Adsorbent synthesis
The described process addresses impurity issues in zeolite production by calcining and leaching clay materials to form high-purity zeolites, utilizing mining tailings efficiently and reducing costs and environmental impact.
Patent Information
- Application Number
- JP2021571791
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-05
- Filing Date
- 2020-05-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-05-08
AI Technical Summary
Current industrial zeolite production methods face challenges with impurities in clay materials, leading to reduced zeolite quality and increased technical complexity, while mining tailings containing clay pose environmental and financial burdens.
A process involving calcination of clay materials to form amorphous material, followed by leaching with an alkaline solution to separate aluminum and silica, and crystallizing zeolite from the solution, effectively removing impurities and minimizing yield loss.
Produces high-purity zeolites from inexpensive and impure starting materials, reducing energy costs and environmental impact by utilizing mining tailings, and enhancing process efficiency through precise control of calcination and leaching steps.
Smart Images

Figure 0007571058000007 
Figure 0007571058000008 
Figure 0007571058000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an absorbent, more particularly, to a method for producing a zeolite. [Background technology]
[0002] Zeolites are microporous aluminosilicate materials. Zeolites are widely used commercially as adsorbents and catalysts. Zeolites used on a commercial scale are synthesized in industrial processes to ensure that the desired purity of the zeolite is achieved for use in commercial processes. Zeolites also occur in nature, but natural zeolites are usually found with impurity elements and minerals, making them less useful for commercial use.
[0003] Currently, the industrial production of zeolites involves forming solutions of aluminum and silicate salts and mixing the solutions together under conditions that result in the precipitation of the zeolite. In one example, a sodium aluminate solution is mixed with a sodium silicate solution at an alkaline pH (resulting from the aluminic acid in the solution) in the presence of seed particles and / or a template agent, with stirring and at a temperature of about 90° C. This causes the zeolite to precipitate.
[0004] Zeolites are crystalline microporous aluminosilicates with a three-dimensional framework made of SiO4 and AlO4. Zeolites contain molecular-sized cages that can have a large central pore formed by rings of different diameters. Zeolites have many applications in various fields such as laundry detergents, ion exchange, and water treatment due to their microporous properties. There are many different zeolites, some of which exist in nature and some that can be synthesized, and of these, synthetic zeolites, although more expensive, have a much wider range of applications than natural zeolites. One of the main research topics is the ability of zeolites to adsorb metal cations and remove them from wastewater streams due to their net negative charge, high porosity, and potential low cost. Most reports related to this issue have focused on zeolite LTA (also called zeolite 4A because of its pore size of 4 Å; in this specification, the two terms are used interchangeably). Zeolite 4A has been synthesized from coal fly ash (CFA) and is a zeolite that is capable of adsorbing metal cations from wastewater streams. 2+ The coal fly ash-synthesized zeolite A (LTA) showed very similar maximum adsorption capacities with a difference of 3 mg / g (50.45 and 53.45 mg / g for CFA and commercial, respectively) for Cu. 2+ and Zn 2+ The adsorption capacity achieved was obtained using 0.5 g of LTA, which is a very small amount when compared to the capacities of other synthetic zeolites or even for some natural zeolitic materials.
[0005] In general, as shown in Figure 1, the synthesis of zeolites from kaolinite-containing minerals requires two major steps: (i) amorphization -meaning the conversion of kaolinite to an amorphous solid (metakaolin) by thermal activation (>500 °C), and (ii) zeolitization -meaning the dissolution of the amorphous solid with caustic solution to synthesize zeolite. In the amorphous transformation step, temperature and time in the thermal activation process are the key process parameters. Studies on the amorphous transformation of kaolinite have been conducted by different groups, resulting in various views. Chandrasekhar investigated the effect of metakaolinization temperature on the formation of zeolite 4A from kaolinite. The results showed that a calcination temperature of 900 °C with a heating time of 1 h was optimal for the transformation of this clay into reactive metakaolin. Later, investigations reported that temperatures of 600-700 °C were the optimal range. For the zeolitization step, there are several sub-steps to achieve this hydrothermal synthesis, such as forming a slurry gel, heating the slurry gel to form zeolite crystals, and calcining the crystalline zeolite to remove the organic template when an organic template was added to the solution for phase and morphology control. As shown in Equations 1 and 2, the process of zeolitization is complex and is influenced by many factors, such as the silicate to aluminate ratio, starting materials, organic template, aging conditions, crystallization time and temperature, and alkalinity.
[0006] Most kaolin ores contain significant amounts of other mineral impurities, especially quartz, feldspar, and muscovite. These impurities often affect the quality of the clay and the final properties of the adsorption zeolite. To minimize the impurities, it is necessary to purify the kaolin for the synthesis of zeolites. The purification step in known processes may remove some of the impurities by mechanical separation to separate the coarse fraction. However, this increases the technical complexity of the process, while the remaining impurities still remain in the clay. Very few studies have looked at the removal of impurities, but generally the impurities end up in the final zeolite product. [ka] [ka]
[0007] With the progress associated with industrial development since the 20th century, the consumption of primary metals and coal has increased significantly in the past 100 years. The accumulation of mining tailings has caused serious environmental and financial burdens to industries and governments due to land occupation as well as soil and water pollution. Disposal or utilization or reclamation of these mining tailings has become an urgent issue. Recently, many research studies have been carried out to utilize these mining tailings as potential materials or feedstocks for recovering valuable components. Most mining tailings contain significant amounts of clay materials, e.g., kaolin minerals. And kaolin minerals are rich sources of Si and Al. Kaolinite (Al2[Si2O5](OH)4) is the major phase of the kaolin group of clay minerals. It is formed when anhydrous aluminosilicates found in feldspar-rich rocks are altered by weathering or hydrothermal processes. The crystal structure of kaolinite consists of planes (layers) of SiO4 tetrahedra joined by oxygen atoms parallel to the planes (layers) of AlO2(OH)4 octahedra.
