Boron nitride sintered body, composite body, their manufacturing method, and heat dissipation member
A boron nitride sintered body with controlled pore size and porosity, combined with a resin, addresses the need for high thermal conductivity and insulation in electronic components, achieving thermal conductivity of 40 W/(m·K) or more in a composite body.
Patent Information
- Application Number
- JP2022512551
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-31
- Filing Date
- 2021-03-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-03-30
AI Technical Summary
There is a demand for heat dissipation members with higher thermal conductivity to address the increased heat generation in electronic components due to higher circuit integration, and existing composites using boron nitride do not adequately meet these demands in terms of thermal conductivity and insulation properties.
A boron nitride sintered body with controlled pore size, porosity, and orientation index is developed, combined with a resin to form a composite body, which includes boron nitride particles and pores with an average diameter less than 2 μm, porosity between 30 to 65% by volume, and a bulk density of 800-1500 kg/m³, resulting in high thermal conductivity and insulation properties.
The composite body achieves thermal conductivity of 40 W/(m·K) or more, with reduced anisotropy and improved insulation, suitable for use as a heat dissipation member in electronic components.
Smart Images

Figure 0007566883000003 
Figure 0007566883000004 
Figure 0007566883000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a boron nitride sintered body, a composite body, and methods for producing the same, and a heat dissipation member. [Background technology]
[0002] Components such as power devices, transistors, thyristors, and CPUs are required to efficiently dissipate heat generated during use. To meet this demand, conventional methods have been to increase the thermal conductivity of the insulating layer of printed wiring boards on which electronic components are mounted, or to attach electronic components or printed wiring boards to heat sinks via thermal interface materials having electrical insulation. For such insulating layers and thermal interface materials, composites (heat dissipation members) made of resin and ceramics such as boron nitride are used.
[0003] As such a composite, the use of a composite in which a porous ceramic body is impregnated with a resin has been considered. Since boron nitride has lubricity, high thermal conductivity, and insulating properties, the use of ceramics containing boron nitride in heat dissipation members has been considered. Patent Document 1 proposes a technology that reduces the anisotropy of thermal conductivity while improving thermal conductivity by setting the degree of orientation and graphitization index within a predetermined range. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-162697 A Summary of the Invention [Problem to be solved by the invention]
[0005] 2. Description of the Related Art With the recent trend toward higher integration of circuits in electronic components, there is a demand for heat dissipation members having even higher heat dissipation characteristics than before, and for composites suitable for use therewith.
[0006] Therefore, the present disclosure provides a boron nitride sintered body and a composite having sufficiently high thermal conductivity. The present disclosure also provides a manufacturing method capable of manufacturing such a boron nitride sintered body and composite. The present disclosure also provides a heat dissipation member having sufficiently high thermal conductivity by including the above-mentioned composite. [Means for solving the problem]
[0007] In one aspect, the present disclosure provides a boron nitride sintered body that includes boron nitride particles and pores, the average pore size of the pores being less than 2 μm. Since the size of the pores in such a boron nitride sintered body is sufficiently small, the contact area between the primary particles of boron nitride can be sufficiently large. Therefore, the thermal conductivity can be sufficiently high.
[0008] The porosity of the boron nitride sintered body may be 30 to 65% by volume. The bulk density may be 800 to 1500 kg / m 3 The boron nitride sintered body may have a thermal conductivity of 40 W / (m·K) or more. By having at least one of the porosity and bulk density within this range, the resin composition can be sufficiently impregnated while the thermal conductivity is sufficiently high. Such a boron nitride sintered body can form a composite body that can simultaneously achieve excellent thermal conductivity and high levels of insulation. The thermal conductivity of the boron nitride sintered body may be 40 W / (m·K) or more. Such a boron nitride sintered body can form a composite body having a sufficiently high thermal conductivity.
[0009] The orientation index of the boron nitride sintered body may be equal to or less than 40. This makes it possible to sufficiently reduce the anisotropy of thermal conductivity.
[0010] The boron nitride sintered body may be in the form of a sheet with a thickness of less than 2 mm, which allows smooth impregnation of the resin composition into the pores.
[0011] In one aspect, the present disclosure provides a boron nitride sintered body according to any one of the above, a resin filled in at least a portion of the pores of the boron nitride sintered body, of The composite material contains the above-mentioned boron nitride sintered body and a resin, and therefore has both excellent thermal conductivity and excellent insulating properties.
[0012] In one aspect, the present disclosure provides a heat dissipation member having the above-mentioned composite. Since the heat dissipation member has the above-mentioned composite, the heat dissipation member has a sufficiently high thermal conductivity.
[0013] In one aspect, the present disclosure provides a method for producing a boron nitride sintered body, comprising: a nitriding step of sintering boron carbide powder in a nitrogen atmosphere to obtain a sintered body containing boron carbonitride; and a sintering step of molding and heating a compound containing the sintered body and a sintering aid to obtain a boron nitride sintered body containing boron nitride particles and pores, wherein the sintering aid contains a boron compound and a calcium compound, and the compound contains 1 to 20 parts by mass in total of the boron compound and the calcium compound per 100 parts by mass of the sintered body.
