Composition for manufacturing top antireflection film, top antireflection film, and fluorine-containing composition

A fluorine-containing polymer-based composition with controlled content distribution addresses the issues of decomposition and accumulation in existing anti-reflective coatings, achieving uniform film formation and reduced application amounts, enhancing photolithography quality and yield.

JP7569587B2Active Publication Date: 2024-10-18GANSU HUALONG SEMICON MATERIAL TECH CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023550682
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-01-07
Filing Date
2022-12-30
Publication Date
2024-10-18
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

Existing fluorine-containing compounds used in top anti-reflective coatings for photolithography suffer from decomposition and accumulation issues, leading to environmental and health concerns, and require large amounts for effective application, resulting in non-uniform film thickness and pattern defects.

Method used

A composition comprising a fluorine-containing polymer with specific structural formulae and controlled content distribution, along with a water-soluble resin, alkali, acid, and surfactant, is used to create a top anti-reflective coating with a low refractive index, ensuring stability and uniform film formation with minimal application.

Benefits of technology

The composition achieves a refractive index of 1.41-1.44, reducing light scattering and standing wave effects, while maintaining uniformity and reducing the amount of coating needed, thus improving photolithography process yield and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569587000003
    Figure 0007569587000003
  • Figure 0007569587000004
    Figure 0007569587000004
  • Figure 0007569587000005
    Figure 0007569587000005
Patent Text Reader

Abstract

The present invention relates to the field of advanced optical material technology, in particular to a composition for producing a top antireflective coating for photoresist, a top antireflective coating for photoresist, and a fluorine-containing composition. The composition for producing a top antireflective coating for photoresist includes a fluorine-containing composition, an alkali, an acid, and a surfactant. The fluorine-containing composition includes a fluorine-containing polymer. The fluorine-containing composition includes a fluorine-containing polymer having n=1, 2, 3, 4, and ≧5 fluorine-containing polyether groups, respectively. The content of the above fluorine-containing polymer is 0-10wt%, 30wt-68wt%, 32wt-60wt%, 0-15wt%, and 0-8wt%, respectively. The content of the fluorine-containing composition in the composition for producing a top antireflective coating for photoresist is 1wt-15wt%. The antireflective coating can avoid light scattering and standing wave effect, and at the same time, the pH of the composition and the photoresist are well matched, thereby improving the problems of the pores and uniformity of the film surface, and the large difference in thickness between the center point and the edge after coating, and improving the yield rate of the photolithography process.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of advanced optical material technology, and in particular to a composition for producing a top antireflective coating for photoresist, a top antireflective coating for photoresist, and a fluorine-containing composition. [Background technology]

[0002] Photolithography technology is a method of transferring a semiconductor circuit pattern on a photomask onto a silicon wafer. The photomask is irradiated with a laser or electron beam, which causes the photosensitive material on the wafer to be exposed to light and change its material properties, completing the pattern transfer process. Existing photolithography technology has a technical problem of light scattering, which results in low dimensional accuracy of photoresist imaging. At present, the mainstream solution is to add a top anti-reflective film of a fluorine-containing compound with a low refractive index and high transmittance before and after photoresist coating to reduce the interference of light in the photoresist and prevent the change in photolithography line width caused by the change in photoresist thickness.

[0003] The present inventors found that there are many kinds of fluorine-containing compounds currently used in anti-reflective coatings for photolithography, such as perfluorooctanoic acid, perfluorooctane sulfonic acid, and fluorine-containing polymers, all of which belong to fluorine-containing non-cyclic small molecule materials. Patent application CN1666154A mainly focuses on alkali-soluble fluorine-containing polymers-[CF 2 Patent application CN101568991A discloses an antireflective coating composition consisting of a specific naphthalene compound, a polymer (-[CF(ORfCOOH)]- (Rf represents a linear or branched perfluoroalkyl group that may contain ether oxygen atoms), an acid, an amine and a solvent. 2 Patent application JP10069091A discloses a composition for forming an anti-reflective coating comprising a perfluoroalkyl ether carboxylic acid (F-[CF(CF 3 )CF 2 -O] m -CF(CF3 Patent application TW200928594A discloses a composition for use in a top anti-reflective coating, comprising an aqueous solution of a homopolymer or copolymer of N-vinylpyrrolidone, Rf-O-[CF(CF 3 )CF 2 -O] m -CF(CF 3 The present invention discloses a composition for a top antireflective coating, which comprises a fluorine-containing compound represented by the formula (I)COOH (Rf is a partially or completely fluorine-substituted alkyl group, and m is an integer of 0 to 10), an amine compound, and a water-soluble polymer.

[0004] However, fluorine-containing compounds have problems with decomposition and accumulation in the human body. In the semiconductor industry, it is expected that the amount of coating of the film-forming composition will be reduced in order to minimize the impact on the environment. Due to the health and environmental problems caused by the low decomposition and accumulation of fluorine-containing compounds in the human body, it is necessary to reduce the amount of the composition of fluorine-containing compounds to be applied when forming a top antireflective coating. Chinese patent application CN101849209A discloses a fluorine-containing acyclic composition for forming a top antireflective coating, which comprises at least one fluorine-containing compound and a quaternary ammonium compound, and optionally a water-soluble polymer, an acid, a surfactant, and an aqueous solvent. When the composition for forming the top antireflective coating is applied in a relatively small amount, it can perform at the same level as the conventional composition for forming the top antireflective coating. Chinese patent application CN112034683B discloses a fluorine-containing acyclic composition for a top antireflective layer. This composition has a problem that a large amount is used to achieve the 40 to 45 nm thickness required for the top antireflective layer, and there is a large difference in thickness between the center and edge after coating, resulting in a T-shaped top.

[0005] The compositions for top antireflective coatings in the above-mentioned prior art can be used to form top antireflective coatings for photolithography, but they have some drawbacks in terms of processability, film formability, refractive index, coating amount, or raw material cost. Summary of the Invention

[0006] In view of the above technical problems existing in the prior art, the present invention provides a composition for preparing a top anti-reflective coating for photoresist, a top anti-reflective coating for photoresist, and a fluorine-containing composition. The pH value of the composition for preparing a top anti-reflective coating can match the pH value of the photoresist, and can produce a top anti-reflective coating with good stability and film-forming properties, which can be applied in a relatively small amount and has a relatively low refractive index, thereby reducing pattern defects that may occur in the photolithography process, improving the quality of the photolithography pattern, and improving the problem of the relatively large difference in thickness between the center point and the edge after application. At the same time, the addition of an appropriate amount of acid to the top anti-reflective layer system can reduce the H in the photoresist. + This can suppress the diffusion of the photoresist into the anti-reflection film, thereby avoiding the problem of the formation of a T-shaped top.

