HOT PRESSED MEMBER, STEEL PLATE FOR HOT PRESSING, AND METHOD FOR MANUFACTURING HOT PRESSED MEMBER

The Al-Fe intermetallic compound layer and plating composition in the hot press member address hydrogen embrittlement issues in Al-based plated steel sheets by reducing hydrogen intrusion and enhancing rapid release, facilitating high-strength part production with improved fracture resistance and productivity.

JP7568115B2Active Publication Date: 2024-10-16JFE STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023540210
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-06-03
Filing Date
2023-03-27
Publication Date
2024-10-16
Estimated Expiration
2043-03-27

AI Technical Summary

Technical Problem

Conventional Al-based plated steel sheets used in hot pressing face challenges with high hydrogen embrittlement due to excessive hydrogen intrusion during the manufacturing process, leading to low hydrogen release rates and reduced productivity, which is exacerbated by the need for prolonged residence times to release hydrogen, hindering the production of high-strength parts.

Method used

A hot press member with an Al-Fe based intermetallic compound layer and a diffusion layer on the steel surface, featuring a specific thickness and phase composition, along with a plating layer containing Si and optionally Mg, to minimize hydrogen intrusion and enhance rapid hydrogen release.

Benefits of technology

The solution effectively reduces hydrogen embrittlement by minimizing hydrogen entry during hot pressing and facilitating rapid hydrogen release, enabling the production of high-strength hot-pressed members with improved delayed fracture resistance and productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568115000001
    Figure 0007568115000001
  • Figure 0007568115000002
    Figure 0007568115000002
  • Figure 0007568115000003
    Figure 0007568115000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide a hot-pressed member in which the amount of hydrogen penetrated during a hot pressing process is reduced, from which the penetrated hydrogen can be released within a short time, and which has excellent delayed fracture resistance properties. Provided is a hot-pressed member comprising a steel material, an Al-Fe-based intermetallic compound layer provided on at least one surface of the steel material and having a thickness of 10 to 35 μm, and a diffusion layer provided at the boundary between the Al-Fe-based intermetallic compound layer and the steel material, in which the Al-Fe-based intermetallic compound layer comprises an Al-rich phase having an Al concentration of 40% by mass or more and a Fe-rich phase having an Al concentration of less than 40% by mass, and the average length of the direction perpendicular to the thickness direction in a cross section of the Fe-rich phase is 10 μm or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hot-pressed member, a steel plate for hot-pressing, and a method for manufacturing a hot-pressed member. [Background technology]

[0002] In recent years, in the field of automobiles, the use of high-strength hot-dip galvanized steel sheets or electrolytic galvanized steel sheets with rust-resistant properties has been increasing, as the performance of steel sheets has improved and weight reduction has been promoted. However, in many cases, the press formability of steel sheets decreases as the strength of the steel sheets increases, making it difficult to obtain complex part shapes. For example, in automobile applications, parts that require rust resistance and are difficult to form include chassis and other underbody components and frame structural components such as B-pillars.

[0003] In light of this, the manufacture of automotive parts by hot pressing, which is easier to achieve both press formability and high strength compared to cold pressing, has been rapidly increasing in recent years. Among these, Al-based plated steel sheets have attracted attention as steel sheets for hot pressing due to their excellent resistance to high-temperature oxidation, and various Al-based plated steel sheets suitable for hot pressing and hot-pressed members using the Al-based plated steel sheets have been proposed.

[0004] For example, Patent Document 1 proposes an Al-based plated steel sheet for hot press use having an Al-based plated layer containing 1 to 15 mass % of Si and 0.5 to 10 mass % of Mg. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2003-034845 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the conventional technique proposed in Patent Document 1 has the following problems.

[0007] That is, as described above, hot pressing is widely used in the manufacture of automotive frame structural members, etc. And, while hot press members mainly have a tensile strength of 1.5 GPa after hot press forming, there is a demand for higher strength, such as a tensile strength of 1.8 GPa or more, in order to further reduce the weight of automobile bodies.

[0008] However, as the strength of steel material increases, the problem of hydrogen embrittlement becomes more pronounced. Therefore, in order to increase the strength of hot-pressed members, more advanced measures against hydrogen embrittlement are required.

[0009] Here, the causes of the penetration of diffusible hydrogen into steel, which causes hydrogen embrittlement, can be broadly divided into two categories: hydrogen penetration during the manufacturing process of hot-pressed components, and hydrogen penetration caused by corrosion reactions when the hot-pressed components are actually used. However, in the general operating environment of automobiles, the corrosion rate of hot-pressed components made of Al-based plated steel sheets is low, and the amount of hydrogen generated by corrosion reactions is also relatively small.

[0010] On the other hand, examples of hydrogen that enters during the manufacturing process of hot-pressed members include hydrogen introduced during the manufacturing of steel sheets for hot-pressing, hydrogen introduced during the hot-pressing process, hydrogen introduced during the painting process, etc. In the case of hot-pressed members using Al-based plated steel sheets as their raw material, it is known that the amount of hydrogen introduced during the hot-pressing process is extremely large.

[0011] Therefore, when using Al-based plated steel sheets as materials, it is particularly important to reduce the amount of diffusible hydrogen introduced during the hot pressing process.

[0012] On the other hand, even if a large amount of hydrogen is introduced into the steel during the hot pressing process, it may be possible to release the hydrogen and reduce the amount of hydrogen in the steel by providing a sufficient residence time after the hot pressing.

[0013] However, in hot-pressed parts made of existing Al-based plated steel sheets, the rate at which hydrogen is released through the plated layer is extremely low, and so in order to reduce the amount of diffusible hydrogen to a level that does not cause practical problems, a significantly long residence time is required, which reduces productivity.

[0014] Therefore, hot-pressed members are required to have a small amount of hydrogen absorbed during the hot-pressing process, and to be able to release absorbed hydrogen in a short period of time.

[0015] However, conventional hot-pressed members have not been found to have sufficient performance both in terms of reducing the amount of absorbed hydrogen and in terms of releasing the absorbed hydrogen.

[0016] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a hot-pressed component which absorbs a small amount of hydrogen during the hot pressing process, can release the absorbed hydrogen in a short period of time, and has excellent resistance to delayed fracture. [Means for solving the problem]

[0017] The present invention has an object to solve the above-mentioned problems, and its gist is as follows.

[0018] 1. Steel material and An Al-Fe intermetallic compound layer having a thickness of 10 to 35 μm arranged on at least one surface of the steel material; a diffusion layer disposed at an interface between the Al-Fe-based intermetallic compound layer and the steel material, the Al-Fe-based intermetallic compound layer includes an Al-rich phase having an Al concentration of 40 mass% or more and an Fe-rich phase having an Al concentration of less than 40 mass%, The hot-pressed member has an average length of the Fe-rich phase in a cross section in a direction perpendicular to the plate thickness direction of 10 μm or less.

[0019] 2. The hot-pressed member according to claim 1, wherein the amount of diffusible hydrogen in the steel material is 0.30 ppm by mass or less.

[0020] 3. A base steel plate; A plating layer having a thickness of 10 to 35 μm is provided on at least one surface of the base steel sheet, The plating layer is An interface alloy layer disposed on the base steel sheet; a metal layer disposed on the interface alloy layer, the metal layer having an Al content of 50 mass% or more; the interface alloy layer includes a Si-rich phase having a Si concentration of 4 mass% or more, The steel sheet for hot pressing has a cross-sectional area ratio of the Si-rich phase to the entire interface alloy layer of 5% to 30%.

[0021] 4. The metal layer is Si: 0.5 to 7.0 mass%; and 4. The steel sheet for hot press use according to 3 above, containing 0 to 30 mass % of Fe.

[0022] 5. The metal layer further comprises: 5. The steel sheet for hot press use according to 4 above, containing 0.1 to 4.0 mass % of Mg.

