All-solid secondary battery

By integrating metal particles with oxide films in the battery structure, the issue of non-uniform heat dissipation in all-solid-state secondary batteries is addressed, resulting in improved thermal uniformity and cycle characteristics.

JP7568509B2Active Publication Date: 2024-10-16TDK CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020557782
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-11-30
Filing Date
2019-11-27
Publication Date
2024-10-16
Estimated Expiration
2039-11-27

AI Technical Summary

Technical Problem

All-solid-state secondary batteries face issues with non-uniform heat dissipation due to low thermal conductivity, leading to uneven temperature distribution and accelerated deterioration in high-temperature parts, which affects lithium ion movement and cycle characteristics.

Method used

Incorporation of metal particles with an oxide film in the battery structure, specifically in the positive and negative electrode layers and the solid electrolyte layers, to enhance heat dissipation and uniformity, using materials like copper, nickel, silver, platinum, iron, aluminum, and palladium, with controlled particle size and thickness.

Benefits of technology

The solution results in improved heat dissipation uniformity and lithium ion movement, enhancing the battery's cycle characteristics and reducing the risk of short circuits while maintaining high capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568509000006
    Figure 0007568509000006
  • Figure 0007568509000001
    Figure 0007568509000001
  • Figure 0007568509000002
    Figure 0007568509000002
Patent Text Reader

Abstract

Provided is an all-solid-state secondary battery that has high uniformity in dissipating heat generated by the battery reaction. The all-solid-state lithium-ion secondary battery (100) includes a positive electrode layer (1) including a positive electrode current collector layer (1A) and a positive electrode active material layer (1B), a negative electrode layer (2) including a negative electrode current collector layer (2A) and a negative electrode active material layer (2B), a solid electrolyte layer (3) including a solid electrolyte, and margin layers (4) including a solid electrolyte arranged alongside the positive electrode layer (1) and the negative electrode layer (2), respectively, and also includes a laminate (5) in which the positive electrode layer (1) and the negative electrode layer (2) are alternately stacked with the solid electrolyte layer (3) including the solid electrolyte interposed therebetween, and the laminate (5) includes metal particles (10) having an oxide coating in the positive electrode active material layer (1B), the negative electrode active material layer (2B), the solid electrolyte layer (3), and the margin layer (4).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an all-solid-state secondary battery. This application claims priority based on Japanese Patent Application No. 2018-225662, filed on November 30, 2018, the contents of which are incorporated herein by reference. [Background technology]

[0002] In recent years, electronics technology has made remarkable progress, and portable electronic devices have become smaller, lighter, thinner, and more multifunctional. Accordingly, there is a strong demand for batteries that serve as the power source for these electronic devices to be smaller, lighter, thinner, and more reliable, and all-solid-state lithium-ion secondary batteries made of solid electrolytes have attracted attention.

[0003] Generally, all-solid-state lithium-ion secondary batteries are classified into two types: thin-film and bulk. Thin-film batteries are produced using thin-film techniques such as the PVD method and the sol-gel method, while bulk batteries are produced by powder molding of active materials and sulfide-based solid electrolytes with low grain boundary resistance. However, thin-film batteries have problems such as low capacity and high manufacturing costs because it is difficult to thicken the active material layer or to stack them highly.

[0004] On the other hand, the bulk type uses a sulfide-based solid electrolyte, which generates hydrogen sulfide when it reacts with water, making it difficult to handle in the atmosphere, and therefore the batteries had to be manufactured in a glove box where the dew point was controlled. In addition, because it is difficult to make a sheet, there are challenges in making the solid electrolyte layer thinner and increasing the number of layers in the battery.

[0005] For oxide-based solid electrolytes that are chemically stable in the atmosphere, the manufacturing method of a laminated capacitor can be applied, and for example, a laminated all-solid-state secondary battery can be manufactured by laminating a positive electrode layer consisting of a positive electrode active material layer and a positive electrode current collector layer, a solid electrolyte layer, and a negative electrode layer consisting of a negative electrode active material layer and a negative electrode current collector layer. For example, a slurry in which the constituent materials of each component are kneaded with a binder and a solvent is applied by screen printing or a doctor blade method, processed into sheets, laminated, and fired to manufacture a laminated all-solid-state secondary battery (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2014-192041 A [Patent Document 2] JP 2009-181905 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, because the thermal conductivity of the materials that make up the all-solid-state secondary battery is low, the heat generated by the battery reaction cannot be dissipated uniformly. Therefore, the internal temperature of a stacked all-solid-state secondary battery with a large number of stacked layers is likely to be uneven from the battery surface temperature. Therefore, the migration speed of lithium ions inside the battery differs between high-temperature and low-temperature parts, and the migration of lithium ions is particularly promoted in the high-temperature part, which causes a problem of accelerated deterioration of the battery in the high-temperature part. As a result, it is difficult to obtain excellent cycle characteristics.

[0008] In regard to the problem of heat dissipation of such all-solid-state secondary batteries, Patent Document 2 reports that the above problem can be solved by forming a layer having voids of 50 vol% or more on the current collectors formed on both the positive and negative electrodes. However, in the all-solid-state secondary battery in which the layer having voids is formed, there is a problem that electronic conductivity is reduced and it is difficult to obtain a desired charge / discharge capacity.

[0009] An object of the present invention is to provide an all-solid-state secondary battery that has high uniformity in dissipating heat generated by a battery reaction. [Means for solving the problem]

[0010] In order to solve the above problems, the present invention provides the following means.

[0011] (1) An all-solid-state secondary battery according to an aspect of the present invention includes a positive electrode layer including a positive electrode current collector layer and a positive electrode active material layer, a negative electrode layer including a negative electrode current collector layer and a negative electrode active material layer, a solid electrolyte layer including a solid electrolyte, and a margin layer including a solid electrolyte arranged alongside each of the positive electrode layer and the negative electrode layer, and further includes a laminate in which the positive electrode layer and the negative electrode layer are alternately stacked with the solid electrolyte layer interposed therebetween, and the laminate includes metal particles having an oxide coating in at least any of the positive electrode active material layer, the negative electrode active material layer, the solid electrolyte layer, and the margin layer.

[0012] (2) In the all-solid-state secondary battery described in (1) above, metal particles having the oxide film may be provided on both ends of the surface of the laminate in the lamination direction.

[0013] (3) In the all-solid-state secondary battery according to either of (1) or (2) above, the metal particles having the oxide film may have an average particle size of 0.1 μm to 20 μm.

