it is proposed according to the present invention that the formation of the antiresonant element pre-stage comprises the creation of elongated pressure chambers, each of which is adjacent to a wall deformable by pressure and heat in the region of the target position of the antiresonant element, and that when carrying out the process according to step (c), as a result of the pressure and heat, a bulge occurs in part of the deformable wall in the direction of the inner bore of the cladding tube while forming the antiresonant element or precursor.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention provides a method for making an anti-resonant hollow-core fiber having a hollow core extending along a longitudinal axis of the fiber and a cladding region surrounding the hollow core, the cladding region including a plurality of anti-resonant elements, comprising: (a) providing a primary preform for a hollow-core fiber having at least one cladding tube, a cladding tube interior bore, a cladding tube longitudinal axis, and a cladding tube wall defined by an inner and outer side extending along the cladding tube longitudinal axis; (b) forming a plurality of precursors for anti-resonant elements at target locations on the cladding wall; (c) drawing the primary preform into a hollow-core fiber or further processing the primary preform into a secondary preform from which a hollow-core fiber is drawn; Equipped with In the further processing step, (i) Stretching; (ii) Collapse, (iii) collapsing and simultaneous stretching; (iv) Collapse of additional cladding material; (v) collapse of additional cladding material followed by stretching; (vi) collapsing and simultaneously stretching additional cladding material; One or more of the thermoforming processes are carried out once or repeatedly.

[0002] The present invention further relates to a method for making an anti-resonant hollow-core fiber preform having a hollow core extending along a longitudinal axis of the fiber and a cladding region surrounding the hollow core, the cladding region including a plurality of anti-resonant elements, the method comprising: (a) providing a primary preform for a hollow-core fiber having at least one cladding tube, a cladding tube interior bore, a cladding tube longitudinal axis, and a cladding tube wall defined by an inner and outer side extending along the cladding tube longitudinal axis; (b) forming a plurality of precursors for anti-resonant elements at target locations on the cladding wall; (c) optionally further processing the primary preform into a secondary preform for a hollow-core fiber; Equipped with In the further processing step, (i) Stretching; (ii) Collapse, (iii) collapsing and simultaneous stretching; (iv) Collapse of additional cladding material; (v) collapse of additional cladding material followed by stretching; (vi) collapsing and simultaneously stretching additional cladding material; One or more of the thermoforming processes are carried out once or repeatedly. [Background technology]

[0003] Conventional single-mode optical fibers made from solid materials have a glass core surrounded by a cladding region made of glass with a low refractive index. The propagation of light is based on total internal reflection between the core and cladding regions. However, the interaction of the guided light with the solid material is associated with increased delay times in data transmission and a relatively low damage threshold for energetic radiation.

[0004] These disadvantages are avoided or mitigated by "hollow-core fibers", whose core consists of a vacuum cavity filled with a gas or liquid. In hollow-core fibers, the interaction of light with the glass is reduced compared to solid-core fibers. Since the refractive index of the core is smaller than that of the cladding, light propagation by total internal reflection is not possible, and light is usually considered to leak from the core into the cladding. Depending on the physical mechanism of light propagation, hollow-core fibers are distinguished into "photonic bandgap fibers" and "antiresonant reflecting fibers".

[0005] In a "photonic bandgap fiber", a hollow core region is surrounded by a cladding that contains a periodic arrangement of small hollow channels. The periodic structure of the hollow channels in the cladding has an effect called "photonic bandgap" in semiconductor technology, which means that light in a certain wavelength range that scatters into the cladding structure cannot spread laterally within the cladding because it interferes constructively in the central cavity based on Bragg reflection.

[0006] In hollow-core fiber embodiments, called "antiresonant hollow-core fibers" (ARHCF), a hollow core region is surrounded by an inner cladding region and is located within so-called "antiresonant elements" (or "antiresonant elements"; abbreviation "AREs"). The walls of the antiresonant elements, evenly distributed around the hollow core, function as an antiresonantly operated Fabry-Perot cavity that can reflect incoming light and pass it through to the fiber core.

[0007] This fiber technology allows for reduced optical attenuation, a very wide transmission spectrum (even in the ultraviolet or infrared wavelength ranges), and low latency during data transmission.

[0008] Potential applications of hollow-core fibers lie in the fields of high-performance beam control for data transmission, material processing, modal filtering, and nonlinear optics, especially for generating supercontinuums from the extreme ultraviolet to the infrared wavelength range.

[0009] Prior Art A drawback of anti-resonant hollow-core fibers is that higher order modes are not automatically suppressed, so they often do not become purely single mode over long transmission distances, resulting in poor quality output beams.

[0010] Francesco Poletti, "Nested antiresonant nodeless hollow core fiber"; Optics Express, Vol. 22, No. 20 (2014); DOI: 10.1364 / OE 22.023807, proposes a fiber design in which the antiresonant element is not formed as a simple single structural element, but is composed of multiple structural elements nested within each other. The nested antiresonant elements are designed in such a way that the higher-order core modes are phase-matched to the cladding modes and suppressed, but the fundamental core mode is not suppressed. This ensures that the fundamental core mode always propagates, making the hollow core fiber effectively single-mode over a limited wavelength band.

[0011] Efficient mode suppression depends on the central wavelength of the propagating light as well as on structural parameters of the fiber design, such as the radius of the hollow core and the diameter difference of the nested ring structures within the anti-resonant element.

