Substrates and metal laminates
A tetrafluoroethylene polymer-based substrate with inorganic filler and surfactants addresses the challenges of dielectric and mechanical properties in printed wiring boards, providing low dielectric and thermal expansion with enhanced mechanical strength for reliable performance in vibrating environments.
Patent Information
- Application Number
- JP2021537258
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-06
- Filing Date
- 2020-07-29
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-07-29
AI Technical Summary
Existing insulating layers for printed wiring boards face challenges in achieving low dielectric constant, low dielectric loss tangent, low coefficient of thermal expansion, and mechanical strength, particularly when incorporating inorganic fillers, which can increase dielectric constant and compromise mechanical integrity, limiting their use in vibrating environments.
A substrate composed of a tetrafluoroethylene polymer and inorganic filler, with specific properties and additives, such as silica and surfactants, to maintain low dielectric properties and enhance mechanical strength, while minimizing changes in dielectric loss tangent after exposure to harsh conditions.
The substrate achieves low dielectric loss tangent, dielectric constant, and thermal expansion, along with excellent mechanical strength, suitable for use in environments with vibrations, ensuring reliable performance in printed wiring boards.
Smart Images

Figure 0007567794000003 
Figure 0007567794000004 
Figure 0007567794000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a substrate and a metal laminate. [Background technology]
[0002] As electronic devices are required to be smaller and more functional, the insulating layer (substrate) that constitutes the printed wiring boards used in electronic devices is required to have electrical properties such as low dielectric constant and low dielectric tangent, as well as low thermal expansion coefficient and heat resistance. In particular, to stably mount electronic components on the printed wiring board, it is important to suppress warping of the printed wiring board caused by heat during mounting. To suppress warping of the printed wiring board, it is important that the insulating layer has a low thermal expansion coefficient. As an insulating layer with a low thermal expansion coefficient, an insulating layer containing an inorganic filler and a resin has been proposed (Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2006-228871 A [Patent Document 2] Japanese Patent Application Publication No. 63-259907 Summary of the Invention [Problem to be solved by the invention]
[0004] In order to reduce the thermal expansion coefficient of the insulating layer, it is preferable to add a large amount of inorganic filler to the resin. However, since the relative dielectric constant of the inorganic filler is higher than that of the resin, there is a problem that the relative dielectric constant of the insulating layer increases when the amount of inorganic filler added increases. If a fluororesin is used as the resin, electrical properties such as dielectric tangent and dielectric constant are improved, but simply mixing a fluororesin with an inorganic filler causes problems such as a decrease in the mechanical strength of the insulating layer and an increase in transmission loss. If the mechanical strength of the insulating layer is low, it cannot be used for printed wiring boards used in environments with vibration, such as automobiles, and its applications are limited.
[0005] The present invention provides a substrate having low dielectric tangent, relative dielectric constant, transmission loss and coefficient of thermal expansion and excellent mechanical strength, and a metal laminate using the same. [Means for solving the problem]
[0006] The present invention has the following aspects. [1] A substrate comprising a tetrafluoroethylene-based polymer and an inorganic filler, A substrate, in which a test piece with a thickness of 127 μm cut from the substrate is subjected to an unsaturated pressure cooker test at 120° C. and 85% RH for 72 hours, and the rate of change in dielectric tangent at 10 GHz is 30% or less. [2] The substrate according to [1], wherein the tetrafluoroethylene-based polymer is a polymer having units based on tetrafluoroethylene and units based on perfluoro(alkyl vinyl ether) or units based on hexafluoropropylene. [3] The substrate according to [1] or [2], wherein the tetrafluoroethylene-based polymer is a polymer having at least one functional group selected from the group consisting of a carbonyl group-containing group, a hydroxyl group, an epoxy group, an amide group, an amino group, and an isocyanate group. [4] The substrate according to [3], wherein the polymer having the functional group is a polymer having a monomer unit having the functional group.
[0007] [5] The substrate according to any one of [1] to [4], wherein the inorganic filler is silica. [6] The substrate according to any one of [1] to [5], wherein the thickness of the substrate is 60 to 500 μm. [7] The substrate according to any one of [1] to [6], further comprising a surfactant. [8] The substrate according to [7], wherein the surfactant is a fluorosurfactant.
[0008] [9] A metal laminate comprising the substrate according to any one of [1] to [8] above and a metal layer located in contact with at least one surface of the substrate.
[10] The metal laminate of [9], wherein the metal layer is a layer made of copper foil.
[11] The metal laminate according to [9] or
[10] , wherein the ten-point average roughness of the surface of the metal layer in contact with the substrate is 2.0 μm or less.
[12] The metal laminate according to any one of [9] to
[11] , wherein the peel strength of the interface between the substrate and the metal layer is 5 N / cm or more. Effect of the Invention
[0009] The substrate of the present invention has low dielectric tangent, dielectric constant, transmission loss and thermal expansion coefficient, and is excellent in mechanical strength. A substrate including the metal laminate of the present invention has low dielectric tangent, relative dielectric constant, transmission loss and thermal expansion coefficient, and is excellent in mechanical strength. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a metal laminate of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing another example of the metal laminate of the present invention. [Diagram 3] 1 is a graph showing the dependency of the rate of change in dielectric tangent before and after the unsaturated pressure cooker test on the time period during which the substrates of Examples 1 and 2 are placed in the unsaturated pressure cooker test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The following terms are defined as follows: The Unsaturated Pressure Cooker Test (hereinafter, also referred to as "USPCT") is a pressure cooker test at 85% RH, also known as HAST (High Accelerated Stress Test). The USPCT is performed according to the method specified in IEC 60068-2-66:1994 (corresponding JIS standard: JIS C 0096:2001). The rate of change in the dielectric tangent at 10 GHz before and after a 127 μm-thick test piece is subjected to USPCT at 120° C. and 85% RH for 72 hours is calculated by the following formula (1). Percentage change in dielectric tangent (%) = (dielectric tangent of test piece after USPCT - dielectric tangent before USPCT) / dielectric tangent before USPCT × 100 (1). The dielectric loss tangent and the relative dielectric constant are values measured at 25°C and 10 GHz using a cavity resonator and a vector network analyzer in accordance with the method specified in JIS R 1641:2007. The ten-point average roughness (hereinafter also referred to as "Rzjis") is a value measured using a Surfcorder SE600 manufactured by Kosaka Laboratory in accordance with the method specified in Appendix JA of JIS B 0601:2013. The peel strength is a value measured by the method described in the examples below.
