Composite positive electrode active material, positive electrode and lithium battery using the same, and manufacturing method thereof

A composite positive electrode active material with a nickel-based core and multilayer shell addresses the issues of poor lifetime and thermal stability in nickel-based materials by stabilizing the surface and reducing side reactions, leading to improved cycling and thermal performance in lithium batteries.

JP7570750B2Active Publication Date: 2024-10-22SAMSUNG ELECTRONICS CO LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2019192711
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-10-24
Filing Date
2019-10-23
Publication Date
2024-10-22
Estimated Expiration
2039-10-23

AI Technical Summary

Technical Problem

Conventional nickel-based positive electrode active materials for lithium batteries suffer from poor lifetime characteristics and thermal stability due to high surface residual lithium content and side reactions, necessitating a solution to prevent battery performance deterioration.

Method used

A composite positive electrode active material is developed with a core containing nickel-based first lithium transition metal oxide, surrounded by a multilayer shell comprising a first layer with a specific metal composition and a second layer containing phosphorus, which stabilizes the surface and suppresses side reactions with the electrolyte.

Benefits of technology

The composite structure improves cycling characteristics and thermal stability of lithium batteries by reducing surface lithium content, suppressing side reactions, and forming a stable solid electrolyte interface, thereby enhancing battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570750000028
    Figure 0007570750000028
  • Figure 0007570750000029
    Figure 0007570750000029
  • Figure 0007570750000030
    Figure 0007570750000030
Patent Text Reader

Abstract

To provide a composite positive electrode active material, a positive electrode and a lithium cell employing the same, and a manufacturing method thereof.SOLUTION: A composite positive electrode active material comprises a core containing multiple primary particles, and a shell placed on the core, where the primary particle contains a nickel-based first lithium transition metal oxide, the shell comprises a first layer, and a second layer placed on the first layer. The first layer comprises a first composition containing a first metal, the second layer comprises a second composition containing phosphorus (P), and the first metal is one or more metals belonging to the 2 to 5 groups, and the 7 to 15 groups of an element periodic table other than nickel. A positive electrode and a lithium cell containing the same, and a composite positive electrode active material production method are also provided.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite positive electrode active material, a positive electrode and a lithium battery employing the same, and a method for producing the same. [Background technology]

[0002] In order to meet the trend of miniaturization and high performance of various devices, it is becoming important for lithium batteries to have high energy density in addition to miniaturization and weight reduction, i.e., high capacity lithium batteries are becoming important.

[0003] In order to realize a lithium battery suitable for this purpose, positive electrode active materials having high capacity are being investigated.

[0004] Conventional nickel-based positive electrode active materials have a high surface residual lithium content and side reactions due to cation mixing, which reduces their life characteristics and also causes poor thermal stability.

[0005] Therefore, a method is required that can prevent deterioration of battery performance while containing a nickel-based positive electrode active material. Summary of the Invention [Problem to be solved by the invention]

[0006] The problem to be solved by the present invention is to provide a new composite positive electrode active material capable of suppressing side reactions of the composite positive electrode active material and preventing deterioration of battery performance.

[0007] Another problem to be solved by the present invention is to provide a positive electrode comprising the above-mentioned composite positive electrode active material.

[0008] Another problem to be solved by the present invention is to provide a lithium battery employing the above-mentioned positive electrode.

[0009] Another problem to be solved by the present invention is to provide a method for producing the above-mentioned composite positive electrode active material. [Means for solving the problem]

[0010] From one aspect, a core comprising a plurality of primary particles; a shell disposed on the core; the primary particles include a nickel-based first lithium transition metal oxide; the shell includes a first layer and a second layer disposed on the first layer; the first layer comprises a first composition comprising a first metal; the second layer comprises a second composition comprising phosphorus (P); A composite active cathode material is provided in which the first metal is one or more metals from Groups 2 through 5 and Groups 7 through 15 of the Periodic Table of the Elements other than nickel.

[0011] From another perspective, A positive electrode is provided that includes a composite active positive electrode material. In yet another aspect, A lithium battery is provided that includes a positive electrode.

[0012] In yet another aspect, providing a first lithium transition metal oxide; combining a first lithium transition metal oxide with a first metal precursor to provide a first composition of a first lithium transition metal oxide; mixing a first composition of a first lithium transition metal oxide with a phosphorus (P) precursor to provide a second composition of a first lithium transition metal oxide; and drying the first lithium transition metal oxide second composition and heat-treating it in an oxidizing atmosphere at 400° C. to 1,000° C. to produce a composite positive electrode active material. Effect of the Invention

[0013] According to one aspect of the present invention, a composite positive electrode active material includes a multi-layer coating layer in which a first layer including a first metal and a second layer including phosphorus (P) are sequentially laminated, thereby improving cycle characteristics and thermal stability of a lithium battery. [Brief description of the drawings]

[0014] [Figure 1A] 2 is a schematic diagram partially illustrating an internal structure of a composite positive electrode active material according to an embodiment; FIG. [Figure 1B] 1 is a schematic cross-sectional view of a composite positive electrode active material according to an embodiment; [Figure 2A] 1 is an XRD (X-ray diffraction) spectrum of the composite positive electrode active material prepared in Reference Example 1. [Figure 2B] 1 is an XRD (X-ray diffraction) spectrum of the composite positive electrode active material prepared in Example 1. [Figure 3A] 1 shows high-angle annular dark field (HAADF) STEM (scanning transmission electron microscopy) and energy dispersive X-ray spectrometry (EDS) images of a cross section of a composite positive electrode active material prepared in Reference Example 1. [Figure 3B] 1 shows HAADF STEM and EDS images of a cross section of the composite positive electrode active material prepared in Reference Example 1. [Figure 3C] 1 shows HAADF STEM and EDS images of a cross section of the composite positive electrode active material prepared in Reference Example 1. [Figure 4A] 1 shows high-angle annular dark field (HAADF) STEM and EDS images of a cross section of a composite positive electrode active material prepared in Example 1. [Figure 4B] 1 shows HAADF STEM and EDS images of a cross section of the composite positive electrode active material prepared in Example 1. [Figure 4C] 1 shows HAADF STEM and EDS images of a cross section of the composite positive electrode active material prepared in Example 1. [Figure 4D] 1 shows HAADF STEM and EDS images of a cross section of the composite positive electrode active material prepared in Example 1. [Diagram 5]1 shows differential scanning calorimetry (DSC) thermograms of composite positive electrode active materials in Example 1 and Comparative Example 3. [Figure 6] 1 is a schematic diagram of a lithium battery according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present inventive concept described below can be modified in various ways and can have various embodiments, but specific embodiments are illustrated in the drawings and described in detail in the detailed description. However, it should be understood that they do not limit the present inventive concept to specific embodiments, but include all modifications, equivalents, or alternatives that fall within the technical scope of the present inventive concept.

[0016] The terms used below are merely used to describe specific embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In the following, terms such as "include" or "have" indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, and should be understood not to preclude the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. In the following, " / " can be interpreted as "and" or "or" depending on the context.

[0017] In the drawings, the thickness of the various layers and regions is exaggerated or reduced for clarity. Similar parts are designated by the same reference numerals throughout the specification. Throughout the specification, when a part, such as a layer, film, region, or plate, is said to be "on" or "above" another part, this includes not only when it is directly on top of the other part, but also when there is another part between them. Throughout the specification, terms such as first and second are used to describe various components, but the components are not limited by the terms. The terms are used only to distinguish one component from another.

[0018] As used herein, a transition metal is an element belonging to groups 3 to 12 of the periodic table of the elements.

[0019] Hereinafter, a composite positive electrode active material, a positive electrode and a lithium battery including the same, and a method for manufacturing the same according to example embodiments will be described in more detail.

[0020] According to an embodiment, the composite positive electrode active material includes a core including a plurality of primary particles and a shell disposed on the core, the primary particles including a nickel-based first lithium transition metal oxide, the shell including a first layer and a second layer disposed on the first layer, the first layer including a first composition including a first metal, the second layer including a second composition including phosphorus (P), and the first metal being one or more metals belonging to Groups 2 to 5 and Groups 7 to 15 of the Periodic Table of the Elements other than nickel.

[0021] Referring to FIG. 1A, the composite positive electrode active material 300 includes a core 100 including a plurality of primary particles 10 and a shell 200 disposed on the core 100. The core 100 is a secondary particle including a plurality of primary particles 10. The primary particles 10 are, for example, crystallites having the same crystal structure within the primary particles 10. The primary particles 10 include a nickel-based first lithium transition metal oxide, and the shell 200 has a multi-layer structure including a first layer (not shown) and a second layer (not shown) disposed on the first layer. The first layer includes a first composition including a first metal, and the second layer includes a second composition including phosphorus (P). The first metal is one or more metals belonging to Groups 2 to 5 and Groups 7 to 15 of the Periodic Table of Elements other than nickel. The nickel-based first lithium transition metal oxide has a layered crystal structure.

[0022] Hereinafter, the theoretical basis for why the composite positive electrode active material according to one embodiment provides excellent effects will be described. However, this is intended to aid in understanding the present invention and is not intended to limit the present invention in any manner.

[0023] A first layer including a first composition including a first metal is disposed on the core 100 of the composite positive electrode active material 300, for example, to stabilize the surface of the core 100 and recover the active material performance caused by washing the core with water. The metal contained in the core 100 is intermixed with the metal contained in the first layer by heat treatment during the manufacturing process of the first layer, and the core 100 exhibits the effects of stabilizing the surface structure and recovering the active material performance. A second layer including a second composition including phosphorus (P) is additionally disposed on the first layer. The second layer acts as a surface protection layer that protects the core and / or the first layer, and suppresses side reactions between them and the electrolyte. In addition, by additionally disposing the second layer including the second composition including phosphorus (P) on the first layer, for example, nickel ion elution from the core 100 into the electrolyte is effectively suppressed. In addition, in the process of forming the second layer, the precursor of the second composition reacts with the lithium remaining on the core 100 and / or the first layer, thereby reducing the amount of lithium remaining on the surface of the composite positive electrode active material 300. Therefore, for example, side reactions between the composite positive electrode active material 300 and the electrolyte and gas generation are effectively suppressed. In addition, the second layer forms a stable artificial solid electrolyte interface (SEI) by reacting with moisture, HF, etc. during the initial charge and discharge of the lithium battery, thereby suppressing the generation of by-products due to additional side reactions between the composite positive electrode active material 300 and moisture, HF, etc. remaining in the electrolyte. Therefore, the surface of the composite positive electrode active material 300 is stabilized. That is, the second layer acts as a protecting layer having lithium ion conductivity, thereby improving the stability of the composite positive electrode active material 300. In addition, the second layer has a polarity and therefore has excellent wettability to the electrolyte, thereby reducing the interfacial resistance between the composite positive electrode active material 300 and the electrolyte. Therefore, despite the addition of the second layer, the internal resistance of the lithium battery including the composite positive electrode active material 300 is maintained or reduced. As a result, the cycle characteristics and thermal stability of the lithium battery including the composite positive electrode active material 300 are improved.

[0024] In the composite positive electrode active material, the nickel content in the transition metal contained in the first lithium transition metal oxide is 70 mol% or more, 71 mol% or more, 75 mol% or more, 80 mol% or more, 85 mol% or more, 90 mol% or more, 93 mol% or more, 95 mol% or more, 97 mol% or more, 71 mol% to 99 mol%, 75 mol% to 98 mol%, or 78 mol% to 90 mol%. Since the nickel content in the first lithium transition metal active material is 70 mol% or more, high capacity can be achieved. Therefore, a lithium battery providing high capacity is realized.

