Film mold
A resin film mold with controlled surface free energy and free volume ranges addresses wettability and releasability issues, enabling effective transfer of uneven shapes onto curable resin surfaces, enhancing the quality of optical functional sheets.
Patent Information
- Application Number
- JP2021173337
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-10-22
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-10-22
AI Technical Summary
Existing film molds exhibit poor wettability and releasability with curable resin materials, particularly when forming uneven shapes, leading to issues such as air bubble formation and shape damage during peeling.
A film mold made of a resin film with a controlled surface free energy and free volume, within specific ranges, ensuring good wettability and releasability by satisfying the formulas S_E > 35.7, S_V > 0, and S_E < -296.77×S_V + 77.371, allowing for effective transfer of uneven shapes onto curable resin surfaces.
The film mold achieves satisfactory formation of uneven shapes on curable resin materials with improved wettability and releasability, preventing air bubble formation and shape damage, thereby producing high-quality optical functional sheets.
Smart Images

Figure 0007568601000002 
Figure 0007568601000003 
Figure 0007568601000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a film mold for transferring a concave-convex shape onto the surface of a curable resin material. [Background technology]
[0002] Liquid crystal display devices are widely used as display devices for various electronic devices. In recent years, such electronic devices have become increasingly smaller, and liquid crystal display devices are also being required to become smaller and lighter.
[0003] In such liquid crystal display devices, optical functional sheets that mainly utilize the effects of reflection, refraction, scattering, etc., or sheets that combine these are used. As such optical functional sheets, shaped films that are formed by giving a predetermined uneven shape to the surface of a resin film are known. Such shaped films are usually produced by press molding using a mold plate with a desired uneven shape or by injection molding.
[0004] As another method for imparting a predetermined uneven shape to the surface of a resin film, for example, Patent Document 1 proposes a method using a film mold (a release film for molding). In the technology of Patent Document 1, from the viewpoint of releasability with respect to the film material on which the uneven shape is to be formed, a releasing compound such as a silicone compound or a fluorine compound is used as a material for forming the uneven shape of the film mold. On the other hand, in the technology of Patent Document 2, a specific example discloses a technology in which poly-4-methylpentene-1 is used as a release sheet of a thermoplastic resin. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-73022 A [Patent Document 2] JP 2001-225376 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the technology described in the above Patent Document 1, although the film mold has sufficient releasability with respect to the film material on which the uneven shape is to be formed, the wettability is insufficient, and therefore the transferability of the uneven shape is not necessarily sufficient, and such a problem is particularly prominent when a curable resin material is used as the film material on which the uneven shape is to be formed. The technology of Patent Document 2 only discloses an embodiment in which poly-4-methylpentene-1 is used as a thermoplastic resin release sheet, and the index for selecting an appropriate material is unclear.
[0007] An object of the present invention is to provide a film mold that exhibits good wettability and peelability with respect to a curable resin material and is capable of favorably forming an uneven shape on the surface of the curable resin material. [Means for solving the problem]
[0008] As a result of intensive research conducted by the present inventors in order to achieve the above object, it has been found that a film mold made of a resin film having an uneven surface for transferring an uneven shape to the surface of a curable resin material has a surface free energy S E and the free volume S of the rough surface measured by positron annihilation. V The present inventors have found that the above object can be achieved by controlling the above and other factors within a predetermined range, and have thus completed the present invention.
