Curable composition and panel structure using the same

A curable composition with polyalkylene oxide, glass frit, inorganic compounds, and calcium carbonate addresses the vulnerability of fireproof seals by maintaining sealing integrity and preventing flame spread through controlled expansion and residue formation.

JP7570683B2Active Publication Date: 2024-10-22SEKISUI FULLER CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021005994
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-17
Filing Date
2021-01-18
Publication Date
2024-10-22
Estimated Expiration
2041-01-18

AI Technical Summary

Technical Problem

Existing fireproof sealing materials in building structures are vulnerable to combustion, brittle from foaming, and fail to maintain sealing integrity due to dimensional changes during fires, leading to insufficient fire resistance.

Method used

A curable composition comprising polyalkylene oxide with hydrolyzable silyl groups, glass frit, inorganic compounds, calcium carbonate, and a silanol condensation catalyst, balanced in specific ratios to provide rubber elasticity and expandability, ensuring the composition follows dimensional changes and maintains sealing integrity during fires.

Benefits of technology

The composition maintains sealing integrity and prevents flame spread by expanding to match dimensional changes, forming a strong combustion residue that retains the seal, enhancing fire resistance in building structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570683000001
    Figure 0007570683000001
  • Figure 0007570683000002
    Figure 0007570683000002
Patent Text Reader

Abstract

To provide a curable composition capable of imparting an excellent fire resistance performance to building structures by smoothly tracking the dimensional change of a sealing part generated by heat during fire, by surely keeping the packed state of the sealing part and by inhibiting flame from spreading from the sealing part.SOLUTION: A curable composition of the present invention is characterized in that the composition includes: 100 pts.mass of polyalkylene oxide having a hydrolyzable silyl group(s); 20-150 pts.mass of glass frit; an inorganic compound(s) which generates a gas of 0.5-20% in a total amount at 150-300°C; 50-300 pts.mass of calcium carbonate; and a silanol condensation catalyst, and a mass ratio of the content of the glass frit to that of the inorganic compound(s) (content of glass frit / content of inorganic compound(s)) is in a range of 0.1 to 40.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable composition and a panel structure using the curable composition. [Background technology]

[0002] The panel structure of an architectural structure is constructed by arranging panels in a panel arrangement section of the architectural structure, and filling with sealing material the gaps formed between the opposing surfaces of the panel arrangement section and the panel members, and the gaps formed between the panel members (these gaps are sometimes collectively referred to as "sealing sections").

[0003] In the above-mentioned panel structure, since the sealing material is an organic substance, it is vulnerable to combustion, and in the event of a fire, the sealing material may fall off from the sealing part, allowing flames to penetrate through the sealing part, resulting in the problem that the fire resistance of the wall part of the building structure is insufficient.

[0004] Furthermore, the heat of a fire can cause the panel members to shrink or deform, and this deformation of the panel members can change the dimensions of the sealing part. If the sealant cannot keep up with the dimensional changes in the sealing part, flames can seep in through the sealing part, which, as mentioned above, can result in insufficient fire resistance in the walls of architectural structures.

[0005] Patent Document 1 discloses a fireproof sealant comprising (A) a polyalkylene ether having a silicon-containing functional group at its end that can form a silanol group by hydrolysis, (B) a microencapsulated ammonium polyphosphate powder, (C) a calcium carbonate powder, and (D) a silanol condensation catalyst. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 3848379 Summary of the Invention [Problem to be solved by the invention]

[0007] However, the fireproof sealant foams due to the heat of a fire and then forms a carbonized layer. The foaming makes the combustion residue brittle, so it is easily destroyed by the wind pressure of the combustion flame and falls off from the sealing part. Furthermore, the fireproof sealant cannot follow the dimensional change of the sealing part caused by the deformation of the panel member due to the heat of a fire, and a gap is generated in the sealing part. Therefore, the fireproof sealant has a problem that the fire resistance is still insufficient.

[0008] The present invention provides a curable composition that smoothly follows dimensional changes in a sealing part caused by heat during a fire, reliably maintains the filled state of the sealing part, prevents flames from penetrating through the sealing part, and provides excellent fire resistance to architectural structures, as well as a panel structure using the same. [Means for solving the problem]

[0009] The curable composition of the present invention comprises 100 parts by mass of a polyalkylene oxide having a hydrolyzable silyl group; 20 to 150 parts by mass of glass frit; An inorganic compound having a total gas generation amount of 0.5 to 20% at 150 to 300 ° C. 50 to 300 parts by mass of calcium carbonate and a silanol condensation catalyst, The mass ratio of the content of the glass frit to the content of the inorganic compound (content of the glass frit / content of the inorganic compound) is characterized in being 0.1-40.

[0010] The curable composition of the present invention further comprises 100 parts by mass of a polyalkylene oxide having a hydrolyzable silyl group; 20 to 150 parts by mass of glass frit; An inorganic compound having a heat loss of 0.5 to 20% at 150 to 300°C; 50 to 300 parts by mass of calcium carbonate and a silanol condensation catalyst, The mass ratio of the content of the glass frit to the content of the inorganic compound (content of the glass frit / content of the inorganic compound) is characterized in being 0.1-40.

[0011] [Polyalkylene oxide having hydrolyzable silyl groups at the terminals] The polyalkylene oxide has a hydrolyzable silyl group. It is preferable that the polyalkylene oxide has a hydrolyzable silyl group at the end of the main chain. In the presence of water, the hydrolyzable group of the hydrolyzable silyl group of the polyalkylene oxide is hydrolyzed to generate a silanol group (-SiOH). Then, the silanol groups are dehydrated and condensed to form a crosslinked structure.