[0025] The first composition contained in the first layer includes a first phase, and the second composition contained in the second layer includes a second phase distinct from the first phase. The first and second phases have different crystal structures, for example.

[0026] The first composition includes, for example, one or more selected from a phase having a layered crystal structure and a phase having a spinel crystal structure. The first composition includes, for example, a phase having a layered crystal structure belonging to the R-3m space group. The first composition includes, for example, a phase having a spinel crystal structure belonging to the Fd-3m space group. When the first composition includes such a phase, the cycle characteristics and thermal stability of the lithium battery are further improved.

[0027] A first layer is disposed on the primary particles constituting the core, and for example, the concentration of the first metal contained in the first layer is higher than the concentration of the first metal contained in the primary particles. Referring to Figures 3B and 4B, a first layer is disposed on the primary particles constituting the core, and the concentration of Co contained in the first layer is higher than the concentration of Co contained in the primary particles. In Figures 3B and 4B, the higher the concentration, the brighter the color. For example, the concentration per unit area of ​​the first metal contained in the first layer is higher than the concentration per unit area of ​​the first metal contained in the primary particles.

[0028] In the composite positive electrode active material, for example, the second layer is thicker than the first layer contained in the shell. The second layer is thicker than the first layer, so that the elution of metal ions and the side reaction between the composite positive electrode active material and the electrolyte are more effectively suppressed. Therefore, even though the second layer, which is thicker than the first layer, is added, the cycle characteristics of a lithium battery including the composite positive electrode active material are improved.

[0029] The thickness of the first layer is, for example, 50 nm or less, 40 nm or less, 30 nm or less, 20 nm or less, 10 nm or less, or 5 nm or less. The thickness of the first layer is, for example, 1 nm to 50 nm, 1 nm to 40 nm, 1 nm to 30 nm, 1 nm to 20 nm, 1 nm to 10 nm, 1 nm to 5 nm, 2 nm to 50 nm, 4 nm to 40 nm, 6 nm to 30 nm, or 8 nm to 20 nm. When the first layer has a thickness in such a range, the cycle characteristics and thermal stability of the lithium battery are further improved. The thickness of the second layer is, for example, 500 nm or less, 400 nm or less, 300 nm or less, 200 nm or less, 100 nm or less, or 50 nm or less. The thickness of the first layer is, for example, 10 nm to 500 nm, 10 nm to 400 nm, 10 nm to 300 nm, 10 nm to 200 nm, 10 nm to 100 nm, 20 nm to 500 nm, 30 nm to 400 nm, or 50 nm to 300 nm. When the second layer has a thickness in such a range, the cycle characteristics and thermal stability of the lithium battery are further improved.

[0030] In the composite positive electrode active material, the thickness of the shell including the first layer and the second layer is, for example, 550 nm or less, 450 nm or less, 350 nm or less, 250 nm or less, 150 nm or less, or 50 nm or less. The thickness of the shell is, for example, 10 nm to 550 nm, 10 nm to 450 nm, 10 nm to 350 nm, 10 nm to 250 nm, 10 nm to 150 nm, 10 nm to 50 nm, 20 nm to 550 nm, 40 nm to 450 nm, 60 nm to 350 nm, 80 nm to 250 nm, or 100 nm to 150 nm. When the shell has a thickness in such a range, the cycle characteristics and thermal stability of the lithium battery are further improved.

[0031] In the composite positive electrode active material, the shell covers a part or the whole of the core surface. For example, the shell covers 10% or more, 20% or more, 30% or more, 40% or more, or 50% or more of the core; 10% to 100%, 20% to 98%, or 30% to 90%. The shell is arranged on the core in the form of discontinuous islands or in a continuous form. Referring to Figures 4A to 4D, the shell is arranged, for example, on two or more primary particles exposed on the surface of the core.

[0032] The first composition is, for example, disposed on (eg, directly on) the primary particles constituting the core and / or on the secondary particles corresponding to the core.

[0033] The first metal contained in the first composition is selected from, for example, Co, Mg, Zr, Al, Mn, Si, Pd, Ti, Sn, Ir, Pt, Ru, Ce, B, Nb, V, Fe, and Zn. When the first composition contains such a first metal, the cycle characteristics and thermal stability of a lithium battery containing the composite positive electrode active material are further improved. When the first layer contains, for example, Co, which provides discharge capacity, the capacity reduction of the composite positive electrode active material is prevented. When the first layer contains, for example, Mg, the structural stability of the composite positive electrode active material is improved, and as a result, the life characteristics of a lithium battery containing the composite positive electrode active material are improved.

[0034] In the composite positive electrode active material, the first composition is, for example, a composition including a first metal and oxygen, or a composition including lithium, a first metal, and oxygen. The first composition includes, for example, about 0 to about 3.3 moles of lithium per mole of the first composition, about 0.7 to about 3.3 moles of the first metal per mole of the first composition, and about 1.7 to about 4.3 moles of oxygen per mole of the first composition. The first composition includes, for example, about 0 to about 3.2 moles of lithium per mole of the first composition, about 0.8 to about 3.2 moles of the first metal per mole of the first composition, and about 1.8 to about 4.2 moles of oxygen per mole of the first composition. The first composition includes, for example, about 0 to about 3.1 moles of lithium per mole of the first composition, about 0.9 to about 3.1 moles of the first metal per mole of the first composition, and about 1.9 to about 4.1 moles of oxygen per mole of the first composition. When the first composition has a composition within such a range, the cycle characteristics and thermal stability of a lithium battery including the composite positive electrode active material are further improved.

[0035] The first composition may, for example, have a composition represented by the following formula 1:

[0036] [ka]

[0037] In the above Chemical Formula 1, M1 is one or more selected from Co, Mg, Zr, Al, Mn, Si, Pd, Ti, Sn, Ir, Pt, Ru, Ce, B, Nb, V, Fe, and Zn, and 0≦a≦3.1, 0.9≦b≦3.1, and 1.9≦c≦4.1.

[0038] The first composition may be, for example, Co 3 O 4 , MgO, Li x Chief of Staff 2 (0 <x≦1.5)、Li 2 ZrO 3 The term "selected" includes one or more of the following:

[0039] In the composite positive electrode active material, the content of the first composition or the content of the first metal contained in the first layer is, for example, 10 parts by weight or less, 5 parts by weight or less, 4 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, or 1 part by weight or less, relative to 100 parts by weight of the first lithium transition metal oxide. The content of the first composition or the content of the first metal contained in the first layer is, for example, 0.01 to 10 parts by weight or less, 0.05 to 5 parts by weight or less, 0.1 to 4 parts by weight or less, 0.1 to 3 parts by weight or less, 0.1 to 2 parts by weight or less, or 0.1 to 1 part by weight or less, relative to 100 parts by weight of the first lithium transition metal oxide. When the first layer contains the first composition or the first metal in such a content range, the cycle characteristics and thermal stability of a lithium battery including the composite positive electrode active material are further improved.

[0040] In the composite positive electrode active material, the second composition is, for example, a composition including a first metal, phosphorus (P) and oxygen, or a composition including lithium, a first metal, phosphorus (P) and oxygen. The second composition includes, for example, 0 to about 3.3 moles of lithium per mole of the second composition, about 0.7 to about 3.3 moles of the first metal per mole of the second composition, about 0.7 to about 2.3 moles of phosphorus per mole of the second composition, and about 3.7 to about 8.3 moles of oxygen per mole of the second composition. The second composition includes, for example, 0 to about 3.2 moles of lithium per mole of the second composition, about 0.8 to about 3.2 moles of the first metal per mole of the second composition, about 0.8 to about 2.2 moles of phosphorus per mole of the second composition, and about 3.8 to about 8.2 moles of oxygen per mole of the second composition. The second composition may, for example, contain 0 to about 3.1 moles of lithium per mole of the second composition, about 0.9 to about 3.1 moles of the first metal per mole of the second composition, about 0.9 to about 2.1 moles of phosphorus per mole of the second composition, and about 3.6 to about 8.4 moles of oxygen per mole of the second composition. The second composition having such a composition range further improves the cycle characteristics and thermal stability of a lithium battery including the composite positive electrode active material. The second composition may, for example, contain a phosphate compound.

[0041] The second composition may, for example, have a composition represented by Formula 2:

[0042] [ka]

[0043] In the above Chemical Formula 2, M2 is one or more selected from Co, Mg, Zr, Al, Mn, Si, Pd, Ni, Ti, Sn, Mo, Ir, Pt, Ru, Ce, B, Nb, V, Fe, and Zn, and 0≦a≦3.1, 0.9≦b≦3.1, and 0.9≦c≦2.1.

[0044] The second composition may be, for example, Li 3 PO 4 , LiCoPO 4 , Co 3 (PO 4 ) 2 The term "selected" includes one or more of the following:

[0045] In the composite positive electrode active material, the content of the second composition or the content of phosphorus (P) contained in the second layer is, for example, 10 parts by weight or less, 5 parts by weight or less, 4 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, or 1 part by weight or less, relative to 100 parts by weight of the first lithium transition metal oxide. The content of the second composition or the content of phosphorus (P) contained in the second layer is, for example, 0.01 to 10 parts by weight or less, 0.05 to 5 parts by weight or less, 0.1 to 4 parts by weight or less, 0.1 to 3 parts by weight or less, 0.1 to 2 parts by weight or less, or 0.1 to 1 part by weight or less, relative to 100 parts by weight of the first lithium transition metal oxide. When the second layer contains the second composition or phosphorus (P) in such a content range, the cycle characteristics and thermal stability of a lithium battery including the composite positive electrode active material are further improved.

[0046] The second composition can be disposed on the primary particles constituting the core and / or on the secondary particles corresponding to the core. The second layer is disposed, for example, on the first layer and optionally on the core. A portion of the second layer is disposed, for example, on the surface of the core.

[0047] 1A and 1B, in the composite positive electrode active material 300, the core 100 includes a grain boundary 20 disposed between adjacent primary particles 10 of the plurality of primary particles 10, and the grain boundary 20 includes a third composition including a second metal. Since the grain boundary between adjacent primary particles 10 of the plurality of primary particles 10 constituting the core 100 of the composite positive electrode active material 300 includes the third composition, lithium ion conduction in the core 100 is facilitated, and the elution of nickel ions from the primary particles 10 in the core 100 to the electrolyte that has permeated into the core 100 is suppressed. In addition, a side reaction between the primary particles 10 and the electrolyte in the core 100 is suppressed. Therefore, the cycle characteristics of a lithium battery including the composite positive electrode active material 300 are improved. In addition, the content of residual lithium on the surface of the plurality of primary particles 10 disposed in the core 100 is reduced, deterioration of the composite positive electrode active material 300 is suppressed, and gas generation is reduced, thereby improving the thermal stability of the lithium battery. The third composition disposed at the grain boundaries 20 between adjacent primary particles 10 prevents surface damage to the primary particles 10 that occurs during the cleaning process of the composite positive electrode active material 300, thereby preventing a decrease in the life characteristics of the lithium battery. The third composition disposed at the grain boundaries 20 between adjacent primary particles 10 accommodates the volume change caused by charging and discharging the primary particles 10 and suppresses cracks between the primary particles 10, thereby suppressing a decrease in the mechanical strength of the composite positive electrode active material 300 even after long-term charging and discharging, thereby preventing deterioration of the lithium battery. In addition, the second metal contained in the third composition is doped into the lithium transition metal oxide contained in the primary particles 10, thereby stabilizing the crystal structure of the lithium transition metal oxide, and further improving the cycle characteristics of a lithium battery including the composite positive electrode active material.

