Method for preparing synthetic quartz glass
By adjusting the flame shape and oxygen ratio, a targetless flame is formed, and the deposition process is optimized, the deposition efficiency of synthetic quartz glass is improved and production costs are reduced.
Patent Information
- Application Number
- JP2021202995
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-16
- Filing Date
- 2021-12-15
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-12-15
AI Technical Summary
The prior art has low deposition efficiency when producing synthetic quartz glass, resulting in high production costs, and it is necessary to improve the deposition efficiency to reduce costs.
A new synthetic flame method is adopted to optimize the deposition process by adjusting the shape and oxygen ratio of the flame to ensure that the luminous intensity of the flame in the vertical and horizontal directions meets specific conditions, form a targetless flame, and control the oxygen ratio below 1.
The deposition efficiency of SiO2 is improved and the production cost of synthetic quartz glass is reduced.
Smart Images

Figure 0007568604000005 
Figure 0007568604000001 
Figure 0007568604000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing synthetic quartz glass and to a corresponding device for carrying out the method according to the invention. [Background technology]
[0002] To produce synthetic quartz glass, SiO is produced by hydrolysis or oxidation of silicon-containing starting materials using a CVD process. 2 Particles are generated and deposited on a moving carrier. They can be divided into external and internal deposition processes. In the external deposition process, SiO 2 The particles are deposited on the outside of a rotating carrier. Examples of such external deposition processes are the so-called OVD process (Out-side Vapour Phase Deposition), the VAD process (Vapour Phase Axial Deposition) and the PECVD process (Plasma Enhanced Chemical Vapour Deposition). The best known example of an internal deposition process is the deposition of SiO 2 This is a modified chemical vapor deposition (MCVD) process that deposits particles.
[0003] In the region of the support surface, at a sufficiently high temperature, SiO 2 The particles are directly vitrified, which is also called "direct vitrification". In contrast, in the so-called "soot process", SiO 2 The temperature during particle deposition is so low that the porous SiO 2 A soot layer is obtained, which is sintered in a separate step to produce transparent quartz glass. Both the direct vitrification method and the soot method produce dense, transparent, high-purity synthetic quartz glass.
[0004] Prior art processes for the production of synthetic quartz glass generally involve the use of SiO 2A method is used to ensure sufficient deposition efficiency of the particles, where the deposition efficiency is determined by the weight of the soot body produced and the amount of SiO 2 that can be produced assuming complete conversion of silicon from the silicon-containing starting compound used. 2 This is understood to be the quotient of the mathematical maximum sum of .
[0005] In order to provide a carbonaceous soot body which has a low OH value after vitrification (good for fiber applications), DE 10 2011 121 153 A discloses a carbonaceous soot body having a SiO 2 It is proposed to supply the polysiloxane compound to the flame superstoichiometrically compared to the oxygen during deposition of the particles, ie to use a so-called rich flame during deposition.
[0006] Another process for the production of synthetic quartz glass is disclosed in DE 101 02 611 A, in which SiO 2 It is stated that non-uniformity in the deposited quartz glass can be avoided if the deposition is performed with a burner flame opening angle of 3°-15° when the particles impinge on the deposition surface and a distance between the deposition burner and the deposition surface of 160mm-240mm. The publication does not disclose any further information on how the deposition efficiency can be improved.
[0007] Overall, the prior art processes still need to be improved with respect to the deposition efficiency of silicon-containing starting materials, and therefore there is a need for a process for the production of synthetic quartz glass that can improve the deposition efficiency of silicon-containing starting materials. Improved deposition efficiency is accompanied by a reduction in the production cost of synthetic quartz glass. DISCLOSURE OF THEINVENTION
[0008] Within the scope of the present invention, the deposition efficiency is determined by the mathematically generated SiO 2 The total amount of SiO deposited on the target tube 2 (assuming complete conversion of all silicon from the amount of precursor used).
[0009] According to the invention, this problem is solved by a method for producing synthetic quartz glass, which method is characterized firstly by the following steps: (1) vaporizing a feedstock comprising at least one organosilicon starting compound to form a feedstock vapor; (2) The raw material vapor from step (1) is supplied to a reaction section, and the raw material vapor is burned in a flame in the presence of oxygen to produce SiO by oxidation and / or hydrolysis. 2 converting the soot particles into (3) The SiO produced by step (2) 2 depositing soot particles onto a deposition surface to form a soot body; and (4) Optionally, drying and vitrifying the soot body produced in step (3) to form synthetic quartz glass.
[0010] The method according to the present invention is characterized in that the synthetic flame used in the method has a full width at half maximum (FWHM) of the vertical emission intensity in the absence of a target. vert ) of the horizontal emission intensity full width at half maximum (FWHM hori ) is greater than 10.
[0011] The half-width of the emission intensity in the vertical and horizontal directions is obtained by the following procedure.