[0014] (4) In the all-solid-state secondary battery according to any one of (1) to (3) above, the average thickness of the oxide film may be 10% or less of the average particle diameter of the metal particles and may be in the range of 0.001 μm to 2 μm.

[0015] (5) In the all-solid-state secondary battery according to any one of (1) to (4) above, the metal particles may contain at least one selected from copper, nickel, silver, platinum, iron, aluminum, bismuth, and palladium.

[0016] (6) In the all-solid-state secondary battery according to any one of (1) to (5) above, the metal particles may be contained in an amount of 0.1 to 10% by weight based on the weight of the all-solid-state secondary battery. Effect of the Invention

[0017] According to the present invention, it is possible to provide an all-solid-state secondary battery that has high uniformity in dissipating heat generated by a battery reaction. [Brief description of the drawings]

[0018] [Figure 1] FIG. 2 is an enlarged cross-sectional view illustrating a main part of the all-solid-state secondary battery according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present embodiment will be described in detail below with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the characteristics of the present embodiment easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present embodiment is not limited to them. They can be modified as appropriate within the scope of the effects of the present invention.

[0020] Examples of all-solid-state secondary batteries include all-solid-state lithium ion secondary batteries, all-solid-state sodium ion secondary batteries, all-solid-state magnesium ion secondary batteries, etc. In the following, an all-solid-state lithium ion secondary battery will be described as an example, but the present invention is generally applicable to all-solid-state secondary batteries.

[0021] FIG. 1 is an enlarged cross-sectional view that illustrates a schematic view of a main portion of an all-solid-state lithium-ion secondary battery according to this embodiment. The all-solid-state lithium-ion secondary battery shown in FIG. 1 includes a laminate having a first electrode layer, a second electrode layer, and a solid electrolyte. Hereinafter, one of the first electrode layer and the second electrode layer functions as a positive electrode, and the other functions as a negative electrode. The positive and negative polarities of the electrode layers change depending on which polarity is connected to the external terminal. In the following, for ease of understanding, the first electrode layer will be described as a positive electrode layer, and the second electrode layer as a negative electrode layer.

[0022] The all-solid-state lithium-ion secondary battery 100 includes a positive electrode layer 1 including a positive electrode current collector layer 1A and a positive electrode active material layer 1B, a negative electrode layer 2 including a negative electrode current collector layer 2A and a negative electrode active material layer 2B, a solid electrolyte layer 3 including a solid electrolyte, and a margin layer 4 including a solid electrolyte arranged alongside each of the positive electrode layer 1 and the negative electrode layer 2, and also includes a laminate 5 in which the positive electrode layer 1 and the negative electrode layer 2 are alternately laminated with the solid electrolyte layer 3 including the solid electrolyte interposed therebetween, and the laminate 5 includes metal particles 10 having an oxide coating in the positive electrode active material layer 1B, the negative electrode active material layer 2B, the solid electrolyte layer 3, and the margin layer 4.

[0023] The positive electrode layers 1 are each connected to a first external terminal 6, and the negative electrode layers 2 are each connected to a second external terminal 7. The first external terminal 6 and the second external terminal 7 are electrical contacts with the outside.

[0024] (Laminate) The laminate 5 includes a positive electrode layer 1, a negative electrode layer 2, a solid electrolyte layer 3, a margin layer 4, and metal particles 10 having an oxide film.

[0025] In the laminate 5, the positive electrode layers 1 and the negative electrode layers 2 are alternately laminated with the solid electrolyte layers 3 (more specifically, the interlayer solid electrolyte layers 3A) interposed therebetween. The all-solid-state lithium-ion secondary battery 100 is charged and discharged by the exchange of lithium ions between the positive electrode layers 1 and the negative electrode layers 2 via the solid electrolyte layer 3.

[0026] (Positive and negative electrode layers) The positive electrode layer 1 has a positive electrode current collector layer 1A and a positive electrode active material layer 1B containing a positive electrode active material. The negative electrode layer 2 has a negative electrode current collector layer 2A and a negative electrode active material layer 2B containing a negative electrode active material.

[0027] The positive electrode collector layer 1A and the negative electrode collector layer 2A are made of at least one material having high electrical conductivity. Examples of the material having high electrical conductivity include metals or alloys containing at least one metal element selected from silver (Ag), palladium (Pd), gold (Au), platinum (Pt), aluminum (Al), copper (Cu), and nickel (Ni), and nonmetals such as carbon (C). Among these metal elements, copper and nickel are preferable in consideration of the manufacturing cost in addition to the high electrical conductivity. Furthermore, copper is difficult to react with the positive electrode active material, the negative electrode active material, and the solid electrolyte. Therefore, when copper is used for the positive electrode collector layer 1A and the negative electrode collector layer 2A, the internal resistance of the all-solid-state lithium-ion secondary battery 100 can be reduced. The materials constituting the positive electrode collector layer 1A and the negative electrode collector layer 2A may be the same or different. There are no limitations on the thickness of the positive electrode current collector layer 1A and the negative electrode current collector layer 2A, but as a guideline, for example, it is in the range of 0.5 μm to 30 μm.

[0028] The positive electrode active material layer 1B is formed on one or both sides of the positive electrode collector layer 1A. For example, the positive electrode layer 1 located at the top of the stacking direction of the all-solid-state lithium-ion secondary battery 100 does not have the negative electrode layer 2 facing it on the upper side of the stacking direction. Therefore, in the positive electrode layer 1 located at the top of the all-solid-state lithium-ion secondary battery 100, the positive electrode active material layer 1B may be formed only on one side of the lower side of the stacking direction, but there is no particular problem even if it is formed on both sides. The negative electrode active material layer 2B is also formed on one or both sides of the negative electrode collector layer 2A, similar to the positive electrode active material layer 1B. The thickness of the positive electrode active material layer 1B and the negative electrode active material layer 2B is preferably in the range of 0.5 μm to 5.0 μm. By making the thickness of the positive electrode active material layer 1B and the negative electrode active material layer 2B 0.5 μm or more, the electric capacity of the all-solid-state lithium ion secondary battery can be increased, while by making the thickness 5.0 μm or less, the diffusion distance of lithium ions is shortened, and therefore the internal resistance of the all-solid-state lithium ion secondary battery can be further reduced.

[0029] The positive electrode active material layer 1B and the negative electrode active material layer 2B each contain a positive electrode active material or a negative electrode active material that donates and receives electrons to and from lithium ions. In addition, they may contain a conductive assistant, a conductive ion assistant, etc. It is preferable that the positive electrode active material and the negative electrode active material can efficiently insert and extract lithium ions.