[0048] The third composition contained in the grain boundary 20 has, for example, a third phase that is distinct from the phase contained in the primary particles. The third phase is distinct from the phase of the primary particles 10 in structure, composition, or both. The third phase has, for example, a monoclinic crystal structure. Since the third composition has a monoclinic crystal structure, two-dimensional movement of lithium ions is possible in the grain boundary 20 containing the third composition, and therefore lithium ion conduction is further facilitated in the core 100, improving cycle characteristics. The third composition has, for example, a monoclinic crystal structure belonging to the C2 / m, C12 / c1, or C2 / c space group. The third composition has a monoclinic crystal structure belonging to the C2 / m, C12 / c1 or C2 / c space group, so that the cycle characteristics and thermal stability of a lithium battery including the composite positive electrode active material are further improved.

[0049] The second metal contained in the third composition is, for example, selected from Zr, Al, Co, Mg, Mn, Si, Mo, Pd, Ti, Sn, Ir, Pt, Ru, Ce, B, Nb, V, Fe, and Zn. When the third composition contains such a second metal, the charge and discharge characteristics of a lithium battery containing the composite positive electrode active material are further improved.

[0050] In the composite positive electrode active material, the third composition may include lithium, a second metal, and oxygen. The third composition may, for example, include about 1.7 to about 2.3 moles of lithium per mole of the third composition, about 0.7 to about 1.3 moles of the second metal per mole of the third composition, and about 2.7 to about 3.3 moles of oxygen per mole of the third composition. The third composition may, for example, include about 1.8 to about 2.2 moles of lithium per mole of the third composition, about 0.8 to about 1.2 moles of the second metal per mole of the third composition, and about 2.8 to about 3.2 moles of oxygen per mole of the third composition. The third composition may, for example, include about 1.9 to about 2.1 moles of lithium per mole of the third composition, about 0.9 to about 1.1 moles of the second metal per mole of the third composition, and about 2.9 to about 3.1 moles of oxygen per mole of the third composition.

[0051] The third composition may, for example, have a composition represented by the following formula 3:

[0052] [ka]

[0053] In the above Chemical Formula 3, M3 is one or more selected from Zr, Al, Co, Mg, Mn, Si, Pd, Ni, Ti, Sn, Ir, Pt, and Ru, and 1.9≦a≦2.1, 0.9≦b≦1.1, and 2.9≦a≦3.1.

[0054] 1B, in the core 100 of the composite positive electrode active material 300, the grain boundaries 20 have, for example, a substantially straight line shape. Since the primary particles 10 adjacent to the grain boundaries 20 include the first lithium transition metal oxide having a layered crystal structure, the primary particles 10 have a polyhedral shape, and therefore the grain boundaries 20 disposed between the adjacent primary particles 10 also have a straight line shape. Alternatively, the grain boundaries 20 have, for example, a substantially curved shape. The radius of curvature of the curve is, for example, more than 0 and not more than 1 m.

[0055] 1B, in the composite positive electrode active material 300, the grain boundaries 20 are arranged in a direction (21) that is, for example, parallel to the surface of the adjacent primary particle 10. In addition, the direction (21) in which the grain boundaries 20 are arranged is, for example, different from the tangent direction (101) of the surface of the core 100 that is closest to the grain boundary 20.

[0056] 1B, in the composite positive electrode active material 300, the core 100 includes a first grain boundary 32 and a second grain boundary 33, the first grain boundary 32 and the second grain boundary 33 are directly disposed on the same primary particle 30, and the first grain boundary 32 and the second grain boundary 33 intersect at an angle (α) determined by the shape of the primary particle 30. The angle (α) at ​​which the first grain boundary 32 and the second grain boundary 33 intersect is, for example, more than 0° and less than 180°, 10° to 170°, 20° to 160°, 30° to 150°, 40° to 140°, 50° to 130°, 60° to 120°, 70° to 110°, or 80° to 110°.

[0057] 1B, in the composite positive electrode active material 300, the core 100 includes a plurality of grain boundaries 32, 42 adjacent to a plurality of primary particles 30, 40, respectively. The grain boundaries 32, 42 are each arranged in a direction (31, 41) parallel to the surface of the adjacent primary particles 30, 40. The directions (31, 41) in which the grain boundaries 32, 42 are each arranged are different from each other.

[0058] 1B, the core 100 of the composite positive electrode active material 300 has an average grain boundary length of about 50 nm to about 1,000 nm and an average grain boundary thickness of about 1 nm to about 200 nm. The length direction of the grain boundary is parallel to the surface of the adjacent primary particles 20, 30, 40, and the thickness direction of the grain boundary is perpendicular to the surface of the adjacent primary particles 20, 30, 40. The average grain boundary length is, for example, about 50 nm to about 950 nm, about 100 nm to about 900 nm, about 150 nm to about 800 nm, or about 200 nm to about 700 nm. The average grain boundary thickness is about 2 nm to about 100 nm, about 5 nm to about 100 nm, about 10 nm to about 100 nm, or about 20 nm to about 100 nm. Within such ranges of average grain boundary length and average grain boundary thickness, a lithium battery including the composite positive electrode active material provides improved cycle characteristics and thermal stability. The average grain boundary length is the average value of the grain boundary length (d1) arranged in one direction. The average grain boundary thickness is the average value of the grain boundary thickness (d2) arranged in one direction.

[0059] In the composite positive electrode active material, the average particle size of the primary particles is, for example, about 50 nm to about 500 nm, about 50 nm to about 450 nm, about 50 nm to about 400 nm, about 50 nm to about 350 nm, about 50 nm to about 300 nm, about 50 nm to about 250 nm, or about 50 nm to about 200 nm, but is not necessarily limited to such ranges, and is adjusted within a range that provides improved cycle characteristics and thermal stability.

[0060] In the composite positive electrode active material, the average particle size of the core, which is a secondary particle formed by agglomeration of the primary particles, is, for example, about 1 μm to about 30 μm, about 2 μm to about 28 μm, about 4 μm to about 26 μm, about 6 μm to about 24 μm, about 8 μm to about 22 μm, about 10 μm to about 20 μm, about 12 μm to about 18 μm, about 12 μm to about 16 μm, or about 13 μm to about 15 μm, but is not necessarily limited to such ranges, and is adjusted within a range that provides improved cycle characteristics and thermal stability.

[0061] In the composite positive electrode active material, for example, the shell further comprises a third composition comprising a second metal. The third composition is disposed outside the grain boundaries in the core, in addition to the shell disposed on the surface of the core. The third composition contained in the shell has, for example, the same composition and the same crystal structure as the third composition disposed on the grain boundaries in the core. The third composition contained in the shell has, for example, a monoclinic crystal structure belonging to the C2 / m, C12 / c1 or C2 / c space group. The third composition contained in the shell has, for example, a composition represented by the above-mentioned chemical formula 3.

[0062] In the composite positive electrode active material, the first lithium transition metal oxide is doped with a second metal, and the structural stability of the first lithium transition metal oxide is improved by doping the first lithium transition metal oxide with the second metal.

[0063] In the composite positive electrode active material, the first lithium transition metal oxide may include lithium, nickel, a second metal, a third metal, and oxygen, where the third metal refers to a metal other than lithium, nickel, and the second metal.

[0064] In the composite active cathode material, the first lithium transition metal oxide may include about 0.1 to about 1.3 moles of lithium per mole of the first lithium transition metal oxide, about 0.7 to about 0.99 moles of nickel per mole of the first lithium transition metal oxide, about 0.001 to about 0.01 moles of a second metal per mole of the first lithium transition metal oxide, about 0.01 to about 0.3 moles of a third metal per mole of the first lithium transition metal oxide, and about 1.7 to about 2.3 moles of oxygen per mole of the first lithium transition metal oxide.

[0065] The first lithium transition metal oxide is represented, for example, by the following chemical formula 4:

[0066] [ka]

[0067] In the formula 4, 0.9≦a≦1.1 and 0≦α<2; M4 is nickel, a second metal, and a third metal, and the third metal is at least one element selected from the group consisting of Groups 2 to 13 excluding nickel and the second metal, and the nickel content in M4 is 70 mol% to less than 100 mol%, and X is an element selected from the group consisting of O, F, S, and P. The first lithium transition metal oxide represented by Formula 4 includes a doped second metal.

[0068] The first lithium transition metal oxide is represented, for example, by the following formula 5:

[0069] [ka]

[0070] In the above formula 5, 0.9≦a≦1.1, 0.7 <b<1.0、0<c<0.3、0<d<0.3、0≦e<0.1、b+c+d+e=1、0≦α<2であり、 M5, M6 and M7 are different from each other and are each one selected from the group consisting of cobalt (Co), manganese (Mn), zirconium (Zr), aluminum (Al), rhenium (Re), vanadium (V), chromium (Cr), iron (Fe), boron (B), ruthenium (Ru), titanium (Ti), niobium (Nb), molybdenum (Mo), magnesium (Mg) and platinum (Pt), and X is an element selected from the group consisting of O, F, S and P. The first lithium transition metal oxide represented by formula 5 includes a doped second metal.

[0071] The first lithium transition metal oxide is represented, for example, by the following formula 6 or 7:

[0072] [ka]

[0073] [ka]

[0074] In the chemical formulas 6 and 7, 0.9≦a≦1.1, 0.7 <b<1.0、0<c<0.1、0<d<0.1、0≦e<0.01、b+c+d+e=1、0≦α<2であり、

[0075] M8 is one selected from the group consisting of zirconium (Zr), aluminum (Al), vanadium (V), chromium (Cr), iron (Fe), rhenium (Re), boron (B), ruthenium (Ru), titanium (Ti), niobium (Nb), molybdenum (Mo), magnesium (Mg) and platinum (Pt), and X is an element selected from the group consisting of O, F, S and P. The first lithium transition metal oxide represented by formula 6 or 7 includes a doped second metal.

[0076] In the composite positive electrode active material, the first lithium transition metal oxide includes, for example, one or more of a first layered structure crystal phase belonging to a C2 / m space group and a second layered structure crystal phase belonging to an R-3m space group, and is also, for example, a composite of the first layered structure crystal phase and the second layered structure crystal phase.

[0077] The first lithium transition metal oxide has a composition represented by, for example, the following chemical formula 8a and includes a second layer-structure crystal phase belonging to the C2 / m space group, and a third layer-structure crystal phase having a composition represented by the following chemical formula 8b and belonging to the R-3m space group.

[0078] [ka]

[0079] [ka]

[0080] In the above chemical formulas 8a and 8b, M is two or more elements selected from nickel (Ni), cobalt (Co), manganese (Mn), vanadium (V), chromium (Cr), iron (Fe), zirconium (Zr), rhenium (Re), aluminum (Al), boron (B), ruthenium (Ru), titanium (Ti), niobium (Nb), molybdenum (Mo), magnesium (Mg) and platinum (Pt), and X is an element selected from the group consisting of O, F, S and P, and 0≦α<2. At least a part of M is Ni. In M, the Ni content is 70 mol% or more, 71 mol% to 99 mol%, 75 mol% to 98 mol%, 78 mol% to 90 mol%, 71 mol% to 99 mol%, 75 mol% to 98 mol%, or 78 mol% to 90 mol% based on the total transition metal content contained in the first lithium transition metal oxide. The second layered-structure crystalline phase represented by Formula 8b includes, for example, a doped second metal.