[0012] The hydrolyzable silyl group is a group in which 1 to 3 hydrolyzable groups are bonded to a silicon atom. The hydrolyzable group of the hydrolyzable silyl group is not particularly limited, and examples thereof include a hydrogen atom, a halogen atom, an alkoxy group, an acyloxy group, a ketoximate group, an amino group, an amide group, an acid amide group, an aminooxy group, a mercapto group, an alkenyloxy group, and an oxime group.

[0013] Among them, as the hydrolyzable silyl group, alkoxysilyl group is preferred because hydrolysis reaction is mild.Alkoxysilyl group includes trialkoxysilyl group such as trimethoxysilyl group, triethoxysilyl group, triisopropoxysilyl group, and triphenoxysilyl group; dialkoxysilyl group such as propyldimethoxysilyl group, methyldimethoxysilyl group, and methyldiethoxysilyl group; and monoalkoxysilyl group such as dimethylmethoxysilyl group and dimethylethoxysilyl group, dialkoxysilyl group is more preferred, dimethoxysilyl group and methyldimethoxysilyl group are more preferred, and methyldimethoxysilyl group is more preferred.

[0014] The polyalkylene oxide having a hydrolyzable silyl group preferably has 1 to 4 hydrolyzable silyl groups on average in one molecule. When the number of hydrolyzable silyl groups in the polyalkylene oxide having a hydrolyzable silyl group is within the above range, the cured product of the curable composition retains excellent rubber elasticity even when heated to about 400°C, smoothly follows the dimensional change of the sealing part due to heat during a fire, and can stably maintain the filling state of the sealing part. Furthermore, the combustion residue of the cured product of the curable composition can be stably held in the sealing part, and the fire resistance of the building structure can be maintained. The polyalkylene oxide having a hydrolyzable silyl group preferably has hydrolyzable silyl groups at both ends of its main chain.

[0015] In addition, the average number of hydrolyzable silyl groups per molecule in the polyalkylene oxide having hydrolyzable silyl groups is 1 It can be calculated based on the concentration of hydrolyzable silyl groups in the polyalkylene oxide determined by H-NMR and the number average molecular weight of the polyalkylene oxide determined by GPC.

[0016] The polyalkylene oxide constituting the polyalkylene oxide having a hydrolyzable silyl group has a main chain represented by the general formula: -(RO) n - (wherein R represents an alkylene group having 1 to 14 carbon atoms, and n represents the number of repeating units and is a positive integer) is preferred. The main chain skeleton of the polyalkylene oxide may be composed of only one type of repeating unit, or may be composed of two or more types of repeating units.

[0017] Examples of the main chain skeleton of the polyalkylene oxide include polyethylene oxide, polypropylene oxide, polybutylene oxide, polytetramethylene oxide, polyethylene oxide-polypropylene oxide copolymer, and polypropylene oxide-polybutylene oxide copolymer. Among them, polypropylene oxide is preferable. With polypropylene oxide, the cured product of the curable composition maintains excellent rubber elasticity even when heated to about 400°C, and the combustion residue of the cured product of the curable composition can be stably held in the sealing part.

[0018] The number average molecular weight of the polyalkylene oxide having a hydrolyzable silyl group is preferably 3000 or more, more preferably 10000 or more. The number average molecular weight of the polyalkylene oxide having a hydrolyzable silyl group is preferably 50000 or less, more preferably 30000 or less. When the number average molecular weight of the polyalkylene oxide is 3000 or more, the cured product of the curable composition maintains excellent rubber elasticity even when heated to about 400 ° C. When the number average molecular weight of the polyalkylene oxide is 50000 or less, the cured product of the curable composition maintains excellent rubber elasticity even when heated to about 400 ° C., smoothly follows the dimensional change of the sealing part due to heat during a fire, and can stably maintain the filling state of the sealing part.

[0019] In the present invention, the number average molecular weight of the polyalkylene oxide having a hydrolyzable silyl group is a value measured by GPC (gel permeation chromatography) and converted into polystyrene. Specifically, 6 to 7 mg of the polyalkylene oxide having a hydrolyzable silyl group is collected, the collected polyalkylene oxide is fed to a test tube, and then an o-DCB (ortho-dichlorobenzene) solution containing 0.05% by mass of BHT (dibutylhydroxytoluene) is added to the test tube to dilute the polyalkylene oxide to a concentration of 1 mg / mL to prepare a diluted solution.

[0020] The dilution solution is shaken at 145° C. and 25 rpm for 1 hour using a dissolution filter to dissolve the polyalkylene oxide in the o-DCB solution containing BHT to obtain a measurement sample. The number average molecular weight of the polyalkylene oxide can be measured by the GPC method using this measurement sample.

[0021] The number average molecular weight of the polyalkylene oxide having a hydrolyzable silyl group can be measured, for example, using the following measuring device and measuring conditions. Measuring device: TOSOH product name "HLC-8121GPC / HT" Measurement conditions Column: TSKgelGMHHR-H(20)HT x 3 TSKguardcolumn-HHR(30)HT x 1 Mobile phase: o-DCB 1.0mL / min Sample concentration: 1mg / mL Detector: Bryce type refractometer Standard material: Polystyrene (TOSOH, molecular weight: 500-8420000) Elution conditions: 145℃ SEC temperature: 145℃

[0022] The polyalkylene oxide having a hydrolyzable silyl group can be a commercially available product. For example, the polyalkylene oxide having a hydrolyzable silyl group includes the product names "MS Polymer S-203", "MS Polymer S-303", "Silyl Polymer SAT-200", "Silyl Polymer SAT-350" and "Silyl Polymer SAT-400" manufactured by Kaneka Corporation. The polyalkylene oxide having a hydrolyzable silyl group includes the product names "Exestar S3620", "Exestar S2420", "Exestar S2410" and "Exestar S3430" manufactured by AGC Corporation.

