Hot-rolled steel sheet with excellent crashworthiness and its manufacturing method
A high-strength hot-rolled steel sheet with a bainitic ferrite and martensite/austenite composite phase microstructure addresses yield strength and collision resistance issues, providing enhanced safety and formability.
Patent Information
- Application Number
- JP2023516578
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-22
- Filing Date
- 2021-09-13
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-09-13
AI Technical Summary
Existing hot-rolled steel sheets used in automobile chassis components lack sufficient yield strength and collision resistance, leading to inferior crash performance, while also facing challenges in formability and anisotropy during deformation.
A high-strength hot-rolled steel sheet with a microstructure comprising 55% bainitic ferrite and 10% martensite/austenite composite phase, controlled through specific alloy compositions and cooling processes, ensuring a yield strength of 750 MPa or more, tensile strength of 950 MPa or more, and minimal anisotropy.
The steel sheet achieves excellent yield strength, tensile strength, and formability, with a hole expandability of 25% or more, enhancing collision resistance and ensuring passenger safety.
Smart Images

Figure 0007569927000007 
Figure 0007569927000008 
Figure 0007569927000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a hot-rolled steel sheet that can be used for chassis structural members of automobiles, and more particularly to a high-strength hot-rolled steel sheet having excellent crash resistance and a method for manufacturing the same. [Background technology]
[0002] In recent years, the production and sales of environmentally friendly vehicles, including electric vehicles, have increased rapidly in order to curb global warming. When switching from internal combustion engine vehicles to electric vehicles, parts such as engines and transmissions are removed, so the design of electric vehicles tends to change in the direction of shortening the front structure of the vehicle. Since the front structure functions as an engine room and absorbs the energy of a frontal collision when a vehicle is rear-ended, structural members that are responsible for collision performance are also applied to the chassis parts under the body when designing electric vehicles, and this compensates for the inferior collision performance caused by the shortening of the front structure of the body. Since the collision performance of parts is proportional to the yield strength of the steel, a method is needed to improve the yield strength of hot-rolled steel sheets used for chassis parts.
[0003] On the other hand, since chassis parts are located at the lower end of the vehicle's center of gravity, reducing the weight of these parts is an area where fuel economy can be greatly improved. In order to maximize the weight reduction effect, technologies have been proposed that ensure formability suitable for press forming and improve the strength of steel sheets.
[0004] As an example, Patent Document 1 presents a manufacturing method of a steel sheet in which after finish rolling, ferrite is formed by maintaining the temperature in the 750-600°C range for a certain time, and then cooling to a martensite formation temperature range to form a microstructure consisting of 10-55% ferrite and 45-90% bainite and martensite, and which has a tensile strength of 950 MPa or more and excellent elongation and hole expandability. However, Patent Document 1 only considers the tensile strength and formability of the steel sheet, and does not mention the improvement of yield strength to ensure the safety of passengers in the event of a vehicle collision.
[0005] On the other hand, Patent Document 2 proposes a method of controlling the microstructure to 90% or more of bainitic ferrite and to improve hole expandability by controlling the fractions of martensite and bainite to 5% or less, respectively. According to the method of Patent Document 2, the tensile strength of the hot-rolled steel sheet is 980 MPa or more, and the hole expandability is 70% or more, but the yield ratio is 0.8 or less, so that the crash performance is degraded.
[0006] In Patent Document 3, in order to improve the yield strength of a steel sheet, a rolling temperature is controlled to be low to induce ferrite transformation during hot rolling, and the ferrite generated during rolling is work-hardened by continuous hot rolling, and the yield strength of the steel sheet is improved by the work-hardening of the ferrite. However, although Patent Document 3 is suitable as a method for improving the yield strength of a steel sheet, when the rolling temperature is low and deformation is applied to the ferrite, texture develops, and the difference in strength and formability depending on the deformation direction becomes large, which may cause restrictions when forming parts.
[0007] Therefore, in order to maximize the weight reduction of chassis parts, it is necessary to develop a steel material that has excellent strength and no anisotropy in formability, in particular, excellent yield strength, and can ensure the safety of passengers in the event of a rear-end collision. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Korean Patent Publication No. 2012-0011475 [Patent Document 2] Korean Patent Publication No. 2008-255484 [Patent Document 3] Korean Patent Publication No. 2020-0047625 Summary of the Invention [Problem to be solved by the invention]
[0009] An aspect of the present invention is to provide a hot-rolled steel sheet having high yield strength and excellent crashworthiness, and a method for manufacturing the same.
[0010] Meanwhile, the object of the present invention is not limited to the above-mentioned contents. The object of the present invention can be understood from the entire contents of this specification, and a person having ordinary skill in the art to which the present invention belongs will have no difficulty in understanding further object of the present invention. [Means for solving the problem]
[0011] One aspect of the present invention is In weight percent, it contains carbon (C): 0.05-0.13%, silicon (Si): 0.2-2.0%, manganese (Mn): 1.3-3.0%, aluminum (Al): 0.01-0.1%, phosphorus (P): 0.001-0.05%, sulfur (S): 0.001-0.05%, nitrogen (N): 0.001-0.02%, and the balance is Fe and other unavoidable impurities. The steel microstructure comprises, by area percentage, 55% or more of bainitic ferrite, 10% or more of martensite / austenite complex (MA), 95% or more of the sum of bainitic ferrite and martensite / austenite complex (MA), and less than 5% in total of granular ferrite, retained austenite, and carbides; The bainitic ferrite has an intragranular orientation difference of 1.5° or more and 10.5° or less, and the area fraction of the bainitic ferrite is 55% or more of the total area of the bainitic ferrite, The present invention relates to a high-strength hot-rolled steel sheet having an excellent yield strength, in which the average grain size of the martensite / austenite composite phase (MA) is 2.0 μm or less and the average interval is 0.3 μm or more.
[0012] The above-mentioned hot-rolled steel sheet may further contain, by weight percent, one or more of chromium (Cr): 0.01 to 2.0%, molybdenum (Mo): 0.01 to 2.0%, titanium (Ti): 0.01 to 0.2%, and niobium (Nb): 0.01 to 0.1%.