[0030] There is no clear distinction between the active materials constituting the positive electrode active material layer 1B and the negative electrode active material layer 2B, and by comparing the potentials of two types of compounds, a compound showing a more noble potential can be used as the positive electrode active material, and a compound showing a more base potential can be used as the negative electrode active material. Therefore, the active materials will be collectively described below.

[0031] The active material may be a transition metal oxide, a transition metal composite oxide, or the like. For example, the transition metal oxide or transition metal composite oxide may be a lithium manganese composite oxide, Li 2 Mn a Ma 1-a O 3 (0.8≦a≦1, Ma=Co, Ni), lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), Lithium Manganese Spinel (LiMn 2 O 4 ), general formula: LiNi x Co y Mn z O 2 A composite metal oxide represented by (x+y+z=1, 0≦x≦1, 0≦y≦1, 0≦z≦1), a lithium vanadium compound (LiV 2 O 5 ), olivine-type LiM b PO 4 (However, M b is one or more elements selected from Co, Ni, Mn, Fe, Mg, Nb, Ti, Al, and Zr), lithium vanadium phosphate (Li 3 V 2 (PO 4 ) 3 or LiVOPO 4 ), Li 2 MnO 3 -LiM c O 2 (Mc = Mn, Co, Ni) - based Li - excess solid - solution cathode, lithium titanate (Li 4 Ti 5 O 12 ), Li s Ni t Co u Al v O 2 (0.9 < s < 1.3, 0.9 < t + u + v < 1.1), and composite metal oxides represented thereby, etc. are exemplified. Further, in addition to the above - mentioned composite metal oxides, Li metal, Li - Al alloy, Li - In alloy, carbon, silicon (Si), silicon oxide (SiO x ), titanium oxide (TiO 2 ), and other metals, alloys, and metal oxides are exemplified.

[0032] As the active material of this embodiment, it is preferably contained mainly composed of a phosphate compound. For example, lithium vanadium phosphate (LiVOPO 4 , Li 3 V 2 (PO 4 ) 3 , Li 4 (VO)(PO 4 ) 2) , lithium vanadium pyrophosphate (Li 2 VOP 2 O 7 , Li 2 VP 2 O 7) , and Li 9 V 3 (P 2 O 7 ) 3 (PO 4 ) 2 , and it is preferably any one or more of them. In particular, it is preferably one or both of LiVOPO 4 and Li 3 V 2 (PO 4 ) 3 .

[0033] In this embodiment, the main component refers to a phosphate compound that accounts for more than 50 parts by mass, and preferably 80 parts by weight or more, of the entire active material in the active material layer.

[0034] In addition, these active materials may have some of the elements substituted with different elements, or may be deviated from the stoichiometric composition. 4 and Li 3 V 2 (PO 4 ) 3 It is preferable that there is a lithium deficiency in Li x VOPO 4 (0.94≦x≦0.98) and Li x V 2 (PO 4 ) 3 It is more preferable if (2.8≦x≦2.95).

[0035] Examples of the conductive assistant include carbon materials such as carbon black, acetylene black, ketjen black, carbon nanotubes, graphite, graphene, and activated carbon, and metal materials such as gold, silver, palladium, platinum, copper, and tin.

[0036] The ion-conducting assistant is, for example, a solid electrolyte. Specifically, for example, the same material as that used for the solid electrolyte layer 3 can be used as the solid electrolyte.

[0037] When a solid electrolyte is used as the ion-conducting assistant, it is preferable that the ion-conducting assistant and the solid electrolyte used in the solid electrolyte layer 3 are made of the same material.

[0038] The positive electrode current collector layer 1A and the negative electrode current collector layer 2A may contain a positive electrode active material and a negative electrode active material, respectively. The content ratio of the active materials contained in each current collector is not particularly limited as long as it functions as a current collector. For example, the volume ratio of the positive electrode current collector / positive electrode active material or the negative electrode current collector / negative electrode active material is preferably in the range of 90 / 10 to 70 / 30.

[0039] The positive electrode current collector layer 1A and the negative electrode current collector layer 2A each contain a positive electrode active material and a negative electrode active material, thereby improving adhesion between the positive electrode current collector layer 1A and the positive electrode active material layer 1B, and between the negative electrode current collector layer 2A and the negative electrode active material layer 2B.

[0040] (Solid electrolyte layer) As shown in FIG. 1, the solid electrolyte layer 3 has an interlayer solid electrolyte layer 3A located between a positive electrode active material layer 1B and a negative electrode active material layer 2B. The solid electrolyte layer 3 may further include an outermost solid electrolyte layer 3B located on the outside of at least one of the positive electrode layer 1 (positive electrode current collector layer 1A) and the negative electrode layer 2 (negative electrode current collector layer 2A) (both in FIG. 1). Here, the "outside" refers to the outside of the positive electrode layer 1 or the negative electrode layer 2 closest to the surfaces 5A, 5B of the laminate 5. The solid electrolyte layer 3 does not necessarily have to have the outermost solid electrolyte layer 3B. In this case, the surfaces 5A, 5B of the laminate 5 become the positive electrode layer 1 and the negative electrode layer 2.

[0041] For the solid electrolyte layer 3, it is preferable to use a solid electrolyte material with low electronic conductivity and high lithium ion conductivity. For example, general solid electrolyte materials such as oxide-based lithium ion conductors having a Nasicon-type, garnet-type, or perovskite-type crystal structure can be used. Examples of lithium ion conductors having a Nasicon-type crystal structure include ion conductors having a Nasicon-type crystal structure containing at least Li, M (M is at least one of Ti, Zr, Ge, Hf, and Sn), P, and O, ion conductors having a garnet-type crystal structure containing at least Li, Zr, La, and O, or ion conductors having a garnet-type similar structure, and at least one ion conductor having a perovskite-type structure containing at least Li, Ti, La, and O. In other words, these ion conductors may be used alone or in combination of two or more.

[0042] As the solid electrolyte material of this embodiment, it is preferable to use a lithium ion conductor having a Nasicon type crystal structure, for example, LiTi 2 (PO 4) 3 (LTP), LiZr 2 (PO 4 ) 3 (LZP), Li 1+x Al x Ti 2-x (PO 4 ) 3 (LATP, 0 < x ≤ 0.6)), Li 1+x Al x Ge 2-x (PO 4 ) 3 (LAGP, 0 < x ≤ 0.6)), Li 1+x Y x Zr 2-x (PO 4 ) 3 (LYZP, 0 < x ≤ 0.6)) preferably contains a solid electrolyte material represented thereby.

