Laminated Sheet
Patent Information
- Application Number
- JP2020065218
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-31
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-03-31
Smart Images

Figure 0007567195000002 
Figure 0007567195000003 
Figure 0007567195000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a laminate sheet, a decorative sheet using the laminate sheet, a decorated resin molded product, and methods for producing these. [Background technology]
[0002] Decorative resin molded products in which a decorative sheet is laminated on the surface of a resin molded product are used for vehicle interior parts, building material interior materials, home appliance housings, etc. Known molding methods for such decorated resin molded products include an insert molding method (see, for example, Patent Document 1) in which a decorative sheet is molded into a three-dimensional shape in advance using a vacuum molding die, and the molded sheet is inserted into an injection molding die and a resin in a fluid state is injected into the die to integrate the resin and the molded sheet, and an injection molding simultaneous decoration method (see, for example, Patent Documents 2 and 3) in which a decorative sheet inserted into a die during injection molding is integrated with molten resin injected into the cavity to decorate the surface of a resin molded product.
[0003] In recent years, with the diversification of consumer needs, there is a demand for decorative resin molded products with various designs. In order to keep up with such diversifying consumer needs, there is a demand for the development of decorative resin molded products that have a design feel and a texture based on the uneven shape of the surface.
[0004] In the manufacture of a decorated resin molded product having a concave-convex shape on its surface, for example, a decorative sheet having a concave-convex shape formed in advance on its surface is used. However, when a decorated resin molded product is manufactured using a decorative sheet having a concave-convex shape, there is a problem that it is difficult to maintain the concave-convex shape, since the concave-convex shape is deformed or lost due to heat or pressure when the decorative sheet is subjected to injection molding or the preliminary molding (vacuum molding) that precedes the injection molding. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2004-322501 A [Patent Document 2] Special Publication No. 50-19132 [Patent Document 3] Special Publication No. 61-17255 Summary of the Invention [Problem to be solved by the invention]
[0006] As mentioned above, in recent years, there has been a demand for the development of decorated resin molded products that have a design feel and a texture based on the uneven surface shape. However, when manufacturing decorated resin molded products using a decorative sheet with an uneven surface shape, there is a problem in that it is difficult to maintain the uneven surface shape, as the uneven surface shape can be deformed or lost due to heat and pressure when the decorative sheet is subjected to injection molding or the preliminary molding that precedes it (vacuum molding).
[0007] In this situation, the main object of the present disclosure is to provide a laminate sheet that can favorably maintain its uneven shape even when molded in a high-temperature and high-pressure environment. Further, the present disclosure also aims to provide a decorative sheet and a decorated resin molded product that use the laminate sheet, and methods for manufacturing the same. [Means for solving the problem]
[0008] The inventors of the present disclosure have conducted intensive studies to solve the above problems. As a result, it has been found that, in a laminate sheet formed by laminating at least a thermoplastic elastomer layer and a thermoplastic resin layer, by setting the softening point of the thermoplastic elastomer contained in the thermoplastic elastomer layer higher than the softening point of the thermoplastic resin contained in the thermoplastic resin layer, the uneven shape can be favorably maintained even by molding in a high-temperature, high-pressure environment. Specifically, it has been found that when an uneven shape is formed on the surface of the laminate sheet, the uneven surface shape formed on the laminate sheet is favorably maintained even by molding in a high-temperature, high-pressure environment. In addition, in a decorative sheet in which the laminate sheet is laminated with a surface protection layer, a pattern layer, etc., when an uneven shape is formed on the surface of the decorative sheet (whether the laminate sheet has an uneven shape or not), it has been found that the uneven surface shape formed on the decorative sheet is favorably maintained even by molding in a high-temperature, high-pressure environment. The present disclosure has been completed based on such findings and through further studies.
[0009] That is, the present disclosure provides the inventions of the following aspects. Item 1. At least a thermoplastic elastomer layer and a thermoplastic resin layer are laminated together, A laminate sheet, wherein the softening point of the thermoplastic elastomer contained in the thermoplastic elastomer layer is higher than the softening point of the thermoplastic resin contained in the thermoplastic resin layer. Item 2. The laminate sheet according to item 1, wherein the difference between the softening point of the thermoplastic elastomer and the softening point of the thermoplastic resin is 10° C. or more. Item 3. The laminate sheet according to item 1 or 2, wherein the thermoplastic elastomer layer and the thermoplastic resin layer are in contact with each other. Item 4. The laminate sheet according to any one of Items 1 to 3, wherein the thermoplastic elastomer layer and the thermoplastic resin layer are laminated via an adhesive layer. Item 5. A decorative sheet comprising the laminate sheet according to any one of items 1 to 4. Item 6. The decorative sheet according to item 5, further comprising a surface protective layer on the thermoplastic elastomer layer side of the laminate sheet. Item 7. The decorative sheet according to item 5 or 6, further comprising a pattern layer on at least one of the thermoplastic elastomer layer side of the laminate sheet and the thermoplastic resin layer side of the laminate sheet. Item 8. The decorative sheet according to any one of Items 5 to 7, wherein the surface of the laminate sheet on the side of the thermoplastic elastomer layer has an uneven shape. Item 9. A decorated resin molded product comprising at least a molded resin layer and the decorative sheet according to any one of items 5 to 8. Item 10. A method for producing a decorated resin molded product, comprising laminating at least a molded resin layer and the decorative sheet according to any one of items 5 to 8, A step of preparing a decorative sheet according to any one of items 5 to 8; a step of molding the decorative sheet at a temperature equal to or lower than the softening point of the thermoplastic elastomer and equal to or higher than the softening point of the thermoplastic resin, and laminating the decorative sheet with a molded resin layer; A method for manufacturing a decorated resin molded product comprising the steps of: Effect of the Invention