[0012] The "vertical emission intensity" (and its full width at half maximum FWHM) of the flame at a certain height above the burner vert ) is calculated by integrating each horizontal pixel row of the two-dimensional camera image in the horizontal direction to obtain the flame emission intensity (unit: cd / mm 2 ) is determined. This horizontal intensity sum is calculated for each burner distance (each row) or flame height (results in cd / mm). This integrated horizontal luminous intensity of the flame is then obtained as a function of the vertical distance from the burner (this function is called the "vertical luminous intensity"). From the shape of the curve that is maximum at a certain burner distance, the half-width of the vertical luminous intensity (unit: mm) can be calculated.
[0013] The "horizontal emission intensity" of the flame (and its full width at half maximum FWHM) between two specific distances to the left and right of the central axis of the burner hori ) is calculated by vertically integrating each vertical pixel row of the two-dimensional camera image to obtain the flame emission intensity (unit: cd / mm 2 ) is calculated. This vertical intensity sum is calculated for each horizontal distance to the left and right of the burner central axis (located at position "0") (results in units of cd / mm). The integrated vertical luminous intensity of the flame is then obtained as a function of the horizontal distance to the left and right of the burner central axis (this function is called the "horizontal luminous intensity"), and the half-width (units: mm) of the horizontal luminous intensity can be determined from the shape of the curve that is maximum near the horizontal distance "0" (represented by the burner central axis). The FWHM value is then given as the horizontal distance between the two points to the left and right of the burner axis where the horizontal luminous intensity is half its maximum value.
[0014] According to the present invention, SiO 2 It has been found that for the deposition of particles, introducing a target (tube, rod or soot body) into the flame defined above gives good deposition efficiency.
[0015] Thus, the present invention relates to a synthetic flame operated targetless, which means a synthetic flame operated without the use of a growth tube, since otherwise the flame shape would depend on the thickness of the target tube (or soot body) and the distance of the burner from the target surface, as well as the target temperature, in which case the synthetic flame is generally essentially undisturbed.
[0016] The improved deposition efficiency according to the present invention, as previously defined, is a function of the weight of the soot body produced and the amount of SiO 2 that can be produced assuming complete conversion of silicon from the silicon-containing starting compound used. 2 This is obtained by quotienting the maximum mathematical quantity of
[0017] Each flame used in a typical process emits a characteristic radiation (chemiluminescence) due to chemically formed short-lived intermediates such as the radicals OH*, CH* and C2*, which are responsible for the glow of the flame in the ultraviolet and visible spectral range.
[0018] Because chemiluminescence occurs very locally and it is difficult to measure the intensity of ultraviolet and infrared light, the flame shape is measured using a camera calibrated to the SI unit of candela, as described in the experimental section below. Candela generally corresponds to the sensation of the human eye and does not take into account the ultraviolet and infrared components that require special cameras and windows. Therefore, most of the intensity calibrated in candela is determined by the SiO 2 This is due to the blackbody radiation of the ionizing radiation and carbon soot particles.
[0019] The above-mentioned characteristics of the synthetic flame used in the method according to the invention are achieved in the absence of a target. The measures for providing such a target-free flame are known to the person skilled in the art and can be achieved in particular by the number of nozzles, the type of burner, the other gases and the gas amounts. In any case, the person skilled in the art can easily prepare and verify a targetless flame in the sense of the invention.
[0020] In a preferred embodiment of the method according to the invention, the flame shape of the burner is determined by the Full Width at Half Maximum (FWHM) of the vertical emission intensity. vert ) and the horizontal emission intensity full width at half maximum (FWHM hori ) is 12 or more (targetless), more preferably 14 or more, and even more preferably 15 or more, and the emission intensity of these is candela / mm 2 The value measured in the above is used.
[0021] In the present invention, it is more preferable that the conversion of the raw material vapor in the step (2) is carried out with an air number in the burner of 1.00 or less.
[0022] In particular, preferred air numbers in the process according to the present invention are 0.95 or less, more preferably 0.90 or less, more preferably 0.85 or less, more preferably 0.80 or less, more preferably 0.78 or less, more preferably 0.76 or less.
[0023] It is desirable for said air number to be maintained in the method according to the invention for at least 20% of the growth time as defined above, more preferably at least 30%, even more preferably at least 40%, even more preferably at least 50%, even more preferably at least 60%, even more preferably at least 70%, even more preferably at least 80%, even more preferably at least 90%, even more preferably at least 95%, even more preferably at least 97%, even more preferably at least 98%, even more preferably at least 99%.
[0024] According to the present invention, if the total amount of oxygen actively and centrally supplied to the burner during the reaction provided in step (2) is stoichiometric or preferably less than stoichiometric, resulting in an air number of 1 or less, then SiO 2 It has additionally been found that the efficiency of particle deposition can be significantly improved.
