Photosensitive resin composition, cured film obtained by curing the same, and display device having the cured film

The photosensitive resin composition forms a protective film with enhanced transparency, chemical resistance, and low gas emission properties, addressing the challenges faced by existing films in LCDs, particularly in advanced display systems.

JP7568413B2Active Publication Date: 2024-10-16NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2020056205
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-12
Filing Date
2020-03-26
Publication Date
2024-10-16
Estimated Expiration
2040-03-26

AI Technical Summary

Technical Problem

Existing protective films for color filters in LCDs face challenges in maintaining transparency, chemical resistance, adhesion, hardness, and low gas emission properties, particularly in advanced display systems like IPS mode, where gas and moisture impurities affect display quality.

Method used

A photosensitive resin composition containing a specific alkali-soluble resin with polymerizable unsaturated groups, photopolymerizable monomers, and a photopolymerization initiator, which forms a cured film with reduced gas emission properties, suitable for photolithography processes.

Benefits of technology

The composition provides a protective film with excellent transparency, chemical resistance, adhesion, and hardness, effectively reducing gas emissions, thereby improving display reliability and preventing display defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568413000001
    Figure 0007568413000001
  • Figure 0007568413000002
    Figure 0007568413000002
  • Figure 0007568413000003
    Figure 0007568413000003
Patent Text Reader

Abstract

To provide: a photosensitive resin composition applicable, e.g., to colored films including a light shielding film and a protection film generating little gas; a cured film formed by curing the composition; and a display device with the cured film.SOLUTION: A photosensitive resin composition contains the (A) to (D) components as essential components: (A) a polymerizable unsaturated group-containing alkali-soluble resin of general formula (1), (B) a photopolymerizable monomer with at least three ethylenically unsaturated bonds, (C) a photoinitiator, and (D) a solvent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive resin composition containing an alkali-soluble resin containing a polymerizable unsaturated group having a specific structure, a cured film obtained by curing the photosensitive resin composition, and a touch panel and a color filter containing the cured film as a constituent component. [Background technology]

[0002] Conventionally, a transparent cured film (hereinafter also referred to as a "protective film") is formed as a protective layer on the surface of a color filter used in the manufacture of a color liquid crystal display (LCD). The protective film of a color filter is formed for the purposes of flattening unevenness occurring between pixels of the color filter, improving the durability of the color filter against heat treatment and chemical treatment in a post-process, and improving the reliability of the color liquid crystal display. The protective film of a color filter is required to be excellent in transparency, chemical resistance, adhesion, hardness, flatness, heat resistance, electrical reliability, etc.

[0003] On the other hand, the method of forming the protective film includes a method of forming the protective film on the front surface by thermal curing and a method of forming the protective film by photolithography. The method of forming the protective film can be selected depending on the characteristics that the protective film should have and the necessity of patterning during the design of the panel and processing process of the color filter. Here, the characteristics of the protective film that are important when forming it by photolithography are transparency, chemical resistance, adhesion, hardness, and electrical reliability, on the premise that it can have development characteristics that can form the desired protective film pattern.

[0004] For example, in terms of transparency, the protective film is required to have no absorption in the visible light wavelength range so as not to impair the color characteristics of the color filter. In terms of chemical resistance, the protective film is required to be stable against acids, alkalis, solvents, etc. used in later processes. In terms of adhesion, when a substrate is laminated on the protective film when a liquid crystal display panel is produced, the protective film is required not to peel off even if the base of the protective film at that site is a glass substrate, an ITO substrate, a MAM substrate, etc. In terms of hardness, the protective film is required to have high hardness from the viewpoint of durability. In terms of electrical reliability, it is required that the protective film maintains its insulating properties and that impurities contained in the protective film do not contaminate the liquid crystal.

[0005] The requirements for the above protective film properties are becoming stricter as LCD panels become more functional, and wider viewing angles and faster response times are required. In display methods such as IPS (In-plane Switching) mode, gaseous or liquid components or water generated or bleed-out from the color filter layer can enter the liquid crystal layer through the protective layer, causing an increase in the concentration of moisture or ionic impurities in the liquid crystal layer or forming bubbles in the liquid crystal layer, which can cause display defects. For this reason, it is particularly important to prevent the passage of the above-mentioned impurities, as well as to have low gas generation properties, since gas generation from the protective film in direct contact with the liquid crystal layer directly leads to display defects.

[0006] Furthermore, there are also issues in the LCD panel manufacturing process, such as photo-alignment treatment of the liquid crystal alignment film after the protective film is formed, and issues such as reducing the effects of external light, including various display devices such as organic electroluminescence (EL).For this reason, there are cases where the protective film is required to have the ability to absorb short-wavelength ultraviolet light that does not contribute to color display, while still ensuring its transparency (high transmittance) as a protective film. Summary of the Invention [Problem to be solved by the invention]

[0007] It is desired that the photosensitive resin composition can form an appropriate protective film pattern by photolithography, and that the protective film pattern can be sufficiently reduced in gas generation that affects electrical reliability while adequately maintaining properties such as transparency, chemical resistance, adhesion, hardness, etc. Also, in color resists that form RGB pixels, black resists that form light-shielding films, and the like, there are cases where a cured film that has excellent low gas generation properties in addition to the necessary properties is desired.

[0008] The present invention has been made in consideration of the above points, and an object of the present invention is to provide a photosensitive resin composition that can be applied to protective films that generate little gas, colored films including light-shielding films, etc., a cured film obtained by curing the same, and a display device having the cured film. [Means for solving the problem]

[0009] Means for Solving the Problems The inventors of the present invention have conducted studies to solve the problems associated with the above-mentioned photosensitive resin composition for a light-shielding film, and as a result have found that a specific colorant is suitable as a light-shielding component for the desired photosensitive resin composition for a light-shielding film, thereby completing the present invention.

[0010] The photosensitive resin composition of the present invention contains the following components (A) to (D) as essential components: (A) an alkali-soluble resin containing a polymerizable unsaturated group represented by general formula (1), (B) a photopolymerizable monomer having at least three ethylenically unsaturated bonds, (C) a photopolymerization initiator, and (D) a solvent.

[0011] [ka]

[0012] (In formula (1), Ar are each independently an aromatic hydrocarbon group having 6 to 14 carbon atoms, and a portion of the bonded hydrogen atoms may be substituted with an alkyl group having 1 to 10 carbon atoms, an aryl group or arylalkyl group having 6 to 10 carbon atoms, a cycloalkyl group or cycloalkylalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or a halogen group. Each R1 is independently an alkylene group having 2 to 4 carbon atoms, and each 1 is independently a number from 0 to 3. Each G is independently a substituent represented by general formula (2) or general formula (3), and Y is a tetravalent carboxylic acid residue. Each Z is independently a hydrogen atom or a substituent represented by general formula (4), and at least one Z is a substituent represented by general formula (4). n is a number having an average value of 1 to 20.)

[0013] [ka]

[0014] [ka]

[0015] (In formulas (2) and (3), R2 is a hydrogen atom or a methyl group, R3 is a divalent alkylene group or alkylarylene group having 2 to 10 carbon atoms, R4 is a divalent saturated or unsaturated hydrocarbon group having 2 to 20 carbon atoms, and p is a number from 0 to 10.)

[0016] [ka]

[0017] (In formula (4), W is a divalent or trivalent carboxylic acid residue, and m is 1 or 2.)

[0018] The cured film of the present invention is obtained by curing the above-mentioned photosensitive resin composition.

[0019] The display device of the present invention has the above-mentioned cured film. Effect of the Invention

[0020] According to the present invention, it is possible to provide a photosensitive resin composition that can be applied to protective films that generate little gas, colored films including light-shielding films, etc., a cured film obtained by curing the same, and a display device having the cured film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited to the following embodiment. In addition, in the present invention, when the first decimal place of the content of each component is 0, the notation after the decimal point may be omitted.

[0022] The polymerizable unsaturated group-containing alkali-soluble resin of component (A) represented by general formula (1) of the present invention can be obtained by reacting a reaction product of an epoxy compound (a-1) having two glycidyl ether groups and a (meth)acrylic acid derivative with a dicarboxylic acid or tricarboxylic acid or its monoanhydride (b), and a tetracarboxylic acid or its dianhydride (c). Note that "(meth)acrylic acid" is a general term for acrylic acid and methacrylic acid, and means either or both of them.

[0023] The above-mentioned polymerizable unsaturated group-containing alkali-soluble resin is characterized in that it uses, as a raw material epoxy compound, a compound in which Ar in general formula (1) is an aromatic hydrocarbon group having 6 to 14 carbon atoms, which may contain several oxyalkylene groups in one molecule.

[0024] Preferred examples of the aromatic hydrocarbon group having 6 to 14 carbon atoms include a divalent naphthyl group and a phenylene group in which a part of hydrogen atoms may be substituted with an alkyl group or the like. Here, in the (A) polymerizable unsaturated group-containing alkali-soluble resin of the present invention, it is preferable that both of the two Ars bonded to the fluorene group in the general formula (1) are naphthyl groups (having a bisnaphtholfluorene skeleton) or both are phenylene groups (having a bisphenolfluorene skeleton), and it is more preferable that both of the Ars bonded to the fluorene group are naphthyl groups. This is because the cured film (coating film) obtained by curing the (A) polymerizable unsaturated group-containing alkali-soluble resin in which both of the two Ars bonded to the fluorene group are naphthyl groups generates a small amount of gas when heated.

