Method for manufacturing metal joint

A bonding layer with pile-shaped protrusions from the iron base into intermetallic compounds addresses the instability of dissimilar metal joints, providing a stable and reliable bond between steel and aluminum plates.

JP7570998B2Active Publication Date: 2024-10-22KK TOYOTA CHUO KENKYUSHO +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021177025
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-10-22
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

Existing methods for joining dissimilar metals like steel and aluminum plates, such as spot welding, result in unstable bond quality and reliability due to the formation of a fragile intermetallic compound layer, which limits practical application.

Method used

A bonding layer structure is developed with a pile-shaped first protrusion from the iron base into an intermetallic compound, enhancing the anchor effect and inhibiting crack propagation, comprising a first intermetallic compound on the iron substrate side and a second intermetallic compound on the aluminum substrate side.

Benefits of technology

The proposed structure achieves stable and reliable bonding strength, suitable for practical use, by ensuring a strong and durable joint through the pile-shaped protrusions and intermetallic compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570998000001
    Figure 0007570998000001
  • Figure 0007570998000002
    Figure 0007570998000002
  • Figure 0007570998000003
    Figure 0007570998000003
Patent Text Reader

Abstract

To provide a new metal joined body in which an iron base and an aluminum base are joined to each other.SOLUTION: There is provided a metal joined body in which an iron base and an aluminum base are joined to each other through a joint layer. The joint layer has a first layer composed of a first intermetallic compound made on the side of the iron base, and a second layer composed of a second intermetallic compound made on the side of the aluminum base. The first layer has a first projection which is integrally continuous from the iron base and extends in a pile shape to the first intermetallic compound. The second layer preferably has a second projection which is made of a second intermetallic compound and extends in a columnar shape to the aluminum base. The first intermetallic compound contains Al5Fe2, and the second intermetallic compound may contain Al3Fe. The total thickness of the first layer and the second layer is, for example, 2-15 μm.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a joint between an iron substrate and an aluminum substrate. [Background technology]

[0002] In order to reduce weight and improve functionality, dissimilar metals are bonded together (called dissimilar metal bonded bodies). For example, roofs and outer panels made of lightweight aluminum alloy sheets bonded to steel sheets that form the skeleton or frame are increasingly being used in automobiles.

[0003] Up until now, dissimilar metal plates have mainly been joined by riveting (self-piercing rivet joining, etc.) or clinching. Such mechanical joining methods require auxiliary materials (rivets, etc.) and dedicated equipment, which can increase the weight and cost of the joined body. In addition, protrusions that form at mechanically joined parts can cause interference with surrounding parts and reduce workability.

[0004] In view of this, it has been proposed to join dissimilar metal plates (particularly steel plates and aluminum alloy plates) by spot welding in the same manner as steel plates, and for example, there is a related description in the following patent documents. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2006-289452 [Patent Document 2] Patent Publication No. 2013-78804 [Patent Document 3] Patent Publication No. 2013-27890 Summary of the Invention [Problem to be solved by the invention]

[0006] Patent Documents 1 to 3 describe a joint in which a steel sheet and an aluminum alloy sheet are spot-welded by passing a constant large current between them for a short period of time. The current (density) value is set to be large so that the aluminum alloy sheet itself is directly melted by resistance heating (Joule heating). The current passing time is set to be short so that the joint layer made of a brittle intermetallic compound is thin.

[0007] In all of the joints, a substantially homogeneous Al5Fe2 layer was formed with a substantially constant thickness on the steel plate side near the joint interface. According to the inventor's research, such joints have been hardly put to practical use because they are unstable in joint quality (joint strength, durability, etc.) and lack reliability.

[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a joined body of dissimilar metals suitable for practical use. [Means for solving the problem]

[0009] As a result of intensive research by the inventors to solve this problem, they succeeded in obtaining a highly reliable metal joint by forming a joint layer between an iron substrate and an aluminum substrate with a structure in which a part of the iron substrate protrudes like a pile into an intermetallic compound (called a "pile structure"). By expanding on this result, they have completed the present invention described below.

[0010] 《Metal joint》 The present invention provides a metal joined body in which an iron base and an aluminum base are joined via a joining layer, the joining layer having a first layer made of a first intermetallic compound formed on the iron base side and a second layer made of a second intermetallic compound formed on the aluminum base side, the first layer having a first projection integrally continuing from the iron base and extending like a pile into the first intermetallic compound.

[0011] The metal joined body of the present invention has a stable joining strength, is highly reliable, and can be put into practical use. The reason why such excellent effects are obtained is considered to be as follows. The first layer according to the present invention is composed of a composite structure (pile structure) in which pile-like first projections (piles) extending from the iron substrate extend into the first intermetallic compound. The first intermetallic compound is firmly joined to the iron substrate, which is comb-shaped by the first projections, by an anchor effect or the like. Furthermore, the first projections, which are made of an iron substrate and have high toughness or ductility, can sufficiently suppress the development and propagation of cracks occurring in the first intermetallic compound. It is considered that the metal joined body of the present invention thus stably maintains a strong joining state at least on the iron substrate side.

