Hydrolyzable silyl group-containing polyoxyalkylene polymer, curable composition, and cured product

The development of a polyoxyalkylene polymer with a specific hydrolyzable silyl group structure and ruthenium complex catalyst addresses the challenges of side reactions in hydrosilylation, achieving high strength and curability in the cured product.

WO2024225205A1PCT designated stage expired Publication Date: 2024-10-31KANEKA CORP

Patent Information

Application Number
PCT/JP2024/015651
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-09-25
Filing Date
2024-04-19
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Hydrolyzable silyl group-containing polyoxyalkylene polymers face challenges in achieving both high strength and curability due to side reactions during hydrosilylation, such as isomerization and hydrogenation, which limit the introduction rate of silyl groups and the molecular weight of the resulting cured products.

Method used

A polyoxyalkylene polymer with a hydrolyzable silyl group-containing structure, represented by a specific general formula, is developed, which suppresses side reactions and enhances the introduction rate of silyl groups, achieving high molecular weight and improved curability through a hydrosilylation reaction using a ruthenium complex catalyst.

Benefits of technology

The polymer achieves a high silyl group introduction rate, resulting in a cured product with improved mechanical properties, including tensile strength and elongation, while maintaining good curability and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015651_31102024_PF_FP_ABST
    Figure JP2024015651_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a polyoxyalkylene polymer containing a polyoxyalkylene polymer molecule having a hydrolyzable silyl group-containing structure represented by formula (1), wherein: the ratio of the number of hydrolyzable silyl group-containing structures represented by formula (1) to the total number of hydrolyzable silyl, 1-propenyl, propyl and allyl groups is 0.85-1.00 inclusive; and the number average molecular weight of the polymer exceeds 3,000. In formula (1), R moieties are the same or different, and each represent a substituted or unsubstituted monovalent hydrocarbon group having 1-20 carbon atoms. X moieties are the same or different, and each represent a hydroxyl group or a hydrolyzable group. a represents 0, 1 or 2.
Need to check novelty before this filing date? Find Prior Art

Description

Hydrolyzable silyl group-containing polyoxyalkylene polymer, curable composition, and cured product

[0001] The present invention relates to a polyoxyalkylene polymer having a hydrolyzable silyl group, a curable composition containing the polymer, and a cured product thereof.

[0002] Polyoxyalkylene polymers having hydroxyl or hydrolyzable groups on silicon atoms and silyl groups capable of forming siloxane bonds (hereinafter referred to as "hydrolyzable silyl groups") are known as moisture-reactive polymers. These polymers cure through hydrolysis to form flexible rubber-like cured products, and are therefore used in many industrial products, such as sealants, adhesives, coatings, paints, and pressure-sensitive adhesives.

[0003] A commonly known method for obtaining such hydrolyzable silyl group-containing polyoxyalkylene polymers is to subject an allyl group-containing polyoxyalkylene polymer to a hydrosilane compound to hydrosilylation in the presence of a metal catalyst. However, a common problem with hydrosilylation of allyl group-containing compounds using a metal catalyst is the occurrence of side reactions such as isomerization of the allyl group to a 1-propenyl group (internal olefin) and hydrogenation during the reaction. When the widely used Karstedt catalyst (platinum divinyldisiloxane complex) is used in the hydrosilylation reaction of allyl group-containing polymers, the above-mentioned side reactions proceed at a rate of approximately 20%, limiting the rate of silyl group introduction. As a result, the rubber-like cured products obtained by curing curable compositions containing the resulting hydrolyzable silyl group-containing polymers have room for improvement in terms of modulus, tensile strength, etc.

[0004] A known method for improving the introduction rate of silyl groups is to subject a hydrosilane compound to a hydrosilylation reaction with a methallyl group rather than an allyl group. Patent Document 1 discloses that, while the introduction rate of silyl groups in the hydrosilylation reaction with an allyl group is approximately 80%, the introduction rate of silyl groups in the hydrosilylation reaction with a methallyl group is improved to 90 to 97%.

[0005] Furthermore, Patent Documents 2 and 3 describe hydrolyzable silyl group-containing polyoxyalkylene polymers in which the average ratio of hydrolyzable silyl groups located at molecular chain terminals to the number of molecular chain terminals is 85% or more. This polymer also achieves a silyl group introduction rate of 85% or more by subjecting a polymer having both methallyl groups and allyl groups to a hydrosilylation reaction.

[0006] On the other hand, Patent Document 4 reports that the hydrosilylation reaction of an allyl ether compound with a hydrosilane compound in the presence of a specific ruthenium complex can efficiently produce the corresponding silylated product. However, this method is limited to the production of silylated products having a molecular weight of 3,000 or less, and it has been shown that as the molecular weight of the silylated product increases, the rate of side reactions increases and the selectivity for the silylated product decreases.

[0007] International Publication No. WO 99 / 24489 International Publication No. WO 2022 / 163563 International Publication No. WO 2022 / 163562 JP 2021-11456 A

[0008] As described in Patent Documents 1 to 3, by utilizing a hydrosilylation reaction of methallyl groups, a silyl group introduction rate of 85% or more can be achieved, thereby increasing the strength after curing. However, the hydrolyzable silyl group-containing polymer obtained by hydrosilylation of methallyl groups tends to have a slower rate of hydrolysis and condensation reaction (curing reaction) of the hydrolyzable silyl groups than polymers obtained from allyl groups. This is presumably because the hydrolyzable silyl group-containing polymer obtained has a methyl group derived from the methallyl group near the silicon atom, which sterically hinders the hydrolysis and condensation reaction from proceeding.

[0009] Furthermore, Patent Document 4 reports that a corresponding silylated product can be efficiently produced by a hydrosilylation reaction of an allyl group, but the production of such a silylated product is limited to a molecular weight of 3,000 or less, making it difficult to achieve sufficient strength after curing.

[0010] As described above, it has been difficult for the previously reported hydrolyzable silyl group-containing polyoxyalkylene polymers to achieve both high strength after curing and curability.

[0011] In view of the above-mentioned current situation, an object of the present invention is to provide a hydrolyzable silyl group-containing polyoxyalkylene polymer that can achieve both high strength after curing and curability.

[0012] As a result of extensive investigations, the present inventors have succeeded in suppressing side reactions such as isomerization to 1-propenyl groups (internal olefins) and hydrogenation in a hydrosilylation reaction between an allyl group-containing polyoxyalkylene polymer and a hydrosilane compound, thereby achieving a high silyl group introduction rate, even when the allyl group-containing polyoxyalkylene polymer has a high molecular weight, and have found that the resulting high-molecular-weight hydrolyzable silyl group-containing polyoxyalkylene polymer has good curability and can exhibit high strength after curing, thereby completing the present invention.

[0013] That is, the present invention provides a compound of general formula (1):

[0014]

[0015] (wherein R may be the same or different and represent a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms; X may be the same or different and represent a hydroxyl group or a hydrolyzable group; and a represents 0, 1, or 2), a ratio of the number of hydrolyzable silyl group-containing structures represented by general formula (1) to the total number of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups measured on the polymer is 0.85 to 1.00, and the number average molecular weight of the polymer exceeds 3,000. The present invention also relates to a polymer mixture containing the polyoxyalkylene polymer (E) and a ruthenium complex (A). The present invention also relates to a curable composition containing the polyoxyalkylene polymer (E) or the polymer mixture. The present invention also relates to a curable composition containing a reinforcing filler in addition to the polyoxyalkylene polymer (E) or the polymer mixture, and a cured product obtained by curing the curable composition.

[0016] According to the present invention, it is possible to provide a hydrolyzable silyl group-containing polyoxyalkylene polymer that can achieve both high strength after curing and curability, and further to provide a polymer mixture or curable composition containing the polymer, and a cured product obtained by curing the curable composition.

[0017] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The polyoxyalkylene polymer (E) according to the present invention contains polymer molecules having a hydrolyzable silyl group-containing structure represented by the following general formula (1).

[0018]

[0019] The divalent group sandwiched between the oxygen atom and the silicon atom in the general formula (1) is —CH 2 -CH 2 -CH 2In general formula (1), the silicon atom is bonded to a trimethylene group having 3 carbon atoms, and the trimethylene group has no substituent. In this formula, the silicon atom is bonded to a trimethylene group having no substituent, so that there is little steric hindrance that would impede the condensation reaction, and the polyoxyalkylene polymer (E) according to this embodiment can achieve good curability. In addition, the trimethylene group has no unsaturated bond, so that the stability is good.

[0020] As will be described later, this trimethylene group is an allyl group (CH 2 =CH-CH 2 -) by hydrosilylation reaction. 2 =C(CH 3 )-CH 2 In the hydrosilylation reaction with the methyl group, a 4-carbon isobutylene group (-CH 2 -CH(CH 3 )-CH 2 -), the resulting hydrolyzable silyl group-containing structure is not that represented by general formula (1).

[0021] The polyoxyalkylene polymer (E) according to this embodiment is a polymer having a high proportion of hydrolyzable silyl group-containing structures represented by general formula (1). Specifically, the ratio of the number of hydrolyzable silyl group-containing structures represented by general formula (1) to the total number of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups measured for the polyoxyalkylene polymer (E) according to this embodiment is 0.85 or more and 1.00 or less. Such a high proportion of hydrolyzable silyl group-containing structures represented by general formula (1) improves the crosslink density in the cured product, thereby enabling high strength after curing to be achieved.

[0022] The "hydrolyzable silyl group" in the "total number of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups" is a concept that includes not only the hydrolyzable silyl group-containing structure represented by general formula (1) but also hydrolyzable silyl group-containing structures not represented by general formula (1).

[0023] The polyoxyalkylene polymer (E) according to the present embodiment may contain, in addition to the hydrolyzable silyl group-containing structure represented by general formula (1), a hydrolyzable silyl group-containing structure not represented by general formula (1). However, it is preferable that the polyoxyalkylene polymer (E) does not contain a hydrolyzable silyl group-containing structure not represented by general formula (1).

[0024] The higher the ratio of the hydrolyzable silyl group-containing structure represented by general formula (1), the better, and it is preferably 0.90 or more, more preferably 0.95 or more, even more preferably 0.97 or more, and most preferably 0.98 or more.

[0025] The polyoxyalkylene polymer (E) according to this embodiment can be produced by subjecting an allyl group-containing polyoxyalkylene polymer to a hydrosilylation reaction with a hydrosilane compound. In this hydrosilylation reaction, a 1-propenyl group (internal olefin) may be generated by isomerization of the allyl group, or a propyl group may be generated by hydrogenation of the allyl group. Furthermore, the allyl group may remain unreacted. As a result, the resulting hydrolyzable silyl group-containing polyoxyalkylene polymer may have at least one of a 1-propenyl group, a propyl group, and an allyl group in addition to the hydrolyzable silyl group-containing structure represented by general formula (1). The polyoxyalkylene polymer (E) according to this embodiment is a polymer in which the formation of the 1-propenyl group, the propyl group, and the allyl group is suppressed, and the proportion of the hydrolyzable silyl group-containing structure represented by general formula (1) is controlled to be highly concentrated.

[0026] In the hydrosilylation reaction of a methallyl group-containing polymer as described in Patent Document 1, a high silyl group introduction rate can be achieved. However, the hydrolyzable silyl group-containing structure derived from the methallyl group formed in this reaction is not represented by general formula (1). Therefore, as shown in the comparative examples described later, the proportion of the hydrolyzable silyl group-containing structure represented by general formula (1) cannot reach 0.85 or more.

[0027] Furthermore, a high silyl group introduction rate can be achieved by a hydrosilylation reaction of a polymer having both a methallyl group and an allyl group as described in Patent Documents 2 and 3. However, this reaction also results in the formation of a hydrolyzable silyl group-containing structure derived from the methallyl group and not represented by general formula (1), and the proportion of the hydrolyzable silyl group-containing structure represented by general formula (1) cannot reach 0.85 or more. Therefore, Patent Documents 1 to 3 do not disclose polymers in which the proportion of the hydrolyzable silyl group-containing structure represented by general formula (1) is 0.85 or more.

[0028] The ratio of the number of hydrolyzable silyl group-containing structures represented by general formula (1) to the total number of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups is 1 The silyl groups can be determined by H NMR based on the integral values ​​of the signals corresponding to each group. For example, a polyoxyalkylene polymer having a hydrolyzable silyl group is dissolved in deuterated chloroform, 1 When H NMR measurement is performed, the peaks of the hydrolyzable silyl group, 1-propenyl group, propyl group, and allyl group can be clearly distinguished. For example, in the case of a 3-(dimethoxymethylsilyl)propyloxy group, which is an example of a hydrolyzable silyl group-containing structure represented by general formula (1), a peak derived from two protons is observed near 0.6 ppm. In addition, in the case of a 1-propenyl group, multiple peaks derived from one proton are observed near 5.9 to 6.3 ppm. In addition, in the case of a propyl group, a peak derived from three protons is observed near 0.9 ppm. In addition, in the case of an allyl group, two peaks derived from two protons are observed near 5.1 to 5.3 ppm. The ratio can be determined based on the integral values ​​of these peaks.

[0029] The polyoxyalkylene polymer (E) according to this embodiment is mainly composed of polyoxyalkylene polymer molecules having a hydrolyzable silyl group-containing structure represented by general formula (1). The polymer molecules may further have a group selected from the group consisting of a 1-propenyl group, a propyl group, and an allyl group. The polyoxyalkylene polymer (E) according to this embodiment may be composed only of the above polymer molecules, or may further contain other polymer molecules such as those listed below, as long as the proportion of the hydrolyzable silyl group-containing structure represented by general formula (1) measured for the entire polymer is satisfied. - Polyoxyalkylene polymer molecules that do not have a hydrolyzable silyl group-containing structure represented by general formula (1) and have a hydrolyzable silyl group-containing structure not represented by general formula (1) - Polyoxyalkylene polymer molecules that do not have a hydrolyzable silyl group and have a group selected from the group consisting of a 1-propenyl group, a propyl group, and an allyl group

[0030] The oxygen atom on the left side in general formula (1) is bonded to the polymer skeleton of the polyoxyalkylene polymer. The bonding position of the hydrolyzable silyl group-containing structure represented by general formula (1) to the polymer skeleton is not particularly limited, and it may be bonded to the end of the polymer skeleton, or to the polymer skeleton other than the end, or may be bonded to both. When the polyoxyalkylene polymer (E) according to this embodiment is used as a curable resin for adhesives, sealing materials, elastic coating agents, pressure-sensitive adhesives, etc., it is preferable that the hydrolyzable silyl group-containing structure represented by general formula (1) is bonded to at least the end of the polymer skeleton. Moreover, the hydrolyzable silyl group-containing structure represented by general formula (1) may be bonded only to the end of the polymer skeleton.

[0031] R in general formula (1) represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. When general formula (1) contains multiple Rs, they may be the same or different. The hydrocarbon group may be saturated or unsaturated, and may be aliphatic, alicyclic, or aromatic. The hydrocarbon group preferably has 1 to 10 carbon atoms, more preferably 1 to 8 carbon atoms, even more preferably 1 to 6 carbon atoms, even more preferably 1 to 3 carbon atoms, and particularly preferably 1 or 2 carbon atoms. When the hydrocarbon group has a substituent, the substituent is not particularly limited, and examples thereof include halogeno groups such as a chloro group, alkoxy groups such as a methoxy group, and amino groups such as an N,N-diethylamino group.

[0032] Examples of R include unsubstituted alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-hexyl, 2-ethylhexyl, and n-dodecyl; substituted alkyl groups such as chloromethyl, methoxymethyl, and N,N-diethylaminomethyl; unsaturated hydrocarbon groups such as vinyl, isopropenyl, and allyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, toluoyl, and 1-naphthyl; and aralkyl groups such as benzyl. A substituted or unsubstituted alkyl group is preferred, and a methyl group, an ethyl group, a chloromethyl group, or a methoxymethyl group is more preferred, and a methyl group or a methoxymethyl group is particularly preferred. When a plurality of Rs are present, they may be the same or different.

