Silane-Based Coating Compositions Containing Metal Alkoxide Catalysts - Patent application

A silane-based coating composition with metal alkoxide catalysts addresses the need for low-temperature curing and environmental compliance in automotive coatings, providing enhanced mechanical and optical properties and humidity resistance.

JP7566898B2Active Publication Date: 2024-10-15BASF COATINGS GMBH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022528242
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-15
Filing Date
2020-11-03
Publication Date
2024-10-15
Estimated Expiration
2040-11-03

AI Technical Summary

Technical Problem

Current clearcoat compositions in the automotive industry face challenges with the use of isocyanates due to environmental regulations, requiring alternatives that cure quickly at low temperatures without using isocyanate or tin-containing catalysts, while maintaining mechanical and optical properties, and providing resistance to humidity and UV exposure.

Method used

A coating composition comprising silane-based compounds with specific alkoxysilane moieties and metal alkoxide catalysts, which cure at low temperatures without isocyanates or tin catalysts, enhancing resistance to humidity and UV exposure, and offering improved mechanical and optical properties.

Benefits of technology

The composition achieves fast curing, excellent mechanical and optical properties, and improved resistance to humidity and UV exposure, making it suitable for automotive coatings, particularly OEM and refinish applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566898000001
    Figure 0007566898000001
  • Figure 0007566898000002
    Figure 0007566898000002
  • Figure 0007566898000003
    Figure 0007566898000003
Patent Text Reader

Abstract

The present invention relates to silane-based coating compositions, particularly clearcoat compositions, containing a metal alkoxide catalyst. The present invention also relates to silane-based coating compositions, particularly clearcoat compositions, containing a silane-based compound having two different alkoxysilane moieties. The present invention also relates to a method for coating a substrate with such a coating composition, and to the coated substrate obtained by the method. Finally, the present invention relates to a multilayer coating and a substrate coated with the multilayer coating.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a silane-based coating composition, particularly a clearcoat composition, comprising a metal alkoxide catalyst. Furthermore, the present invention relates to a silane-based coating composition, particularly a clearcoat composition, comprising a silane-based compound having two different alkoxysilane moieties. Furthermore, the present invention relates to a method of coating a substrate with such a coating composition, and to a coated substrate obtained by said method. Finally, the present invention relates to a multi-layer coating and a substrate coated with said multi-layer coating. [Background technology]

[0002] In today's clearcoat industry, the application of isocyanates as crosslinkers and tin catalysts is becoming more and more desirable due to tightening regulatory classifications and maximum allowable values.

[0003] However, polyisocyanates are widely used crosslinker materials in many coating systems, especially clearcoats. Reasonable alternatives that meet future environmental, health and safety requirements, as well as technical minimum requirements, are not yet available. To increase the economic efficiency of the coating process, rapid low-temperature curing coating systems are desired.

[0004] However, coatings based solely on the condensation of alkoxysilanes often exhibit undesirable properties such as severe post-cure and brittle films that make them unsuitable as clearcoats in automotive applications, particularly in automotive repair applications, which use non-crosslinked basecoats and require custom clearcoats.

[0005] Alkoxysilane crosslinked clearcoats suitable for automotive applications in general, and repair applications in particular, are not yet available because key parameters such as fast cure, rapid sandability and finish sandability, scratch resistance, good appearance, interlayer adhesion, resistance to moisture and UV radiation cannot be fully achieved in said clearcoats so far.

[0006] EP2641925A1 discloses coating compositions containing adducts of isocyanatoalkyltrialkoxysilanes and diols. However, these adducts are used in the examples of EP2641925A1 together with a large amount of polyacrylate polyol. When used as the sole resin together with a suitable crosslinking catalyst, such as potassium neodecanoate and DBU, these adducts show relatively long tack-free times and poor crosscut adhesion even before carrying out certain weathering tests.

[0007] WO 03 / 054049 discloses isocyanate-functional silanes as adhesion promoters in polyurethane-based adhesives or coatings, but these silanes are isocyanate-containing, which should be avoided in the present invention.

[0008] Patent Document 3 (JP 2005-015644 A) describes adducts of polyisocyanates with an NCO to OH ratio of 1:0.05 to 1:0.9, i.e., with an excess of isocyanate groups, and aminosilanes. These adducts are used in curable resin compositions together with further resins. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] EP2641925A1 [Patent Document 2] WO03 / 054049 [Patent Document 3] Patent Publication No. 2005-015644 Summary of the Invention [Problem to be solved by the invention]

[0010] Therefore, what would be advantageous is a coating composition, preferably a clearcoat composition, preferably one that is free of isocyanates, that has improved resistance to humidity exposure and can be cured at low temperatures. The resulting coating should exhibit good mechanical and optical properties. Furthermore, no tin-containing catalysts should be required.

[0011] Therefore, the object of the present invention was to provide a fast curing coating composition, preferably a clear coating composition, which can be cured at low temperatures without the use of isocyanate or aminoplast crosslinkers and tin-containing catalysts. The coating composition should be particularly suitable for automotive coatings, such as automotive OEM and automotive repair coatings. The coating should have a long pot life and exhibit improved resistance to humidity exposure. The coating obtained from said coating composition should be solvent resistant and exhibit good adhesion, scratch resistance, as well as UV and weather resistance, high gloss and good appearance. [Means for solving the problem]

[0012] The above mentioned objects are achieved by the subject matter set forth in the claims and by preferred embodiments of that subject matter as set forth in the following description.

[0013] A first subject of the present invention is therefore a coating composition comprising: a) has an isocyanate content of less than 1%; At least one silane group of general formula (I) * -NR 1 X-SiR 2 a (OR 3 ) 3-a (I) Optionally at least one silane group of general formula (II) * -N[X-SiR 2 a (OR 3 ) 3-a ] n [X'-SiR 2 b (OR 3 ) 3-b ] m (II) At least one silane-based compound R1, During the ceremony, X, X' are each independently a linear and / or branched alkylene or cycloalkylene radical having 1 to 20 carbon atoms; R 1 is an alkyl group containing 1 to 10 carbon atoms, R 2 , R 3 are each independently an alkyl, cycloalkyl, aryl, or aralkyl group, and the carbon chain of the alkyl, cycloalkyl, aryl, or aralkyl group is not terminated by adjacent oxygen, sulfur, or NR a can be interrupted by a R a is alkyl, cycloalkyl, aryl, or aralkyl; n and m are each independently 0 to 2, provided that m+n=2; a, b are independently 0 to 2; b) at least one catalyst C1 of general formula (III), z[C(R 4 )(R 5 )(R 6 )-(CH2) n -C(=O)-O - ]M z+ (III) During the ceremony, R 4 ~R 6 are each independently hydrogen or an alkyl group containing 1 to 6 carbon atoms, provided that the residue R 4 ~R 6 The total number of carbon atoms is within the range of 3 to 8; z is 1 to 4; and n is 0 or 1 to 8; however, When z=1, M is selected from the group consisting of Li, K and Na; When z=2, M is selected from the group consisting of Zn and Zr; When z=3, M is selected from the group consisting of Bi and Al; When z=4, M is selected from the group consisting of Zr and Ti; c) at least one metal alkoxide C2; d) one or more aprotic organic solvents; and A coating composition comprising:

[0014] A second subject of the invention is therefore a coating composition comprising: a) has an isocyanate content of less than 1%; At least one silane group of general formula (I) * -NR 1 X-SiR 2 a (OR 3 ) 3-a (I) At least one silane group of general formula (II) * -N[X-SiR 2 a (OR 3 ) 3-a ] n [X'-SiR 2 b (OR 3 ) 3-b ] m (II) At least one silane-based compound R2, During the ceremony, X, X' are each independently a linear and / or branched alkylene or cycloalkylene radical having 1 to 20 carbon atoms; R 1 is an alkyl group containing 1 to 10 carbon atoms, R2 , R 3 are each independently an alkyl, cycloalkyl, aryl, or aralkyl group, and the carbon chain of the alkyl, cycloalkyl, aryl, or aralkyl group is not terminated by adjacent oxygen, sulfur, or NR a can be interrupted by a R a is alkyl, cycloalkyl, aryl, or aralkyl; n and m are each independently 0 to 2, provided that m+n=2; a, b are independently 0 to 2; b) at least one catalyst C1 of general formula (III), z[C(R 4 )(R 5 )(R 6 )-(CH2) n -C(=O)-O - ]M z+ (III) During the ceremony, R 4 ~R 6 are each independently hydrogen or an alkyl group containing 1 to 6 carbon atoms, provided that the residue R 4 ~R 6 The total number of carbon atoms is within the range of 3 to 8; z is 1 to 4; and n is 0 or 1 to 8; however, When z=1, M is selected from the group consisting of Li, K and Na; When z=2, M is selected from the group consisting of Zn and Zr; When z=3, M is selected from the group consisting of Bi and Al; When z=4, M is selected from the group consisting of Zr and Ti; c) one or more aprotic organic solvents; A coating composition comprising:

[0015] The above coating composition is hereinafter also referred to as the coating composition of the invention and is therefore a subject of the present invention. Preferred embodiments of the coating composition of the invention are also evident from the following description and the dependent claims.

[0016] In light of the prior art, it was surprising and unpredictable for the skilled artisan that the object on which the present invention is based can be achieved by using a specific silane-based compound R1 in combination with a specific catalyst mixture C1 and C2, or a specific silane-based compound R2 in combination with catalyst C1 in a coating composition. The use of said silane-based compound R1 or R2 in combination with a specific catalyst results in a low-cure coating composition that provides a coating layer with excellent mechanical and optical properties without the use of isocyanate and aminoplast crosslinkers and tin-containing catalysts. Thus, the coating composition of the present invention is particularly suitable for OEM repair and refinishing applications where low curing temperatures are used. The use of metal alkoxide C2 and silane-based compound R1 in combination with catalyst C1 of general formula (III) can improve the resistance of the resulting clear coat layer to humidity exposure.

[0017] A further subject of the invention is a method for forming a coating on a substrate (S), comprising the following steps: (1) applying a coating composition of the present invention onto a substrate (S); (2) forming a coating film from the coating composition applied in step (1); (3) curing the coating film formed in step (2); Includes.

[0018] Another subject of the invention is the coated substrates obtainable according to the method of the invention.

[0019] Yet another subject of the present invention is a multilayer coating comprising at least two coating layers, preferably at least one base coat layer and at least one clear coat layer, in which at least one of the coating layers, preferably the clear coat layer, is formed from a coating composition according to the invention.

[0020] A final subject of the present invention is a substrate coated with the multi-layer coating of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Detailed Description The measurement methods employed in the context of the present invention to determine certain characteristic variables can be found in the Examples section. Unless expressly indicated otherwise, these measurement methods are employed to determine the respective characteristic variables. In the context of the present invention, when reference is made to an official standard without an indication of its official validity period, the reference is implicitly to the version of the standard in force at the filing date, or to the latest valid version if no version in force at that time exists.

[0022] The term "silane-based compound" refers to a compound comprising at least one silane group of formula (I) or (II) above. The silane group is * The silane groups (I) and optionally (II) are attached to the backbone of the compound via a linker, preferably via a urea bond. As used herein, the "backbone" of a compound is the portion of the compound other than structures (I) and optionally (II). When the appropriate backbone of the compound is a polymer, the silane groups (I) and optionally (II) may be pendant from the polymer chain, incorporated into the polymer chain, or a combination thereof.

[0023] The term "poly(meth)acrylate" refers to both polyacrylates and polymethacrylates. Poly(meth)acrylates may therefore be composed of acrylates and / or methacrylates and may further comprise ethylenically unsaturated monomers such as styrene or acrylic acid.

[0024] As used herein, the term "aliphatic" includes the term "alicyclic," each of which refers to non-aromatic groups, moieties, and compounds.

