Processed wood disk material and manufacturing method thereof

JP7569040B2Active Publication Date: 2024-10-17FUKUOKA PREFECTURAL GOVERNMENT
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022086173
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-05-26
Publication Date
2024-10-17
Estimated Expiration
2042-05-26

Smart Images

  • Figure 0007569040000002
    Figure 0007569040000002
  • Figure 0007569040000003
    Figure 0007569040000003
  • Figure 0007569040000004
    Figure 0007569040000004
Patent Text Reader

Abstract

To provide a processed ligneous disk material in which shrinkage is suppressed and eluviation of agent is suppressed, and a production method thereof.SOLUTION: A production method of a processed ligneous disk material having a sapwood part and a heart wood part comprises: an impregnation process of impregnating the ligneous disk material with solution including saccharide by contacting the ligneous disk material with the solution including the saccharide; and a dry process of drying the ligneous disk material impregnated with the solution including the saccharide at a temperature equal to or lower than 100°C to make its equilibrium moisture content 5 to 15%, its average shrinkage ratio in a tangential direction on a surface layer of the sapwood part 0.15 or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a processed wood disk and a method for producing the processed wood disk. [Background technology]

[0002] Wood discs, cut from logs, can be used for interior decoration, furniture, building materials, etc. by taking advantage of the warmth and soft texture of wood and the annual ring patterns on the cut ends. However, wood discs are prone to cracking due to shrinkage caused by drying, so they are treated with chemicals to prevent shrinkage.

[0003] For example, as disclosed in Patent Document 1, the present inventors have developed a method for manufacturing processed disc material, which includes a chemical impregnation step in which a disc material having a moisture content of 30% or more is impregnated with an aqueous polyethylene glycol solution, and a drying step in which the polyethylene glycol-impregnated disc material is dried at 70 to 100°C after the chemical impregnation step, and in which the disc material is dried in the drying step so that the moisture content is 5 to 10% and the average tangential shrinkage rate in the sapwood is 0.10% or less. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2004-268292 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, it has been found that, depending on conditions such as the high temperature and humidity of the rainy season, the processed wood discs produced by the method of Patent Document 1 may have a chemical agent (polyethylene glycol) seep out onto the surface of the processed wood discs, causing stickiness and dripping on the surface of the processed wood discs. This phenomenon in which stickiness and dripping occur on the surface of wood materials due to the seepage of the chemical agent is called leaching. Therefore, there has been a demand for a technology that can suppress the shrinkage of processed wood discs and prevent the chemical agent from leaching out.

[0006] Under such circumstances, an object of the present invention is to provide a processed wood disk material in which shrinkage and leaching of chemicals are suppressed, and a manufacturing method thereof. [Means for solving the problem]

[0007] As a result of intensive research aimed at solving the above problems, the present inventors have found that the following invention meets the above object, and have completed the present invention.

[0008] [1] A method for producing a processed wood disc having a sapwood portion and a heartwood portion, comprising: an impregnation step of contacting a wood disc with an aqueous solution containing a sugar and impregnating the wood disc with the aqueous solution containing the sugar; and a drying step of drying the sugar-impregnated wood disc impregnated with the aqueous solution containing the sugar at 100°C or less to bring the equilibrium moisture content to 5 to 15% and the average tangential shrinkage rate at the surface of the sapwood portion to 0.15% or less. [2] A method for producing the processed wood disc described in [1] above, further comprising a coating process for coating the surface of the sugar-impregnated wood disc after the drying process. [3] The method for producing processed wood disc material described in [1] or [2] above, wherein the aqueous solution containing sugar is an aqueous solution consisting of sugar and water. [4] A method for producing processed wood disc material described in any one of [1] to [3] above, wherein the sugar is sucrose and / or erythritol. [5] The amount of sugar impregnated in the sugar-impregnated wood disc is 70 kg / m 3The above is a method for producing a processed wood disc material described in any one of [1] to [4] above. [6] A method for producing a processed wood disc as described in any one of [1] to [5] above, wherein the leaching rate of the processed wood disc is 5 mass% or less. [7] A method for manufacturing a processed wood disc as described in any one of [1] to [6] above, wherein the wood disc has a thickness of 10 cm or less and a diameter of 30 cm or more.