[0012] In the present invention, a tetrafluoroethylene-based polymer (hereinafter also referred to as a "TFE-based polymer") means a polymer having units based on tetrafluoroethylene (hereinafter also referred to as "TFE"). In this specification, a "unit based on a monomer" is also referred to as a "monomer unit." For example, a "unit based on TFE" is also referred to as a "TFE unit." The dimensional ratios in FIGS. 1 and 2 are different from the actual ones for the sake of convenience of explanation.
[0013] 〔substrate〕 The substrate of the present invention (hereinafter also referred to as "the substrate") contains a TFE-based polymer and an inorganic filler.
[0014] The relative dielectric constant of the TFE-based polymer is preferably 6.0 or less, more preferably 3.5 or less, and particularly preferably 3.0 or less. If the relative dielectric constant is equal to or less than the upper limit, the present substrate can be suitably used for printed wiring boards and the like that require a low dielectric constant. The relative dielectric constant of the TFE polymer is preferably 1.5 or more from the viewpoint of the electrical characteristics of the substrate.
[0015] The TFE-based polymer is preferably a polymer that can be melt molded. "Melt moldable" means that it exhibits melt fluidity. "Exhibiting melt fluidity" means that there is a temperature at which the melt flow rate is 0.1 to 1000 g / 10 min at a temperature 20° C. or more higher than the melting point of the TFE-based polymer under a load of 49 N. "Melt flow rate" means the melt mass flow rate (MFR) defined in JIS K 7210:1999 (ISO 1133:1997). The melting point of the TFE-based polymer is preferably higher than 260° C., more preferably higher than 260° C. but not higher than 320° C., and particularly preferably 275 to 320° C. When the melting point of the TFE-based polymer is within the above range, the TFE-based polymer is fired while retaining adhesiveness based on its elasticity, making it easier to form a dense substrate. The MFR of the TFE polymer is preferably from 0.5 to 100 g / 10 min, more preferably from 1 to 30 g / 10 min, and particularly preferably from 5 to 20 g / 10 min.
[0016] The TFE-based polymer preferably has a temperature range of 260° C. or less in which it exhibits a storage modulus of 0.1 to 5.0 MPa. In the above temperature range, the storage modulus of the TFE-based polymer is preferably 0.2 to 4.4 MPa, and more preferably 0.5 to 3.0 MPa. The temperature range in which the TFE-based polymer exhibits such a storage modulus is preferably 180 to 260° C., and more preferably 200 to 260° C. In the above temperature range, the TFE-based polymer is likely to effectively exhibit adhesion based on its elasticity.
[0017] The TFE-based polymer may be a homopolymer of TFE, or a copolymer of TFE and another monomer (hereinafter also referred to as a comonomer) copolymerizable with TFE. The TFE polymer preferably contains 75 to 100 mol % of TFE units and 0 to 25 mol % of comonomer units based on all units constituting the TFE polymer.
[0018] Examples of TFE-based polymers include polytetrafluoroethylene, copolymers having TFE units and ethylene units, copolymers having TFE units and propylene units, copolymers having TFE units and perfluoro(alkyl vinyl ether) (hereinafter also referred to as "PAVE") units, copolymers having TFE units and hexafluoropropylene (hereinafter also referred to as "HFP") units, copolymers having TFE units and fluoroalkylethylene (hereinafter also referred to as "FAE") units, and copolymers having TFE units and chlorotrifluoroethylene units.
[0019] Examples of PAVE include CF2=CFOCF3, CF2=CFOCF2CF3, CF2=CFOCF2CF2CF3 (hereinafter also referred to as "PPVE"), CF2=CFOCF2CF2CF2CF3, and CF2=CFO(CF2)8F. Examples of FAE include CH2=CH(CF2)2F, CH2=CH(CF2)3F, CH2=CH(CF2)4F, CH2=CF(CF2)3H, and CH2=CF(CF2)4H.
[0020] A preferred embodiment of the TFE-based polymer is a polymer having TFE units and PAVE units or HFP units (hereinafter, both are also collectively referred to as "comonomer units F"). The polymer of this embodiment preferably has 90 to 99 mol % of TFE units and 0.5 to 10 mol % of comonomer units F based on all units constituting the polymer. The polymer of this embodiment may be composed of only TFE units and comonomer units F, or may further have other units.
[0021] Another preferred embodiment of the TFE-based polymer is a polymer having a TFE unit (hereinafter also referred to as "polymer F1") having at least one functional group (hereinafter also simply referred to as "functional group") selected from the group consisting of a carbonyl group-containing group, a hydroxy group, an epoxy group, an amide group, an amino group, and an isocyanate group. If the TFE-based polymer has a functional group, it is easy to make the rate of change in dielectric tangent, which will be described later, 30% or less. In addition, if the TFE-based polymer has a functional group, when a metal layer is laminated on at least one surface of the substrate, the adhesion between the substrate and the metal layer is likely to be good even if the surface of the metal layer that contacts the substrate is not roughened (for example, when Rzjis is 2.0 μm or less).
[0022] The functional group may be contained in a monomer unit in the polymer F1, or may be contained in a terminal group of the main chain of the polymer F1. The latter polymer may be a polymer having a functional group as a terminal group derived from a polymerization initiator, a chain transfer agent, or the like. The polymer F1 is preferably a polymer having a monomer unit having a functional group and a TFE unit. In this case, the polymer F1 preferably further has other units, and more preferably has a comonomer unit F.
