Method for manufacturing film-shaped sintered material with support sheet, roll body, laminate and device

The film-like fired material with a support sheet is effectively attached to semiconductor wafers by designing it to fit within the inner periphery, addressing thickness uniformity and stability issues, reducing damage and ensuring reliable attachment.

JP7571014B2Active Publication Date: 2024-10-22LINTEC CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021522263
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-24
Filing Date
2020-05-20
Publication Date
2024-10-22
Estimated Expiration
2040-05-20

AI Technical Summary

Technical Problem

The challenge of attaching a film-like fired material with a support sheet to the back surface of semiconductor wafers is hindered by the difficulty in achieving uniform thickness and stability, especially when the wafers become thinner, increasing the risk of damage during processing and transportation.

Method used

A film-like fired material with a support sheet is designed to have a diameter smaller than the inner periphery of the wafer, featuring an adhesive layer on a base film, allowing it to be attached to the inner circumferential portion of the wafer with an annular convex portion, ensuring proper attachment and reducing damage.

Benefits of technology

The solution enables stable attachment of the film-like fired material to the wafer, preventing damage during processing and transportation, while maintaining uniform thickness and alignment, thereby enhancing the reliability of the semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571014000002
    Figure 0007571014000002
  • Figure 0007571014000003
    Figure 0007571014000003
  • Figure 0007571014000004
    Figure 0007571014000004
Patent Text Reader

Abstract

A film-like firing material 100 with a support sheet, which is provided with a support sheet 2 that has an adhesive layer 4 on a base material film 3 and a film-like firing material 1 that is provided on the adhesive layer 4, and which is used for the purpose of bonding the film-like firing material to an inner peripheral part of a wafer that has an annular projected part in an outer peripheral part, said inner peripheral part being on the side of the wafer having the annular projected part. With respect to this film-like firing material 100 with a support sheet, the diameter of the film-like firing material 1 is not more than the diameter of the inner peripheral part of the wafer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a film-shaped sintered material with a support sheet, a roll body, a laminate, and an apparatus. This application claims priority based on Japanese Patent Application No. 2019-097544 filed in Japan on May 24, 2019, the contents of which are incorporated herein by reference. [Background technology]

[0002] In recent years, the demand for power semiconductor elements (power devices) has increased along with the trend toward higher voltages and currents in automobiles, air conditioners, personal computers, etc. Since power semiconductor elements are characterized by their use under high voltages and currents, heat generation from the semiconductor elements can easily become a problem. Conventionally, a heat sink is sometimes attached around a semiconductor element to dissipate heat generated from the semiconductor element, but if the thermal conductivity at the joint between the heat sink and the semiconductor element is not good, efficient heat dissipation is hindered.

[0003] As a bonding material with excellent thermal conductivity, for example, Patent Document 1 discloses a paste-like metal microparticle composition in which specific heat-sinterable metal particles, a specific polymer dispersant, and a specific volatile dispersion medium are mixed. When the composition is sintered, it is said to become a solid metal with excellent thermal conductivity.

[0004] However, when the firing material is in a paste form as in Patent Document 1, it is difficult to make the thickness of the applied paste uniform, and the thickness tends to be unstable.

[0005] Therefore, in order to solve the problem of thickness stability, the inventors came up with the idea of ​​providing a fired material, which has conventionally been provided as a paste-like composition, in the form of a film. To make a fired material into a film, a binder component may be added to the fired material to form it into a film.

[0006] Such a film-shaped sintered material can be used, for example, for sintering the chips obtained by dicing a semiconductor wafer to a substrate. In addition, if a support sheet is provided on one side (surface) of the film-shaped sintered material, it can be used as a dicing sheet used when dicing a semiconductor wafer into chips. Furthermore, by dicing together with the semiconductor wafer using a blade or the like, it can be processed into a film-shaped sintered material of the same shape as the chip.

[0007] On the other hand, in recent years, semiconductor chips have been made thinner, and there is now a demand to thin wafers, which were previously around 350 μm thick, to 50 to 100 μm or even less. However, as semiconductor wafers become thinner, the risk of breakage during processing and transportation increases.

[0008] For this reason, it has been proposed that when grinding the back surface of a wafer, only the inner peripheral part of the back surface is ground, leaving an annular protrusion on the outer peripheral part of the back surface to give the wafer rigidity (Patent Documents 2 to 4). Because the annular protrusion has a relatively high rigidity, a wafer ground to the above shape can be transported and stored stably and is less likely to be damaged during processing. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2014-111800 A [Patent Document 2] JP 2007-19379 A [Patent Document 3] JP 2007-266352 A [Patent Document 4] JP 2007-287796 A Summary of the Invention [Problem to be solved by the invention]

[0010] However, when the film-shaped sintered material with support sheet is applied to a semiconductor wafer as described in Patent Documents 2 to 4, the film-shaped sintered material with support sheet may not be properly attached to the back surface of the wafer.

[0011] The present invention has been made to solve the problems described above, and aims to provide a film-shaped sintering material with a support sheet, which can be appropriately attached to the inner peripheral portion of the surface of a wafer having a ring-shaped protrusion on its outer periphery, the film-shaped sintering material being capable of being properly attached to the inner peripheral portion of the surface of the wafer having the ring-shaped protrusion. [Means for solving the problem]

[0012] That is, the present invention has the following aspects.

[0013] <1> A film-like sintered material with a support sheet, comprising a support sheet having an adhesive layer on a base film, and a film-like sintered material provided on the adhesive layer, It is used to attach the film-shaped sintering material to the inner periphery of a wafer having an annular convex portion on the outer periphery, the inner periphery of the surface having the annular convex portion, A film-shaped sintered material with a support sheet, the diameter of the film-shaped sintered material being equal to or smaller than the diameter of the inner periphery of the wafer. <2> A film-like sintered material with a support sheet, comprising a support sheet having an adhesive layer on a base film, and a film-like sintered material provided on the adhesive layer, The diameter of the film-shaped sintered material with a support sheet is 130 to 146 mm, 180 to 196 mm, 280 to 296 mm, or 430 to 446 mm. <3> The thickness of the support sheet is 120 μm or less, The load of the support sheet at 5% elongation measured by the following measurement method is 13 N / 15 mm or less. <1> or <2> A film-shaped sintered material with a support sheet according to claim 1, Measurement method: The support sheet is cut into a test piece having a width of 15 mm and a length of 150 mm (however, if the adhesive layer is curable, the test piece is used before curing). The test piece is pulled under conditions of a chuck distance of 100 mm and a tensile speed of 200 mm / min in an environment of 23°C and 50% RH, and the load relative to the amount of displacement is measured. <4> The support sheet has an absorbance of 0.22 or less at a wavelength of 355 nm. <1> ~ <3> 2. A film-shaped sintered material with a support sheet according to claim 1 . <5> The pressure-sensitive adhesive layer is energy ray curable. <1> ~ <4> 2. A film-shaped sintered material with a support sheet according to claim 1 . <6> The pressure-sensitive adhesive layer contains a pressure-sensitive adhesive resin, and the pressure-sensitive adhesive resin has an energy ray-polymerizable unsaturated group in its side chain. <5> The film-shaped sintered material with a support sheet according to claim 1. <7> The pressure-sensitive adhesive layer contains a pressure-sensitive adhesive resin, and the pressure-sensitive adhesive resin contains a structural unit derived from a (meth)acrylate having an alkoxy group in a side chain with a carbon number of 8 to 18. <1> ~ <6> 2. A film-shaped sintered material with a support sheet according to claim 1 . <8> The thickness of the film-shaped fired material before firing is 10 to 200 μm. <1> ~ <7> 2. A film-shaped sintered material with a support sheet according to claim 1 . <9> The above-mentioned is applied onto a long release film. <1> ~ <8> The film-shaped sintered material with a support sheet according to any one of the above items is laminated with the film-shaped sintered material on the inside, The release film and the film-shaped sintered material with the support sheet are wound into a roll. <10> The above <1> ~ <8> A laminate in which a film-shaped sintered material with a support sheet described in any one of the above items is attached to the inner peripheral portion of the surface side of a wafer having a ring-shaped convex portion on its outer periphery, and the support sheet, the film-shaped sintered material, and the wafer are stacked in this order. <11> A method for manufacturing an apparatus comprising the steps of (1) to (5) below in sequence: Step (1): <10> A step of cutting the annular convex portion of the laminate described in Step (2): dicing the wafer and the film-shaped sintered material of the laminate from which the annular protrusion has been removed; Step (3): peeling off the diced film-shaped sintered material and the support sheet to obtain a chip with the film-shaped sintered material; Step (4): A step of attaching the film-shaped sintered material of the chip with the film-shaped sintered material to a surface of a substrate; Step (5): A step of firing the film-shaped sintered material of the chip with the film-shaped sintered material, and bonding the chip and the substrate. Effect of the Invention

[0014] According to the present invention, it is possible to provide a film-shaped sintering material with a support sheet, which can be appropriately attached to the inner periphery of a wafer having a ring-shaped protrusion on its outer periphery, on the side having the ring-shaped protrusion. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a cross-sectional view showing a film-shaped sintered material with a support sheet according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a plan view of a circuit-forming surface of a semiconductor wafer. [Diagram 3] 1 is a perspective view of a semiconductor wafer having an annular protrusion formed on the outer periphery of the rear surface. [Figure 4] 1 is a cross-sectional view showing a state in which a film-shaped sintered material with a support sheet according to one embodiment of the present invention is attached to a semiconductor wafer and a ring frame. [Diagram 5] 1 is a perspective view showing a state in which a film-shaped sintered material with a support sheet according to one embodiment of the present invention is attached to a semiconductor wafer and a ring frame. FIG. [Figure 6] FIG. 2 is a cross-sectional view showing a schematic diagram of a roll body according to one embodiment of the present invention. [Figure 7A] 1A to 1C are cross-sectional views that diagrammatically show a method for manufacturing a device according to one embodiment of the present invention. [Figure 7B]1A to 1C are cross-sectional views that diagrammatically show a method for manufacturing a device according to one embodiment of the present invention. [Figure 7C] 1A to 1C are cross-sectional views that diagrammatically show a method for manufacturing a device according to one embodiment of the present invention. [Figure 7D] 1A to 1C are cross-sectional views that diagrammatically show a method for manufacturing a device according to one embodiment of the present invention. [Figure 7E] 1A to 1C are cross-sectional views that diagrammatically show a method for manufacturing a device according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment of the present invention will be described with reference to the drawings as appropriate. In addition, the figures used in the following explanation may show key parts enlarged for convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may not necessarily be the same as the actual ones.

[0017] <Film-shaped baking material with support sheet> The film-shaped sintered material with support sheet of this embodiment is a film-shaped sintered material with support sheet comprising a support sheet having an adhesive layer on a base film and a film-shaped sintered material provided on the adhesive layer, and is used to attach the film-shaped sintered material to the inner peripheral portion of the surface side of a wafer having an annular convex portion on its outer periphery, the surface side having the annular convex portion, and the diameter of the film-shaped sintered material is less than the diameter of the inner peripheral portion of the wafer.

[0018] 1 is a cross-sectional view showing a film-shaped sintered material with a support sheet according to the present embodiment. The film-shaped sintered material with a support sheet 100 includes a film-shaped sintered material 1 containing sinterable metal particles 10 and a binder component 20, and a support sheet 2 provided on at least one side of the film-shaped sintered material 1. The film-shaped sintered material 100 with support sheet of this embodiment is configured by temporarily and releasably attaching the film-shaped sintered material 1 to the inner periphery of the support sheet 2 consisting of a base film 3 and an adhesive layer 4. The film-shaped sintered material 1 is provided in direct contact with the adhesive layer 4, and the inner periphery surface of the adhesive layer 4 is covered by the film-shaped sintered material 1, with the adhesive portion exposed on the outer periphery. In this configuration example, it is preferable that the film-shaped sintered material 1, which has a smaller diameter than the support sheet 2, is peelably laminated concentrically on the adhesive layer 4 of the support sheet 2. The film-shaped sintered material with support sheet of this embodiment can be used as a dicing sheet used when dividing a semiconductor wafer into chips. By dividing it together with the semiconductor wafer using a blade or the like, it can be processed into a film-shaped sintered material of the same shape as the chip, and a chip with the film-shaped sintered material can be manufactured.

[0019] 2-3 are schematic diagrams showing an example of a wafer 18 having an annular convex portion on the outer periphery, which is the target of the film-like sintered material 1 with a support sheet. Hereinafter, the surface of the wafer on which the circuit is formed may be referred to as the "front surface", and the surface having the annular convex portion may be referred to as the "back surface". As shown in FIG. 2, the front surface of the wafer 18 has an excess portion 15 on which the circuit 13 is not formed within a range of several mm from the outer periphery, and the circuit 13 is formed on the front surface inner periphery 14 excluding the excess portion. In the wafer having the annular convex portion, the back surface inner periphery 16 corresponding to the front surface circuit forming portion (front surface inner periphery 14) is ground to a predetermined thickness, and the back surface outer periphery corresponding to the excess portion 15 on which the circuit is not formed remains without being ground, forming the annular convex portion 17. Since the annular convex portion 17 has a relatively high rigidity, the wafer 18 ground to the above shape can be transported and stored stably, and is less likely to be damaged during processing. FIG. 3 shows a perspective view from the back surface side on which the annular convex portion 17 is formed.

[0020] Examples of the wafer or chip include a semiconductor wafer or chip, an insulator wafer or chip, a conductor wafer or chip, etc. Examples of the insulator wafer include, but are not limited to, a glass wafer and a sapphire wafer. In the embodiment, a case where a semiconductor wafer or chip is used as the wafer or chip will be described.

[0021] The film-shaped sintered material 1 can be used by being attached to the inner periphery 16 of the back surface of the wafer 18, but the film-shaped sintered material is brittle when used alone, and therefore tends to be difficult to handle when attached. Therefore, by attaching the support sheet and the film-shaped sintered material in advance, as in the case of the film-shaped sintered material with support sheet of the embodiment, the state of the attached film-shaped sintered material can be made uniform and damage to the film-shaped sintered material can be prevented. Furthermore, alignment between the inner periphery of the back surface and the film-shaped sintered material when attached is made easy.

[0022] Below, we will explain the relationship between the wafer 18 and the film-like sintered material 100 with support sheet when attaching the film-like sintered material 1 of the embodiment of the film-like sintered material 100 with support sheet to the inner peripheral portion 16 of the back surface of the wafer 18, which has a ring-shaped protrusion 17 on the outer peripheral portion of the back surface. In this specification, the "inner peripheral portion of the back surface" of the wafer refers to the portion of the wafer on the side having the annular protrusion, excluding the annular protrusion on the outer periphery, toward the center of the annular protrusion on the outer periphery.

[0023] Fig. 4 is a cross-sectional view showing a structure in which a film-shaped sintered material 1 is attached to the back surface inner periphery 16. Fig. 4 is also a cross-sectional view showing a laminate 120 according to one embodiment of the present invention described below. In the film-shaped sintered material 100 with support sheet, the diameter D1 of the film-shaped sintered material is equal to or smaller than the diameter D3 of the back surface inner periphery of the wafer, and from the viewpoint of ease of attachment, as shown in Fig. 4, it is preferable that the diameter D1 is smaller than the diameter D3. Conventionally, in the film-shaped sintered material with support sheet, the diameter D4 of the wafer and the diameter D1 of the film-shaped sintered material are the same, or the diameter D1 of the film-shaped sintered material is larger than the diameter D4 of the wafer. However, it was difficult to attach the film-shaped sintered material to the back inner periphery 16 of the wafer 18 on the side having the annular convex portion 17 using such a film-shaped sintered material with support sheet, because the film-shaped sintered material was damaged. Even if the film-shaped sintered material is not damaged, if the diameter of the wafer and the diameter of the film-shaped sintered material are the same, or the diameter of the film-shaped sintered material is larger than the diameter of the wafer, the film-shaped sintered material 1 will adhere to the inner surface 12 of the annular convex portion, etc., and the thickness of the film-shaped sintered material 1 attached to the back inner periphery 16 will vary. Therefore, as shown in Figure 4, in the film-shaped sintered material 100 with support sheet, the diameter D1 of the film-shaped sintered material is less than the diameter D3 of the inner circumference of the back surface of the wafer, making it possible to properly attach the film-shaped sintered material 1 to the inner circumference 16 of the back surface.