[0010] According to the present disclosure, it is possible to provide a laminate sheet capable of favorably maintaining a concave-convex shape even when molded in a high-temperature, high-pressure environment. In addition, according to the present disclosure, it is also possible to provide a decorative sheet and a decorated resin molded product using the laminate sheet, and a manufacturing method thereof. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic diagram of a cross-sectional structure of one embodiment of a decorative sheet according to the present disclosure. [Diagram 2] 1 is a schematic diagram of a cross-sectional structure of one embodiment of a decorative sheet according to the present disclosure. [Diagram 3] 1 is a schematic diagram of a cross-sectional structure of one embodiment of a decorative sheet according to the present disclosure. [Figure 4] 1 is a schematic diagram of a cross-sectional structure of one embodiment of a decorative sheet according to the present disclosure. [Diagram 5] 1 is a schematic diagram of a cross-sectional structure of one embodiment of a decorated resin molded product according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] 1.Laminated sheet The laminated sheet of the present disclosure is characterized in that at least a thermoplastic elastomer layer and a thermoplastic resin layer are laminated together, and the softening point of the thermoplastic elastomer contained in the thermoplastic elastomer layer is higher than the softening point of the thermoplastic resin contained in the thermoplastic resin layer. The decorative sheet of the present disclosure, which includes the laminated sheet of the present disclosure, has such a specific configuration, and therefore can favorably maintain the uneven shape even when molded in a high-temperature and high-pressure environment. The mechanism of this can be considered as follows. That is, in the decorative sheet of the present disclosure, the softening point of the thermoplastic elastomer is higher than that of the thermoplastic resin. For this reason, for example, in the preforming (vacuum molding) prior to injection molding, when molding is performed in a temperature range below the softening point of the thermoplastic elastomer and above the softening point of the thermoplastic resin, the thermoplastic elastomer layer exhibits rubber elasticity even when it is below its softening point, and therefore deforms. On the other hand, the thermoplastic resin layer is above its softening point and undergoes plastic deformation. In addition, the thermoplastic resin with low elasticity can fix the shape of the thermoplastic elastomer layer by cooling after molding. This allows preforming of the decorative sheet while maintaining the embossing applied to the thermoplastic elastomer layer. In addition, in injection molding, the layer that is shaped to have the uneven shape becomes a thermoplastic elastomer layer, and the uneven shape is maintained by its rubber elasticity. In general, the decorative sheet with the uneven shape is pressed against the mold with high pressure during injection molding, so that the uneven shape is deformed following the surface shape of the mold. Therefore, if the surface of the mold is flat, the uneven shape of the decorative sheet becomes flat accordingly. This is because the base layer is a decorative sheet made of a thermoplastic resin, and the unevenness is pressed against the mold with high pressure, causing plastic deformation beyond the yield point. In the laminated sheet of the present disclosure, the shaping layer with the uneven shape is a thermoplastic elastomer layer that exhibits rubber elasticity, so it is deformed following the surface shape of the mold and then restored. Therefore, it is possible to maintain the uneven shape even after injection molding. The laminated sheet of the present disclosure will be described in detail below.
[0013] In this specification, the numerical range indicated by "-" means "more than or equal to" or "less than or equal to", except where it is clearly stated as "more than or equal to". For example, the expression "2-15 mm" means 2 mm or more and 15 mm or less. In addition, in this specification, "(meth)acrylate" means "acrylate or methacrylate", and other similar terms have the same meaning. In addition, the decorative sheet of the present disclosure may not have a pattern layer, and may be transparent, for example.
[0014] As shown in the schematic diagram of FIG. 1, the laminate sheet 10 of the present disclosure is a laminate in which at least a thermoplastic elastomer layer 1 and a thermoplastic resin layer 2 are laminated. As shown in FIG. 1, both sides of the laminate sheet 10 may be flat, or the surface on the thermoplastic elastomer layer 1 side may have an uneven shape as shown in the schematic diagrams of FIG. 2 and FIG. 3. In the laminate sheet 10, the uneven shape on the surface on the thermoplastic elastomer layer 1 side may not be formed on the thermoplastic resin layer 2 as shown in the schematic diagram of FIG. 2, or may be formed on the thermoplastic resin layer 2 as shown in the schematic diagram of FIG. 3. The shape change during molding of the laminate sheet is smaller when the thermoplastic resin layer 2 does not have an uneven shape. Also, even when an uneven shape is formed on the thermoplastic resin layer 2, it is desirable that the uneven shape formed on the thermoplastic resin layer 2 is small. Although not shown, the surface on the thermoplastic resin layer 2 side of the laminate sheet 10 may have an uneven shape. Furthermore, when the surface of the laminate sheet 10 on the thermoplastic elastomer layer 1 side has an uneven shape, the concaves of the uneven shape may reach the thermoplastic resin layer 2. In this case, the surface of the thermoplastic elastomer layer 1 side of the thermoplastic resin layer 2 has an uneven shape formed thereon that corresponds to the uneven shape of the surface of the thermoplastic elastomer layer 1 side of the laminate sheet 10. As described later, these uneven shapes can be suitably formed by embossing or the like.
[0015] (Thermoplastic elastomer layer) The thermoplastic elastomer layer is a layer containing a thermoplastic elastomer. The softening point of the thermoplastic elastomer is higher than that of the thermoplastic resin contained in the thermoplastic resin layer described later. From the viewpoint of favorably achieving the effects of the present disclosure, the softening point of the thermoplastic elastomer is preferably equal to or higher than the temperature at which the laminated sheet is subjected to molding. The softening point of the thermoplastic elastomer is preferably about 120°C or higher, more preferably about 140°C or higher, even more preferably about 150°C or higher, and particularly preferably about 160°C or higher. In addition, the upper limit of the softening point of the thermoplastic elastomer is not particularly limited, but from the viewpoint of forming an uneven shape by rolling shaping using an embossing roll, it is preferably about 200°C or lower, more preferably 180°C or lower. Preferred ranges of the softening point of the thermoplastic elastomer include about 120 to 200°C, about 120 to 180°C, about 140 to 200°C, about 140 to 180°C, about 150 to 200°C, about 150 to 180°C, about 160 to 200°C, and about 160 to 180°C.
[0016] From the viewpoint of suitably achieving the effects of the present disclosure, the difference between the softening point of the thermoplastic elastomer and the softening point of the thermoplastic resin described below is preferably about 10° C. or more, more preferably about 20° C. or more, even more preferably about 30° C. or more, even more preferably about 40° C. or more, and even more preferably about 50° C. or more. From the same viewpoint, the difference in softening point is preferably about 80° C. or less, more preferably about 70° C. or less, and even more preferably about 60° C. or less. Preferred ranges of the difference in softening point include about 20 to 80° C., about 20 to 70° C., about 20 to 60° C., about 30 to 80° C., about 30 to 70° C., about 30 to 60° C., about 40 to 80° C., about 40 to 70° C., about 40 to 60° C., about 50 to 80° C., about 50 to 70° C., and about 50 to 60° C.
