HOT-ROLLED STEEL SHEET AND ITS MANUFACTURING METHOD
A hot-rolled steel sheet with specific composition and processing achieves high yield strength and bending workability by forming fine Ti-containing carbides, addressing the limitations of conventional methods and enhancing automotive applications.
Patent Information
- Application Number
- JP2024504861
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-11-16
- Filing Date
- 2023-09-19
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2043-09-19
AI Technical Summary
Conventional techniques fail to achieve both high yield strength of 680 MPa and excellent bending workability and toughness in hot-rolled steel sheets, and often compromise manufacturability due to stringent hot rolling temperature control.
A hot-rolled steel sheet composition with specific elements (C, Si, Mn, P, S, Al, N, Ti, and optionally others) and a manufacturing process involving high coiling temperatures, precise rolling conditions, and controlled cooling rates to form fine Ti-containing carbides, resulting in a unique microstructure with large crystal strain.
The solution produces a steel sheet with a yield strength of 680 MPa or more, exhibiting superior bending workability and toughness, suitable for automobile parts, enabling weight reduction.
Smart Images

Figure 0007569028000001 
Figure 0007569028000002 
Figure 0007569028000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a hot-rolled steel sheet having a yield strength of 680 MPa or more and excellent bending workability and toughness, and a method for producing the same. [Background technology]
[0002] In recent years, from the perspective of protecting the global environment, the entire automobile industry has been oriented toward improving automobile fuel efficiency in order to regulate CO2 emissions. The most effective way to improve automobile fuel efficiency is to reduce the weight of automobiles by making the parts thinner, so in recent years the amount of high-strength steel sheets used as materials for automobile parts has been increasing. Generally, as the strength of steel plate increases, the formability and toughness tend to deteriorate. Therefore, in order to further expand the use of high-strength steel plate, it is essential that high strength, formability and toughness are achieved simultaneously.
[0003] In order to solve these problems, various techniques have been proposed to increase the strength and improve the formability of steel sheets.
[0004] For example, Patent Document 1 discloses a hot-rolled steel sheet in which Ti carbides with an average grain size of less than 6 nm and TiS with an average grain size of 0.5 μm or less are dispersed in ferrite crystals with an area ratio of 95% or more, and it is said that this results in a high-tensile hot-rolled steel sheet with a tensile strength of 780 MPa to 900 MPa and excellent bending workability.
[0005] Patent Document 2 discloses a technique in which a steel slab containing one or more of Ti and Nb is heated and roughly hot rolled to produce a steel plate, which is joined to the rear end of a preceding roughly rolled steel plate and then hot finish rolled in the range of Ar3 to Ar3 + 50° C. It is said that this produces a hot-rolled steel plate for processing with good toughness. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2013 / 099196 [Patent Document 2] Japanese Patent Application Publication No. 09-227949 Summary of the Invention [Problem to be solved by the invention]
[0007] However, the conventional techniques disclosed in the above-mentioned patent documents have the following problems.
[0008] The technique described in Patent Document 1 does not allow the microstructure required by the present invention to be obtained, as seen in, for example, steel plate No. 5 in the examples. Therefore, it is not possible to achieve both good bending workability and toughness at a yield strength of 680 MPa or more.
[0009] In addition, the technology described in Patent Document 2 does not provide a high strength of 680 MPa or more in yield strength, and does not suggest any requirements for obtaining good bendability. Furthermore, narrow range control of the hot rolling temperature to obtain high toughness significantly impedes manufacturability, and in some cases was not feasible depending on the manufacturing size.
[0010] The present invention has been developed in consideration of the above-mentioned problems associated with the conventional technology, and aims to provide a hot-rolled steel sheet having a yield strength (YS) of 680 MPa or more and excellent bending workability and toughness, and a manufacturing method thereof. [Means for solving the problem]
[0011] In order to solve the above problems, the inventors have thoroughly studied the requirements for combining bending workability and toughness in a hot-rolled steel sheet with a yield strength of 680 MPa or more. Since high ductility is necessary to obtain good bending workability, they have studied a process that assumes a high coiling temperature, which provides high total elongation, although this is a disadvantageous condition for high strength. In order to obtain a yield strength of 680 MPa or more at a coiling temperature of 600°C or more, they decided to strengthen the hot-rolled steel sheet with extremely fine nano-sized carbides containing Ti.
[0012] However, it was previously common knowledge that when the coiling temperature of hot-rolled steel sheets is 600°C or higher, which causes the precipitation of carbides containing Ti, a ferrite phase that does not contain many dislocations is formed in the steel sheet. The fracture surface unit that has a significant effect on the toughness of this ferrite structure is said to be equivalent to the ferrite grain size. As a result of investigating how to refine the ferrite phase, it was concluded that it would be difficult to stably obtain the desired toughness.
[0013] Therefore, the inventors conducted extensive research into the possibility of the formation of crystal structures other than ferrite when the coiling temperature of this hot-rolled steel sheet is 600°C or higher. As a result, they obtained a new structure that cannot be classified as either ferrite or bainite, and discovered that this structure has good strength, bending workability and toughness. It was discovered that this new structure is formed from fine recrystallized austenite grains that are recrystallized during the finish rolling process of hot rolling.
