Etching method for MRAM magnetic tunnel junctions
A combined etching method using IBE and RIE with specific parameters forms a rectangular trench and in-situ protection, addressing challenges of conventional etching methods by enhancing TMR performance and product lifespan in MRAM.
Patent Information
- Application Number
- JP2023519989
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-23
- Filing Date
- 2021-06-17
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-06-17
AI Technical Summary
Conventional etching methods for magnetic tunnel junctions in MRAM face challenges in maintaining high profile, preventing re-deposition on sidewalls, and achieving high selectivity and yield, especially for smaller and denser patterns, which are critical for improving TMR performance and product lifespan.
A combined etching method using ion beam etching (IBE) and reactive ion etching (RIE) with specific parameters and sequences, including varying incident angles, gas compositions, and cleaning steps to form a rectangular trench, followed by in-situ protection with a deposited film.
The method enhances etching effectiveness for small and high-density magnetic tunnel junctions, improving TMR performance, reducing residue, and forming a rectangular trench that prevents short circuits, thereby increasing product life and yield.
Smart Images

Figure 0007568841000001 
Figure 0007568841000002 
Figure 0007568841000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of magnetic random access memories, and in particular to a method for etching MRAM magnetic tunnel junctions. [Background technology]
[0002] Currently, the most widely used memories are SRAM (Static Random Access Memory), DRAM (Dynamic Random Access Memory), and Flash (Flash Memory). SRAM has high performance because it can retain stored data without requiring a refresh circuit. However, its integration level is low. DRAM has high integration level and low power consumption, but it needs a refresh circuit to retain data. In contrast, magnetic random access memory (MRAM) has the high read / write speed of SRAM and the high integration level of DRAM, and can be rewritten almost unlimitedly, so it can be used in systems that require high-speed storage of large amounts of data, as well as the ability to retain data and quickly recover data even after a power outage. Currently, only MRAM and Flash have the characteristic of being "non-volatile," but Flash lacks the function of "random access." Therefore, MRAM has great potential for the future, and can play an important role in fields such as automobiles, industry, military, and space.
[0003] Unlike conventional memories that use electric charge to store data, MRAM stores data by magnetization. Figure 1 shows a magnetic tunnel junction, which is the basic structure of an MRAM memory cell. Magnetic tunnel junctions consist of a top layer, which is a free layer whose magnetization direction is not fixed, an intermediate layer, which is a tunnel barrier layer, and a bottom layer, which is a fixed layer whose magnetization direction is fixed. When the magnetization directions of the free layer and the fixed layer are parallel, the electrical resistance of the memory cell is low, and when the magnetization directions are antiparallel, the electrical resistance is high. MRAM determines whether the stored data is 0 or 1 by detecting the magnitude of the electrical resistance of the memory cell.
[0004] Etching of magnetic tunnel junctions is an extremely important part of the manufacturing process of MRAM. Etching equipment mainly uses reactive ion etching (RIE) and ion beam etching (IBE). RIE is an etching method that uses chemical reactions and the collision of ion species. IBE is an etching method that uses an ion beam with a certain energy to collide with the material surface, and has strong directionality. Currently, RIE and IBE are the mainstream etching methods for magnetic tunnel junctions. In both IBE and RIE, the following requirements must be met.
[0005] 1. Maintain a high magnetic tunnel junction profile during etching to improve the performance and lifetime of the Tunnel Magnetoresistance (TMR). 2. To prevent short circuits, the magnesium oxide layer in the magnetic tunnel junction must not re-deposit on the sidewalls. 3. To improve the yield rate of products in subsequent processes, more mask (HM) remains and less residue is left.
[0006] As shown in Figure 2, the conventional IBE has high selectivity, but it causes large damage to the magnesium oxide layer and leaves a lot of residue. In addition, the conventional RIE has low selectivity and poor profile. Therefore, it is difficult to simultaneously meet the above three etching requirements.
[0007] In addition, as the volume of magnetic memory becomes smaller, the spin-polarized current injected for writing and conversion operations also becomes smaller. Therefore, it is desirable to create smaller and denser magnetic tunnel junction patterns and reduce the reduction in the lifetime of memories containing magnetic tunnel junctions due to control. However, it is more difficult to meet the above three etching requirements for smaller and denser magnetic tunnel junctions by conventional IBE or RIE. Summary of the Invention
[0008] The present invention has been made in consideration of the above-mentioned shortcomings of the conventional technology, and provides an etching method for MRAM magnetic tunnel junctions that significantly improves the etching effect on small, high-density magnetic tunnel junctions by combining conventional RIE and IBE and setting the etching order and selecting each etching parameter, while also being applicable to etching of low-density magnetic tunnel junctions.
[0009] In order to solve the above technical problems, the technical solution of the present invention is: A method for etching an MRAM magnetic tunnel junction includes the following steps.
