Granulated silica powder and method for producing the same
The granulated silica powder with tailored properties addresses the issues of fluidity and melting uniformity in quartz glass production, ensuring high purity and reduced bubble formation in molded products.
Patent Information
- Application Number
- JP2020158922
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-23
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-09-23
AI Technical Summary
Conventional silica powders with a particle size of 100 μm to 200 μm exhibit poor fluidity and uneven melting, leading to non-uniformity and bubble formation in quartz glass molded products.
Development of granulated silica powder with specific properties, including a D50 particle size of 75 μm to 200 μm, an angle of repose of 20 to 35 degrees, and a specific surface area of 0.3 to 10 m²/g, produced through a sol-gel method, slurry granulation, and firing at 1000°C to 1300°C, using polyvinylpyrrolidone as a binder.
The granulated silica powder provides high purity and excellent fluidity, resulting in a highly uniform molded product with suppressed bubble generation.
Smart Images

Figure 0007567316000001 
Figure 0007567316000002 
Figure 0007567316000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a granulated silica powder suitable for producing semiconductor jigs and optical fibers made of quartz glass. [Background technology]
[0002] The Verneuil process and plasma spraying are known as methods for manufacturing quartz glass molded bodies. In these methods, silica powder is passed through the high-temperature region of an oxyhydrogen flame or plasma by dropping or spraying, and in a molten state, it is attached to a substrate and laminated to produce a quartz glass molded body. The silica powder used here is natural quartz powder with a particle size of 100μm to 200μm, or synthetic quartz powder derived from the sol-gel process. For example, Patent Document 1 proposes that silica gel obtained by the sol-gel method is dried in a dryer and then fired to obtain synthetic quartz powder that can provide a quartz glass molded body with reduced impurities and foaming. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 4391529 Summary of the Invention [Problem to be solved by the invention]
[0004] However, conventionally used natural silica powders and synthetic silica powders with particle sizes of 100 μm to 200 μm have problems such as poor flowability due to their crushed particle shape, and a tendency for uneven melt viscosity within the particle, in which the particle surface melts but the center is insufficiently melted. These problems cause non-uniformity in molded products, such as striae, and improvements are desired.
[0005] That is, the properties of silica powder required for the Verneuil process and the plasma spraying process are (I) appropriate fluidity (ability to feed quantitatively to high temperature regions), (II) ease of melting, (III) ability to produce bubble-free molded products, and (IV) ability to obtain uniform molded products. In short, there is a demand for silica powder that is high in purity, has good fluidity, and can produce highly uniform molded products with suppressed bubble generation. An object of the present invention is to provide a silica powder that satisfies such requirements. [Means for solving the problem]
[0006] The present inventors have conducted intensive research under the above circumstances, and have found that a granulated silica powder produced by granulating silica fine particle powder having a specific particle size can solve the above problems, thereby completing the present invention. The present invention includes the following.
[0007] (1) The D50 particle size (median diameter) is 75 μm or more and 200 μm or less, the angle of repose is 20 degrees or more and 35 degrees or less, and the specific surface area is 0.3 m 2 / g or more 10m 2 / g or less, The granulated silica powder is an agglomerated particle containing 15% to 40% of particles having a particle diameter of 10 μm or less. (2) The granulated silica powder according to (1), having a silanol concentration of 200 ppm or less and an adsorbed moisture content of 1% or less. (3) A granulated silica powder according to (1) or (2), having an Fe content of 1 ppm or less, an Al content of 0.1 ppm or less, and a Ti content of 0.01 ppm or less. (4) The manufacturing method according to any one of (1) to (3), wherein the average pore size is 1 μm or more and 10 μm or less. Granular silica powder. (5) preparing raw silica obtained by a sol-gel method, the raw silica containing particles having a particle diameter of 10 μm or less at 15% to 40%; A granulation step in which the raw silica is slurried, a binder is added, and the mixture is spray-granulated; and A method for producing a granulated silica powder, comprising: a calcining step of calcining the obtained granulated particles at 1000°C or higher and 1300°C or lower. (6) The method for producing a granulated silica powder according to (5), wherein in the granulation step, the medium used for slurrying is water and the binder is polyvinylpyrrolidone. Effect of the Invention
[0008] According to the present invention, it is possible to provide a granulated silica powder which has high purity, good flowability, and enables the production of highly uniform molded products with reduced bubble generation. [Brief description of the drawings]
[0009] [Figure 1A] 1 is a graph showing the particle size distribution of raw material silica powder used in the examples. [Figure 1B] 1 is a graph showing the particle size distribution of raw material silica powder used in the examples. [Diagram 2] 1 is a graph showing the measurement results of particle size of granulated silica powder obtained in the examples. [Diagram 3] 1 shows an SEM image of the granulated silica powder obtained in the example (a photograph in place of a drawing). [Figure 4] FIG. 2 is a schematic diagram showing a Verneuil process (oxyhydrogen flame fusion process) apparatus used in the examples. [Diagram 5] 1 is an image of an ingot produced in an embodiment (a photograph substituting a drawing). [Figure 6] 1 shows an SEM image of the granulated silica powder obtained in the comparative example (a photograph substituting a drawing). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below. However, the description of the constituent elements described below is one example (representative example) of an embodiment of the present invention, and the present invention is not limited to these contents, and can be implemented in various modifications within the scope of the gist of the present invention.