[0014] In the above manufacturing method, a fired material containing boron carbonitride is used in the sintering step. Therefore, compared to the case where scaly boron nitride particles are used, the sintering property can be improved while suppressing the orientation of the particles. Therefore, the orientation of the generated boron nitride particles can be reduced. In addition, the compound contains a predetermined sintering aid together with the fired material containing boron carbonitride. Due to these factors, the grain growth of the primary particles of boron nitride proceeds appropriately. Therefore, the size of the pores contained in the boron nitride sintered body can be sufficiently small while the contact area between the boron nitride particles can be sufficiently large, resulting in a boron nitride sintered body having a sufficiently high thermal conductivity. The average pore size of the pores contained in the boron nitride sintered body obtained in the above sintering step may be less than 2 μm.
[0015] The compound in the above manufacturing method may contain 0.5 to 40 atomic % of calcium constituting the calcium compound relative to 100 atomic % of boron constituting the boron compound. By containing boron and calcium in such a ratio, the average pore size of the pores contained in the boron nitride sintered body can be further reduced.
[0016] The boron nitride sintered body obtained in the sintering step may be in a sheet shape and may have a thickness of less than 2 mm. By forming a sheet-shaped boron nitride sintered body in this way in the sintering step, it is possible to reduce material loss and produce a sheet-shaped boron nitride sintered body with a high yield, compared to cutting a block-shaped boron nitride sintered body into a sheet shape. In addition, by making the thickness as thin as less than 2 mm, it is possible to smoothly impregnate the resin composition.
[0017] In one aspect, the present disclosure provides a method for producing a composite comprising a boron nitride sintered body and a resin filled in at least a part of the pores, the method comprising an impregnation step of impregnating the boron nitride sintered body obtained by any one of the above-mentioned production methods with a resin composition. The composite obtained by such a production method has a sufficiently high thermal conductivity because it is obtained using the above-mentioned boron nitride sintered body. Effect of the Invention
[0018] According to the present disclosure, it is possible to provide a boron nitride sintered body and a composite having sufficiently high thermal conductivity. In addition, the present disclosure can provide a manufacturing method capable of manufacturing such a boron nitride sintered body and composite. In addition, the present disclosure can provide a heat dissipation member having sufficiently high thermal conductivity by including the above-mentioned composite. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a perspective view showing an example of a boron nitride sintered body. [Diagram 2] FIG. 2 is a graph showing the Log differential pore volume distribution of Examples 1 and 2. [Diagram 3] FIG. 3 is a graph showing the Log differential pore volume distribution of Examples 3 and 4. [Figure 4] FIG. 4 is a graph showing the Log differential pore volume distributions of Comparative Examples 1 and 2. [Diagram 5] FIG. 5 is a graph showing the cumulative pore volume distributions of Examples 1 and 2 and Comparative Examples 1 and 2. [Figure 6] FIG. 6 is a graph showing the cumulative pore volume distribution of Examples 3 and 4. [Figure 7] FIG. 7 is an SEM photograph showing a cross section of the boron nitride sintered body of Example 1. [Figure 8] FIG. 8 is an SEM photograph showing a cross section of the boron nitride sintered body of Example 2. [Figure 9] FIG. 9 is an SEM photograph showing a cross section of the boron nitride sintered body of Example 3. [Figure 10] FIG. 10 is an SEM photograph showing a cross section of the boron nitride sintered body of Example 4. [Figure 11] FIG. 11 is an SEM photograph showing a cross section of the boron nitride sintered body of Comparative Example 1. [Figure 12] FIG. 12 is an SEM photograph showing a cross section of the boron nitride sintered body of Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings as needed. However, the following embodiments are merely examples for explaining the present disclosure, and are not intended to limit the present disclosure to the following contents.
[0021] The boron nitride sintered body according to one embodiment contains boron nitride particles formed by sintering primary particles of boron nitride together and pores. The boron nitride sintered body includes boron nitride particles and pores. The average pore size of the pores is less than 2 μm. Since the size of the pores in this boron nitride sintered body is sufficiently small, the contact area between the primary particles of the boron nitride particles can be sufficiently large. Therefore, the thermal conductivity can be sufficiently high. From the viewpoint of further increasing the thermal conductivity, the average pore size of the pores may be less than 1 μm, may be less than 0.8 μm, or may be less than 0.6 μm. From the viewpoint of facilitating the impregnation of the resin composition into the boron nitride sintered body, the average pore size of the pores may be 0.1 μm or more, or may be 0.2 μm or more.
[0022] The average pore diameter of the pores is determined based on the pore diameter distribution when the pressure is increased from 0.0042 MPa to 206.8 MPa using a mercury porosimeter. With the pore diameter on the horizontal axis and the cumulative pore volume on the vertical axis, the pore diameter at which the cumulative pore volume reaches 50% of the total pore volume is the average pore diameter. The mercury porosimeter manufactured by Shimadzu Corporation can be used.
[0023] The peak pore diameter of the pores may be less than 2 μm, less than 1 μm, less than 0.8 μm, or less than 0.6 μm. In the present disclosure, the "peak pore diameter" is the pore diameter at which the value obtained by dividing the differential pore volume (dV) by the logarithmic differential value d (logD) of the pore diameter is maximized in a graph showing the Log differential pore volume distribution.
[0024] The porosity of the boron nitride sintered body, i.e., the volume ratio of the pores in the boron nitride sintered body, may be 30 to 65 volume %, or 35 to 55 volume %. If the porosity is too large, the strength of the boron nitride sintered body tends to decrease. On the other hand, if the porosity is too small, the resin content when the composite is produced decreases, and the insulating properties tend to decrease.