[0025] [ka]

[0026] (In formula (1), Ar are each independently an aromatic hydrocarbon group having 6 to 14 carbon atoms, and a portion of the bonded hydrogen atoms may be substituted with an alkyl group having 1 to 10 carbon atoms, an aryl group or arylalkyl group having 6 to 10 carbon atoms, a cycloalkyl group or cycloalkylalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or a halogen group. Each R1 is independently an alkylene group having 2 to 4 carbon atoms, each 1 is independently a number from 0 to 3, the average value of 1 in one molecule is also a number from 0 to 3, and the average value of 1 in the composition is also a number from 0 to 3. Each G is independently a substituent represented by general formula (2) or general formula (3), and Y is a tetravalent carboxylic acid residue. Each Z is independently a hydrogen atom or a substituent represented by general formula (4), and at least one Z is a substituent represented by general formula (4). n is a number having an average value of 1 to 20.)

[0027] [ka]

[0028] [ka]

[0029] (In formulas (2) and (3), R2 is a hydrogen atom or a methyl group, R3 is a divalent alkylene group or alkylarylene group having 2 to 10 carbon atoms, R4 is a divalent saturated or unsaturated hydrocarbon group having 2 to 20 carbon atoms, and p is 0 to 10.)

[0030] [ka]

[0031] (In formula (4), W is a divalent or trivalent carboxylic acid residue, and m is 1 or 2.)

[0032] A method for producing the alkali-soluble resin having a polymerizable unsaturated group represented by the general formula (1) will be described in detail below.

[0033] First, an epoxy compound (a-1) (hereinafter simply referred to as "epoxy compound (a-1)") having a bisnaphtholfluorene skeleton or a bisphenolfluorene skeleton, which may have several oxyalkylene groups in one molecule and which is represented by general formula (5), is reacted with either one or both of a (meth)acrylic acid derivative represented by general formula (6) or general formula (7) to obtain an epoxy (meth)acrylate.

[0034] [ka]

[0035] (In formula (5), each Ar is independently an aromatic hydrocarbon group having 6 to 14 carbon atoms, and a portion of the bonded hydrogen atoms may be substituted with an alkyl group having 1 to 10 carbon atoms, an aryl group or arylalkyl group having 6 to 10 carbon atoms, a cycloalkyl group or cycloalkylalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or a halogen group. Each R1 is independently an alkylene group having 2 to 4 carbon atoms, and each 1 is independently a number from 0 to 3.)

[0036] [ka]

[0037] [ka]

[0038] (In formulas (6) and (7), R2 is a hydrogen atom or a methyl group, R3 is a divalent alkylene group or alkylarylene group having 2 to 10 carbon atoms, R4 is a divalent saturated or unsaturated hydrocarbon group having 2 to 20 carbon atoms, and p is a number from 0 to 10.)

[0039] The reaction between the epoxy compound (a-1) and the (meth)acrylic acid derivative can be carried out by a known method. For example, Japanese Patent Application Laid-Open No. 4-355450 discloses that a diol compound containing a polymerizable unsaturated group can be obtained by using about 2 moles of (meth)acrylic acid per mole of an epoxy compound having two epoxy groups. In the present invention, the compound obtained by the reaction is a diol (d) containing a polymerizable unsaturated group represented by formula (8) (hereinafter, also simply referred to as "diol (d) represented by general formula (8)").

[0040] [ka]

[0041] (In formula (8), each Ar is independently an aromatic hydrocarbon group having 6 to 14 carbon atoms, and a portion of the bonded hydrogen atom may be substituted with an alkyl group having 1 to 10 carbon atoms, an aryl group or arylalkyl group having 6 to 10 carbon atoms, a cycloalkyl group or cycloalkylalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or a halogen group. Each G is independently a substituent represented by general formula (2) or general formula (3), each R1 is independently an alkylene group having 2 to 4 carbon atoms, and each 1 is independently a number from 0 to 3.)

[0042] [ka]

[0043] [ka]

[0044] (In formulas (2) and (3), R2 is a hydrogen atom or a methyl group, R3 is a divalent alkylene group or alkylarylene group having 2 to 10 carbon atoms, R4 is a divalent saturated or unsaturated hydrocarbon group having 2 to 20 carbon atoms, and p is a number from 0 to 10.)

[0045] In the synthesis of the diol (d) represented by the general formula (8) and the subsequent production of the alkali-soluble resin containing a polymerizable unsaturated group represented by the general formula (1) by reacting the diol (d) with a polycarboxylic acid or anhydride thereof, the reaction is usually carried out in a solvent using a catalyst as necessary.

[0046] Examples of the solvent include cellosolve-based solvents such as ethyl cellosolve acetate and butyl cellosolve acetate, high-boiling ether or ester-based solvents such as diglyme, ethyl carbitol acetate, butyl carbitol acetate, and propylene glycol monomethyl ether acetate, and ketone-based solvents such as cyclohexanone and diisobutyl ketone. There are no particular limitations on the reaction conditions such as the solvent and catalyst used, but it is preferable to use, for example, a solvent that does not have a hydroxyl group and has a boiling point higher than the reaction temperature as the reaction solvent.

[0047] In addition, it is preferable to use a catalyst in the reaction between an epoxy group and a carboxy group or a hydroxyl group. JP-A-9-325494 describes ammonium salts such as tetraethylammonium bromide and triethylbenzylammonium chloride, and phosphines such as triphenylphosphine and tris(2,6-dimethoxyphenyl)phosphine.

[0048] Next, the diol (d) represented by general formula (8) obtained by the reaction of the epoxy compound (a-1) with the (meth)acrylic acid derivative is reacted with a dicarboxylic acid or tricarboxylic acid or its acid anhydride (b) and a tetracarboxylic acid or its acid dianhydride (c) to obtain an alkali-soluble resin having a carboxy group and a polymerizable unsaturated group in one molecule represented by general formula (1).

[0049] [ka]

[0050] (In formula (1), Ar are each independently an aromatic hydrocarbon group having 6 to 14 carbon atoms, and a portion of the bonded hydrogen atoms may be substituted with an alkyl group having 1 to 10 carbon atoms, an aryl group or arylalkyl group having 6 to 10 carbon atoms, a cycloalkyl group or cycloalkylalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or a halogen group. Each R1 is independently an alkylene group having 2 to 4 carbon atoms, and each 1 is independently a number from 0 to 3. Each G is independently a substituent represented by general formula (2) or general formula (3), and Y is a tetravalent carboxylic acid residue. Each Z is independently a hydrogen atom or a substituent represented by general formula (4), and at least one Z is a substituent represented by general formula (4). n is a number having an average value of 1 to 20.)

[0051] [ka]

[0052] [ka]

[0053] (In formulas (2) and (3), R2 is a hydrogen atom or a methyl group, R3 is a divalent alkylene group or alkylarylene group having 2 to 10 carbon atoms, R4 is a divalent saturated or unsaturated hydrocarbon group having 2 to 20 carbon atoms, and p is a number from 0 to 10.)

[0054] [ka]

[0055] (In formula (4), W is a divalent or trivalent carboxylic acid residue, and m is 1 or 2.)

[0056] Next, the substituent represented by general formula (2) or (3) derived from the (meth)acrylic acid derivative represented by general formula (6) or general formula (7) constituting the alkali-soluble resin represented by general formula (1) will be described in detail.

[0057] The general formulae (2), (3), (6) and (7) each have a polymerizable unsaturated group and at least one ester bond.

[0058] [ka]

[0059] [ka]

[0060] [ka]

[0061] [ka]

[0062] In the general formulas (2), (3), (6) and (7), R2 is a hydrogen atom or a methyl group.

[0063] In addition, in the general formulae (2), (3), (6) and (7), R3 is a divalent alkylene or alkylarylene group having 2 to 10 carbon atoms.

[0064] The alkylene group may be either straight-chain or branched, and examples thereof include ethylene, ethylidene, vinylene, vinylidene, propylene, trimethylene, propenylene, isopropylidene, and tetramethylene groups.

[0065] Furthermore, the alkylarylene group may be an unsubstituted arylene group as long as it is within the range of the carbon number, and examples thereof include o-, m-, or p-phenylene, toluylene, ethylphenylene, n-propylphenylene, isopropylphenylene, linear or branched butylphenylene, and pentylphenylene groups.

[0066] In the general formulae (2), (3), (6) and (7), R4 is a saturated or unsaturated aliphatic or aromatic hydrocarbon group having 2 to 20 carbon atoms.

[0067] The above-mentioned saturated and unsaturated aliphatic hydrocarbon groups may be either straight-chain or branched, and include ethylene, ethylidene, vinylene, vinylidene, propylene, trimethylene, propenylene, isopropylidene, and tetramethylene groups.

[0068] The aromatic hydrocarbon group may be unsubstituted within the range of the carbon number, for example, o-, m-, or p-phenylene, toluylene, ethylphenylene, n-propylphenylene, isopropylphenylene, linear or branched butylphenylene, pentylphenylene, etc., and may be substituted with 2 to 4 substituents as long as the carbon number does not exceed the range. The aliphatic hydrocarbon group may be interrupted by an unsaturated bond, an ether bond, or an ester bond.

[0069] Furthermore, when synthesizing the alkali-soluble resin represented by general formula (1), p is independently a number from 0 to 10, but the average value of p in the resin is preferably a number from 0 to 5, and more preferably a number from 0 to 2. When the average value of p is within the above range, the distribution of the flexible structure, alkylene oxide, can be prevented from becoming wide, so that sufficient curability as a cured film can be imparted without deteriorating the resin performance.

[0070] The acid component used to synthesize the alkali-soluble resin represented by general formula (1) is a polyvalent acid component capable of reacting with the hydroxyl group in the diol (d) molecule represented by general formula (8), and it is necessary to use a dicarboxylic acid or tricarboxylic acid or its monoanhydride (b) in combination with a tetracarboxylic acid or its dianhydride (c). The carboxylic acid residue of the acid component may be either a saturated or unsaturated hydrocarbon group. In addition, these carboxylic acid residues may contain bonds containing heteroatoms such as -O-, -S-, and carbonyl groups.