[0009] That is, according to the present invention, there is provided a film mold made of a resin film having an uneven surface for transferring an uneven shape to a surface of a curable resin material, comprising: The surface free energy S of the uneven surface E [unit: mN / m] and the free volume S of the rough surface measured by positron annihilation method V [Unit: nm 3and] satisfy the following formulas (1) to (3): S E >35.7 (1) S V >0 (2) S E <-296.77×S V +77.371 (3)
[0010] The film mold of the present invention is preferably a long film obtained by imparting a continuous or intermittent uneven shape to the surface of a resin film formed by a melt extrusion method. Alternatively, the film mold of the present invention is preferably a long film obtained by continuously or intermittently applying an ultraviolet-curable resin to the surface of a base film and curing the resin to impart an uneven shape to the surface. The film mold of the present invention preferably has an average thickness of 10 to 200 μm. Effect of the Invention
[0011] According to the present invention, it is possible to provide a film mold that exhibits good wettability and peelability with respect to a curable resin material and is capable of forming a concave-convex shape well on the surface of the curable resin material. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a diagram showing an example of a shaped film manufacturing apparatus using a film mold according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a graph showing the relationship between the surface free energy SE and the free volume SV of the resin films according to the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Fig. 1 is a diagram showing an example of a shaped film manufacturing apparatus using a film mold according to an embodiment of the present invention. In the following, the manufacturing apparatus shown in Fig. 1 will be mainly illustrated and described, but the present invention is not particularly limited to the embodiment shown in Fig. 1.
[0014] In the manufacturing apparatus shown in Fig. 1, first, a substrate film 40 is continuously fed from a substrate feed roll 10, and the substrate film 40 passes through a guide roll 11 and is then coated on its surface with a curable resin material in a T-die 20, thereby forming a curable resin material layer 50 on the surface. The thickness of the curable resin material layer 50 is controlled by adjusting the clearance formed between the T-die 20 and the nip roll 12 and the feeding speed.
[0015] 1, the film mold 60 is continuously fed from the film mold feed roll 13. The base film 40 on which the curable resin material layer 50 is formed and the film mold 60 are superimposed by the laminating roll 15 and the upstream backup roll 16. Here, the film mold 60 has a predetermined uneven shape on the surface side facing the curable resin material layer 50, and the base film 40, the curable resin material layer 50, and the film mold 60 are superimposed in this order to form a laminate in a state in which the surface having the predetermined uneven shape is in contact with the curable resin material layer 50.
[0016] Then, the laminate in which the base film 40, the curable resin material layer 50, and the film mold 60 are stacked in this order is irradiated with ultraviolet light by the ultraviolet irradiation device 30, so that the curable resin material constituting the curable resin material layer 50 is cured in a state in which the predetermined uneven shape formed on the surface of the film mold 60 is transferred, thereby forming a cured resin layer 50a having a desired uneven shape on its surface. Next, after undergoing a curing reaction by ultraviolet irradiation, the film mold 60 passes between the laminating roll 15 and the downstream backup roll 17, and the film mold 60 is peeled off from the base film 40 having the cured resin layer 50a, and the film mold 60 is taken up by the film mold take-up roll 14, and the base film 40 having the cured resin layer 50a is taken up by the base take-up roll 19 via the guide roll 18.
[0017] 1, the substrate film 40 having the cured resin layer 50a is continuously produced as described above. The substrate film 40 having the cured resin layer 50a produced in this manner has a desired uneven shape on its surface by transferring the predetermined uneven shape formed in the film mold 60, and is therefore used as a shaping film, and is suitably used for various optical applications, for example, as an optical functional sheet utilizing the effects of reflection, refraction, scattering, etc.
[0018] In this embodiment, the film mold 60 is a resin film having an uneven surface, and the surface free energy S E [unit: mN / m] and the free volume S of the rough surface measured by positron annihilation V [Unit: nm 3 A resin film that satisfies the following formulas (1) to (3) is used. S E >35.7 (1) S V >0 (2) S E <-296.77×S V +77.371 (3)
[0019] The film mold 60 has a surface free energy S E and the free volume S V It is sufficient that the uneven shape is formed so as to satisfy the above formulas (1) to (3), and such uneven shape may be formed on both faces.
[0020] In this embodiment, the film mold 60 is laminated onto the base film 40 on which the curable resin material layer 50 is formed, with the uneven shape of the film mold 60 pressed against the surface of the curable resin material layer 50, and while maintaining this state, the curable resin material that constitutes the curable resin material layer 50 is cured by exposure to ultraviolet light, thereby forming a cured resin layer 50a in which the uneven shape of the film mold 60 is transferred.