[0023] 6. A method for producing a hot-pressed member, comprising hot-pressing the steel sheet for hot-pressing according to any one of 3 to 5 above to obtain a hot-pressed member. Effect of the Invention

[0024] According to the present invention, the amount of hydrogen absorbed during the hot pressing step is small, and absorbed hydrogen can be released in a short time, thereby making it possible to obtain a hot pressed member having excellent delayed fracture resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Hereinafter, an embodiment of the present invention will be described. Note that the following description shows a preferred embodiment of the present invention, and the present invention is not limited by the following description. Furthermore, the unit of content, "%", represents "mass%" unless otherwise specified.

[0026] (1) Hot-pressed parts A hot-pressed member according to an embodiment of the present invention includes a steel material as a base material, an Al-Fe-based intermetallic compound layer disposed on at least one surface of the steel material, and a diffusion layer formed at the interface between the Al-Fe-based intermetallic compound layer and the steel material. Each part will be described below.

[0027] [Steel] In the present invention, as described later, the above-mentioned problems are solved by providing an Al-Fe intermetallic compound layer and a diffusion layer that satisfy predetermined conditions on the surface of a steel material. Therefore, the steel material is not particularly limited and any steel material can be used.

[0028] The hot-pressed member of the present invention is manufactured by hot pressing a steel plate for hot pressing as described later. Therefore, the steel material can be said to be a steel plate formed by hot pressing. As the steel plate, either a cold-rolled steel plate or a hot-rolled steel plate can be used.

[0029] From the viewpoint of use as an automobile member, etc., it is preferable that the hot-pressed member has high strength. In particular, in order to obtain a hot-pressed member having a tensile strength of more than 980 MPa, preferably 1.8 GPa or more, it is preferable to use a steel material having the following composition.

[0030] C: 0.05 to 0.50%, Si: 0.1 to 1.5%, Mn: 0.5-5.0%, P: 0.1% or less, S: 0.01% or less, Al: 0.10% or less, and N: Contains 0.01% or less, The balance consists of Fe and unavoidable impurities.

[0031] The effects and preferred contents of each element in the above-mentioned preferred composition will be described below.

[0032] C: 0.05 to 0.50% C is an element that has the effect of improving strength by forming a structure such as martensite. From the viewpoint of obtaining a strength exceeding 980 MPa class, the C content is preferably 0.05% or more, and more preferably 0.10% or more. On the other hand, if the C content exceeds 0.50%, the toughness of the spot welded portion deteriorates. Therefore, the C content is preferably 0.50% or less, more preferably 0.45% or less, even more preferably 0.43% or less, and most preferably 0.40% or less.

[0033] Silicon: 0.1 to 1.5% Silicon is an effective element for strengthening steel to obtain good material properties. In order to obtain the above effect, the silicon content is preferably 0.1% or more, and more preferably 0.2% or more. On the other hand, if the silicon content exceeds 1.5%, ferrite is stabilized, and hardenability is reduced. Therefore, the silicon content is preferably 1.5% or less, more preferably 1.3% or less, and even more preferably 1.1% or less.

[0034] Mn: 0.5 to 5.0% Mn is an effective element for obtaining high strength regardless of the cooling rate. From the viewpoint of ensuring excellent mechanical properties and strength, the Mn content is preferably 0.5% or more, more preferably 0.7% or more, and even more preferably 1.0% or more. On the other hand, if the Mn content exceeds 5.0%, not only will the cost increase, but the effect of adding Mn will saturate. Therefore, the Mn content is preferably 5.0% or less, more preferably 4.5% or less, and even more preferably 4.0% or less.

[0035] P:0.1% or less If the P content is excessive, local ductility is deteriorated due to grain boundary embrittlement caused by P segregation to the austenite grain boundaries during casting. As a result, the balance between the strength and ductility of the steel sheet is deteriorated. Therefore, from the viewpoint of improving the balance between the strength and ductility of the steel sheet, it is preferable that the P content is 0.1% or less. On the other hand, from the viewpoint of refining costs, it is preferable that the P content is 0.01% or more.

[0036] S: 0.01% or less S becomes inclusions such as MnS, which causes deterioration of impact resistance and cracks along the metal flow of welds. Therefore, it is desirable to reduce the S content as much as possible, and specifically, it is preferable to set it to 0.01% or less. From the viewpoint of ensuring good stretch flangeability, it is more preferable to set it to 0.005% or less, and even more preferable to set it to 0.001% or less. On the other hand, from the viewpoint of refining costs, it is preferable to set the S content to 0.0002% or more.

[0037] Al: 0.10% or less Al is an element that acts as a deoxidizer. However, if the Al content exceeds 0.1%, the blanking workability and hardenability of the steel sheet material are reduced. Therefore, the Al content is preferably 0.10% or less, more preferably 0.07% or less, and even more preferably 0.04% or less. On the other hand, from the viewpoint of ensuring the effect as a deoxidizer, the Al content is preferably 0.01% or more.

[0038] N: 0.01% or less If the N content exceeds 0.01%, nitrides of AlN are formed during hot rolling or heating before hot pressing, which reduces the blanking workability and hardenability of the steel sheet material. Therefore, the N content is preferably 0.01% or less. On the other hand, from the viewpoint of refining costs, the N content is preferably 0.001% or more.

[0039] The above component composition may further include, optionally, Nb: 0.10% or less, Ti: 0.05% or less, B: 0.0002~0.005%, Cr: 0.1-1.0%, and Sb: 0.003 to 0.03% The composition may contain at least one selected from the group consisting of:

[0040] Nb: 0.10% or less Nb is an effective component for strengthening steel, but if it is contained in excess, the rolling load increases. Therefore, when Nb is added, the Nb content is preferably 0.10% or less, and more preferably 0.05% or less. On the other hand, the lower limit of the Nb content is not particularly limited and may be 0%, but from the viewpoint of refining costs, the Nb content is preferably 0.005% or more.

[0041] Ti: 0.05% or less Ti, like Nb, is an effective component for strengthening steel, but if it is contained in excess, shape fixability decreases. Therefore, when Ti is added, the Ti content is preferably 0.05% or less, and more preferably 0.03% or less. On the other hand, the lower limit of the Ti content is not particularly limited and may be 0%, but from the viewpoint of refining costs, the Ti content is preferably 0.005% or more.

[0042] B: 0.0002~0.005% B has the effect of suppressing the formation and growth of ferrite from the austenite grain boundaries. When B is added, in order to obtain the above effect, the B content is preferably 0.0002% or more, and more preferably 0.0010% or more. On the other hand, excessive addition of B reduces formability. Therefore, when B is added, the B content is preferably 0.005% or less, and more preferably 0.003% or less.

[0043] Cr: 0.1-1.0% Like Mn, Cr is a useful element for strengthening steel and improving hardenability. When Cr is added, the Cr content is preferably 0.1% or more, more preferably 0.2% or more, in order to obtain the above effect. On the other hand, since Cr is an expensive element, the addition of excessive Cr leads to a significant increase in cost. Therefore, when Cr is added, the Cr content is preferably 1.0% or less, more preferably 0.6% or less.

[0044] Sb: 0.003 to 0.03% Sb is an element that has the effect of suppressing decarburization of the surface layer of a steel sheet during the annealing process when manufacturing a base steel sheet. When Sb is added, in order to obtain the above effect, the Sb content is preferably 0.003% or more, and more preferably 0.005% or more. On the other hand, if the Sb content exceeds 0.03%, the rolling load increases, and the productivity decreases. Therefore, when Sb is added, the Sb content is preferably 0.03% or less, more preferably 0.02% or less, and even more preferably 0.01% or less.

[0045] [Al-Fe intermetallic compound layer] The hot-pressed member of the present invention has an Al-Fe intermetallic compound layer on at least one surface of the steel material. By providing a layer made of an Al-Fe intermetallic compound on the surface of the hot-pressed member, it is possible to prevent the generation and intrusion of hydrogen associated with corrosion of the steel material. For example, even if a coating film is provided on the surface of the hot-pressed member, corrosion usually progresses from a location where the rust prevention function of the coating film is reduced, such as a scratched part of the coating film or a painted edge. However, the presence of an Al-Fe intermetallic compound suppresses corrosion even in such a case, and as a result, it is possible to prevent the generation and intrusion of hydrogen.