[0007] The object of the present invention is achieved by the following technical solutions: A composition for producing a top antireflective coating for a photoresist, comprising: A) A fluorine-containing composition comprising a fluorine-containing polymer having the following structural formula: CF 2 (CF 3 )CF 2 -[O-CF(CF 3 )CF 2 ] n -O-CF(CF 3 )COO-R In the formula, n is in the range of 1 to 8, and R is H, NH 4 or other similar structures, a fluorine-containing composition in which the content a of the fluorine-containing polymer where n is 1 is 0 to 10 wt%, the content b of the fluorine-containing polymer where n is 2 is 30 wt% to 68 wt%, the content c of the fluorine-containing polymer where n is 3 is 32 wt% to 60 wt%, the content d of the fluorine-containing polymer where n is 4 is 0 to 15 wt%, the content e of the fluorine-containing polymer where n is 5 is 0 to 8 wt%, and the content b + the content c ≧ 80 wt%, and the content a, the content d and the content e are simultaneously 0, or any of them are 0, or not simultaneously 0, relative to the total weight of the fluorine-containing composition; B) a water-soluble resin, C) an alkali, D) an acid, and E) a surfactant.

[0008] By weight, the composition for producing a top antireflective coating contains 1 wt % to 15 wt % of a fluorine-containing composition, preferably 1.5 wt % to 12 wt % of a fluorine-containing composition, and more preferably 1.5 wt % to 8 wt % of a fluorine-containing composition.

[0009] Detailed studies have revealed that: When the composition of the above composition according to the present application satisfies the above conditions, the composition solution has good stability and film-forming properties, and can be applied in a relatively small amount to form an anti-reflective film with the same performance as that of the anti-reflective film in the prior art; The refractive index of the anti-reflective film at 248 nm is 1.41 to 1.44, and the refractive index under irradiation with a laser having a wavelength of 248 nm can be effectively reduced, and the anti-reflective film can be used as a top anti-reflective film for photoresist.

[0010] Detailed studies show that: when the content a is greater than 10 wt%, the composition has poor film-forming properties, and the surface of the film is prone to pores; when the content e is greater than 8 wt%, the composition has poor film-forming properties, and the distribution of the formed film is non-uniform, and the surface of the film is prone to pores; when the content d is greater than 15 wt%, the composition has poor film-forming properties, and the distribution of the formed film is non-uniform, and the surface of the film is prone to pores.

[0011] Additionally, applicants have discovered that portions of the photoresist illuminated by a particular light source undergo a photochemical reaction to produce H + As a result, the pH of the photoresist exposed to light falls to between 1.5 and 2.5. If the pH value of the top antireflective layer is relatively high, H + The H diffuses into the boundary area between the top antireflective layer and the photoresist, and at the same time the pH of the area increases, and the H cannot be completely removed by the developer in the development process, thus forming a T-shaped top. By adding an appropriate amount of acid to the top antireflective layer system, the H in the photoresist can be removed. + The diffusion of H into the anti-reflective coating can be suppressed, thereby preventing the formation of a T-shaped top. When the content of large molecular weight compounds such as c (pentamer) is increased, the strength of the anti-reflective coating itself and its affinity with the photoresist layer are improved. On the other hand, when the content of c (pentamer) is greater than 30 wt%, H + The diffusion of H into the anti-reflective coating becomes intense, so an appropriate amount of acid is added to adjust the pH value and reduce the H in the photoresist. + It is necessary to suppress the diffusion of the anti-reflection coating.

[0012] When the content c (pentamer) is greater than 60 wt%, a uniform, non-porous film can be formed, but a relatively large coating weight is required. When the content b (tetramer) is less than 30 wt%, a uniform, non-porous film can be formed, but a relatively large coating weight is required. Also, when the composition does not contain a surfactant, a uniform, non-porous film can be formed, but a relatively large coating weight is required, and the solution is unstable and prone to precipitation. When the composition does not contain an acid, the pH value of the composition is too high, so that a T-top of the photoresist occurs during the photolithography process using the top antireflective film produced therefrom.

[0013] Furthermore, the number average molecular weight of the fluorine-containing polymer is between 600 and 1300, more preferably between 650 and 1100. The composition for producing a top antireflective coating for photoresist has a viscosity at 25° C. of 1.3 to 1.5 cp.

[0014] Furthermore, the content a is 0 to 9 wt%, preferably 0 to 8 wt%, and more preferably 2 to 8 wt%. The content b is 35 to 68 wt%, and preferably 35 to 65 wt%. The content c is 35 to 55 wt%, and preferably 35 to 50 wt%. The content d is 3 to 15 wt%, and preferably 5 to 15 wt%. The content e is 0 to 6 wt%, and more preferably 0 to 4 wt%.

[0015] The fluorine-containing polymer can be prepared by polymerizing hexafluoropropylene oxide through photo-oxidation, catalytic oligomerization, plasma or anionic polymerization, and then reacting with water, amine and ester compounds, respectively, to form the corresponding fluorine-containing polymer containing carboxyl groups, amine groups and ester groups.

[0016] Further, the molar ratio of the fluorine-containing polymer to the water-soluble resin is from 1:2 to 1:30, and preferably from 1:3 to 1:25.

[0017] The water-soluble resin is one or a mixture of polyvinylpyrrolidones, polyacrylic acids, polyurethanes, fluorine-containing polyvinylpyrrolidones, fluorine-containing polyacrylic acids, and fluorine-containing polyurethanes. The water-soluble resin may be one or a mixture of polyvinylpyrrolidones, polyacrylic acids, and polyurethanes, or may be a water-soluble resin obtained by substituting all or a part of the hydrogen atoms of the alkyl groups of the water-soluble resins with fluorine atoms. The number average molecular weight of the water-soluble resin is 3,000 to 30,000, preferably 4,000 to 26,000, and more preferably 6,000 to 22,000.

[0018] The polyvinylpyrrolidones may be polyvinylpyrrolidone or may be polymers of polyvinylpyrrolidone and other monomers. The polyvinylpyrrolidones may be used alone or in combination.

[0019] The polyacrylic acids may be polyacrylic acid or may be polymers of polyacrylic acid and other monomers. The polyacrylic acids may be used alone or in combination.

[0020] The polyurethanes may refer to polyurethane or to polymers of polyurethane and other monomers. The polyurethanes may be used alone or in combination.

[0021] Furthermore, the alkali may be one or more of the structures of ammonia water, tetramethylammonium hydroxide, alkanolamine, aromatic amine, alkylamine, etc., and is preferably tetramethylammonium hydroxide. Based on the total weight of the composition for preparing the top anti-reflective coating, the content of tetramethylammonium hydroxide is 0.2wt%-2wt%, preferably 0.2wt%-1wt%.