[0011] One embodiment of the present invention is a granular material having a D50 particle size (median diameter) of 75 μm or more and 200 μm or less, an angle of repose of 20 degrees or more and 35 degrees or less, and a specific surface area of 0.3 m 2 / g or more 10m 2 / g or less, wherein the granulated silica powder is an agglomerated particle containing 15% to 40% particles with a particle diameter of 10 μm or less. Conventionally used natural silica powders and synthetic silica powders with particle sizes of 100 μm to 200 μm have problems such as poor fluidity due to their crushed particle shape, and a tendency for uneven melt viscosity within the particle, in which the particle surface melts but the center is not fully melted. In this embodiment, however, the above problems can be solved by using a granulated silica powder with specific properties.
[0012] By using granulated silica powder, it is possible to produce spherical particles with good flowability, and since the granulated particles are produced by granulating fine particles, there is less uneven melting when the particles are melted.
[0013] The granulated silica powder has a D50 particle size (median size) of 75 μm or more and 200 μm or less, preferably 100 μm or more and 150 μm or less. The median size is the particle size at which the cumulative frequency is 50%, and can be calculated by plotting a particle size distribution curve as shown in Figure 2, as an example of a calculation method. By setting the D50 particle size of the granulated silica powder in the above range, the flowability is high and the quantitative transfer of the powder is good. The D50 particle size of the granulated particles can be calculated from the particle size distribution by the sieving method or the laser diffraction scattering method, and the D50 particle size can be adjusted to the above range by classification using a sieve or the like.
[0014] The granulated silica powder has an angle of repose of 20 degrees or more and 35 degrees or less, preferably 25 degrees or more and 30 degrees or less. By setting the angle of repose of the granulated silica powder within the above range, the fluidity is high and the quantitative transfer of the powder is good. The angle of repose can be measured using a cylinder rotation method angle of repose measuring device (manufactured by Tsutsui Rikagaku Kikai Co., Ltd.). The method for adjusting the angle of repose is not particularly limited, but the angle of repose can be adjusted to within the above range by using a raw material of a specific particle size described in this specification and granulating it by a spray granulation method.
[0015] Granulated silica powder has a specific surface area of 0.3 m 2 / g or more 10m 2 / g or less, and 0.5m 2 / g or more, and 2 It is preferable that the molecular weight is not more than 1 / g. By setting the specific surface area of the granulated silica powder within the above range, the powder can be used to obtain a highly uniform molded product with reduced bubble generation. The specific surface area can be measured using a mercury porosimeter, and the specific surface area can be adjusted to within the above range by granulating the granulated silica powder using a spray granulation method using a raw material with a particle size as described below.
[0016] The granulated silica powder of this embodiment is an agglomerated particle granulated from silica fine particles, and is an agglomerated particle containing 15% or more and 40% or less of particles with a particle diameter of 10 μm or less, preferably containing 20% or more, and preferably containing 30% or less of particles with a particle diameter of 10 μm or less. By including particles with a particle size of 10 μm or less in the above range, the fine particles function as a binder during firing, improving the strength of the granulated molded body, and the pore size and pore volume of the granulated silica powder become appropriate values. In addition, with regard to the removal of silanol, which causes bubbles in the molded body, the finer the particles, the faster the silanol removal speed, which is advantageous for reducing the silanol concentration in the granulated product.
