Refractory molding method

By shaping refractories parallel to the trunnion axis to prevent damage from scrap chutes, the refractory weirs maintain a stable slag removal rate, addressing the issue of wear and tear in steel refining processes.

JP7568899B2Active Publication Date: 2024-10-17NIPPON STEEL CORPORATION
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020153956
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-14
Publication Date
2024-10-17
Estimated Expiration
2040-09-14

AI Technical Summary

Technical Problem

Existing refractory weirs at the furnace mouth are prone to damage and destruction due to collisions with scrap chutes, leading to irregular shapes and reduced slag removal efficiency during intermediate slag removal in steel refining processes.

Method used

Constructing refractories at the furnace mouth in a specific shape, with a line segment parallel to the trunnion axis, to prevent partial destruction and maintain a stable slag removal rate, using a plastic material that deforms without cracking.

Benefits of technology

The refractory shape maintains the slag removal rate even with wear and tear, ensuring consistent operation and improved intermediate slag removal efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568899000002
    Figure 0007568899000002
  • Figure 0007568899000003
    Figure 0007568899000003
  • Figure 0007568899000004
    Figure 0007568899000004
Patent Text Reader

Abstract

To provide a method of molding a refractory body to curb damage or wear of the refractory body constructed in a throat, the refractory body configured to prevent molten iron from flowing out when performing intermediate slag-discharging.SOLUTION: A method of molding a refractory body, with respect to a converter, in which a contour of a throat consists of an arc and a first line segment in a shape of the throat viewed in a direction of a furnace body axis, the line segment is parallel to a trunnion axis, and a portion, including the first line segment so as to be present on an opposite side of a steel exit hole across the trunnion axis is constructed by the refractory body, comprises pressing / molding the refractory body in the throat with a plane having a width L as a second line segment using a member having the width L as the second line segment shorter than the first line segment and parallel to the trunnion axis.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] In particular, the present invention relates to a method for forming a refractory material that is adapted to achieve a high intermediate slag removal rate. [Background technology]

[0002] In recent years, in order to improve refining efficiency, a refining method in which the dephosphorization and decarburization processes of molten iron are separated has been widely used. Among them, when the dephosphorization and decarburization processes of molten iron are performed consecutively in the same converter, intermediate slag removal is performed after the dephosphorization process, in which the converter is turned over while the molten iron is still held in the converter, and only the slag in the upper layer is discharged.

[0003] When refining is performed continuously in the same converter, it is desirable to discharge as much slag as possible in the intermediate discharge in order to reduce the amount of carried-over slag, which is an impurity, during the decarburization process. For this reason, various methods for efficiently discharging only the upper layer of slag have been proposed. Patent Documents 1 and 2 disclose a method for discharging slag by installing a weir at the throat of the converter in order to prevent the outflow of molten iron. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 4206050 [Patent Document 2] Japanese Patent Application Laid-Open No. 62-161912 Summary of the Invention [Problem to be solved by the invention]

[0005] However, even if a weir as described in Patent Documents 1 and 2 is installed at the furnace throat, there is a problem that it is technically difficult to maintain the effect through repeated operation. If a refractory weir is installed at the furnace throat, when scrap is charged into the converter, the scrap chute collides with the weir, placing a large load on the weir, and furthermore, the impact of the discharged slag destroys part of the weir. If part of the weir is destroyed, the shape of the weir becomes irregular, and partial destruction of the weir is likely to progress. Therefore, even if a weir is installed at the furnace throat, the weir falls off early, making it impossible to perform stable operation.

[0006] In view of the above-mentioned problems, the present invention has an object to provide a method for forming a refractory material for repairing wear and tear of the refractory material applied to the furnace throat in order to prevent the outflow of molten iron during intermediate slag removal. [Means for solving the problem]

[0007] The inventors of the present invention have made extensive research and have come up with the idea of ​​forming a refractory material, such as a weir, at the furnace opening and constantly forming the refractory material into a shape that makes it difficult for partial destruction of the refractory material to progress. For example, the bottom shape of a typical scrap chute is rounded, so if the scrap chute is tilted near the furnace opening when scrap is charged, the bottom of the scrap chute collides with the weir-shaped refractory material, and the refractory material is formed into a rounded shape. If the refractory material progresses to a rounded shape, the weir-shaped refractory material cannot provide the effect of improving the slag discharge rate when the slag is discharged.