[0025] According to the invention, it is thus provided that the gas flow in the burner of the device according to the invention, i.e. the ratio of oxygen (including the supplied oxygen) actively (i.e. pressurized) supplied from the burner to all combustibles actively (i.e. pressurized) supplied to the burner, is adjusted so as to achieve an air number of less than or equal to 1 relative to all gases actively (i.e. pressurized) supplied to the burner.
[0026] The air number λ is defined as the ratio of the amount of oxygen actually available to the theoretical minimum amount of oxygen required for complete stoichiometric combustion.
[0027] Within the scope of the present invention, the total amount of oxygen used (at most) stoichiometrically for the conversion of the organosilicon starting compound in the burner is understood to be the amount of oxygen actively supplied to the burner under pressure.From this definition of the total amount of oxygen, it follows that the amount of oxygen passively (i.e. not pressurized) supplied from the atmosphere to the flame is not added to the total amount of oxygen supplied according to the present invention.In particular, the oxygen diffused from the atmosphere surrounding the burner to the flame during the combustion of the organosilicon starting compound and the oxygen sucked in by negative pressure are excluded.
[0028] It is also understood that the amount of oxygen stoichiometrically used (at most) to convert the organosilicon starting compound (and the combustible auxiliary gas) in the burner is the total amount of oxygen supplied centrally to the burner.
[0029] The term "oxygen supplied to the burner" in the context of a concentric burner means the total amount of oxygen actively leaving the burner at the surface area on the flame side of the burner, which surface area is formed by a substantially circular area having a radius r, where the radius r extends perpendicularly from the center of the feed nozzle or the center of the feed nozzles (nozzles for supplying silicon-containing starting compounds) to the direction of the bait rod rotation axis, and the radius r corresponds to about 1 / 5 of the average spacing of the feed nozzles from the deposition surface of the formed soot body.
[0030] The term oxygen supplied centrally to the burner is understood to mean, in the case of a linear burner, the total amount of oxygen actively leaving the latter on the flame side of the burner in a surface area, where the surface area is formed by a surface, i.e. a surface having a distance d perpendicular to the direction of the bait rod rotation axis from the center of the material nozzle or the centerline of the material nozzle group (nozzle (or nozzles) for supplying the silicon-containing starting compound), the distance d corresponding to approximately 1 / 5 of the average distance of the material nozzle (or nozzles) from the deposition surface of the formed soot body.
[0031] The (maximum) stoichiometric use of oxygen is preferably maintained for the complete growth time of the solid, where the growth time is the time required to supply the silicon-containing starting compound to the process according to the invention. t 成長時間 = t 開始-終了 ケイ素含有出発化合物の供給
[0032] Within the scope of the present invention, by applying the method so that the air number during combustion is 1 or less, the following technical effects are obtained.
[0033] However, it is necessary to set up a targetless flame in which the number of air particles in the combustion is 1 or less, and to obtain the full width at half maximum (FWHM) of the vertical emission intensity in the absence of a target. vert ) of the horizontal emission intensity full width at half maximum (FWHM hori ) ratio is not sufficient for flames with a value greater than 10. For flames operated with an air number of 1 or less, in the absence of a target, the full width at half maximum (FWHM) of the vertical emission intensity is vert ) of the horizontal emission intensity full width at half maximum (FWHM hori ) does not automatically have to be greater than 10.
[0034] In other words, the use of flames in prior art processes with air numbers of 1 or less results in a vertical full width at half maximum (FWHM vert ) of the horizontal emission intensity full width at half maximum (FWHM hori ) is not mandatorily held to the claimed ratio of greater than 10.
[0035] The use of rich combustion mixtures (with air numbers less than 1) increases the O 2 The ignition occurs slower and more locally only at the periphery of the flame, where the mixture is already sufficiently diffused. The center of the flame is more difficult to ignite due to the mixture being too rich. As a result, less gas can ignite at the same time, and the oxygen must diffuse inwards first. This prevents the hot combustion gases from expanding from the ignited area into other flame areas, resulting in less turbulence of the flame.
[0036] In the method according to the invention, the gas volume with the ignitable mixture extends more upwards and expands less laterally. This results in a more laminar flame. A related effect is that the narrower, more laminar flame attaches itself better to the soot body and forms a more stable dwell point directly below the soot body. This reduces the amount of SiO 2 The diffusion path of the particles is shortened and the residence time at the residence point is increased, resulting in an overall higher deposition efficiency.
[0037] The method according to the invention is in particular an Outside Vapor Deposition Method (OVD) process, a Vapor Axial Deposition (VAD) process or a Soot-Boule process. Corresponding OVD and VAD processes are well known to the person skilled in the art, the Soot-Boule process being known, for example, from US 8,230,701.
[0038] Setting the air number at the above value less than 1 further supports the flame shape according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0039] The individual steps of the method according to the invention are explained in more detail below.
[0040] [Step (1) - Evaporation of Feedstock] In step (1), a feedstock containing at least one organosilicon starting compound is vaporized to form a feedstock vapor. The polymerizable silicon-containing starting compound is preferably a polymerizable polyalkylsiloxane compound.