[0008] Where a prior art publication is referred to in this specification, it will be expressly understood that this reference is not an admission that the publication forms part of the general knowledge in the art in Australia or any other country. Summary of the Invention
[0009] The present invention is directed to a process for producing zeolites that may at least partially overcome at least one of the above disadvantages or provide a useful or commercial choice to consumers.
[0010] In view of the foregoing, the invention in one aspect resides broadly in a process for producing a zeolite comprising: a) calcining a clay-containing material to form an amorphous material from the clay components in the clay material; b) Below 70℃ leaching the material from step (a) in a leach solution to produce a solution containing dissolved aluminium and dissolved silica and a solid residue; c) separating the solid residue from the solution; and d) crystallizing zeolite from the solution from step (c).
[0011] The process of the present invention utilizes clay-containing materials as feed for use in the production of zeolites. Clay materials are widespread, readily available, and inexpensive. Clay materials are also commonly found in mining tailings and overburden removed from mining operations. These sources promise to provide large amounts of inexpensive feed material for current processes while simultaneously adding value to otherwise problematic waste products.
[0012] Most clay materials typically include hydrated silicates of aluminum with impurities that may include quartzite, feldspar, muscovite, metal oxides, and organic matter. A wide variety of clay materials can be used in the present invention. Kaolin clays are particularly preferred. Types of clay that can be used in the present invention include kaolinite, (A l4Si4O 10 (OH)8), halloysite (Al2Si2O5(OH)4), and montmorillonite (Al4(Si4O 10 Other materials that contain kaolinite, halloysite, or montmorillonite phases and that can be used in the present invention include mining tailings such as mining tailings from kaolin mining, coal gangue kaolin, bentonite clays, and beausite mine or flotation tailings, coal flotation tailings, and beausite.
[0013] The firing step is used to convert the clay component of the clay material to an amorphous material. In one embodiment, the firing step includes using in situ high temperature XRD (X-ray diffraction) to characterize the phase transformation of the clay material. In one embodiment, one or more samples of the clay material are subjected to a programmed heating rate and time, and in situ XRD is used to obtain an XRD phase transformation pattern of the clay material. After obtaining a complete XRD phase transformation pattern, the optimal firing temperature and firing time are determined and a large-scale firing of the clay material is directed using conventional firing equipment (such as a furnace). This can avoid overheating the clay material in the firing step, which can advantageously minimize the energy costs required in the firing step.
[0014] In another embodiment, the calcination step involves heating the clay material to a predetermined temperature for a predetermined period of time. In some embodiments, the present invention encompasses an optional calcination step, preferably an optional calcination step that converts most or all of the clay material to an amorphous material.
[0015] The temperature used in the firing step may vary from 600°C to 900°C. The time for which the clay material is heated in the firing step may vary depending on the temperature; the higher the temperature, the less time required for firing. It should be mentioned that both temperature and time may vary depending on the mineralogical characteristics of different minerals and the efficiency of the firing equipment.
[0016] In one embodiment, the clay material is placed in a furnace in a firing step, and the furnace is heated to a temperature of between 600°C and 900°C, or between 625°C and 800°C, or between 650°C and 750°C.
[0017] In some embodiments, the clay material is heated in the calcination step for a period of 1 minute to 2 hours. As noted above, the higher the temperature used in the calcination step, the shorter the time required to achieve conversion of the clay material to the amorphous phase. In one embodiment, the heating time used in the calcination step is from 5 minutes to 1.5 hours, or from 8 minutes to 1.5 hours. Some times and temperatures that may be suitable for calcining kaolin materials include the following: 650℃ for 1.5 hours 700℃ for 0.5 hours 750℃ for 8 minutes.
[0018] In the calcination step, the clay material undergoes a dehydroxylation process and is converted to an amorphous material. If a kaolin clay material is used in the calcination step, the kaolinite is converted to metakaolin in the calcination step.
[0019] It has been found that impurity materials in the clay material fed to the calcination step are typically not affected by the calcination step. For example, the impurities quartz, muscovite, and feldspar remain essentially unchanged in the calcination step. In some embodiments, the calcination step is carried out at a temperature below the temperature at which quartz, feldspar, or muscovite undergo a phase transformation.
[0020] Following the calcination step, the amorphous material is removed from the furnace. In some embodiments, the amorphous material is allowed to cool to at least a temperature equivalent to the temperature at which the leaching step is performed. In other embodiments, the amorphous material is removed from the furnace and transported and / or placed in storage so that it can be subjected to leaching at a different location or at a later stage.
[0021] In the leaching step, the amorphous material recovered from the calcination step is leached in a leaching solution. This dissolves the aluminum and silicate components from the amorphous material. However, the impurity components present in the amorphous material do not dissolve and remain as a solid residue. It will be appreciated that the undissolved solid residue in the leaching step is in the form of particulate matter. The leaching step is generally carried out with stirring to ensure proper mixing between the solid material and the leaching solution, which improves the leaching rate.
[0022] In one embodiment, the leaching solution comprises an alkaline solution, which preferably comprises a sodium hydroxide solution, although other hydroxide solutions such as KOH may also be used. Sodium hydroxide is widely available and relatively inexpensive, and is therefore preferred for use in the leaching step.