[0010] Step 1 is a main etching step of the magnetic tunnel junction, which uses ion beam etching and / or reactive ion etching to etch the magnetic tunnel junction under the condition that the etching amount is t1, in which the incident angle of the ion beam is 10-60°, and the bias voltage of the reactive ion etching is 400-1000V.
[0011] Step 2 is a cleaning step of the magnetic tunnel junction, in which the magnetic tunnel junction obtained by the magnetic main etching step is etched under the condition that the etching amount is t2. t1:t2 is 0.5 or more, and the etching in the cleaning step includes reactive ion etching in a continuous mode or a pulse mode. The bias voltage of the reactive ion etching is 50V to 400V, and the pulse duty ratio is 5% to 50%. After the etching in the cleaning step is performed, the etching shape formed in the lower electrode or the lower insulating layer is a rectangular trench.
[0012] In step 2, the etching in the cleaning step utilizes a combination of ion beam etching and reactive ion etching. The beam voltage of the ion beam etching is 50V to 200V.
[0013] Further, the method includes step 3, which is an in-situ protection step of the magnetic tunnel junction, in which an insulating layer is grown around the magnetic tunnel junction obtained by etching in the cleaning step using a chemical vapor deposition method to provide in-situ protection.
[0014] The etching amount t2 in the cleaning step is 5 to 100 nm.
[0015] In step 1, the ion beam etching includes ion beam etching with a large incidence angle and ion beam etching with a small incidence angle.
[0016] In ion beam etching with a large incidence angle, the incidence angle of the ion beam is 30 to 60°, and in ion beam etching with a small incidence angle, the incidence angle of the ion beam is 10 to 30°. If the time of ion beam etching with a large incidence angle is T1 and the time of ion beam etching with a small incidence angle is T2, then T1≧1.5T2.
[0017] When ion beam etching is utilized in the main etching step and the cleaning step, the gas used in the ion beam chamber is one or any combination of an inert gas, nitrogen gas, oxygen gas, a fluorine-based gas, an amino-based gas, carbon monoxide gas, carbon dioxide gas, and alcohol.
[0018] When reactive ion etching is used in the main etching step and the cleaning step, the ion source power in the reactive ion chamber is 50 to 1000 W, the pressure in the chamber is 0.5 to 10 mT, the gas flow rate is 10 to 500 sccm, and the gas is one or any combination of an inert gas, nitrogen gas, oxygen gas, a fluorine-based gas, an amino group gas, carbon monoxide gas, carbon dioxide gas, and alcohol.
[0019] If the length of the bottom base of the rectangular trench is L1, the length of the top base of the rectangular trench is L2, the height of the rectangular trench is H1, and the angle between the bottom base and the side edge of the rectangular trench is α, then L1:L2=0.3 to 1.0, H1:L2=0.1 to 2.0, and α=90 to 130°.
[0020] The etching method for MRAM magnetic tunnel junctions includes the following steps. Step 1 is a main etching step of the magnetic tunnel junction, in which the magnetic tunnel junction is etched by ion beam etching under the condition that the etching amount t1 is 35 nm. The ion beam etching is performed by placing the magnetic tunnel junction sample in an ion beam etching chamber and etching under the conditions that the ion beam incidence angle is 25°, the energy is 600 V, and the shield gas is argon gas. The magnetic tunnel junction sample is composed of a mask layer, a cap layer, a magnetic tunnel junction, a lower electrode metal layer, and a lower insulating layer from the top. In the lower insulating layer, metal lower electrodes, the number of which is the same as the number of masks in the mask layer, are fitted at equal intervals corresponding to the positions of the masks. The ion beam etching stops at a position where there is 5 nm left of the lower electrode metal layer. In this case, the ion beam etching amount is 35 nm. Step 2 is a cleaning step of the magnetic tunnel junction, in which the magnetic tunnel junction obtained by the main etching step is etched by reactive ion etching under the condition that the etching amount t2 is 30 nm. The reactive ion etching is performed in a vacuum chamber by moving the magnetic tunnel junction sample obtained by the ion beam etching in step 1 from the ion beam etching chamber to the reactive ion etching chamber. The reactive ion etching parameters are a reactive ion pulse duty ratio of 20%, an ion source power of 700 W, a bias voltage of 400 V, a chamber pressure of 5 mT, an argon gas flow rate of 100 sccm, and a reactive ion etching amount of 30 nm. After the etching in the cleaning step is performed, the etching shape formed in the lower insulating layer is a rectangular trench. Step 3 is an in situ protection step of the magnetic tunnel junction, in which the magnetic tunnel junction sample obtained by etching in the cleaning step in the vacuum transport chamber is transferred to a plasma-enhanced chemical vapor deposition chamber and a 35 nm SiN film is deposited for in situ protection.
[0021] The etching method for MRAM magnetic tunnel junctions includes the following steps.