[0012] <<Method for manufacturing a metal bonded body>> The present invention can also be understood as a method for producing a metal joined body. For example, the present invention may be a method for producing the above-mentioned metal joined body, comprising a heating step of applying an electric current through electrodes pressed against the outer surfaces of an iron base and an aluminum base to be joined, to generate a liquid phase of the aluminum base on a solid phase of the iron base at a joined portion of the iron base and the aluminum base, and a cooling step of cooling the joined portion after the heating step.

[0013] According to this manufacturing method, the liquid phase of the aluminum substrate generated in the joining portion (near the joining interface) in the heating step reacts with the solid phase of the iron substrate to generate the first intermetallic compound. At this time, for example, by adjusting the heating time and degree (current value during resistance heating, etc.), the unreacted portion of the solid phase of the iron substrate remains in the first intermetallic compound in the shape of a pile to form the first protrusion, and thus the first layer described above can be formed.

[0014] In the cooling step, the liquid phase containing Al and Fe remaining on the first layer can react with the solid phase of the aluminum substrate and solidify to form the second layer made of the above-mentioned second intermetallic compound. Thus, the iron substrate and the aluminum substrate can be firmly and stably joined to each other by the joining layer including the first layer and the second layer to form a metal joined body.

[0015] "others" (1) For ease of explanation, the one on the iron substrate side will be designated "first" and the one on the aluminum substrate side will be designated "second", as appropriate.

[0016] (2) Unless otherwise specified, "x to y" in this specification includes a lower limit value x and an upper limit value y. Any numerical value included in the various numerical values ​​or numerical ranges described in this specification may be used as a new lower limit or upper limit value to create a new range such as "a to b". Furthermore, unless otherwise specified, "x to y μm" in this specification means x μm to y μm. The same applies to other units (ms, kA, etc.). [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic diagram showing an overview of spot welding. [Diagram 2] 4 is an example of a time chart relating to spot welding. [Figure 3A] 1 is a micrograph showing a cross section of a joint for Sample 1. [Figure 3B] 1 is a micrograph showing a cross section of a bonding layer between an Al alloy plate and a steel plate for Sample 1. [Figure 3C] 1 is a micrograph showing an example of an area for identifying parameters, with reference to sample 1. [Figure 3D] 1 is a micrograph illustrating the thickness (t1) of the first layer and the width (w) of the primary projections, taking Sample 1 as a reference. [Figure 3E] 1A to 1C are reference diagrams each showing a schematic example of a form of a bonding layer. [Figure 4A] 1 is a micrograph showing a cross section of a joint for Sample 2. [Figure 4B] 1 is a micrograph showing a cross section of a bonding layer between an Al alloy plate and a steel plate for sample 2. [Diagram 5] 1 is a micrograph showing the cross section of a crack that occurred in the bonding layer between the Al alloy plate and the steel plate for sample 2 and sample C. [Figure 6] FIG. 1 is a temperature distribution diagram during a heating process obtained by a simulation using Sample 1 as a model. [Figure 7] FIG. 2 is a schematic diagram showing the process (mechanism) of generating a bonding layer. [Figure 8] FIG. 1 is a schematic diagram showing an evaluation test of bonding strength. [Figure 9] 1 is a schematic diagram showing an example of use of a metal bonded body. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] One or more components selected arbitrarily from the present specification may be added to the above-mentioned components of the present invention. The contents described in this specification may also be appropriately applied to the metal bonded body as well as its manufacturing method. Which embodiment is best depends on the target, required performance, etc.

[0019] Iron and aluminum substrates The iron substrate and the aluminum substrate may be of any material (composition) or shape. The iron substrate may be pure iron or an iron alloy (particularly steel). The aluminum substrate may be pure aluminum or an aluminum alloy. The iron substrate and the aluminum substrate may be of the same shape or different shapes. For ease of explanation, the following description will be given taking as appropriate a steel plate and an aluminum alloy plate (referred to as "Al alloy plate") as typical examples of the iron substrate and the aluminum substrate.

[0020] The steel plate and the Al alloy plate may each be one sheet, or at least one of them may be multiple sheets. The multiple sheets may be the same or different in thickness, composition, surface treatment state (plating or not, etc.).

[0021] The steel sheet may be, for example, a cold-rolled steel sheet, a hot-rolled steel sheet, a high-strength steel sheet, a hot-stamped steel sheet, or the like. At least one steel sheet may be surface-treated on one or both sides. Examples of the surface-treated layer of the steel sheet include a zinc-plated layer, an Al-Si-based plating layer, a zinc oxide layer, a Zn-Fe alloy layer, or the like. Representative examples of zinc-plated steel sheets include hot-dip galvanized steel sheets, electrogalvanized steel sheets, and alloyed hot-dip galvanized steel sheets. The alloyed hot-dip galvanized steel sheet may be an aluminum-zinc alloy-plated steel sheet (so-called Galvalume Steel Sheet (registered trademark)).

[0022] At least the surface treatment layer on the side of the surface to be joined may be made of a metal with a lower melting point than the Al base material (Al alloy, etc.) that constitutes the aluminum substrate. Such a surface treatment layer (plating layer) melts before (prioritizes) the aluminum substrate, wets and spreads between the surfaces to be joined, and excess low-melting point metal is expelled to the outer periphery of the joint. For this reason, even a surface-treated iron substrate can be joined to an aluminum substrate by a bonding layer made of a desired intermetallic compound.