[0014] The hot-rolled steel sheet according to the present invention, which has been developed based on the above findings, has the following configuration. [1] In mass%, C: 0.035% or more but less than 0.110%, Si: 1.5% or less, Mn: 1.3% or less, P: 0.05% or less, S: 0.010% or less, Al: 0.005% or more but less than 0.080%, N: 0.0060% or less, Ti: 0.08% or more but less than 0.20%, Optionally, it further contains one or both of the following group A and group B: Group A; B: 0.0002% or more and 0.0050% or less, Group B: Nb, V, Mo, Sb, REM, Mg, Ca, Sn, Ni, Cu, Co, As, Cr, W, Ta, Pb, Cs, Zr, Hf, Te, Bi, and Se, total of 1% or less The hot-rolled steel sheet has a composition with the balance consisting of Fe and unavoidable impurities, and in terms of area ratio of the metal structure, ferrite is 0% to 85%, retained austenite is 3% or less, lath structure is 5% or less, and structure with a KAM value of 1.0 or more is 15% or more. The hot-rolled steel sheet has carbides containing Ti and an average particle size of 8 nm or less, and has a yield strength of 680 MPa or more. [2] In the above [1], the hot-rolled steel sheet has a plating layer on a surface thereof.
[0015] The method for producing a hot-rolled steel sheet according to the present invention, which was developed based on the above findings, is configured as follows. [3] A method for producing a hot-rolled steel sheet, comprising: a rough rolling step of heating a steel material having the composition described in [1] above to a heating temperature of 1200°C or higher, or without heating after casting, to a sheet bar, a finish rolling step of finish rolling the sheet bar to a hot-rolled steel sheet at a rolling start temperature of 950°C or higher, a total reduction rate from the first pass to the fifth pass of 75% or higher, and a rolling completion temperature of 860°C to 910°C, and a cooling step of cooling the hot-rolled steel sheet at an average cooling rate of 40°C / s or higher to a cooling stop temperature of 600°C to 700°C, and a coiling step of coiling the cooled hot-rolled steel sheet at a coiling temperature of 600°C to 700°C. [4] In the above [3], a casting process is included in which a steel material having a thickness of 35 mm or more and 200 mm or less and having the component composition described in [1] is cast before the rough rolling process or the finish rolling process, and the hot-rolled steel sheet is made into a sheet bar with or without applying the rough rolling process. [5] The method for producing a hot-rolled steel sheet according to [3] above further comprises a joining step of joining the roughly rolled sheet bar and a preceding sheet bar at 1050°C or higher between the rough rolling step and the finish rolling step, and in the finish rolling step, the joined sheet bar is finish-rolled. [6] In any one of the above [3] to [5], the method for producing a hot-rolled steel sheet further includes a hot-rolled sheet annealing step of annealing the hot-rolled steel sheet at an annealing temperature of 720°C or less, and a plating step of plating the annealed hot-rolled steel sheet. [7] The method for producing a hot-rolled steel sheet according to the above [6], further comprising an alloying step of subjecting the plated hot-rolled steel sheet to an alloying treatment at a temperature of 480°C or higher and 600°C or lower. Effect of the Invention
[0016] According to the present invention, it is possible to manufacture a hot-rolled steel sheet having a high strength of 680 MPa or more in yield strength (YS), excellent bending workability and toughness. Since the hot-rolled steel sheet according to the present invention is suitable as a material for automobile suspension members, when it is applied to automobile parts, further weight reduction of the automobile parts is realized. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, the hot-rolled steel sheet according to this embodiment will be described. <Chemical composition of hot-rolled steel sheet> The composition of the hot-rolled steel sheet is, in mass%, C: 0.035% or more and less than 0.110%, Si: 1.5% or less, Mn: 1.3% or less, P: 0.05% or less, S: 0.010% or less, Al: 0.005% or more and 0.080% or less, N: 0.0060% or less, Ti: 0.08% or more and 0.20% or less. Each component is explained below. In the following explanation, "%" representing the content of a component means "mass%".
[0018] C: 0.035% or more and less than 0.110% C combines with Ti to contribute to increasing the strength of the steel sheet and forming a highly dislocated structure during isothermal transformation. To obtain a steel sheet with a yield strength of 680 MPa or more, the C content is set to 0.035% or more. On the other hand, if the C content is 0.110% or more, coarse cementite precipitates, increasing the risk of reducing bending workability and toughness. Therefore, the C content is set to 0.035% or more and less than 0.110%. It is preferably 0.035% or more and 0.10% or less.
[0019] Si: 1.5% or less Si is an effective element for improving workability, since it increases the elongation of the steel sheet and suppresses cementite precipitation. On the other hand, if the Si content exceeds 1.5%, the effect of improving bending workability is reduced, and the surface properties and weldability are deteriorated, and the adverse effects of adding a large amount of Si become large. Therefore, the Si content is set to 1.5% or less. Preferably, the Si content is 1.2% or less. Note that even if the Si content is 0%, the effect of this embodiment is not impaired, but in order to generate a structure that does not stably have a lath structure and has large crystal distortion, the Si content is preferably 0.15% or more.