[0023] From the viewpoint of adhesion to inorganic fillers and metal layers, the functional group is preferably a carbonyl group-containing group. Examples of the carbonyl group-containing group include carbonate groups, carboxy groups, haloformyl groups, alkoxycarbonyl groups, acid anhydride residues (-C(O)OC(O)-), and fatty acid residues, with carboxy groups and acid anhydride residues being preferred. As the monomer unit having a functional group, a monomer unit having a carbonyl group-containing group, a monomer unit having a hydroxyl group, a monomer unit having an epoxy group, and a monomer unit having an isocyanate group are preferred, and a monomer unit having a carbonyl group-containing group is particularly preferred.
[0024] As the monomer having a carbonyl group-containing group, a cyclic monomer having an acid anhydride residue, a monomer having a carboxy group, a vinyl ester, and a (meth)acrylate are preferred, and a cyclic monomer having an acid anhydride residue is particularly preferred. As the cyclic monomer, itaconic anhydride, citraconic anhydride, 5-norbornene-2,3-dicarboxylic anhydride (also called himic anhydride, hereinafter also referred to as "NAH"), and maleic anhydride are preferable.
[0025] The polymer F1 is preferably a polymer containing a monomer unit having a functional group, a TFE unit, and a comonomer unit F. A specific example of such a polymer F1 is the polymer (X) described in WO 2018 / 16644. The proportion of TFE units in polymer F1 is preferably 90 to 99 mol % of all units constituting polymer F1. The proportion of the comonomer units F in the polymer F1 is preferably 0.5 to 9.97 mol % of all the units constituting the polymer F1. The proportion of monomer units having a functional group in polymer F1 is preferably 0.01 to 3 mol % of all units constituting polymer F1.
[0026] The inorganic filler is preferably one having a low relative dielectric constant, dielectric tangent, and thermal expansion coefficient, and examples of the inorganic filler include silica, alumina, glass, stearite, beryllium oxide, aluminum nitride, magnesia ceramics, and boron nitride. The inorganic filler may be porous or non-porous. The shape of the inorganic filler may be, for example, crushed, spherical, approximately spherical, oval, needle-like, plate-like, scaly, rod-like, or cube-like, with crushed being preferred. Crushed inorganic fillers have many surface irregularities, and are expected to provide strong adhesion to TFE-based polymers due to the anchor effect. The inorganic fillers may be used alone or in combination of two or more kinds.
[0027] As the inorganic filler, silica is preferred. Examples of silica include fused silica, fumed silica, nonporous silica, porous silica (mesoporous silica, microporous silica), hollow silica, etc. These silicas may be used in a dry state, a sol state or a slurry state, or may be used after being subjected to a baking treatment at a temperature of 600° C. or higher to reduce the number of silanol groups. The silica is preferably in a crushed form. In order to improve the dispersibility of the silica in the TFE-based polymer, the silica may be subjected to a surface treatment with a surface treatment agent such as a silane coupling agent or a titanate coupling agent.
[0028] The inorganic filler may be washed with an alkali, which is effective in reducing the dielectric tangent since it can remove water adsorbed on the surface of the inorganic filler. The alkali used in the alkaline cleaning includes, for example, NaOH, KOH, and mixed alkalis thereof. The inorganic filler is preferably alkali-washed silica.
[0029] The average particle size of the inorganic filler is preferably 100 μm or less, more preferably 60 μm or less, and particularly preferably 40 μm or less. When the average particle size of the inorganic filler is equal to or less than the upper limit, the inorganic filler is unlikely to protrude from the substrate surface when the substrate has a thickness of 500 μm or less, and stable dielectric properties are easily obtained.
[0030] The average particle size of the inorganic filler is the volume-based cumulative 50% diameter (D50) determined by the laser diffraction / scattering method. In other words, the particle size distribution is measured by the laser diffraction / scattering method, and a cumulative curve is calculated with the total volume of the particle group as 100%, and the average particle size is the particle size at the point on the cumulative curve where the cumulative volume is 50%.
[0031] When the inorganic filler is in a crushed form, it is preferable that the inorganic filler can pass through a sieve with an opening of 45 μm. If the inorganic filler can pass through a sieve with an opening of 45 μm, when the thickness of the substrate is 500 μm or less, the inorganic filler is unlikely to protrude from the substrate surface, and stable dielectric properties are likely to be obtained.
[0032] The inorganic filler may have two or more peaks in the particle size distribution curve measured by a laser diffraction / scattering method. For example, when two or more inorganic fillers having different average particle sizes are mixed and used, the particle size distribution curve has two or more peaks. When the amount of inorganic filler added increases, the inorganic fillers come into contact with each other, resulting in a region surrounded by the inorganic filler. When the number of peaks is one, the variation in size of the inorganic filler is relatively small, so other inorganic fillers are difficult to pass through the gaps between the inorganic fillers constituting the region, and it is difficult to further fill the region with other inorganic fillers. When the number of peaks is two or more, the variation in size of the inorganic filler is relatively large, so other inorganic fillers are easy to pass through the gaps between the inorganic fillers constituting the region, and other inorganic fillers can be further filled in the region, making it easy to improve the filling rate.
[0033] The substrate may further comprise a surfactant. The surfactant is used, for example, to improve the dispersibility of the resin powder and the compatibility of the inorganic filler when mixing a dispersion of a resin powder containing a TFE-based polymer with an inorganic filler in producing the present substrate. Examples of the surfactant include nonionic surfactants, anionic surfactants, cationic surfactants, and amphoteric surfactants, and the most suitable compound is appropriately selected. As the surfactant, a nonionic surfactant is preferred from the viewpoint of low dielectric tangent.