[0043] Also, it is preferable to select the solid electrolyte layer 3 according to the active material used for the positive electrode layer 1 and the negative electrode layer 2. For example, it is more preferable that the solid electrolyte layer 3 contains the same element as the element constituting the active material. By the solid electrolyte layer 3 containing the same element as the element constituting the active material, the bonding at the interface between the positive electrode active material layer 1B and the negative electrode active material layer 2B and the solid electrolyte layer 3 becomes strong. Also, the contact area at the interface between the positive electrode active material layer 1B and the negative electrode active material layer 2B and the solid electrolyte layer 3 can be widened.

[0044] The thickness of the interlayer solid electrolyte layer 3A is preferably in the range of 0.5 μm or more and 20.0 μm or less. By setting the thickness of the interlayer solid electrolyte layer 3A to 0.5 μm or more, a short circuit between the positive electrode layer 1 and the negative electrode layer 2 can be surely prevented, and by setting the thickness to 20.0 μm or less, the migration distance of lithium ions becomes short, so that the internal resistance of the all-solid-state lithium ion secondary battery can be further reduced.

[0045] The thickness of the outermost solid electrolyte layer 3B is not particularly limited, but for example, it may be in the same thickness range as the interlayer solid electrolyte layer 3A, that is, 0.5 μm or more and 20.0 μm or less.

[0046] (Margin layer) Margin layer 4 contains a solid electrolyte, and is disposed next to each of positive electrode layer 1 and negative electrode layer 2. The solid electrolyte contained in margin layer 4 may be the same as or different from the solid electrolyte contained in solid electrolyte layer 3. The margin layer 4 is preferably provided to eliminate the step between the interlayer solid electrolyte layer 3A and the positive electrode layer 1, and the step between the interlayer solid electrolyte layer 3A and the negative electrode layer 2. Therefore, the margin layer 4 is formed in an area other than the positive electrode layer 1 and the negative electrode layer 2 on the main surface of the solid electrolyte layer 3, at approximately the same height as the positive electrode layer 1 or the negative electrode layer 2 (i.e., arranged alongside the positive electrode layer 1 and the negative electrode layer 2, respectively). The presence of the margin layer 4 eliminates the step between the solid electrolyte layer 3 and the positive electrode layer 1, and between the solid electrolyte layer 3 and the negative electrode layer 2, so that the density of the solid electrolyte layer 3 and each electrode layer is increased, and delamination and warping due to firing of the all-solid-state battery are less likely to occur.

[0047] The material constituting the margin layer 4 preferably contains, for example, lithium titanium aluminum phosphate, which is the same material as the solid electrolyte layer 3. Therefore, lithium titanium aluminum phosphate is Li 1+x Al x Ti 2-x (PO 4 ) 3 (0≦x≦0.6) is preferable. The solid electrolyte layer 3 may contain a solid electrolyte material other than lithium titanium aluminum phosphate. For example, Li 3+x1 S x1 P 1-x1 O 4 (0.4≦x1≦0.6), Li 3.4 V 0.4 Ge 0.6 O 4 , lithium germanium phosphate (LiGe 2 (PO 4 ) 3 ), Li 2 O.V. 2 O 5 -SiO 2 , Li 2 OP 2 O 5 -B 2 O 3 , Li3 PO 4 , Li 0.5 La 0.5 TiO 3 , Li 14 Zn(GeO 4 ) 4 , Li 7 La 3 Zr 2 O 12 It is preferable that the compound contains at least one selected from the group consisting of:

[0048] (Metal particles with oxide coating) The metal particles 10 having an oxide coating facilitate dissipation of heat generated by the battery reaction. As a result, the heat distribution in the all-solid-state secondary battery becomes uniform, and the uniformity of lithium ion movement due to the charge-discharge reaction is improved, resulting in excellent cycle characteristics.

[0049] Furthermore, the metal particles 10 having an oxide film have insulating properties and therefore do not short-circuit. In the case of metal particles without an oxide film, the insulating properties cannot be guaranteed and there is a possibility of short-circuiting.

[0050] In the all-solid-state lithium-ion secondary battery 100 shown in FIG. 1, the metal particles 10 having an oxide film are present in the positive electrode active material layer 1B, the negative electrode active material layer 2B, the solid electrolyte layer 3, and the margin layer 4, but it is sufficient for the metal particles 10 to be present in any one of the positive electrode active material layer 1B, the negative electrode active material layer 2B, the solid electrolyte layer 3, and the margin layer 4. In addition, when metal particles 10 having an oxide film are located at the interface between positive electrode active material layer 1B and solid electrolyte layer 3, or at the interface between negative electrode active material layer 2B and solid electrolyte layer 3, and straddle both layers, they are considered to be present in both layers. In order to improve the uniformity of heat dissipation, it is preferable that all of the positive electrode active material layer 1B, the negative electrode active material layer 2B, the solid electrolyte layer 3, and the margin layer 4 have metal particles 10 having an oxide film.

[0051] The all-solid-state lithium-ion secondary battery 100 shown in Fig. 1 further has metal particles 10 having an oxide film on surfaces 5A and 5B, which are both ends in the stacking direction of the laminate. The all-solid-state lithium-ion secondary battery 100 shown in Fig. 1 has metal particles 10 having an oxide film on both surfaces 5A and 5B of the laminate, but may have the metal particles 10 on only one side.

[0052] Metal particles 10 having an oxide film present on surfaces 5A and 5B of the laminate can suitably release heat generated by the battery reaction to the outside.

[0053] There are no particular limitations on the form in which the metal particles having an oxide film are present on the surface of the laminate, and the metal particles having an oxide film may be substantially entirely placed on the surface, or may be partially exposed from the surface.

[0054] The average particle size of the metal particles having an oxide film is preferably 0.1 μm to 20 μm. When the average particle size is 0.1 μm or more, the desired heat dissipation properties are obtained, and as a result, excellent cycle characteristics are obtained, and when the average particle size is 20 μm or less, the metal particles having an oxide film are easily dispersed uniformly in the all-solid-state secondary battery, and the desired heat dissipation properties are easily obtained.

[0055] A method for measuring the average particle size of metal particles having an oxide film will be described. (When metal particles having an oxide film are included inside the laminate of the all-solid-state secondary battery) In order to observe the metal particles having an oxide film inside the laminate of the all-solid-state secondary battery, for example, an arbitrary cross section is produced by ion milling or cross-section polisher (CP) processing, and the metal particles having an oxide film can be identified by, for example, backscattered electron imaging (COMPO), X-ray photoelectron spectroscopy (XPS), or electron probe microanalyzer (EPMA) analysis. Next, for example, by observation with a field emission scanning electron microscope (FE-SEM), the diameter of the metal particles having an oxide film is measured by the distance between any two points, and the average particle diameter of the metal particles having an oxide film can be calculated from a predetermined number of measurement points, for example, n=20.