[0071] Examples of the dicarboxylic acid or tricarboxylic acid or the acid monoanhydride thereof (b) include chain hydrocarbon dicarboxylic acid or tricarboxylic acid, alicyclic hydrocarbon dicarboxylic acid or tricarboxylic acid, aromatic hydrocarbon dicarboxylic acid or tricarboxylic acid, or the acid monoanhydride thereof, and the like.

[0072] Examples of the acid monoanhydrides of the above-mentioned chain hydrocarbon dicarboxylic acids or tricarboxylic acids include acid monoanhydrides of succinic acid, acetylsuccinic acid, maleic acid, adipic acid, itaconic acid, azelaic acid, citramalic acid, malonic acid, glutaric acid, citric acid, tartaric acid, oxoglutaric acid, pimelic acid, sebacic acid, suberic acid, diglycolic acid, and the like, and acid monoanhydrides of dicarboxylic acids or tricarboxylic acids into which any substituent has been introduced.

[0073] Examples of the acid monoanhydrides of the alicyclic dicarboxylic acid or tricarboxylic acid include acid monoanhydrides of cyclobutanedicarboxylic acid, cyclopentanedicarboxylic acid, hexahydrophthalic acid, tetrahydrophthalic acid, norbornanedicarboxylic acid, and acid monoanhydrides of dicarboxylic acids or tricarboxylic acids into which any substituent has been introduced.

[0074] Examples of the acid monoanhydrides of the aromatic dicarboxylic or tricarboxylic acids include acid monoanhydrides of phthalic acid, isophthalic acid, trimellitic acid, and the like, and acid monoanhydrides of dicarboxylic acids or tricarboxylic acids having any substituent introduced therein.

[0075] Among the above dicarboxylic acid or tricarboxylic acid monoanhydrides, succinic acid, itaconic acid, tetrahydrophthalic acid, hexahydrotrimellitic acid, phthalic acid, and trimellitic acid are preferred, and succinic acid, itaconic acid, and tetrahydrophthalic acid are more preferred.

[0076] In addition, in the case of dicarboxylic acids or tricarboxylic acids, it is preferable to use their acid monoanhydrides. The above-mentioned acid monoanhydrides of dicarboxylic acids or tricarboxylic acids may be used alone or in combination of two or more kinds.

[0077] Examples of the tetracarboxylic acid or its dianhydride (c) include chain hydrocarbon tetracarboxylic acid, alicyclic hydrocarbon tetracarboxylic acid, aromatic hydrocarbon tetracarboxylic acid, or dianhydrides thereof.

[0078] Examples of the chain hydrocarbon tetracarboxylic acid include butane tetracarboxylic acid, pentane tetracarboxylic acid, hexane tetracarboxylic acid, and chain hydrocarbon tetracarboxylic acids having a substituent such as an alicyclic hydrocarbon group or an unsaturated hydrocarbon group introduced therein.

[0079] Examples of the alicyclic tetracarboxylic acid include cyclobutane tetracarboxylic acid, cyclopentane tetracarboxylic acid, cyclohexane tetracarboxylic acid, cycloheptane tetracarboxylic acid, norbornane tetracarboxylic acid, and alicyclic tetracarboxylic acids having a substituent such as a chain hydrocarbon group or an unsaturated hydrocarbon group introduced therein.

[0080] Examples of aromatic tetracarboxylic acids include pyromellitic acid, benzophenone tetracarboxylic acid, biphenyl tetracarboxylic acid, diphenyl ether tetracarboxylic acid, diphenyl sulfone tetracarboxylic acid, naphthalene-1,4,5,8-tetracarboxylic acid, and naphthalene-2,3,6,7-tetracarboxylic acid.

[0081] In addition, bis(trimellitic anhydride) aryl esters can also be used. Bis(trimellitic anhydride) aryl esters are a group of compounds produced, for example, by the method described in International Publication No. 2010 / 074065, and are structurally dianhydrides in which two hydroxyl groups of an aromatic diol (such as naphthalenediol, biphenol, terphenyldiol, etc.) react with the carboxyl groups of two molecules of trimellitic anhydride to form an ester bond. Hereinafter, these compounds will be referred to as bis(trimellitic anhydride) esters of aromatic diols.

[0082] Among the above tetracarboxylic acids or their dianhydrides, biphenyltetracarboxylic acid, benzophenonetetracarboxylic acid, and diphenylethertetracarboxylic acid are preferred, and biphenyltetracarboxylic acid and diphenylethertetracarboxylic acid are more preferred. In addition, among the above tetracarboxylic acids or their dianhydrides, it is preferred to use the dianhydrides. Furthermore, bis(trimellitic anhydride) esters of naphthalene diols can also be preferably used. The above tetracarboxylic acids or their dianhydrides, and bis(trimellitic anhydride) esters of aromatic diols may be used alone or in combination of two or more.

[0083] The reaction of the diol (d) represented by the general formula (8) with the acid components (b) and (c) is not particularly limited, and any known method can be used. For example, JP-A-9-325494 describes a method of reacting an epoxy (meth)acrylate with a tetracarboxylic dianhydride at a reaction temperature of 90 to 140° C.

[0084] Here, it is preferable to react the compound so that the terminals of the compound become carboxy groups, and so that the molar ratio of the compound with the epoxy (meth)acrylate (d), dicarboxylic acid or tricarboxylic acid or their monoanhydrides (b), and tetracarboxylic dianhydride (c) is (d):(b):(c)=1.0:0.01-1.0:0.2-1.0.

[0085] For example, when an acid monoanhydride (b) and an acid dianhydride (c) are used, it is preferable to react them so that the molar ratio [(d) / [(b) / 2+(c)]] of the amount of the acid component to the diol (d) containing a polymerizable unsaturated group is 0.5 to 1.0. Here, when the molar ratio is 1.0 or less, the content of the diol containing an unreacted polymerizable unsaturated group is not increased, so the stability over time of the alkali-soluble resin composition can be improved. On the other hand, when the molar ratio exceeds 0.5, the terminal of the alkali-soluble resin represented by formula (2) does not become an acid anhydride, so that the content of the unreacted acid dianhydride can be suppressed from increasing, so the stability over time of the alkali-soluble resin composition can be improved. In addition, in order to adjust the acid value and molecular weight of the alkali-soluble resin represented by general formula (2), the molar ratio of each component (b), (c) and (d) can be arbitrarily changed within the above-mentioned range.

[0086] The acid value of the alkali-soluble resin represented by the general formula (1) is preferably in the range of 20 to 180 mgKOH / g, and more preferably 40 mgKOH / g or more and 120 mgKOH / g or less. When the acid value is 20 mgKOH / g or more, residues are less likely to remain during alkaline development, and when the acid value is 180 mgKOH / g or less, the penetration of the alkaline developer is not too fast, so peeling development can be suppressed. The acid value can be determined by titration with a 1 / 10N-KOH aqueous solution using a potentiometric titrator "COM-1600" (manufactured by Hiranuma Sangyo Co., Ltd.).

[0087] The weight average molecular weight (Mw) of the alkali-soluble resin represented by the general formula (1) in terms of polystyrene, as measured by gel permeation chromatography (GPC) (HLC-8220GPC, manufactured by Tosoh Corporation), is usually 1000 to 100000, preferably 2000 to 20000, and more preferably 2000 to 6000. When the weight average molecular weight is 1000 or more, it is possible to suppress a decrease in the adhesion of the pattern during alkali development. In addition, when the weight average molecular weight (Mw) is less than 100000, it is easy to adjust the solution viscosity of the photosensitive resin composition to a suitable level for application, and alkali development does not take too long.

[0088] Next, a photosensitive resin composition using the alkali-soluble resin represented by the general formula (1) of the present invention will be described.

[0089] In the photosensitive resin composition of the present invention, the content of component (A) is preferably 10 to 90% by mass based on the total mass of the solid content, the content of component (B) is preferably 5 to 200 parts by mass based on 100 parts by mass of component (A), and the content of component (C) is preferably 0.1 to 30 parts by mass based on 100 parts by mass of the combined amount of components (A) and (B).

[0090] Examples of the photopolymerizable monomer (B) having at least three ethylenically unsaturated bonds in the photosensitive resin composition of the present invention include (meth)acrylic acid esters such as trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, sorbitol penta(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, sorbitol hexa(meth)acrylate, alkylene oxide-modified hexa(meth)acrylate of phosphazene, and caprolactone-modified dipentaerythritol hexa(meth)acrylate; dendrimer-type multifunctional acrylates, etc. These photopolymerizable monomers may be used alone or in combination of two or more.

[0091] The content of the (B) component is preferably 5 to 200 parts by mass relative to 100 parts by mass of the (A) component, more preferably 10 to 80 parts by mass relative to 100 parts by mass of the (A) component, and even more preferably 10 to 60 parts by mass. When the content of the (B) component is 5 parts by mass or more relative to 100 parts by mass of the (A) component, the photoreactive functional group in the resin is sufficient, so that a sufficient crosslinked structure is formed. In addition, since the acid value of the resin component does not become too high, the solubility in an alkaline developer in the exposed area is reduced, so that the formed pattern can be prevented from becoming thinner than the target line width and the pattern can be prevented from being missing. In addition, when the content of the (B) component is 200 parts by mass or less relative to 100 parts by mass of the (A) component, a cured film having sufficient curability can be obtained, so that the pattern edge can be made sharp.