[0017] The thermoplastic elastomer is not particularly limited in type as long as it has a softening point higher than that of the thermoplastic resin contained in the thermoplastic resin layer described later. From the viewpoint of favorably achieving the effects of the present disclosure, specific examples of the thermoplastic elastomer include polyester-based elastomers, polystyrene-based elastomers, olefin-based elastomers, polyvinyl chloride-based elastomers, polyurethane-based elastomers, and polyamide-based elastomers. Among these, polyester-based elastomers are preferred from the viewpoint of particularly favorably achieving the effects of the present disclosure. The thermoplastic elastomer contained in the thermoplastic elastomer layer may be one type or two or more types. Note that a thermoplastic elastomer is an elastomer (polymer exhibiting elasticity) that has the property of softening and exhibiting fluidity when heated and returning to a rubber-like state when cooled, and can be molded by injection molding or the like involving heating. On the other hand, a thermosetting elastomer is an elastomer that does not exhibit fluidity due to softening even when heated, unlike a thermoplastic elastomer, and is generally referred to as rubber, such as silicone rubber, fluororubber, and some urethane rubber.
[0018] From the viewpoint of suitably achieving the effects of the present disclosure, the thermoplastic elastomer contained in the thermoplastic elastomer layer is, for example, about 50% by mass or more, preferably about 60% by mass or more, more preferably about 70% by mass or more, even more preferably about 80% by mass or more, still more preferably about 90% by mass or more, and may be about 99% by mass or about 100% by mass. The thermoplastic elastomer layer may be formed substantially only from a thermoplastic elastomer.
[0019] In order to improve adhesion to a layer provided thereon, the thermoplastic elastomer layer may be subjected to physical or chemical surface treatment such as oxidation or roughening on one or both sides as necessary. Examples of the oxidation method used for the surface treatment of the thermoplastic elastomer layer include corona discharge treatment, chromium oxidation treatment, flame treatment, hot air treatment, and ozone ultraviolet treatment. Examples of the roughening method used for the surface treatment of the thermoplastic elastomer layer include sandblasting and solvent treatment. These surface treatments are appropriately selected depending on the type of thermoplastic elastomer constituting the thermoplastic elastomer layer, but from the viewpoints of effect and operability, a corona discharge treatment is preferred.
[0020] The thermoplastic elastomer layer may be colored, for example, with a colorant, or may not be colored. The thermoplastic elastomer layer may be colorless and transparent, colored and transparent, or translucent. The colorant used in the thermoplastic elastomer layer is not particularly limited, but is preferably a colorant that does not discolor even at temperatures of 150° C. or higher, and specifically includes existing dry colors, paste colors, masterbatch resin compositions, and the like.
[0021] The thickness of the thermoplastic elastomer layer is not particularly limited, but from the viewpoint of suitably achieving the effects of the present disclosure, it is preferably about 10 μm or more, more preferably about 30 μm or more, even more preferably about 50 μm or more, and even more preferably about 70 μm or more. From the same viewpoint, the thickness of the thermoplastic elastomer layer is preferably about 250 μm or less, about 200 μm or less, about 150 μm or less, etc. Preferred ranges of the thickness of the thermoplastic elastomer layer include about 10 to 250 μm, about 10 to 200 μm, about 10 to 150 μm, about 30 to 250 μm, about 30 to 200 μm, about 30 to 150 μm, about 50 to 250 μm, about 50 to 200 μm, about 50 to 150 μm, about 70 to 250 μm, about 70 to 200 μm, and about 70 to 150 μm. Among these, a thickness of about 70 to 250 μm is particularly preferable. When the thermoplastic elastomer layer has an uneven shape, the thickness means the thickness at a position where no recesses are formed.
[0022] (thermoplastic resin layer) The thermoplastic resin layer is a layer containing a thermoplastic resin. The softening point of the thermoplastic resin is lower than the softening point of the thermoplastic elastomer contained in the thermoplastic elastomer layer. From the viewpoint of suitably achieving the effects of the present disclosure, the softening point of the thermoplastic resin is preferably equal to or lower than the temperature at which the laminated sheet is subjected to molding. From the same viewpoint, the softening point of the thermoplastic resin is preferably about 70°C or higher, more preferably about 80°C or higher, even more preferably about 90°C or higher, and particularly preferably about 100°C or higher. From the same viewpoint, the upper limit of the softening point of the thermoplastic resin is not particularly limited, but from the viewpoint of improving moldability, it is preferably about 140°C or lower, more preferably about 120°C or lower. Preferred ranges of the softening point of the thermoplastic resin include about 70 to 140°C, about 70 to 120°C, about 80 to 140°C, about 80 to 120°C, about 90 to 140°C, about 90 to 120°C, about 100 to 140°C, and about 100 to 120°C.
[0023] The thermoplastic resin is not particularly limited in type as long as it has a softening point lower than that of the thermoplastic elastomer contained in the thermoplastic elastomer layer. From the viewpoint of favorably achieving the effects of the present disclosure, specific examples of the thermoplastic resin include acrylonitrile-butadiene-styrene resin (hereinafter sometimes referred to as "ABS resin"), acrylonitrile-styrene-acrylic acid ester resin (hereinafter sometimes referred to as "ASA resin"), acrylonitrile-ethylene-propylene-diene-styrene resin, acrylic resin, polyolefin resin such as polypropylene and polyethylene, polycarbonate resin, vinyl chloride resin, polyethylene terephthalate (PET), and the like. Among these, ABS resin and acrylic resin are preferable from the viewpoint of three-dimensional moldability. The thermoplastic resin contained in the thermoplastic resin layer may be one type or two or more types.
[0024] From the viewpoint of suitably achieving the effects of the present disclosure, the thermoplastic resin contained in the thermoplastic resin layer is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and even more preferably 90% by mass or more, and may be 99% by mass or 100% by mass. The thermoplastic resin layer may be formed substantially only from a thermoplastic resin.
[0025] In order to improve the adhesion with the layer provided thereon, the thermoplastic resin layer may be subjected to physical or chemical surface treatment such as oxidation or roughening on one or both sides as necessary. Examples of the oxidation method performed as the surface treatment of the thermoplastic resin layer include corona discharge treatment, chromium oxidation treatment, flame treatment, hot air treatment, ozone ultraviolet treatment, etc. Examples of the roughening method performed as the surface treatment of the thermoplastic resin layer include sandblasting and solvent treatment. These surface treatments are appropriately selected depending on the type of thermoplastic resin constituting the thermoplastic resin layer, and from the viewpoint of effect and operability, etc., corona discharge treatment is preferably used.
[0026] The thermoplastic resin layer may be colored or uncolored, for example, using a colorant. The thermoplastic resin layer may be colorless and transparent, colored and transparent, or translucent. The colorant used in the thermoplastic resin layer is not particularly limited, but is preferably a colorant that does not discolor even at a temperature of 150° C. or higher, and specifically includes existing dry colors, paste colors, masterbatch resin compositions, and the like.