[0009] [8] A processed wood disc having a sapwood portion and a heartwood portion and impregnated with sugars, the processed wood disc having an equilibrium moisture content of 5 to 15% and an average tangential shrinkage rate at the surface layer of the sapwood portion of 0.15% or less. [9] The processed wood disc material described in [8] above, having a coating film on at least a portion of its surface. Effect of the Invention

[0010] According to the present invention, there is provided a processed wood disk in which shrinkage and leaching of chemicals are suppressed, and a method for producing the same. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a schematic diagram of a wood disk used in the manufacturing method of the present invention. [Diagram 2] FIG. 1 is a plot of the amount of sucrose impregnation and the average shrinkage rate in the surface layer of the sapwood. [Diagram 3] This is a plot of the amount of sucrose impregnation and the average shrinkage rate at the surface layer of the heartwood. [Figure 4] 1 is a photograph showing the appearance of the processed wood disc of Comparative Example 2 after being left to stand for one week in an environment of 40° C. and 90% RH. [Diagram 5] 1 is a graph showing the average shrinkage rate in the tangential direction of the test piece of Reference Example 1. [Figure 6] 1 is a graph showing the leaching rate of the test piece of Reference Example 2. [Figure 7] 1 is a graph showing the leaching rate of the test piece of Reference Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The following is a detailed description of the embodiments of the present invention, but the following description of the constituent elements is one example (representative example) of the embodiment of the present invention, and the present invention is not limited to the following content as long as the gist of the present invention is not changed. Note that in this specification, when the expression "~" is used, it is used as an expression including the numerical value or physical property value before and after it.

[0013] [Manufacturing method for processed wood discs] The present invention relates to a method for producing a processed wood disc having a sapwood portion and a heartwood portion, which includes an impregnation step of contacting a wood disc with an aqueous solution containing sugars to impregnate the wood disc with the aqueous solution containing sugars, and a drying step of drying the sugar-impregnated wood disc impregnated with the aqueous solution containing sugars at 100°C or less to have an equilibrium moisture content of 5 to 15% and an average tangential shrinkage rate in the surface layer of the sapwood portion of 0.15% or less (hereinafter, sometimes referred to as the "production method of the present invention").

[0014] The inventors have found that by using sugars, it is possible to suppress shrinkage while significantly suppressing the leaching of chemicals. In particular, they have found that it is possible to produce processed wood disks in which chemicals are less likely to leach out even under conditions that tend to cause chemicals to leach out, such as high temperature and humidity. The obtained processed wood disks can be used in applications that make use of the annual ring pattern on the cut surface.

[0015] [Impregnation process] The chemical impregnation step is a step of contacting an aqueous solution containing sugars with the wood disk, thereby impregnating the wood disk with the aqueous solution containing sugars.

[0016] (Wood Disc Material) In the present invention, "wood disc material" refers to a material cut into round slices of a log, as shown in Figure 1, and has heartwood and sapwood. "Heartwood" refers to the darker part near the center of the tree, and "sapwood" refers to the lighter part near the surface of the tree. "Surface layer" refers to the part up to 5 mm in thickness from the butt end.

[0017] Generally, wood disks are prone to large V-shaped cracks (V-cracks) from the periphery to the center due to shrinkage during drying. In particular, large V-shaped cracks are likely to occur in large, thick wood disks, and wood disks with such cracks are not suitable for use as materials for interior decoration, furniture, building materials, etc. The manufacturing method of the present invention can suppress the shrinkage of the wood disks while suppressing the leaching of the chemicals, making it easy to manufacture processed wood disks without V-cracks. Therefore, the manufacturing method of the present invention can be suitably used for wood disks with a thickness of 10 cm or less and a diameter of 30 cm or more (i.e., large-diameter wood disks). More suitable targets are wood disks with a thickness of 8 cm or less and a diameter of 50 cm or more. Depending on the application, the lower limit of the thickness of the wood disks may be 1 cm or more or 5 cm or more. In addition, the upper limit of the diameter of the wood disks may be 150 cm or less or 100 cm or less. In the present invention, the "diameter" refers to the diameter of the butt end of a wood disc, as shown in FIG. 1, and when the butt end is not circular, the diameter is the equivalent diameter of a circle.

[0018] The type of tree for the disk material is not particularly limited, and coniferous trees such as cedar and cypress, broad-leaved trees, etc. can be used. One of the preferred trees is cedar.

[0019] The wood discs used may be in a green or semi-dried state. Wood discs with a moisture content of 28% or more that are less likely to crack before the impregnation process may be used, or wood discs with a moisture content of 28% or less that are more easily impregnated with the sugar-containing aqueous solution may be used.

[0020] The moisture content can be calculated by the total drying method in accordance with JIS Z 2101: 2009. Specifically, the moisture content of the wood disc material used can be calculated by taking a strip in the diameter direction from an untreated disc cut from the same log, evaporating the moisture in a 105°C oven, and calculating the moisture content from the weight difference before and after.