[0022] Step 1 is a main etching step of the magnetic tunnel junction, which uses reactive ion etching to etch the magnetic tunnel junction under the condition that the etching amount t1 is 20 nm. The reactive ion etching is performed by placing the magnetic tunnel junction sample in a reactive ion etching chamber and etching under the conditions that the ion source power of the reactive ion etching is 600 W, the bias voltage is 600 V, the pressure in the chamber is 10 mT, and the argon gas flow rate is 150 sccm. The magnetic tunnel junction sample to be etched is composed of a mask layer, a cap layer, a magnetic tunnel junction, a lower electrode layer, and a lower insulating layer from the top. The reactive ion etching is stopped at the position where the lower electrode layer is consumed by 3 nm. In this case, the reactive ion etching amount is 20 nm.
[0023] Step 2 is a cleaning step of the magnetic tunnel junction, in which the magnetic tunnel junction obtained by the main etching step is etched by reactive ion etching under the condition that the etching amount t2 is 15 nm. The etching parameters of the reactive ion etching are a reactive ion pulse duty ratio of 30%, an ion source power of 300 W, a bias voltage of 600 V, a chamber pressure of 1.5 mT, an argon gas flow rate of 200 sccm, and a reactive ion etching amount t2 of 15 nm. After the etching in the cleaning step is performed, the etching shape formed in the lower insulating layer is a rectangular trench.
[0024] Step 2A is an ion beam cleaning step in which the magnetic tunnel junction sample obtained by etching in the cleaning step in a vacuum chamber is moved to an ion beam etching chamber and etched so as to stop on the lower electrode layer in an argon atmosphere under conditions of an ion beam incidence angle of 45°, an ion beam energy of 100 V, and an etching depth of 3 nm.
[0025] Step 3 is an in situ protection step of the magnetic tunnel junction, in which the magnetic tunnel junction sample obtained by the ion beam cleaning step in the vacuum transport chamber is transferred to a plasma enhanced chemical vapor deposition chamber and a 10 nm SiN film is deposited for in situ protection.
[0026] The present invention has the following beneficial effects. By combining conventional RIE and IBE, and setting the etching sequence and selecting each etching parameter, the present invention can greatly improve the etching effect for small and high-density magnetic tunnel junctions, and can also be applied to etching for non-high-density magnetic tunnel junctions. Therefore, the problems of low selectivity and low profile in etching of high-density patterns are solved. Furthermore, the most important feature of the present invention is that a rectangular etching trench can be formed at the bottom. This can greatly improve the TMR and product life of the magnetic tunnel junction, and can remove the deposition at the bottom. [Brief description of the drawings]
[0027] [Figure 1] FIG. 1 is a schematic diagram of the structure of a magnetic tunnel junction. [Diagram 2] FIG. 1 is a comparison diagram of the etching effect of the present invention with that of conventional RIE or IBE, in which etching stops at the insulator SiO2. [Diagram 3] FIG. 2 is a schematic diagram of a layered configuration of a sample formed by etching according to the present invention. [Figure 4] FIG. 1 is a comparison diagram of the etching effect of the present invention with that of conventional RIE or IBE, in which the etching stops at the bottom electrode metal. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] The present invention will now be described in more detail with reference to the drawings and preferred specific embodiments.
[0029] In the description of the present invention, the directions or positional relationships expressed by terms such as "left", "right", "upper", and "lower" are based on the drawings and are merely for the purpose of conveniently and simply describing the present invention, and do not necessarily expressly or imply that the relevant device or element has a specific direction, or is configured or operated in a specific direction. It should be understood that "first", "second", etc. do not indicate the importance of the parts, and therefore do not limit the present invention. The specific dimensions used in this embodiment are merely examples for explaining the technical solution, and do not limit the protection scope of the present invention.
[0030] As shown in FIG. 1, the etching method for MRAM magnetic tunnel junctions includes the following steps:
[0031] Step 1, which is the main etching step: reactive ion etching (RIE) or ion beam etching (IBE).
[0032] The wafer is placed in a corresponding reaction chamber and the first etching is carried out on the magnetic tunnel junction sample to be etched.
[0033] As shown in Figure 2, the magnetic tunnel junction sample to be etched is composed of, from top to bottom, a mask layer, a metal layer (also called a cap layer or cover layer), a magnetic tunnel junction, a metal layer (also called a seed layer), and a lower insulating layer.
[0034] The mask layer includes several masks arranged at equal intervals on the cap layer. In the lower insulating layer, the same number of lower electrodes as the number of masks are fitted at equal intervals at positions corresponding to the masks. Furthermore, the lower insulating layer is preferably made of silicon dioxide or the like.