[0022] Furthermore, the acid may be an organic acid, an inorganic acid, or an amino acid. The inorganic acid is preferably hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, or hydrofluoric acid. The organic acid is preferably oxalic acid, citric acid, alkylsulfonic acid, alkylcarboxylic acid, alkylbenzenesulfonic acid, alkylbenzenecarboxylic acid, or alkylsulfonic acid, alkylcarboxylic acid, alkylbenzenesulfonic acid, or alkylbenzenecarboxylic acid obtained by substituting all or part of the hydrogen atoms of the alkyl group with fluorine atoms. The number of carbon atoms contained in the alkyl group is in the range of 1 to 20, preferably 3 to 15. The amino acid is preferably aminoacetic acid, alanine, valine, leucine, isoleucine, proline, phenylalanine, tryptophan, methionine, serine, threonine, γ-aminobutyric acid, β-cyanoalanine, aspartic acid, or the like.

[0023] The content of the acid is usually 0.3 wt % to 5 wt %, preferably 0.5 wt % to 3 wt %, based on the total weight of the composition for producing a top anti-reflective coating.

[0024] Furthermore, the surfactant is isopropanol, hexafluoroisopropanol, methanol, dodecyl carboxylic acid, dodecyl benzene sulfonic acid, etc., and its content is 0.1 wt% to 5 wt%, preferably 0.3 wt% to 4 wt%, based on the total weight of the composition for manufacturing the top anti-reflective coating for photoresist.

[0025] Furthermore, the composition for preparing a top anti-reflective coating further comprises water and / or a water-soluble organic solvent, which is an alcohol, a ketone or an ester. Preferably, the water-soluble organic solvent is methanol, ethanol, isopropanol, acetone, methyl acetate, ethyl acetate, ethyl lactate, dimethylformamide or dimethyl sulfoxide.

[0026] The present invention further provides a top antireflective coating for photoresist prepared from any of the above-described fluorine-containing compositions for preparing a top antireflective coating.

[0027] The present invention further provides a fluorine-containing composition comprising a fluorine-containing polymer, the structural formula of which is as follows: CF 2 (CF 3 )CF 2 -[O-CF(CF 3 )CF 2 ] n -O-CF(CF 3 )COO-R In the formula, n is in the range of 1 to 8, and R is H, NH 4 one or more of In the weight of the fluorine-containing composition, the content a of the fluorine-containing polymer where n is 1 is 0 to 10 wt%, the content b of the fluorine-containing polymer where n is 2 is 30 wt% to 68 wt%, the content c of the fluorine-containing polymer where n is 3 is 32 wt% to 60 wt%, the content d of the fluorine-containing polymer where n is 4 is 0 to 15 wt%, and the content e of the fluorine-containing polymer where n is 5 is 0 to 8 wt%, and the content b + the content c is 80 wt%, and the content a, the content d and the content e are simultaneously 0, or any of them is 0, or are not simultaneously 0. Effect of the Invention

[0028] The present invention obtains a fluorine-containing composition that meets the specific composition requirements of the present invention by controlling the synthetic polymerization degree of the fluorine-containing polymer and the content distribution of the fluorine-containing polymer component in the fluorine-containing composition. This fluorine-containing composition is easy to produce, has low raw material costs, is easy to decompose, has low toxicity, and is environmentally friendly. The composition solution for producing a top antireflective coating produced therefrom has good solution stability and film-forming properties, and at the same time, the refractive index of the antireflective coating produced therefrom under a 248 nm light source is 1.41 to 1.44, and the amount of use is reduced, there is no haze, and light scattering and standing wave effects can be avoided. At the same time, the pH of the composition for producing a top antireflective coating matches well with the pH of the photoresist, and it can be used as a top antireflective coating for photoresist to reduce the standing wave effect in the photolithography process. The composition for producing a top antireflective coating also reduces the viscosity of the system and improves the surface pores and uniformity by adding a preferred surfactant, while improving the problem of the relatively large difference in thickness between the center point and the edge after coating, thereby improving the yield rate of the photolithography process. [Brief description of the drawings]

[0029] [Figure 1a] 1 shows a photograph of the state of the composition solution of Example 1 on the first day. [Figure 1b] 1 shows a photograph of the state of the composition solution of Example 1 on the 14th day. [Figure 1c] 1 shows a photograph of the state of the composition solution of Comparative Example 7 on the third day. [Figure 1d] 1 shows a photograph of the state of the composition solution of Comparative Example 7 on the 14th day. [Diagram 2] 1 shows a micrograph of a film formed from the composition of Example 1. [Diagram 3] 1 shows a photomicrograph of a film formed from the composition of Example 2. [Figure 4] 1 shows a micrograph of a film formed from the composition of Comparative Example 1. [Diagram 5]1 shows a micrograph of a film formed from the composition of Comparative Example 4. [Figure 6] 1 shows a micrograph of a film formed from the composition of Comparative Example 5. [Figure 7] 1 shows a photoresist pattern formed using a top antireflective coating made from the composition of Example 1 in a photolithography process. [Figure 8] 3 shows a photoresist pattern formed using a top antireflective coating prepared from the composition of Comparative Example 6 in a photolithography process. [Figure 9a] 1 shows an SEM photograph of the thickness measurement at the center point of a top anti-reflective coating produced from a sample of Example 1. [Figure 9b] 4 shows an SEM photograph of the edge thickness measurement of the top anti-reflective coating produced from the sample of Example 1. [Figure 10a] 1 shows an SEM photograph of the thickness measurement at the center point of a top anti-reflective coating produced from a sample of Comparative Example 9. [Figure 10b] 1 shows an SEM photograph of the edge thickness measurement of a top anti-reflective coating produced from a sample of Comparative Example 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] The contents of the present invention will now be described with reference to some exemplary embodiments. It should be understood that these embodiments are provided only to enable those skilled in the art to better understand and realize the contents of the present invention, and are not intended to limit the scope of the present invention.

[0031] As used herein, the term "including" and variations thereof should be interpreted as an open-ended term meaning "including but not limited to." The term "based on" should be interpreted as "based at least in part on." The terms "one embodiment" and "one type of embodiment" should be interpreted as "at least one embodiment." The term "another embodiment" should be interpreted as "at least one other embodiment."

[0032] This example discloses a method for preparing a fluorine-containing polymer, i.e., a perfluoropolyether carboxylic acid, for making a top antireflective coating.

[0033] Preparation of perfluoropolyether carboxylic acids (1) First, 50ml of acetonitrile and 50ml of tetraethylene glycol dimethyl ether were put into a 1L polymerization kettle, then 5g of catalyst KF was put into the polymerization kettle, and after uniform stirring and mixing, it was replaced with high purity nitrogen three times, sucked until the negative pressure was -0.1MPa, cooled to the set temperature of 0 ° C, fed 50g of hexafluoropropylene oxide, and controlled the reaction process using regular feeding (50g / h), and controlled the temperature between 0 ~ 10 ° C. After adding 1000g of hexafluoropropylene oxide, it was returned to normal pressure, and after the reaction was completed, it was continued to stir for 2 hours, stopped stirring, returned to room temperature, and obtained a mixture. (2) The mixture was layered, and the lower layer product was centrifuged and filtered to separate reaction product 1, which was then placed in a distillation apparatus. Perfluoropolyether acyl fluoride with a purity of 99% or more (purity was measured by gas chromatography) was obtained by rectification purification. (3) The above perfluoropolyether acyl fluoride was placed in a 1 L acid conversion vessel, and water was added so that the volume ratio of perfluoropolyether acyl fluoride to water was 1:3. The mixture was heated under reflux for 4 hours, and the heating was continued up to 90°C. After demulsification, the mixture was allowed to stand and separate to remove the upper water. The above demulsification and demulsification steps were repeated twice, and the temperature was then raised to 110°C to remove the remaining water and hydrogen fluoride, thereby obtaining perfluoropolyether carboxylic acid.