[0021] (Sugar-containing aqueous solution) In the manufacturing method of the present invention, an aqueous solution containing sugars is used as a chemical solution to be impregnated into the wood disk. By using an aqueous solution containing sugars, the filling effect of the sugars can suppress the shrinkage of the wood disk and improve leaching. Since sugars are also used for food, they are also preferable from the viewpoint of the safety of the processed wood disk.

[0022] The saccharides are sugars and / or sugar alcohols. One type of saccharide may be used alone, or two or more types may be used in combination. Examples of the sugars include monosaccharides such as glucose, fructose, galactose, and mannose; disaccharides such as sucrose, lactose, maltose, and trehalose; oligosaccharides such as fructooligosaccharides, galactooligosaccharides, mannanoligosaccharides, and stachyose; and polysaccharides such as starch, cellulose, amylose, and chitin. Examples of the sugar alcohols include lactitol, sorbitol, mannitol, maltitol, and erythritol. Among these, the saccharides are preferably disaccharides and / or sugar alcohols.

[0023] Among them, sucrose or erythritol is preferred, and sucrose is particularly preferred. For example, trehalose can provide shrinkage suppression effects and leaching suppression effects, but it is more difficult to impregnate wood disks with trehalose than sucrose, and a complex impregnation method is required to impregnate a sufficient amount of trehalose into wood disks, and cracks tend to occur over time. On the other hand, sucrose can be easily impregnated into wood disks without strictly controlling the impregnation conditions. In addition, sucrose can provide a large shrinkage suppression effect and stable dimensional stability over time by drying to an equilibrium moisture content of 5 to 15% even without strictly controlling the drying conditions, and processed wood disks in which V-shaped cracks are unlikely to occur and leaching of the agent is suppressed can be produced.

[0024] The concentration of the sugar in the aqueous solution containing the sugar (mass of sugar / mass of the aqueous solution containing the sugar×100(%)) can be appropriately determined depending on the type and size of the wood disk, the type of sugar, the intended use, and the like. On the other hand, if the concentration of the sugar is too high, the viscosity of the aqueous solution increases, and it may be difficult to impregnate the wood disk with the desired amount of sugar, or it may take a long time to impregnate the wood disk with the sugar. Also, if the concentration of the sugar is too low, it may be difficult to impregnate the wood disk with the desired amount of sugar. Therefore, the concentration of the sugar in the aqueous solution containing the sugar is preferably 70% by mass or less, more preferably 60% by mass or less. The lower limit is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 30% by mass or more. For example, the concentration of the sugar in the aqueous solution containing the sugar is preferably 10 to 70% by mass, more preferably 15 to 60% by mass.

[0025] Furthermore, the proportion of the total mass of sugars and water in an aqueous solution containing sugars (total mass of sugars and water / mass of aqueous solution×100(%)) is preferably 97% by mass or more, 98% by mass or more, and 99% by mass or more in that order, and it is more preferable for the aqueous solution to consist of sugars and water. Note that an aqueous solution consisting of sugars and water need only consist essentially of sugars and water, and does not necessarily exclude the inclusion of unavoidable impurities.

[0026] For example, the aqueous solution containing sugars may be an aqueous solution having a sugar concentration of 10% by mass or more and a total mass ratio of sugars and water to the aqueous solution containing sugars of 97% by mass or more, or an aqueous solution having a sugar concentration of 15 to 60% by mass and a total mass ratio of sugars and water to the aqueous solution containing sugars of 98% by mass or more.

[0027] The impregnation method with the aqueous solution containing the saccharide may be a conventionally known method, and may be performed under reduced pressure, pressure, or atmospheric pressure. For example, a dipping method, a hot / cold bath method, a reduced pressure injection method, a reduced pressure and pressure injection method, etc. may be used. These impregnation methods may also be combined.

[0028] If the amount of sugar impregnation is too small, the sugar may not penetrate sufficiently to the center of the wood disc, making it difficult to obtain the effect of suppressing shrinkage. Therefore, the amount of sugar impregnation is set at 70 kg / m 3 It is preferable that the saturation temperature is 100 kg / m or more. 3 More than 150kg / m 3 On the other hand, if the amount of impregnation of the sugar exceeds a certain level, there is a risk that leaching may occur, so the amount of impregnation of the sugar may be set to 500 kg / m or more. 3 Less than 400kg / m 3 Below 300kg / m 3 Below 250kg / m 3 It may be set as follows:

[0029] The "amount of sugar impregnated" is calculated by multiplying the weight difference (kg) of the wood disc before and after impregnation with the sugar solution by the concentration of the sugar in the sugar solution, as shown below, and calculating the volume (m 3 ) can be found by dividing it by