[0023] In one embodiment, the alkaline solution comprises a hydroxide solution having a molar content of hydroxide ions of at least 1 M, or between 1 M and 6 M, or between 1 M and 5 M, or between 1 M and 4 M, or between 2 M and 6 M. In the experimental work carried out by the inventors, a sodium hydroxide solution with a concentration of 4 M was used as the leaching solution.
[0024] The leaching step may be carried out at a temperature at which precipitation of crystallization of zeolite or other desiliconization products (DSP) is inhibited or minimized. In this respect, solutions containing dissolved aluminum and dissolved silica or dissolved silicates are metastable and tend to precipitate solids from them. Such solutions tend to become less stable at higher temperatures. In the leaching step, undissolved solid residues including undissolved impurity particles are mixed with the leaching solution. Therefore, if there is any precipitation of zeolite or DSP in the leaching step, it tends to occur on the undissolved impurity particles. This material needs to be separated from the solution and can be discarded. Thus, precipitation of zeolite or DSP in the leaching step represents a loss of yield and needs to be avoided. DSP that may otherwise precipitate may include amorphous zeolite, sodalite, zeolite LTN, or other zeolite phases such as cancrinite.
[0025] In one embodiment, the temperature used in the leaching step is 70° C. below , or 50°C to 70°C. It has been found that at temperatures between 50°C and 70°C, leaching occurs at a rate high enough to be useful, and that precipitation of zeolite or DSP can be avoided by controlling the time for which leaching is carried out. For example, if leaching is carried out for less than an hour, such as 5 minutes to 1 hour, or 10 minutes to 30 minutes, or 15 minutes to 30 minutes, most of the aluminum and silica in the amorphous material will dissolve, but precipitation of zeolite or DSP is unlikely to occur. In this regard, the inventors have found that leaching temperatures between 50°C to 70°C, and times between 10 minutes to 30 minutes, result in good dissolution of the aluminum and silica components, with little or no formation of precipitated zeolite or DSP. In general terms, using leaching temperatures in the lower part of the range allows for longer leaching times to be used, while using leaching temperatures in the higher part of the range requires the use of shorter leaching times.
[0026] The inventors have also found that impurities such as quartz, muscovite, and feldspar do not dissolve in the leaching step, but rather remain as solid particles mixed with the leaching solution. Since these materials become impurities when incorporated into the zeolite product, the mixture of pregnant leaching solution and solid residue is subjected to a solid-liquid separation step to separate the undissolved solid residue from the pregnant leaching solution. Any suitable solid-liquid separation technique may be used. Filtration is just one example. Other possible solid-liquid separation steps that may be used include settling, decantation, centrifugation, cyclonic separation, hydrocyclonic separation, and the like. Those skilled in the art will appreciate that there are many different solid-liquid separation processes or techniques that may be used in this step.
[0027] The solid-liquid separation step results in a purified pregnant leach solution. The solid residue separated from the pregnant leach solution may be discarded or may be subjected to a second leaching step to further extract aluminium and silicate components therefrom, or subjected to further processing. For example, if the clay material contains bauxite, the solid residue from the leaching step will contain bauxite with a lower silica content, which may be sent to a Bayer process plant / alumina refinery to recover alumina therefrom. In other embodiments, the solid residue may be used as a building product, road base, or as feed to a fertiliser plant.
[0028] The purified pregnant leach liquor is then used to form a zeolite. The purified pregnant leach liquor contains dissolved aluminum and dissolved silicates. Because the pH of the pregnant leach liquor is alkaline, the dissolved aluminum is likely to be present as aluminates and the dissolved silica species are likely to be present as silicates. This solution may be processed using conventional techniques to form a zeolite.
[0029] In some embodiments, additional materials can be added to the pregnant leach solution to vary the ratio of Al to Si in the pregnant leach solution. For example, silica gel can be added to increase the amount of Si in the solution. Adjusting the ratio of Al to Si in the pregnant leach solution can provide some control over the zeolite product formed, e.g., zeolite X, A, sodalite, etc. Varying the process conditions during the crystallization stage can also provide some control over the product made. It is noted that in the prior art methods described herein, silica gel could not be added (except when NaOH was added) because it was difficult or impossible to disperse it.
[0030] In one embodiment, the pregnant leach liquor is heated to a temperature of 80° C. to 100° C. and agitated to cause precipitation of the zeolite. In one embodiment, the pregnant leach liquor is heated to a temperature of about 90° C. and agitated to cause precipitation of the zeolite. Agitation is used to keep the zeolite particles suspended in solution and to prevent the particles from agglomerating into overly large particles.
[0031] Residence times of 30 minutes to 10 hours, or 1 hour to 5 hours, or 1 hour to 4 hours may be used in the crystallization step.
[0032] It may also be possible to add templating agents, such as organic templating agents, seed particles, and / or other additives as are commonly used in conventional zeolite production in the zeolite crystallization step of the present invention.
[0033] Once the zeolite particles are formed, they are usually separated from the solution, washed, and dried. The zeolite may also be calcined, for example, to remove any organic templating agent.
[0034] The solution separated from the zeolite can be returned or recycled to the leaching step, or it can be used to perform a second leaching step on the solid residue removed from the first leaching step. In some embodiments, make-up leach solution is added to the solution recovered from the crystallization step. It may also be necessary to bleed off (remove) some of the leach solution to prevent the accumulation of impurities in the recycle solution.