[0034] The surfactant is preferably a surfactant having a fluorine-containing group and a hydrophilic group (hereinafter, also referred to as "fluorine-based surfactant"). By using a fluorine-based surfactant, the surface tension of the liquid medium is reduced, the wettability to the surface of the resin powder is improved, and the dispersibility of the resin powder is improved. At the same time, the fluorine-containing group is adsorbed to the surface of the resin powder containing the TFE-based polymer, and the hydrophilic group extends into the liquid medium, and the steric hindrance of the hydrophilic group prevents the aggregation of the resin powder, thereby improving the dispersion stability.
[0035] The fluorine-containing group is preferably one having high hydrophobicity, and examples thereof include fluorinated hydrocarbon groups such as perfluoroalkyl groups and perfluoroalkenyl groups (e.g., hexafluoropropylene trimer groups). The perfluoroalkyl groups and perfluoroalkenyl groups may each have a straight-chain structure or a branched structure. The number of carbon atoms in the fluorine-containing group is preferably 2 or more, and more preferably 4 to 20. As the fluorine-containing group, a fluorine-containing group having a branched structure such as -CF(CF3)C(=C(CF3)2)(CF(CF3)2) is preferred because it is bulky and has excellent adsorptive ability.
[0036] The hydrophilic group is a group that is relatively hydrophilic to the fluorine-containing group, and may be a general hydrophilic group, or may be a group that is usually considered to be a hydrophobic group, as long as it is relatively hydrophilic to the fluorine-containing group. For example, a polyoxypropylene group is relatively hydrophobic to a polyoxyethylene group, which is a hydrophilic group, and is usually considered to be a hydrophobic group, but is relatively less hydrophobic (highly hydrophilic) to the fluorine-containing group, and is therefore a hydrophilic group in the present invention. Examples of the hydrophilic group include a polyoxyethylene group, a polyoxypropylene group, a polyoxybutylene group, a polyoxytetramethylene group, an amino group, a ketone group, a carboxyl group, and a sulfone group. As the hydrophilic group, a polyoxyalkylene group consisting of an oxyalkylene group having 2 to 4 carbon atoms is preferable, and a polyoxyethylene group is particularly preferable.
[0037] The fluorosurfactant may also be a copolymer of a monomer having a fluorine-containing group and a monomer having a hydrophilic group, and as such a surfactant, a copolymer of a monomer having a fluorine-containing group and a monomer having a polyoxyalkylene group is particularly preferred.
[0038] When the fluorosurfactant is a copolymer of a monomer having a fluorine-containing group and a monomer having a hydrophilic group, the weight-average molecular weight of the fluorosurfactant is preferably 1000 to 150000, more preferably 3000 to 100000, and particularly preferably 5000 to 30000. In this case, the fluorine-containing group is more likely to be adsorbed to the surface of the resin powder than to the liquid medium, and the dispersibility and dispersion stability of the resin powder are likely to be improved. In addition, the dispersion in which the resin powder is dispersed can be made to have excellent mixability with different resin materials and their varnishes and excellent coatability. The weight average molecular weight of the fluorosurfactant is measured by gel permeation chromatography (GPC).
[0039] Specific examples of fluorine-based surfactants include perfluoroalkyl group-containing Ftergent M series, Ftergent F209, Ftergent 222F, Ftergent 208G, Ftergent 218GL, Ftergent 710FL, Ftergent 710FM, Ftergent 710FS, Ftergent 730FL, Ftergent 730LM (manufactured by Neos Corporation), Megafac series such as Megafac F-553, Megafac F-555, Megafac F-556, Megafac F-557, Megafac F-559, Megafac F-562, Megafac F-565 (manufactured by DIC Corporation), Unidyne series such as Unidyne DS-403N (manufactured by Daikin Industries, Ltd.), and the like. Among these, FTERGENT 710FL, FTERGENT 710FM and FTERGENT 710FS, which are surfactants in which the fluorine-containing group has a branched structure and three-dimensional bulkiness, are preferred.
[0040] Two or more surfactants may be used in combination. In this case, at least a part of the two or more surfactants is preferably a fluorine-based surfactant. A part of the two or more surfactants may be a surfactant that does not have a fluorine-containing group.
[0041] The present substrate may further contain other components other than the TFE-based polymer, inorganic filler, and surfactant, as necessary, within the scope of not impairing the effects of the present invention. Examples of other components include resins other than TFE-based polymers (eg, polyimides), thickeners, and the like.
[0042] In the present substrate, the ratio of the volume of the inorganic filler to the total volume of the TFE-based polymer and the inorganic filler is preferably 40 to 90 volume%, more preferably 45 to 85 volume%, and particularly preferably 50 to 80 volume%. If the ratio of the inorganic filler is equal to or greater than the lower limit, the thermal expansion coefficient and dielectric loss tangent of the substrate can be made lower. If the ratio of the inorganic filler is equal to or less than the upper limit, the relative dielectric constant of the substrate can be made lower and the mechanical strength can be made higher. The volumes are at 25°C.
[0043] The ratio of the total volume of the TFE polymer and the inorganic filler to the total volume of the present substrate is preferably 80% by volume or more, more preferably 90% by volume or more, and particularly preferably 95% by volume or more. If the ratio of the total volume of the TFE polymer and the inorganic filler is equal to or more than the lower limit, the dielectric loss tangent, relative dielectric constant, and thermal expansion coefficient of the substrate can be reduced, and the mechanical strength can be increased.
[0044] The content of the surfactant is preferably from 1 to 30% by mass, and more preferably from 2 to 10% by mass, based on the total mass of the TFE-based polymer and the inorganic filler.
[0045] The thickness of the present substrate is preferably 60 to 500 μm, more preferably 80 to 400 μm, and still more preferably 100 to 300 μm. When the thickness of the substrate is equal to or less than the upper limit, the mountability is superior. When the thickness of the substrate is equal to or more than the lower limit, the substrate rigidity is superior.