[0034] By controlling the degree of polymerization of the perfluoropolyether acyl fluorides, perfluoropolyether carboxylic acids having the following general structures were obtained, respectively. CF 2 (CF 3 )CF 2 -[O-CF(CF 3 )CF 2 ] n-O-CF(CF 3 )COOH

[0035] Based on the weight of the entire polymer, the content a of perfluoropolyether carboxylic acid A where n is 1 is 0 to 10 wt%, the content b of perfluoropolyether carboxylic acid B where n is 2 is 30 wt% to 68 wt%, the content c of perfluoropolyether carboxylic acid C where n is 3 is 32 wt% to 60 wt%, the content d of perfluoropolyether carboxylic acid D where n is 4 is 0 to 15 wt%, perfluoropolyether carboxylic acids where n is 5 include perfluoropolyether carboxylic acid E where n is 5 and perfluoropolyether carboxylic acid F where n is 8, the total content e of perfluoropolyether carboxylic acid E and perfluoropolyether carboxylic acid F is 0 to 8 wt%, the content b + the content c ≧ 80 wt%, the content a, the content d and the content e are simultaneously 0, or any of them are 0, or not simultaneously 0. Example 1

[0036] The above perfluoropolyether carboxylic acids with different polymerization degrees were mixed. The mixing ratio, by weight, was 4 wt% perfluoropolyether carboxylic acid A, 55 wt% perfluoropolyether carboxylic acid B, 38 wt% perfluoropolyether carboxylic acid C, and 3 wt% perfluoropolyether carboxylic acid D. As a result, a perfluoropolyether carboxylic acid composition was obtained, and its specific composition is shown in Table 1.

[0037] 0.0064 moles of perfluoropolyether carboxylic acid was prepared as a 2 wt% aqueous solution, and then blended with a 2 wt% aqueous polyvinylpyrrolidone solution so that the molar ratio of perfluoropolyether carboxylic acid to polyvinylpyrrolidone was 10:1, and stirred until a transparent solution was obtained. Then, under stirring conditions, a 2 wt% tetramethylammonium hydroxide solution was added to the solution. The amount of tetramethylammonium hydroxide used was 0.584 g. Then, 1.32 g of surfactant isopropanol was added, and 2.0 g of oxalic acid was added to adjust the pH value to 2.0-2.5. The composition solution was obtained by filtration.

[0038] The composition of the composition solution was calculated to be, by weight, 1.727 wt% perfluoropolyether carboxylic acid composition, 0.027 wt% polyvinylpyrrolidone, 0.221 wt% tetramethylammonium hydroxide, 0.499 wt% isopropanol, 0.756 wt% oxalic acid, and 96.77 wt% water. Example 2

[0039] The above perfluoropolyether carboxylic acids with different polymerization degrees were mixed. The mixing ratio, by weight, was 2 wt% perfluoropolyether carboxylic acid A, 40 wt% perfluoropolyether carboxylic acid B, 48 wt% perfluoropolyether carboxylic acid C, and 10 wt% perfluoropolyether carboxylic acid D. As a result, a perfluoropolyether carboxylic acid composition was obtained, and its specific composition is shown in Table 1.

[0040] A composition solution was obtained in the same manner as in Example 1, except that 1.32 g of surfactant hexafluoroisopropanol was used instead of isopropanol. By weight, the composition solution had the following composition: 1.74 wt% perfluoropolyether carboxylic acid composition, 0.026 wt% polyvinylpyrrolidone, 0.21 wt% tetramethylammonium hydroxide, 0.475 wt% hexafluoroisopropanol, 0.72 wt% oxalic acid, and 96.829 wt% water. Example 3

[0041] The above perfluoropolyether carboxylic acids with different polymerization degrees were mixed. The mixing ratio, by weight, was 8wt% perfluoropolyether carboxylic acid A, 54wt% perfluoropolyether carboxylic acid B, 36wt% perfluoropolyether carboxylic acid C, 1wt% perfluoropolyether carboxylic acid D, and 1wt% perfluoropolyether carboxylic acid F. As a result, a perfluoropolyether carboxylic acid composition was obtained, and its specific composition is shown in Table 1.

[0042] A composition solution was obtained in the same manner as in Example 1, except that 0.11 g of polyacrylic acid was used instead of polyvinylpyrrolidone, and surfactant methanol was used instead of isopropanol. The polyacrylic acid had Mw=3000 and was a 50 wt% aqueous solution.

[0043] By weight, the composition solution had the following composition by weight: 1.709 wt% perfluoropolyether carboxylic acid composition, 0.042 wt% polyacrylic acid, 0.223 wt% tetramethylammonium hydroxide, 0.504 wt% methanol, 0.764 wt% oxalic acid, and 96.758 wt% water. Example 4

[0044] The above perfluoropolyether carboxylic acids with different polymerization degrees were mixed. The mixing ratio, by weight, was 2 wt% perfluoropolyether carboxylic acid A, 32 wt% perfluoropolyether carboxylic acid B, 58 wt% perfluoropolyether carboxylic acid C, 2 wt% perfluoropolyether carboxylic acid D, and 6 wt% perfluoropolyether carboxylic acid E. As a result, a perfluoropolyether carboxylic acid composition was obtained, and its specific composition is shown in Table 1.

[0045] A composition solution was obtained in the same manner as in Example 1, except that citric acid was used instead of oxalic acid, and a surfactant, dodecyl carboxylic acid, was used instead of isopropanol.

[0046] By weight, the composition solution had the following composition by weight: 1.750 wt% perfluoropolyether carboxylic acid composition, 0.024 wt% polyvinylpyrrolidone, 0.201 wt% tetramethylammonium hydroxide, 0.455 wt% dodecyl carboxylic acid, 0.690 wt% citric acid, and 96.880 wt% water. Example 5

[0047] The above perfluoropolyether carboxylic acids with different polymerization degrees were mixed. The mixing ratio by weight was 61 wt% perfluoropolyether carboxylic acid B, 37 wt% perfluoropolyether carboxylic acid C, and 2 wt% perfluoropolyether carboxylic acid D. As a result, a perfluoropolyether carboxylic acid composition was obtained, and its specific composition is shown in Table 1.