[0008] Therefore, it was found that the effect of improving the slag discharge rate during slag discharge can be maintained by forming the refractory so that the tip of the refractory forms a line segment parallel to the trunnion axis of the converter. The refractory is plastic and does not crack or break when pressed by something like a scrap chute cover, but deforms. For example, if the bottom of the scrap chute is parallel to the trunnion axis of the converter, the bottom of the scrap chute presses the refractory when scrap is charged, and the tip of the refractory can also be formed parallel to the trunnion axis.

[0009] The present invention is as follows. (1) In a converter having a shape of a furnace throat as viewed in the direction of a furnace body central axis, the outline of the furnace throat is composed of a circular arc and a first line segment, the first line segment is parallel to a trunnion axis, and the portion including the first line segment is constructed of refractory material so that the first line segment is on the opposite side of the trunnion axis from the steel tapping hole. In this converter, a member having a plane with a width L of a second line segment that is shorter than the first line segment and parallel to the trunnion axis is used to Pressing the refractory material of the first line segment of the furnace throat; A plane with width L on the second line segment To 1. A method for forming a refractory material, comprising the steps of: (2) The method for forming a refractory material according to (1) above, wherein the member is a member constituting the bottom of a scrap chute. (3) The method for forming a refractory material according to claim 1 or 2, characterized in that, when the length of a straight line connecting two intersection points where a straight line projecting the trunnion axis onto the furnace throat and the arc overlap is defined as D0, a ratio L / D0 is 0.2 or more and less than 0.8. Effect of the Invention

[0010] According to the present invention, even if the refractory material is worn or has metal or the like attached thereto, it can be formed into a weir shape, so that the effect of improving the intermediate slag removal rate can be maintained even when operations are repeated. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a diagram for explaining a refractory material forming method according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram for explaining a typical method of charging scrap through a scrap chute. [Diagram 3] FIG. 2 is a diagram for explaining the shape of a refractory material applied to a furnace throat. [Figure 4] FIG. 2 is a diagram for explaining the wear state of refractory material when operating using a general scrap chute. [Diagram 5] FIG. 1 is a diagram for explaining the wear state of refractory material when operating using a scrap chute equipped with a cover having a width L. [Figure 6] FIG. 13 is a graph showing the transition of the intermediate slag removal rate in level 2, which is a comparative example. [Figure 7] FIG. 13 is a graph showing the transition of the intermediate slag removal rate at level 3, which is an example of the invention. [Figure 8] FIG. 13 is a graph showing the transition of the intermediate slag removal rate at level 4, which is an example of the invention. [Figure 9] FIG. 13 is a graph showing the transition of the intermediate slag removal rate at level 6, which is an example of the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a diagram for explaining a refractory molding method according to the present embodiment. Fig. 1(a) shows an outline of the appearance of a scrap chute, and a cover 1 having a flat surface with a width L (mm) is attached to the bottom of the tip of the scrap chute 2 so as to cover the bottom.

[0013] Fig. 1(b) is a diagram for explaining the state in which the scrap chute is inclined near the throat when scrap is charged into the converter. As shown in Fig. 1(b), when the scrap chute is inclined, the throat 3 of the converter comes into contact with both ends of the cover 1 having a width L. When a weir-shaped refractory is formed at the tip of the throat 3, the refractory is pushed in by the cover 1, and the refractory is shaped to form a line segment parallel to the trunnion axis. The inclination angle of the scrap at this time is not particularly limited, but it is preferably set to an angle of repose at which the scrap can be charged and 50° or less.

[0014] Figure 2(a) shows an overview of the appearance of a typical scrap chute, and the bottom of the scrap chute is generally rounded so that the scrap can easily fall. When scrap is charged into a converter using a scrap chute with such a shape, the center of the bottom of the scrap chute comes into contact with the throat of the converter, as shown in Figure 2(b).

[0015] FIG. 3 is a diagram for explaining the shape of the refractory material applied to the throat. As shown in FIG. 3, in this embodiment, the throat 3 of the converter has an inner contour consisting of a circular arc C and a line segment AB with a length D1, the line segment AB is parallel to the trunnion axis, and the line segment AB is on the opposite side of the trunnion axis from the tapping hole (not shown). The straight line S indicates a straight line obtained by projecting the trunnion axis, which is the axis when tilting the furnace body, onto the throat 3, and is parallel to the line segment AB. The circular arc C corresponds to a part of a circle with a diameter D0 (mm) that forms the throat 3. In other words, the length of the straight line connecting the two intersections of the circular arc C and the line S corresponds to the diameter D0. The refractory material 4 is applied to the part surrounded by the line segment AB and the major arc AB.