[0023] A polyalkylene oxide having a polypropylene oxide main chain and a (methoxymethyl)dimethoxysilyl group at the end of the polypropylene oxide is commercially available from Kaneka Corporation under the product name "HS-2."

[0024] A polyalkylene oxide having a polypropylene oxide main chain and an isopropyldimethoxymethylsilyl group at the end of the polypropylene oxide is commercially available from Kaneka Corporation under the product name "SAX720."

[0025] [Glass frit] The curable composition contains a glass frit. The glass frit acts as a binder for binding the polyalkylene oxide and / or inorganic compound having a hydrolyzable silyl group together in the combustion residue of the cured product of the curable composition. The glass frit may be used alone or in combination of two or more kinds.

[0026] Examples of the glass constituting the glass frit include phosphate glass, borate glass, bismuth oxide glass, silicate glass, and sodium oxide glass, with phosphate glass and borate glass being preferred, and phosphate glass being more preferred. These glass frits can be obtained by adjusting B2O3, P2O5, ZnO, SiO2, Bi2O3, Al2O3, BaO, CaO, MgO, MnO2, ZrO2, TiO2, CeO2, SrO, V2O5, SnO2, Li2O, Na2O, K2O, CuO, Fe2O3, and the like in a predetermined component ratio. The glass frits may be used alone or in combination of two or more kinds.

[0027] The softening point of the glass constituting the glass frit is preferably 350°C or higher, more preferably 360°C or higher, more preferably 370°C or higher, and more preferably 380°C or higher. The softening point of the glass constituting the glass frit is preferably 650°C or lower, more preferably 560°C or lower, more preferably 540°C or lower, and more preferably 520°C or lower. When the softening point of the glass constituting the glass frit is 350°C or higher, the polyalkylene oxide having a hydrolyzable silyl group softened by the heat during a fire is reinforced, and the shape retention of the cured product of the curable composition is improved. When the softening point of the glass constituting the glass frit is 650°C or lower, the glass effectively acts as a binder for binding the polyalkylene oxide having a hydrolyzable silyl group and / or inorganic compound together in the combustion residue of the cured product of the curable composition in a temperature range of about 650 to 945°C. The softening point of the glass constituting the glass frit is the temperature at which the viscosity of the glass becomes 107.6 dPa·s (log η = 7.6).

[0028] The content of the glass frit in the curable composition is 20 parts by mass or more, preferably 25 parts by mass or more, more preferably 30 parts by mass or more, and more preferably 35 parts by mass or more, relative to 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group. The content of the glass frit in the curable composition is 150 parts by mass or less, preferably 100 parts by mass or less, more preferably 80 parts by mass or less, more preferably 70 parts by mass or less, and more preferably 60 parts by mass or less, relative to 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group. When the content of the glass frit is 20 parts by mass or more, the combustion residue of the cured product of the curable composition can be stably held in the sealing part. When the content of the glass frit is 150 parts by mass or less, the cured product of the curable composition maintains excellent rubber elasticity even when heated to about 400 ° C.

[0029] [Inorganic compounds] The curable composition contains an inorganic compound that generates gas in a total amount of 0.5 to 20% at 150 to 300°C, or an inorganic compound that loses heat in a total amount of 0.5 to 20% at 50 to 300°C.

[0030] The cured product of the curable composition is filled into the sealing parts of building structures, but the panel members that make up the walls may shrink due to the heat during a fire, in which case the sealing parts will expand.

[0031] Therefore, by incorporating the above-mentioned inorganic compound into the curable composition, the cured product of the curable composition can be expanded before it becomes a combustion residue, and can smoothly follow the expansion of the sealing part, thereby reliably maintaining the closure of the sealing part.

[0032] The curable composition contains a polyalkylene oxide having a hydrolyzable silyl group, glass frit, a specific inorganic compound, and calcium carbonate in a specific mixing ratio. Therefore, the cured product of the curable composition maintains excellent rubber elasticity even when heated to about 400°C in the event of a fire. In this state, the cured product of the curable composition is expanded by the inorganic compound, so that the cured product smoothly follows the expansion of the sealed part, and the sealing of the sealed part can be reliably maintained.

[0033] The inorganic compound has a total gas generation amount of 0.5% or more, preferably 1% or more, more preferably 2% or more, and more preferably 3% or more at 150 to 300° C. When the total gas generation amount is 0.5% or more at 150 to 300° C., the cured product of the curable composition expands smoothly at a temperature of 300° C. or less when heated by heat during a fire, and can smoothly follow the expansion of the sealed parts of the architectural structure to reliably maintain the closure of the sealed parts.

[0034] The inorganic compound has a total gas generation amount of 20% or less, preferably 15% or less, more preferably 12% or less, and more preferably 10% or less at 150 to 300° C. When the total gas generation amount is 20% or less at 1150 to 300° C., the cured product of the curable composition expands smoothly at a temperature of 300° C. or less when heated by heat during a fire, and can smoothly follow the expansion of the sealed parts of the architectural structure to reliably maintain the closure of the sealed parts.