[0025] All film thicknesses reported in the context of the present invention should be understood as dry film thicknesses. In each case, therefore, it is the thickness of the cured film. Thus, when a coating material is reported to be applied at a specific film thickness, this means that the coating material is applied in such a way that it will have the stated film thickness after curing.

[0026] All temperatures resolved in the context of the present invention should be understood as the temperature of the room in which the substrate or coated substrate is located, and therefore do not imply that the substrate itself must have the temperature in question.

[0027] The coating composition of the present invention: Each coating composition of the present invention comprises at least one aprotic solvent, and is therefore preferably a solvent-based coating composition.In the context of the present invention, a solvent-based coating composition preferably comprises a total amount of water and / or protic solvent of less than 10% by weight, preferably less than 5% by weight, more preferably less than 1% by weight, very preferably 0% by weight, in each case based on the total weight of the coating composition.

[0028] A coating composition according to the invention comprising a silane-based compound R1 and a catalyst mixture C1 and C2:

[0029] Silane-based compounds R1(a) The coating composition of the present invention comprises as a first essential component (a) a silane having an isocyanate content (hereinafter also referred to as NCO content) of less than 1% and at least one silane group of general formula (I): * -NR 1 X-SiR 2 a (OR 3 ) 3-a(I) Optionally at least one silane group of general formula (II) * -N[X-SiR 2 a (OR 3 ) 3-a ] n [X'-SiR 2 b (OR 3 ) 3-b ] m (II) and a silane-based compound R1 comprising During the ceremony, R 1 ~R 3 , X, X', a, b, m and n are as defined above. The silane groups of formulae (I) and (II) are as defined above: * It is attached to the backbone of the silane-based compound R1 via the symbol.

[0030] The silane-based compound R1 preferably contains an isocyanate content of less than 0.5%, more preferably between 0.05 and 0%, ensuring that the silane-based compound R1 contains only a fairly small amount of free NCO groups or is essentially free of NCO groups, thereby allowing the compound to be used in isocyanate-free coating compositions.

[0031] The reactivity of the organofunctional silanes can be significantly influenced by the length of the spacer X, X' between the silane functional group and the organofunctional group serving for reaction with the backbone of the silane-based compound R1. X and X' in the general formulae (I) and (II) preferably represent, independently of one another, a linear alkylene radical having 1 to 10, more preferably 1 to 6, even more preferably 2 to 5 and very preferably 3 carbon atoms.

[0032] R in general formula (I) 1 is preferably an alkyl group containing from 2 to 8 carbon atoms, more preferably from 4 to 6 carbon atoms, and most preferably 4 carbon atoms.

[0033] Each preferred alkoxy radical (OR 3 ) influences the reactivity of the hydrolyzable silane group. Particularly preferred are radicals R which increase the reactivity of the silane group, i.e. which constitute good leaving groups. 3 Thus, the methoxy radical is preferred to the ethoxy radical, which in turn is preferred to the propoxy radical. Particular preference is therefore given to R 3 are independent of each other, C1 to C 10 It represents an alkyl group, more preferably a C1 to C6 alkyl group, and most preferably a C1 alkyl group.

[0034] The silane group of general formula (II) contains two alkoxysilane moieties, so the sum of n and m is 2. Each alkoxysilane moiety may be the same or different from each other. In the case of different alkoxysilane moieties, if m=n=1, then R 3 and R 4 are different. For the same alkoxysilane moiety, R 3 and R 4 are the same and m=n=1, or m=0 and n=2 or vice versa.

[0035] The preferred silane groups of general formula (I) and, when present, of general formula (II) each contain three alkoxy moieties, and therefore a in formulas (I) and (II) and b in formula (II) are preferably, independently of each other, 0.

[0036] The silane-based compound R1(a) is a compound which comprises at least one polyisocyanate, General formula (Ia) HNR 1 -X-SiR 2 a (OR 3 ) 3-a (Ia) and at least one compound of Optionally, the general formula (IIa) HN[X-SiR 2 a(OR 3 ) 3-a ] n [X'-SiR 2 b (OR 3 ) 3-b ] m (IIa) and at least one compound of It can be prepared by reacting

[0037] R in general formula (Ia) and (IIa) 1 ~R 3 , X, X', a, b, m and n are as defined above.

[0038] In principle, all aliphatic, cycloaliphatic, araliphatic and aromatic polyisocyanates can be used as polyisocyanates. Examples of polyisocyanates that are preferably used are: 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, diphenylmethane 4,4'-diisocyanate, diphenylmethane 2,4'-diisocyanate, p-phenylene diisocyanate, biphenyl diisocyanate, 3,3'-dimethyl-4,4'-diphenyl diisocyanate, tetramethylene 1,4-diisocyanate, hexamethylene 1,6-diisocyanate, 2,2,4-trimethylhexane 1,6-diisocyanate, isophorone diisocyanate, ethylene ... diisocyanate, 1,12-dodecane diisocyanate, cyclobutane 1,3-diisocyanate, cyclohexane 1,3-diisocyanate, cyclohexane 1,4-diisocyanate, methylcyclohexyl diisocyanate, hexahydrotoluene 2,4-diisocyanate, hexahydrotoluene 2,6-diisocyanate, hexahydrophenylene 1,3-diisocyanate, hexahydrophenylene 1,4-diisocyanate, perhydrodiphenylmethane 2,4'-diisocyanate, 4,4'-methylenedicyclohexyl diisocyanate (e.g. Desmodur® W from Covestro AG), tetramethylxylyl diisocyanate (e.g. TMXDI® from American Cyanamid), and mixtures of the aforementioned polyisocyanates. Further preferred polyisocyanates are those derived from polyisocyanates by trimerization, dimerization, urethanization, biuretization or allophanation. Particularly preferred polyisocyanates are hexamethylene diisocyanate urethione, hexamethylene diisocyanate, 1-isocyanato-4-[(4-isocyanatocyclohexyl)-methyl]-cyclohexane and hexamethylene diisocyanate trimer.

[0039] Inventively preferred compounds (Ia) are aminoalkyltrialkoxysilanes, for example and preferably 2-aminoethyltrimethoxysilane, 2-aminoethyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 4-aminobutyltrimethoxysilane, 4-aminobutyltriethoxysilane. Particularly preferred compounds (Ia) are N-(2-(trimethoxysilyl)ethyl)alkylamines, N-(3-(trimethoxysilyl)propyl)alkylamines, N-(4-(trimethoxysilyl)butyl)alkylamines, N-(2-(triethoxysilyl)ethyl)alkylamines, N-(3-(triethoxysilyl)-propyl)alkylamines and / or N-(4-(triethoxysilyl)butyl)alkylamines. Particularly preferred aminosilanes of formula (Ia) are α-aminosilanes (X=CH2) and γ-aminosilanes (X=n-propyl), with γ-aminosilanes being the most preferred in the present invention. Particularly preferred are N-alkylamino-alkyl-trialkoxysilanes, among which n-alkylamino-propyltrimethoxysilanes, such as n-butylamino-propyl-trimethoxysilane, are the most preferred. Aminosilanes of this type are available, for example, under the trade names DYNASYLAN® from DEGUSSA or Silquest® from Momentive.

[0040] Preferred compounds (IIa) are bis(2-ethyltrimethoxysilyl)amine, bis(3propyltrimethoxysilyl)amine, bis(4-butyltrimethoxysilyl)amine, bis(2ethyltriethoxysilyl)amine, bis(3-propyltriethoxysilyl)amine and / or bis(4butyltrimethoxysilyl)amine. Highly preferred is bis(3propyltrimethoxysilyl)amine.

[0041] Preferred compounds (IIa) are available, for example, under the trade names DYNASILAN® from DEGUSSA or Silquest® from Momentive.

[0042] The reaction of the at least one polyisocyanate with the compound of general formula (Ia) and optionally the compound of general formula (IIa) can be carried out without a solvent or in the presence of an aprotic solvent until essentially all, preferably all, of the free isocyanate groups of the at least one polyisocyanate are consumed. The reaction is preferably carried out in an inert gas at a temperature below 100° C., preferably below 60° C.

[0043] According to the invention, it is preferred that the silane-based compound R1 contains in each case 50-100 mol %, preferably 80-100 mol %, more preferably 95-100 mol %, of at least one silane group of general formula (I) and 0-50 mol %, preferably 0-20 mol %, more preferably 0-5 mol %, of at least one silane group of general formula (II), based on the total silane groups of general formulas (I) and (II). It has been found that in particular the ratio of silane groups of general formula (I) to silane groups of general formula (II) has a very significant influence on the occurrence of cracks in the resulting coating. In this context, generally speaking, the occurrence of cracks in the resulting coating increases as the proportion of monosilane groups of general formula (I) decreases and as the proportion of bissilane groups of general formula (II) increases. Thus, particularly preferred silane-based compounds R1 contain 100 mol % of silane groups of general formula (I) and 0 mol % of silane groups of general formula (II).

[0044] What is very surprising and very advantageous is the fact that an increase in the proportion of monosilane groups of general formula (I) and a decrease in the proportion of bissilane groups of general formula (II) reduces the occurrence of cracks while at the same time only slightly decreasing the scratch resistance of the resulting coating.

[0045] The silane-based compound R1 is preferably present in a total amount of 25 to 95% by weight, more preferably 35 to 90% by weight, and most preferably 40 to 80% by weight, in each case based on the total weight of the coating composition. The amount of this silane-based compound R1 employed in the coating composition is the calculated theoretical amount of silane-based compound R1, based on the condition that the sum of the masses of the reactants employed in the preparation of the silane-based compound R1 is equal to the final mass of the silane-based compound R1. Catalyst C1 of general formula (III)(b): The coating composition of the present invention comprises, as a second essential component (b), at least one catalyst C1 of general formula (III), z[C(R 4 )(R 5 )(R 6 )-(CH2) n -C(=O)-O - ]M z+ (III) During the ceremony, R 4 ~R 6 are each independently hydrogen or an alkyl group containing 1 to 6 carbon atoms, provided that the residue R 4 ~R 6 the total number of carbon atoms is within the range of 3 to 8; z is 1 to 4; and n is 0 or 1 to 8 (however, When z=1, M is selected from the group consisting of Li, K and Na; When z=2, M is selected from the group consisting of Zn and Zr; When z=3, M is selected from the group consisting of Bi and Al; When z=4, M is selected from the group consisting of Zr and Ti).

[0046] Residue R in general formula (III) 4 ~R 6 The sum of the numbers of carbon atoms is preferably 3 to 5 or 5 to 8.

[0047] In formula (III), z is preferably 1, 3 or 4, and more preferably 1 or 4.

[0048] In the general formula (III), n is preferably 0 or 2 to 6, and more preferably 0 or 4. When n is 0, the residue R 4 and R 5 are each independently a linear or branched C3-C5 alkyl group, and the residue R 6 is a methyl group (whereas residue R 4 ~R 6 The sum of all carbon atoms in the formula (III) is 8. When n in the formula (III) is 1 to 8, preferably 4, the residue R 4 ~R 6 are each independently a methyl group.

[0049] M in the general formula (III) is preferably potassium, lithium or titanium, and more preferably potassium or titanium.

[0050] Particularly preferred catalysts C1 of general formula (III) are potassium, lithium or titanium neodecanoates and / or ethylhexanoates, preferably potassium(I) neodecanoate, potassium(I) 2-ethylhexanoate, titanium(IV) neodecanoate or titanium(IV) 2-ethylhexanoate. Very preferably, exactly one catalyst C1, particularly preferably potassium(I) neodecanoate, titanium(IV) neodecanoate or titanium(IV) 2-ethylhexanoate, is contained in the coating composition of the invention. The use of titanium(IV) 2-ethylhexanoate is particularly preferred, since the resulting coating layer shows a significantly improved appearance.