[0056] (When the all-solid-state secondary battery contains metal particles having an oxide film on the surface of both ends in the stacking direction of the stack) In order to observe metal particles having an oxide film on the surfaces of both ends in the stacking direction of the laminate of the all-solid-state secondary battery, the metal particles having an oxide film are identified, for example, by analysis using COMPO, XPS, or EPMA, and then the diameter of the metal particles having an oxide film is measured by the distance between any two points, for example, by FE-SEM observation, and the average particle size of the metal particles can be calculated from a predetermined number of measurement points, for example, n=20. In addition, since the metal particles present on the surface of the all-solid-state secondary battery have a gloss, they can be easily identified using a microscope (stereo microscope), and the average particle size may be calculated using a similar method.

[0057] The average thickness of the oxide film is preferably 10% or less of the average particle diameter of the metal particles having the oxide film, and is within the range of 0.001 μm to 2 μm. When the average thickness of the oxide film is 10% or less of the average particle size of the metal particles having the oxide film, the metal particles have excellent heat dissipation while maintaining their insulating properties. When the thickness of the oxide film is 0.001 μm or more, the insulating properties can be ensured and short circuits can be prevented. When the average thickness of the oxide film is 2 μm or less, the insulating properties can be ensured while preventing a decrease in the heat dissipation properties of the metal particles. By "average thickness" is meant the average thickness of the oxide layer measured on each of a given number, for example 20, of the metal particles.

[0058] The thickness of the oxide film of the metal particles can be measured, for example, by a depth profile of XPS. In the present invention, the term "oxide film" is a general term for metal oxides. For example, when the metal particles are Cu particles, the thickness of the oxide film of Cu 2 O, CuO, CuCO 3 , Cu(OH) 2 etc.

[0059] The material of the metal particles preferably contains at least one selected from copper, nickel, silver, platinum, iron, aluminum, bismuth, and palladium. Copper, nickel, silver, platinum, iron, aluminum, bismuth, and palladium have excellent heat dissipation properties, and therefore can provide an all-solid-state secondary battery with excellent cycle characteristics.

[0060] The metal particles are preferably contained in an amount of 0.1 to 20% by weight based on the weight of the all-solid-state secondary battery. When the metal particles are 0.1% by weight or more relative to the weight of the all-solid-state secondary battery, the battery has excellent heat dissipation properties and therefore excellent cycle characteristics.When the metal particles are 20% by weight or less, the battery's internal resistance can be reduced, resulting in excellent cycle characteristics, and the decrease in the composition ratio of the active material can be suppressed, allowing the battery to be designed with a high capacity.

[0061] A method for calculating the content of metal particles contained in an all-solid-state secondary battery will be described taking as an example a case in which the metal particles are Cu particles. Chips of an all-solid-state secondary battery are crushed and dissolved by heating in an acid solution. This is then adjusted to a predetermined volume and further diluted to a predetermined ratio to obtain a measurement sample (n=4). The measurement sample is measured for the Cu content of the measurement sample (n=4) using an inductively coupled plasma emission spectrometer (Shimadzu Corporation, ICPS-8100CL), and the average value is regarded as the Cu content. Here, in order to exclude the Cu content contained in the current collector layer, the Cu content in the region other than the current collector layer is calculated by subtracting the Cu content of an all-solid-state secondary battery to which no Cu particles including an oxide film were added.

[0062] (Terminal) It is preferable to use a material with high electrical conductivity for the first external terminal 6 and the second external terminal 7 of the all-solid-state lithium-ion secondary battery 100. For example, silver (Ag), gold (Au), platinum (Pt), aluminum (Al), copper (Cu), tin (Sn), nickel (Ni), and chromium (Cr) can be used. The terminals may be single-layered or multi-layered.

[0063] (protective layer) The all-solid-state lithium-ion secondary battery 100 may also have a protective layer (not shown) on the outer periphery of the laminate 5 for electrically, physically, and chemically protecting the laminate 5 and the terminals. The material constituting the protective layer is preferably excellent in insulation, durability, and moisture resistance, and is environmentally safe. For example, it is preferable to use glass, ceramics, thermosetting resin, or photocurable resin. The protective layer may be made of one type of material, or a combination of two or more types of materials. The protective layer may be a single layer, but it is preferable to have a plurality of layers. Among them, an organic-inorganic hybrid in which a thermosetting resin and ceramic powder are mixed is particularly preferable.

[0064] (Manufacturing method of all-solid-state lithium-ion secondary battery) The all-solid-state lithium-ion secondary battery 100 may be manufactured by a co-firing method or a sequential firing method. The co-firing method is a method in which materials for forming each layer are stacked and a laminate is manufactured by simultaneous firing. The sequential firing method is a method in which each layer is manufactured in order, and a firing step is inserted after each layer is manufactured. The co-firing method can reduce the number of work steps for the all-solid-state lithium-ion secondary battery 100. Furthermore, the co-firing method makes the obtained laminate 5 denser. The case in which the co-firing method is used will be described below as an example.

[0065] The co-firing method includes a step of preparing a paste of each material that constitutes the laminate 5, a step of applying and drying the paste to prepare a green sheet, a step of stacking the green sheets, and a step of co-firing the prepared laminate sheet.

[0066] First, the materials constituting the laminate 5, that is, the positive electrode collector layer 1A, the positive electrode active material layer 1B, the solid electrolyte layer 3, the negative electrode active material layer 2B, the negative electrode collector layer 2A, and the margin layer 4, are made into a paste.

[0067] The method of making the paste is not particularly limited. For example, the powder of each material is mixed with a vehicle to obtain a paste. Here, the vehicle is a general term for a medium in a liquid phase. The vehicle includes a solvent and a binder. By this method, a paste for the positive electrode collector layer 1A, a paste for the positive electrode active material layer 1B, a paste for the solid electrolyte layer 3, a paste for the negative electrode active material layer 2B, a paste for the negative electrode collector layer 2A, and a paste for the margin layer 4 are prepared.