[0033] X in general formula (1) represents a hydroxyl group or a hydrolyzable group. When general formula (1) contains multiple Xs, they may be the same or different. The hydrolyzable group is not particularly limited and may be a known hydrolyzable group, such as a hydrogen atom, a halogen atom, an alkoxy group, an acyloxy group, a ketoximate group, an amino group, an amide group, an acid amide group, an aminooxy group, a mercapto group, or an alkenyloxy group. Among these, an alkoxy group, an acyloxy group, a ketoximate group, and an alkenyloxy group are preferred. Because of their mild hydrolysis and ease of handling, an alkoxy group is more preferred, a methoxy group and an ethoxy group are even more preferred, and a methoxy group is particularly preferred. When multiple Xs are present, they may be the same or different.

[0034] In the general formula (1), a represents 0, 1, or 2. From the viewpoint of curability, a is preferably 0 or 1.

[0035] -SiR in general formula (1) a X 3-aSpecific examples include, but are not limited to, trimethoxysilyl, triethoxysilyl, tris(2-propenyloxy)silyl, triacetoxysilyl, dimethoxymethylsilyl, diethoxymethylsilyl, dimethoxyethylsilyl, (chloromethyl)dimethoxysilyl, (chloromethyl)diethoxysilyl, (methoxymethyl)dimethoxysilyl, (methoxymethyl)diethoxysilyl, (N,N-diethylaminomethyl)dimethoxysilyl, and (N,N-diethylaminomethyl)diethoxysilyl. Of these, dimethoxymethylsilyl, trimethoxysilyl, triethoxysilyl, and (methoxymethyl)dimethoxysilyl are preferred because they provide cured products with good mechanical properties. From the viewpoint of activity, trimethoxysilyl group, (chloromethyl)dimethoxysilyl group, and (methoxymethyl)dimethoxysilyl group are more preferred, and trimethoxysilyl group and (methoxymethyl)dimethoxysilyl group are particularly preferred. From the viewpoint of stability, dimethoxymethylsilyl group and triethoxysilyl group are more preferred, and dimethoxymethylsilyl group is particularly preferred.

[0036] The number of hydrolyzable silyl group-containing structures represented by general formula (1) contained in one molecule of the polyoxyalkylene polymer (E) according to this embodiment is, from the viewpoint of strength after curing, preferably 0.85 or more, more preferably 1.7 or more, even more preferably 1.8 or more, and particularly preferably 1.9 or more on average. There is no particular upper limit, but it is preferably 5 or less, more preferably 4 or less, and even more preferably 3 or less.

[0037] The polyoxyalkylene polymer (E) according to this embodiment has a polyoxyalkylene polymer skeleton. The polymer skeleton is preferably a polymer skeleton composed solely of a plurality of oxyalkylene repeating units linked together, or a polymer skeleton composed solely of the plurality of oxyalkylene repeating units and a structure derived from the initiator used during polymerization. Here, the oxyalkylene repeating unit refers to a repeating unit constituting a polyether, such as an oxyalkylene unit having 2 to 6 carbon atoms, preferably 2 to 4 carbon atoms.

[0038] The polymer skeleton may be linear or branched. A linear polymer skeleton is preferred in that the cured product of the curable composition has high elongation, and a branched polymer skeleton is preferred in that the cured product of the curable composition has high strength. A linear polymer skeleton can be formed by using an initiator having one or two hydroxyl groups per molecule in the polymerization method for forming the polymer skeleton, and a branched polymer skeleton can be formed by using an initiator having three or more hydroxyl groups per molecule. Furthermore, a polymer having a linear polymer skeleton and a polymer having a branched polymer skeleton may be used in combination.

[0039] Specific examples of the polyoxyalkylene polymer backbone include, but are not limited to, polyoxyethylene, polyoxypropylene, polyoxybutylene, polyoxytetramethylene, polyoxyethylene-polyoxypropylene copolymer, polyoxypropylene-polyoxybutylene copolymer, etc. Polyoxypropylene is preferred. As the polymer backbone, only one type may be used, or two or more types may be used in combination.

[0040] When the polyoxyalkylene polymer (E) according to the present embodiment is used as a curable resin for a sealant, adhesive, or the like, a polyoxypropylene polymer having oxypropylene repeating units in an amount of 50% by weight or more, more preferably 80% by weight or more, of the polymer skeleton is preferred because it is amorphous and has a relatively low viscosity.

[0041] The polyoxyalkylene polymer (E) according to this embodiment has a number average molecular weight, as measured by GPC and converted into polystyrene, of more than 3,000. Because of this relatively high molecular weight, the polymer can exhibit good mechanical properties after curing, such as higher tensile strength at break and tensile elongation at break, and can be suitably used as a curable resin for adhesives, sealing materials, elastic coating agents, pressure-sensitive adhesives, and the like.

[0042] The number average molecular weight is preferably 5,000 or more, more preferably 10,000 or more, and even more preferably 20,000 or more. There is no particular upper limit to the number average molecular weight, but from the perspective of ease of handling, it is preferably 100,000 or less, more preferably 60,000 or less, and even more preferably 40,000 or less.

[0043] The molecular weight distribution (Mw / Mn) of the polyoxyalkylene polymer (E) according to this embodiment is not particularly limited. The molecular weight distribution is preferably narrow, preferably less than 2.0, more preferably 1.6 or less, even more preferably 1.5 or less, even more preferably 1.4 or less, and most preferably 1.2 or less. The molecular weight distribution of the polyoxyalkylene polymer (E) can be determined from the number average molecular weight and weight average molecular weight obtained by GPC measurement.

[0044] <Method for producing polyoxyalkylene polymer (E) according to this embodiment> Next, a specific example of a method for producing the polyoxyalkylene polymer (E) according to this embodiment will be described in detail, but the method for producing the polyoxyalkylene polymer (E) is not limited to the following description.

[0045] (Polymerization) The polymer backbone of the polyoxyalkylene polymer can be formed by a conventionally known method by ring-opening polymerization of a cyclic ether compound in the presence of an initiator using a polymerization catalyst, thereby obtaining a hydroxyl-terminated polyoxyalkylene polymer (F). Although the specific polymerization method is not particularly limited, a polymerization method using a composite metal cyanide complex catalyst such as a zinc hexacyanocobaltate glyme complex is preferred because it produces a hydroxyl-terminated polymer with a narrow molecular weight distribution (Mw / Mn).

[0046] Examples of cyclic ether compounds include ethylene oxide, propylene oxide, butylene oxide, tetramethylene oxide, and tetrahydrofuran. These cyclic ether compounds may be used alone or in combination of two or more. Among the cyclic ether compounds, propylene oxide is particularly preferred because it can produce an amorphous polyoxyalkylene polymer with a relatively low viscosity.

[0047] The initiator having a hydroxyl group is not particularly limited, and examples thereof include alcohols such as butanol, ethylene glycol, propylene glycol, propylene glycol monoalkyl ether, butanediol, hexamethylene glycol, neopentyl glycol, diethylene glycol, dipropylene glycol, triethylene glycol, glycerin, trimethylolmethane, trimethylolpropane, pentaerythritol, and sorbitol; and hydroxyl group-terminated polyoxyalkylene polymers having a number average molecular weight of 300 to 4,000, such as polyoxypropylene diol, polyoxypropylene triol, polyoxyethylene diol, and polyoxyethylene triol.

[0048] Examples of synthesis methods for polyoxyalkylene polymers include, but are not limited to, polymerization methods using an alkali catalyst such as KOH, polymerization methods using a transition metal compound-porphyrin complex catalyst such as the complex obtained by reacting an organoaluminum compound with porphyrin disclosed in JP-A-61-215623, polymerization methods using a composite metal cyanide complex catalyst disclosed in JP-B-46-27250, JP-B-59-15336, U.S. Pat. Nos. 3,278,457, 3,278,458, 3,278,459, 3,427,256, 3,427,334, and 3,427,335, polymerization methods using a catalyst made of a polyphosphazene salt exemplified in JP-A-10-273512, and polymerization methods using a catalyst made of a phosphazene compound exemplified in JP-A-11-060722. A polymerization method using a composite metal cyanide complex catalyst is more preferred for reasons such as production costs and the fact that a polymer with a narrow molecular weight distribution can be obtained.

[0049] (Reaction with Alkali Metal Salt) When introducing allyl groups into the hydroxyl-terminated polyoxyalkylene polymer (F), it is preferable to first react the hydroxyl-terminated polyoxyalkylene polymer (F) with an alkali metal salt to convert the terminal hydroxyl groups into alkoxides. Alternatively, a double metal cyanide complex catalyst can be used instead of the alkali metal salt.

[0050] The alkali metal salt is not particularly limited, and examples thereof include sodium hydroxide, sodium alkoxide, potassium hydroxide, potassium alkoxide, lithium hydroxide, lithium alkoxide, cesium hydroxide, and cesium alkoxide. In view of ease of handling and solubility, sodium hydroxide, sodium methoxide, sodium ethoxide, sodium tert-butoxide, potassium hydroxide, potassium methoxide, potassium ethoxide, and potassium tert-butoxide are preferred, with sodium methoxide and sodium tert-butoxide being more preferred. In view of availability, sodium methoxide is particularly preferred, and in view of reactivity, sodium tert-butoxide is particularly preferred. The alkali metal salt may be subjected to the reaction in a state dissolved in a solvent.

[0051] The amount of the alkali metal salt used is not particularly limited, but the molar ratio to the hydroxyl groups of the hydroxyl-terminated polyoxyalkylene polymer (F) is preferably 0.5 or more, more preferably 0.6 or more, even more preferably 0.7 or more, and even more preferably 0.8 or more, and the molar ratio is preferably 1.2 or less, more preferably 1.1 or less.

[0052] The alkali metal salt is used to convert the hydroxyl groups of the hydroxyl-terminated polyoxyalkylene polymer (F) into alkoxides, and in order to efficiently proceed with this conversion reaction, it is preferable to remove water and substances having hydroxyl groups other than the polyoxyalkylene polymer from the reaction system in advance. For removal, any known method may be used, such as thermal evaporation, reduced pressure devolatilization, spray evaporation, thin film evaporation, azeotropic devolatilization, etc.

[0053] The temperature for reacting the alkali metal salt can be appropriately set by those skilled in the art, but is preferably from 50° C. to 150° C., more preferably from 110° C. to 145° C. The time for reacting the alkali metal salt is preferably from 10 minutes to 5 hours, more preferably from 30 minutes to 3 hours.

[0054] (Reaction with an organic halide (H) having an allyl group) After reacting an alkali metal salt with the hydroxyl-terminated polyoxyalkylene polymer (F) as described above, the polymer is reacted with an organic halide (H) having an allyl group. The organic halide (H) having an allyl group reacts with the alkoxide through a halogen substitution reaction to form an ether bond, thereby introducing an allyl group into the molecular chain terminal of the polyoxyalkylene polymer. This allows the formation of a polyoxyalkylene polymer (C) having an allyl group.

[0055] Specific examples of the organic halide (H) having an allyl group include, but are not limited to, allyl chloride, allyl bromide, allyl iodide, etc. Allyl chloride is preferred from the viewpoint of ease of handling.

[0056] The amount of the organic halide (H) having an allyl group to be added is not particularly limited, but the molar ratio of the organic halide (H) to the hydroxyl groups of the polyoxyalkylene polymer (F) is preferably 0.7 or more, more preferably 1.0 or more, and the molar ratio is preferably 5.0 or less, more preferably 2.0 or less.

[0057] The temperature when reacting the organic halide (H) having an allyl group is preferably from 50° C. to 150° C., more preferably from 110° C. to 140° C. The reaction time is preferably from 10 minutes to 5 hours, more preferably from 30 minutes to 3 hours.

[0058] (Introduction of Hydrolyzable Silyl Group) The polyoxyalkylene polymer (C) having an allyl group obtained as described above is subjected to a hydrosilylation reaction with a hydrosilane compound (D) having a hydrolyzable silyl group, whereby a hydrolyzable silyl group-containing structure represented by general formula (1) can be introduced into the polymer.

[0059] The hydrosilylation catalyst that can be used in this case is not particularly limited, and examples thereof include metals such as iron, cobalt, nickel, iridium, platinum, palladium, rhodium, and ruthenium, as well as complexes thereof. However, by carrying out the hydrosilylation reaction in the presence of a ruthenium complex (A), in particular, it is possible to produce a polyoxyalkylene polymer (E) according to this embodiment having a high proportion of the hydrolyzable silyl group-containing structure represented by general formula (1).

[0060] <Hydrosilane Compound (D)> The hydrosilane compound (D) is not particularly limited, but preferably has a structure represented by formula (2): HSiR a X 3-a (2)

[0061] In general formula (2), R, X, and a are as described above in relation to general formula (1). Specific examples of such hydrosilane compound (D) include trimethoxysilane, triethoxysilane, triphenoxysilane, tris(2-propenyloxy)silane, triacetoxysilane, dimethoxymethylsilane, diethoxymethylsilane, dimethoxyethylsilane, (chloromethyl)dimethoxysilane, (chloromethyl)diethoxysilane, (methoxymethyl)dimethoxysilane, (methoxymethyl)diethoxysilane, (N,N-diethylaminomethyl)dimethoxysilane, and (N,N-diphenylsilane). Examples of such silanes include (ethylaminomethyl)diethoxysilane, diphenoxymethylsilane, methylsilane, dimethylsilane, trimethylsilane, ethylsilane, diethylsilane, triethylsilane, methyldiethylsilane, dimethylethylsilane, chlorodimethylsilane, dichloromethylsilane, phenylsilane, diphenylsilane, triphenylsilane, phenylmethylsilane, phenyldimethylsilane, diphenylmethylsilane, ethylphenylsilane, diethylphenylsilane, and ethyldiphenylsilane.

[0062] From the viewpoint of the curability and post-curing strength of the polyoxyalkylene polymer (E) according to this embodiment, trimethoxysilane and dimethoxymethylsilane are particularly preferred as the hydrosilane compound (D).

[0063] The amount of the hydrosilane compound (D) used (charged) is, in terms of the amount of substance, preferably 1 molar equivalent or more, more preferably 3 molar equivalents or more, and more preferably 5 molar equivalents or more, relative to the allyl groups in the allyl group-containing polyoxyalkylene polymer (C). The amount is usually 20 molar equivalents or less, and preferably 10 molar equivalents or less. Within this range, the viscosity of the resulting polyoxyalkylene polymer can be kept low, and a polyoxyalkylene polymer (E) with good workability can be obtained.

[0064] <Ruthenium Complex (A)> The ruthenium complex (A) is a ruthenium complex having the compound (B) as a ligand. Compared with known hydrosilylation catalysts such as Karstedt's catalyst (platinum divinyldisiloxane complex), the ruthenium complex (A) exhibits high selectivity as a catalyst for the hydrosilylation reaction of an allyl group-containing polyoxyalkylene polymer with a hydrosilane compound, suppresses the by-production of 1-propenyl groups or propyl groups, and enables efficient production of a polyoxyalkylene polymer (E) having a high proportion of the hydrolyzable silyl group-containing structure represented by general formula (1) and a number-average molecular weight of more than 3,000.

[0065] The specific type of ruthenium complex (A) is not particularly limited, except that it has compound (B) as a ligand. The type of compound (B) that the ruthenium complex (A) has as a ligand may be one type or two or more types.

[0066] Ruthenium complex (A) can be produced by a method similar to a known production method. Examples of raw materials for ruthenium complex (A) include anhydrides and hydrates of compounds selected from ruthenium chloride (III), ruthenium bromide (III), and ruthenium iodide (III). A specific production method for ruthenium complex (A) is, for example, to add compound (B) to an ethanol solution of ruthenium chloride (III) hydrate, heat reflux, filter, and then dry. When ruthenium chloride (III) hydrate is used as the raw material, heating reflux may be performed in the presence of a basic compound such as sodium carbonate or sodium bicarbonate to neutralize the hydrogen chloride generated during heating reflux. When reacting ruthenium chloride (III) hydrate with compound (B), it is preferable to use 1 molar equivalent or more of compound (B) relative to the raw ruthenium compound from the viewpoint of reaction rate.