[0051] In many cases, catalysts C1 of formula (III) are supplied by the manufacturer in an acid-stabilized form. It is preferable to use such acid-stabilized catalysts C1 of formula (III) not only because of their higher storage stability, but also because they introduce free acids into the coating composition according to the invention. Such free acids are known to be beneficial in combination with catalysts C2 and can further improve silane hydrolysis and thus network formation. The stabilizing acids are generally protonated residues C(R 4 )(R 5 )(R 6 )-(CH2) n -C(=O)-OH. The catalyst C1 is supplied in the form of a stabilizing acid C(R 4 )(R 5 )(R 6 )-(CH2) n When it contains --C(.dbd.O)--OH, the content of this acid is included in the carboxylic acid of formula (IV) as described below.

[0052] The amount of the at least one catalyst C1, in particular potassium neodecanoate or titanium neodecanoate, is preferably in the range from 1 mmol to 50 mmol, more preferably from 5 mmol to 40 mmol, most preferably from 15 to 25 mmol metal in each case, based on 100 g of silane-based compound R1 solid. Metal alkoxide C2(c): The coating composition of the present invention comprises, as a third essential component (c), at least one metal alkoxide, which is used as a cocatalyst, resulting in improved resistance to humidity conditions compared to compositions containing a nitrogen compound such as DBU as a cocatalyst (in combination with catalyst C1, preferably potassium neodecanoate or titanium neodecanoate). Without wishing to be bound by a particular theory, it is believed that the titanium alkoxide acts to convert the silane-based compound R into a nitrogen compound during curing. 1 It is believed that it can participate in the condensation reaction of

[0053] The at least one metal alkoxide C2 is preferably selected from metal alkoxides of general formula (IV) M 1 [(OR 7 ) m (R 8 ) n-m ] n (IV) During the ceremony, R 7 is a linear or branched C1-C 10 is an alkyl group of the formula R 8 is a halogen group, an acetylacetonate group, an alkylacetoacetate group, or an ethanolaminato group, M 1 represents at least one metal selected from silicon, titanium, tantalum, zirconium, boron, aluminum, magnesium, and zinc; m is an integer from 0 to 4; n is M 1 Represents atomic valences of 2 to 5.

[0054] R in general formula (IV) 7 is preferably selected from C3 to C5 alkyl groups, more preferably C3 or C4 alkyl groups.

[0055] R in general formula (IV) 8 is preferably an alkyl acetoacetate group, more preferably an ethyl acetoacetate group.

[0056] In the general formula (IV), m is preferably 0 or 1 to 4, more preferably 0 or 2 to 4, and most preferably 0, 2 or 4.

[0057] M in formula (IV) 1 is a metal preferably chosen from titanium and n represents a valence of 4.

[0058] Particularly preferred catalysts C2 are selected from titanium(IV) isopropoxide and / or titanium(IV) n-butoxide and / or titanium(IV) bis(ethylacetoacetate)diisopropoxide.

[0059] The at least one metal alkoxide C2, preferably a metal alkoxide of the general formula (III), is preferably present in a total amount of in each case 2.5 to 40 mmol metal, based on 100 g of silane-based compound R1 solid.

[0060] The metal to metal ratio of catalyst C1 of general formula (II) to at least one metal alkoxide C2, preferably a metal alkoxide of general formula (III), is preferably 1:2 to 2:1. The use of said catalyst mixture in the above ratios results in improved humidity resistance and thus significantly reduces blistering and whitening of the cured coating layer obtained from the coating composition of the present invention after exposure to humidity conditions, compared to a cured coating layer prepared using a nitrogen-containing cocatalyst, e.g. DBU, instead of metal alkoxide C2.

[0061] Aprotic Solvents (d): The coating composition of the present invention is a solvent-based coating composition, and therefore contains at least one aprotic solvent as the fourth essential component (d). The aprotic solvent in the coating composition is chemically inert to the silane-based compound R1, i.e., does not react with the silane-based compound R1 during storage and curing of the coating composition of the present invention.

[0062] Suitable aprotic solvents are selected from aliphatic and / or aromatic hydrocarbons, such as toluene, xylene, solvent naphtha, Solvesso 100 or Hydrosol® (APAL), ketones, such as acetone, methyl ethyl ketone or methyl amyl ketone, esters, such as ethyl acetate, butyl acetate, pentyl acetate or ethyl ethoxypropionate, ethers or mixtures of said solvents. The aprotic solvent or solvent mixtures preferably have a water content of less than or equal to 1% by weight, more preferably less than or equal to 0.5% by weight, based on the solvent. However, some of the additives or catalysts used herein are sold in protic organic solvents and therefore, in some cases, the introduction of some undesirable protic solvents cannot be avoided unless a solvent exchange is carried out before use. If the amount of such protic solvents is kept within the above limits, such an amount can usually be neglected. If undesirable premature crosslinking occurs, for example, due to the presence of protic solvents introduced by additives, such additives are preferably introduced into the coating composition immediately before application of the coating composition. Another possibility is to carry out a solvent exchange.

[0063] As mentioned above, the coating composition of the present invention preferably comprises water and / or protic solvents in an amount of less than 10% by weight, preferably less than 5% by weight, more preferably less than 1% by weight, very preferably 0% by weight, in each case based on the total weight of the coating composition. Since the silane-based compound R1 reacts with water and protic solvents, said solvents are preferably absent in order to maximize the pot life and storage stability of the coating composition of the present invention.

[0064] The aprotic solvent is typically introduced by using a solution or dispersion of the silane-based compound R1 in an aprotic solvent or a mixture of aprotic solvents. A further amount is introduced to adjust the viscosity of the coating composition to a suitable application viscosity. The at least one aprotic solvent is preferably present in a total amount of 1 to 70% by weight, more preferably 20 to 60% by weight, most preferably 30 to 50% by weight, in each case based on the total weight of the coating composition.

[0065] A coating composition according to the invention comprising a silane-based compound R2 and a catalyst C1: Silane-based compounds R2(a): The coating composition of the present invention has, as a first essential component (a), an isocyanate content (hereinafter also referred to as NCO content) of less than 1%, a silane-based compound R2 containing at least one silane group of general formula (I) * -NR 1 X-SiR 2 a (OR 3 ) 3-a (I) At least one silane group of general formula (II): * -N[X-SiR 2 a (OR 3 ) 3-a ] n [X'-SiR 2 b (OR 3 ) 3-b ] m (II) During the ceremony, R 1 ~R 3 , X, X', a, b, m and n are as defined above. The silane groups of formulae (I) and (II) are as defined above: * It is attached to the backbone of the silane-based compound R2 via the symbol.

[0066] According to the invention, it is preferred if the silane-based compound R2 contains, in each case based on the total of the silane groups of the general formulas (I) 50-99.9 mol %, preferably 80-99.9 mol %, more preferably 95-99.9 mol %, of at least one silane group of the general formula (I) and 0.01-50 mol %, preferably 0.01-20 mol %, more preferably 0.01-5 mol %, of at least one silane group of the general formula (II). It has been found that an increase in the proportion of bis-silane groups, especially of the general formula (II), leads to the formation of cracks in the respective coating layer. Particularly preferred silane-based compounds R2 therefore contain only a fairly small amount of silane groups of the general formula (II).

[0067] For further preferred embodiments of the silane-based compound R2 and the amount of the silane-based compound R2 in the coating composition, see silane-based compound R1 above.

[0068] Catalyst C1 of general formula (III)(b): The coating composition of the present invention comprises, as a second essential component (b), at least one catalyst C1 of general formula (III), z[C(R 4 )(R 5 )(R 6 )-(CH2) n -C(=O)-O - ]M z+ (III) In the formula, R 4 ~R 6 , z and n are as defined above.

[0069] For further preferred embodiments of the catalyst C1 of general formula (III), see the above catalyst C1 of general formula (III).

[0070] Aprotic Solvents (c): The coating composition of the present invention is a solvent-based coating composition and therefore comprises at least one aprotic solvent as the fourth essential component (c). For further preferred embodiments of the aprotic solvent, see the aprotic solvents mentioned above.

[0071] Further optional components of the coating composition of the present invention: Carboxylic acids of general formula (V): The coating composition of the present invention may further comprise at least one carboxylic acid of general formula (V): C(R 4 )(R 5 )(R 6 )-(CH2) n -C(=O)-OH (V) During the ceremony, R 4 ~R 6 are each independently hydrogen or an alkyl group containing 1 to 6 carbon atoms, provided that the residue R 4 ~R 6 the total number of carbon atoms is within the range of 3 to 8, preferably 5 to 8; n is 0 or 1 to 8, and preferably 0 or 4.

[0072] Particularly preferred carboxylic acids of general formula (V) are the free carboxylic acids corresponding to the carboxylate anions of the catalysts of general formula (III), which are introduced into the coating compositions of the invention using the aforementioned catalysts C1 stabilized by said carboxylic acids.

[0073] A particularly preferred carboxylic acid of general formula (V) is neodecanoic acid.

[0074] The at least one carboxylic acid of general formula (V), preferably neodecanoic acid, is present in a total amount of preferably 0 to 80% by weight, more preferably 30 to 70% by weight and very preferably 50 to 60% by weight, in each case based on the total amount of catalyst C1 of general formula (III).

[0075] Epoxy-functional compounds of general formula (VI): The coating composition of the present invention may further comprise at least one epoxy-functional compound of general formula (VI): (X) n -R 9 -Ox (VI) During the ceremony, Ox is an oxirane group; R 9 is an aliphatic hydrocarbyl group containing 2 to 15 carbon atoms and optionally containing ether and / or ester groups; n is 1 to 5; and X is independently Ox or * -Si(R g ) 3-v (R h ) v The group (v is 0 or 1, R g is an alkoxy group containing 1 to 4 carbon atoms, R h is an alkyl group containing 1 to 4 carbon atoms, or an alkoxy group containing 1 to 4 carbon atoms.

[0076] R in general formula (VI) 9 is an aliphatic hydrocarbyl group * -(CH2)3-O-CH2- # or a cyclohexylethyl group. * is an aliphatic hydrocarbyl group * -(CH2)3-O-CH2- # to the X residue, and the symbol # is a hydrocarbyl group * -(CH2)3-O-CH2- # to the oxirane group. Thus, the aliphatic hydrocarbyl group * -(CH2)3-O-CH2- # R 9 The structure of the epoxy functional compound of general formula (VI) obtained from the above is (X) n -(CH2)3-O-CH2-Ox.

[0077] In the general formula (VI), n is preferably 1.

[0078] When the X group is an oxirane group, the compound of general formula (VI) is an aliphatic diglycidyl ether, an aliphatic polyglycidyl ether, an aliphatic diglycidyl ester and / or an aliphatic polyglycidyl ester.

[0079] Examples of aliphatic diglycidyl ethers or polyglycidyl ethers are 1,4-butanediol diglycidyl ether (Heloxy 67), 1,6-hexanediol diglycidyl ether (Heloxymodifier HD), trimethylolpropane triglycidyl ether (Heloxy 48), and neopentyl glycol diglycidyl ether (Heloxy 68), hydrogenated bisphenol A diglycidyl ether (sold, for example, under the trade names Epalloy 5000 and Epalloy 5001 from CVC Specialty Chemicals; or YX8000 from Japanese Epoxy Resins), cyclohexanedimethylol diglycidyl ether (sold, for example, under the trade name Heloxy from Hexion), 107), tricyclodecane dimethanol diglycidyl ether (for example, sold under the trade name EP4088S by Adeka), and a compound synthesized from 2,2-bis(hydroxymethyl)-1,3-propanediol and 2-(chloromethyl)oxirane (Basocoll OV) or glycerol diglycidyl ether.