[0020] Mn: 1.3% or less Mn increases hardenability and suppresses the formation of ferrite with small crystal strain during the cooling process after hot rolling. In order to stably manufacture hot-rolled steel sheets, the Mn content is preferably 0.2% or more. In addition, in order for austenite to stably recrystallize during hot rolling, it is preferable that hot working strain is stably present, and it is effective to control the contents of Si and Mn, which are substitutional solid solution elements, within a narrow range. For this purpose, it is preferable to satisfy the following formula (1). 1.1≦0.8[%Si]+[%Mn]≦1.5···(1) Here, [%Si] and [%Mn] refer to the Si content and Mn content in mass%. On the other hand, if the Mn content exceeds 1.3%, the driving force for the transformation from austenite to ferrite is excessively reduced, and a structure with small crystal strain cannot be obtained. Therefore, the Mn content is set to 1.3% or less. Preferably, the Mn content is 1.2% or less.
[0021] P:0.05% or less Since P is a harmful element that segregates at grain boundaries and reduces toughness, it is preferable to reduce it as much as possible. In this embodiment, the P content can be tolerated up to 0.05%. Preferably, the P content is 0.04% or less, but for use in environments where stricter toughness is required, it is more preferable to make it 0.02% or less. Meanwhile, 0.002% P may be inevitably mixed in during manufacturing.
[0022] S: 0.010% or less S forms coarse sulfides in steel, which expand during hot rolling to become wedge-shaped inclusions, adversely affecting toughness. Therefore, since S is also a harmful element, it is preferable to reduce it, and the allowable content is up to 0.010%. The S content is preferably 0.003% or less, but for use in environments where stricter toughness is required, it is more preferable to keep it 0.001% or less. In manufacturing, 0.0001% S may be unavoidably mixed in.
[0023] Al: 0.005% or more and 0.080% or less When Al is added as a deoxidizer at the steelmaking stage, the Al content is 0.005% or more. Al forms oxides, which reduces bending workability and toughness. Therefore, the Al content is set to 0.080% or less. The Al content is preferably 0.010% or more and 0.070% or less.
[0024] N: 0.0060% or less N is a harmful element that combines with Ti to form coarse TiN, reducing strength, bending workability, and toughness. Therefore, it is preferable to reduce the N content as much as possible, and up to 0.0060% is acceptable. The N content is preferably 0.0050% or less. In manufacturing, about 0.0005% N may be inevitably mixed in.
[0025] Ti: 0.08% or more and 0.20% or less Ti combines with C to form fine carbides containing Ti, which contributes to increasing the strength of the steel plate. In order to obtain a yield strength of 680 MPa or more, the Ti content is 0.08% or more. On the other hand, if the Ti content exceeds 0.20%, the coarse carbides containing Ti cannot be dissolved in the heating process before hot rolling, and not only does the effect of increasing the strength saturate, but it also has a negative effect on bending workability and toughness. Therefore, the Ti content is set to 0.08% or more and 0.20% or less. Preferably, the Ti content is 0.09% or more and 0.19% or less.
[0026] As described above, C contributes to the formation of a structure with large crystal strain, while it is also used to form carbides containing Ti by combining with Ti. Therefore, in order to stably obtain the metal structure required for the hot-rolled steel sheet according to this embodiment, it is preferable to satisfy the following formula (2). In particular, if the formula (2) is below 1.4, the concentration of C accumulating at the grain boundaries during isothermal transformation decreases, making it impossible to stably obtain a structure with large crystal strain. Therefore, it is preferable that the formula (2) is 1.4 or more. On the other hand, to obtain a steel sheet with a yield strength of 680 MPa or more, it is necessary to strengthen the steel sheet with fine Ti-containing carbides on the nano-order. However, if the value of formula (2) exceeds 2.8, the coarse TiC particles cannot be dissolved during reheating of the slab, which leads to a decrease in the strength of the steel sheet and a decrease in the bending workability of the steel sheet. Therefore, it is preferable to set the value of formula (2) to 2.8 or less. 1.4≦([%C] / 12) / ([%Ti * ] / 48)≦2.8···(2) However, [%Ti * ]=[%Ti]-48[%N] / 14. Here, [%C], [%Ti], and [%N] refer to the C content, Ti content, and N content in mass%.
[0027] The above is the basic composition of the hot-rolled steel sheet according to the embodiment, but optionally, one or both of the following group A and group B components may further be contained. Group A; B: 0.0002% or more and 0.0050% or less Group B: Nb, V, Mo, Sb, REM, Mg, Ca, Sn, Ni, Cu, Co, As, Cr, W, Ta, Pb, Cs, Zr, Hf, Te, Bi, and Se, total of 1% or less
[0028] B: 0.0002% or more and 0.0050% or less B is an element effective for improving hardenability, and it is necessary to ensure hardenability in order to obtain a structure with large crystal strain. The B content of 0.0002% or more contributes to stably obtaining a desired structure. On the other hand, if the B content exceeds 0.0050%, the effect on the hardenability of the steel is saturated, so the B content is set to 0.0050% or less. More preferably, the B content is 0.0004% or more and 0.0030% or less.
[0029] Nb, V, Mo, Sb, REM, Mg, Ca, Sn, Ni, Cu, Co, As, Cr, W, Ta, Pb, Cs, Zr, Hf, Te, Bi, and Se, total of 1% or less The total content of any one or more elements within the range of 1% or less is permissible since it has little effect on the properties of the hot-rolled steel sheet according to the present embodiment. On the other hand, the content of each element is preferably limited to 0.03% or less.
[0030] The chemical composition of the hot-rolled steel sheet according to this embodiment contains the above elements with the balance being Fe and unavoidable impurities.
