Insulated wire manufacturing method and insulated wire manufacturing device

The floating coating die method and apparatus minimize non-smooth areas on the insulating coating, providing a wire with uniform flexibility and electrical properties, suitable for medical catheters.

JP7567584B2Active Publication Date: 2024-10-16PROTERIAL LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021042379
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-16
Publication Date
2024-10-16
Estimated Expiration
2041-03-16

AI Technical Summary

Technical Problem

Conventional insulated wire manufacturing methods result in the formation of non-smooth portions on the insulating coating, leading to local variations in flexibility and electrical characteristics, which can deteriorate the appearance and performance of the wire.

Method used

A method and apparatus where the coating die floats on the surface of the paint, maintaining one surface in contact with the liquid level to prevent excess paint from adhering to the die, ensuring the formation of non-smooth areas is minimized, with the number of such areas limited to one or less per 0.8 m of conductor length, and the film thickness ratio maintained at 0.70 < d1/d2 <= 1.

Benefits of technology

The insulated wire achieves uniform bending and electrical properties along its length, with minimal local changes, making it suitable for applications like medical catheters, by suppressing non-smooth portions and ensuring a uniform appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567584000001
    Figure 0007567584000001
  • Figure 0007567584000002
    Figure 0007567584000002
  • Figure 0007567584000003
    Figure 0007567584000003
Patent Text Reader

Abstract

To provide an insulated wire that suppresses occurrence of non-smooth parts on a surface of a coating layer and has unconventionally high quality.SOLUTION: An insulated wire has a conductor, and a coating layer surrounding the conductor. The coating layer has non-smooth parts locally formed on its surface, the number of the non-smooth parts being at most 1 for 0.8 m of a longitudinal length of the conductor.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention , Absolute The present invention relates to a method for manufacturing an insulated electric wire and an apparatus for manufacturing an insulated electric wire. [Background technology]

[0002] 2. Description of the Related Art Conventionally, an insulated wire having a conductor and a coating film (insulating coating) formed by applying paint to the outer periphery of the conductor has been known (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Jitszen No. 54-111786 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the inventors noticed that conventional methods can result in the formation of unintended uneven portions (such as convex portions) on the surface of the insulating coating, which can result in localized changes in the flexibility of the insulated wire, localized changes in the electrical characteristics, and localized deterioration of the appearance.

[0005] An object of the present invention is to provide an insulated wire of unprecedented quality by suppressing the appearance of uneven portions on the surface of an insulating coating. [Means for solving the problem]

[0006] According to a first aspect of the present invention, A conductor; A coating film provided on the outer periphery of the conductor; The number of uneven portions locally formed on the surface of the coating film is 1 or less per 0.8 m of the longitudinal length of the conductor. An insulated wire is provided.

[0007] According to a second aspect of the present invention, (a) a step of immersing a conductor in paint contained in a paint tank and applying the paint around the conductor; (b) pulling the conductor out of the coating liquid surface and passing it through a through hole in a coating die; (b) at the start and during the process, the coating die is floated such that one surface of the coating die is in contact with the liquid surface of the coating material, and the coating material is maintained free from the other surface of the coating die opposite the one surface. A method for making an insulated wire is provided.

[0008] According to a third aspect of the present invention, A paint tank for containing paint; a lifting mechanism that pulls the conductor immersed in the paint from one end side of the conductor in a longitudinal direction and lifts the conductor above a liquid surface of the paint; a coating die having a through hole through which the conductor is passed and around which the coating material is applied; An insulated wire manufacturing apparatus comprising: The coating die is configured such that when starting to pull up the conductor and during the pulling up, one surface of the coating die floats in contact with the liquid surface of the paint, and the paint is not placed on another surface opposite to the one surface of the coating die. An apparatus for manufacturing insulated electrical wire is provided. Effect of the Invention

[0009] According to the present invention, it is possible to suppress the appearance of uneven portions on the surface of an insulating coating and to provide an insulated wire of unprecedented quality. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a partially enlarged perspective view of an insulated wire 10 according to one embodiment of the present invention. [Diagram 2]FIG. 2 is a schematic diagram showing a cross section obtained by cutting the insulated wire 10 along a plane along the longitudinal direction. [Diagram 3] FIG. 3 is a scanning electron microscope photograph of an arbitrary region of the insulating coating of the insulated wire 10 according to one embodiment of the present invention. [Figure 4] FIG. 4 is a scanning electron microscope photograph of an arbitrary region of the insulating coating of the insulated wire 10 according to one embodiment of the present invention. [Diagram 5] FIG. 5 is an explanatory diagram that illustrates a schematic configuration of an insulated electric wire manufacturing apparatus 100 according to one embodiment of the present invention. [Figure 6] Fig. 6(a) is a plan view (top view) of the coating die 52 when viewed from the pulling direction of the conductor 11. Fig. 6(b) is a schematic diagram showing a cross section (longitudinal cross section) obtained by cutting the coating die 52 along the pulling direction of the conductor 11. [Figure 7] FIG. 7 is a scanning electron microscope photograph of a region having an uneven portion that appears in the insulating coating of the insulated electric wire of Example 1. [Figure 8] FIG. 8 is a scanning electron microscope photograph of a region having an uneven portion that appears in the insulating coating of the insulated wire of Comparative Example 1. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] <One embodiment of the present invention> (1) Example of the configuration of the insulated wire 10 First, a configuration example of an insulated wire 10 according to one embodiment of the present invention will be described. As shown in Fig. 1, the insulated wire 10 according to this embodiment includes a conductor 11 and a coating film (hereinafter, also referred to as an insulating coating film) 12.