[0041] In principle, any polymerizable polyalkylsiloxane compound suitable for the production of synthetic quartz glass can be used according to the invention. Within the scope of the present invention, the term polyalkylsiloxane includes both linear (including branched) and cyclic molecular structures.
[0042] Particularly preferred cyclic representatives have the general empirical formula S p O p (R) 2p Here, p is an integer equal to or greater than 3, and the group "R" is an alkyl group, in the simplest case a methyl group.
[0043] Polyalkylsiloxanes are characterized by a particularly high silicon content per weight fraction, which contributes to the economy of their use in the production of synthetic quartz glass.
[0044] The polyalkylsiloxane compound is preferably selected from the group consisting of hexamethylcyclotrisiloxane (D3), octamethylcyclotetrasiloxane (D4), decamethylcyclopentasiloxane (D5), dodecamethylcyclohexasiloxane (D6), tetradecamethylcycloheptasiloxane (D7), hexadecamethylcyclooctasiloxane (D8), their linear homologues, and any mixtures of these compounds. The designations D3, D4, D6, D7, and D8 are adapted from the designation introduced by General Electric Inc., where "D" represents the group [(CH 3 ) 2 Si]-O-.
[0045] Within the scope of the present invention, mixtures of the aforementioned polyalkylsiloxane compounds may also be used.
[0046] Octamethylcyclotetrasiloxane (OMCTS) is currently preferred due to its availability in high purity and in large quantities, and therefore, within the scope of the present invention, it is particularly preferred if the polyalkylsiloxane compound is octamethylcyclotetrasiloxane (D4).
[0047] In principle, it is possible for the feedstock to be subjected to purification before being introduced into step (1). Such purification processes are known to those skilled in the art. However, in a preferred embodiment, the feedstock is not previously subjected to an upstream purification process.
[0048] The evaporation of the raw material can be carried out in the presence or absence of a carrier gas component. Preferably, the raw material is evaporated in the presence of a carrier gas, since the evaporation can be carried out at a temperature below the boiling point of the organosilicon starting compound. As the carrier gas, an inert gas, such as nitrogen or argon, is typically used. When a carrier gas is used, the molar ratio of the organosilicon starting compound to the carrier gas is preferably in the range of 0.01 to 2; more preferably in the range of 0.02 to 1.5, and most preferably in the range of 0.05 to 1.25. In particular, it is preferred to use nitrogen with a moisture content of <40 ppm by volume as the carrier gas and OMCTS as the organosilicon starting compound. Furthermore, it is preferred that the molar ratio of OMCTS to nitrogen is in the range of 0.015 to 1.5.
[0049] The evaporation step is known to the person skilled in the art. Depending on the selected molar ratio of organosilicon starting compound and carrier gas, the organosilicon starting compound is converted into the vapor phase, preferably at a temperature of 120-200 ° C. The evaporation temperature in the evaporation chamber is preferably always at least a few degrees higher than the dew point of the organosilicon starting compound. The evaporation temperature in the evaporation chamber is preferably always at least a few degrees higher than the dew point of the organosilicon starting compound. The dew point likewise depends on the selected molar ratio of organosilicon starting compound and carrier gas. In a preferred embodiment, this is achieved by preheating the organosilicon starting compound to a temperature of 40-120 ° C before evaporation and then spraying it into the evaporation chamber, which has a higher temperature than the preheat of the raw material. In a preferred embodiment, the inert carrier gas can additionally be preheated to a temperature of up to 250 ° C before being fed into the evaporation chamber. It is advantageous that the temperature in the evaporation chamber is always on average higher than the dew point temperature of the mixture of organosilicon starting compound and carrier gas. Suitable evaporation processes are described, for example, in International Applications WO2013 / 087751A and WO2014 / 187513A and in German Patent Application DE 10 2013 209 673.
[0050] Within the scope of the present invention, the term "dew point" describes the temperature at which equilibrium is reached between condensing and evaporating liquids.
[0051] Within the scope of the present invention, "vaporization" is understood to be the process in which raw material is essentially converted from liquid phase to gas phase.This is preferably carried out by using a temperature that is equal to or higher than the dew point of the organosilicon starting compound as the main component of the raw material, as described above.Those skilled in the art will recognize that, from the viewpoint of process engineering, the possibility of small liquid droplets of raw material being entrained cannot be excluded.Thus, in step (1), a raw material containing preferably more than 97 mol%, preferably more than 98 mol%, particularly preferably more than 99 mol%, very particularly preferably more than 99.9 mol% of gaseous components is generated.
[0052] The vaporized organosilicon starting compound, or a mixture of vaporized organosilicon starting compound and carrier gas, is typically removed from the evaporation chamber and fed to a burner. Prior to being fed to the burner, the vaporizable material or mixture of vaporizable material and carrier gas is preferably mixed with oxygen. In the flame, the organosilicon starting compound is converted to SiO 2 The fine particles of amorphous SiO 2 (SiO 2 A porous mass (soot) is formed which is deposited in the form of a porous mass, first on the surface of the carrier and then on the surface of the forming soot body.