[0067] The ruthenium complex (A) may be a nanoparticle catalyst. The particle size (cumulative median diameter) of the nanoparticles of the ruthenium complex (A) is not particularly limited as long as the hydrosilylation reaction proceeds to the desired extent. The particle size is preferably 0.3 nm or more and 200 nm or less. The lower limit of the particle size is more preferably 0.5 nm or more, and even more preferably 1 nm or more. The upper limit of the particle size is more preferably 100 nm or less, even more preferably 50 nm or less, and particularly preferably 10 nm or less. The cumulative median diameter can be measured using a transmission electron microscope (TEM).

[0068] Ruthenium complex (A) may have, as a ligand, compound (B) as well as compound (B') which does not fall under compound (B). Compound (B') is a compound which can be coordinated to ruthenium complex (A) and does not fall under compound (B). Examples of compound (B') which can serve as a ligand include a 2,5-norbornadiene ligand, a 1,5-cyclooctadiene ligand, a p-cymene ligand, a mesitylene ligand, a benzene ligand, a carbonyl ligand, an isocyanide ligand, and an arene ligand.

[0069] When ruthenium complex (A) has both compound (B) and compound (B') as ligands, it is preferable that the proportion of compound (B) in all ligands of ruthenium complex (A) is as high as possible, since this can provide better selectivity. The proportion of compound (B) in all ligands is preferably 1 to 100 mol%, more preferably 50 to 100 mol%, even more preferably 70 to 100 mol%, and even more preferably 90 to 100 mol%.

[0070] Ruthenium complex (A) having compound (B) as a ligand can also be obtained by adding compound (B) to a system containing ruthenium compound (A') that does not have compound (B) as a ligand, thereby converting ruthenium compound (A') into ruthenium complex (A), by the method described below.

[0071] <Compound (B)> Compound (B), which is a ligand of ruthenium complex (A), is a compound that can be coordinated to a ruthenium complex. Compound (B) has at least one carbon-carbon double bond in one molecule, and an electron-withdrawing group is bonded to at least one of the carbon atoms forming the carbon-carbon double bond.

[0072] Examples of the basic skeleton containing a carbon-carbon double bond in compound (B) include a norbornadiene skeleton, a cyclooctadiene skeleton, a benzene ring skeleton, a benzoquinone skeleton, etc. More specific examples include a 2,5-norbornadiene skeleton, a 1,5-cyclooctadiene skeleton, a p-cymene skeleton, a mesitylene skeleton, a benzene ring skeleton, a benzoquinone skeleton, etc. A norbornadiene skeleton or a benzene ring skeleton is preferred.

[0073] Examples of the electron-withdrawing group include halogeno groups such as a fluoro group, a chloro group, a bromo group, and an iodo group, as well as a cyano group, an aldehyde group, and a nitro group. When a single molecule contains multiple electron-withdrawing groups, the electron-withdrawing groups may be different types. Compound (B) may contain one or more electron-withdrawing groups in a single molecule, but preferably contains two or more, more preferably two to four, and particularly preferably two or three.

[0074] Furthermore, the type of electron-withdrawing group is preferably a halogeno group, more preferably a fluoro group, a bromo group, or an iodo group, even more preferably a bromo group or an iodo group, and particularly preferably a bromo group. In particular, compound (B) preferably has one or more electron-withdrawing groups selected from a fluoro group, a bromo group, and an iodo group per molecule, more preferably two or more. Furthermore, compound (B) preferably has one or more electron-withdrawing groups selected from a bromo group and an iodo group per molecule. In this case, compound (B) may further have a fluoro group in addition to a bromo group and / or an iodo group. These electron-withdrawing groups are preferably directly bonded to the carbon atom forming the carbon-carbon double bond of compound (B). In particular, when compound (B) has a benzene ring skeleton, these electron-withdrawing groups are preferably directly bonded to the benzene ring.

[0075] The structure of compound (B) is a combination of the above-described basic skeleton and an electron-withdrawing group. The specific type of compound (B) is not particularly limited, and examples thereof include 2-bromonorbornadiene, 2,3-dibromonorbornadiene, 1,4-dibromobenzene and its structural isomers, 1-bromo-4-iodobenzene and its structural isomers, 1,3,5-tribromobenzene and its structural isomers, 1,2,4,5-tetrabromobenzene and its structural isomers, hexabromobenzene, 1-bromo-3,5-difluorobenzene and its structural isomers, 1-bromo-3,5-dichlorobenzene and its structural isomers, 1-bromo-3,5-diiodobenzene and its structural isomers, 1-bromo-3-chloro-5-fluorobenzene and its structural isomers, 1,4-diiodobenzene and its structural isomers, 1,3,5-triiodobenzene and its structural isomers, 1,2 , 4,5-tetraiodobenzene and its structural isomers, hexaiodobenzene, 1,3-difluoro-5-iodobenzene and its structural isomers, 1,3-dichloro-5-iodobenzene and its structural isomers, 1,3-dibromo-5-iodobenzene and its structural isomers, 1,3-dibromo-5-chlorobenzene and its structural isomers, 1-chloro-3,5-diiodobenzene and its structural isomers, 1-fluoro-3,5-dibromobenzene and its structural isomers, 1-fluoro-3,5-diiodobenzene and its structural isomers, 1-chloro-3-fluoro-5-iodobenzene and its structural isomers, 1-bromo-3-chloro-5-iodobenzene and its structural isomers, 1-bromo-3-fluoro-5-iodobenzene and its structural isomers. Among these, from the viewpoint of suppressing by-products, compound (B) is preferably 2,3-dibromonorbornadiene, 1,4-dibromobenzene, 1-bromo-3,5-difluorobenzene, 1-bromo-2,6-difluorobenzene, 1,3,5-tribromobenzene, 1,4-diiodobenzene, or hexabromobenzene, and particularly preferably 2,3-dibromonorbornadiene, 1,4-dibromobenzene, 1-bromo-3,5-difluorobenzene, 1-bromo-2,6-difluorobenzene, 1,4-diiodobenzene, or 1,3,5-tribromobenzene.As the compound (B), one type may be used alone, or two or more types may be used in combination.

[0076] The amount of the ruthenium complex (A) used (charged amount) is, in weight ratio relative to the allyl group-containing polyoxyalkylene polymer (C), usually 0.01 ppm or more, preferably 0.1 ppm or more, more preferably 1 ppm or more, and usually 10% or less, preferably 1% or less, more preferably 0.1% or less. Within this range, hydrolyzable silyl groups can be introduced with high efficiency.

[0077] The hydrosilylation reaction may be carried out in the presence of a solvent or without a solvent. When a solvent is used, the type of solvent is not particularly limited, and it is preferably a compound that does not react with the raw materials or catalyst. Specific examples include hydrocarbon solvents such as hexane, and halogenated solvents such as dichloromethane. The solvent is preferably dehydrated and deoxygenated before use.

[0078] The reaction temperature for the hydrosilylation reaction can be determined appropriately taking into consideration the reactivity (reaction rate) and the heat resistance temperature of the reaction vessel, but is usually 0°C or higher, preferably 20°C or higher, more preferably 40°C or higher, and usually 200°C or lower, preferably 150°C or lower. A higher reaction temperature may result in the reaction being completed in a shorter time and side reactions being more effectively suppressed. The reaction time is also not particularly limited and may be about 5 minutes to 12 hours, or about 10 minutes to 5 hours.

[0079] The hydrosilylation reaction is preferably carried out in an inert atmosphere such as nitrogen or argon.

[0080] In the hydrosilylation reaction, in addition to adding a ruthenium complex (A) to the reaction system, further adding and mixing a compound (B) can improve the proportion of the hydrolyzable silyl group-containing structure represented by general formula (1), which is preferable. One possible cause of the improvement in the silyl group proportion is that, for example, when the amount of compound (B) used in the synthesis of the ruthenium complex (A) is insufficient and ruthenium chloride (III) is partially contained in the ruthenium complex (A), the ruthenium chloride (III) reacts with the added compound (B) to convert it to the ruthenium complex (A). Therefore, it is preferable that the ruthenium complex (A) and the compound (B) come into contact with each other before the start of the hydrosilylation reaction. For example, one preferred embodiment includes a method in which the ruthenium complex (A) and the compound (B) are added and mixed while stirring the allyl group-containing polyoxyalkylene polymer (C) charged in a reaction vessel at a predetermined temperature, and then the hydrosilane compound (D) is added. The time interval between the addition of the ruthenium complex (A) and the compound (B) and the addition of the hydrosilane compound (D) is not particularly limited and may be appropriately determined in consideration of the desired silyl group ratio, the time required for production, and the like.

[0081] In another embodiment, the polyoxyalkylene polymer (E) according to the present embodiment can also be produced by mixing a polyoxyalkylene polymer (C) having an allyl group, a hydrosilane compound (D), a ruthenium compound (A′) not having the compound (B) as a ligand, and the compound (B), followed by a hydrosilylation reaction.

[0082] According to this embodiment, unlike the above-described production method, a pre-synthesized ruthenium complex (A) is not used; instead, the ruthenium compound (A') and the compound (B) are mixed in a reaction vessel to form the ruthenium complex (A) in the system, which then functions as a catalyst, thereby efficiently producing the hydrolyzable silyl group-containing polyoxyalkylene polymer (E). The allyl group-containing polyoxyalkylene polymer (C), the hydrosilane compound (D), and the compound (B) are as described above. The order of mixing the allyl group-containing polyoxyalkylene polymer (C), the hydrosilane compound (D), the ruthenium compound (A'), and the compound (B) is not particularly limited, and they can be mixed in any order.

[0083] <Ruthenium Compound (A')> The ruthenium compound (A') is not particularly limited except that it does not have compound (B) as a ligand. As the ruthenium compound (A'), ruthenium(III) chloride hydrate and a ruthenium complex having compound (B') as a ligand that does not fall under compound (B) can be used. Examples of types of compound (B') include a 2,5-norbornadiene ligand, a 1,5-cyclooctadiene ligand, a p-cymene ligand, a mesitylene ligand, a benzene ligand, a carbonyl ligand, an isocyanide ligand, and an arene ligand.

[0084] From the viewpoint of suppressing by-products, the ruthenium compound (A') is preferably a ruthenium complex having a ligand selected from a 2,5-norbornadiene ligand, a benzene ligand, and a p-cymene ligand.

[0085] The preferred conditions for the amount (charge amount) of the hydrosilane compound (D) used in the reaction step, the type of solvent used in the reaction step, and the reaction temperature are the same as those described above. The preferred amount (charge amount) of the ruthenium compound (A') used is the same as the above-mentioned amount (charge amount) of the ruthenium complex (A). This production method includes a step of mixing the ruthenium compound (A') and the compound (B) in a reaction vessel to produce the ruthenium complex (A) in the system. Therefore, for example, it is preferred to add the ruthenium compound (A') and the compound (B) to the allyl group-containing polyoxyalkylene polymer (C) charged in the reaction vessel while stirring at a predetermined temperature, and then add the hydrosilane compound (D). The time interval between the addition of the ruthenium compound (A') and the compound (B) and the addition of the hydrosilane compound (D) is not particularly limited and may be determined appropriately taking into account the desired introduction rate of silyl groups and the production time.

[0086] The amount of compound (B) added is not particularly limited, and is usually 0.01 ppm or more, preferably 0.1 ppm or more, more preferably 1 ppm or more, and usually 10% or less, preferably 1% or less, more preferably 0.1% or less, by weight, relative to the allyl group-containing polyoxyalkylene polymer (C).

[0087] When the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment is produced by the production method described above, a polymer mixture containing the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) and the ruthenium complex (A) can be obtained.

[0088] In the polymer mixture, the content of the ruthenium complex (A) corresponds to the amount (charge amount) of the ruthenium complex (A) or ruthenium compound (A') used. Specifically, the content of the ruthenium complex (A) is usually 0.01 ppm or more, preferably 0.1 ppm or more, and more preferably 1 ppm or more, by weight, relative to the hydrolyzable silyl group-containing polyoxyalkylene polymer (E), and is usually 10% or less, preferably 1% or less, and more preferably 0.1% or less.

[0089] <Curable Composition> The hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment and a polymer mixture containing the polymer (E) can constitute a curable composition. In addition, a cured product can be obtained by curing the curable composition.

[0090] (Polyoxyalkylene Polymer (E')) The curable composition according to this embodiment may contain, in addition to the polyoxyalkylene polymer (E), another hydrolyzable silyl group-containing polyoxyalkylene polymer (E') that does not meet the definition of polymer (E). Particularly preferred examples of such polymer (E') include polymers that contain polyoxyalkylene polymer molecules having a hydrolyzable silyl group-containing structure represented by the general formula (1), and in which the ratio of the number of hydrolyzable silyl group-containing structures represented by the general formula (1) to the total number of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups measured for the polymer (E') is 0.05 or more and less than 0.85. By incorporating such a polymer (E'), a cured product with good curability and low modulus can be formed. A curable composition that gives a cured product with a low modulus, i.e., high flexibility, is particularly suitable for use as a sealant.

[0091] The polyoxyalkylene polymer (E′) is similar to the polyoxyalkylene polymer (E), except that the number average molecular weight is not limited to more than 3,000 and the ratio of the hydrolyzable silyl group-containing structure represented by general formula (1) is 0.05 or more and less than 0.85.

[0092] The main chain structure of the polyoxyalkylene polymer (E') may be linear or branched. In order to provide a curable composition with excellent curability and a cured product with a low modulus, it is preferred that the polyoxyalkylene polymer (E') has the hydrolyzable silyl group-containing structure at only one end of the linear main chain.

[0093] The number average molecular weight of the polyoxyalkylene polymer (E') is not particularly limited, but is preferably at least 800. The upper limit of the number average molecular weight of the polyoxyalkylene polymer (E') is not particularly limited, but is preferably less than 20,000, more preferably less than 10,000. From the viewpoint of reducing the viscosity of the curable composition and providing an easy-to-handle curable composition, the number average molecular weight of the polyoxyalkylene polymer (E') is preferably smaller than the number average molecular weight of the polyoxyalkylene polymer (E).

[0094] A preferred combination of the polyoxyalkylene polymer (E) and the polyoxyalkylene polymer (E') is a combination of a polyoxyalkylene polymer (E) having a number average molecular weight of 20,000 or more and 100,000 or less and a polyoxyalkylene polymer (E') having a number average molecular weight of 800 or more and less than 20,000.

[0095] In the polyoxyalkylene polymer (E'), the ratio of the number of hydrolyzable silyl group-containing structures represented by general formula (1) to the total number of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups is 0.05 or more and less than 0.85, preferably 0.10 or more and less than 0.85, more preferably 0.30 or more and less than 0.85, still more preferably 0.50 or more and less than 0.85, and particularly preferably 0.70 or more and less than 0.85.

[0096] The method for producing the polyoxyalkylene polymer (E') is not particularly limited as long as the ratio of the number of hydrolyzable silyl group-containing structures represented by general formula (1) falls within the above-mentioned range. The polyoxyalkylene polymer (E') can be produced by a hydrosilylation reaction between an allyl group-containing polyoxyalkylene polymer (C) and a hydrosilane compound (D), similarly to the polyoxyalkylene polymer (E), except that the production conditions are appropriately adjusted so that the ratio of the number of hydrolyzable silyl group-containing structures represented by general formula (1) falls within the above-mentioned range.

[0097] For example, by adjusting the amount of the hydrosilane compound (D) used, the amount of remaining allyl groups can be adjusted, and the proportion of the number of hydrolyzable silyl group-containing structures represented by general formula (1) can be controlled.