[0031] <Metal structure of hot-rolled steel sheet> Next, the metal structure of the hot-rolled steel sheet will be described. The metal structure of the hot-rolled steel sheet of this embodiment has an area fraction of ferrite of 0% or more and 85% or less, an area fraction of retained austenite of 3% or less, an area fraction of a structure having a lath morphology of 5% or less, and an area fraction of a structure having a KAM value of 1.0 or more of 15% or more, and has carbides containing Ti with an average particle size of 8 nm or less. In the following description, "%" representing the metal structure means "area ratio".
[0032] Ferrite area ratio is 0% to 85% Ferrite is a structure with inferior toughness because the fracture surface unit during brittle fracture is larger than that of the new structure of this embodiment with large crystal strain. Since ferrite has small crystal strain within the grains, the KAM value is less than 1.0. To obtain the desired toughness, the area ratio of ferrite must be limited to 85% or less. Preferably, the area ratio of ferrite is 80% or less, and more preferably, 70% or less.
[0033] Retained austenite is 3% or less (including 0%) The bainite and tempered martensite defined in this embodiment are those in which a lath structure is observed within the grains. Martensite is a structure observed as a white contrast on an SEM, but since it may be cementite, it is sufficient to separate them by crystal structure using electron backscatter diffraction (EBSD) analysis. For example, it is possible to determine whether or not bainite, martensite, and tempered martensite that satisfy the Kurdjumov-Sachs relationship with the parent phase are applicable by obtaining a (001)α pole figure of a single prior γ grain region. The retained austenite can be obtained by XRD analysis using a sample that has been chemically polished 0.1 mm or more after grinding the steel sheet surface to 1 / 4 of the sheet thickness from the surface. These structures reduce the strength, workability, and toughness of the hot-rolled steel sheet of this embodiment. It is preferable to reduce these structures as much as possible, and the retained austenite is 3% or less. Preferably, the total of bainite, martensite, tempered martensite, martensite, and retained austenite is 5% or less, and more preferably, 3% or less.
[0034] The area ratio of the structure with lath morphology is 5% or less, and the area ratio of the structure with KAM value of 1.0 or more is 15% or more. The greatest technical feature of this embodiment is that a structure having large crystal strain and no lath structure is strengthened with carbides containing Ti of 8 nm or less. Ferrite has small crystal strain, that is, the KAM value is less than 1. Low-temperature transformation phases such as bainite, martensite, and tempered martensite have a lath structure. A structure having large crystal strain and no lath structure is a structure that cannot be classified as ferrite or bainite. Lath is a structure observed as a plate-like form within grains by transmission electron microscope (TEM) or EBSD analysis. A structure having this lath structure is hard, but has poor workability and does not obtain the desired bendability. The structure having large crystal strain of the present invention is one having a KAM value of 1.0 or more obtained by EBSD analysis. The KAM value indicates a disorder of the crystal structure, and this crystal disorder makes the effective fracture surface unit fine, achieving toughness greater than that of ferritic structure steel. From the above, this structure makes it possible to obtain a steel plate having good workability and toughness. Therefore, a structure without a lath structure refers to a structure with a lath morphology having an area ratio of 5% or less, and a structure with a large crystal distortion refers to a structure with a KAM value of 1.0 or more having 15% or more. More preferably, a structure with a KAM value of 1.0 or more has a KAM value of 1.0 or more having 20% or more. Note that the KAM value of grain boundaries is often 1.0 or more, and even in a ferrite single-phase structure, the area ratio of a structure with a KAM value of 1.0 or more is not 0%, and about 3% is inevitably included. The measurement of the ferrite area ratio is determined from the morphology within the grains, and the grain boundaries are not judged, so the sum of the area ratio of the KAM value of 1.0 or more and the ferrite area ratio may exceed 100%.
[0035] Carbide containing Ti with an average particle size of 8 nm or less In this embodiment, the steel sheet is strengthened by carbides containing Ti. To obtain a high-strength hot-rolled steel sheet having a yield strength of 680 MPa or more, it is necessary to set the average particle size of the carbides containing Ti dispersed in the steel to 8 nm or less. To stably obtain a strength having a yield strength of 680 MPa or more, it is preferable to set the average particle size of the carbides containing Ti to 5 nm or less.
[0036] Furthermore, when the coiling temperature is 600°C or higher, Ti, even though it is a substitutional element, diffuses sufficiently in the steel. By utilizing this property of Ti to diffuse and precipitate Ti, a steel sheet with a yield strength of 680 MPa or more can be obtained even if the structure of bainite, martensite, and tempered martensite, which are often used in high-strength steel sheets, is small. To obtain a steel sheet with a yield strength of 680 MPa or more, 80% or more of the contained Ti is utilized for precipitation. Preferably, 85% or more of the contained Ti is utilized.
[0037] The hot-rolled steel sheet according to the present embodiment preferably has a plating layer on the surface. Even if the plating layer is formed, the function of the hot-rolled steel sheet is not impaired. The composition of the plating layer is preferably one or more selected from Zn, Si, Al, Ni, and Mg. In this embodiment, the plated steel sheet includes any of those that have been subjected to hot-dip galvanizing treatment (GI), those that have been subjected to hot-dip galvanizing treatment followed by alloying treatment (GA), and those that have been subjected to electrolytic galvanizing treatment (EG).