[0027] The thickness of the thermoplastic resin layer is not particularly limited, but from the viewpoint of suitably achieving the effects of the present disclosure, it is preferably 100 μm or more, more preferably 150 μm or more, even more preferably 200 μm or more, and even more preferably 300 μm or more. From the same viewpoint, the thickness of the thermoplastic resin layer is preferably 950 μm or less, more preferably 600 μm or less, and even more preferably 500 μm or less. Preferred ranges of the thickness of the thermoplastic resin layer include about 100 to 950 μm, about 100 to 600 μm, about 100 to 500 μm, about 150 to 950 μm, about 150 to 600 μm, about 150 to 500 μm, about 200 to 950 μm, about 200 to 600 μm, about 200 to 500 μm, about 300 to 950 μm, about 300 to 600 μm, and about 300 to 500 μm. When the thermoplastic resin layer has an uneven shape, the thickness means the thickness at a position where no recesses are formed.
[0028] In the laminate sheet of the present disclosure, the thermoplastic elastomer layer and the thermoplastic resin layer may be in contact with each other, or another layer (such as an adhesive layer) may be laminated between these layers. That is, in addition to the thermoplastic elastomer layer and the thermoplastic resin layer, the laminate sheet of the present disclosure may further include another layer. Examples of the other layer include an adhesive layer, which will be described later. The other layer may be laminated between the thermoplastic elastomer layer and the thermoplastic resin layer, may be laminated on the side of the thermoplastic elastomer layer opposite to the thermoplastic resin layer side, or may be laminated on the side of the thermoplastic resin layer opposite to the thermoplastic elastomer layer side.
[0029] For example, the thermoplastic elastomer layer and the thermoplastic resin layer can be laminated, for example, via an adhesive layer. The adhesive layer laminated between the thermoplastic elastomer layer and the thermoplastic resin layer is a layer that bonds the thermoplastic elastomer layer and the thermoplastic resin layer. When the thermoplastic elastomer layer and the thermoplastic resin layer are laminated via an adhesive layer, the laminated sheet of the present disclosure can be manufactured by a dry lamination method. In addition, when the thermoplastic elastomer layer and the thermoplastic resin layer are laminated so that they come into contact with each other, a laminated film can be manufactured by subjecting the resins forming these layers to co-extrusion molding. In addition, the lamination of these layers can also be performed by a method such as a sand lamination method or a thermal lamination method. Preferred lamination configurations of the laminated sheet of the present disclosure include a two-layer configuration of a thermoplastic elastomer layer and a thermoplastic resin layer, and a three-layer configuration in which a thermoplastic elastomer layer, an adhesive layer, and a thermoplastic resin layer are laminated in this order.
[0030] The adhesive forming the adhesive layer is not particularly limited as long as it can bond the thermoplastic elastomer layer and the thermoplastic resin layer, and examples of the adhesive include polyester resins, polyether resins, polyurethane resins, epoxy resins, phenol resins, polyamide resins, polyolefin resins, polyvinyl acetate resins, cellulose resins, (meth)acrylic resins, polyimide resins, amino resins, rubber, silicone resins, etc. The thickness of the adhesive layer may be, for example, 1 to 10 μm.
[0031] The thickness of the laminate sheet of the present disclosure is not particularly limited, but from the viewpoint of suitably achieving the effects of the present disclosure, it is preferably 110 μm or more, more preferably 150 μm or more, even more preferably 200 μm or more, and even more preferably 300 μm or more. From the same viewpoint, the thickness of the laminate sheet is preferably 1000 μm or less, more preferably 800 μm or less, and even more preferably 600 μm or less. Preferred ranges of the thickness of the laminate sheet include about 110 to 1000 μm, about 110 to 800 μm, about 110 to 600 μm, about 150 to 1000 μm, about 150 to 800 μm, about 150 to 600 μm, about 200 to 1000 μm, about 200 to 800 μm, about 200 to 600 μm, about 300 to 1000 μm, about 300 to 800 μm, and about 300 to 600 μm. In addition, when the laminate sheet has an uneven shape, the thickness means the thickness at a position where no recesses are formed.
[0032] When forming a surface unevenness on the laminate sheet of the present disclosure, the unevenness can be suitably formed using a mold such as an embossing plate. That is, a laminate sheet having a surface unevenness can be obtained by embossing using a plate (embossing plate) that is manufactured so as to form a predetermined unevenness on the surface of the laminate sheet.
[0033] The embossing may be performed by any suitable known method, and is not particularly limited. A typical embossing method is, for example, as follows: The surface of the laminate sheet is heated and softened, and an embossing plate is pressed against the surface to form the uneven shape of the embossing plate on the laminate sheet surface. The laminate sheet is then cooled and solidified to fix the uneven shape on the surface of the laminate sheet. Thereafter, the laminate sheet with the uneven shape formed on the surface is released from the embossing plate.
[0034] When the surface of the laminate sheet 10 is uneven, the depth of the recesses is not particularly limited, but may be, for example, about 10 to 50 μm, about 50 to 150 μm, or about 150 to 200 μm.
[0035] The laminate sheet of the present disclosure is preferably subjected to molding at a temperature equal to or lower than the softening point of the thermoplastic elastomer contained in the thermoplastic elastomer layer and equal to or higher than the softening point of the thermoplastic resin contained in the thermoplastic resin layer. The molding method is not particularly limited, and examples thereof include an insert molding method and an injection molding simultaneous decoration method described later.
[0036] The uses of the laminate sheet of the present disclosure are not particularly limited, but since the uneven shape can be favorably maintained even when molded in a high-temperature, high-pressure environment, it can be favorably used as a base material for a decorative sheet.
[0037] A decorative sheet using the laminate sheet of the present disclosure will be described below.
[0038] 2.Decorative sheet The decorative sheet of the present disclosure preferably has a surface protective layer on the thermoplastic elastomer layer side of the laminate sheet of the present disclosure. The decorative sheet of the present disclosure preferably has a pattern layer on at least one of the thermoplastic elastomer layer side and the thermoplastic resin layer side of the laminate sheet of the present disclosure. For example, the schematic diagram of FIG. 4 shows a decorative sheet 20 having a surface protective layer 3, a pattern layer 4, and a primer layer 5 on the thermoplastic elastomer layer 1 side of the laminate sheet 10 of the present disclosure.