[0030] Sugar impregnation amount (kg / m 3 ) = [(mass (kg) of the wood disc after impregnation with the sugar solution) - (mass (kg) of the wood disc before impregnation with the sugar solution)] × sugar concentration in the sugar solution (%) ÷ volume of the wood disc (m 3 )÷100

[0031] The soaking time can be appropriately determined depending on the type and size of the wood disk, the concentration of the sugar in the aqueous solution, etc. In order to allow the sugar to penetrate deeper into the center of the wood disk, the soaking time is preferably 1 day or more, more preferably 2 days or more, and more preferably 5 days or more. There is no particular upper limit, but it is preferably 20 days or less, and more preferably 15 days or less.

[0032] [Drying process] The drying process is a process in which the sugar-impregnated wood disc, which has been impregnated with an aqueous solution containing sugars, is dried at 100°C or less until the equilibrium moisture content reaches 5 to 15% and the average tangential shrinkage rate in the surface layer of the sapwood is 0.15% or less.

[0033] The drying temperature is adjusted as appropriate depending on the size of the wood disc, but if the drying temperature is too high, the wood disc is prone to browning, so the upper limit is 100° C. or less, and may be 95° C. or less or 90° C. or less. The lower limit may be 50° C. or more, 60° C. or more, 70° C. or more, 80° C. or more, etc. The drying temperature may be constant or may be changed according to the progress of drying of the saccharide-impregnated wood disc.

[0034] The drying time is adjusted appropriately depending on the size of the wood disk, the drying temperature, etc., and may be such that the equilibrium moisture content is 5 to 15%. The saccharide-impregnated wood disk may be dried until it reaches a constant weight with an equilibrium moisture content of 5 to 15%, and the drying time is not particularly limited, but may be, for example, 1 day or more, 2 days or more, or 10 days or less, 7 days or less, or 5 days or less.

[0035] Drying can be performed at a constant or variable relative humidity. For example, when the relative humidity is varied in accordance with the decrease in moisture content of the sugar-impregnated wood disk due to drying, the relative humidity can be varied to 90% or less, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, etc., in accordance with the decrease in moisture content of the sugar-impregnated wood disk.

[0036] The equilibrium moisture content of the processed wood disc after drying is 5 to 15%. This makes the processed wood disc less likely to dry out and less likely to crack. As mentioned above, the "equilibrium moisture content" can be measured by a method conforming to JIS Z 2101:2009.

[0037] The average tangential shrinkage rate of the surface layer of the sapwood of the processed wood disc is 0.15% or less. This can suppress cracks. Since there is a risk that cracks may occur more easily over time, it is particularly preferable that the average tangential shrinkage rate of the surface layer of the sapwood of the processed wood disc is 0.10% or less. By setting the average tangential shrinkage rate of the surface layer of the sapwood to 0.10% or less, the occurrence of large cracks such as V-shaped cracks can be more stably suppressed. The "average tangential shrinkage rate" can be measured according to JIS Z 2101:2009. Details will be described later in the examples.

[0038] In order to further suppress shrinkage, it is preferable that the average tangential shrinkage rate of the processed wood disc be 0.15% or less from the surface layer to the central layer of the sapwood (the central layer in the thickness direction of the sapwood), and it is even more preferable that it be 0.10% or less.

[0039] The average tangential shrinkage of the surface layer of the core can be, for example, 0.20% or less or 0.18% or less. The average tangential shrinkage of the processed wood disc from the surface layer to the center layer of the core can be, for example, 0.25% or less or 0.22% or less.

[0040] After the impregnation step, the saccharide-impregnated wood disk may be subjected to a curing treatment and then a drying step.

[0041] The saccharide-impregnated wood disks after the drying process can be used as they are for interior and building materials. In the manufacturing method of the present invention, the saccharide-impregnated wood disks after the drying process may be subjected to a finishing process such as painting.

[0042] [Painting process] The manufacturing method of the present invention may include a coating step of coating the surface of the wood disk after the drying step. By carrying out the coating step, a processed wood disk having a coating film formed on the surface can be obtained. The processed wood disk subjected to such a coating treatment can further suppress leaching, and the coating film can also have a function such as decay prevention. The thickness of the coating film formed is preferably 50 to 200 μm, more preferably 100 to 150 μm. If the coating film is too thin, the effect of improving leaching prevention is small, and if the coating film is too thick, the texture of the wood is impaired, so it is preferable that the coating film thickness is within the above range.