[0023] The aluminum substrate (Al alloy plate) is made of, for example, an Al alloy of 2000 series to 8000 series, particularly 5000 series or 6000 series. For the 5000 series, for example, an Al alloy equivalent to A5052, A5083, A5005, etc., specified in JIS is used. For the 6000 series, for example, an Al alloy equivalent to A6022, A6016, A6N01, A6061, A6082, etc., specified in JIS is used. Note that the Al alloy referred to in this specification also includes the A1000 series.

[0024] When the iron substrate is a steel plate, the thickness is, for example, 0.4 to 2.5 mm, or 0.6 to 1.8 mm. When the aluminum substrate is an Al alloy plate, the thickness is, for example, 0.8 to 3 mm, or 1 to 2 mm. The thicknesses of the plates may be the same or different.

[0025] 《Joining layer》 The bonding layer formed between the iron substrate and the aluminum substrate has at least a first layer made of a first intermetallic compound formed on the iron substrate side, and a second layer made of a second intermetallic compound formed on the aluminum substrate side. The first layer and the second layer will be described below.

[0026] (1)First layer The first layer is located on the iron substrate side of the bonding layer and has a first intermetallic compound and a first protrusion. The first intermetallic compound is mainly composed of, for example, Al5Fe2. The first protrusion is integrally connected to the iron substrate and protrudes in a pile-like shape into the layered first intermetallic compound. In other words, the first protrusion extends from the iron substrate in a comb-like shape, and the first intermetallic compound fills the spaces between the first protrusions while covering the bonding interface of the iron substrate. The first protrusion is made of an iron base material like the iron substrate, but the composition of the components does not have to be the same. For example, the first protrusion may be an iron alloy containing more Al or plating components (e.g., Zn) than the iron substrate itself.

[0027] The more uniformly a plurality (a large number) of primary projections are distributed in the first intermetallic compound layer, the stronger the bond between the first layer and the iron substrate, and the more the propagation and growth of cracks that may occur in the first layer can be suppressed. For example, the number of such primary projections per reference length (50 μm) along the first layer (referred to as the "pile distribution") may be 2 to 60, 10 to 55, 20 to 50, or even 30 to 45. If the pile distribution is too small, the interval between the primary projections (pile) becomes wide, and cracks that occur in the first layer tend to grow. If the pile distribution is too large, the growth of the first layer made of the first intermetallic compound (particularly Al5Fe2) becomes insufficient, and the stability of the bonding strength may decrease.

[0028] The primary projections may penetrate the first intermetallic compound or may be embedded in the first intermetallic compound. In either case, it is preferable that the thickness of the first layer and the thickness of the primary projections (the "width" in cross section) are within a desired range. For example, the ratio of the thickness (t1) of the first layer to the width (w) of the primary projections (referred to as the "width-thickness ratio") is preferably 1 to 20, 2 to 10, or even 3 to 5. If the width-thickness ratio (t1 / w) is too small, the growth of the first layer made of the first intermetallic compound (particularly Al5Fe2) becomes insufficient, and the bonding strength may decrease. If the width-thickness ratio is too large, the primary projections (pile) become thin, and cracks generated in the first layer become more likely to progress.

[0029] To ensure stable bonding, the thickness of the first layer is, for example, 1 to 10 μm, 2 to 7 μm, or even 3 to 5 μm, and the combined thickness of the first and second layers is, for example, 2 to 15 μm, 3 to 10 μm, or even 4 to 8 μm.

[0030] Unless otherwise specified, the projection distribution, width-thickness ratio, thickness of each layer, shape of projection, etc., referred to in this specification are determined based on an image (SEM image) obtained by observing a cross section of a joint (particularly an outer peripheral region excluding a central region of a nugget (for example, within 40% of a nugget diameter)) with a microscope. Details will be described later (see Figs. 3C to 3E).

[0031] (2)Second layer The second layer is located on the aluminum substrate side of the bonding layer and is made of a second intermetallic compound. The second intermetallic compound is mainly composed of, for example, Al3Fe. The second layer may be in the form of a layer having a substantially constant thickness or in the form of a comb tooth. The comb tooth-shaped second layer further has, in addition to a base layer made of the second intermetallic compound, second projections extending in a columnar shape toward the aluminum substrate side. The second projections enhance the anchor effect and firmly bond the second layer to the aluminum substrate. In addition, the aluminum substrate present between the multiple (large number) second projections can suppress the propagation and development of cracks that may occur in the second layer (particularly the second intermetallic compound layer).

[0032] 《Manufacturing method》 The metal joined body is obtained, for example, through a heating step in which a liquid phase of an aluminum substrate is generated on a solid phase of an iron substrate, and a cooling step in which the joined parts are cooled after the heating step. The heating step and the cooling step will be described below. For convenience of explanation, the case of spot joining (welding) a steel plate and an Al alloy plate will be described as an example.