[0035] As shown in Fig. 4, the magnetic tunnel junction sample to be etched is composed of a mask layer, a metal layer (also called a cap layer or cover layer), a magnetic tunnel junction (MTJ), a metal layer (also called a seed layer), a lower electrode, and a lower insulating layer, from the top. The arrangement of the masks in the mask layer is the same as that in Fig. 2. Preferably, the lower insulating layer is made of silicon dioxide or the like.
[0036] Preferably, the process conditions for ion beam etching (IBE) are an ion beam incidence angle of 10 to 60° (the angle between the ion beam and the normal to the wafer), energy of 200 to 1000 V, and a shield gas of one or any combination of an inert gas, nitrogen gas, oxygen gas, fluorine-based gas, amino-based gas, carbon monoxide gas, carbon dioxide gas, alcohol, etc. Furthermore, preferably, an inert gas such as argon gas, krypton gas, or xenon gas is used.
[0037] Preferably, the reactive ion etching (RIE) process conditions are an ion source power of 50 to 1000 W, a chamber pressure of 0.5 to 30 mT, a gas flow rate of 10 to 500 sccm, and the gas is one or any combination of an inert gas, nitrogen gas, oxygen gas, a fluorine-based gas, an amino group gas, carbon monoxide gas, carbon dioxide gas, and alcohol.
[0038] In step 1, the etching amount of the main etching step is t1.
[0039] Using ion beam etching (IBE) or reactive ion etching (RIE) in step 1 provides the following beneficial effects.
[0040] 1. By setting the incidence angle of the ion beam, the profile of the first etching can be effectively guaranteed and the CD (the dimension of the magnesium oxide layer in the magnetic tunnel junction) consumption can be reduced. The main etching step by RIE can etch the metal layer quickly and cause less damage to the sidewall of the magnesium oxide layer.
[0041] In the IBE of this embodiment, the incidence angle of the ion beam is preferably variable. The IBE includes an IBE with a large incidence angle and an IBE with a small incidence angle. The large incidence angle usually refers to an incidence angle of the ion beam of 30 to 60°, and the small incidence angle usually refers to an incidence angle of the ion beam of 10 to 30°. If the time of the IBE with the large incidence angle is T1 and the time of the IBE with the small incidence angle is T2, it is preferable that T1≧1.5T2.
[0042] 2. Etching is performed using an inert gas, resulting in clean sidewalls with high profiles.
[0043] 3. By increasing the ratio of the etching amount t1 in the main etching step, the recess amount and profile can be improved.
[0044] Step 2 is a cleaning step. The magnetic tunnel junction sample obtained by performing the main etching step, which is step 1, in a vacuum chamber is moved to a chamber performing the corresponding cleaning step, and a secondary etching in the cleaning step is performed in the chamber performing the cleaning step.
[0045] The etching in the cleaning step has two preferred embodiments:
[0046] First embodiment: Reactive ion etching in continuous or pulsed mode.
[0047] Second embodiment: Reactive ion etching in continuous or pulsed mode, and low energy ion beam etching.
[0048] Preferably, the reactive ion etching (RIE) process conditions are a reactive ion pulse (Pulsing) duty ratio of 5% to 50%, an ion source power (Source) of 50 to 1000 W, a bias voltage of 10 to 1000 V, a chamber pressure of 0.5 to 10 mT, a gas flow rate of 10 to 500 sccm, and one or any combination of an inert gas, nitrogen gas, oxygen gas, a fluorine-based gas, an amino group gas, carbon monoxide gas, carbon dioxide gas, alcohol, etc. Furthermore, preferably, an inert gas such as argon gas or an oxygen-containing gas is used.
[0049] Preferably, the process conditions for ion beam etching (IBE) are an incidence angle of 30 to 60° (the angle between the ion beam and the normal to the wafer), energy of 50 to 200 V, and a shield gas of one or any combination of an inert gas, nitrogen gas, oxygen gas, fluorine-based gas, amino-based gas, carbon monoxide gas, carbon dioxide gas, alcohol, etc. Furthermore, it is preferable to use an inert gas such as argon gas, krypton gas, or xenon gas.
[0050] In step 2, the etching amount in the cleaning step is t2. Preferably, t2 is 5 to 40 nm, and t1:t2 is 0.5 or more. Preferably, the ratio of the etching amounts in the two etching steps is t1:t2=1.5 to 4.0.
[0051] After the second etching is performed, the etched shape of the lower electrode and / or the lower insulating layer becomes the rectangular trench shown in FIGS.
[0052] The rectangular etched trench of the MRAM magnetic tunnel junction formed at the bottom is formed in the lower electrode or the lower insulating layer, and is formed to have a substantially rectangular shape. As shown in FIG. 2, the rectangular trench is formed in the lower insulating layer. As shown in FIG. 4, the rectangular trench is formed in the lower electrode. Alternatively, the rectangular trench may be formed in both the lower electrode and / or the lower insulating layer in FIG. 4.