[0081] The first lithium transition metal oxide is represented, for example, by the following formula 8:

[0082] [ka]

[0083] In the above formula 8, 0 <a<1、0≦α<2であり、 M is two or more elements selected from nickel (Ni), cobalt (Co), manganese (Mn), zirconium (Zr), aluminum (Al), rhenium (Re), vanadium (V), chromium (Cr), iron (Fe), boron (B), ruthenium (Ru), titanium (Ti), niobium (Nb), molybdenum (Mo), magnesium (Mg) and platinum (Pt), and X is an element selected from the group consisting of O, F, S and P. At least a part of M is Ni. In M, the Ni content is 70 mol% or more, 71 mol% to 99 mol%, 75 mol% to 98 mol%, 78 mol% to 90 mol%, 71 mol% to 99 mol%, 75 mol% to 98 mol%, or 78 mol% to 90 mol% based on the total transition metal content contained in the first lithium transition metal oxide. The first lithium transition metal oxide represented by Formula 8 includes a doped second metal.

[0084] According to another embodiment, a positive electrode includes the composite positive electrode active material, which provides improved cycle characteristics and thermal stability.

[0085] The positive electrode can be produced, for example, by the following exemplary method, but is not necessarily limited to such a method, and can be adjusted according to required conditions.

[0086] First, the composite positive electrode active material, a conductive agent, a binder, and a solvent are mixed to prepare a positive electrode active material composition. The prepared positive electrode active material composition is directly coated on an aluminum current collector and dried to manufacture a positive electrode plate having a positive electrode active material layer. Alternatively, the positive electrode active material composition is cast on a separate support and then peeled off from the support to obtain a film, which is then laminated on the aluminum current collector to manufacture a positive electrode plate having a positive electrode active material layer.

[0087] Examples of the conductive agent include carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, ketjen black, carbon fibers, carbon nanotubes, metal powders, metal fibers or metal tubes such as copper, nickel, aluminum, and silver, and conductive polymers such as polyphenylene derivatives, but are not limited to these, and any conductive agent that is used as a conductive agent in the relevant technical field is acceptable.

[0088] The binder may be vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), a mixture of the above polymers, a styrene-butadiene rubber-based polymer, or the like, and the solvent may be N-methylpyrrolidone (NMP), acetone, water, or the like, but is not necessarily limited to these, and any solvent used in the relevant technical field may be used.

[0089] A plasticizer or pore-forming agent may be further added to the positive electrode active material composition to form pores within the electrode plate.

[0090] The contents of the composite positive electrode active material, conductive agent, binder, and solvent used in the positive electrode are at levels generally used in lithium batteries, and one or more of the conductive agent, binder, and solvent may be omitted depending on the application and configuration of the lithium battery.

[0091] In addition, the positive electrode may further include other common positive electrode active materials in addition to the composite positive electrode active material described above.

[0092] The common positive electrode active material may be any lithium-containing metal oxide that is generally used in the art, without any limitations. For example, one or more of composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof may be used. Specific examples of the composite oxides include Li a A 1-b B' bD 2 (wherein 0.90≦a≦1 and 0≦b≦0.5); Li a E 1-b B' b O 2-c D c (wherein, 0.90≦a≦1, 0≦b≦0.5, and 0≦c≦0.05); LiE 2-b B' b O 4-c D c (wherein, 0≦b≦0.5 and 0≦c≦0.05); Li a Ni 1-b-c Co b B' c D α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Co b B' c O 2-α F' α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Co b B' c O 2-α F' 2 (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B' c D α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Mn b B' c O 2-α F' α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B' c O 2-α F' 2 (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Lia Ni b E c G d O 2 (wherein, 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, and 0.001≦d≦0.1); Li a Ni b Co c Mn d G e O 2 (wherein, 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, and 0.001≦e≦0.1); Li a NiG b O 2 (wherein, 0.90≦a≦1, 0.001≦b≦0.1); Li a CoG b O 2 (wherein, 0.90≦a≦1, 0.001≦b≦0.1); Li a MnG b O 2 (wherein, 0.90≦a≦1, 0.001≦b≦0.1); Li a Mn 2 G b O 4 (wherein, 0.90≦a≦1 and 0.001≦b≦0.1); QO 2 ;QS 2 ;LiQS 2 ;V 2 O 5 ;LiV 2 O 5 ;LiI'O 2 ;LiNiVO 4 Li 3-f J 2 (PO 4 ) 3 (0≦f≦2);Li 3-f Fe 2 (PO 4 ) 3 (0≦f≦2); LiFePO 4 A compound represented by any one of the following chemical formulas can be used.

[0093] In the chemical formula representing the aforementioned compound, A is Ni, Co, Mn, or a combination thereof; B' is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F' is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I' is Cr, V, Fe, Sc, Y, or a combination thereof; and J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof.

[0094] It is also possible to use a compound in which a coating layer is added to the surface of the above-mentioned compound, and it is also possible to use a mixture of the above-mentioned compound and a compound to which a coating layer is added. The coating layer added to the surface of the above-mentioned compound includes, for example, a coating element compound such as an oxide / hydroxide of the coating element, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element. The compound forming such a coating layer is amorphous or crystalline. The coating element contained in the coating layer is Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method of forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method is, for example, a spray coating method, a dipping method, etc. A specific coating method is a content that is widely understood by those skilled in the art in this field, so a detailed description is omitted.

[0095] The positive electrode includes, for example, the above-mentioned composite positive electrode active material and olivine-based positive electrode active material.

[0096] The olivine-based positive electrode active material is represented, for example, by the following chemical formula 9.

[0097] [ka]

[0098] In the above Chemical Formula 9, 0.90≦x≦1.1, 0≦y≦0.9, 0≦z≦0.5, 1-yz≧0, 0≦α≦2, M8 is one or more metals selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Al, Mg, Zr, and B, M9 is at least one element selected from the group consisting of Mg, Ca, Sr, Ba, Ti, Zr, Nb, Mo, W, Zn, Al, Si, Ni, Mn, Cr, Fe, Mg, Sr, V, or rare earth elements, and X is an element selected from the group consisting of O, F, S, and P.

[0099] The olivine-based positive electrode active material is, for example, LiFePO 4 , LiNiPO 4 , LiMnPO 4 , LiCoPO 4 And so on.

[0100] The content of the olivine-based positive electrode active material contained in the positive electrode is, for example, 10 wt% or less, 9 wt% or less, 8 wt% or less, 7 wt% or less, 6 wt% or less, or 5 wt% or less of the total weight of the positive electrode active material. The content of the olivine-based positive electrode active material contained in the positive electrode is, for example, 1 to 10 wt%, 1 to 9 wt%, 1 to 8 wt%, 1 to 7 wt%, 1 to 6 wt%, or 1 to 5 wt% of the total weight of the positive electrode active material. The content of the olivine-based positive electrode active material contained in the positive electrode is, for example, 1 to 10 parts by weight, 1 to 9 parts by weight, 1 to 8 parts by weight, 1 to 7 parts by weight, 1 to 6 parts by weight, or 1 to 10 parts by weight, relative to 100 parts by weight of the composite positive electrode active material. When the positive electrode further contains an olivine-based positive electrode active material in such a content range, the cycle characteristics and mixture density of the lithium battery are further improved.

[0101] According to still another embodiment, a lithium battery employs a positive electrode including the composite positive electrode active material described above.

[0102] The lithium battery employs a positive electrode containing the aforementioned composite positive electrode active material, thereby providing improved cycleability and thermal stability.

[0103] The lithium battery is manufactured, for example, by the following exemplary method, but is not necessarily limited to such a method, and may be adjusted according to required conditions.

[0104] First, the positive electrode is produced by the above-mentioned positive electrode production method.

[0105] Next, the negative electrode is prepared as follows. The negative electrode is prepared in substantially the same manner as the positive electrode, except that, for example, a negative electrode active material is used instead of the composite positive electrode active material. In addition, the conductive agent, binder, and solvent in the negative electrode active material composition may be substantially the same as those in the positive electrode.

[0106] For example, the negative active material, a conductive agent, a binder, and a solvent are mixed to prepare a negative active material composition, which is then directly coated onto a copper current collector to prepare a negative electrode plate. Alternatively, the negative active material composition prepared is cast onto a separate support, and the negative active material film peeled off from the support is laminated onto a copper current collector to prepare a negative electrode plate.

[0107] The negative electrode active material may be any material known in the art that is used as a negative electrode active material for lithium batteries, including at least one selected from the group consisting of lithium metal, metals that can be alloyed with lithium, transition metal oxides, non-transition metal oxides, and carbonaceous materials.

[0108] Examples of metals that can be alloyed with lithium include Si, Sn, Al, Ge, Pb, Bi, SbSi-Y alloys (wherein Y is an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, or a combination thereof, and is not Si), and Sn-Y alloys (wherein Y is an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, or a combination thereof, and is not Sn). The element Y is, for example, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, or a combination thereof.

[0109] The transition metal oxide is, for example, lithium titanium oxide, vanadium oxide, lithium vanadium oxide, or the like.

[0110] The non-transition metal oxide is, for example, SnO 2 , SiO x (0 <x<2)などである。

[0111] The carbon-based material may be, for example, crystalline carbon, amorphous carbon, or a mixture thereof. The crystalline carbon may be, for example, graphite, such as amorphous, plate-like, flake-like, spherical, or fibrous natural or artificial graphite. The amorphous carbon may be, for example, soft carbon (low-temperature sintered carbon), hard carbon, mesophase pitch carbide, calcined coke, etc.

[0112] The contents of the negative electrode active material, conductive agent, binder, and solvent are at levels generally used in lithium batteries, and one or more of the conductive agent, binder, and solvent may be omitted depending on the application and configuration of the lithium battery.

[0113] Next, a separator to be inserted between the positive electrode and the negative electrode is prepared.

[0114] The separator may be any separator that is generally used in lithium batteries. For example, the separator may have low resistance to ion migration of the electrolyte and excellent electrolyte moisture-absorbing ability. The separator may be selected from glass fiber, polyester, Teflon (registered trademark), polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or a combination thereof, and may be in the form of a nonwoven or woven fabric. For example, a rollable separator such as polyethylene or polypropylene is used for the lithium ion battery, and a separator with excellent organic electrolyte impregnation ability is used for the lithium ion polymer battery.

[0115] The separator is manufactured by the following exemplary method, but is not necessarily limited to such method, and may be adjusted according to required conditions.

[0116] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated on the electrode and dried to form a separator. Alternatively, the separator composition is cast on a support and dried, and the separator film is peeled off from the support and laminated on the electrode to form a separator.

[0117] The polymer used to manufacture the separator is not particularly limited, and any polymer that is used as a binder for electrode plates can be used, such as vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or a mixture thereof.

[0118] Next, the electrolyte is prepared.

[0119] The electrolyte is, for example, an organic electrolyte solution, which is produced, for example, by dissolving a lithium salt in an organic solvent.