[0046] The Al-Fe intermetallic compound layer may be provided on at least one surface of the steel material, but is preferably provided on both surfaces.

[0047] The type of intermetallic compound constituting the Al-Fe-based intermetallic compound layer is not particularly limited. 3 , Fe 4 Al 13 , Fe 2 Al 5 The Fe-rich phase may be composed of FeAl, Fe 3 The Al-Fe intermetallic compound is, for example, Fe. 2 Al 5 In other words, the Al-Fe-based intermetallic compound layer in one embodiment of the present invention may contain FeAl 3 , Fe 4 Al 13 , Fe 2 Al 5 , FeAl, Fe 3 Al, and Fe 2 Al 5 The Al-Fe based intermetallic compound layer may be a layer containing at least one selected from the group consisting of FeAl 3 , Fe 4 Al 13 , Fe 2 Al 5 , FeAl, Fe 3 Al, and Fe 2 Al 5 The layer may be made of at least one selected from the group consisting of Si and Si. The types of these intermetallic compounds can be identified by X-ray diffraction.

[0048] Average length: 10μm or less In the hot-pressed member of the present invention, the Al-Fe-based intermetallic compound layer includes an Al-rich phase having an Al concentration of 40% or more and an Fe-rich phase having an Al concentration of less than 40%. In the present invention, it is important that the average length of the Fe-rich phase in the cross section in the direction perpendicular to the sheet thickness direction is 10 μm or less. The reason for this will be explained below.

[0049] In general, when an Al-based plated steel sheet is hot pressed, an Al-Fe-based intermetallic compound layer is formed, and the Al-Fe-based intermetallic compound layer has a layered structure. Typically, the Al-Fe-based intermetallic compound layer has a structure in which an Al-rich phase and an Fe-rich phase are alternately laminated in three or more layers, more generally five or more layers.

[0050] As a result of the study by the present inventors, it was found that when the Al-Fe intermetallic compound layer has the above-mentioned layer structure, hydrogen is trapped at the interface between the layers, and thus hydrogen release is inhibited. That is, in conventional hot-pressed members, the rate at which hydrogen that has entered the steel during the hot-pressing process is released is extremely slow due to the structure of the Al-Fe intermetallic compound layer.

[0051] In contrast, in the hot-pressed member of the present invention, the average length of the Fe-rich phase in the cross section in the direction perpendicular to the plate thickness direction (hereinafter, sometimes simply referred to as "average length") is 10 μm or less. This indicates that the Fe-rich phase is finely divided in the plate surface direction. The hot-pressed member of the present invention has a structure in which the Fe-rich phase is divided in this way, and therefore has excellent hydrogen release properties. Thus, the present invention is based on a completely new technical idea of ​​promoting hydrogen release by dividing the Fe-rich phase.

[0052] From the viewpoint of hydrogen release characteristics, the average length is preferably 8 μm or less, and more preferably 6 μm or less. On the other hand, although there is no particular lower limit to the average length, from the viewpoint of scratch resistance, the average length is preferably 2 μm or more, and more preferably 3 μm or more.

[0053] In addition, the cross-sectional area ratio of the Fe-rich phase in the Al-Fe intermetallic compound layer is not particularly limited, but from the viewpoint of further improving the hydrogen release rate, it is preferably 30% or less, more preferably 20% or less, and even more preferably 10% or less. On the other hand, the lower limit of the cross-sectional area ratio of the Fe-rich phase is not particularly limited, but since Al is softer than Fe, if there is no Fe-rich phase and there is only an Al-rich phase, the scratch resistance is reduced. Therefore, from the viewpoint of scratch resistance, the cross-sectional area ratio of the Fe-rich phase is preferably 3% or more, and more preferably 5% or more.

[0054] From the viewpoint of further improving the hydrogen release rate, it is preferable that the Fe-rich phase is distributed in the Al-rich phase in an island-like manner.

[0055] The structure of the Al-Fe intermetallic compound layer, the dimensions of each phase, and the cross-sectional area ratio can be measured by observing the cross section of the Al-Fe intermetallic compound layer with a scanning electron microscope (SEM) equipped with an energy dispersive X-ray analyzer (EDX) and analyzing the obtained image. More specifically, they can be measured by the method described in the Examples.

[0056] Thickness: 10~35μm The thickness of the Al-Fe intermetallic compound layer depends on the thickness of the plating layer of the hot press steel sheet used and the hot press conditions. If the thickness of the Al-Fe intermetallic compound layer is less than 10 μm, the desired post-painting corrosion resistance cannot be obtained. Therefore, the thickness of the Al-Fe intermetallic compound layer is set to 10 μm or more, preferably 13 μm or more, and more preferably 15 μm or more. On the other hand, if the thickness of the Al-Fe intermetallic compound layer exceeds 35 μm, the time required for dehydrogenation will be long even if the form of the Fe-rich phase satisfies the requirements of the present invention. Therefore, the thickness of the Al-Fe intermetallic compound layer is set to 35 μm or less, preferably 30 μm or less, and more preferably 25 μm or less.

[0057] The thickness of the Al-Fe intermetallic compound layer can be measured by the method described in the Examples. When the Al-Fe intermetallic compound layer is provided on both sides of the steel material, the thickness of the Al-Fe intermetallic compound layer on each side is set to 10 to 35 μm. However, the thickness of the Al-Fe intermetallic compound layer on one side may be the same as or different from the thickness of the Al-Fe intermetallic compound layer on the other side.

[0058] [Diffusion layer] The hot-pressed member of the present invention has a diffusion layer formed at the interface between the Al-Fe intermetallic compound layer and the steel material. The diffusion layer has a larger hydrogen diffusion coefficient than the intermetallic compound layer, and therefore does not inhibit hydrogen release. Therefore, the thickness of the diffusion layer is not limited in the present invention, but is preferably 1 μm or more in order to maintain good adhesion between the Al-Fe intermetallic compound layer and the steel material. For the same reason, the thickness of the diffusion layer is preferably 20 μm or less.

[0059] The amount of diffusible hydrogen in the steel material in the hot-pressed member of the present invention is not particularly limited, but is preferably 0.30 ppm by mass or less. If the amount of diffusible hydrogen is 0.30 ppm by mass or less, the risk of delayed fracture when residual stress occurs due to assembly, welding, etc. of the hot-pressed member can be further reduced. In order to further reduce the risk of delayed fracture, it is more preferable to set the amount of diffusible hydrogen in the steel material to 0.20 ppm by mass or less, and even more preferable to set it to 0.10 ppm by mass or less. The lower the amount of diffusible hydrogen, the better, so the lower limit is not particularly limited, and may be 0 ppm by mass, but may be 0.01 ppm by mass or more in consideration of the quantitative limit of analysis.

[0060] In the present invention, the amount of diffusible hydrogen is defined as the integrated value of the amount of hydrogen when the temperature is raised to 300° C. by thermal desorption analysis after removing the Al-Fe intermetallic compound layer by grinding or the like.

[0061] The strength of the hot press member is not particularly limited, but since hot press members are generally used for applications requiring strength, such as automobile parts, it is desirable that the strength is high. In particular, tensile strength exceeding 1320 MPa is required for frame parts such as center pillars that suppress deformation due to collision. Therefore, the tensile strength of the hot press member is preferably more than 1320 MPa, more preferably more than 1.5 GPa, and even more preferably more than 1.8 GPa. On the other hand, the upper limit of the tensile strength is not particularly limited, but may typically be 2.5 GPa or less, or may be 2.2 GPa or less.

[0062] Furthermore, when used in components such as side members that require energy absorption, excellent yield strength and elongation are required. Therefore, the yield strength of the hot press member is preferably greater than 700 MPa. Furthermore, the total elongation of the hot press member is preferably greater than 7%. On the other hand, the upper limit of the yield strength is not particularly limited, but may typically be 1100 MPa or less, or 900 MPa or less. Furthermore, the upper limit of the total elongation is not particularly limited, but may typically be 20% or less, or 15% or less.