[0068] The method for producing metal particles having an oxide film is not particularly limited. For example, the metal particles are heat-treated at a temperature of 200 to 400° C. in air, H 2 O+N 2 , or O 2 The oxide film formed on the surface of the metal particles can be confirmed by, for example, XPS. If an oxide film with a desired thickness cannot be obtained by a single oxidation treatment, the heat treatment temperature, heat treatment time, and number of heat treatments can be adjusted to obtain metal particles with the desired oxide film. The obtained metal particles having an oxide film can be mixed with one or more of the pastes for the positive electrode current collector layer 1A, the paste for the positive electrode active material layer 1B, the paste for the solid electrolyte layer 3, the paste for the negative electrode active material layer 2B, the paste for the negative electrode current collector layer 2A, and the paste for the margin layer 4 to obtain one or more pastes containing the metal particles having an oxide film. The metal particles having an oxide film are added in a manner that adjusts the content thereof in advance to a desired amount relative to the weight of the all-solid-state secondary battery after firing.

[0069] Next, a green sheet is prepared. The green sheet is obtained by applying the prepared paste onto a substrate such as PET (polyethylene terephthalate) in a desired order, drying as necessary, and then peeling off the substrate. The method of applying the paste is not particularly limited. For example, known methods such as screen printing, application, transfer, doctor blade, etc. can be adopted.

[0070] When producing the laminate 5, a positive electrode unit and a negative electrode unit described below are prepared, and the laminate can be produced.

[0071] First, the paste for the solid electrolyte layer 3 is formed into a sheet shape on a PET film by a doctor blade method, and then dried to form a solid electrolyte layer sheet. On the obtained solid electrolyte layer sheet, the paste for the positive electrode active material layer 1B is printed by screen printing and dried to form the positive electrode active material layer 1B.

[0072] Next, the paste for the positive electrode collector layer 1A is printed on the prepared positive electrode active material layer 1B by screen printing and dried to form the positive electrode collector layer 1A. The paste for the positive electrode active material layer 1B is printed again on the positive electrode collector layer 1A by screen printing and dried. Then, the paste for the margin layer is screen printed on the area of ​​the solid electrolyte layer sheet other than the positive electrode layer and dried to form a margin layer having a height approximately equal to that of the positive electrode layer. Then, the PET film is peeled off to obtain a positive electrode unit in which the positive electrode layer 1, in which the positive electrode active material layer 1B / positive electrode collector layer 1A / positive electrode active material layer 1B are laminated in this order, and the margin layer 4 is formed on the main surface of the solid electrolyte layer 3.

[0073] Using a similar procedure, a negative electrode unit is obtained in which the negative electrode layer 2 and the margin layer 4 are formed on the main surface of the solid electrolyte layer 3, and the negative electrode layer 2 is formed by laminating the negative electrode active material layer 2B / negative electrode current collector layer 2A / negative electrode active material layer 2B in this order.

[0074] The positive electrode units and the negative electrode units are alternately stacked with an offset such that one end of each unit does not coincide with the other, to produce a stack of an all-solid-state battery. Note that for the positive electrode units or the negative electrode units arranged at both ends of the stack in the stacking direction of the stack, the outermost solid electrolyte layer 3B is used as the solid electrolyte layer 3, and for the positive electrode units or the negative electrode units arranged therebetween, the interlayer solid electrolyte layer 3A is used as the solid electrolyte layer 3.

[0075] The above-described manufacturing method is for producing a parallel-type all-solid-state battery, but in a manufacturing method for a series-type all-solid-state battery, one end of the positive electrode layer 1 and one end of the negative electrode layer 2 may be stacked so as to coincide with each other, that is, without offsetting.

[0076] When it is desired to produce an all-solid-state secondary battery having a configuration in which metal particles having an oxide film are not provided on the surfaces of both ends in the stacking direction of the laminate, the outermost solid electrolyte layer paste should not contain metal particles having an oxide film.

[0077] Furthermore, the produced laminate can be pressed collectively using a mold press, hot isostatic press (WIP), cold isostatic press (CIP), isostatic press, etc. Pressing is preferably performed while heating, and can be performed at, for example, 40 to 95°C.

[0078] The produced laminate is cut into chips using a dicing device, and then the laminate is debindered and fired to produce a laminate for an all-solid-state battery.

[0079] The produced laminate 5 is heated to 600°C to 1000°C in a nitrogen atmosphere, for example, and sintered to obtain a sintered body. The sintering time is, for example, 0.1 to 3 hours. If the sintering atmosphere is a reducing atmosphere, sintering may be performed in, for example, an argon atmosphere or a nitrogen / hydrogen mixed atmosphere, instead of a nitrogen atmosphere.

[0080] Prior to the firing step, a binder removal treatment can be carried out as a separate step from the firing step. By thermally decomposing the binder component contained in the laminate 5 before firing, it is possible to suppress the binder component from being rapidly decomposed in the firing step. The binder removal treatment is carried out, for example, in a nitrogen atmosphere at a temperature in the range of 300°C to 800°C for 0.1 to 10 hours. If a reducing atmosphere is used, firing may be carried out in, for example, an argon atmosphere or a nitrogen / hydrogen mixed atmosphere instead of a nitrogen atmosphere.

[0081] The sintered body may be placed in a cylindrical container together with an abrasive such as alumina and barrel polished. This allows the corners of the laminate to be chamfered. Alternatively, polishing by sandblasting may be used. This method is preferable because it allows only specific portions to be polished.

[0082] (Terminal formation) A first external terminal 6 and a second external terminal 7 are attached to the sintered laminate 5 (sintered body). The first external terminal 6 and the second external terminal 7 are formed so as to be in electrical contact with the positive electrode current collector layer 1A and the negative electrode current collector layer 2A, respectively. For example, they can be formed by a known method such as a sputtering method, a dipping method, or a spray coating method on the positive electrode current collector layer 1A and the negative electrode current collector layer 2A exposed from the side surfaces of the sintered body. When forming the insulating film only on a predetermined portion, the insulating film is formed after masking with tape, for example.

[0083] The above describes the embodiments of the present invention in detail with reference to the drawings. However, each configuration and combination thereof in each embodiment is merely an example, and addition, omission, substitution, and other modifications of the configuration are possible without departing from the spirit of the present invention. EXAMPLES

[0084] (Examples 1 to 6) (Preparation of Cu particles with oxide film) The Cu particles having an oxide film according to Examples 1 to 6 were prepared by subjecting Cu particles having a diameter of 1 μm to a heat treatment at a temperature of 200° C. in a nitrogen atmosphere. 2As described above, the particles after the treatment were checked for the presence of an oxide film on the particle surface using an XPS device (ULVAC-PHI, PHI Quantera II), and the conditions were adjusted until the desired film thickness was obtained, producing metal particles with an oxide film 0.01 μm thick.