[0024] The shape of the film-shaped sintered material 1 is preferably formed to be approximately the same as the shape of the back surface inner periphery 16 to which it is attached. The shape of the back surface inner periphery 16 may be circular or approximately circular, and the shape of the film-shaped sintered material 1 may also be circular or approximately circular. The shapes of the wafer and the support sheet 2 may also be circular or approximately circular. Specific examples of approximately circular wafers include wafers having a V-notch or a straight portion (orientation flat) (however, even if the shape of the wafer 18 is approximately circular, the shape of its back surface inner periphery 16 may also be circular). In this specification, when the shape of each of the above-mentioned parts is not circular or approximately circular, the diameter may be the diameter when the shape is converted into a perfect circle based on the area, and when the shape of each part is circular or approximately circular but the shape is not a perfect circle, the diameter is the diameter at which the length of the circle is maximum.

[0025] The current wafer size is standardized by a standard, and the diameter (D4 in FIG. 4) is 150 mm, 200 mm, 300 mm, 450 mm, etc. are used. The thickness (T4 in FIG. 4) of the annular protrusion 17 varies depending on the product. The thicker the annular protrusion 17, the higher the rigidity, but the smaller the area of ​​the circuit formation part. The thinner the annular protrusion 17, the larger the area of ​​the circuit formation part, but the lower the rigidity. Considering these, the thickness (T4 in FIG. 4) of the annular protrusion 17 is usually 2 to 5 mm, and the diameter (D3 in FIG. 4) of the back inner periphery 16 corresponding to the above-mentioned standard wafer is assumed to be 140 to 146 mm, 190 to 196 mm, 290 to 296 mm, and 440 to 446 mm, respectively.

[0026] The size of the film-shaped sintered material 1 is preferably large enough to efficiently cover the back surface portion corresponding to the circuit formation portion of the wafer, and the value of the diameter of the back surface inner circumference 16 - the diameter of the film-shaped sintered material 1 (D3 - D1) may be, for example, 0 to 10 mm, or 2 to 7 mm.

[0027] Here, the part of the back surface inner periphery 16 that is further out than the attached part of the film-shaped sintered material 1, which may correspond to the part indicated by D3-D1, is defined as the outer periphery 16a of the back surface inner periphery (FIG. 4).

[0028] Assuming that the value of D3-D1 is 0 to 10 mm, one embodiment of the film-shaped sintered material with support sheet is as follows: the film-shaped sintered material with support sheet comprises a support sheet having an adhesive layer on a base film, and a film-shaped sintered material provided on the adhesive layer, wherein the diameter D1 of the film-shaped sintered material is 130 to 146 mm, 180 to 196 mm, 280 to 296 mm, or 430 to 446 mm. The film-shaped sintering material with support sheet can be suitably used for attaching the film-shaped sintering material to the inner periphery of the back surface of a wafer having an annular protrusion on the outer periphery.

[0029] 4, the adhesive layer 4 (see FIG. 1) of the support sheet 2 is preferably attached to the outer periphery 16a of the inner periphery of the back surface of the wafer 18. This covers the film-shaped sintered material 1 with the adhesive layer 4, and the film-shaped sintered material 1 and the wafer 18 are fixed by the adhesive layer 4, and in the step of cutting the annular convex portion in the manufacturing method of the device described later, the support sheet 2 plays a role in reinforcing the periphery of the outer periphery 16a of the inner periphery of the back surface of the portion to be cut, thereby more effectively preventing damage to the wafer. To achieve this configuration, the diameter D1 of the film-shaped sintered material 1 is preferably less than the diameter D3 of the inner periphery 16 of the back surface of the wafer. The diameter of the adhesive layer 4 is preferably greater than the diameter D1 of the film-shaped sintered material 1. When the size of the adhesive layer 4 matches the size of the support sheet 2, the diameter D2 of the support sheet 2 is preferably greater than the diameter D1 of the film-shaped sintered material 1.

[0030] 4, the adhesive layer 4 (see FIG. 1) of the support sheet 2 is preferably attached to the inner surface 12 of the annular convex portion of the wafer 18. This covers the film-shaped sintered material 1 with the adhesive layer 4, and the film-shaped sintered material 1 and the wafer 18 are fixed by the adhesive layer 4, and in the step of cutting the annular convex portion in the manufacturing method of the device described later, the support sheet 2 plays a role in reinforcing the outer peripheral portion 16a of the inner peripheral portion of the back surface of the portion to be cut and the periphery of the inner surface 12 of the annular convex portion, thereby more effectively preventing damage to the wafer. To achieve this configuration, the diameter of the adhesive layer 4 is preferably larger than the diameter D1 of the film-shaped sintered material 1, and more preferably larger than the diameter D3 of the back surface inner periphery 16. When the size of the adhesive layer 4 matches the size of the support sheet 2, the diameter D2 of the support sheet 2 is preferably larger than the diameter D1 of the film-shaped sintered material 1, and more preferably larger than the diameter D3 of the back surface inner periphery 16.

[0031] That is, when the film-shaped sintered material 1 is attached to the inner periphery 16 of the back surface of the wafer 18, it is preferable that the adhesive layer 4 contacts at least a part of the outer periphery 16a of the inner periphery of the back surface of the wafer 18, and it is more preferable that the adhesive layer 4 contacts at least a part of the inner surface 12 of the wafer 18. The value of the diameter of the support sheet 2 - the diameter of the film-shaped sintered material 1 (D2-D1) may be, for example, 35 mm or more, or 50 mm or more.

[0032] The diameter D2 of the support sheet 2 is preferably larger than the diameter D4 of the wafer 18. The film-shaped sintered material 100 with support sheet attached to the wafer 18 has an adhesive portion where the adhesive layer 4 is exposed on the outer periphery of the support sheet 2. The adhesive portion on the outer periphery is used to fix the ring frame 5 as shown in the figure. The value of the diameter of the support sheet 2 minus the diameter of the wafer 18 (D2-D4) may be, for example, 30 mm or more, 50 mm or more, or 60 mm or more. The upper limit of the value of D2-D4 can be appropriately determined taking into account the size of the ring frame, and the value of D2-D4 may be, for example, 550 mm or less, 30 to 200 mm, 50 to 150 mm, or 60 to 100 mm.

[0033] A ring-shaped double-sided tape or adhesive layer may be provided separately on the margin for the ring frame (the adhesive layer exposed at the outer periphery of the adhesive sheet). The double-sided tape has a structure of adhesive layer / core material / adhesive layer, and the adhesive layer in the double-sided tape is not particularly limited, and adhesives such as rubber-based resin, acrylic resin, silicone resin, polyvinyl ether, etc. are used. The adhesive layer is attached to the ring frame at its outer periphery when manufacturing the chip-attached substrate described later. As the core material of the double-sided tape, for example, polyester film, polypropylene film, polycarbonate film, polyimide film, fluororesin film, liquid crystal polymer film, etc. are preferably used.

[0034] To summarize the configuration related to the size of each of the above-mentioned parts, it is preferable to satisfy the relationship: diameter D1 of film-shaped sintered material 1≦ diameter D3 of inner circumference 16 of the back surface< diameter D4 of wafer 18< diameter D2 of support sheet 2, and it is more preferable to satisfy the relationship: diameter D1 of film-shaped sintered material 1< diameter D3 of inner circumference 16 of the back surface< diameter D4 of wafer 18< diameter D2 of support sheet 2.

[0035] In the configuration shown in FIG. 4, a metal film 18a (also called a back electrode) is provided on the back inner periphery 16 of the wafer 18. The film-shaped sintered material with support sheet of the embodiment is suitable for application to the wafer 18 having the metal film 18a provided on the back inner periphery 16. The metal film 18a may be provided to enhance electrical and thermal conductivity. In order to protect the wafer, it is possible to increase the thickness of the wafer by additionally attaching, for example, a backgrind tape to the circuit formation surface side. However, when the metal film 18a is provided, sputtering decompression may be used, and if a backgrind tape or the like is attached at this time, there is a concern that the performance of the metal film 18a may be reduced due to the adhesion of organic matter derived from the backgrind tape. Thus, the wafer 18 provided with the metal film 18a is not sufficiently protected, and there is a high risk of it being damaged during processing or transportation. Therefore, by using the film-shaped sintered material with support sheet of the embodiment and attaching it to the wafer 18 provided with the metal film 18a, there are advantages in that it is possible to protect the wafer, function as a dicing tape, and form a sintered body with excellent heat dissipation function via the metal film 18a.

[0036] The metal film 18a can be made of a metal such as gold, silver, copper, titanium, nickel, or cobalt. Methods for forming the metal film include deposition of these metals by PVD (physical vapor deposition) methods such as vacuum deposition, sputtering, and ion plating, as well as electrolytic plating and electroless plating.

[0037] The total thickness T1 of the annular protrusion 17 (see FIG. 4) is not particularly limited as long as it provides the necessary rigidity to the wafer and does not impair the handleability, and is generally about 400 to 780 μm, or 400 to 725 μm. The thickness T2 of the backside inner periphery 16 depends on the device design, and is usually about 25 to 200 μm, or may be 25 to 100 μm. Therefore, the step T3 (= T1 - T2) between the backside inner periphery 16 and the annular protrusion 17 is about 200 to 755 μm.

[0038] The thickness of the film-shaped sintered material before sintering is preferably smaller than the step T3. This allows the adhesive layer 4 of the support sheet 2 to be attached to the inner surface 12 of the annular convex when the film-shaped sintered material with the support sheet is attached to the wafer 18, and in the step of cutting the annular convex in the manufacturing method of the device described later, the support sheet 2 plays a role in reinforcing the outer periphery 16a of the inner periphery of the back surface of the part to be cut and the periphery of the inner surface 12 of the annular convex, thereby more effectively preventing damage to the wafer. Considering that the step T3 (=T1-T2) is about 200 to 755 μm, the thickness of the film-shaped fired material before firing may be less than 200 μm, may be 200 μm or less, may be 10 μm or more and less than 200 μm, may be 10 to 200 μm, may be 20 to 150 μm, or may be 30 to 90 μm. In the manufactured product, by setting the thickness of the film-shaped sintered material before sintering to the above lower limit or more, peeling is unlikely to occur between the chip and the substrate, and the reliability of the package can be further improved. By setting the thickness of the film-shaped sintered material before sintering to the above upper limit or less, chip vibration is suppressed, and the reliability of the package can be further improved.

[0039] Here, "thickness of the film-shaped sintered material" means the thickness of the entire film-shaped sintered material; for example, the thickness of a film-shaped sintered material consisting of multiple layers means the total thickness of all layers that make up the film-shaped sintered material.

[0040] In this specification, the "thickness" is a value expressed as an average value of thicknesses measured at any five points, and can be obtained using a constant pressure thickness measuring device in accordance with JIS K7130.

[0041] In the film-shaped sintered material with support sheet of this embodiment, a release film may be provided on either or both of the surfaces of the film-shaped sintered material and the adhesive portion for the purpose of surface protection to prevent contact with the outside until use.

[0042] The surface protection film (release film) can also be obtained by subjecting the surface of a substrate film such as polyethylene, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, or polypropylene, which will be described later, to a release treatment using a release agent. Examples of the release agent used in the release treatment include the release agents exemplified in the description of the substrate film.

[0043] The thickness of the film-shaped sintered material with a support sheet is preferably 40 to 500 μm, more preferably 50 to 300 μm, and even more preferably 60 to 200 μm.

[0044] Here, the "thickness of the film-shaped fired material with a support sheet" means the overall thickness of the film-shaped fired material with a support sheet, and refers to the total thickness of all layers that make up the film-shaped fired material with a support sheet.

[0045] <Film-shaped firing material> As shown in FIG. 1, the film-shaped sintered material 1 contains sinterable metal particles 10 and a binder component 20.

[0046] The film-shaped sintered material may be one layer (single layer) or two or more layers. When the film-shaped sintered material is made up of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited as long as it does not impair the effects of the present invention. In this specification, not only in the case of a film-shaped fired material, "multiple layers may be the same or different" means "all layers may be the same, all layers may be different, or only some layers may be the same", and further, "multiple layers are different" means "at least one of the constituent materials, the composition ratio of the constituent materials, and the thickness of each layer is different".

[0047] (Release film) The film-shaped sintered material can be provided with a release film laminated thereon. When using, the release film is peeled off and the film-shaped sintered material is placed on the object to be sintered and bonded. The release film also functions as a protective film to prevent damage to the film-shaped sintered material and adhesion of dirt. The release film may be provided on at least one side of the film-shaped sintered material.

[0048] Examples of the release film include transparent films such as polyethylene films, polypropylene films, polybutene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polyethylene naphthalate films, polybutylene terephthalate films, polyurethane films, ethylene vinyl acetate copolymer films, ionomer resin films, ethylene-(meth)acrylic acid copolymer films, ethylene-(meth)acrylic acid ester copolymer films, polystyrene films, polycarbonate films, polyimide films, and fluororesin films. Crosslinked films of these films are also used. Furthermore, laminated films of these films may be used. Furthermore, colored films and opaque films of these films may be used. Examples of the release agent include silicone-based, fluorine-based, olefin-based, alkyd-based, and long-chain alkyl group-containing carbamates.

[0049] The thickness of the release film is usually about 10 to 500 μm, preferably about 15 to 300 μm, and particularly preferably about 20 to 250 μm.

[0050] (Sinterable metal particles) Sinterable metal particles are metal particles that can be fused and bonded together to form a sintered body by heat treatment at a temperature equal to or higher than the melting point of the metal particles as the sintering of the film-shaped sintered material. By forming a sintered body, it is possible to sinter-bond the film-shaped sintered material and an article that is sintered in contact with it. Specifically, it is possible to sinter-bond a chip and a substrate via the film-shaped sintered material.

[0051] The constituent materials of the sinterable metal particles include simple metals, barium titanate, oxides and alloys of the simple metals. The simple metals include silver, gold, copper, iron, nickel, aluminum, silicon, palladium, platinum, titanium, etc. The constituent materials of the sinterable metal particles are preferably silver and silver oxide. The sinterable metal particles may be mixed in one type or in a combination of two or more types.

[0052] The sinterable metal particles are preferably silver nanoparticles, which are nano-sized silver particles.

[0053] The particle size of the sinterable metal particles contained in the film-shaped sintered material is not particularly limited as long as it can exhibit the above sinterability, but may be 100 nm or less, 50 nm or less, or 30 nm or less. The particle size of the metal particles contained in the film-shaped sintered material is the diameter of the projected area circle equivalent of the particle size of the metal particles observed with an electron microscope. Metal particles falling within the above particle size range are preferable because they have excellent sinterability. The particle size of the sinterable metal particles contained in the film-shaped sintered material may be 0.1 to 95 nm, 0.3 to 50 nm, or 0.5 to 30 nm, as determined by observing the particle size of the metal particles with a projected area circle equivalent diameter of 100 nm or less under an electron microscope. The number of metal particles to be measured is 100 or more randomly selected per film-shaped sintered material.

[0054] Before mixing with the binder component and other additive components, the sinterable metal particles may be dispersed in a high-boiling point solvent such as isobornylcyclohexanol or decyl alcohol in advance to make the particles free of agglomerates. The boiling point of the high-boiling point solvent may be, for example, 200 to 350°C. In this case, if a high-boiling point solvent is used, the sinterable metal particles are prevented from becoming concentrated because the solvent hardly volatilizes at room temperature, improving workability and preventing re-agglomeration of the sinterable metal particles, resulting in good quality. Examples of dispersion methods include a kneader, a triple roll mill, a bead mill, and ultrasonic waves.