[0016] When tilting the converter to remove slag from the throat, providing a refractory material 4 at the throat can prevent the molten iron from flowing out and increase the tilting angle, thereby increasing the intermediate slag removal rate.

[0017] In addition, when the length of the line segment AB is D1 (mm), it is preferable that the refractory is installed so that the ratio D1 / D0 is more than 0.2 and not more than 0.8. If the ratio D1 / D0 is 0.2 or less, the improvement effect of the intermediate slag removal rate decreases early. If the ratio D1 / D0 exceeds 0.8, the improvement effect of the intermediate slag removal rate saturates, but it is undesirable for the operation of the converter because it causes problems in charging molten iron, scrap, and auxiliary materials, and increases the amount of metal attached to the vicinity of the furnace throat and the amount of dust generated.

[0018] In addition, the refractory material 4 is installed in the area surrounded by the line segment AB and the major arc AB, but the refractory material 4 may be installed as a weir, or instead of a weir, the refractory material 4 may be installed so as to give the furnace mouth a flat shape.

[0019] Fig. 4 is a diagram for explaining the wear state of the refractory when operating using the scrap chute shown in Fig. 2. When the refractory 4 is installed at the furnace throat in the shape shown in Fig. 3, scrap is charged using the scrap chute shown in Fig. 2, and dephosphorization and intermediate slag discharge are repeated, the refractory 4 is worn, and further, the bottom of the scrap chute repeatedly comes into contact with the refractory, causing the refractory to assume the shape shown in Fig. 4. When the refractory assumes such a shape, molten iron is likely to flow out during intermediate slag discharge, the tilting angle cannot be increased, and the intermediate slag discharge rate drops significantly.

[0020] Fig. 5 is a diagram for explaining the wear state of the refractory when the scrap chute shown in Fig. 1 is used for operation. When the refractory 4 is installed at the furnace throat in the shape shown in Fig. 3, scrap is charged using the scrap chute shown in Fig. 1, and dephosphorization and intermediate slag discharge are repeated, the refractory 4 is worn, and further, the bottom of the scrap chute repeatedly comes into contact with the refractory, so that the refractory takes the shape shown in Fig. 5. The portion of the line segment CD is newly formed when the cover 1 at the bottom of the scrap chute 2 comes into contact with the refractory 4. In other words, the length D2 (mm) of the line segment CD is approximately the same as the width L of the cover at the bottom of the scrap chute 2.

[0021] As described above, in order to form the refractory, the width L of the cover 1 at the bottom of the scrap chute 2 must be smaller than the length D1 of the line segment AB when the refractory is installed. When performing intermediate slag discharge in a state in which the refractory 4 is worn, it is preferable that the ratio D2 / D0 of the diameter D0 forming the furnace throat 3 and the length D2 of the line segment CD is 0.2 or more and less than 0.8. Therefore, it is also preferable that the ratio of the diameter D0 forming the furnace throat 3 and the width L of the cover 1 shown in FIG. 1 is 0.2 or more and less than 0.8. If the ratio L / D0 (ratio D2 / D0) is less than 0.2, the pressure is concentrated on the part of the width L, so that the dent of the refractory 4 becomes large, and the effect of improving the intermediate slag discharge rate is reduced. Also, if the ratio L / D0 is 0.8 or more, even if a refractory with a ratio D1 / D0 of 0.8 is installed, the refractory 4 cannot be formed if it is worn. More preferably, the ratio of the diameter D0 that defines the furnace throat 3 to the width L of the cover 1 shown in FIG. 1 is equal to or greater than 0.20 and less than 0.70.

[0022] Furthermore, the width L of the cover 1 at the bottom of the scrap chute 2 and the length D2 of the line segment CD are approximately the same length, but there are some variations depending on the degree of wear of the refractory material and the left-right shaking when the cover 1 of the scrap chute 2 is pressed, and the lengths may differ by about 10%. Furthermore, in this embodiment, an example has been described in which the refractory material is formed using a cover installed at the bottom of the scrap chute because this is the easiest to install without requiring any extra equipment, but the refractory material may be formed using something other than the scrap chute as long as it has a portion of a similar shape. EXAMPLES

[0023] Next, an embodiment of the present invention will be described, but the conditions in the embodiment are merely an example of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to this example of conditions. Various conditions can be adopted in the present invention as long as they do not deviate from the gist of the present invention and achieve the object of the present invention.

[0024] First, before the test, refractory was installed at the throat of a 300t converter so as to form a bow shape consisting of a major arc AB and an intersection point AB between a parallel line that is parallel to the trunnion axis and exists in the slag discharge direction and the throat contour, as shown in Fig. 3. At this time, in levels 2 to 6, the ratio was 80% of the throat diameter D0 (i.e., the ratio D1 / D0 = 0.80). In level 1, no refractory was installed.