[0035] The total amount of gas generated in an inorganic compound at 150 to 300°C is measured as follows. 100 g of an inorganic compound is prepared as sample A. The mass W1 of this sample A is measured. Next, sample A is left in a thermostatic chamber maintained at 150°C for one hour, and then sample A is removed from the thermostatic chamber and left in an atmosphere at 25°C for one hour. Thereafter, the mass W2 of sample A after heating is measured. The heat loss D1 at 150°C is calculated based on the following formula. Heat loss at 150℃ D1(%)=100×(W1-W2) / W1

[0036] Also, 100 g of another inorganic compound is prepared as sample B. The mass W3 of this sample B is measured. Next, sample B is left in a thermostatic chamber maintained at 300°C for 1 hour, and then sample B is removed from the thermostatic chamber and left in an atmosphere of 25°C for 1 hour. Thereafter, the mass W4 of sample A after heating is measured. The heat loss D2 at 300°C is calculated based on the following formula. The total amount of gas generated at 150 to 300°C is calculated based on the following formula. Heat loss at 300℃ D2(%)=100×(W3-W4) / W3 Total amount of gas generated at 150-300℃ (%) = (D2 heat loss at 300°C) - (D1 heat loss at 150°C)

[0037] The inorganic compound has a heat loss of 0.5% or more, preferably 1% or more, more preferably 2% or more, and more preferably 3% or more at 150 to 300° C. When the heat loss at 150 to 300° C. is 0.5% or more, the cured product of the curable composition smoothly expands at a temperature of 300° C. or less when heated by heat during a fire, and can smoothly follow the expansion of the sealed part of the architectural structure to reliably maintain the closure of the sealed part.

[0038] The inorganic compound has a heat loss of 20% or less, preferably 15% or less, more preferably 12% or less, and still more preferably 10% or less at 150 to 300° C. When the heat loss at 1150 to 300° C. is 20% or less, the cured product of the curable composition smoothly expands at temperatures of 300° C. or less when heated by heat during a fire, and smoothly follows the expansion of the sealed parts of architectural structures, thereby reliably maintaining the closure of the sealed parts.

[0039] The amount of loss on heating of an inorganic compound at 150 to 300°C is measured as follows. 100 g of an inorganic compound is prepared as sample E. The mass W5 of this sample E is measured. Next, sample E is left in a thermostatic chamber maintained at 150°C for one hour, and then sample E is removed from the thermostatic chamber and left in an atmosphere at 25°C for one hour. Thereafter, the mass W6 of sample E after heating is measured. The loss on heating D3 at 150°C is calculated based on the following formula. Heat loss at 150℃ G3(%)=100×(W5-W6) / W5

[0040] Also, 100 g of another inorganic compound is prepared as sample F. The mass W7 of this sample F is measured. Next, sample F is left in a thermostatic chamber maintained at 300°C for 1 hour, and then sample F is removed from the thermostatic chamber and left in an atmosphere at 25°C for 1 hour. Thereafter, the mass W8 of sample F after heating is measured. The heat loss D4 at 300°C is calculated based on the following formula. The heat loss at 150 to 300°C is calculated based on the following formula. Heat loss at 300℃ D4(%)=100×(W7-W8) / W7 Heat loss at 150-300℃ (%) = (D4 loss on heating at 300°C) - (D3 loss on heating at 150°C)

[0041] The inorganic compound is not particularly limited as long as the total amount of gas generated at 150 to 300°C is 0.5 to 20%, and examples thereof include aluminum phosphate (AlPO4), aluminum phosphite [Al2(PHO3)3], expanded graphite, aluminum hydroxide, and sodium bicarbonate (sodium hydrogen carbonate). Ammonium polyphosphate, aluminum phosphate (AlPO4), aluminum phosphite [Al2(PHO3)3], and expanded graphite are preferred, and ammonium polyphosphate, aluminum phosphate (AlPO4), and expanded graphite are more preferred. The inorganic compounds may be used alone or in combination of two or more.

[0042] Expanded graphite is produced by treating natural or synthetic graphite with an intercalant such as an acid, oxidant, or halide to create an intercalation compound, and then rapidly heating the powder (1000 to 1200°C) to expand the graphite in the c-axis direction by approximately 150 to 700 times.

[0043] Intercalant materials include sulfuric acid, nitric acid, chromic acid, boric acid, SO3, or halides such as FeCl3, ZnCl2, and SbCl5.

[0044] The content of the inorganic compound in the curable composition is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and more preferably 30 parts by mass or more, relative to 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group. The content of the inorganic compound in the curable composition is preferably 150 parts by mass or less, more preferably 120 parts by mass or less, more preferably 100 parts by mass or less, more preferably 80 parts by mass or less, and more preferably 70 parts by mass or less, relative to 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group. When the content of the inorganic compound in the curable composition is within the above range, the cured product of the curable composition can be smoothly expanded at 300 ° C. or less in the event of a fire, and the sealing part of the building structure can be smoothly followed by the expansion of the sealing part to reliably maintain the sealing part.

[0045] In the curable composition, the mass ratio of the glass frit content to the inorganic compound content (glass frit content / inorganic compound content) is 0.1 or more, preferably 0.2 or more, more preferably 0.3 or more, more preferably 0.4 or more, more preferably 0.5 or more, and more preferably 0.6 or more. In the curable composition, the mass ratio of the glass frit content to the inorganic compound content (glass frit content / inorganic compound content) is 40 or less, preferably 37 or less, more preferably 35 or less, more preferably 33 or less, more preferably 30 or less, more preferably 28 or less, more preferably 20 or less, more preferably 15 or less, more preferably 13 or less, more preferably 11 or less, more preferably 9 or less, more preferably 7 or less, and more preferably 5 or less. When the mass ratio of the glass frit content to the inorganic compound content (glass frit content / inorganic compound content) is 0.1 or more, the combustion residue of the cured product of the curable composition can be stably held in the sealing part. When the mass ratio of the glass frit content to the inorganic compound content (glass frit content / inorganic compound content) is 40 or less, polyalkylene oxides and / or inorganic compounds having hydrolyzable silyl groups can be strongly bonded to each other in the combustion residue of the cured product of the curable composition, which is preferable.