[0013] The area fraction of the martensite / austenite composite phase (MA) may be 10 to 45%.
[0014] The hot-rolled steel sheet may have a yield strength of 750 MPa or more, a tensile strength of 950 MPa or more, an elongation rate of 8% or more, a hole expandability of 25% or more, and a difference in elongation rate measured in the direction perpendicular to the rolling direction and the direction parallel to the rolling direction of 3% or less.
[0015] Another aspect of the present invention is reheating the steel slab having the above-mentioned alloy composition at 1100-1350 ° C; finish hot rolling the reheated steel slab while satisfying the following Relational Formula 1 and Relational Formula 2, in which the FDT (℃) of the hot rolled steel sheet immediately after the finish hot rolling is between 750 and 1150℃, and controlling the total reduction amount of the two passes of the final rolling to 10 to 40%; a step of primarily cooling the hot-rolled steel sheet to a temperature equal to or lower than the T1 temperature defined by the following Relation 3 between Ms and 520°C at a cooling rate of 50°C / s or more, and then secondary cooling to a coiling temperature between T1 and Ms-50°C at a cooling rate of 50°C / s or less; and and a step of final cooling the coiled hot-rolled steel sheet after the secondary cooling to room temperature. [Equation 1] FDT≧Tnr-50℃ Here, Tnr is the temperature at which recrystallization retardation begins, and Tnr = 795 + 88 × [C] + 45 × [Mn] + 23 × [Cr] + 760 × [Ti] + 480 × [Nb] - 80 × [Si], and each element represents weight percent. [Equation 2] Du = 3.7 + 0.36 × [C] - 1.21 × [Si] - 0.23 × [Mn] - 0.19 × [Cr] - 41.63 × [Ti] - 54.44 × [Nb] + 0.049 × [FDT-773] ≦ 10, Du is an index showing the effective grain size of austenite just before the first cooling after finish hot rolling, and each element means weight percentage. [Equation 3]
number
[0016] Ms is the temperature at which martensite begins to form upon cooling, and Ms = 550 - 330 x [C] - 41 x [Mn] - 20 x [Cr] - 10 x [Mo] + 30 x [Al] - 20 x [Si], where Ms is expressed in degrees Celsius and each element represents weight percent.
[0017] The above-mentioned hot-rolled steel sheet may contain one or more of chromium (Cr): 0.01 to 2.0%, molybdenum (Mo): 0.01 to 2.0%, titanium (Ti): 0.01 to 0.2%, and niobium (Nb): 0.01 to 0.1% by weight.
[0018] The method may further include pickling and oiling the steel sheet after the final cooling.
[0019] The method may further include a step of pickling the steel sheet after the final cooling and then heating it at a temperature range of 400 to 750° C. to hot-dip galvanize it. Effect of the Invention
[0020] According to the present invention, it is possible to provide a high-strength hot-rolled steel sheet having excellent yield strength, in which the yield strength is 750 MPa or more, the tensile strength is 950 MPa or more, and the difference in elongation between the direction perpendicular to the rolling and the direction perpendicular to the rolling is 3% or less. [Brief description of the drawings]
[0021] [Figure 1] 1A and 1B are photographs of the microstructure of steel in the examples of the present invention observed by an electron backscattering diffraction method attached to a scanning electron microscope, in which (a) shows Example 1 and (b) shows Comparative Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, preferred embodiments of the present invention will be described. However, the embodiments of the present invention can be modified into several other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those having average knowledge in the art.
[0023] The present inventors recognized that, although it is possible to manufacture a steel material having a tensile strength of 950 MPa or more in a conventional hot-rolled steel sheet, there is a problem in that the yield strength is low and the crash performance is deteriorated, and conducted in-depth research to solve this problem.
[0024] In order to increase the yield strength, it is effective to increase the dislocation density of the matrix structure in a microstructure composed of composite phases, thereby improving strength. However, when deformation is applied after or during the phase transformation of the matrix structure to cause work hardening, it was confirmed that although the yield strength is improved, the formation of texture increases the differences in material properties depending on the forming direction, resulting in inferior anisotropy.
[0025] Meanwhile, bainite is defined as a complex structure composed of bainitic ferrite formed by displacive phase transformation without diffusion, and secondary products produced by the subsequent diffusion of interstitial alloying elements such as carbon. The secondary products can exist as carbides, pearlite, or martensite / austenite complex phases depending on the temperature at which bainite is formed and the type of alloying elements.
[0026] Bainitic ferrite is formed by shear transformation, so screw dislocations are regularly arranged in the structure to reduce the amount of shear deformation generated during the transformation. After the transformation of edge dislocations generated in austenite to accommodate the volume expansion accompanying the formation of bainitic ferrite progresses, the transformation is completed by accumulating in the bainitic ferrite matrix. Therefore, the dislocation density of bainitic ferrite is at a high level, which is suitable for improving the yield strength of steel without the problem of poor anisotropy. However, since the density of dislocations generated in bainitic ferrite gradually decreases due to the recovery phenomenon while maintained in a temperature range above room temperature where bainitic transformation progresses, it was realized that it is important to manage the dislocation density in bainitic ferrite so that it can be maintained at an appropriate level, and researched this. As a result, it was recognized that a steel plate having excellent collision performance and high strength can be obtained by appropriately controlling the alloy composition range of the steel plate and the hot rolling and cooling conditions to optimize the fraction and size of the microstructure matrix and secondary phase, and the present invention was completed.
[0027] Hereinafter, a hot-rolled steel sheet having excellent yield strength according to one aspect of the present invention will be described in detail.
