Positive electrode material for alkali metal-sulfur battery and alkali metal-sulfur battery having the same

Metal-doped carbonaceous materials in alkali metal-sulfur batteries address the stability issue by enhancing polysulfide binding, resulting in improved battery capacity and cycle life.

JP7570614B2Active Publication Date: 2024-10-22JIKU CHEM CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020150417
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-08
Publication Date
2024-10-22
Estimated Expiration
2040-09-08

AI Technical Summary

Technical Problem

Existing alkali metal-sulfur battery materials face issues with long-term cycling performance due to weak interactions between non-polar carbon and charged sulfur species, leading to insufficient stability during repeated charging and discharging.

Method used

Development of carbonaceous materials doped with metals such as Co and Ni, which enhance the binding of polysulfides and improve the stability of battery capacity by using a combination of metals, metal oxides, or metal salts with carbon materials.

Benefits of technology

The use of metal-doped carbonaceous materials results in improved stability of battery capacity during repeated charging and discharging cycles, outperforming previous materials in terms of specific capacity and cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570614000001
    Figure 0007570614000001
  • Figure 0007570614000002
    Figure 0007570614000002
  • Figure 0007570614000003
    Figure 0007570614000003
Patent Text Reader

Abstract

To provide a positive electrode material for an alkali metal-sulfur battery, improved in stability of battery capacity when charging and discharging are repeated, and an alkali metal-sulfur battery including the same.SOLUTION: There is provided a carbonaceous material used for a positive electrode material for an alkali metal-sulfur battery. The carbonaceous material includes: two or more kinds of metals, metal oxides or metal salts selected from a group consisting of Mn, Fe, Co, Ni, Cu, Zn, Mo, W, V, Zr, Sn, Sb, In, Bi, Fe2O3, Fe3O4, Co3O4, CoO, NiO, MnO2, Mn3O4, MnO, VO2, V2O5, MoO2, ZnO, ZrO2, Co(NO3)2, Ni(NO3)2, Fe(NO3)3, CoCl2, NiCl2, FeCl3, Fe(SO4)3, Co(CH3COO)2, and Ni(CH3COO)2; and a carbon material.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode material for an alkali metal-sulfur battery and an alkali metal-sulfur battery including the same. [Background technology]

[0002] As lithium-ion batteries are required to become larger, perform better, and cost less, alkali metal-sulfur batteries such as lithium secondary batteries are attracting attention as next-generation storage batteries that are superior in terms of safety, reliability, etc.

[0003] In alkali metal-sulfur batteries, a carbonaceous material with sulfur incorporated is typically used for the positive electrode, a material that absorbs and releases lithium ions is used for the negative electrode, and an electrolyte with lithium ion conductivity is used to fill the space between the positive and negative electrodes.

[0004] The positive electrode carbonaceous material has good electrical conductivity and large surface area, so when it is used as a sulfur host in lithium sulfur batteries (LSB), it ensures effective sulfur accommodation and rapid electron / ion transfer in the electrochemical process. However, due to the weak interaction between non-polar carbon and charged sulfur species, the long-term cycling performance is still insufficient. To solve these problems, the use of metal-doped carbonaceous materials as sulfur hosting materials is very promising for the realization of high-performance alkali metal-sulfur batteries, because the metal dopant can effectively bind to polysulfides and inhibit the back-and-forth transfer of polysulfides.

[0005] Non-Patent Document 1 discloses embedding monodisperse cobalt atoms in nitrogen-doped graphene and using it as a sulfur host material. Non-Patent Document 2 discloses the synthesis of cobalt-embedded nitrogen-doped hollow carbon nanorods using polydopamine. The carbon nanorods have excellent electrochemical performance as sulfur hosts in the positive electrodes of alkali metal-sulfur batteries. [Prior art documents] [Non-patent literature]

[0006] [Non-Patent Document 1] Journal of the American Chemical Society 141(2019):3977-3985 [Non-Patent Document 2] Energy Storage Materials 5(2016):223-229 Summary of the Invention [Problem to be solved by the invention]

[0007] However, the materials in the above-mentioned non-patent documents 1 and 2 have one or more drawbacks, either in the complexity of synthesis or in the poor stability of long-term cycle performance. Therefore, it is important to develop new sulfur host materials with high electrochemical performance, which are produced by a simple and low-cost method for synthesizing metal-doped carbonaceous materials for alkali metal-sulfur batteries.

[0008] Therefore, an object of the present invention is to provide a positive electrode material for an alkali metal-sulfur battery having improved stability of battery capacity during repeated charging and discharging, and an alkali metal-sulfur battery including the same. [Means for solving the problem]

[0009] As a result of intensive research into achieving the above object, the inventors have found that the above object can be achieved when a carbonaceous material containing cobalt (Co) and nickel (Ni) is used as a metal-doped carbonaceous material for a positive electrode of an alkali metal-sulfur battery, and have thus completed the present invention.