[0039] The decorative sheet of the present disclosure preferably has an uneven shape on the surface opposite to the laminate sheet side. By using the laminate sheet of the present disclosure described above as a base material for the decorative sheet, the surface uneven shape of the decorative sheet can be favorably maintained even when molded in a high-temperature and high-pressure environment. From the viewpoint of more favorably maintaining the surface uneven shape, it is preferable that the uneven shape corresponding to the surface uneven shape of the decorative sheet reaches the thermoplastic elastomer layer of the laminate sheet. For example, when the decorative sheet has a surface protective layer and a pattern layer on the thermoplastic elastomer layer side of the laminate sheet, it is preferable that the uneven shape of the surface of the decorative sheet is formed in the surface protective layer 3, the pattern layer 4, and the thermoplastic elastomer layer. For example, when the decorative sheet has a surface protective layer on the thermoplastic elastomer layer side of the laminate sheet and a pattern layer on the thermoplastic resin layer side of the laminate sheet, it is preferable that the uneven shape of the surface of the decorative sheet is formed in the surface protective layer 3 and the thermoplastic elastomer layer.
[0040] The decorative sheet of the present disclosure is preferably molded at a temperature below the softening point of the thermoplastic elastomer contained in the thermoplastic elastomer layer of the laminate sheet of the present disclosure described above, and at a temperature above the softening point of the thermoplastic resin contained in the thermoplastic resin layer.
[0041] As shown in the schematic diagram of Figure 4, when the decorative sheet 20 of the present disclosure has a surface protective layer 3, a primer layer 5 may be provided as necessary to improve adhesion between the surface protective layer 3 and the layer located below it (e.g., the laminate sheet 10, a pattern layer 4 that is provided as necessary, etc.).
[0042] The pattern layer 4, which is provided as necessary, is a layer that imparts decorativeness to the decorative sheet. The pattern layer 4 is suitably provided, for example, between the surface protective layer 3 and the laminate sheet 10. Furthermore, if the laminate sheet 10 is transparent, the pattern layer 4 can be provided on the opposite side of the laminate sheet 10 to the surface protective layer 3. That is, in this case, the decorative sheet has a pattern layer on the thermoplastic resin layer side, and the pattern layer can be observed through the transparent laminate sheet. Note that, with respect to the laminate sheet, the concept of transparency includes not only colorless transparency, but also colored transparency and translucency.
[0043] In addition, a concealing layer (not shown) may be provided between the laminate sheet 10 and the surface protective layer 3 or the pattern layer 4, if necessary, for the purpose of suppressing color change or variation in the laminate sheet 10. For example, if a primer layer 5 is provided, the concealing layer may be provided between the laminate sheet 10 and the primer layer 5, and if a pattern layer 4 is provided, the concealing layer may be provided between the laminate sheet 10 and the pattern layer 4.
[0044] Furthermore, for the purpose of improving abrasion resistance (scratch resistance), a transparent resin layer (not shown) may be provided as necessary. For example, in the case where the design layer 4 and the primer layer 5 are provided, the transparent resin layer may be provided between the design layer 4 and the primer layer 5.
[0045] Furthermore, in the decorative sheet of the present disclosure, a back adhesive layer (not shown) may be provided, if necessary, on the back surface of the decorative sheet (i.e., the surface on the laminated sheet side) in order to increase adhesion with the molding resin when the decorative sheet is molded.
[0046] Examples of the laminate structure of the decorative sheet of the present disclosure include a laminate structure in which a thermoplastic resin layer / thermoplastic elastomer layer / design layer is laminated; a laminate structure in which a thermoplastic resin layer / thermoplastic elastomer layer / surface protective layer is laminated; a laminate structure in which a thermoplastic resin layer / thermoplastic elastomer layer / design layer / surface protective layer is laminated; a laminate structure in which a thermoplastic resin layer / thermoplastic elastomer layer / design layer / primer layer / surface protective layer is laminated; a laminate structure in which a thermoplastic resin layer / thermoplastic elastomer layer / hiding ... Examples of such laminated structures include a laminated structure having a resin layer / thermoplastic elastomer layer / pattern layer / primer layer / surface protective layer; a laminated structure having a pattern layer / thermoplastic resin layer / thermoplastic elastomer layer / surface protective layer; a laminated structure having a pattern layer / thermoplastic resin layer / thermoplastic elastomer layer / primer layer / surface protective layer; a laminated structure having a back adhesive layer / pattern layer / thermoplastic resin layer / thermoplastic elastomer layer / surface protective layer; and a laminated structure having a back adhesive layer / pattern layer / thermoplastic resin layer / thermoplastic elastomer layer / primer layer / surface protective layer.
[0047] The design layer is formed, for example, by printing various patterns using ink and a printing machine. The pattern formed by the design layer is not particularly limited, and examples thereof include geometric patterns, wood grain patterns, stone patterns imitating the surface of rocks such as marble patterns (e.g., travertine marble patterns), fabric patterns imitating fabric grain or cloth-like patterns, tile patterns, brick masonry patterns, and patterns such as marquetry and patchwork that combine these. These patterns are formed by multi-color printing using ordinary process colors of yellow, red, blue, and black, as well as by multi-color printing using special colors that are performed by preparing plates of the individual colors that make up the pattern.
[0048] The design ink used in the design layer is a mixture of a binder with a suitable amount of a colorant such as a pigment or dye, an extender pigment, a solvent, a stabilizer, a plasticizer, a catalyst, a hardener, etc. The binder is not particularly limited, and examples thereof include polyurethane resins, vinyl chloride-vinyl acetate copolymer resins, mixed resins of vinyl chloride-vinyl acetate copolymers and acrylic copolymers, chlorinated polypropylene resins, acrylic resins, polyester resins, polyamide resins, butyral resins, polystyrene resins, nitrocellulose resins, and cellulose acetate resins. These resins may be used alone or in combination of two or more.
[0049] The colorant is not particularly limited, and examples thereof include inorganic pigments such as carbon black (ink), iron black, titanium white, antimony white, yellow lead, titanium yellow, red iron oxide, cadmium red, ultramarine blue, and cobalt blue; organic pigments or dyes such as quinacridone red, isoindolinone yellow, and phthalocyanine blue; metal pigments consisting of scaly foil flakes of aluminum, brass, and the like; and pearlescent pigments consisting of scaly foil flakes of titanium dioxide-coated mica, basic lead carbonate, and the like.
[0050] The thickness of the design layer is not particularly limited, but may be, for example, about 1 to 30 μm, and preferably about 1 to 20 μm.
[0051] The surface protective layer is a layer provided to enhance the scratch resistance and weather resistance of the decorative sheet. The surface protective layer can be formed using a thermoplastic resin, a thermosetting resin, an ionizing radiation curable resin, etc. Among these, the surface protective layer is preferably formed from a cured product of an ionizing radiation curable resin composition. The ionizing radiation curable resin used to form the surface protective layer is a resin that crosslinks and hardens by irradiation with ionizing radiation, and specifically includes a suitable mixture of at least one of prepolymers, oligomers, and monomers having polymerizable unsaturated bonds or epoxy groups in the molecule. Here, ionizing radiation means electromagnetic waves or charged particle beams that have an energy quantum capable of polymerizing or crosslinking molecules, and usually ultraviolet rays (UV) or electron beams (EB) are used, but also includes electromagnetic waves such as X-rays and gamma rays, and charged particle beams such as alpha rays and ion beams. Among ionizing radiation curable resins, electron beam curable resins are preferably used in the formation of the surface protective layer because they can be made solvent-free, do not require a photopolymerization initiator, and have stable curing properties.