[0012] From EP 3136143 A1 an anti-resonant hollow-core fiber (called "hollow-core fiber without band gap") is known, whose core is capable of propagating other modes besides the fundamental mode. For this purpose, the core is surrounded by an inner cladding with "anti-resonant elements" that provide phase matching of the anti-resonant mode and higher modes. The production of hollow-core fibers is carried out by the so-called "stack and draw" method, in which a preform is formed by arranging and fixing the starting elements in an axially parallel collection, and then drawing the preform. Here, a cladding tube with a hexagonal inner cross section is used, to whose inner edge six so-called "ARE preforms" (anti-resonant element preforms) are fixed. The hollow-core fiber is formed by drawing the preform in two stages.

[0013] From International Patent Application 2018 / 169487 A1 a method for manufacturing a preform for an antiresonant hollow core fiber is known, in which a first cladding region is made up of a number of rods and a second cladding region is made up of a number of tubes surrounded by an outer cladding tube. The rods, tubes and cladding tube are joined by a "stack and draw" method to form the preform. Before the preform is drawn, sealing is performed by applying a sealant to the preform ends. As sealant a UV adhesive is used, for example. Summary of the Invention [Problem to be solved by the invention]

[0014] Anti-resonant hollow-core fibers, and especially those with nested structural elements, have complex internal geometries that make them difficult to manufacture accurately and reproducibly. This is compounded by the fact that resonance or anti-resonance conditions cannot be met without small dimensional tolerances on the magnitude of the operating wavelength of the propagating light. Deviations from the target shape can be caused during the construction of the fiber preform, but can also occur during the fiber drawing process due to inappropriate deformations that are not to scale.

[0015] In the known "stack and draw" method, a large number of elements have to be joined in precise positions. For example, to produce a hollow-core fiber of the "NANF" design known from the literature mentioned at the beginning, six anti-resonant element preforms, each consisting of an outer anti-resonant preform tube (abbreviated as "ARE outer tube") and an inner anti-resonant preform tube (abbreviated as "ARE inner tube"), which is welded on one side to the inner cladding surface of the outer ARE tube, have to be mounted inside the cladding tube.

[0016] In order to achieve low attenuation values ​​and wide propagation ranges, the azimuthal position of the anti-resonant element inside the cladding tube is also important, in addition to the uniform wall thickness of the anti-resonant element walls, which cannot be easily achieved by the "stack and draw" method. It is an object of the present invention to provide a manufacturing method for achieving anti-resonant hollow-core fibers at low cost, avoiding the limitations of conventional manufacturing methods.

[0017] In particular, it is an object of the present invention to provide a method for manufacturing anti-resonant hollow-core fibers and anti-resonant hollow-core fiber preforms, which makes it possible to achieve high precision of the structural elements and exact positioning of the anti-resonant elements within the fiber in a sufficiently stable and reproducible manner.

[0018] Furthermore, the drawbacks of the conventional "stack and draw" method, in which the required construction precision, in particular the uniform wall thickness and precise positioning of the anti-resonant elements in defined azimuthal positions, are not easily achievable, must be avoided as far as possible. [Means for solving the problem]

[0019] With regard to a method for producing an antiresonant hollow-core fiber, this problem is solved according to the invention, starting from a method of the type mentioned at the beginning, in that the formation of a pre-stage antiresonant element comprises the formation of an elongated pressure chamber, which is adjacent to a wall deformable by pressure and heat, respectively, in the target location region of the antiresonant element, and when carrying out the process according to step (c), as a result of the pressure and heat, a bulge is produced in a part of the deformable wall in the direction of the inner bore of the cladding tube while forming the antiresonant element or precursor.

[0020] The starting point for the manufacture of anti-resonant hollow-core fibers is again a preform, called the "primary preform". This preform includes a cladding tube, which contains a precursor or preform for forming an anti-resonant element in the hollow-core fiber (herein called "anti-resonant element" for short). The primary preform can be drawn to form a hollow-core fiber, but typically additional cladding material is added to the primary preform to create a preform, called here "secondary preform". If necessary, the hollow-core fiber is produced by drawing this secondary preform. Alternatively, the primary or secondary preform is surrounded by one or more outer cylinders, forming a coaxial collection of components, which is directly drawn to form the hollow-core fiber. In this case, the general term "preform" is understood as the name of the component or coaxial collection of components from which the hollow-core fiber is finally drawn.

[0021] The positioning accuracy of the anti-resonant element is improved by configuring the precursor for the anti-resonant element in the form of an elongated pressure chamber formed in the target position area of ​​the anti-resonant element, the pressure chamber being designed in such a way that the wall section of the inner cladding tube adjacent thereto softens and bulges in the direction of the cladding tube longitudinal axis when gas pressure is applied in the pressure chamber.

[0022] The elongated pressure chamber, when carrying out the process according to step (c), causes an elongated bulge in the elongated portion of the deformable wall in the direction of the cladding tube inner bore as a result of pressure and heat, forming an elongated anti-resonant element or precursor.

[0023] The corresponding bulging wall section of the deformable wall is elongated and extends into the preform along the pressure chamber and the target position of the pre-antiresonant element. In the simplest case, which will be described in detail below, the bulging wall section of the deformable wall belongs to a glass tube.

[0024] In a first preferred variant, the pressure chamber is formed inside the wall of the glass tube, forming a hollow channel which runs parallel to the longitudinal axis of the glass tube from one end of the glass tube wall to the other end and which is completely defined by the glass of the glass tube. In another preferred variant, the pressure chamber is provided by a separate component adjacent to the outer cladding surface of the deformable glass tube wall, in which case the pressure chamber forms a hollow channel which runs parallel to the longitudinal axis of the glass tube along the glass tube wall from one end to the other and is bounded on one side by the glass of the glass tube. In a further preferred variant, the pressure chamber is formed in a recess in the outer cladding surface of the glass tube wall, in which case it likewise forms a hollow channel which runs parallel to the longitudinal axis of the glass tube along the glass tube wall from one end to the other and which is bounded by the glass of the glass tube in the region of the recess.