[0010] The present invention encompasses the embodiments described below. Item 1. A carbonaceous material used as a positive electrode material for an alkali metal-sulfur battery, comprising: Mn, Fe, Co, Ni, Cu, Zn, Mo, W, V, Zr, Sn, Sb, In, Bi, Fe 2 O3 , Fe 3 O 4 , Co 3 O 4 , CoO, NiO, MnO 2 , Mn 3 O 4 , MnO, VO 2 , V 2 O 5 , MoO 2 , ZnO, ZrO 2 , Co(NO 3 ) 2 , Ni(NO 3 ) 2 , Fe(NO 3 ) 3 , CoCl 2 , NiCl 2 , FeCl 3 , Fe(SO 4 ) 3 , Co(CH 3 COO) 2 , and Ni(CH 3 COO) 2 and a carbon material. Item 2. The carbonaceous material according to Item 1, wherein the carbon material is one or more selected from the group consisting of glucose, cellulose, lignin, chitosan, cellulose acetate, polythiophene; ethylenediaminetetraacetic acid (EDTA) or a salt thereof; glycolic acid, citric acid or a salt thereof, an organic salt derived from biomass; a nitrogen-containing carbon organic material which is polyaniline (PANI), polypyrrole (PPy), polyacrylonitrile, melamine, urea, monocyanamide, dicyandiamide, or cyanamide; biomass; a metal-organic framework; graphene; natural graphite or artificial graphite; acetylene black; carbon nanotubes; and carbon nanofibers. Item 3. The metal, metal oxide, or metal salt is Co 3 O 4 , CoO, Co(NO 3 ) 2 , CoCl 2 , and Co(CH 3 COO) 2At least one selected from the group consisting of Ni, NiO, Ni(NO 3 ) 2 , NiCl 2 , and Ni(CH 3 COO) 2 and at least one selected from the group consisting of: Item 4. A positive electrode material for an alkali metal-sulfur battery, comprising sulfur and the carbonaceous material according to any one of Items 1 to 3. Item 5. An alkali metal-sulfur battery comprising a positive electrode made of the positive electrode material according to item 4, a negative electrode, and an electrolyte filled between the positive electrode and the negative electrode. Item 6.Mn, Fe, Co, Ni, Cu, Zn, Mo, W, V, Zr, Sn, Sb, In, Bi, Fe 2 O 3 , Fe 3 O 4 , Co 3 O 4 , CoO, NiO, MnO 2 , Mn 3 O 4 , MnO, VO 2 , V 2 O 5 , MoO 2 , ZnO, ZrO 2 , Co(NO 3 ) 2 , Ni(NO 3 ) 2 , Fe(NO 3 ) 3 , CoCl 2 , NiCl 2 , FeCl 3 , Fe(SO 4 ) 3 , Co(CH 3 COO) 2 , and Ni(CH 3 COO) 2 mixing two or more metals, metal oxides, or metal salts selected from the group consisting of: Heating water or a solution containing the two or more metals, metal oxides, or metal salts and the carbon material to a temperature of 300° C. or higher and drying the water or solution. The present invention relates to a method for producing a carbonaceous material used as a positive electrode material for an alkali metal-sulfur battery, the method comprising the steps of: Item 7. Suspending the carbonaceous material according to any one of items 1 to 3 and sulfur powder in a solvent; and heating the resulting suspension to remove the solvent. The method for producing a positive electrode material for an alkali metal-sulfur battery includes the steps of: Effect of the Invention