[0098] Furthermore, when hydrosilylation is carried out in the presence of a platinum catalyst, such as a Karstedt catalyst, the value of the ratio of the number of hydrolyzable silyl group-containing structures represented by general formula (1) can be increased and the amount of remaining allyl groups can be reduced, within the range of 0.10 or more and less than 0.85. Specific examples of platinum catalysts include catalysts in which platinum is supported on a carrier such as alumina, silica, or carbon black; chloroplatinic acid; chloroplatinic acid complexes composed of chloroplatinic acid and alcohols, aldehydes, ketones, or the like; platinum-olefin complexes [e.g., Pt(CH 2 =CH 2 ) 2 (PPh 3 ), Pt(CH 2 =CH 2 ) 2 Cl 2 platinum divinyldisiloxane complexes [e.g., Pt{(vinyl)Me 2 SiOSiMe 2 (vinyl)} (Karstedt catalyst), Pt{Me(vinyl)SiO} 4 platinum-phosphine complexes [e.g., Ph(PPh 3 ) 4 , Pt(PBu 3 ) 4 ]; platinum-phosphite complexes [e.g., Pt{P(OPh) 3} 4 ] etc.

[0099] The weight ratio of the polyoxyalkylene polymer (E) to the polyoxyalkylene polymer (E') is not particularly limited, and may be, for example, (E):(E') = 1:99 to 99:1, preferably 10:90 to 90:10, more preferably 20:80 to 80:20, and even more preferably 30:70 to 70:30.

[0100] When the polyoxyalkylene polymer (E) and the polyoxyalkylene polymer (E') are used in combination, the expression "100 parts by weight of the polyoxyalkylene polymer (E)" in the present specification shall be read as "100 parts by weight of the total of the polyoxyalkylene polymer (E) and the polyoxyalkylene polymer (E')."

[0101] (Curing Catalyst) The curable composition according to the present embodiment preferably contains a curing catalyst, also known as a condensation catalyst, for the purpose of promoting the hydrolysis and condensation reaction of the hydrolyzable silyl group, i.e., the curing reaction.

[0102] As the curing catalyst, a conventionally known one can be used, and specifically, an organic tin compound, a metal carboxylate, an amine compound, a carboxylic acid, an alkoxy metal, an inorganic acid, a mixture thereof, etc. can be used.

[0103] Specific examples of organic tin compounds include dibutyltin dilaurate, dibutyltin dioctanoate, dibutyltin bis(butyl maleate), dibutyltin diacetate, dibutyltin oxide, dibutyltin bis(acetylacetonate), a reaction product of dibutyltin oxide with a silicate compound, a reaction product of dibutyltin oxide with a phthalate ester, dioctyltin diacetate, dioctyltin dilaurate, dioctyltin bis(ethyl maleate), dioctyltin bis(octyl maleate), dioctyltin bis(acetylacetonate), dioctyltin distearate, dioctyltin oxide, and a reaction product of dioctyltin oxide with a silicate compound. In view of the growing concern about the environment in recent years, dioctyltin compounds are preferred.

[0104] Specific examples of metal carboxylates include tin carboxylate, bismuth carboxylate, titanium carboxylate, zirconium carboxylate, iron carboxylate, potassium carboxylate, calcium carboxylate, etc. The carboxylic acid group can be a combination of the following carboxylic acids with various metals.

[0105] Specific examples of the amine compound include amines such as octylamine, 2-ethylhexylamine, laurylamine, stearylamine, piperidine, 4-methylpiperidine, and hexamethyleneimine; nitrogen-containing heterocyclic compounds such as pyridine, 1,8-diazabicyclo[5,4,0]undecene-7 (DBU), and 1,5-diazabicyclo[4,3,0]nonene-5 (DBN); guanidines such as guanidine, phenylguanidine, and diphenylguanidine; biguanides such as butylbiguanide, 1-o-tolylbiguanide, and 1-phenylbiguanide; and ketimine compounds.

[0106] Specific examples of carboxylic acids include acetic acid, propionic acid, butyric acid, 2-ethylhexanoic acid, lauric acid, stearic acid, oleic acid, linoleic acid, neodecanoic acid, and versatic acid.

[0107] Specific examples of alkoxy metals include titanium compounds such as tetrabutyl titanate, titanium tetrakis(acetylacetonate), titanium ethylacetoacetate, and diisopropoxytitanium bis(ethylacetoacetate); aluminum compounds such as aluminum tris(acetylacetonate) and diisopropoxyaluminum ethylacetoacetate; and zirconium compounds such as zirconium tetrakis(acetylacetonate).

[0108] Other curing catalysts that can be used include fluorine anion-containing compounds, photoacid generators, and photobase generators.

[0109] The curing catalyst may be a combination of two or more different catalysts. For example, the combination of the amine compound and a carboxylic acid or the amine compound and an alkoxy metal may provide an effect of improving reactivity.

[0110] The amount of the curing catalyst is preferably 0.001 to 20 parts by weight, more preferably 0.01 to 15 parts by weight, and particularly preferably 0.01 to 10 parts by weight, per 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment. Furthermore, some curing catalysts may ooze onto the surface of the cured product after the curable composition has cured, or may contaminate the surface of the cured product. In such cases, by using 0.01 to 3.0 parts by weight of the curing catalyst, it is possible to maintain good surface condition of the cured product while ensuring curability.

[0111] The curable composition according to this embodiment may contain other additives, such as silicon compounds, adhesion promoters, plasticizers, solvents, diluents, silicates, fillers, anti-sagging agents, antioxidants, light stabilizers, UV absorbers, physical property adjusters, tackifier resins, epoxy compounds, photocurable substances, oxygen-curable substances, surface property improvers, other resins, flame retardants, and foaming agents. Furthermore, the curable composition according to this embodiment may contain various additives as needed to adjust the physical properties of the composition or the cured product. Examples of such additives include curability adjusters, radical inhibitors, metal deactivators, antiozonants, phosphorus-based peroxide decomposers, lubricants, pigments, and mildew inhibitors.

[0112] (Filler) The curable composition according to the present embodiment may contain various fillers, such as heavy calcium carbonate, colloidal calcium carbonate, magnesium carbonate, diatomaceous earth, clay, talc, titanium oxide, silicic anhydride, hydrated silicic acid, ferric oxide, fine aluminum powder, zinc oxide, activated zinc oxide, PVC powder, PMMA powder, glass fiber, filament, and reinforcing filler.

[0113] The reinforcing filler is generally known as a reinforcing filler for rubber, and known fillers can be used. The reinforcing filler improves the mechanical properties of the cured product, increasing the modulus and breaking strength, and is used in sealing materials for automobile glass, etc., which require strength.

[0114] Specific examples of the reinforcing filler include carbon black such as channel black, furnace black, thermal black, lamp black, and acetylene black, and silica such as fume silica, precipitated silica, crystalline silica, and fused silica. These may be used alone or in combination.

[0115] Examples of carbon black include Printex 30, Printex 25, HIBLACK 30, HIBLACK 10, HIBLACK 5L, HIBLACK 20L, and HIBLACK 30L (manufactured by Orion Engineered Carbons), Monarch M430 and Monarch M570 (manufactured by Cabot), Showblack N-219 and Showblack N-220 (manufactured by Showa Cabot), Niteron #200, #300, and HTC #SL (manufactured by Shin-Nichika Carbon), Asahi #120, Asahi #55, Asahi #60, Asahi #70, Asahi Thermal, and Asahi #15 (manufactured by Asahi Carbon), Seest S (manufactured by Tokai Carbon), Diablack SA and Diablack N234 (manufactured by Mitsubishi Chemical), and Statex Examples include N121 (Columbia Carbon Japan), HTC#20 (Shin-Nichika Carbon), Huber N-907 (Huber), and Denka Acetylene Black (Denki Kagaku). Among carbon blacks, carbon blacks with small primary particle diameters are preferred, and the primary particle diameter is preferably 10 nm or more and 80 μm or less, and more preferably 15 nm or more and 50 μm or less. The reinforcing filler may be used alone or in combination of two or more types.

[0116] The amount of the filler used is preferably 1 to 300 parts by weight, more preferably 10 to 250 parts by weight, per 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment.

[0117] Organic or inorganic balloons may be added to the composition to reduce its weight (lower its specific gravity). The balloons are hollow spherical fillers, and examples of the materials for the balloons include inorganic materials such as glass, shirasu, and silica, and organic materials such as phenolic resin, urea resin, polystyrene, and saran.

[0118] The amount of balloons used is preferably 0.1 to 100 parts by weight, more preferably 1 to 20 parts by weight, per 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment.

[0119] (Adhesion imparting agent) The curable composition according to the present embodiment may contain an adhesion imparting agent. Examples of the adhesion imparting agent that may be added include a silane coupling agent and a reaction product of a silane coupling agent.

[0120] Specific examples of the silane coupling agent include amino group-containing silanes such as γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldimethoxysilane, N-β-aminoethyl-γ-aminopropyltrimethoxysilane, N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, and (2-aminoethyl)aminomethyltrimethoxysilane; γ-isocyanatepropyltrimethoxysilane, γ-isocyanatepropyltriethoxysilane, and γ-isopropyltriethoxysilane; Examples of suitable adhesion promoters include isocyanate group-containing silanes such as cyanatepropylmethyldimethoxysilane, α-isocyanatomethyltrimethoxysilane, and α-isocyanatomethyldimethoxymethylsilane; mercapto group-containing silanes such as γ-mercaptopropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, and γ-mercaptopropylmethyldimethoxysilane; and epoxy group-containing silanes such as γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. Condensates of various silane coupling agents, such as condensates of amino group-containing silanes and condensates of amino group-containing silanes with other alkoxysilanes, and reaction products of various silane coupling agents, such as reaction products of amino group-containing silanes and epoxy group-containing silanes and reaction products of amino group-containing silanes and (meth)acrylic group-containing silanes, can also be used. The adhesion promoters may be used alone or in combination.

[0121] The amount of the silane coupling agent used is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, per 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment.

[0122] (Plasticizer) The curable composition according to this embodiment may further contain a plasticizer. Specific examples of plasticizers include phthalate ester compounds such as dibutyl phthalate, diisononyl phthalate (DINP), diheptyl phthalate, di(2-ethylhexyl) phthalate, diisodecyl phthalate (DIDP), and butyl benzyl phthalate; terephthalate ester compounds such as bis(2-ethylhexyl)-1,4-benzenedicarboxylate; non-phthalate ester compounds such as 1,2-cyclohexanedicarboxylic acid diisononyl ester; aliphatic polycarboxylic acid ester compounds such as dioctyl adipate, dioctyl sebacate, dibutyl sebacate, diisodecyl succinate, and acetyl tributyl citrate; unsaturated fatty acid ester compounds such as butyl oleate and methyl acetylricinoleate; alkylsulfonic acid phenyl esters; phosphate ester compounds; trimellitic acid ester compounds; chlorinated paraffins; hydrocarbon oils such as alkyl diphenyls and partially hydrogenated terphenyls; process oils; and epoxy plasticizers such as epoxidized soybean oil and epoxy benzyl stearate.

[0123] Furthermore, a polymer plasticizer can be used. Specific examples of the polymer plasticizer include vinyl polymers; polyester plasticizers; polyether polyols such as polyethylene glycol and polypropylene glycol having a number average molecular weight of 500 or more, and polyethers such as derivatives in which the hydroxy groups of these polyether polyols are converted into ester groups, ether groups, etc.; polystyrenes; polybutadiene, polybutene, polyisobutylene, butadiene-acrylonitrile, polychloroprene, etc. The plasticizers may be used alone or in combination of two or more.

[0124] The polymeric plasticizer may not have a reactive silyl group, but may have a reactive silyl group. When it has a reactive silyl group, it acts as a reactive plasticizer and can prevent the plasticizer from migrating from the cured product. When it has a reactive silyl group, it is preferable that the number of reactive silyl groups per molecule is 1 or less, more preferably 0.8 or less. When using a plasticizer having a reactive silyl group, particularly an oxyalkylene polymer having a reactive silyl group, its number average molecular weight is preferably lower than that of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E).

[0125] The amount of the plasticizer used is preferably 5 to 150 parts by weight, more preferably 10 to 120 parts by weight, and even more preferably 20 to 100 parts by weight, per 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment.

[0126] According to one aspect of the present invention, the curable composition exhibits good curability and can provide a cured product with a low modulus. Therefore, the curable composition according to this embodiment contains a polyoxyalkylene polymer (E), a plasticizer, a filler, and a curing catalyst, and the proportion of the polyoxyalkylene polymer (E) is preferably 5% by weight or more and 20% by weight or less, the proportion of the plasticizer is preferably 5% by weight or more and 65% by weight or less, the proportion of the filler is preferably 15% by weight or more and 90% by weight or less, and the total proportion of the polyoxyalkylene polymer (E), the plasticizer, and the filler is preferably 80% by weight or more and 100% by weight or less. Each of these proportions is a ratio to the total of the components of the curable composition other than the curing catalyst.

[0127] The proportion of the polyoxyalkylene polymer (E) is more preferably 7% by weight or more and 18% by weight or less. The proportion of the plasticizer is more preferably 7% by weight or more and 60% by weight or less, and even more preferably 10% by weight or more and 50% by weight or less. The proportion of the filler is more preferably 20% by weight or more and 80% by weight or less, and even more preferably 30% by weight or more and 70% by weight or less. The total proportion of the polyoxyalkylene polymer (E), the plasticizer, and the filler is more preferably 85% by weight or more and 100% by weight or less, and even more preferably 90% by weight or more and 99% by weight or less.

[0128] (Solvent, Diluent) A solvent or diluent can be added to the curable composition according to this embodiment. The solvent and diluent are not particularly limited, but aliphatic hydrocarbons, aromatic hydrocarbons, alicyclic hydrocarbons, halogenated hydrocarbons, alcohols, esters, ketones, ethers, etc. can be used. When using a solvent or diluent, in view of the problem of air pollution when the composition is used indoors, the boiling point of the solvent is preferably 150°C or higher, more preferably 200°C or higher, and particularly preferably 250°C or higher. The above solvents or diluents may be used alone or in combination of two or more.

[0129] (Anti-sagging agent) If necessary, an anti-sagging agent may be added to the curable composition according to this embodiment in order to prevent sagging and improve workability. The anti-sagging agent is not particularly limited, and examples thereof include polyamide waxes; hydrogenated castor oil derivatives; and metal soaps such as calcium stearate, aluminum stearate, and barium stearate. These anti-sagging agents may be used alone or in combination of two or more.

[0130] The amount of the anti-sagging agent used is preferably 0.1 to 20 parts by weight based on 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment.

[0131] (Antioxidant) An antioxidant (antiaging agent) can be used in the curable composition according to this embodiment. The use of an antioxidant can improve the weather resistance of the cured product. Examples of antioxidants include hindered phenols, monophenols, bisphenols, and polyphenols. Examples include Irganox 245, Irganox 1010, Irganox 1035, Irganox 1076, Irganox 1135, Irganox 1330, and Irganox 1520 (all manufactured by BASF); SONGNOX 1076 (manufactured by SONGWON), and BHT. Similarly, hindered amine light stabilizers such as TINUVIN 622LD, TINUVIN 144, TINUVIN 292, CHIMASSORB 944LD, and CHIMASSORB 119FL (all manufactured by BASF); Adeka STAB LA-57, Adeka STAB LA-62, Adeka STAB LA-67, Adeka STAB LA-63, and Adeka STAB LA-68 (all manufactured by ADEKA Corporation); Sanol LS-2626, Sanol LS-1114, and Sanol LS-744 (all manufactured by Sankyo Lifetech Co., Ltd.); and Nocrac CD (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) can also be used. Other antioxidants that can be used include SONGNOX 4120, Nauguard 445, and OKABEST CLX050. Specific examples of antioxidants are also described in Japanese Patent Application Laid-Open Nos. 4-283259 and 9-194731.

[0132] The amount of the antioxidant used is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, per 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment.

[0133] (Light Stabilizer) A light stabilizer can be used in the curable composition according to this embodiment. The use of a light stabilizer can prevent photo-oxidative degradation of the cured product. Examples of light stabilizers include benzotriazole-based, hindered amine-based, and benzoate-based compounds, with hindered amine-based compounds being particularly preferred.

[0134] The amount of the light stabilizer used is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, based on 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment.