[0038] Next, a first embodiment of the method for producing a hot-rolled steel sheet according to the present embodiment will be described. In general, hot-rolled steel sheets are manufactured by casting a slab (steel material) whose temperature has been reduced to 1000°C or less, loading it into a heating furnace, heating it for a short time, and then reducing the thickness to a specified thickness in a hot rolling line and winding it into a coil. Alternatively, after casting, the slab (steel material) that has been cooled to room temperature is heated for a long time in a heating furnace, and then reduced to a specified thickness in a hot rolling line and winding it into a coil. There is also a manufacturing method in which the cast slab (steel material) is directly sent to a hot rolling line without being heated in a heating furnace, and reduced to a specified thickness and wound into a coil. The manufacturing method of the hot-rolled steel sheet according to this embodiment can be applied not only to a process in which the steel material is heated after casting, but also to a process in which the steel material is directly sent to a hot rolling line without being heated after casting.
[0039] <First form steel material> The smelting method for producing the steel material of this embodiment is not particularly limited, and known smelting methods such as converters and electric furnaces can be adopted. Secondary refining may also be performed in a vacuum degassing furnace. The molten steel thus adjusted to the above-mentioned composition is then preferably made into a slab (steel material) by a continuous casting method, taking into consideration productivity and quality. Alternatively, the slab may be made into a slab by an ingot casting-blooming rolling method or other known casting methods.
[0040] <First type of rough rolling process> In this embodiment, the steel material is heated to a heating temperature of 1200° C. or higher, or is not heated after casting, and is roughly rolled to form a sheet bar. <First type of finish rolling process> Next, hot rolling is performed in which the starting temperature of finish rolling is 950°C or higher, the total rolling reduction from the first to fifth passes is 75% or higher, and the completion temperature of finish rolling is 860°C to 910°C, to produce a hot-rolled steel sheet. <Cooling step of the first embodiment> Next, the hot-rolled steel sheet is cooled to a cooling stop temperature of 600° C. or more and 700° C. or less at an average cooling rate of 40° C. / s or more. <Winding process of the first embodiment> Thereafter, the cooled hot-rolled steel sheet is coiled at a coiling temperature of 600°C or higher and 700°C or lower.
[0041] Heating of steel material: Heating to 1200℃ or above, or not heating By dissolving the coarse carbides containing Ti precipitated in the slab (steel material) in a heating process before hot rolling, fine carbides containing Ti precipitate after hot rolling. Therefore, in order to obtain carbides containing Ti with an average particle size of 8 nm or less, the slab (steel material) is heated to 1200°C or higher. The temperature is preferably 1220°C or higher, and when the Ti content is 0.12% or more, it is more preferable to heat the slab (steel material) to 1240°C or higher. There is no particular upper limit, but 1300°C is a manufacturing constraint in order to avoid thermal damage to the heating furnace. If the steel material is directly sent to the hot rolling line after being kept at 1200°C or higher after casting, the steel material is not heated after casting.
[0042] Finish rolling start temperature: 950°C or higher, total reduction rate from 1st to 5th passes: 75% or higher, finish rolling end temperature: 860°C to 910°C In order to generate a structure with large crystal strain, which is a feature of the hot-rolled steel sheet according to this embodiment, it is necessary to precisely control the hot-rolling conditions. Specifically, fine austenite is formed by recrystallization of austenite during finish rolling. For this purpose, the start temperature of the finish rolling is 950°C or higher, and the total reduction rate from the first pass to the fifth pass is 75% or higher. If the chemical composition of the hot-rolled steel sheet according to this embodiment is within the range, austenite recrystallization occurs in the finish rolling stand after the fifth pass. Therefore, the finish rolling is performed in 5 passes or more. If the finish rolling start temperature is below 950°C, the austenite will recrystallize early in the finish rolling, and the recrystallized austenite will be rolled again. This will result in the formation of ferrite, and a structure with large crystal distortion will not be obtained. If the finish rolling start temperature exceeds 1100°C, there is a high possibility that austenite recrystallization will not occur in the finish rolling stand. Therefore, the finish rolling start temperature is preferably 1100°C or lower.
[0043] If the finish rolling completion temperature is below 860°C, the risk of ferrite formation during rolling increases. On the other hand, if the finish rolling completion temperature exceeds 910° C., austenite cannot be recrystallized during the finish rolling. Therefore, the finish rolling completion temperature is set to 860° C. or higher and 910° C. or lower. To stably obtain austenite recrystallization, the finish rolling completion temperature is preferably set to 890° C. or lower.
[0044] As described above, in order to recrystallize austenite by finish rolling, it is necessary to accumulate strain from the first pass to the fifth pass of finish rolling. Therefore, if the rolling interval from the first pass to the fifth pass is long, the strain imparted by rolling will recover, and austenite cannot be recrystallized stably by finish rolling. Therefore, from the viewpoint of avoiding the adverse effects of this austenite recovery, it is preferable to set the rolling interval time from the first pass to the fifth pass to at least 1.5 seconds or less.