[0028] A hot rolled steel sheet having excellent yield strength according to one aspect of the present invention contains, by weight %, 0.05 to 0.13% carbon (C), 0.2 to 2.0% silicon (Si), 1.3 to 3.0% manganese (Mn), 0.01 to 0.1% aluminum (Al), 0.001 to 0.05% phosphorus (P), 0.001 to 0.05% sulfur (S), 0.001 to 0.02% nitrogen (N), the balance being Fe and other unavoidable impurities, and the steel microstructure contains, by area %, 55% or more bainitic ferrite, a martensite / austenite composite phase The bainitic ferrite has an intragranular orientation difference of 1.5° or more and 10.5° or less, and the area fraction of the bainitic ferrite is 55% or more of the total area of the bainitic ferrite. The martensite / austenite composite phase (MA) has an average grain size of 2.0 μm or less, and an average spacing of 0.3 μm or more.
[0029] Hereinafter, first, the reasons for limiting the alloy composition of the hot-rolled steel sheet of the present invention will be described in detail. In this case, unless otherwise specified, the content of each element means weight %.
[0030] Carbon (C): 0.05~0.13% Carbon (C) is the most economical and effective element for strengthening steel. As the C content increases, it suppresses the formation of granular ferrite during cooling, contributes to an increase in the bainite structure fraction, and diffuses into austenite during bainite transformation to stabilize the austenite, remaining in the martensite / austenite composite phase (MA) during the final cooling process, improving tensile strength.
[0031] If the C content is less than 0.05%, the fraction of martensite / austenite composite phase (MA) is low and tensile strength cannot be ensured. On the other hand, if the C content exceeds 0.13%, there is a problem that the tensile strength increases excessively and the formability and weldability decrease. Therefore, the C content in the present invention is preferably 0.05 to 0.13%. More preferably, it can be contained in a range of 0.06 to 0.11%.
[0032] Silicon (Si): 0.2-2.0% Silicon (Si) is an element that improves the hardening ability of steel, and plays a role in improving strength through the solid solution strengthening effect. It also delays the formation of carbides after bainite transformation, and improves tensile strength by making the secondary phase a martensite / austenite composite phase (MA).
[0033] If the Si content is less than 0.2%, carbides are formed, the fraction of martensite / austenite composite phase is low, and it is difficult to ensure tensile strength. On the other hand, if the Si content exceeds 2.0%, Fe-Si composite oxides are formed on the surface of the slab during reheating, which not only deteriorates the surface quality of the steel sheet, but also reduces weldability. Therefore, the Si content in the present invention is preferably 0.2 to 2.0%. More preferably, it can be contained in a range of 0.3 to 1.2%.
[0034] Manganese (Mn): 1.3-3.0% Manganese (Mn) is an element that improves the hardenability of steel, prevents the formation of granular ferrite during cooling after finish rolling and facilitates the formation of bainite.
[0035] If the Mn content is less than 1.3%, the hardening ability is insufficient and the fraction of granular ferrite increases excessively. On the other hand, if the Mn content exceeds 3.0%, the hardening ability increases significantly, the transformation of bainite does not occur smoothly in the cooling zone, and the internal dislocation density of bainitic ferrite decreases due to the temperature increase caused by reheating after coiling, which may cause buckling. Therefore, the Mn content in the present invention is preferably 1.3 to 3.0%, and more preferably 1.8 to 2.3%.
[0036] Aluminum (Al): 0.01-0.1% Aluminum (Al) is an element added for deoxidation, and some of it is present in the steel after deoxidation. If the content of Al exceeds 0.1%, it increases oxide and nitride inclusions in the steel, lowering the formability of the steel sheet. On the other hand, if the Al content is excessively reduced to less than 0.01%, it will result in an unnecessary increase in refining costs. Therefore, the content of Al in the present invention is preferably 0.01 to 0.1%.
[0037] Phosphorus (P): 0.001 to 0.05% Phosphorus (P) is an inevitable impurity and is a major cause of the deterioration of steel workability due to segregation, so it is preferable to control its content as low as possible. In theory, it is advantageous to limit the phosphorus content to 0%, but in order to reduce the P content to less than 0.001%, the manufacturing costs will increase excessively. Therefore, the P content in the present invention is preferably 0.001 to 0.05%.
[0038] Sulfur (S): 0.001-0.05% Sulfur (S) is an inevitable impurity that combines with Mn and other elements to form nonmetallic inclusions, which are the main cause of the deterioration of steel workability, and therefore it is preferable to control the content as low as possible. In theory, it is advantageous to limit the S content to 0%, but in order to reduce the S content to less than 0.001%, the manufacturing costs will increase excessively. Therefore, the S content in the present invention is preferably 0.001 to 0.05%.
[0039] Nitrogen (N): 0.001-0.02% Nitrogen is an element that is inevitably contained as an impurity and reacts with aluminum to precipitate fine nitrides, which reduces the workability of steel, so it is preferable to control its content as low as possible. In theory, it is advantageous to limit the N content to 0%, but in order to manufacture the N content to less than 0.001%, the manufacturing cost increases excessively. Therefore, in the present invention, the N content is preferably 0.001 to 0.02%.
[0040] In addition, in addition to the above-mentioned compositional components, the present invention can further contain, as necessary, one or more of chromium (Cr): 0.01 to 2.0%, molybdenum (Mo): 0.01 to 2.0%, titanium (Ti): 0.01 to 0.2%, and niobium (Nb): 0.01 to 0.1%.
[0041] Chromium (Cr): 0.01-2.0% Chromium (Cr) is an element that improves the hardening ability of steel, and inhibits the formation of ferrite during cooling after finish rolling, facilitating the formation of bainite. If the Cr content is less than 0.01%, the effect of adding Cr cannot be fully obtained. On the other hand, if the Cr content exceeds 2.0%, the hardening ability increases excessively, and there is a problem that bainite transformation does not occur smoothly in the cooling zone. Therefore, the Cr content in the present invention is preferably 0.01 to 2.0%, and more preferably 0.1 to 1.5%.