[0080] Examples of aliphatic diglycidyl or polyglycidyl esters are the glycidyl ester of linoleic acid dimer (e.g., sold under the trade name Erisys GS-120 by CVC Specialty Chemicals), dimer acid diglycidyl ester (e.g., sold under the trade name Heloxy Modifier 71 by Hexion), and diglycidyl 1,2-cyclohexanedicarboxylate (e.g., sold under the trade name Epaloy 5200 by CVC Specialty Chemicals).

[0081] At least one of the X groups is -Si(R g ) 3-v (R h ) v When X is a group, the compound of general formula (VI) is an epoxy silane. According to a preferred embodiment of the coating composition of the present invention, the epoxy-functional compound of general formula (VI) is an epoxy silane. X in general formula (VI) is therefore preferably * -Si(R g ) 3-v (R h ) v group, where v is 0 or 1, and R g is an alkoxy group containing 1 to 4 carbon atoms, R h is an alkoxy group containing one carbon atom or an alkyl group containing one carbon atom.

[0082] Particularly preferred epoxy compounds of the general formula (VI) are (3-glycidoxypropyl) trimethoxysilane, dimethoxy(3-glycidyloxypropyl)methylsilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, trimethylolpropane triglycidyl ether, triglycidylether, and the reaction product of 2,2-bis(hydroxymethyl)-1,3-propanediol with 2-(chloromethyl)oxirane, very preferably (3-glycidoxypropyl)trimethoxysilane, trimethylolpropane triglycidyl ether, and the reaction product of 2,2-bis(hydroxymethyl)-1,3-propanediol with 2-(chloromethyl)oxirane.

[0083] The at least one epoxy-functional compound of general formula (VI) is preferably present in a total amount of 0 to 20% by weight, more preferably 2.5 to 15% by weight and most preferably 5 to 10% by weight, in each case based on the solids content of the coating composition.

[0084] Further additives: The coating composition of the invention may further comprise at least one customary and well-known coating additive in a typical amount, i.e. preferably in an amount of 0 to 20% by weight, more preferably 0.005 to 15% by weight, in particular 0.01 to 10% by weight, in each case based on the total weight of the coating composition. The aforementioned weight percentage ranges apply analogously to the sum of all additives.

[0085] Examples of suitable coating additives are (i) UV absorbers; (ii) light stabilizers, such as HALS compounds, benzotriazoles or oxalanilides; (iii) rheology modifiers, such as sag control agents (urea crystal modified resins), organic thickeners and inorganic thickeners; (iv) free radical scavengers; (v) slip additives; (vi) polymerization inhibitors; (vii) defoamers; (viii) wetting agents; (ix) fluorine compounds; (x) adhesion promoters; (xi) leveling agents; (xii) film forming aids, such as cellulose derivatives; (xiii) fillers, such as nanoparticles based on silica, alumina or zirconium oxide; (xiv) flame retardants; and (xv) mixtures thereof.

[0086] Of the above additives, the most preferred additives are UV absorbers, preferably present in an amount of 0.25-2.5 wt%, light stabilizers, preferably present in an amount of 0.25-2.5 wt%, and leveling agents, preferably present in an amount of 0.005-2.5 wt%, the ranges being based on the total weight of the coating composition.

[0087] It is possible, but not desirable, for the coating composition to further comprise at least one further binder different from the silane-based compounds R1 and R2 and the epoxy-functional compound of formula (VI). In the context of the present invention and according to DIN EN ISO 4618:2007-03, a "binder" is a non-volatile component of the coating composition, free of pigments and fillers. However, in the following, this expression is mainly used in the context of certain physically curable polymers, which may also be optionally thermosetting, for example polyurethanes, polyesters, polyethers, polyureas, polyacrylates, polysiloxanes and / or copolymers of the mentioned polymers. Copolymers in the context of the present invention refer to polymer particles formed from different polymers. This explicitly includes both polymers that are covalently bonded to each other and those in which different polymers are bonded to each other by adhesion. Combinations of the two types of bonds are also covered by this definition.

[0088] However, if present, such binders are preferably contained in the coating composition according to the invention in an amount of less than 10% by weight, more preferably less than 5% by weight, based on the total weight of the silane-based compounds R1 or R2 present in the coating composition according to the invention. Most preferably, the coating composition according to the invention does not comprise at least one further binder, in particular a hydroxy-functional polysiloxane and / or an alkoxy-functional polysiloxane, i.e. said further binder is present in an amount of 0% by weight, based on the total weight of the silane-based compounds R1 or R2.

[0089] The additive may include a further catalyst C3 different from the aforementioned catalysts C1 and C2. The further catalyst C3 is preferably included in the coating composition comprising the silane-based compound R2 and the catalyst C1. Suitable further catalysts C3 are, for example, bicyclic tertiary amines. Most preferred bicyclic tertiary amines are 1,5-diaza-bicyclo[4.3.0]non-5-ene (hereinafter referred to as DBN), 1,5-diaza-bicyclo(4,4,0)decene-5 (hereinafter referred to as DBD) or 1,8-diaza-bicyclo[5,4,0]undec-7-ene (hereinafter referred to as DBU) and 1,4-diazabicyclo[2,2.2]octane (hereinafter referred to as DABCO). Among them, DBU and DBN are preferred. Particularly preferred is DBU. Such bicyclic tertiary amines may be used alone or in combination of two or more of them. The use of such a further catalyst C3 in a coating composition comprising a silane-based compound R2 results in improved adhesion compared to the use of catalyst C1 alone. Therefore, the combination of catalyst C1 with a further co-catalyst C3, preferably DBU, is usually preferred in coating compositions comprising a silane-based compound R2.

[0090] When said further catalyst, preferably DBU, is present, the mass ratio of catalyst C1 to further catalyst C3 is preferably 1:1 to 8:1, more preferably 2:1 to 6:1, most preferably 3:1 to 5:1, for example 4:1.

[0091] The coating composition of the present invention can be formulated as a tinted clearcoat composition, which, when applied to a substrate, is neither completely transparent and colorless as a clearcoat, nor completely opaque as a typical pigmented coating. Thus, a tinted clearcoat is transparent and colored or semi-transparent and colored. Coloring can be achieved by adding at least one pigment commonly used in coating compositions. Suitable pigments are, for example, organic and inorganic color pigments, effect pigments and mixtures thereof. Such color pigments and effect pigments are known to those skilled in the art and are described, for example, in Roempp-Lexikon Lacke und Druckfarben, Georg Thieme Verlag, Stuttgart, New York, 1998, pages 176 and 451. The terms "coloring pigment" and "color pigment" are interchangeable, as are the terms "visual effect pigment" and "effect pigment". Suitable inorganic colour pigments are selected from (i) white pigments such as titanium dioxide, white zinc, coloured zinc oxide, zinc sulphide, lithopone; (ii) black pigments such as iron oxide black, iron manganese black, spinel black, carbon black; (iii) colour pigments such as ultramarine green, ultramarine blue, manganese blue, ultramarine violet, manganese violet, iron oxide red, molybdenum red, ultramarine red, iron oxide brown, mixed brown, spinel and corundum phases, iron oxide yellow, bismuth vanadate; (iv) filler pigments such as silicon dioxide, quartz flour, aluminium oxide, aluminium hydroxide, natural mica, natural and precipitated chalk, barium sulphate, and (vi) mixtures thereof.

[0092] Suitable organic colored pigments are (i) monoazo pigments, such as CI Pigment Brown 25, CI Pigment Orange 5, 36 and 67, CI Pigment Orange 5, 36 and 67, CI Pigment Red 3, 48:2, 48:3, 48:4, 52:2, 63, 112 and 170 and CI Pigment Yellow 3, 74, 151 and 183; (ii) diazo pigments, such as CI Pigment Red 144, 166, 214 and 242, CI Pigment Red 144, 166, 214 and 242 and CI Pigment Yellow 83; (ii) anthraquinone pigments, such as CI Pigment Yellow 147 and 177, CI Pigment Violet 31; (iv) benzimidazole pigments, such as CI Pigment Orange 64; (v) quinacridone pigments, such as CI Pigment Orange 48 and 49, CI Pigment Red 122, 202 and 206 and CI Pigment Violet 19; (vi) quinophthalone pigments, such as CI Pigment Yellow 138; (vii) diketopyrrolopyrrole pigments, such as CI Pigment Orange 71 and 73 and CI Pigment Violet 19; (viii) dioxazine pigments, such as CI Pigment Violet 23 and 37; (ix) indanthrone pigments, such as CI Pigment Blue 60; (x) isoindoline pigments, such as CI Pigment Yellow 139 and 185; (xi) isoindolinone pigments, such as CI Pigment Orange 61 and CI Pigment Yellow 109 and 110; (xii) metal complex pigments, such as CI Pigment Yellow 153; (xiii) perinone pigments, such as CI Pigment Orange 43; (xiv) perylene pigments, such as CI Pigment Black 32, CI Pigment Red 149, 178 and 179, CI Pigment Violet 29; (xv) phthalocyanine pigments, such as CI Pigment Violet 29, Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, 15:6 and 16, and CI Pigment Green 7 and 36; (xvi) aniline blacks, such as CI Pigment Black 1; (xvii) azomethine pigments; and (xviii) mixtures thereof.

[0093] Suitable effect pigments may be selected from the group consisting of: (i) plate-shaped metallic effect pigments, such as plate-shaped aluminum pigments, gold bronzes, flame bronze, iron oxide-aluminum pigments; (ii) pearlescent pigments, such as metal oxide mica pigments; (iii) plate-shaped graphite pigments; (iv) plate-shaped iron oxide pigments; (v) multilayer effect pigments from PVD films; (vi) liquid crystal polymer pigments; and (vii) mixtures thereof.

[0094] The coating composition preferably comprises at least one colour and / or effect pigment in a total amount of 0.1 to 10% by weight, preferably 1 to 4% by weight, based on the total weight of the coating composition.

[0095] If the coating compositions of the invention are formulated as clearcoat compositions, they preferably do not contain color and / or effect pigments, i.e. the amount of color and / or effect pigments is preferably 0% by weight, based on the total weight of the coating composition. However, it is likewise possible to add filler materials and matting agents to adjust the gloss of the clearcoat material.

[0096] The coating composition of the present invention preferably comprises only a fairly small amount of crosslinking agent, and very preferably does not comprise any crosslinking agent conventionally used in coating compositions.Thus, the coating composition preferably comprises a total of less than 2% by weight, more preferably 0% by weight, of at least one crosslinking agent and / or tin-containing compound, based on the total weight of the coating composition.

[0097] The crosslinking agents, which are preferably present in the coating composition in small amounts or not at all, are amino resins, polyisocyanates, blocked polyisocyanates, polycarbodiimides, photoinitiators, and mixtures thereof.The tin-containing compounds, which are preferably not present, are tin catalysts.The combination of silane-based compound R1 with the mixture of catalysts C1 and C2, or the combination of silane-based compound R2 with catalyst C1, provides sufficient crosslinking at low curing temperatures without the use of polyisocyanates or melamine resins, and tin-containing compounds, which are not preferred from an ecological point of view.

[0098] The coating composition of the present invention may be a one-component or two-component coating composition. When the coating composition of the present invention is formulated as a one-component composition, traces of water need to be removed to avoid crosslinking reactions during storage of the coating composition. Preferably, the coating composition of the present invention is formulated as a two-component coating composition. The two-component coating composition preferably comprises the silane-based compound R1 or R2 (optionally diluted with an aprotic solvent) and, if present, the optional epoxy-functional compound of general formula (VI) in a first container, the catalysts C1 and C2 or C1 and optionally C3, optionally at least one coating additive and at least an aprotic solvent in a second container. The components of containers 1 and 2 are then mixed before use. Formulating the coating composition of the present invention as a two-component composition provides a higher storage stability since there is no need to remove traces of water.