[0011] The positive electrode material for the alkali metal-sulfur battery of the present invention is Mn, Fe, Co, Ni, Cu, Zn, Mo, W, V, Zr, Sn, Sb, In, Bi, Fe 2 O 3 , Fe 3 O 4 , Co 3 O 4 , CoO, NiO, MnO 2 , Mn 3 O 4 , MnO, VO 2 , V 2 O 5 , MoO 2 , ZnO, ZrO 2 , Co(NO 3 ) 2 , Ni(NO 3 ) 2 , Fe(NO 3 ) 3 , CoCl 2 , NiCl 2 , FeCl 3 , Fe(SO 4 ) 3 , Co(CH 3 COO) 2 , and Ni(CH 3 COO) 2 Since the positive electrode material contains two or more metals, metal oxides, or metal salts selected from the group consisting of: [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic exploded cross-sectional side view of an alkali metal-sulfur battery including a positive electrode made of a positive electrode material according to one embodiment of the present invention. [Diagram 2] Scanning electron microscope (SEM) photographs of various positive electrode materials: (A) nitrogen-doped carbon nanotubes doped with Co and Ni (Production Example 1), (B) nitrogen-doped carbon nanotubes doped with Ni (Comparative Production Example 1), (C) nitrogen-doped carbon nanotubes doped with Co (Comparative Production Example 2), (D) nitrogen-doped carbon nanotubes doped with Co and Ni and with sulfur added (Production Example 2), (E) nitrogen-doped carbon nanotubes doped with Ni and with sulfur added (Comparative Production Example 4), (F) nitrogen-doped carbon nanotubes doped with Co and with sulfur added (Comparative Production Example 5). [Diagram 3] Graph of XRD patterns of nitrogen-doped carbon nanotubes doped with Co and Ni with sulfur (top), nitrogen-doped carbon nanotubes doped with Co and Ni (middle), and sulfur (bottom). [Figure 4] Graphs showing the charge / discharge characteristics of alkali metal-sulfur batteries using as the positive electrode material (1) nitrogen-doped carbon nanotubes doped with Co and Ni with added sulfur, (2) nitrogen-doped carbon nanotubes doped with Ni with added sulfur, and (3) nitrogen-doped carbon nanotubes doped with Co with added sulfur. [Diagram 5] Graph showing the charge / discharge characteristics of alkali metal-sulfur batteries using as the positive electrode materials (1) nitrogen-doped carbon nanotubes doped with Co and Ni with added sulfur, and (2) doped carbon nanotubes without added metal doping with sulfur. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] FIG. 1 is a schematic exploded side view of an alkali metal-sulfur battery including a positive electrode made of a positive electrode material according to one embodiment of the present invention. A lithium-sulfur secondary battery 1, as an example of an alkali metal-sulfur secondary battery, includes a positive electrode (positive electrode layer, also referred to as a cathode) 10, a negative electrode (negative electrode layer, also referred to as an anode) 12 that absorbs and releases lithium ions, an electrolyte solution 14 having lithium ion conductivity that is filled between the positive electrode 10 and the negative electrode 12, a separator 16 that is disposed between the positive electrode 10 and the negative electrode 12 and provides insulation between the positive electrode 10 and the negative electrode 12 in the electrolyte solution 14, a positive electrode current collector 18 on the side of the positive electrode 10 opposite the separator 16, and a negative electrode current collector 20 on the side of the negative electrode 12 opposite the separator 16.

[0014] The positive electrode current collector 18 may be a general one made of a metal or the like, and may be, for example, an Al film, a Ni film, etc. The shape of the positive electrode current collector 18 is not particularly limited, but it may be a flat foil having a predetermined cross-sectional shape, such as a substantially circular or substantially rectangular shape, that matches the outer shape of the battery.

[0015] The positive electrode 10 is made of a carbonaceous material layer. The carbonaceous material layer is made of sulfur and Mn, Fe, Co, Ni, Cu, Zn, Mo, W, V, Zr, Sn, Sb, In, Bi, Fe 2 O 3 , Fe 3 O 4 , Co 3 O 4 , CoO, NiO, MnO 2 , Mn 3 O 4 , MnO, VO 2 , V 2 O 5 , MoO 2 , ZnO, ZrO 2 , Co(NO 3 ) 2 , Ni(NO 3 ) 2 , Fe(NO 3 ) 3 , CoCl 2 , NiCl 2 , FeCl 3 , Fe(SO 4 ) 3 , Co(CH 3 COO) 2 , and Ni(CH 3 COO)2 and a carbon material capable of retaining sulfur. More specifically, the carbonaceous material layer contains sulfur and Mn, Fe, Co, Ni, Cu, Zn, Mo, W, V, Zr, Sn, Sb, In, Bi, Fe 2 O 3 , Fe 3 O 4 , Co 3 O 4 , CoO, NiO, MnO 2 , Mn 3 O 4 , MnO, VO 2 , V 2 O 5 , MoO 2 , ZnO, ZrO 2 , Co(NO 3 ) 2 , Ni(NO 3 ) 2 , Fe(NO 3 ) 3 , CoCl 2 , NiCl 2 , FeCl 3 , Fe(SO 4 ) 3 , Co(CH 3 COO) 2 , and Ni(CH 3 COO) 2 and a carbonaceous material, which is a composite containing a carbon material and two or more metals, metal oxides, or metal salts selected from the group consisting of the above, in which sulfur is attached to the surface of the carbonaceous material.

[0016] The total amount of metal elements (i.e., metal content) derived from one or more of the above metals, metal oxides, or metal salts relative to the amount of carbon material (also referred to as the amount of carbon content) is not particularly limited, but from the viewpoint of improving the stability of the battery capacity during repeated charging and discharging, it is preferably 1 wt % to 20 wt %, more preferably 10 wt % to 15 wt %, relative to the amount of carbon material.