[0025] The porosity is calculated from the volume and mass of the boron nitride sintered body by the bulk density [B(kg / m 3 )] was calculated, and this bulk density was compared with the theoretical density of boron nitride [2280 (kg / m 3 )], it can be calculated using the following formula (1). Porosity (volume%) = [1-(B / 2280)] x 100 (1)
[0026] Bulk density B is 800-1500kg / m 3 may be 1000 to 1400 kg / m 3 If the bulk density B is too small, the strength of the boron nitride sintered body tends to decrease. On the other hand, if the bulk density B is too large, the amount of resin impregnation decreases, and the insulating properties of the composite tend to decrease.
[0027] The thermal conductivity of the boron nitride sintered body may be 20 W / (m·K) or more, 40 W / (m·K) or more, 45 W / (m·K) or more, or 57 W / (m·K) or more. By using a boron nitride sintered body with high thermal conductivity, a heat dissipation component with sufficiently excellent heat dissipation performance can be obtained. Thermal conductivity (H) can be calculated using the following formula (2). H=A×B×C (2)
[0028] In equation (2), H is the thermal conductivity (W / (m K)) and A is the thermal diffusivity (m 2 / sec), B is bulk density (kg / m 3 ), and C indicate the specific heat capacity (J / (kg K)). Thermal diffusivity A can be measured by the laser flash method. Bulk density B can be measured from the volume and mass of the boron nitride sintered body. Specific heat capacity C can be measured using a differential scanning calorimeter.
[0029] The content of boron nitride in the boron nitride sintered body may be 90 mass % or more, 95 mass % or more, or 98 mass % or more.
[0030] The compressive strength of the boron nitride sintered body may be, for example, 3 MPa or more, 5 MPa or more, or 10 MPa or more. By having a high compressive strength, it is possible to suppress breakage when used as a component. The compressive strength can be measured using a compression tester (e.g., Autograph AG-X, manufactured by Shimadzu Corporation) in accordance with JIS K7181. The measurement conditions are as follows. Compression speed: 1mm / min Load cell: 100kN Test temperature: 200℃ Sample size: length x width x height = 10mm x 10mm x 4mm
[0031] The compressive elastic modulus of the boron nitride sintered body may be 1 GPa or more, or 1.5 GPa or more. By increasing the compressive elastic modulus, deformation can be suppressed. The compressive elastic modulus may be 4 GPa or less, or 3 GPa or less. This allows the boron nitride sintered body or a composite obtained using the same to be sandwiched between a pair of opposing members and pressed to bond, thereby allowing it to deform moderately and increase adhesion to the members.
[0032] The boron nitride sintered body may be in a sheet (thin plate) shape as shown in FIG. 1. The boron nitride sintered body 10 has a small thickness, so that the resin composition can be smoothly impregnated. This allows the pores of the boron nitride sintered body to be sufficiently filled with the resin, and a composite body having excellent insulating properties can be obtained. The thickness t of the boron nitride sintered body 10 may be less than 2 mm, less than 1 mm, or less than 0.5 mm. From the viewpoint of ease of producing a molded body, the thickness t of the boron nitride sintered body 10 may be 0.1 mm or more, or 0.2 mm or more. An example of the thickness t of the boron nitride sintered body 10 is 0.1 mm or more and less than 2 mm. The area of the main surface 10a of the boron nitride sintered body 10 is 500 mm 2 It may be more than 800 mm 2 It may be more than 1000 mm 2 It may be more than that.
[0033] The shape of the boron nitride sintered body is not limited to the shape shown in FIG. 1, and may be, for example, a disk-shaped sheet or a C-shaped sheet. A block-shaped boron nitride sintered body may be cut and / or polished to be processed into a sheet as shown in FIG. 1. However, when processing such as cutting is performed, material loss occurs. For this reason, if a sheet-shaped boron nitride sintered body is produced using a sheet-shaped molded body, the material loss can be reduced. This can improve the yield of the boron nitride sintered body and the composite. Note that, when the block-shaped boron nitride sintered body is, for example, a polyhedron, all sides have a suitable length and have a thickness greater than that of a sheet-shaped boron nitride sintered body. In other words, the block-shaped boron nitride sintered body refers to a shape that can be divided into a plurality of sheet-shaped (thin plate-shaped) pieces by cutting.
[0034] The orientation index of the boron nitride crystals in the boron nitride sintered body may be 40 or less, 15 or less, or 10 or less. This allows the anisotropy of thermal conductivity to be sufficiently reduced. Therefore, in the case of a sheet-like boron nitride sintered body 10, the thermal conductivity along the thickness direction can be sufficiently increased. The thermal conductivity along the thickness direction may be 40 W / (m·K) or more, 45 W / (m·K) or more, or 57 W / (m·K) or more. The orientation index of the boron nitride sintered body may be 2.0 or more, 3.0 or more, or 4.0 or more. The orientation index in the present disclosure is an index for quantifying the degree of orientation of the boron nitride crystals. The orientation index can be calculated from the peak intensity ratio [I(002) / I(100)] of the (002) plane and the (100) plane of boron nitride measured by an X-ray diffraction device.