[0085] (Preparation of paste for outermost solid electrolyte layer) The outermost solid electrolyte layer paste was prepared using Li 1+x Al x Ti 2-x (PO 4 ) 3 (0≦x≦0.6) and Cu particles having an oxide film were mixed at a predetermined weight ratio, and then 100 parts of this powder were wet mixed with 100 parts of ethanol and 200 parts of toluene as a solvent in a ball mill. Then, 16 parts of polyvinyl butyral binder and 4.8 parts of benzyl butyl phthalate as a plasticizer were further added and mixed to prepare an outermost solid electrolyte layer paste. The Cu particles having an oxide film were added in advance so that the content shown in Table 1 was obtained based on the weight of the all-solid-state secondary battery after firing. The paste for the outermost solid electrolyte layer was formed into a sheet using a doctor blade method on a PET film as a substrate to obtain an outermost solid electrolyte layer sheet having a thickness of 15 μm.

[0086] (Preparation of paste for interlayer solid electrolyte layer) An interlayer solid electrolyte layer paste was prepared in the same manner as in the preparation of the outermost solid electrolyte layer paste, except that Cu particles having an oxide film were not mixed. The interlayer solid electrolyte layer paste was formed into a sheet using a doctor blade method on a PET film as a substrate to obtain an interlayer solid electrolyte layer sheet having a thickness of 15 μm.

[0087] (Preparation of Positive Electrode Active Material Layer Paste and Negative Electrode Active Material Layer Paste) The paste for the positive electrode active material layer and the paste for the negative electrode active material layer are Li 3 V 2 (PO4 ) 3 After mixing these in a predetermined weight ratio, 15 parts of ethyl cellulose as a binder and 65 parts of dihydroterpineol as a solvent were added to 100 parts of this powder, and the mixture was mixed and dispersed to prepare a paste for a positive electrode active material layer and a paste for a negative electrode active material layer.

[0088] (Preparation of Positive Electrode Current Collector Paste and Negative Electrode Current Collector Paste) The paste for the positive electrode current collector and the paste for the negative electrode current collector are both made of Cu and Li that do not contain an oxide film. 3 V 2 (PO 4 ) 3 After mixing them in a volume ratio of 80 / 20, 10 parts of ethyl cellulose as a binder and 50 parts of dihydroterpineol as a solvent were added to 100 parts of this powder, and the mixture was mixed and dispersed to prepare a paste for a positive electrode current collector layer and a paste for a negative electrode current collector layer.

[0089] (Preparation of electrode unit) The positive electrode unit and the negative electrode unit were prepared as follows. On the above solid electrolyte layer sheet, the active material paste was printed by screen printing to a thickness of 5 μm. Next, the printed active material paste was dried at 80° C. for 5 minutes, and the current collector paste was printed thereon to a thickness of 5 μm by screen printing. Next, the printed current collector paste was dried at 80° C. for 5 minutes, and the active material paste was printed again thereon to a thickness of 5 μm by screen printing. The printed active material paste was dried at 80° C. for 5 minutes, and then the PET film was peeled off. In this way, an electrode unit sheet was obtained in which the active material paste, the current collector paste, and the active material paste were printed and dried in this order on the solid electrolyte layer sheet.

[0090] (Preparation of Laminate) Five solid electrolyte layer sheets for the outermost solid electrolyte layer 3B were stacked, and 50 active material units (10 positive electrode units, 10 negative electrode units) were stacked alternately on top of them with the interlayer solid electrolyte layer 3A interposed therebetween. At this time, each unit was stacked with a shift so that the collector paste layer of the odd-numbered active material units extended only to one end face, and the collector paste layer of the even-numbered active material units extended only to the opposite end face. Six solid electrolyte layer sheets for the outermost solid electrolyte layer 3B were stacked on top of the stacked units. After that, this was molded by thermocompression bonding, and then cut to produce a laminated chip. Then, the laminated chips were simultaneously fired to obtain a laminated body 5. For the simultaneous firing, the temperature was raised to a firing temperature of 840°C at a heating rate of 200°C / hour in a nitrogen atmosphere, and the temperature was maintained for 2 hours, and the firing was allowed to cool naturally.

[0091] (Production and evaluation of all-solid-state secondary batteries) A first external terminal and a second external terminal were attached to the sintered laminate (sintered body) by a known method to prepare an all-solid-state secondary battery. Lead wires were attached to the first external terminal and the second external terminal, respectively, and a charge / discharge test was performed to measure the initial discharge capacity and the capacity retention rate after 500 cycles of the all-solid-state secondary battery. The measurement conditions were a current of 2.0 μA during both charging and discharging, and a cut-off voltage of 1.6 V and 0 V during charging and discharging, respectively. The results are shown in Table 1. The capacity during the first discharge was taken as the initial discharge capacity. The capacity retention rate was calculated by dividing the discharge capacity at the 500th cycle by the initial discharge capacity. Table 1 also shows the percentage of short-circuited batteries (short-circuit rate) among the evaluated all-solid-state secondary batteries.

[0092] Comparative Example 1 Comparative Example 1 differs from Example 1 in that the paste for the outermost solid electrolyte layer did not contain Cu particles having an oxide film. The other conditions were the same as those of Example 1.

[0093] [Table 1]

[0094] The "average thickness of oxide film" in Table 1 is the average thickness of the oxide film measured from the depth profile of 20 metal particles using an XPS apparatus. The "average particle size" in Table 1 is the average particle size of 20 metal particles measured using an FE-SEM device (SU8220, manufactured by Hitachi High-Technologies Corporation). The "average oxide film thickness ratio" in Table 1 is the ratio of the "average oxide film thickness" to the "average particle size" of the metal particles. The "content" in Table 1 is the ratio of the weight of the metal particles to the weight of the all-solid-state secondary battery. The "short circuit rate" in Table 1 is the percentage of all-solid-state secondary batteries that short-circuited after fabrication or during charge-discharge cycles among multiple all-solid-state secondary batteries fabricated under the same conditions.

[0095] As is clear from the results in Table 1, when comparing Examples 1 to 6 with Comparative Example 1, in all of Examples 1 to 6 containing Cu particles having an oxide film, both the initial discharge capacity and the capacity retention rate after 500 cycles were improved compared to Comparative Example 1 which did not contain Cu particles having an oxide film.

[0096] For Examples 7 to 33, all-solid-state secondary batteries were fabricated in the same manner as for Examples 1 to 6, except that the conditions shown in Tables 2 to 5 were different.