[0043] The coating material is not particularly limited, and known film-forming coating materials can be used. For example, urethane resin coating materials, amino alkyd resin coating materials, unsaturated polyester resin coating materials, UV coating materials (UV-curable polyester resins and UV-curable acrylic resins), glass coating materials, fluororesin coating materials, and other materials can be used. In addition, conventionally known coating methods can be used, and multiple coatings such as undercoating, intermediate coating, and top coating can be used.

[0044] [Processed wood disc material] The present invention also relates to a processed wood disc having a sapwood portion and a heartwood portion, impregnated with sugars, having an equilibrium moisture content of 5 to 15%, and an average tangential shrinkage rate in the surface layer of the sapwood portion of 0.15% or less (hereinafter, this may be referred to as the "processed wood disc of the present invention").

[0045] Such processed wood discs are less likely to crack during processing or use, have excellent dimensional stability, and are also inhibited from leaching. In particular, even under conditions of high temperature and humidity where leaching is likely to occur, the surface of the processed wood discs can be inhibited from becoming sticky or dripping due to the seepage of sugars. The processed wood discs of the present invention can be homogeneous processed wood discs without large cracks such as V-shaped cracks on the butt end surface, and can be suitably manufactured by the manufacturing method of the present invention described above. Such processed wood discs are suitable for use as materials for interior decoration, furniture, building materials, etc.

[0046] The preferred size of the processed wood disc is a wood disc with a thickness of 10 cm or less and a diameter of 30 cm or more (i.e., a large diameter wood disc), and more preferably a thickness of 8 cm or less and a diameter of 50 cm or more. The lower limit of the thickness of the processed wood disc may be 1 cm or more or 5 cm or more. The upper limit of the diameter of the processed wood disc may be 150 cm or less or 100 cm or less.

[0047] The processed wood disc of the present invention has an equilibrium moisture content of 5 to 15%. The processed wood disc of the present invention can be suitably manufactured by the manufacturing method of the present invention described above. The equilibrium moisture content of the processed wood disc changes depending on the number of days that have passed since manufacture and the humidity in the air, so the equilibrium moisture content in the air can be 5% or more or 10% or more. Although it depends on the number of days that have passed since manufacture, the equilibrium moisture content in the air is usually 15% or less (about 12 to 15%).

[0048] The amount of sugar impregnated in the processed wood disc of the present invention is 70 kg / m 3 It is preferable that the density is 100 kg / m or more. 3 More than 150kg / m 3 The upper limit is not particularly limited, but may be, for example, 500 kg / m 3 Less than 400kg / m 3 Below 300kg / m 3 Below 250kg / m 3 It can be something like the following:

[0049] In order to further improve the dimensional stability, it is particularly preferable that the processed wood disc of the present invention has an average shrinkage rate in the tangential direction in the surface layer of the sapwood of 0.10% or less.

[0050] The average tangential shrinkage from the surface layer to the central layer of the sapwood (the layer at the center in the thickness direction of the sapwood) can be 0.15% or less or 0.10% or less. The average tangential shrinkage in the surface layer of the heartwood can be 0.20% or less or 0.18% or less, and the average tangential shrinkage from the surface layer to the central layer of the heartwood can be 0.25% or less or 0.22% or less.

[0051] The processed wood disc of the present invention can have a leaching rate of 5% by mass or less, and can also have a leaching rate of 3% by mass or less, or 1% by mass or less. Because of this leaching rate, even when used in a hot and humid environment, the surface of the processed wood disc is less likely to become sticky or drip. The leaching rate can be calculated by the method described in the examples.

[0052] For example, the processed wood disk of the present invention has a leaching amount of 0.1 kg / m in a leaching test. 3 Less than 0.05kg / m 3 Below, 0.01kg / m 3 It can be very low, such as:

[0053] The processed wood disk of the present invention preferably has a coating film on at least a part of its surface. That is, the processed wood disk of the present invention preferably has a coating applied to at least a part of its surface. By having a coating film, the processed wood disk can be made to have further improved leaching.

[0054] The processed wood disk of the present invention can be used as it is for interior items such as tables and furniture, etc. Also, the processed wood disk of the present invention can be further processed to produce the desired products (tables, chairs, furniture, etc.). EXAMPLES

[0055] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples unless the gist of the present invention is changed.

[0056] [Example 1] 1) Specimen Cedar disc material: φ500mm x thickness 10mm, 20mm, 30mm, 40mm, 50mm The cedar discs were cut from three Kyushu cedar logs with an end diameter (φ) of approximately 500 mm, designated log (1), log (2), and log (3), and 12 discs each of 10 mm and 40 mm thickness were cut from log (1), 20 mm and 30 mm thickness from log (2), and 50 mm thickness from log (3), for a total of 60 discs. The cut discs were cured in the laboratory for three days before use.