[0025] These variants can also be combined with one another: in order to be able to introduce a pressurized gas into the hollow channel, the hollow channel is open at one end, and advantageously from a manufacturing point of view, at both ends.

[0026] The pre-antiresonant element is formed at this location during the manufacturing process by the application of pressure from outside the glass tube causing the corresponding wall section to bulge towards the inner bore of the glass tube, for example during drawing of the preform into a hollow-core fiber or semi-finished product.

[0027] This completely eliminates the need to position and fix pre-manufactured anti-resonant element preforms at the corresponding positions on the inner wall of the cladding tube, as is known in the stack and draw method, or at least reduces the number of anti-resonant element preforms that need to be so positioned.

[0028] The present invention allows for precise and reproducible manufacture of anti-resonant hollow-core fibers, as well as preforms therefor.

[0029] The pressure chamber is advantageously designed as a hollow channel which is adjoined by a deforming wall section of the glass tube.

[0030] The hollow channel forms a pressure chamber into which a pressurized gas can be introduced during the manufacturing process, so that the wall portion of the glass tube in contact with the pressurized gas is deformed by the gas pressure.

[0031] Hollow channels formed by drilling holes into the wall of a deformable glass tube In some preferred methods already mentioned above, a hollow channel is formed inside the glass tube wall, which runs parallel to the longitudinal axis of the glass tube.

[0032] The cross section of the hollow channel may be circular or polygonal, in particular triangular or rectangular. In the case of a rectangular hollow channel, the long side of the rectangle extends tangentially to the wall section that is deformed (bulging). In the case of a triangular hollow channel, one side of the triangle extends tangentially to the wall section that is deformed (bulging). This causes the gas pressure to act more strongly on this wall section than in other directions.

[0033] In this case, in particular for producing complexly formed anti-resonant element preforms with nested structural elements, a variant has proven advantageous in which a coaxial glass tube arrangement is formed comprising an inner peripheral row of hollow channels in the wall of the inner glass tube and an outer peripheral row of hollow channels in the wall of the outer glass tube, the inner and outer peripheral rows of hollow channels being on a common radial connecting line and spatially separated from one another by at least one inwardly deformable glass wall running around the periphery.

[0034] The surrounding glass wall separates the pressure spaces of the inner and outer hollow channel rows from each other and is caused to bulge inward by the outer hollow channel row during the thermoforming process. Because the surrounding glass wall belongs to the inner glass tube, the deformation of the outer glass tube can penetrate into the bulge of the inner glass tube, thereby creating an anti-resonant element preform of the nested anti-resonant element.

[0035] A hollow channel formed by a longitudinal slot in an intermediate tube wall adjacent to the deformable glass tube. A particularly sophisticated method for forming a hollow channel comprises the steps of placing an intermediate tube having an intermediate tube longitudinal axis between the glass tube and the outer tube, extending along said intermediate tube longitudinal axis an intermediate tube wall defined by an inner and outer side, in which a longitudinal slot is provided, from which the hollow channel is formed when the process according to step (c) is carried out.

[0036] The longitudinal slots pass through the wall of the intermediate tube (preferably except at both end face regions) and have parallel longitudinal edges.

[0037] The intermediate tube may be in contact with the outer wall of the glass tube and fused thereto, or in contact with the inner wall of the outer tube and fused thereto. The longitudinal slot is between the glass tube and the outer tube and is located at a position where the glass tube wall portion bulges. The longitudinal slot forms a hollow channel or a precursor to a hollow channel through which pressure can be applied to the outside of the glass tube in a later manufacturing process, so that the softened glass tube material bulges in the direction of the inner bore. The hollow channel is then deformed by pressure and heat into an elongated bulge.

[0038] An advantage of this embodiment is that the distances of the hollow channels to the inner bore are particularly uniform from one another over the length of the hollow channels.

[0039] Advantageously, during the thermoforming process according to step (c), an internal pressure is generated in the hollow channel by the introduction of a pressurized gas, which causes the glass tube wall portion in contact with the pressurized gas through the longitudinal slot to deform, resulting in a long bulge in the glass tube facing inwardly toward the glass tube inner bore and toward the hollow core, which bulge is used as an anti-resonant element preform or an anti-resonant element.

[0040] The longitudinal slots preferably terminate before the end face ends of the intermediate tube to ensure retention of the remaining longitudinal webs.

[0041] In this case, in particular for producing complexly formed anti-resonant element preforms with nested structural elements, a variant has proven advantageous in which a coaxial glass tube arrangement is formed comprising an inner glass tube, an inner intermediate tube, an inner outer tube which simultaneously forms an outer glass tube, an outer intermediate tube and an outer outer tube, the longitudinal slots of the inner and outer intermediate tubes being radially on a common connecting line and spatially separated from one another by at least one inwardly deformable glass wall circumferentially.

[0042] A coaxial tube arrangement of this type is used to form at least two hollow channels or pressure chambers arranged radially one behind the other in a pair. A circumferential glass wall separates the pressure spaces of the inner and outer hollow channel rows from each other and is bulged inwards by the outer hollow channel row during the thermoforming process. Since the circumferential glass wall belongs to the inner glass tube, deformations of the outer glass tube can be transferred to the bulging of the inner glass tube, thereby producing an antiresonant element preform for the nested antiresonant element.