[0017] The amount of particles with a particle size of 10 μm or less contained in the granulated silica powder can be determined by sieving or laser diffraction scattering method before granulation, and the method is not limited if it is after granulation, and it can be measured by crushing the granulated powder using ultrasound or the like to an extent that the original silica is not crushed, and by SEM observation or laser diffraction scattering particle size distribution measurement. In a particularly simple case, the particles may be embedded and cut as appropriate, and the proportion of particles with a particle size of 10 μm or less may be estimated based on that.
[0018] The granulated silica powder of this embodiment has a silanol concentration of preferably 200 ppm or less, more preferably 100 ppm or less. By setting the silanol concentration within the above range, the amount of water vapor generated from silanol during melting is reduced, and the generation of bubbles derived from water vapor in the glass molded body is suppressed, which is preferable. The silanol concentration can be measured by an infrared spectrophotometer. In addition, the granulated silica powder preferably has an adsorbed moisture content of 1% or less, more preferably 0.1% or less. By setting the adsorbed moisture content within the above range, the generation of bubbles derived from water vapor in the glass molded body is suppressed, similar to silanol, and is therefore preferable. The adsorbed moisture content can be measured by an infrared moisture meter. The silanol concentration and the adsorbed water content can be adjusted to the desired range by adjusting the firing temperature and firing time in the production of the granulated silica powder.
[0019] The granulated silica powder preferably has an Fe content of 1 ppm or less, an Al content of 0.1 ppm or less, and a Ti content of 0.01 ppm or less. Such a low metal content makes the silica powder suitable for manufacturing semiconductor jigs and optical fibers. The metal content can be measured by inductively coupled plasma mass spectrometry (ICP-MS) after dissolving the granulated silica powder with hydrofluoric acid.
[0020] The granulated silica powder preferably has an average pore size of 1 μm or more and 10 μm or less. It is more preferable that the average pore size is 0.15 cc / g or more and 0.35 cc / g or less, and more preferably 0.2 cc / g or more and 0.3 cc / g or less. The average pore size and the average pore volume are in the above ranges, which is preferable because they can produce a powder that can produce a highly uniform molded product with reduced bubble generation. The average pore size and the average pore volume can be measured by a mercury porosimeter.
[0021] The crushing strength of the granulated silica powder must be strong enough not to collapse during handling, but if the strength is too high, gas escape during melting becomes poor. Therefore, the crushing strength is preferably 0.5 MPa or more and 10 MPa or less, and more preferably 1 MPa or more and 5 MPa or less. The crushing strength can be measured using a microcompression tester.
[0022] The method for producing the granulated silica powder of the present embodiment will be described below. The method for producing the granulated silica powder is another embodiment of the present invention. Another aspect of the present invention is a method for producing a granulated silica powder, the method comprising: a preparation step of preparing raw silica powder obtained by a sol-gel method, the raw silica powder containing 15% to 40% particles with a particle diameter of 10 μm or less; a granulation step of slurried the raw silica powder, adding a binder, and spray granulating the slurry; and a firing step of firing the obtained granulated particles at 1000°C to 1300°C.
[0023] <Preparation steps> The preparation step is a step of preparing raw silica powder obtained by the sol-gel method, containing 15% to 40% particles with a particle diameter of 10 μm or less. Silica powder produced by the sol-gel method is highly pure and tends to have an appropriate particle diameter. Therefore, it has a low metal content and is preferable as a raw material for semiconductors. In addition, it has excellent dispersibility in the slurry preparation in the granulation step described later.
[0024] Furthermore, by including the fine particles having a particle diameter of 10 μm or less in the above ratio, the fine particles act as a binder appropriately, and the pore diameter and pore volume of the granulated silica powder become appropriate values. In addition, since it is possible to remove silanol, which is a cause of bubbles in the molded body, the strength of the granulated molded body can be improved. The sol-gel method can be carried out by a known method, and from the standpoint of purity, it is preferable to carry out hydrolysis using tetramethoxysilane or tetraethoxysilane as the silicon source.