[0092] Examples of the photopolymerization initiator (C) in the photosensitive resin composition of the present invention include acetophenones such as acetophenone, 2,2-diethoxyacetophenone, p-dimethylacetophenone, p-dimethylaminopropiophenone, dichloroacetophenone, trichloroacetophenone, and p-tert-butylacetophenone; benzophenones such as benzophenone, 2-chlorobenzophenone, and p,p'-bisdimethylaminobenzophenone; benzil, benzoin, benzoin methyl ether, benzoin isopropyl ether, benzoin benzoin ethers such as phenyl isobutyl ether; biimidazole compounds such as 2-(o-chlorophenyl)-4,5-phenylbiimidazole, 2-(o-chlorophenyl)-4,5-di(m-methoxyphenyl)biimidazole, 2-(o-fluorophenyl)-4,5-diphenylbiimidazole, 2-(o-methoxyphenyl)-4,5-diphenylbiimidazole, and 2,4,5-triarylbiimidazole; 2-trichloromethyl-5-styryl-1,3,4-oxadiazole, 2-trichloromethyl-5-(p halomethyldiazole compounds such as 2,4,6-tris(trichloromethyl)-1,3,5-triazine, 2-methyl-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-phenyl-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-chlorophenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, halomethyl-s-triazine compounds such as 2-(4-methoxynaphthyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxystyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(3,4,5-trimethoxystyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine, and 2-(4-methylthiostyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine;O-Acyloxime compounds such as 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime), 1-(4-phenylsulfanylphenyl)butane-1,2-dione-2-oxime-O-benzoate, 1-(4-methylsulfanylphenyl)butane-1,2-dione-2-oxime-O-acetate, 1-(4-methylsulfanylphenyl)butan-1-one oxime-O-acetate; benzyl dimethyl ketal, thioxanthone, 2-chlorothioxanthone, 2,4-diethylthioxanthone Examples of the photopolymerization initiator include sulfur compounds such as 2-ethylanthraquinone, 2-methylthioxanthone, and 2-isopropylthioxanthone; anthraquinones such as 2-ethylanthraquinone, octamethylanthraquinone, 1,2-benzanthraquinone, and 2,3-diphenylanthraquinone; organic peroxides such as azobisisobutyronitrile, benzoyl peroxide, and cumene peroxide; thiol compounds such as 2-mercaptobenzimidazole, 2-mercaptobenzoxazole, and 2-mercaptobenzothiazole; and tertiary amines such as triethanolamine and triethylamine. These photopolymerization initiators may be used alone or in combination of two or more kinds.

[0093] In particular, when preparing a photosensitive resin composition containing a colorant, it is preferable to use O-acyloxime compounds (including ketoxime). Specific compound groups include O-acyloxime photopolymerization initiators represented by general formula (9) or general formula (10). Among them, when using a colorant at a high pigment concentration or forming a light-shielding film pattern, it is preferable to use an O-acyloxime photopolymerization initiator having a molar absorption coefficient at 365 nm of 10,000 L / mol cm or more. In the present invention, the term "photopolymerization initiator" is used to include a sensitizer.

[0094] [ka]

[0095] (In formula (9), R5 and R6 are each independently an alkyl group having 1 to 15 carbon atoms, an aryl group having 6 to 18 carbon atoms, an arylalkyl group having 7 to 20 carbon atoms, or a heterocyclic group having 4 to 12 carbon atoms; and R7 is an alkyl group having 1 to 15 carbon atoms, an aryl group having 6 to 18 carbon atoms, or an arylalkyl group having 7 to 20 carbon atoms. Here, the alkyl group and the aryl group may be substituted with an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkanoyl group having 1 to 10 carbon atoms, or a halogen, and the alkylene portion may contain an unsaturated bond, an ether bond, a thioether bond, or an ester bond. In addition, the alkyl group may be any of a linear, branched, and cyclic alkyl group.)

[0096] [ka]

[0097] (In formula (10), R8 and R9 each independently represent a linear or branched alkyl group having 1 to 10 carbon atoms, a cycloalkyl group, a cycloalkylalkyl group, or an alkylcycloalkyl group having 4 to 10 carbon atoms, or a phenyl group which may be substituted with an alkyl group having 1 to 6 carbon atoms. R 10 are each independently a linear or branched alkyl or alkenyl group having 2 to 10 carbon atoms, and some of the -CH2- groups in the alkyl or alkenyl group may be substituted with -O- groups. 10 A portion of the hydrogen atoms in the group may be substituted with halogen atoms.

[0098] The content of component (C) is preferably 0.1 to 30 parts by mass, more preferably 1 to 25 parts by mass, per 100 parts by mass of the total amount of components (A) and (B). When the content of component (C) is 0.1 parts by mass or more, the photopolymerization speed is appropriate, and therefore a decrease in sensitivity can be suppressed. When the content is 30 parts by mass or less, the line width can be faithfully reproduced on the mask, and the pattern edge can be sharpened.

[0099] Examples of the solvent contained in the (D) photosensitive resin composition include alcohols such as methanol, ethanol, n-propanol, isopropanol, ethylene glycol, propylene glycol, 3-methoxy-1-butanol, ethylene glycol monobutyl ether, 3-hydroxy-2-butanone, and diacetone alcohol; terpenes such as α- or β-terpineol; ketones such as acetone, methyl ethyl ketone, cyclohexanone, and N-methyl-2-pyrrolidone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; cellosolve, methyl cellosolve, ethyl cellosolve, carbitol, methyl carbitol, ethyl carbitol, butyl carbitol, diethylene glycol ethyl methyl ether, and propylene glycol monomethyl ether. Examples of the solvent include glycol ethers such as propylene glycol monoethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, triethylene glycol monomethyl ether, and triethylene glycol monoethyl ether; and esters such as ethyl acetate, butyl acetate, ethyl lactate, 3-methoxybutyl acetate, 3-methoxy-3-butyl acetate, 3-methoxy-3-methyl-1-butyl acetate, cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, carbitol acetate, ethyl carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate. By dissolving and mixing using these, a uniform solution-like composition can be obtained. These solvents may be used alone or in combination of two or more to obtain the necessary characteristics such as coatability. The amount of the solvent varies depending on the target viscosity, but is preferably 60 to 90% by mass in the photosensitive resin composition solution.

[0100] The photosensitive resin composition contains a colorant as component (E). When used as a resist for a light-shielding film, the component (E) is one or more light-shielding components selected from the group consisting of black organic pigments, mixed-color organic pigments, and light-shielding materials, and is preferably a black organic pigment and / or a mixed-color organic pigment. The average secondary particle size of the black organic pigment and / or the mixed-color organic pigment is preferably 20 to 500 nm. The average secondary particle size of the black organic pigment and the mixed-color organic pigment can be measured by the cumulant method using a particle size distribution meter "Particle Size Analyzer FPAR-1000" (manufactured by Otsuka Electronics Co., Ltd.) that uses a dynamic light scattering method.

[0101] The content of the colorant, which is component (E), can be determined arbitrarily depending on the desired light blocking degree, but is preferably 1 to 80 mass % based on the solid content in the photosensitive resin composition, and more preferably 20 to 60 mass % when an organic pigment or a carbon-based inorganic pigment is used.

[0102] Examples of the black organic pigments that are the component (E) include perylene black, aniline black, cyanine black, and lactam black.

[0103] Examples of mixed-color organic pigments, which are component (E), include pseudo-black pigments obtained by mixing at least two colors selected from organic pigments such as azo pigments, condensed azo pigments, azomethine pigments, phthalocyanine pigments, quinacridone pigments, isoindolinone pigments, isoindoline pigments, dioxazine pigments, threne pigments, perylene pigments, perinone pigments, quinophthalone pigments, diketopyrrolopyrrole pigments, and thioindigo pigments.

[0104] Examples of the light-shielding material (E) include carbon black, chromium oxide, iron oxide, titanium black, etc. These (E) components may be appropriately surface-treated depending on the function of the intended photosensitive resin composition. These (E) components may be used alone or in combination of two or more.

[0105] Examples of organic pigments that can be used as component (E) include, but are not limited to, those having the following Color Index numbers: Pigment Red 2, 3, 4, 5, 9, 12, 14, 22, 23, 31, 38, 112, 122, 144, 146, 147, 149, 166, 168, 170, 175, 176, 177, 178, 179, 184, 185, 187, 188, 202, 207, 208, 209, 210, 213, 214, 220, 221, 242, 247, 253, 254, 255, 256, 257, 262, 264, 266, 272, 279 etc. Pigment Orange 5, 13, 16, 34, 36, 38, 43, 61, 62, 64, 67, 68, 71, 72, 73, 74, 81 etc. Pigment Yellow 1, 3, 12, 13, 14, 16, 17, 55, 73, 74, 81, 83, 93, 95, 97, 109, 110, 111, 117, 120, 126, 127, 128, 129, 130, 136, 138, 139, 150, 151, 153, 154, 155, 173, 174, 175, 176, 180, 181, 183, 185, 191, 194, 199, 213, 214 etc. Pigment Green 7, 36, 58 etc. Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 60, 80 etc. Pigment Violet 19, 23, 37 etc.

[0106] In addition, it is preferable that the colorant (E) is dispersed in the (D) solvent together with the (F) dispersant in advance to form a colorant dispersion, and then blended into the photosensitive resin composition. Here, the solvent for dispersion becomes a part of the (D) component, so any solvent contained in the above-mentioned (D) component can be used. Among the above-mentioned (D) components, propylene glycol monomethyl ether acetate, 3-methoxybutyl acetate, 3-methoxy-3-methyl-1-butyl acetate, etc. are preferable.

[0107] The content of the component (E) is preferably 1 to 80% by mass, more preferably 30 to 60% by mass, based on the total solid content of the photosensitive resin composition of the present invention. The solid content means the components of the photosensitive resin composition excluding the component (D). The solid content also includes the component (B) that becomes a solid content after photocuring. When the component (E) is 1% by mass or more, it is easy to set the desired light-shielding properties. When the component (E) is 80% by mass or less, the desired development characteristics and film-forming ability are obtained.

