Cerium 12 boride and its manufacturing method

By applying ultra-high pressure and high-temperature conditions with a laser-heated diamond anvil cell, CeB12 is successfully synthesized, providing stable crystals for magnetic, electronic, and hard materials, addressing the synthesis challenges of cerium dodecoboride.

JP7569038B2Active Publication Date: 2024-10-17NAT INST FOR MATERIALS SCI +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020193300
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-20
Publication Date
2024-10-17
Estimated Expiration
2040-11-20

AI Technical Summary

Technical Problem

The synthesis of cerium dodecoboride (CeB12) has been challenging due to its high melting point and the difficulty in incorporating larger cerium atoms into the boron cage structure, requiring ultra-high pressures that are difficult to achieve and often cause equipment problems.

Method used

A method involving ultra-high pressure and high-temperature conditions using a laser-heated diamond anvil cell to synthesize CeB12, allowing cerium atoms to be incorporated into a boron cage structure by reducing their size through increased valence, enabling production under pressures of 15 GPa or higher and temperatures of 2000K or higher.

Benefits of technology

The synthesized CeB12 is stable at normal pressure and temperature, offering new crystals with various functionalities as magnetic, electronic, and hard materials, overcoming the limitations of previous synthesis methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569038000003
    Figure 0007569038000003
  • Figure 0007569038000004
    Figure 0007569038000004
  • Figure 0007569038000005
    Figure 0007569038000005
Patent Text Reader

Abstract

To produce a cerium polyboride that has been impossible to conventionally synthesize, the cerium polyboride having a high potential as a functional material.SOLUTION: The inventive cerium boride compound is a CeBn compound including the crystal that can be represented by the general formula CeB12, with 9<n<15. The polyboride cerium compound is thought to have various functionalities such as semiconductivity, superconductivity, diamagnetism, paramagnetism, ferromagnetism, antiferromagnetism, light absorbency, thermoelectricity, hardness. The cerium is larger in ion radius or the like than heavy rare earth elements and has not been conventionally synthesized. Thus, under ultra high pressure and high temperature conditions, a polyboride cerium compound including a cerium 12 boride is produced.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to cerium dodecaboride and a method for producing the same. [Background technology]

[0002] It is known that rare earth elements such as lanthanides form boron-rich borides. These are relatively stable even at high temperatures and are sparingly soluble, and have attracted attention as semiconductors, superconductors, diamagnetic materials, paramagnetic materials, ferromagnetic materials, and antiferromagnetic materials. For example, lanthanum hexaboride is a heat-resistant, inert, and sparingly soluble compound, and is known to be suitable for thermal cathodes due to its low work function for electrode emission, and to be an excellent light absorber (for example, Patent Document 1). In addition, yttrium boride (YB6, YB 12 , Y.B. 25 , Y.B. 50 , Y.B. 66 ) are known to be hard solids with high melting points, and YB6 in particular exhibits superconductivity at relatively high temperatures (8.4 K) and is suitable for cathode ray tubes, just like LaB6, but has the same structure as other hexaborides such as LaB6. 12 Its structure is cubic and its density is 3.44 g cm -3 It has a Pearson symbol cF52, a space group Fm-3m (No. 225), and a lattice constant a = 0.7468 nm, making it an excellent thermoelectric material. Other rare earth borides, based on their properties, are also used as semiconductors, superconductors, diamagnetic, paramagnetic, ferromagnetic, and antiferromagnetic materials, as well as light absorbers and thermoelectric materials (e.g., Patent Document 2), and even as hard materials (or hard substances) (e.g., Patent Document 3).

[0003] However, it is not desirable from the viewpoint of productivity to rely on only limited rare earth elements such as yttrium and lanthanum, and considering the scarcity of rare earth elements, it is desirable to be able to use borides of other types of rare earth elements as well. Rare earth elements share common properties and are considered to be interchangeable.

[0004] In particular, polyboride crystals in which the skeleton is formed by boron share common properties such as crystal hardness, so the functionality can be enhanced depending on the type of rare earth element contained. For example, TbB 12 , DyB 12 , HoB 12 , ErB 12 , TmB 12 In the above, the antiferromagnetic transition temperatures are T N =19.2, 16.5, 7.5, 6.7, and 3.4 K (for example, Non-Patent Document 1). The ionic radii of these rare earth elements decrease in this order.