[0048] A composition solution was obtained in the same manner as in Example 1, except that hexafluoroisopropanol was used instead of isopropanol.

[0049] By weight, the composition solution had the following composition by weight: 1.729 wt% perfluoropolyether carboxylic acid composition, 0.027 wt% polyvinylpyrrolidone, 0.219 wt% tetramethylammonium hydroxide, 0.495 wt% hexafluoroisopropanol, 0.75 wt% oxalic acid, 96.78 wt% water. Example 6

[0050] The above perfluoropolyether carboxylic acids with different polymerization degrees were mixed. The mixing ratio, by weight, was 2 wt% perfluoropolyether carboxylic acid A, 65 wt% perfluoropolyether carboxylic acid B, 32 wt% perfluoropolyether carboxylic acid C, and 1 wt% perfluoropolyether carboxylic acid F. As a result, a perfluoropolyether carboxylic acid composition was obtained, and its specific composition is shown in Table 1.

[0051] A composition solution was obtained in the same manner as in Example 1, except that perfluorohexanesulfonic acid was used instead of oxalic acid.

[0052] By weight, the composition solution had the following composition by weight: 1.725 wt% perfluoropolyether carboxylic acid composition, 0.027 wt% polyvinylpyrrolidone, 0.223 wt% tetramethylammonium hydroxide, 0.504 wt% isopropanol, 0.763 wt% perfluorohexane sulfonic acid, and 96.758 wt% water. Example 7

[0053] The above perfluoropolyether carboxylic acids with different polymerization degrees were mixed. The mixing ratio was 52 wt% perfluoropolyether carboxylic acid B and 48 wt% perfluoropolyether carboxylic acid C by weight. As a result, a perfluoropolyether carboxylic acid composition was obtained, and the specific composition is shown in Table 1.

[0054] A composition solution was obtained in the same manner as in Example 1, except that aminoacetic acid was used instead of oxalic acid.

[0055] By weight, the composition solution had the following composition by weight: 1.733 wt% perfluoropolyether carboxylic acid composition, 0.026 wt% polyvinylpyrrolidone, 0.216 wt% tetramethylammonium hydroxide, 0.488 wt% isopropanol, 0.74 wt% aminoacetic acid, 96.797 wt% water. Comparative Example 1

[0056] A composition solution was obtained in the same manner as in Example 1, and the following perfluoropolyether carboxylic acids were used. The above perfluoropolyether carboxylic acids with different polymerization degrees were mixed. The mixing ratio, by weight, was 11 wt% perfluoropolyether carboxylic acid A, 48 wt% perfluoropolyether carboxylic acid B, 38 wt% perfluoropolyether carboxylic acid C, and 3 wt% perfluoropolyether carboxylic acid D. As a result, a perfluoropolyether carboxylic acid composition was obtained, and its specific composition is shown in Table 2. Comparative Example 2

[0057] A composition solution was obtained in the same manner as in Example 1, and the following perfluoropolyether carboxylic acids were used. The above perfluoropolyether carboxylic acids with different polymerization degrees were mixed. The mixing ratio, by weight, was 4 wt% perfluoropolyether carboxylic acid A, 28 wt% perfluoropolyether carboxylic acid B, 56 wt% perfluoropolyether carboxylic acid C, and 12 wt% perfluoropolyether carboxylic acid D. As a result, a perfluoropolyether carboxylic acid composition was obtained, and its specific composition is shown in Table 2. Comparative Example 3

[0058] A composition solution was obtained in the same manner as in Example 1, and the following perfluoropolyether carboxylic acids were used. The above perfluoropolyether carboxylic acids with different polymerization degrees were mixed. The mixing ratio, by weight, was 4 wt% perfluoropolyether carboxylic acid A, 32 wt% perfluoropolyether carboxylic acid B, 61 wt% perfluoropolyether carboxylic acid C, and 3 wt% perfluoropolyether carboxylic acid D. As a result, a perfluoropolyether carboxylic acid composition was obtained, and its specific composition is shown in Table 2. Comparative Example 4

[0059] A composition solution was obtained in the same manner as in Example 1, and the following perfluoropolyether carboxylic acids were used. The above perfluoropolyether carboxylic acids with different polymerization degrees were mixed. The mixing ratio, by weight, was 4 wt% perfluoropolyether carboxylic acid A, 42 wt% perfluoropolyether carboxylic acid B, 38 wt% perfluoropolyether carboxylic acid C, and 16 wt% perfluoropolyether carboxylic acid D. As a result, a perfluoropolyether carboxylic acid composition was obtained, and its specific composition is shown in Table 2. Comparative Example 5 A composition solution was obtained in the same manner as in Example 1, and the following perfluoropolyether carboxylic acids were used. The above perfluoropolyether carboxylic acids with different polymerization degrees were mixed. The mixing ratio, by weight, was 4 wt% perfluoropolyether carboxylic acid A, 46 wt% perfluoropolyether carboxylic acid B, 38 wt% perfluoropolyether carboxylic acid C, 3 wt% perfluoropolyether carboxylic acid D, and 9 wt% perfluoropolyether carboxylic acid E. As a result, a perfluoropolyether carboxylic acid composition was obtained, and its specific composition is shown in Table 2. Comparative Example 6

[0060] The composition solution was obtained in the same manner as in Example 1, but oxalic acid was not used. Perfluoropolyether carboxylic acids with different polymerization degrees produced by the above-mentioned method were mixed. The mixing ratio, by weight, was 4 wt% perfluoropolyether carboxylic acid A, 55 wt% perfluoropolyether carboxylic acid B, 38 wt% perfluoropolyether carboxylic acid C, and 3 wt% perfluoropolyether carboxylic acid D. As a result, a perfluoropolyether carboxylic acid composition was obtained, and its specific composition is shown in Table 2. Comparative Example 7

[0061] A composition solution was obtained in the same manner as in Example 1, but without using the surfactant isopropanol.

[0062] The following methods were used to evaluate the solution stability, film-forming property, minimum coating weight and refractive index of each prepared composition, as well as the applicability of the prepared top anti-reflective coating in photolithography process. The results are shown in Table 2 and the attached figures. Comparative Example 8

[0063] Using the blending ratio of Patent CN112034683B, the perfluoropolyether carboxylic acids with different polymerization degrees prepared by the above disclosed method were mixed without adding surfactant and organic acid. The blending ratio, by weight, was 10wt% perfluoropolyether carboxylic acid A, 66wt% perfluoropolyether carboxylic acid B, 19wt% perfluoropolyether carboxylic acid C, 1wt% perfluoropolyether carboxylic acid D, and 4wt% perfluoropolyether carboxylic acid E. As a result, a perfluoropolyether carboxylic acid composition was obtained, the specific composition of which is shown in Table 2.