[0012] The conductor 11 constitutes the core wire (also called the core wire) of the insulated electric wire 10. The conductor 11 is composed of a stranded wire in which a plurality of metal wires are stranded together, or a single metal wire. The conductor 11 is composed of, for example, copper (Cu), a Cu alloy, aluminum (Al), an Al alloy, or the like. The cross-sectional shape of the conductor 11 is substantially circular. The diameter of the conductor 11 is not particularly limited, but when the insulated electric wire 10 is used as an electric wire inside a catheter to be inserted into a medical catheter, it can be, for example, 10 μm to 200 μm, preferably 50 μm to 160 μm. The length of the conductor 11 is also not particularly limited, but when the insulated electric wire 10 is used as an electric wire inside a catheter to be inserted into a medical catheter, it can be, for example, a length within a range of 1.5 to 3 m.

[0013] The lateral periphery of the conductor 11, i.e., the outer periphery, is covered with an insulating coating 12. Note that the insulating coating 12 is provided over the entire length of the conductor 11 in the longitudinal direction, but for convenience, Fig. 1 illustrates a state in which the insulating coating 12 has been removed by a predetermined length from one end of the insulated wire 10.

[0014] The insulating coating 12 can be formed by applying paint W (see FIG. 5) to the outer circumference of the conductor 11, drying the coating, and hardening the coating. The material of the insulating coating 12 is not particularly limited as long as it has excellent adhesion to the conductor 11, a predetermined flexibility, and high electrical insulation and can be applied, and for example, silicone resin, fluorine resin, and olefin resin can be preferably used. When the insulated electric wire 10 is an electric wire in a medical catheter, the material of the insulating coating 12 is preferably silicone resin, and in this case, the paint W is preferably a silicone resin-containing paint obtained by dissolving a silicone resin in an organic solvent or the like. The thickness d1 of the insulating coating 12 (see FIG. 2) is not particularly limited, and can be, for example, within a range of 3 to 6 μm. To make the thickness d1 of the insulating coating 12 as described above, a paint with a relatively low viscosity, for example, a viscosity of 150 to 650 mPa·s, is preferably used as the paint W.

[0015] The insulating coating 12 is formed on the outer circumference of the conductor 11 with a substantially uniform thickness d1. The insulating coating 12 has a substantially uniform thickness d1 over substantially the entire length of the conductor 11 in the longitudinal direction, and its surface is configured as a smooth region with no or almost no non-smooth portions X such as convex portions. In a medical catheter wire that requires a highly flexible bending operation with high followability and reliable transmission of weak signals, the bending property and electrical properties are required to be substantially uniform over the longitudinal direction, and since a medical professional performs delicate operations under visual observation, it is also required to have a substantially uniform appearance over the longitudinal direction. Since the insulating coating 12 of the insulated wire 10 in this embodiment is configured as described above, the bending property and electrical properties are substantially uniform over the longitudinal direction, with almost no local changes, and the wire has a substantially uniform appearance over the longitudinal direction and almost no localized singular points in appearance, which are very suitable characteristics for a medical catheter wire. In the case of a multi-core cable in which a plurality of insulated wires 10 are collectively covered with a sheath, since the insulating coating 12 is configured as described above, the sheath can be filled with the insulating coating 12 without any gaps.

[0016] As described above, the surface of the insulating coating 12 is completely or almost completely free of uneven portions X. However, in rare cases, uneven portions X (re-adhesion traces) may be formed locally on the surface of the insulating coating 12 due to redeposition or dripping of the paint W onto the coating film during the formation of the insulating coating 12 (see FIG. 2). The uneven portions X formed by redeposition of the paint W tend to have a so-called spindle shape, for example, in which the film thickness is thickest near the center along the longitudinal direction of the conductor 11 and gradually becomes thinner at both ends (approaching the above-mentioned film thickness d1).