[0042] Molybdenum (Mo): 0.01-2.0% Molybdenum (Mo) is an element that improves the hardening ability of steel and plays a role in improving strength through the solid solution strengthening effect, so that it prevents the formation of ferrite during cooling after finish rolling and facilitates the formation of bainite. The Mo content slows down the diffusion rate of carbon and retards the rate of bainite transformation, so that if the Mo content exceeds 2.0%, there is a problem that bainite transformation does not occur smoothly in the cooling zone. On the other hand, if the Mo content is less than 0.01%, the additive effect of suppressing the formation of ferrite during cooling after finish rolling cannot be sufficiently obtained. Therefore, the Mo content in the present invention is preferably 0.01 to 2.0%, and more preferably 0.05 to 1.0%.
[0043] Titanium (Ti): 0.01-0.2% Titanium (Ti) is an element that forms carbonitrides, and refines the grains of austenite by delaying recrystallization during hot rolling, promotes the transformation of bainite in the cooling zone, and refines the grain size of martensite / austenite composite phase (MA) in the microstructure, thereby improving the strength of the steel. If the Ti content is less than 0.01%, the effect of adding the Ti cannot be fully obtained. On the other hand, if the Ti content exceeds 0.2%, coarse carbonitrides are generated, which reduces the toughness of the steel plate. Therefore, in the present invention, the Ti content is preferably 0.01 to 0.2%, and more preferably 0.02 to 0.10%.
[0044] Niobium (Nb): 0.01-0.1% Niobium (Nb) is an element that forms carbonitrides similarly to Ti. When niobium is added, it refines the grains of austenite by delaying recrystallization during hot rolling, promotes the transformation of bainite in the cooling zone, and refines the grain size of martensite / austenite composite phase (MA) in the microstructure, thereby improving the strength of the steel. When the content of Nb is less than 0.01%, the effect of addition is not sufficiently obtained, whereas when the content exceeds 0.1%, coarse carbonitrides are generated, reducing the toughness of the steel plate and increasing the rolling load during rolling, thereby reducing workability. Therefore, the content of Nb in the present invention is preferably 0.01 to 0.1%, and more preferably 0.01 to 0.05%.
[0045] The remaining component of the present invention is iron (Fe). However, in normal manufacturing processes, unintended impurities may be inevitably mixed in from raw materials or the surrounding environment, and this cannot be excluded. Since these impurities are known to anyone skilled in normal manufacturing processes, the contents of all of them are not specifically mentioned in this specification.
[0046] In the steel sheet of the present invention satisfying the above-mentioned alloy composition, the total area fraction of bainitic ferrite and martensite / austenite composite phase (MA: Martensite-Austenite constituents) is preferably 95% or more. If the total area fraction of bainitic ferrite and martensite / austenite composite phase (MA) is less than 95%, there is a problem that the excellent yield strength and tensile strength intended in the present invention cannot be ensured. In this case, the area fraction of the bainitic ferrite in the steel microstructure is preferably 55% or more, but if the area fraction is less than 55%, there is a problem that a yield strength of 750 MPa or more cannot be ensured.
[0047] Furthermore, the area fraction of the bainitic ferrite having an intragranular orientation difference of 1.5° or more and 10.5° or less is preferably 55% or more of the total area of the bainitic ferrite.
[0048] An important feature of the present invention is to control the dislocation density of the bainitic ferrite forming the matrix structure to an appropriate level. Dislocations in the bainitic ferrite remain in the structure due to delayed recovery of dislocations generated during shear transformation, or due to austenite after coiling being transformed into martensite and being introduced into the bainitic ferrite structure. Theoretically, it is possible to measure the dislocation density in such bainitic ferrite by measuring the thickness using a transmission electron microscope, calculating the number of observed dislocations, and measuring the density. However, since this method is not economical in considering the distribution of dislocation density by particle position, it was indirectly quantified through electron backscatter diffraction phase analysis (EBSD). The intra-particle orientation difference is a value calculated after defining adjacent grains as independent crystal grains when the orientation difference is 15° or more. On the other hand, when the intragranular orientation difference is 10.5° or more, it may be confused with a sibling crystal (variant) of adjacent bainitic ferrite, so the upper limit is set to 10.5°, and when the intragranular orientation difference is less than 1.5°, it falls within the measurement deviation range of EBSD analysis, and the accuracy decreases. In the present invention, it has been confirmed that the yield strength is improved when bainitic ferrite with an intragranular orientation difference of 1.5° to 10.5° accounts for 55% or more of the total bainitic ferrite area. More preferably, it may include 60% or more. There is no need to limit the upper limit, but when it exceeds 95%, the elongation rate may deteriorate, so it is also preferable to control it to 95% or less.
[0049] On the other hand, the area fraction of the martensite / austenite composite phase (MA) is preferably 10% or more. In the present invention, the martensite / austenite composite phase (MA) plays a role of improving the tensile strength of the steel by dispersing in the structure and acting as an obstacle to hinder the movement of dislocations, and at the same time plays a role of introducing additional dislocations into the inside of the bainitic ferrite by transforming austenite to martensite during cooling after coiling, thereby improving the yield strength of the steel. If the area fraction of the martensite / austenite composite phase (MA) is less than 10%, the intended improvement in tensile strength and yield strength cannot be expected. On the other hand, if the area fraction of the martensite / austenite composite phase (MA) is excessive, the strength of the steel increases excessively and the formability decreases. Therefore, in the present invention, the area fraction of the martensite / austenite composite phase (MA) is preferably 10 to 45%, more preferably 15 to 35%.
[0050] In this case, it is preferable that the average grain size of the martensite / austenite composite phase (MA) is 2.0 μm or less and the average interval is 0.3 μm or more. The martensite / austenite composite phase (MA) improves the tensile strength of steel by a mechanism such as dispersion strengthening, so when it is evenly dispersed in fine sizes, the strengthening efficiency is high. The present inventors have confirmed that when the average grain size of the martensite / austenite composite phase (MA) is 2.0 μm or less and the average interval is 0.3 μm or more, the hole expandability is excellent. Considering that chassis parts are often manufactured by burring molding, it is preferable that the hole expandability is as excellent as possible. Generally, the hole expandability of steel utilizing the martensite / austenite composite phase (MA) is not excellent because the hardness difference with the matrix structure is large, but it has been confirmed that good hole expandability can be ensured when the hardness difference is reduced by introducing dislocations into the matrix structure as in the present invention, and the size of the martensite / austenite composite phase (MA) is finely controlled to prevent local deformation concentration. In order to prevent localized deformation concentration, the average grain size of the martensite / austenite composite phase (MA) is preferably 2.0 μm or less, and the average spacing of the composite phase is preferably 0.3 μm or more so that deformation concentrations occurring at different positions do not overlap.