[0055] In addition to metal particles (sinterable metal particles) having a particle diameter of 100 nm or less, the film-shaped fired material may further contain non-sinterable metal particles having a particle diameter exceeding 100 nm that do not fall under the above. The particle diameter of the non-sinterable metal particles having a particle diameter exceeding 100 nm may be a number average particle diameter of more than 150 nm and not more than 50,000 nm, 150 to 10,000 nm, or 180 to 5,000 nm, calculated by measuring the particle diameter of the metal particles observed by an electron microscope and the projected area circle equivalent diameter of the particles exceeding 100 nm.

[0056] Examples of the metal species of the non-sinterable metal particles having a particle size of more than 100 nm include the same metal species as those exemplified above for the sinterable metal particles, and silver, copper, and oxides thereof are preferred. The metal particles having a particle size of 100 nm or less and the non-sintered metal particles having a particle size of more than 100 nm may be the same metal type or different metal types. For example, the metal particles having a particle size of 100 nm or less may be silver particles, and the non-sintered metal particles having a particle size of more than 100 nm may be silver or silver oxide particles. For example, the metal particles having a particle size of 100 nm or less may be silver or silver oxide particles, and the non-sintered metal particles having a particle size of more than 100 nm may be copper or copper oxide particles.

[0057] In the film-shaped sintered material, the content of the sinterable metal particles relative to the total mass (100 mass%) of all the metal particles may be 10 to 100 mass%, or may be 20 to 95 mass%.

[0058] The surfaces of the sinterable metal particles and / or the non-sinterable metal particles may be coated with an organic material. By having an organic coating, the compatibility with the binder component is improved, the aggregation of the particles can be prevented, and the particles can be dispersed uniformly. When the surfaces of the sinterable metal particles and / or the non-sinterable metal particles are coated with an organic substance, the mass of the sinterable metal particles and the non-sinterable metal particles includes the coating.

[0059] (Binder component) By adding the binder component, the fired material can be formed into a film shape and the film-shaped fired material before firing can be given adhesiveness. The binder component may be pyrolytic, which is pyrolyzed by heat treatment in firing the film-shaped fired material. The binder component is not particularly limited, but a suitable example of the binder component is a resin. Examples of the resin include acrylic resin, polycarbonate resin, polylactic acid, and polymers of cellulose derivatives, and acrylic resin is preferred. The acrylic resin includes a homopolymer of a (meth)acrylate compound, a copolymer of two or more kinds of (meth)acrylate compounds, and a copolymer of a (meth)acrylate compound and another copolymerizable monomer.

[0060] In this specification, the term "derivative" refers to a compound in which one or more hydrogen atoms of the original compound have been replaced with a group (substituent) other than a hydrogen atom.

[0061] In the resin constituting the binder component, the content of the structural unit derived from the (meth)acrylate compound is preferably 50 to 100 mass%, more preferably 80 to 100 mass%, and further preferably 90 to 100 mass%, relative to the total mass (100 mass%) of the structural units. "Derived from" in this context means that the monomer has undergone the structural changes necessary to be polymerized.

[0062] Specific examples of the (meth)acrylate compound include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, and octyl (meth)acrylate, alkyl (meth)acrylates such as isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, and isostearyl (meth)acrylate; hydroxyalkyl (meth)acrylates such as hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 3-hydroxybutyl (meth)acrylate; phenoxyalkyl (meth)acrylates such as phenoxyethyl (meth)acrylate and 2-hydroxy-3-phenoxypropyl (meth)acrylate; Alkoxyalkyl (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-propoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, and 2-methoxybutyl (meth)acrylate; Polyalkylene glycol (meth)acrylates such as polyethylene glycol mono(meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, nonylphenoxypolyethylene glycol (meth)acrylate, polypropylene glycol mono(meth)acrylate, methoxypolypropylene glycol (meth)acrylate, ethoxypolypropylene glycol (meth)acrylate, and nonylphenoxypolypropylene glycol (meth)acrylate; cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate, 4-butylcyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentadienyl (meth)acrylate, bornyl (meth)acrylate, isobornyl (meth)acrylate, and tricyclodecanyl (meth)acrylate; Examples of the (meth)acrylate compound include benzyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, etc. Alkyl (meth)acrylate or alkoxyalkyl (meth)acrylate is preferred, and particularly preferred (meth)acrylate compounds include butyl (meth)acrylate, ethylhexyl (meth)acrylate, lauryl (meth)acrylate, isodecyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and 2-ethoxyethyl (meth)acrylate.

[0063] In this specification, the term "(meth)acrylate" is a concept that encompasses both "acrylate" and "methacrylate". The acrylic resin is preferably a methacrylate. When the binder component contains a structural unit derived from a methacrylate, the binder can be fired at a relatively low temperature, and the condition for obtaining sufficient adhesive strength after sintering can be easily satisfied.

[0064] In the resin constituting the binder component, the content of the methacrylate-derived structural unit relative to the total mass (100 mass%) of the structural units is preferably 50 to 100 mass%, more preferably 80 to 100 mass%, and even more preferably 90 to 100 mass%.

[0065] The other copolymerizable monomer is not particularly limited as long as it is a compound copolymerizable with the above-mentioned (meth)acrylate compound, and examples thereof include unsaturated carboxylic acids such as (meth)acrylic acid, vinyl benzoic acid, maleic acid, and vinyl phthalic acid; and vinyl group-containing radical polymerizable compounds such as vinyl benzyl methyl ether, vinyl glycidyl ether, styrene, α-methylstyrene, butadiene, and isoprene.

[0066] The mass average molecular weight (Mw) of the resin constituting the binder component is preferably 1,000 to 1,000,000, and more preferably 10,000 to 800,000. When the mass average molecular weight of the resin is within the above range, the film exhibits sufficient film strength and can easily be imparted with flexibility. In this specification, unless otherwise specified, the "mass average molecular weight" is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0067] The glass transition temperature (Tg) of the resin constituting the binder component can be calculated using the Fox formula shown below, and is preferably -60 to 50°C, more preferably -30 to 10°C, and even more preferably -20°C or more and less than 0°C. When the Tg of the resin calculated from the Fox formula is equal to or less than the upper limit, the adhesive strength between the film-shaped sintered material and the adherend (e.g., chip, substrate, etc.) before sintering is improved. In addition, the flexibility of the film-shaped sintered material is increased. On the other hand, when the Tg of the resin calculated from the Fox formula is equal to or more than the lower limit, the film shape can be maintained, and the film-shaped sintered material can be more easily separated from the support sheet, etc. 1 / Tg=(W1 / Tg1)+(W2 / Tg2)+...+(Wm / Tgm) (wherein Tg is the glass transition temperature of the resin constituting the binder component, Tg1, Tg2,...Tgm are the glass transition temperatures of the homopolymers of the monomers that are the raw materials of the resin constituting the binder component, and W1, W2,...Wm are the mass fractions of the monomers. However, W1+W2+...+Wm=1.) As the glass transition temperature of the homopolymer of each monomer in the Fox formula, the value described in the Polymer Data Handbook or the Adhesive Handbook can be used.

[0068] The binder component may be pyrolytic, that is, pyrolyzed by heat treatment as firing of the film-shaped fired material. The pyrolysis of the binder component can be confirmed by the mass reduction of the binder component by firing. The components blended as the binder component may be almost pyrolyzed by firing, but the total mass of the components blended as the binder component may not be pyrolyzed by firing. The binder component may be one whose mass after firing is 10% by mass or less, 5% by mass or less, or 3% by mass or less, relative to the total mass (100% by mass) of the binder components before firing.

[0069] In addition to the above-mentioned sinterable metal particles, non-sinterable metal particles, and binder components, the film-shaped sintered material may contain other additives that do not fall under the category of sinterable metal particles, non-sinterable metal particles, and binder components, within a range that does not impair the effects of the present invention.

[0070] Other additives that may be contained in the film-shaped sintered material include solvents, dispersants, plasticizers, tackifiers, storage stabilizers, antifoamers, thermal decomposition promoters, and antioxidants. Only one type of additive may be contained, or two or more types may be contained. These additives are not particularly limited, and can be appropriately selected from those commonly used in this field.

[0071] Since the binder component is preferably thermally decomposed by heat treatment in the firing of the film-shaped fired material, the content of thermosetting resin such as epoxy resin is preferably 10 mass% or less, more preferably 5 mass% or less, relative to 100 mass% of the binder component, and even more preferably contains substantially no thermosetting resin. From a similar viewpoint, in the resin constituting the binder component, the content of acrylate-derived structural units, out of "acrylate" and "methacrylate", relative to the total mass (100 mass%) of the structural units is preferably 10 mass% or less, more preferably 5 mass% or less, and even more preferably it does not substantially contain any acrylate-derived structural units.

[0072] <Composition> The film-shaped sintered material may be composed of sinterable metal particles, a binder component, and other additives, and the sum of their contents (mass%) may be 100 mass%. When the film-shaped sintered material contains non-sinterable metal particles, the film-shaped sintered material may be composed of sinterable metal particles, non-sinterable metal particles, a binder component, and other additives, and the sum of their contents (mass%) may be 100 mass%.

[0073] In the film-shaped fired material, the content of the sinterable metal particles relative to the total mass (100 mass%) of all components other than the solvent (hereinafter referred to as "solid content") is preferably 15 to 98 mass%, more preferably 15 to 90 mass%, and even more preferably 20 to 80 mass%. When the content of the sinterable metal particles is equal to or less than the above upper limit, the content of the binder component can be sufficiently ensured, making it easy to maintain the film shape. On the other hand, when the content of the sinterable metal particles is equal to or more than the above lower limit, the sinterable metal particles are fused to each other or to the non-sinterable metal particles during firing, and the effect of exhibiting high bonding adhesive strength (shear adhesive strength) after firing is obtained.

[0074] When the film-shaped sintered material contains non-sinterable metal particles, the total content of the sinterable metal particles and non-sinterable metal particles relative to the total mass (100 mass%) of the solid contents in the film-shaped sintered material is preferably 50 to 98 mass%, more preferably 70 to 95 mass%, and even more preferably 80 to 95 mass%.

[0075] The content of the binder component relative to the total mass (100 mass%) of the solid content in the film-shaped sintered material is preferably 2 to 50 mass%, more preferably 5 to 30 mass%, and even more preferably 5 to 20 mass%. By making the content of the binder component equal to or less than the upper limit, the content of the sinterable metal particles can be sufficiently ensured, and the bonding adhesive strength between the film-shaped sintered material and the adherend is further improved. On the other hand, by making the content of the binder component equal to or more than the lower limit, the film shape can be easily maintained.

[0076] In the film-shaped sintered material, the mass ratio of the sinterable metal particles to the binder component (sinterable metal particles:binder component) is preferably 50:1 to 1:5, more preferably 20:1 to 1:2, and even more preferably 10:1 to 1:1. When the film-shaped sintered material contains non-sinterable metal particles, the mass ratio of the sinterable metal particles and non-sinterable metal particles to the binder component ((sinterable metal particles + non-sinterable metal particles):binder component) is preferably 50:1 to 1:1, more preferably 20:1 to 2:1, and even more preferably 9:1 to 4:1.

[0077] The film-shaped sintered material may contain a high-boiling point solvent used when mixing the sinterable metal particles, non-sinterable metal particles, binder components, and other additive components. The content of the high-boiling point solvent relative to the total mass (100 mass%) of the film-shaped sintered material is preferably 20 mass% or less, more preferably 15 mass% or less, and even more preferably 10 mass% or less.

[0078] [Manufacturing method of film-shaped fired material] The film-shaped sintered material can be formed using a sintered material composition containing its constituent materials. For example, a sintered material composition containing each component and a solvent for constituting the film-shaped sintered material is coated or printed on the target surface of the film-shaped sintered material, and the solvent is evaporated as necessary to form the film-shaped sintered material at the desired location. The surface on which the film-shaped fired material is formed can be the surface of a release film.

[0079] When applying the fired material composition, the solvent preferably has a boiling point of less than 200° C., such as n-hexane (boiling point: 68° C.), ethyl acetate (boiling point: 77° C.), 2-butanone (boiling point: 80° C.), n-heptane (boiling point: 98° C.), methylcyclohexane (boiling point: 101° C.), toluene (boiling point: 111° C.), acetylacetone (boiling point: 138° C.), n-xylene (boiling point: 139° C.), and dimethylformamide (boiling point: 153° C.). These may be used alone or in combination.

[0080] The firing material composition may be applied by a known method, for example, a method using various coaters such as an air knife coater, a blade coater, a bar coater, a gravure coater, a Comma Coater (registered trademark), a roll coater, a roll knife coater, a curtain coater, a die coater, a knife coater, a screen coater, a Mayer bar coater, or a kiss coater.

[0081] When printing the sintered material composition, the solvent may be one that can be evaporated and dried after printing, and preferably has a boiling point of 65 to 350° C. Examples of such solvents include the above-mentioned solvents with a boiling point of less than 200° C., as well as isophorone (boiling point: 215° C.), butyl carbitol (boiling point: 230° C.), 1-decanol (boiling point: 233° C.), butyl carbitol acetate (boiling point: 247° C.), and isobornyl cyclohexanol (boiling point: 318° C.). If the boiling point exceeds 350°C, the solvent will not volatilize easily during drying after printing, making it difficult to obtain the desired shape, or the solvent may remain in the film during baking, causing deterioration of bonding and adhesion. If the boiling point is below 65°C, the solvent will volatilize during printing, which may cause the thickness stability to be impaired. If a solvent with a boiling point of 200 to 350°C is used, the viscosity increase due to the evaporation of the solvent during printing can be suppressed, and printing suitability can be obtained.

[0082] The printing of the sintered material composition can be carried out by a known printing method, for example, letterpress printing such as flexographic printing, intaglio printing such as gravure printing, lithographic printing such as offset printing, screen printing such as silk screen printing and rotary screen printing, and printing with various printers such as inkjet printers.

[0083] The shape of the film-shaped sintered material may be appropriately set according to the shape of the object of sintering and bonding, and is preferably circular, approximately circular, or rectangular. A circular or approximately circular shape corresponds to the shape of a semiconductor wafer. A rectangular shape corresponds to the shape of a chip. The corresponding shape may be the same or approximately the same as the shape of the object of sintering and bonding. In particular, by printing the sintered material composition, a film-like sintered material having a desired shape can be easily formed.

[0084] The drying conditions for the sintered material composition are not particularly limited. When the sintered material composition contains a solvent, it is preferable to dry it by heating. In this case, it is preferable to dry it under conditions of, for example, 70 to 250°C, e.g., 80 to 180°C, for 10 seconds to 10 minutes.

[0085] <Support sheet> In the film-shaped sintered material with support sheet of this embodiment, the load of the support sheet at 5% elongation measured by the following measurement method is preferably 13N / 15mm or less, more preferably 10N / 15mm or less, and even more preferably 9N / 15mm or less. The inventors have found that in a film-shaped sintered material with support sheet in which the load of the support sheet at 5% elongation is equal to or less than the upper limit, damage to the wafer is more effectively prevented in the step of cutting the annular convex portion in the manufacturing method of the device described below. This is thought to be because, when the load of the support sheet at 5% elongation is equal to or less than the upper limit, the support sheet is more firmly attached toward the boundary between the inner surface 12 of the annular convex portion and the inner periphery 16 of the back surface, resulting in an excellent effect of preventing damage to the wafer.

[0086] The lower limit of the load at 5% elongation of the support sheet is, for example, preferably 2 N / 15 mm or more, more preferably 3 N / 15 mm or more, and even more preferably 4 N / 15 mm or more. When the load at 5% elongation is equal to or more than the lower limit, the reinforcing effect of the wafer is preferably exhibited in the step of cutting the annular convex portion and the step of dicing in the manufacturing method of the device described later, and damage to the wafer can be prevented more effectively. An example of the range of the load at 5% elongation of the support sheet may be 2N / 15mm to 13N / 15mm, 3N / 15mm to 10N / 15mm, or 4N / 15mm to 9N / 15mm.

[0087] The load at 5% elongation is determined in accordance with JIS K7161 1994, and specifically, can be measured by the following method. Measurement method: The support sheet is cut into a test piece having a width of 15 mm and a length of 150 mm (however, if the adhesive layer is curable, the test piece is used before curing). The test piece is pulled under conditions of a 23°C, 50% RH environment, a chuck distance of 100 mm, and a tensile speed of 200 mm / min, and the load relative to the amount of displacement when the test piece is elongated by 5% is measured.