[0052] The thickness of the surface protective layer is not particularly limited, but from the viewpoint of improving the scratch resistance, weather resistance, etc. of the decorative sheet, it is, for example, 5 to 20 μm, and preferably 5 to 10 μm.
[0053] The primer layer is a layer that is provided, if necessary, in contact with the surface protective layer for the purpose of increasing the adhesion between the surface protective layer and the layer located thereunder.
[0054] As the primer composition constituting the primer layer, those containing urethane resin, (meth)acrylic resin, (meth)acrylic-urethane copolymer resin, vinyl chloride-vinyl acetate copolymer, polyester resin, butyral resin, chlorinated polypropylene, chlorinated polyethylene, etc. as a binder resin are preferably used, and these resins can be used alone or in combination of two or more. Among these, urethane resin, (meth)acrylic resin, and (meth)acrylic-urethane copolymer resin are preferred.
[0055] The concealing layer is provided to prevent the laminated sheet used as the base material from adversely affecting the color tone and pattern of the decorative sheet, and is therefore generally formed as a layer of an opaque color.
[0056] The concealing layer is formed by using an ink composition in which a binder is appropriately mixed with a colorant such as a pigment or a dye, an extender pigment, a solvent, a stabilizer, a plasticizer, a catalyst, a hardener, etc. The ink composition for forming the concealing layer is appropriately selected from those used for the above-mentioned design layer.
[0057] The concealing layer is usually set to a thickness of about 1 to 20 μm, and is desirably formed as a so-called solid print layer.
[0058] The back surface adhesive layer is made of a thermoplastic resin or a curable resin depending on the molding resin used in the decorated resin molded product.
[0059] Examples of thermoplastic resins used to form the back surface adhesive layer include acrylic resins, acrylic-modified polyolefin resins, chlorinated polyolefin resins, vinyl chloride / vinyl acetate copolymers, thermoplastic urethane resins, thermoplastic polyester resins, polyamide resins, rubber-based resins, etc. These thermoplastic resins may be used alone or in combination of two or more.
[0060] Examples of the thermosetting resin used to form the back adhesive layer include urethane resin, Epoxy resins, etc. These thermosetting resins may be used alone or in combination of two or more.
[0061] When forming a surface uneven shape on the decorative sheet of the present disclosure, the uneven shape can be suitably formed using a mold such as an embossing plate. That is, the decorative sheet can be obtained by embossing using a plate (embossing plate) that is manufactured so as to form a predetermined uneven shape on the surface of the decorative sheet.
[0062] The embossing may be performed by any suitable known method, and is not particularly limited. A typical method of embossing is as follows: The surface of the decorative sheet is heated and softened, and an embossing plate is pressed against the surface to form the uneven shape of the embossing plate on the surface of the decorative sheet. The decorative sheet is then cooled and solidified to fix the uneven shape on the surface of the decorative sheet. The decorative sheet with the uneven shape formed on the surface is then released from the embossing plate.
[0063] Alternatively, a decorative sheet having an uneven surface can be produced by sequentially laminating a design layer, a surface protective layer, etc. on the uneven surface of a laminate sheet having an uneven surface in advance.
[0064] The uses of the decorative sheet are not particularly limited, and examples thereof include interior materials for buildings such as walls, floors, and ceilings; exterior materials for building exterior walls, roofs, gates, walls, and fences; surface materials for fittings such as doors, window frames, and door frames, moldings, baseboards, handrails, and other fixtures; surface materials for the housings of home appliances such as television sets and refrigerators; surface materials for furniture such as chests of drawers; surface materials for containers such as boxes and plastic bottles; interior or exterior materials for vehicles, and interior or exterior materials for ships.
[0065] 3. Decorative resin moldings The decorated resin molded product of the present disclosure is formed by integrating a molded resin with the decorative sheet of the present disclosure. That is, the decorated resin molded product of the present disclosure includes a molded resin layer and the decorative sheet of the present disclosure. As described above, the decorative sheet of the present disclosure preferably has an uneven surface, and when the decorative sheet has an uneven surface, the decorated resin molded product of the present disclosure includes at least the molded resin layer and the decorative sheet of the present invention, and is a decorated resin molded product having an uneven surface on the side opposite to the molded resin layer.
[0066] FIG. 5 shows a cross-sectional structure of one embodiment of the decorated resin molded product of the present disclosure.
[0067] The case where the decorated resin molded product of the present disclosure is manufactured using the decorative sheet of the present disclosure will be described below. In addition, when the decorated resin molded product of the present disclosure does not have a surface protection layer or a pattern layer, the decorated resin molded product may be manufactured using the laminate sheet of the present disclosure.
[0068] The decorated resin molded product of the present disclosure can be produced, for example, by a method including a step of forming a molded resin layer by injecting a resin onto the laminate sheet side of the decorative sheet of the present disclosure. Specifically, the decorated resin molded product is produced by various injection molding methods such as insert molding, simultaneous injection molding and decoration, blow molding, and gas injection molding using the decorative sheet of the present disclosure.
[0069] In the insert molding method, first, in a vacuum forming step, the decorative sheet of the present disclosure is vacuum-formed in advance into the surface shape of the molded product (offline preforming) using a vacuum forming mold, and then excess parts are trimmed as necessary to obtain a molded sheet. This molded sheet is inserted into an injection mold, the injection mold is closed, and a resin in a fluid state is injected into the mold and solidified. At the same time as injection molding, the laminated sheet side of the decorative sheet is integrated with the outer surface of the resin molded product, thereby producing a decorated resin molded product.
[0070] More specifically, the decorated resin molded product of the present disclosure is produced by an insert molding method including the following steps.
[0071] A vacuum forming process in which the decorative sheet of the present disclosure is formed into a three-dimensional shape in advance using a vacuum forming mold; A step of trimming an excess portion of the vacuum-formed decorative sheet to obtain a formed sheet; and A process in which the molded sheet obtained in the previous process is inserted into an injection mold, the injection mold is closed, and the resin in a fluid state is injected into the mold to integrate the resin and the molded sheet.