[0035] In one embodiment, the conjugate comprises: Boron NitrideIt is a composite of a sintered body and a resin, and has the above-mentioned boron nitride sintered body and a resin filled in at least a part of the pores of the boron nitride sintered body. Examples of the resin that can be used include epoxy resin, silicone resin, cyanate resin, silicone rubber, acrylic resin, phenol resin, melamine resin, urea resin, unsaturated polyester, fluororesin, polyimide, polyamideimide, polyetherimide, polybutylene terephthalate, polyethylene terephthalate, polyphenylene ether, polyphenylene sulfide, wholly aromatic polyester, polysulfone, liquid crystal polymer, polyethersulfone, polycarbonate, maleimide resin, maleimide-modified resin, ABS (acrylonitrile-butadiene-styrene) resin, AAS (acrylonitrile-acrylic rubber-styrene) resin, AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resin, polyglycolic acid resin, polyphthalamide, polyacetal, etc. One of these may be contained alone, or two or more may be contained in combination.
[0036] When the composite is used for an insulating layer of a printed wiring board, the resin may contain an epoxy resin from the viewpoint of improving heat resistance and adhesive strength to a circuit. When the composite is used for a thermal interface material, the resin may contain a silicone resin from the viewpoint of improving heat resistance, flexibility, and adhesion to a heat sink or the like. The resin may be a cured product (C-stage state) or a semi-cured product (B-stage state). Whether the resin is in a semi-cured state can be confirmed, for example, by a differential scanning calorimeter.
[0037] The content of boron nitride particles in the composite may be 40 to 70 volume % or 45 to 65 volume % based on the total volume of the composite. The content of resin in the composite may be 30 to 60 volume % or 35 to 55 volume % based on the total volume of the composite. A composite containing boron nitride particles and resin in such ratios can achieve both high insulation properties and high thermal conductivity.
[0038] The resin content in the composite may be 10 to 70 mass%, 10 to 60 mass%, 20 to 60 mass%, 20 to 55 mass%, or 25 to 55 mass% based on the total mass of the composite. A composite containing resin in such a ratio can achieve both high insulation and high thermal conductivity. The resin content in the composite can be determined by heating the composite to decompose and remove the resin, and calculating the mass of the resin from the difference in mass before and after heating.
[0039] The composite may further contain other components in addition to the boron nitride sintered body and the resin filled in the pores. Examples of the other components include a curing agent, an inorganic filler, a silane coupling agent, an antifoaming agent, a surface conditioner, and a wetting and dispersing agent. The inorganic filler may contain one or more types selected from the group consisting of aluminum oxide, silicon oxide, zinc oxide, silicon nitride, aluminum nitride, and aluminum hydroxide. This can further improve the thermal conductivity of the composite.
[0040] The composite of the present embodiment contains the above-mentioned boron nitride sintered body and resin, and therefore has both excellent thermal conductivity and excellent insulating properties. Therefore, it can be suitably used as, for example, a heat dissipation member. The heat dissipation member may be composed of the above-mentioned composite, or may be composed of a combination of the composite and another member (for example, a metal plate such as aluminum).
[0041] An example of a method for manufacturing a boron nitride sintered body, a composite, and a heat dissipation member is described below. The above description of the boron nitride sintered body, the composite, and the heat dissipation member is applied to the following manufacturing method. The manufacturing method for the boron nitride sintered body of this example includes a nitriding step of sintering boron carbide powder under a nitrogen pressure atmosphere to obtain a sintered product containing boron carbonitride, and a sintering step of molding and heating a compound containing the sintered product and a sintering aid to obtain a boron nitride sintered body containing boron nitride particles and pores.
[0042] The boron carbide powder can be prepared, for example, by the following procedure. After mixing boric acid and acetylene black, the mixture is heated in an inert gas atmosphere at 1800 to 2400°C for 1 to 10 hours to obtain a boron carbide block. The boron carbide block can be crushed, washed, subjected to impurity removal, and dried to prepare the boron carbide powder.
[0043] In the nitriding step, the boron carbide powder is sintered in a nitrogen atmosphere to obtain a sintered material containing boron carbonitride (B4CN4). The sintering temperature in the nitriding step may be 1800°C or higher, or may be 1900°C or higher. The sintering temperature may be 2400°C or lower, or may be 2200°C or lower. The sintering temperature may be, for example, 1800 to 2400°C.
[0044] The pressure in the nitriding step may be 0.6 MPa or more, or 0.7 MPa or more. The pressure may be 1.0 MPa or less, or 0.9 MPa or less. The pressure may be, for example, 0.6 to 1.0 MPa. If the pressure is too low, the nitriding of boron carbide tends to be difficult to proceed. On the other hand, if the pressure is too high, the manufacturing cost tends to increase. Note that the pressure in the present disclosure is an absolute pressure.
[0045] The nitrogen gas concentration in the nitrogen atmosphere in the nitriding step may be 95% by volume or more, or may be 99.9% by volume or more. The partial pressure of nitrogen may be in the above-mentioned pressure range. The firing time in the nitriding step is not particularly limited as long as the nitriding proceeds sufficiently, and may be, for example, 6 to 30 hours, or 8 to 20 hours.
[0046] In the sintering step, the fired product containing the boron carbonitride particles obtained in the nitriding step is mixed with a sintering aid to obtain a compound. The sintering aid includes a boron compound and a calcium compound. The compound contains 1 to 20 parts by mass of the boron compound and the calcium compound in total per 100 parts by mass of the fired product. By setting the content in this range, it is possible to suppress excessive grain growth of the primary particles while promoting sintering by moderate grain growth, and to reduce the pores remaining in the boron nitride sintered body.