[0046] [Calcium carbonate] The curable composition contains calcium carbonate. The calcium carbonate is not particularly limited, and examples thereof include colloidal calcium carbonate, heavy calcium carbonate, light calcium carbonate, etc., with colloidal calcium carbonate and heavy calcium carbonate being preferred, and colloidal calcium carbonate being more preferred.

[0047] The average particle size of calcium carbonate is preferably 0.01 to 5 μm, more preferably 0.05 to 2.5 μm. With calcium carbonate having such an average particle size, the combustion residue of the cured product of the curable composition has excellent strength, and the combustion residue does not become too hard and crack. Therefore, the sealing part such as the joint part can be reliably maintained in a filled state, and excellent fire resistance can be imparted to the panel structure of the building structure. The average particle size of calcium carbonate refers to a value calculated by the arithmetic average of the diameters of 10 particles measured on a scale by observation with a SEM. The particle diameter is the diameter of the smallest circle that can surround the particle in a micrograph obtained by a SEM (scanning electron microscope).

[0048] In addition, the calcium carbonate is preferably surface-treated with a fatty acid, a fatty acid ester, etc. Calcium carbonate surface-treated with a fatty acid, a fatty acid ester, etc. can impart thixotropy to the hardenable composition and can inhibit the calcium carbonate from aggregating.

[0049] The content of calcium carbonate in the curable composition is 50 parts by mass or more, preferably 70 parts by mass or more, more preferably 100 parts by mass or more, and more preferably 120 parts by mass or more, relative to 100 parts by mass of polyalkylene oxide having a hydrolyzable silyl group. The content of calcium carbonate in the curable composition is 300 parts by mass or less, preferably 250 parts by mass or less, more preferably 200 parts by mass or less, and more preferably 160 parts by mass or less, relative to 100 parts by mass of polyalkylene oxide having a hydrolyzable silyl group. When the content of calcium carbonate in the curable composition is 50 parts by mass or more, it exerts a reinforcing effect on the polyalkylene oxide having a hydrolyzable silyl group softened by the heat during a fire, and the shape retention of the cured product of the curable composition is improved. When the content of calcium carbonate in the curable composition is 300 parts by mass or less, the cured product of the curable composition retains excellent rubber elasticity even when heated to about 400°C, smoothly follows dimensional changes in the sealing part due to heat during a fire, and can stably maintain the filling state of the sealing part.

[0050] [Silanol condensation catalyst] The curable composition preferably contains a silanol condensation catalyst. The silanol condensation catalyst is a catalyst for promoting a dehydration condensation reaction between silanol groups formed by hydrolysis of a hydrolyzable silyl group contained in a polyalkylene oxide.

[0051] Examples of the silanol condensation catalyst include organic tin compounds such as 1,1,3,3-tetrabutyl-1,3-dilauryloxycarbonyl-distannoxane, dibutyltin dilaurate, dibutyltin oxide, dibutyltin diacetate, dibutyltin phthalate, bis(dibutyltin laurate) oxide, dibutyltin bis(acetylacetonate), dibutyltin bis(monoester maleate), tin octoate, dibutyltin octoate, dioctyltin oxide, dibutyltin bis(triethoxysilicate), bis(dibutyltin bistriethoxysilicate) oxide, and dibutyltin oxybisethoxysilicate; organic titanium compounds such as tetra-n-butoxy titanate and tetraisopropoxy titanate. These silanol condensation catalysts may be used alone or in combination of two or more.

[0052] The silanol condensation catalyst is preferably 1,1,3,3-tetrabutyl-1,3-dilauryloxycarbonyl-distannoxane, which makes it possible to easily adjust the curing rate of the curable composition.

[0053] The content of the silanol condensation catalyst in the curable composition is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and more preferably 0.3 parts by mass or more, relative to 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group. The content of the silanol condensation catalyst in the curable composition is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, more preferably 6 parts by mass or less, and more preferably 5 parts by mass or less, relative to 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group. When the content of the silanol condensation catalyst in the curable composition is 0.1 parts by mass or more, the curing speed of the curable composition can be increased, and the time required for curing the curable composition can be shortened. When the content of the silanol condensation catalyst in the curable composition is 10 parts by mass or less, the curable composition has an appropriate curing speed, and the storage stability and handling of the curable composition can be improved.

[0054] [Plasticizer] The curable composition preferably contains a plasticizer. Examples of the plasticizer include phthalates such as dimethyl phthalate, diethyl phthalate, dibutyl phthalate, diisobutyl phthalate, di-n-hexyl phthalate, bis(2-ethylhexyl) phthalate, di-n-octyl phthalate, diisononyl phthalate, dinonyl phthalate, diisodecyl phthalate, diisoundecyl phthalate, and bisbutylbenzyl phthalate; and polyalkylene glycols such as diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, tetrapropylene glycol, and polypropylene glycol. Among these, polyalkylene glycols are preferred, and polypropylene glycol is more preferred. The plasticizer is preferably a phthalate having a viscosity of 1.01×10 at 23° C. and 1.01×10 5 It is preferable that the material is in a liquid state at 1 atm.

[0055] When the plasticizer is a polymer, the number average molecular weight of the plasticizer is preferably at least 1000, more preferably at least 2000. When the plasticizer is a polymer, the number average molecular weight of the plasticizer is preferably at most 10000, more preferably at most 5000. When the number average molecular weight of the plasticizer is within the above range, the cured product of the curable composition maintains excellent rubber elasticity even when heated to about 400°C, and the combustion residue of the cured product of the curable composition can be stably held in the sealing portion.

[0056] In the present invention, when the plasticizer is a polymer, the number average molecular weight of the plasticizer is a value measured in terms of polystyrene by GPC (gel permeation chromatography). The specific measurement method and measurement conditions are the same as those for the polyalkylene oxide described above.