[0063] (2) Steel sheets for hot pressing A steel sheet for hot press use in one embodiment of the present invention comprises a base steel sheet and a plating layer having a thickness of 10 to 35 μm arranged on at least one surface of the steel sheet. The plating layer has an interface alloy layer arranged on the base steel sheet and a metal layer having an Al content of 50% or more arranged on the interface alloy layer. The interface alloy layer includes a Si-rich phase having a Si concentration of 4% or more, and the cross-sectional area ratio of the Si-rich phase to the entire interface alloy layer is 5% or more and 30% or less.

[0064] [Plating layer] If the thickness of the plating layer is less than 10 μm, sufficient corrosion resistance cannot be obtained, and the amount of hydrogen that penetrates due to corrosion increases, decreasing the delayed fracture resistance. Therefore, the thickness of the plating layer is set to 10 μm or more, preferably 12 μm or more, and more preferably 15 μm or more. On the other hand, if the thickness of the plating layer exceeds 35 μm, the amount of oxidation of the plating layer increases, and the amount of diffusible hydrogen cannot be sufficiently reduced. Therefore, the thickness of the plating layer is set to 35 μm or less, preferably 30 μm or less, and more preferably 25 μm or less. In addition, when the plating layer exists on both sides of the base steel sheet, the thickness of the plating layer on each side is set to 10 μm or more and 35 μm or less. The thickness of the plating layer can be directly measured by using an electromagnetic film thickness gauge.

[0065] The thickness of the plating layer on one side of the base steel sheet and the thickness of the plating layer on the other side may be the same or different. In other words, it is sufficient that the thickness of the plating layer on one side of the base steel sheet is 10 μm or more and 35 μm or less, and the thickness of the plating layer on the other side is also 10 μm or more and 35 μm or less.

[0066] The plating layer may be provided directly on the surface of the base steel sheet, or another layer (undercoat) may be provided between the base steel sheet and the plating layer. The undercoat may be, for example, a second plating layer (undercoat plating layer) having a different composition from the plating layer. As the second plating layer, it is preferable to use, for example, an undercoat plating layer mainly composed of Fe or Ni.

[0067] The steel sheet for hot press use of the present invention may further include another layer (upper layer coating) on ​​the plating layer. As the upper layer coating, for example, a third plating layer having a composition different from that of the plating layer or a chemical conversion coating can be used. As the third plating layer, for example, a post-plating layer mainly composed of Ni is preferably used. As the chemical conversion coating, for example, a chemical conversion coating containing a phosphate, a zirconium compound, a titanium compound, etc. is preferably used.

[0068] [Interfacial alloy layer] The above-mentioned steel sheet for hot pressing is typically produced by hot-dip galvanizing a base steel sheet as described below. During this process, Fe, Mn, etc. contained in the base steel sheet react with components such as Al, Si, etc. contained in the plating bath to form an interfacial alloy layer at the interface between the base steel sheet and the metal layer.

[0069] Cross-sectional area ratio of Si-rich phase: 5% to 30% In the steel sheet for hot press use according to the present invention, it is important that the interface alloy layer contains a Si-rich phase having a Si concentration of 4% or more, and that the cross-sectional area ratio of the Si-rich phase to the entire interface alloy layer is 5% or more and 30% or less. The reason for this will be explained below.

[0070] As described above, in the hot-pressed member of the present invention, the Fe-rich phase contained in the Al-Fe-based intermetallic compound layer is finely divided in the sheet surface direction, thereby realizing excellent hydrogen release characteristics.

[0071] Furthermore, as a result of the inventors' investigations, it was found that the structure of the Fe-rich phase in the Al-Fe-based intermetallic compound layer of the hot-pressed component depends on the proportion of the Si-rich phase in the interface alloy layer of the steel plate for hot pressing.

[0072] Although the detailed mechanism is unclear, it is presumed that the Si-rich phase has a relatively high melting point compared to phases with low Si concentration, and does not melt during the hot pressing process. By controlling the ratio of the Si-rich phase in the interface alloy layer within an appropriate range, the cross-sectional area ratio and length of the Fe-rich phase in the Al-Fe intermetallic compound layer of the hot-pressed component can be reduced, resulting in a hot-pressed component with a high hydrogen desorption rate.

[0073] If the cross-sectional area ratio of the Si-rich phase to the entire interface alloy layer is higher than 30%, the Fe-rich phase in the Al-Fe intermetallic compound layer of the hot press member becomes continuous, and the desired hydrogen desorption characteristics cannot be obtained. Therefore, the cross-sectional area ratio of the Si-rich phase is set to 30% or less. On the other hand, the Si-rich phase also has the effect of reducing the diffusion of Fe from the base steel sheet to the plating layer in the hot press process and suppressing excessive thickening of the Al-Fe intermetallic compound layer in the hot press member. As mentioned above, if the Al-Fe intermetallic compound layer is excessively thick, the hydrogen desorption rate decreases. Therefore, the cross-sectional area ratio of the Si-rich phase is set to 5% or more. If the cross-sectional area ratio of the Si-rich phase is 5% or more, it becomes easy to set the thickness of the Al-Fe intermetallic compound layer to a desired range, and as a result, the manufacturing conditions (heating conditions, etc.) for obtaining the hot press member are relaxed, and productivity is improved.

[0074] In this case, the Si-rich phase refers to a phase in which the Si concentration is 4% or more.

[0075] The upper limit of the Si concentration in the Si-rich phase is not particularly limited, but is preferably 30% or less. Furthermore, the components other than Si in the Si-rich phase are not particularly limited, but in one embodiment of the present invention, the Si-rich layer may contain any components derived from the base steel sheet and the plating layer in addition to Si. The Si-rich phase preferably contains Fe, Mn, and Al in addition to Si. A typical composition of the Si-rich phase is, for example, one containing 20 to 40% Fe, 4 to 30% Si, and 0.1 to 5% Mn, with the balance being Al and unavoidable impurities.

[0076] In the present invention, the structure of the Al-Fe intermetallic compound layer in the hot press steel sheet is controlled by controlling the cross-sectional area ratio of the Si-rich phase in the interface alloy layer. Therefore, the distribution and shape of the Si-rich phase in the interface alloy layer are not particularly limited. The Si-rich phase may be, for example, laminar.

[0077] The phases in the interface alloy layer can be determined by image analysis of images obtained by observation with a SEM equipped with an EDX. More specifically, they can be measured by the method described in the Examples.

[0078] [Metal layer] The steel sheet for hot press use of the present invention has a metal layer on the interface alloy layer. The metal layer only needs to have an Al content of 50% or more, and other compositions are not particularly limited.

[0079] In one embodiment of the present invention, the metal layer may contain 0.5 to 7.0% Si and 0 to 30% Fe, the reason for which will be described below.

[0080] Si: 0.5 to 7.0% The Si in the metal layer is alloyed with Al and Fe during the hot pressing process to form an Al-Fe-Si intermetallic compound, particularly the above-mentioned Fe-rich phase. In order to make the Fe-rich phase in the Al-Fe intermetallic compound layer of the hot press member discontinuous, it is essential to limit the amount of Si in the metal layer, so the Si concentration in the metal layer is preferably 7.0% or less. The Si concentration in the metal layer is more preferably 5.0% or less, and even more preferably 3.0% or less. On the other hand, if the Si concentration is less than 0.5%, it becomes difficult to form an Fe-rich phase in the Al-Fe intermetallic compound layer of the hot press member, and as a result, the scratch resistance is reduced. Therefore, the Si concentration in the metal layer is preferably 0.5% or more, and more preferably 1.0% or more.