[0051] In another aspect of the present invention, the steel microstructure may contain less than 5% total of granular ferrite, retained austenite and carbides.
[0052] Ferrite formed during cooling after finish rolling is usually formed by diffusion transformation, and is characterized by low strength. However, when less than 5% is added as in the present invention, the residual austenite after ferrite formation transforms into bainite and martensite, and the previously formed ferrite also undergoes shear deformation to accommodate particle deformation during the transformation, so that the dislocation density inside the granular ferrite is maintained at a high level and the strength of the steel is not significantly reduced. On the other hand, if it is present at 5% or more, it reduces the strength of the steel, so it is necessary to control the upper limit to less than 5%.
[0053] When the transformation of bainite progresses during cooling in the cooling zone or after coiling, carbon diffuses and moves from bainitic ferrite to untransformed austenite. The carbon diffusion coefficient in austenite is significantly reduced, and the carbon concentration inside the austenite has an uneven distribution, so that in the area where carbon is locally excessively concentrated, it cannot be transformed into martensite during cooling to room temperature and may remain as austenite. Since the phase stability of such retained austenite is not high, even if it is observed as austenite after manufacturing the steel plate, it transforms into martensite by induced plastic transformation at the stage of manufacturing parts and applying deformation, thereby playing a role in increasing the tensile strength of the steel. Therefore, in the present invention, the fractions of martensite and austenite are not separately controlled. However, if the content of such austenite is too high, it may induce embrittlement phenomenon related to hydrogen accumulation, so it is necessary to control the upper limit to less than 5%.
[0054] Iron carbides can be generated with the diffusion of carbon into austenite during bainite transformation. In the present invention, the strength is improved by utilizing the martensite / austenite composite phase (MA), so the generation of iron carbides may cause a decrease in the fraction of the martensite / austenite composite phase (MA). Therefore, excessive generation of iron carbides hinders the strengthening effect intended by the present invention. On the other hand, when Ti and Nb are added, alloy carbonitrides may be present. In this case, further strengthening effects due to grain refinement can be expected, but since coarse carbides reduce the toughness of the steel, it is necessary to control the carbides present in the steel to less than 5% in terms of area fraction.
[0055] The steel plate of the present invention having the above-mentioned alloy composition and microstructure has a yield strength of 750 MPa or more, a tensile strength of 950 MPa or more, an elongation rate of 8% or more, and a hole expandability of 25% or more, thereby ensuring excellent collision performance.
[0056] Next, a method for producing a high strength hot rolled steel sheet excellent in yield strength, which is another aspect of the present invention, will be described in detail.
[0057] The high-strength hot-rolled steel sheet having excellent yield strength according to the present invention can be produced through a series of steps of reheating, hot rolling, cooling and coiling a steel slab having the alloy composition as described above. Specifically, the method for producing a hot-rolled steel sheet of the present invention includes the steps of reheating a steel slab having the above-mentioned alloy composition at 1100 to 1350°C; finish hot rolling the reheated steel slab while satisfying the following Relational Formula 1 and Relational Formula 2 and controlling the total reduction amount of two passes of final rolling to 10 to 40% so that FDT (°C), which is the temperature of the hot-rolled steel sheet immediately after finish hot rolling, is between 750 and 1150°C. The steps are: primary cooling of the hot-rolled steel sheet to a temperature equal to or lower than T1 temperature defined by the following Relational Formula 3 between Ms and 520°C at a cooling rate of 50°C / s or more, followed by secondary cooling to a coiling temperature between T1 and Ms-50°C at a cooling rate of 50°C / s or less; and final cooling of the coiled hot-rolled steel sheet after the secondary cooling to room temperature.
[0058] The conditions for each manufacturing step will be described in detail below.
[0059] steel slab reheating In the present invention, it is preferable to reheat the steel slab and perform a homogenization process before hot rolling, and the reheating process is preferably performed at 1100 to 1350°C. If the reheating temperature is less than 1100°C, there is a problem that the homogenization of the alloy elements is insufficient. On the other hand, if the temperature exceeds 1350°C, oxides are excessively formed on the slab surface, which deteriorates the surface quality of the steel sheet, and this is not preferable.
[0060] Hot rolling The reheated steel slab is hot-rolled to produce a hot-rolled steel sheet. At this time, it is preferable that the rolling is performed while controlling the total reduction amount of the final two rolling passes to be 10 to 40%, and that the FDT (°C), which is the temperature of the hot-rolled steel sheet immediately after the finish hot rolling, is between 750 and 1150°C and satisfies the following Relational Formula 1 and Relational Formula 2. [Equation 1] FDT≧Tnr-50℃ Here, Tnr is the temperature at which recrystallization retardation begins, and Tnr = 795 + 88 × [C] + 45 × [Mn] + 23 × [Cr] + 760 × [Ti] + 480 × [Nb] - 80 × [Si], and each element represents weight percent. [Equation 2] Du = 3.7 + 0.36 × [C] - 1.21 × [Si] - 0.23 × [Mn] - 0.19 × [Cr] - 41.63 × [Ti] - 54.44 × [Nb] + 0.049 × [FDT-773] ≦ 10, Du is an index showing the effective grain size of austenite just before the first cooling after finish hot rolling, and each element means weight percentage.
[0061] If the hot rolling is started at an FDT higher than 1150°C, oxides are excessively formed on the surface of the steel sheet after rolling and are not effectively removed even after pickling, resulting in poor surface quality. On the other hand, if hot rolling is performed at an FDT lower than 750°C, the rolling load increases excessively, resulting in poor workability, and ferrite is formed during rolling, resulting in poor anisotropy.