[0035] The process embodiment of the first aspect of the invention allows zeolites to be formed from inexpensive and impure starting materials. The zeolites can have high purity because impurity components are removed after the leaching step and before the zeolite crystallization step. By avoiding precipitation of zeolite or DSP during the leaching step, yield losses are minimized. The solution recovered from the zeolite crystallization step can be recycled to the leaching step or the second leaching step, thereby further improving the economics of the process.
[0036] In a second aspect, the present invention provides a method for controlling the firing step, comprising the steps of firing a material at an elevated temperature, monitoring one or more phases of the material being fired during firing using in situ high temperature XRD, determining when a desired phase transformation in the material is complete, and reducing the heating in the furnace or removing the material from the furnace once the desired phase transformation in the material is complete.
[0037] In one embodiment of the second aspect of the invention, the method further comprises controlling the temperature of the furnace to increase the temperature of the furnace if a phase transformation in the material is not occurring, or is occurring at a rate determined to be too slow.
[0038] The method of the second aspect of the invention may be used to control the calcination of clay materials as part of a process for producing a zeolite according to the first aspect of the invention. The method of the second aspect of the invention may also be used to control the calcination of other materials, where calcination is used to effect a phase transformation in the material.
[0039] Using in situ high temperature XRD, it is possible to closely monitor the phase or phases of the material present during the calcination step. If the in situ high temperature XRD indicates that the desired phase transformation has completely occurred, the material may be removed from the furnace, or the heat in the furnace may be reduced to minimize heating costs during the calcination step.
[0040] The method of the second aspect of the invention provides significantly more accurate determination of both the time and temperature required to affect the desired phase transformation during firing. Thus, much more effective control of the firing step can be achieved, which can enhance the economics of the firing process.
[0041] Any of the features described herein may be combined in any combination with any one or more of the other features described herein within the scope of the present invention.
[0042] The reference to any prior art in this specification is not, and should not be construed as, an acknowledgment or any form of suggestion that the prior art forms part of the common general knowledge. [Brief description of the drawings]
[0043] Various embodiments of the present invention will now be described with reference to the following drawings: [Figure 1] 1 is a flow sheet of a prior art process for synthesizing zeolite from kaolin mineral. [Diagram 2] 1 is a flow sheet of a process for synthesizing zeolite from kaolin mineral according to an embodiment of the present invention. [Diagram 3] FIG. 1 shows in situ XRD patterns of kaolinite heat-treated at 550° C. to 675° C. [Figure 4] FIG. 1 shows SEM images of (a) kaolin sample and (b) metakaolin after heat treatment at 650° C. [Diagram 5]FIG. 5 is a graph of aqueous silicate concentration versus time during kaolin leaching (FIG. 5a) and metakaolin leaching (FIG. 5b). [Figure 6] FIG. 1 shows XRD patterns for amorphous phase and zeolite LTA using kaolin sample heated at 650° C. [Figure 7] FIG. 1 shows SEM images of (a) amorphous zeolite, (b) zeolite LTA, cubic, Pm3m, and (c) sodalite, wool spherical particles, P43n. [Figure 8] FIG. 1 shows in situ XRD patterns of heat treated feed material in Example 2. [Figure 9] Figure 9 shows an XRD pattern for the zeolite-containing product formed in Example 2. Figure 9 also shows an XRD pattern for the zeolite-containing product formed according to a prior art method, as described herein. [Figure 10] FIG. 2 shows the XRD pattern for zeolite LTA formed in Example 2. [Figure 11] FIG. 1 shows XRD patterns for the kaolinite feed and calcined feed materials in Example 3. [Figure 12] FIG. 2 shows an XRD pattern for the zeolite-containing product formed in Example 3. [Figure 13] FIG. 1 shows XRD patterns for bauxite feed and calcined feed in Example 4. [Figure 14] FIG. 1 shows an XRD pattern for the zeolite-containing product formed in Example 4. [Figure 15] FIG. 13 shows XRD patterns for the coal flotation tailings feed and the calcined feed in Example 5. [Figure 16] FIG. 1 shows an XRD pattern for the zeolite-containing product formed in Example 5. [Figure 17] FIG. 2 shows an SEM micrograph of the zeolite product obtained in Example 2. [Figure 18]FIG. 2 shows an SEM micrograph of the zeolite product obtained in Example 3. [Figure 19] FIG. 1 shows an SEM micrograph of the zeolite product obtained in Example 4. [Figure 20] FIG. 1 shows an SEM micrograph of the zeolite product obtained in Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0044] It will be understood that the following examples are provided for the purpose of illustrating preferred embodiments of the present invention, and therefore, those skilled in the art will understand that the present invention should not be considered limited solely to the features as described in the examples.
[0045] FIG. 2 shows a flow sheet of a process for synthesizing zeolites from clay minerals according to an embodiment of the present invention. In the flow sheet of FIG. 2, kaolin mineral 10 is fed to a calcination step 12 carried out in a furnace. The furnace is operated at a temperature between 600° C. and 750° C. and the kaolin mineral is kept in the furnace for a period between 30 minutes and 1 hour. This converts the kaolinite to metakaolin. The metakaolin is fed to a leaching step 14 where it is mixed with a 4M sodium hydroxide solution 16. In the leaching step 14, the aluminum and silicon components in the metakaolin are dissolved in solution to form an aluminosilicate solution (likely consisting of aluminates and silicates in solution). Impurities such as quartz, muscovite, feldspar, etc. do not dissolve in the leaching step 14. A solid-liquid separation step 15, such as filtration, is used to separate the pregnant leach liquor 18 from the solid impurities 20.