[0017] However, in the insulated electric wire 10 according to the present embodiment, the frequency of occurrence of the uneven portion X is much lower than that of the conventional insulated electric wire. Specifically, the number of uneven portions X locally formed on the surface of the insulating coating 12 is one or less per 0.8 m of the longitudinal length of the conductor 11. That is, the frequency of occurrence of the uneven portion X on the surface of the insulating coating 12 is very low, that is, no uneven portion X is formed (zero) per 0.8 m of the longitudinal length of the conductor 11, or even if the uneven portion X is formed, the frequency is one at most. With such a configuration, the insulated electric wire 10 according to the present embodiment has characteristics that are very suitable for applications such as an electric wire in a medical catheter, in that the flexibility and electrical characteristics are substantially uniform over the longitudinal direction, there are almost no local changes, and the insulated electric wire 10 has a substantially uniform appearance over the longitudinal direction, and there are almost no localized singular points in appearance.

[0018] The number of non-smooth portions X is measured using a scanning electron microscope (200x magnification). Specifically, as shown in Fig. 3, a straight line is connected between point A at the top of the left end of the insulated electric wire 10 in Fig. 3 and point B at the top of the right end, and a straight line is connected between point C at the bottom of the left end of the insulated electric wire 10 and point II at the bottom of the right end. Then, the portions protruding from the region between line segments I, I, and Ha, (portions having a thickness 1.1 times or more that of line segment I, Ha) are identified as non-smooth portions X, and the number of such portions is measured.

[0019] In this embodiment, three evaluation samples with a longitudinal length of the conductor 11 exceeding 0.8 m (for example, 1 m) are prepared, and photographs are taken at five points (0 to 0.8 m) every 0.2 m for each evaluation sample (3 evaluation samples x 5 evaluation points = 15 photographs). Then, the number of non-smooth portions X per 0.8 m of the longitudinal length of the conductor 11 is calculated by dividing the total count number of non-smooth portions X by 3. The method of measuring the number of non-smooth portions is the same in the examples and comparative examples described later.

[0020] Further, in the insulated wire 10 according to the present embodiment, even if a non-smooth portion X appears, its size is extremely small compared to that of a conventional insulated wire. Specifically, when the film thickness of the portion other than the non-smooth portion X (i.e., the smooth portion) of the insulating coating 12 in the cross-section of the insulated wire 10 along the longitudinal direction of the insulated wire 10 (the cross-section shown in FIG. 2) is d1, and the maximum film thickness of the non-smooth portion X is d2, the relationship of 0.70 < d1 / d2 ≦ 1, preferably 0.85 < d1 / d2 ≦ 1 is always maintained. With such a configuration, the insulated wire 10 according to the present embodiment has substantially uniform flexibility and electrical characteristics over its longitudinal direction, with almost no local changes, and also has a substantially uniform appearance over its longitudinal direction and almost no local appearance singularities, which are very suitable for applications such as the inner wire of a medical catheter.

[0021] Note that the film thicknesses d1 and d2 of the insulating coating 12 are mainly obtained using a scanning electron microscope (200 times magnification). Specifically, as shown in FIG. 4, the lengths D1 of the portions other than the non-smooth portion X (i.e., the smooth portions) of the insulating coating 12 and the portion with the maximum length D2 of the non-smooth portion X are visually determined, and their respective lengths are measured. Then, using the measured D1 and D2 and the diameter R of the conductor 11 measured in advance, d1 is obtained as (D1 - R) / 2, and d2 is obtained as (D2 - R) / 2. The method for obtaining the film thicknesses of the smooth and non-smooth portions of these insulating coatings 12 is the same in the examples and comparative examples described later.

[0022] (2) Configuration example of the insulated wire manufacturing apparatus 100 Next, a configuration example of the insulated wire manufacturing apparatus 100 according to an embodiment of the present invention will be described. As shown in FIG. 5, the insulated wire manufacturing apparatus 100 includes a paint tank 50, a coating die 52, a baking furnace 54, a cooling unit 55, a feeding mechanism 56, a pulling-up mechanism 57, and bobbins 70, 71.

[0023] The paint tank 50 has an open upper portion and is formed in a hollow cylindrical shape with a bottom. The upper opening and the inner cross-section of the cylindrical portion of the paint tank 50 are formed in a circular shape in a plan view.

[0024] As an example, the coating die 52 is formed in a film shape, and its upper surface does not contact the liquid surface of the paint W, and only its lower surface is in contact with the liquid surface of the paint W and is configured to float. In a plan view (hereinafter simply referred to as "plan view") when viewed from the direction in which the conductor 11 is pulled up, the coating die 52 is configured to have a circular shape that is slightly smaller in diameter than the upper opening of the paint tank 50 (see FIG. 6(a)), and the diameter can be, for example, within a range of 10 to 100 mm. In addition, the coating die 52 is configured such that its outer circumferential end (a part corresponding to a flange) is curved in a direction away from the liquid surface of the paint W in the paint tank 50 toward the upper side (in a direction away from the liquid surface of the paint W) as it moves toward the radial outside of the coating die 52. The distance between the uppermost part of the curved portion and the liquid surface of the coating material W can be, for example, within a range of 1 to 10 mm. The specific gravity of the coating die 52 is preferably smaller than that of the coating material W. When a silicone-based resin-containing coating material is used as the coating material W, the weight of the coating die 52 can be, for example, within a range of 0.01 to 0.3 g. The curved portion of the coating die 52 can be formed, for example, by subjecting the outer peripheral end of a film to a heat press process. The outer peripheral end of the coating die 52 may be formed to stand vertically instead of being curved. The coating die 52 may also be in the form of a sheet having a thickness of 1 to 10 mm, formed of a foamed resin material or the like.