[0053] [Step (2): A raw material vapor is supplied to a reaction section, and the raw material vapor is burned in a flame in the presence of oxygen to produce SiO by oxidation and / or hydrolysis. 2 Convert to soot particles] In step (2), the gaseous raw material vapor obtained in step (1) is supplied to a reaction section, and the raw material vapor is oxidized and / or hydrolyzed to produce SiO 2 Convert it into particles.
[0054] This step corresponds in particular to the known soot process or to the known direct vitrification, the possible designs of these two processes being known to the person skilled in the art.
[0055] For the combustion of the raw material vapor, a concentric burner in which a plurality of gas outlet nozzles are arranged in a circle around the center of the burner port is usually used.
[0056] Within the scope of the present invention, a method is preferred in which the first, silicon-containing starting component is fed to the deposition burner in a central region, an oxygen flow is fed to the burner in an outer region, and a separation gas flow (hydrogen) is fed between the central and outer regions.
[0057] A central nozzle is typically used to feed the feed steam, which within the scope of the present invention is typically premixed with a carrier gas, and preferably oxygen is added to the feed steam, resulting in a feed stream from the central nozzle of a typically used concentric burner that contains carrier gas and oxygen in addition to the feed steam.
[0058] The central nozzle of the burner is usually surrounded by a second nozzle, arranged concentrically around the central nozzle, through which a separation gas is introduced into the burner. This separation gas is a mixture of SiO2 and SiO3 from a further oxygen stream entering the burner through another concentric nozzle arranged concentrically around the central nozzle and the separation gas nozzle. 2 The starting compound is separated.
[0059] According to the present invention, in a target-free and generally substantially undisturbed flame, the full width at half maximum (FWHM) of the vertical emission intensity is vert ) of the horizontal emission intensity full width at half maximum (FWHM hori ) is greater than 10, where the luminous intensity is in candela / mm 2 First, the gas flow rate is made the same in a targetless flame, and the half-width of the emission intensity in the horizontal and vertical directions is measured.
[0060] SiO produced by deposition torch 2 The soot particles are usually deposited on a carrier tube rotating about its longitudinal axis, such that the soot body is built up layer by layer. For this purpose, the deposition torch can be moved back and forth along the longitudinal axis of the carrier tube between two turning points. Furthermore, it is preferred to use a burner block in which several deposition burners, each with one flame, are arranged. When using a burner block, at least one flame is preferably provided with the characteristic according to the invention (full width at half maximum of the emission intensity in the vertical direction (FWHM vert ) of the horizontal emission intensity full width at half maximum (FWHM horiIn a further preferred embodiment, all flames of the burner block have the properties according to the invention.
[0061] In the scope of the present invention, it has been found that the yield is further favorable when the air ratio, i.e., the ratio of oxygen to the raw material, is 1 or less. Therefore, according to the present invention, in step (2), the raw material steam to be hydrolyzed and / or polymerized and other fuel gases (e.g., H from another nozzle) are 2 or CH 4 ), it is further preferred that oxygen be used in less than stoichiometric amounts.
[0062] More preferably, the air number is 0.95 or less, even more preferably 0.90 or less, even more preferably 0.85 or less, even more preferably 0.80 or less, even more preferably 0.78 or less, even more preferably 0.76 or less.
[0063] Even by setting the air number to a value less than 1, the characteristics of the flame used according to the invention are influenced, resulting in an increase in deposition efficiency, so that the full width at half maximum (FWHM) of the vertical emission intensity according to the invention is vert ) of the horizontal emission intensity full width at half maximum (FWHM hori By adjusting the ratio of the air flow rate to the total air volume, and setting the air number within the above-mentioned preferred range, it is possible to further improve the deposition efficiency.
[0064] The use of a more concentrated combustion mixture (with an air number less than 1) leads to slower, localized ignition only at the periphery of the flame. Initially, sufficient O2 is released from the oxidizer nozzle. 2Only the outer edge of the delivery nozzle flow, where the oxygen has already diffused, ignites. The center of the flame is more difficult to ignite due to the excessively rich mixture. As a result, less gas can ignite at the same time and the oxygen must first diffuse inwards. The flame becomes more turbulent due to the expansion of the hot combustion gases from the ignited area. This effect is self-reinforcing, as the increased turbulence promotes mixing with the oxygen. The gas body with the ignitable mixture extends further upwards in the method of the invention and expands less laterally. This results in a much more laminar flame. A related effect is that the narrower, more laminar flame attaches itself better to the soot body and forms more stable stagnation points. This reduces the amount of SiO 2 The particles have a shorter diffusion path to the deposition surface of the soot body and a longer residence time at the residence point, resulting in an overall higher deposition efficiency.