[0057] The content of the plasticizer in the curable composition is preferably 1 part by mass or more, more preferably 10 parts by mass or more, per 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group. The content of the plasticizer in the curable composition is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, per 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group.

[0058] [Dehydrating agent] The curable composition preferably further contains a dehydrating agent, which can prevent the curable composition from being cured due to moisture contained in the air or the like during storage of the curable composition.

[0059] Examples of the dehydrating agent include silane compounds such as vinyltrimethoxysilane, dimethyldimethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, tetramethoxysilane, phenyltrimethoxysilane, and diphenyldimethoxysilane; and ester compounds such as methyl orthoformate, ethyl orthoformate, methyl orthoacetate, and ethyl orthoacetate. These dehydrating agents may be used alone or in combination of two or more. Among them, vinyltrimethoxysilane is preferred.

[0060] The content of the dehydrating agent in the curable composition is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, based on 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group. The content of the dehydrating agent in the curable composition is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, based on 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group. When the content of the dehydrating agent in the curable composition is 0.5 parts by mass or more, the effect obtained by the dehydrating agent can be sufficiently obtained. In addition, when the content of the dehydrating agent in the curable composition is 20 parts by mass or less, the curable composition has excellent curability.

[0061] [Other additives] The curable composition may contain other additives such as a thixotropic agent, an antioxidant, an ultraviolet absorber, a pigment, a dye, an antisettling agent, an aminosilane coupling agent, a thixotropic agent, and a solvent. Among these, the thixotropic agent, the ultraviolet absorber, and the antioxidant are preferred.

[0062] The thixotropy-imparting agent may be any agent capable of imparting thixotropy to the curable composition. Preferred examples of the thixotropy-imparting agent include hydrogenated castor oil, fatty acid bisamide, and fumed silica.

[0063] The content of the thixotropy-imparting agent in the curable composition is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, relative to 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group. The content of the thixotropy-imparting agent in the curable composition is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, relative to 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group. When the content of the thixotropy-imparting agent in the curable composition is 0.1 parts by mass or more, the thixotropy can be effectively imparted to the curable composition. In addition, when the content of the thixotropy-imparting agent in the curable composition is 200 parts by mass or less, the curable composition has an appropriate viscosity, and the handleability of the curable composition is improved.

[0064] Examples of the ultraviolet absorbent include benzotriazole-based ultraviolet absorbents and benzophenone-based ultraviolet absorbents, and benzotriazole-based ultraviolet absorbents are preferred. The content of the ultraviolet absorbent in the curable composition is preferably 0.1 parts by mass or more per 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group. The content of the ultraviolet absorbent in the curable composition is preferably 20 parts by mass or less, more preferably 10 parts by mass or less per 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group.

[0065] Examples of the antioxidant include hindered phenol-based antioxidants, monophenol-based antioxidants, bisphenol-based antioxidants, and polyphenol-based antioxidants, and the like, and the hindered phenol-based antioxidants are preferred. The content of the antioxidant in the curable composition is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, relative to 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group. The content of the antioxidant in the curable composition is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, relative to 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group.

[0066] [Light stabilizer] The curable composition preferably contains a hindered amine-based light stabilizer. The hindered amine-based light stabilizer can provide a curable composition that can maintain excellent rubber elasticity for a long period of time after curing.

[0067] Examples of the hindered amine light stabilizer include a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate and methyl 1,2,2,6,6-pentamethyl-4-piperidylsebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, dibutylamine·1,3,5-triazine·N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl-1,6-hexamethylenediamine and N-(2,2,6,6 poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}], and a polycondensate of dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol.

[0068] The hindered amine-based light stabilizer is preferably a NOR-type hindered amine-based light stabilizer. The NOR-type hindered amine-based light stabilizer can provide a curable composition in which the decrease in rubber elasticity over time after curing is suppressed.

[0069] The NOR type hindered amine light stabilizer has a NOR structure in which an alkyl group (R) is bonded to a nitrogen atom (N) contained in a piperidine ring skeleton via an oxygen atom (O). The number of carbon atoms in the alkyl group in the NOR structure is preferably 1 to 20, more preferably 1 to 18, and particularly preferably 18. Examples of the alkyl group include a linear alkyl group, a branched alkyl group, and a cyclic alkyl group (a saturated alicyclic hydrocarbon group).

[0070] Examples of linear alkyl groups include methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-octyl, n-nonyl, and n-decyl groups. Examples of branched alkyl groups include isopropyl, isobutyl, sec-butyl, and tert-butyl. Examples of cyclic alkyl groups (saturated alicyclic hydrocarbon groups) include cyclopentyl, cyclohexyl, and cyclooctyl groups. In addition, the hydrogen atoms constituting the alkyl groups may be substituted with halogen atoms (e.g., fluorine, chlorine, and bromine atoms) or hydroxyl groups.

[0071] The NOR type hindered amine light stabilizer includes a hindered amine light stabilizer represented by the following formula (I).

[0072] [ka]

[0073] When a NOR type hindered amine light stabilizer is used, it is preferable to use the NOR type hindered amine light stabilizer in combination with a benzotriazole type ultraviolet absorber or a triazine type ultraviolet absorber, which can provide a curable composition in which the decrease in rubber elasticity over time after curing is more significantly suppressed.

[0074] The content of the hindered amine light stabilizer in the curable composition is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, based on 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group. The content of the hindered amine light stabilizer in the curable composition is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, based on 100 parts by mass of the polyalkylene oxide having a hydrolyzable silyl group.