[0120] The organic solvent can be any organic solvent that is used as an organic solvent in the technical field.The organic solvent can be, for example, propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methylethyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, methylisopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethylsulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.

[0121] The lithium salt may be any lithium salt used in the art. For example, LiPF 6 , LiBF 4 , LiSbF 6 , LiAsF 6 , LiClO 4 , LiCF 3 SO 3 , Li(CF 3 SO 2 ) 2 N, LiC 4 F 9 SO 3 , LiAlO 2 , LiAlCl 4 , LiN(C x F 2x+1 SO 2 )(C y F 2y+1 SO 2 ) (where x and y are natural numbers), LiCl, LiI, or a mixture thereof.

[0122] Alternatively, the electrolyte is a solid electrolyte, such as, but not limited to, boron oxide, lithium oxynitride, etc., and may be any solid electrolyte used in the art. The solid electrolyte is formed on the negative electrode, for example, by a method such as sputtering, or a separate solid electrolyte sheet is laminated on the negative electrode.

[0123] As can be seen from Fig. 6, the lithium battery 1 includes a positive electrode 3, a negative electrode 2, and a separator 4. The positive electrode 3, the negative electrode 2, and the separator 4 are wound or folded and housed in a battery case 5. An organic electrolyte is injected into the battery case 5, and the battery case 5 is sealed with a cap assembly 6 to complete the lithium battery 1. The battery case 5 is cylindrical, but is not necessarily limited to such a shape, and may be, for example, a square shape, a thin film type, etc.

[0124] A pouch-type lithium battery includes one or more battery structures. A separator is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are stacked in a bi-cell structure, impregnated with an organic electrolyte, and housed and sealed in a pouch to complete a pouch-type lithium battery. A plurality of such battery structures are stacked to form a battery pack, which is used in all devices that require high capacity and high output. For example, it is used in notebook computers, smartphones, electric vehicles (EVs), etc.

[0125] The lithium battery has excellent life characteristics and high rate characteristics, and is therefore used, for example, in electric vehicles (EVs), hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs), and fields requiring large amounts of power storage, such as electric bicycles and power tools.

[0126] According to yet another embodiment, a method for preparing a composite positive electrode active material includes the steps of preparing a first composition of the first lithium transition metal oxide by mixing the first composition of the first lithium transition metal oxide with a first metal precursor, preparing a second composition of the first lithium transition metal oxide by mixing the first composition of the first lithium transition metal oxide with a phosphorus (P) precursor, and drying the second composition of the first lithium transition metal oxide and heat-treating it in an oxidizing atmosphere at 400° C. to 1,000° C. to prepare a composite positive electrode active material.

[0127] The step of preparing the first composition and the second composition is performed, for example, by a wet method using a solvent. The first composition and the second composition include a solvent capable of dissolving the first metal precursor and the phosphorus (P) precursor, and the type of the solvent is not particularly limited, and any solvent that can be used as a solvent in the art is possible. The solvent is, for example, distilled water.

[0128] The first metal precursor may be, but is not limited to, a nitrate, oxychloride, or oxynitrate of the first metal, and may be any dissociable salt containing the first metal and used in the art. For example, the first metal precursor may be Co(NO 3 ) 2 6H 2 O, Mg(NO 3 ) 2 6H 2 In the first composition, a hydroxide of a first metal is precipitated on the surface of the first lithium metal oxide. The hydroxide of the first metal is, for example, Co(OH) 2 , Mg(OH) 2 And so on.

[0129] The phosphorus (P) precursor may be any dissociable salt containing phosphorus (P) and used in the art, such as, but not limited to, a metal or ammonium phosphate. For example, the phosphorus (P) precursor may be (NH 4 ) 2 HPO 4 , (NH 4 ) 3 PO 4 In the second composition, a precursor of the second composition is precipitated on the surface of the first lithium metal oxide.

[0130] An oxidizing atmosphere is an atmosphere that contains oxygen or air. The oxidizing atmosphere may contain oxygen, air, or a combination thereof, for example, air with an increased oxygen content.

[0131] In the first composition, the content of the first metal precursor is 30 parts by weight or less, 20 parts by weight or less, or 10 parts by weight or less, based on 100 parts by weight of the first lithium transition metal oxide. In the first composition, the content of the solvent is 300 parts by weight or less, 200 parts by weight or less, or 100 parts by weight or less, based on 100 parts by weight of the first lithium transition metal oxide. In the second composition, the content of the phosphorus (P) precursor is 30 parts by weight or less, 20 parts by weight or less, or 10 parts by weight or less, based on 100 parts by weight of the first lithium transition metal oxide. In the second composition, the content of the solvent is 300 parts by weight or less, 200 parts by weight or less, or 100 parts by weight or less, based on 100 parts by weight of the first lithium transition metal oxide.

[0132] The heat treatment is carried out at, for example, 400 to 1,000°C, 500 to 900°C, 600 to 800°C, or 700 to 750°C. The heat treatment time is, for example, 3 to 20 hours, 3 to 15 hours, 3 to 10 hours, 3 to 7 hours, or 4 to 6 hours. The temperature rise rate to reach the temperature at which the heat treatment is carried out is, for example, 1 to 10°C / min. When the heat treatment temperature, heat treatment time, and temperature rise rate are within the above-mentioned ranges, a shell is formed on the core, including a first layer and a second layer disposed on the first layer.

[0133] In the method for manufacturing a composite positive electrode active material, the step of preparing a first lithium transition metal oxide includes the steps of mixing a precursor of the first lithium transition metal oxide with a second metal precursor to prepare a mixture, and heat-treating the mixture in an oxidizing atmosphere at 400°C to 1,000°C to manufacture the first lithium transition metal oxide.

[0134] The step of preparing the mixture is, for example, performed in a dry manner without a solvent. The mixture is, for example, a dry powder obtained by mixing a precursor powder of the first lithium transition metal oxide and a precursor powder of the second metal. Alternatively, the step of preparing the mixture is, for example, performed in a wet manner including a solvent. The mixture includes a solvent capable of dissolving the precursor of the first lithium transition metal oxide and the precursor of the second metal, and the type of the solvent is not particularly limited, and any solvent that can be used as a solvent in the art is possible. The solvent is, for example, distilled water. By using the wet method, the third composition including the second metal can be formed at a higher concentration at the grain boundaries between the primary particles.

[0135] The oxidizing atmosphere is an atmosphere that contains oxygen or air. The oxidizing atmosphere contains oxygen, air, or a combination thereof, for example, air with an increased oxygen content.

[0136] The second metal precursor may be, but is not limited to, an oxide or hydroxide of the second metal, and may be any material that can be used in the art as a material containing the second metal. For example, the second metal precursor may be, for example, ZrO 2 , Al 2 O 3 And so on.

[0137] In the mixture, the content of the second metal precursor is 30 parts by weight or less, 20 parts by weight or less, or 10 parts by weight or less, based on 100 parts by weight of the first lithium transition metal oxide precursor.

[0138] The heat treatment is carried out at, for example, 400 to 1,000°C, 500 to 900°C, 600 to 800°C, or 700 to 750°C. The heat treatment time is, for example, 3 to 20 hours, 3 to 15 hours, 3 to 10 hours, 3 to 7 hours, or 4 to 6 hours. The temperature rise rate to reach the temperature at which the heat treatment is carried out is, for example, 1 to 10°C / min. When the heat treatment temperature, heat treatment time, and temperature rise rate are within the above-mentioned ranges, a third composition including the second metal is formed at the grain boundaries between the primary particles, and the first lithium transition metal oxide is doped with the second metal.

[0139] The present invention will be described in more detail with reference to the following examples and comparative examples. However, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.

[0140] (Production of composite positive electrode active material) Example 1: Ni 88 +Al-Zr doping, Li 2 ZrO 3 Grain boundary coating + Co / Mg:P=0.25wt%:0.25wt%, two-layer coating layer

[0141] (Core manufacturing stage) The second metal precursor, zirconium oxide (ZrO 2 ) and alumina (Al 2 O 3 ), the first lithium transition metal oxide precursor, Ni 0.88 Co 0.08 Mn 0.04 (OH) 2 , and the lithium precursor LiOH H 2 A mixture was prepared by mixing Ni and O in a molar ratio that would give a core with the following composition: 0.88 Co 0.08 Mn 0.04 (OH) 2 , and the lithium precursor LiOH H 2 The mixture was placed in a furnace and subjected to a primary heat treatment at 720° C. for 5 hours while flowing oxygen to produce a core.

[0142] The first heat treatment process produces the first lithium transition metal oxide, Al and Zr doped Li(Ni 0.88 Co 0.08 Mn 0.04 ) 1-x-y Al x Zr y O 2 (x=0.001, y=0.0025) core was obtained.

[0143] In addition, the surface of the core and the grain boundaries between the primary particles of the core contain Li having a monoclinic crystal structure. 2 ZrO 3 A coating layer was formed.

[0144] (Shell manufacturing stage) In the first layer of the composite positive electrode active material, the content of Co and Mg was 0.25 parts by weight per 100 parts by weight of the first lithium transition metal oxide. 3 ) 2 6H 2 O and Mg(NO 3 ) 2 6H 2 A precursor was prepared by mixing O and ZnO in a molar ratio of 3:2, and then the precursor was added to 10 parts by weight of distilled water and stirred at room temperature (25° C.) for 1 minute to prepare a first aqueous solution.

[0145] In the second layer of the composite positive electrode active material, the content of P is 0.25 parts by weight based on 100 parts by weight of the first lithium transition metal oxide. 4 H 2 PO 4 After preparing the above, the above was added to 10 parts by weight of distilled water and stirred at room temperature (25° C.) for 1 minute to prepare a second aqueous solution.

[0146] Li(Ni) 0.88 Co 0.08 Mn 0.04 ) 1-x-y Al x Zr y O 2(x=0.001, y=0.0025) 100 parts by weight of the core powder was added to 90 parts by weight of distilled water to prepare a third aqueous solution. While stirring at room temperature for 10 minutes, the first aqueous solution was added, and then the second aqueous solution was added sequentially to prepare a mixture.

[0147] The mixture was dried in an oven at 150° C. for 15 hours to prepare a dried product.

[0148] The dried material was placed in a furnace and heat-treated at 720° C. for 5 hours while flowing oxygen, to produce a composite positive electrode active material.

[0149] Li(Ni) 0.88 Co 0.08 Mn 0.04 ) 1-x-y Al x Zr y O 2 (x=0.001, y=0.0025) On the surface of the core, Co 3 O 4 and a first layer including MgO, and Li x CoPO 4 (0 <x<2)、Li 3 PO 4 and Co 3 (PO 4 ) 2 A second layer was formed containing

[0150] In the first layer, the Co and Mg contents were 0.25 parts by weight based on 100 parts by weight of the first lithium transition metal oxide, and in the second layer, the P content was 0.25 parts by weight based on 100 parts by weight of the first lithium transition metal oxide.

[0151] Example 2: Ni88+Al-Zr doping, Li 2 ZrO 3 Grain boundary coating + Co / Mg:P=0.50wt%:0.25wt%, two-layer coating layer In the first layer of the composite positive electrode active material, the content of Co and Mg was 0.5 parts by weight per 100 parts by weight of the first lithium transition metal oxide. 3 ) 2 6H 2 O and Mg(NO 3) 2 6H 2 A composite positive electrode active material was prepared in the same manner as in Example 1, except that the content of the precursor mixed with O in a molar ratio of 3:2 was changed.