[0064] The following methods were used to evaluate the solution stability, film-forming property, minimum coating weight and refractive index of each prepared composition, as well as the applicability of the prepared top anti-reflective coating in the photolithography process. The results are shown in Table 2. Comparative Example 9

[0065] Using the blending ratio of Patent CN112034683B, the perfluoropolyether carboxylic acids with different polymerization degrees prepared by the above disclosed method were mixed without adding surfactant and organic acid. The blending ratio, by weight, was 4wt% perfluoropolyether carboxylic acid A, 58wt% perfluoropolyether carboxylic acid B, 28wt% perfluoropolyether carboxylic acid C, 8wt% perfluoropolyether carboxylic acid D, and 2wt% perfluoropolyether carboxylic acid E. As a result, a perfluoropolyether carboxylic acid composition was obtained, the specific composition of which is shown in Table 2.

[0066] The following methods were used to evaluate the solution stability, film-forming property, minimum coating weight and refractive index of each prepared composition, as well as the applicability of the prepared top anti-reflective coating in the photolithography process. The results are shown in Table 2. Comparative Example 10

[0067] Using the blending ratio of Example 4 of Patent CN112034683B, without adding surfactant and organic acid, the perfluoropolyether carboxylic acids with different polymerization degrees prepared by the above disclosed method were mixed. The blending ratio, by weight, was 4wt% perfluoropolyether carboxylic acid A, 58wt% perfluoropolyether carboxylic acid B, 32wt% perfluoropolyether carboxylic acid C, 4wt% perfluoropolyether carboxylic acid D, and 2wt% perfluoropolyether carboxylic acid E. As a result, a perfluoropolyether carboxylic acid composition was obtained, the specific composition of which is shown in Table 2.

[0068] The following methods were used to evaluate the solution stability, film-forming property, minimum coating weight and refractive index of each prepared composition, as well as the applicability of the prepared top anti-reflective coating in the photolithography process. The results are shown in Table 2. Comparative Example 11

[0069] Using the blending ratio of Example 4 of Patent CN112034683B, surfactant isopropanol and oxalic acid were added, and perfluoropolyether carboxylic acids with different polymerization degrees prepared by the above disclosed method were mixed. The blending ratio, by weight, was 4wt% perfluoropolyether carboxylic acid A, 58wt% perfluoropolyether carboxylic acid B, 32wt% perfluoropolyether carboxylic acid C, 4wt% perfluoropolyether carboxylic acid D, and 2wt% perfluoropolyether carboxylic acid E. As a result, a perfluoropolyether carboxylic acid composition was obtained, the specific composition of which is shown in Table 2.

[0070] The following methods were used to evaluate the solution stability, film-forming properties, minimum coating weight and refractive index of each prepared composition, as well as the applicability of the prepared top antireflective coating in photolithography processes. The results are shown in Table 2. How to measure number average molecular weight

[0071] The number average molecular weight of the perfluoropolyether carboxylic acid was measured by the acid value method as follows. 1 ml of the perfluoropolyether carboxylic acid to be measured was pipetted, and the data m (g) was weighed and recorded. 35 ml of water and 15 ml of absolute ethanol were added, and titrated with sodium hydroxide solution of standard concentration c (mol / ml). When the titration reached pH = 7, the volume v (ml) of sodium hydroxide consumed was recorded. The number average molecular weight of the perfluoropolyether carboxylic acid was calculated according to the following formula. Number average molecular weight of perfluoropolyether carboxylic acid = m / cv. Solution stability evaluation method

[0072] 250 ml of the solution of the composition for manufacturing an anti-reflective coating prepared was placed in a 500 ml beaker and allowed to stand. The state of the solution was visually observed, and the time when a flocculent precipitate appeared was recorded as the stability time h (in days), and the stability was evaluated, with 14 days being the cut-off time for observation. The larger the h value, the better the stability of the solution. Method for evaluating film-forming properties

[0073] A solution of each composition for manufacturing an anti-reflective film was applied onto a silicon wafer (4 inches, boron-doped, approximately 525 μm thick, approximately 100 mm in diameter) using a spin coater, baked at 100° C. for 90 seconds, and cooled to form a corresponding film. The state of the formed film was visually observed, microscopically observed using a metallurgical microscope, and microscopic photographs were taken to evaluate the film-forming properties of the composition. Minimum application amount evaluation method

[0074] A positive photoresist was applied onto a silicon wafer using a spin coater, and then prebaked on a hot plate at 130° C. for 60 seconds to form a photoresist film having a thickness of 800 nm on the silicon wafer. The film thickness was measured using a film thickness measuring device. Then, using the same spin coater as above, a composition for forming an antireflective film was applied onto the photoresist film, and prebaked on a hot plate at 90° C. for 60 seconds to form an antireflective film having a thickness of 45 nm on the photoresist film. The minimum amount of the antireflective film composition that can cover the edge portion of the photoresist film and form a uniformly applied film by visual observation was recorded as the minimum amount of application to form an antireflective film, and the results are shown in Tables 1 and 2. How to measure the refractive index

[0075] A solution of each composition for manufacturing an anti-reflective coating was applied onto a silicon wafer (4 inches, boron-doped, about 525 μm thick, about 100 mm in diameter) using a spin coater, baked at 100° C. for 90 seconds, and cooled to form a corresponding film. The film was tested using an ellipsometer to measure the refractive index at 248 nm. How to measure viscosity

[0076] Using a digital viscometer, the instrument was first preheated for 20 minutes, and at the same time the base nut was adjusted so that the instrument was parallel to the ground. The rotor and rotating cylinder were then attached, and the liquid to be measured was then poured in (rotor No. 0 was used). The temperature was set to 25°C using a cooling circulation pump, the circulation cup was connected, and the water temperature in the circulation cup was allowed to reach 25°C. The rotating cylinder was completely immersed in water and left for 20 minutes until it reached a constant temperature. The liquid viscosity was measured at a rotation speed of 60 r / min and a rotation time of 10 minutes, and the measurement was repeated five times to obtain the average value. The results are shown in Tables 1 and 2. Applicability evaluation method during photolithography process

[0077] A solution of each composition for manufacturing an antireflective coating was applied onto a silicon wafer (4 inches, doped with boron, about 525 μm thick, about 100 mm in diameter) coated with photoresist using a spin coater, baked at 100° C. for 90 seconds, and cooled to form a coating film to be used as a top antireflective coating for the photoresist. The coated sample was exposed through a photomask in a 248 nm photolithography machine, then baked at 100° C. for 60 seconds, and then developed with a 2.38 wt% tetramethylammonium hydroxide (TMAH) developer for 60 seconds. The developed silicon wafer was frozen and cut, and the slices were sprayed with gold, then placed under a scanning electron microscope for observation, defects were searched for, and screenshots were taken to evaluate the effect of the top antireflective coating on the photoresist in use. JPEG0007569587000001.jpg117170JPEG0007569587000002.jpg169170Note: 1) The percentages in the table are weight percentages, and the number average molecular weight refers to the number average molecular weight of perfluoropolyether carboxylic acid.