[0025] The coating die 52 can be made of a film having at least one of the properties of water repellency and hydrophobicity. The film here is a resin thin film member having a thickness in the range generally called a film or sheet, and the thickness can be, for example, within the range of 0.05 to 0.2 mm. The term "hydrophobic" refers to a property of having little chemical interaction with water and little affinity for water. The term "water repellency" refers to a property of having low wettability of water to the surface of a substance. For example, the surface of the coating die 52 can be coated with a non-polar substance such as a fluorine-based resin to impart hydrophobicity to the coating die 52. For example, the surface of the coating die 52 can be coated with a fine pigment such as silica to form fine irregularities, or the surface of the coating die 52 can be formed with fine irregularities like lotus leaves or water strider feet to impart water repellency to the coating die 52. When a silicone-based resin-containing paint is used, the material of the coating die 52 can be, for example, polytetrafluoroethylene (PTFE).

[0026] A through hole 53 for passing the conductor 11 is provided near the center of the coating die 52 in a plan view. The through hole 53 is configured so that excess paint W attached to the outer periphery of the conductor 11 can be wiped off (removed) when the conductor 11 is pulled up from the liquid surface of the paint W. The through hole 53 is formed in a circular shape in a plan view, and its diameter is configured to be slightly larger than the diameter of the conductor 11. The diameter of the through hole 53 can be set to a dimension equal to or slightly larger than the diameter of the conductor 11 (e.g., 200 μm) plus twice the thickness of the insulating coating 12 to be formed (e.g., 5 μm), and can be set to a size within a range of, for example, 210 to 300 μm.

[0027] A feed mechanism 56 for the conductor 11 is disposed inside the paint tank 50. The feed mechanism 56 is configured to move (feed out) the conductor 11 wound around a bobbin 70 disposed nearby, upward (to the through hole 53 of the coating die 52). The feed mechanism 56 is provided so that the conductor 11 and the coating die 52 do not come into contact with each other.

[0028] Above the paint tank 50, a baking furnace 54 for baking the paint adhering to the surface of the conductor 11 that has passed through the paint tank 50 and the coating die 52 onto the surface of the conductor 11, and a cooling section 55 for cooling the conductor 11 and the insulating coating 12 after the baking process are arranged in that order. Depending on the type of paint, at least one of these may be omitted. The baking furnace 54 may be a heating furnace for drying and hardening the paint by heating, an ultraviolet irradiation furnace for hardening the paint by irradiating ultraviolet rays, or a cross-linking furnace for cross-linking and hardening the paint by moisture or the like.

[0029] A lifting mechanism 57 for the conductor 11 is disposed above the cooling section 55. The lifting mechanism 57 is configured to lift upward the conductor 11 that has passed through the cooling section 55. A bobbin 71 is disposed near the lifting mechanism 57, around which the conductor 11 (insulated wire 10) on which the insulating coating 12 is formed is wound.

[0030] (3) Example of Manufacturing Method for Insulated Wire 10 Next, an example of a method for producing the insulated wire 10 according to one embodiment of the present invention will be described.

[0031] The method for manufacturing the insulated wire 10 mainly includes step a of immersing the conductor 11 in paint W contained in a paint tank 50 and applying the paint W around the conductor 11, and step b of lifting the conductor 11 out of the liquid surface of the paint W and passing it through the through hole 53 of the coating die 52.

[0032] The method for producing the insulated wire 10 will be described in detail below.

[0033] First, in step a, the conductor 11 wound around the bobbin 70 is conveyed in the direction of arrow A shown in Fig. 5, and moved from the upper side of the paint tank 50 into the paint tank 50. In this manner, the conductor 11 is immersed in the paint W, and the paint W is adhered to the outer periphery of the conductor 11. As described above, the paint W may be a silicone-based resin-containing paint having a relatively low viscosity in the range of 150 to 650 mPa s, for example.

[0034] The movement of the conductor 11 described above is performed, for example, by the coordinated operation of a feed mechanism 56 that transports the conductor 11 in the direction of arrow A and supplies the conductor 11 into the paint tank 50, and a pull-up mechanism 57 that winds up the conductor 11 unwound from the feed mechanism 56.