[0021] According to this embodiment, the film mold 60 has a surface free energy S E and the free volume S of the rough surface V However, by using a resin film that satisfies the above formulas (1) to (3), the film mold 60 can be made to exhibit good wettability with respect to the curable resin material that constitutes the curable resin material layer 50, and can also exhibit excellent peelability, thereby making it possible to satisfactorily form the cured resin layer 50a having the desired uneven shape.
[0022] In particular, the present inventors have conducted research into the resin material constituting the film mold 60, and have obtained the following findings. That is, if a resin material with excellent releasability is used as the resin material constituting the film mold 60, the wettability with respect to the curable resin material constituting the curable resin material layer 50 is deteriorated, the material is not uniformly wetted, and air bubbles are easily trapped between the film mold 60 and the curable resin material layer 50. Such air bubbles become defects, and the cured resin layer 50a having the desired uneven shape cannot be formed. On the other hand, if a resin material with excellent wettability with respect to the curable resin material constituting the curable resin material layer 50 is selected, the adhesive force with respect to the curable resin material becomes too strong, the releasability is deteriorated, and there is a problem that the shape of the cured resin layer 50a is damaged during peeling.
[0023] In response to this, the inventors conducted further investigations and found that the surface free energy S E and the free volume S of the rough surface V It has been found that by setting the range satisfying the above formulas (1) to (3), the film mold 60 can exhibit good wettability with respect to the curable resin material constituting the curable resin material layer 50, and can also exhibit excellent peelability, and thus a cured resin layer 50a having a desired uneven shape can be satisfactorily formed.
[0024] In the film mold 60, the surface free energy S E and the free volume S of the rough surface V It is sufficient that the above formulas (1) to (3) are satisfied, however, in order to achieve a higher balance between wettability and peelability with respect to the curable resin material constituting the curable resin material layer 50, it is preferable that any one or all of the following formulas (4) to (6) are satisfied, and it is even more preferable that any one or all of the following formulas (7) to (9) are satisfied. 40≦S E <= 60 (4) 0.06≦S V ≦0.1 (5) -296.77×S V +67≦S E ≦-296.77×S V +77 (6)
[0025] Surface free energy S of a rough surface E However, if it is less than 35.7 N / m, the wettability of the curable resin material constituting the curable resin material layer 50 will deteriorate, making it easier for air bubbles to become trapped between the film mold 60 and the curable resin material layer 50, and it will not be possible to form a cured resin layer 50a having the desired uneven shape.
[0026] Free volume S of the rough surface V However, preferably 0.06 nm 3 If the ratio is equal to or greater than this, the permeability of the curable resin material constituting the curable resin material layer 50 into the film mold 60 can be increased, and this makes it possible to ensure sufficient adhesion required for molding. V It is more preferable that it is ≦0.08.
[0027] Also, S E >-296.77×S V If the value is +77.371, the adhesion to the curable resin material will be too strong, resulting in poor peelability. When peeled off, the shape of the cured resin layer 50a will be damaged, and it will not be possible to form a cured resin layer 50a having the desired uneven shape.
[0028] The surface free energy S of the uneven surface of the film mold 60 E The contact angles of water, diiodomethane, and ethylene glycol on the uneven surface of the film mold 60 are measured, and the free volume S of the uneven surface can be calculated from the measured contact angle data by the analytical theory of Kitazaki and Hata. Vcan be obtained by measuring the uneven surface of the film mold 60 by a positron annihilation method. The positron annihilation method is a type of positron annihilation lifetime measurement method, in which the time from when a positron is incident on a sample until it annihilates is measured, and the free volume of the voids is calculated from the annihilation lifetime.