[0152] In the first layer, the Co and Mg contents were 0.5 parts by weight based on 100 parts by weight of the first lithium transition metal oxide, and in the second layer, the P content was 0.25 parts by weight based on 100 parts by weight of the first lithium transition metal oxide.

[0153] Example 3: Ni88+Al-Zr doping, Li 2 ZrO 3 Grain boundary coating + Co / Mg:P=0.75wt%:0.25wt%, two-layer coating layer In the first layer of the composite positive electrode active material, the content of Co and Mg was 0.75 parts by weight per 100 parts by weight of the first lithium transition metal oxide. 3 ) 2 6H 2 O and Mg(NO 3 ) 2 6H 2 A composite positive electrode active material was prepared in the same manner as in Example 1, except that the content of the precursor mixed with O in a molar ratio of 3:2 was changed.

[0154] In the first layer, the Co and Mg contents were 0.75 parts by weight based on 100 parts by weight of the first lithium transition metal oxide, and in the second layer, the P content was 0.25 parts by weight based on 100 parts by weight of the first lithium transition metal oxide.

[0155] Example 4: Ni88+Al doping (Zr not added)+Co / Mg:P=0.25wt%:0.25wt%, two-layer coating layer In the core manufacturing stage, alumina (Al 2 O 3 ) and zirconium oxide (ZrO 2 The preparation was carried out in the same manner as in Example 1, except that no ethyl acetate was used.

[0156] The first heat treatment produced Al-doped Li(Ni 0.88 Co 0.08 Mn 0.04 )1-x Al x O 2 (x=0.001) core was obtained.

[0157] In the first layer, the Co and Mg contents were 0.25 parts by weight based on 100 parts by weight of the first lithium transition metal oxide, and in the second layer, the P content was 0.25 parts by weight based on 100 parts by weight of the first lithium transition metal oxide.

[0158] Comparative Example 1: Ni88 core Li(Ni 0.88 Co 0.08 Mn 0.04 ) 1-x-y Al x Zr y O 2 (x=0.001, y=0.0025) The core powder was used as is.

[0159] Comparative Example 2: Ni88 core + water wash Li(Ni 0.88 Co 0.08 Mn 0.04 ) 1-x-y Al x Zr y O 2 (x=0.001, y=0.0025) 100 parts by weight of the core powder was added to 90 parts by weight of distilled water and stirred, and then the precipitate was filtered and separated, and a water washing step was performed once to remove residual lithium.

[0160] The separated precipitate was dried in an oven at 150° C. for 15 hours to prepare a dried product.

[0161] The dried material was placed in a furnace and heat-treated at 720° C. for 5 hours while flowing oxygen, to produce a composite positive electrode active material.

[0162] Comparative Example 3: Ni88+Al-Zr doping, Li 2 ZrO 3 Grain boundary coating + Co / Mg:P=0.75wt%:0.0wt%, 1-layer coating layer In the shell preparation step, the first layer of the composite positive electrode active material was prepared by mixing Co(NO 3 ) 2 6H 2 O and Mg(NO 3 ) 2 6H 2 The content of the precursor was changed to 3:2 molar ratio of NH:O. 4 H 2 PO 4 A composite positive electrode active material was prepared in the same manner as in Example 1, except that the second aqueous solution containing

[0163] Li(Ni) 0.88 Co 0.08 Mn 0.04 ) 1-x-y Al x Zr y O 2 (x=0.001, y=0.0025) On the surface of the core, Co 3 O 4 A first layer containing ZnO and MgO was formed. A second layer was not formed.

[0164] In the first layer, the content of Co and Mg was 0.75 parts by weight based on 100 parts by weight of the first lithium transition metal oxide.

[0165] Comparative Example 4: Ni88+Al-Zr doping, Li2ZrO3 grain boundary coating+Co / Mg:P=0.25wt%:0.25wt%, one-layer structure composite coating layer A composite positive electrode active material was prepared in the same manner as in Example 1, except that in the shell preparation step, the first and second aqueous solutions were simultaneously added to the third aqueous solution.

[0166] Li(Ni) 0.88 Co 0.08 Mn 0.04 ) 1-x-y Al x Zr y O 2 (x=0.001, y=0.0025) A composite layer containing Co, Mg and P was formed on the surface of the core.

[0167] In the first layer, the contents of Co and Mg were 0.25 parts by weight based on 100 parts by weight of the first lithium transition metal oxide, and the content of P was 0.25 parts by weight based on 100 parts by weight of the first lithium transition metal oxide.

[0168] Reference Example 1: Ni88+Al-Zr doping, Li 2 ZrO 3 Grain boundary coating + Co / Mg:P=0.25wt%:0.0wt%, 1st layer coating composition During the shell manufacturing stage, NH 4 H 2 PO 4 A composite positive electrode active material was prepared in the same manner as in Example 1, except that the second aqueous solution containing

[0169] Li(Ni) 0.88 Co 0.08 Mn 0.04 ) 1-x-y Al x Zr y O 2 (x=0.001, y=0.0025) On the surface of the core, Co 3 O 4 A first layer containing ZnO and MgO was formed. A second layer was not formed.

[0170] In the first layer, the content of Co and Mg was 0.25 parts by weight based on 100 parts by weight of the first lithium transition metal oxide. For comparison with Example 1, this is the same as the composite positive electrode active material of Example 1 except that the second layer is omitted.

[0171] (Lithium battery (half cell) manufacturing)

[0172] Example 5 (Production of positive electrodes) The composite positive electrode active material prepared in Example 1, a carbon conductive agent (Denka Black), and polyvinylidene fluoride (PVdF) were mixed in a weight ratio of 92:4:4, and the mixture was mixed with N-methylpyrrolidone (NMP) in an agate mortar to prepare a slurry. The slurry was bar-coated on an aluminum collector having a thickness of 15 μm, dried at room temperature, and then dried again under vacuum at 120° C., followed by roll pressing and punching to prepare a positive electrode plate having a thickness of 55 μm.

[0173] (Coin cell manufacturing) Using the positive electrode plate manufactured above, lithium metal was used as the counter electrode, and a PTFE separator and 1.15M LiPF 6 However, a coin cell was fabricated using an electrolyte, which was a solution of ethylene carbonate (EC) + ethyl methyl carbonate (EMC) + dimethyl carbonate (DMC) (volume ratio 3:4:3).

[0174] Examples 6 to 8 A coin cell was prepared in the same manner as in Example 5, except that the composite positive electrode active material prepared in Examples 2 to 4 was used instead of the composite positive electrode active material prepared in Example 1.

[0175] Example 9: LFP addition 100 parts by weight of the composite positive electrode active material prepared in Example 1 was mixed with LiFePO 4 A coin cell was manufactured in the same manner as in Example 5, except that 5 parts by weight were added.

[0176] Comparative Examples 5 to 8 Coin cells were prepared in the same manner as in Example 5, except that the composite positive electrode active materials prepared in Comparative Examples 1 to 4 were used instead of the composite positive electrode active material prepared in Example 1.

[0177] (Manufacture of lithium batteries (full cell))

[0178] Example 10 (Production of positive electrodes) The composite positive active material prepared in Example 1, a carbon conductive agent (Denka Black), and polyvinylidene fluoride (PVdF) were mixed in a weight ratio of 92:4:4, and the mixture was mixed with N-methylpyrrolidone (NMP) in an agate mortar to prepare a positive active material slurry. The slurry was bar-coated on an aluminum collector having a thickness of 15 μm, dried at room temperature, and then dried again under vacuum at 120° C., followed by rolling and punching to prepare a positive plate having a thickness of 55 μm.

[0179] (Production of negative electrodes) Graphite particles with an average particle size of 25 μm, styrene-butadiene rubber (SBR) binder (ZEON), and carboxymethyl cellulose (CMC, NIPPON A&L) were mixed in a weight ratio of 97:1.5:1.5, then added to distilled water and stirred for 60 minutes using a mechanical stirrer to prepare a negative electrode active material slurry. The slurry was applied to a 10 μm thick copper current collector using a doctor blade, dried in a hot air dryer at 100°C for 0.5 hours, and then dried again in a vacuum at 120°C for 4 hours, followed by rolling and punching to prepare a 65 μm thick negative electrode plate.

[0180] (Coin cell manufacturing) The positive and negative electrodes prepared above were used, and a PTFE separator and 1.15M LiPF 6 However, a coin cell was fabricated using an electrolyte, which was a solution of ethylene carbonate (EC) + ethyl methyl carbonate (EMC) + dimethyl carbonate (DMC) (volume ratio 3:4:3).

[0181] Examples 11 to 13 A coin cell was prepared in the same manner as in Example 10, except that the composite positive electrode active material prepared in Examples 2 to 4 was used instead of the composite positive electrode active material prepared in Example 1.

[0182] Example 14: LFP addition 100 parts by weight of the composite positive electrode active material prepared in Example 1 was mixed with LiFePO 4 A coin cell was prepared in the same manner as in Example 10, except that 5 parts by weight was added.

[0183] Comparative Examples 9 to 12 Coin cells were prepared in the same manner as in Example 10, except that the composite positive electrode active materials prepared in Comparative Examples 1 to 4 were used instead of the composite positive electrode active material prepared in Example 1.

[0184] Evaluation example 1: XRD (X-ray diffraction) spectrum evaluation The XRD spectra of the composite positive electrode active materials of Reference Example 1 and Example 1 were measured, and the results are shown in Figures 2A and 2B, respectively. Cu Kα radiation was used for the XRD spectrum measurement.

[0185] As can be seen from Fig. 2A, the XRD spectrum of the composite cathode active material of Reference Example 1 in which only the first layer was formed as the coating layer showed only peaks associated with a phase having a layered crystal structure belonging to the R-3m space group. Therefore, it was confirmed that the composition contained in the first layer has a first phase having a layered crystal structure belonging to the R-3m space group.

[0186] 2B, the XRD spectrum of the composite cathode active material of Example 1 in which a second layer was added to a first layer as a coating layer showed additional peaks at diffraction angles (2θ) of 20° to 35° in addition to the peaks associated with the layered crystal structure, confirming that a second phase structurally distinct from the phase contained in the first layer was additionally formed.

[0187] Through Reitveld analysis, the first layer is Co 3 O 4 phase and MgO phase, and the second layer is Li 3PO 4 Phase, Li a Co b (PO 4 ) c (0.5 < a < 1.5, 0.9 < b < 1.5, 0.9 < c < 1.5) Phase and Co 3 (PO 4 ) 2 It was confirmed to contain the phase.

[0188] Evaluation example 2: Composition evaluation inside the core and on the surface Figures 3A to 3C are HAADF (high-angle annular dark field) STEM and EDS (energy dispersive X-ray spectrometry) images of the cross-section of a composite positive electrode active material including a secondary particle core in which a plurality of primary particles prepared in Reference Example 1 are aggregated, and a first layer disposed on the core.

[0189] Figures 4A to 4D are HAADF (high-angle annular dark field) STEM and EDS (energy dispersive X-ray spectrometry) images of the cross-section of a composite positive electrode active material including a secondary particle core in which a plurality of primary particles prepared in Example 1 are aggregated, and a first layer and a second layer disposed on the core.

[0190] As can be seen from Figures 3A to 3C, it was confirmed that a first layer containing Co and Mg was formed on the core.