[0075] The curable composition can be produced by mixing a polyalkylene oxide having a hydrolyzable silyl group, glass frit, an inorganic compound having a total gas generation amount of 0.5 to 20% at 150 to 300°C, calcium carbonate, and additives added as necessary. The curable composition may be in the form of a suspension or emulsion by being suspended or emulsified in an aqueous solvent. The curable composition may be in the form of a solution dissolved in a solvent. Examples of the aqueous solvent include alcohols such as ethyl alcohol, methyl alcohol, and isopropyl alcohol, and water. Examples of the solvent include xylene, toluene, and acetone.

[0076] After the curing, the curable composition, i.e., the cured product of the curable composition, preferably has a volume expansion coefficient of at least 2 times when heated for 30 minutes at 250° C. When the cured product of the curable composition has a volume expansion coefficient of at least 2 times when heated for 30 minutes at 250° C., the cured product of the curable composition expands quickly due to heat during a fire, smoothly follows the expansion of the sealed part, and can stably maintain the closure of the sealed part.

[0077] The volume expansion coefficient of the cured product of the curable composition when heated at 250°C for 30 minutes is measured as follows. The volume W1 of a test piece made of the cured product of the curable composition before heating is measured. Next, the test piece is fed into a thermostatic chamber at 250°C and left there for 30 minutes. The test piece is removed from the thermostatic chamber and left at 25°C for 3 hours to cool. Thereafter, the volume W2 of the test piece after heating is measured and calculated based on the following formula. The volume W of the test piece is measured by completely immersing the test piece in water and subtracting the volume of water before immersion from the volume of water containing the test piece after immersion. Volume expansion rate (%) when heated at 250℃ for 30 minutes = Volume of test piece after heating W2 / Volume of test piece before heating W1

[0078] The curable composition after its curing, i.e., the cured product of the curable composition, has a rubber elasticity of 5 or more at 23°C according to Shore A, more preferably 10 or more. The curable composition after its curing, i.e., the cured product of the curable composition, has a rubber elasticity of 50 or less at 23°C according to Shore A, more preferably 40 or less. When the cured product of the curable composition has a rubber elasticity of 5 or more at 23°C according to Shore A, the cured product of the curable composition has excellent rubber elasticity despite being heated by heat during a fire, smoothly follows the expansion of the sealing part, and can stably maintain the closure of the sealing part. When the cured product of the curable composition has a rubber elasticity of 50 or less at 23°C according to Shore A, the cured product of the curable composition smoothly expands without breaking bubbles due to gas generated from the inorganic compound during a fire, smoothly follows the expansion of the sealing part, and can stably maintain the closure of the sealing part. The Shore A rubber elasticity of the cured product of the curable composition refers to a value measured at a measurement temperature of 23° C. using an A-type durometer in accordance with JIS K6253.

[0079] After the curable composition is cured, the cured product of the curable composition preferably has a rubber elasticity at 23° C. of 40 or more according to Shore A after being left for 1 hour at 23° C. following combustion at 600° C. When the rubber elasticity at 23° C. of 40 or more according to Shore A after being left for 1 hour at 23° C. following combustion at 600° C., the combustion residue of the cured product of the curable composition can be stably retained in the sealing portion, and the closure of the sealing portion can be stably maintained.

[0080] The rubber elasticity at 23°C according to Shore A of the cured product of the curable composition after burning at 600°C and leaving at 23°C for 1 hour is measured as follows. 100 g of the cured product of the curable composition is prepared as a sample. The sample is fed into a combustion furnace. The sample is burned in the combustion furnace at 600°C for 30 minutes. The combustion residue obtained by burning the sample is immediately left in an atmosphere at 23°C for 1 hour after the end of burning. Next, the rubber elasticity of the combustion residue according to Shore A is measured using an A-type durometer at a measurement temperature of 23°C in accordance with JIS K6253.

[0081] The curable composition can be suitably used as a sealing material. A panel structure can be constructed using the curable composition as a sealing material. As a method for constructing a panel structure by applying the curable composition to a sealing part of an architectural structure, a method is used in which the curable composition is filled into the sealing part and then cured to harden it. The obtained panel structure includes a panel installation part of the architectural structure, a panel member installed in the panel installation part of the architectural structure, and a hardened product of the curable composition filled between the opposing surfaces of the panel installation part and the panel member. Examples of the panel member include mortar board, flexible board, gypsum board, calcium silicate board, medium density fiberboard, particle board, wood-based plywood, and hard fiberboard.

[0082] The sealing portion is not particularly limited, and examples thereof include a gap formed between a panel arrangement portion formed in an architectural structure and a panel member arranged in this panel arrangement portion, and a gap formed between opposing surfaces of adjacent panel members.

[0083] In the event of a fire, the panel members constituting the panel structure may be heated to about 300°C by the heat of the fire and shrink, causing the sealing portion to expand. On the other hand, the cured product of the curable composition maintains excellent rubber elasticity and expands smoothly even when heated to about 400°C by the heat of the fire, so it smoothly follows the expansion of the sealing portion and can reliably maintain the closed state of the sealing portion.

[0084] The cured product of the curable composition produces strong combustion residues when burned by the heat of a fire. This combustion residue fills the sealing parts of architectural structures, reliably keeping them sealed even in the event of a fire, preventing flames from penetrating through the sealing parts and imparting excellent fire resistance to the panel structure of the architectural structure. Effect of the Invention

[0085] The curable composition of the present invention has excellent rubber elasticity and expands smoothly by heat when it is heated up to about 400° C. Therefore, when the curable composition is used as a sealant, the cured product of the curable composition smoothly follows the expansion of the sealed part even if the sealed part expands in the event of a fire, and can stably maintain the closed state of the sealed part.