[0035] Next, in step b, the conductor 11 with the coating material W attached thereto is inserted into a through hole 53 formed in a coating die 52 floating on the surface of the coating material W. The conductor 11 with the coating material W attached thereto is pulled up from the surface of the coating material W, and as the conductor 11 passes through the through hole 53, the coating material W attached to the outer periphery of the conductor 11 is brought into contact with the through hole 53, thereby removing excess coating material. In this manner, the amount of coating material W to be applied can be adjusted. The pulling speed of the conductor 11 in this embodiment can be set to, for example, within a range of 1 to 30 m / min.

[0036] In this embodiment, at the start and during step b, the coating die 52 is floated so that one surface of the coating die 52 (i.e., the lower surface of the coating die 52) is in contact with the liquid surface of the paint W, and the coating die 52 maintains a state in which no paint W is placed on the other surface opposite to the one surface of the coating die 52 (i.e., the upper surface of the coating die 52) (see FIG. 5). To create the above-mentioned state, it is preferable to float the coating die 52 on the liquid surface of the paint W before the start of step b without immersing it in the paint W, and to start step b from this state.

[0037] The above-mentioned state can be reliably created by utilizing the surface tension of the liquid surface of the coating die 52 that floats the coating die 52. By appropriately selecting the material (water repellency or hydrophobicity of the lower surface side of the coating die 52) and shape of the coating die 52, the magnitude of the surface tension of the coating die W acting between the coating die 52 and the coating die 52 at the start and during step (b) can be optimized, thereby making it possible to reliably maintain the above-mentioned state.

[0038] In this embodiment, at the start and during step (b), the coating die 52 is adapted to maintain a state in which it is in close contact with the liquid surface of the paint W and floats on the liquid surface without being separated (lifted) from the liquid surface of the paint W (see FIG. 5). This state can also be reliably created by utilizing the surface tension of the liquid surface of the paint W that floats the coating die 52. By appropriately selecting the material (wettability of the lower surface side of the coating die 52) and shape of the coating die 52, the viscosity of the paint W, the lifting speed of the conductor 11, and the like, it is possible to optimize the magnitude of the surface tension of the paint W acting between the coating die 52 and the coating die 52 at the start and during step (b), thereby making it possible for the coating die 52 to maintain a state in which it is in close contact with the liquid surface of the paint W and floats on the liquid surface (floating state).

[0039] After step b is completed, the conductor 11 with the paint W attached thereto is moved into a baking furnace 54, where the paint W attached to the outer periphery of the conductor 11 is baked and dried, and the coating film is solidified to a predetermined hardness. Next, the conductor 11 with the coating film hardened is moved into a cooling section 55, where the coating film formed on the outer periphery of the conductor 11 is cooled.

[0040] Then, by performing a series of steps including the above-mentioned application of the paint W, adjustment of the amount of paint applied, baking, and drying a predetermined number of times (once, or multiple times in some cases), it is possible to form the insulating coating 12 with a desired thickness around the outer periphery of the conductor 11. This series of steps can be performed multiple times by moving the conductor 11 taken up by the lifting mechanism 57 to the delivery mechanism 56 and then taking it up again by the lifting mechanism 57.

[0041] Through the above steps, it is possible to manufacture an insulated wire 10 having an insulating coating 12 with a desired thickness on a conductor 11. The manufactured insulated wire 10 is transported from the pulling mechanism 57 in the direction of arrow B shown in FIG. 5 and wound around a bobbin 71.

[0042] (5) Effects of this embodiment According to this embodiment, one or more of the following advantages are achieved.

[0043] (a) In manufacturing the insulated wire 10, at the start and during step b, the coating die 52 is floated so that its lower surface is in contact with the liquid surface of the coating material W, and the coating material W is maintained in a state where the upper surface of the coating die 52 is not coated with the coating material W, thereby making it possible to prevent unnecessary coating material W (e.g., the coating material W on the upper surface of the coating die 52) from being redeposited on the surface of the conductor 11 from which excess coating material has been squeezed out by passing through the through hole 53 of the coating die 52, i.e., on the surface of the coating film formed around the conductor 11. This makes it possible to prevent the formation of non-smooth portions X, which are traces of redeposited coating material W, on the surface of the insulating coating 12.

[0044] (b) Furthermore, when manufacturing the insulated wire 10, by using the coating die 52 made of a film having at least one of water repellency and hydrophobicity, it is possible to utilize the surface tension of the paint W to reliably float the coating die 52 on the liquid surface of the paint W. As a result, even when the above-mentioned low-viscosity paint is used as the paint W, it is possible to reliably maintain a state in which the paint W does not rest on the upper surface of the coating die 52, and it is possible to reliably obtain the above-mentioned effects.

[0045] (c) Furthermore, when manufacturing the insulated wire 10, by using a coating die 52 having an outer circumferential end (brim) with a shape (for example, a curved shape or a vertically standing shape) that faces in a direction away from the liquid surface of the paint W, it is possible to prevent the paint W from entering the upper surface of the coating die 52 and to reliably float the coating die 52 on the liquid surface of the paint W. As a result, even when the above-mentioned low-viscosity paint is used as the paint W, it is possible to reliably maintain a state in which the paint W does not come onto the upper surface of the coating die 52, and it is possible to reliably obtain the above-mentioned effects.