[0046] The substrate has a dielectric tangent change rate of 30% or less before and after a 127 μm thick test piece cut from the substrate is subjected to USPCT at 120° C. and 85% RH for 72 hours. The change rate is preferably 25% or less, more preferably 20% or less. If the change rate is equal to or less than the upper limit, the substrate has excellent mechanical strength and is less likely to break when bent or vibrated. Therefore, by using the substrate, a highly reliable printed wiring board can be obtained. The rate of change of the dielectric loss tangent is considered to indicate the amount of voids at the interface between the TFE-based polymer and the inorganic filler in the present substrate. If many voids exist at the interface, moisture penetrates into the voids during USPCT and is adsorbed on the surface of the inorganic filler. As a result, the moisture content of the substrate increases and the dielectric loss tangent becomes high. If the rate of change of the dielectric loss tangent is equal to or less than the upper limit, there are no or only a few voids at the interface between the TFE-based polymer and the inorganic filler in the present substrate, and they are sufficiently adhered to each other, so that the mechanical strength is considered to be excellent.
[0047] The present substrate can be produced, for example, by preparing a paste composition containing a TFE-based polymer, an inorganic filler, and a liquid medium, applying the paste composition onto an adherend, and drying and baking the composition. This results in the present substrate being formed on the adherend. If necessary, the present substrate is peeled off from the adherend. When the present substrate is used for a metal laminate plate, a material capable of forming a metal layer (metal foil, etc.) may be used as the adherend, and the present substrate may be used for the metal laminate plate without peeling it off.
[0048] Examples of the liquid medium include inorganic solvents such as water, organic solvents, and the like. Examples of the organic solvent include the organic solvents described in International Publication No. 2018 / 16644. The liquid medium may be a mixture of two or more compatible liquid media. For example, it may be a mixture of a water-soluble organic solvent and water, or a mixture of two or more organic solvents. The liquid medium is preferably one capable of dissolving the TFE-based polymer.
[0049] In the paste composition, the content of the liquid medium is preferably 30 to 95 parts by mass, more preferably 40 to 90 parts by mass, and particularly preferably 50 to 85 parts by mass, based on 100 parts by mass of the total of the TFE-based polymer and the inorganic filler. When the content of the liquid medium is equal to or more than the lower limit, the surface smoothness of the substrate formed is more excellent. When the content of the liquid medium is equal to or less than the upper limit, the thick-film coating property is more excellent.
[0050] The paste composition can be prepared by mixing the TFE-based polymer, the inorganic filler, and the liquid medium. If necessary, a surfactant or other components may be mixed with these materials. More specifically, the method for preparing the paste composition includes a method of adding an inorganic filler to a solution of a TFE-based polymer or a dispersion of a resin powder containing a TFE-based polymer and mixing the inorganic filler, and a method of mixing a solution of a TFE-based polymer or a dispersion of a resin powder containing a TFE-based polymer with a dispersion of an inorganic filler (let-down method). Each material can be mixed using a mixing device such as a rotary shear type mixer, a colloid mill, a roll mill, an ultrasonic disperser, a container-driven mill, or a media stirring mill.
[0051] The mixing conditions for preparing the paste composition are set so that the rate of change in the dielectric tangent is 30% or less. The rate of change in the dielectric tangent can be adjusted, for example, by varying the strength of shear when mixing the materials. By applying stronger shear when mixing, the rate of change in the dielectric tangent can be made smaller. This is thought to be because applying stronger shear makes it less likely for voids to form at the interface between the TFE-based polymer and the inorganic filler.
[0052] The method for applying the paste composition is not particularly limited, and can be, for example, by using a coating device such as a spinner, a screen printer, a blade coater, or a die coater. The method for drying the applied paste composition is not particularly limited. For example, a method of heating using a heating device such as a hot plate or an oven can be mentioned. The heating conditions may be set appropriately depending on the type of liquid medium as long as the liquid medium can be removed.
[0053] The tensile strength of the substrate is preferably 7.0 MPa or more, more preferably 8.0 MPa or more, and even more preferably 10.0 MPa or more.The tensile modulus of elasticity is preferably 1.0 GPa or more, more preferably 1.5 GPa or more, and even more preferably 2.0 GPa or more.
[0054] The substrate described above contains a TFE-based polymer and an inorganic filler, and has a dielectric tangent change rate of 30% or less under specific conditions, so that it has low dielectric tangent, relative dielectric constant, and thermal expansion coefficient, and also has excellent mechanical strength. In particular, if the TFE-based polymer has a functional group, it is easy to obtain superior mechanical strength and excellent adhesion between the substrate and the metal layer.
[0055] [Metal laminate] The metal laminate of the present invention comprises a substrate and a metal layer located in contact with at least one surface of the substrate. The metal laminate may have one or more main substrates. When the metal laminate has more than one main substrate, the substrates may be the same or different. The metal laminate may have one or more metal layers, and when it has more than one metal layer, the metal layers may be the same or different. In addition to the main substrate and metal layer, the metal laminate may further include other substrates (e.g., FR4 substrate, LCP (liquid crystal polymer) substrate, PPE (polyphenylene ether) substrate, etc.) FR4 is an abbreviation for "Flame Retardant Type 4" and refers to a glass fiber cloth impregnated with epoxy resin and subjected to a heat curing process to form it into a plate shape.
[0056] An example of the metal laminate of the present invention is shown in Figure 1. The metal laminate 1 of this example is a single-sided metal laminate having a substrate 3 and a metal layer 5 located in contact with one surface 3a of the substrate 3. The substrate 3 is the substrate. Another example of the metal laminate of the present invention is shown in Figure 2. The metal laminate 1 of this example is a double-sided metal laminate having a substrate 3 and metal layers 5 located in contact with both one surface 3a and the other surface 3b of the substrate 3.