[0043] Preferably, an intermediate tube is provided and machined with a circular internal cross section. The longitudinal slots are radially continuous and can be produced simply and precisely, for example by milling, drilling or notching. The internal shape of the longitudinal slots or grooves is, for example, rectangular or V-shaped.

[0044] The longitudinal slots are preferably produced by machining the intermediate tube wall, in particular by cutting, drilling, sawing, milling or grinding.

[0045] By cutting is meant cutting machining techniques such as turning, cutting, drilling, sawing, milling or grinding, which provide more precise and extremely fine structures than other known deformation techniques using heat or pressure and avoid surface contamination by forming tools such as nozzles, presses or casting moulds.

[0046] It has proven to be advantageous if the longitudinal slot has longitudinal edges, and the glass tube and the outer tube are connected to the longitudinal edges by softening.

[0047] For this purpose, a coaxial tube assembly consisting of an outer tube, an intermediate tube with a longitudinal slot and a glass tube is heated, during which the cut edges of the longitudinal slots are connected over their entire length to the outer wall of the glass tube and to the inner wall of the outer tube. The simultaneous drawing prevents undesirable radial deformations. Alternatively, the tubes are connected to each other in pairs in two process steps, one after the other.

[0048] A preform is thus obtained in which the original longitudinal slots are enclosed as hollow channels, which can be exposed on one or both sides by removing the end regions on the closed end faces of the preform.

[0049] A hollow channel formed by a longitudinal groove in the deformable glass tube and / or an intermediate tube adjacent to the glass tube. As an alternative or complement to the above-mentioned hollow channel formation method, it has also proven advantageous if the formation of the hollow channel comprises the use of a glass tube and an intermediate tube coaxially surrounding said glass tube, said glass tube having an outer cladding surface on which longitudinal grooves extending parallel to the glass tube longitudinal axis are attached, and / or said intermediate tube having an inner cladding surface on which longitudinal grooves extending parallel to the intermediate tube longitudinal axis are attached, and the hollow channel is formed from the longitudinal grooves when carrying out the process according to step (c), and the hollow channel is deformed into an elongated bulge by pressure and heat.

[0050] The longitudinal grooves in the outer cladding surface of the glass tube similarly form channels by interaction with the tube wall surrounding the glass tube, thus forming pressure chambers for deformation of the wall portions through which the longitudinal grooves extend. The longitudinal grooves in the inner cladding surface of the intermediate tube are used to form hollow channels in a similar manner as the longitudinal grooves in the intermediate tube, as detailed above.

[0051] For the application of pressure, it is advantageous for the longitudinal grooves to be continuous, i.e. they preferably extend from one end of each tube to the opposite end.

[0052] The above-stated technical problem with regard to the production of a preform for a hollow-core fiber is solved according to the invention, starting from a method of the type mentioned at the beginning, in that the formation of a pre-stage antiresonant element comprises the formation of elongated pressure chambers, each of which is adjacent to a wall deformable by pressure and heat in the target location region of the antiresonant element, and when carrying out the process according to step (c), as a result of the pressure and heat, a bulge is produced in a part of the deformable wall in the direction of the inner bore of the cladding tube while forming the antiresonant element or precursor.

[0053] The preform is the starting point for the fabrication of antiresonant hollow-core fiber. Antiresonant hollow-core fiber can be drawn directly by drawing the preform, or a blank can be made first and then the antiresonant hollow-core fiber can be drawn from the blank. Fabrication of the preform involves expanding the wall of a glass tube in the region of the desired location of the antiresonant element by applying pressure in a pressure chamber.

[0054] The glass tube wall section to be expanded is elongated and extends into the preform along the target position of the anti-resonant element pre-stage, which is formed at this position during the manufacturing process by the corresponding wall section expanding in the direction of the cladding tube inner bore by application of pressure from the opposing wall side. This completely eliminates the need to position and fix pre-manufactured anti-resonant element preforms at the corresponding positions on the cladding tube inner wall, as is known from the stack and draw method, or at least reduces the number of anti-resonant element preforms to be so positioned. The measures for manufacturing the preforms have been described in detail above in connection with the manufacture of hollow-core fibers, and these descriptions are incorporated herein by reference.

[0055] definition The following are supplementary definitions for the individual steps and terms in the above-mentioned specification. These definitions are part of the present specification. If there is a substantial discrepancy between any of the following definitions and the rest of the specification, the definitions mentioned in the rest of the specification shall prevail.

[0056] anti-resonance element The anti-resonant element may be a simple structural element or a nested structural element of the hollow-core fiber. It has at least two walls with negative curvature (convex) or no curvature (flat, straight) as viewed in the direction of the hollow core. Typically, the anti-resonant element consists of a material transparent to the operating light, such as glass (especially doped or undoped SiO2), plastic (especially polymers), composite materials or crystalline materials.

[0057] Anti-resonant element preform / anti-resonant element pre-stage The anti-resonant element preform is a component or a preform component that becomes an anti-resonant element in a hollow-core fiber mainly by simple drawing in a fiber drawing process. The anti-resonant element pre-stage is a component or a preform component that becomes an anti-resonant element preform or directly an anti-resonant element only by deformation. The anti-resonant element preform can be a simple component or a nested component to which additional positioning aids can be fixed. The anti-resonant element preform is originally present in the primary preform.

[0058] The nested anti-resonant element preform forms an anti-resonant element nested within a hollow-core fiber. It is composed of an outer tube and at least one further structural element disposed within the inner bore of the outer tube. The further structural element may be a further tube that is in contact with the inner cladding surface of the outer tube. The outer tube is also referred to as the "anti-resonant element outer tube" or "ARE outer tube" for short, and the further tube is also referred to as the "anti-resonant element inner tube" or "ARE inner tube" for short, or "nested ARE inner tube".