[0005] As mentioned above, research into the synthesis of rare earth polyborides has been conducted for a long time in the context of research into magnetic materials and field emission electron sources, but due to the high melting point of boron (2180°C), they have been synthesized under one atmosphere using the FZ (float zoning) method, which allows for high temperatures to be generated. Rare earth boron compounds are extremely hard substances, which is thought to be due to the extremely high stability of the cage-like structure of boron. However, with regard to rare earth dodecaborides, cerium dodecaboride (CeB 12 The inventors of the present application have never heard of any reports of the synthesis of light rare earth compounds such as cerium (Ce). One of the reasons for this is thought to be that the atomic and ionic radii of elements such as cerium (Ce) are larger than those of heavy rare earth elements such as gadolinium (Gd), terbium (Tb), dysprosium (Dy), holonium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu) (Figure 9). This is thought to be because the ionic radii of heavier elements become smaller due to lanthanide contraction. GdB 12 and SmB 12 The synthesis of RB6 and RB has been reported (for example, Non-Patent Document 2 and Non-Patent Document 3). 12 Polyborides with high boron concentrations, such as PrB (where R is a rare earth element), have a boron cage structure of a truncated cubic or truncated octahedral shape, with the rare earth element located at the center, making it difficult to incorporate large elements. 12 and CeB 12Although it has not been synthesized, it is expected to have a multipole order, and from the electron-hole symmetry, it is expected to be a Kondo insulator (for example, Non-Patent Document 4, Non-Patent Document 5, Non-Patent Document 6, Non-Patent Document 7, Non-Patent Document 8, Non-Patent Document 9). Furthermore, even if high pressure is applied, it is not clear how much pressure is required to synthesize this material. In particular, ultra-high pressure of 20 GPa or more is likely to cause various problems in the device and is not easily achievable. Incidentally, Patent Document 4 also mentions that the thermionic emission cathode is made of CeB 12 Although an X-ray inspection apparatus characterized by including the above is claimed, it is not enabled. Therefore, it is not substantially described. 12 Attempts have been made to replace part of the Y with other elements (e.g., Ce, Pr, Nd), but the Y substitution rate is not very high, and CeB 12 It cannot be said that the product was manufactured in this state (Non-Patent Document 9). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Laid-Open No. 2014-84385 [Patent Document 2] Japanese Patent Application Laid-Open No. 2012-44201 [Patent Document 3] Japanese Patent Application Laid-Open No. 2002-294384 [Patent Document 4] Japanese Patent Application Laid-Open No. 2005-207945 [Non-patent literature]

[0007] [Non-Patent Document 1] "Handbook on the Physics and Chemistry of Rare Earths", Vol. 38 2008 Elsevier BV ISSN 0168-1273 [Non-patent document 2] "High-Pressure Synthesis of Rare Earth Borides" High Pressure Science and Technology vol.26, No.3 216-224 (2016) [Non-patent document 3] "High Pressure Syntheses of SmB2 and GdB12" Journal of the Less-Common Metals, 56 (1977) 83-90 [Non-patent document 4] Grant-in-Aid for Scientific Research (16K05431) Research Report "High-Pressure Synthesis and Extreme Condition Physical Properties of Novel Cage-Shaped Rare Earth Borides" (June 26, 2020) [Non-patent document 5] 74th Annual Meeting of the Physical Society of Japan (2019) "High-Pressure Synthesis and Physical Properties of Novel Rare Earth Dodecaborides (Y,R)B12 (R=Ce, Pr, Nd)" [Non-patent document 6] FY2019 Institute for Solid State Physics Short-Term Workshop "Development of New Materials by High-Pressure Synthesis and Combination of High-Pressure Measurement Techniques" July 5-6, 2019 C8 "Development and Properties of Kondo Insulator Substituted Alloys by High-Pressure Synthesis" [Non-Patent Document 7] Poster session at the Autumn Meeting of the Physical Society of Japan (2019) "Material Development and Fundamental Properties of Light Rare Earth Dodecaborides (R=Ce~Gd) Synthesized under Ultra-High Pressure" [Non-patent document 8] 60th High Pressure Symposium of the Japan High Pressure Society, October 23, 2019, "Preparation and Properties of Substituted Alloys of the Kondo Insulator YbB12 and New Rare Earth Dodecaborides" [Non-Patent Document 9] 74th Annual Meeting of the Physical Society of Japan (2019) "Attempt to prepare substitution alloys Y1-xRxB12 (R = Ce, Pr, Nd) by high-pressure synthesis" Summary of the Invention [Problem to be solved by the invention]

[0008] As mentioned above, rare-earth borides are expected to be used as magnetic materials, semiconductors, topological insulators, electronic materials such as superconductors, and other electromagnetic materials. 12are considered to be excellent electronic materials such as Kondo insulators. However, due to the high melting points and size of each rare earth element, their production is not easy, and so far, production has been achieved in order from small size under normal pressure to pressurized conditions (low). However, there have been no reports of the production of praseodymium (Pr) or cerium (Ce). This is thought to be because a higher pressure than ever before is required. Overcoming these difficult conditions, CeB, which is particularly expected to be a Kondo insulator, 12 The purpose is to provide. [Means for solving the problem]

[0009] The polyborides according to the embodiment of the present invention are CeB 12 As shown in FIG. 9, rare earth element ions (Ln 3+ The size of the elements increases in the order of Ho, Dy, Tb, Gd, Eu, Sm, Pm, Nd, and Pr in the coordination number 6 or 9. The dodecaborides of the smaller elements can be prepared under one atmosphere or by the floating zone method. For example, GdB 12 , SmB 12 In the study, the production of CeB under high pressure of 5-10 GPa was reported. 12 It is conceivable that production could be carried out under pressure of 50 GPa, but it is extremely difficult to achieve such pressure and heat the material to the required temperature.