[0065] The reduced ignition ability in the richer gas configuration also reduces the average diameter of the gas region that ignites (smaller "flamelets"). The large increase in volume due to thermal expansion and molar increase from decomposition (e.g., one mole of OMCTS gas produces x times the number of moles of combusted gas) creates pressure waves that make the flame more turbulent. The longer combustion region from the richer gas configuration therefore results in a laminar flame with a longer burn length with the advantages mentioned above. At the burner and flame center in the process according to the invention, only the feed stream (containing oxygen) and hydrogen are present, both of which are too concentrated to ignite quickly, and the oxygen O from the outer nozzle is too low. 2 However, it must be taken into account that due to the lower turbulence, it will be dispersed over a longer distance and reach the center slower.
[0066] Within the scope of the present invention, the feedstock is preferably fed to the combustion section together with carrier gas and oxygen from the central nozzle of the concentric burner, so it must be taken into account that the amount of oxygen used in the air number calculation results from a mixture of the oxygen contained in the feedstock stream and the additional oxygen used in the outer nozzle (combustion gas or oxidizing gas) of the concentric burner.
[0067] [Step (3)-SiO 2 Particle Deposition In step (3), the SiO 2 The particles are deposited on a deposition surface, the design of which is within the knowledge of one skilled in the art.
[0068] For this purpose, the SiO 2 The particles are deposited layer by layer on a rotating carrier to form a porous soot body.
[0069] During deposition of the soot particles, the distance between the torch and the support is varied as necessary to satisfy the above conditions.
[0070] [Step (4) - Drying and vitrification (if necessary)] In step (4), the SiO 2 produced in step (3) is optionally 2 The particles are dried and vitrified to form synthetic quartz glass, a step which is particularly necessary if the previous steps were carried out according to the soot process, the design of which is within the knowledge of a person skilled in the art.
[0071] SiO in step (3) 2 The temperature during particle deposition is so low that the porous SiO 2 The method according to the invention is particularly suitable for the production of quartz glass by the "soot process", in which a soot layer is obtained, which is dried and vitrified in a separate step (4) to form synthetic quartz glass.
[0072] The method according to the invention is suitable for the production of synthetic quartz glass carried out as an external deposition process or an internal deposition process. If the method according to the invention is carried out as an external deposition process, it is preferably an OVD process (outside vapor deposition), a VAD process (vapor axial deposition) or a soot boule process.
[0073] The process according to the invention can reduce the manufacturing costs of quartz glass.
[0074] A further object of the present invention is to provide an apparatus for producing synthetic quartz glass, said apparatus comprising: (a) at least one vaporizer section for vaporizing at least one feedstock material comprising at least one organosilicon starting compound to form a feedstock vapor; (b) The raw material vapor is supplied from the evaporator section (a), and the raw material is thermally decomposed or hydrolyzed to produce SiO 2 At least one reaction section for converting the gas into particles, the reaction section including a burner; (c) SiO produced by the reaction part (c) 2 At least one deposition station for depositing particles to form synthetic quartz glass, said deposition station consisting of a soot body.
[0075] The device according to the present invention is characterized in that the burner used has a vertical full width at half maximum (FWHM) of the emission intensity in the absence of a target. vert ) of the horizontal emission intensity full width at half maximum (FWHM hori ) is designed to produce a flame with a ratio of greater than 10.
[0076] For the definition of vertical and horizontal luminance intensity, see above.
[0077] In accordance with the above considerations of the method according to the invention, the burner flame, in the absence of a target, has a vertical full width at half maximum (FWHM vert ) of the horizontal emission intensity full width at half maximum (FWHM hori ) is adjusted to be preferably greater than 12, more preferably greater than 14, and even more preferably greater than 15.
[0078] Further relevant features are described in the method description above.
[0079] Finally, the invention relates to the use of the device for the production of synthetic quartz glass.
[0080] [Example] In a vaporizer according to the embodiment of International Patent Application PCT / EP2012 / 075346, the liquid feedstock OMCTS is vaporized at 170° C. with nitrogen as carrier gas preheated to 180° C. The nitrogen-OMCTS vapor mixture is mixed with oxygen (mixed O 2 ) into a concentric burner, the burner being operated under the following conditions:
[0081] [Table 1]
[0082] [Table 2]
[0083] [Table 3]
[0084] [Table 4] [Brief description of the drawings]
[0085] The burner configuration used in these examples is shown in FIG. 1, and its meaning is as follows. 1: inner nozzle, 2: Intermediate nozzle, and 3: Outer nozzle.
[0086] The method according to the invention (Example 1) results in improved deposition efficiency over the comparative examples (Examples 2 and 3).
[0087] In the above experiment, SiO 2 The synthetic flame emission intensity was calibrated as follows.
[0088] Calibration of the flame emission intensity was performed against calibrated light sources (K-150WH from LOT-Oriel and constant SLP120-80 / snTD4541060001 from Gossen-Metrawatt; first calibration opto.cal SCS 053, certificate number 09333, 4.11.2009; second calibration opto.cal SCS 053, certificate number 16428, 9.12.2016).