[0059] In the case where the anti-resonant element preforms are nested multiple times within the inner bore of the nested inner ARE tube, at least one further structural element may be disposed, for example a third tube, which is in contact with the inner cladding surface of the nested inner ARE tube.

[0060] When the anti-resonant element preforms are nested multiple times, a distinction is made between a "nested outer ARE inner tube" and a "nested inner ARE inner tube" as necessary to distinguish between the multiple tubes disposed within the outer ARE tube.

[0061] The term "cross section" in connection with cylindrical anti-resonant element preforms and their cylindrical structural elements always refers to a cross section perpendicular to the respective cylinder longitudinal axis and, unless otherwise specified, refers to a cross section of the external contour of the tubular component (and not a cross section of the internal contour).

[0062] Further processing of the primary preform, in particular by a thermoforming process, can produce intermediate products in which the original anti-resonant element preform is present in a modified shape relative to its initial shape, which modified shape is also referred to herein as the anti-resonant element preform or anti-resonant element pre-stage.

[0063] Preform / Primary preform / Secondary preform / Core preform (Cane) A preform is a component from which an anti-resonant hollow-core fiber is drawn. It can be a primary preform or a secondary preform produced by further processing of a primary preform. A primary preform can be an assembly of at least one cladding tube and a preform or precursor for an anti-resonant element housed therein in a loosely or rigidly fixed manner. Further processing of a primary preform into a secondary preform from which a hollow-core fiber is drawn can be performed by: (i) Stretching; (ii) Collapse, (iii) collapsing and simultaneous stretching; (iv) Collapse of additional cladding material; (v) collapse of additional cladding material followed by stretching; (vi) collapsing and simultaneously stretching additional cladding material; The thermoforming process may include performing one or more of the following steps once or repeatedly:

[0064] In the literature, a core preform (English: cane) is a preform obtained by collapsing and / or stretching a primary preform. Usually, the core preform is covered with additional cladding material before or during the drawing of the hollow-core fiber.

[0065] Stretching / Collapse In drawing, the primary preform is stretched to an elongation. This drawing may be performed without simultaneous collapse. The drawing may be performed to scale, so that, for example, the shape and arrangement of the components of the primary preform are reflected in the final drawn product. However, in drawing, the primary preform may not be drawn to size, and the geometry may change.

[0066] Collapsing involves narrowing the internal bore or closing or narrowing the annular gap between the tubular components, and is usually accomplished in parallel with stretching.

[0067] Hollow core / inner cladding region / outer cladding region The assembly consisting of at least one cladding tube and the preform or precursor of the anti-resonant element housed therein in a loosely or rigidly fixed manner is also referred to herein as the "primary preform". This primary preform consists of a hollow core and a cladding region. This cladding region is also referred to as the "internal cladding region" when there is an "external cladding region" formed, for example by collapsing into the assembly, and it is necessary to distinguish between these cladding regions. The names "internal cladding region" and "external cladding region" are also used for the corresponding regions of the hollow-core fiber or intermediate product obtained by further processing of the primary preform.

[0068] The term "inside the tube" is also used as a synonym for "inner cladding surface of the tube," and the term "outside the tube" is also used as a synonym for "outer cladding surface of the tube." The term "internal bore" in reference to a tube does not imply that the internal bore is formed by a drilling operation.

[0069] Cutting processing A mechanical manufacturing method for isolating a workpiece, which means in particular turning, cutting, drilling, sawing, milling or grinding, which results in a longitudinal structure extending in the direction of the cladding tube longitudinal axis, which serves as a positioning aid for the anti-resonant element preform, which is accessible from the inside of the cladding tube and may extend through the entire cladding tube wall to the outside.

[0070] Particle size and particle size distribution The particle size and particle size distribution of SiO2 particles are 50 This value is read from a particle size distribution curve that shows the cumulative amount of SiO2 particles according to their size. The particle size distribution is 10 Value, D 50 Value, D 90 It is often characterized based on the value of D 10 The value indicates the particle size that does not reach 10% of the cumulative amount of SiO2 particles, and correspondingly, D 50 Value and D 90 indicates the particle size at which the cumulative amount of SiO2 particles does not reach 50% or 90%. The particle size distribution is detected by scattered light and laser diffraction spectroscopy according to ISO13320.

[0071] Working Example The invention is explained in more detail below on the basis of an embodiment with the aid of the figures, the details of which are shown in the figures. [Brief description of the drawings]

[0072] [Figure 1] 1A and 1B show a side view and a cross-sectional top view of a first embodiment of an intermediate tube with longitudinal grooves for use in the method according to the invention; [Diagram 2] FIG. 1 shows a process for manufacturing a preform for a hollow-core fiber (b) using a tube assembly (a) comprising multiple slotted intermediate tubes according to a first embodiment. [Diagram 3]FIG. 2(b) is an enlarged view of a portion of the preform of FIG. 2(b), in which the preform of FIG. 3 is drawn into fiber to form a hollow-core fiber while forming an anti-resonant element. [Figure 4] FIG. 2 shows (a) a side view and (b) a cross-sectional top view of a second embodiment of an intermediate tube with longitudinal grooves. [Diagram 5] FIG. 1 shows a process for producing a hollow-core fiber preform (b) using a tube assembly with one slotted intermediate tube (a) according to a second embodiment. [Figure 6] FIG. 5(b) is an enlarged view of a portion of the preform of FIG. 5(a) showing the preform of FIG. 5 being drawn into fiber to form a hollow-core fiber while forming an anti-resonant element. [Figure 7] FIG. 1 is a plan view of a coaxial arrangement of glass tubes having a thermally deformable wall containing a hollow channel and an outer cylinder. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0073] FIG. 1(a) shows an intermediate tube 10, in whose wall elongated longitudinal slots 13 are cut, e.g. by mechanical sawing, water jet cutting, laser, etc., at predefined azimuthal positions and at equal intervals. These longitudinal slots 13 are used to form antiresonant elements in a finished hollow-core fiber or antiresonant element preforms in a fiber preform, the number of longitudinal slots 13 corresponding to the number of antiresonant element preforms or antiresonant elements that can be formed by the corresponding intermediate tube 10. In this example, there are six antiresonant element preforms or antiresonant elements. The longitudinal slots 13 terminate short of the tube end, so that the end regions 12 on the end faces are still closed around and connect the remaining webs 14 to each other. The cut edges are then vitrified. The cut width of the longitudinal slots 13 is uniform and is 2 mm.