[0088] The thickness of the support sheet is preferably 120 μm or less, more preferably 35 to 120 μm, and more preferably 50 to 110 μm. When the thickness of the support sheet is equal to or less than the upper limit, the support sheet is firmly attached toward the boundary between the inner surface 12 of the annular convex portion and the inner periphery 16 of the back surface, and is considered to be excellent in preventing damage to the wafer. When the thickness of the support sheet is equal to or more than the lower limit, the reinforcing effect of the wafer is preferably exerted in the process of cutting the annular convex portion and the process of dicing in the manufacturing method of the device described later, and damage to the wafer can be prevented more effectively. Here, "thickness of the support sheet" means the thickness of the entire support sheet. For example, the thickness of a support sheet consisting of multiple layers means the total thickness of all layers that make up the support sheet.

[0089] In the film-shaped sintered material with support sheet of this embodiment, the support sheet preferably has an absorbance of 0.22 or less at the light wavelength of the laser irradiation, more preferably 0 to 0.2, and even more preferably 0 to 0.18. The support sheet having the above configuration can prevent the support sheet from being broken when laser processing is performed in the step of cutting the annular convex portion or the step of dicing in the manufacturing method of the device described later. In the process of cutting the annular convex portion and the process of dicing in the manufacturing method of the device described later, processing is often performed with a laser having a wavelength of 355 nm. The support sheet preferably has an absorbance at a wavelength of 355 nm of 0.22 or less, more preferably 0 to 0.2, and even more preferably 0 to 0.18.

[0090] (Base film) The base film 3 of the support sheet 2 is not particularly limited, and examples thereof include films made of low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), ethylene-propylene copolymer, polypropylene, polybutene, polybutadiene, polymethylpentene, ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-methyl (meth)acrylate copolymer, ethylene-ethyl (meth)acrylate copolymer, polyvinyl chloride, vinyl chloride-vinyl acetate copolymer, polyurethane film, ionomer, etc. In this specification, "(meth)acrylic" is used to mean both acrylic and methacrylic. Furthermore, when higher heat resistance is required for the support sheet, examples of the base film 3 include polyester films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, and polyolefin films such as polypropylene and polymethylpentene. Crosslinked films of these films and films modified by radiation, discharge, etc. can also be used. The base film may be a laminate of the above films.

[0091] These films may be laminated or combined. Furthermore, these films may be colored or printed. The film may be a sheet made by extrusion molding of a thermoplastic resin, or may be a stretched film, or a sheet made by thinning and curing a curable resin by a predetermined means may be used.

[0092] The thickness of the base film is not particularly limited, and is preferably 30 to 300 μm, more preferably 50 to 200 μm. By setting the thickness of the base film within the above range, the base film is less likely to break even when cut by dicing. In addition, the film-shaped sintered material with support sheet is given sufficient flexibility, so that it shows good attachment to the work (e.g., semiconductor wafer, etc.).

[0093] The substrate film can also be obtained by applying a release agent to the surface and carrying out a release treatment. Examples of the release agent used in the release treatment include alkyd-based, silicone-based, fluorine-based, unsaturated polyester-based, polyolefin-based, and wax-based release agents, and the alkyd-based, silicone-based, and fluorine-based release agents are particularly preferred because of their heat resistance.

[0094] In order to perform a release treatment on the surface of a base film using the above-mentioned release agent, the release agent may be applied as is without a solvent or after dilution with a solvent or emulsification using a gravure coater, a Mayer bar coater, an air knife coater, a roll coater or the like, and the base film to which the release agent has been applied may be subjected to curing at room temperature or under heating, or may be cured with an electron beam, or a laminate may be formed by wet lamination, dry lamination, hot melt lamination, melt extrusion lamination, coextrusion processing or the like.

[0095] (Adhesive layer) The pressure-sensitive adhesive layer 4 is in the form of a sheet or film, and can contain a pressure-sensitive adhesive. The support sheet 2 has an adhesive part at least on its outer periphery. The adhesive part has a function of temporarily fixing the ring frame 5 on the outer periphery of the film-like sintered material 100 with the support sheet, and it is preferable that the ring frame 5 is peelable after the required process. Therefore, the adhesive layer 4 may be weakly adhesive, or may be energy ray curable, the adhesive strength of which decreases when irradiated with energy rays. The adhesive layer may be energy ray curable or non-energy ray curable. The removable adhesive layer can be formed from various known adhesives (for example, general-purpose adhesives such as rubber-based resins, acrylic resins, silicone resins, urethane resins, and polyvinyl ethers, adhesives with uneven surfaces, energy ray curable adhesives, adhesives containing thermal expansion components, etc.).

[0096] In this specification, the term "energy ray" refers to electromagnetic waves or charged particle beams that have an energy quantum, and examples of such beams include ultraviolet rays, radioactive rays, and electron beams. The ultraviolet light can be irradiated by using, for example, a high-pressure mercury lamp, a fusion lamp, a xenon lamp, a black light, an LED lamp, etc. as an ultraviolet light source. The electron beam can be generated by an electron beam accelerator or the like. In this specification, "energy ray curable" means a property that is cured by irradiation with energy rays, and "non-energy ray curable" means a property that is not cured even when irradiated with energy rays.

[0097] As shown in Fig. 1, the support sheet 2 may have a pressure-sensitive adhesive layer 4 on the entire upper surface of the base film 3, the inner peripheral surface of the pressure-sensitive adhesive layer 4 being covered with a film-like sintered material, and the adhesive portion being exposed on the outer peripheral portion. In this case, the outer peripheral portion of the pressure-sensitive adhesive layer 4 is used to fix the ring frame 5 described above, and the film-like sintered material is peelably laminated on the inner peripheral portion. As the pressure-sensitive adhesive layer 4, a weakly adhesive one may be used as described above, or an energy ray-curable pressure-sensitive adhesive may be used.

[0098] As the weakly adhesive agent, an acrylic resin or a silicone resin is preferably used.

[0099] In the support sheet having the configuration of FIG. 1, when an energy ray-curable re-peelable adhesive layer is used, the area where the film-like sintered material is laminated may be irradiated with energy rays in advance to reduce the adhesiveness. In this case, the other areas may not be irradiated with energy rays, and the adhesive strength may be maintained high, for example, for the purpose of adhesion to the ring frame 5. In order to avoid irradiating only the other areas with energy rays, for example, an energy ray shielding layer may be provided by printing or the like in the area corresponding to the other areas of the base film, and energy rays may be irradiated from the base film side. In addition, in the support sheet having the configuration of FIG. 1, in order to strengthen the adhesion between the base film 3 and the adhesive layer 4, the surface of the base film 3 on which the adhesive layer 4 is provided may be subjected to a roughening treatment such as sandblasting or solvent treatment, or an oxidation treatment such as corona discharge treatment, electron beam irradiation, plasma treatment, ozone / ultraviolet irradiation treatment, flame treatment, chromate treatment, and hot air treatment, if desired. A primer treatment may also be applied.

[0100] The thickness of the pressure-sensitive adhesive layer is not particularly limited, but is preferably 1 to 100 μm, more preferably 2 to 80 μm, and particularly preferably 3 to 50 μm.

[0101] The adhesive layer may be one layer (single layer) or two or more layers. When the adhesive layer is made up of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited as long as it does not impair the effects of the present invention.

[0102] <Adhesive composition> The adhesive layer can be formed using an adhesive composition containing an adhesive. For example, the adhesive composition is applied to the surface on which the adhesive layer is to be formed, and dried as necessary to form the adhesive layer at the desired location. A more specific method for forming the adhesive layer will be described in detail later, together with the method for forming other layers. The ratio of the contents of the components that do not vaporize at room temperature in the adhesive composition is usually the same as the ratio of the contents of the components in the adhesive layer.

[0103] The pressure-sensitive adhesive composition may be applied by a known method, for example, a method using various coaters such as an air knife coater, a blade coater, a bar coater, a gravure coater, a roll coater, a roll knife coater, a curtain coater, a die coater, a knife coater, a screen coater, a Mayer bar coater, or a kiss coater.

[0104] The drying conditions for the pressure-sensitive adhesive composition are not particularly limited, but when the pressure-sensitive adhesive composition contains a solvent described below, it is preferable to heat-dry the pressure-sensitive adhesive composition. The pressure-sensitive adhesive composition containing the solvent is preferably dried, for example, at 70 to 130° C. for 10 seconds to 5 minutes.

[0105] When the pressure-sensitive adhesive layer is energy ray-curable, the pressure-sensitive adhesive composition containing an energy ray-curable pressure-sensitive adhesive, i.e., the energy ray-curable pressure-sensitive adhesive composition, can be, for example, A pressure-sensitive adhesive composition (I-1) containing a non-energy ray-curable pressure-sensitive adhesive resin (I-1a) (hereinafter sometimes abbreviated as "pressure-sensitive adhesive resin (I-1a)") and an energy ray-curable compound; a pressure-sensitive adhesive composition (I-2) containing an energy ray-curable pressure-sensitive adhesive resin (I-2a) (hereinafter sometimes abbreviated as "pressure-sensitive adhesive resin (I-2a)") in which an unsaturated group has been introduced into the side chain of a non-energy ray-curable pressure-sensitive adhesive resin (I-1a); An example of the adhesive composition is an adhesive composition (I-3) containing the adhesive resin (I-2a) and an energy ray-curable compound.

[0106] When the pressure-sensitive adhesive layer 4 is non-energy ray-curable, examples of the non-energy ray-curable pressure-sensitive adhesive composition include the pressure-sensitive adhesive composition (I-4) containing the pressure-sensitive adhesive resin (I-1a).

[0107] In this specification, the term "adhesive resin" is a concept that includes both a resin having adhesive properties and a resin having adhesive properties, and includes, for example, not only resins that are adhesive in themselves, but also resins that exhibit adhesive properties when used in combination with other components such as additives, and resins that exhibit adhesive properties in the presence of a trigger such as heat or water.

[0108] Among the above-mentioned adhesive compositions, adhesive composition (I-2) or adhesive composition (I-4) is preferred. By using adhesive composition (I-2) or adhesive composition (I-4), the adhesive force at the interface between the adhesive layer and the film-shaped sintered material is reduced, and the diced chip with the film-shaped sintered material can be picked up more stably.

[0109] Although the adhesive composition (I-1) may be used, as described above, it is more preferable to use the adhesive composition (I-2) because the adhesive composition (I-2) can exhibit energy ray curability without using an energy ray curable compound, and can be used without problems even with an adhesive resin that has low compatibility with the energy ray curable compound. For example, in the adhesive composition (I-1), a highly polar adhesive resin may be selected to enhance compatibility with the energy ray curable compound. However, the adhesive strength of the highly polar adhesive resin tends to increase over time after application. For example, an adhesive resin containing a structural unit derived from a (meth)acrylate having an alkoxy group in a side chain with 8 to 18 carbon atoms is unlikely to increase in adhesive strength over time after application, but may have low compatibility with energy ray curable compounds. However, when the adhesive resin is contained in an adhesive composition (I-2) and has an energy ray polymerizable unsaturated group in its side chain, it is possible to achieve a high level of both energy ray curability and reduced adhesive strength without considering the problem of compatibility with energy ray curable compounds.

[0110] When the adhesive layer is energy ray curable, the adhesive layer formed using the adhesive composition (I-2) may, for example, contain an adhesive resin having an energy ray polymerizable unsaturated group in its side chain.

[0111] An example of the adhesive layer is one that contains an adhesive resin, the adhesive resin having an energy ray-polymerizable unsaturated group in its side chain, and the adhesive resin containing a structural unit derived from a (meth)acrylate having an alkoxy group in the side chain with 8 to 18 carbon atoms.

[0112] <Adhesive composition (I-1)> As described above, the pressure-sensitive adhesive composition (I-1) contains a non-energy ray-curable pressure-sensitive adhesive resin (I-1a) and an energy ray-curable compound.

[0113] [Adhesive resin (I-1a)] The adhesive resin (I-1a) is preferably an acrylic resin. The acrylic resin may be, for example, an acrylic polymer having at least a structural unit derived from an alkyl (meth)acrylate. The structural unit contained in the acrylic resin may be of only one type, or of two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0114] In the adhesive resin constituting the adhesive layer, the content of structural units derived from (meth)acrylate compounds is preferably 50 to 100 mass%, more preferably 80 to 100 mass%, and even more preferably 90 to 100 mass%, relative to the total mass (100 mass%) of the structural units. "Derived from" in this context means that the monomer has undergone the structural changes necessary to be polymerized.

[0115] Specific examples of the (meth)acrylate compound include those exemplified above as the binder component.

[0116] The weight average molecular weight (Mw) of the acrylic resin is preferably 10,000 to 2,000,000, and more preferably 100,000 to 1,500,000. When the weight average molecular weight of the acrylic resin is within such a range, it becomes easy to adjust the adhesive strength between the pressure-sensitive adhesive layer and the adherend within a preferred range. On the other hand, when the weight average molecular weight of the acrylic resin is equal to or greater than the lower limit, the shape stability (stability over time during storage) of the pressure-sensitive adhesive layer is improved. Also, when the weight average molecular weight of the acrylic resin is equal to or less than the upper limit, the pressure-sensitive adhesive layer is more likely to conform to the uneven surface of the adherend, and the occurrence of voids between the adherend and the pressure-sensitive adhesive layer is more suppressed. In this specification, unless otherwise specified, the "weight average molecular weight" is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0117] The glass transition temperature (Tg) of the acrylic resin is preferably −60 to 70° C., more preferably −30 to 50° C. When the Tg of the acrylic resin is equal to or higher than the lower limit, the adhesive strength between the adhesive layer and the adherend is suppressed, and the chip with the film-shaped fired material can be more easily detached from the support sheet (described later) when picked up. When the Tg of the acrylic resin is equal to or lower than the upper limit, the adhesive strength between the adhesive layer and the chip is improved.

[0118] The adhesive resin preferably contains a structural unit derived from an alkyl (meth)acrylate among (meth)acrylate compounds, preferably contains a structural unit derived from a (meth)acrylate having an alkoxy group in a side chain with 8 to 18 carbon atoms, and more preferably contains a structural unit derived from an alkyl (meth)acrylate having an alkoxy group in a side chain with 8 to 18 carbon atoms. The number of carbon atoms in the alkoxy group in the side chain is preferably 8 to 18, more preferably 8 to 12, and even more preferably 8 to 10. The alkoxy group in the side chain may be linear or branched. By containing a structural unit derived from a (meth)acrylate having an alkoxy group in a side chain with 8 to 18 carbon atoms, the adhesive force at the interface between the adhesive layer and the film-shaped sintered material is reduced, and the diced chip with the film-shaped sintered material can be picked up more stably.

[0119] In the adhesive resin constituting the adhesive layer, the content of structural units derived from a (meth)acrylic acid ester having an alkoxy group in a side chain having 8 to 18 carbon atoms is preferably 50 to 100 mass%, more preferably 60 to 95 mass%, and even more preferably 70 to 90 mass%, relative to the total mass (100 mass%) of the structural units.

[0120] The acrylic polymer preferably further contains a structural unit derived from a functional group-containing monomer in addition to the structural unit derived from an alkyl (meth)acrylate. Examples of the functional group-containing monomer include those in which the functional group reacts with a crosslinking agent described below to become a crosslinking starting point, and those in which the functional group reacts with an unsaturated group in an unsaturated group-containing compound described below to enable the introduction of an unsaturated group into a side chain of an acrylic polymer.

[0121] Examples of the functional group in the functional group-containing monomer include a hydroxyl group, a carboxyl group, an amino group, and an epoxy group. That is, examples of functional group-containing monomers include hydroxyl group-containing monomers, carboxyl group-containing monomers, amino group-containing monomers, and epoxy group-containing monomers.

[0122] Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and non-(meth)acrylic unsaturated alcohols (i.e., unsaturated alcohols not having a (meth)acryloyl skeleton) such as vinyl alcohol and allyl alcohol.