[0029] The average thickness of the film mold 60 is not particularly limited, but is preferably 10 to 200 μm, more preferably 20 to 100 μm, and even more preferably 30 to 60 μm. By setting the average thickness of the film mold 60 within the above range, the cured resin layer 50a having a desired uneven shape can be produced with higher productivity. Examples of the uneven shape that can be produced by the film mold include a continuous or discontinuous shape with a height of 1 to 30 μm, an aspect ratio of 0.5 to 1.0, and an interval of 0 to 20 times the height.
[0030] The manufacturing method of the film mold 60 is not particularly limited, but examples thereof include a method of obtaining a resin film by melt extrusion, heating the obtained resin film, and pressing the film against a shaping roll having a predetermined uneven shape formed on its surface to form an uneven shape continuously or intermittently on the surface to obtain a long film. The heating temperature of the resin film when pressing the film against the shaping roll having a predetermined uneven shape formed on its surface is not particularly limited, but examples thereof include a method of heating the film to a temperature equal to or higher than the glass transition temperature of the resin material constituting the resin film.
[0031] Alternatively, the film mold 60 can be manufactured by continuously or intermittently applying an ultraviolet-curable resin to the surface of a resin film that serves as the base film, and then curing the applied resin to form an uneven shape using the ultraviolet-curable resin, thereby obtaining a long film having an uneven surface.
[0032] The resin material constituting the resin film forming the film mold 60 is not particularly limited, but is preferably a thermoplastic resin, for example, polyester resin such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT), acrylic resin such as polymethyl methacrylate (PMMA), carbonate resin such as polycarbonate (PC), amide resin such as nylon 6, cyclic olefin resin (COP), ethylene-vinyl alcohol copolymer (EVOH), polyphenylene sulfide (PPS), etc. Two or more of these may be laminated or mixed for use.
[0033] In addition, when a method of forming a concave-convex shape using an ultraviolet curing resin is adopted, the ultraviolet curing resin can be a radical curing acrylic monomer, an acrylic oligomer such as urethane acrylate, epoxy acrylate, or polyester acrylate, an unsaturated polyester, or a cationic curing epoxy resin, oxetane resin, vinyl ether, etc. In addition, examples of the substrate film used in this case include those made of the above-mentioned resin materials.
[0034] The surface free energy S of the uneven surface of the film mold 60 E , and the free volume of the rough surface S V The method for setting the surface free energy S to the above range is not particularly limited, but examples thereof include a method of selecting a resin material constituting the resin film forming the film mold 60, a method of modifying the surface by corona treatment, a method of adjusting wettability by a surface modifier, a method of adjusting free volume by adding inorganic fine particles, and a method of adjusting the crystallinity when the resin material is a crystalline resin. In particular, in the case of a crystalline resin such as polyethylene terephthalate, the crystallinity can be increased by controlling the heating conditions and the stretching conditions when forming the film, and the like, thereby increasing the number of densely arranged molecular portions, thereby decreasing the surface free energy S E Without changing the free volume S V can be made smaller.
[0035] The curable resin material constituting the curable resin material layer 50 is not particularly limited, and may be either a thermosetting resin or an ultraviolet curing resin, but is preferably an ultraviolet curing resin from the viewpoint of excellent production efficiency. The ultraviolet curing resin may be the same resin as that exemplified when the uneven shape of the film mold is formed with an ultraviolet curing resin, and is not particularly limited, but is preferably an acrylic resin with good transparency from the viewpoint of imparting optical functionality. Furthermore, when applying the curable resin material to the surface of the T-die 20 in the manufacturing device shown in FIG. 1, it is more preferable that the resin is a solventless ultraviolet curing resin (a resin having a viscosity that can be applied even without a solvent). When a thermosetting resin is used as the curable resin material constituting the curable resin material layer 50, a heating device such as a heater may be used instead of the ultraviolet irradiation device 30 shown in FIG. 1, and the resin may be cured by heating.