[0081] Fe: 0-30% When a plating layer is formed by hot-dip plating, Fe is included in the metal layer by forming an alloy layer due to the reaction between the plating bath and the base material, and also when the base material dissolves into the plating bath and is hot-dip plated. The Fe concentration in the metal layer is determined mainly by the thickness of the alloy layer formed by the reaction between the plating bath and the base material, and therefore varies depending on the plating bath temperature, the temperature and surface condition of the sheet when it is immersed in the bath, the time the sheet remains in the bath, etc.

[0082] If the Fe concentration in the metal layer exceeds 30%, an excessive amount of intermetallic compounds containing Fe will precipitate in the metal layer. As a result, the alloying rate will increase, and the intermetallic compound layer in the hot-pressed member will tend to become thicker. Therefore, the Fe concentration in the metal layer is preferably 30% or less, more preferably 18% or less, and even more preferably 12% or less. On the other hand, from the viewpoint of reducing intermetallic compounds in the hot-pressed steel sheet, it is preferable that the Fe concentration in the metal layer is low. Therefore, the lower limit of the Fe concentration in the metal layer is set to 0%.

[0083] In the steel sheet for hot press use in one embodiment of the present invention, the metal layer preferably has a component composition containing 0.5 to 7.0% Si, 0 to 30% Fe, and the balance being Al and unavoidable impurities.

[0084] The inevitable impurities include components derived from the base steel sheet and inevitable impurities in the plating bath. The total content of the inevitable impurities is not particularly limited. However, from the viewpoint of preventing deterioration of the corrosion resistance of the plating layer due to precipitation of an intermetallic compound having a potential difference with the metal layer, the total amount of inevitable impurities contained in the plating layer is preferably 1% or less.

[0085] The metal layer preferably further contains Mg: 0.1 to 4.0%, the reason for which will be explained below.

[0086] Mg: 0.1-4.0% Diffusible hydrogen in hot-pressed components is generated when the metal in the plating layer is oxidized by water vapor contained in the atmosphere during the hot-pressing process. For example, metallic Al and Si exist on the surface of a typical Al-plated steel sheet for hot-pressing, and hydrogen atoms are generated when these react with water vapor. Since the atomic valence of Al is 3, three hydrogen atoms are generated when Al reacts with water vapor. Similarly, since the atomic valence of Si is 4, four hydrogen atoms are generated when Si reacts with water vapor.

[0087] In contrast, the atomic valence of Mg is 2, so the amount of hydrogen generated per atom is less than that of Al and Si. In addition, Mg is more easily oxidized than Al and Si, so when Mg is present, water vapor reacts preferentially with Mg. Therefore, by including Mg in the plating layer, the amount of hydrogen generated can be reduced.

[0088] If the Mg concentration in the metal layer is 0.1% or more, the oxidation of Al is sufficiently suppressed, and the amount of diffusible hydrogen is further reduced. Therefore, from the viewpoint of further reducing the amount of diffusible hydrogen, the Mg concentration in the metal layer is preferably 0.1% or more, more preferably 0.3% or more, and even more preferably 1% or more. On the other hand, if the Mg concentration is 4.0% or less, the oxide formed by the oxidation of Mg is not granular but film-like, and the protection against oxidation of Mg itself is improved. As a result, the amount of diffusible hydrogen is further reduced. Therefore, from the viewpoint of further reducing the amount of diffusible hydrogen, the Mg concentration is preferably 4.0% or less, more preferably 3.0% or less, and even more preferably 2.0% or less.

[0089] In another embodiment of the present invention, the composition of the metal layer may further contain at least one selected from the group consisting of Mn, V, Cr, Mo, Ti, Ni, Co, Sb, Zr, and B in a total amount of 1% or less.

[0090] (3) Manufacturing method of hot-pressed parts Next, a preferred method for producing the hot-pressed member of the present invention will be described.

[0091] In one embodiment of the present invention, the above-mentioned plated steel sheet for hot press is hot pressed to produce a hot press member. By hot pressing the steel sheet for hot press that satisfies the above-mentioned conditions under general conditions, a hot press member that satisfies the above-mentioned conditions can be obtained.

[0092] The method of hot pressing is not particularly limited, and can be performed according to a conventional method. Typically, the hot press steel sheet is heated to a predetermined heating temperature (heating step), and then the hot press steel sheet heated in the heating step is hot pressed (hot pressing step). Preferred hot pressing conditions are described below.

[0093] [heating] If the heating temperature in the heating step is lower than the Ac3 transformation point of the base steel plate, the strength of the final hot press member will be low. Therefore, the heating temperature is preferably equal to or higher than the Ac3 transformation point of the base steel plate. The heating temperature is preferably equal to or higher than 860°C. On the other hand, if the heating temperature exceeds 1000°C, the oxide layer formed by oxidation of the base material or the coating layer becomes excessively thick, which may deteriorate the paint adhesion of the obtained hot press member. Therefore, the heating temperature is preferably equal to or lower than 1000°C, more preferably equal to or lower than 960°C, and even more preferably equal to or lower than 920°C. The Ac3 transformation point of the base steel plate varies depending on the steel composition, but is determined by a Formaster test.

[0094] The temperature at which the heating is started is not particularly limited, but is generally room temperature.

[0095] The time required for the temperature to rise from the start of heating to the heating temperature (temperature rise time) is not particularly limited and can be any time. However, if the temperature rise time exceeds 300 seconds, the time of exposure to high temperatures will be long, and the oxide layer generated by oxidation of the base material and plating layer will become excessively thick. Therefore, from the viewpoint of suppressing the decrease in paint adhesion due to oxides, the temperature rise time is preferably 300 seconds or less, more preferably 270 seconds or less, and even more preferably 240 seconds or less. On the other hand, if the temperature rise time is less than 150 seconds, the coating layer may melt excessively during heating, causing the heating device and the mold to be soiled. Therefore, from the viewpoint of further enhancing the effect of preventing the heating device and the mold from being soiled, the temperature rise time is preferably 150 seconds or more, more preferably 180 seconds or more, and even more preferably 210 seconds or more.

[0096] After reaching the heating temperature, the temperature may be held at the heating temperature. When the temperature is held, the holding time is not particularly limited and can be held for any length of time. However, if the holding time exceeds 300 seconds, the oxide layer formed by oxidation of the base material or coating layer becomes excessively thick, which may deteriorate the paint adhesion of the obtained hot-pressed member. Therefore, the holding time is preferably 300 seconds or less, more preferably 210 seconds or less, and even more preferably 120 seconds or less. On the other hand, the lower limit of the holding time is not limited and may be 0 seconds, but from the viewpoint of homogeneously austenitizing the base steel sheet, it is preferable to set the holding time to 10 seconds or more.

[0097] The atmosphere in the heating step is not particularly limited, and heating can be performed in the air or in an atmosphere into which the air flows. From the viewpoint of further reducing the amount of diffusible hydrogen remaining in the member after hot pressing, it is preferable that the dew point of the atmosphere is 0° C. or lower. The lower limit of the dew point is not particularly limited, and may be, for example, −40° C. or higher.

[0098] The method for heating the steel sheet for hot pressing is not particularly limited, and it can be heated by any method. The heating can be performed, for example, by furnace heating, electric heating, induction heating, high frequency heating, flame heating, etc. As the heating furnace, any heating furnace such as an electric furnace or a gas furnace can be used.

[0099] [Hot press] After the above heating, the steel sheet is hot-pressed to obtain a hot-pressed member. In the hot pressing, cooling is performed using a mold or a coolant such as water at the same time as or immediately after the processing. In the present invention, the hot pressing conditions are not particularly limited. For example, pressing can be performed at a general hot pressing temperature range of 600 to 800°C.

[0100] (4) Manufacturing method of hot-press steel sheets Next, a preferred method for producing the steel sheet for hot press use of the present invention will be described.