[0053] If the length of the lower base of the rectangular trench (corresponding to the square trench length in FIG. 3) is L1, the length of the upper base of the rectangular trench (corresponding to the space in FIG. 3) is L2, the height of the rectangular trench (corresponding to the recess in FIG. 3) is H1, and the angle between the lower base and the side of the rectangular trench is α, then α=90-130°, which means that the rectangular trench is substantially L-shaped, and thus the rectangular trench is formed substantially rectangular. Preferably, L1:L2=0.3-1.0, and H1:L2=0.1-2.0.
[0054] Due to factors such as charge accumulation effect and selectivity, it is more difficult to form a rectangular etching trench with a small-sized dense pattern than with a conventional pattern. According to the present invention, it is possible to form a rectangular trench by etching even when the pattern density is 80 to 100 nm pitch.
[0055] In step 2, the use of low energy ion beam etching or reactive ion etching in continuous or pulsed mode provides the following beneficial effects:
[0056] 1. Low energy and pressure improves the ability to remove residues and ensure no sidewall redeposition in the right process window.
[0057] 2. The low energy reduces damage to the sidewall of the magnesium oxide layer.
[0058] 3. Etching with an inert gas such as argon also results in clean sidewalls with high profiles. Also, etching with an oxygen-containing gas oxidizes the sidewalls, so etching with a reactive gas can increase the selectivity.
[0059] 4. The profile formed in the main etching step can be maintained, so the final profile is 75 to 90 degrees. Even if the center distance (pitch) of the two units is 100 nm or less, the profile can be 85 degrees or more.
[0060] 5. Significantly improve the selectivity compared with conventional single etching methods.
[0061] 6. A rectangular etching trench may be formed at the bottom. The bottom of the rectangular trench is flat and no or only a small amount of residue is left. The rectangular etching trench may be formed in the insulating layer or the lower electrode layer. The corner of the bottom of the rectangular trench may be formed in an L-shape. After etching and deposition, the deposition remains in an L-shape.
[0062] 7. The angle of the obtained rectangular trench is 90 to 130°. The length L1 of the lower bottom of the rectangular trench is 0.5 to 1.0 times the length L2 of the upper bottom of the rectangular trench. When the recess:space is 0.5 to 2 and the depth to width ratio (total height:space) is 1.0 to 5.0, a good rectangular trench shape is obtained.
[0063] Step 3 is deposition. Deposition is performed on the magnetic tunnel junction sample obtained by etching. The deposition layer is made of silicon nitride or silicon dioxide, or a combination of both. The thickness of the deposition layer is 10-100 nm, and the deposition temperature is 150-350°C. Such an in-situ protective film can prevent the metal stack of the magnetic tunnel junction from being corroded by water vapor in the air, which may cause the device to short circuit.
[0064] The present invention will now be described in further detail with the aid of the following four specific preferred embodiments.
[0065] Example 1 Step 1 is the main etching step using reactive ion etching. The magnetic tunnel junction sample shown in Figure 2 was placed in the RIE chamber and the main etching was performed. In the main etching step, the ion source power, which is the energy, was 500 W, the bias voltage power was 600 W, the chamber pressure was 20 mTorr, and the etching gas was Kr.
[0066] The reactive ion etching is stopped at a position from 10 nm remaining in the lowermost metal layer to a depth of 40 nm in the lower insulating layer. In the first embodiment, the primary etching is preferably stopped at a position where 5 nm remains in the lowermost metal layer, and the etching amount t1 is 35 nm.
[0067] Step 2 is a cleaning step that utilizes a combination of reactive ion etching (RIE) and ion beam etching (IBE).
[0068] Step 21 is reactive ion etching (RIE). In a vacuum chamber, the magnetic tunnel junction sample obtained by the main etching step of step 1 was subjected to secondary reactive ion etching. The parameters of the secondary reactive ion etching were an ion source power of 700 W, a bias voltage of 400 V, a pressure in the chamber of 5 mT, and an argon gas flow rate of 100 sccm.
[0069] Step 22 is ion beam etching. The magnetic tunnel junction sample obtained by performing the secondary reactive ion etching in step 21 in the vacuum chamber is moved from the RIE chamber to the IBE chamber, and ion beam etching is performed. Preferably, the process conditions of the ion beam etching are BMV of 100 V, incident angle of 60°, and etching gas of Ar. The etching depth, i.e., the ion beam etching amount t2, is 30 nm. After the secondary etching is performed, the etching shape formed on the lower insulating layer is a rectangular trench.
[0070] Step 3 is deposition: the sample obtained by ion beam etching in the vacuum transfer chamber was transferred to a plasma enhanced chemical vapor deposition chamber to deposit a 30 nm SiN film for in situ protection.