[0017] A preferred combination of two or more of the above metals, metal oxides, or metal salts is Co. 3 O 4 , CoO, Co(NO3 ) 2 , CoCl 2 , and Co(CH 3 COO) 2 At least one selected from the group consisting of Ni, NiO, Ni(NO 3 ) 2 , NiCl 2 , and Ni(CH 3 COO) 2 and at least one selected from the group consisting of: When a preferred combination of two or more metals, metal oxides, or metal salts is a combination of cobalt metal, oxide, or metal salt and nickel metal, oxide, or metal salt, from the viewpoint of improving the stability of the battery capacity during repeated charging and discharging, the amount of cobalt metal element (i.e., the metal content) derived from the cobalt metal, oxide, or metal salt is preferably 0.5 wt % to 10 wt %, more preferably 5 wt % to 7.5 wt %, relative to the amount of the carbon material, and the amount of nickel metal element (i.e., the metal content) derived from the nickel metal, oxide, or metal salt is preferably 0.5 wt % to 10 wt %, more preferably 5 wt % to 7.5 wt %, relative to the amount of the carbon material.

[0018] Examples of carbonaceous materials include, but are not limited to, carbon-rich organic materials including glucose, cellulose, lignin, chitosan, cellulose acetate, polythiophene, and the like; ethylenediaminetetraacetic acid (EDTA) or its salts; glycolic acid, citric acid or its salts; organic salts derived from biomass; nitrogen-containing carbonaceous organic materials such as polyaniline (PANI), polypyrrole (PPy), polyacrylonitrile, melamine, urea, monocyanamide, dicyandiamide, and cyanamide; biomass; metal-organic frameworks; graphene; graphite including natural graphite and artificial graphite; acetylene black; carbon nanotubes; and carbon nanofibers. One or more of these can be used in the synthesis of a carbonaceous material containing cobalt and nickel. The carbonaceous material is preferably a carbonaceous material such as graphite or carbon nanotubes, in that it has voids that can hold sulfur and can ensure electrical conductivity.

[0019] Mn, Fe, Co, Ni, Cu, Zn, Mo, W, V, Zr, Sn, Sb, In, Bi, Fe 2 O 3 , Fe 3 O 4 , Co 3 O 4 , CoO, NiO, MnO 2 , Mn 3 O 4 , MnO, VO 2 , V 2 O 5 , MoO 2 , ZnO, ZrO 2 , Co(NO 3 ) 2 , Ni(NO 3 ) 2 , Fe(NO 3 ) 3 , CoCl 2 , NiCl 2 , FeCl 3 , Fe(SO 4 ) 3 , Co(CH 3 COO) 2 , and Ni(CH 3 COO) 2 The total amount of the two or more metals, metal oxides, or metal salts selected from the group consisting of and the carbon material is preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, more preferably 90% by weight or more, and more preferably 95% by weight or more, based on the total amount of the carbonaceous material.

[0020] In one embodiment, the carbonaceous material is selected from the group consisting of Mn, Fe, Co, Ni, Cu, Zn, Mo, W, V, Zr, Sn, Sb, In, Bi, Fe 2 O 3 , Fe 3 O 4 , Co 3 O 4 , CoO, NiO, MnO 2 , Mn 3 O 4 , MnO, VO 2 , V 2 O 5 , MoO 2, ZnO, ZrO 2 , Co(NO 3 ) 2 , Ni(NO 3 ) 2 , Fe(NO 3 ) 3 , CoCl 2 , NiCl 2 , FeCl 3 , Fe(SO 4 ) 3 , Co(CH 3 COO) 2 , and Ni(CH 3 COO) 2 In another embodiment, the carbonaceous material consists essentially of two or more metals, metal oxides, or metal salts selected from the group consisting of Mn, Fe, Co, Ni, Cu, Zn, Mo, W, V, Zr, Sn, Sb, In, Bi, Fe 2 O 3 , Fe 3 O 4 , Co 3 O 4 , CoO, NiO, MnO 2 , Mn 3 O 4 , MnO, VO 2 , V 2 O 5 , MoO 2 , ZnO, ZrO 2 , Co(NO 3 ) 2 , Ni(NO 3 ) 2 , Fe(NO 3 ) 3 , CoCl 2 , NiCl 2 , FeCl 3 , Fe(SO 4 ) 3 , Co(CH 3 COO) 2 , and Ni(CH 3 COO) 2 The composite material is composed of two or more metals, metal oxides, or metal salts selected from the group consisting of the above, and a carbon material.

[0021] The positive electrode 10 is made of a positive electrode material containing Mn, Fe, Co, Ni, Cu, Zn, Mo, W, V, Zr, Sn, Sb, In, Bi, and Fe. 2 O 3 , Fe 3 O 4 , Co 3 O 4 , CoO, NiO, MnO 2 , Mn 3 O 4 , MnO, VO 2 , V 2 O 5 , MoO 2 , ZnO, ZrO 2 , Co(NO 3 ) 2 , Ni(NO 3 ) 2 , Fe(NO 3 ) 3 , CoCl 2 , NiCl 2 , FeCl 3 , Fe(SO 4 ) 3 , Co(CH 3 COO) 2 , and Ni(CH 3 COO) 2 By using a carbonaceous material containing two or more metals, metal oxides, or metal salts selected from the group consisting of, and a carbon material, it is possible to improve the stability of the alkali metal-sulfur battery capacity during repeated charging and discharging, compared to a positive electrode that does not contain any of these metals, metal oxides, or metal salts, or a positive electrode material that contains only one of these metals, metal oxides, or metal salts.