[0062] The total reduction in the last two passes during finish hot rolling is preferably between 10 and 40%. Usually, the main reason for performing hot rolling in multiple passes is to reduce the rolling load and precisely control the thickness. If the total reduction in the last two passes exceeds 40%, the rolling load in the last two passes increases excessively, resulting in poor workability. On the other hand, if the total reduction in the last two passes is less than 10%, the temperature of the steel sheet drops rapidly, resulting in poor workability.
[0063] In steel sheets during or after hot rolling, work hardening, recovery, and recrystallization occur, causing changes in the grain size and internal energy of austenite. In general, in order to improve material anisotropy, it is common to minimize the formation of texture by controlling the finish hot rolling temperature (FDT) to be equal to or higher than the recrystallization temperature (Tnr). Meanwhile, in bainite transformation, the microstructure differentiates into multiple variants to internally accommodate the shear deformation accompanying the phase transformation. Due to this characteristic, bainite generated by shear transformation forms a texture without being affected much by the rolling temperature compared to ferrite generated by diffusion transformation. However, when the rolling temperature is low and the accumulated deformation of austenite is large, the formation of variants may occur selectively in a direction that offsets the internal deformation of austenite, in which case texture is formed and anisotropy is poor. Therefore, it is preferable to perform the rolling end temperature at a temperature equal to or higher than the temperature defined in the above Relation 1.
[0064] Meanwhile, the grain size of austenite after hot rolling is affected by alloy components, rolling end temperature and reduction amount, and affects the ferrite and bainite formation behavior and final microstructure in the subsequent cooling process. In the present invention, the size of martensite / austenite composite phase (MA), which is one of the important constituent phases, increases as the austenite grain size after hot rolling increases. In the present invention, it was confirmed that the grain size of austenite can be calculated as Du in the above Relational Equation 2 depending on the rolling end temperature and the type of alloying elements added under the condition that the total final rolling reduction is 10 to 40%, and that if the value exceeds 10, the grain size of martensite / austenite composite phase (MA) exceeds 2 μm, resulting in a decrease in hole expandability.
[0065] Cooling Phase After the above hot rolling, the hot-rolled steel sheet is preferably primarily cooled at a cooling rate of 50°C / s or more to a temperature T1 between Ms and 520°C that satisfies the following relational expression 3, and then secondarily cooled at a cooling rate of 50°C / s or less to a coiling temperature between T1 and Ms-50°C.
[0066] The density of dislocations generated during bainite transformation gradually decreases due to a recovery phenomenon, and the degree of dislocation density disappearance increases as the bainite transformation temperature increases. In order to maintain the dislocation density intended in the present invention, the bainite transformation temperature must be less than 520°C, so the upper limit of the first cooling end temperature T1 is preferably 520°C. On the other hand, if the first cooling end temperature is equal to or lower than Ms, the martensitic transformation will progress rapidly and the fraction of martensite / austenite composite phase (MA) will increase excessively. Therefore, the first cooling end temperature T1 is preferably between Ms and 520°C.
[0067] On the other hand, in the present invention, since the total area fraction of bainitic ferrite and martensite / austenite composite phase (MA) must be 95% or more, it is necessary to effectively suppress the formation of granular ferrite during the primary cooling process. It has been confirmed that when the alloy composition proposed in the present invention satisfies the above-mentioned relational expression 2, it is possible to control the formation of granular ferrite to less than 5% when the primary cooling rate is 50°C / s or more. There is no particular upper limit to the primary cooling rate, but since there is a possibility that the plate may warp if the steel plate is cooled rapidly, it is preferable to control it to 200°C / s or less.
[0068] Furthermore, the inventors have confirmed that it is possible to manufacture a steel sheet having excellent strength using a steel having the alloy composition proposed in the present invention, but have conducted repeated research and experiments to solve the phenomenon in which buckling after coiling reduces the workability of subsequent processes. As a result, it has been confirmed that the cause of buckling is that the amount of bainite formed before coiling is small, and that buckling occurs due to transformation sintering as phase transformation progresses after coiling. It has also been confirmed that in order to prevent buckling from occurring after coiling, the generation of bainite needs to be 60% or more in the cooling stage before coiling. However, in order to increase the generation fraction of bainite before coiling, it is most effective to increase the maintenance time before coiling.
[0069] In the manufacturing process of steel products, rolling-cooling-coiling are performed by equipment arranged in a continuous manner, so that the maintenance time before coiling can be increased by increasing the length of the cooling zone or decreasing the rolling speed. However, since increasing the length of the cooling zone incurs costs and decreasing the rolling speed induces a decrease in productivity, the time required to pass through the cooling zone can be limited in a conventional hot rolling manufacturing process. Therefore, the present invention is characterized in that it is proposed to ensure the fraction of bainite transformation amount before coiling at a level at which buckling does not occur in a given time.
[0070] The present inventors confirmed that in order to prevent buckling, the fraction of phase transformation completed in the cooling zone before coiling must be 60% or more, and, taking into consideration that the cooling time that can be secured in a normal hot rolling process is 15 seconds or less, it was found that the primary cooling end temperature should be within the T1 temperature range defined by the following relational expression 3 while satisfying the range of Ms to 520°C. [Equation 3]
number
[0071] In the present invention, after the primary cooling, secondary cooling is performed at a cooling rate of 50°C / s or less to a coiling temperature between T1 and Ms-50°C. During the secondary cooling, austenite in which bainite transformation has progressed is stabilized, and the actual Ms temperature drops. Therefore, the lower limit of the secondary cooling end temperature can be applied to a temperature lower than the Ms temperature at which carbon concentration in untransformed austenite is not taken into consideration, and when bainite transformation has progressed by 60% or more, a temperature of Ms-50°C or more can be applied. Since bainite transformation progresses during the secondary cooling, a sudden temperature change may induce plate warpage, so the upper limit of the secondary cooling rate is set to 50°C / s.