[0101] The steel sheet for hot press use of the present invention can be produced by hot-dip galvanizing a base steel sheet. However, in order to make the cross-sectional area ratio of the Si-rich phase in the obtained steel sheet for hot press use 30% or less, it is necessary to carry out both of the following (A) and (B) in the production process. (A) Reduction of the amount of Si in the plating bath (B) Reduction of the amount of Si in the outermost layer of the steel sheet

[0102] Specific examples of the above method (B) include the following methods (B-1) to (B-3). (B-1) Increasing the coiling temperature after hot rolling (B-2) High dew point for recrystallization annealing (B-3) Formation of Fe-based pre-plating layer

[0103] Hereinafter, specific conditions for producing a steel sheet for hot press use using these techniques will be described.

[0104] [Base material steel plate] The base steel sheet is not particularly limited and any steel sheet can be used. The composition of the base steel sheet is not particularly limited, but it is preferably the same as the suitable composition of the steel material described above.

[0105] The base steel sheet may be either a hot-rolled steel sheet or a cold-rolled steel sheet.

[0106] When a hot-rolled steel sheet is used as the base steel sheet, the hot-rolled steel sheet can be manufactured according to a conventional method. Typically, a steel slab as a material is heated and then hot-rolled. In the hot rolling, rough rolling and finish rolling can be performed in sequence. After the hot rolling, pickling is preferably performed.

[0107] (B-1) Increasing the coiling temperature after hot rolling The obtained hot-rolled steel sheet is wound into a coil. At that time, by increasing the winding temperature, an internal oxide can be formed inside the surface layer of the steel sheet. By forming the internal oxide, the diffusion rate of Si to the outermost layer of the steel sheet during the hot-dip plating process can be reduced, and as a result, the cross-sectional area ratio of the Si-rich phase in the steel sheet for hot pressing can be reduced. Therefore, in order to make the cross-sectional area ratio of the Si-rich phase 30% or less, the winding temperature is set to 600°C or more, preferably 620°C or more, more preferably 630°C or more, and even more preferably 650°C or more. On the other hand, if the winding temperature is too high, the internal oxide layer of the steel sheet becomes too thick, and the weldability is reduced. Therefore, from the viewpoint of weldability, it is preferable to set the winding temperature to 800°C or less.

[0108] When a cold-rolled steel sheet is used as the base steel sheet, the hot-rolled steel sheet may be pickled and then cold-rolled in a conventional manner. The reduction in the cold rolling is not particularly limited, but from the viewpoint of the mechanical properties of the steel sheet, the reduction is preferably 30% or more. From the viewpoint of rolling costs, the reduction is preferably 90% or less.

[0109] The steel sheet may be subjected to recrystallization annealing prior to hot-dip plating. The conditions of the recrystallization annealing are not particularly limited, and the recrystallization annealing can be performed according to a conventional method. For example, after the steel sheet is subjected to a cleaning treatment such as degreasing, an annealing furnace can be used to perform a heat treatment in which the steel sheet is heated to a predetermined temperature in a heating zone in the first stage, and a predetermined heat treatment can be performed in a soaking zone in the second stage. The atmosphere in the annealing furnace is not particularly limited, but it is preferable to use a reducing atmosphere in order to activate the surface layer of the steel sheet.

[0110] (B-2) High dew point for recrystallization annealing When the recrystallization annealing is performed, by increasing the dew point of the atmosphere during the recrystallization annealing, an internal oxide is formed inside the surface layer of the steel sheet, and the diffusion rate of Si to the outermost surface layer of the steel sheet during the hot-dip plating process can be reduced. In order to obtain the above effect, the dew point needs to be 0°C or higher. Although there are no particular limitations on the upper limit of the dew point, in order to stably control the dew point at 20°C or higher, a large-scale humidification facility is required, which increases the facility cost. Therefore, the dew point is preferably 20°C or lower.

[0111] (B-3) Formation of Fe-based pre-plating layer It is preferable to form an Fe-based pre-plating layer on the base steel sheet prior to hot-dip plating. By forming an Fe-based pre-plating layer on the surface of the base steel sheet, the amount of Si in the outermost layer of the steel sheet can be reduced, and as a result, the cross-sectional area ratio of the Si-rich phase in the hot press steel sheet can be reduced. The composition of the Fe-based pre-plating layer is not particularly limited, but from this viewpoint, it is preferable that the Si concentration in the Fe-based pre-plating layer is less than 0.1%, and it is more preferable that the Fe-based pre-plating layer does not substantially contain Si. It is preferable that the total concentration of components other than Fe contained in the Fe-based pre-plating layer is less than 10%. In other words, it is preferable that the Fe-based pre-plating layer is a plating layer containing 90% or more Fe. The Fe-based pre-plating layer may be, for example, an Fe plating layer, an Fe-P alloy plating layer, an Fe-B alloy plating layer, or an Fe-O alloy plating layer.

[0112] The method for forming the Fe-based pre-plating layer is not particularly limited, but it is preferable to form the layer by an electroplating method, which is excellent in film formation speed and economy. From the viewpoint of stabilizing plating quality, the deposition amount of the Fe-based pre-plating layer is 100 mg / m 2 On the other hand, if the coating weight is excessively large, the effect of reducing the Si content in the outermost layer of the steel sheet is saturated, and the manufacturing cost increases. Therefore, the coating weight of the Fe-based pre-plating layer is set to 10 g / m or more. 2 It is preferable that:

[0113] [Hot-dip plating] In the present invention, a steel sheet is immersed in a hot-dip galvanizing bath to form a coating layer. The coating bath must have the following component composition. The reasons for this will be explained below. Si: 0.5 to 7.0%, and Fe: 0-10.0% The balance is aluminum and unavoidable impurities.

[0114] Si: 0.5 to 7.0% Si is an element that reacts with Al in the bath and Fe, Mn, etc. in the base material to form an interface alloy layer in the hot press steel sheet. If the Si content in the plating bath is less than 0.5%, the growth of the interface alloy layer in the plating bath is extremely fast, resulting in a film with poor cold workability, and it is difficult to stably obtain a plating layer with a thickness of 10 to 30 μm. Therefore, the Si content is set to 0.5% or more. On the other hand, if the Si content is higher than 7.0%, the cross-sectional area ratio of the Si-rich phase in the hot press steel sheet becomes higher than 30%. Therefore, the Si content is set to 7.0% or less.

[0115] In order to obtain a steel sheet for hot pressing in which the cross-sectional area ratio of the Si-rich phase is 30% or less, as described above, in addition to setting the Si content in the plating bath to 7.0% or less, it is necessary to carry out at least one of the above-mentioned (B-1), (B-2), and (B-3).

[0116] Fe: 0 to 10.0% Fe is a component that is present in the bath by dissolving from the steel sheet or equipment in the bath. If the Fe content in the coating bath exceeds 10.0%, the amount of dross in the bath becomes excessive, and adheres to the coated steel sheet, causing deterioration of the appearance quality. Therefore, the Fe concentration in the coating bath is set to 10.0% or less, preferably 5.0% or less, and more preferably 3.0% or less. From the viewpoint of appearance quality, the lower the Fe concentration in the coating bath, the better. Therefore, the lower limit of the Fe content in the coating bath is set to 0%. Note that even if the Fe content in the coating bath is 0%, an intermetallic compound layer is formed by the reaction between the base steel and the components of the coating bath during hot dip coating.

[0117] The composition of the plating bath may further contain Mg.

[0118] Mg: 0.1-4.0% For the purpose of further reducing the amount of hydrogen that penetrates during the hot pressing process, as described above, Mg may be added to the metal layer of the steel sheet for hot pressing, and for this purpose, an appropriate amount of Mg may be added to the coating bath as well. Since the Mg concentration in the metal layer is approximately the same as the Mg concentration in the coating bath, the preferred range of Mg content in the coating bath and the reasons therefor are the same as those described for the Mg concentration in the metal layer.

[0119] The inevitable impurities include components derived from the base steel sheet and inevitable impurities contained in metal materials (ingots, etc.) for supplying hot-dip galvanizing bath components. The total content of the inevitable impurities is not particularly limited, but is preferably 1% or less in total.