[0045] Cooling stop temperature after finish rolling is 600℃ to 700℃, with an average cooling rate of 40℃ / s or more If the cooling rate to 700°C or less after hot rolling is slow, polygonal ferrite (ferrite) that is coarse and has small crystal distortion within the grains will form at high temperatures. To suppress the formation of this ferrite, it is necessary to cool the material at an average cooling rate of 40°C / s or more after hot rolling, and it is preferable to cool the material to 700°C or less at an average cooling rate of 50°C / s within 2 seconds after hot rolling. On the other hand, if the cooling stop temperature is below 600°C, it becomes difficult to obtain carbides containing Ti, and a steel sheet having a yield strength of 680 MPa or more cannot be obtained. Therefore, the cooling stop temperature is set to a range of 600°C to 700°C. Preferably, the cooling stop temperature is set to a range of 610°C to 690°C. Here, the average cooling rate may be calculated by {(cooling start temperature)-(cooling completion temperature)} / (forced cooling time other than natural cooling) after hot rolling, in which forced cooling other than natural cooling is performed. An example of the forced cooling method is water cooling.
[0046] Winding temperature: 600℃ or more and 700℃ or less For the same reason as the cooling stop temperature, the coiling temperature is set to 600° C. or higher and 700° C. or lower, and preferably 610° C. or higher and 690° C. or lower. If coiling is performed in this temperature range, the generation of ferrite, bainite, martensite, and retained austenite can be suppressed as much as possible.
[0047] Next, a second embodiment of the method for producing a hot-rolled steel sheet according to the present embodiment will be described. In this embodiment, the difference from the first embodiment will be described. <Second type casting process> The hot rolled steel sheet according to the present embodiment can also be produced by the thin slab continuous casting method. When produced by the thin slab continuous casting method, a steel material having a thickness of 35 mm or more and 200 mm or less is cast. <Second type of rough rolling process> The cast steel material is heated to a heating temperature of 1200° C. or higher, or is not heated after casting, and is roughly rolled as necessary to form a sheet bar. The process after the finish rolling step is the same as that of the first embodiment.
[0048] Here, we will explain the slab (steel material) thickness that is specific to the thin slab continuous casting method.
[0049] Slab (steel material) thickness: 35mm to 200mm Unlike the continuous casting method, the thin slab before hot rolling is thin in the thin slab casting method, and the degree of austenite processing in the hot rolling is low. If the slab thickness is less than 35 mm, the desired total reduction rate from the first to fifth passes cannot be obtained. On the other hand, if the slab thickness exceeds 200 mm, the casting speed becomes slow and the productivity advantage of the thin slab casting method compared to the continuous casting method is lost. From the above viewpoints, the slab thickness in the thin slab casting method is set to be 35 mm or more and 200 mm or less.
[0050] Next, a third embodiment of the method for producing a hot-rolled steel sheet according to the present embodiment will be described. In this embodiment, the difference from the first and second embodiments will be described. In the third embodiment, a continuous hot rolling technique can be applied. <Third type of joining process> The sheet bar obtained in the first or second form is joined to the preceding sheet bar at 1050°C or higher before finish rolling. If the temperature is lower than 1050°C, it becomes difficult to roll at the finish rolling start temperature of 950°C or higher. The preferred heating temperature for the sheet bar during joining is 1070°C or higher. The steps after the cooling step are the same as those in the first embodiment.
[0051] In the manufacturing method of the hot-rolled steel sheet according to the present embodiment, an annealing step of annealing in a continuous annealing line with an annealing temperature of 720°C or less and a plating step of plating in a continuous plating line can be applied. Furthermore, an alloying step of heating the plated hot-rolled steel sheet to 480°C or more and 600°C or less and performing an alloying treatment may be included. This annealing treatment or this plating treatment does not affect the material properties of the hot-rolled steel sheet according to the present embodiment. Therefore, it is possible to further perform a plating treatment on the surface of the hot-rolled steel sheet to provide a plating layer on the surface of the steel sheet.
[0052] As described above, the coating process and the composition of the coating bath do not affect the material properties of the hot-rolled steel sheet according to the present embodiment, and therefore, any of hot-dip galvanizing, galvannealing, and electrolytic galvanizing processes can be used as the coating process. The composition of the coating bath can include one or more of Zn, Al, Mg, Si, and Ni. That is, the composition of the coating layer formed on the surface of the hot-rolled steel sheet in the coating process can include one or more of Zn, Si, Al, Ni, and Mg. EXAMPLES
[0053] The embodiments of the present invention will be further described with reference to examples. Note that the present invention is not limited to the manufacturing conditions and product performance shown in the following examples. The embodiments can achieve the desired performance within the scope of the present invention.
[0054] <First form using continuous casting method> Steel material having a thickness of 250 mm and having the chemical composition shown in Table 1 was hot rolled under the rough rolling and finish rolling conditions shown in Table 2, and then temper rolled at an elongation rate of 0.1 to 0.5% and pickled to produce steel plates for evaluation.
[0055] <Second form using thin slab continuous casting method> Steel having the chemical composition shown in Table 1 was hot rolled into thin slabs under the conditions shown in Table 3, and then the slabs were temper rolled to an elongation rate of 0.1 to 0.5% and pickled to produce steel sheets for evaluation.
[0056] <Third form by hot continuous rolling method> Steel having the chemical composition shown in Table 1 was joined into a sheet bar under the conditions shown in Table 4, and the joined sheet bar was hot rolled, temper rolled to an elongation rate of 0.1 to 0.5%, and pickled to produce the steel plate to be evaluated.
[0057] <Manufacturing method for imparting a plating layer to a hot-rolled steel sheet> The hot-rolled coil produced under the conditions in Table 2 was pickled, and then the hot-rolled steel sheet was galvanized in a continuous hot-dip galvanizing line (CGL) under the conditions shown in Table 5. In this manner, a continuous hot-dip galvanized steel sheet (GI) and an alloyed hot-dip galvanized steel sheet (GA) were produced.