[0025] <Granulation step> The granulation step is a step in which the raw silica is slurried, a binder is added, and the mixture is sprayed and granulated. Granulation makes it possible to make the granulated silica powder spherical, and by adopting this method, contamination can be suppressed.
[0026] The solvent used for making the slurry is usually water, but is not limited to this as long as it can be used as a dispersion medium during granulation. The viscosity of the slurry is not particularly limited. A binder may also be added during the preparation of the slurry. The binder is preferably a substance that does not remain in the final granulated silica powder, and is preferably an organic binder that can be burned, decomposed, and removed by firing after granulation. Examples of organic binders include natural polymers, semi-synthetic polymers, and synthetic polymers. From the viewpoint of purity, synthetic polymers such as acrylic polymers, polyacrylamide, polyvinylpyrrolidone, and polyvinyl alcohol are preferred, and polyvinylpyrrolidone is particularly preferred. When using a binder, it is usually used in a ratio of 3 parts by weight to 10 parts by weight per 100 parts by weight of raw silica. The spraying may be performed using a known spray (sprayer) without any particular limitation. The granulated silica produced in the granulation step may be dried.
[0027] <Firing step> The firing step is a step in which the obtained granulated particles are fired at 1000°C or more and 1300°C or less. If the firing temperature is low, the strength of the granulated product will be low, and if the firing temperature is too high, the granulated powder will stick to each other, which is not preferable. The firing temperature is preferably 1100°C or more and 1250°C or less. The firing time affects the strength, and the firing time is usually 10 hours or more and 100 hours or less, preferably 30 hours or more and 60 hours or less. The atmosphere during firing is not particularly limited, but it is preferable to perform the firing in a dry air atmosphere, and the dry air preferably has a dew point of -40°C or less.
[0028] The granulated silica powder is melted by a known method such as the Verneuil method or plasma spraying method to form a glass molded body. The melting conditions are not particularly limited. EXAMPLES
[0029] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to the following examples.
[0030] <Example> (1) Preparation of raw silica powder TMOS (tetramethoxysilane) and 6 times the molar ratio of water were added to a jacketed horizontal cylindrical reactor with ribbon-type stirring blades, and 50°C hot water was passed through the jacket to hydrolyze TMOS, and the resulting wet gel was extracted. The extracted wet gel was pulverized using a high-speed rotary mill-type grinder with a pore size of 1 mm (Quadro, Comil), and the pulverized material was dried at 150°C to obtain a dried silica gel powder. This powder was classified using a sieve with a mesh size of 125 μm, and the powder below the sieve was further classified using a sieve with a finer mesh size to obtain raw silica powder. Two types of raw silica powder, A and B, were prepared, and the particle size distribution of the powder is shown in Figures 1A and 1B. The proportion of particles with a particle size of 10 μm or less was 25% for A and 35% for B.
[0031] (2) Granulation The raw material silica powder prepared in (1) above was dispersed in water to form a slurry containing 30% by weight of raw material silica. Further, as a granulation binder, 5 parts by weight of polyvinylpyrrolidone was added per 100 parts by weight of the raw material silica powder. This slurry was spray-dried at a drying gas temperature of 150 °C using a spray dryer (manufactured by Pulis Co., Ltd.) to obtain granulated particles. These granulated particles were heated at 1220 °C for 40 hours in an air (dew point -68 °C) atmosphere to obtain a granulated silica powder. The physical properties of the obtained granulated silica powder were measured as follows.
[0032] <Particle size distribution> The results of measuring the particle size of the obtained granulated silica powder by sieving are shown in Figure 2. The particle sizes of the granulated silica powders A and B produced from the raw material silica powders A and B were the same. The D50 particle size (median diameter) was 130 μm as shown in the figure. This D50 particle size (median diameter) was determined by using stainless steel JIS standard sieves with mesh openings of 45, 75, 106, 125, 150, 212, and 250 μm in sequence, measuring the passing weight, graphing the cumulative passing weight using Excel, drawing a smooth line, and using this to find the point where the cumulative percentage is 50%.
[0033] <SEM image> Figure 3 shows the SEM image of the obtained granulated silica powder. The particles are spherical (A), and it can be seen that when magnified (B), small particles exist in the gaps between the large particles. <Angle of repose> As a result of measuring the angle of repose of the obtained granulated silica powder using a cylindrical rotation method angle of repose measuring device (manufactured by Tsutsui Rikagaku Kikai Co., Ltd.), the angle of repose of both granulated silica powders A and B was 28 degrees.