[0072] Winding and final cooling stage Then, the hot-rolled steel sheet that has been subjected to the primary and secondary cooling is coiled at the secondary cooling end temperature, and then finally cooled to room temperature.
[0073] In the present invention, the steel sheet after the above-mentioned final cooling can be further subjected to pickling and oiling.
[0074] In addition, a hot-dip galvanizing process can be applied by heating the steel sheet after pickling in a temperature range of 400 to 750° C. The hot-dip galvanizing process can be performed using a zinc-based plating bath, and the alloy composition in the zinc-based plating bath is not particularly limited. EXAMPLES
[0075] The present invention will now be described in more detail with reference to the following examples.
[0076] (Example) A steel slab having the alloy composition shown in Table 1 below was prepared, and the remaining components of the alloy composition were Fe and inevitable impurities. A hot-rolled steel sheet was manufactured from the steel slab prepared in this way under the manufacturing conditions shown in Table 2 below. Specifically, the reheating temperature of the steel slab was 1200°C, the thickness of the hot-rolled steel sheet after hot rolling was 2.6 mm, and the total of the final 2 passes of finish rolling was 25%. Cooling immediately after hot rolling was performed at a cooling rate of 60 to 70°C / s, and the maintenance time from the first cooling to the second cooling was 15 seconds. In Table 2 below, the satisfaction or non-satisfaction of the above-mentioned Relational Formulas 1 to 3 is indicated by ○ and ×, with ○ indicating the case where the relational formula is satisfied and × indicating the case where the relational formula is not satisfied.
[0077] For each of the hot-rolled steel sheets produced above, mechanical properties such as yield strength (YS), tensile strength (TS), elongation (El), difference in elongation between the transverse direction and the direction perpendicular to the rolling (Del_El), and hole expansion (HER) were measured and are shown in Table 3. The microstructure of each of the hot-rolled steel sheets produced above was also observed and the results are also shown in Table 3.
[0078] Meanwhile, in the present invention, the yield strength and elongation indicate 0.2% off-set yield strength and breaking elongation, respectively. The yield strength, tensile strength, and elongation are measured by taking a standard test piece of JIS-5 in a direction perpendicular to the rolling direction and testing it. Meanwhile, Del_El is a result value indicating the difference between the breaking elongation measured in a direction parallel to the rolling direction of the above-mentioned standard test piece and the breaking elongation measured in a direction perpendicular to the rolling direction.
[0079] The fraction of bainitic ferrite phase and martensite / austenite composite phase (MA) formed in the microstructure of the steel was analyzed at 1000x magnification using an optical microscope and an image analyzer after etching the test specimens using the Repera etching method. The misorientation within the grains of bainitic ferrite was measured using electron backscattered diffraction.
[0080] The electron backscatter diffraction method uses a measuring device attached to a scanning electron microscope, an acceleration voltage of 20 kV, and an area of 50 μm x 50 μm is measured at intervals of 70 nm. TM An analysis program was used.
[0081] [Table 1]
[0082] [Table 2]
[0083] [Table 3]
[0084] As shown in Tables 1 to 3, in Examples 1 to 14, which satisfy both the alloy composition and manufacturing conditions proposed in the present invention, the microstructure has an area fraction of bainitic ferrite of 55% or more, an area fraction of martensite / austenite composite phase (MA) of 10% or more, and a total area fraction of these structures of 95% or more. In addition, the average grain size of the martensite / austenite composite phase (MA) is 2.0 μm or less, and the average interval of the composite phase is 0.3 μm or more, thereby ensuring the intended strength and formability.
[0085] This shows that the steel sheet of the present invention can ensure a yield strength of 750 MPa or more, a tensile strength of 950 MPa or more, an elongation rate of 8% or more, a Del_El of less than 3%, and a HER of 25% or more.
[0086] In contrast, in Comparative Example 1, the C content was less than 0.05%, and the martensite / austenite composite phase (MA) could not ensure an area fraction of 10%, and a tensile strength of 950 MPa or more could not be ensured.
[0087] In Comparative Example 2, the Mn content was excessively high, and a sufficient amount of bainite transformation did not occur before coiling, so there was a risk of buckling occurring after coiling.
[0088] In Comparative Example 3, the Cr content was excessively high, and a sufficient amount of bainite transformation did not occur before coiling, so there was a risk of buckling occurring after coiling.
[0089] In Comparative Example 4, the primary cooling end temperature and secondary cooling end temperature were too high, causing excessive disappearance of internal dislocations in bainitic ferrite, and the area fraction of bainitic ferrite grains with an orientation difference of 1.5° to 10.5° could not be ensured to be 55% or more, resulting in deterioration of yield strength and tensile strength.
[0090] In Comparative Example 5, the rolling end temperature was too low to satisfy Relation 1, and selective formation of sibling crystals occurred, resulting in excessive material anisotropy, and the difference in elongation rate in each measurement direction exceeded 3%.
[0091] In Comparative Example 6, the primary cooling end temperature and the secondary cooling end temperature were excessively high, causing excessive disappearance of internal dislocations in bainitic ferrite, deteriorating the yield strength, and at the same time failing to satisfy Relational Formula 3. Therefore, the bainite transformation rate was slow, and the amount of bainite transformed before coiling could not be ensured to be 60% or more, resulting in problems with poor material quality and the risk of buckling occurring after coiling.
[0092] In Comparative Example 7, the rolling end temperature was too high to satisfy Relation 2, and the grain size of the martensite / austenite composite phase (MA) was excessively coarse. As a result, the hole expandability of 25% or more could not be ensured.
[0093] 1 shows photographs of the steel microstructures in the examples of the present invention observed by electron backscattering attached to a scanning electron microscope, where (a) shows Example 1 and (b) shows Comparative Example 4. In each photograph, black indicates the martensite / austenite composite phase (MA), white indicates regions where the intragranular misorientation of bainitic ferrite is less than 1.5°, and grey indicates regions where the intragranular misorientation of bainitic ferrite is 1.5° to 10.5°.