[0033] (1)Heating process The heating step is performed, for example, by passing electricity through electrodes pressed against the outer surfaces of the iron and aluminum substrates to be joined. This current should be passed within a range in which the aluminum substrate itself does not melt directly by resistance heating alone. In other words, current should be passed within a range in which the aluminum substrate produces a liquid phase near the joining interface, with the heat transferred from the resistance-heated iron substrate also being used.

[0034] The heating process causes a melting reaction (solid-liquid interdiffusion layer reaction) between the liquid phase of the aluminum substrate and the solid phase of the iron substrate, and thus a first layer (solid-liquid interdiffusion layer) mainly composed of a first intermetallic compound (e.g., Al5Fe2) is formed on the iron substrate side of the joint.

[0035] The value of the current flowing through the parts to be joined is, for example, 10 to 15 kA (or even less than 15 kA), 11 to 14.5 kA, 11.5 to 14 kA, or even 12 to 13 kA. The current density calculated by dividing the current value by the tip area (second tip area) of the electrode (second electrode) on the Al alloy plate side is, for example, 50 to 300 A / mm 2 Furthermore, 100~250A / mm 2 That's fine too.

[0036] The current application time is, for example, 200 to 500 ms, 250 to 450 ms, or 300 to 400 ms. The current value may be changed with respect to the current application time. For example, upslope current application in which the current value increases monotonically (differential coefficient ≧0) may be performed. This makes it possible to efficiently generate a liquid phase of the aluminum substrate in the vicinity of the bonding interface while suppressing sputtering and dust.

[0037] When the current value changes, it is preferable that the upper and lower limits are within the above range. As the current value serving as the index, for example, the average value obtained by dividing the integral value of the current value (absolute value) over the current flow time by the current flow time can be used. In this case, it is preferable that the average value is within the above range.

[0038] A pre-current-passing step may be carried out before the above-mentioned current-passing (heating step) to familiarize the contact state between the iron substrate and the aluminum substrate. The pre-current-passing step is preferably carried out by current-passing to an extent that does not generate a liquid phase near the bonding interface. For example, the pre-current-passing step may be carried out at a current value smaller than that in the heating step (for example, 3 to less than 10 kA, or even 5 to 9.5 kA). After the pre-current-passing step (before the main current-passing step in the heating step), the current to the electrodes may be cut off (non-current-passing) or reduced to lower the temperature near the bonding interface and reduce the electrical resistance value. The period of time is, for example, 10 to 200 ms, or even 50 to 150 ms.

[0039] (2) Cooling process In the cooling step, the parts to be joined after the heating step are cooled through the electrodes by cutting off (non-energizing) the current after the heating step or by passing a small current (which may be constant or monotonically decreasing, etc.). The cooling step causes the remaining liquid phase containing at least Fe and Al to solidify after or in parallel with the formation of the first layer, and the liquid phase further melts and reacts with the aluminum substrate. In this way, a second layer mainly composed of the second intermetallic compound (e.g., Al3Fe) can be formed on the aluminum substrate side of the parts to be joined.

[0040] "electrode" Electricity is usually passed through the iron and aluminum substrates through electrodes pressed against them. It is advisable to use electrodes suited to the characteristics (shape, size, material, etc.) of the iron and aluminum substrates. As an example, we will explain the electrodes used for spot joining (welding) steel sheets and Al alloy sheets.

[0041] (1) Form The electrodes for spot welding may be either detachable from the shank (cap tip type) or integral with the shank (integral type). Usually, cap tip type electrodes (also called "tips") are used to reduce costs.

[0042] The electrode (tip) has, for example, a bottomed, generally cylindrical tip portion and a generally cylindrical body portion continuing from the tip portion. The outer surface (pressure contact surface) of the tip portion may be convex or concave. The size of the electrode is not important. The outer diameter (nominal diameter / D2) of the body portion is, for example, φ10 to 20 mm, or φ12 to 18 mm. The tip diameter (D1) is, for example, φ6 to 14 mm, or φ8 to 12 mm.

[0043] It is advisable to introduce a coolant (cooling liquid / cooling water) into the inner tube at the inside of the tip of the electrode. When the coolant is forcibly circulated, it is possible to suppress the temperature rise of the electrode and to stably cool the plate material through the electrode.

[0044] The basic shape of the tip of an electrode (especially a convex electrode) is specified in JIS C9304 (1999). For example, there are flat (F type), radius (R type), dome (D type), dome radius (DR type), truncated cone (CF type), truncated cone radius (CR type), etc. For spot welding of steel plates and Al alloy plates, it is recommended to use electrodes of DR type or R type, for example, from the viewpoint of versatility.

[0045] (2)Material The electrode (at least the tip) is preferably made of a material having excellent thermal conductivity, electrical conductivity, strength, etc. For example, an electrode made of a copper alloy having an electrical conductivity of 75 to 95% IACS, or even 80 to 90% IACS, is used. Examples of copper alloys include chromium copper, zirconium copper, chromium-zirconium copper, alumina-dispersed copper, and beryllium copper.

[0046] The electrode in contact with the steel plate and the electrode in contact with the Al alloy plate may be the same or different in form (shape, size (diameter)) and material.