[0025] After the refractory material was installed, molten iron and scrap were charged into the converter until the total amount reached 300t, and then auxiliary materials containing lime were added and dephosphorization blowing was performed. At the end of the dephosphorization blowing, the amount of slag in the furnace was 40-70 (kg / t of molten iron), and the temperature of the molten iron was 1340-1380°C. After the dephosphorization blowing, intermediate slag removal was performed by tilting the converter. After intermediate slag removal was completed, the furnace was returned to the blowing position, auxiliary materials were added, and decarburization blowing was performed. After the decarburization blowing, molten steel was tapped from the tap hole, and the slag was appropriately removed so that an appropriate amount of slag remained in the furnace. The above series of processes was counted as one test, and an evaluation was performed by repeating 50 times, which is an indicator of durability that will not cause problems in actual operation.

[0026] The shape of the scrap chute when charging the scrap was different for each of levels 1 to 6. In levels 1 and 2, a scrap chute with a rounded bottom shape as shown in Figure 2 was used. In levels 3 to 6, a scrap chute with a flat cover of width L installed at the bottom as shown in Figure 1 was used, and the width L was different for each of levels 3 to 6. Then, the average slag discharge rate at intermediate slag discharge was calculated for each level. Specifically, the intermediate slag discharge rate was calculated by the mass of discharged CaO / the mass of initially charged CaO x 100, and the average value was calculated as the average slag discharge rate. The results are shown in Table 1.

[0027] [Table 1]

[0028] As shown in Table 1, in level 1, because refractory material was not installed, the intermediate slag discharge rate was always low, and the average slag discharge rate was a low value of 47%. In level 2, the refractory material was worn down to the shape shown in Figure 4, and as shown in Figure 6, in level 2, the intermediate slag discharge rate decreased early, and in the seventh test it became equal to that of level 1, and further tests were discontinued. The average slag discharge rate for the first to sixth tests, which had an effect of improving the intermediate slag discharge rate, was 51%, and the intermediate slag discharge rate during that period was slightly higher than that of level 1, but since the intermediate slag discharge rate reached a low value early on, it can be said that there was almost no effect on increasing the intermediate slag discharge rate.

[0029] In addition, in level 3, the dents in the refractory became too large after the 24th test, and the intermediate slag discharge rate was equivalent to that of level 1, so further tests were discontinued. However, as shown in Figure 7, the intermediate slag discharge rate was able to be maintained at a higher level than that of level 1, confirming the effect of increasing the intermediate slag discharge rate.

[0030] On the other hand, in levels 4 to 6, the intermediate slag discharge rate was higher than level 1 in all 50 tests, as shown in Figures 8 and 9. In particular, in level 6, the scrap chute cover of the present invention had a large width L, which prevented the furnace throat shape from deforming from the beginning, and therefore it was possible to achieve a high intermediate slag discharge rate as shown in Figure 9 while maintaining durability equivalent to that of the conventional furnace throat in level 1. [Explanation of symbols]

[0031] 1 Cover 2. Scrap Shoot 3 Hearth 4 Refractories

Claims

1. A method for forming a refractory material, comprising the steps of: for a converter in which a portion including a refractory material is constructed so that, in the shape of a furnace throat when viewed in the direction of the furnace body central axis, the contour of the furnace throat consists of an arc and a first line segment, the first line segment is parallel to a trunnion axis, and the portion including the first line segment is located on the opposite side of the trunnion axis from a steel tapping hole; using a member having a plane with a width L that is a second line segment that is shorter than the first line segment and parallel to the trunnion axis, the refractory material of the first line segment of the furnace throat is press-formed into a plane with a width L of the second line segment.

2. 2. The method for forming a refractory material according to claim 1, wherein the member is a member constituting a bottom portion of a scrap chute.

3. The length of the straight line connecting the two intersection points where the straight line projected onto the furnace throat of the trunnion axis and the arc overlap is defined as D. 0 In this case, the ratio L / D 0 3. The method for forming a refractory material according to claim 1, wherein the value of is 0.2 or more and less than 0.8.

Citation Information

Patent Citations

  • Scrap steel hopper capable of effectively improving scrap steel loading efficiency

    CN211112077U

  • JP1979107607U

  • Each of the converter device for removing metal port

    JP1981019556U

  • JP1987136555U

  • Method for discharging slag during refining in converter

    JP1987161912A