[0123] Examples of the carboxy group-containing monomer include ethylenically unsaturated monocarboxylic acids (i.e., monocarboxylic acids having an ethylenically unsaturated bond) such as (meth)acrylic acid and crotonic acid; ethylenically unsaturated dicarboxylic acids (i.e., dicarboxylic acids having an ethylenically unsaturated bond) such as fumaric acid, itaconic acid, maleic acid and citraconic acid; anhydrides of the ethylenically unsaturated dicarboxylic acids; and (meth)acrylic acid carboxyalkyl esters such as 2-carboxyethyl methacrylate.

[0124] From the viewpoint of further reducing the adhesive strength of the adhesive resin with the film-shaped sintered material containing sinterable metal particles, the content of structural units derived from (meth)acrylic acid relative to the total mass (100 mass%) of the structural units of the adhesive resin is preferably 10 mass% or less, more preferably 5 mass% or less, and even more preferably 2 mass% or less, and it is particularly preferable that the adhesive resin contains substantially no structural units derived from (meth)acrylic acid.

[0125] The functional group-containing monomer is preferably a hydroxyl group-containing monomer or a carboxyl group-containing monomer, more preferably a hydroxyl group-containing monomer.

[0126] The hydroxyl group-containing monomer is preferably hydroxyalkyl(meth)acrylate. By using the hydroxyl group-containing monomer, the adhesive strength at the interface between the adhesive layer and the film-shaped sintered material can be reduced, and the diced chip with the film-shaped sintered material can be picked up more stably.

[0127] The functional group-containing monomer constituting the acrylic polymer may be of only one type, or of two or more types. When two or more types are used, the combination and ratio thereof can be selected arbitrarily.

[0128] In the acrylic polymer, the content of the structural units derived from functional group-containing monomers is preferably 1 to 35 mass%, more preferably 2 to 32 mass%, and particularly preferably 3 to 30 mass%, based on the total amount of structural units.

[0129] The acrylic polymer can be used as the non-energy ray-curable adhesive resin (I-1a) described above. On the other hand, a compound obtained by reacting a functional group in the acrylic polymer with an unsaturated group-containing compound having an energy ray-polymerizable unsaturated group (energy ray-polymerizable group) can be used as the above-mentioned energy ray-curable adhesive resin (I-2a).

[0130] The pressure-sensitive adhesive composition (I-1) may contain only one type of pressure-sensitive adhesive resin (I-1a), or may contain two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0131] In the pressure-sensitive adhesive composition (I-1), the content of the adhesive resin (I-1a) relative to the total mass of the pressure-sensitive adhesive composition (I-1) is preferably 5 to 99 mass%, more preferably 10 to 95 mass%, and particularly preferably 15 to 90 mass%.

[0132] [Energy ray curable compounds] The energy ray-curable compound contained in the pressure-sensitive adhesive composition (I-1) includes a monomer or oligomer having an energy ray-polymerizable unsaturated group and capable of being cured by irradiation with energy rays. Among the energy ray-curable compounds, examples of the monomer include polyvalent (meth)acrylates such as trimethylolpropane tri(meth)acrylate, pentaerythritol (meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, and 1,6-hexanediol (meth)acrylate; urethane (meth)acrylate; polyester (meth)acrylate; polyether (meth)acrylate; and epoxy (meth)acrylate. Among the energy ray-curable compounds, examples of the oligomer include oligomers obtained by polymerizing the above-exemplified monomers. The energy ray curable compound is preferably a urethane (meth)acrylate or a urethane (meth)acrylate oligomer, since it has a relatively large molecular weight and is less likely to reduce the storage modulus of the pressure-sensitive adhesive layer.

[0133] The pressure-sensitive adhesive composition (I-1) may contain only one type of the energy ray-curable compound, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.

[0134] In the pressure-sensitive adhesive composition (I-1), the content of the energy ray-curable compound relative to the total mass of the pressure-sensitive adhesive composition (I-1) is preferably 1 to 95 mass%, more preferably 5 to 90 mass%, and particularly preferably 10 to 85 mass%.

[0135] [Crosslinking agent] When the acrylic polymer having a structural unit derived from a functional group-containing monomer in addition to a structural unit derived from an alkyl (meth)acrylate is used as the adhesive resin (I-1a), it is preferable that the adhesive composition (I-1) further contains a crosslinking agent.

[0136] The crosslinking agent reacts with the functional group, for example, to crosslink the adhesive resins (I-1a) together. Examples of the crosslinking agent include isocyanate-based crosslinking agents such as tolylene diisocyanate (TDI), hexamethylene diisocyanate (HDI), xylylene diisocyanate (XDI), and adducts of these diisocyanates (i.e., crosslinking agents having an isocyanate group); organic polyvalent isocyanate-based crosslinking agents, epoxy-based crosslinking agents such as ethylene glycol glycidyl ether (i.e., crosslinking agents having a glycidyl group); aziridine-based crosslinking agents such as hexa[1-(2-methyl)-aziridinyl]triphosphatriazine (i.e., crosslinking agents having an aziridinyl group); metal chelate-based crosslinking agents such as aluminum chelate (i.e., crosslinking agents having a metal chelate structure); and isocyanurate-based crosslinking agents (i.e., crosslinking agents having an isocyanuric acid skeleton). The crosslinking agent is preferably an isocyanate-based crosslinking agent from the viewpoints of improving the cohesive strength of the pressure-sensitive adhesive and thereby improving the adhesive strength of the pressure-sensitive adhesive layer, and of easy availability.

[0137] More specific examples of the organic polyisocyanate compound include 2,4-tolylene diisocyanate; 2,6-tolylene diisocyanate; 1,3-xylylene diisocyanate; 1,4-xylylene diisocyanate; diphenylmethane-4,4'-diisocyanate; diphenylmethane-2,4'-diisocyanate; 3-methyldiphenylmethane diisocyanate; hexamethylene diisocyanate; isophorone diisocyanate; dicyclohexylmethane-4,4'-diisocyanate; dicyclohexylmethane-2,4'-diisocyanate; a compound in which one or more of tolylene diisocyanate, hexamethylene diisocyanate, and xylylene diisocyanate are added to all or a portion of the hydroxyl groups of a polyol such as trimethylolpropane; lysine diisocyanate, and the like.

[0138] The crosslinking agent contained in the pressure-sensitive adhesive composition (I-1) may be one type only, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.

[0139] When a crosslinking agent is used, the content of the crosslinking agent in the pressure-sensitive adhesive composition (I-1) is preferably 0.01 to 50 parts by mass, more preferably 0.1 to 20 parts by mass, and particularly preferably 0.3 to 15 parts by mass, per 100 parts by mass of the pressure-sensitive adhesive resin (I-1a).

[0140] [Photopolymerization initiator] The pressure-sensitive adhesive composition (I-1) may further contain a photopolymerization initiator. The pressure-sensitive adhesive composition (I-1) containing a photopolymerization initiator sufficiently undergoes a curing reaction even when irradiated with relatively low-energy energy rays such as ultraviolet rays.

[0141] Examples of the photopolymerization initiator include benzoin compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin benzoic acid, benzoin methyl benzoate, and benzoin dimethyl ketal; acetophenone compounds such as acetophenone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, and 2,2-dimethoxy-1,2-diphenylethane-1-one; acyl phosphinates such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 2,4,6-trimethylbenzoyldiphenylphosphine oxide; Examples of such compounds include phosphine oxide compounds; sulfide compounds such as benzyl phenyl sulfide and tetramethylthiuram monosulfide; α-ketol compounds such as 1-hydroxycyclohexyl phenyl ketone; azo compounds such as azobisisobutyronitrile; titanocene compounds such as titanocene; thioxanthone compounds such as thioxanthone; peroxide compounds; diketone compounds such as diacetyl; benzyl; dibenzyl; benzophenone; 2,4-diethylthioxanthone; 1,2-diphenylmethane; 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone; and 2-chloroanthraquinone. As the photopolymerization initiator, for example, a quinone compound such as 1-chloroanthraquinone; a photosensitizer such as an amine, and the like can also be used.

[0142] The photopolymerization initiator contained in the pressure-sensitive adhesive composition (I-1) may be one type only, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.

[0143] When a photopolymerization initiator is used, the content of the photopolymerization initiator in the pressure-sensitive adhesive composition (I-1) is preferably 0.01 to 20 parts by mass, more preferably 0.03 to 10 parts by mass, and particularly preferably 0.05 to 5 parts by mass, relative to 100 parts by mass of the energy ray-curable compound.

[0144] [Other additives] The pressure-sensitive adhesive composition (I-1) may contain other additives that do not fall into any of the above-mentioned components, as long as the effects of the present invention are not impaired. Examples of the other additives include known additives such as antistatic agents, antioxidants, softeners (plasticizers), fillers, rust inhibitors, colorants (pigments, dyes), sensitizers, tackifiers, reaction retarders, and crosslinking accelerators (catalysts). The reaction retarder is, for example, a retarder that suppresses the unintended crosslinking reaction from proceeding in the pressure-sensitive adhesive composition (I-1) during storage due to the action of the catalyst mixed in the pressure-sensitive adhesive composition (I-1). For example, the reaction retarder can be a retarder that forms a chelate complex by chelation with the catalyst, and more specifically, a retarder that has two or more carbonyl groups (-C(=O)-) in one molecule.

[0145] The other additives contained in the pressure-sensitive adhesive composition (I-1) may be one type only, or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0146] When other additives are used, the content of the other additives in the pressure-sensitive adhesive composition (I-1) is not particularly limited and may be appropriately selected depending on the type of the additives.

[0147] [solvent] The pressure-sensitive adhesive composition (I-1) may contain a solvent. By containing a solvent, the pressure-sensitive adhesive composition (I-1) has improved suitability for application to a surface to be coated.

[0148] The solvent is preferably an organic solvent, and examples of the organic solvent include ketones such as methyl ethyl ketone and acetone; esters (e.g., carboxylates) such as ethyl acetate; ethers such as tetrahydrofuran and dioxane; aliphatic hydrocarbons such as cyclohexane and n-hexane; aromatic hydrocarbons such as toluene and xylene; and alcohols such as 1-propanol and 2-propanol.

[0149] As the solvent, for example, the solvent used during the production of the adhesive resin (I-1a) may be used as it is in the adhesive composition (I-1) without being removed from the adhesive resin (I-1a), or a solvent of the same or different type as that used during the production of the adhesive resin (I-1a) may be added separately during the production of the adhesive composition (I-1).

[0150] The pressure-sensitive adhesive composition (I-1) may contain one kind of solvent or two or more kinds of solvents. When two or more kinds of solvents are contained, the combination and ratio thereof can be selected arbitrarily.

[0151] When a solvent is used, the content of the solvent in the pressure-sensitive adhesive composition (I-1) is not particularly limited and may be appropriately adjusted.

[0152] <Adhesive composition (I-2)> As described above, the adhesive composition (I-2) contains an energy ray-curable adhesive resin (I-2a) in which an unsaturated group has been introduced into the side chain of a non-energy ray-curable adhesive resin (I-1a).

[0153] [Adhesive resin (I-2a)] The adhesive resin (I-2a) can be obtained, for example, by reacting a functional group in the adhesive resin (I-1a) with an unsaturated group-containing compound having an energy ray-polymerizable unsaturated group.

[0154] The unsaturated group-containing compound is a compound that, in addition to the energy ray-polymerizable unsaturated group, further has a group that can bond to the adhesive resin (I-1a) by reacting with a functional group in the adhesive resin (I-1a). Examples of the energy ray-polymerizable unsaturated group include a (meth)acryloyl group, a vinyl group (also known as an ethenyl group), and an allyl group (also known as a 2-propenyl group), with a (meth)acryloyl group being preferred. Examples of groups capable of bonding to functional groups in the adhesive resin (I-1a) include isocyanate groups and glycidyl groups capable of bonding to hydroxyl groups or amino groups, and hydroxyl groups and amino groups capable of bonding to carboxy groups or epoxy groups.

[0155] Examples of the unsaturated group-containing compound include (meth)acryloyloxyethyl isocyanate, (meth)acryloyl isocyanate, and glycidyl (meth)acrylate.

[0156] The pressure-sensitive adhesive composition (I-2) may contain only one type of pressure-sensitive adhesive resin (I-2a), or may contain two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0157] In the pressure-sensitive adhesive composition (I-2), the content of the adhesive resin (I-2a) relative to the total mass of the pressure-sensitive adhesive composition (I-2) is preferably 5 to 99 mass%, more preferably 10 to 95 mass%, and particularly preferably 10 to 90 mass%.

[0158] In the pressure-sensitive adhesive composition (I-2), the ratio of the content of the adhesive resin (I-1a) to the total content of all components other than the solvent (i.e., the ratio of the content of the adhesive resin (I-1a) in the pressure-sensitive adhesive layer to the total mass of the pressure-sensitive adhesive layer) is preferably 50 to 100 mass%, and may be, for example, 65 to 99 mass%.

[0159] [Crosslinking agent] When the adhesive resin (I-2a) is, for example, an acrylic polymer having a structural unit derived from a functional group-containing monomer similar to that in the adhesive resin (I-1a), the adhesive composition (I-2) may further contain a crosslinking agent.

[0160] The crosslinking agent in the pressure-sensitive adhesive composition (I-2) may be the same as the crosslinking agent in the pressure-sensitive adhesive composition (I-1). The pressure-sensitive adhesive composition (I-2) may contain only one type of crosslinking agent, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.

[0161] When a crosslinking agent is used, the content of the crosslinking agent in the pressure-sensitive adhesive composition (I-2) is preferably 0.01 to 50 parts by mass, more preferably 0.1 to 20 parts by mass, and particularly preferably 0.3 to 3 parts by mass, per 100 parts by mass of the pressure-sensitive adhesive resin (I-2a).

[0162] By setting the content of the crosslinking agent in the adhesive composition (I-2) within the above range, the adhesive strength at the interface between the adhesive layer and the film-shaped sintered material is reduced, and the diced chips with the film-shaped sintered material can be picked up more stably.

[0163] [Photopolymerization initiator] The pressure-sensitive adhesive composition (I-2) may further contain a photopolymerization initiator. The pressure-sensitive adhesive composition (I-2) containing a photopolymerization initiator sufficiently undergoes a curing reaction even when irradiated with relatively low-energy energy rays such as ultraviolet rays.

[0164] The photopolymerization initiator in the pressure-sensitive adhesive composition (I-2) may be the same as the photopolymerization initiator in the pressure-sensitive adhesive composition (I-1). The photopolymerization initiator contained in the pressure-sensitive adhesive composition (I-2) may be one kind or two or more kinds, and when there are two or more kinds, the combination and ratio thereof can be selected arbitrarily.

[0165] When a photopolymerization initiator is used, the content of the photopolymerization initiator in the pressure-sensitive adhesive composition (I-2) is preferably 0.01 to 20 parts by mass, more preferably 0.03 to 10 parts by mass, and particularly preferably 0.05 to 5 parts by mass, per 100 parts by mass of the pressure-sensitive adhesive resin (I-2a).

[0166] [Other additives] The pressure-sensitive adhesive composition (I-2) may contain other additives that do not fall under any of the above-mentioned components, as long as the effects of the present invention are not impaired. The other additives in the pressure-sensitive adhesive composition (I-2) include the same additives as those in the pressure-sensitive adhesive composition (I-1). The other additives contained in the pressure-sensitive adhesive composition (I-2) may be one type only, or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0167] When other additives are used, the content of the other additives in the pressure-sensitive adhesive composition (I-2) is not particularly limited and may be appropriately selected depending on the type of the additives.

[0168] [solvent] The pressure-sensitive adhesive composition (I-2) may contain a solvent for the same purpose as in the case of the pressure-sensitive adhesive composition (I-1). The solvent in the pressure-sensitive adhesive composition (I-2) may be the same as the solvent in the pressure-sensitive adhesive composition (I-1). The pressure-sensitive adhesive composition (I-2) may contain one kind of solvent or two or more kinds of solvents. When two or more kinds of solvents are contained, the combination and ratio thereof can be selected arbitrarily. When a solvent is used, the content of the solvent in the pressure-sensitive adhesive composition (I-2) is not particularly limited and may be appropriately adjusted.