[0047] From the viewpoint of making the pores contained in the boron nitride sintered body sufficiently small, the compound may contain, for example, 1 to 20 parts by mass, 3 to 15 parts by mass, or 4 to 10 parts by mass of the boron compound and calcium compound in total relative to 100 parts by mass of the fired product. If the total content of the boron compound and calcium compound is excessive, the grain growth of the primary particles of boron nitride will proceed too much, and the average pore size of the pores contained in the boron nitride sintered body will tend to become large. On the other hand, if the total content of the boron compound and calcium compound is too small, the grain growth of the primary particles of boron nitride will not proceed easily, and the porosity of the boron nitride sintered body will tend to become high.
[0048] The sintering aid may contain 0.5 to 40 atomic % or 0.7 to 30 atomic % of calcium constituting the calcium compound relative to 100 atomic % of boron constituting the boron compound. By containing boron and calcium in such a ratio, the average pore size of the pores contained in the boron nitride sintered body can be further reduced. If the content ratio of the boron compound is too large, the pores Diameter On the other hand, if the content ratio of the calcium compound is too high, the pore size tends to become large.
[0049] Examples of boron compounds include boric acid, boron oxide, and borax. Examples of calcium compounds include calcium carbonate and calcium oxide. The sintering aid may contain components other than boric acid and calcium carbonate. Examples of such components include alkali metal carbonates such as lithium carbonate and sodium carbonate. In addition, a binder may be added to the compound to improve moldability. Examples of binders include acrylic compounds.
[0050] When mixing the fired product and the sintering aid, the fired product may be pulverized using a general pulverizer or crusher. For example, a ball mill, a Henschel mixer, a vibration mill, a jet mill, or the like may be used. In this disclosure, "pulverization" also includes "crushing". The fired product may be pulverized and then the sintering aid may be mixed, or the fired product and the sintering aid may be mixed and then pulverized and mixed at the same time.
[0051] The compound may be powder pressed or molded into a molded body, or may be molded into a sheet-like molded body by a doctor blade method. The molding pressure may be, for example, 5 to 350 MPa. The shape of the molded body is not particularly limited, and may be, for example, a sheet-like body with a thickness of 1 mm or less. If a boron nitride sintered body is produced using a sheet-like molded body, impregnation with resin proceeds smoothly. In addition, compared with the case where a block-like boron nitride sintered body or composite is cut into a sheet-like body, material loss due to processing can be reduced by forming the molded body into a sheet-like body. Therefore, a sheet-like boron nitride sintered body or composite can be produced with a high yield.
[0052] The compact thus obtained is heated and fired, for example, in an electric furnace. The heating temperature may be, for example, 1800°C or higher, or 1900°C or higher. The heating temperature may be, for example, 2200°C or lower, or 2100°C or lower. If the heating temperature is too low, grain growth tends not to proceed sufficiently. The heating time may be 0.5 hours or more, 1 hour or more, 3 hours or more, 5 hours or more, or 10 hours or more. The heating time may be 40 hours or less, 30 hours or less, or 20 hours or less. The heating time may be, for example, 0.5 to 40 hours, or 1 to 30 hours. If the heating time is too short, grain growth tends not to proceed sufficiently. On the other hand, if the heating time is too long, it tends to be industrially disadvantageous. The heating atmosphere may be, for example, an inert gas atmosphere such as nitrogen, helium, or argon. When a binder is added to the compound, the compound may be calcined at a temperature and atmosphere at which the binder decomposes before the above-mentioned heating to degrease it.
[0053] By the above steps, a boron nitride sintered body containing boron nitride particles and pores can be obtained. In this boron nitride sintered body, the primary particles of boron nitride using boron carbonitride have grown to an appropriate size, so the size of the pores can be made sufficiently small. Therefore, the contact area between the boron nitride particles can be made sufficiently large, resulting in a boron nitride sintered body with sufficiently high thermal conductivity.
[0054] An example of a method for producing a composite includes an impregnation step of impregnating a boron nitride sintered body with a resin composition. The boron nitride sintered body may be one produced by the above-mentioned method. The resin composition may contain a resin component, a curing agent, and a solvent from the viewpoint of improving fluidity and handling. In addition to these, the resin composition may contain an inorganic filler, a silane coupling agent, an antifoaming agent, a surface conditioner, a wetting and dispersing agent, etc.
[0055] As the resin component, for example, those which become the resins mentioned in the description of the composite by a curing or semi-curing reaction can be used. As the solvent, for example, aliphatic alcohols such as ethanol and isopropanol, ether alcohols such as 2-methoxyethanol, 1-methoxyethanol, 2-ethoxyethanol, 1-ethoxy-2-propanol, 2-butoxyethanol, 2-(2-methoxyethoxy)ethanol, 2-(2-ethoxyethoxy)ethanol, and 2-(2-butoxyethoxy)ethanol, glycol ethers such as ethylene glycol monomethyl ether and ethylene glycol monobutyl ether, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and diisobutyl ketone, and hydrocarbons such as toluene and xylene can be mentioned. Among these, one type may be contained alone, or two or more types may be contained in combination.
[0056] The impregnation is carried out by attaching the resin composition to the boron nitride sintered body. For example, the boron nitride sintered body may be immersed in the resin composition. The impregnation may be carried out under pressurized or reduced pressure conditions while immersed. In this way, the pores of the boron nitride sintered body can be filled with the resin.