[0099] The method of the present invention: The present invention also relates to a method of coating a substrate with the coating composition of the present invention, in which the coating composition of the present invention is applied onto a substrate to form a coating film, and then the coating film is cured.

[0100] According to a first alternative, the substrate (S) is preferably selected from metal substrates, metal substrates coated with a cured electrocoat and / or a cured filler, plastic substrates and substrates comprising metal and plastic components, particularly preferably from metal substrates. In the case of metal and plastic substrates or substrates comprising metal and plastic components, said substrate may be pretreated before step (1) of the method of the invention in any conventional manner, i.e. for example by cleaning (for example mechanically and / or chemically) and / or by known conversion coatings (for example by phosphating and / or chromating) or surface activation pretreatments (for example by flame treatment, plasma treatment and corona discharge).

[0101] In this respect, preferred metal substrates (S) are selected from iron, aluminum, copper, zinc, magnesium and their alloys, and steel.Preferred substrates are iron and steel substrates, for example typical iron and steel substrates as used in the automotive industry.The substrate itself may be of any shape, i.e., for example, a simple metal panel or a complex part, such as, in particular, the body and parts of an automobile.

[0102] Preferred plastic substrates (S) are essentially substrates comprising or consisting of (i) polar plastics, such as polycarbonates, polyamides, polystyrene, styrene copolymers, polyesters, polyphenylene oxides and blends of these plastics, (ii) synthetic resins, such as polyurethanes RIM, SMC, BMC, (iii) polyolefin substrates of the polyethylene and polypropylene type with a high rubber content, such as PP-EPDM, and surface-activated polyolefin substrates. The plastics may furthermore be fibre-reinforced, in particular using carbon fibres and / or metal fibres.

[0103] It is also possible to use substrates (S) which contain both metal and plastic fractions, for example vehicle bodies which contain plastic parts.

[0104] A metal substrate with a cured electrocoating can be obtained by electrophoretically applying an electrocoating material onto a metal substrate (S) and curing said applied material at a temperature of 100-250°C, preferably 140-220°C, for 5-60 minutes, preferably 10-45 minutes. Before curing, said material can be flashed off, for example at 15-35°C, for example for 0.5-30 minutes, and / or intermediately dried, for example at a temperature of 40-90°C, for example for 1-60 minutes. Suitable electrocoat materials and also their curing are described in WO2017 / 088988A1 and comprise hydroxy-functional polyetheramines as binders and blocked polyisocyanates as crosslinkers. Before application of the electrocoating material, a conversion coating, for example a zinc phosphate coat, can be applied to the metal substrate. The film thickness of the cured electrocoating is, for example, 10-40 micrometers, preferably 15-25 micrometers.

[0105] A metal substrate with a cured electrocoating and / or a cured filler can be obtained by applying a filler composition to a metal substrate, optionally with a cured electrocoating, or to a metal substrate and / or a plastic substrate, and curing said filler composition at a temperature of 40-100° C., preferably 60-80° C., for 5-60 minutes, preferably 3-8 minutes. Suitable filler compositions are well known to the person skilled in the art and are commercially available, for example under the trade name Glasurit from BASF Coatings GmbH. The film thickness of the cured filler is, for example, 30-100 micrometers, preferably 50-70 micrometers.

[0106] According to a second alternative, the substrate in step (1) is a multi-layer coating with defects. This substrate with defects is therefore the original finish (i.e. the multi-layer coating) to be repaired or completely recoated. The defects of the multi-layer coating can be repaired by the method of the invention. For this purpose, the surface to be repaired in the multi-layer coating can first be polished. Polishing is preferably carried out by partially polishing or polishing off any or all of the coating layers, the base coat and the clear coat layers. Polishing only the base coat and the clear coat layers is particularly established in the OEM automotive repair segment, where, in contrast to factory repairs, defects generally occur only in the base coat and / or clear coat areas, in particular not in the area of ​​the underlying filler layer. If the filler layer is also defective, for example scratches caused by mechanical influences and often extending to the substrate surface (metal or plastic substrate), polishing of all coating layers present on the substrate is required.

[0107] Step (1): In step (1) of the method of the present invention, the coating composition of the present invention is applied onto a substrate (S). The application of the coating composition onto the substrate (S) is understood as follows: the coating composition is applied such that the coating film produced in step (2) is disposed on the substrate, but does not necessarily have to be in direct contact with the substrate. For example, another coating may be disposed between the coating film and the substrate. Preferably, the coating composition is applied directly onto the substrate (S) in step (1), i.e., the coating film produced in step (2) is in direct contact with the substrate (S).

[0108] The coating composition of the present invention can be applied by methods known to those skilled in the art for applying liquid coating materials, such as dipping, knife coating, spraying, roller, etc. Preference is given to employing spray application methods, such as compressed air spray (pneumatic application), airless spray, high-speed rotation, electrostatic spray application (ESTA), optionally in combination with hot spray application, such as hot air (hot spray). Very particularly preferably, the coating composition is applied by pneumatic spray application or electrostatic spray application.

[0109] Step (2): In step (2) of the method of the present invention, a coating film is formed from the coating composition applied in step (1). The formation of the film from the applied coating composition is achieved, for example, by flushing off the applied coating composition. The term "flushing off" is understood in principle as a designation for passive or active evaporation of the solvent from the coating composition, usually at ambient temperature (i.e. room temperature). The coating material is still liquid immediately after application and at the beginning of flushing, and therefore can flow to form a uniform and smooth coating film. Thus, after the flushing stage, a relatively smooth coating film is obtained that contains less solvent compared to the applied coating composition. Although the film is no longer flowable, it is still, for example, soft. In particular, the coating film is not yet cured, as will be described below.

[0110] The formation of the coating film in step (2) is carried out at a temperature of 20 to 60° C. for 5 to 80 minutes, preferably at a temperature of 20 to 35° C. for 5 to 70 minutes.

[0111] Step (3): In step (3) of the method of the present invention, the coating film is cured. Curing of a coating film or composition is therefore understood to be the conversion of such a film or composition into a usable state, i.e. into a state in which the substrate provided with said coating film can be transported, stored and used in its intended manner. The cured coating film is thus prepared in particular as a solid coating film that is no longer soft, but instead no longer shows substantial changes in properties such as hardness or adhesion to the substrate, even when further exposed to the curing conditions described below.

[0112] As a rule, curing is carried out for 5 to 80 minutes, preferably 10 to 50 minutes, at a temperature of 10 to 180° C., for example in particular at 40 to 90° C. Since the method of the invention is particularly suitable for repair applications requiring low curing conditions, the curing in step (3) is preferably carried out at a temperature of 20 to 30° C., for 10 to 70 minutes, preferably 20 to 60 minutes.

[0113] Typically, the thickness of the layer obtained after step (3) is in the range of 15 μm to 80 μm, preferably 20 μm to 70 μm or 30 μm to 65 μm, for example 40 μm to 60 μm.

[0114] The coating layers produced from the coating composition of the present invention have improved resistance to humidity conditions compared to coating compositions containing DBU instead of metal alkoxides as cocatalysts. Moreover, the curing of the coating composition can be carried out at low temperatures, making the method of the present invention particularly suitable for repair applications. The cured coatings exhibit good adhesion, fast sanding and finish sanding, good appearance, and high scratch and solvent resistance. Furthermore, thick coating layers can be produced without defects or stresses. Due to the absence of commonly used isocyanate and melamine crosslinkers and tin catalysts, the method of the present invention has a good ecological profile and can meet stringent environmental regulations.

[0115] What has been said about the coating compositions of the invention applies mutatis mutandis to the further preferred embodiments of the method of the invention for preparing the coated substrates.

[0116] The coated substrate of the present invention: The end product after completion of step (3) of the method of the present invention is a coated substrate of the present invention.

[0117] Depending on the substrate selected, the coating composition can be applied to a wide range of different application areas. Many types of substrates can be coated. Therefore, the coating composition of the present invention is very suitable for use as a decorative and protective coating system, especially on the body or parts of transportation means (especially motor vehicles, such as motorcycles, buses, trucks or automobiles). The substrate preferably comprises a multi-layer coating used for automotive coating.

[0118] The coating compositions of the present invention are also suitable for use on construction, interior and exterior; furniture, windows and doors; plastic moldings, especially CDs and windows; small industrial parts, coils, containers and packaging; white goods; sheeting; optical, electrical and mechanical parts, as well as hollow glass products and everyday use items.

[0119] What has been said regarding the inventive coating composition and the inventive method applies mutatis mutandis with respect to the further preferred embodiments of the coated substrate according to the invention.

[0120] The multi-layer coating of the present invention: Yet another object of the present invention is a multi-layer coating consisting of at least two coating layers, at least one of which is formed from a coating composition according to the invention.

[0121] Typically, a multi-layer coating comprises at least two coating layers.

[0122] A preferred multi-layer coating comprises at least a basecoat layer and a clearcoat layer. The coating composition of the present invention preferably forms the clearcoat layer.

[0123] Further preferred are multi-layer coatings comprising at least one filler coat layer coated with at least one base coat layer, which in turn is coated with at least one clear coat layer, the clear coat layer preferably being formed from the coating composition of the present invention.

[0124] In particular, but not limited to automotive coatings, the multi-layer coating preferably includes an electrocoat layer, at least one filler coat layer over the electrocoat layer, at least one basecoat layer over the electrocoat layer, and at least one clearcoat layer over the basecoat layer, the clearcoat layer preferably being formed from the coating composition of the present invention.

[0125] Said multi-layer coating can be prepared as described above in connection with the method of the present invention. The applied coating layers can be cured separately or at least two coating layers can be cured simultaneously. Particularly preferably, at least one base coat layer and a clear coat layer are cured simultaneously. The application, drying or flashing off and curing of the coating layers of the multi-layer coating can be carried out according to the methods known in the state of the art. Suitable electrocoating, filler and base coat compositions are, for example, commercially available. Suitable substrates have already been mentioned in connection with the method of the present invention.

[0126] What has been said regarding the coating composition according to the invention, the method according to the invention and the coated substrate according to the invention applies mutatis mutandis with respect to the further preferred embodiments of the multilayer coating according to the invention.

[0127] Substrates coated with multi-layer coatings: A final subject of the invention is a substrate coated with the multilayer film described above.

[0128] What has been said regarding the inventive coating composition, the inventive method, the coated substrate according to the invention and the inventive multilayer coating applies mutatis mutandis with respect to the further preferred embodiments of the inventive substrate coated with a multilayer coating.