[0047] (3) Pressure The pressure applied to press the electrode onto the steel plate or Al alloy plate is, for example, 2 to 6 kN, or even 3 to 5 kN. If the pressure is too low, dust and spatters are likely to occur. If the pressure is too high, deep dents (depressions) caused by the electrode and deformation and wear of the electrode are likely to occur. The contact area between the plate material and the electrode (the tip area of ​​the electrode) required for calculating the current density can be substituted by the projected area of ​​the indentation made on the plate material after joining.

[0048] "others" (1) The current value (current density) may be constant, or may vary according to a desired pattern. For example, by providing an upslope process in which the amount of current is gradually increased at the start of current flow (initial period of current flow), it is possible to prevent the generation of spatter due to a sudden increase in the current value. Also, by providing a downslope process in which the amount of current is gradually decreased at the end of current flow (final period of current flow), it is possible to prevent weld cracks (solidification cracks due to solidification shrinkage of the molten pool, hot cracks that may occur near the recrystallization temperature, etc.) due to a sudden drop in the current value.

[0049] The electrode pressure is sufficient as long as it can maintain the contact state necessary for current flow and cooling and does not cause excessive reduction in plate thickness, etc. The pressure may vary during the process, but it is usually sufficient if it is approximately constant throughout the process.

[0050] (2) After joining, the iron base and the aluminum base may be subjected to a heat treatment such as annealing or tempering. The heat treatment can adjust the structure of the joint (nugget) or its vicinity (heat-affected zone) or remove residual stress. The heating temperature is, for example, 120 to 250°C or 150 to 200°C. The heating time is, for example, 10 to 180 minutes or 30 to 120 minutes. The heating range may be the entire joint or a part of it (joint, etc.).

[0051] 《Application》 The metal joined body of the present invention is used for various members and structures. For example, when a vehicle panel or the like is formed from the metal joined body of the present invention, the vehicle can be made lighter. The vehicle panel is formed, for example, by joining an Al alloy plate constituting an exterior surface to a framework (platform, etc.) made of steel plates. Examples of the vehicle panel that is the upper structure of the vehicle include a roof panel, a side outer panel, etc. (see FIG. 9). EXAMPLES

[0052] A metal joint was produced by spot welding a steel plate and an Al alloy plate stacked together, and the joint structure, joint strength, etc. were evaluated. The present invention will be described in more detail with reference to these specific examples.

[0053] [First Example] An overview of spot welding according to this embodiment is shown in Fig. 1. Fig. 1 shows a plate assembly in which a first steel plate, a second steel plate, and an Al alloy plate are laminated in this order as the materials to be welded. Spot welding is performed by passing electricity through a pair of electrodes that are pressed against each surface of the plate assembly (the lower surface of the first steel plate and the upper surface of the Al alloy plate). For convenience of explanation, in this embodiment, unless otherwise specified, the direction of the arrows shown in Fig. 1 is the up-down direction or the left-right direction.

[0054] <Sample Preparation> (1) Board material The first steel plate was a non-coated cold-rolled steel plate (440 MPa grade / plate thickness: 1.4 mm), the second steel plate was a galvannealed steel plate (270 MPa grade / plate thickness: 0.8 mm), and the Al alloy plate was a wrought material equivalent to JIS A6022 / plate thickness: 1.2 mm). The galvanized steel plate had a galvanized layer (metal layer) of approximately 8 μm in thickness. The melting point of the galvanized layer itself is approximately 420°C, and the melting point of the Al alloy plate is approximately 650°C.

[0055] Each plate material was used for spot welding as it was, without surface polishing, etc. Also, each plate material was cut into strips (30 mm x 100 mm) before use.

[0056] (2) Electrode The first electrode on the first steel plate side and the second electrode on the Al alloy plate side used the same DR type (JIS C9304) commercially available tip (OBARA Corporation). The tip was forcibly cooled by supplying forced circulating cooling water (flow rate: 2.7 L / min) to the inside (inner cylindrical part) of the tip. The electrode was made of chromium copper (Cr: 1 mass%, Cu: balance) and had an electrical conductivity of 80% IACS.

[0057] As shown in the enlarged view of Figure 1, the electrode size was as follows: tip diameter (nominal diameter D2): φ16 mm, thickness of the bottom tip: 12 mm, radius of curvature of the tip shoulder: 8 mm, radius of curvature of the tip surface: R1: 40 mm, and tip diameter (D1) was 12 mm.

[0058] (3) Welding conditions Spot welding was performed using a servo pressure spot welding machine (ARO PA235KVAMF). An example of the current pattern is shown in Figure 2. In this case, the pressure (F) applied to the plate assembly by the electrodes was constant at 4kN. Current was applied by controlling the DC current as follows:

[0059] A first current application process (pre-current application process) was carried out with a first current value (I1) of 8 kA and current application time of 100 ms. After this current application, a non-current state was maintained for 100 ms, and the plate assembly was cooled through both electrodes (first cooling process). This reduced the electrical resistance between each plate (particularly between the second steel plate and the Al alloy plate) to a predetermined range, allowing the subsequent second current application process to be carried out stably.