[0057] Examples of metals constituting the metal layer include copper, copper alloys, stainless steel, nickel, nickel alloys (including alloy 42), aluminum, aluminum alloys, titanium, titanium alloys, etc. Copper is preferred in terms of electrical conductivity and chemical resistance. The metal layer is preferably a layer made of a metal foil, and particularly preferably a layer made of copper foil. Examples of copper foil include rolled copper foil and electrolytic copper foil. An anti-rust layer (such as an oxide film of chromate) and a heat-resistant layer may be formed on the surface of the metal foil.
[0058] The thickness of the metal layer is preferably from 1 to 40 μm, and more preferably from 10 to 30 μm. The surface of the metal layer may be treated with a silane coupling agent. In this case, the entire surface of the metal layer may be treated with the silane coupling agent, or only a part of the surface of the metal layer may be treated with the silane coupling agent.
[0059] The Rzjis of the surface of the metal layer that contacts the main substrate is preferably 5.0 μm or less, more preferably 3.0 μm or less, even more preferably 2.0 μm or less, and particularly preferably 1.0 μm or less. If Rzjis is equal to or less than the upper limit, a printed wiring board with excellent transmission characteristics is easily obtained. In terms of transmission characteristics, the smaller the Rzjis, the better, and the lower limit of Rzjis is not particularly limited, but is, for example, 0.1 μm.
[0060] The peel strength of the interface between the substrate and the metal layer is preferably 5 N / cm or more, more preferably 8 N / cm or more. If the peel strength is equal to or more than the lower limit, the reliability is better. The higher the peel strength, the more preferable it is, and there is no particular upper limit for the peel strength.
[0061] The metal laminate plate of the present invention can be produced, for example, by (1) a method in which a material capable of forming a metal layer is laminated on at least one surface of the present substrate and then thermocompression-bonded; (2) a method in which the present substrate is formed on a material capable of forming a metal layer, and if necessary, a material capable of forming another metal layer is laminated on the surface of the formed present substrate and then thermocompression-bonded; or (3) a method in which two of the present substrates formed on a material capable of forming a metal layer are prepared, and then the present substrate sides are brought together to laminate and thermocompress the substrates. An example of a material that can form the metal layer is a metal foil.
[0062] In the methods (1), (2), and (3), the temperature during thermocompression bonding is equal to or higher than the melting point of the TFE-based polymer, and is preferably at least 10° C. higher than the melting point, more preferably at least 20° C. higher than the melting point, and particularly preferably at least 40° C. higher than the melting point. The temperature during thermocompression bonding is preferably not higher than a temperature 100° C. higher than the melting point. If the temperature during thermocompression bonding is within the above range, the substrate and the metal layer can be sufficiently bonded while suppressing thermal degradation of the TFE-based polymer. The temperature during thermocompression is the temperature of the heating platen of the compression device.
[0063] The pressure during thermocompression bonding is preferably 0.2 MPa or more, more preferably 0.5 MPa or more, and even more preferably 1.0 MPa or more. The pressure during thermocompression bonding is preferably 10.0 MPa or less. If the pressure during thermocompression bonding is within the above range, the present substrate and the metal layer can be sufficiently bonded together without damaging the present substrate.
[0064] The thermocompression bonding is preferably performed in a vacuum atmosphere. The degree of vacuum during thermocompression bonding is preferably 100 kPa or less, more preferably 50 kPa or less, and even more preferably 20 kPa or less. If the degree of vacuum is equal to or less than the upper limit, the inclusion of air bubbles at the interfaces between the main substrate and the metal layer constituting the metal laminate can be suppressed, and at the same time, deterioration of the metal layer due to oxidation can be suppressed. It is also preferable to raise the temperature after the vacuum level is reached, since raising the temperature before the vacuum level is reached may cause air bubbles. In the thermocompression bonding, it is preferable to apply pressure after the temperature of the main substrate reaches the melting point. If the thermocompression bonding is performed before the temperature reaches the melting point, voids may occur between the main substrate and the metal layer, or unevenness in the adhesion strength may occur.
[0065] In the methods (2) and (3), in order to form the present substrate on a material capable of forming a metal layer, for example, as described above, a paste composition containing a TFE-based polymer, an inorganic filler, and a liquid medium is prepared, and the paste composition is applied onto a material capable of forming a metal layer (adherend), and then dried. EXAMPLES
[0066] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following description. Example 1 is an example, and Example 2 is a comparative example.
[0067] (Proportion of each unit in TFE-based polymer) The proportion of NAH units was determined by infrared absorption spectroscopy, and the proportions of units other than NAH units were determined by melting NMR analysis and fluorine content analysis.
[0068] <Infrared absorption spectrum analysis> The TFE-based polymer was press-molded to obtain a film having a thickness of 200 μm. The film was analyzed by infrared spectroscopy to obtain an infrared absorption spectrum. In the infrared absorption spectrum, the absorption peak of the NAH unit in the TFE-based polymer was at 1778 cm -1 The absorbance of this absorption peak was measured, and the molar extinction coefficient of NAH was 20810 mol -1 L cm -1 The proportion of NAH units in the TFE-based polymer was calculated using the formula:
[0069] (Melting Point) Using a differential scanning calorimeter (Seiko Instruments Inc., DSC-7020), the melting peak was recorded when the TFE-based polymer was heated at a rate of 10° C. / min, and the temperature (° C.) corresponding to the maximum value was taken as the melting point.
[0070] (MFR) Using a melt indexer (manufactured by Technoseven), the mass (g) of the TFE-based polymer flowing out from a nozzle with a diameter of 2 mm and a length of 8 mm in 10 minutes at 372° C. under a load of 49 N was measured and used as the MFR.
[0071] (Storage modulus) Based on ISO 6721-4:1994, a dynamic viscoelasticity measuring device (DMS6100, manufactured by SII Nano Technology Co., Ltd.) was used to measure the storage modulus at 260°C by raising the temperature of the TFE-based polymer from 20°C at a rate of 2°C / min under conditions of a frequency of 10 Hz, a static force of 0.98 N, and a dynamic displacement of 0.035%.