[0057] The impregnation step may be performed in an impregnation device equipped with a sealed container. As an example, impregnation may be performed under reduced pressure in the impregnation device, and then the pressure in the impregnation device may be increased to a value higher than atmospheric pressure to perform impregnation under pressurized conditions. By performing both reduced pressure and pressurized conditions in this way, the pores of the boron nitride sintered body can be sufficiently filled with resin. The reduced pressure and pressurized conditions may be repeated multiple times. The impregnation step may be performed while heating. The resin composition impregnated into the pores of the boron nitride sintered body becomes a resin (cured or semi-cured) after curing or semi-curing progresses or the solvent evaporates. In this way, a composite having a boron nitride sintered body and a resin filled in its pores is obtained. It is not necessary that all the pores are filled with resin, and some pores may not be filled with resin. The boron nitride sintered body and the composite may include both closed pores and open pores.
[0058] The impregnation step may be followed by a curing step of curing the resin filled in the pores. In the curing step, for example, the composite filled with the resin is taken out of the impregnation device, and the resin is cured or semi-cured by heating and / or light irradiation depending on the type of resin (or the type of curing agent added as necessary).
[0059] The composite thus obtained has excellent thermal conductivity because the average pore size of the pores in the boron nitride sintered body is small. In addition, the pores are filled with resin, so the composite also has excellent insulating properties. The composite may be used as a heat dissipating member as it is, or may be processed into a predetermined shape to be used as a heat dissipating member.
[0060] Although several embodiments have been described above, the present disclosure is not limited to the above-described embodiments. For example, in the sintering step, the boron nitride sintered body may be obtained by hot pressing, which simultaneously performs molding and sintering. EXAMPLES
[0061] The present disclosure will be described in more detail with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.
[0062] [Boron nitride sintered body] Example 1 <Preparation of boron nitride sintered body> 100 parts by mass of orthoboric acid manufactured by Nippon Denko Co., Ltd. and 35 parts by mass of acetylene black (product name: HS100) manufactured by Denka Co., Ltd. were mixed using a Henschel mixer. The resulting mixture was filled into a graphite crucible and heated in an arc furnace in an argon atmosphere at 2200°C for 5 hours to obtain lumpy boron carbide (B4C). The resulting lumps were coarsely crushed using a jaw crusher to obtain coarse powder. This coarse powder was further crushed using a ball mill having silicon carbide balls (φ10 mm) to obtain pulverized powder. The carbon content of the obtained boron carbide powder was 19.9% by mass. The carbon content was measured using a carbon / sulfur simultaneous analyzer.
[0063] The prepared boron carbide powder was filled into a crucible made of boron nitride. The crucible was then heated for 10 hours in a resistance heating furnace under conditions of 2000°C and 0.85 MPa in a nitrogen gas atmosphere. In this way, a fired material containing boron carbonitride (B4CN4) was obtained.
[0064] A sintering aid was prepared by blending powdered boric acid and calcium carbonate. In the preparation, 2.0 parts by mass of calcium carbonate was blended with 100 parts by mass of boric acid. The atomic ratio of boron to calcium at this time was 100 atomic % of boron and 0.7 atomic % of calcium. 6 parts by mass of sintering aid was blended with 100 parts by mass of the fired product, and mixed using a Henschel mixer to obtain a powdered blend.
[0065] The compound was pressed at 150 MPa for 30 seconds using a powder press to obtain a sheet-shaped compact (length x width x thickness = 49 mm x 25 mm x 0.38 mm). The compact was placed in a boron nitride container and introduced into a batch-type high-frequency furnace. In the batch-type high-frequency furnace, it was heated for 5 hours under conditions of normal pressure, nitrogen flow rate of 5 L / min, and 2000°C. Thereafter, the boron nitride sintered body was removed from the boron nitride container. In this way, a sheet-shaped (flat) boron nitride sintered body was obtained. The thickness of the boron nitride sintered body was 0.40 mm.
[0066] <Measurement of thermal conductivity> The thermal conductivity (H) of the boron nitride sintered body in the thickness direction was calculated using the following formula (3). H=A×B×C (3)
[0067] In equation (3), H is the thermal conductivity (W / (m K)) and A is the thermal diffusivity (m 2 / sec), B is bulk density (kg / m 3 ), and C indicate the specific heat capacity (J / (kg K)). Thermal diffusivity A was measured by the laser flash method using a boron nitride sintered body processed into a sample with dimensions of length x width x thickness = 10 mm x 10 mm x 0.40 mm. The measuring device used was a xenon flash analyzer (manufactured by NETZSCH, product name: LFA447NanoFlash). Bulk density B was calculated from the volume and mass of the boron nitride sintered body. The results are shown in Table 1.
[0068] <Measurement of peak pore size and average pore size> The pore volume distribution of the obtained boron nitride sintered body was measured by using a mercury porosimeter (apparatus name: Autopore IV9500) manufactured by Shimadzu Corporation while increasing the pressure from 0.0042 MPa to 206.8 MPa. Figure 2 is a graph showing the Log differential pore volume distribution. The pore diameter at which the value obtained by dividing the differential pore volume (dV) by the logarithmic difference value d (logD) of the pore diameter was maximized was determined as the "peak pore diameter". D is the diameter when all pores are assumed to be cylindrical. Figure 5 is a graph showing the cumulative pore volume distribution. Based on the results of Figure 5, the pore diameter at which the cumulative pore volume reaches 50% of the total pore volume was determined as the "average pore diameter". The results are shown in Table 1.