[0108] The above-mentioned (F) dispersant can be any known compound used for dispersing colorants (pigments) (compounds commercially available under names such as dispersants, dispersion wetting agents, and dispersion promoters) without any particular restrictions.

[0109] Examples of the dispersant, which is the component (F), include cationic polymer dispersants, anionic polymer dispersants, nonionic polymer dispersants, and pigment derivative-type dispersants (dispersing aids). In particular, the dispersant is preferably a cationic polymer dispersant having a cationic functional group such as an imidazolyl group, a pyrrolyl group, a pyridyl group, or a primary, secondary, or tertiary amino group as an adsorption site to the colorant, an amine value of 1 to 100 mgKOH / g, and a number average molecular weight in the range of 1,000 to 100,000. The blending amount of this dispersant is preferably 1 to 35% by mass, more preferably 2 to 25% by mass, based on the colorant. Note that, although high-viscosity substances such as resins generally have the effect of stabilizing dispersion, those that do not have the ability to promote dispersion are not treated as dispersants. However, there is no restriction on using them for the purpose of stabilizing dispersion.

[0110] In addition, when preparing the colorant dispersion, by co-dispersing a part of the polymerizable unsaturated group-containing alkali-soluble resin of the component (A) in addition to the dispersant (F), it is possible to obtain a photosensitive resin composition that is easy to maintain high exposure sensitivity, has good adhesion during development, and is less likely to cause residue problems. The content of the component (A) in the colorant dispersion is preferably 2 to 20 mass %, more preferably 5 to 15 mass %. When the component (A) is 2 mass % or more, the effects of co-dispersion such as improved sensitivity, improved adhesion, and reduced residue can be obtained. When the content is 20 mass % or less, a cured film (coating film) in which the component (E) is uniformly dispersed can be obtained.

[0111] The colorant dispersion can be mixed with the component (A) (if the component (A) is co-dispersed when the colorant dispersion is prepared, the remaining component (A)), the component (B), the component (C), and the remaining component (E) to form a photosensitive resin composition for a light-shielding film.

[0112] The photosensitive resin composition of the present invention may be used in combination with other resin components that polymerize or harden by light or heat, if necessary. Examples of other resin components include novolac epoxy resins derived from novolacs such as phenol novolac and cresol novolac, epoxy resins such as bisphenol type epoxy resins, and alkali-soluble resins (excluding component (A)) obtained by reacting the epoxy resins with (meth)acrylic acid and acid anhydrides, copolymers with (meth)acrylic acid and / or (meth)acrylic acid esters, and alkali-soluble resins obtained by reacting the carboxyl groups in the copolymers with epoxy group-containing (meth)acrylates.

[0113] The photosensitive resin composition of the present invention may contain additives such as a curing agent, a curing accelerator, a thermal polymerization inhibitor, an antioxidant, a plasticizer, a filler, a leveling agent, an antifoaming agent, a surfactant, and a coupling agent, as necessary.

[0114] Examples of curing agents include amine compounds, polyvalent carboxylic acid compounds, phenolic resins, amino resins, dicyandiamide, Lewis acid complex compounds, etc., which contribute to the curing of epoxy resins. Examples of curing accelerators include tertiary amines, quaternary ammonium salts, tertiary phosphines, quaternary phosphonium salts, boric acid esters, Lewis acids, organometallic compounds, imidazoles, etc., which contribute to the curing acceleration of epoxy resins. Examples of thermal polymerization inhibitors and antioxidants include hydroquinone, hydroquinone monomethyl ether, pyrogallol, tert-butylcatechol, phenothiazine, hindered phenol compounds, etc. Examples of plasticizers include dibutyl phthalate, dioctyl phthalate, tricresyl phosphate, etc. Examples of fillers include glass fiber, silica, mica, alumina, etc. Examples of defoamers and leveling agents include silicone-based, fluorine-based, and acrylic compounds. Examples of surfactants include fluorine-based surfactants, silicone-based surfactants, etc. Examples of coupling agents include 3-(glycidyloxy)propyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-ureidopropyltriethoxysilane, and the like.

[0115] The cured film (coating film) of the present invention can be formed by a photolithography method using the photosensitive resin composition of the present invention. The above method is a method in which a photosensitive resin composition solution is first applied to a substrate surface, the solvent is dried (pre-baked), a photomask is placed on the coating film, ultraviolet rays are irradiated to cure the exposed parts, and development is performed to dissolve the unexposed parts using an alkaline aqueous solution to form a pattern, and post-baking is further performed as post-curing. Here, examples of the substrate to which the photosensitive resin composition solution is applied include glass, transparent films (e.g., polycarbonate, polyethylene terephthalate, polyethersulfone, etc.), etc.

[0116] The substrate may be a transparent substrate or a substrate other than a transparent substrate. Examples of the transparent substrate to which the photosensitive resin composition is applied include a glass substrate and a transparent film (e.g., polycarbonate, polyethylene terephthalate, polyethersulfone, etc.) on which a transparent electrode such as ITO or gold is vapor-deposited or patterned.

[0117] The method of applying the photosensitive resin composition solution onto the substrate may be a known solution immersion method, a spray method, or a method using a roller coater, a land coater, a slit coater, or a spinner. After applying the solution to a desired thickness by the above method, the solvent is dried (prebaked) to form a coating. The prebaking is performed by heating in an oven, a hot plate, or the like. The heating temperature and heating time in the prebaking are appropriately selected depending on the solvent used, and are performed, for example, at a temperature of 60 to 110°C for 1 to 3 minutes.

[0118] The exposure performed after the pre-baking is performed by an ultraviolet exposure device, and only the resist in the portion corresponding to the pattern is exposed by exposing through a photomask. The exposure device and the exposure irradiation conditions are appropriately selected, and the exposure is performed using a light source such as an ultra-high pressure mercury lamp, a high pressure mercury lamp, a metal halide lamp, or a far ultraviolet lamp, to photocure the photosensitive resin composition in the coating film.

[0119] Examples of radiation used for exposure include visible light, ultraviolet light, far ultraviolet light, electron beams, and X-rays, and the wavelength range of the radiation is preferably 250 to 450 nm. Examples of developers suitable for this alkaline development include aqueous solutions of sodium carbonate, potassium carbonate, potassium hydroxide, diethanolamine, and tetramethylammonium hydroxide. These developers can be appropriately selected according to the characteristics of the resin layer, and it is also effective to add a surfactant as necessary. The development temperature is preferably 20 to 35°C, and fine images can be precisely formed using a commercially available developing machine or ultrasonic cleaner. After alkaline development, the film is usually washed with water. Examples of development methods that can be used include shower development, spray development, dip (immersion) development, and puddle (liquid puddle) development.

[0120] The alkaline development after exposure is carried out for the purpose of removing the photosensitive resin composition in the unexposed portion, and the desired pattern is formed by this development. Examples of the developer suitable for this alkaline development include an aqueous solution of carbonate of an alkali metal or an alkaline earth metal, an aqueous solution of hydroxide of an alkali metal, etc., but it is particularly preferable to use a weakly alkaline aqueous solution containing 0.03 to 1% by weight of carbonate such as sodium carbonate or potassium carbonate at a temperature of 23 to 27°C, and fine images can be precisely formed using a commercially available developing machine, ultrasonic cleaner, etc.

[0121] After development in this manner, heat treatment (post-baking) is performed at 180 to 250°C for 20 to 100 minutes. However, when the heat resistance of the substrate on which the film is formed is low, the composition can be designed so that the post-baking conditions are 80 to 180°C and 30 to 100 minutes. This post-baking is performed for the purpose of increasing the adhesion between the patterned coating film and the substrate. This is performed by heating in an oven, a hot plate, or the like, as in the pre-baking. The patterned cured film of the present invention is formed through each process of the photolithography method described above. EXAMPLES

[0122] Hereinafter, the embodiments of the present invention will be described in detail based on examples and comparative examples, but the present invention is not limited to these.

[0123] First, the synthesis examples of the alkali-soluble resin containing a polymerizable unsaturated group, which contains a structure represented by general formula (1), will be described. The evaluation of the resin in these synthesis examples was performed as follows unless otherwise specified. When the same model of measuring equipment was used, the name of the equipment manufacturer is omitted from the second position. In addition, in Examples 1 and 2, the glass substrates used for preparing the substrates with the cured film for measurement were all glass substrates that had been subjected to the same treatment.

[0124] [Solid content concentration] 1 g of the resin solution obtained in Synthesis Example was impregnated into a glass filter (weight: W0(g)), weighed [W1(g)], and the weight after heating at 160°C for 2 hours [W2(g)] was calculated from the following formula (1). Solid content concentration (weight%) = 100 × (W2-W0) / (W1-W0) (1)

[0125] [Epoxy equivalent] The resin solution was dissolved in dioxane, and then a solution of tetraethylammonium bromide in acetic acid was added. The content was determined by titration with a 1 / 10N perchloric acid solution using a potentiometric titrator "COM-1600" (manufactured by Hiranuma Sangyo Co., Ltd.).

[0126] [Acid value] The resin solution was dissolved in dioxane and titrated with a 1 / 10N KOH aqueous solution using a potentiometric titrator "COM-1600" to determine the content.

[0127] [Molecular weight] Measurement was performed using gel permeation chromatography (GPC) "HLC-8220GPC" (manufactured by Tosoh Corporation, solvent: tetrahydrofuran, columns: TSKgelSuperH-2000 (2 columns) + TSKgelSuperH-3000 (1 column) + TSKgelSuperH-4000 (1 column) + TSKgelSuperH-5000 (1 column) (manufactured by Tosoh Corporation), temperature: 40°C, speed: 0.6 ml / min), and the weight average molecular weight (Mw) was calculated as a value converted into standard polystyrene (manufactured by Tosoh Corporation, PS-oligomer kit).