[0010] Therefore, we used a device that can apply ultra-high pressure of at least 20 GPa and heat up to high temperatures to test the CeB 12 When they attempted to produce cerium dodecaboride, they succeeded in producing this compound, CeB 12 The crystal expressed by (hereinafter referred to as "CeB 12 The compound may contain Ce in a tetradecahedron structure (truncated octahedron) formed by boron atoms. 12Compounds containing crystals can have various functionalities, such as semiconductivity, diamagnetism, paramagnetism, ferromagnetism, antiferromagnetism, light absorption, thermoelectricity, or hardness. Therefore, it is considered that they can constitute semiconductor materials, superconductor materials, diamagnetic materials, paramagnetic materials, ferromagnetic materials, antiferromagnetic materials, light absorption materials, thermoelectric materials, or hard materials. These materials can be subjected to predetermined processing and shaped to form the respective elements.

[0011] As for cerium borides, CeB4 and CeB6 are known as tetragonal and cubic cerium borides, respectively. 12 The crystal is characterized by a cage-like structure of boron and is expected to be a hard material with various functions. 12 The crystal has not yet been synthesized by anyone other than the present inventors. Furthermore, there are no CeB crystals with structures other than the cage structure inferred from other rare earth borides. n Crystals (n>6, e.g., n=12) are also expected to have more favorable functions. n The compounds may include those having these possible crystal structures.

[0012] The tetradecahedral structure of boron atoms is rigid, and Ce has a larger atomic and ionic radius than gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), or lutetium (Lu). For example, the atomic and trivalent ionic radii disclosed in Shanon (1976) [(RD Shanon, Acta Cryst. A32, 751 (1976))] are plotted as shown in Figure 9. In particular, the ionic radius tends to become smaller as the atomic number increases due to the so-called lanthanide contraction. Therefore, CeB 12 In the case of cerium (Ce), it is thought to be particularly difficult to enter the crystal represented by CeB 12 This is because polyboride crystals with a high boron concentration, such as those described above, have a truncated octahedral boron cage structure with Ce located at the center.

[0013] In order to incorporate light rare earth elements with a larger size than heavy rare earth elements into the boron cage structure, a synthesis method in a state where the atomic size is reduced is considered suitable. However, under high pressure, it is also considered that not only the atomic size but also the boron cage structure shrinks. On the other hand, similar to the synthesis method at atmospheric pressure, since the melting point of boron is high in the synthesis of borides, a higher temperature is required even in the synthesis under high pressure. Therefore, by combining laser heating under high pressure, a high-pressure and high-temperature state was generated to synthesize cerium polyboride.

[0014] More specifically, the following can be provided. A cerium boride compound represented by the general formula CeB n and containing CeB 12 crystals, characterized in that 9 < n < 15. The above-mentioned cerium boride compound, characterized in that Ce in the CeB 12 crystals has a valence greater than 3. The above-mentioned cerium boride compound, characterized in that the crystal structure of the CeB 12 crystals may belong to the cubic crystal structure of the space group Fm-3m, and the space group number may be 225. The above-mentioned cerium boride compound, characterized in that in the CeB 12 crystals, the lattice constant a = 7.54 ± 0.4 Å. A magnetic material characterized by containing any of the above-mentioned cerium boride compounds. A Kondo insulator material characterized by containing any of the above-mentioned cerium boride compounds. A thermoelectric material characterized by containing any of the above-mentioned cerium boride compounds. A superconducting material characterized by containing any of the above-mentioned cerium boride compounds. Mixing raw materials of one or more CeB m compounds (0 < m ≤ 6) and boron in a predetermined ratio and heating them to a temperature of 2000 K or higher under ultra-high pressure, with the general formula CeBn represented by (9 < n < 15), and CeB 12 A method for producing a compound (particularly, a cerium boride compound) characterized by containing crystals. The method for producing the above-described compound, characterized in that the ultrahigh pressure may be a pressure of 15 GPa or more. A method for producing any of the above-described compounds, characterized by laser heating using a diamond anvil cell. Here, for n described above, it may be 11 < n, it may be n < 13, or it may be expressed as 11 < n < 13. Also, the valence exceeding 3 means that Ce 3+ and Ce 4+ may mean a state in which they are mixed. Particularly, the relative molar% of Ce with respect to the combined total of both is preferably 10% or more, preferably 20% or more, preferably 40% or more, or preferably 50% or more. It is preferably 100% or less or less than 100%. Specifically, the valence may be 3.1 or more, 3.2 or more, or 3.3 or more. Also, it may be 4 or less or less than 4. [Advantages of the Invention]

[0015] By confining a compound that can be a raw material for cerium polyboride under ultrahigh pressure (for example, 15 GPa or more) and further heating it to a high temperature by laser, cerium polyboride can be synthesized under conditions of high temperature (for example, 2000 - 3000 K). The synthesized cerium polyboride is stable even when taken out under normal pressure and normal temperature. In that cerium polyboride, mainly CeB 12 crystals may be included. All of these CeB 12 crystals are novel crystals that have not been reported so far and are also compounds. Thus, since cerium polyboride is stable under normal pressure and normal temperature, it can be used as a material in fields that utilize its function in various forms. [Brief Description of the Drawings]