[0036] The curable resin material constituting the curable resin material layer 50 preferably has a viscosity (B-type viscosity) at a temperature of 25°C before curing of 10 to 600 cps, more preferably 20 to 100 cps, and even more preferably 20 to 70 cps, from the viewpoint of better transferring the uneven shape by the film mold 60, and the viscosity of the curable resin material in a state in which it does not substantially contain a solvent is preferably within this range. Furthermore, when a solventless ultraviolet curable resin is used, by having the viscosity in a state in which it does not substantially contain a solvent within this range, it is possible to provide excellent applicability when applying with the T-die 20 in the manufacturing apparatus shown in FIG. 1.
[0037] The average thickness of the curable resin material layer 50 before curing and the average thickness of the cured resin layer 50a after curing are not particularly limited and may be appropriately selected depending on the characteristics and use of the resulting shaped film, but are preferably 1 to 100 μm, more preferably 5 to 20 μm.
[0038] In addition, the base film 40 is not particularly limited, but when an ultraviolet-curable resin is used as the curable resin material constituting the curable resin material layer 50, or when the base film 40 having the finally obtained cured resin layer 50a is used for optical purposes, a light-transmitting resin film is preferable, and examples of the resin material constituting such a resin film include acrylic resin, polycarbonate resin, acrylic-modified polycarbonate resin, and cyclic olefin resin.
[0039] The average thickness of the base film 40 is not particularly limited and may be appropriately selected depending on the properties and applications of the resulting shaped film, but is preferably 10 to 200 μm, more preferably 20 to 40 μm.
[0040] According to this embodiment, the film mold 60 has a surface free energy S E and the free volume S of the rough surface V The film mold 60 uses a resin film that satisfies the above formulas (1) to (3). Such a film mold 60 exhibits good wettability and peelability with respect to the curable resin material that constitutes the curable resin material layer 50, and therefore can satisfactorily form a cured resin layer 50a having a desired uneven shape on its surface. EXAMPLES
[0041] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The evaluation methods for each characteristic are as follows.
[0042] <Surface free energy S E > Using a fully automatic contact angle meter (trade name "DM-701", manufactured by Kyowa Interface Science Co., Ltd.), the contact angles of water, diiodomethane, and ethylene glycol on the resin film surface were measured under the following conditions, and the surface free energy S was calculated by the Kitazaki-Hata method. E [Unit: mN / m] was calculated. Measurement temperature: 25±2℃ Measurement humidity: 50±10%RH Appropriate amount of liquid: 3μL Retention time after liquid contact: 10sec
[0043] <Free volume S V > The resin film was attached to a 15 mm x 15 mm silicon wafer and degassed in vacuum at 25°C. The positron annihilation lifetime was measured under the following conditions. Measurement equipment: Fuji Invac small positron annihilation generator PALS-200A Positron source: 22 Na-based positron annihilation Gamma-ray detector: BaF2 scintillator and photomultiplier tube Beam intensity: 5keV Measurement temperature: 25℃ Measurement atmosphere: Vacuum Total count: Approximately 5,000,000 counts The obtained positron annihilation lifetime curve was subjected to a three-component analysis using the nonlinear least squares program POSITRONFIT, and the annihilation lifetimes were determined as τ1, τ2, and τ3 in ascending order of annihilation lifetime. The free volume radius R3 was calculated using the following formula from the longest average annihilation lifetime τ3, and the free volume S of the film surface was calculated from the obtained free volume radius R3. V [Unit: nm 3 ] was calculated. τ3=(1 / 2)[1-{R3 / (R3+0.166)}+(1 / 2π)sin{2πR3 / (R3+0.166)}] -1 S V =(4 / 3)π(R3) 3
[0044] <Peel strength> A sample 25 mm wide x 150 mm long was prepared using a laminate of a resin film as the substrate 40, a cured acrylic resin film as the cured resin layer 50a, and a resin film that would become the film mold 60. A 90° peel test was performed on the adhesive surface between the cured acrylic resin film as the cured resin layer 50a and the resin film that would become the film mold 60 using a tensile tester (product name "Tensilon Universal Material Tester RTC-1210A", manufactured by ORIENTEC Corporation) to measure the 90° peel strength [unit: N / 25 mm]. From the viewpoint of good peeling when used as a film mold, a sample with a 90° peel strength of 2 N / 25 mm or less was deemed to pass.