[0069] <Porosity measurement> The volume and mass of the obtained boron nitride sintered body were measured, and the bulk density B (kg / m 3 ) was calculated. This bulk density and the theoretical density of boron nitride (2280 kg / m 3 The porosity was calculated from the above data using the following formula (4). The results are shown in Table 1. Porosity (volume%) = [1-(B / 2280)] x 100 (4)
[0070] <Measurement of Orientation Index> The orientation index [I(002) / I(100)] of the boron nitride sintered body was determined using an X-ray diffractometer (manufactured by Rigaku Corporation, product name: ULTIMA-IV). A measurement sample (boron nitride sintered body) set in the sample holder of the X-ray diffractometer was irradiated with X-rays and baseline correction was performed. The peak intensity ratio of the (002) and (100) planes of boron nitride was then calculated. This was taken as the orientation index [I(002) / I(100)]. The results are shown in Table 1.
[0071] <Cross-section observation using an electron microscope> The boron nitride sintered body was cut along the thickness direction using a CP polisher to obtain a cross section. This cross section was observed with a scanning electron microscope (SEM). Figure 7 is an SEM photograph (500x) showing the cross section of the boron nitride sintered body of Example 1.
[0072] Example 2 A fired product was prepared in the same manner as in Example 1. Separately, a sintering aid was prepared by blending powdered boric acid and calcium carbonate. In the preparation, the blending ratio of boric acid and calcium carbonate was changed to set the atomic ratio of boron and calcium to 100 atomic % boron and 0.6 atomic % calcium. 16 parts by mass of this sintering aid was blended with 100 parts by mass of fired product, and mixed using a Henschel mixer to obtain a powdered blend. A sheet-shaped boron nitride sintered body (thickness: 0.40 mm) was manufactured in the same manner as in Example 1, except that this blend was used.
[0073] Measurements and cross-sectional observations using an electron microscope were performed in the same manner as in Example 1. The measurement results are shown in Table 1, Figures 2 and 5. Figure 8 is an SEM photograph (500x) showing the cross section of the boron nitride sintered body of Example 2.
[0074] Example 3 A sheet-shaped boron nitride sintered body (thickness: 0.40 mm) was obtained in the same manner as in Example 2, except that the pressing pressure when obtaining the compact was increased. Measurements and cross-sectional observations using an electron microscope were performed in the same manner as in Example 2. The measurement results are as shown in Table 1, Figures 3 and 6. Figure 9 is an SEM photograph (500x) showing the cross-section of the boron nitride sintered body of Example 3.
[0075] Example 4 A fired product was prepared in the same manner as in Example 1. Separately, a sintering aid was prepared by blending powdered boric acid and calcium carbonate. In the preparation, the blending ratio of boric acid and calcium carbonate was changed to set the atomic ratio of boron and calcium to 9.2 atomic % calcium per 100 atomic % boron. 20 parts by mass of this sintering aid was blended with 100 parts by mass of fired product, and mixed using a Henschel mixer to obtain a powdered blend. A sheet-shaped boron nitride sintered body (thickness: 0.40 mm) was manufactured in the same manner as in Example 1, except that this blend was used.
[0076] Measurements and cross-sectional observations using an electron microscope were performed in the same manner as in Example 1. The measurement results are shown in Table 1, Figures 3 and 6. Figure 10 is an SEM photograph (500x) showing the cross section of the boron nitride sintered body of Example 4.
[0077] Comparative Example 1 A fired product was prepared in the same manner as in Example 1. Separately, a sintering aid was prepared by blending powdered boric acid and calcium carbonate. In the preparation, the blending ratio of boric acid and calcium carbonate was changed to set the atomic ratio of boron and calcium to 13.2 atomic % calcium relative to 100 atomic % boron. 25 parts by mass of this sintering aid was blended with 100 parts by mass of fired product, and mixed using a Henschel mixer to obtain a powdered blend. A sheet-shaped boron nitride sintered body (thickness: 0.40 mm) was manufactured in the same manner as in Example 1, except that this blend was used.
[0078] Measurements and cross-sectional observations by an electron microscope were performed in the same manner as in Example 1. The measurement results are shown in Table 1 and Figures 4 and 5. Figure 11 is an SEM photograph (500x) showing the cross section of the boron nitride sintered body of Comparative Example 1.
[0079] Comparative Example 2 9 parts by mass of amorphous boron nitride powder with an oxygen content of 2.0% and an average particle size of 3.4 μm, 13 parts by mass of hexagonal boron nitride powder with an oxygen content of 0.3% and an average particle size of 12.5 μm, 0.1 parts by mass of calcium carbonate (manufactured by Shiraishi Kogyo Co., Ltd., product name: PC-700), and 0.2 parts by mass of boric acid were mixed using a Henschel mixer. Then, 76.0 parts by mass of water were added and pulverized in a ball mill for 5 hours to obtain a water slurry. Furthermore, polyvinyl alcohol (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name: Gohsenol) was added to the water slurry so that the amount was 0.5% by mass, and the mixture was heated and stirred at 50° C. until dissolved, and then spheroidized in a spray dryer at a drying temperature of 230° C. A rotary atomizer was used as the spheroidizing device of the spray dryer.