[0016] [Figure 1] It is a schematic diagram showing the crystal structure of CeB12 in an embodiment of the present invention.​​ [Figure 2] FIG. 1 is a schematic diagram showing the entire diamond anvil cell equipped with diamond anvils. [Figure 3] FIG. 3 is a schematic diagram showing details of the diamond anvil cell of FIG. 2. [Figure 4] FIG. 1 is a diagram showing a measurement system for X-ray structural analysis. [Figure 5] FIG. 2 is a diagram showing the results of X-ray diffraction of a sample in Experimental Example 2 in an example of the present invention. [Figure 6] This is a diagram outlining the measurement system for X-ray absorption near-edge structure. [Figure 7] 1 is a graph showing the results of XANES measurements. [Figure 8] 1 is a graph plotting the a-axis sizes of rare earth dodecaboride crystals synthesized by the present inventors. [Figure 9] 1 is a graph plotting the trivalent ionic radii of La-based rare earth elements (in the cases of coordination numbers 6 and 9). DETAILED DESCRIPTION OF THE INVENTION

[0017] Hereinafter, an embodiment of the present invention will be described with reference to the drawings, in which like elements are designated by like reference numerals and their description will be omitted.

[0018] Rare earth borides have been obtained by, for example, mixing rare earth oxide powder and boron powder in a predetermined ratio, compressing the mixture, and heating it in a vacuum or in an inert gas. The chemical reaction is expected to be as follows: where R is the rare earth element. R2O3+(2n+3)B → 2RB n +3BO↑ In this process, rare earth borides can be produced by changing n. However, if n is large, the reaction may not proceed sufficiently. Therefore, here, CeB6 is produced first. The reaction formula is as follows. Although trivalent Ce oxide can also be used, tetravalent Ce oxide is used here. CeO2+8B → CeB6+2BO↑

[0019] Specifically, CeO2 powder and B powder are weighed out in equal amounts, stirred and mixed in an automatic mortar for 30 minutes, and the mixed powder is compressed using a rubber press or similar, and fired for a predetermined time at a temperature of 1000°C or higher in a non-oxidizing atmosphere such as a vacuum or inert gas. The CeB6 after the reaction is then crushed and powdered. At this time, if there are impurities or unreacted reactants remaining, they are washed with hydrochloric acid or similar. Then, CeB6 is weighed according to the following formula and mixed with B powder to obtain CeB6. 12 It is used as a mixed powder raw material for synthesis. CeB6+6B → CeB 12 The mixed powder raw material is compressed using a rubber press or the like and fired for a predetermined time at a temperature of 1000°C or higher in a non-oxidizing atmosphere. The pressure and other conditions at this time will be described later. 12 It can be confirmed that it is a single phase by X-ray diffraction analysis. CeB4 can be used instead of or in addition to CeB6. CeB4 can be obtained, for example, by mixing raw materials according to the following formula, compacting the mixture, and firing it. CeO2+6B → CeB4+2BO↑ And CeB 12 can also be obtained by mixing raw materials according to the following formula, pressing the mixture into powder, and firing it in the same manner. CeB4+8B → CeB 12

[0020] As mentioned above, the target boride cannot be obtained without high pressure, so a method and apparatus that combines ultra-high pressure and high temperature is used. That is, by heating predetermined amounts of raw material powders of CeB6 powder and B powder to high temperature under ultra-high pressure, CeB6 powder can be obtained. n The inventors of the present invention have succeeded in synthesizing a novel cerium boride (n=12) compound. The produced cerium boride (12B) is a compound (including its crystal structure) that has not been reported before, and it has been confirmed to be a novel crystalline compound based on its constituent components and crystal structure.

[0021] In an embodiment of the present invention, FIG. 1 shows a graph of cerium 12 boride (CeB 12 The crystal structure of CeB synthesized by the present inventors is shown in Fig. 12 Single crystal structure analysis of the CeB 12 The crystal belongs to the cubic crystal system and belongs to the Fm-3m (where "-" indicates an overline of 3) space group (space group 225 of the International Tables for Crystallography), with the crystal parameters and atomic coordinate positions shown in Table 1. This crystal structure is a tetradecahedron with B atoms located at the 24 vertices of a truncated octahedron, and Ce is contained within the tetradecahedron. In Table 1, the lattice constant a indicates the length of the axis of the unit cell, and α, β, and γ indicate the angles between the axes of the unit cell. The atomic coordinates indicate the position of each atom in the unit cell. The lattice constant may be within the range of a = 7.54 ± 0.4 Å (or ± 5%). The angles α, β, and γ between the axes of the unit cell may each be within the range of 90 degrees ± 4 degrees.

[0022] [Table 1]

[0023] CeB 12 The crystal shown by (CeB 12The lattice constant of the crystalline structure of CeB can change by changing the ratio of the constituent elements Ce and B or by substituting other elements, but the crystal structure and the atomic positions given by the sites and their coordinates do not change so much that the chemical bonds between the skeletal atoms are broken. Here, by changing the ratio of Ce and B or substituting other elements, the general formula becomes CeB 12±d E e (d and e are real numbers equal to or greater than 0, and E is a substituting element). In the examples of the present invention, the length of the Ce-B chemical bond calculated from the lattice constant and atomic coordinates obtained by Rietveld analysis of the results of X-ray diffraction or the like of the target substance in the space group Fm-3m is CeB shown in Table 1. 12 If the difference between the lattice constant of the crystal and the calculated atomic coordinates is within ±5%, it can be determined that the crystal structure is the same. If the length of the chemical bond exceeds ±5%, the chemical bond may break and a different crystal may be formed. Another simple method of determination is CeB 12 The main peaks (for example, about 10 peaks with the strongest diffraction intensity) of the X-ray diffraction of the crystal may be compared with those of the target substance. In the embodiment of the present invention, the cerium boride compound is CeB 12 It may contain crystals. 12 The crystal may be the main component.