[0086] The curable composition of the present invention produces a strong combustion residue upon combustion, which reliably fills and seals the sealing section even in the event of a fire, preventing flames from penetrating through the sealing section and imparting excellent fire resistance to the panel structure of an architectural structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0087] The present invention will be described in more detail below using examples, but the present invention is not limited thereto. EXAMPLES

[0088] The following raw materials were used in producing the curable compositions of the Examples and Comparative Examples.

[0089] [Polyalkylene oxide having hydrolyzable silyl groups] Polyalkylene oxide (polyalkylene oxide whose main chain skeleton is made of polypropylene oxide and has a methyldimethoxysilyl group at the end of the main chain, number average molecular weight: 16,000, manufactured by Asahi Glass Co., Ltd., product name "Exestar S3430")

[0090] [Glass frit] Glass frit (phosphate glass, "VY0144" manufactured by Nippon Frit Co., Ltd., main components: P2O5, AI2O3 and R2O, where R is an alkali metal atom, softening point: 404°C)

[0091] [Inorganic compounds] Aluminum phosphite (total gas generated: 9%, loss on heating: 9%) Expandable graphite (manufactured by Air Water Corporation, product name "TEG", Mohs hardness: 1, total gas generated: 3%, heat loss: 3%) Sodium bicarbonate (total gas generated: 1%, loss from heating: 1%)

[0092] [Calcium carbonate] Colloidal calcium carbonate (Shiraishi Kogyo Co., Ltd., product name "CCR", average particle size: 0.08 μm)

[0093] [Silanol condensation catalyst] Silanol condensation catalyst (1,1,3,3-tetrabutyl-1,3-dilauryloxycarbonyl-distannoxane, manufactured by Nitto Kasei Co., Ltd., product name "Neostan U-130")

[0094] [Antioxidants] Hindered phenol antioxidant (BASF Japan product name "Irganox 1010")

[0095] (Example 1 to 5 , Comparative Example 1 ~3 ) A polyalkylene oxide having a hydrolyzable silyl group, glass frit, an inorganic compound, calcium carbonate, a silanol condensation catalyst, and a hindered phenol-based antioxidant were mixed in the amounts shown in Table 1 using a planetary mixer under a vacuum atmosphere for 60 minutes until the mixture became uniform, thereby obtaining a curable composition.

[0096] The obtained curable composition was measured in the above manner for the volume expansion coefficient of the cured product when heated at 250°C for 30 minutes, the rubber elasticity at 23°C by Shore A of the cured product, and the rubber hardness at 23°C by Shore A after burning at 600°C and leaving at 23°C for 1 hour, and the results are shown in Table 1. In Table 1, "volume expansion coefficient of the cured product when heated at 250°C for 30 minutes" is represented as "volume expansion coefficient," "rubber elasticity at 23°C by Shore A of the cured product" is represented as "rubber elasticity (before burning)," and "rubber elasticity at 23°C by Shore A after burning at 600°C and leaving at 23°C for 1 hour" is represented as "rubber elasticity (after burning)."

[0097] [Table 1]

Claims

1. 100 parts by mass of a polyalkylene oxide having a hydrolyzable silyl group; 20 to 150 parts by mass of glass frit; 2 to 70 parts by mass of an inorganic compound having a total gas generation amount of 0.5 to 20% at 150 to 300° C.; 50 to 300 parts by mass of calcium carbonate, and a silanol condensation catalyst, a mass ratio of the content of the glass frit to the content of the inorganic compound (content of the glass frit / content of the inorganic compound) is 0.1 to 40; A curable composition, wherein the inorganic compound comprises at least one selected from the group consisting of aluminum phosphate, aluminum phosphite, expandable graphite, aluminum hydroxide, and sodium bicarbonate.

2. 100 parts by mass of a polyalkylene oxide having a hydrolyzable silyl group; 20 to 150 parts by mass of glass frit; 2 to 70 parts by mass of an inorganic compound having a heat loss of 0.5 to 20% at 150 to 300° C.; 50 to 300 parts by mass of calcium carbonate, and a silanol condensation catalyst, a mass ratio of the content of the glass frit to the content of the inorganic compound (content of the glass frit / content of the inorganic compound) is 0.1 to 40; A curable composition, wherein the inorganic compound comprises at least one selected from the group consisting of aluminum phosphate, aluminum phosphite, expandable graphite, aluminum hydroxide, and sodium bicarbonate.

3. 3. The curable composition according to claim 1, wherein the polyalkylene oxide has a hydrolyzable silyl group at a terminal thereof.

4. 4. The curable composition according to claim 1, wherein the inorganic compound contains at least one inorganic compound selected from the group consisting of aluminum phosphate, aluminum phosphite, and sodium bicarbonate.

5. The curable composition according to any one of claims 1 to 4, characterized in that after curing, the volume expansion coefficient when heated at 250°C for 30 minutes is 2 times or more, the rubber elasticity at 23°C by Shore A is 5 to 50, and the rubber elasticity at 23°C by Shore A after being left at 23°C for 1 hour after combustion at 600°C is 40 or more.

6. The curable composition according to any one of claims 1 to 5, which is used as a sealing material.

7. A panel installation section of the architectural structure; A panel member disposed in a panel installation section of the architectural structure; A panel structure comprising: a cured product of the curable composition according to any one of claims 1 to 6, filled between the opposing surfaces of the panel mounting portion and the panel member.

8. The panel structure according to claim 7, comprising a cured product of the curable composition according to any one of claims 1 to 6, filled in a joint formed between adjacent panel members.

Citation Information

Patent Citations

  • Fireproof sealing material

    JP1996081674A

  • Hardening composition for fire protection

    JP1996259794A

  • Room temperature curing composition for fire retarder

    JP1997071780A

  • Curable composition

    JP2018039997A

  • Curable composition

    JP2019014885A