[0128] The abbreviations used in the Synthesis Examples and Comparative Synthesis Examples are as follows. BPFE: Bisphenol fluorene type epoxy resin (Epoxy resin with general formula (5) where Ar is a benzene ring and l is 0, epoxy equivalent 256) BNFE: Bisnaphthol fluorene type epoxy resin (Epoxy resin with general formula (5) where Ar is a naphthalene ring and l is 0, epoxy equivalent 281) HOA-HH: 2-acryloyloxyethyl hexahydrophthalic acid (Light Acrylate HOA-HH(N), manufactured by Kyoeisha Chemical Co., Ltd.) BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride BTDA: Benzophenonetetracarboxylic dianhydride BTANE: Bis(trimellitic anhydride) ester of naphthalenediol (DHN-D1, manufactured by Honshu Chemical Industry Co., Ltd.) THPA: 1,2,3,6-Tetrahydrophthalic anhydride TPP: Triphenylphosphine TBPC: 2,6-di-tert-butyl-p-cresol AA: Acrylic acid MAA: Methacrylic acid MMA: Methyl methacrylate CHMA: Cyclohexyl methacrylate AIBN: Azobisisobutyronitrile GMA: Glycidyl methacrylate PGMEA: Propylene glycol monomethyl ether acetate

[0129] [Synthesis Example 1] In a 250 mL four-neck flask equipped with a reflux condenser, BPFE (46.64 g, 0.09 mol), AA (13.12 g, 0.18 mol), TPP (0.24 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105 ° C for 12 hours to obtain a reaction product. Then, PGMEA (20.00 g) was charged and adjusted so that the solid content was 50 mass %.

[0130] Next, BPDA (13.45 g, 0.05 mol) and THPA (6.96 g, 0.05 mol) were added to the obtained reaction product and stirred at 115 to 120 ° C for 6 hours to obtain a polymerizable unsaturated group-containing alkali-soluble resin solution (A)-1. The solid content concentration of the obtained resin solution was 57.3 mass%, the acid value (solid content equivalent) was 96 mg KOH / g, and the Mw by GPC analysis was 3600.

[0131] [Synthesis Example 2] In a 250 mL four-neck flask equipped with a reflux condenser, BNFE (47.60 g, 0.08 mol), AA (12.18 g, 0.17 mol), TPP (0.22 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (20.00 g) was charged and adjusted so that the solid content was 50 mass%.

[0132] Next, BPDA (12.49 g, 0.04 mol) and THPA (6.46 g, 0.04 mol) were added to the obtained reaction product and stirred at 115 to 120° C. for 6 hours to obtain a polymerizable unsaturated group-containing alkali-soluble resin solution (A)-2. The solid content concentration of the obtained resin solution was 56.9 mass%, the acid value (solid content equivalent) was 90 mg KOH / g, and the Mw by GPC analysis was 4000.

[0133] [Synthesis Example 3] In a 250 mL four-neck flask equipped with a reflux condenser, BNFE (47.60 g, 0.08 mol), AA (12.18 g, 0.17 mol), TPP (0.22 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (20.00 g) was charged and adjusted so that the solid content was 50 mass%.

[0134] Next, BPDA (8.74 g, 0.03 mol) and THPA (10.34 g, 0.07 mol) were added to the obtained reaction product and stirred at 115 to 120°C for 6 hours to obtain a polymerizable unsaturated group-containing alkali-soluble resin solution (A)-3. The solid content concentration of the obtained resin solution was 56.9 mass%, the acid value (solid content equivalent) was 90 mgKOH / g, and the Mw by GPC analysis was 2600.

[0135] [Synthesis Example 4] In a 250 mL four-neck flask equipped with a reflux condenser, BNFE (47.60 g, 0.08 mol), AA (12.18 g, 0.17 mol), TPP (0.22 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (20.00 g) was charged and adjusted so that the solid content was 50 mass%.

[0136] Next, BPDA (16.49 g, 0.06 mol) and THPA (0.26 g, 0.002 mol) were added to the obtained reaction product and stirred at 115 to 120 ° C for 6 hours to obtain a polymerizable unsaturated group-containing alkali-soluble resin solution (A)-4. The solid content concentration of the obtained resin solution was 56.1 mass%, the acid value (solid content equivalent) was 83 mg KOH / g, and the Mw by GPC analysis was 7000.

[0137] [Synthesis Example 5] In a 250 mL four-neck flask equipped with a reflux condenser, BNFE (30.53 g, 0.05 mol), HOA-HH (29.33 g, 0.11 mol), TPP (0.14 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105 ° C for 12 hours to obtain a reaction product. Then, PGMEA (20.00 g) was charged and adjusted so that the solid content was 50 mass %.

[0138] Next, BPDA (8.00 g, 0.03 mol) and THPA (4.14 g, 0.03 mol) were added to the obtained reaction product and stirred at 115 to 120 ° C for 6 hours to obtain a polymerizable unsaturated group-containing alkali-soluble resin solution (A)-5. The solid content concentration of the obtained resin solution was 54.6 mass%, the acid value (solid content equivalent) was 63 mg KOH / g, and the Mw by GPC analysis was 5300.

[0139] [Synthesis Example 6] In a 250 mL four-neck flask equipped with a reflux condenser, BNFE (47.60 g, 0.08 mol), AA (12.18 g, 0.17 mol), TPP (0.22 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (20.00 g) was charged and adjusted so that the solid content was 50 mass%.

[0140] Next, BTDA (13.68 g, 0.04 mol) and THPA (6.46 g, 0.04 mol) were added to the obtained reaction product and stirred at 115 to 120 ° C for 6 hours to obtain a polymerizable unsaturated group-containing alkali-soluble resin solution (A)-6. The solid content concentration of the obtained resin solution was 54.6 mass%, the acid value (solid content equivalent) was 92 mg KOH / g, and the Mw by GPC analysis was 4100.

[0141] [Synthesis Example 7] In a 250 mL four-neck flask equipped with a reflux condenser, BNFE (47.60 g, 0.08 mol), AA (12.18 g, 0.17 mol), TPP (0.22 g), and PGMEA (40.00 g) were charged and stirred at 100 to 105° C. for 12 hours to obtain a reaction product. Then, PGMEA (20.00 g) was charged and adjusted so that the solid content was 50 mass%.

[0142] Next, BTANE (21.58 g, 0.04 mol) and THPA (6.46 g, 0.04 mol) were added to the obtained reaction product and stirred at 115 to 120° C. for 7 hours to obtain a polymerizable unsaturated group-containing alkali-soluble resin solution (A)-7. The solid content concentration of the obtained resin solution was 54.6 mass%, the acid value (solid content equivalent) was 91 mgKOH / g, and the Mw by GPC analysis was 5000.

[0143] [Synthesis Example 8] MAA (51.65g, 0.60mol), MMA (36.04g, 0.36mol), CHMA (40.38g, 0.24mol), AIBN (5.91g), and PGMEA (360g) were charged into a 1000ml four-neck flask equipped with a nitrogen inlet tube and a reflux condenser, and the mixture was polymerized by stirring for 8 hours under a nitrogen stream at 80-85°C. Furthermore, GMA (61.41g, 0.43mol), TPP (2.27g), and TBPC (0.086g) were charged into the flask, and the mixture was stirred for 16 hours at 80-85°C to obtain a polymerizable unsaturated group-containing alkali-soluble resin solution (A)-8. The solid content concentration of the obtained resin solution was 35.7% by mass, the acid value (solid content equivalent) was 50mgKOH / g, and the Mw by GPC analysis was 19600.

[0144] (Alkali-soluble resin solution) (A)-1: Alkali-soluble resin solution obtained in Synthesis Example 1 above (A)-2: Alkali-soluble resin solution obtained in Synthesis Example 2 above (A)-3: Alkali-soluble resin solution obtained in Synthesis Example 3 above (A)-4: Alkali-soluble resin solution obtained in Synthesis Example 4 above (A)-5: Alkali-soluble resin solution obtained in Synthesis Example 5 above (A)-6: Alkali-soluble resin solution obtained in Synthesis Example 6 above (A)-7: Alkali-soluble resin solution obtained in Synthesis Example 7 above (A)-8: Alkali-soluble resin solution obtained in Synthesis Example 8 above

[0145] (Photopolymerizable monomer) (B): DPHA (a mixture of dipentaerythritol hexaacrylate and dipentaerythritol pentaacrylate, manufactured by Nippon Kayaku Co., Ltd.)

[0146] (Photopolymerization initiator) (C): Irgacure OXE02 (ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(0-acetyloxime), manufactured by BASF, "Irgacure" is a registered trademark of the company)

[0147] (solvent) (D)-1: Propylene glycol monomethyl ether acetate (D)-2: 3-Methoxy-3-methyl-1-butyl acetate

[0148] (Surfactant) BYK-330 in PGMEA solution (solid content 1.0%) (BYK-Chemie)

[0149] [Example 1] Photosensitive resin compositions of Examples 1 to 10 and Comparative Examples 1 and 2 were prepared by mixing the components (A) to (D) and the surfactant in the ratios shown in Table 1. (D)-1 in the solvent column does not include the amount of PGMEA (same as (D)-1) in the unsaturated group-containing resin solution (polymerizable unsaturated group-containing alkali-soluble resin solution), the solvent in the light-shielding pigment dispersion, and the solvent in the surfactant. All values ​​in Table 1 are in mass %.

[0150] [Table 1]

[0151] [evaluation] The photosensitive resin compositions of Examples 1 to 10 and Comparative Examples 1 and 2 were used to carry out the following evaluations.