[0060] After the first cooling step, the second current value (I2): 10 to 14 kA (current density: 88 to 123.8 A / mm 2 ), and current flow time: 400 ms. The second current flow process was performed using upslope current flow, where the current value linearly and monotonically increased from an initial value (I2i): 10 kA to a final value (I2f): 14 kA. This ensured the amount of current flow while suppressing the generation of dust, and allowed the bonding layer and nugget to grow. The metal bonded body obtained in this manner is referred to as "Sample 1."

[0061] "observation" (1) Figure 3A shows a photograph of the cross section of the joint of Sample 1 observed with an inverted metallurgical microscope (GX53 manufactured by Olympus Corporation). As is clear from Figure 3A, it was confirmed that the first steel plate and the second steel plate were joined via the first nugget located between the opposing surfaces of the plates, and the second steel plate and the Al alloy plate were joined via the second nugget located between the opposing surfaces of the plates.

[0062] From Fig. 3A, it can be seen that the first nugget was formed when the first and second steel plates melted together and then solidified. It can also be seen that the second nugget was formed when the molten Al alloy plate reacted with the second steel plate (solid-liquid mutual diffusion / melting reaction). As can be seen from Fig. 3A, both the first and second nuggets had sufficient size (diameter) and thickness (length in the plate thickness direction). The indentation (depression, depression) on the Al alloy plate side caused by the electrode was only about 0.3 mm deep (plate thickness reduction: about 25%).

[0063] (2) A photograph (SEM image) of the structure near the bonding interface between the second steel plate and the Al alloy plate observed with a scanning electron microscope (S-3600N, Hitachi High-Tech Corporation) is shown in Figure 3B. When the structure was observed with an energy dispersive X-ray spectrometer (EDX) attached to the microscope, the intermetallic compounds were observed to include the Al5Fe2 phase and the Al3Fe phase, as well as the Fe-Al-Zn phase (mainly Al5Fe2 with Zn in solid solution) or the Al-Zn phase.

[0064] However, it was confirmed that the bonding layer between the second steel plate and the Al alloy plate was mainly composed of a first layer consisting of the Al5Fe2 phase (first intermetallic compound) on the second steel plate side, and a second layer consisting of the Al3Fe phase (second intermetallic compound) on the Al alloy plate side.

[0065] As is clear from Fig. 3B, in the first layer, slender pile-like primary projections (denoted as "piles" as appropriate) extending integrally from the second steel plate were distributed approximately uniformly in the Al5Fe2 phase. On the other hand, in the second layer, relatively thick columnar secondary projections extending integrally from the Al3Fe phase formed on the first layer (Al5Fe2 phase) and growing so as to bite into the Al alloy plate were distributed approximately uniformly.

[0066] (3) In general, it is said that the intermetallic compound layer (interface reaction layer) is fragile and therefore its thickness is preferably 1 to 2 μm or less. However, in the case of this embodiment, the thickness of the bonding layer made of the intermetallic compound was about 4.6 μm (thickness of the first layer (Al5Fe2 phase): about 3.5 μm, thickness of the second layer (Al3Fe phase): about 1.1 μm).

[0067] The pile distribution (protrusion distribution) was sufficient, with 41.6 protrusions per 50 μm (reference length: L) along the surface direction of the first layer. Furthermore, the ratio of the thickness (t1) of the first layer to the pile width (w) (width-thickness ratio: t1 / w) was 3.1, which was within the desired range.

[0068] The thickness, projection distribution, and width-thickness ratio of each layer described above were determined as follows. First, as shown in Figures 3C and 3D, the vicinity of the bonded layer in the outer periphery of the bonded portion (nugget) between the iron substrate and the aluminum substrate was observed under magnification. Next, within a field of view of a given size (e.g., 25 μm × 40 μm) cut out from the observed image (SEM image), the layer thickness, pile width, and number of piles were determined. Specifically, this is as follows (see Figure 3E).

[0069] The layer thickness is defined as the shortest distance between the boundary between the iron substrate and the first layer (referred to as the "base line") and the boundary between the first layer and the second layer (referred to as the "layer interface"). The "layer thickness" determined for each field of view is defined as the maximum value of the shortest distance measured continuously or discretely (e.g., at 0.5 μm intervals) along the base line.

[0070] The width of the pile is the length of the base of the pile that touches the base line (the distance between the contact points). The "pile width" determined for each field of view is the arithmetic average of the base lengths of each pile measured along the base line. The "number of piles" determined for each field of view is the total number counted within the same field of view.

[0071] The layer thickness, pile width, and number of piles are determined for each of 10 visual fields appropriately selected from the outer periphery of the joint. The arithmetic average values ​​for the 10 visual fields are defined as the layer thickness (t1, t2), pile width (w), and number of piles (N) in this specification. The protrusion distribution and width-thickness ratio in this specification are calculated based on these. When the width of the observation visual field is x μm (≠ 50 μm), a conversion value is obtained by multiplying the number of piles (N) by a coefficient (50 / x), and the average value for the 10 visual fields is defined as the protrusion distribution.

[0072] "evaluation" Spot welding was performed under the above conditions to produce two types of test pieces, as shown in Figures 8(a) and (b). Tensile tests were performed using each test piece, and the tensile shear strength (average of five tests) was 4780N, and the cross tensile strength (average of five tests) was 1080N. As mentioned above, it was confirmed that sufficient joint strength could be obtained even when a thick joint layer was formed. Note that each joint strength is the load at break.