[0080] The granulated material obtained by the spheroidizing process was pressed at 25 MPa for 30 seconds using a powder press to obtain a sheet-like molded body (length x width x thickness = 49 mm x 25 mm x 0.38 mm). The molded body was placed in a boron nitride container and introduced into a batch-type high-frequency furnace. In the batch-type high-frequency furnace, it was heated for 10 hours under conditions of normal pressure, nitrogen flow rate of 5 L / min, and 2050°C. Thereafter, the boron nitride sintered body was removed from the boron nitride container. In this way, a sheet-like (flat) boron nitride sintered body was obtained. The thickness of the boron nitride sintered body was 0.40 mm.
[0081] Measurements and cross-sectional observations using an electron microscope were performed in the same manner as in Example 1. The measurement results are shown in Table 1 and Figures 4 and 5. Figure 12 is an SEM photograph (500x) showing the cross section of the boron nitride sintered body of Comparative Example 2.
[0082] [Table 1]
[0083] [Complex] <Preparation of Complex> Resin composition containing epoxy resin (product name: Epicoat 807, manufactured by Mitsubishi Chemical Corporation) and hardener (product name: Acmex H-84B, manufactured by Nippon Synthetic Chemical Industry Co., Ltd.) Things The boron nitride sintered bodies of Examples 1 to 4 were coated with the resin composition using a bar coater under atmospheric pressure, and the boron nitride sintered bodies were impregnated with the resin composition. After impregnation, the resin was cured by heating at a temperature of 120°C for 120 minutes under atmospheric pressure to obtain a composite body. This composite body had the same thickness and thermal conductivity as the boron nitride sintered body. Therefore, it is useful as a heat dissipation member for electronic components.
[0084] <Measurement of resin content> The resin content in each composite was as shown in Table 2. The resin content (mass%) is the mass ratio of the resin to the entire composite. The resin content was measured by heating the composite to decompose and remove the resin. Specifically, the mass of the resin was calculated from the mass difference between the boron nitride sintered body and the composite after the resin was decomposed, and the resin content (mass%) was calculated by dividing the mass of the resin by the mass of the composite.
[0085] [Table 2] [Industrial Applicability]
[0086] According to the present disclosure, there are provided a boron nitride sintered body and a composite body which are thin and suitable as members for electronic components, etc., and a method for producing the same. In addition, there is provided a heat dissipation member which is suitable as a member for electronic components, etc. [Explanation of symbols]
[0087] 10...Boron nitride sintered body.
Claims
1. A boron nitride sintered body comprising boron nitride particles and pores, The average pore size of the pores is less than 2 μm, and the porosity is 30 to 65 volume %.
2. A boron nitride sintered body comprising boron nitride particles and pores, The average pore size of the pores is less than 2 μm, and the bulk density is 800 to 1500 kg / m 3 A boron nitride sintered body.
3. A boron nitride sintered body comprising boron nitride particles and pores, A boron nitride sintered body having an average pore size of less than 2 μm and a thermal conductivity of 40 W / (m·K) or more.
4. A boron nitride sintered body comprising boron nitride particles and pores, A boron nitride sintered body, wherein the pores have an average pore size of less than 2 μm and an orientation index of 40 or less.
5. A boron nitride sintered body described in any one of claims 1 to 4, wherein the average pore diameter of the pores is less than 0.6 μm.
6. The boron nitride sintered body according to any one of claims 1 to 5, which is in a sheet form and has a thickness of less than 2 mm.
7. A composite comprising the boron nitride sintered body according to any one of claims 1 to 6, and a resin filled in at least a portion of the pores of the boron nitride sintered body.
8. A heat dissipation member comprising the composite according to claim 7.
9. a nitriding step of sintering the boron carbide powder in a nitrogen atmosphere to obtain a sintered product containing boron carbonitride; and a sintering step of forming and heating a mixture containing the fired product and a sintering aid to obtain a boron nitride sintered body containing boron nitride particles and pores, The sintering aid contains a boron compound and a calcium compound, The method for producing a boron nitride sintered body, wherein the mixture contains 1 to 20 parts by mass of the boron compound and the calcium compound in total per 100 parts by mass of the fired product.
10. 10. The method for producing a boron nitride sintered body according to claim 9, wherein the average pore size of pores contained in the boron nitride sintered body obtained in the sintering step is less than 2 μm.
11. The method for producing a boron nitride sintered body according to claim 9 or 10, wherein the blend contains 0.5 to 40 atomic % of calcium constituting the calcium compound relative to 100 atomic % of boron constituting the boron compound.
12. The method for producing a boron nitride sintered body according to any one of claims 9 to 11, wherein the boron nitride sintered body obtained in the sintering step is in a sheet shape and has a thickness of less than 2 mm.
13. A method for producing a composite having a boron nitride sintered body obtained by the production method according to any one of claims 9 to 12 and a resin filled in at least a part of the pores, comprising an impregnation step of impregnating the boron nitride sintered body obtained by the production method according to any one of claims 9 to 12 with a resin composition.
Citation Information
Patent Citations
Heat conductive sheet and power module
JP2010157563A
Boron nitride molding, and production method and application of the same
JP2014162697A
Heat radiation member and its use
JP2015096456A
Boron nitride resin composite circuit board
JP2016103611A
Heat-conducting member and heat-dissipating structure including said heat-conducting member
WO2018181606A1