[0152] (Preparation of cured film (coating film)) The photosensitive resin composition shown in Table 1 was previously exposed to a low-pressure mercury lamp with an illumination intensity of 1000 mJ / cm at a wavelength of 254 nm. 2 The coating was applied using a spin coater onto a 50 mm x 50 mm glass substrate "EAGLEXG" (manufactured by Corning Incorporated) (hereinafter referred to as "glass substrate"), an indium-tin oxide vapor-deposited glass substrate (hereinafter referred to as "ITO substrate"), and a molybdenum-aluminum alloy vapor-deposited substrate (hereinafter referred to as "MAM substrate") whose surfaces had been cleaned by irradiating them with ultraviolet light of 365 nm, so that the film thickness after heat curing would be 1.5 μm, and the substrate was prebaked at 90°C for 1 minute using a hot plate to prepare a coated substrate. Next, the coating was applied using a spin coater onto a 50 mm x 50 mm glass substrate "EAGLEXG" (manufactured by Corning Incorporated ... 2 100mJ / cm 2 Thereafter, a curing treatment was carried out at 230° C. for 30 minutes using a hot air dryer, thereby obtaining cured films (coating films) according to Examples 1 to 10 and Comparative Examples 1 and 2.

[0153] The cured films (coatings) made of the photosensitive resin compositions of Examples 1 to 10 and Comparative Examples 1 and 2 obtained above were evaluated for the following items, and the results are shown in Table 2. These evaluations were performed as follows. Note that the high-temperature and high-humidity resistant adhesion and the chemical resistant adhesion were evaluated not only for the cured films (coatings) on the glass substrate, but also for the cured films (coatings) formed on the ITO substrate and the MAM substrate.

[0154] (film thickness measurement) The thickness of the cured films (coating films) of Examples 1 to 10 and Comparative Examples 1 and 2 was measured using a stylus-type step shape measuring device "P-17" (manufactured by KLA-Tencol Corporation).

[0155] [High temperature and humidity resistance] (Evaluation method) The cured films (coatings) prepared on the glass substrate, ITO substrate, and MAM substrate were left to stand for 5 hours under the conditions of a temperature of 121°C, humidity of 100%, and atmospheric pressure of 2 atm. After that, a cross-cut peeling test was performed in which 100 1mm x 1mm squares were cut into the substrate using a SuperCutterGuide (manufactured by Taiyu Kizai Co., Ltd.), and cellophane tape (manufactured by Nichiban Co., Ltd.) was applied to the squares and then peeled off.

[0156] (Evaluation Criteria) ○: The cured film (coating film) in the square has not peeled off at all. △: Less than 1 / 3 of the cured film (coating film) in the square has peeled off ×: 1 / 3 or more peeled off

[0157] [Chemical resistance and adhesion] (Evaluation method) The cured films (coatings) prepared on the glass substrate, ITO substrate, and MAM substrate were immersed in a petri dish containing N-methyl-2-pyrrolidone at 60°C for 2 minutes, then washed with pure water and wiped dry. After that, the substrate was cut using a SuperCutterGuide to form 100 1mm x 1mm squares, and a cross-cut peeling test was performed by applying cellophane tape to the squares and peeling them off.

[0158] (Evaluation Criteria) ○: The cured film (coating film) in the square has not peeled off at all. △: Less than 1 / 3 of the cured film (coating film) in the square has peeled off ×: 1 / 3 or more peeled off

[0159] [Coating film hardness 1] (Evaluation method) A load of 750 g was applied to the cured film (coating film) formed on the glass substrate using a pencil hardness tester in accordance with the test method of JIS-K5600-5-4, and the highest pencil hardness that did not scratch the cured film (coating film) was indicated. The pencil used was "Mitsubishi Hi-Uni" (manufactured by Mitsubishi Pencil Co., Ltd.). This evaluation was carried out as an index of resistance to lateral forces (scratching) on ​​the coating film surface.

[0160] (Evaluation Criteria) ○: 3H or more △:2H ×: H or less

[0161] [Coating film hardness 2] (Evaluation method) The hardness of the cured film (coating film) formed on the glass substrate was measured using a microfilm hardness tester "HM2000" (manufactured by Fisher Instruments). The indenter was a Vickers indenter with a hardness of 5 mN / μm. 2 A load of 0.25 mN / sec was applied, and the load was removed after one second, to measure Martens hardness (based on ISO14577). This evaluation was carried out as an index of the resistance of the cured film (coating) surface to vertical forces (indentation). Note that "Martens hardness" is the hardness calculated from the load-penetration depth curve.

[0162] (Evaluation Criteria) ○: 65N / mm 2 End △: 60N / mm 2 More than 65N / mm 2 less than ×:60N / mm 2 less than

[0163] [Transmittance 1] (Evaluation method) The transmittance of a cured film (coating film) formed on a glass substrate "EAGLE XG" with a thickness of 2 μm was measured using a transmittance meter "SPECTRO PHOTOMETER SD5000" (manufactured by Nippon Denshoku Industries Co., Ltd.).

[0164] (Evaluation Criteria) ○: Transmittance at a wavelength of 400 nm is 95% or more △: Transmittance at a wavelength of 400 nm is 90% or more but less than 95% ×: Less than 90%

[0165] [Transmittance 2] The transmittance of a cured film (coating film) formed on a glass substrate "EAGLE XG" with a thickness of 3 μm was measured using a transmittance meter "SPECTRO PHOTOMETER SD5000."

[0166] (Evaluation Criteria) ○: Transmittance at a wavelength of 340 nm is less than 20% △: Transmittance at a wavelength of 340 nm is 20% or more and less than 65% ×: 65% or more

[0167] [Gas generation] (Evaluation method) The cured film (coating) produced on the glass substrate "EAGLE XG" was scraped off with a scraper or the like, and the thermal weight loss of 10 mg of the resulting powder-like cured film (coating) was measured using a differential thermal analyzer (TG / DTA) "EXSTAR6000" (Hitachi High-Tech Science Corporation). The measurement conditions were pretreatment at 120°C for 30 minutes in air, followed by holding at 230°C for 3 hours. Gas generation was evaluated from the weight loss rate, which was calculated from the weight loss before and after heating at 230°C.

[0168] (Evaluation Criteria) ◎: Weight loss rate is less than 3% ○: Weight loss rate is 3% or more and less than 7% △: Weight loss rate is 7% or more and less than 15% ×: Weight loss rate is 15% or more

[0169] [Water absorption] (Evaluation method) The cured film (coating) prepared on the glass substrate "EAGLE XG" was left to stand at a constant temperature and humidity of 40°C and 90% for 24 hours, then scraped off with a scraper or similar, and the thermal weight loss of 10 mg of the resulting powder-like cured film (coating) was measured using a differential thermal thermogravimetry (TG / DTA) "EXSTAR6000". The measurement conditions were: in a nitrogen atmosphere, the temperature was raised to 120°C at 10°C / min, and held for 1 hour. Water absorption was evaluated from the weight loss rate.

[0170] (Evaluation Criteria) ○: Weight loss rate is less than 2% △: Weight loss rate is 2% or more and less than 5% ×: Weight loss rate is 5% or more

[0171] [Development characteristics] (Preparation of evaluation samples) The photosensitive resin composition shown in Table 1 was applied to a 125 mm × 125 mm glass substrate "EAGLE XG" using a spin coater so that the film thickness after heat curing would be 1.5 μm, and the substrate was prebaked at 90 °C for 1 minute using a hot plate. After that, a photomask was placed so that the exposure gap was 150 μm, and the illuminance of the 365 nm wavelength was 30 mW / cm 2 100mJ / cm 2 The exposed portion was exposed to ultraviolet light for a photo-curing reaction.

[0172] Next, the exposed cured film (coating film) was developed with 0.05% potassium hydroxide aqueous solution or 0.2% sodium carbonate aqueous solution at 23°C under a pressure of 0.1 MPa for 60 seconds, and further washed with water to remove the unexposed part of the cured film (coating film). After that, a heat curing treatment was performed at 230°C for 30 minutes using a hot air dryer to obtain the cured films (patterns) according to Examples 1 to 10 and Comparative Examples 1 and 2.

[0173] (Evaluation method and criteria) The formation of fine lines in the obtained pattern was confirmed using an optical microscope and evaluated according to the following three levels. ○: Patterns with L / S of 15μm / 15μm or more are formed without residue △: A pattern with an L / S of 30 μm / 30 μm or more is formed without any residue. ×: No pattern with L / S less than 50μm / 50μm is formed, or pattern bottoming or residue is noticeable

[0174] [Table 2]

[0175] [Example 2] Photosensitive resin compositions containing light-shielding pigment dispersions of Examples 11 to 16 and Comparative Examples 11 to 13 were prepared by mixing the components (A) to (E) and the surfactant in the ratios shown in Table 3. (D)-1 in the solvent column is the amount excluding PGMEA (same as (D)-1) in the unsaturated group-containing resin solution (polymerizable unsaturated group-containing alkali-soluble resin solution), the solvent in the light-shielding pigment dispersion, and the solvent in the surfactant. Note that all values ​​in Table 3 are in mass %.

[0176] (Light-blocking pigment dispersion) (E)-1: PGMEA dispersion (solid content 19.5%) containing 15.0% by mass of lactam black pigment and 4.5% by mass of polymer dispersant (E)-2: PGMEA dispersion (solid content 30.0%) of 25.0% by mass of resin-coated carbon-based black pigment and 5.0% by mass of polymer dispersant

[0177] [Table 3]

[0178] [evaluation] The following evaluations were carried out using the photosensitive resin compositions of Examples 11 to 16 and Comparative Examples 11 to 13. The evaluation results are shown in Table 4.