[0022] Next, a method for synthesizing the carbonaceous material that constitutes the carbonaceous material layer will be described. (1) For example, Mn, Fe, Co, Ni, Cu, Zn, Mo, W, V, Zr, Sn, Sb, In, Bi, Fe 2 O 3 , Fe 3 O 4 , Co 3 O 4 , CoO, NiO, MnO 2 , Mn 3 O 4 , MnO, VO 2 , V2 O 5 , MoO 2 , ZnO, ZrO 2 , Co(NO 3 ) 2 , Ni(NO 3 ) 2 , Fe(NO 3 ) 3 , CoCl 2 , NiCl 2 , FeCl 3 , Fe(SO 4 ) 3 , Co(CH 3 COO) 2 , and Ni(CH 3 COO) 2 If the two or more metals, metal oxides, or metal salts selected from the group consisting of are soluble in water, they are dissolved in water or an aqueous solution. The resulting aqueous solution containing the two or more metals, metal oxides, or metal salts is then mixed with the carbon material, stirred, dried, and the solvent is removed.

[0023] (2)Mn, Fe, Co, Ni, Cu, Zn, Mo, W, V, Zr, Sn, Sb, In, Bi, Fe 2 O 3 , Fe 3 O 4 , Co 3 O 4 , CoO, NiO, MnO 2 , Mn 3 O 4 , MnO, VO 2 , V 2 O 5 , MoO 2 , ZnO, ZrO 2 , Co(NO 3 ) 2 , Ni(NO 3 ) 2 , Fe(NO 3 ) 3 , CoCl 2 , NiCl 2 , FeCl 3 , Fe(SO 4 ) 3 , Co(CH 3 COO) 2 , and Ni(CH 3COO) 2 When the two or more metals, metal oxides, or metal salts selected from the group consisting of are insoluble in water, they are pulverized and mixed with the carbon material by a ball mill or the like. (1) and (2) may be combined.

[0024] (3) Next, after steps (1) and / or (2), the mixture of two or more metals, metal oxides, or metal salts and a carbon material obtained is heated for a certain period of time at a temperature of 300° C. or higher. The reaction temperature is preferably 300° C. to 1000° C. The heating time is not particularly limited, but may be 30 minutes to 24 hours.

[0025] (4) Optionally, the resulting product is washed repeatedly with an acid such as hydrochloric acid at room temperature.

[0026] The method for producing the positive electrode material for an alkali metal-sulfur battery containing sulfur and a carbonaceous material is not limited, but for example, sulfur powder is mixed with CS 2 The positive electrode material can be suitably produced by dissolving sulfur in a carbonaceous material, adding the carbonaceous material thereto, dispersing the mixture with ultrasonic waves at, for example, 15 to 40°C, and then heating the mixture at a temperature exceeding 100°C, for example, 140 to 200°C, for 10 to 30 hours to remove the solvent. The ratio of sulfur and the carbonaceous material can be appropriately set so that the resulting positive electrode material has a desired composition. The mass ratio of sulfur to the carbonaceous material (sulfur:carbonaceous material) in the positive electrode material is, for example, 1:10 to 10:1, but is not limited thereto.

[0027] All or a portion of the sulfur in the positive electrode material is elemental sulfur, but at least a portion of the sulfur held in the carbonaceous material may be modified with an organic component including a surface treatment agent such as a surfactant, a polymer pigment, or a silicone resin.

[0028] A common material for the negative electrode of a lithium ion secondary battery or a lithium sulfur secondary battery can be used as the negative electrode 12. Specifically, the material of the negative electrode layer 12 can be, for example, metallic lithium, a lithium alloy (Li-In, Li-Al, Li-Si, etc.), or lithium ion-doped Si, SiO, Sn, SnO, etc. 2Alternatively, hard carbon can be used. These negative electrode materials can be used in the form of a metal foil.

[0029] The electrolyte 14 is not particularly limited as long as it is used as a nonaqueous electrolyte for lithium ion secondary batteries or lithium sulfur secondary batteries, but a nonaqueous electrolyte in which a lithium salt is dissolved in an organic solvent is preferably used.

[0030] An example of the lithium salt is LiClO 4 , LiBF 4 , LiPF 6 , LiAsF 6 Inorganic lithium salts such as LiCl, LiBr, and LiB(C 6 H 5 ) 4 , LiN(SO 2 CF 3 ) 2 , LiC(SO 2 CF 3 ) 3 , LiiOSO 2 CF 3 , LiiOSO 2 C 2 F 5 , LiiOSO 2 C 4 F 9 , LiiOSO 2 C 5 F 11 , LiiOSO 2 C 6 F 13 , and LiiOSO 2 C 7 F 15 Representative examples include organic lithium salts such as:

[0031] Examples of the organic solvent used to dissolve the lithium salt include cyclic esters, chain esters, cyclic ethers, and chain ethers.