[0078] 2) The contents a, b, c, d, and e are each defined as in the specification of the present application. For example, the content a is the content of the perfluoropolyether carboxylic acid component in which n is 1.

[0079] As can be seen from Table 1, the compositions prepared by perfluoropolyether carboxylic acid, water-soluble resin, acid and surfactant, etc., which satisfy the composition requirements of the present application according to Examples 1 to 7 of the present application, have good solution stability, can obtain a film with a uniform surface and no holes with a minimum application amount of 2.0 to 2.3 ml, and have good film formability. At the same time, the anti-reflective film produced therefrom has a refractive index of 1.41 to 1.44 at 248 nm, can effectively reduce the refractive index under laser irradiation with a wavelength of 248 nm, does not cause light scattering or standing wave effect, and can be used as a top anti-reflective film for photoresist. Meanwhile, the perfluoropolyether carboxylic acid of Comparative Example 2 contains 28 wt% of the perfluoropolyether carboxylic acid component with n being 2, that is, the content of component b is less than 30 wt%, so the minimum application amount of the composition to obtain a film with a uniform surface and no holes is 3.8 ml. The perfluoropolyether carboxylic acid of Comparative Example 3 contains 61 wt% of the perfluoropolyether carboxylic acid component with n being 3, that is, the content of component c is greater than 60 wt%, so the minimum application amount of the composition to obtain a film with a uniform surface and no pores is 4.5 ml. The composition of Comparative Example 7 does not use the surfactant isopropanol, so the minimum application amount of the composition to obtain a film with a uniform surface and no pores is 5.5 ml. Comparative Examples 8 and 9 use the compounding ratio of Patent CN112034683B, and do not add surfactant and organic acid, but the minimum application amount is 2.5 ml, and the viscosity is significantly higher than Examples 1 to 7. Comparative Example 10 uses the compounding ratio of Example 4 of Patent CN112034683B. Comparative Example 11 adds surfactant isopropanol and oxalic acid based on the compounding ratio of Example 4 of Patent CN112034683B.

[0080] 1a, 1b, 1c and 1d, the composition solution of Example 1, which meets the requirements of the present application, remains transparent after 14 days of standing, does not produce flocculent precipitates, and has good solution stability. The composition solution of Comparative Example 7, which does not use the surfactant isopropanol, does not have good stability, produces precipitates after 3 days of standing, and still has obvious precipitates in the solution even after 14 days of standing.

[0081] As can be seen from Figures 2-6, the compositions of Examples 1 and 2 that meet the requirements of the present application can obtain a film with a uniform surface and no holes, and have good film-forming properties (see Figures 2-3). On the other hand, the perfluoropolyether carboxylic acid of Comparative Example 1 contains 11 wt% of a perfluoropolyether carboxylic acid component with n being 1, that is, the content of component a is greater than 10 wt%, so the film-forming properties of the composition prepared therefrom are not good, and the film formed has many obvious holes (see Figure 4). The perfluoropolyether carboxylic acid of Comparative Example 4 contains 16 wt% of a perfluoropolyether carboxylic acid component with n being 4, that is, the content of component d is greater than 15 wt%, so the film-forming properties of the composition prepared therefrom are poor, and the film formed has obvious non-uniform distribution and many holes (see Figure 5). The perfluoropolyether carboxylic acid of Comparative Example 5 contained 9 wt% of perfluoropolyether carboxylic acid component with n≧5, i.e., the content of component e was greater than 8 wt%, so the composition prepared therefrom had poor film-forming properties, and the film formed was non-uniformly distributed and had many obvious holes (see FIG. 6).

[0082] As can be seen from Figures 7-8, when the top antireflective coating made from the composition of Example 1, which meets the requirements of the present application, was used in a photolithography process, the photoresist pattern was formed normally (see Figure 7). Meanwhile, no oxalic acid was used in the composition of Comparative Example 6. When the top antireflective coating made from the composition was used in a photolithography process, a T-top occurred in the photoresist (see Figure 8). The reason for this is as follows: The part of the photoresist irradiated by a specific light source undergoes a photochemical reaction to form H + As a result, the pH of the photoresist exposed to light falls to between 1.5 and 2.5. If the pH value of the top antireflective layer is relatively high, H +The H diffuses into the boundary area between the top antireflective layer and the photoresist, and at the same time the pH of the area increases, and the H cannot be completely removed by the developer in the development process, thus forming a T-shaped top. By adding an appropriate amount of acid to the top antireflective layer system, the H in the photoresist can be removed. + The diffusion of the fluorine into the anti-reflection film can be suppressed, thereby preventing the formation of a T-shaped top.

[0083] As can be seen from Comparative Example 10 and Comparative Example 11, the addition of isopropanol and oxalic acid improves the problem of the surface of the membrane layer being uneven and having many holes, and at the same time reduces the viscosity and coating amount. This is because isopropanol plays the role of promoting dissolution, increasing the solubility of perfluoropolyether acid in water, and optimizing the uniformity of the blended solution. At the same time, the use of isopropanol reduces the viscosity of the system, making it easier for the blended system to become uniform during the stirring process, and the reduced viscosity also reduces the coating amount.

[0084] Example 1 and Comparative Example 9 were selected to prepare samples, and coating experiments were carried out according to the disclosed minimum coating amount evaluation method. The thicknesses of the center point and edge point of the film layer of the composition obtained in Example 1 were both 253A, as shown in Figures 9a and 9b, respectively.

[0085] The thicknesses of the film layer of the composition obtained in Comparative Example 9 at the center and edge points were 332A and 228A, respectively, as shown in Figures 10a and 10b.

[0086] Under the same manufacturing process, the top anti-reflective coating of the composition of Example 1 has better thickness uniformity at the center and edge points of the coating layer compared with Comparative Example 9 which uses the solution of Patent CN112034683B.

[0087] As can be seen from this, the solution of the composition for the top antireflective coating satisfying the requirements of the present application has good solution stability and good film forming properties, and can form a uniform antireflective coating with a predetermined thickness on a substrate with a relatively small coating amount. The antireflective coating has a refractive index of 1.41 to 1.44 under a 248 nm light source, can avoid the occurrence of light scattering and standing wave effect, and can be used as a top antireflective coating for photoresist to form a normal photoresist pattern.

[0088] As shown in Comparative Examples 1 to 11, compositions that exceed the requirements of the limited features of the present application have problems of poor solution stability and / or poor film forming properties, and as a result, cannot be used as a top antireflective coating for photoresist, or have problems of relatively large minimum coating weight, or the top antireflective coating produced causes T-top in the photoresist during the photolithography process, or has uneven thickness between the center and edge points of the coating layer.