[0071] In the rectangular trench obtained in this embodiment, the length of the lower base (corresponding to the square trench length in FIG. 3) is L1, the length of the upper base (corresponding to the space in FIG. 3) is L2, the height (corresponding to the recess in FIG. 3) is H1, and the angle between the lower base and the side is α, so α=120°, i.e., it is approximately L-shaped, so it is formed into an approximately rectangular shape. Also, L1:L2=0.5, H1:L2=0.5.
[0072] Example 2 Step 1 is the main etching step using reactive ion etching. The magnetic tunnel junction sample shown in Figure 4 was placed in the reactive ion chamber. In the reactive ion etching, the ion source power was 600 W, the bias voltage was 600 V, the chamber pressure was 10 mT, and the argon gas flow rate was 150 sccm. The magnetic tunnel junction sample to be etched is composed of a mask layer, a cap layer, a magnetic tunnel junction, a lower electrode layer, and a lower insulating layer, from the top. The reactive ion etching is stopped at the position where the lower electrode layer is consumed by 3 nm. In this case, the reactive ion etching amount is 20 nm.
[0073] Step 2 is a cleaning step using reactive ion etching. Preferably, the process conditions for the secondary etching are a reactive ion pulse duty ratio of 5%, a reactive ion source power of 300 W, a bias voltage of 600 V, a chamber pressure of 1.5 mT, an argon gas flow rate of 200 sccm, and etching to the seed layer by 30 nm, i.e., a reactive ion etching amount t2 of 15 nm. After the secondary etching is performed, the etching shape formed on the lower electrode is a rectangular trench.
[0074] Step 2A is ion beam cleaning. In the vacuum chamber, the secondary etching sample was moved to the IBE chamber and etched under the conditions of ion beam angle 45°, ion beam energy 100V, and argon gas atmosphere. The etching depth was 3 nm and stopped at the bottom electrode layer. Figure 4 shows a comparison diagram of the shapes.
[0075] Step 3 is in-situ protection for the magnetic tunnel junctions. In the vacuum transport chamber, the magnetic tunnel junction samples after ion beam cleaning were transferred to a plasma enhanced chemical vapor deposition chamber, where a 10 nm SiN film was deposited for in-situ protection.
[0076] In the rectangular trench obtained in this embodiment, the length of the lower base (corresponding to the square trench length in FIG. 3) is L1, the length of the upper base (corresponding to the space in FIG. 3) is L2, the height (corresponding to the recess in FIG. 3) is H1, and the angle between the lower base and the side is α, so α=110°, that is, it is approximately L-shaped, so it is formed into an approximately rectangular shape. Also, L1:L2=0.6, H1:L2=0.8.
[0077] Example 3 Step 1 is the main etching step using ion beam etching. The magnetic tunnel junction sample was placed in an ion beam etching chamber and etched under the conditions of an ion beam incidence angle of 25°, energy of 600V, and argon gas as the shielding gas. The magnetic tunnel junction sample is composed of a mask layer, a cap layer, a magnetic tunnel junction, a lower electrode metal layer, and a lower insulating layer from the top. In the lower insulating layer, metal lower electrodes, the number of which is the same as the number of masks in the mask layer, are fitted at equal intervals corresponding to the positions of the masks. The ion beam etching stops at a position where 5 nm remains in the bottom metal layer, i.e., the ion beam etching amount t1 is 35 nm.
[0078] Step 2 is a cleaning step using reactive ion etching. The magnetic tunnel junction sample obtained by ion beam etching in step 1 in a vacuum chamber was moved from the ion beam etching chamber to the reactive ion etching chamber for secondary etching. The parameters of the secondary etching were reactive ion pulse duty ratio of 20%, ion source power of 700 W, bias voltage of 400 V, chamber pressure of 5 mT, argon gas flow rate of 100 sccm, and reactive ion etching amount t2 of 30 nm. After the secondary etching, the etched shape formed on the lower insulating layer was a rectangular trench.
[0079] Step 3 is deposition: After the second etching in the vacuum transfer chamber, the sample was transferred to a plasma-enhanced chemical vapor deposition chamber, where a 35 nm SiN film was deposited for in situ protection.
[0080] In the rectangular trench obtained in this embodiment, the length of the lower base (corresponding to the square trench length in FIG. 3) is L1, the length of the upper base (corresponding to the space in FIG. 3) is L2, the height (corresponding to the recess in FIG. 3) is H1, and the angle between the lower base and the side is α, so that α=100°, i.e., it is approximately L-shaped, and therefore it is formed into an approximately rectangular shape. Also, L1:L2=0.8, H1:L2=1.0.
[0081] Example 4 Step 1 is the main etching step using reactive ion etching. The magnetic tunnel junction sample shown in Figure 2 was placed in a RIE chamber and the main etching was performed. In the main etching step, the ion source power, which is the energy, was 700 W, the bias voltage power was 400 W, the chamber pressure was 15 mTorr, the chamber pressure was 10 mTorr, and the etching gas was ethanol.