[0129] The present invention is particularly illustrated by the following embodiments: Embodiment 1: a) has an isocyanate content of less than 1%; At least one silane group of general formula (I) * -NR 1 X-SiR 2 a (OR 3 ) 3-a (I) Optionally at least one silane group of general formula (II) * -N[X-SiR 2 a (OR 3 ) 3-a ] n [X'-SiR 2 b (OR 3 ) 3-b ] m (II) At least one silane-based compound R1, During the ceremony, X, X' are each independently a linear and / or branched alkylene or cycloalkylene radical having 1 to 20 carbon atoms; R 1 is an alkyl group containing 1 to 10 carbon atoms, R 2 , R 3 are each independently an alkyl, cycloalkyl, aryl, or aralkyl group, and the carbon chain of the alkyl, cycloalkyl, aryl, or aralkyl group is not terminated by adjacent oxygen, sulfur, or NR acan be interrupted by a R a is alkyl, cycloalkyl, aryl, or aralkyl; n and m are each independently 0 to 2, provided that m+n=2; a, b are independently 0 to 2; b) at least one catalyst C1 of general formula (III), z[C(R 4 )(R 5 )(R 6 )-(CH2) n -C(=O)-O - ]M z+ (III) During the ceremony, R 4 ~R 6 are each independently hydrogen or an alkyl group containing 1 to 6 carbon atoms, provided that the residue R 4 ~R 6 The total number of carbon atoms is within the range of 3 to 8; z is 1 to 4; and n is 0 or 1 to 8; however, When z=1, M is selected from the group consisting of Li, K and Na; When z=2, M is selected from the group consisting of Zn and Zr; When z=3, M is selected from the group consisting of Bi and Al; When z=4, M is selected from the group consisting of Zr and Ti; c) at least one metal alkoxide C2; d) one or more aprotic organic solvents; and 1. A coating composition comprising:

[0130] Embodiment 2: a) has an isocyanate content of less than 1%; At least one silane group of general formula (I) * -NR 1 X-SiR 2 a (OR 3 ) 3-a (I) At least one silane group of general formula (II) * -N[X-SiR 2 a (OR 3 ) 3-a ] n [X'-SiR 2 b (OR 3 ) 3-b ] m (II) At least one silane-based compound R2, During the ceremony, X, X' are each independently a linear and / or branched alkylene or cycloalkylene radical having 1 to 20 carbon atoms; R 1 is an alkyl group containing 1 to 10 carbon atoms, R 2 , R 3 are each independently an alkyl, cycloalkyl, aryl, or aralkyl group, and the carbon chain of the alkyl, cycloalkyl, aryl, or aralkyl group is not terminated by adjacent oxygen, sulfur, or NR a can be interrupted by a R a is alkyl, cycloalkyl, aryl, or aralkyl; n and m are each independently 0 to 2, provided that m+n=2; a, b are independently 0 to 2; b) at least one catalyst C1 of general formula (III), z[C(R 4 )(R 5 )(R 6 )-(CH2) n -C(=O)-O - ]M z+ (III) During the ceremony, R 4 ~R 6 are each independently hydrogen or an alkyl group containing 1 to 6 carbon atoms, provided that the residue R 4 ~R 6 The total number of carbon atoms is within the range of 3 to 8; z is 1 to 4; and n is 0 or 1 to 8; however, When z=1, M is selected from the group consisting of Li, K and Na; When z=2, M is selected from the group consisting of Zn and Zr; When z=3, M is selected from the group consisting of Bi and Al; When z=4, M is selected from the group consisting of Zr and Ti; c) one or more aprotic organic solvents; 1. A coating composition comprising:

[0131] Embodiment 3: A coating composition according to embodiment 1 or 2, characterized in that the silane-based compounds R1 and R2, respectively, have an isocyanate content of less than 0.5%, more preferably between 0.05 and 0%.

[0132] Embodiment 3: A coating composition according to any one of the preceding embodiments, characterized in that X and X' in general formulas (I) and (II) represent, independently of one another, a linear alkylene radical having 1 to 10, preferably 1 to 6, more preferably 2 to 5, very preferably 3 carbon atoms.

[0133] Embodiment 4: R in general formula (I) 1 The coating composition according to any one of the preceding embodiments, characterized in that is an alkyl group containing 2 to 8 carbon atoms, preferably 4 to 6 carbon atoms, and very preferably 4 carbon atoms.

[0134] Embodiment 5: R in Formulas (I) and (II) 2 are independent of each other, C1 to C 10 A coating composition according to any one of the preceding embodiments, characterized in that it represents an alkyl group, preferably a C1-C6 alkyl group, very preferably a C1 alkyl group.

[0135] Embodiment 6: A coating composition according to any one of the preceding embodiments, characterized in that a in formulas (I) and (II) and b in formula (II) are, independently of each other, 0.

[0136] Embodiment 7: A coating composition according to any one of embodiments 1 and 3 to 6, characterized in that the silane-based compound R1 contains in each case 50 to 100 mol %, preferably 80 to 100 mol %, more preferably 95 to 100 mol %, of at least one silane group of general formula (I) and 0 to 50 mol %, preferably 0 to 20 mol %, more preferably 0 to 5 mol %, of at least one silane group of general formula (II), based on the totality of the silane groups of general formulas (I) and (II).

[0137] Embodiment 8: A coating composition according to any one of embodiments 2 to 6, characterized in that the silane-based compound R2 contains in each case 50 to 99.9 mol %, preferably 80 to 99.9 mol %, more preferably 95 to 99.9 mol %, of at least one silane group of general formula (I) and 0.01 to 50 mol %, preferably 0.01 to 20 mol %, more preferably 0.01 to 5 mol %, of at least one silane group of general formula (II), based on the totality of the silane groups of general formulas (I) and (II).

[0138] Embodiment 9: The silane-based compound R1 is a compound comprising at least one polyisocyanate having the general formula (Ia) HNR 1 -X-SiR 2 a (OR 3 ) 3-a (Ia) and reacting the compound with at least one of the following: and optionally a compound of the general formula (IIa) HN[X-SiR 2 a (OR 3 ) 3-a ] n [X'-SiR 2 b (OR3 ) 3-b ] m (IIa) with at least one compound of During the ceremony, X, X' are each independently a linear and / or branched alkylene or cycloalkylene radical having 1 to 20 carbon atoms, preferably a linear alkylene radical having 3 carbon atoms, R 1 is an alkyl group containing 1 to 10 carbon atoms, preferably a linear alkyl group containing 4 carbon atoms, R 2 , R 3 are each independently an alkyl, cycloalkyl, aryl, or aralkyl group, and the carbon chain of the alkyl, cycloalkyl, aryl, or aralkyl group is not terminated by adjacent oxygen, sulfur, or NR a can be interrupted by a R a is an alkyl, cycloalkyl, aryl, or aralkyl group, preferably a C alkyl group; n and m are each independently 0 to 2, provided that m+n=2; a and b are each independently 0 to 2, preferably 0. A coating composition according to any one of embodiments 1 and 3 to 7, characterized in that

[0139] Embodiment 10: The silane-based compound R2 is a compound comprising at least one polyisocyanate having the general formula (Ia) HNR 1 -X-SiR 2 a (OR 3 ) 3-a (Ia) reacting with at least one compound, and optionally a compound of the general formula (IIa) HN[X-SiR 2 a (OR 3 ) 3-a ] n [X'-SiR 2 b(OR 3 ) 3-b ] m (IIa) with at least one compound of During the ceremony, X, X' are each independently a linear and / or branched alkylene or cycloalkylene radical having 1 to 20 carbon atoms, preferably a linear alkylene radical having 3 carbon atoms; R 1 is an alkyl group containing 1 to 10 carbon atoms, preferably a linear alkyl group containing 4 carbon atoms, R 2 , R 3 are each independently an alkyl, cycloalkyl, aryl, or aralkyl group, and the carbon chain of the alkyl, cycloalkyl, aryl, or aralkyl group is not terminated by adjacent oxygen, sulfur, or NR a can be interrupted by a R a is an alkyl, cycloalkyl, aryl, or aralkyl group, preferably a C alkyl group; n and m are each independently 0 to 2, provided that m+n=2; a and b are each independently 0 to 2, preferably 0. 9. A coating composition according to any one of embodiments 2 to 6 and 8, characterized in that

[0140] Embodiment 11: A coating composition according to embodiment 9 or 10, characterized in that the at least one polyisocyanate has an average isocyanate functionality of 2 to 6, preferably 2 to 5, very preferably 2 to 3.5.

[0141] Embodiment 12: A coating composition according to any one of embodiments 9 to 11, characterized in that the polyisocyanate is selected from hexamethylene diisocyanate urethione, hexamethylene diisocyanate, 1-isocyanato-4-[(4-isocyanatocyclohexyl)methyl]-cyclohexane and hexamethylene diisocyanate trimer.

[0142] Embodiment 13: A coating composition according to any one of the preceding embodiments, characterized in that the silane-based compounds R1 and R2 are each present in a total amount of 25 to 95% by weight, more preferably 35 to 90% by weight, most preferably 40 to 80% by weight, in each case based on the total weight of the coating composition.

[0143] Embodiment 14: Residue R in general formula (III) 4 ~R 6 wherein the sum of the number of carbon atoms in is 3 to 5 or 5 to 8.

[0144] Embodiment 15: A coating composition according to any one of the preceding embodiments, characterized in that z in general formula (III) is 1, 3 or 4, preferably 1 or 4.

[0145] Embodiment 16: A coating composition according to any one of the preceding embodiments, characterized in that n in general formula (III) is 0 or 2 to 6, preferably 0 or 4.

[0146] Embodiment 17: In the general formula (III), n is 0 and the residue R 4 and R 5 are each independently a linear or branched C3-C5 alkyl group, and the residue R 6 is a methyl group, with the exception that the residue R 4 ~R 6 wherein the sum of all carbon atoms in is 8.

[0147] Embodiment 18: In the general formula (III), n is 1 to 8, preferably 4, and the residue R 4 ~R 6 17. The coating composition according to any one of the preceding embodiments, wherein, independently of one another, are methyl groups.

[0148] Embodiment 19: A coating composition according to any one of the preceding embodiments, characterized in that M in general formula (III) is potassium, lithium or titanium, preferably potassium or titanium.

[0149] Embodiment 20: A coating composition according to any one of the preceding embodiments, characterized in that the at least one catalyst C1 of general formula (III) is a potassium, lithium or titanium neodecanoate and / or ethylhexanoate, preferably potassium(I) neodecanoate, titanium(IV) neodecanoate, potassium(I) 2-ethylhexanoate, or titanium(IV) 2-ethylhexanoate.

[0150] Embodiment 21: A coating composition according to any one of the preceding embodiments, characterized in that the at least one catalyst C1 is present in a total amount of 1 mmol to 50 mmol, preferably 5 mmol to 40 mmol, very preferably 15 to 25 mmol metal per 100 g of silane-based compound R1 or R2 solids.

[0151] Embodiment 22: The at least one metal alkoxide C2 has the general formula (IV) M 1 [(OR 7 ) m (R 8 ) n-m ] n (IV) During the ceremony, R 7 is a linear or branched C1 to C10 alkyl group, R 8 is a halogen group, an acetylacetonate group, an alkylacetoacetate group, or an ethanolaminato group, M 1 represents at least one metal selected from silicon, titanium, tantalum, zirconium, boron, aluminum, magnesium, and zinc; m is an integer from 0 to 4; n is M 1 Representing valences of 2 to 5, The coating composition according to any one of embodiments 1, 3 to 7, 9 and 11 to 21, characterized in that the metal alkoxide is selected from the group consisting of:

[0152] Embodiment 23: The R in general formula (IV) 7 is selected from C3 to C5 alkyl groups, preferably C3 or C4 alkyl groups, and / or R 7 23. The coating composition according to embodiment 22, wherein is selected from alkyl acetoacetate groups, preferably from ethyl acetoacetate groups.

[0153] Embodiment 24: A coating composition according to embodiment 22 or 23, characterized in that in general formula (IV) m is 0 or 1-4, more preferably 0 or 2-4, very preferably 0, 2 or 4.

[0154] Embodiment 25: M in formula (IV) 1 25. The coating composition according to any one of embodiments 22 to 24, characterized in that: is a metal selected from titanium, and n represents a valence of 4.

[0155] Embodiment 26: A coating composition according to any one of embodiments 1, 3 to 7, 9 and 11 to 25, characterized in that the metal alkoxide C2 is selected from titanium(IV) isopropoxide and / or titanium(IV) n-butoxide and / or titanium(IV) bis(ethylacetoacetate)diisopropoxide.

[0156] Embodiment 27: A coating composition according to any one of embodiments 1, 3 to 7, 9 and 11 to 26, characterized in that the at least one metal alkoxide C2, preferably a metal alkoxide of general formula (IV), is present in a total amount of in each case from 2.5 to 40 mmol metal, based on 100 g of silane-based compound R1 solids.