[0032] Examples of the cyclic esters include propylene carbonate, butylene carbonate, γ-butyrolactone, vinylene carbonate, 2-methyl-γ-butyrolactone, acetyl-γ-butyrolactone, and γ-valerolactone.

[0033] Examples of the chain esters include dimethyl carbonate, diethyl carbonate, dibutyl carbonate, dipropyl carbonate, methyl ethyl carbonate, methyl butyl carbonate, methyl propyl carbonate, ethyl butyl carbonate, ethyl propyl carbonate, butyl propyl carbonate, alkyl propionates, dialkyl malonates, and alkyl acetates.

[0034] Examples of the cyclic ethers include tetrahydrofuran, alkyltetrahydrofuran, dialkyltetrahydrofuran, alkoxytetrahydrofuran, dialkoxytetrahydrofuran, 1,3-dioxolane, alkyl-1,3-dioxolane, and 1,4-dioxolane.

[0035] Examples of the chain ethers include 1,2-dimethoxyethane, 1,2-diethoxyethane, diethyl ether, ethylene glycol dialkyl ether, diethylene glycol dialkyl ether, triethylene glycol dialkyl ether, and tetraethylene glycol dialkyl ether.

[0036] Known separators for lithium ion secondary batteries and lithium-sulfur secondary batteries can be used as the separator 16. For example, materials such as polyolefin resins such as polyethylene and polypropylene, polyimide, polyvinyl alcohol, fluororesins such as aminated polyethylene oxide polytetrafluoroethylene, acrylic resins, nylon, aromatic aramid, inorganic glass, and ceramics can be used in the form of porous membranes, nonwoven fabrics, woven fabrics, and the like.

[0037] The negative electrode current collector 20 can be formed from a metal foil such as copper (Cu). The shape of the negative electrode current collector 20 is not particularly limited, but it can be a flat foil having a predetermined cross-sectional shape, such as a substantially circular or rectangular shape, that matches the outer shape of the battery.

[0038] The method for assembling the alkali metal-sulfur secondary battery is not particularly limited, and the secondary battery can be obtained by the same method as that for assembling a known secondary battery. EXAMPLES

[0039] The present invention will be specifically described with reference to the following Production Examples, Comparative Production Examples, and Test Examples, although the present invention is not limited thereto.

[0040] Production Example 1 Synthesis of carbonaceous material for positive electrodes consisting of nitrogen-doped carbon nanotubes doped with Ni and Co (Co-Ni N-CNT) 1.2346g Co(NO 3 ) 2 6H 2 O and 1.2388g Ni(NO 3 ) 2 6H 2 O was dissolved in 40 ml of distilled water, and 3.0 g of melamine was added. The mixed solution was stirred for 2 hours and then dried at 60°C for 48 hours. The resulting mixed solid was then calcined in a tubular furnace at 800°C for 2 hours. The resulting product was added to 1M HCl and stirred for 24 hours. Finally, it was washed several times with distilled water and dried in a vacuum oven at 60°C for 24 hours to synthesize a Ni- and Co-doped carbon nanotube, a Co-Ni N-CNT carbonaceous material.

[0041] Production Example 2: Synthesis of carbonaceous material for positive electrodes consisting of Co-Ni N-CNT / S with added sulfur (S) First, sulfur powder was mixed with CS 2 Next, the Co-NiN-CNT powder obtained in Production Example 1 was added to the above solution in a mass ratio of Co-NiN-CNT:S=4:6. The resulting suspension was then dissolved in CS 2After ultrasonic dispersion treatment until completely evaporated, the mixture was placed in a tubular furnace and heated to 155°C at a heating rate of 2°C / min. After heating at 155°C for 12 hours, S-added Co-Ni N-CNT / S was obtained.

[0042] Comparative Production Example 1 Synthesis of Ni-doped Ni-doped Carbon Nanotubes (NiN-CNT) 2.4776g Ni(NO 3 ) 2 6H 2 O was dissolved in 40 ml of distilled water and stirred for 2 hours, after which 3.0 g of melamine was added. The mixed solution was stirred for 2 hours and then dried at 60°C for 48 hours. The resulting mixed solid was then calcined in a tubular furnace at 800°C for 2 hours. The resulting product was added to 1M HCl and stirred for 24 hours. Finally, it was washed several times with distilled water and dried in a vacuum oven at 60°C for 24 hours to synthesize a NiN-CNT carbonaceous material, which is a nitrogen-doped carbon nanotube doped with Ni.