[0191] Also, in Figures 3B to 3C, it was confirmed that the concentration of Co and / or Mg contained in the first layer is higher than the concentration of Co and / or Mg contained in the primary particles. In Figures 3B to 3C, the higher the concentration of the metal, the higher the brightness of the color corresponding to the metal. That is, it was confirmed that a coating layer containing a high concentration of Co and Mg was formed on the primary particles contained in the core.

[0192] 4A to 4D, it was confirmed that a second layer containing Co and P was formed on the first layer. Although not shown in the drawings, it was confirmed that the second layer contained a mixed phase containing Li, Co, P, and O.

[0193] 4A and 4B, the thickness of the second layer was greater than that of the first layer, and the thickness of the first layer was about 20 nm, and the thickness of the second layer was about 100 nm.

[0194] Although not shown in the drawing, additional high-resolution analysis confirmed that a separate phase containing Zr exists at the grain boundaries between the primary particles of the core and on the core surface. The separate phase is Li 2 ZrO 3 It was a phase.

[0195] Evaluation example 3: Residual lithium content evaluation The surface residual lithium contents of the composite positive electrode active materials prepared in Comparative Examples 1 to 3 and Example 1 were measured, and some of the results are shown in Table 1 below.

[0196] The surface residual lithium content is the Li remaining on the surface of the composite positive electrode active material. 2 CO 3 The Li content in LiOH was evaluated by measuring it using a wet method (or a titration method).

[0197] For a specific measurement method, for example, the method disclosed in paragraph

[0054] of Japanese Patent Application Publication No. 2016-081903 can be referred to.

[0198] [Table 1]

[0199] As can be seen from Table 1, the composite positive electrode active material of Example 1 exhibits a reduced amount of residual lithium on the surface compared to the composite positive electrode active materials of Comparative Examples 1 to 3.

[0200] It is believed that this is because the residual lithium on the surface of the first lithium transition metal oxide reacted sequentially with the precursor of the first composition and the precursor of the second composition to form a multi-layer coating layer on the core.

[0201] Therefore, the lithium battery including the second composite positive electrode active material of Example 1 suppresses gas generation during charging and discharging and suppresses side reactions with the electrolyte, thereby improving the life characteristics, compared to the lithium batteries including the composite positive electrode active materials of Comparative Examples 1 to 3.

[0202] Evaluation example 4: DSC measurement of composite positive electrode active material Differential scanning calorimetry (DSC) thermograms were measured at temperatures from 30° C. to 350° C. for the composite positive electrode active materials prepared in Example 1 and Comparative Example 3, and the results are shown in Table 2 and FIG.

[0203] [Table 2]

[0204] As can be seen from Table 2, the composite positive electrode active material of Example 1 having a multi-layer coating layer had a lower heat generation amount than the composite positive electrode active material of Comparative Example 3 having a single-layer coating layer.

[0205] In addition, as can be seen from FIG. 5, the onset temperature at which thermal decomposition begins for the composite positive electrode active material of Example 1 was shifted to a higher temperature compared to the composite positive electrode active material of Comparative Example 3.

[0206] Therefore, it was confirmed that the composite positive electrode active material of Example 1 had improved thermal stability compared to the composite positive electrode active material of Comparative Example 3.

[0207] Evaluation example 5: Room temperature charge / discharge characteristic evaluation The lithium batteries prepared in Examples 5 to 8 and Comparative Examples 5 to 8 were charged at a constant current of 0.1 C rate at 25° C. until the voltage reached 4.35 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.35 V in constant voltage mode. Next, the batteries were discharged at a constant current of 0.1 C rate until the voltage reached 2.8 V (vs. Li) (initial cycle, formation cycle).

[0208] The lithium battery after the first cycle was charged at a constant current of 1.0 C rate at 25°C until the voltage reached 4.35 V (vs. Li), then the current was cut off at a rate of 0.05 C while maintaining 4.35 V in constant voltage mode, and then discharged at a constant current of 0.2 C rate until the voltage reached 2.8 V (vs. Li) (second cycle).

[0209] The lithium battery after the second cycle was charged at a constant current of 1C rate at 25°C until the voltage reached 4.35V (vs. Li), and then cut off the current at a rate of 0.05C while maintaining 4.35V in constant voltage mode. Next, the battery was discharged at a constant current of 1C rate until the voltage reached 2.8V (vs. Li) (third cycle), and such cycles were repeated under the same conditions until the 52nd cycle (50 times).

[0210] In all charge / discharge cycles, a 10-minute rest period was allowed after each charge / discharge cycle.

[0211] Some of the results of the charge / discharge experiment are shown in Table 3. The capacity retention rate at the 52nd cycle is defined by the following formula 1.

[0212]

number

[0213] [Table 3]

[0214] As can be seen from Table 3, the lithium batteries of Examples 5 and 6 had improved life characteristics compared to the lithium batteries of Comparative Examples 6 to 8 without a substantial decrease in capacity.

[0215] Such improved life characteristics are believed to be due to the fact that the surface of the composite positive electrode active material contained in the lithium batteries of Examples 5 and 6 is further stabilized by the two-layer coating, thereby suppressing side reactions with the electrolyte.

[0216] In addition, it is believed that the composite positive electrode active material contained in the lithium batteries of Examples 5 and 6 additionally contains a second layer compared to the composite positive electrode active material contained in the lithium battery of Comparative Example 7, and that the second layer more effectively suppresses side reactions with the electrolyte.

[0217] For example, the lithium batteries of Examples 5 and 6 include a second layer disposed on the surface of the composite positive electrode material, which is Li 3 PO 4 etc., the second layer has improved wettability with respect to the electrolyte, and during initial charge / discharge, the second layer reacts with moisture and HF in the electrolyte to form a stable solid electrolyte film, thereby suppressing additional side reactions with the electrolyte, and stabilizing the surface of the composite positive electrode active material.

[0218] In addition, the composite positive electrode active material contained in the lithium batteries of Examples 5 and 6 had a multilayer structure including a first layer and a second layer, and thus had improved life characteristics compared to a composite single-layer structure including the same components as the composite positive electrode active material contained in the lithium battery of Comparative Example 8. In addition, although not disclosed in Table 3, the life characteristics of the lithium battery of Example 8 were also improved compared to the lithium battery of Comparative Example 8.

[0219] The lithium battery of Example 5 has a further improved life characteristic compared to the lithium battery of Example 8. Such improved life characteristic is due to the fact that the lithium battery of Example 5 contains the composite positive electrode active material, Li 2 ZrO 3This is believed to be because the second phase is arranged not only on the core surface but also on the grain boundaries between the primary particles inside the core, coating the primary particles, thereby suppressing side reactions between the primary particles arranged inside the core and the electrolyte, and the elution of transition metals from the primary particles, and ensuring a three-dimensional transmission path for lithium ions by the second phase on the core surface and inside the core.

[0220] Evaluation example 6: High temperature charge / discharge characteristic evaluation The lithium batteries prepared in Examples 10 to 13 and Comparative Examples 9 to 12 were charged at a constant current of 0.1 C rate at 45° C. until the voltage reached 4.30 V (vs. Gr), and then cut off at a current of 0.05 C rate while maintaining 4.30 V in constant voltage mode. Next, the batteries were discharged at a constant current of 0.1 C rate until the voltage reached 2.8 V (vs. Gr) (initial cycle, chemical cycle). Gr is graphite.

[0221] The lithium battery after the first cycle was charged at a constant current of 1.0 C rate at 45°C until the voltage reached 4.30 V (vs. Gr), then the current was cut off at a rate of 0.05 C while maintaining 4.30 V in constant voltage mode, and then discharged at a constant current of 0.2 C rate until the voltage reached 2.8 V (vs. Gr) (second cycle).

[0222] The lithium battery after the second cycle was charged at a constant current of 1C rate at 45°C until the voltage reached 4.30V (vs. Gr), and then cut off the current at a rate of 0.05C while maintaining 4.30V in constant voltage mode. Next, the battery was discharged at a constant current of 1C rate until the voltage reached 2.8V (vs. Gr) (third cycle), and such cycles were repeated under the same conditions up to the 300th cycle (300 repetitions).

[0223] In all the above charge / discharge cycles, a 10 minute rest period was allowed after each charge / discharge cycle.

[0224] Some of the results of the charge / discharge experiment are shown in Table 4. The capacity retention rate at the 302nd cycle is defined by the following Equation 2.

[0225]

number

[0226] [Table 4]

[0227] As can be seen from Table 4, the lithium battery of Example 10 had improved high-temperature life characteristics compared to the lithium battery of Comparative Example 11.

[0228] Such an improvement in high-temperature life characteristics is believed to be due to the fact that the composite positive electrode active material contained in the lithium battery of Example 10 additionally includes a second layer compared to the composite positive electrode active material contained in the lithium battery of Comparative Example 11, thereby further stabilizing the surface of the composite positive electrode active material.

[0229] For example, it is believed that this is because the second layer acts as a protective layer, thereby more effectively suppressing the elution of metal ions at high temperatures.

[0230] Evaluation example 7: Evaluation of room temperature charge / discharge characteristics (evaluation of the effect of adding 5% LFP) The lithium batteries prepared in Examples 5 and 9 were charged at a constant current of 0.1 C rate at 25° C. until the voltage reached 4.30 V (vs. Li), and then cut off at a current of 0.05 C rate while maintaining 4.30 V in constant voltage mode. Next, the batteries were discharged at a constant current of 0.2 C rate until the voltage reached 2.8 V (vs. Gr) (initial cycle, chemical formation cycle).

[0231] The lithium battery after the first cycle was charged at a constant current of 0.33 C rate at 25°C until the voltage reached 4.30 V (vs. Li), and then cut off the current at a rate of 0.05 C while maintaining 4.30 V in constant voltage mode. Next, the battery was discharged at a constant current of 0.2 C rate until the voltage reached 2.8 V (vs. Li) (second cycle).

[0232] The lithium battery after the second cycle was charged at a constant current of 0.33 C rate at 25°C until the voltage reached 4.30 V (vs. Li), then the current was cut off at a 0.05 C rate while maintaining 4.30 V in constant voltage mode, and then discharged at a constant current of 0.2 C rate until the voltage reached 2.8 V (vs. Li) (third cycle).

[0233] The lithium battery that had undergone the third cycle was charged at a constant current of 1C rate at 25°C until the voltage reached 4.30V (vs. Li), and then the current was cut off at a 0.05C rate while maintaining 4.30V in constant voltage mode.

[0234] The discharge capacity at the third cycle was taken as the standard capacity.

[0235] The initial efficiency is defined by the following equation 3.

[0236]

number

[0237] [Table 5]

[0238] As can be seen from Table 5, LiFePO 4 The lithium battery of Example 9 further comprising the above-mentioned compound had improved initial discharge capacity, initial charge / discharge efficiency, and standard capacity compared to the lithium battery of Example 5.

[0239] Evaluation example 8: DC resistance (DC-IR) evaluation at room temperature (25°C) (evaluation of the effect of adding 5% LFP) For the lithium batteries prepared in Examples 5 and 9, the initial direct current resistance (DC-IR) was measured at room temperature (25° C.) by the following method.