[0072] (average particle size of granular polymer) A 2.000 mesh sieve (opening 2.400 mm), a 1.410 mesh sieve (opening 1.705 mm), a 1.000 mesh sieve (opening 1.205 mm), a 0.710 mesh sieve (opening 0.855 mm), a 0.500 mesh sieve (opening 0.605 mm), a 0.250 mesh sieve (opening 0.375 mm), a 0.149 mesh sieve (opening 0.100 mm), and a tray were stacked in this order from above. A sample (polymer) was placed on top of them, and sieving was performed with a shaker for 30 minutes. Thereafter, the mass of the sample remaining on each sieve was measured, and the cumulative total of the passing mass for each opening value was graphed, and the particle diameter when the cumulative total of the passing mass was 50% was taken as the average particle diameter of the sample.
[0073] (Resin powder D50 and D90) The resin powder was dispersed in water and the volumetric particle size distribution was measured using a laser diffraction / scattering particle size distribution analyzer (LA-920, manufactured by Horiba, Ltd.), and D50 and D90 were calculated.
[0074] (average silica particle size) Silica was dispersed in water and the volumetric particle size distribution was measured using a laser diffraction / scattering particle size distribution analyzer (MICROTRAC HRA DHSX100, manufactured by Nikkiso Co., Ltd.) to determine the average particle size (D50).
[0075] (Dielectric constant and dielectric tangent) The relative dielectric constant and dielectric loss tangent of the substrate (thickness 127 μm) were measured at 25° C. and 10 GHz according to the method specified in JIS R 1641:2007 using a cavity resonator and a vector network analyzer. The substrate was obtained by removing the copper foil of a composite CCL described below with ferric chloride (same below).
[0076] (Thermal expansion coefficient) A test piece of 10 mm x 10 mm was cut out from the substrate. The linear expansion coefficient CTE (z) in the thickness direction of this test piece was measured using a thermomechanical analyzer (TMA402 F1 Hyperion, manufactured by NETZSCH). Specifically, the sample was heated at a rate of 2°C / min in a nitrogen atmosphere with a load of 19.6 mN in a temperature range of -65°C to 150°C, and the amount of change in the thickness of the sample was measured. After the measurement was completed, the linear expansion coefficient (CTE) at -40 to 125°C was calculated from the amount of change in the sample from -40°C to 125°C.
[0077] (Change in dielectric tangent by USPCT) A test piece measuring 35 mm in length and 35 mm in width was cut out from the substrate. The test piece was placed in a pressure cooker at 120°C and 85% RH, and subjected to USPCT. The dielectric tangent (tan δ) of the test piece was measured 5 hours, 24 hours, 48 hours, and 72 hours after placement, and the rate of change in the dielectric tangent before and after USPCT was calculated using the above formula (1).
[0078] (mechanical strength) A test piece measuring 60 mm in length and 5 mm in width was cut out from the substrate. The test piece was bent 180° at a position 30 mm from one end in the longitudinal direction with a radius of curvature of 2 mm, alternately in the forward and reverse directions, and repeated 100 times. The substrate was then visually observed and evaluated according to the following criteria. ◯ (Fair): The board was not broken and no cracks or crevices were observed. × (Not acceptable): The board has cracks or chips.
[0079] (peel strength) A rectangular test piece measuring 100 mm in length and 10 mm in width was cut out from the composite CCL described below. The copper foil was peeled off from the substrate to a position 10 mm from one end in the longitudinal direction of the test piece. One end of the peeled copper foil was peeled off at a 90° angle at a tensile speed of 50 mm / min using a tensile tester (Shimadzu Autograph AGS-X), and the maximum load was recorded as the peel strength (N / cm).
[0080] (Transmission loss) A grounded coplanar line (G-CPW) with a line length of 12.5 mm was fabricated on the composite CCL described later, and the transmission loss at 80 GHz was measured. The impedance was 50 Ω.
[0081] (Production Example 1) Polymer X, which is a TFE-based polymer, was produced by the procedure described in paragraph
[0123] of WO 2016 / 017801 using NAH (himic acid anhydride, manufactured by Hitachi Chemical Co., Ltd.), TFE and PPVE (CF2=CFO(CF2)3F, manufactured by AGC) as monomers. The copolymerization composition of polymer X was NAH unit / TFE unit / PPVE unit=0.1 / 97.9 / 2.0 (mol%). The melting point of polymer X was 300° C., the MFR was 17.6 g / 10 min, the relative dielectric constant (10 GHz) was 2.0, and the storage modulus at 260° C. was 1.1 MPa. The obtained polymer X was granular, and the average particle size was 1554 μm.
[0082] Next, the polymer X was pulverized using a jet mill (Seishin Enterprise Co., Ltd., single track jet mill FS-4 type) under conditions of a pulverization pressure of 0.5 MPa and a processing speed of 1 kg / hr to obtain a resin powder P-1. The resin powder P-1 had a D50 of 2.58 μm and a D90 of 7.1 μm.
[0083] (Example 1) Silica (Tatsumori, crushed silica E-1, average particle size 11 μm) was divided using a Fritsch sieve shaker ANALYSETTE3, and the silica that passed through a sieve with 45 μm openings was collected. The average particle size of the collected silica was 10 μm. 100 g of resin powder P-1, 6 g of a nonionic fluorosurfactant (Neos Corporation, Futergent 710FL), 137 g of cyclohexanone, and 151 g of the silica recovered above were placed in a pot and vibration-mixed for 20 minutes with a low-frequency resonant acoustic mixer (LabMASII) manufactured by Lesodyne Corporation, applying an acceleration of approximately 80 G to obtain a slurry.