[0082] The reactive ion etching is stopped at a position from the remaining 5 nm of the bottom metal layer to a depth of 40 nm of the lower insulating layer. In this embodiment, the primary etching is preferably stopped at the interface between the metal and the insulator, and the etching amount t1 is 20 nm.
[0083] Step 2 is a cleaning step using reactive ion etching. Secondary etching is then performed in a reactive ion etching chamber. Preferably, the process conditions for the secondary etching are a reactive ion pulse duty ratio of 30%, a reactive ion source power of 300 W, a bias voltage of 100 V, a chamber pressure of 5 mT, an argon gas flow rate of 200 sccm, and etching to the seed layer by 30 nm, i.e., an etching amount t2 of 15 nm. After the secondary etching is performed, the etching shape formed on the lower electrode is a rectangular trench.
[0084] Step 3 is deposition: After the second etching in the vacuum transfer chamber, the sample was transferred to a plasma-enhanced chemical vapor deposition chamber, where a 25 nm SiN film was deposited for in situ protection.
[0085] In the rectangular trench obtained in this embodiment, the length of the lower base (corresponding to the square trench length in FIG. 3) is L1, the length of the upper base (corresponding to the space in FIG. 3) is L2, the height (corresponding to the recess in FIG. 3) is H1, and the angle between the lower base and the side is α, so α=95°, that is, it is approximately L-shaped, so it is formed into an approximately rectangular shape. Also, L1:L2=1.0, H1:L2=1.5.
[0086] Although the preferred embodiments of the present invention have been described in detail above, the present invention is not limited to the specific contents of the above embodiments, and various equivalent transformations can be made to the technical solutions of the present invention within the scope of the technical idea of the present invention, and all of these equivalent transformations belong to the protection scope of the present invention.
Claims
1. 1. A method for etching an MRAM magnetic tunnel junction, comprising: A magnetic tunnel junction main etching step of etching the magnetic tunnel junction by using ion beam etching and / or reactive ion etching under the condition that the etching amount is t1, in which the incident angle of the ion beam is 10-60° and the bias voltage of the reactive ion etching is 400-1000V; a step 2 of cleaning the magnetic tunnel junction by etching the magnetic tunnel junction obtained by carrying out the main etching step under a condition that an etching amount is t2, where t1 / t2 is 0.5 or more, and the etching in the cleaning step includes reactive ion etching in a continuous mode or a pulse mode; The method for etching an MRAM magnetic tunnel junction, wherein the bias voltage of the reactive ion etching in step 2 is 50V to 400V, the pulse duty ratio is 5% to 50%, and after the etching in the cleaning step, the etching shape formed in the lower electrode or the lower insulating layer is a rectangular trench.
2. 2. The etching method for MRAM magnetic tunnel junctions according to claim 1, wherein in step 2, the etching in the cleaning step uses a combination of ion beam etching and reactive ion etching, and the beam voltage of the ion beam etching is 50V to 200V.
3. 2. The method for etching an MRAM magnetic tunnel junction according to claim 1, further comprising step 3, which is an in-situ protection step of the magnetic tunnel junction, by using a chemical vapor deposition method to grow an insulating layer around the magnetic tunnel junction obtained by etching in the cleaning step, thereby providing in-situ protection.
4. 2. The method for etching an MRAM magnetic tunnel junction according to claim 1, wherein an etching amount t2 of the etching in the cleaning step is 5 to 100 nm.
5. 2. The method of claim 1, wherein in step 1, the ion beam etching includes ion beam etching with a large incidence angle and ion beam etching with a small incidence angle.
6. 6. The method for etching an MRAM magnetic tunnel junction according to claim 5, wherein the ion beam etching with the large incidence angle has an ion beam incidence angle of 30 to 60 degrees, and the ion beam etching with the small incidence angle has an ion beam incidence angle of 10 to 30 degrees, and the time of the ion beam etching with the large incidence angle is T1 and the time of the ion beam etching with the small incidence angle is T2, where T1≧1.5T2.
7. 3. The etching method for MRAM magnetic tunnel junctions according to claim 1 or 2, characterized in that, when ion beam etching is used in the main etching step and the cleaning step, the gas used in the ion beam chamber is one or any combination of an inert gas, nitrogen gas, oxygen gas, fluorine-based gas, amino-based gas, carbon monoxide gas, carbon dioxide gas, and alcohol.
8. The etching method for MRAM magnetic tunnel junctions according to claim 1 or 2, characterized in that, when reactive ion etching is used in the main etching step and the cleaning step, the ion source power in the reactive ion chamber is 50 to 1000 W, the pressure in the chamber is 0.5 to 10 mT, the gas flow rate is 10 to 500 sccm, and the gas is one or any combination of an inert gas, a nitrogen gas, an oxygen gas, a fluorine-based gas, an amino-based gas, a carbon monoxide gas, a carbon dioxide gas, and an alcohol.