[0169] <Adhesive composition (I-3)> As described above, the pressure-sensitive adhesive composition (I-3) contains the pressure-sensitive adhesive resin (I-2a) and an energy ray-curable compound.

[0170] In the pressure-sensitive adhesive composition (I-3), the content of the adhesive resin (I-2a) relative to the total mass of the pressure-sensitive adhesive composition (I-3) is preferably 5 to 99 mass%, more preferably 10 to 95 mass%, and particularly preferably 15 to 90 mass%.

[0171] [Energy ray curable compounds] The energy ray-curable compound contained in the pressure-sensitive adhesive composition (I-3) includes monomers and oligomers that have an energy ray-polymerizable unsaturated group and are curable by irradiation with energy rays, and includes the same as the energy ray-curable compound contained in the pressure-sensitive adhesive composition (I-1). The pressure-sensitive adhesive composition (I-3) may contain only one type of the energy ray-curable compound, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.

[0172] In the pressure-sensitive adhesive composition (I-3), the content of the energy ray-curable compound is preferably 0.01 to 300 parts by mass, more preferably 0.03 to 200 parts by mass, and particularly preferably 0.05 to 100 parts by mass, per 100 parts by mass of the pressure-sensitive adhesive resin (I-2a).

[0173] [Photopolymerization initiator] The pressure-sensitive adhesive composition (I-3) may further contain a photopolymerization initiator. The pressure-sensitive adhesive composition (I-3) containing a photopolymerization initiator sufficiently undergoes a curing reaction even when irradiated with relatively low-energy energy rays such as ultraviolet rays.

[0174] The photopolymerization initiator in the pressure-sensitive adhesive composition (I-3) may be the same as the photopolymerization initiator in the pressure-sensitive adhesive composition (I-1). The photopolymerization initiator contained in the pressure-sensitive adhesive composition (I-3) may be one type only, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.

[0175] When a photopolymerization initiator is used, the content of the photopolymerization initiator in the pressure-sensitive adhesive composition (I-3) is preferably 0.01 to 20 parts by mass, more preferably 0.03 to 10 parts by mass, and particularly preferably 0.05 to 5 parts by mass, relative to 100 parts by mass of the total content of the pressure-sensitive adhesive resin (I-2a) and the energy ray-curable compound.

[0176] [Other additives] The pressure-sensitive adhesive composition (I-3) may contain other additives that do not fall under any of the above-mentioned components, as long as the effects of the present invention are not impaired. Examples of the other additives include the same additives as those in the pressure-sensitive adhesive composition (I-1). The other additives contained in the pressure-sensitive adhesive composition (I-3) may be one type only, or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0177] When other additives are used, the content of the other additives in the pressure-sensitive adhesive composition (I-3) is not particularly limited and may be appropriately selected depending on the type of the additives.

[0178] [solvent] The pressure-sensitive adhesive composition (I-3) may contain a solvent for the same purpose as in the case of the pressure-sensitive adhesive composition (I-1). The solvent in the pressure-sensitive adhesive composition (I-3) may be the same as the solvent in the pressure-sensitive adhesive composition (I-1). The pressure-sensitive adhesive composition (I-3) may contain one kind of solvent, or two or more kinds of solvents. When two or more kinds of solvents are contained, the combination and ratio thereof can be selected arbitrarily. When a solvent is used, the content of the solvent in the pressure-sensitive adhesive composition (I-3) is not particularly limited and may be appropriately adjusted.

[0179] <Adhesive compositions other than the adhesive compositions (I-1) to (I-3)> So far, the adhesive composition (I-1), the adhesive composition (I-2) and the adhesive composition (I-3) have been mainly explained, but the components explained as contained therein can be similarly used in general adhesive compositions other than these three types of adhesive compositions (referred to in this specification as "adhesive compositions other than adhesive compositions (I-1) to (I-3)").

[0180] Examples of pressure-sensitive adhesive compositions other than the pressure-sensitive adhesive compositions (I-1) to (I-3) include energy ray-curable pressure-sensitive adhesive compositions as well as non-energy ray-curable pressure-sensitive adhesive compositions. Examples of the non-energy ray curable adhesive composition include an adhesive composition (I-4) containing a non-energy ray curable adhesive resin (I-1a) such as an acrylic resin, a urethane resin, a rubber-based resin, a silicone resin, an epoxy resin, a polyvinyl ether, a polycarbonate, or an ester-based resin, and those containing an acrylic resin are preferred.

[0181] It is preferable that the pressure-sensitive adhesive compositions other than the pressure-sensitive adhesive compositions (I-1) to (I-3) contain one or more crosslinking agents, and the content thereof can be the same as that of the above-mentioned pressure-sensitive adhesive composition (I-1) etc.

[0182] <Adhesive composition (I-4)> A preferred pressure-sensitive adhesive composition (I-4) is, for example, one containing the pressure-sensitive adhesive resin (I-1a) and a crosslinking agent.

[0183] [Adhesive resin (I-1a)] The adhesive resin (I-1a) in the adhesive composition (I-4) may be the same as the adhesive resin (I-1a) in the adhesive composition (I-1). The pressure-sensitive adhesive composition (I-4) may contain only one type of pressure-sensitive adhesive resin (I-1a), or may contain two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0184] In the pressure-sensitive adhesive composition (I-4), the content of the adhesive resin (I-1a) relative to the total mass of the pressure-sensitive adhesive composition (I-4) is preferably 5 to 99 mass%, more preferably 10 to 95 mass%, and particularly preferably 15 to 90 mass%.

[0185] In the pressure-sensitive adhesive composition (I-4), the ratio of the content of the adhesive resin (I-1a) to the total content of all components other than the solvent (i.e., the ratio of the content of the adhesive resin (I-1a) in the pressure-sensitive adhesive layer to the total mass of the pressure-sensitive adhesive layer) is preferably 50 to 100 mass%, and may be, for example, 65 to 99 mass%, or may be 80 to 98 mass%.

[0186] [Crosslinking agent] When the acrylic polymer having a structural unit derived from a functional group-containing monomer in addition to a structural unit derived from an alkyl (meth)acrylate is used as the adhesive resin (I-1a), it is preferable that the adhesive composition (I-4) further contains a crosslinking agent.

[0187] The crosslinking agent in the pressure-sensitive adhesive composition (I-4) may be the same as the crosslinking agent in the pressure-sensitive adhesive composition (I-1). The crosslinking agent contained in the pressure-sensitive adhesive composition (I-4) may be one type or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.

[0188] In the pressure-sensitive adhesive composition (I-4), the content of the crosslinking agent is preferably 0.01 to 50 parts by mass, more preferably 0.1 to 20 parts by mass, and particularly preferably 4 to 15 parts by mass, per 100 parts by mass of the pressure-sensitive adhesive resin (I-1a).

[0189] By setting the content of the crosslinking agent in the adhesive composition (I-4) within the above range, the adhesive strength at the interface between the adhesive layer and the film-shaped sintered material is reduced, and the diced chips with the film-shaped sintered material can be picked up more stably.

[0190] [Other additives] The pressure-sensitive adhesive composition (I-4) may contain other additives that do not fall into any of the above-mentioned components, as long as the effects of the present invention are not impaired. Examples of the other additives include the same additives as those in the pressure-sensitive adhesive composition (I-1). The other additives contained in the pressure-sensitive adhesive composition (I-4) may be of only one type, or of two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0191] When other additives are used, the content of the other additives in the pressure-sensitive adhesive composition (I-4) is not particularly limited and may be appropriately selected depending on the type of the additives.

[0192] [solvent] The pressure-sensitive adhesive composition (I-4) may contain a solvent for the same purpose as in the case of the pressure-sensitive adhesive composition (I-1). The solvent in the pressure-sensitive adhesive composition (I-4) may be the same as the solvent in the pressure-sensitive adhesive composition (I-1). The pressure-sensitive adhesive composition (I-4) may contain one kind of solvent, or two or more kinds of solvents. When two or more kinds of solvents are contained, the combination and ratio thereof can be selected arbitrarily. When a solvent is used, the content of the solvent in the pressure-sensitive adhesive composition (I-4) is not particularly limited and may be appropriately adjusted.

[0193] [Method of manufacturing adhesive composition] The pressure-sensitive adhesive compositions other than the pressure-sensitive adhesive compositions (I-1) to (I-3), such as the pressure-sensitive adhesive compositions (I-4), can be obtained by blending the pressure-sensitive adhesive and, as necessary, components other than the pressure-sensitive adhesive, for example, components for constituting the pressure-sensitive adhesive composition. The order of addition of the components when blending is not particularly limited, and two or more components may be added simultaneously. When a solvent is used, the solvent may be used by mixing it with any of the other ingredients to pre-dilute the ingredients, or the solvent may be used by mixing it with any of the other ingredients without pre-diluting the ingredients. The method for mixing the components during blending is not particularly limited, and may be appropriately selected from known methods such as a method of mixing by rotating a stirrer or stirring blades, a method of mixing using a mixer, a method of mixing by adding ultrasound, etc. The temperature and time during addition and mixing of each component are not particularly limited as long as the components do not deteriorate, and may be adjusted appropriately. A temperature of 15 to 30°C is preferred.

[0194] [Manufacturing method of film-shaped sintered material with support sheet] The film-shaped sintered material with a support sheet of this embodiment can be produced by laminating the above-mentioned layers in order so that they are in a corresponding positional relationship. For example, when laminating a pressure-sensitive adhesive layer on a base film, a pressure-sensitive adhesive composition containing the components and a solvent for constituting the pressure-sensitive adhesive layer is applied onto a release film, and if necessary, dried to volatilize the solvent to form a film, thereby forming the pressure-sensitive adhesive layer on the release film in advance, and the exposed surface of the formed pressure-sensitive adhesive layer opposite to the side in contact with the release film is bonded to the surface of the base film. The release film may be removed as necessary after the formation of the laminate structure.

[0195] For example, in the case of producing a film-like sintered material with a support sheet (a film-like sintered material with a support sheet in which a support sheet is a laminate of a base film and an adhesive layer) in which an adhesive layer is laminated on a base film and a film-like sintered material is laminated on the adhesive layer, the adhesive layer is laminated on the base film by the above-mentioned method, and a sintered material composition containing components and a solvent for constituting the film-like sintered material is separately coated or printed on a release film, and if necessary, dried to volatilize the solvent to form a film-like sintered material on the release film, and the exposed surface of this film-like sintered material is attached to the exposed surface of the adhesive layer already laminated on the base film, and the film-like sintered material is laminated on the adhesive layer to obtain a film-like sintered material with a support sheet. When forming a film-like sintered material on a release film, it is preferable to coat or print the sintered material composition on the release-treated surface of the release film, and the release film may be removed as necessary after the formation of the laminated structure.

[0196] In this way, all of the layers other than the base film that make up the film-like sintered material with a support sheet can be formed in advance on a release film and then laminated by bonding it to the surface of the desired layer.Therefore, the layer for which such a process is to be adopted can be appropriately selected as necessary to produce the film-like sintered material with a support sheet.

[0197] After all the necessary layers have been provided, the film-shaped sintered material with support sheet may be stored with a release film attached to the surface of the outermost layer opposite the support sheet.

[0198] <Roll body> As one embodiment of the present invention, the film-shaped sintered material with the support sheet is laminated on a long release film with the film-shaped sintered material on the inside, The release film and the film-shaped sintered material with the support sheet are rolled up into a roll body.

[0199] 6 is a cross-sectional view showing a schematic diagram of a roll according to one embodiment of the present invention, showing a state in which the roll has been unwound and partly spread out. The roll 110 is formed by laminating two or more units of the film-shaped sintered material 100 with a support sheet, which has been processed into a predetermined shape, on a release film 30, with the film-shaped sintered material facing inward. The release film 30 and the film-shaped sintered material 100 with a support sheet are rolled up so that the side on which the film-shaped sintered material 100 with a support sheet is laminated faces the center. The direction of the roll is the longitudinal direction of the long release film 30.

[0200] The one unit of the film-shaped sintered material with a support sheet may be a portion of the film-shaped sintered material with a support sheet used for attachment to one attachment object or one attachment object, and may be a portion included in unit P in FIG. 6. In FIG. 6, one film-shaped sintered material 1 is included in each unit P, and two or more units P are consecutively arranged at a predetermined interval. The film-shaped sintered materials with a support sheet included in each unit P may be processed to have the same shape. A preferred shape of the film-shaped sintered material with a support sheet is one in which a circular support sheet and a circular film-shaped sintered material with a smaller diameter than the support sheet are concentrically laminated.

[0201] The film-shaped sintered material 1 can be easily attached to a semiconductor wafer or the like (object to be affixed) and has adhesive properties, so by sandwiching the film-shaped sintered material 1 between a release film 30, which has poor adhesive properties, and a support sheet 2, it is suitable for storage in roll form. The roll body is also suitable as a distribution form for the film-like sintered material with the support sheet.

[0202] The roll body can be produced by laminating the film-shaped sintered material with the support sheet and a release film in a corresponding positional relationship.

[0203] <Laminate> As one embodiment of the present invention, there is provided a laminate in which the film-shaped sintered material with a support sheet and a wafer are attached, and the support sheet, the film-shaped sintered material, and the wafer are laminated in this order. The laminate can be used as an intermediate in the device manufacturing method described below.

[0204] 4 is also a cross-sectional view showing a schematic diagram of a laminate according to one embodiment of the present invention. The laminate 120 is a laminate of the film-shaped sintered material 100 with a support sheet and a semiconductor wafer 18, in which the support sheet 2, the film-shaped sintered material 1, and the semiconductor wafer 18 are stacked in this order. The semiconductor wafer 18 may be provided in direct contact with the film-shaped sintered material 1. In the configuration shown here, the film-shaped sintered material 1 is provided in direct contact with a metal film 18a (also called a back electrode), which is one element of the semiconductor wafer 18.

[0205] The semiconductor wafer may be a silicon wafer or a silicon carbide wafer, or may be a compound semiconductor wafer such as gallium arsenide. A circuit may be formed on the surface of the semiconductor wafer. The formation of a circuit on the wafer surface may be performed by various methods including conventionally widely used methods such as an etching method and a lift-off method. The surface opposite to the circuit surface (back surface) of the semiconductor wafer may be ground by a known means using a grinder or the like. During back grinding, an adhesive sheet called a surface protection sheet can be attached to the circuit surface to protect the circuit on the front surface. In back grinding, the circuit surface side (i.e., the surface protection sheet side) of the wafer can be fixed by a chuck table or the like, and the back surface side on which no circuit is formed can be ground by a grinder. Explaining with reference to Figures 2 to 3, during back grinding, first, the entire back surface is ground to a predetermined thickness, and then only the back surface inner peripheral portion 16 corresponding to the front circuit forming portion (front surface inner peripheral portion 14) is ground, and the back surface area corresponding to the surplus portion 15 on which no circuit 13 is formed is left unground. As a result, after grinding, only the back surface inner peripheral portion 16 of the semiconductor wafer 18 is further ground thin, and an annular protrusion 17 remains on the outer peripheral portion. Such back surface grinding can be performed by the known methods described in the above-mentioned Patent Documents 2 to 4. Thereafter, if necessary, the fractured layer generated during back surface grinding is removed. The fractured layer can be removed by chemical etching, plasma etching, etc. After grinding, a metal film 18a may be provided on the back surface, and the metal film may be a single film or multiple films. Various methods such as electrolytic or electroless plating, sputtering, etc. can be used to form the metal film.

[0206] The shape of the workpiece (wafer, etc.) to be attached is usually circular or approximately circular, and therefore, it is preferable that the shape of the film-shaped sintered material 1 and the support sheet 2 are also circular or approximately circular.

[0207] The laminate can be produced by laminating the film-shaped sintered material with the support sheet and a wafer in a corresponding positional relationship.