[0074] From a top plan view of the cross section of the intermediate tube 10 taken along section line A-A in FIG. 1(b), it can be seen that the six longitudinal slots 13 are evenly distributed around the tube wall and extend all the way from the intermediate tube outer wall to the intermediate tube inner wall all the way to the internal bore 16.

[0075] Figure 2(a) shows a top view of a coaxial arrangement 19 of five silica glass tubes, two of which, the intermediate tubes 10; 20, are each provided with a longitudinal slot 13. The coaxial tube arrangement 19 is made up of two coaxial stacks, each of which consists of a deformable glass tube (21; 22), an intermediate tube (10; 20) and a cladding tube (22; 23). The tube 22 has a double function: in the inner stack it forms the "cladding tube", whose wall becomes part of the wall of the hollow channel, and in the outer stack it forms the "glass tube" with a deformable wall.

[0076] Details of the tube dimensions and materials are summarized in Table 1 below. [Table 1] BZ: Symbol in Figure 2a F-doped; F320: Fluorine-doped silica glass / low viscosity Undoped: Undoped silica glass / high viscosity

[0077] In this case, the materials used differ with respect to viscosity: the raw tubes 21 and 22 are made of commercially available fluorine-doped silica glass (trade name: F320) and have a lower viscosity than the slotted intermediate tubes 10, 20 and the outermost cladding tube 23 (enveloping tube).

[0078] FIG. 2(b) shows that the coaxial tube assembly 19 is subsequently collapsed onto the primary preform 26 and simultaneously drawn. In this way, the annular gaps between the tubes disappear and the tubes are firmly joined together to form a cladding tube with a common cladding wall 24. From the longitudinal slots 13 of the slotted intermediate tubes 10; 20, hollow channels arise which can be used as front and rear pressure chambers 25a; 25b during the subsequent fiber drawing process. The two pressure chambers 25a, 25b are arranged radially one behind the other in pairs. Before the fiber drawing process, at least one of the closed end regions of the primary preform 26 without longitudinal slots is removed, resulting in pressure chambers 25a, 25b open at the end faces, into which pressure gas can be introduced. The primary preform 26 has a hollow core region 27 surrounded by a cladding (cladding wall 24). Pressure chambers 25a; 25b form within the cladding wall 24 a precursor to drawing the anti-resonant element of the hollow-core fiber.

[0079] Part of Fig. 3(a) shows an enlarged view of the pressure chambers 25a; 25b created in the cladding tube wall 24 from the original longitudinal slots. During fiber drawing of the so obtained preform, a pressure difference is applied between the pressure chambers 25a; 25b and the hollow core region 27, so that the deformable wall portions of the original glass tubes 21; 22 adjacent to the pressure chambers 25a; 25b bulge inwards along the pressure chambers 25a; 25b.

[0080] Figure 3(b) shows that the hollow-core fibre 29 now has a first bulge 28a on the inside 27 of the former innermost glass tube, which surrounds a second bulge 28b. The first and second bulges 28a; 28b form nested anti-resonant elements made up of two glass films with negatively curved surfaces.

[0081] Where the same reference numerals are used in the following description of Figures 4 to 7 as in Figures 1 to 3, they indicate the same or equivalent components as explained in detail above with reference to these figures.

[0082] FIG. 4(a) shows another intermediate tube 110, in whose wall elongated longitudinal slots 13 are cut, for example by mechanical sawing, water jet cutting, laser, etc., at predefined azimuthal positions and at equal intervals. These longitudinal slots 13 are used to form antiresonant elements in a finished hollow-core fiber or antiresonant element preforms in a fiber preform, the number of longitudinal slots 13 corresponding to the number of antiresonant element preforms or antiresonant elements that can be formed by the corresponding intermediate tube 10. In this example, there are five antiresonant element preforms or antiresonant elements. The longitudinal slots 13 terminate short of the tube end, so that the end regions 12 on the end faces are still closed around and connect the remaining webs 14 to each other. The cut edges are then vitrified. The cut width of the longitudinal slots 13 is uniform and is 2 mm.

[0083] From a top plan view of the cross section of the intermediate tube 110 taken along section line A-A in FIG. 4(b), it can be seen that the five longitudinal slots 13 are evenly distributed around the tube wall at a circumferential angle of 72 degrees and extend all the way from the intermediate tube outer wall to the intermediate tube inner wall all the way to the internal bore 16.

[0084] Figure 5(a) shows a top plan view of a coaxial assembly of three silica glass tubes, including a slotted intermediate tube 110. The coaxial tube assembly is composed of a deforming glass tube 21, an intermediate tube 110 with a longitudinal slot 13, and a cladding tube 22.