[0057] 2) Aqueous solutions containing sugars (medicinal solutions) Sucrose was a food additive product manufactured by Ensuiko Sugar Refining Co., Ltd. The sucrose aqueous solution was adjusted to 50 wt% with pure water. The density of the aqueous solution was 1.228 g / cm 3 It was.

[0058] 3) Impregnation (injection) method Of the 12 wood disks cut out of each thickness, the first, fifth and ninth disks from the distal end were subjected to sucrose impregnation treatment (immersion method). The aqueous sucrose solution was placed in a container, and then the wood disk was placed in the container. The wood disk was immersed in the aqueous sucrose solution at room temperature for 12 days.

[0059] 4) Drying The wood disc was then removed from the container and cured for 7 days, after which it was left to dry in a thermo-hygrostat at 60°C and 70% RH (equilibrium moisture content of 10%) until it reached a constant weight, yielding the processed wood disc of Example 1 (impregnated wood disc).

[0060] The amount of sugar (sucrose) impregnated into the processed wood disks of each thickness was calculated from the weight difference before and after impregnation (injection) and the concentration of the sucrose solution. The results are shown in Table 1.

[0061] [Table 1]

[0062] [Comparative Example 1] Of the 12 wood disks cut out of each thickness, the 4th, 8th, and 12th disks from the end were impregnated with pure water and used as controls. Except for using pure water instead of the sucrose solution, the soaking and drying were carried out in the same manner as in Example 1 to obtain a processed wood disk of Comparative Example 1.

[0063] [Measurement of shrinkage rate] Of the processed wooden disks of Example 1 (impregnated wooden disks after drying), one piece of each thickness was divided, and the average shrinkage rate was measured by a method in accordance with JIS Z 2101:2009.

[0064] For the 20mm to 50mm thick pieces, 4 pieces were cut from the heartwood and 2 pieces from the sapwood to a tangential direction of 50mm and a radial direction of 40mm, and further divided into 5mm thick pieces from the butt end (surface layer) to the center layer, and these were used as test pieces for evaluation. Since it was difficult to divide the 10mm thick pieces in the thickness direction, they were not divided in the thickness direction, but were cut from the heartwood and 2 pieces from the sapwood to a tangential direction of 50mm and a radial direction of 40mm, and these were used as test pieces for evaluation.

[0065] Similarly, for the processed wooden disks of Comparative Example 1, one piece of each thickness was divided and the average shrinkage rate was measured by a method in accordance with JIS Z 2101:2009.

[0066] In the processed wood disc material (thickness 10mm to 50mm) of Example 1, the average tangential shrinkage rate at the surface layer of the sapwood was 0.04 to 0.10%, the average tangential shrinkage rate from the surface layer to the central layer of the sapwood was 0.04 to 0.10%, the average tangential shrinkage rate at the surface layer of the heartwood was 0.11 to 0.16% or less, and the average tangential shrinkage rate from the surface layer to the central layer of the heartwood was 0.11 to 0.21%.

[0067] In the processed wood disc material (thickness 10mm to 50mm) of Comparative Example 1, the average tangential shrinkage rate at the surface layer of the sapwood was 0.21 to 0.27%, the average tangential shrinkage rate from the surface layer to the central layer of the sapwood was 0.21 to 0.27%, the average tangential shrinkage rate at the surface layer of the heartwood was 0.21 to 0.27%, and the average tangential shrinkage rate from the surface layer to the central layer of the sapwood was 0.21 to 0.27%.

[0068] Figure 2 shows the results of plotting the amount of sucrose impregnation and the average shrinkage rate in the surface layer of the sapwood. The average shrinkage rate for each amount of sucrose impregnation was the average value of the average shrinkage rates measured using two test pieces cut out as described above from the sapwood of the processed wood disc of each thickness corresponding to each amount of sucrose impregnation. In Comparative Example 1, the average value of the average shrinkage rates of all test pieces cut out from the sapwood of the processed wood disc of each thickness was plotted with the amount of sucrose impregnation set to 0, and the range between the maximum and minimum values ​​was displayed with error bars.

[0069] Figure 3 shows the results of plotting the amount of sucrose impregnation and the average shrinkage rate at the surface layer of the heartwood. The average shrinkage rate for each amount of sucrose impregnation was the average value of the average shrinkage rates measured using four test pieces cut out as described above from the heartwood of the processed wood disc of each thickness corresponding to each amount of sucrose impregnation. In Comparative Example 1, the average value of the average shrinkage rates of all test pieces cut out from the heartwood of the processed wood disc of each thickness was plotted with the amount of sucrose impregnation set to 0, and the range between the maximum and minimum values ​​was displayed with error bars.