[0046] The pregnant leach liquor 20 is then treated in a crystallization step 22 to form zeolites. The crystallization step 22 is carried out at a temperature of 80-100°C for 1-4 hours with stirring to cause precipitation of the zeolites. Other components that may be used in zeolite crystallization, such as template agents, seed particles, etc., may also be added to the crystallization step 22. Additional materials 23 may be added to vary the Al to Si ratio. For example, silica gel may be added. The zeolite particles are then separated from the liquid phase and the zeolite particles are recovered at 24. The zeolite particles may be washed and dried as necessary and calcined to remove the organic template agent if required. The desilicate solution 26 is recycled to the leaching step 14. In another embodiment, the solid impurities 20 may be mixed with the desilicate solution 26 to further leach aluminum and silicon components from the solid impurities. Where leachate recycling is used, it may be necessary to add make-up leachate and to obtain a bleed stream from the recycled leachate to prevent the build-up of unwanted impurities.
[0047] Example 1 In this example, zeolites were synthesized according to one embodiment of the present invention. Kaolinite (composition shown in Table 1), sodium hydroxide (2.2 wt% Na2CO3), and aluminum hydroxide (99.4%) were supplied by Sigma-Aldrich. Lead nitrate (99%) and copper(II) nitrate (98%) were supplied by ThermoFisher Scientific, and cobalt(II) chloride hexahydrate (98%) was supplied by Sigma-Aldrich. [Table 1]
[0048] Zeolite Synthesis Kaolin (about 20 grams) was placed in a muffle furnace preheated to the target temperature (650°C) for 0.5 hours to obtain the calcined product (amorphous metakaolin). Then, 2.5 g of the calcined product was added to a 250 ml glass beaker (with magnetic stirrer) containing 200 ml of 4M NaOH solution preheated to 60°C. The slurry was allowed to infuse for 15 or 30 minutes and then filtered at the same temperature. 0.2 ml of the filtered liquid solution was sampled and diluted 10 times for ICP analysis. The filtered liquid solution was transferred to a plastic bottle (250 ml) with two steel balls for mixing. The container was then placed in a water bath preheated to the target temperature (90°C) with a stirring speed of 500 rpm for 4 hours, which is sufficient time for the complete crystallization and formation of zeolite LTA. Based on the chemical composition of the liquid solution, it may be necessary to use additional gibbsite (Al(OH)3) to bring the Al / Si molar ratio up to 1. After crystallization, the slurry was filtered. The solid sample was washed and dried in an oven overnight for future adsorption testing. The filtrate liquid solution was recycled for use in the next round of kaolin leaching. 0.2 ml of the filtrate was sampled and diluted 10 times for ICP analysis. Based on the chemical composition of the liquid solution, it may be necessary to use additional amounts of NaOH to make up a caustic solution up to 4M. For comparison, we synthesize sodalite (SOD) samples and amorphous zeolite samples using kaolin or metakaolin feed samples.
[0049] Sample characterization In situ high-temperature XRD analysis was performed using Rigaku Smartlab to determine the phase transformation of kaolin. Crushed solid powder was added to a small container made of corundum. The loaded container was placed on a sampler holder and sealed by a dome. The heating rate was set at 50 °C / min. The hold time per scan at each temperature was 10 min before the X-ray scan time, which was approximately 15 min to cover the 2θ angle range of 5-40 ° using Cu Kα radiation (λ = 1.5406 A) at 40 kV with a scan rate of 0.05 ° per second.
[0050] Other crystalline solid phases were identified by X-ray diffraction (XRD) using a Bruker D8 Advance XRD equipped with a LynxEye detector and Cu Kα radiation (λ = 1.5406 A) at 40 kV with a scan rate of 0.05° per second over the 2θ angle range of 5-40°. The 2014 PDF database from BRUKER was used for the identification of reflections. The morphology of the solid particles was observed by scanning electron microscopy (SEM, HITACHI SU3500) using an accelerating voltage of 5 kV and a spot size of 30.
[0051] Characterization of solution samples was performed using inductively coupled plasma atomic emission spectrometry (ICP-AES).
[0052] result Thermal activation of kaolin. Accurately determining the kaolin-to-amorphous transition temperature is particularly useful in synthesis processes related to energy costs. Most previous researchers utilize thermogravimetric analysis (TGA) to determine the temperature and time of phase transition. Previously, most investigations implemented the thermogravimetric (TG) method to estimate the weight loss of kaolin samples. Based on the chemical formula shown in Equation 3, the weight loss is approximately 14% if pure kaolin is fully dehydroxylated. However, most kaolin samples contain impurities, and the weight loss technique is not very accurate. This results in thermal activation usually being reported over a wide temperature range of 550-1000 °C, which typically overestimates the calcination time from 1 to 12 h. Here, we implemented an in situ high-temperature XRD methodology to monitor the phase transition of kaolin with programmed heating rates (5-200 °C / min) and short scan times (5-16 min). Instead of measuring the weight loss, the intensity change of the major phase peaks in the (001) and (002) planes of kaolin was recorded at different temperatures and heating times. The kaolin samples do not change significantly below 500 °C. As shown in Figure 3, the 550 °C sample still has the characteristic peaks of kaolinite and impurity anatase (2θ = 25.33 °). The intensity of the peaks of the kaolinite crystal planes decreases with increasing temperature. At 625 °C, the peaks in the range of 20-22 ° and 35-40 ° for the kaolin phase were not detectable, while the peaks of the (001) and (002) crystal planes are still detectable. At 650 °C, the XRD pattern shows only anatase peaks. This indicates that kaolinite has been completely dehydroxylated into the X-ray amorphous phase. The dehydroxylation to the amorphous phase that occurs in the temperature range of 600-675 °C is shown in Equation 3. Al2[Si2O5](OH)4→Al2O3·2SiO2+2H2O…………………………(3)
[0053] SEM images show that the metakaolin has begun to lose the edge sheet structure of kaolin as shown in Figure 4, but still has a layered structure of crystals indicating a lack of long range crystal structure.