[0073] [Second Example] The workpieces, consisting of a total of three plates used in the first embodiment, were replaced with a total of two plates consisting of one steel plate (first steel plate) and one Al alloy plate stacked in sequence, and spot welding was performed. Cold-rolled steel plates (440 MPa class / plate thickness: 1.0 mm) and aluminum extrusion material (6N01 / plate thickness: 3.0 mm) were used as the steel plate and the Al alloy plate, respectively.

[0074] <Sample Preparation> Samples 2 and C were produced under the welding conditions shown below using the spot welding device shown in Figure 1. In both cases, direct current was applied and the applied pressure (F) was 4 kN (constant).

[0075] The specimen 2 was fabricated in the same manner as the specimen 1, with the following conditions: first current value (I1): 8 kA, first current application time: 100 ms, first cooling time: 100 ms, second current value (I2): 10 to 14 kA (current density: 88 to 123.8 A / mm 2 ), and the second current application time: 400 ms. In the second current application step, similarly to the first embodiment, up-slope current application was performed from an initial current value (I2i): 10 kA to a final current value (I2f): 14 kA according to the chart shown in FIG.

[0076] For sample C, the first current value (I1): 8 kA, the first current application time: 100 ms, the first cooling time: 100 ms, the second current value (I2): 13 kA (current density: 115 A / mm 2 ), and second current application time: 500 ms. In the second current application step, the second current value was kept constant.

[0077] "observation" The cross section of the joint of each sample was observed with the inverted metallurgical microscope described above. In addition, for each sample, the structure near the joint interface between the steel sheet and the Al alloy sheet was magnified and observed with the scanning electron microscope described above. As an example, each observation image of sample 2 is shown in Figure 4A and Figure 4B (both figures are simply referred to as "Figure 4").

[0078] As is clear from Fig. 4, a joint layer similar to that of the metal joined body according to Example 1 was confirmed in the metal joined body consisting of a pair of a steel plate and an Al alloy plate. That is, when observed by EDX in the same manner as in Example 1, a first layer mainly composed of an Al5Fe2 phase (first intermetallic compound) was confirmed on the steel plate side, and a second layer mainly composed of an Al3Fe phase (second intermetallic compound) was confirmed on the Al alloy plate side.

[0079] Furthermore, in the first layer, pile-like primary projections extending integrally from the steel plate were distributed approximately uniformly in the Al5Fe2 phase, and in the second layer, columnar secondary projections extending integrally from the Al3Fe phase formed on the first layer and growing into the Al alloy plate were distributed approximately uniformly.

[0080] On the other hand, no primary piles were observed in the first layer of sample C (see Figure 5). It is believed that the piles disappeared due to the long-term application of current, and the entire first layer became the Al5Fe2 phase. In addition, in the second layer of sample C, many fine projections were observed that had grown integrally from the Al3Fe phase into the aluminum alloy plate.

[0081] "evaluation" (1) The tensile test shown in FIG. 8 was also carried out on Sample 2 and Sample C. For Sample 2, the tensile shear strength was 4870 N. For Sample C, the tensile shear strength was 4230 N and the cross tensile strength was 500 N. Sample 2 had a sufficiently high bonding strength, but Sample C had a smaller bonding strength than Sample 2.

[0082] (2) For Sample 1 and Sample C, the outer periphery of the joint of the broken cross tensile test pieces (Fig. 8(b)) was observed using the scanning electron microscope described above. Both images are shown together in Fig. 5. As is clear from Fig. 5, in Sample 1, the crack that occurred in the joint layer at the time of fracture progressed by bypassing the pile, and the progression of the crack was suppressed by the pile. It is believed that this fracture process allowed Sample 1 to demonstrate high joint strength. The same fracture process was observed for Sample 2.

[0083] On the other hand, in sample C, because there was no pile in the first layer, the crack that occurred at the time of fracture propagated through the first layer and advanced far, reaching the steel plate. This is thought to have resulted in the lower bonding strength of sample C.

[0084] [Consideration] The mechanism by which the bonding layer according to the present invention is formed was examined.

[0085] (1)Temperature distribution The temperature distribution in the joint during spot welding of Sample 1 (first embodiment) was numerically analyzed using the resistance welding simulation software SORPAS. The analytical model used and an example of the analytical result (temperature distribution during the second current flow) are shown in Figure 6.

[0086] As is clear from Figure 6, the second current flow causes a first liquid phase to form between the joining interface of the first and second steel sheets. The first liquid phase solidifies by the second cooling after the second current flow to become the first nugget that joins the first and second steel sheets.

[0087] It is also seen that the second current flow causes a second liquid phase in which the Al alloy plate melts to be generated at the joint interface between the second steel plate and the Al alloy plate. Here, under the welding conditions (second current value) shown in the first embodiment, the Al alloy plate does not melt directly by resistance heating (Joule heating) alone. Therefore, it is considered that the Al alloy plate melts due to its own resistance heating and the heat conducted from the second steel plate side. The second liquid phase solidifies by the second cooling after the second current flow to become a second nugget (joint) that joins the Al alloy plate and the second steel plate.