[0045] <Presence or absence of air bubbles> The laminate of the resin film as the substrate 40, the cured acrylic resin film as the cured resin layer 50a, and the resin film that would become the film mold 60 was visually inspected for the presence or absence of air bubbles at the interface therebetween.
[0046] <Example 1> The surface free energy S of the unstretched polybutylene terephthalate resin film (IV=1.0, melt extrusion at 260°C to a thickness of 40 μm) was measured by the above method. E and the free volume S V The results are shown in Table 1.
[0047] Next, an acrylic resin (product name "PAK-02", manufactured by Toyo Gosei Co., Ltd., B-type viscosity at 25°C: 70 cps or less) was applied using a bar coater to the surface of a polyester film with an easy-adhesion layer (product name "Cosmoshine A4300", manufactured by Toyobo Co., Ltd., thickness 38 μm) as the substrate 40 to form an acrylic resin layer with a thickness of 10 μm as the curable resin material layer 50. Then, a polybutylene terephthalate resin film to be the film mold 60 was laminated on the surface of the acrylic resin layer side of the laminate in which an acrylic resin layer as the curable resin material layer 50 was formed on the surface of the polyester film with an easy-adhesion layer thus obtained as the substrate 40, and then a UV irradiation amount of 971 mJ / cm was applied using a UV irradiation device from the side of the polyester film with an easy-adhesion layer as the substrate 40. 2 The laminate was obtained by curing the polyester film with the easy-adhesion layer as the substrate 40, the cured acrylic resin film as the cured resin layer 50a, and the polybutylene terephthalate resin film as the film mold 60, and the peel strength and the presence or absence of air bubbles were measured according to the above-mentioned method. The results are shown in Table 1.
[0048] <Examples 2 to 10> The surface free energy S E and the free volume S V The peel strength and the presence or absence of air bubbles were measured in the same manner as in Example 1, and a laminate of a polyester film with an easy-adhesion layer as the substrate 40, a cured acrylic resin film as the cured resin layer 50a, and a resin film to become the film mold 60 was obtained. The results are shown in Table 1.
[0049] The resin films used in Examples 2 to 10 are as follows. Example 2 (PBT(2)): Biaxially stretched polybutylene terephthalate resin film (product name "BOBLET BO-PBT", manufactured by Kohjin Film & Chemicals Co., Ltd., thickness 25 μm) Example 3 (PBT(3)): A polybutylene terephthalate resin film obtained by forming a polybutylene terephthalate resin (product name "GelaNex 700FP", manufactured by Polyplastics Co., Ltd.) into a film having a thickness of 40 μm by melt extrusion at 250° C. Example 4 (Nylon 6): Nylon 6 film (product name "Harden N1100", manufactured by Toyobo Co., Ltd., thickness 20 μm) Example 5 (PPS): Polyphenylene sulfide resin film (product name "TORELINA", manufactured by Toray Industries, Inc., thickness 100 μm) Example 6 (EVOH): Ethylene-vinyl alcohol copolymer resin film (product name "EVAL", manufactured by Kuraray Co., Ltd., thickness 20 μm) Example 7 (COP): Cycloolefin resin film (product name "ZEONOR", manufactured by Zeon Corporation, thickness 130 μm) Example 8 (PMMA (1)): A polymethyl methacrylate resin film obtained by forming a film of polymethyl methacrylate resin (average molecular weight = 120,000 to 150,000, glass transition temperature = 124°C) by melt extrusion, biaxially stretching the film to a thickness of 40 μm. Example 9 (PMMA (2)): A polymethyl methacrylate resin film obtained by forming a film of polymethyl methacrylate resin (average molecular weight = 90,000 to 110,000, glass transition temperature = 122°C) by melt extrusion, biaxially stretching the film to a thickness of 40 μm. Example 10 (PET (1)): A polyethylene terephthalate resin (IV = 0.9, modified with 15 mol of isophthalic acid) was formed into a film having a thickness of 100 μm by melt extrusion at 270° C., and then biaxially stretched and heat set to obtain a polyethylene terephthalate resin film with a high degree of crystallinity (1730 cm -1 The degree of crystallinity calculated from the half-width (Δν) of the crystallinity is 43.68% (degree of crystallinity = 100 × ((305-Δν) / 209-1.335) / (1.455-1.335)).