[0054] Hydrothermal synthesis of zeolites In the synthesis process used in this example, kaolinite or metakaolin is dissolved in highly alkaline solutions and then reprecipitated as insoluble sodium aluminate silicates known as zeolites based on Equations 1 and 2.
[0055] Figure 5a shows the leaching / dissolution of kaolin feed material with 4M NaOH solution. As can be seen from Figure 5, kaolin dissolves very slowly in the leachate. As kaolin dissolves, the silicate concentration in the solution increases. However, the desilicate product (DSP) starts to precipitate after about 50 minutes, which reduces the silicate concentration in the solution due to the precipitation of DSP. In contrast, when metakaolin is sent to the leaching test, it dissolves very quickly and almost complete dissolution is obtained after 10-15 minutes. DSP starts to precipitate after about 25-30 minutes, and the maximum concentration of silica in the solution is obtained at 10-30 minutes. Thus, by leaching metakaolin at 70°C for 10-30 minutes, the loss of silicate to DSP in the leaching step can be avoided. It will be appreciated that all DSP that precipitates in the leaching step is precipitated on solid impurities that are not soluble in the leaching solution. Since in order to obtain pure zeolite, the undissolved solid impurities must be separated from the leaching solution prior to zeolite crystallization, the DSP that precipitates during the leaching step will precipitate on the solid impurity particles, which represents a loss in yield. In Figure 5, the silicate concentration in the solution (expressed as g / L SiO2) is monitored and the kaolin and DSP are calculated from the mass balance.
[0056] Zeolite LTA is the only phase in the case of the zeolite made from the feed material where the solid sample was heated at 650° C., as shown in FIG 6. SEM images in FIG 7 show the cubic structure of zeolite LTA shape.
[0057] Example 2 In this example, materials having the compositions as set forth in Table 2 were used as feed materials. [Table 2]
[0058] The feed material was subjected to the following treatments: Heat activation step: 25 grams of the sample was placed in a ceramic container and transferred to a muffle furnace, which was then preheated to a target temperature of 750° C. for 1.5 hours. Figure 8 shows the XRD patterns for the feed material and the calcined feed material.
[0059] Leaching and aging stages: Synthetic caustic solution (50 mL) with a caustic concentration of 4 M was magnetically stirred at 300-500 rpm in a 150 mL Erlenmeyer flask and sealed with parafilm to prevent excessive liquid loss due to evaporation. The solution was heated by a hotplate equipped with a feedback controller. When the set temperature of 60 °C was reached, the activated solid sample (1.5 g) was added to the heated solution. Once the leaching reaction was complete in 1 h, the solid and liquid were separated by vacuum filtration. The filtrate solution was used for precipitation of the zeolite 4A product.
[0060] Crystallization stage: The solution obtained from the leaching test was transferred into 100 or 200 ml Teflon bottles or steel containers. To synthesize different types of zeolites, additional silica or aluminum sources are added to the solution to balance the SiO2 / Al2O3 molar ratio. The bottles were then placed in a water bath at a temperature of 90°C for 2-4 hours. The solid was filtered and washed with deionized water until the pH value was less than 9. The solid product was dried in an oven at 105°C for 2-4 hours.
[0061] Figure 9 shows the XRD pattern for the zeolite-containing product formed in Example 2. Figure 9 also shows the XRD pattern for the zeolite-containing product formed according to the prior art method, as described herein. As can be seen from Figure 9, the zeolite-containing product formed according to an embodiment of the present invention has much lower levels of other components than the zeolite-containing product formed according to the prior art method. Figure 10 shows the XRD pattern for the zeolite LTA formed in Example 2.
[0062] Example 3 In this embodiment, the table 3 A material having the composition as described in was used as the feed material. [Table 3]
[0063] The feed material was subjected to the following treatments: Heat activation step: Five grams of sample was placed in a ceramic container and transferred to a muffle furnace, which was subsequently preheated to a target temperature of 650°C for 1 h.
[0064] Leaching and aging stages: Synthetic caustic solution (50 mL) with a caustic concentration of 4 M was magnetically stirred at 300-500 rpm in a 150 mL Erlenmeyer flask and sealed with parafilm to prevent excessive liquid loss due to evaporation. The solution was heated by a hotplate equipped with a feedback controller. Once the set temperature of 70 °C was reached, the activated solid sample (1 g) was added to the heated solution. Once the leaching reaction was complete in 0.5 h, the solid and liquid were separated by vacuum filtration. The filtrate solution was used for precipitation of the zeolite 4A product.
[0065] Crystallization stage: The solution obtained from the leaching test was transferred into 100 or 200 ml Teflon bottles or steel containers. To synthesize different types of zeolites, additional silica or aluminum sources are added to the solution to balance the SiO2 / Al2O3 molar ratio. The bottles were then placed in a water bath at a temperature of 90°C for 2 hours. The solid was filtered and washed with deionized water until the pH value was less than 9. The solid product was dried in an oven at 105°C for 2-4 hours.
[0066] Figure 11 shows the XRD patterns for the kaolinite feed material and the calcined kaolinite. Figure 12 shows the XRD pattern of the zeolite formed in this example. The zeolite is primarily zeolite LTA.