[0089] To calibrate the camera sensitivity, a calibration light source was installed at a typical distance where measurements will be performed. In our setup, the working distance is 450mm. Due to the perfect Lambertian emission characteristics, the emission intensity follows a 1 / r2 behavior, so in the experiment the luminous flux can be calculated in opto.cal using the distance used for the calibration as the working distance.
[0090] In the calibration protocol, illuminance is the parameter to be calibrated. In this calibration, luminance is more appropriate since it refers to the luminous area. Therefore, the unit of illuminance is [Ev]=lm / m 2 =lx is the unit of luminance [Lv]=cd / m 2 or Cd / mm 2 was converted to.
[0091] For Lambertian radiators, this conversion requires additional knowledge of distance during calibration and measurement. This particular source has an illuminance of Ev=293.5lx at a distance of 250mm and an illuminance of Iv=90.59Cd at a distance of 450mm, the working distance of the experiment. The units of luminance are in detector units, i.e., relative to the area of the detector, integrated over the total emitted light. Emitter-based measurements include the effective area of the emitter, resulting in units of luminance.
[0092] The application of photometric units (lux / lumens / candela) uses the CIE luminance function to mimic the spectral sensitivity of the human eye. Calibration light sources and flame radiation have different spectral characteristics. Therefore, the CIE luminance function is used to weight the wavelength-dependent emission to obtain the photometric units.
[0093] The camera used was a Basler acA1300-200um equipped with a Basler C125-0818-5M-P f8mm. The camera was set up once to obtain a technically useful measurement signal, and then the focal length, aperture and camera position relative to the flame were fixed and kept constant during the measurements.
[0094] The spectrally resolved emission spectra of the calibration sources are reported in the calibration protocol with a wavelength resolution of 2 nm from 280 nm to 800 nm, which is large enough to cover the entire CIE luminous intensity function. The emission from the flame was spectrally resolved at different conditions.
[0095] With these prerequisites, it is possible to measure the luminous intensity of a flame against a calibrated light source that is traceable to the Swiss Metrology Office.
Claims
1. (1) vaporizing a feedstock comprising at least one organosilicon starting compound to form a feedstock vapor; (2) The raw material vapor from step (1) is supplied to a reaction section, and the raw material vapor is burned in a flame in the presence of oxygen to produce SiO by oxidation and / or hydrolysis. 2 converting the soot particles into (3) The SiO produced in step (2) 2 depositing soot particles on a deposition surface to form a soot body; (4) optionally drying and vitrifying the soot body produced in step (3) to form synthetic quartz glass; A method for producing a synthetic quartz glass comprising the steps of: The synthetic flame used in the method has a vertical full width at half maximum (FWHM) of luminous intensity in the absence of a target. vert ) of the horizontal emission intensity full width at half maximum (FWHM hori ) is greater than 12; The full width at half maximum of the vertical emission intensity (FWHM vert ) is calculated as follows: From the two-dimensional camera image, each horizontal pixel row of the camera is integrated in the horizontal direction to determine the integrated horizontal luminous intensity, which is the luminous intensity of the flame (unit: cd / mm2); The horizontal integrated luminous intensity is calculated per burner distance (each row) or flame height (results in cd / mm); the horizontal integrated luminous intensity is obtained as a function of vertical distance from the burner; The full width at half maximum (unit: mm) of the emission intensity in the vertical direction is calculated from the curve shape in which the function of the vertical distance from the burner is maximized at a predetermined burner distance; and The full width at half maximum of the horizontal light emission intensity (FWHM hori ) is calculated as follows: From the two-dimensional camera image, each vertical pixel row of the camera is vertically integrated to obtain the integrated vertical luminous intensity, which is the luminous intensity of the flame (unit: cd / mm2); The vertical integrated luminous intensity is calculated for each horizontal distance to the left and right from the burner central axis (results in units of cd / mm); the vertical integrated luminous intensity is obtained as a function of horizontal distance to the left and right of the burner central axis; The function of horizontal distance to the left and right of the burner central axis determines the half-width (unit: mm) of the horizontal emission intensity from the curve shape that is maximum near the burner central axis. A method for producing synthetic quartz glass comprising the steps of:
2. The flame used in the method has a vertical full width at half maximum (FWHM) of luminous intensity in the absence of a target. vert ) of the horizontal emission intensity full width at half maximum (FWHM hori 2. The method of claim 1, wherein the ratio of
3. The flame used in the method has a vertical full width at half maximum (FWHM) of luminous intensity in the absence of a target. vert ) of the horizontal emission intensity full width at half maximum (FWHM hori 3. The method of claim 1, wherein the ratio of 1 to 15 is greater than 15.
4. 4. The method according to any one of claims 1 to 3, characterized in that the burner gases actively supplied in step (2) have a total air number of 1 or less.