9. The etching method for MRAM magnetic tunnel junctions according to claim 1, characterized in that, when the length of the lower bottom of the rectangular trench is L1, the length of the upper bottom of the rectangular trench is L2, the height of the rectangular trench is H1, and the angle between the lower bottom and the side of the rectangular trench is α, L1 / L2=0.3 to 1.0, H1 / L2=0.1 to 2.0, and α=90 to 130°.
10. a main etching step of the magnetic tunnel junction, in which the magnetic tunnel junction is etched by ion beam etching under the condition that the etching amount t1 is 35 nm, the ion beam etching is performed by placing the magnetic tunnel junction sample in an ion beam etching chamber and etching under the conditions that the ion beam incidence angle is 25°, the energy is 600 V, and the shield gas is argon gas, the magnetic tunnel junction sample is composed of a mask layer, a cap layer, a magnetic tunnel junction, a lower electrode metal layer, and a lower insulating layer in order from the top, the lower insulating layer has metal lower electrodes, the number of which is the same as the number of masks in the mask layer, fitted at equal intervals corresponding to the positions of the masks, the ion beam etching is stopped at a position where there is 5 nm remaining in the lower electrode metal layer, and the ion beam etching amount is 35 nm at this time; a cleaning step of the magnetic tunnel junction, in which the magnetic tunnel junction obtained by the main etching step is etched by reactive ion etching under the condition that the etching amount t2 is 30 nm, the reactive ion etching is performed in a vacuum chamber by moving the magnetic tunnel junction sample obtained by the ion beam etching of step 1 from the ion beam etching chamber to the reactive ion etching chamber, the reactive ion etching parameters are a reactive ion pulse duty ratio of 20%, an ion source power of 700 W, a bias voltage of 400 V, a chamber pressure of 5 mT, an argon gas flow rate of 100 sccm, a reactive ion etching amount of 30 nm, and an etching shape formed in the lower insulating layer after the etching in the cleaning step is a rectangular trench; Step 3 is an in-situ protection step of the magnetic tunnel junction, in which the magnetic tunnel junction sample obtained by etching in the cleaning step in the vacuum transport chamber is transferred to a plasma enhanced chemical vapor deposition chamber and a 35 nm SiN film is deposited thereon for in-situ protection; 2. The method of claim 1, further comprising:
11. a main etching step of the magnetic tunnel junction, which uses reactive ion etching to etch the magnetic tunnel junction at an etching amount t1 of 20 nm, in which the reactive ion etching is performed by placing the magnetic tunnel junction sample in a reactive ion etching chamber under the conditions of an ion source power of 600 W, a bias voltage of 600 V, a pressure inside the chamber of 3 mT, and an argon gas flow rate of 150 sccm, in which the magnetic tunnel junction sample to be etched is composed of a mask layer, a cap layer, a magnetic tunnel junction, a lower electrode layer, and a lower insulating layer in order from the top, and the reactive ion etching is stopped at a position where the lower electrode layer is consumed by 3 nm, and at this time, the reactive ion etching amount is 20 nm; a step 2 of cleaning the magnetic tunnel junction by etching the magnetic tunnel junction obtained by the main etching step using reactive ion etching under the condition that the etching amount t2 is 15 nm, the etching parameters of the reactive ion etching are reactive ion pulse duty ratio 5%, ion source power 300 W, bias voltage 600 V, chamber pressure 1.5 mT, argon gas flow rate 200 sccm, reactive ion etching amount t2 is 15 nm, and the etching shape formed in the lower insulating layer after the etching in the cleaning step is a rectangular trench; Step 2A is an ion beam cleaning step in which the magnetic tunnel junction sample obtained by etching in the cleaning step in the vacuum chamber is moved to an ion beam etching chamber and etched in an argon atmosphere so as to stop at the lower electrode layer under the conditions of an ion beam incidence angle of 45°, an ion beam energy of 100 V, and an etching depth of 3 nm; Step 3 is an in-situ protection step of the magnetic tunnel junction, in which the magnetic tunnel junction sample obtained by the ion beam cleaning step in the vacuum transport chamber is transferred to a plasma enhanced chemical vapor deposition chamber and a 10 nm SiN film is deposited for in-situ protection.
2. The method of claim 1, further comprising:
Citation Information
Patent Citations
Etching method and substrate processing apparatus
JP2014112664A
Method and apparatus for manufacturing semiconductor apparatus
JP2015173231A
Magnetic storage device and manufacturing method thereof
JP2020043104A
Method to Minimize MTJ Sidewall Damage and Bottom Electrode Redeposition Using IBE Trimming
US20170069834A1
Fabrication of Large Height Top Metal Electrode for Sub-60nm Magnetoresistive Random Access Memory (MRAM) Devices
US20200075847A1