[0208] As one embodiment of the present invention, there is provided a method for manufacturing a laminate, which includes a step of attaching a film-shaped sintered material to the inner peripheral portion of a surface side of a wafer having an annular convex portion on its outer periphery, thereby obtaining a laminate in which the support sheet, the film-shaped sintered material, and the wafer are stacked in this order. Regarding the film-shaped sintered material with support sheet, wafers, etc., their positional relationships, the size of each part, etc., the configuration shown in the above <<Film-shaped sintered material with support sheet>> can be exemplified.

[0209] As shown in Figure 4, in the laminate of the embodiment, in the film-shaped sintered material 100 with support sheet, the diameter D1 of the film-shaped sintered material is less than the diameter D3 of the inner circumference 16 of the back surface of the wafer, so that even in the case of a wafer 18 having an annular protrusion 17 on its outer periphery, the film-shaped sintered material 1 can be properly attached to the inner circumference 16 of the back surface, and the laminate of the embodiment can be provided.

[0210] <Device manufacturing method> Next, a method of using the film-shaped sintered material with a support sheet of this embodiment will be described by taking as an example a case where a semiconductor wafer is used as the wafer and the sintered material is applied to the manufacture of a semiconductor device.

[0211] As one embodiment of the present invention, a method for manufacturing a semiconductor device using a film-shaped sintered material with a support sheet according to the present invention is a method for manufacturing a semiconductor device using a film-shaped sintered material with a support sheet, which comprises sequentially carrying out the following steps (1) to (5).

[0212] Step (1): A step of cutting the annular convex portion of the laminate of the embodiment; Step (2): dicing the wafer and the film-shaped sintered material of the laminate from which the annular protrusion has been removed; Step (3): peeling off the diced film-shaped sintered material and the support sheet to obtain a chip with the film-shaped sintered material; Step (4): A step of attaching the film-shaped sintered material of the chip with the film-shaped sintered material to a surface of a substrate; Step (5): A step of firing the film-shaped sintered material of the chip with the film-shaped sintered material, and bonding the chip and the substrate.

[0213] Hereinafter, the above steps (1) to (5) of the method for manufacturing a semiconductor device will be described with reference to FIG.

[0214] ·Process (1) In step (1), as shown in FIG. 7A, a laminate 120 is used in which a film-shaped sintered material 1 of a film-shaped sintered material with a support sheet is attached to a semiconductor wafer 18, and the support sheet 2, the film-shaped sintered material 1, and the semiconductor wafer 18 are laminated in this order.

[0215] Next, the annular convex portion is cut. The cutting of the annular convex portion can be performed by a known method, and is not particularly limited. For example, the annular convex portion can be cut by a method of cutting into the wafer, such as a method using a blade or a method using laser irradiation, with the method using laser irradiation being preferred. The wavelength of the light beam used for the laser irradiation can be exemplified by those used when the following dicing is performed by laser irradiation, and any wavelength of light beam that can be used to cut the annular convex portion can be used. The intensity and illuminance of the laser light depends on the thickness of the wafer to be cut, but may be sufficient if it is strong enough to fully cut the wafer. 7A, a case will be exemplified in which a laser beam (illustrated as LD) is applied from the semiconductor wafer 18 side to cut the annular convex portion 17 of the semiconductor wafer 18 of the laminate 120. The cutting is performed by forming a notch C1 in the annular convex portion 17. The notch C1 is not formed in the support sheet 2 (the pressure-sensitive adhesive layer 4 and the base film 3), or even if it is formed, it is to an extent that it does not affect subsequent processes.

[0216] When the annular convex portion is cut by laser irradiation, in the film-shaped sintered material with support sheet of the embodiment, the support sheet preferably has an absorbance of 0.22 or less at the light wavelength of the laser irradiation, more preferably 0 to 0.2, and even more preferably 0 to 0.18. The support sheet preferably has an absorbance of 0.22 or less at a wavelength of 355 nm, more preferably 0 to 0.2, and even more preferably 0 to 0.18. The step of cutting the annular convex portion is often performed by processing with a laser having a wavelength of 355 nm, and the support sheet having the above configuration can prevent the support sheet from being broken when processing with the laser is performed.

[0217] In the film-shaped sintered material with support sheet of this embodiment, the load of the support sheet at 5% elongation may be 2N / 15mm to 13N / 15mm, 3N / 15mm to 10N / 15mm, or 4N / 15mm to 9N / 15mm. In the film-shaped sintered material with support sheet in which the load at 5% elongation of the support sheet is equal to or less than the upper limit, damage to the wafer is effectively prevented in the step of cutting the annular convex portion. In addition, by having the load at 5% elongation be equal to or more than the lower limit, the wafer is reinforced in the step of cutting the annular convex portion and the step of dicing, and damage to the wafer can be prevented more effectively.

[0218] ·Process (2) Step (2) is a step of dicing the wafer and the film-shaped sintered material of the laminate from which the annular protrusion has been removed. The dicing of the semiconductor wafer can be carried out by a known method, and is not particularly limited. For example, dicing of a semiconductor wafer can be performed by a method of cutting the semiconductor wafer, such as a method using a blade (i.e., blade dicing), a method using laser irradiation (i.e., laser dicing), or a method using water containing an abrasive (i.e., water dicing).

[0219] Here, as shown in Fig. 7B, a case is exemplified in which the semiconductor wafer 18 and the film-shaped sintered material 1 of the laminate 120 are diced from the semiconductor wafer 18 side using a dicing blade. Dicing cuts both the semiconductor wafer 18 and the film-shaped sintered material 1 by forming a notch C2, and divides the semiconductor wafer to form a semiconductor chip 19. The notch C2 preferably reaches the adhesive layer 4, but does not have to reach the base film 3.

[0220] Incidentally, individual pieces (chips) obtained by dividing a semiconductor wafer having circuits formed on its surface are also called elements or semiconductor elements.

[0221] In blade dicing, the rotation speed of the dicing blade is preferably 10,000 to 60,000 rpm, and more preferably 20,000 to 50,000 rpm. The moving speed of the dicing blade is preferably 5 to 100 mm / s, and more preferably 20 to 60 mm / s. During operation of the dicing blade, it is preferable to flow cutting water at a rate of, for example, about 0.5 to 1.5 L / min to the area where dicing is being performed.

[0222] Although not shown in the figure, it is also possible to irradiate laser light from the semiconductor wafer 18 side to laser dicing the semiconductor wafer 18 and the film-shaped sintered material 1 of the laminate 120. In laser dicing, the wavelength of the light irradiated to the laminate may be any wavelength of 300 to 1200 nm, any wavelength of 320 to 600 nm, any wavelength of 325 to 540 nm, or any wavelength of 330 to 400 nm. Any wavelength of 300 to 1200 nm may be any wavelength that falls within the wavelength range of 300 to 1200 nm, and more specifically, 355 nm, 532 nm, 1064 nm, etc. can be exemplified. These specific wavelengths are the laser wavelengths mounted on current laser dicers, but in this embodiment, any wavelength of light that can be used for dicing within the wavelength range of 300 to 1200 nm can be used. The light beam is usually a laser beam, and the intensity and illuminance of the laser beam depend on the thickness of the wafer and the film-like fired material to be cut, but need only be sufficient to fully cut the wafer.

[0223] The method of cutting the annular convex portion in step (1) and the method of dicing in step (2) may be combined in any manner. For example, any of the following combinations may be used. A combination of step (1): laser and step (2): laser, A combination of step (1): blade and step (2): laser. A combination of step (1): laser and step (2): blade. A combination of process (1): blade and process (2): blade. Laser cutting is preferred since it allows high speed processing on thinned wafers.

[0224] ·Process (3) In step (3), the diced film-shaped sintered material 1 and the support sheet 2 are peeled off to obtain chips 130 with the film-shaped sintered material. As shown in Figure 7C, after the notch C2 is formed, force is applied to the laminate 120 from the base film 3 side, and the semiconductor chip 19, together with the diced film-shaped sintered material 1, is pulled away (picked up) from the adhesive layer 4 of the support sheet to obtain a chip 130 with film-shaped sintered material.

[0225] Here, as one embodiment, a chip 130 with a film-shaped baking material, which includes the chip 19 and the film-shaped baking material 1, can be manufactured.

[0226] 7C shows an example in which a protrusion (pin) 70 is protruded from a push-up unit (not shown) in a semiconductor device manufacturing apparatus, and the tip of the protrusion 70 pushes up the laminate 120 from the base film 3 side, thereby applying a force in the protruding direction of the protrusion 70 to the laminate 120 after the notch C2 and the semiconductor chip 19 are formed. At this time, the push-up conditions such as the protrusion amount (push-up amount) of the protrusion 70, the protrusion speed (push-up speed), and the time for which the protrusion state is maintained (lift-up waiting time) can be appropriately adjusted. The number of protrusions 70 is not particularly limited and may be selected appropriately.

[0227] 7C shows an example in which the semiconductor chip 19 is lifted up by a lifting unit 71 of a semiconductor device manufacturing device, thereby peeling the semiconductor chip 19 together with the film-shaped sintered material 1 from the adhesive layer 4. Here, the lifting direction of the semiconductor chip 19 is indicated by an arrow I.

[0228] In addition, in the pickup, the method of pushing up the stack 120 may be a known method, and in addition to the method of pushing up using a protrusion as described above, there is also a method of pushing up the stack 120 by moving a slider along the stack 120.

[0229] The method for lifting up the semiconductor chip 19 may be a known method, for example, a method in which the surface of the semiconductor chip 19 is attracted to a vacuum collet and lifted up.

[0230] In addition, when the adhesive layer 4 has a curing property such as energy ray curing property, the adhesive layer 4 can be cured by energy ray irradiation or the like after dicing and before peeling (pickup) the film-shaped sintered material 1 and the support sheet 2, thereby reducing the adhesive strength of the adhesive layer 4. This prevents chips from scattering during dicing due to the high adhesive strength, and during pick-up, the adhesive strength is reduced by the curing, making it easier to peel (pick up) the film-shaped sintered material 1 and the support sheet 2.

[0231] ·Process (4) Next, in step (4), as shown in FIG. 7D, the film-shaped sintered material 1 of the chip 130 with film-shaped sintered material is attached to the surface of the substrate 6. As a result, the chip 19 is attached to the substrate 6 via the film-shaped sintered material 1. The substrate 6 also includes a lead frame and a heat sink. According to the film-shaped sintered material with support sheet of this embodiment, it is expected that adhesive force will be exerted between the film-shaped sintered material and the substrate. Even when the chip and the substrate are temporarily fixed with the film-shaped sintered material before sintering, it is possible to suppress the chip position from shifting during transportation, etc.

[0232] ·Process (5) Next, in step (5), the film-shaped sintered material is sintered to sinter-bond the chip 19 and the substrate 6 (FIG. 7E). The exposed surface of the film-shaped sintered material 1 of the chip 130 with film-shaped sintered material is attached to the substrate 6, and the substrate 6 and the chip 19 can be sinter-bonded via the film-shaped sintered material 1. By sintering, the sinterable metal particles of the film-shaped sintered material 1 are fused and bonded to each other to form a sintered body 11, and the chip 19 and the substrate 6 are sinter-bonded to each other, thereby obtaining a semiconductor device 140.

[0233] The heating temperature for firing the film-shaped fired material may be appropriately determined in consideration of the type of the film-shaped fired material, etc., but is preferably 100 to 600° C., more preferably 150 to 550° C., and even more preferably 200 to 400° C. The heating time may be appropriately determined in consideration of the type of the film-shaped fired material, etc., but is preferably 5 seconds to 60 minutes, more preferably 5 seconds to 30 minutes, and even more preferably 10 seconds to 10 minutes.

[0234] The film-shaped sintered material may be sintered under pressure by applying pressure to the film-shaped sintered material. For example, the pressure condition may be about 5 to 15 MPa.

[0235] In the above embodiment, an example is given of sintering joining of a chip of a film-shaped sintered material and a substrate, but the objects to be sintered joined with the film-shaped sintered material are not limited to those exemplified above, and sintering joining is possible for various articles that are sintered in contact with the film-shaped sintered material.

[0236] In the above embodiment, the film-shaped sintered material can be processed into a film-shaped sintered material of the same shape as the chip by dicing it together with the semiconductor wafer using a blade or the like, and a chip with the film-shaped sintered material can be manufactured. That is, in the chip with the film-shaped sintered material, the size (area) of the contact surface of the film-shaped sintered material and the contact surface of the chip are the same, but they may be different. For example, the substrate and the chip may be bonded together via the film-shaped sintered material in a state in which the contact surface of the film-shaped sintered material is larger than the contact surface of the chip. Specifically, a film-shaped sintered material of a desired size may be placed on the substrate, and a chip with a contact surface smaller than that of the film-shaped sintered material may be attached onto the film-shaped sintered material.

[0237] According to the manufacturing method of the embodiment, the device can be manufactured with high efficiency by using a film-shaped sintered material with a support sheet that has excellent dicing suitability. EXAMPLES

[0238] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to the following examples.

[0239] [Example 1] <Manufacture of Support Sheet> (Production of Pressure-Sensitive Adhesive Composition) A non-energy ray curable adhesive composition was produced with a solid content concentration of 30% by mass, containing 100 parts by mass (solid content) of an acrylic polymer, 0.8 parts by mass (solid content) of a tolylene diisocyanate adduct of trimethylolpropane ("Coronate L" manufactured by Tosoh Corporation) as a crosslinking agent, and a mixed solvent of methyl ethyl ketone, toluene and ethyl acetate as a solvent. The acrylic polymer is a copolymer having a weight average molecular weight of 600,000 and having methacryloyloxy groups in the side chains, obtained by copolymerizing 80 parts by mass of 2-ethylhexyl acrylate (2EHA) and 20 parts by mass of 2-hydroxyethyl acrylate (HEA) to a copolymer in which 2-methacryloyloxyethyl isocyanate (hereinafter abbreviated as "MOI") is added in an amount such that the total number of moles of isocyanate groups in the MOI is 0.8 times the total number of moles of hydroxyl groups derived from HEA in the acrylic polymer. (Manufacture of support sheets) A release film ("SP-PET381031" manufactured by Lintec Corporation, thickness 38 μm) in which one side of a polyethylene terephthalate film was treated for release by silicone treatment was used, and the pressure-sensitive adhesive composition obtained above was applied to the release-treated surface, followed by heating and drying at 120° C. for 2 minutes to form an energy ray-curable pressure-sensitive adhesive layer. At this time, the pressure-sensitive adhesive composition was applied under conditions set so that the thickness of the pressure-sensitive adhesive layer after drying would be 10 μm. A polypropylene (PP) film having a thickness of 80 μm was attached as a base film to the exposed surface of this pressure-sensitive adhesive layer to obtain a support sheet.

[0240] <Production of fired material composition> The components used in the preparation of the sintered material composition are shown below. Here, metal particles with a particle size of 100 nm or less are referred to as "sinterable metal particles." (Sinterable metal particle-containing paste material) Alko Nano Silver Paste ANP-4 (organic coated composite silver nano paste, manufactured by Applied Nanoparticles Research Institute: alcohol derivative coated silver particles, metal content 80% or more by mass, silver particles with an average particle size of 100 nm or less (sintered metal particles) 25% or more by mass) (Binder component) Acrylic polymer 1 (2-ethylhexyl methacrylate polymer, mass average molecular weight 260,000, Tg: -10°C) The Tg of the acrylic polymer 1 is a calculated value using the Fox formula.

[0241] A mixture of 86.8 parts by mass of sinterable metal particle-containing paste material and 13.2 parts by mass of binder component was mixed to obtain a sintered material composition. The sinterable metal particle-containing paste material is sold containing a high-boiling point solvent, and this remains in the film-shaped sintered material after coating or drying, so the components of the sinterable metal particle-containing paste material are listed including these. Considering that the solvent in the binder component evaporates during drying, the solid mass parts excluding the solvent component are shown.

[0242] <Production of film-shaped fired material> The sintered material composition obtained above was printed on one side of a 230 mm wide release film (thickness 38 μm, SP-PET381031, manufactured by Lintec Corporation) to give a coating diameter of 190 mm, and dried at 150°C for 10 minutes to obtain a film-like sintered material with a thickness of 40 μm.