[0046] (d) With the above-described manufacturing apparatus and manufacturing method, it is possible to reduce the number of uneven portions X locally formed on the surface of the insulating coating 12 to 1 or less per 0.8 m of the longitudinal length of the conductor 11. In other words, it is possible to reduce the frequency of appearance of uneven portions X on the surface of the insulating coating 12 to a very low frequency, such that no uneven portions X are formed (zero portions) per 0.8 m of the longitudinal length of the conductor 11, or, if any, a maximum of 1 portion is formed.

[0047] As a result, the insulated wire 10 according to this embodiment has substantially uniform bendability and electrical properties along its length with almost no local variation, making it extremely suitable for applications such as wires in medical catheters that require delicate bending properties and reliable transmission of weak signals. The insulated wire 10 according to this embodiment also has substantially uniform appearance along its length with almost no localized appearance irregularities, making it extremely suitable for applications such as wires in medical catheters.

[0048] (e) Furthermore, according to the above-described manufacturing apparatus and manufacturing method, even if a non-smooth portion X appears on the surface of the insulating coating 12, the non-smooth portion X is not caused by re-adhesion of unnecessary paint W (e.g., paint W on the upper surface of the coating die 52), and therefore the size of the non-smooth portion X can be made very small.

[0049] Specifically, when the film thickness of the portion other than the non-smooth portion X of the insulating coating 12 (i.e., the smooth portion) in the cross-section of the insulated wire 10 along the longitudinal direction of the insulated wire 10 (the cross-section shown in FIG. 2) is d1 and the maximum film thickness of the non-smooth portion X is d2, it is possible to maintain 0.70 < d1 / d2 ≦ 1.

[0050] As a result, the insulated wire 10 according to the present embodiment has characteristics that are very suitable for applications such as the inner wire of a medical catheter, in which the flexibility and electrical characteristics are substantially uniform over its longitudinal direction and there are almost no local changes. Further, the insulated wire 10 according to the present embodiment has an appearance that is substantially uniform over its longitudinal direction and has almost no local appearance singularities, which is very suitable for applications such as the inner wire of a medical catheter.

[0051] (f) When manufacturing the insulated wire 10, by utilizing the surface tension of the paint W (the wettability on the lower surface side of the coating die 52) at the start and during the execution of step (b), it is possible to create a state (floating state) in which the coating die 52 floats while being in close contact with the liquid surface of the paint W without separating from (being lifted from) the liquid surface of the paint W.

[0052] As a result, the excess paint adhering to the surface of the conductor 11 can be reliably squeezed out, and the insulated wire 10 according to the present embodiment has characteristics that are very suitable for applications such as the inner wire of a medical catheter, in which the flexibility and electrical characteristics are substantially uniform over its longitudinal direction and there are almost no local changes.

[0053] (g) When manufacturing the insulated wire 10, by floating the film-shaped coating die 52 having a planar shape that is a similar shape with a slightly smaller diameter than the upper opening of the paint tank 50 on the liquid surface of the paint W, it is possible to cover the liquid surface of the paint W over a wide range by the coating die 52. As a result, unnecessary volatilization of the solvent from the paint W can be suppressed, and a change in the viscosity of the paint W during the execution of step (b) can be avoided. Also, it is possible to avoid the entry of foreign matter into the paint W during the execution of step (b).

[0054] <Other embodiments> Although one embodiment of the present invention has been specifically described above, the present invention is not limited to the above-described embodiment, and can be modified as appropriate without departing from the gist of the present invention.

[0055] In the above embodiment, the resin forming the insulating coating 12 is a silicone resin, but the present invention is not limited to this. For example, the enameled wire may be formed using a polyamide-imide resin as the resin forming the insulating coating 12. Even in this case, substantially the same effects as in the above embodiment can be obtained.

[0056] In the above embodiment, the conductor 11 having a circular cross-sectional shape has been described as an example, but the present invention is not limited thereto. For example, a rectangular conductor having a substantially rectangular cross-sectional shape may be used. In this case, in order to uniformly apply the paint W to the rectangular conductor, it is preferable that the through hole 53 has a substantially rectangular shape in a plan view. Even in this case, substantially the same effect as the above embodiment can be obtained. EXAMPLES

[0057] Next, the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.

[0058] [Example 1] (Making insulated wire) First, as a conductor constituting the core of the insulated wire, for example, a copper wire made of Tough-Pitch Copper (TPC) and having a diameter of 100 to 200 μm was prepared.