[0097] First, the results of similar evaluations performed on different layers containing Cu particles having an oxide film are shown in Table 2. Examples 7 to 11 respectively show the case where the layer containing Cu particles having an oxide film is an outermost solid electrolyte layer, a positive electrode active material layer, a negative electrode active material layer, an interlayer solid electrolyte layer, a margin layer, an outermost solid electrolyte layer, a positive electrode active material layer, a negative electrode active material layer, an interlayer solid electrolyte layer, and a margin layer.

[0098] [Table 2]

[0099] As is clear from the results in Table 2, among Examples 3 and 7 to 11, Example 3 contained Cu particles having an oxide film only in the outermost solid electrolyte layer, and had the highest initial discharge capacity and the highest capacity retention rate after 500 cycles.

[0100] Next, the results of similar evaluations performed on Cu particles having an oxide film with different average particle sizes are shown in Table 3. The Cu particles having an oxide film were contained only in the outermost solid electrolyte layer.

[0101] [Table 3]

[0102] As is clear from the results in Table 3, in Examples 3 and 13 to 15, the average particle diameter of the Cu particles having an oxide film was 0.1 μm to 20 μm, and the initial discharge capacity and the capacity retention rate after 500 cycles were high. In Example 12, the average particle diameter was 0.05 μm, and the initial discharge capacity was lower than those in Examples 3 and 13 to 15. In Example 16, the average particle diameter was 30 μm, and the initial discharge capacity was lower than those in Examples 3 and 13 to 15.

[0103] Next, the results of similar evaluations performed on Cu particles having oxide films with different average thickness ratios are shown in Table 4. The results of similar evaluations performed on Cu particles having oxide films with average particle sizes of 0.1 μm, 1 μm, and 20 μm are also shown in the same table. The Cu particles having oxide films were contained only in the outermost solid electrolyte layer.

[0104] Comparative Example 2 As Comparative Example 2, a similar evaluation was performed on a case in which the outermost solid electrolyte layer contained Cu particles having no oxide film. The results are shown in Table 4.

[0105] In Comparative Example 2, before Cu particles were mixed into the paste for the outermost solid electrolyte layer, N 2 +H 2The particles were subjected to reduction treatment in a mixed atmosphere, and XPS was used to confirm that there was no oxide film on the particle surface. When the oxide film could not be reduced by one reduction treatment, the heat treatment temperature, heat treatment time, and number of heat treatments were adjusted in various ways to produce Cu particles without an oxide film.

[0106] [Table 4]

[0107] As is clear from the results in Table 4, in Examples 13, 17, and 18, when the average particle size of the Cu particles having an oxide film was 0.1 μm and the average thickness ratio of the oxide film was 1%, 5%, or 10%, the initial discharge capacity and the capacity retention rate after 500 cycles were higher than in Example 19, in which the average thickness ratio of the oxide film was 15%. Similarly, in Examples 3, 20, and 21, when the average particle size of the Cu particles having an oxide film was 1 μm and the average thickness ratio of the oxide film was 1%, 5%, or 10%, the initial discharge capacity and the capacity retention rate after 500 cycles were higher than in Example 22, in which the average thickness ratio of the oxide film was 15%. In addition, in Examples 23 to 25, when the average particle size of the Cu particles having an oxide film was 20 μm and the average thickness ratio of the oxide film was 1%, 5%, or 10%, the initial discharge capacity and the capacity retention rate after 500 cycles were higher than in Example 26, in which the average thickness ratio of the oxide film was 15%. On the other hand, in Comparative Example 2, the initial discharge capacity and the capacity retention rate after 500 cycles were comparable to those of Example 20, but short circuits occurred at a rate of 5%.

[0108] Table 5 shows the results of similar evaluations performed when the Cu particles having an oxide film were replaced with other metal particles having an oxide film.

[0109] [Table 5]

[0110] As is clear from the results in Table 5, in Examples 27 to 33, when the metal species constituting the metal particles having an oxide film was Ni, Fe, Ag, Pt, Al, Bi, or Pd, an initial discharge capacity and capacity retention rate after 500 cycles similar to those obtained when the metal species was Cu were obtained. [Explanation of symbols]

[0111] 1 Positive electrode layer 1A Positive electrode current collector layer 1B Cathode active material layer 2. Negative electrode layer 2A negative electrode current collector layer 2B Negative electrode active material layer 3 Solid electrolyte layer 3A interlayer solid electrolyte layer 3B Outermost solid electrolyte layer 4 Margin Layer 5. Laminate 10 metal particles

Claims

1. a positive electrode layer including a positive electrode current collector layer and a positive electrode active material layer; a negative electrode layer including a negative electrode current collector layer and a negative electrode active material layer; a solid electrolyte layer including a solid electrolyte; a margin layer including a solid electrolyte and disposed next to each of the positive electrode layer and the negative electrode layer, and a laminate in which the positive electrode layer and the negative electrode layer are alternately laminated with a solid electrolyte layer including a solid electrolyte interposed therebetween; the laminate contains metal particles having an oxide film in at least one of the positive electrode active material layer, the negative electrode active material layer, the solid electrolyte layer, and the margin layer, the metal particles having the oxide film are included in the solid electrolyte layer and the margin layer, an average thickness of the oxide film is 0.1% or more and 10% or less of an average particle diameter of the metal particles.

2. The all-solid-state secondary battery according to claim 1 , wherein the metal particles having the oxide film are also provided on both surfaces of the laminate in the lamination direction.

3. 3. The all-solid-state secondary battery according to claim 1, wherein the average particle diameter of the metal particles having the oxide film is 0.1 μm to 20 μm.

4. The all-solid-state secondary battery according to any one of claims 1 to 3, wherein the oxide film has an average thickness in the range of 0.001 µm to 2 µm.

5. The all-solid-state secondary battery according to any one of claims 1 to 4, wherein the metal particles contain at least one selected from copper, nickel, silver, platinum, iron, aluminum, bismuth, and palladium.

6. The all-solid-state secondary battery according to any one of claims 1 to 5, wherein the metal particles are contained in an amount of 0.1 to 10% by weight based on the weight of the all-solid-state secondary battery.

7. 7. The all-solid-state secondary battery according to claim 1, wherein the metal particles having the oxide film are contained in all of the positive electrode active material layer, the negative electrode active material layer, the solid electrolyte layer, and the margin layer.

Citation Information

Patent Citations

  • Solid battery

    JP2006351326A

  • Solid battery and battery pack using the same

    JP2009181905A

  • Secondary battery

    JP2012190588A

  • All-solid type secondary battery

    JP2014192041A

  • Battery

    JP2018110098A