[0120] In another embodiment of the present invention, the composition of the hot-dip galvanizing bath may further contain at least one selected from the group consisting of Mn, V, Cr, Mo, Ti, Ni, Co, Sb, Zr, and B in a total amount of 1% or less.

[0121] The temperature of the plating bath is preferably in the range of the solidification start temperature +20°C to 700°C. If the temperature of the plating bath is (solidification start temperature +20°C) or higher, local solidification of components caused by a local temperature drop in the plating bath can be prevented. Furthermore, if the temperature of the plating bath is 700°C or lower, rapid cooling after plating can be easily performed, and the intermetallic compound layer formed between the steel sheet and the metal layer can be prevented from becoming excessively thick.

[0122] The temperature of the base steel sheet immersed in the coating bath (immersion sheet temperature) is not particularly limited, but is preferably controlled to within ±20°C of the coating bath temperature in order to ensure the coating characteristics in continuous hot-dip coating operations and to prevent changes in the bath temperature.

[0123] The immersion time of the steel sheet in the hot-dip galvanizing bath is not particularly limited, but is preferably 1 second or more from the viewpoint of stably securing the thickness of the galvanizing layer. On the other hand, the upper limit of the immersion time is also not particularly limited, but is preferably 5 seconds or less from the viewpoint of preventing the intermetallic compound layer formed between the steel sheet and the metal layer from becoming excessively thick.

[0124] The conditions for immersing the base steel sheet in the plating bath are not particularly limited. For example, when plating a relatively thin steel sheet having a thickness of 0.6 mm or more and less than 1.6 mm, the line speed is preferably about 150 to 230 mpm. When plating a relatively thick steel sheet having a thickness of 1.6 mm or more and 3.0 mm or less, the line speed is preferably about 40 mpm. The immersion length is preferably about 5 to 7 m.

[0125] In the present invention, the method of cooling the base steel sheet after immersion in the coating bath is not particularly limited, and any method can be used. The cooling is preferably performed in a nitrogen gas atmosphere. The reason why the cooling is preferably performed in a nitrogen gas atmosphere is that it is economical because it is not necessary to extremely increase the cooling rate and does not require large-scale cooling equipment. The nitrogen gas atmosphere may contain 4 volume % or less of hydrogen gas.

[0126] Although not particularly limited, the steel sheet for hot press use is preferably manufactured in a continuous hot-dip galvanizing facility. As the continuous galvanizing facility, either a continuous galvanizing facility with a non-oxidizing furnace or a continuous galvanizing facility without a non-oxidizing furnace can be used. The steel sheet for hot press use of the present invention does not require such special facilities and can be manufactured using a general hot-dip galvanizing facility, and is therefore excellent in terms of productivity. EXAMPLES

[0127] The functions and effects of the present invention will be described below using examples, although the present invention is not limited to the following examples.

[0128] First, a base steel sheet was prepared in the following manner.

[0129] A steel having a composition containing, by mass%, C: 0.34%, Si: 0.25%, Mn: 1.20%, P: 0.005%, S: 0.001%, Al: 0.03%, N: 0.004%, Ti: 0.02%, B: 0.002%, Cr: 0.18%, and Sb: 0.008%, with the balance being Fe and unavoidable impurities, was melted in a converter and cooled in air to obtain a steel slab. 3 The transformation point is 783℃, Ar 3 The transformation point was 706°C.

[0130] The steel slab was heated to 1200°C and then hot rolled to obtain a hot rolled steel sheet having a thickness of 3.0 mm. The finishing temperature in the hot rolling was 930°C. The obtained hot rolled steel sheet was wound into a coil at the winding temperature shown in Table 1, and then cooled in the air.

[0131] The hot-rolled steel sheet was pickled and then cold-rolled to obtain a cold-rolled steel sheet having a thickness of 1.4 mm.

[0132] An Fe plating layer was formed as a pre-plating layer on the surface of the obtained cold-rolled steel sheet. The Fe plating layer was formed by electroplating under the following conditions. For comparison, the Fe plating layer was not formed in some examples (Table 1). Plating solution composition Ferrous sulfate: 300g / L Sodium sulfate: 50g / L pH: 1.8~2.2 Liquid temperature: 55℃ ·Current density: 100A / dm 2 -Fe plating layer adhesion: 500mg / m 2

[0133] The above-mentioned base steel sheet was immersed in a plating bath having the composition shown in Table 1 to perform hot-dip plating. The temperature of the plating bath used was 660°C. After the steel sheet was pulled out of the plating bath, it was cooled at an average cooling rate of 15°C / sec to solidify the plating layer, thereby obtaining a steel sheet for hot pressing. The cooling was performed using N 2 This was done by gas wiping.

[0134] For the obtained steel sheets for hot press use, the thickness of the plating layer, the component composition of the metal layer, and the cross-sectional area ratio of the Si-rich layer were measured by the following methods. The measurement results are shown in Table 2.

[0135] (Thickness of plating layer) Each of the hot press steel sheets was embedded in a conductive resin, and the cross section was observed by SEM to obtain a backscattered electron image. The observation was performed at a magnification of 500 times in five randomly selected fields of view. The obtained backscattered electron images were subjected to image analysis based on the contrast, and the area of ​​the plating layer in the field of view was calculated and divided by the width of the field of view to obtain the average thickness of the plating layer in that field of view. The arithmetic mean of the average thicknesses of the five fields of view was determined to be the thickness of the plating layer in that hot press steel sheet.

[0136] (Cross-sectional area ratio of Si-rich phase) The element distribution and concentration of the interface alloy layer of each of the hot press steel sheets were quantified by an electron probe microanalyzer (EPMA). The observation was performed at a magnification of 1000 times in five randomly selected fields of view. First, a contrast threshold value of the backscattered electron image was set, the interface alloy layer between the metal layer and the base material was extracted, and the cross-sectional area (S1) of the interface alloy layer was obtained. Note that the hot press steel sheets of all the examples had an interface alloy layer and a metal layer on the interface alloy layer.

[0137] Next, the region where the Si concentration was 4 mass% or more as quantified by EPMA was determined as the Si-rich phase, and the cross-sectional area (S2) of the Si-rich phase was calculated. The cross-sectional area ratio of the Si-rich phase to the entire interface alloy layer was calculated by dividing the obtained S2 by S1 for each of the five fields of view, and the average value was determined as the cross-sectional area ratio of the Si-rich layer in the steel sheet for hot press use.

[0138] (Composition of metal layer) The element distribution and concentration of the metal layer of each of the hot press steel sheets were measured by EPMA in the same manner as the interface alloy layer. The measurement was performed at 1000x magnification in five randomly selected fields. First, the metal layer was extracted by setting a contrast threshold of the backscattered electron image, and the average composition of the metal layer was measured by performing surface analysis of the metal layer by EPMA. The measured values ​​in the five fields were averaged to obtain a representative value.

[0139] Next, the obtained steel plate for hot pressing was hot pressed in the following manner to produce a hot pressed member. First, a test piece of 100 mm x 200 mm was taken from the steel plate for hot pressing and was subjected to a heat treatment in an electric furnace. The heating temperature in the heat treatment was 910°C, the temperature rise time was 210 seconds, and the holding time was 180 seconds. The heating was performed in an atmosphere with a dew point of 10°C.

[0140] After the specified holding time had elapsed, the test piece was removed from the electric furnace and immediately hot pressed using a hat-shaped die at a forming start temperature of 720°C to obtain a hot-pressed part. The shape of the obtained hot-pressed part had a flat part length of 100 mm on the top surface, a flat part length of 30 mm on the side surface, and a flat part length of 20 mm on the bottom surface. The bending radius of the die was 7R on both shoulders of the top surface and both shoulders of the bottom surface.

[0141] The thickness of the Al-Fe intermetallic compound layer, composition analysis, and the morphology of the Fe-rich phase were measured for the hot-pressed members obtained by the following methods. The measurement results are shown in Table 3.