[0157] Embodiment 28: A coating composition according to any one of embodiments 1, 3 to 7, 9 and 11 to 27, characterized in that the metal-to-metal ratio of the at least one metal alkoxide C2, preferably the catalyst C1 of general formula (III) to the metal alkoxide of general formula (IV), is from 1:2 to 2:1.

[0158] Embodiment 29: A coating composition according to any one of the preceding embodiments, characterized in that the at least one aprotic solvent is selected from the group consisting of aliphatic and / or aromatic hydrocarbons, ketones, esters, ethers, or mixtures thereof, preferably an ester, very preferably butyl acetate.

[0159] Embodiment 30: A coating composition according to any one of the preceding embodiments, characterized in that the coating composition comprises a total amount of water and / or protic solvents of less than 10% by weight, preferably less than 5% by weight, more preferably less than 1% by weight and very preferably 0% by weight, in each case based on the total weight of the coating composition.

[0160] Embodiment 31: A coating composition according to any one of the preceding embodiments, characterized in that the at least one aprotic solvent is present in a total amount of 1 to 70% by weight, more preferably 20 to 60% by weight, most preferably 30 to 50% by weight, in each case based on the total weight of the coating composition.

[0161] Embodiment 32: General formula (V) C(R 4 )(R 5 )(R 6 )-(CH2) n -C(=O)-OH (V) During the ceremony, R 4 ~R 6 are each independently hydrogen or an alkyl group containing 1 to 6 carbon atoms, provided that the residue R 4 From R 6 the total number of carbon atoms is 3 to 8, preferably 5 to 8; n is 0 or 1 to 8, preferably 0 or 4. 3. A coating composition according to any one of the preceding embodiments, further comprising at least one carboxylic acid of

[0162] Embodiment 33: A coating composition according to embodiment 32, characterized in that the at least one carboxylic acid of general formula (V) is neodecanoic acid.

[0163] Embodiment 34: A coating composition according to embodiment 32 or 33, characterized in that the at least one carboxylic acid of general formula (V), preferably neodecanoic acid, is present in a total amount of 0 to 80% by weight, preferably 30 to 70% by weight, very preferably 50 to 60% by weight, in each case based on the total amount of catalyst C1 of general formula (III).

[0164] Embodiment 35: General formula (VI) (X) n -R 9 -Ox (VI) During the ceremony, Ox is an oxirane group; R 9 is an aliphatic hydrocarbyl group containing 2 to 15 carbon atoms and optionally containing ether and / or ester groups; n is 1 to 5; and X is independently Ox or * -Si(R g ) 3-v (R h ) v group, v is 0 or 1, R g is an alkoxy group containing 1 to 4 carbon atoms, R h is an alkyl group containing 1 to 4 carbon atoms or an alkoxy group containing 1 to 4 carbon atoms; 20. The coating composition according to any one of the preceding embodiments, further comprising at least one epoxy-functional compound of

[0165] Embodiment 36: R in formula (VI)9 is an aliphatic hydrocarbyl group * -(CH2)3-O-CH2- # or a cyclohexylethyl group.

[0166] Embodiment 37: A coating composition according to embodiment 35 or 36, characterized in that n in general formula (VI) is 1.

[0167] Embodiment 38: X in formula (VI) is * -Si(R g ) 3-v (R h ) v group, where v is 0 or 1, and R g is an alkoxy group containing 1 to 4 carbon atoms, R h 38. The coating composition according to any one of embodiments 35 to 37, wherein is an alkoxy group containing one carbon atom or an alkyl group containing one carbon atom.

[0168] Embodiment 39: The at least one epoxy compound of general formula (VI) is selected from the group consisting of (3-glycidoxypropyl) trimethoxysilane, dimethoxy(3-glycidyloxypropyl)methylsilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, trimethylolpropane triglycidyl ether ... 39. The coating composition according to any one of embodiments 35 to 38, characterized in that the reactive functional group is selected from (3-glycidoxypropyl)trimethoxysilane, trimethylolpropane triglycidyl ether, and the reaction product of 2,2-bis(hydroxymethyl)-1,3-propanediol with 2-(chloromethyl)oxirane, preferably (3-glycidoxypropyl)trimethoxysilane, trimethylolpropane triglycidyl ether, and the reaction product of 2,2-bis(hydroxymethyl)-1,3-propanediol with 2-(chloromethyl)oxirane.

[0169] Embodiment 40: A coating composition according to any one of embodiments 35 to 39, characterized in that the at least one epoxy-functional compound of general formula (VI) is present in a total amount of 0 to 20% by weight, more preferably 2.5 to 15% by weight, most preferably 5 to 10% by weight, in each case based on the solids content of the coating composition.

[0170] Embodiment 41: A coating composition according to any one of the preceding embodiments, characterized in that the coating composition further comprises at least one catalyst C3 different from catalysts C1 and C2, wherein the catalyst C3 is selected from bicyclic tertiary amines, very preferably DBU.

[0171] Embodiment 42: The coating composition according to embodiment 41, characterized in that the mass ratio of catalyst C1 to the further catalyst C3 is preferably from 1:1 to 8:1, more preferably from 2:1 to 6:1, most preferably from 3:1 to 5:1, for example 4:1.

[0172] Embodiment 43: A coating composition according to any one of the preceding embodiments, characterized in that the coating composition further comprises at least one coating additive selected from the group consisting of: (i) UV absorbers; (ii) light stabilizers such as HALS compounds, benzotriazoles or oxalanilides; (iii) rheology modifiers such as sag control agents (urea crystal modified resins), organic thickeners and inorganic thickeners; (iv) free radical scavengers; (v) slip additives; (vi) polymerization inhibitors; (vii) defoamers; (viii) wetting agents; (ix) fluorine compounds; (x) adhesion promoters; (xi) leveling agents; (xii) film-forming aids such as cellulose derivatives; (xiii) fillers such as nanoparticles based on silica, alumina or zirconium oxide; (xiv) flame retardants; and (xv) mixtures thereof.

[0173] Embodiment 44: A coating composition according to any one of the preceding embodiments, characterized in that it is a clearcoat composition or a tinted clearcoat composition.

[0174] Embodiment 45: A coating composition according to any one of the preceding embodiments, characterized in that the coating composition comprises a total amount of less than 2 wt.-%, preferably 0 wt.-%, of at least one crosslinker and / or tin-containing compound, based on the total weight of the coating composition.

[0175] Embodiment 46: The coating composition according to embodiment 45, wherein the crosslinking agent is selected from the group consisting of amino resins, polyisocyanates, blocked polyisocyanates, polycarbodiimides, photoinitiators, and mixtures thereof.

[0176] Embodiment 47: A coating composition according to any one of the preceding embodiments, characterized in that it is a two-component coating composition, preferably comprising the silane-based compound R1 or R2 and, if present, the epoxy functional compound of general formula (VI) in a first container, and the catalysts C1 and C2, or C1 and optionally C3, the optional at least one coating additive and the at least aprotic solvent in a second container.

[0177] Embodiment 48: A method for forming a coating on a substrate (S), comprising the following steps: (1) applying a coating composition according to any one of embodiments 1 to 47 onto a substrate (S); (2) forming a coating film from the coating composition applied in step (1); (3) curing the coating film formed in step (2); and A method comprising:

[0178] Embodiment 49: Method according to embodiment 48, characterized in that the substrate (S) is selected from metal substrates, metal substrates coated with a cured electrocoat and / or a cured filler, plastic substrates and substrates comprising metal and plastic components, particularly preferably from metal substrates.

[0179] Embodiment 50: The method according to embodiment 49, characterized in that the metal substrate (S) comprises or is selected from the group consisting of iron, aluminum, copper, zinc, magnesium and their alloys, and steel.

[0180] Embodiment 51: The method according to embodiment 48, wherein the substrate in step (1) is a multilayer coating having a defect site.

[0181] Embodiment 52: The method according to any one of embodiments 48 to 51, characterized in that the formation of the coating film in step (2) is carried out at a temperature of 20 to 60°C for 5 to 80 minutes, preferably at a temperature of 20 to 35°C for 5 to 70 minutes.

[0182] Embodiment 53: The method according to any one of embodiments 48 to 52, characterized in that the curing in step (3) is carried out at a temperature of 20 to 30° C. for 10 to 70 minutes, preferably 20 to 60 minutes.

[0183] Embodiment 54: A coated substrate obtained by the method of any one of embodiments 48 to 53.

[0184] Embodiment 55: A multi-layer coating comprising at least two coating layers, at least one of the coating layers being formed from a coating composition according to any one of embodiments 1-47.

[0185] Embodiment 56: A substrate coated with a multi-layer coating as defined in embodiment 55.

[0186] Working Example Next, the present invention will be described in more detail using examples, but the present invention is by no means limited to these examples. Furthermore, "parts", "%" and "ratio" in the examples represent "parts by mass", "% by mass" and "mass ratio", respectively, unless otherwise specified.

[0187] 1. Method of decision 1.1 Solid content (solids, non-volatiles) The non-volatile fraction is determined according to DIN EN ISO 3251 (date: June 2008). It involves weighing 1 g of sample onto a pre-dried aluminum dish, drying for 60 min in a drying oven at 130 °C, cooling in a desiccator and weighing again. The remaining amount relative to the total amount of sample used corresponds to the non-volatile content.

[0188] 1.2 Isocyanate content (NCO content) The isocyanate content was determined by adding an excess of a 2% N,N-dibutylamine solution in xylene to a homogeneous solution of the sample in acetone / N-ethylpyrrolidone (1:1 vol.%) and potentiometric back titration of the amine excess with 0.1 N hydrochloric acid according to methods based on DIN EN ISO 3251:2008-06, DIN EN ISO 11909:2007-05 and DIN EN ISO 14896:2009-07. The NCO content of the silane-based compounds R based on solids can be calculated by the proportion of polymer in the solution (solids content):

[0189] 1.3 Preparation of multilayer coating (MC) The steel panels were first pretreated with Gardobond® zinc phosphate (commercially available from Chemetall GmbH) and then coated with an ED coat (Cathogard 800, commercially available from BASF Coatings GmbH) at a dry film thickness of 17-25 μm.

[0190] The electrocoated panels were then coated with a pneumatic spray gun at a temperature of 25°C and a relative humidity of 65% as follows: A primer (Glasurit 285-270, BASF Coatings GmbH) was applied to the electrocoated panels to a film thickness of 50-70 μm after curing at 60°C. The primer was then sanded off and a commercial water-based basecoat (Glasurit Line 90-1250 Deep Black, BASF Coatings GmbH) was applied to a film thickness of 10-20 μm after flash-off until dry to the touch for approximately 30 minutes. In a final step, each of the clearcoats C-C1 and C-I1 to C-I7 listed in Table 1 below was applied on top of the respective basecoat layer and cured at ambient conditions until dry to the touch for approximately 15-30 minutes. The dry film thickness of the clearcoat layer was 35-80 μm. For each clearcoat C-C1 and C-I1 to C-I7, two panels were prepared as described above.

[0191] 1.4 Test Measurements 1.4.1 Adhesive free time The tack-free time is determined with a guillotine test according to DIN EN ISO 9117-5:2012-11. In this test, 1.5 g of sea sand are poured onto the clear coat. The excess sand flows off the panel. The panel is then transferred to a device (guillotine) that can drop in a self-guided manner from 30 cm above the surface. The panel falls on the edge of the surface and is then checked for remaining grains of sand. If no grains of sand remain on the coating surface, the guillotine test is OK and the coating is considered to be "tack-free".

[0192] 1.4.2 Xylene test Seven days after preparation of the multi-layer coating described above, a large drop of xylene (approximately 2 mL) is applied to the coating and removed again after 4 minutes. After one hour, the surface is cleaned with PK700 cleaner (available from RM Automotive Refinish Paints) and the coating is inspected. The visibility of the edge of the drop is measured on a scale of 0 to 5 (0 meaning no ring is visible and 5 meaning the clearcoat has been completely removed).