[0135] (Ultraviolet Absorber) An ultraviolet absorber can be used in the curable composition according to this embodiment. Use of an ultraviolet absorber can improve the surface weather resistance of the cured product. Examples of ultraviolet absorbers include benzophenone-based, benzotriazole-based, salicylate-based, substituted acrylonitrile-based, and metal chelate-based compounds, with benzotriazole-based compounds being particularly preferred, and examples thereof include those commercially available under the names Tinuvin P, Tinuvin 213, Tinuvin 234, Tinuvin 326, Tinuvin 327, Tinuvin 328, Tinuvin 329, Tinuvin 571, Tinuvin 1600, and Tinuvin B75 (all manufactured by BASF).

[0136] The amount of the ultraviolet absorber used is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, per 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment.

[0137] (Physical Property Modifier) ​​A physical property modifier may be added to the curable composition according to this embodiment as needed to adjust the tensile properties of the resulting cured product. The physical property modifier is not particularly limited, but examples include alkylalkoxysilanes such as phenoxytrimethylsilane, methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, and n-propyltrimethoxysilane; arylalkoxysilanes such as diphenyldimethoxysilane and phenyltrimethoxysilane; alkylisopropenoxysilanes such as dimethyldiisopropenoxysilane, methyltriisopropenoxysilane, and γ-glycidoxypropylmethyldiisopropenoxysilane; trialkylsilylborates such as tris(trimethylsilyl)borate and tris(triethylsilyl)borate; silicone varnishes; and polysiloxanes. The use of the physical property modifier can increase the hardness of the curable composition according to this embodiment when cured, or conversely, decrease the hardness and increase the elongation at break. The physical property modifiers may be used alone, or two or more types may be used in combination.

[0138] In particular, compounds that upon hydrolysis produce compounds having monovalent silanol groups in the molecule have the effect of reducing the modulus of the cured product without increasing the stickiness of the surface of the cured product. Compounds that produce trimethylsilanol are particularly preferred. Examples of compounds that upon hydrolysis produce compounds having monovalent silanol groups in the molecule include silicon compounds that are derivatives of alcohols such as hexanol, octanol, phenol, trimethylolpropane, glycerin, pentaerythritol, and sorbitol and that produce silane monool upon hydrolysis. Specific examples include phenoxytrimethylsilane and tris((trimethylsiloxy)methyl)propane.

[0139] The amount of the physical property adjuster used is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 5 parts by weight, per 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment.

[0140] (Tackifying Resin) A tackifying resin can be added to the curable composition according to the present embodiment for the purpose of improving adhesion or adhesion to a substrate, or as otherwise required. The tackifying resin is not particularly limited, and any commonly used tackifying resin can be used.

[0141] Specific examples include terpene resins, aromatic modified terpene resins, hydrogenated terpene resins, terpene-phenol resins, phenol resins, modified phenol resins, xylene-phenol resins, cyclopentadiene-phenol resins, coumarone-indene resins, rosin resins, rosin ester resins, hydrogenated rosin ester resins, xylene resins, low molecular weight polystyrene resins, styrene copolymer resins, styrene block copolymers and hydrogenated products thereof, petroleum resins (e.g., C5 hydrocarbon resins, C9 hydrocarbon resins, C5C9 hydrocarbon copolymer resins, etc.), hydrogenated petroleum resins, DCPD resins, etc. These may be used alone or in combination of two or more.

[0142] The amount of the tackifier resin used is preferably 2 to 100 parts by weight, more preferably 5 to 50 parts by weight, and even more preferably 5 to 30 parts by weight, per 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment.

[0143] (Epoxy Compound) The curable composition according to this embodiment may further contain an epoxy compound. By incorporating an epoxy compound, it is possible to obtain a cured product having good curability and high tensile shear strength. In addition, it is possible to improve the recovery of the cured product. The number of epoxy groups in the epoxy compound is 1 or more, and preferably 2 or more.

[0144] Specific preferred examples of epoxy compounds include bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol AD ​​epoxy resins, bisphenol S epoxy resins, hydrogenated products of these bisphenol epoxy resins, glycidyl ester epoxy compounds, glycidyl amine epoxy compounds, alicyclic epoxy compounds, phenol novolac epoxy resins, cresol novolac epoxy resins, naphthol novolac epoxy resins, urethane-modified epoxy resins, fluorinated epoxy resins, epoxidized rubbers such as epoxidized polybutadiene, and brominated epoxy compounds such as tetrabromobisphenol A diglycidyl ether. Of these, bisphenol A epoxy resins are preferred because they are capable of easily forming cured products that are excellent in both strength and elongation.

[0145] The amount of the epoxy compound is not particularly limited as long as the desired effect is not impaired. The amount of the epoxy compound is preferably 0.1 parts by weight or more and 500 parts by weight or less, more preferably 10 parts by weight or more and 200 parts by weight or less, and even more preferably 20 parts by weight or more and 100 parts by weight or less, relative to 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment. When the amount of the epoxy compound used is within the above range, a cured product having sufficiently high tensile shear strength is easily formed, and the peel strength of the cured product is less likely to decrease.

[0146] In addition, as the epoxy compound, epoxidized unsaturated fats and oils, epoxidized unsaturated fatty acid esters, alicyclic epoxy compounds, compounds shown in the epichlorohydrin derivatives, and mixtures thereof can also be used. Specific examples include epoxidized soybean oil, epoxidized linseed oil, bis(2-ethylhexyl)-4,5-epoxycyclohexane-1,2-dicarboxylate (E-PS), epoxy octyl stearate, and epoxy butyl stearate. These epoxy compounds are preferably used in an amount of 0.5 to 50 parts by weight per 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment.

[0147] <Epoxy Curing Agent> When the curable composition according to this embodiment contains an epoxy compound, it is preferable that the composition further contains an epoxy curing agent as a component that cures the epoxy compound.

[0148] As the epoxy curing agent, compounds that have conventionally been used as curing agents for various epoxy compounds can be used appropriately, as long as the desired effect is not impaired. Specific examples of epoxy curing agents include chain aliphatic amine compounds, alicyclic amine compounds, aromatic amine compounds, polyaminoamides, imidazoles, dicyandiamides, epoxy-modified amines, Mannich-modified amines, Michael addition-modified amines, ketimines, polycarboxylic acid anhydrides, alcohols, and phenols. These epoxy curing agents may be used alone or in combination of two or more.

[0149] The amount of the epoxy curing agent is not particularly limited. In order to rapidly cure the epoxy compound, the amount of the epoxy curing agent is preferably 0.1 parts by weight or more and 300 parts by weight or less, more preferably 1 part by weight or more and 200 parts by weight or less, and even more preferably 5 parts by weight or more and 100 parts by weight or less, relative to 100 parts by weight of the epoxy compound.

[0150] (Photocurable Substance) A photocurable substance can be used in the curable composition according to this embodiment. When a photocurable substance is used, a film of the photocurable substance is formed on the surface of the cured product, improving the stickiness and weather resistance of the cured product. Many compounds of this type are known, such as organic monomers, oligomers, resins, and compositions containing them. Representative examples include unsaturated acrylic compounds, which are monomers or oligomers having one or more acrylic or methacrylic unsaturated groups, or mixtures thereof, polyvinyl cinnamates, and azido resins.

[0151] The amount of the photocurable substance used is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, per 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to this embodiment.

[0152] (Oxygen-Curable Substance) An oxygen-curable substance can be used in the curable composition according to this embodiment. Examples of oxygen-curable substances include unsaturated compounds that can react with oxygen in the air, which react with oxygen in the air to form a cured film near the surface of the cured product, preventing stickiness of the surface and adhesion of dirt and dust to the surface of the cured product. Specific examples of oxygen-curable substances include drying oils such as tung oil and linseed oil, and various alkyd resins obtained by modifying such compounds; acrylic polymers, epoxy resins, and silicone resins modified with drying oils; and liquid polymers such as 1,2-polybutadiene, 1,4-polybutadiene, and polymers of C5 to C8 dienes obtained by polymerizing or copolymerizing diene compounds such as butadiene, chloroprene, isoprene, and 1,3-pentadiene. These substances may be used alone or in combination of two or more.

[0153] The amount of the oxygen-curable substance used is preferably in the range of 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, per 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E) according to the present embodiment. As described in JP-A-3-160053, the oxygen-curable substance is preferably used in combination with a photo-curable substance.

[0154] <<Preparation of Curable Composition>> The curable composition according to this embodiment can be prepared as a one-component composition in which all components are mixed in advance and stored in a sealed state, and which is cured by moisture in the air after application. Alternatively, it can be prepared as a two-component composition in which components such as a curing catalyst, a filler, a plasticizer, and water are mixed separately as a curing agent, and the curing agent and a base agent containing a polyoxyalkylene polymer (E) are mixed before use. From the viewpoint of workability, the one-component composition is preferred.

[0155] In an embodiment in which the curable composition contains an epoxy compound, the curable composition cures quickly. Therefore, it is preferable that the one-component curable composition is prepared at the site where the curable composition is to be applied and used promptly after preparation.

[0156] When the curable composition containing an epoxy compound does not contain an epoxy curing agent, a two-component curable composition consisting of two liquids can be prepared so that the polyoxyalkylene polymer (E) and the curing catalyst are separated. In this case, examples of the two-component curable composition include a two-component curable composition consisting of a main component containing the polyoxyalkylene polymer (E) and an epoxy compound, and a curing agent containing a curing catalyst, and a two-component curable composition consisting of a first component containing the polyoxyalkylene polymer (E) and a second component containing the epoxy compound and a curing catalyst.

[0157] Furthermore, when the curable composition containing an epoxy compound contains an epoxy curing agent, examples thereof include a two-component curable composition consisting of a main component containing the polyoxyalkylene polymer (E) and the epoxy compound, and a curing agent containing the curing catalyst and the epoxy curing agent, and a two-component curable composition consisting of a first component containing the polyoxyalkylene polymer (E) and the epoxy curing agent, and a second component containing the epoxy compound and the curing catalyst. In the two-component curable composition, components other than the polyoxyalkylene polymer (E), the epoxy compound, the curing catalyst, and the epoxy curing agent may be blended in either liquid.

[0158] When the curable composition according to the present embodiment is a one-component type, all of the components are blended in advance, and therefore it is preferable to dehydrate and dry the components containing water before use, or to dehydrate them under reduced pressure during blending and kneading. In addition to the dehydration and drying method, the storage stability can be further improved by adding an alkoxysilane compound such as methyltrimethoxysilane, phenyltrimethoxysilane, n-propyltrimethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropylmethyldiethoxysilane, or γ-glycidoxypropyltrimethoxysilane.

[0159] <Uses> The curable composition according to this embodiment can be used as a pressure-sensitive adhesive, a sealing material for buildings, ships, automobiles, roads, etc., an adhesive, a waterproofing material, a waterproof coating material, a mold release agent, an anti-vibration material, a vibration-damping material, a sound-proofing material, a foam material, a paint, or a spray material. The cured product obtained by curing the curable composition according to this embodiment has excellent flexibility and adhesiveness, and therefore can be suitably used as a sealant or adhesive.

[0160] Furthermore, the curable composition according to this embodiment can be used in a wide range of applications, including electrical and electronic component materials such as solar cell rear surface sealing materials, electrical and electronic components such as insulating coating materials for electric wires and cables, electrical insulating materials for devices, acoustic insulating materials, elastic adhesives, binders, contact adhesives, spray-type sealants, crack repair materials, tiling adhesives, adhesives for asphalt waterproofing materials, powder coatings, casting materials, medical rubber materials, medical pressure-sensitive adhesives, medical adhesive sheets, medical device sealants, dental impression materials, food packaging materials, and joint sealants for exterior materials such as sizing boards. These compounds can be used in a variety of applications, including adhesives, coatings, non-slip coatings, buffer materials, primers, conductive materials for electromagnetic wave shielding, thermally conductive materials, hot melt materials, potting agents for electrical and electronic applications, films, gaskets, concrete reinforcing materials, temporary adhesives, various molding materials, and liquid sealants for rust prevention and waterproofing of wired glass and laminated glass edge (cut portions), automobile parts, large vehicle parts such as trucks and buses, train car parts, aircraft parts, marine parts, electrical parts, and various machine parts. Taking automobiles as an example, they can be used in a wide variety of applications, including adhesive attachment of plastic covers, trim, flanges, bumpers, window mounting, interior components, exterior components, etc. Furthermore, because they can adhere to a wide range of substrates, such as glass, porcelain, wood, metal, and resin moldings, either alone or with the aid of a primer, they can also be used as various types of sealing and adhesive compositions. The curable composition according to this embodiment can also be used as an adhesive for interior panels, exterior panels, tile adhesives, stone veneers, ceiling finishing adhesives, floor finishing adhesives, wall finishing adhesives, vehicle panels, electrical, electronic, and precision equipment assembly adhesives, adhesives for bonding leather, textile products, fabrics, paper, boards, and rubber, reactive post-crosslinking pressure-sensitive adhesives, direct glazing sealants, double-glazing sealants, SSG construction sealants, or building working joint sealants, civil engineering and bridge materials, and can also be used as adhesive materials such as adhesive tapes and adhesive sheets.

[0161] The following items are preferred embodiments of the present disclosure, but the present invention is not limited to them. [Item 1] A polyoxyalkylene polymer (E) containing polyoxyalkylene polymer molecules having a hydrolyzable silyl group-containing structure represented by general formula (1) (wherein R are the same or different and represent a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms; X are the same or different and represent a hydroxyl group or a hydrolyzable group; and a represents 0, 1, or 2), wherein the ratio of the number of hydrolyzable silyl group-containing structures represented by general formula (1) to the total number of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups measured for the polymer is 0.85 to 1.00, and the number average molecular weight of the polymer exceeds 3,000. [Item 2] The polyoxyalkylene polymer (E) according to Item 1, wherein the ratio of the number of hydrolyzable silyl group-containing structures represented by general formula (1) to the total number of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups measured for the polymer is 0.90 or more and 1.00 or less. [Item 3] The polyoxyalkylene polymer (E) according to Item 1 or 2, wherein the hydrolyzable silyl groups, 1-propenyl groups, and propyl groups are groups generated from allyl groups during a hydrosilylation reaction. [Item 4] The polyoxyalkylene polymer (E) according to any one of Items 1 to 3, wherein the number-average molecular weight of the polymer is 10,000 or more. [Item 5] The polyoxyalkylene polymer (E) according to Item 4, wherein the number-average molecular weight of the polymer is 20,000 or more. [Item 6] A polymer mixture comprising the polyoxyalkylene polymer (E) according to any one of Items 1 to 5, and a ruthenium complex (A). [Item 7] The polymer mixture according to Item 6, wherein the ruthenium complex (A) has a compound (B) as a ligand, and the compound (B) has at least one carbon-carbon double bond in one molecule, and at least one of the carbon atoms forming the carbon-carbon double bond has an electron-withdrawing group bonded to it. [Item 8] The polymer mixture according to Item 7, wherein the compound (B) has a benzene ring skeleton as the skeleton containing the carbon-carbon double bond.[Item 9] The polymer mixture according to item 7, wherein compound (B) has a norbornadiene skeleton as the skeleton containing the carbon-carbon double bond. [Item 10] The polymer mixture according to any one of items 7 to 9, wherein the electron-withdrawing group is at least one selected from the group consisting of a fluoro group, a bromo group, and an iodo group. [Item 11] A curable composition containing the polyoxyalkylene polymer (E) according to any one of items 1 to 5 or the polymer mixture according to any one of items 6 to 10. [Item 12] The curable composition according to item 11, further containing a reinforcing filler. [Item 13] The curable composition according to Item 11 or 12, further comprising a plasticizer, a filler, and a curing catalyst, wherein the ratio of the polyoxyalkylene polymer (E) to the total of all components of the curable composition other than the curing catalyst is 5% by weight or more and 20% by weight or less, the ratio of the plasticizer to the total of all components of the curable composition other than the curing catalyst is 5% by weight or more and 65% by weight or less, the ratio of the filler to the total of all components of the curable composition other than the curing catalyst is 15% by weight or more and 90% by weight or less, and the ratio of the total of the polyoxyalkylene polymer (E), the plasticizer, and the filler to the total of all components of the curable composition other than the curing catalyst is 80% by weight or more and 100% by weight or less. [Item 14] The curable composition according to any one of Items 11 to 13, further comprising a polyoxyalkylene polymer (E') containing polyoxyalkylene polymer molecules having a hydrolyzable silyl group-containing structure represented by General Formula (1), wherein the ratio of the number of hydrolyzable silyl group-containing structures represented by General Formula (1) to the total number of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups measured for the polymer (E') is 0.05 or more and less than 0.85. [Item 15] The curable composition according to Item 14, wherein the number average molecular weight of the polyoxyalkylene polymer (E) is 20,000 or more and 100,000 or less, and the number average molecular weight of the polyoxyalkylene polymer (E') is 800 or more and less than 20,000. [Item 16] The curable composition according to Item 14 or 15, wherein the main chain structure of the polyoxyalkylene polymer (E) is branched.[Item 17] The curable composition according to any one of items 14 to 16, wherein the main chain structure of the polyoxyalkylene polymer (E') is linear, and the polyoxyalkylene polymer (E') has the hydrolyzable silyl group-containing structure at only one end of the linear main chain. [Item 18] The curable composition according to any one of items 11 to 17, further comprising an epoxy compound. [Item 19] The curable composition according to item 18, further comprising an epoxy curing agent. [Item 20] A cured product obtained by curing the curable composition according to any one of items 11 to 19.