[0142] (Thickness of Al-Fe intermetallic compound layer) The flat top portion of the obtained hot-pressed member was embedded in a conductive resin, and the cross section was observed by SEM to obtain a backscattered electron image. The observation was performed at a magnification of 500 times in five randomly selected fields of view. The obtained backscattered electron image was subjected to image analysis based on the contrast, and the area of ​​the Al-Fe intermetallic compound layer in the field of view was calculated and divided by the width of the field of view to obtain the average thickness of the Al-Fe intermetallic compound layer in that field of view. The arithmetic mean of the average thicknesses of the five fields of view was used as the representative value of the thickness of the Al-Fe intermetallic compound layer in that hot-pressed member.

[0143] (Analysis of the morphology of Al-Fe intermetallic compound layer) The flat top portion of the obtained hot press member was embedded in a conductive resin, and the element distribution and concentration were quantified by EPMA in a field including the entire thickness of the Al-Fe alloy layer. The observation was performed at a magnification of 1000 times in five randomly selected fields. The region where the Al concentration was less than 40 mass% in the quantitative value by EPMA was defined as the Fe-rich phase, and the remaining part, i.e., the region where the Al concentration was 40 mass% or more, was defined as the Al-rich phase. The cross-sectional area ratio of the Fe-rich phase was calculated by dividing the area of ​​the Fe-rich phase in each field by the area of ​​the Al-Fe intermetallic compound layer, and the average value of the cross-sectional area ratios in the five fields was defined as the cross-sectional area ratio of the Fe-rich phase in the hot press steel sheet. In addition, the length of the cross-sectional direction in the sheet plane direction of the independent Fe-rich phase present in each field was measured, and the measured values ​​for all five fields were averaged to determine the average length in the direction perpendicular to the sheet thickness direction in the cross section of the Fe-rich phase.

[0144] In order to evaluate the resistance of the obtained hot-pressed parts to hydrogen embrittlement caused by hydrogen that entered during the hot-pressing process, the amount of diffusible hydrogen in the steel immediately after pressing was measured, and the hydrogen desorption rate was measured by measuring the change in the amount of hydrogen over time during storage at room temperature.

[0145] (Diffusible hydrogen content in steel) The amount of diffusible hydrogen in the hot-pressed parts immediately after pressing was measured by the following method. A small piece of 10 x 15 mm was cut from the flat part of the hot-pressed part with a small degree of processing, and the intermetallic compound layer and the diffusion layer on both sides were removed by grinding with a precision router. Then, a thermal desorption analysis was performed, and the integrated value of the amount of hydrogen when the temperature was raised to 300 degrees was taken as the amount of diffusible hydrogen. For the thermal desorption analysis, a thermal desorption analyzer manufactured by J Science Corporation was used, the carrier gas was argon, and the heating rate was 200°C / s. The amount of diffusible hydrogen in the steel obtained was evaluated according to the following criteria. The evaluation results are shown in Table 3. 1: Less than 0.30 ppm by mass 2: 0.30 mass ppm or more and less than 0.50 mass ppm 3: 0.50 mass ppm or more and less than 1.00 mass ppm 4:1.00 mass ppm or more

[0146] (Hydrogen desorption time) After hot pressing, small pieces were cut out from the hot pressed members stored in a constant temperature room at 25°C for 24 hours or one week, and the amount of diffusible hydrogen in the steel was measured in the same manner as in the measurement of the amount of diffusible hydrogen immediately after pressing. For the time change in the amount of diffusible hydrogen, an exponential approximation formula was created using the least squares method from three data points: immediately after hot pressing, 24 hours, and one week. From the approximation formula, the time required for the amount of diffusible hydrogen in the steel to decrease to 0.20 ppm by mass was estimated, and this was taken as the hydrogen desorption time. Note that hydrogen desorption was not evaluated for hot pressed members whose amount of diffusible hydrogen immediately after heat treatment was less than 0.20 ppm by mass. Based on the obtained hydrogen desorption time, the hydrogen desorption characteristics were evaluated according to the following criteria. The evaluation results are shown in Table 3. 1: Less than 24 hours 2: 24 hours or more but less than 120 hours 3: 120 hours or more but less than 240 hours 4: More than 240 hours -: Evaluation was not performed because the amount of diffusible hydrogen immediately after heat treatment was less than 0.20 mass ppm.

[0147] Based on the evaluation results of the amount of diffusible hydrogen in the steel and the hydrogen desorption time, a comprehensive evaluation was made according to the following criteria. 1: The amount of diffusible hydrogen in steel is 1 2: The amount of diffusible hydrogen in steel is 2 or 3, and the hydrogen desorption time is 1 or 2 3: The amount of diffusible hydrogen in steel is 2 or 3, and the hydrogen desorption time is 3 4: At least one of the amount of diffusible hydrogen in steel and the hydrogen desorption time is 4

[0148] As can be seen from the results shown in Table 3, hot-pressed members that satisfied the conditions of the present invention received an overall rating of 2 or 1. In other words, the hot-pressed members of the present invention have a low amount of diffusible hydrogen immediately after hot pressing of 0.30 mass ppm or less, so that the risk of hydrogen embrittlement is low, or even if the amount of hydrogen immediately after hot pressing is high at more than 0.30 mass ppm, it can be reduced to 0.20 mass ppm or less by storing at room temperature for 120 hours or less, so that the risk of embrittlement due to hydrogen that penetrates during manufacturing can be easily reduced. On the other hand, hot-pressed members that did not satisfy the conditions of the present invention had a high amount of hydrogen immediately after hot pressing, and it was difficult to reduce the amount of hydrogen in a short period of time.

[0149] [Table 1]

[0150] [Table 2]

[0151] [Table 3]

Claims

1. Steel and An Al-Fe intermetallic compound layer having a thickness of 10 to 35 μm arranged on at least one surface of the steel material; a diffusion layer disposed at an interface between the Al-Fe intermetallic compound layer and the steel material, the Al-Fe-based intermetallic compound layer includes an Al-rich phase having an Al concentration of 40 mass% or more and an Fe-rich phase having an Al concentration of less than 40 mass%, The Al-rich phase includes at least one of FeAl 3 , Fe 4 Al 13 , and Fe 2 Al 5 ; The hot-pressed member, wherein the average length of the Fe-rich phase in a cross section in a direction perpendicular to the plate thickness direction is 10 μm or less.

2. The hot-pressed member according to claim 1 , wherein the amount of diffusible hydrogen in the steel material is 0.30 ppm by mass or less.

3. A base steel plate; A plating layer having a thickness of 10 to 35 μm is provided on at least one surface of the base steel sheet, The plating layer is An interface alloy layer disposed on the base steel sheet; a metal layer disposed on the interface alloy layer, the metal layer having an Al content of 50 mass% or more; the interface alloy layer includes a Si-rich phase having a Si concentration of 4 mass% or more, The steel sheet for hot press use has a cross-sectional area ratio of the Si-rich phase to the entire interface alloy layer of 5% or more and 30% or less.

4. The metal layer is Si: 0.5 to 7.0 mass%; and The steel sheet for hot press use according to claim 3, containing Fe: 0 to 30 mass%.

5. The metal layer further comprises: The steel sheet for hot press use according to claim 4, containing Mg: 0.1 to 4.0 mass%.

6. A method for manufacturing a hot press member, comprising hot pressing the steel plate for hot press according to any one of claims 3 to 5 to obtain a hot press member.

Citation Information

Patent Citations

  • Aluminum-base plated steel sheet for hot press superior in corrosion resistance and heat resistance, and member for automobile using it

    JP2003034845A

  • Aluminum-iron alloy plated steel sheet for hot forming with excellent corrosion resistance and heat resistance, hot press formed member, and manufacturing method thereof

    JP2022513132A

  • Iron-aluminum plated steel sheet for hot pressing with excellent hydrogen delayed fracture properties and spot weldability, and its manufacturing method

    JP2022513133A

  • Hot stamping component and method of manufacturing the same

    US20210187583A1

  • Hot stamp-molded high-strength component having excellent corrosion resistance after coating, and method for manufacturing same

    WO2012137687A1