[0243] <Production of film-shaped fired material with support sheet> A film-like sintered material printed in a circular shape with a diameter of 190 mm was attached to the adhesive layer surface of the above support sheet (after peeling off the release film), and the support sheet was cut into a circular shape with a diameter of 270 mm from the base film side, obtaining a film-like sintered material with support sheet in which a circular film-like sintered material and a release film were laminated on top of the support sheet having an adhesive layer on the base film.

[0244] Table 1 shows the configuration of each part.

[0245] [Example 2] A film-shaped sintered material with a support sheet of Example 2 was obtained in the same manner as in Example 1 above, except that the diameter of the film-shaped sintered material was changed as shown in Table 1.

[0246] [Example 3] A film-shaped sintered material with a support sheet of Example 3 was obtained in the same manner as in Example 1 above, except that the base film was changed to a 60 μm thick film made of ethylene-methacrylic acid copolymer (EMAA).

[0247] [Example 4] A film-shaped sintered material with a support sheet of Example 4 was obtained in the same manner as in Example 1 above, except that the base film was changed to a low-density polyethylene (LDPE) film having a thickness of 80 μm.

[0248] [Example 5] A film-like sintered material with a support sheet of Example 5 was obtained in the same manner as in Example 1 above, except that the base film was changed to a polyurethane (PU) film having a thickness of 100 μm.

[0249] [Example 6] The acrylic polymer was changed to a copolymer having a weight average molecular weight of 600,000, obtained by copolymerizing 80 parts by mass of 2-ethylhexyl acrylate (2EHA) and 20 parts by mass of 2-hydroxyethyl acrylate (HEA), the amount of crosslinking agent was changed as shown in Table 1, and the base film was changed to a polyvinyl chloride (PVC) film having a thickness of 80 μm. Except for this, the film-shaped sintered material with support sheet of Example 6 was obtained in the same manner as in Example 1 above.

[0250] [Example 7] A film-like sintered material with a support sheet of Example 7 was obtained in the same manner as in Example 1 above, except that the base film was changed to a polypropylene (PP) film having a thickness of 140 μm.

[0251] [Example 8] A film-like sintered material with a support sheet of Example 8 was obtained in the same manner as in Example 6 above, except that the base film was changed to a polyethylene terephthalate (PET) film having a thickness of 50 μm.

[0252] [Example 9] A film-shaped sintered material with a support sheet of Example 9 was obtained in the same manner as in Example 6 above, except that the base film was changed to a polyimide (PI) film having a thickness of 50 μm.

[0253] [Comparative Example 1] The film-shaped sintered material (without a support sheet) produced in Example 1 was used. The diameter of the film-shaped sintered material was changed as shown in Table 1 so that the diameter of the film-shaped sintered material exceeded the diameter of the inner circumference of the back surface of the wafer.

[0254] [Comparative Example 2] A film-shaped sintered material with a support sheet of Comparative Example 2 was obtained in the same manner as in Example 1 above, except that the diameter of each part was changed as shown in Table 1 so that the diameter of the film-shaped sintered material exceeded the diameter of the inner circumference of the back surface of the wafer.

[0255] <Measurement and Evaluation> (Measurement of the load when the support sheet is stretched by 5%) The film-like sintered material with support sheet obtained in each of the above examples and comparative examples was cut to a width of 15 mm and a length of 150 mm to prepare a test piece. After removing the release film from the test piece, it was set in a universal testing machine (Shimadzu Corporation, Autograph AG-IS 500N) so that the chuck distance was 100 mm, and measurements were performed at a speed of 200 mm / min in a 23°C, 50% RH environment. The load at 5% (i.e., 5 mm) elongation was read and used as the load at 5% elongation. When an energy ray-curable adhesive was used in the adhesive layer (Examples 1 to 5, Example 7, and Comparative Example 2), the measurement was performed on the test piece before the energy ray irradiation.

[0256] (Measurement of absorbance of support sheet) For the support sheets obtained in each of the above examples and comparative examples, an ultraviolet-visible-near infrared spectrophotometer (Shimadzu UV-3101PC) using an integrating sphere as a detector was used to measure the absorbance at a wavelength of 355 nm by irradiating light from the base film side of the support sheet.

[0257] (Evaluation of dicing suitability (adhesion, dicing, pick-up)) The film-shaped sintered material with support sheet obtained in each of the above examples and comparative examples (film-shaped sintered material in the case of Comparative Example 1) was stretched on a SUS ring frame with an inner diameter of 250 mm using a wafer bonding device RAD-2500m / 12 (manufactured by Lintec Corporation) at 23°C and 20 mm / s. Next, using a reduced pressure wafer attachment device RAD-2512m / 12 (manufactured by Lintec Corporation), the above film-like fired material was attached to the inner periphery (inner periphery of the back surface) of the surface side having the annular convex portion of the silicon wafer having an annular convex portion on the outer periphery under the conditions of a table temperature of 90°C and a differential pressure of 0.2 kPa, and the attachment property was evaluated. After that, the following rim dicing and dicing were performed, and the dicing suitability was evaluated. The shape of the silicon wafer is as follows: Inner thickness: 100μm -Thickness of annular protrusion: 400μm Wafer diameter: 200mm -Diameter of inner circumference of back surface of wafer: 194.8mm

[0258] [Applicability (circular convex part)] The film-shaped sintered materials obtained in each of the above examples and comparative examples were judged as A if they could be attached to the outer periphery of the inner periphery of the back surface (16a in Figure 4) without being damaged, and B if they could not be attached.

[0259] [Adhesiveness (wafer)] The film-shaped sintered materials obtained in each of the above examples and comparative examples were judged as A if they could be attached to the inner circumference of the back surface (inner circumference 16 of the back surface, metal film 18a in Figure 4) without damaging the film-shaped sintered materials, and B if they could not be attached.

[0260] [Rim dicing (ring-shaped convex part / blade)] Using a blade dicer DFD6361 (Disco Corporation), the annular convex portion on the outer periphery of the wafer was circle-cut under the following conditions: When an energy ray-curable adhesive was used for the adhesive layer, only the outer periphery was irradiated with ultraviolet light from the support sheet 2 side, and only the cut outer periphery of the wafer was peeled off and removed from the support sheet. Blade thickness: 25μm width (27HECC) Blade rotation speed: 30000 rpm Cutting conditions: The substrate film is cut to a depth of 20 μm from the wafer side. Cutting speed: 5deg / s Circle cut range: Wafer diameter - 6mmφ ·Cutting water amount: 1.5L / min Cutting water temperature: 24°C. If the circle cut was made without any damage to the inner circumference of the wafer, it was judged as A. If damage occurred to the inner circumference of the wafer, it was judged as B.

[0261] [Rim dicing (ring-shaped convex part, laser)] Using a laser dicer DFL7160 (manufactured by Disco Corporation), the annular convex portion on the outer periphery of the wafer was circle-cut under the following conditions: When an energy ray-curable adhesive was used for the adhesive layer, only the outer periphery was irradiated with ultraviolet light from the side of the support sheet 2, and only the cut outer periphery of the wafer was peeled off and removed from the support sheet. Circle cut range: Wafer diameter - 6mmφ Laser wavelength: 355nm Cutting speed: 40deg / s The case where the circle cut was made without any damage to the inner circumference of the wafer or complete breakage of the support sheet was rated as A, and the case where the inner circumference of the wafer was damaged or the support sheet was completely broken was rated as B.

[0262] [Dicing (chip blade)] Dicing was performed using a blade dicer DFD6362 (manufactured by Disco Corporation) under the following conditions. Dicing conditions: Each chip is 5mm x 5mm in size. Blade thickness: 25μm width (27HECC) Blade rotation speed: 30000 rpm Cutting conditions: The base film is cut to a depth of 20 μm from the side of the film-shaped fired material. Cutting speed: 30mm / s Cutting range: Wafer diameter + 20mmφ ·Cutting water amount: 1.5L / min ·Cutting water temperature: 24℃ The cases where the wafer and film-shaped sintered material could be diced were rated as A, and the cases where they could not be diced were rated as B.

[0263] [Dicing (chip laser)] Dicing was performed using a laser dicer DFL7160 (manufactured by Disco Corporation) under the following conditions. Dicing conditions: Each chip is 5mm x 5mm in size. Laser wavelength: 355nm Cutting speed: 100mm / s The case where the wafer and film-shaped fired material were completely cleaved without the support sheet breaking was rated as A, and the case where the support sheet broke completely was rated as B.

[0264] [Pickup] When an energy ray curable adhesive was used for the adhesive layer, ultraviolet light was irradiated from the side of the support sheet 2, and five chips having a size of 5 mm x 5 mm obtained by the above dicing were picked up in succession using a die bonder (BESTEM D02, manufactured by Canon Machinery) under conditions of a needle height of 0.3 mm and a pick-up speed of 5 mm / s. If 5 chips were picked up without any problems, it was judged as an A.

[0265] The above ultraviolet irradiation was performed using Adwill RAD2000m / 12, with a dominant wavelength of 365 nm and 200 mW / cm 2 , 200mJ / cm 2The adhesive layer was cured with ultraviolet light under the above conditions by irradiating it from the side of the support sheet 2.

[0266] The above evaluation results are shown in Table 1 below.

[0267] [Table 1]

[0268] In Examples 1 to 9, in which the diameter of the film-shaped sintered material satisfies the provision of being equal to or smaller than the diameter of the inner periphery of the back surface of the wafer, it can be seen that the film-shaped sintered material could be uniformly affixed to the inner periphery of the back surface of the wafer without being damaged, as shown in the evaluation item of attachment (wafer) in Table 1, in comparison with Comparative Examples 1 to 2, which do not satisfy the provision. In Comparative Examples 1 and 2, the diameter of the film-shaped sintered material is larger than the diameter of the inner periphery of the back surface of the wafer, so that damage to the film-shaped sintered material and uneven attachment were observed when attaching the film-shaped sintered material to the wafer. In addition, in Comparative Example 1, since there was no support sheet in the first place, the sintered material was fixed directly to the ring frame, and it was difficult to attach the film-shaped sintered material uniformly to the wafer without damaging it.

[0269] The film-shaped sintered materials with support sheets of Examples 1 to 6, in which the load at 5% elongation of the support sheet was 13 N / 15 mm or less, had good adhesion to the boundary between the inner surface 12 of the annular convexity and the inner circumference 16 of the back surface, and no damage occurred to the inner circumference of the wafer when the annular convexity was diced, and the evaluation results for the dicing (annular convexity) item were good.

[0270] In addition, from the evaluation results of the dicing (laser) item in Examples 6 and 9, it can be seen that when laser dicing with a wavelength of 355 nm is used for dicing, it is preferable that the absorbance of the support sheet at 355 nm is 0.22 or less in order to prevent the support sheet from breaking.

[0271] The configurations and combinations thereof in each embodiment are merely examples, and additions, omissions, substitutions, and other modifications of the configurations are possible without departing from the spirit of the present invention. Furthermore, the present invention is not limited to each embodiment, but is limited only by the scope of the claims. [Explanation of symbols]

[0272] 1...film-like sintered material, 2...support sheet, 3...base film, 4...adhesive layer, 5...ring frame, 6...substrate, 10...sinterable metal particles, 11...sintered body, 12...inner surface of annular convex portion, 13...circuit, 14...inner periphery of front surface, 15...surplus portion, 16...inner periphery of back surface, 16a...outer periphery of inner periphery of back surface, 17...annular convex portion, 18...wafer, 18a...metal film, 19...chip, 20...binder component, 30...release film, 70...projection, 71...lifting portion, 100...film-like sintered material with support sheet, 110...roll body, 120...laminated body, 130...chip with film-like sintered material, 140...apparatus, D1...diameter of film-like sintered material, D2...diameter of support sheet, D3...diameter of inner periphery of back surface, D4...diameter of wafer, P...unit, C1, C2...slit, LD...laser light irradiation

Claims

1. A film-like sintered material with a support sheet, comprising a support sheet having an adhesive layer on a base film, and a film-like sintered material provided on the adhesive layer, It is used to attach the film-shaped sintering material to the inner periphery of a wafer having an annular convex portion on the outer periphery, the inner periphery of the surface having the annular convex portion, The diameter of the film-shaped fired material is equal to or smaller than the diameter of the inner periphery of the wafer; The thickness of the support sheet is 120 μm or less, A film-shaped fired material with a support sheet, wherein the load of the support sheet at 5% elongation measured by the following measurement method is 13 N / 15 mm or less: Measurement method: The support sheet is cut into a test piece having a width of 15 mm and a length of 150 mm (however, if the pressure-sensitive adhesive layer is curable, the test piece is used before curing). The test piece is pulled under conditions of a chuck distance of 100 mm and a pulling speed of 200 mm / min in an environment of 23°C and 50% RH, and the load relative to the amount of displacement is measured.

2. A film-like sintered material with a support sheet, comprising a support sheet having an adhesive layer on a base film, and a film-like sintered material provided on the adhesive layer, The diameter of the film-shaped fired material is 130 to 146 mm, 180 to 196 mm, 280 to 296 mm, or 430 to 446 mm; The thickness of the support sheet is 120 μm or less, A film-shaped fired material with a support sheet, wherein the load of the support sheet at 5% elongation measured by the following measurement method is 13 N / 15 mm or less: Measurement method: The support sheet is cut into a test piece having a width of 15 mm and a length of 150 mm (however, if the pressure-sensitive adhesive layer is curable, the test piece is used before curing). The test piece is pulled under conditions of a chuck distance of 100 mm and a pulling speed of 200 mm / min in an environment of 23°C and 50% RH, and the load relative to the amount of displacement is measured.

3. 3. The film-shaped sintered material with support sheet according to claim 1, wherein the support sheet has an absorbance of 0.22 or less at a wavelength of 355 nm.

4. The film-shaped sintered material with a support sheet according to any one of claims 1 to 3, wherein the pressure-sensitive adhesive layer is energy ray curable.

5. 5. The film-shaped sintered material with a support sheet according to claim 4, wherein the adhesive layer contains an adhesive resin, and the adhesive resin has an energy ray-polymerizable unsaturated group in its side chain.

6. The adhesive layer contains an adhesive resin, and the adhesive resin contains a structural unit derived from a (meth)acrylate having an alkoxy group in a side chain with a carbon number of 8 to 18. A film-shaped sintered material with a support sheet according to any one of claims 1 to 5.

7. The film-shaped sintered material with a support sheet according to any one of claims 1 to 6, wherein the thickness of the film-shaped sintered material before sintering is 10 to 200 µm.

8. A film-shaped sintered material with a support sheet according to any one of claims 1 to 7 is laminated on a long release film with the film-shaped sintered material on the inside, The release film and the film-shaped sintered material with the support sheet are wound into a roll.

9. A laminate in which a film-shaped sintered material with a support sheet according to any one of claims 1 to 7 is attached to the inner peripheral portion of the surface side of a wafer having a ring-shaped convex portion on its outer periphery, and the support sheet, the film-shaped sintered material, and the wafer are stacked in this order.

10. A method for manufacturing an apparatus comprising the steps of (1) to (5) below in sequence: Step (1): A step of cutting the annular convex portion of the laminate according to claim 9; Step (2): Dicing the wafer and the film-shaped sintered material of the laminate from which the annular protrusion has been removed; Step (3): A step of peeling off the diced film-shaped sintered material and the support sheet to obtain a chip with the film-shaped sintered material; Step (4): A step of attaching the film-shaped sintered material of the film-shaped sintered material-attached chip to a surface of a substrate; Step (5): A step of firing the film-shaped fired material of the chip with the film-shaped fired material, and bonding the chip and the substrate.

Citation Information

Patent Citations

  • Method for processing wafer

    JP2007019379A

  • Wafer processing method

    JP2007266352A

  • Processing method of wafer

    JP2007287796A

  • Protective film forming sheet and method for fabricating semiconductor chip

    JP2012216625A

  • Pasty metal particulate composition, method for manufacturing solid metal or solid metal alloy, method for joining metallic members, method for manufacturing print wire board, and method for manufacturing bump for connecting electric circuits

    JP2014111800A