[0162] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The number average molecular weight in the examples is a GPC molecular weight measured under the following conditions: Solution delivery system: HLC-8420GPC manufactured by Tosoh Corporation Column: TSKgel Super H series manufactured by Tosoh Corporation Solvent: THF (tetrahydrofuran) Molecular weight: Polystyrene equivalent Measurement temperature: 40°C

[0163] The proportion of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, or allyl groups was calculated using the following nuclear magnetic resonance (NMR) spectrometer: 1 H NMR measurement was performed. Apparatus: AVANCE III HD500 digital instrument (manufactured by BRUKER)

[0164] Synthesis Example 1 Using polyoxypropylene glycol having a number-average molecular weight of approximately 4,500 as an initiator, propylene oxide was polymerized in the presence of a zinc hexacyanocobaltate glyme complex catalyst to obtain a hydroxyl-containing polyoxyalkylene polymer (F-1) having hydroxyl groups at both ends and a number-average molecular weight of 27,600. To the hydroxyl-containing polyoxyalkylene polymer (F-1), 1.1 molar equivalents of sodium methoxide relative to the hydroxyl groups of the polymer (F-1) were added as a 28% methanol solution. After removing the methanol by distillation under reduced pressure, 1.3 molar equivalents of allyl chloride relative to the hydroxyl groups of the polymer (F-1) were added and the mixture was reacted at 130°C for 1 hour, after which the allyl chloride was distilled off under reduced pressure. The resulting unpurified allyl-containing polyoxyalkylene polymer was mixed and stirred with n-hexane and water, after which the water was removed by centrifugation. The hexane was then distilled off under reduced pressure from the resulting hexane solution to remove metal salts from the polymer. As a result, an allyl group-containing polyoxyalkylene polymer (C-1) was obtained, which had a number average molecular weight of 27,600.

[0165] Example 1 An allyl group-containing polyoxyalkylene polymer (C-1) was reacted with a ruthenium compound (A') [RuCl 2 (nbd)] n 48 ppm of methyl silane and 120 ppm of 2,3-dibromonorbornadiene, which is compound (B), were added, and the mixture was stirred at 90° C. for 10 minutes. Further, dimethoxymethylsilane, which is hydrosilane compound (D) (5.0 molar equivalents relative to the allyl groups in polymer (C-1)), was added, and a hydrosilylation reaction of the allyl groups in polymer (C-1) was carried out at 90° C. Every hour from the start of the reaction, 1 H NMR measurement confirmed that the allyl groups in the polymer (C-1) were completely consumed within 2 hours from the start of the reaction, and the volatile components were distilled off under reduced pressure to obtain a hydrolyzable silyl group-containing polyoxyalkylene polymer (E-1). The polymer skeleton of the polymer (E-1) was linear. 1By H NMR measurement, the proportion of each group to the total of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups was calculated, and it was found that the hydrolyzable silyl group-containing structure represented by general formula (1) accounted for 99%, 1-propenyl groups for 0%, propyl groups for 1%, and allyl groups for 0%.

[0166] Comparative Example 1 To an allyl group-containing polyoxyalkylene polymer (C-1), 50 ppm of a commercially available Karstedt catalyst and dimethoxymethylsilane (5.0 molar equivalents relative to the allyl groups in the polymer (C-1)), which is a hydrosilane compound (D), were added, and a hydrosilylation reaction of the allyl groups in the polymer (C-1) was carried out at 90°C. 1 H NMR measurement was carried out, and it was confirmed that the allyl groups in the polymer (C-1) were completely consumed within 1 hour from the start of the reaction. The volatile components were then distilled off under reduced pressure to obtain a hydrolyzable silyl group-containing polyoxyalkylene polymer (E'-1). 1 By H NMR measurement, the proportion of each group relative to the total of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups was calculated, and it was found that the hydrolyzable silyl group-containing structure represented by general formula (1) accounted for 79%, the 1-propenyl groups for 20%, the propyl groups for 1%, and the allyl groups for 0%.

[0167] Comparative Example 2 To the hydroxyl group-containing polyoxyalkylene polymer (F-1) obtained in Synthesis Example 1, 0.9 molar equivalents of sodium methoxide relative to the hydroxyl groups of the polymer (F-1) were added as a 28% methanol solution. After removing the methanol by distillation under reduced pressure, 1.2 molar equivalents of 3-chloro-2-methyl-1-propene (methallyl chloride) relative to the hydroxyl groups of the polymer (F-1) were added and the mixture was reacted at 130°C for 1 hour to convert the terminal hydroxyl groups to methallyl groups, after which the 3-chloro-2-methyl-1-propene (methallyl chloride) was distilled off under reduced pressure. Thereafter, 0.6 molar equivalents of sodium methoxide relative to the hydroxyl groups of the polymer (F-1) were added as a 28% methanol solution. After removing the methanol by distillation under reduced pressure, 0.7 molar equivalents of 3-chloro-2-methyl-1-propene (methallyl chloride) relative to the hydroxyl groups of polymer (F-1) were added and the reaction was carried out at 130°C for 1 hour to convert the remaining terminal hydroxyl groups to methallyl groups, and then the 3-chloro-2-methyl-1-propene (methallyl chloride) was distilled off under reduced pressure. The resulting unpurified methallyl group-containing polyoxyalkylene polymer was mixed and stirred with n-hexane and water, after which the water was removed by centrifugation. The hexane was then distilled off under reduced pressure from the resulting hexane solution to remove the metal salts in the polymer. In this manner, a methallyl group-containing polyoxyalkylene polymer (G-1) was obtained.

[0168] To the methallyl group-containing polyoxyalkylene polymer (G-1), 100 ppm of Karstedt's catalyst and 1,000 ppm of 2,5-di-t-butyl-1,4-benzoquinone were added, and further, dimethoxymethylsilane (1.5 molar equivalents relative to the methallyl groups in the polymer (G-1)) as the hydrosilane compound (D) was added, and the hydrosilylation reaction of the methallyl groups in the polymer (G-1) was carried out at 100°C. 1 H NMR measurement was carried out, and it was confirmed that the methallyl groups in the polymer (G-1) were completely consumed 6 hours after the start of the reaction, and the volatile components were distilled off under reduced pressure to obtain a hydrolyzable silyl group-containing polyoxyalkylene polymer (E'-2). 1By H NMR measurement, the proportion of each group to the total of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups was calculated, and the proportion of hydrolyzable silyl groups was 95%. However, the hydrolyzable silyl group-containing structure not represented by general formula (1) (hydrolyzable silyl group-containing structure having an isobutylene group instead of the trimethylene group in general formula (1)) was predominant, and the proportion of hydrolyzable silyl group-containing structure represented by general formula (1) was less than 85%.

[0169] Example 2 Using a 5 L planetary mixer (manufactured by Dalton Co., Ltd.), a one-component curable composition was prepared according to the formulation shown in Table 1. First, 160 parts by weight of Ultra-Pflex (manufactured by Specialty Minerals: colloidal calcium carbonate), 54 parts by weight of Q3T (manufactured by Huber: surface-untreated heavy calcium carbonate), and 20 parts by weight of Ti-Pure R-902+ (manufactured by Chemours: titanium oxide) were dried under reduced pressure at 120°C for 2 hours. Next, 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E-1) obtained in Example 1, 90 parts by weight of DINP (diisononyl phthalate manufactured by J-Plus Corporation), 2 parts by weight of Crayvallac SL (fatty acid amide wax manufactured by ARKEMA), 1 part by weight of Tinuvin 328 (ultraviolet absorber manufactured by BASF), and 1 part by weight of Tinuvin 770 (light stabilizer manufactured by BASF) were each charged into a mixer and kneaded for 10 minutes. The resulting mixture was removed and passed through a three-roll mill once to uniformly disperse the mixture, and then charged back into the mixer and dehydrated under reduced pressure for 2 hours. After dehydration under reduced pressure, the mixture was cooled to 50°C or below, and then 3 parts by weight of A-171 (manufactured by Momentive: vinyltrimethoxysilane), 3 parts by weight of A-1120 (manufactured by Momentive: N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane), and 2 parts by weight of Neostan U-220H (manufactured by Nitto Kasei Co., Ltd., dibutyltin bis(acetylacetonate)) were added and kneaded for 3 minutes. Subsequently, the mixture was degassed under reduced pressure for 2 minutes, and the resulting mixture was immediately filled into a moisture-proof aluminum cartridge and sealed to obtain a curable composition.

[0170] (Skinning Time) The obtained curable composition was filled into a mold about 5 mm thick using a spatula under an atmosphere of 23°C and 50% relative humidity, and the time when the surface was smoothed to a flat surface was defined as the curing initiation time. The surface was touched with the spatula, and the time when the composition to be evaluated no longer adhered to the spatula was defined as the skinning time. The results are shown in Table 1.

[0171] (Dumbbell Tensile Properties) The resulting curable composition was filled into a mold and aged for 3 days at 23°C and 50% relative humidity, and then for 4 days at 50°C to produce a sheet-like cured product approximately 3 mm thick. The sheet-like cured product was punched into a No. 3 dumbbell shape and subjected to a tensile strength test in an atmosphere of 23°C and 50% relative humidity to measure the modulus at 50% and 100% elongation (M50 and M100). The strength at break (TB) and elongation (EB) were also measured. The measurements were performed using an autograph (AGS-J) manufactured by Shimadzu Corporation at a tensile speed of 200 mm / min. The results are shown in Table 1.

[0172] (Tear Strength) The obtained curable composition was filled into a 3 mm thick sheet mold at 23°C and 50% relative humidity. After curing for 3 days at 23°C and 50% relative humidity, the composition was aged in a 50°C dryer for 4 days to obtain a sheet-like cured product. The obtained cured product was punched into a dumbbell shape (JIS Type A) for tear testing to obtain a test piece. Using the obtained test piece, a tear test (tensile speed 200 mm / min) was performed using an autograph at 23°C and 50% relative humidity to measure the stress at break (TB). The results are shown in Table 1.

[0173] (Tensile Shear Strength) An aluminum plate was used as the adherend. At 23°C and 50% relative humidity, a curable composition was applied to a 25 mm x 25 mm adhesive surface of the aluminum plate to a thickness of 50 μm. Two minutes after application, an aluminum plate not coated with the curable composition was pressed against the coated surface of the aluminum plate to bond the aluminum plates together. The resulting test specimen was left standing at a constant temperature and humidity of 23°C and 50% relative humidity. After 1 hour, 3 hours, and 24 hours had elapsed since being placed under the constant temperature and humidity conditions, a tensile shear test (tensile speed 50 mm / min) was performed using an autograph to measure the stress at break (TB). The resulting test specimen was aged for 3 days at 23°C and 50% relative humidity, and then for 4 days at 50°C, after which a tensile shear test was performed using an autograph to measure the stress at break (TB). The strength development rate at each time point was calculated as follows: Strength development rate (%) = (shear strength at each time) ÷ (shear strength after aging at 23°C and 50% relative humidity for 3 days and then at 50°C for 4 days) × 100 The results are shown in Table 1.

[0174] Comparative Example 3 A curable composition was obtained in the same manner as in Example 2, except that 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E'-1) obtained in Comparative Example 1 was used instead of 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E-1). Using the obtained curable composition, the skin-strength time, dumbbell tensile properties, tear strength, and tensile shear strength were evaluated in the same manner as in Example 2. The results are shown in Table 1.

[0175] Comparative Example 4 A curable composition was obtained in the same manner as in Example 2, except that 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E'-2) obtained in Comparative Example 2 was used instead of 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E-1). Using the obtained curable composition, the skinning time, dumbbell tensile properties, tear strength, and tensile shear strength were evaluated in the same manner as in Example 2. The results are shown in Table 1.

[0176]

[0177] As can be seen from Table 1, polyoxyalkylene polymer (E-1) having a proportion of hydrolyzable silyl group-containing structures represented by general formula (1) of 85% or more was obtained in a shorter hydrosilylation reaction time than polyoxyalkylene polymer (E'-2) having a total proportion of hydrolyzable silyl group-containing structures of 85% or more but a proportion of hydrolyzable silyl group-containing structures represented by general formula (1) of less than 85%. Polyoxyalkylene polymer (E-1) having a proportion of hydrolyzable silyl group-containing structures represented by general formula (1) of 85% or more exhibited a shorter skinning time and better curing properties than polyoxyalkylene polymer (E'-1) having a same proportion of less than 85% and polyoxyalkylene polymer (E'-2) having a total proportion of hydrolyzable silyl group-containing structures of 85% or more but a proportion of hydrolyzable silyl group-containing structures represented by general formula (1) of less than 85%. Furthermore, it exhibited better tear strength and tensile shear strength. Furthermore, when comparing the rise in tensile shear strength, the tensile shear strength of polymer (E-1) after 1 hour at 23°C was significantly greater than that of polymer (E'-2), demonstrating a better-than-expected improvement. Furthermore, in a dumbbell tensile test, hydrolyzable silyl group-containing polyoxyalkylene polymer (E-1) exhibited higher modulus and strength than hydrolyzable silyl group-containing polyoxyalkylene polymer (E'-1), and showed values ​​comparable to those of hydrolyzable silyl group-containing polyoxyalkylene polymer (E'-2).

[0178] Synthesis Example 2 Using polyoxypropylene triol having a number-average molecular weight of approximately 4,500 as an initiator, propylene oxide was polymerized in the presence of a zinc hexacyanocobaltate glyme complex catalyst to obtain a hydroxyl-containing polyoxyalkylene polymer (F-2) having hydroxyl groups at both ends and a number-average molecular weight of 24,000. To the hydroxyl-containing polyoxyalkylene polymer (F-2), 1.1 molar equivalents of sodium methoxide relative to the hydroxyl groups of polymer (F-2) were added as a 28% methanol solution. After removing the methanol by distillation under reduced pressure, 1.3 molar equivalents of allyl chloride relative to the hydroxyl groups of polymer (F-2) were added and the mixture was reacted at 130°C for 1 hour, after which the allyl chloride was distilled off under reduced pressure. The resulting unpurified allyl-containing polyoxyalkylene polymer was mixed and stirred with n-hexane and water, after which the water was removed by centrifugation. The hexane was then distilled off under reduced pressure from the resulting hexane solution to remove metal salts from the polymer. As a result, an allyl group-containing polyoxyalkylene polymer (C-2) was obtained, which had a number average molecular weight of 24,000.