[0240] In the first cycle, charge the battery at a current of 0.5C up to a voltage of 50% SOC (state of charge), then cut off at 0.02C and rest for 10 minutes. Discharge at a constant current of 0.5C for 30 seconds, then rest for 30 seconds, charge at a constant current of 0.5C for 30 seconds, then rest for 10 minutes, Discharge at a constant current of 1.0C for 30 seconds, then rest for 30 seconds, charge at a constant current of 0.5C for 1 minute, then rest for 10 minutes, Discharge at a constant current of 2.0C for 30 seconds, then rest for 30 seconds, charge at a constant current of 0.5C for 2 minutes, then rest for 10 minutes, The battery was discharged at a constant current of 3.0C for 30 seconds, then rested for 30 seconds, and then charged at a constant current of 0.5C for 3 minutes and rested for 10 minutes.

[0241] The average voltage drop value for 30 seconds for each C-rate is the DC voltage value. The DC resistance was calculated from the measured DC voltage and is shown in Table 6 below.

[0242] [Table 6]

[0243] As can be seen from Table 6, LiFePO 4 The lithium battery of Example 9 further containing had a lower initial DC resistance than the lithium battery of Example 5.

[0244] Evaluation example 9: Evaluation of high temperature charge / discharge characteristics (evaluation of the effect of adding 5% LFP) The lithium batteries prepared in Examples 10 and 14 were charged at a constant current of 0.1 C rate at 45° C. until the voltage reached 4.30 V (vs. Gr), and then cut off at a current of 0.05 C rate while maintaining 4.30 V in constant voltage mode. Next, the batteries were discharged at a constant current of 0.1 C rate until the voltage reached 2.8 V (vs. Gr) (initial cycle, chemical formation cycle).

[0245] The lithium battery after the first cycle was charged at a constant current of 1.0 C rate at 45°C until the voltage reached 4.30 V (vs. Gr), then the current was cut off at a rate of 0.05 C while maintaining 4.30 V in constant voltage mode, and then discharged at a constant current of 0.2 C rate until the voltage reached 2.8 V (vs. Gr) (second cycle).

[0246] The lithium battery after the second cycle was charged at a constant current of 1C rate at 45°C until the voltage reached 4.30V (vs. Gr), and then cut off the current at a rate of 0.05C while maintaining 4.30V in constant voltage mode. It was then discharged at a constant current of 1C rate until the voltage reached 2.8V (vs. Gr) (third cycle), and such cycles were repeated under the same conditions until the 202nd cycle (200 repetitions).

[0247] In all the above charge / discharge cycles, a 10 minute rest period was allowed after each charge / discharge cycle.

[0248] Some of the results of the charge / discharge experiment are shown in Table 7. The capacity retention rate at the 202nd cycle is defined by the following Equation 4.

[0249]

number

[0250] [Table 7]

[0251] As can be seen from Table 7, LiFePO 4 The lithium battery of Example 14 further containing the above had improved high-temperature life characteristics compared to the lithium battery of Example 11. [Industrial Applicability]

[0252] INDUSTRIAL APPLICABILITY The composite positive electrode active material, the positive electrode and lithium battery using the same, and the manufacturing method thereof according to the present invention can be effectively applied to, for example, battery-related technical fields. [Explanation of symbols]

[0253] 1 Lithium battery 2 negative electrode 3 Positive electrode 4. Separator 5 Battery case 6 Cap Assembly 10,30,40 Primary particles 20,32,33,42 grain boundaries 21,31,41 Grain boundary direction 100 cores 101 Core tangential direction 200 shells 300 Composite positive electrode active material

Claims

1. a core including a plurality of primary particles and grain boundaries disposed between the plurality of primary particles; a shell disposed on the core; the primary particles comprise a nickel-based first lithium transition metal oxide; the shell includes a first layer and a second layer disposed on the first layer; the first layer comprises a first composition including a first metal, the first composition comprising Co3O4 and MgO; the second layer comprises a second composition comprising phosphorus (P), the second composition comprising Li 3 PO 4 , LiCoPO 4 and Co 3 (PO 4 ) 2 ; the first metal is Co and Mg; the grain boundaries include a third composition comprising a second metal, the third composition comprising Li 2 ZrO 3 , the second metal being Zr; A composite positive electrode active material, wherein the second layer is thicker than the first layer, the first layer is 50 nm or less, and the second layer is 500 nm or less.

2. 2. The composite positive electrode active material of claim 1, wherein the first composition includes a first phase, and the second composition includes a second phase that is distinct from the first phase in at least one of composition and structure.

3. 2. The composite positive electrode active material of claim 1, wherein the first composition includes at least one selected from a phase having a layered crystal structure and a phase having a spinel crystal structure.

4. 4. The composite cathode active material of claim 3, wherein the layered crystal structure belongs to the R-3m space group and the spinel crystal structure belongs to the Fd-3m space group.

5. 2. The composite positive electrode active material according to claim 1, wherein the first layer is disposed on a surface of at least one of the plurality of primary particles, and the first layer contains a first metal at a higher concentration than the first metal contained in the plurality of primary particles.

6. 2. The composite positive electrode active material of claim 1, wherein the first layer contains a first composition or a first metal in an amount of 10 parts by weight or less based on 100 parts by weight of the first lithium transition metal oxide.

7. 2. The composite positive electrode active material of claim 1, wherein the second layer contains a second composition or a phosphorus (P) content of 10 parts by weight or less based on 100 parts by weight of the first lithium transition metal oxide.

8. 2. The composite active cathode material of claim 1 , wherein the third composition comprises a third phase having a monoclinic crystal structure, the monoclinic crystal structure belonging to a C2 / m, C12 / c1, or C2 / c space group.

9. 10. The composite active cathode material of claim 1, wherein the shell further comprises a third composition comprising a second metal.

10. 2. The composite positive electrode active material of claim 1, wherein the first lithium transition metal oxide is doped with a second metal.

11. 2. The composite positive electrode active material of claim 1, wherein the first lithium transition metal oxide comprises lithium, nickel, a second metal, a third metal, and oxygen, and comprises 0.1 to 1.3 mol of lithium per mol of the first lithium transition metal oxide, 0.7 to 0.99 mol of nickel per mol of the first lithium transition metal oxide, 0.001 to 0.01 mol of a second metal per mol of the first lithium transition metal oxide, 0.01 to 0.3 mol of a third metal per mol of the first lithium transition metal oxide, and 1.7 to 2.3 mol of oxygen per mol of the first lithium transition metal oxide, and the third metal is a metal other than lithium, nickel, and the first metal.

12. 2. The composite positive electrode active material of claim 1, wherein the first lithium transition metal oxide is represented by the following formula 1: 【Chemistry 1】 In the formula 1, 0.9≦a≦1.1 and 0≦α<2; M4 is nickel, a second metal, and a third metal, and the third metal is one or more elements selected from the group consisting of Groups 2 to 13 elements excluding nickel and the second metal, and the nickel content in M4 is 70 mol% to less than 100 mol%, and X is an element selected from the group consisting of O, F, S, and P.

13. 2. The composite positive electrode active material of claim 1, wherein the first lithium transition metal oxide is represented by the following formula 2: 【Chemistry 2】 In the formula 2, 0.9≦a≦1.1, 0.7<b<1.0, 0<c<0.3, 0<d<0.3, 0≦e<0.1, b+c+d+e=1, and 0≦α<2; M5, M6 and M7 are different from one another and are each selected from cobalt (Co), manganese (Mn), zirconium (Zr), aluminum (Al), rhenium (Re), vanadium (V), chromium (Cr), iron (Fe), boron (B), ruthenium (Ru), titanium (Ti), niobium (Nb), molybdenum (Mo), magnesium (Mg) and platinum (Pt), and X is an element selected from the group consisting of O, F, S and P.

14. 2. The composite positive electrode active material of claim 1, wherein the first lithium transition metal oxide is represented by the following formula 3 or 4: 【Chemistry 3】 【Chemistry 4】 In Formula 3 and Formula 4, 0.9≦a≦1.1, 0.7<b<1.0, 0<c<0.1, 0<d<0.1, 0≦e<0.01, b+c+d+e=1, and 0≦α<2; M8 is one selected from zirconium (Zr), aluminum (Al), vanadium (V), chromium (Cr), iron (Fe), rhenium (Re), boron (B), ruthenium (Ru), titanium (Ti), niobium (Nb), molybdenum (Mo), magnesium (Mg) and platinum (Pt), and X is an element selected from the group consisting of O, F, S and P.

15. 2. The composite positive electrode active material of claim 1, wherein the first lithium transition metal oxide is represented by the following formula 5: 【Chemistry 5】 In the formula 5, 0<a<1 and 0≦α<2; M is two or more elements selected from nickel (Ni), cobalt (Co), manganese (Mn), zirconium (Zr), aluminum (Al), rhenium (Re), vanadium (V), chromium (Cr), iron (Fe), boron (B), ruthenium (Ru), titanium (Ti), niobium (Nb), molybdenum (Mo), magnesium (Mg), and platinum (Pt), and X is an element selected from the group consisting of O, F, S, and P.

16. A cathode comprising the composite cathode active material of claim 1 .

17. The positive electrode of claim 16 , further comprising an olivine-based positive electrode active material.

18. The positive electrode of claim 17, wherein the content of the olivine-based positive electrode active material is 10 wt % or less of the total weight of the positive electrode active material.

19. The positive electrode according to claim 16 ; A negative electrode; and an electrolyte disposed about the positive electrode and negative electrode.

20. Providing a nickel-based first lithium transition metal oxide; mixing the first lithium transition metal oxide with a first metal precursor to provide a first composition of a first lithium transition metal oxide; mixing the first composition of the first lithium transition metal oxide with a phosphorus (P) precursor to prepare a second composition of the first lithium transition metal oxide containing phosphorus (P); and drying the first lithium transition metal oxide second composition and heat-treating it in an oxidizing atmosphere at 400° C. to 1,000° C. to prepare a composite positive electrode active material. The first metal is Co and Mg, and the first composition is Co. 3 O 4 and MgO, the nickel-based first lithium transition metal oxide constitutes a core including a plurality of primary particles and grain boundaries disposed between the plurality of primary particles; The grain boundaries include a third composition including a second metal, the third composition including Li 2 ZrO 3 , and the second metal is Zr.

21. providing the first lithium transition metal oxide, mixing the first lithium transition metal oxide precursor with a second metal precursor to prepare a mixture; 21. The method of claim 20, further comprising: heat-treating the mixture in an oxidizing atmosphere at 400° C. to 1,000° C. to prepare a first lithium transition metal oxide.

22. a core comprising a plurality of primary particles; a shell disposed on the core; the primary particles comprise a nickel-based first lithium transition metal oxide; the shell includes a first layer and a second layer disposed on the first layer; the first layer comprises a first composition including a first metal, the first composition comprising Co3O4 and MgO; the second layer comprises a second composition comprising phosphorus (P), the second composition comprising Li 3 PO 4 , LiCoPO 4 and Co 3 (PO 4 ) 2 ; the first metal is Co and Mg; the core comprises a grain boundary disposed between a plurality of primary particles, the grain boundary comprising a third composition comprising a second metal; the third composition comprises a third phase of Li 2 ZrO 3 having a monoclinic crystal structure; The composite positive electrode active material, wherein the second metal is Zr.

Citation Information

Patent Citations

  • Continuous manufacture of oxygen-containing compound

    JP1985075440A

  • Battery active material and secondary battery

    JP2007213866A

  • Lithium composite metal oxide and production method thereof

    JP2015214465A

  • Lithium manganese composite oxide powder and production method therefor

    JP2017031006A

  • Positive electrode active material for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery using the same

    JP2018067549A