[0034] <Specific surface area> As a result of measuring the specific surface area of the obtained granulated silica powder using a mercury porosimeter, the specific surface area of A was 0.68 m 2 / g, and that of B was 2.2 m 2 / g. The pore volume of A was 0.25 cc / g, and that of B was 0.29. The pore diameter of both A and B was 3.7 μm. <Hardness> The breaking strength of the resulting granulated silica powder was measured and found to be 1.4 MPa for both A and B, which was sufficiently hard for normal handling. <Impurity concentration> The concentrations of Fe, Al, and Ti were measured by ICP-MS. As a result, the concentrations of Fe, Al, and Ti in granulated silica powder A were 0.68, 0.04, and <0.01 ppm, respectively, and those in granulated silica powder B were 0.55, 0.07, and <0.01 ppm.
[0035] (3) Manufacturing of molded bodies A glass ingot was produced using the granulated silica powder obtained above in a Verneuil process (oxyhydrogen flame fusion process) device, the schematic diagram of which is shown in Figure 4. A photograph of the molten ingot (thumb-sized) is shown in Figure 5. Although several bubbles were generated in both granulated silica powders A and B, they were well within the acceptable range.
[0036] <Comparative Example> The silica gel powder on the 125 μm sieve in Example (1) was calcined at 1220° C. for 40 hours in the same manner as in the Example, and then sieved through a 212 μm sieve to obtain the silica powder under the sieve. The D50 of the powder was the same as that of the granulated powder in the Example. The specific surface area of the powder was 0.1 m 2 The particle size was less than 1.0 mm / g, and the pore volume was less than 0.01 cc / g. The SEM image is shown in Figure 6, but the particles were crushed and no fine particle aggregate structure like that of the granulated particles in Figure 3 was observed. The angle of repose of this silica powder was measured and found to be 37 degrees. An attempt was made to produce a glass ingot using the same Verneuil process apparatus as in the embodiment, but blockage occurred in the piping downstream of the powder reservoir, preventing the powder from flowing smoothly. [Explanation of symbols]
[0037] 1 Powder Hopper 2 Powder Pit 3. Vibrator 4 Nozzle Cushion 5 Quartz nozzle 6 Heat-resistant bricks 7 Ingot 8 Support Rotating Rod 9 Motor 10. Lifting Stage
Claims
1. The D50 particle size (median diameter) is 75 μm or more and 200 μm or less, the angle of repose is 20 degrees or more and 35 degrees or less, and the specific surface area is 0.3 m 2 / g or more 10m 2 / g or less, The granulated silica powder is an agglomerated particle containing 15% by weight or more and 40% by weight or less of silica fine particles having a particle diameter of 10 μm or less.
2. 2. The granulated silica powder according to claim 1, having a silanol concentration of 200 ppm or less and an adsorbed moisture content of 1% or less.
3. 3. The granulated silica powder according to claim 1 or 2, having an Fe content of 1 ppm or less, an Al content of 0.1 ppm or less, and a Ti content of 0.01 ppm or less.
4. The granulated silica powder according to any one of claims 1 to 3, having an average pore diameter of 1 µm or more and 10 µm or less.
5. A preparation step of preparing raw material silica obtained by a sol-gel method, the raw material silica containing 15% by weight or more and 40% by weight or less of silica fine particles having a particle diameter of 10 μm or less; A granulation step in which the raw silica is slurried, a binder is added, and the mixture is spray-granulated; and The method for producing granulated silica powder according to any one of claims 1 to 4, further comprising a calcining step of calcining the obtained granulated particles at 1000°C or more and 1300°C or less.
6. The method for producing granulated silica powder according to claim 5, wherein in the granulation step, the medium used for forming a slurry is water, and the binder is polyvinylpyrrolidone.
Citation Information
Patent Citations
Ammonia treatment of silicon dioxide powder in the preparation of quartz glass
JP2019503961A
Quartz glass excellent in plasma corrosion resistance and its manufacturing method
JP4391529B2
Spray granulation of silicon dioxide in the preparation of quartz glass
US20190077691A1