[0085] Details of the tube dimensions and materials are summarized in Table 2 below. [Table 2] BZ: Symbol in Figure 5a F-doped; F320: Fluorine-doped silica glass / low viscosity Undoped: Undoped silica glass / high viscosity

[0086] In this case, the materials used differ with respect to viscosity: the non-mechanically processed tube 21 is made of commercially available fluorine-doped silica glass (trade name: F320) and has a lower viscosity than the slotted intermediate tube 110 and the cladding tube 22 (outer layer tube).

[0087] FIG. 5(b) shows that the coaxial tube assembly is subsequently collapsed onto the primary preform 126, which is drawn simultaneously to eliminate the annular gaps between the tubes 21, 22, 110, so that they are rigidly joined together and form a common cladding wall 124. The longitudinal slots 13 of the slotted intermediate tube 110 then form hollow channels in the cladding wall 124, which can be used as pressure chambers 125 during the subsequent fiber drawing process. The primary preform 126 has a hollow core region 127 surrounded by a cladding (cladding wall 124). The pressure chamber 125 forms a precursor for an anti-resonant element in the cladding region of the hollow-core fiber to be drawn.

[0088] Prior to the fiber drawing process, at least one of the closed end regions of the preform 126 that does not have a longitudinal slot is removed, thereby opening up the end side of the pressure chamber 125 to allow the introduction of pressurized gas.

[0089] Portion of Figure 6(a) is an enlarged view of the pressure chamber 125 formed from the original longitudinal slot 13. During fiber drawing of the resulting preform 126, a pressure differential is applied between the pressure chamber 125 and the internal bore 16, causing the wall area adjacent the pressure chamber 125 to bulge inwardly along the pressure chamber 125.

[0090] FIG. 6(b) shows that a bulge 128a now appears in the hollow-core fiber 129 on the inside 17 of the former glass tube, and this bulge forms an anti-resonant element due to the glass film having a negative surface curvature.

[0091] Instead of the longitudinal grooves 13, the intermediate tubes 10, 20, 110 may also be provided with longitudinal grooves in their inner cladding surface, which are formed, if necessary, by mechanical milling in the inner cladding surface of the intermediate tube.

[0092] As an alternative or complement to intermediate tubes provided with longitudinal slots or grooves, the glass tubes 21;22 with heat-deformable walls may be provided with longitudinal grooves in their outer cladding surface, which may be formed, if necessary, by mechanical milling.

[0093] As an alternative or complement to the glass tubes and / or intermediate tubes with longitudinal slots or grooves described above, the glass tubes 21;22 with heat-deformable walls may be provided with hollow channels. An example for this is shown diagrammatically in FIG. 7. The coaxial arrangement comprises a glass tube 221 with a heat-deformable wall and an outer cylinder 22 (cladding tube). Inside the wall of the glass tube 221 and close to the inner cladding surface 221a, four hollow channels 213 evenly distributed around the circumference run parallel to the glass tube longitudinal axis (running perpendicular to the plane of the paper). The hollow channels 213 are produced by laser cutting and are through (running from one end of the wall to the other). In the cross-section shown, these hollow channels have a rectangular shape, the long sides of which run tangentially to the adjacent wall parts of the inner cladding surface 221a.

[0094] In this embodiment, the intermediate tube may be omitted. Details of the tube dimensions and materials are summarized in Table 3 below. [Table 3] BZ: Symbol in Figure 7 F-doped; F320: Fluorine-doped silica glass / low viscosity Undoped: Undoped silica glass / high viscosity

[0095] During the hot forming process, an internal pressure is generated by introducing a pressurized gas into the hollow channel 213, which can deform the wall portion of the glass tube 221 that defines the hollow channel 213 inwardly. At this time, a long bulge is generated in the glass tube 221 that faces inwardly toward the glass tube inner bore 16, and this bulge is used as the anti-resonant element preform.

Claims

1. 1. A method for making an anti-resonant hollow-core fiber (29; 129) having a hollow core extending along a longitudinal axis of the fiber and a cladding region surrounding the hollow core, the cladding region including a plurality of anti-resonant elements, comprising: (a) providing a primary preform (26; 126) for a hollow-core fiber having at least one cladding tube, a cladding tube inner bore, a cladding tube longitudinal axis, and a cladding tube wall (24; 124) defined by an inner side and an outer side extending along said cladding tube longitudinal axis; (b) forming a plurality of precursor stages (25a; 25b; 125; 213) for anti-resonant elements (28a; 28b; 128) at targeted positions on the cladding wall (24; 124); (c) drawing the primary preform (26; 126) into a hollow-core fiber (29; 129) or further processing the primary preform (26; 126) into a secondary preform from which a hollow-core fiber is drawn; Equipped with In the further processing step, (i) stretching; (ii) collapse, (iii) collapsing and simultaneous stretching; (iv) collapse of additional cladding material; (v) collapsing of additional cladding material followed by stretching; (vi) collapsing and simultaneously stretching additional cladding material; In a manufacturing method, one or more of the following thermoforming processes are carried out once or repeatedly: a method according to claim 1, characterized in that the formation of the precursor (25a; 25b; 125; 213) of the anti-resonant element comprises the formation of elongated pressure chambers (25a; 25b; 125; 213), each of which is adjacent to a pressure- and heat-deformable wall (21; 22) in the region of the target position of the anti-resonant element (28a; 28b; 128), and when the process according to step (c) is carried out, as a result of the pressure and heat, a bulge occurs in the part of the deformable wall (21; 22) in the direction of the cladding tube inner bore (16), thereby forming the anti-resonant element (28a; 28b; 128) or a precursor thereof, the deformable wall parts being formed by wall parts of a glass tube (21; 221), and each of the pressure chambers is designed as a hollow channel adjacent to a wall part of the glass tube (21; 221).