[0058] [Table 1]
[0059] [Table 2]
[0060] [Table 3]
[0061] [Table 4]
[0062] [Table 5]
[0063] [Table 6]
[0064] The hot-rolled steel sheets obtained under the conditions shown in Tables 2 to 5 were evaluated in terms of metal structure, tensile properties, bending workability, and toughness by the following methods. The results are shown in Table 6.
[0065] (i) Area ratio of metal structure Test pieces were cut out from the hot-rolled steel plate so that the cross section parallel to the rolling direction was the observation surface, and the center of the plate thickness was etched with 1% nital to reveal the structure. Photographs of the 1 / 4t portion of the plate thickness were then taken using a scanning electron microscope (SEM) at 2000x magnification and an accelerating voltage of 15 kV, covering 10 fields of view. Ferrite is a crystal grain that does not show any corrosion marks within the grains and is observed with a lower brightness than martensite (gray on SEM). Bainite and tempered martensite are crystal grains in which three or more adjacent lath-shaped corrosion marks with a width of 500 nm or less are observed within the grains. Martensite is a crystal grain that does not show any corrosion marks within the grains, but is observed with a higher brightness than ferrite (white on SEM). The area ratio of the metal structure was determined using image analysis software (Photoshop elements and Image J) for the structures separated in the above manner. The retained austenite was measured by grinding the surface of the test piece to 3 / 4 of the total thickness, chemically polishing it to 0.1 mm or more, and then measuring the polished surface by X-ray diffraction. The volume fraction of the retained austenite was measured from the peaks of (200)α, (211)α, (220)α, (200)γ, (220)γ, and (311)γ using MoKα radiation as the incident radiation source. The volume fraction of the retained austenite phase obtained in this way was taken as the area fraction of the retained austenite.
[0066] The area ratio of the structure with large crystal distortion that does not have a lath structure was measured using SEM and EBSD. Before observation, the test piece was marked with a Vickers tester or the like so that the same field of view could be obtained for SEM and EBSD. When observed with SEM, the structure with large crystal distortion that does not have a lath structure has corrosion marks within the grains. In this case, depending on the shape of the corrosion marks, there may be some that are not laths but look like laths. In this case, to distinguish between the structure that looks like lath and the lath structure, a rectangular structure that occurs within a grain with a short side width of more than 500 nm and two or less adjacent grains is not considered to be a lath structure. A structure with a short side width of 500 nm or less and three or more adjacent grains was considered to have a lath structure observed in bainite or tempered martensite. This lath structure can be more clearly distinguished by observation with a transmission electron microscope (TEM). Then, EBSD analysis was performed using OIM Analysis software (TSL). The KAM value analysis was performed under the condition of 1st nearest neighbor. By EBSD analysis, the grains surrounded by high-angle grain boundaries with an angle difference of 15° or more, in which the required KAM value exceeds 1.0 and the structure does not have a lath structure, are defined as structures with large crystal distortion without a lath structure, and are classified as 1 mm 2 The area ratio was calculated for the above fields of view.
[0067] (ii) Average particle size of Ti-containing carbides A thin film for observation was taken from a location equivalent to 1 / 4 of the plate thickness of the hot-rolled steel plate, and 300 or more Ti-containing carbides were photographed at a magnification of 600,000 or more using a transmission electron microscope. The circle equivalent diameters of the photographed Ti-containing carbides were calculated, and the average value was used as the average particle size. Ti-containing carbides can be identified by checking the presence or absence of a peak derived from Ti using EDX, which is attached to the TEM.
[0068] (iii) Analysis of Ti-containing carbide precipitation amount The front and back surfaces of the test piece were ground by 25% of the plate thickness, then dissolved in a 10% AA electrolytic solution, the solution was filtered through a filter with a mesh size of 0.2 μm, and the Ti concentration in the filtered electrolytic solution was analyzed using ICP-MS. Furthermore, the amount of Ti precipitated as TiN was calculated from [amount of Ti contained] × 48 / 14. The amount of Ti precipitated as TiS was calculated from [amount of Ti contained] × 48 / 32. The amount of Ti precipitated was calculated by subtracting the Ti concentration contained in the electrolytic solution, the amount of Ti precipitated as TiN, and the amount of Ti precipitated as TiS from the amount of Ti contained.
[0069] (iv) Tensile test From the hot-rolled steel sheets obtained under the conditions shown in Tables 2 to 5, JIS No. 5 tensile test pieces were prepared in the direction perpendicular to the rolling direction, and tensile tests were performed five times in accordance with the provisions of JIS Z 2241 (2011) to determine the average yield strength (YS) and tensile strength (TS). The crosshead speed of the tensile test was 10 mm / min. In Table 6, the steel sheets with a yield strength of 680 MPa or more were considered to be examples of the invention.
[0070] (v) Bending test From the hot-rolled steel sheets obtained under the conditions shown in Tables 2 to 5, test pieces with a width of 35 mm and a length of 100 mm were taken from which the end faces were ground, and a bending test was carried out five times using the V-block method described in JIS Z 2248. Test pieces with an R / t of 0.5 or less were marked with "◯" as they had the characteristics required by the present invention, and test pieces in which cracks were found on the surface of the test piece at least once under conditions of an R / t of 0.5 or less were marked with "X" as they did not have the characteristics required by the present invention.