[0067] Example 4: This example uses a high silica bauxite as the feedstock. The high silica bauxite had the composition shown in Table 4. [Table 4]
[0068] The high silica bauxite feed consisted of gibbsite, boehmite, hematite, kaolinite, quartz, anatase, and organic matter. The feed was subjected to the following treatments:
[0069] Heat activation step: 10 grams of the sample was placed in a ceramic container and transferred to a muffle furnace, which was then preheated to a target temperature of 650° C. for 1 hour. Figure 13 shows the XRD patterns for the bauxite feed material and the calcined bauxite feed material.
[0070] Leaching and aging stages: Synthetic caustic solution (50 mL) with a caustic concentration of 4 M was magnetically stirred at 300-500 rpm in a 150 mL Erlenmeyer flask and sealed with parafilm to prevent excessive liquid loss due to evaporation. The solution was heated by a hotplate equipped with a feedback controller. When the set temperature of 60 °C was reached, the activated solid sample (2.5 g) was added to the heated solution. Once the leaching reaction was complete in 0.5 h, the solid and liquid were separated by vacuum filtration. The filtrate solution was used for precipitation of the 4A product.
[0071] With this feedstock, the solid impurities 20 resulting from the leaching step 14 shown in Figure 2 include desilicate bauxite which can be fed to the Bayer process plant / alumina refinery. Because the silica has been removed from the bauxite, some processing difficulties that arise in the Bayer process plant / alumina refinery due to having excess silica in the bauxite feed, such as excess sodium hydroxide consumption and precipitation of the desiliconization product on heat exchange surfaces causing fouling, can be alleviated.
[0072] Crystallization stage: The solution obtained from the leaching test is transferred into 100 or 200 ml Teflon bottles or steel containers. To synthesize different types of zeolites, additional silica or aluminum sources are added to the solution to balance the SiO2 / Al2O3 molar ratio. The bottles were then placed in a water bath at a temperature of 90°C for 2 hours. The solid was filtered and washed with deionized water until the pH value was less than 9. The solid product was dried in an oven at 105°C for 2-4 hours.
[0073] Figure 14 shows the XRD pattern of the zeolite formed in this example. The zeolite is primarily zeolite LTA.
[0074] Example 5 In this example, coal flotation tailings were used as the feed material. Although a full analysis of this feed material has not been completed, it is expected to contain approximately 20% Al2O3. The coal flotation tailings were processed in the following steps: Heat activation step: 15 grams of the sample was placed in a ceramic container and transferred to a muffle furnace, which was subsequently preheated to a target temperature of 650° C. for 1 hour. Figure 15 shows the XRD patterns for the coal tailings feed product and the calcined coal tailings.
[0075] Leaching and aging stages: Synthetic caustic solution (50 mL) with a caustic concentration of 4 M was magnetically stirred at 300-500 rpm in a 150 mL Erlenmeyer flask and sealed with parafilm to prevent excessive liquid loss due to evaporation. The solution was heated by a hotplate equipped with a feedback controller. When the set temperature of 70 °C was reached, the activated solid sample (1.5 g) was added to the heated solution. Once the leaching reaction was complete in 0.5 h, the solid and liquid were separated by vacuum filtration. The filtrate solution was used for product precipitation.
[0076] Crystallization stage: The solution obtained from the leaching test is transferred into a 100 or 200 ml Teflon bottle or steel container. To synthesize different types of zeolite, additional silica or aluminum source is added to the solution to balance the SiO2 / Al2O3 molar ratio. The bottle was then placed in a water bath at a temperature of 90°C for 2 hours. The solid was filtered and washed with deionized water until the pH value was less than 9. The solid product was dried in an oven at 105°C for 2-4 hours. Figure 16 shows the XRD pattern of the zeolite formed in this example. The zeolite is mainly zeolite LTA.
[0077] 17-20 show SEM micrographs of the zeolite products obtained in Examples 2, 3, 4, and 5, respectively.
[0078] The zeolites produced according to the present invention can be used to remove heavy metals from solution, and in fact, the inventors have performed experimental tests showing that the zeolites produced according to the present invention can be used to remove heavy metal ions, such as Cu, Pb, and Co, from solution.
[0079] The zeolites produced according to the present invention can also be used in any other applications for which zeolites are known to be useful. Examples include gas separation, detergents, ethanol drying, water and heavy metal absorption, and catalysis. Those skilled in the art will appreciate that the end use of the zeolites produced according to the present invention is not limited to any of the above applications, but can extend to any possible application of zeolites.
[0080] In this specification and the claims (if any), the word "comprising" and its derivatives including "comprises" and "comprise" include each of the listed integers but do not exclude the inclusion of one or more additional integers.
[0081] References throughout this specification to "one embodiment" or "an embodiment" mean that a particular feature, structure, or characteristic described in connection with the embodiment is included in at least one embodiment of the invention. Thus, the appearances of the phrase "in one embodiment" or "in an embodiment" in various places throughout this specification do not necessarily all refer to the same embodiment. Furthermore, the particular features, structures, or characteristics may be combined in any suitable manner in one or more combinations.
[0082] In compliance with the statute, the invention has been described in language more or less specific to structural or systematic features. It is to be understood that the invention is not limited to the specific features shown or described, since the means described herein include preferred forms of carrying out the invention. The invention is therefore claimed in any of its forms or modifications within the proper scope of the appended claims (if any) as appropriately interpreted by those skilled in the art.