[0179] [Optical density measurement] The photosensitive resin composition shown in Table 3 was applied onto a 125 mm x 125 mm glass substrate using a spin coater so that the film thickness after heat curing treatment would be 1.1 μm, and prebaked at 90°C for 1 minute. Then, a heat curing treatment was performed at 230°C for 30 minutes using a hot air dryer, to obtain cured films (coatings) according to Examples 11 to 16 and Comparative Examples 11 to 13. Next, the optical density (OD) of the obtained cured films (coatings) was measured using a Macbeth transmission densitometer, and evaluated as the optical density per unit film thickness.

[0180] [Volume resistivity measurement] (Measurement method) Each photosensitive resin composition shown in Table 3 was applied to a portion of a 100 mm x 100 mm Cr-deposited glass substrate with a thickness of 1.2 mm except for the electrodes, so that the film thickness after heat curing treatment would be 3.5 μm, and the substrate was pre-baked at 90° C. for 1 minute. Then, a heat curing treatment was performed at 230° C. for 30 minutes using a hot air dryer, to obtain cured films (coatings) according to Examples 11 to 16 and Comparative Examples 11 to 13. Then, an aluminum electrode was formed on the cured film (coating) to prepare a substrate for measuring volume resistivity. Next, the volume resistivity was measured at applied voltages of 1 V to 10 V using an electrometer "6517A" (manufactured by Keithley). The measurements were performed under conditions of holding the voltage at each applied voltage for 60 seconds in 1 V steps.

[0181] [Measurement of dielectric constant] (Measurement method) Each photosensitive resin composition shown in Table 3 was applied to a portion of a 100 mm x 100 mm Cr-deposited glass substrate with a thickness of 1.2 mm except for the electrodes, so that the film thickness after heat curing treatment would be 3.5 μm, using a spin coater, and pre-baked at 90 ° C for 1 minute. Then, heat curing treatment was performed at 230 ° C for 30 minutes using a hot air dryer, and cured films (coating films) according to Examples 11 to 16 and Comparative Examples 11 to 13 were obtained. Then, aluminum electrodes were formed on the coating films to prepare substrates for measuring dielectric constant. Next, an electrometer "6517A type" was used to measure the electric capacitance at frequencies from 1 Hz to 100,000 Hz, and the dielectric constant was calculated from the electric capacitance.

[0182] [Gas generation] (Evaluation method) The cured film (coating) produced on the glass substrate "EAGLE XG" was scraped off with a scraper, etc., and the thermal weight loss of 10 mg of the resulting powder-like cured film (coating) was measured using a differential thermal analyzer (TG / DTA) "EXSTAR6000." The measurement conditions were as follows: pretreatment was performed at 120°C for 30 minutes in air, followed by holding at 230°C for 3 hours.

[0183] (Evaluation Criteria) ◎: Weight loss rate is less than 3% ○: Weight loss rate is 3% or more and less than 7% △: Weight loss rate is 7% or more and less than 10% ×: Weight loss rate is 10% or more

[0184] [Measurement of elastic recovery rate of spacer] (Measurement method) Each photosensitive resin composition shown in Table 3 was applied onto a 125 mm × 125 mm glass substrate "EAGLE XG" using a spin coater so that the film thickness after heat curing would be 3.0 μm, and the substrate was prebaked at 90 °C for 1 minute. A photomask having a dot pattern was then attached to the substrate, and a 500 W high-pressure mercury lamp was used to apply a 365 nm wavelength, 30 mW / cm illuminance to the substrate. 2 100mJ / cm2 ultra-high pressure mercury lamp 2 The exposed portion was exposed to ultraviolet light for a photo-curing reaction.

[0185] Next, the exposed glass substrate was developed using a 0.05% potassium hydroxide aqueous solution at 24°C and a pressure of 0.1 MPa for 60 seconds to remove the unexposed portion of the cured film (coating). Then, a heat curing treatment was performed at 230°C for 30 minutes using a hot air dryer to obtain the cured films (coatings) according to Examples 11 to 16 and Comparative Examples 11 to 13. The spacer characteristics of the obtained cured film (coating) pattern were evaluated using an ultra-microhardness tester "Fisherscope HM2000Xyp" (manufactured by Fisher Instruments). A 100 μm square flat indenter was pressed at a loading speed of 5.0 mN / sec, a load was applied up to 50 mN, and then the load was removed at a loading speed of 5.0 mN / sec to create a displacement curve.

[0186] The elastic recovery rate was calculated from the following formula (2) using the displacement amount at a load of 50 mN when loaded as L1 and the displacement amount at the time of unloading as L2. Elastic recovery rate (%) = (L1-L2) / L1 × 100 (2)

[0187] [Development characteristics] (Preparation of evaluation samples) The photosensitive resin composition shown in Table 3 was applied to a 125 mm × 125 mm glass substrate "EAGLE XG" using a spin coater so that the film thickness after heat curing treatment would be 1.5 μm, and the substrate was prebaked at 90 °C for 1 minute using a hot plate. After that, a photomask was placed so that the exposure gap was 150 μm, and the illuminance of the 365 nm wavelength was 30 mW / cm 2 100mJ / cm 2 The exposed portion was exposed to ultraviolet light for a photo-curing reaction.

[0188] Next, the exposed cured film (coating film) was developed with 0.05% potassium hydroxide aqueous solution or 0.2% sodium carbonate aqueous solution at 23°C under a pressure of 0.1 MPa for 60 seconds, and further washed with water to remove the unexposed part of the cured film (coating film). Thereafter, a heat curing treatment was performed at 230°C for 30 minutes using a hot air dryer to obtain the cured films (patterns) according to Examples 11 to 16 and Comparative Examples 11 to 13.

[0189] (Evaluation method and criteria) The formation of fine lines in the obtained pattern was confirmed using an optical microscope and evaluated according to the following three levels. ○: Patterns with L / S of 15μm / 15μm or more are formed without residue △: A pattern with an L / S of 30 μm / 30 μm or more is formed without any residue. ×: No pattern with L / S less than 50μm / 50μm is formed, or pattern bottoming or residue is noticeable

[0190] [Table 4]

[0191] A photosensitive resin composition was obtained that can provide a cured film having high light-shielding and insulating properties, excellent adhesion to a substrate, and excellent elastic modulus, deformation amount, and elastic recovery rate. [Industrial Applicability]

[0192] The cured film of the photosensitive resin composition of the present invention is extremely useful as a component of color filters including organic EL devices, quantum dot displays, TFT arrays, and wavelength conversion devices, etc. In addition, the resin composition having a bisnaphtholfluorene skeleton is useful because it functions as a light transmission control layer that blocks ultraviolet light in a specific range.

Claims

1. The following components (A) to (D): (A) a polymerizable unsaturated group-containing alkali-soluble resin represented by general formula (1), (B) a (meth)acrylic acid ester selected from the group consisting of trimethylolpropane trimethacrylate, trimethylolethane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, sorbitol penta(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, sorbitol hexa(meth)acrylate, alkylene oxide-modified hexa(meth)acrylate of phosphazene, and caprolactone-modified dipentaerythritol hexa(meth)acrylate; (C) a photopolymerization initiator; and (D) a solvent; as an essential component, with the proviso that no o-naphthoquinone diazide sulfonic acid ester is contained, and the component (A) is a compound in which Ar in general formula (1) contains a naphthalene skeleton. 【Chemistry 1】 In formula (1), each Ar is independently an aromatic hydrocarbon group having 6 to 14 carbon atoms, and a portion of the bonded hydrogen atom may be substituted with an alkyl group having 1 to 10 carbon atoms, an aryl group or an arylalkyl group having 6 to 10 carbon atoms, a cycloalkyl group or a cycloalkylalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or a halogen group. R 1 are each independently an alkylene group having 2 to 4 carbon atoms, and each 1 is independently a number from 0 to 3. Each G is independently a substituent represented by general formula (2) or general formula (3), and Y is a tetravalent carboxylic acid residue. Each Z is independently a hydrogen atom or a substituent represented by general formula (4), and at least one Z is a substituent represented by general formula (4). n is a number having an average value of 1 to 20. 【Chemistry 2】 【Chemistry 3】 (In formulas (2) and (3), R 2 is a hydrogen atom or a methyl group, R 3 is a divalent alkylene or alkylarylene group having 2 to 10 carbon atoms; R 4 is a divalent saturated or unsaturated hydrocarbon group having 2 to 20 carbon atoms, and p is a number from 0 to 10. 【Chemistry 4】 (In formula (4), W is a divalent or trivalent carboxylic acid residue, and m is 1 or 2.)

2. 2. The photosensitive resin composition according to claim 1, wherein a content of the component (A) is 10 to 90% by mass based on the total mass of the solid contents, a content of the component (B) is 5 to 200 parts by mass based on 100 parts by mass of the component (A), and a content of the component (C) is 0.1 to 30 parts by mass based on 100 parts by mass of the combined amount of the component (A) and the component (B).

3. The photosensitive resin composition according to claim 1 , further comprising (E) a colorant.

4. 4. The photosensitive resin composition according to claim 3, wherein the colorant (E) is one or more light-shielding components selected from the group consisting of black organic pigments, mixed-color organic pigments, and light-shielding materials.

5. 5. The photosensitive resin composition according to claim 3, wherein the content of the component (E) is 1 to 80 mass % based on the total mass of the solid content of the photosensitive resin composition.

6. A cured film obtained by curing the photosensitive resin composition according to any one of claims 1 to 5.

7. A display device comprising the cured film according to claim 6.

Citation Information

Patent Citations

  • Photosensitive Resin Composition Used For Black Matrix And Application Thereof

    CN106918994A

  • Alkali-soluble resin, method for producing the same, and photosensitive resin composition prepared by using the same

    JP2010229173A