[0070] [Leaching test (I)] The processed wood disk (10 mm to 50 mm thick) of Example 1 was left standing for one week at 40°C and 90% RH. The settings were then changed to 40°C and 40% RH and the disk was left standing for one week. Visual inspection revealed no leaching of the agent or stickiness on the surface of the processed wood disk.

[0071] [Leaching test (II)] A 50 mm thick processed wood disk from Example 1 was dried at 80°C until it reached a constant weight. After drying, it was placed in a thermohygrostat and tilted 60° to the horizontal plane and placed on a tray. After conditioning at 40°C and 90% RH for 24 hours, it was dried at 60°C with air for 24 hours, and this operation was repeated 5 times, and the tray and the surface of the material were observed to evaluate the leaching property. It was then dried at 80°C until it reached a constant weight, and the weight change of the processed wood disk before and after the test was confirmed.

[0072] As a result of the leaching test, no crystallized solvent was observed on the surface of the processed wood disc of Example 1. Also, no leaching of the chemical solution into the tray was confirmed. Furthermore, the weight change (amount of leaching) of the processed wood disc of Example 1 before and after the leaching test was extremely small, at 0.01 kg (before leaching test: 5.605 kg, after leaching test: 5.595 kg). The leaching rate (weight change of the processed wood disc before and after the test (kg) / amount of sugar impregnated (kg / m 3 ) × 100(%) was 0.01%.

[0073] [Evaluation of cracking of processed wood discs] A total of 10 sheets, one each for each thickness of Example 1 and Comparative Example 1, were placed in a thermo-hygrostat. The temperature and relative humidity were set to 40°C and 90% RH, and the sheets were left standing for one week, after which the settings were changed to 40°C and 40% RH, and the sheets were left standing for one week, and the state of cracking was observed.

[0074] As a result of the crack evaluation, no peripheral cracks occurred in all five processed wood disks (thickness 10 mm to 50 mm) of Example 1. On the other hand, in the pure water treatment of Comparative Example 1, cracks occurred before the crack evaluation test started, except for the 20 mm thick wood disk, and the cracks expanded. In addition, a peripheral crack measuring 15 mm wide occurred in the pure water treated 20 mm thick processed wood disk that had no cracks before the crack evaluation test.

[0075] [Comparative Example 2] A processed wood disk of Comparative Example 2 was obtained in the same manner as in Example 1, except that an aqueous polyethylene glycol solution was used as the chemical solution to be impregnated into a cedar disk (approximately φ500 mm × thickness 50 mm). The polyethylene glycol aqueous solution was prepared by adjusting polyethylene glycol having an average molecular weight of 1000 (hereinafter referred to as "PEG1000") to 50 wt % with pure water.

[0076] Fig. 4 is a photograph showing the processed wood disk of Comparative Example 2 after being left for one week in an environment of 40°C and 90% RH. When the processed wood disk of Comparative Example 2 was left for one week in an environment of 40°C and 90% RH, leaching of polyethylene glycol was confirmed and the surface was also sticky, as shown in Fig. 4.

[0077] [Reference Example 1]: Dimensional stabilization effect of other sugar alcohols 1) Test piece Cedar sapwood: 40mm (T: tangential direction) x 20mm (L: fiber direction) x 15mm (R: radial direction)

[0078] 2) Aqueous solutions containing sugars (medicinal solutions) As the aqueous solution containing a sugar, a 50 wt % sucrose aqueous solution or a 30 wt % erythritol aqueous solution was used.

[0079] 3) Impregnation (injection) method The test piece was impregnated with the sucrose aqueous solution using vacuum impregnation. First, the test piece was placed in the sucrose aqueous solution and immersed for 1 hour at 40°C and 20 mmHg, and then immersed for 1 hour at 40°C and normal pressure. This immersion for 1 hour at 40°C and 20 mmHg and immersion for 1 hour at 40°C and normal pressure were repeated until the mass of the test piece did not change. The same procedure was carried out for the erythritol aqueous solution, and the test piece was impregnated with the erythritol aqueous solution.

[0080] 4) Drying It was dried at 60°C and 70% RH to an equilibrium moisture content of 10%.

[0081] [Measurement of shrinkage rate] The average shrinkage rate of each test piece was measured by a method in accordance with JIS Z 2101:2009. The results are shown in Figure 5. As shown in Figure 5, not only for sucrose, a sugar, but also for erythritol, a sugar alcohol, the average shrinkage rate in the tangential direction was 0.10% or less, confirming the effect of improving dimensional stability.