[0024] From this viewpoint, in the cerium boride compounds of the examples of the present invention, CeB 12 The crystal shown by is CeB 12 The molar ratio of Ce to B may be different from the equivalence (i.e., Ce-rich or B-rich), or a part of Ce and B may be replaced by other elements (e.g., C, N, O, H, etc.). 12 As shown in Table 1, the crystal represented by is a cubic crystal with the symmetry of the space group Fm-3m, but the lattice constant a may be in the range of a = 7.54 ± 0.4 Å (or ± 5%). If it is within this range, the crystal is considered to be stable.

[0025] In an embodiment of the present invention, the cerium boride compound containing cerium diboride (CeB 12 ) compound may have CeB 12 crystal as the main component. The cerium diboride (CeB 12 ) compound preferably contains 70% by weight or more of CeB 12 crystal. More preferably, it contains 90% by weight or more. Still more preferably, it contains 95% by weight or more.

[0026] In an embodiment of the present invention, the cerium diboride compound may be composed of crystals represented by CeB 12 , but in addition to the crystals represented by CeB 12 , it may contain cerium boride crystals or compounds represented by CeB x (9 < x < 12 or 12 < x < 15). Also, in CeB x , 11 < x < 12 or 12 < x < 13 may be satisfied. The content of such CeBx may be 0% by weight or more. Also, it may be less than 5% by weight.

[0027] In an embodiment of the present invention, the cerium diboride compound may preferably have a molar ratio of B to Ce of 9 or more and 15 or less. Also, the molar ratio of B to Ce may be 11 or more and 13 or less. Also, the molar ratio of B to Ce may be 11.5 or more and 12.5 or less.

[0028] In an embodiment of the present invention, an exemplary method for producing the CeB y compound will be described.

[0029] In the examples of the present invention, the raw material powder may be Ce elemental and / or Ce-containing compounds such as oxides and carbonates, and B elemental (for example, crystalline boron) and / or B compounds. Alternatively, low boride cerium may be prepared first and used as the raw material. The raw material powder is preferably a powder having a particle size of 100 nm or more and 500 μm or less. This can further promote the reaction. Preferably, the raw material powder may be a powder having a particle size of 200 nm or more and 200 μm or less. The particle size may be the volume-based median diameter (d50) measured by a microtrack or laser scattering method. The raw material powder may be 12-cerium boride (CeB 12 The mixed raw material powder may be compacted by CIP or the like, or may be subjected to the subsequent high-temperature and high-pressure treatment as is.

[0030] In the embodiment of the present invention, in the manufacturing process, the starting material contains low cerium boride (CeB m (m≦6)) and boron may also be used. For example, CeB6 (e.g., homemade or manufactured by Kojundo Chemical Laboratory Co., Ltd., 12008-02-5, CeB6) can be used. The inventors of the present application have found that the truncated octahedral boron cage structure is very strong, and that under high-temperature and ultra-high-pressure conditions, the change in bond length between the boron atoms constituting the boron cage structure is at least relatively small. Therefore, under the same conditions, cerium atoms or ions become relatively small and are incorporated into the boron cage structure, resulting in the formation of a high-boride cerium compound.

[0031] The duration of the high-temperature, high-pressure treatment varies depending on the amount of raw materials and the apparatus used, but may be, for example, from 5 minutes to 24 hours. This treatment step may be performed by high-temperature, high-pressure treatment or shock compression using at least one apparatus selected from the group consisting of a diamond anvil cell, a multi-anvil apparatus, and a belt-type high-pressure apparatus. These methods may be capable of achieving a temperature range of, for example, 2000 K or higher, 2200 K or higher, or 2500 K or higher. There is no particular upper limit, but from an industrial standpoint or productivity standpoint, a temperature range of 3300 K or lower, 3100 K or lower, or 3000 K or lower may be achieved. Furthermore, a pressure range of 10 GPa or higher, 20 GPa or higher, 30 GPa or higher, or 40 GPa or higher may be achieved. There is no particular upper limit, but from an industrial standpoint or productivity standpoint, a pressure range of 100 GPa or lower, 80 GPa or lower, or 60 GPa or lower may be achieved. However, as long as the desired temperature and pressure are achieved, the apparatuses are not limited to those described above.

[0032] Here, we will explain the case where raw material powder is filled into a diamond anvil cell and processed. Figure 2 is a schematic diagram showing the entire diamond anvil cell (DAC). Figure 3 is a schematic diagram showing the details of the diamond anvil cell of Figure 2. An existing diamond anvil cell can be used, and as shown in Figure 2, diamond anvils 10 polished to have flat bottom surfaces are placed with their bottom surfaces facing each other, and pressure is applied to these bottom surfaces. As shown in Figure 3, 12-cerium boride (CeB 12 The raw material powder used for the reaction is held between a gasket 12 and a diamond anvil. The high-pressure section is filled with sodium chloride 14, which functions as a medium for transmitting temperature and pressure to the heating section 16 set inside. In particular, since the reaction sample (raw material) 18 is colored, such as blue or black, while sodium chloride is colorless, the energy from the laser beam 20 is concentrated exclusively on the heating section, such as the reaction sample or the capsule containing the reaction sample. This makes it easy to achieve high temperatures locally.