5. 5. The method according to any one of claims 1 to 4, characterized in that the burner gases actively supplied in step (2) have a total air number of 0.85 or less.
6. 6. The method according to any one of claims 1 to 5, wherein the burner gases actively supplied in step (2) have a total air number of 0.76 or less.
7. 7. The method according to claim 1, wherein step (2) is performed by a burner having a concentric cross-section, within which the feed steam is introduced into a burner flame together with oxygen as a feed mixture, and the feed mixture is separated from the oxygen-containing oxidizing gas by a separation gas.
8. 8. The method according to claim 1, wherein the organosilicon starting compound is selected from the group consisting of hexamethylcyclotrisiloxane (D3), octamethylcyclotetrasiloxane (D4), decamethylcyclopentasiloxane (D5), decamethylcyclohexasiloxane (D6), tetradecamethylcycloheptasiloxane (D7), hexadecamethylcyclooctasiloxane (D8), their linear homologues and any mixtures of these compounds.
9. 9. The method of claim 8, wherein the polyalkylsiloxane compound is octamethylcyclotetrasiloxane (D4).
10. Furthermore, determining the full width at half maximum of the vertical emission intensity (FWHM vert ); determining a full width at half maximum (FWHM hori ) of the horizontal light emission intensity; adjusting the synthetic flame used in the method to have a ratio of full width at half maximum of vertical light intensity (FWHM vert ) to full width at half maximum of horizontal light intensity (FWHM hori ) greater than 12 in the absence of a target; 10. The method according to any one of claims 1 to 9, comprising:
11. (a) at least one vaporizer section for vaporizing at least one feedstock material comprising at least one organosilicon starting compound to form a feedstock vapor; (b) The raw material vapor is supplied from the evaporator section (a), and the raw material is converted into SiO by thermal decomposition or hydrolysis. 2 At least one reaction section for converting the gas into particles, the reaction section including a burner having a flame; (c) SiO produced by the reaction section (c) 2 At least one deposition section for depositing particles to form synthetic quartz glass, said deposition section being made of a soot body; A synthetic quartz glass manufacturing apparatus comprising: The burner is designed so that its flame, without a target, has a vertical full width at half maximum (FWHM vert ) of the horizontal emission intensity full width at half maximum (FWHM hori ) is adjusted to be greater than 12, and the luminous intensity is in candela / mm 2 It was measured at The full width at half maximum of the vertical luminous intensity (FWHM vert ) is determined by integrating each horizontal pixel row of the camera in the horizontal direction from the two-dimensional camera image to determine the integrated luminous intensity in the horizontal direction, which is the luminous intensity of the flame (unit: cd / mm 2 ); The horizontal integrated luminous intensity is calculated per burner distance (each row) or flame height (results in cd / mm); the horizontal integrated luminous intensity is obtained as a function of vertical distance from the burner; A half-width (unit: mm) of the emission intensity in the vertical direction is calculated from the curve shape in which the function of the vertical distance from the burner is maximized at a predetermined burner distance; and The full width at half maximum of the horizontal luminous intensity (FWHM hori ) is obtained by vertically integrating each vertical pixel row of the camera from a two-dimensional camera image to obtain an integrated luminous intensity in the vertical direction, which is the luminous intensity of the flame (unit: cd / mm 2 ); The vertical integrated luminous intensity is calculated for each horizontal distance to the left and right from the burner central axis (results in units of cd / mm); the vertical integrated luminous intensity is obtained as a function of horizontal distance to the left and right of the burner central axis; The function of horizontal distance to the left and right of the burner central axis determines the half-width (unit: mm) of the horizontal emission intensity from the curve shape that is maximum near the burner central axis. A synthetic quartz glass manufacturing apparatus comprising:
12. 12. The apparatus of claim 11, wherein the apparatus comprises a burner operated with an air number of 1 or less.
13. 13. Apparatus according to claim 11 or claim 12, characterized in that the apparatus comprises a burner operated at an air number of 0.85 or less.
14. 14. Apparatus according to any one of claims 11 to 13, characterized in that the apparatus comprises a burner operated at an air number of 0.76 or less.
15. Determining the full width at half maximum (FWHM vert ) of the vertical luminous intensity; determining the full width at half maximum of the horizontal luminous intensity (FWHM hori ); and 15. Apparatus according to any one of claims 11 to 14, configured to adjust the flame in a target-free condition such that the ratio of the vertical full width at half maximum (FWHM vert ) to the horizontal full width at half maximum (FWHM hori ) is greater than 12.
16. 16. Use of the device according to any one of claims 11 to 15 for producing synthetic quartz glass.
Citation Information
Patent Citations
Production of base material for optical fiber
JP1984232934A
Method for synthesizing porous preform for optical fiber and apparatus therefor
JP1995223834A
Production of optical fiber preform
JP1995267671A
Production of glass article and apparatus therefor
JP1999246232A
Multiple pipe burner for producing porous glass base material and method and device for producing porous glass base material by use of the same
JP2000327341A