[0082] [Reference Example 2]: Effect of preventing leaching 1) Test piece Cedar core: 100mm(T)×20mm(L)×100mm(R)

[0083] 2) Chemical solution 50wt% sucrose aqueous solution 45wt% lactitol aqueous solution 40wt% trehalose aqueous solution 30wt% erythritol aqueous solution 50wt%PEG1000 aqueous solution

[0084] 3) Impregnation (injection) method The test specimen was impregnated with the sucrose aqueous solution using vacuum pressure impregnation. First, the test specimen was placed in the sucrose aqueous solution and immersed at room temperature and -99.5 kPa for 1 hour, and then at room temperature and 0.7 MPa for 1 hour. The same procedure was carried out for the other chemical solutions to prepare test pieces impregnated with each of the chemical solutions.

[0085] 4) Drying After curing at room temperature for 2 days, the pieces were dried at 80°C for 1 week until the equilibrium moisture content reached 10%.

[0086] [Leaching test] The test piece was placed at a 60° angle and treated under five cycles of 40°C, 90% RH, 24 hours and 60°C, 24 hours each, and then dried at 105°C until it reached a constant weight. The difference in mass between the test piece before and after the leaching test was calculated to calculate the chemical leaching rate. The results are shown in Figure 6.

[0087] As shown in Figure 6, the leaching rate of the samples treated with the aqueous solution containing sugars was less than one-tenth that of the samples treated with the aqueous solution of PEG1000, and leaching of the drug was improved.

[0088] [Reference Example 3]: Effect of coating to prevent leaching As the drug solution, a 50 wt % aqueous solution of PEG1000 or a 50 wt % aqueous solution of sucrose was used, and the drug solution was impregnated in the same manner as in Reference Example 2, 3). After the drug injection, the mixture was dried at 60°C and adjusted to an air-dried state. The test piece was adjusted to an air-dried state, and a urethane undercoat of 60-70g / m was applied. 2 , undercoat 60~70g / m 2 , topcoat 60~70g / m 2 was carried out.

[0089] In the same manner as in Reference Example 3, a leaching test was conducted on the wood disk material with a urethane coating, and the leaching rate was calculated. The results are shown in Figure 7. As shown in Figure 7, leaching could be further prevented by applying a urethane coating. [Industrial Applicability]

[0090] The processed wood disk of the present invention is industrially useful since it can be used for products such as interior decoration, furniture, and building materials.

Claims

1. A method for producing a processed wood disc having a sapwood portion and a heartwood portion, comprising: an impregnation step of contacting a wood disk with an aqueous solution containing sugars and impregnating the wood disk with the aqueous solution containing sugars; and drying the saccharide-impregnated wood disk impregnated with the saccharide-containing aqueous solution at 100° C. or less to obtain an equilibrium moisture content of 5 to 15% and an average tangential shrinkage rate of the surface layer of the sapwood of 0.15% or less. the saccharide is erythritol and / or trehalose, The concentration of the sugar in the aqueous solution containing the sugar is 30% by mass or more and 70% by mass or less, A method for producing a processed wood disk, wherein the amount of the sugar impregnated in the sugar-impregnated wood disk is 70 kg / m 3 or more and 250 kg / m 3 or less.

2. The method for producing a processed wood disk according to claim 1, further comprising a coating step of coating the surface of the saccharide-impregnated wood disk after the drying step.

3. The method for producing a processed wood disc according to claim 1 or 2, wherein the aqueous solution containing the saccharide is an aqueous solution consisting of a saccharide and water.

4. The method for producing a processed wood disc according to claim 1 or 2, wherein the leaching rate of the processed wood disc is 5 mass% or less.

5. 3. The method for manufacturing a processed wood disk according to claim 1, wherein the wood disk has a thickness of 10 cm or less and a diameter of 30 cm or more.

6. A processed wood disc having a sapwood portion and a heartwood portion and impregnated with sugars, The equilibrium moisture content is 5-15%; The average shrinkage rate in the tangential direction in the surface layer of the sapwood is 0.15% or less; the saccharide is erythritol and / or trehalose, The processed wood disk has an impregnation amount of the sugar of 70 kg / m 3 or more and 250 kg / m 3 or less.

7. 7. The processed wood disk according to claim 6, having a coating film on at least a part of the surface.

Citation Information

Patent Citations

  • Improved wood

    JP1989080501A

  • Method for stabilizing dimension of wood

    JP1991253304A

  • Method for treating water exposure organic remains for storage

    JP1996057812A

  • Method for preventing cracking of end processed product of log material and end processed product of log material