[0179] Example 3 Allyl group-containing polyoxyalkylene polymer (C-2) was treated with ruthenium compound (A') [RuCl 2 (nbd)] n 100 ppm of 2,3-dibromonorbornadiene (compound (B)), 260 ppm, was added, and the mixture was stirred at 110° C. for 10 minutes. Further, dimethoxymethylsilane (6.0 molar equivalents relative to the allyl groups in polymer (C-2)) (hydrosilane compound (D)) was added, and a hydrosilylation reaction of the allyl groups in polymer (C-2) was carried out at 110° C. Every hour from the start of the reaction, 1 H NMR measurement was carried out, and it was confirmed that the allyl groups in the polymer (C-2) were completely consumed one hour after the start of the reaction. The volatile components were then distilled off under reduced pressure to obtain a hydrolyzable silyl group-containing polyoxyalkylene polymer (E-2). The polymer skeleton of the polymer (E-2) was branched. The obtained polymer was 1By H NMR measurement, the proportion of each group to the total of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups was calculated, and it was found that the hydrolyzable silyl group-containing structure represented by general formula (1) accounted for 98%, the 1-propenyl groups for 2%, the propyl groups for 0%, and the allyl groups for 0%.

[0180] (Comparative Example 5) To an allyl group-containing polyoxyalkylene polymer (C-2), 50 ppm of a commercially available Karstedt catalyst and dimethoxymethylsilane (5.0 molar equivalents relative to the allyl groups in the polymer (C-2)), which is a hydrosilane compound (D), were added, and a hydrosilylation reaction of the allyl groups in the polymer (C-2) was carried out at 90°C. 1 H NMR measurement was carried out, and it was confirmed that the allyl groups in the polymer (C-2) had been completely consumed one hour after the start of the reaction. The volatile components were then distilled off under reduced pressure to obtain a hydrolyzable silyl group-containing polyoxyalkylene polymer (E'-3). 1 By H NMR measurement, the proportion of each group relative to the total of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups was calculated, and it was found that the hydrolyzable silyl group-containing structure represented by general formula (1) accounted for 80%, the 1-propenyl groups for 19%, the propyl groups for 1%, and the allyl groups for 0%.

[0181] Comparative Example 6 To the hydroxyl group-containing polyoxyalkylene polymer (F-2) obtained in Synthesis Example 2, 0.9 molar equivalents of sodium methoxide relative to the hydroxyl groups of the polymer (F-2) were added as a 28% methanol solution. After removing the methanol by distillation under reduced pressure, 1.2 molar equivalents of 3-chloro-2-methyl-1-propene (methallyl chloride) relative to the hydroxyl groups of the polymer (F-2) were added and the mixture was reacted at 130°C for 1 hour to convert the terminal hydroxyl groups to methallyl groups, after which the 3-chloro-2-methyl-1-propene (methallyl chloride) was distilled off under reduced pressure. Thereafter, 0.6 molar equivalents of sodium methoxide relative to the hydroxyl groups of the polymer (F-2) were added as a 28% methanol solution. After removing the methanol by distillation under reduced pressure, 0.7 molar equivalents of 3-chloro-2-methyl-1-propene (methallyl chloride) relative to the hydroxyl groups of polymer (F-2) were added and the reaction was carried out at 130°C for 1 hour to convert the remaining terminal hydroxyl groups to methallyl groups, and then the 3-chloro-2-methyl-1-propene (methallyl chloride) was distilled off under reduced pressure. The resulting unpurified methallyl group-containing polyoxyalkylene polymer was mixed and stirred with n-hexane and water, after which the water was removed by centrifugation. The hexane was then distilled off under reduced pressure from the resulting hexane solution to remove the metal salts in the polymer. In this manner, a methallyl group-containing polyoxyalkylene polymer (G-2) was obtained.

[0182] To the methallyl group-containing polyoxyalkylene polymer (G-2), 100 ppm of Karstedt's catalyst and 1,000 ppm of 2,5-di-t-butyl-1,4-benzoquinone were added, and further, dimethoxymethylsilane (1.5 molar equivalents relative to the methallyl groups in the polymer (G-2)) as the hydrosilane compound (D) was added, and the hydrosilylation reaction of the methallyl groups in the polymer (G-2) was carried out at 100°C. 1 H NMR measurement was carried out, and it was confirmed that the methallyl groups of the polymer (G-2) were completely consumed 6 hours after the start of the reaction, and the volatile components were distilled off under reduced pressure to obtain a hydrolyzable silyl group-containing polyoxyalkylene polymer (E'-4). 1By H NMR measurement, the proportion of each group to the total of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups was calculated, and the proportion of hydrolyzable silyl groups was 97%. However, the hydrolyzable silyl group-containing structure not represented by general formula (1) (hydrolyzable silyl group-containing structure having an isobutylene group instead of the trimethylene group in general formula (1)) was predominant, and the proportion of hydrolyzable silyl group-containing structure represented by general formula (1) was less than 85%.

[0183] Example 4 Using a 5 L planetary mixer (manufactured by Dalton Co., Ltd.), a one-component curable composition was prepared according to the formulation shown in Table 2. First, 160 parts by weight of Hakuenka CCR (manufactured by Shiraishi Calcium Co., Ltd.: precipitated calcium carbonate), 54 parts by weight of Whiten SB (manufactured by Shiraishi Calcium Co., Ltd.: heavy calcium carbonate), and 5 parts by weight of Typen R820 (manufactured by Ishihara Sangyo Kaisha, Ltd.: titanium oxide) were dried under reduced pressure at 120°C for 2 hours. Next, 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E-2) obtained in Example 3, 90 parts by weight of DINP (diisononyl phthalate manufactured by J-Plus Corporation), 2 parts by weight of Disparlon 6500 (fatty acid amide wax manufactured by Kusumoto Chemical Co., Ltd.), 1 part by weight of Tinuvin 326 (2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chlorobenzotriazole manufactured by BASF), and 1 part by weight of Tinuvin 770 (light stabilizer manufactured by BASF) were each charged into a mixer and kneaded for 10 minutes. The resulting mixture was taken out and passed through a three-roll mill once to uniformly disperse the mixture, and then charged back into the mixer and dehydrated under reduced pressure for 2 hours. After dehydration under reduced pressure, the mixture was cooled to 50°C or below, and then 3 parts by weight of A-171 (manufactured by Momentive: vinyltrimethoxysilane), 3 parts by weight of A-1120 (manufactured by Momentive: N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane), and 2 parts by weight of Neostan U-220H (manufactured by Nitto Kasei Co., Ltd.: dibutyltin bis(acetylacetonate)) were added and kneaded for 3 minutes. After degassing under reduced pressure for 2 minutes, the resulting mixture was immediately filled into a moisture-proof aluminum cartridge and sealed to obtain a curable composition. The resulting curable composition was used to evaluate the skinning time, dumbbell tensile properties, and tensile shear strength in the same manner as in Example 2. The results are shown in Table 2.

[0184] Comparative Example 7 A curable composition was obtained in the same manner as in Example 4, except that 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E'-3) obtained in Comparative Example 5 was used instead of 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E-2). Using the obtained curable composition, the skin-stretching time, dumbbell tensile properties, and tensile shear strength were evaluated in the same manner as in Example 4. The results are shown in Table 2.

[0185] Comparative Example 8 A curable composition was obtained in the same manner as in Example 4, except that 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E'-4) obtained in Comparative Example 6 was used instead of 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E-2). Using the obtained curable composition, the skin-stretching time, dumbbell tensile properties, and tensile shear strength were evaluated in the same manner as in Example 4. The results are shown in Table 2.

[0186]

[0187] As can be seen from Table 2, polyoxyalkylene polymer (E-2) having a proportion of hydrolyzable silyl group-containing structures represented by general formula (1) of 85% or more exhibited a shorter skinning time and better curing properties than polyoxyalkylene polymer (E'-3) having a proportion of hydrolyzable silyl group-containing structures less than 85% and polyoxyalkylene polymer (E'-4) having a total proportion of hydrolyzable silyl group-containing structures of 85% or more but a proportion of hydrolyzable silyl group-containing structures represented by general formula (1) less than 85%. It also exhibited better tensile shear strength. Furthermore, in a dumbbell tensile test, hydrolyzable silyl group-containing polyoxyalkylene polymer (E-2) exhibited a higher modulus than hydrolyzable silyl group-containing polyoxyalkylene polymer (E'-3) and a value comparable to that of hydrolyzable silyl group-containing polyoxyalkylene polymer (E'-4).

[0188] Synthesis Example 3 Using polyoxypropylene glycol having a number average molecular weight of about 4,500 as an initiator, propylene oxide was polymerized in the presence of a zinc hexacyanocobaltate glyme complex catalyst to obtain a hydroxyl group-containing polyoxyalkylene polymer (F-3) having hydroxyl groups at both ends and a number average molecular weight of 15,000.

[0189] Example 5 Using a 5 L planetary mixer (manufactured by Dalton Co., Ltd.), a one-component curable composition was prepared according to the formulation shown in Table 3. First, 50 parts by weight of Hakuenka CCR (precipitated calcium carbonate manufactured by Shiraishi Calcium Co., Ltd.) and 70 parts by weight of Hiblack 10 (carbon black manufactured by Orion Engineered Carbons) were dried under reduced pressure at 120°C for 2 hours. Next, 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E-1) obtained in Example 1, 50 parts by weight of the hydroxyl group-containing polyoxyalkylene polymer (F-3) obtained in Synthesis Example 3 as a plasticizer, 1 part by weight of Tinuvin 326 (manufactured by BASF: 2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chlorobenzotriazole), and 1 part by weight of Tinuvin 770 (manufactured by BASF: light stabilizer) were each charged into a mixer and kneaded for 10 minutes. The resulting mixture was removed and passed through a three-roll mill once to uniformly disperse the mixture, and then charged back into the mixer and dehydrated under reduced pressure for 2 hours. After dehydration under reduced pressure, the mixture was cooled to 50°C or below, and then 3 parts by weight of A-171 (manufactured by Momentive: vinyltrimethoxysilane), 3 parts by weight of A-1120 (manufactured by Momentive: N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane), and 2 parts by weight of Neostan U-220H (manufactured by Nitto Kasei Co., Ltd.: dibutyltin bis(acetylacetonate)) were added and kneaded for 3 minutes. After degassing under reduced pressure for 2 minutes, the resulting mixture was immediately filled into a moisture-proof aluminum cartridge and sealed to obtain a curable composition. The resulting curable composition was used to evaluate the skinning time, dumbbell tensile properties, and tensile shear strength in the same manner as in Example 2. The results are shown in Table 3.

[0190] Comparative Example 9 A curable composition was obtained in the same manner as in Example 5, except that 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E'-2) obtained in Comparative Example 2 was used instead of 100 parts by weight of the hydrolyzable silyl group-containing polyoxyalkylene polymer (E-1). Using the obtained curable composition, the skin-strength time, dumbbell tensile properties, and tensile shear strength were evaluated in the same manner as in Example 5. The results are shown in Table 3.

[0191]

[0192] As can be seen from Table 3, polyoxyalkylene polymer (E-1) having a ratio of hydrolyzable silyl group-containing structures represented by general formula (1) of 85% or more exhibited a shorter skinning time and better curing properties than polyoxyalkylene polymer (E'-2) having a total ratio of hydrolyzable silyl group-containing structures of 85% or more but a ratio of hydrolyzable silyl group-containing structures represented by general formula (1) of less than 85%. In addition, the polyoxyalkylene polymer (E-1) exhibited a better rise in tensile shear strength.

[0193] The curable composition of Example 5, which contained carbon black as a reinforcing filler, exhibited a higher stress at break (TB) in a dumbbell tensile test and a higher stress at break (TB) in a tensile shear test after aging at 23°C for 3 days and then at 50°C for 4 days, compared to the curable compositions of Examples 2 and 4, which did not contain a reinforcing filler.

[0194] (Examples 6 and 7, and Comparative Examples 10 and 11) Using a 5 L planetary mixer (manufactured by Dalton Co., Ltd.), one-component curable compositions were prepared according to the formulations shown in Table 4. First, 160 parts by weight of Hakuenka CCR (manufactured by Shiraishi Calcium Co., Ltd.: precipitated calcium carbonate), 54 parts by weight of Whiten SB (manufactured by Shiraishi Calcium Co., Ltd.: heavy calcium carbonate), and 5 parts by weight of Typen R820 (manufactured by Ishihara Sangyo Kaisha, Ltd.: titanium oxide) were dried under reduced pressure at 120°C for 2 hours. Next, the types and amounts of polyoxyalkylene polymers having hydrolyzable silyl groups shown in Table 4, 2 parts by weight of DINP (diisononyl phthalate, manufactured by J-Plus Corporation), Disparlon 6500 (fatty acid amide wax, manufactured by Kusumoto Chemical Co., Ltd.), 1 part by weight of Tinuvin 326 (2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chlorobenzotriazole, manufactured by BASF), and 1 part by weight of Tinuvin 770 (light stabilizer, manufactured by BASF) shown in Table 4 were each charged into a mixer and kneaded for 10 minutes. The resulting mixture was removed and passed through a three-roll mill once to uniformly disperse the mixture, and then charged back into the mixer and dehydrated under reduced pressure for 2 hours. After dehydration under reduced pressure, the mixture was cooled to 50°C or below. Thereafter, 3 parts by weight of A-171 (manufactured by Momentive: vinyltrimethoxysilane), 3 parts by weight of A-1120 (manufactured by Momentive: N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane), and 2 parts by weight of Neostan U-220H (manufactured by Nitto Kasei Co., Ltd., dibutyltin bis(acetylacetonate)) were added and kneaded for 3 minutes. The mixture was then degassed under reduced pressure for 2 minutes, and the resulting mixture was immediately filled into a moisture-proof aluminum cartridge and sealed to obtain a curable composition. The resulting curable composition was used to evaluate the skinning time, dumbbell tensile properties, and tensile shear strength in the same manner as in Example 2. The results are shown in Table 4.

[0195] <Viscosity> In accordance with JIS K 7117-1, the viscosity of the curable composition was measured using a BS-type rotational viscometer (manufactured by Tokyo Keiki Co., Ltd.) with a No. 7 rotor at a measurement temperature of 25°C and a rotation speed of 10 rpm. The results are shown in Table 4.

[0196]

[0197] Table 4 shows that the curable compositions of Examples 6 and 7, which contain a polyoxyalkylene polymer (E), a plasticizer, and a filler, have a shorter skinning time and better curing properties than Comparative Examples 11 and 12. In particular, the curable composition of Example 6, which contains a plasticizer and a filler in a predetermined ratio, not only exhibits good curing properties but also provides a cured product with low viscosity, excellent workability, and a low modulus. Furthermore, the results of measuring the tensile shear strength show that the curable composition of Example 6 has the advantage of exhibiting high tensile shear strength in the early stages of curing.

[0198] (Example 8 and Comparative Examples 12 to 13) According to the compositions shown in Table 5, A-1120 (manufactured by Momentive: N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane) as an adhesion promoter and Ancamine K54 (manufactured by Anchor Chemical Co., Ltd.: 2,4,6-tris(dimethylaminomethyl)phenol) as an epoxy curing agent were added to a polyoxyalkylene polymer, and the mixture was thoroughly mixed with a spatula to obtain component A. Next, Neostan U-220H (manufactured by Nitto Kasei Co., Ltd.: dibutyltin bis(acetylacetonate)) as a curing catalyst was added to EP828 (manufactured by Mitsubishi Chemical Corporation: bisphenol A-type epoxy resin), and the mixture was thoroughly mixed with a spatula to obtain component B. The mixture obtained by mixing components A and B was stirred and degassed using a planetary centrifugal mixer (manufactured by Thinky Corporation: Awatori Rentaro) to obtain a curable composition. The obtained curable composition was used to evaluate the skinning time, dumbbell tensile properties, and tensile shear strength in the same manner as in Example 2. The results are shown in Table 5.

[0199] Table 5 shows that the curable composition of Example 8, which contains the polyoxyalkylene polymer (E) in combination with an epoxy compound, has better curability and gives a cured product with higher tensile shear strength than the curable compositions of Comparative Examples 12 and 13.