[0050] <Comparative Examples 1 to 9> The surface free energy S E and the free volume S V The peel strength and the presence or absence of air bubbles were measured in the same manner as in Example 1, and a laminate of a polyester film with an easy-adhesion layer as the substrate 40, a cured acrylic resin film as the cured resin layer 50a, and a resin film to become the film mold 60 was obtained. The results are shown in Table 1.
[0051] The resin films used in Comparative Examples 1 to 9 are as follows. Comparative Example 1 (PP(1)): Unstretched polypropylene film (product name "RXC22", manufactured by Mitsui Chemicals Tocello, thickness 20 μm) Comparative Example 2 (PP(2)): A non-oriented polypropylene film made by melt extrusion of polypropylene resin (homo-PP) to a thickness of 200 μm. Comparative Example 3 (PP(3)): A non-oriented polypropylene film obtained by forming polypropylene (trade name "SunAllomer", manufactured by SunAllomer Co., Ltd.) into a film having a thickness of 100 μm by melt extrusion at 260° C. Comparative Example 4 (PE): Low-density polyethylene film (thickness 100 μm) Comparative Example 5 (PTFE): Polytetrafluoroethylene film (product name "Naflon", manufactured by Nichias Corporation, thickness 100 μm) Comparative Example 6 (TPX): Polymethylpentene resin film (product name "Opulent X-44B", manufactured by Mitsui Chemicals, Inc., thickness 20 μm) Comparative Example 7 (PET (2)): Polyethylene terephthalate resin film (product name "Cosmoshine A4100", manufactured by Toyobo Co., Ltd., thickness 38 μm) Comparative Example 8 (PET (3)): A non-crystalline polyethylene terephthalate resin film (1730 cm -1The degree of crystallinity calculated from the half-width (Δν) of the crystallinity is 0.88% (degree of crystallinity = 100 × ((305-Δν) / 209-1.335) / (1.455-1.335)). Comparative Example 9 (PC(1)): A polycarbonate resin film obtained by forming a polycarbonate resin (product name "Iupilon 7022J", manufactured by Mitsubishi Engineering Plastics Corporation) into a film having a thickness of 100 μm by melt extrusion at 280° C.
[0052] [Table 1]
[0053] As shown in Table 1, the resin film that becomes the film mold 60 has a surface free energy S E and the free volume S V and Equations (1) to (3) (Equation (1): S E >35.7, formula (2):S V >0, formula (3):S E < -296.77×S V +77.371 ) was used, the peel strength against the cured acrylic resin as the cured resin layer 50a was low, the peelability was excellent, the generation of air bubbles was suppressed, and good wettability was exhibited (Examples 1 to 10). In addition, the spectrum of the interface between the cured resin layer and the film mold was measured by Raman spectroscopy, and the penetration depth of the cured resin was calculated from the intensity ratio of specific peaks. As a result, the penetration depth of the cured resin into the resin film of Example 3 was 0 μm. Furthermore, the penetration depth of the cured resin into the resin film of Comparative Example 9 was 4 μm, and the deeper the penetration depth, the stronger the peel strength tended to be. The measurement results of the penetration depth are shown in Table 1. In Table 1, "ND" indicates that it was difficult to separate the peaks and to measure the penetration depth.