[0072] In the vacuum forming step in the insert molding method, the decorative sheet may be heated and molded. The heating temperature at this time is not particularly limited and may be appropriately selected depending on the type of resin constituting the decorative sheet and the thickness of the decorative sheet. For example, when an ABS resin film is used as the thermoplastic resin of the laminated sheet, the heating temperature can be usually about 100 to 250°C, preferably about 130 to 200°C. In addition, in the integration step, the temperature of the resin in a fluid state is not particularly limited, but can be usually about 180 to 320°C, preferably about 220 to 280°C. As described above, it is preferable that the molding of the decorative sheet is performed at a heating temperature that is equal to or lower than the softening point of the thermoplastic elastomer contained in the thermoplastic elastomer layer of the laminated sheet and equal to or higher than the softening point of the thermoplastic resin contained in the thermoplastic resin layer.
[0073] For example, when manufacturing a decorated resin molded product by laminating at least a molded resin layer and the decorative sheet of the present invention, the method for manufacturing a decorated resin molded product can include the steps of preparing a laminated sheet of the present invention, and molding the decorative sheet at a temperature below the softening point of the thermoplastic elastomer and above the softening point of the thermoplastic resin, and laminating it with the molded resin layer.
[0074] In addition, in the simultaneous injection molding decoration method, the decorative sheet of the present disclosure is placed in a female mold that also serves as a vacuum forming mold and is provided with suction holes for injection molding, and preforming (in-line preforming) is performed using this female mold.The injection molding mold is then clamped, and the resin in a fluid state is injected to fill the mold and solidify.The laminate sheet side of the decorative sheet of the present disclosure is integrated with the outer surface of the resin molded product at the same time as the injection molding to produce a decorated resin molded product.
[0075] More specifically, the decorated resin molded article of the present disclosure is produced by a simultaneous injection molding and decoration method including the following steps.
[0076] a step of preforming the decorative sheet by placing the decorative sheet of the present disclosure against a molding surface of a movable mold having a predetermined shape, with the side of the decorative sheet opposite the laminated sheet facing the molding surface of the movable mold, heating and softening the decorative sheet and vacuum-suctioning the softened decorative sheet from the movable mold side to bring the softened decorative sheet into close contact with the molding surface of the movable mold; an injection molding process in which a movable mold and a fixed mold having a decorative sheet in close contact with each other along their molding surfaces are clamped together, and then a resin molding material in a fluid state is injected into a cavity formed by both molds, filled therein, and solidified to laminate and integrate the formed resin molded body and the decorative sheet; A process of separating the movable mold from the fixed mold to remove a resin molded body including all layers of the decorative sheet laminated thereon.
[0077] In the preforming step of the simultaneous injection molding and decoration method, the heating temperature of the decorative sheet is not particularly limited and may be appropriately selected depending on the type of resin constituting the decorative sheet, the thickness of the decorative sheet, etc., but when a polyester resin film or an acrylic resin film is used as the thermoplastic resin layer of the laminated sheet, it can usually be about 70 to 130° C. In addition, in the injection molding step, the temperature of the resin in a fluid state is not particularly limited, but can usually be about 180 to 320° C., preferably about 220 to 280° C.
[0078] In addition, the decorated resin molded product of the present disclosure can also be produced by a decoration method, such as vacuum pressure bonding, in which the decorative sheet of the present disclosure is attached to a three-dimensional resin molded body (molded resin layer) prepared in advance.
[0079] In the vacuum bonding method, first, the decorative sheet and the resin molded body of the present disclosure are placed in a vacuum bonding machine consisting of a first vacuum chamber located on the upper side and a second vacuum chamber located on the lower side, so that the decorative sheet faces the first vacuum chamber side, the resin molded body faces the second vacuum chamber side, and the laminated sheet side of the decorative sheet faces the resin molded body side, and the two vacuum chambers are placed in a vacuum state. The resin molded body is placed on a lifting platform provided on the second vacuum chamber side that can be raised and lowered up and down. Next, the first vacuum chamber is pressurized, and the lifting platform is used to press the molded body against the decorative sheet, and the decorative sheet is attached to the surface of the resin molded body while being stretched by utilizing the pressure difference between the two vacuum chambers. Finally, the two vacuum chambers are opened to atmospheric pressure, and the excess part of the decorative sheet is trimmed as necessary, thereby obtaining the decorated resin molded product of the present disclosure.
[0080] In the vacuum pressure bonding method, it is preferable to include a step of heating the decorative sheet before the step of pressing the above-mentioned molded body against the decorative sheet in order to soften the decorative sheet and improve its formability. The vacuum pressure bonding method including this step is sometimes called a vacuum heat and pressure bonding method. The heating temperature in this step may be appropriately selected depending on the type of resin constituting the decorative sheet and the thickness of the decorative sheet, but when a polyester resin film or an acrylic resin film is used as the heat-fusible resin layer of the laminated sheet, it can usually be about 60 to 200°C.
[0081] In the decorated resin molded product of the present disclosure, the molded resin layer may be formed by selecting a molding resin according to the application. The molding resin may be a thermoplastic resin or a thermosetting resin.
[0082] Examples of thermoplastic resins used as molding resins include polyolefin resins such as polyethylene and polypropylene, ABS resins, styrene resins, polycarbonate resins, acrylic resins, vinyl chloride resins, etc. These thermoplastic resins may be used alone or in combination of two or more.
[0083] Examples of the thermosetting resin used as the molding resin include urethane resin, epoxy resin, etc. These thermosetting resins may be used alone or in combination of two or more.
[0084] The decorated resin molded product of the present disclosure can be used, for example, as interior or exterior materials for vehicles such as automobiles; fixtures such as baseboards and moldings; window frames, door frames and other fittings; interior materials for buildings such as walls, floors and ceilings; housings for home appliances such as television sets and air conditioners; containers, etc. EXAMPLES
[0085] The present disclosure will be described in detail below with reference to examples and comparative examples. However, the present disclosure is not limited to the examples.
[0086] Example 1 Using a two-type, two-layer T-die extruder, a thermoplastic elastomer (polyester-based elastomer, softening point 163°C) and a thermoplastic resin (ABS resin, softening point 107°C) were co-extruded to obtain a two-layer laminated sheet (480 μm) consisting of a thermoplastic elastomer layer (thickness 80 μm) and a thermoplastic resin layer (thickness 400 μm).
[0087] Next, the obtained laminated sheet was embossed from the thermoplastic elastomer layer side to obtain a decorative sheet having an uneven surface on the thermoplastic elastomer layer side. The embossing was performed using a heatable press and an embossing mold. The embossing mold had a fine line pattern. The embossing height of the decorative sheet having an uneven surface was measured using a laser microscope. This embossing height was defined as the embossing height before molding (reference 100%). The results are shown in Table 1.