[0043] Comparative Production Example 2 Synthesis of Co-doped nitrogen-doped carbon nanotubes (Co N-CNT) 2.4692g Co(NO 3 ) 2 6H 2 O was dissolved in 40 ml of distilled water and stirred for 2 hours, after which 3.0 g of melamine was added. The mixed solution was stirred for 2 hours and then dried at 60 °C for 48 hours. Next, the obtained mixed solid was calcined in a tubular furnace at 800 °C for 2 hours. The obtained product was added to 1 M HCl and stirred for 24 hours. Finally, it was washed several times with distilled water and dried in a vacuum oven at 60 °C for 24 hours to synthesize a carbonaceous material, Co N-CNT, which is a nitrogen-doped carbon nanotube doped with Co.

[0044] Comparative Production Example 3 Synthesis of Nitrogen-Doped Carbon Nanotubes (N-CNT) without Metal Doping 3.0 g of melamine was added to 40 ml of distilled water. The mixed solution was stirred for 2 hours and then dried at 60°C for 48 hours. The resulting mixed solid was then calcined in a tubular furnace at 800°C for 2 hours. The resulting product was added to 1M HCl and stirred for 24 hours. Finally, it was washed several times with distilled water and dried in a vacuum oven at 60°C for 24 hours to synthesize N-CNT carbonaceous material, which is a nitrogen-doped carbon nanotube with no Ni or Co added.

[0045] Comparative Example 4 Synthesis of carbonaceous material for positive electrode consisting of NiN-CNT / S with added sulfur (S) NiN-CNT / S was produced under the same conditions as in Production Example 2, using the NiN-CNT of Comparative Production Example 2 in place of the Co-NiN-CNT of Production Example 1.

[0046] Comparative Example 5 Synthesis of carbonaceous material for positive electrode consisting of CoN-CNT / S with added sulfur (S) CoN-CNT / S was produced under the same conditions as in Production Example 2, using the CoN-CNT of Comparative Production Example 1 in place of the Co—NiN-CNT of Production Example 1.

[0047] Comparative Example 6 Synthesis of carbonaceous material for positive electrode consisting of N-CNT / S doped with sulfur (S) N-CNT / S was produced under the same conditions as in Production Example 2, using the N-CNTs of Comparative Production Example 3 in place of the Co-Ni N-CNTs of Production Example 1.

[0048] Manufacturing Example 3: Manufacturing of Lithium-Sulfur Battery (Li-S Battery) A positive electrode was produced by mixing 80% by weight of a carbonaceous material, 10% by weight of conductive carbon black (SUPER P, Imerys Graphite & Carbon), and 10% by weight of polyvinylidene fluoride (PVDF). The carbonaceous material was either Co-Ni N-CNT / S of Production Example 2, Ni N-CNT / S of Comparative Production Example 4, Co N-CNT / S of Comparative Production Example 5, or N-CNT / S of Comparative Production Example 6. The separator was made of polypropylene. Lithium metal was used for the negative electrode. The electrolyte consisted of 1M lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) salt and 1% lithium nitrate (LiNO) in a 1:1 volume ratio of 1,3-dioxolane (DOL) and 1,2-dimethoxyethane (DME) solvent. 3 ) was dissolved and used.

[0049] To assemble the battery, the positive electrode, separator, and negative electrode were packed into a battery cell with a diameter of 12 mm, and electrolyte was placed between the positive electrode and the separator, and between the separator and the negative electrode. The cell was then pressed for 3 minutes at a pressure of 380 MPa. Aluminum foil was placed on the opposite side of the separator in the positive electrode, and copper foil was placed on the opposite side of the separator in the negative electrode, as counter electrodes, and a pressure of 120 MPa was applied to obtain a test battery.

[0050] Test Example 1 The positive electrode carbonaceous materials, Co-Ni N-CNT produced in Production Example 1, Ni N-CNT produced in Comparative Production Example 1, Co N-CNT produced in Comparative Production Example 2, Co-Ni N-CNT / S produced in Production Example 2, Ni N-CNT / S produced in Comparative Production Example 4, and Co N-CNT / S produced in Comparative Production Example 5, were observed with a scanning microscope.

[0051] As shown in Figures 2A, 2B, and 2C, the carbonaceous materials of Co-NiN-CNT of Production Example 1, NiN-CNT of Comparative Production Example 1, and CoN-CNT of Comparative Production Example 2 all maintained a tubular structure, and the Co-NiN-CNT of Production Example 1 had thicker tubes than the NiN-CNT of Comparative Production Example 1 and the CoN-CNT of Comparative Production Example 2. As shown in Figures 2D, E, and F, respectively, it was found that sulfur coated the surface of the N-CNTs.

[0052] Test Example 2 The Co-Ni N-CNT produced in Production Example 1, the Co-Ni N-CNT / S produced in Production Example 2, and sulfur powder were lightly crushed and subjected to powder X-ray diffraction. For the X-ray diffraction measurement, Rigaku's "SmartLab" was used, and the measurement was performed using a Cu-Kα (λ = 1.540 Å) radiation source in the range of 2θ = 10 to 80°.