[0054] <Penetration depth> The penetration depth was measured under the following conditions. Measurement equipment: Laser Raman spectrophotometer (product name "NRS-5500", manufactured by JASCO Corporation) Laser wavelength: 532.31nm Laser spot diameter: 2μm Number of times accumulated: 1 The specific measurement method was as follows: A cross section of a laminate of a resin film to be the substrate 40, a cured acrylic resin film to be the cured resin layer 50a, and a resin film to be the film mold 60 was measured at multiple points in the thickness direction across the interface between the cured resin layer 50a and the film mold 60 using a laser Raman spectrophotometer. Then, for the measurement spectrum obtained at each thickness position, among the measurement peaks originating from the resin film that becomes the film mold 60, the measurement peak that does not overlap with the measurement peak originating from the cured acrylic resin film as the cured resin layer 50a and has the highest intensity was selected from the measurement peaks that are less affected by the orientation state of the resin film, and the ratio P1 / P2 was calculated between the intensity P1 of the measurement peak that has the highest intensity among the other measurement peaks. The position where the ratio P1 / P2 is stably small is regarded as the cured resin layer 50a, and the position where the ratio P1 / P2 is stably large is regarded as the film mold 60, and the range in which the value of the ratio P1 / P2 changes as the thickness direction between them is specified, and this range is regarded as the region where the cured acrylic resin as the cured resin layer 50a has penetrated into the resin film that becomes the film mold 60, and the width of this range was calculated as the penetration depth.
[0055] In addition, for the resin film of Example 3, a metal shaping roll having an uneven pattern on its surface was used to obtain a resin film having an uneven shape (uneven height: 8 to 12 μm, uneven aspect ratio: 0.7 to 1.0) formed on its surface, and the resin film having an uneven shape formed on its surface was used, and similar results were obtained. Therefore, from these results, it can be said that the resin films of Examples 1 to 10, when used as the film mold 60, exhibit good wettability and peelability with respect to the curable resin material, and can satisfactorily form an uneven shape on the surface of the curable resin material.
[0056] On the other hand, the surface free energy S Eis expressed as formula (1) (formula (1): S E >35.7) was not satisfied, air bubbles were generated between the resin film that became the film mold 60 and the layer made of the cured acrylic resin as the cured resin layer 50a, resulting in poor wettability (Comparative Examples 1 to 6). In addition, the resin film that becomes the film mold 60 has a surface free energy S E and the free volume S V and formula (3) (formula (3): S E <-296.77×S V +77.371) was not satisfied, the peel strength became too high, resulting in poor peelability from the cured resin layer 50a (Comparative Example 7). In particular, in Comparative Examples 8 and 9, debris was generated during peeling. In addition, the surface free energy S of the resin films according to each of the examples and comparative examples is shown in FIG. E and the free volume S V The relationship is shown in a graph. [Explanation of symbols]
[0057] 10~19…Roll 20…T die 30...UV irradiation device 40...Base film 50…Curable resin material layer 50a...cured resin layer 60...Film mold
Claims
1. A film mold made of a resin film having an uneven surface for transferring an uneven shape to a surface of a curable resin material, The surface free energy S of the uneven surface E [unit: mN / m] and the free volume S of the uneven surface measured by positron annihilation method V [Unit: nm 3 ] satisfies the following formulas (1) to (3), A film mold is a long film obtained by continuously or intermittently imparting an uneven surface to a resin film formed by melt extrusion. S E >35.7 (1) S V >0 (2) S E <-296.77×S V +77.371 (3)
2. The film mold according to claim 1, which has an average thickness of 10 to 200 μm.
Citation Information
Patent Citations
Method for producing continuous sheet having optical function
JP2001225376A
Pattern forming method
JP2011165831A
Method for producing laminate, and laminate
JP2015231669A
Mold release film for mold molding and mold molding method