[0088] Next, the decorative sheet with the surface irregularities formed was subjected to vacuum forming and injection molding. Specifically, the decorative sheet was heated to a surface temperature of 140°C by an infrared heater (the hot plate used for heating was 270°C, and the heating time was 20 to 25 seconds), and preformed to conform to the shape (plate shape) in the mold by vacuum forming (maximum stretching ratio 10%). The shape of the decorative sheet after vacuum forming was such that the thermoplastic elastomer layer side was convex and the thermoplastic resin layer side was concave. The emboss height of the decorative sheet after vacuum forming was measured with a laser microscope. The emboss height and the retention rate (%) relative to the standard 100% are shown in Table 1. The emboss height was measured at a portion where the decorative sheet was not substantially stretched (stretching ratio about 0%).
[0089] Next, the vacuum-formed decorative sheet was fitted into a mold (temperature 60°C), and the injection resin was injected into the cavity of the mold, and the thermoplastic resin layer side of the decorative sheet and the injection resin (230°C) were integrally molded (injection pressure 160 MPa), and the molded product was obtained by removing it from the mold. The emboss height of the decorative sheet (after injection molding) constituting the surface of the molded product was measured using a laser microscope. The emboss height and the retention rate (%) relative to the standard of 100% are shown in Table 1. The emboss height was measured at a point where the decorative sheet was not substantially stretched (stretch ratio of about 0%).
[0090] Example 2 A decorative sheet was produced in the same manner as in Example 1, except that the thickness of the thermoplastic elastomer layer was 140 μm and the thickness of the thermoplastic resin layer was 340 μm, and the decorative sheet was subjected to embossing and vacuum forming, and the emboss height of each was measured. The emboss height and the retention rate (%) relative to the standard of 100% are shown in Table 1.
[0091] Comparative Example 1 Except for using a single-layer sheet (thickness 480 μm) of thermoplastic resin (ABS resin, softening point 107° C.), the single-layer sheet was subjected to embossing, vacuum forming, and injection molding in the same manner as in Example 1, and the emboss height of each was measured. The emboss height and the retention rate (%) relative to the standard of 100% are shown in Table 1.
[0092] Comparative Example 2 A laminated sheet was produced in the same manner as in Example 1, except that a thermoplastic elastomer (polyester-based elastomer, softening point 104°C) was used instead of the thermoplastic elastomer (polyester-based elastomer, softening point 163°C), and the laminated sheet was subjected to embossing and vacuum forming, and the emboss height of each was measured. The emboss height and the retention rate (%) relative to the above-mentioned standard of 100% are shown in Table 1. In Comparative Example 2, the emboss height became 0 μm due to vacuum forming, so injection molding was omitted.
[0093] [Table 1]
[0094] The laminated sheet of Example 1 is formed by laminating a thermoplastic elastomer layer and a thermoplastic resin layer, and the softening point of the thermoplastic elastomer contained in the thermoplastic elastomer layer is higher than the softening point of the thermoplastic resin contained in the thermoplastic resin layer. As is clear from the results shown in Table 1, the decorative sheet of Example 1 can maintain the uneven shape favorably even when molded in a high-temperature and high-pressure environment. In contrast, the uneven shape cannot be favorably maintained in Comparative Example 1, which is a single-layer film of ABS resin, and Comparative Example 2, in which the softening point of the thermoplastic elastomer layer is lower than that of the thermoplastic resin layer. In addition, when the vacuum molding temperature of the decorative sheet of Example 1 was set to 180°C, which is higher than the softening point of the thermoplastic elastomer of 163°C, the embossing height after vacuum molding was lower than that of Example 1, in which the vacuum molding temperature was 140°C. From this, it can be seen that the decorative sheet of the present disclosure can more favorably maintain the uneven shape by being molded at a temperature lower than the softening point of the thermoplastic elastomer and higher than the softening point of the thermoplastic resin. [Explanation of symbols]
[0095] 1 Thermoplastic elastomer layer 2 Thermoplastic resin layer 3 Surface protective layer 4. Picture layer 5 Primer layer 6 Molded resin layer 10 Laminated sheet 20 Decorative sheet 30 Decorative resin moldings
Claims
1. A laminate sheet used as a base material for a decorative sheet having an uneven surface, The laminate sheet is formed by laminating at least a thermoplastic elastomer layer and a thermoplastic resin layer, the softening point of the thermoplastic elastomer contained in the thermoplastic elastomer layer is higher than the softening point of the thermoplastic resin contained in the thermoplastic resin layer; The thickness of the thermoplastic resin layer is 100 μm or more, A laminated sheet, wherein the thermoplastic resin layer side is integrally formed with a molded resin layer by injection molding.
2. 2. The laminate sheet according to claim 1, wherein the difference between the softening point of the thermoplastic elastomer and the softening point of the thermoplastic resin is 10° C. or more.
3. The laminate sheet according to claim 1 or 2, wherein the thermoplastic elastomer layer and the thermoplastic resin layer are in contact with each other.
4. The laminate sheet according to claim 1 or 2, wherein the thermoplastic elastomer layer and the thermoplastic resin layer are laminated via an adhesive layer.
5. A decorative sheet comprising the laminate sheet according to any one of claims 1 to 4, The thermoplastic resin layer is integrally molded with the molded resin layer by injection molding, The decorative sheet has an uneven surface on the side of the thermoplastic elastomer layer.
6. The decorative sheet according to claim 5 , further comprising a surface protective layer on the thermoplastic elastomer layer side of the laminate sheet.
7. The decorative sheet according to claim 5 or 6, further comprising a pattern layer on at least one of the thermoplastic elastomer layer side of the laminate sheet and the thermoplastic resin layer side of the laminate sheet.
8. A decorated resin molded product comprising at least the molded resin layer and the decorative sheet according to any one of claims 5 to 7.
9. A method for producing a decorated resin molded product, comprising laminating at least the molded resin layer and the decorative sheet according to any one of claims 5 to 7, A step of preparing a decorative sheet according to any one of claims 5 to 7; a step of forming the decorative sheet at a temperature equal to or lower than the softening point of the thermoplastic elastomer and equal to or higher than the softening point of the thermoplastic resin, and laminating the decorative sheet with the formed resin layer; A method for manufacturing a decorated resin molded product comprising the steps of:
Citation Information
Patent Citations
JP1975019132A
Tape loading mechanism of magnetic recording and reproducing device
JP1986017255A
Highly durable leathery sheet and its production
JP1993025780A
Molding method of decorating molded article and equipment therefor
JP2004322501A
Laminated sheet for coating metal sheet and laminated sheet-coated metal sheet
JP2008254348A