[0053] As shown in Figure 3, the diffraction peak at 2θ = 26.4° for Co-Ni N-CNT corresponds to the diffraction of the (002) crystal plane of graphite-2H (JCPDS No. 41-1487). The diffraction peaks at 2θ = 44.2°, 2θ = 51.5°, and 2θ = 75.9° correspond to the (111), (200), and (220) diffractions, respectively, of Co metal crystal planes (JCPDS No. 15-0806), and the diffraction peaks at 2θ = 44.5°, 2θ = 51.9°, and 2θ = 76.4° correspond to the (200), (220), and (311) diffractions, respectively, of Ni metal crystal planes (JCPDS No. 04-0850). From the XRD pattern of Co-Ni N-CNT / S, almost all of the strong diffraction peaks corresponding to sulfur (JCPDS No. 08-0247) were displayed, indicating that sulfur was supported on the Co-Ni N-CNTs.

[0054] Test Example 3 A constant current charge / discharge experiment was carried out on the lithium-sulfur battery prepared in Preparation Example 3. The battery was tested using a battery test system (LANDCD2001A model, Wu is LANHE Electronic, Ltd.) in the range of 1.7 to 2.8 V.

[0055] As shown in Figure 4, when Co-Ni N-CNT / S of Production Example 2 was used as the carbonaceous material for the positive electrode of a lithium-sulfur battery (1), it was found to have a specific capacity of 724.2 mAhg-1 even after 150 cycles at a charge / discharge rate of 1C. When Co-Ni N-CNT / S of Production Example 2 was used (1) (724.2 mAhg-1), this is much higher than when Ni N-CNT / S of Comparative Production Example 4 (584.4 mAhg-1) (2) and Co N-CNT / S of Comparative Production Example 5 (517.0 mAhg-1) (3) were used under the same conditions.

[0056] Test Example 4 A constant current charge / discharge experiment was carried out on the lithium-sulfur battery prepared in Preparation Example 3. The battery was tested using a battery test system (LANDCD2001A model, Wu is LANHE Electronic, Ltd.) in the range of 1.7 to 2.8 V.

[0057] As shown in Figure 5, when Co-Ni N-CNT / S of Production Example 2 was used as the carbonaceous material for the positive electrode of a lithium-sulfur battery, it was found that the specific capacity was 440.0mAhg-1 even after 350 cycles at a charge-discharge rate of 1C. This is much higher than the case of using N-CNT / S of Comparative Production Example 6 without metal doping (334.4mAhg-1 after 350 cycles).

[0058] The results of the above test examples show that the positive electrode material for an alkali metal-sulfur battery of the present invention improves the stability of the battery capacity of an alkali metal-sulfur battery during repeated charging and discharging, compared to a positive electrode material that does not contain a metal, metal oxide, or metal salt, or a positive electrode material that contains approximately the same amount of one type of metal, metal oxide, or metal salt. [Explanation of symbols]

[0059] 10...positive electrode, 12...negative electrode, 14...electrolyte.

Claims

1. A carbonaceous material used as a positive electrode material for an alkali metal-sulfur battery, comprising: a metal, metal oxide, or metal salt comprising at least one selected from the group consisting of Co3O4, CoO, Co(NO3)2, CoCl2, and Co(CH3COO)2, and at least one selected from the group consisting of Ni, NiO, Ni(NO3)2, NiCl2, and Ni(CH3COO)2; Graphite or carbon nanotubes A carbonaceous material comprising:

2. A positive electrode material for an alkali metal-sulfur battery comprising sulfur and the carbonaceous material of claim 1.

3. An alkali metal-sulfur battery comprising a positive electrode made of the positive electrode material according to claim 2, a negative electrode, and an electrolyte filled between the positive electrode and the negative electrode.

4. A method for producing a carbon material comprising mixing a metal, metal oxide, or metal salt containing at least one selected from the group consisting of Co3O4, CoO, Co(NO3)2, CoCl2, and Co(CH3COO)2, and at least one selected from the group consisting of Ni, NiO, Ni(NO3)2, NiCl2, and Ni(CH3COO)2, in water or a solution; and heating water or a solution containing the metal, metal oxide, or metal salt and the carbon material to a temperature of 300° C. or higher and drying the water or solution; A method for producing the carbonaceous material of claim 1, comprising:

5. suspending the carbonaceous material of claim 1 and sulfur powder in a solvent; and heating the resulting suspension to remove the solvent. The method for producing a positive electrode material for an alkali metal-sulfur battery includes the steps of:

Citation Information

Patent Citations

  • Core-shell structured lithium-sulfur battery cathode material and preparation method thereof

    CN106920953A

  • Preparation method of core-shell covered sulfur-carbon nanotube compound lithium-sulfur battery anode material

    CN109411732A

  • Powder material, electrode structure, manufacture thereof and lithium secondary battery

    JP1999214005A

  • Carbon nanotube-sulfur composite containing carbon nanotube aggregates and method for producing the same

    JP2016535716A

  • Positive electrode active material containing metal nanoparticles, positive electrode, and lithium-sulfur battery containing the same

    JP2018511923A