[0088] (2) Formation of bonding layer Based on the above-mentioned simulation results, it is considered that the bonding layers (first and second layers) between the Al alloy plate and the steel plate were generated as follows.

[0089] First, in the heating process by the second current, the liquid phase (second liquid phase) of the Al alloy sheet melts and comes into contact with the surface of the steel sheet (solid phase), causing a melting reaction (solid-liquid interdiffusion reaction: SLID). Specifically, the liquid phase of the Al alloy penetrates and diffuses from the grain boundaries of the steel sheet, forming a first layer of the first intermetallic compound on the steel sheet side. At this time, by adjusting the transition time from the heating process to the cooling process (the end of the second current flow / the start of the second cooling), some of the Fe-based crystal grains of the steel sheet remain unreacted and become piles (first protrusions) integrated with the steel sheet.

[0090] Next, in the cooling step after the second current application, the liquid phase containing Fe and Al remaining on the steel sheet solidifies. As a result, a second layer made of the second intermetallic compound is formed on the Al alloy sheet side. At this time, the liquid phase solidifies while reacting with the Al alloy sheet, so that columnar second projections made of the second intermetallic compound are formed so as to dig into the Al alloy sheet.

[0091] It is believed that the bonding layer consisting of the first and second layers is formed in the vicinity of the bonding interface between the Al alloy sheet and the steel sheet in this way. A dissimilar metal joint having such a bonding layer exhibits stable bonding strength and is highly reliable.

Claims

1. a heating step in which a current is passed through electrodes pressed against the outer surfaces of the iron base and the aluminum base to be joined, thereby generating a liquid phase of the aluminum base on a solid phase of the iron base at the joint between the iron base and the aluminum base; and a cooling step of cooling the bonded portion after the heating step, Before the heating step, a pre-current application step for familiarizing the contact of the joined parts is performed at a current value of 5 to 9.5 kA; The heating step is performed at a current value of 10 to 15 kA for a current application time of 200 to 500 ms, which is longer than that of the pre-current application step, to obtain a metal joined body.

2. The method for producing a metal joined body according to claim 1 , wherein the heating step is performed by monotonically increasing the current value with respect to the current application time.

3. 3. The method for producing a metal joined body according to claim 1, wherein after the pre-current passing step and before the heating step, no current is passed or a current having a value lower than that in the pre-current passing step is passed, thereby lowering the temperatures of the iron base and the aluminum base.

4. The method for producing a metal joined body according to claim 3, wherein the temperature is lowered for 10 to 200 ms.

5. 5. The method for producing a metal joined body according to claim 1, wherein the pressure applied by the electrodes to the iron base and the aluminum base is 2 to 6 kN.

6. The metal joined body is formed by joining the iron base and the aluminum base via a joining layer, the bonding layer has a first layer made of a first intermetallic compound formed on the iron substrate side, and a second layer made of a second intermetallic compound formed on the aluminum substrate side, 6. The method for producing a metal joined body according to any one of claims 1 to 5, wherein the first layer has first projections in the first intermetallic compound formed by penetration of a liquid phase of the aluminum substrate from crystal grain boundaries of the iron substrate, the first projections being formed as part of crystal grains of the iron substrate remaining in an unreacted state and extending integrally from the iron substrate side.

7. 7. The method for producing a metal joined body according to claim 6, wherein the second layer is made of the second intermetallic compound and has second projections extending into the aluminum base.

8. The first intermetallic compound is Al 5 Fe 2 Including, The second intermetallic compound is Al 3 The method for producing a metal joined body according to claim 6 or 7, further comprising Fe.

9. The method for producing a metal joined body according to any one of claims 6 to 8, wherein the first layer has a thickness of 1 to 10 µm.

10. The method for producing a metal joined body according to any one of claims 6 to 9, wherein the combined thickness of the first layer and the second layer is 2 to 15 µm.

11. The method for producing a metal joined body according to any one of claims 6 to 10, wherein the number of the primary projections per reference length (50 µm) of the first layer is 2 to 60.

12. The method for producing a metal joined body according to any one of claims 6 to 11, wherein a ratio (t1 / w) of a thickness (t1) of said first layer to a width (w) of said first projections is 1 to 20.

13. The iron substrate is a steel plate, The aluminum substrate is an aluminum alloy plate, The method for producing a metal joined body according to any one of claims 6 to 12, wherein the steel plate and the aluminum alloy plate are spot joined.

14. The method for producing a metal joined body according to claim 13, wherein the steel plate has a surface treatment layer on the aluminum alloy plate side.

15. The method for producing a metal joined body according to any one of claims 6 to 14, which is used for a vehicle panel.

Citation Information

Patent Citations

  • Resistance welding method for different kinds of materials and resistance welding member of aluminum alloy material and different kinds of materials

    JP2005288524A

  • Joint body of different materials by steel material and aluminum material

    JP2006289452A

  • Joint body of aluminum alloy plate material to plated steel plate material

    JP2013027890A

  • Dissimilar metal bonding method

    JP2013078804A

  • Joining method of dissimilar metal plate

    JP2019126826A