2. 2. The method according to claim 1, characterized in that the hollow channel (213) is formed inside the tube wall of the glass tube (221), extending parallel to the glass tube longitudinal axis.

3. 3. The method according to claim 2, characterized in that a coaxial glass tube arrangement is formed, comprising an inner peripheral row of hollow channels in the tube wall of an inner glass tube and an outer peripheral row of hollow channels in the tube wall of an outer glass tube, the inner and outer peripheral rows of hollow channels being on a common connecting line as viewed in the radial direction and spatially separated from each other by at least one inwardly deformable glass wall circumferentially extending therearound.

4. 2. The method according to claim 1, characterized in that the formation of the hollow channels (13; 25a; 25b; 125) comprises the steps of placing an intermediate tube (10; 20) having an intermediate tube longitudinal axis between the glass tube (21) and the outer tube (22; 23) and stretching an intermediate tube wall defined by an inside and an outside along the intermediate tube longitudinal axis, in which a longitudinal slot (13) is provided, from which the hollow channels (25a; 25b; 125) are formed during the execution of the process according to step (c), which can be used in a subsequent manufacturing step to apply pressure to the outside of the glass tube (21) in order to expand the respective wall portion in the direction of the cladding tube inner bore.

5. 5. A method according to claim 4, characterized in that an intermediate tube (10; 20) of circular internal cross section is provided and machined.

6. 5. The method according to claim 4, characterized in that the intermediate tube (10; 20) has an end face end and the longitudinal slot (13) terminates before the end face end.

7. 5. The method according to claim 4, characterized in that a coaxial tube arrangement (19) is formed comprising an inner glass tube (21), an inner intermediate tube (10), an inner outer tube (22) which at the same time forms an outer glass tube (22), an outer intermediate tube (20) and an outer outer tube (23), the longitudinal slots (13) of the inner intermediate tube and the outer intermediate tube (10; 20) being radially on a common connecting line and being spatially separated from one another by at least one inwardly deformable glass wall (22) which runs around the circumference.

8. 2. The method according to claim 1, characterized in that the formation of the hollow channel comprises the use of a glass tube and an intermediate tube coaxially surrounding the glass tube, the glass tube having a glass tube outer cladding surface on which a longitudinal groove extending parallel to the longitudinal axis of the glass tube is provided, and / or the intermediate tube having an intermediate tube inner cladding surface on which a longitudinal groove extending parallel to the longitudinal axis of the intermediate tube is provided, the hollow channel being formed from the longitudinal groove when carrying out the process according to step (c), the hollow channel being deformed into an elongated bulge by pressure and heat.

9. Method according to any one of claims 4 to 7, characterized in that the longitudinal slot (13) is made by a cutting, drilling, sawing, milling or grinding process.

10. The method of claim 8, wherein the longitudinal groove is produced by cutting, drilling, sawing, milling or grinding.

11. 8. The method according to any one of claims 4 to 7, characterized in that the longitudinal slots (13) have longitudinal edges which soften and fuse with the surrounding glass material during simultaneous drawing.

12. The method of claim 8, wherein the longitudinal grooves have longitudinal edges which soften and fuse with the surrounding glass material during simultaneous drawing.

13. Method according to any one of the preceding claims, characterized in that the glass tube (21; 22) is made of glass containing a dopant that reduces its viscosity.

14. 1. A method for making an anti-resonant hollow-core fiber preform having a hollow core extending along a longitudinal axis of the fiber and a cladding region including a plurality of anti-resonant elements and surrounding the hollow core, comprising: (a) providing a primary preform (26; 126) for a hollow-core fiber having at least one cladding tube, a cladding tube inner bore, a cladding tube longitudinal axis, and a cladding tube wall (24; 124) defined by an inner side and an outer side extending along said cladding tube longitudinal axis; (b) forming a plurality of precursor stages (25a; 25b; 125; 213) for anti-resonant elements (28a; 28b; 128) at targeted locations on the cladding wall (24; 124); (c) further processing the primary preform (26; 126) into a secondary preform for a hollow-core fiber; Equipped with In the further processing step, (i) stretching; (ii) collapse, (iii) collapsing and simultaneous stretching; (iv) collapse of additional cladding material; (v) collapsing of additional cladding material followed by stretching; (vi) collapsing and simultaneously stretching additional cladding material; In a manufacturing method, one or more of the following thermoforming processes are carried out once or repeatedly: a method according to claim 1, characterized in that the formation of the precursor (25a; 25b; 125; 213) of the anti-resonant element comprises the formation of elongated pressure chambers (25a; 25b; 125; 213), each of which is adjacent to a pressure- and heat-deformable wall (21; 22) in the region of the target position of the anti-resonant element (28a; 28b; 128), and when the process according to step (c) is carried out, as a result of the pressure and heat, a bulge occurs in the part of the deformable wall (21; 22) in the direction of the cladding tube inner bore (16), thereby forming the anti-resonant element (28a; 28b; 128) or a precursor thereof, the deformable wall parts being formed by wall parts of a glass tube (21; 221), and each of the pressure chambers is designed as a hollow channel adjacent to a wall part of the glass tube (21; 221).

Citation Information

Patent Citations

  • Apparatus for installing ring anchor by winding wire

    JP1979030689A

  • Optical fiber and its manufacturing method

    JP2002321935A

  • Method for manufacturing optical fiber preform and method for manufacturing optical fiber using the same

    JP2018043924A

  • Method for manufacturing optical fiber

    JP2018150184A

  • Hollow-core fiber and its manufacturing method

    JP2018533042A