[0084] The slurry was applied to a surface of 18 μm thick copper foil (Mitsui Mining & Smelting Co., Ltd., TQ-M4-VSP) to a thickness of 200 μm by doctor blade method, dried in an atmospheric environment at room temperature for 12 hours, and then heated and dried at 350° C. for 20 minutes in a nitrogen atmosphere to form a substrate. This resulted in a single-sided copper clad laminate in which copper foil was laminated on one surface of the substrate. The Rzjis of the surface of the copper foil to which the slurry was applied was 0.6 μm. The same copper foil as above was laminated on the substrate side of the single-sided copper-clad laminate, and pressed for 60 minutes in a vacuum hot press at 330°C and 8 MPa pressure to obtain a double-sided copper-clad laminate. Hereinafter, this double-sided copper-clad laminate is referred to as "composite CCL." In the obtained composite CCL substrate, the ratio of the volume of silica to the total volume of polymer X and silica was 60 vol%, the ratio of the volume of polymer X and silica to the total volume of the substrate was 100 vol%, and the thickness of the substrate was 127 μm.
[0085] (Example 2) A commercially available composite CCL (RO3003 manufactured by Rogers) was used as the composite CCL in Example 2. The composite CCL substrate contained polytetrafluoroethylene (PTFE) and silica, the ratio of the volume of silica to the total volume of PTFE and silica was 50 volume %, the ratio of the volume of PTFE and silica to the total volume of the substrate was 95 volume %, and the thickness of the substrate was 127 μm. In addition, Rzjis of the surface of the copper foil in contact with the substrate was 7.0 μm.
[0086] The composite CCL of each example was evaluated as described above. The relative permittivity, dielectric loss tangent, CTE, transmission loss, mechanical strength, copper foil peel strength (all before USPCT), and the rate of change in dielectric loss tangent before and after 72 hours of USPCT are shown in Table 1. The relative permittivity, dielectric loss tangent, and the rate of change in dielectric loss tangent before and after 72 hours of USPCT are values at 10 GHz. In addition, Figure 3 shows the relationship between the time elapsed after being placed in a pressure cooker (USPCT placement time) and the rate of change in dielectric loss tangent in Examples 1 and 2 (the dependency of the rate of change in dielectric loss tangent on the USPCT placement time).
[0087] [Table 1]
[0088] (Tensile strength) A test piece 20 mm wide, 200 mm long, and 125 μm thick cut from the substrate was clamped at a position 25 mm from the end, and a load was applied to the test piece at room temperature at a tensile speed of 1 mm / min using a tensile testing machine (Shimadzu Autograph AGX), and the load and the elongation (strain) of the test piece were measured to obtain a stress-strain curve. The tensile strength is the value obtained by dividing the breaking strength or yield strength in the stress-strain curve by the cross-sectional area of the test piece. (tensile modulus) The tensile modulus is the slope of the region (elastic deformation region) in which the tensile strength increases linearly in proportion to the strain in a stress-strain curve. The tensile breaking strength and tensile modulus are shown in Table 2.
[0089] [Table 2]
[0090] The substrate of Example 1 had excellent mechanical strength. In addition, the transmission loss was small because a low-roughness copper foil was used. The substrate of Example 2, in which the change rate of the dielectric tangent before and after 72 hours of USPCT was more than 30%, had poor mechanical strength. In addition, the transmission loss was large because the low-roughness copper foil could not be used. Moreover, the substrate of Example 1 was superior to the substrate of Example 2 in both tensile strength and tensile modulus. [Industrial Applicability]
[0091] According to the present invention, it is possible to provide a substrate and a metal laminate having low relative dielectric constant, dielectric loss tangent, transmission loss, and thermal expansion coefficient, and also having high mechanical strength. Because of the high mechanical strength, by using the substrate and the metal laminate of the present invention, a highly reliable printed wiring board can be formed even in an environment with vibration, such as an automobile. The entire contents of the specification, claims, abstract and drawings of Japanese Patent Application No. 2019-144495, filed on August 6, 2019, are hereby incorporated by reference as the disclosure of the specification of the present invention.
Claims
1. A substrate comprising a tetrafluoroethylene-based polymer and an inorganic filler, the ratio of the volume of the inorganic filler to the total volume of the tetrafluoroethylene-based polymer and the inorganic filler being 40 to 90 volume %, The thickness of the substrate is 60 to 500 μm, The tetrafluoroethylene-based polymer comprises a melt-formable tetrafluoroethylene-based polymer F1 having a carbonyl group-containing group, The average particle size of the inorganic filler is 40 μm or less, A test piece having a thickness of 127 μm cut out from the substrate is subjected to an unsaturated pressure cooker test at 120° C. and 85% RH for 72 hours, and the rate of change in dielectric tangent at 10 GHz is 30% or less before and after the test piece is subjected to an unsaturated pressure cooker test at 120° C. and 85% RH for 72 hours.
2. The substrate of claim 1 , wherein the tetrafluoroethylene-based polymer F1 has units based on tetrafluoroethylene and units based on perfluoro(alkyl vinyl ether) or units based on hexafluoropropylene.
3. The substrate according to claim 1 , wherein the tetrafluoroethylene-based polymer F1 has a monomer unit having the carbonyl group-containing group.
4. The substrate according to any one of claims 1 to 3, wherein the inorganic filler is silica.
5. The substrate according to any one of claims 1 to 4, further comprising a surfactant.
6. The substrate of claim 5 , wherein the surfactant is a fluorosurfactant.
7. A metal laminate comprising the substrate according to any one of claims 1 to 6 and a metal layer located in contact with at least one surface of the substrate.
8. The metal laminate according to claim 7, wherein the metal layer is a layer made of copper foil.
9. 9. The metal laminate according to claim 7, wherein the ten-point average roughness of the surface of the metal layer that contacts the substrate is 2.0 μm or less.
10. The metal laminate according to any one of claims 7 to 9, wherein the peel strength of the interface between the substrate and the metal layer is 5 N / cm or more.
Citation Information
Patent Citations
Electric base body material
JP1988259907A
Wiring board
JP2006228871A
Laminate sheet
JP2019155853A
Process for producing fluorocopolymer nanocomposite
WO2011068129A1