[0059] Next, a material for forming the insulating coating was prepared. In Example 1, a silicone rubber coating agent was prepared as the material for the insulating coating. 80 to 100 parts by mass of this silicone rubber coating agent was mixed with 80 to 100 parts by mass of toluene or the like as a viscosity adjusting solvent to adjust the coating solution (paint) to a viscosity of 150 to 200 mPa s.

[0060] Next, an insulating coating was formed on the outer periphery of the conductor using the same process and conditions as in the insulated wire manufacturing process in the above-mentioned embodiment, using an insulated wire manufacturing apparatus shown in Fig. 5. In this example, the conductor was pulled up at a speed of 10 to 12 m / min. The insulating coating was then subjected to a drying and curing process at a temperature of 150 to 450°C for 5 to 20 minutes. The thickness of the obtained insulating coating was 3 to 6 µm.

[0061] In this manner, the insulated wire of Example 1 was produced.

[0062] [Comparative Example 1] In Comparative Example 1, a copper wire (conductor) and a coating solution (paint) similar to those in Example 1 were prepared, and an insulating coating was formed around the outer periphery of the conductor using a known insulated wire manufacturing apparatus to produce an insulated wire. The main difference between the known insulated wire manufacturing apparatus and the insulated wire manufacturing apparatus shown in Fig. 5 is the configuration of the coating die, which is a component of each insulated wire manufacturing apparatus.

[0063] A known coating die is configured so that when a conductor is immersed in the paint, it is submerged in the paint, and when the conductor is pulled up from the paint, it floats to the surface of the paint due to frictional resistance caused by the viscosity of the paint when the conductor passes through a through hole in the coating die, etc. Then, when the conductor is pulled up from the paint surface, the conductor is passed through the through hole to squeeze out excess paint adhering to the conductor, thereby forming an insulating coating.

[0064] In contrast, the coating die according to the above-mentioned embodiment is configured to maintain one surface of the coating die floating on the surface of the coating due to the surface tension of the coating when the conductor starts to be pulled up and while it is being pulled up. Furthermore, this coating die is configured to maintain a state in which no coating is placed on the coating die (the other surface opposite to the one surface of the coating die) when the conductor starts to be pulled up and while it is being pulled up. In these respects, the coating die according to the above-mentioned embodiment is significantly different from known coating dies.

[0065] For each of the insulated electric wires produced above, the size of the convex portions of the non-smooth portions was measured, and the smoothness of each insulated electric wire was determined. Hereinafter, each measurement method and evaluation criteria will be described.

[0066] (Size of the convex portions of the non-smooth portions) FIG. 7 is a scanning electron micrograph (200 times) of a region having a non-smooth portion of the insulating coating in the insulated electric wire of Example 1. In the insulated electric wire produced in Example 1, the film thickness of the portion other than the non-smooth portion of the insulating coating in the cross-section of the insulated electric wire along the longitudinal direction of the conductor was defined as d3, and the maximum film thickness of the non-smooth portion was defined as d4. By the method described above, the respective film thicknesses were determined. If the obtained d3 and d4 were substituted into the formula of d3 / d4 and 0.70 < d3 / d4 ≦ 1 was satisfied, it was evaluated that the size of the convex portions of the non-smooth portions was sufficiently small and the possibility of inhibiting the smoothness of the insulated electric wire was low. If it was not satisfied, it was evaluated that the convex portions of the non-smooth portions were large and the possibility of inhibiting the smoothness of the insulated electric wire was high.

[0067] FIG. 8 is a scanning electron micrograph of a region having a non-smooth portion of the insulating coating in the insulated electric wire of Comparative Example 1. Similarly for the insulated electric wire produced in Comparative Example 1, the film thickness of the portion other than the non-smooth portion of the insulating coating in the cross-section of the insulated electric wire along the longitudinal direction of the conductor was defined as d5, and the maximum film thickness of the non-smooth portion was defined as d6. By the method described above, the respective film thicknesses were determined and evaluated according to the same method and criteria as in Example 1.

[0068] (Evaluation) In Example 1, the film thickness d3 was 4.3 to 4.4 μm, and the maximum film thickness d4 was 4.5 to 4.6 μm. When these values were substituted into the above-described formula, 0.70 < d3 / d4 ≦ 1 was satisfied respectively. Therefore, it was evaluated that the size of the convex portions of the non-smooth portions was sufficiently small and the possibility of inhibiting the smoothness of the insulated electric wire was low. In Comparative Example 1, the film thickness d5 was 4.2 to 4.4 μm, and the maximum film thickness d6 was 6.4 to 18.0 μm. When these values were substituted into the above-described formula, 0.2 < d5 / d6 ≦ 0.68 was obtained respectively, and the above criteria were not satisfied. Therefore, it was evaluated that the convex portions of the non-smooth portions were large and the possibility of inhibiting the smoothness of the insulated electric wire was high.

[0069] <Preferred Embodiment of the Present Invention> The preferred embodiments of the present invention are appended below.