[0193] 1.4.3 Cross-cut bonding Cross-cut adhesion was carried out according to DIN EN ISO 2409:2013-06 7 days after preparation of the multilayer coatings described above.

[0194] 1.4.4 Visual assessment of blistering, whitening, cracking, swelling and delamination after humidity exposure Seven days after the preparation of the multi-layer coating, each panel was transferred to a climatic chamber at 40°C and 100% humidity for 240 hours. Afterwards, it was visually inspected for blistering and whitening according to DIN EN ISO 4628-2:2016-07. An assessment of cracks, swelling and delamination was also performed visually. If no cracks, swelling or delamination were detected, the assessment of the respective criterion was "no". Otherwise, the assessment was "yes".

[0195] 2. Preparation of different silane-based compounds R-I1–R-I4 2.1 Silane-based compounds R-I1 Silane-based compound R-I1 was prepared by reacting 26.30 g of hexamethylene diisocyanate (HDI, monomer) with 2 equivalents of N-(n-butyl)-3-aminopropyltrimethoxysilane (73.70 g) at 60 °C without solvent until the residual NCO content reached 0%.

[0196] 2.2 Silane-based compound R-I2 Silane-based compound R-I2 was prepared by reacting HDI-based uretdione (35.59 g, DESMODUR XP2840) with 3 equivalents of N-(n-butyl)-3-aminopropyltrimethoxysilane (44.41 g) in 20 g of butyl acetate at 60 °C until the residual NCO content reached 0%.

[0197] 2.3 Silane-based compound R-I3 Silane-based compound R-I3 was prepared by reacting HDI-trimer (35.84 g, Desmodur N3300) with 3 equivalents of N-(n-butyl)-3-aminopropyltrimethoxysilane (44.16 g) in 20 g of butyl acetate at 60 °C until the residual NCO content reached 0%.

[0198] 2.4 Silane-based compounds R-I4 The silane-based compound R-I4 was prepared by reacting 4,4′-methylenebis(cyclohexylisocyanate) (28.60 g, Desmodur W) with 2 equivalents of N-(n-butyl)-3-aminopropyltrimethoxysilane (51.40 g) in 20 g of butyl acetate at 60 °C until the residual NCO content reached 0%.

[0199] 3. Preparation of Clear Coat Compositions C-C1 and C-I1 to C-I7 The components of comparative coating composition C-C1 and inventive coating compositions C-I1 through C-I7 were mixed in the amounts shown in Table 1. Component I was mixed first, followed by the addition of premixed Component II. All amounts are in parts by weight (i.e., grams). All clearcoat compositions had a nonvolatile content of 55.0%.

[0200] [Table 1]

[0201] 4.Achievements The results obtained for multilayer coatings prepared according to point 1.3 using clearcoat compositions C-C1 and C-I1 to C-I7 are given in Tables 2 and 3.

[0202] [Table 2]

[0203] [Table 3]

[0204] The inventive multi-layer coatings MC2-MC8, which include a clearcoat layer prepared from an inventive coating composition containing a mixture of silane-based compound R1 and catalyst C1 with metal alkoxide C2, have similar adhesion properties to the non-inventive multi-layer coating MC1, which is prepared from a clearcoat composition containing silane-based compound R1, catalyst C1 and DBU (see Table 2). However, the inventive multi-layer coatings show significantly improved resistance to humidity conditions (see Table 3). The whitening and blistering observed when the non-inventive multi-layer coating MC1 is exposed to humidity conditions is significantly higher than the whitening and blistering observed when the inventive multi-layer coatings MC2-MC7 are exposed to humidity conditions. When the co-catalyst DBU is combined with the silane-based compound R1, catalyst C1 and metal alkoxide C2 (multi-layer coating MC8), improved humidity resistance is obtained compared to the multi-layer coating MC1 containing catalyst C1 and DBU, showing the beneficial effect that the metal alkoxide C2 introduces into the clearcoat system.

[0205] In summary, the use of silane-based compounds R1 in combination with specific catalyst mixtures allows for sufficient cure and adhesion of coating compositions without the use of undesirable crosslinkers and tin-containing catalysts, such as polyisocyanates and melamine resins. Furthermore, the compositions of the present invention can be cured at room temperature, making them particularly suitable for repair applications.

Claims

1. a) has an isocyanate content of less than 1%; At least one silane group of general formula (I) * -NR 1 X-SiR 2 a (OR 3 ) 3-a (I) Optionally at least one silane group of general formula (II) * -N[X-SiR 2 a (OR 3 ) 3-a ] n [X’-SiR 2 b (OR 3 ) 3-b ] m (II) At least one silane-based compound R1 comprising During the ceremony, X, X' are, independently of one another, linear and / or branched alkylene or cycloalkylene radicals having 1 to 20 carbon atoms; R 1 is an alkyl group containing 1 to 10 carbon atoms, R 2 , R 3 are each independently an alkyl, cycloalkyl, aryl, or aralkyl group, and the carbon chain of the alkyl, cycloalkyl, aryl, or aralkyl group is not adjacent to any oxygen, sulfur, or NR a group, and R a is alkyl, cycloalkyl, aryl, or aralkyl; m and n are each independently 0 to 1, provided that m+n=2; a and b are independently 0 to 2; b) at least one catalyst C1 of general formula (III), z[C(R 4 )(R 5 )(R 6 )-(CH 2 ) n -C(=O)-O - ]M z+ (III) In the formula, R 4 ~R 6 are each independently hydrogen or an alkyl group containing 1 to 6 carbon atoms, provided that the residue R 4 ~R 6 the total number of carbon atoms is in the range of 3 to 8; z is 1 to 4; and n is 0 or 1 to 8; however, When z=1, M is selected from the group consisting of Li, K and Na; When z=2, M is selected from the group consisting of Zn and Zr; When z=3, M is selected from the group consisting of Bi and Al; When z=4, M is selected from the group consisting of Zr and Ti; c) at least one metal alkoxide C2; d) one or more aprotic organic solvents; and 1. A coating composition comprising:

2. a) has an isocyanate content of less than 1%; At least one silane group of general formula (I) * -NR 1 X-SiR 2 a (OR 3 ) 3-a (I) At least one silane group of general formula (II) * -N[X-SiR 2 a (OR 3 ) 3-a ] n [X’-SiR 2 b (OR 3 ) 3-b ] m (II) At least one silane-based compound R2 comprising During the ceremony, X, X' are, independently of one another, linear and / or branched alkylene or cycloalkylene radicals having 1 to 20 carbon atoms; R 1 is an alkyl group containing 1 to 10 carbon atoms, R 2 , R 3 are each independently an alkyl, cycloalkyl, aryl, or aralkyl group, and the carbon chain of the alkyl, cycloalkyl, aryl, or aralkyl group is not adjacent to any oxygen, sulfur, or NR a group, and R a is alkyl, cycloalkyl, aryl, or aralkyl; m and n are each independently 0 to 1, provided that m+n=2; a and b are independently 0 to 2; b) at least one catalyst C1 of general formula (III), z[C(R 4 )(R 5 )(R 6 )-(CH 2 ) n -C(=O)-O - ]M z+ (III) In the formula, R 4 ~R 6 are each independently hydrogen or an alkyl group containing 1 to 6 carbon atoms, provided that the residue R 4 ~R 6 is in the range of 3 to 8 carbon atoms; z is 1 to 4; and n is 0 or 1 to 8; however, When z=1, M is selected from the group consisting of Li, K and Na; When z=2, M is selected from the group consisting of Zn and Zr; When z=3, M is selected from the group consisting of Bi and Al; When z=4, M is selected from the group consisting of Zr and Ti; c) one or more aprotic organic solvents; 1. A coating composition comprising:

3. X and X′ in the general formulae (I) and (II) each independently represent a linear alkylene radical having 1 to 10, preferably 1 to 6, more preferably 2 to 5 and very preferably 3 carbon atoms, and / or R in formula (I) 1 is an alkyl group containing from 2 to 8 carbon atoms, preferably from 4 to 6 carbon atoms, very preferably 4 carbon atoms, and / or R in formulas (I) and (II) 3 are, independently of each other, C 1 ~C 10 Alkyl group, preferably C 1 ~C 6 Alkyl groups, very preferably C 1 represents an alkyl group and / or In the general formulae (I) and (II), a is 0, and / or 3. The coating composition according to claim 1, wherein b in general formula (II) is 0.

4. 4. Coating composition according to any one of claims 1 to 3, characterized in that the silane-based compounds R1 and R2 are each present in a total amount of 25 to 95% by weight, more preferably 35 to 90% by weight, most preferably 40 to 80% by weight, in each case based on the total weight of the coating composition.

5. 5. Coating composition according to any one of claims 1 to 4, characterized in that the at least one catalyst C1 of general formula (III) is a potassium, lithium or titanium neodecanoate and / or ethylhexanoate, preferably potassium(I) neodecanoate, potassium(I) 2-ethylhexanoate, titanium(IV) neodecanoate or titanium(IV) 2-ethylhexanoate.

6. 6. Coating composition according to any one of claims 1 to 5, characterized in that the at least one catalyst C1 is present in a total amount of 1 mmol to 50 mmol, preferably 5 mmol to 40 mmol, very preferably 15 to 25 mmol metal per 100 g of silane-based compound R1 or R2 solids.

7. The at least one metal alkoxide C2 has the general formula (IV) M 1 [(OR 7 ) m (R 8 ) n-m ] n (IV) During the ceremony, R 7 is a linear or branched C1 to C10 alkyl group, R 8 is a halogen group, an acetylacetonate group, an alkylacetoacetate group, or an ethanolaminato group, M 1 represents at least one metal selected from silicon, titanium, tantalum, zirconium, boron, aluminum, magnesium, and zinc; m is an integer from 0 to 4; n is M 1 Representing a valence of 2 to 5; 7. The coating composition according to claim 1, wherein the metal alkoxide is selected from the group consisting of the metal alkoxides listed above.

8. 8. Coating composition according to claim 1, 3 to 7, characterized in that the metal alkoxide C2 is selected from titanium(IV) isopropoxide and / or titanium(IV) n-butoxide and / or titanium(IV) bis(ethylacetoacetate)diisopropoxide.

9. 9. Coating composition according to claim 1, characterized in that the at least one metal alkoxide C2, preferably a metal alkoxide of general formula (IV), is present in a total amount of in each case from 2.5 to 40 mmol metal, based on 100 g of silane-based compound R1 solids.

10. A coating composition according to any one of claims 1 to 9, characterized in that it is a clearcoat composition or a tinted clearcoat composition.

11. 11. The coating composition according to claim 1, characterized in that the coating composition comprises a total of less than 2% by weight, preferably 0% by weight, of at least one crosslinker and / or tin-containing compound, based on the total weight of the coating composition.

12. A method for forming a coating on a substrate (S), comprising the steps of: (1) applying a coating composition according to any one of claims 1 to 11 onto a substrate (S); (2) forming a coating film from the coating composition applied in step (1); (3) curing the coating film formed in step (2); and A method comprising:

13. A coated substrate obtained by the method of claim 12.

14. A multi-layer coating having at least two coating layers, at least one of said coating layers being formed from a coating composition according to any one of claims 1 to 11.

15. A substrate coated with a multi-layer coating as defined in claim 14.

Citation Information

Patent Citations

  • Adducts from isocyanatoalkyl trialkoxysilanes and aliphatic, alkyl-branched diols or polyols

    EP2641925A1

  • New compound and curable resin composition containing the same

    JP2005015644A

  • Coating agent containing an adduct having alkoxysilane functionality

    JP2008516759A

  • Coating agent with improved flow tendency

    JP2013527867A

  • One-component curable coating compositions, methods of making and using them, and coatings and articles made therefrom

    JP2016511774A