[0200] Synthesis Example 4 Propylene oxide was polymerized using butanol as an initiator with a zinc hexacyanocobaltate glyme complex catalyst to obtain a hydroxyl-containing polyoxyalkylene polymer (F-4) having a number average molecular weight of 7,800 and having a hydroxyl group at only one end. To the polymer (F-4), 0.75 mol equivalents of sodium methoxide relative to the hydroxyl groups of the polymer (F-4) were added as a 28% methanol solution. Methanol was removed from the resulting mixture by distillation under reduced pressure, and then 1.3 mol equivalents of allyl chloride relative to the hydroxyl groups of the polymer (F-4) were added, followed by a reaction at 130°C for 1 hour. Thereafter, unreacted allyl chloride was removed by distillation under reduced pressure from the reaction solution. Thereafter, 0.47 mol equivalents of sodium methoxide relative to the hydroxyl groups of the polymer (F-4) were added as a 28% methanol solution to the polymer (F-4). Methanol was removed from the resulting mixture by distillation under reduced pressure at 130°C, and then 2.1 mol equivalents of allyl chloride relative to the hydroxyl groups of polymer (F-4) were added and reacted at 130°C for 2 hours. Unreacted allyl chloride was then removed by distillation from the reaction solution. The resulting unpurified allyl group-containing polyoxypropylene polymer was mixed and stirred with n-hexane and water, and then the water was removed by centrifugation. The hexane was then removed from the resulting hexane solution by distillation under reduced pressure to remove metal salts from the polymer. As a result, an allyl group-containing polyoxyalkylene polymer (C-3) having an allyl group at only one end was obtained.

[0201] To the polymer (C-3), 50 ppm by weight of a commercially available Karstedt catalyst relative to the weight of the polymer (C-3) and 1.0 mol equivalent of dimethoxymethylsilane relative to the allyl groups of the polymer (C-3) were added, and a hydrosilylation reaction between the allyl groups of the polymer (C-3) and dimethoxymethylsilane was carried out at 90°C. 1 H NMR measurement was carried out, and it was confirmed that the allyl groups in the polymer (C-3) had completely disappeared 2 hours after the start of the reaction. Thereafter, volatile components were distilled off from the mixture under reduced pressure to obtain a polyoxyalkylene polymer (E'-5) having a hydrolyzable silyl group at only one end of its linear main chain skeleton. 1H NMR measurement was carried out to calculate the ratio of the number of hydrolyzable silyl groups, the number of 1-propenyl groups, the number of propyl groups, and the number of allyl groups to the total number of each group. As a result, the hydrolyzable silyl group-containing structure represented by general formula (1) was 80%, the 1-propenyl groups were 20%, the propyl groups were 0%, and the allyl groups were 0%.

[0202] Example 9 Using a 5 L planetary mixer (manufactured by Dalton Co., Ltd.), a one-component curable composition was prepared according to the formulation shown in Table 6. First, 160 parts by weight of Hakuenka CCR (manufactured by Shiraishi Calcium Co., Ltd.: precipitated calcium carbonate), 54 parts by weight of Whiten SB (manufactured by Shiraishi Calcium Co., Ltd.: heavy calcium carbonate), and 5 parts by weight of Typen R820 (manufactured by Ishihara Sangyo Kaisha, Ltd.: titanium oxide) were dried under reduced pressure at 120°C for 2 hours. Next, 60 parts by weight of the polyoxyalkylene polymer (E-1) obtained in Example 1, 40 parts by weight of the polyoxyalkylene polymer (E'-5) obtained in Synthesis Example 4, 90 parts by weight of DINP (diisononyl phthalate, manufactured by J-Plus Corporation), 2 parts by weight of Disparlon 6500 (fatty acid amide wax, manufactured by Kusumoto Chemical Co., Ltd.), 1 part by weight of Tinuvin 326 (2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chlorobenzotriazole, manufactured by BASF), and 1 part by weight of Tinuvin 770 (light stabilizer, manufactured by BASF) were each charged into a mixer and kneaded for 10 minutes. The resulting mixture was removed and passed through a three-roll mill once to uniformly disperse the components in the mixture. Thereafter, the mixture was charged into the mixer again and dehydrated under reduced pressure for 2 hours. After dehydration under reduced pressure, the mixture was cooled to 50°C or below. After cooling, 3 parts by weight of A-171 (manufactured by Momentive: vinyltrimethoxysilane), 3 parts by weight of A-1120 (manufactured by Momentive: N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane), and 2 parts by weight of Neostan U-220H (manufactured by Nitto Kasei Co., Ltd., dibutyltin bis(acetylacetonate)) were each added to the cooled mixture and kneaded for 3 minutes. The mixture was then degassed under reduced pressure for 2 minutes, and the resulting mixture was immediately filled into a moisture-proof aluminum cartridge and sealed to obtain a curable composition. The resulting curable composition was used to evaluate the skinning time, dumbbell tensile properties, and tensile shear strength in the same manner as in Example 2. The results are shown in Table 6.

[0203] (Example 10) A curable composition was obtained in the same manner as in Example 9, except that 60 parts by weight of the polyoxyalkylene polymer (E-1) and 40 parts by weight of the polyoxyalkylene polymer (E'-5) were changed to 100 parts by weight of the polyoxyalkylene polymer (E-1). Using the obtained curable composition, the skin-stretching time, dumbbell tensile properties, and tensile shear strength were evaluated in the same manner as in Example 9. The results are shown in Table 6.

[0204] Comparative Example 14 A curable composition was obtained in the same manner as in Example 9, except that 60 parts by weight of the polyoxyalkylene polymer (E-1) was replaced with 60 parts by weight of the polyoxyalkylene polymer (E'-2) obtained in Comparative Example 2. Using the obtained curable composition, the skin-stretching time, dumbbell tensile properties, and tensile shear strength were evaluated in the same manner as in Example 9. The results are shown in Table 6.

[0205] Comparative Example 15 A curable composition was obtained in the same manner as in Example 9, except that 60 parts by weight of the polyoxyalkylene polymer (E-1) and 40 parts by weight of the polyoxyalkylene polymer (E'-5) were changed to 100 parts by weight of the polyoxyalkylene polymer (E'-2). Using the obtained curable composition, the skin-stretching time, dumbbell tensile properties, and tensile shear strength were evaluated in the same manner as in Example 9. The results are shown in Table 6.

[0206]

[0207] Table 6 shows that the curable compositions of Examples 9 and 10 containing the polyoxyalkylene polymer (E) had a shorter skinning time and better curing properties than those of Comparative Examples 14 and 15. In particular, the curable composition of Example 9 containing a combination of the polyoxyalkylene polymer (E) and the polyoxyalkylene polymer (E') had good curing properties and a low modulus. Furthermore, it showed a better rise in tensile shear strength than Comparative Example 14, which had a similar modulus.

[0208] Example 11 A curable composition was obtained in the same manner as in Example 9, except that 60 parts by weight of the polyoxyalkylene polymer (E-1) was changed to 60 parts by weight of the polyoxyalkylene polymer (E-2). Using the obtained curable composition, the skinning time, dumbbell tensile properties, and tensile shear strength were evaluated in the same manner as in Example 9. However, the tensile shear strength test was not performed after 3 hours at 23°C. The results are shown in Table 7.

[0209] Example 12 A curable composition was obtained in the same manner as in Example 10, except that 100 parts by weight of the polyoxyalkylene polymer (E-1) was changed to 100 parts by weight of the polyoxyalkylene polymer (E-2). Using the obtained curable composition, the skin-stretching time, dumbbell tensile properties, and tensile shear strength were evaluated in the same manner as in Example 11. The results are shown in Table 7.

[0210] Comparative Example 16 A curable composition was obtained in the same manner as in Example 9, except that 60 parts by weight of the polyoxyalkylene polymer (E-1) was changed to 60 parts by weight of the polyoxyalkylene polymer (E'-4). Using the obtained curable composition, the skin-stretching time, dumbbell tensile properties, and tensile shear strength were evaluated in the same manner as in Example 11. The results are shown in Table 7.

[0211] Comparative Example 17 A curable composition was obtained in the same manner as in Example 10, except that 100 parts by weight of the polyoxyalkylene polymer (E-1) was changed to 100 parts by weight of the polyoxyalkylene polymer (E'-4). Using the obtained curable composition, the skin-stretching time, dumbbell tensile properties, and tensile shear strength were evaluated in the same manner as in Example 11. The results are shown in Table 7.

[0212]

[0213] Table 7 shows that the curable compositions of Examples 11 and 12 containing the polyoxyalkylene polymer (E) had a shorter skinning time and better curing properties than those of Comparative Examples 16 and 17. In particular, the curable composition of Example 11 containing a combination of the polyoxyalkylene polymer (E) and the polyoxyalkylene polymer (E') had good curing properties and a low modulus. Furthermore, it showed a better rise in tensile shear strength than Comparative Example 16, which had a similar modulus.

[0214] Synthesis Example 5 Using polyoxypropylene glycol having a number-average molecular weight of approximately 4,500 as an initiator, propylene oxide was polymerized in the presence of a zinc hexacyanocobaltate glyme complex catalyst to obtain a linear hydroxyl group-containing polyoxyalkylene polymer (F-5) having hydroxyl groups at both ends and a number-average molecular weight of 13,700. To the polymer (F-5), 1.1 mol equivalent of sodium methoxide relative to the hydroxyl groups of the polymer (F-5) was added as a 28% methanol solution. After removing the methanol from the resulting mixture by distillation under reduced pressure, 1.3 mol equivalent of allyl chloride relative to the hydroxyl groups of the polymer (F-5) was added and the reaction was carried out at 130°C for 1 hour. Thereafter, unreacted allyl chloride was removed by distillation under reduced pressure from the reaction solution. The resulting unpurified allyl group-containing polyoxyalkylene polymer was mixed and stirred with n-hexane and water, after which the water was removed by centrifugation. The hexane was then removed from the resulting hexane solution by distillation under reduced pressure to remove metal salts from the polymer. As a result, a linear allyl group-containing polyoxyalkylene polymer (C-4) was obtained. To the polymer (C-4), 50 ppm by weight of a commercially available Karstedt catalyst based on the weight of the polymer (C-4) and 0.74 mol equivalent of dimethoxymethylsilane based on the allyl groups contained in the polymer (C-4) were added, and a hydrosilylation reaction between the allyl groups contained in the polymer (C-4) and dimethoxymethylsilane was carried out at 90°C. The reaction was continued for 1 hour from the start of the reaction. 1H NMR measurement was carried out, and it was confirmed that the allyl groups in the polymer (C-4) had completely disappeared 2 hours after the start of the reaction. Thereafter, volatile components were distilled off from the mixture under reduced pressure to obtain a linear polyoxyalkylene polymer (E'-6) having a hydrolyzable silyl group. 1 H NMR measurement was carried out to calculate the ratio of the number of hydrolyzable silyl groups, the number of 1-propenyl groups, the number of propyl groups, and the number of allyl groups to the total number of each group. As a result, the hydrolyzable silyl group-containing structure represented by general formula (1) accounted for 74%, the 1-propenyl group for 17%, the propyl group for 0%, and the allyl group for 9%.

[0215] Example 13 A curable composition was obtained in the same manner as in Example 9, except that the blending amount of the polyoxyalkylene polymer (E-1) was changed to 50 parts by weight, and the blending amount of the polyoxyalkylene polymer (E'-5) was changed to 50 parts by weight. Using the obtained curable composition, the skinning time, dumbbell tensile properties, and tensile shear strength were evaluated in the same manner as in Example 9. However, the tensile shear strength test was not performed after 3 hours at 23°C. The results are shown in Table 8.

[0216] For comparison, Table 8 also lists the results of Example 10 and Comparative Example 15.

[0217]

[0218] Table 8 shows that the curable composition of Example 13 containing a combination of the polyoxyalkylene polymer (E) and the polyoxyalkylene polymer (E') has good curability and a low modulus.

Claims

1. General formula (1): (wherein R is the same or different and represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms; X is the same or different and represents a hydroxyl group or a hydrolyzable group; and a is 0, 1 or 2), wherein the ratio of the number of hydrolyzable silyl group-containing structures represented by general formula (1) to the total number of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups measured for the polymer is 0.85 to 1.00, and the number average molecular weight of the polymer exceeds 3,000.

2. The polyoxyalkylene polymer (E) according to claim 1, wherein the ratio of the number of hydrolyzable silyl group-containing structures represented by general formula (1) to the total number of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups measured for the polymer is 0.90 or more and 1.00 or less.

3. The polyoxyalkylene polymer (E) according to claim 1 or 2, wherein the hydrolyzable silyl group, 1-propenyl group, and propyl group are groups generated from an allyl group during a hydrosilylation reaction.

4. The polyoxyalkylene polymer (E) according to claim 1 or 2, wherein the number average molecular weight of the polymer is 10,000 or more.

5. The polyoxyalkylene polymer (E) according to claim 4, wherein the number average molecular weight of the polymer is 20,000 or more.

6. A polymer mixture comprising the polyoxyalkylene polymer (E) according to claim 1 and a ruthenium complex (A).

7. The polymer mixture according to claim 6, wherein the ruthenium complex (A) has a compound (B) as a ligand, and the compound (B) has at least one carbon-carbon double bond in one molecule, and an electron-withdrawing group is bonded to at least one of the carbon atoms forming the carbon-carbon double bond.

8. The polymer mixture according to claim 7, wherein compound (B) has a benzene ring skeleton as the skeleton containing the carbon-carbon double bond.

9. The polymer mixture according to claim 7, wherein compound (B) has a norbornadiene skeleton as the skeleton containing the carbon-carbon double bond.

10. The polymer mixture according to any one of claims 7 to 9, wherein the electron-withdrawing group is at least one selected from the group consisting of a fluoro group, a bromo group, and an iodo group.

11. A curable composition comprising the polyoxyalkylene polymer (E) according to claim 1 or the polymer mixture according to claim 6.

12. The curable composition according to claim 11, further comprising a reinforcing filler.

13. The curable composition according to claim 11, further comprising a plasticizer, a filler, and a curing catalyst, wherein the ratio of the polyoxyalkylene polymer (E) to the total of the components of the curable composition other than the curing catalyst is 5% by weight or more and 20% by weight or less, the ratio of the plasticizer to the total of the components of the curable composition other than the curing catalyst is 5% by weight or more and 65% by weight or less, the ratio of the filler to the total of the components of the curable composition other than the curing catalyst is 15% by weight or more and 90% by weight or less, and the ratio of the sum of the polyoxyalkylene polymer (E), the plasticizer, and the filler to the total of the components of the curable composition other than the curing catalyst is 80% by weight or more and 100% by weight or less.

14. The curable composition according to claim 11, further comprising a polyoxyalkylene polymer (E') containing a polyoxyalkylene polymer molecule having a hydrolyzable silyl group-containing structure represented by general formula (1), wherein the ratio of the number of hydrolyzable silyl group-containing structures represented by general formula (1) to the total number of hydrolyzable silyl groups, 1-propenyl groups, propyl groups, and allyl groups measured for said polymer (E') is 0.05 or more and less than 0.

85.

15. The curable composition according to claim 14, wherein the polyoxyalkylene polymer (E) has a number average molecular weight of 20,000 or more and 100,000 or less, and the polyoxyalkylene polymer (E') has a number average molecular weight of 800 or more and less than 20,000.

16. The curable composition according to claim 14, wherein the main chain structure of the polyoxyalkylene polymer (E) is branched.

17. The curable composition according to claim 14, wherein the polyoxyalkylene polymer (E') has a linear main chain structure, and the polyoxyalkylene polymer (E') has the hydrolyzable silyl group-containing structure only at one end of the linear main chain.

18. The curable composition of claim 11, further comprising an epoxy compound.

19. The curable composition of claim 18, further comprising an epoxy hardener.

20. A cured product obtained by curing the curable composition according to claim 11.

Citation Information

Patent Citations

  • JP1971027250B1

  • Receiving device

    JP1984015336A

  • Production of unsaturated group-terminated polyalkylene oxide

    JP1986215623A

  • Solenoid valve for fluid control

    JP1989060722A

  • Magnetic recording medium

    JP1990073512A

Cited By

  • Method for producing polyoxyalkylene-based polymer, polyoxyalkylene-based polymer, and curable composition

    WO2025063290A1

  • Polyoxyalkylene polymer, method for producing polyoxyalkylene polymer, and curable composition