[0033] Next, the above-mentioned pressure is applied to the diamond anvil cell, and a laser beam such as a fiber laser is irradiated onto the raw material powder. The heating temperature is determined from the color temperature, and the laser irradiation time may be from several minutes to several tens of minutes after the temperature becomes constant. When the above-mentioned treatment is carried out by a high-temperature, high-pressure treatment method using a diamond anvil cell or a multi-anvil apparatus as shown in Figures 2 and 3, the pressure range is preferably 20 GPa or more and 55 GPa or less before treatment, and may be 15 GPa or more and 60 GPa or less after treatment. In the examples of the present invention, it has been found that the pressure before heating (before treatment) and the pressure after heating (after treatment) can be significantly different, and by adjusting these pressures so that they each satisfy the above-mentioned ranges, the above-mentioned cerium 12 boride (CeB 12 It is possible to produce cerium polyboride having a cerium hexaboride (CeB) crystal structure. More preferably, the pressure range may be 25 GPa or more and 50 GPa or less before the treatment, and may be 20 GPa or more and 55 GPa or less after the treatment. The pressure before heating and the pressure after heating can be adjusted so as to respectively satisfy the above-mentioned ranges. In this way, the above-mentioned cerium hexaboride (CeB) can be produced. 12 A compound containing cerium polyboride as a main component, including cerium polyboride crystals, can be produced. The pressure range may be, for example, 45 GPa or less, 40 GPa or less, 35 GPa or less, or 30 GPa or less. Industrially, lower pressures are preferable in terms of cost and production efficiency.

[0034] Furthermore, when the above-mentioned treatment is carried out by a high-temperature, high-pressure treatment method using a diamond anvil cell or a multi-anvil apparatus as shown in FIG. 2 or FIG. 3, the temperature range may be preferably 1000 K (727°C) or more and 4000 K (3727°C) or less. Within this range, the above-mentioned cerium 12 boride (CeB 12) crystals can be produced. More preferably, the temperature range may be 1500K (1227°C) or more and 3500K (3227°C) or less. The pressure range before the treatment may be 20GPa or more and 55GPa or less. After the treatment, the pressure range may be 15GPa or more and 60GPa or less. Such conditions can be selected. In this way, the above-mentioned cerium polyboride (CeB 12 It is possible to produce a compound containing cerium polyboride as a main component, including cerium polyboride crystals, in high yield.

[0035] The present invention will be described in more detail by way of the following examples, but these examples are merely provided to aid in the understanding of the present invention, and the present invention is not limited to these examples.

[0036] [Ingredients used] The raw material powders used were cerium oxide powder (CeO2, purity: 99.99%, average particle size: 8 μm, manufactured by Rare Metallic Co., Ltd.) and boron powder (morphology: crystalline, purity: 99%, manufactured by Kojundo Chemical Laboratory Co., Ltd.).

[0037] [Preparation of CeB6] CeB6 can be produced by the following reaction: As will be described later, this reaction has high reaction efficiency and does not require the mixing of either compound in excess. CeO2+8B → CeB6+2BO↑ The cerium oxide powder and boron powder were weighed according to the equivalent weights in the above formula and stirred and mixed in an automatic mortar for 30 minutes. This mixed powder was packed into a rod-shaped Imamura latex sleeve with a diameter of 8 mm and a length of 5–10 cm. A powder sample was compacted at 2500 atmospheres using a CIP (Crystal Injection Pump) manufactured by Nikkiso Co., Ltd. This compact was removed from the rubber and a heating feed rod, BN tube, carbon crucible, and carbon felt were inserted into a quartz tube placed in a high-frequency induction heating furnace (vacuum furnace manufactured by SELEC Co., Ltd.; heating power supply: transistor inverter type (200 kHz, 20 kW, manufactured by Nisshin Giken Co., Ltd.)). Induction heating was performed at approximately 1700°C for 1 hour in a vacuum atmosphere. The feed rod was then cooled to near room temperature and removed under atmospheric pressure. The feed rod was crushed and examined as follows. X-ray diffraction analysis of the powder revealed that a polycrystalline sample was produced. If unreacted cerium oxide or other materials remain, the sample powder can be removed by washing with hydrochloric acid for a day. Alternatively, the raw material rod after firing in an image furnace can be purified by zone melting using the FZ method. In this experimental example, X-ray diffraction analysis confirmed that no unreacted cerium oxide remained in any of the samples.