[0071] (vi) Charpy impact test From the hot-rolled steel sheets obtained under the conditions shown in Tables 2 to 5, V-notch test pieces as specified in JIS Z2242 were taken so that the longitudinal direction was normal to the rolling direction. When the thickness of the hot-rolled steel sheets was less than 10 mm, multiple test pieces were stacked, holes were drilled at the ends of the test pieces, and the pieces were connected with bolts to adjust the thickness to 10±1 mm. The test pieces were immersed in a bath adjusted to -40°C for 10 minutes or more, and then tested according to the method conforming to JIS Z 2242. The test results are shown in Table 6. When the absorbed energy was 30 J / cm 2 The above are the characteristics required in this invention, and are marked with "○" at 30 J / cm 2 Any level below this level is marked with "X" since it is not a characteristic required by the present invention.
[0072] All of the examples of the present invention had a yield strength (YS) of 680 MPa or more, and good bending workability and toughness were obtained. On the other hand, the comparative examples outside the range of the present invention either did not reach a yield strength of 680 MPa or did not obtain the bending workability or toughness required by the present invention.
Claims
1. In mass percent, C: 0.035% or more and less than 0.110%; Si: 1.5% or less, Mn: 1.3% or less, P: 0.05% or less, S: 0.010% or less, Al: 0.005% or more and 0.080% or less, N: 0.0060% or less, Ti: 0.08% or more and 0.20% or less; Optionally, it further contains one or both of the following components from group A and group B: Note Group A; B: 0.0002% or more and 0.0050% or less, Group B; One or more of Nb, V, Mo, Sb, REM, Mg, Ca, Sn, Ni, Cu, Co, As, Cr, W, Ta, Pb, Cs, Zr, Hf, Te, Bi, and Se are each 0.03% or less, and the total is 1% or less; The balance is Fe and unavoidable impurities. The area ratio of the metal structure is Ferrite is 0% or more and 85% or less. Retained austenite is 3% or less. Lath-shaped structure is 5% or less, The KAM value of the tissue is 1.0 or more and 15% or more of the tissue is A hot-rolled steel sheet having a yield strength of 680 MPa or more and containing Ti-containing carbides with an average grain size of 8 nm or less.
2. The hot-rolled steel sheet according to claim 1, further comprising a plating layer on a surface of the hot-rolled steel sheet.
3. A rough rolling process in which the steel material having the composition according to claim 1 is roughly rolled into a sheet bar by heating the steel material to a heating temperature of 1200 ° C. or more, or by not heating the steel material after casting; a finish rolling step of finish rolling the sheet bar at a start temperature of 950° C. or more and 1100° C. or less, a total reduction rate from the first pass to the fifth pass of 75% or more, and a rolling completion temperature of 860° C. or more and 910° C. or less to obtain a hot-rolled steel sheet; A cooling step of cooling the hot-rolled steel sheet to a cooling stop temperature of 600° C. or more and 700° C. or less at an average cooling rate of 40° C. / s or more; a coiling step of coiling the cooled hot-rolled steel sheet at a coiling temperature of 600° C. or more and 700° C. or less; Including, The obtained hot-rolled steel sheet has the following area ratio of metal structure: Ferrite: 0% to 85% Retained austenite is 3% or less. Lath-shaped structure is 5% or less, The tissue with a KAM value of 1.0 or more is 15% or more, A method for producing a hot-rolled steel sheet, comprising the steps of: forming a hot-rolled steel sheet having a yield strength of 680 MPa or more; and forming a hot-rolled steel sheet having carbides containing Ti having an average particle size of 8 nm or less.
4. A casting process is included prior to the rough rolling process or the finish rolling process, in which a steel material having a thickness of 35 mm or more and 200 mm or less and having the component composition according to claim 1 is cast, The method for producing a hot-rolled steel sheet according to claim 3, characterized in that the rough rolling step is applied or not applied to produce a sheet bar.
5. Between the rough rolling step and the finish rolling step, a joining step of joining the roughly rolled sheet bar and a preceding sheet bar at 1050 ° C. or more is included; The method for producing a hot-rolled steel sheet according to claim 3, characterized in that, in the finish rolling step, the joined sheet bar is finish-rolled.
6. Further, a hot-rolled steel sheet annealing process is performed in which the hot-rolled steel sheet is annealed at an annealing temperature of 720° C. or less. A plating process for plating the annealed hot-rolled steel sheet; The method for producing a hot-rolled steel sheet according to any one of claims 3 to 5, further comprising the steps of:
7. The method for producing a hot-rolled steel sheet according to claim 6, further comprising an alloying step of subjecting the plated hot-rolled steel sheet to an alloying treatment at a temperature of 480°C or higher and 600°C or lower.
Citation Information
Patent Citations
Manufacture of hot rolled steel plate for working, excellent in formability and toughness, by using continuous hot rolling process
JP1997227949A
High strength thin steel sheet having excellent hole expansibility and local ductility and method for producing the same
JP2011225938A
High-strength hot rolling steel sheet and production method thereof
JP2015028207A
High strength hot rolled steel sheet and manufacturing method therefor
JP2017179539A
High-strength steel plate with excellent formability and stability of material properties, and method for manufacturing same
WO2012147898A1