[0089] The use of certain surfactants reduces the viscosity of the system, making it easier for the formulated system to form a homogeneous phase during the stirring process, resulting in a uniform thickness of the formed film, while also reducing the amount of coating due to the reduced viscosity.

[0090] Those skilled in the art will understand that the above-described embodiments are specific examples for realizing the present invention, and that in actual application, various changes in form and details can be made without departing from the spirit and scope of the present invention.

Claims

1. A composition for producing a top anti-reflective coating, comprising: A) A fluorine-containing composition comprising a fluorine-containing polymer having the following structural formula: CF 2 (CF 3 )CF 2 -[O-CF(CF 3 )CF 2 ] n -O-CF(CF 3 )COO-R where n is in the range of 1 to 8 and R is H, NH 4 one or more of a fluorine-containing composition in which, based on the weight of the fluorine-containing composition, the content a of the fluorine-containing polymer where n is 1 is 0 to 10 wt %, the content b of the fluorine-containing polymer where n is 2 is 30 wt % to 68 wt %, the content c of the fluorine-containing polymer where n is 3 is 32 wt % to 60 wt %, the content d of the fluorine-containing polymer where n is 4 is 0 to 15 wt %, the content e of the fluorine-containing polymer where n is 5 is 0 to 8 wt %, and the content b + the content c ≧ 80 wt %, the content a, the content d and the content e are simultaneously 0, or any of them is 0, or not simultaneously 0; B) a water-soluble resin; C) an alkali; D) an acid; E) a surfactant, The composition for producing a top anti-reflective coating is characterized in that the surfactant is one or more of isopropanol, hexafluoroisopropanol, and methanol, the content of the surfactant is 0.1 wt % to 5 wt % based on the total weight of the composition for producing a top anti-reflective coating, and the content of the fluorine-containing composition is 1 wt % to 15 wt % based on the total weight of the composition for producing a top anti-reflective coating.

2. 2. The composition for manufacturing a top anti-reflective coating according to claim 1, wherein the water-soluble resin is one or a mixture of polyvinylpyrrolidones, polyacrylic acids, and polyurethanes.

3. 3. The composition for manufacturing a top anti-reflective coating according to claim 2, wherein the water-soluble resin is one or a mixture of a fluorine-containing polyvinylpyrrolidone, a fluorine-containing polyacrylic acid, and a fluorine-containing polyurethane.

4. The composition for producing a top anti-reflective coating according to any one of claims 1 to 5, characterized in that the viscosity of the composition for producing a top anti-reflective coating at 25°C is 1.3 to 1.5 cp, and the number average molecular weight of the fluorine-containing polymer is between 600 and 1300.

5. 5. The composition for manufacturing a top anti-reflective coating according to claim 4, wherein the content a is 0-9 wt%, the content b is 35 wt%-68 wt%, the content c is 35 wt%-55 wt%, the content d is 3 wt%-15 wt%, the content e is 0-6 wt%, and the sum of the content a, the content b, the content c, the content d, and the content e is 100 wt%.

6. The composition for preparing a top anti-reflective coating according to claim 5, wherein the alkali is one or more of ammonia water, tetramethylammonium hydroxide, alkanolamine, aromatic amine, and alkylamine, and the content of the alkali is 0.2 wt% to 2 wt%.

7. 7. The composition for manufacturing a top anti-reflective coating according to claim 6, wherein the acid is one or more of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, hydrofluoric acid, oxalic acid, citric acid, alkylsulfonic acid, alkylcarboxylic acid, alkylbenzenesulfonic acid, alkylbenzenecarboxylic acid, fluorine-substituted alkylsulfonic acid, fluorine-substituted alkylcarboxylic acid, fluorine-substituted alkylbenzenesulfonic acid, fluorine-substituted alkylbenzenecarboxylic acid and amino acid, and the content of the acid is 0.3 wt % to 5 wt %.

8. The composition for producing a top anti-reflective coating according to claim 7, further comprising water and / or a water-soluble organic solvent, and the molar ratio of the fluorine-containing polymer to the water-soluble resin in the composition for producing a top anti-reflective coating is 1:2 to 1:

30.

9. The molar ratio of the fluorine-containing polymer to the water-soluble resin in the composition for producing a top anti-reflective coating is 1:3 to 1:25, and / or the content of the surfactant is 0.3 wt % to 4 wt %, and / or the content of the acid is 0.5 wt % to 3 wt %, and / or the content of the alkali is 0.2 9. The composition for producing a top anti-reflective coating according to claim 8, wherein the content of the fluorine-containing composition in the composition for producing a top anti-reflective coating is 1.5 wt % to 12 wt %, and / or the number average molecular weight of the fluorine-containing polymer is between 650 and 1100, and / or the content a is 0 to 8 wt %, and / or the content b is 35 wt % to 65 wt %, and / or the content c is 35 wt % to 50 wt %, and / or the content d is 5 wt % to 15 wt %, and / or the content e is 0 to 4 wt %, and the sum of the contents a, b, c, d and e is 100 wt %.

10. The composition for producing a top anti-reflective coating according to claim 9, characterized in that the content of the fluorine-containing composition in the composition for producing a top anti-reflective coating is 1.5 wt % to 8 wt %, and / or the content a is 2 wt % to 8 wt %.

11. A top anti-reflective coating produced from the composition for producing a top anti-reflective coating according to any one of claims 1 to 10.

12. A fluorine-containing composition is used to prepare a composition for producing a top anti-reflective coating according to any one of claims 1 to 10, comprising a fluorine-containing polymer having the following structural formula: CF 2 (CF 3 )CF 2 -[O-CF(CF 3 )CF 2 ] n -O-CF(CF 3 )COO-R where n is in the range of 1 to 8 and R is H, NH 4 one or more of A fluorine-containing composition characterized in that, based on the weight of the fluorine-containing composition, the content a of the fluorine-containing polymer where n is 1 is 0 to 10 wt %, the content b of the fluorine-containing polymer where n is 2 is 30 wt % to 68 wt %, the content c of the fluorine-containing polymer where n is 3 is 32 wt % to 60 wt %, the content d of the fluorine-containing polymer where n is 4 is 0 to 15 wt %, and the content e of the fluorine-containing polymer where n is 5 is 0 to 8 wt %, and said content b + said content c ≧ 80 wt %, said content a, said content d and said content e are simultaneously 0, or any of them are 0, or are not simultaneously 0.

Citation Information

Patent Citations

  • Fluorine-containing polymer for photoresist, top anti-reflection film composition containing fluorine-containing polymer, and application of fluorine-containing polymer in photoresist

    CN112034682A

  • Fluorine-containing polymer for photoresist, top anti-reflection film composition containing fluorine-containing polymer and application of fluorine-containing polymer in photoresist

    CN112034683A

  • Antireflection film material

    JP1998069091A

  • Composition for antireflection coating and pattern forming method

    JP2004037887A

  • Surface antireflection film forming composition and pattern forming method using the same

    JP2009145658A