[0070] (Appendix 1) According to one embodiment of the present invention, a conductor, and a coating film provided on the outer periphery of the conductor, and the number of non-smooth portions locally formed on the surface of the coating film is 1 or less per 0.8 m of the length in the longitudinal direction of the conductor, an insulated wire is provided.

[0071] (Appendix 2) The insulated wire according to Appendix 1, wherein when the film thickness of the portion other than the non-smooth portion of the coating film in the cross section of the insulated wire along the longitudinal direction is d1 and the maximum film thickness of the non-smooth portion is d2, 0.70 < d1 / d2 ≦ 1 is maintained.

[0072] (Appendix 3) The insulated wire according to Appendix 1 or 2, wherein the coating film is a silicone resin-containing film.

[0073] (Appendix 4) The insulated wire according to any one of Appendices 1 to 3, wherein the diameter of the conductor is 200 μm or less.

[0074] (Appendix 5) According to another embodiment of the present invention, (a) a step of immersing a conductor in a paint contained in a paint tank and applying the paint around the conductor; and (b) a step of pulling up the conductor from the liquid surface of the paint and passing it through a through-hole of a coating die, and at the start and during the execution of step (b), the coating die floats such that one surface of the coating die is in contact with the liquid surface of the paint, and the paint is maintained in a state where it does not rest on the other surface facing the one surface of the coating die. A method for making an insulated wire is provided.

[0075] (Appendix 6) A method for producing an insulated wire according to claim 5, (b) At the beginning and throughout the process, the surface tension of the coating maintains the coating die floating above the surface of the coating.

[0076] (Appendix 7) A method for producing an insulated wire according to claim 5 or 6, The viscosity of the coating material is 150 to 650 mPa·s.

[0077] (Appendix 8) A method for producing an insulated electric wire according to any one of appendixes 5 to 7, The paint is a silicone-based resin-containing paint.

[0078] (Appendix 9) A method for producing an insulated wire according to any one of appendixes 5 to 8, The conductor has a diameter of 200 μm or less.

[0079] (Appendix 10) According to yet another aspect of the present disclosure, A paint tank for containing paint; a lifting mechanism that pulls the conductor immersed in the paint from one end side of the conductor in a longitudinal direction and lifts the conductor above a liquid surface of the paint; a coating die having a through hole through which the conductor is passed and around which the coating material is applied; An insulated wire manufacturing apparatus comprising: The coating die is configured such that when starting to pull up the conductor and during the pulling up, one surface of the coating die floats in contact with the liquid surface of the paint, and the paint is not placed on another surface opposite to the one surface of the coating die. An apparatus for manufacturing insulated electrical wire is provided.

[0080] (Appendix 11) 11. An insulated wire manufacturing apparatus according to claim 10, When the pulling of the conductor begins and during the pulling process, the coating die is configured to remain floating on the surface of the paint due to the surface tension of the paint.

[0081] (Appendix 12) 12. An insulated wire manufacturing apparatus according to claim 10 or 11, The coating die is made of a film having water repellency or hydrophobicity.

[0082] (Appendix 13) An insulated electric wire manufacturing apparatus according to any one of appendixes 10 to 12, The coating die is configured so that its outer peripheral edge faces upward and away from the liquid surface. [Explanation of symbols]

[0083] 10 Insulated wire 11 Conductor 12 Coating film (insulating coating) W paint X Non-smooth area 50 Paint tank 52 Coating Dies 53 Through hole 57 Lifting mechanism

Claims

1. (a) immersing a conductor in paint contained in a paint tank and applying the paint around the conductor; (b) pulling the conductor up from the surface of the coating material and passing it through a through hole in a coating die; the coating die is formed in a film shape, and its outer peripheral end is curved in a direction away from the liquid surface of the paint in the paint tank; (b) at the start and during the process, the lower surface of the coating die is in contact with the liquid surface of the paint and floats thereon, and the paint is maintained in a state where it is not placed on the upper surface of the coating die. A method for manufacturing insulated wire.

2. The coating die is made of a film having at least one of water repellency and hydrophobicity properties. The method for producing the insulated wire according to claim 1 .

3. A paint tank for containing paint; a lifting mechanism that pulls the conductor immersed in the paint from one end side of the conductor in a longitudinal direction and lifts the conductor above a liquid surface of the paint; a coating die having a through hole through which the conductor is passed and around which the coating material is applied; An insulated wire manufacturing apparatus comprising: The coating die is formed in a film shape, and its outer peripheral end is curved in a direction away from the liquid surface of the paint in the paint tank, and when starting to pull up the conductor and while pulling up is being performed, the lower surface of the coating die is in contact with the liquid surface of the paint and floats, and the coating die is maintained in a state where the paint is not placed on the upper surface of the coating die. Insulated wire manufacturing equipment.

Citation Information

Patent Citations

  • JP1979111786U

  • JP1980080364U

  • Method of detecting burr of enameled insulated wire

    JP1986024108A