[0038] [CeB 12 Preparation of (Experimental Examples 1 to 13)] The above-mentioned CeB6 powder and boron powder (manufactured by Furuuchi Chemical Co., Ltd., purity: 99%) were weighed out according to the equivalent amounts in the following reaction formula, and stirred and mixed in an automatic mortar for 30 minutes. CeB6+6B → CeB 12 This mixed powder was filled into a rhenium gasket and placed in the sample section (heating section) of the laser-heated diamond anvil cell shown in Figure 3. The diamond anvil cell was pressurized before processing (pre-heating), and a laser beam from a 100-W fiber laser was irradiated onto the raw powder. The laser beam was focused to a diameter of 20 μm and scanned the entire raw powder, resulting in a temperature range shown in Table 2. The heating temperature was determined from the color temperature. The laser irradiation time was several minutes (5–10 minutes) after the temperature stabilized. The post-processing (post-heating) pressure was controlled to be the pressure shown in Table 2. In the case of the DAC high-pressure observation experiment, the pressure values ​​were measured using the Raman scattering spectrum of the diamond anvil and the X-ray diffraction spectrum of sodium chloride mixed into the sample.

[0039] Figure 4 shows the measurement system for X-ray structural analysis. As shown in Figure 4, the diamond anvil cell was used as the measurement system cell without decompressing the sample after processing, and X-ray structural analysis was performed. For example, X-rays from synchrotron radiation (KEK Photon Factory) were monochromatized with silicon (λ = 0.61210 Å) to obtain an X-ray diffraction pattern. X-ray structural analysis was performed from the obtained X-ray diffraction pattern, and crystal structure parameters such as lattice constants were determined.

[0040] Next, the diamond anvil cell was depressurized to 1 atmosphere, and the sample was removed from the cell and subjected to X-ray structural analysis to determine crystal structure parameters such as lattice constant. In this way, samples 1 to 13 in Table 2 were prepared. In Examples 1 and 2, the length of a obtained from X-ray structural analysis of the sample obtained under high pressure at the pressure (34.7 GPa) and laser heating temperature (2000-3000 K) in Example 1 was 7.2241(11) Å. The length of a obtained from the sample obtained under 1 atmosphere was 7.5412(3) Å. Similar results were obtained in Examples 3 and 4, Examples 8 and 9, Examples 10 and 11, and Examples 12 and 13. Under high pressure, the length of a shrank by approximately 4.2% and approximately 4.7% in Examples 1 and 2, and Examples 3 and 4. The volume also shrank similarly. Therefore, CeB, which is considered stable under ultrahigh pressure, was chosen. 12It can be seen that the above is stable even under normal pressure. The pressures in the production process were 34.7 GPa, 30.4 GPa, 35.5 GPa, 30.1 GPa, 28.2 GPa, 29.8 GPa, and 26.5 GPa in Examples 1, 3, 5-8, 10, and 12, respectively, and are considered to be 20 GPa or higher, 25 GPa or higher, or 30 GPa or higher. The production temperature was in the range of 2000-3000 K (1727-2727°C), and is considered to be 1500 K or higher, 1750 K or higher, or 2000 K or higher.

[0041] [Table 2]

[0042] The XRD pattern of the sample obtained in Example 2 is shown in Figure 5. The assigned crystal structure and plane index are noted for each notable peak. The strong NaCl peak is attributed to the contaminating medium, sodium chloride. All notable peaks are CeB 12 Therefore, it can be seen that cerium polyborides as the second component were not detected. However, if the second component is contained, it can be separated by a known method. The CeB 12 The bulk moduli of CeB6 and its raw material were measured, and the results were 204 GPa and 172 GPa, respectively. The measurements were carried out at SPring-8 BL10XU of the Japan Synchrotron Radiation Research Institute. As a result, it was possible to obtain cerium boride with higher rigidity than conventional cerium boride. A compound with high rigidity is expected to have excellent mechanical properties such as hardness, and also to have excellent phonon transmission and heat transmission. Then, the CeB6 according to the embodiment of the present invention 12 The crystal-containing compounds may also be used as acoustic, sensor, and heat transfer materials.

[0043] From the above, by using a compound containing Ce and boron as raw material powder and processing it in the temperature range of 2000 K or more and the pressure range of 25 GPa or more, it is possible to obtain at least CeB 12It can be seen that a cerium polyboride compound containing crystals was produced. This is surprising in light of the prior art, as shown in Figure 9, because the size of Ce is larger than that of other rare earth elements.

[0044] Also, the obtained CeB 12 The crystal has the crystal parameters shown in Table 1, and is a novel crystal that has not been reported before, indicating a polyboride cerium compound. The truncated cubic and truncated octahedral boron cage structures are very strong and are less likely to shrink than rare earth elements. Therefore, the size of rare earth elements becomes relatively smaller under high pressure, which may not be the only reason why the synthesis of dodecaborides is possible.

[0045] Therefore, we performed X-ray absorption fine structure analysis of the Ce region using X-ray absorption spectroscopy. Specifically, we performed X-ray absorption near edge structure (XANES) analysis using an XAFS (Extended X-ray Absorption Fine Structure) apparatus, as shown in Figure 6. Monochromated X-rays were passed through an ion chamber and irradiated onto the sample as incident X-rays while monitoring their intensity. The X-rays transmitted through the sample were passed through an ion chamber and further monitored to obtain spectroscopic results. Specifically, we performed this analysis at BL11S2 of the Aichi Synchrotron Light Center. XANES analysis is based on the shape of the spectrum; for example, the higher the valence number of the cation, the higher the shift in absorption spectrum toward higher energies. Therefore, it is generally believed that the chemical state (electronic state) of atoms, the symmetry of the coordination, and other aspects can be analyzed. Figure 7 shows the spectra of Experimental Example 1, CeO2, and CeB6. CeO2 is shown as a tetravalent form of Ce, and CeB6 is shown as a trivalent form of Ce, and it can be seen that the CeB in this Experimental Example 1 is located somewhere between them. 12 It can be seen that the values ​​are between trivalent and tetravalent. If we read the simple peak positions, they are 5727.2 eV, 5726.2 eV, and 5731.2 eV, respectively. If we can calculate the ratio by proportional calculation, CeB12 The Ce can be considered to consist of 20% tetravalent and 80% trivalent.