[0094] As described above, the detailed description of the present invention has been given of the preferred embodiment of the present invention, but it is obvious that those skilled in the art can make various modifications without departing from the scope of the present invention. Therefore, the scope of the present invention should not be limited to the described embodiment, but should be determined by the claims below as well as equivalents thereto.
Claims
1. By weight, carbon (C): 0.05-0.13%, silicon (Si): 0.2-2.0% , Manganese (Mn): 1.3 to 3.0%, Aluminum (Al): 0.01 to 0.1%, Phosphorus (P): 0.001-0.05%, Sulfur (S): 0.001-0.05%, Nitrogen (N ): 0.001 to 0.02%, with the balance being Fe and other unavoidable impurities; The steel microstructure is, in terms of area percentage, bainitic ferrite: 55% or more, martensite / Austenite complex phase (MA): 10% or more, bainitic ferrite and martensite The total of the ferrite / austenite composite phase (MA): 95% or more, and the remaining total: less than 5% ferrite, retained austenite and carbides. The bainitic ferrite has an intragranular orientation difference of 1.5° or more and 10.5° or less. The area fraction of bainitic ferrite is 55% or more of the total area of bainitic ferrite, The average grain size of the martensite / austenite composite phase (MA) is 2.0 μm or less. and an average spacing of 0.3 μm or more, and thus the high-strength hot-rolled steel sheet has excellent yield strength.
2. The hot-rolled steel sheet contains, by weight percent, chromium (Cr): 0.01 to 2.0%, molybdenum ( Mo): 0.01 to 2.0%, titanium (Ti): 0.01 to 0.2%, and niobium (Nb 2. The composition according to claim 1, further comprising at least one of the following: 0.01 to 0.1% of Cr, High strength hot rolled steel plate.
3. The area fraction of the martensite / austenite composite phase (MA) is 10 to 45%. The high strength hot rolled steel sheet having excellent yield strength according to claim 1.
4. The hot-rolled steel sheet has a yield strength of 750 MPa or more and a tensile strength of 950 MPa or more. The elongation ratio is 8% or more, the hole expansion is 25% or more, and the rolling perpendicular direction and the rolling parallel direction are 2. The high strength film having excellent yield strength according to claim 1, wherein the difference in the elongation ratio measured in the direction is 3% or less. degree hot rolled steel plate.
5. By weight, carbon (C): 0.05-0.13%, silicon (Si): 0.2-2.0% , Manganese (Mn): 1.3 to 3.0%, Aluminum (Al): 0.01 to 0.1%, Phosphorus (P): 0.001-0.05%, Sulfur (S): 0.001-0.05%, Nitrogen (N ): reheating a steel slab containing 0.001-0.02% of Mo, with the balance being Fe and other unavoidable impurities, at 1100-1350°C; The temperature of the hot-rolled steel sheet immediately after the reheated steel slab is FDT (°C) The following relational expressions 1 and 2 are satisfied between 750 and 1150°C, and the second pass of the final rolling a step of finish hot rolling while controlling the total reduction amount of the above to 10 to 40%; The hot-rolled steel sheet is primarily cooled at a cooling rate of 50° C. / s or more to a temperature that is equal to or lower than the T1 temperature defined by the following Relation 3 and satisfies the range of Ms to 520° C., and then T 1 Secondary cooling to a coiling temperature of between Ms-50° C. at a cooling rate of 50° C. / s or less; and The hot-rolled steel sheet is finally cooled to room temperature after the secondary cooling. The method for producing a high strength hot rolled steel sheet according to claim 1, wherein the high strength hot rolled steel sheet has excellent hardness. [Relationship 1] FDT≧Tnr-50℃ Here, Tnr is the temperature at which recrystallization delay begins, Tnr = 795 + 88 × [C] +45×[Mn]+23×[Cr]+760×[Ti]+480×[Nb]-80×[S i], and each element represents weight percent. [Relationship 2] Du=3.7+0.36×[C]-1.21×[Si]-0.23×[Mn]-0.1 9×[Cr]-41.63×[Ti]-54.44×[Nb]+0.049×[FDT- 773]≦10, Du is the effective grain size of austenite immediately before the first cooling after finish hot rolling. The percentages of each element are by weight. [Relationship 3] [0010] Here, T D =820-290×[C]-90×[Mn]-70×[Cr]-62×[ Mo]−35×[Si], where the content of each element means the weight content. Ms is the temperature at which martensite formation begins upon cooling, Ms = 550-330 ×[C]-41×[Mn]-20×[Cr]-10×[Mo]+30×[Al]-20× [Si], Ms is in ° C., and each element means weight %.
6. The hot-rolled steel sheet contains, by weight percent, chromium (Cr): 0.01 to 2.0%, molybdenum ( Mo): 0.01 to 2.0%, titanium (Ti): 0.01 to 0.2%, and niobium (Nb 6. The composition according to claim 5, further comprising at least one of the following: 0.01 to 0.1% of Cr, A method for manufacturing high strength hot rolled steel sheet.
7. The method according to claim 5, further comprising the step of pickling and oiling the steel sheet after the final cooling is completed. A method for manufacturing hot-rolled high-strength steel sheets with excellent yield strength.
8. After the final cooling, the steel plate is pickled and then heated to a temperature range of 400 to 750° C. to form a molten zinc alloy. The hot-rolled steel of claim 5, further comprising a step of plating with lead. The manufacturing method of the plate.
Citation Information
Patent Citations
Ultrahigh strength hot-rolled complex phase steel plate and production method thereof
CN109023036A
High-toughness, low-yield-ratio, high-strength steel sheet excellent in strain aging resistance
JP2013112872A
HIGH STRENGTH HOT ROLLED STEEL SHEET EXCELLENT IN STRETCH FLANGE-ABILITY AND LOW TEMPERATURE TOUGHNESS AND HAVING MAXIMUM TENSILE STRENGTH OF 980 MPa OR MORE AND PRODUCTION METHOD THEREFOR
JP2015196891A
Roll-forming capable high-strength hot-rolled steel sheet having excellent elongation flange formability, and method for producing the same
JP2018532045A
KR2008-255484