Claims
1. 1. A process for producing zeolite LTA comprising: a) calcining a clay material to form an amorphous material from clay components in the clay material; b) leaching the amorphous material from step (a) in a leach solution at or below 70°C to produce a solution containing dissolved aluminium and dissolved silica and a solid residue; c) separating the solid residue from the solution; d) crystallizing zeolite LTA from said solution from step (c).
2. The clay material is kaolin clay, kaolinite (Al 4 S 4 O 10 (OH) 8 ), Halloysite (Al 2 S 2 O 5 (OH) 4 ) and montmorillonite (Al 4 (Si 4 O 10 ) 2 (OH) 4 *xH 2 O)), mining tailings, mining tailings from kaolin mining, coal gangue kaolin, bentonite clay and bauxite mine or flotation tailings, coal flotation tailings and bauxite.
3. 3. The process of claim 1 or claim 2, wherein step (a) comprises: characterizing the phase transformations of the clay material using in situ high temperature XRD (X-ray diffraction) by subjecting one or more samples of the clay material to a programmed heating rate and time; obtaining an XRD phase transformation pattern of the clay material using in situ XRD; and determining an optimal firing temperature and firing time.
4. 3. The process of claim 1 or 2, wherein said step (a) involves calcining the clay material to a predetermined temperature for a predetermined period of time.
5. The process of any one of claims 1 to 4, wherein the temperature used in step (a) is from 600°C to 900°C, or from 625°C to 800°C, or from 650°C to 750°C.
6. 6. The process of any one of claims 1 to 5, wherein the clay material is subjected to heating in step (a) for a period of from 1 minute to 2 hours, or from 5 minutes to 1.5 hours, or from 8 minutes to 1.5 hours.
7. 7. The process according to any one of claims 1 to 6, wherein a kaolin clay material is used in step (a), and kaolinite in the kaolin clay material is converted to metakaolin in step (a).
8. 8. The process of any one of claims 1 to 7, wherein the impurities quartz, muscovite and feldspar remain unchanged in step (a).
9. 9. The process according to any one of claims 1 to 8, wherein in step (b), the amorphous material recovered from step (a) is leached in a leach solution to dissolve the aluminium and silicate components from the amorphous material, whereby impurity components present in the material from step (a) are not dissolved and remain as a solid residue.
10. The process of any one of claims 1 to 9, wherein the leaching solution comprises an alkaline solution.
11. 11. The process of claim 10, wherein the alkaline solution is a sodium hydroxide solution or a potassium hydroxide solution.
12. 12. The process of claim 10 or 11, wherein the alkaline solution comprises a hydroxide solution having a molar hydroxide ion content of at least 1M, or from 1M to 6M, or from 1M to 5M, or from 1M to 4M, or from 2M to 6M.
13. 13. The process of any one of claims 1 to 12, wherein step (b) is carried out at a temperature at which precipitation of zeolite or other desiliconization products (DSP) crystallization is inhibited or minimized.
14. The process according to any one of claims 1 to 13, wherein the temperature used in step (b) is from 50°C to 70°C.
15. 15. The process of any one of the preceding claims, wherein impurities including quartz, muscovite and feldspar do not dissolve in step (b) and remain as solid particles mixed with the leach solution, and the mixture of pregnant leach solution and solid residue is subjected to a solid-liquid separation step to separate undissolved solid residue from the pregnant leach solution.
16. 16. The process of any one of the preceding claims, wherein step (c) results in a purified pregnant leach solution, and the solid residue separated from the pregnant leach solution is either discarded or subjected to a second leaching step to extract further aluminium and silicate components therefrom, or subjected to further processing.
17. The process of any one of the preceding claims, wherein the solution from step (c) comprises a purified pregnant leach solution containing dissolved aluminium and dissolved silicates.
18. 20. The process of claim 17, wherein an additional material is added to the pregnant leach solution to vary the ratio of Al to Si in the pregnant leach solution.
19. 20. The process of claim 18, wherein silica gel is added to increase the amount of Si in the pregnant leach liquor.
20. A process as claimed in any one of claims 17 to 19, wherein the pregnant leach liquor is heated to a temperature of from 80°C to 100°C, or from 90°C to 100°C, and stirred to cause precipitation of zeolite LTA.
21. 21. The process of claim 20, wherein agitation is used to keep the particles of zeolite LTA suspended in the solution and to prevent the particles from agglomerating into excessively large particles.
22. 22. The process of any one of claims 1 to 21, wherein a residence time of from 30 minutes to 10 hours, or from 1 hour to 5 hours, or from 1 hour to 4 hours is used in step (d).
23. A process according to any one of the preceding claims, wherein the particles of zeolite LTA formed in step (d) are separated from the solution, washed and dried.
24. 24. The process according to claim 23, wherein the solution separated from the zeolite LTA is returned or recycled to step (b) or used to carry out a second leaching step on the solid residue obtained in step (c).
25. 25. The process of claim 24, wherein make-up leachate is added to the solution recovered from step (d) and / or a portion of the leachate is bled off to prevent accumulation of impurities in the recycled solution.
26. 26. The process of any one of claims 1 to 25, wherein step (b) has a residence time of less than 1 hour.
Citation Information
Patent Citations
Method for synthesizing pure 4A zeolite, P-shaped zeolite and sodalite with concavo-convex attapulgite clay
CN101618880A
Method for preparing 4A zeolite from gangue serving as raw material through two-step hydrothermal synthesis
CN108483460A
Method for producing aluminum hydroxide by roasting bauxite at low temperature
CN109279633A
Synthesis of 4A zeolite with kaolinite and preparing process thereof
CN1124716A
Process for preparing improved zeolite
JP1978043098A