[0046] From the above, we can see that the valence of Ce is greater than 3. Normally, the larger the valence of a cation, the smaller the ionic radius. Since the valence of Ce is greater than 3, CeB 12 It is expected that the ionic radius of Ce is small. If the ionic radius is small, it is thought that the B element can enter the strong cage structure more easily than expected. Therefore, the unexpected phenomenon mentioned above can be explained by this. Conversely, CeB produced under relatively low ultra-high pressure conditions 12 The valence of Ce may be easily greater than 3. Also, if the valence of Ce contained is greater than 3, CeB 12 is easy to manufacture.

[0047] Figure 8 shows a plot of the lattice constants of rare earth dodecaborides (cubic crystals) that the inventors of the present application have produced, arranged in order of atomic number. From Lu to Pr in this graph, the values ​​rise steadily to the right, showing the same trend as the increase in the trivalent ionic radius in Figure 9. However, CeB 12 In NdB 12 and PrB 12 The lattice constant is smaller than that of CeB 12 This suggests that the radius of the Ce ion in is small (which may be due to the valence being larger than 3).

[0048] Thus, in the examples of the present invention, by increasing the valence of Ce to more than 3, CeB 12 It was also shown that the CeB 12 Unlike CeB6, it was found that the valence of Ce is greater than 3. That is, CeB6 has a valence between 3 and 4. 12We have succeeded in newly producing and identifying its structure. It is a CeB with a cubic crystal structure and a lattice constant a of 7.58 Å or less, 7.57 Å or less, 7.56 Å or less, or 7.55 Å or less. 12 This means that they have succeeded in newly producing the compound and identifying its structure.

[0049] Furthermore, in order to easily realize a structure in which a strong cage structure is formed by the B element and a rare earth element is located at the center of the cage, a method for producing a rare earth boride at a relatively low pressure can be provided in which the rare earth element is at least partially made to have a valence higher than trivalent, which is considered to be common to rare earth elements. Alternatively, a method for producing a rare earth boride at a relatively low pressure using a rare earth element that is likely to have a valence higher than trivalent can be provided. [Industrial Applicability]

[0050] In an embodiment of the present invention, at least CeB 12 Cerium polyboride compounds containing cerium ions can be used as magnetic and electronic materials in the same way as other rare earth polyborides. In addition, due to the different valence states, unique properties are expected, and they may also be used as switching materials. 12 Cerium polyboride compounds containing crystals can be used as light absorbers in glass. Furthermore, their thermoelectric properties suggest potential applications as thermoelectric materials and semiconductors. Furthermore, the addition of B elements creates a rigid cage structure, making them suitable for use in hard materials.

Claims

1. The general formula is CeB n A compound that can be represented by CeB 12 1. A cerium boride compound comprising a CeB 12 crystal, wherein n is 9<n<15, and the crystal structure of the CeB 12 crystal is a cubic crystal structure belonging to the Fm-3m space group and has a space group number of 225.

2. The CeB 12 2. The cerium boride compound according to claim 1, characterized in that the valence of Ce in the crystal exceeds 3.

3. The CeB 12 3. The cerium boride compound according to claim 2, characterized in that in the crystal, the lattice constant a=7.54±0.4 Å.

4. A magnetic material comprising the compound according to any one of claims 1 to 3.

5. A thermoelectric material comprising a compound according to any one of claims 1 to 3.

6. A superconducting material comprising a compound that can be represented by the general formula CeB n , including a CeB 12 crystal, and wherein 9<n<15.

7. One or more CeB m A raw material containing a compound (0<m≦6) and boron mixed in a predetermined ratio is heated by laser to a temperature of 2000K to 3300K under ultra-high pressure of 10GPa to 100GPa. The general formula is CeB n (9<n<15), and CeB 12 A method for producing a compound comprising a crystal.

8. The manufacturing method described in Claim 7, characterized in that the ultra-high pressure may be a pressure of 15 GPa or more.

9. 9. The method according to claim 7, wherein laser heating is performed using a diamond anvil cell.

Citation Information

Patent Citations

  • Electrical contact material

    JP2002294384A

  • X-RAY INSPECTION DEVICE USING CATHODE CONTAINING BORIDE OF Ce (CERIUM) OR Gd (GADOLINIUM)

    JP2005207945A

  • N-type thermoelectric conversion element utilizing carbon- and nitrogen-doped rare-earth polyboride-based high-temperature acid-resistant n-type thermoelectric material

    JP2012044201A

  • Light absorption material

    JP2014084385A

  • Mixed metal dodecaborides and uses thereof

    US20190071318A1