Hemostatic powder
A hemostatic powder using electrophilic polyoxazoline and nucleophilic polymer particles forms a strong gel to stop bleeding by binding to proteins and tissues, addressing the limitations of existing agents in controlling bleeding, especially in anticoagulated blood.
Patent Information
- Application Number
- JP2021577546
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-12
- Filing Date
- 2020-07-09
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-07-09
AI Technical Summary
Existing hemostatic agents struggle to effectively control bleeding, especially in anticoagulated blood, and often require multiple applications due to the formation of weak clots that can be dislodged, leading to further bleeding.
A hemostatic powder comprising electrophilic polyoxazoline and nucleophilic polymer particles that form a strong gel upon contact with blood, binding to proteins and tissues to create a stable clot, with the particles being combined using a non-aqueous granulation method to minimize cross-linking and degradation.
The powder rapidly forms a strong, stable gel that adheres to tissues, effectively stopping bleeding and allowing for easy distribution and additional application if needed, even in anticoagulated conditions.
Smart Images

Figure 0007571065000001 
Figure 0007571065000002 
Figure 0007571065000003
Abstract
Description
Detailed Description of the Invention
[0001] [Technical field of the invention] The present invention provides a hemostatic powder comprising at least 10 wt.% particle aggregates, an electrophilic polyoxazoline particle comprising an electrophilic polyoxazoline carrying at least three reactive electrophilic groups capable of reacting with amine groups in blood under the formation of covalent bonds; Nucleophilic polymer particles containing a nucleophilic polymer bearing at least three reactive nucleophilic groups capable of reacting in the presence of water with the reactive electrophilic groups of the electrophilic polyoxazoline under formation of a covalent bond between the electrophilic polyoxazoline and the nucleophilic polymer. The present invention relates to a hemostatic powder comprising:
[0002] When the hemostatic powder of the present invention is applied to the site of bleeding, the particle aggregates rapidly form a gel and simultaneously bind to proteins present in the blood and surrounding tissue, thereby accelerating hemostasis.
[0003] [Background of the invention] Hemostasis is a tightly regulated process that maintains blood flow through the vascular system while at the same time generating a thrombotic response to tissue injury. Maintaining hemostasis requires a complex interplay between the vessel wall, platelets, and the coagulation and fibrinolytic systems. There are two main phases in hemostasis: the primary (i.e., cellular) and the secondary (i.e., humoral) phase.
[0004] Primary hemostasis begins immediately after endothelial rupture and is characterized by vasoconstriction, platelet adhesion, and the formation of a soft coagulation plug. After injury occurs, a temporary local contraction of vascular smooth muscle occurs, slowing blood flow and promoting platelet adhesion and activation. Within 20 seconds of injury, circulating von Willebrand factor deposits on the subendothelium at the site of injury and adheres to glycoproteins on the platelet surface. As platelets adhere to the injured surface, they are activated by contact with collagen, exposing receptors that bind circulating fibrinogen. A soft plug of clotted platelets and fibrinogen is formed. This hemostatic phase is short-lived, and the soft plug can be easily detached from the injured surface.
[0005] The soft platelet plug is stabilized during secondary hemostasis to form a clot. Vasoconstriction and the resulting reduction in blood flow are maintained by serotonin, prostaglandins and thromboxanes secreted by platelets, while the coagulation cascade is initiated. The coagulation cascade is a series of dependent reactions involving multiple plasma proteins, calcium ions and blood platelets that convert fibrinogen into fibrin. Clotting factors are produced by the liver and circulate in an inactive form until the coagulation cascade is initiated. Each step of the cascade is then initiated and completed by a series of sequential and dependent activation reactions of coagulation factors. In the final step, thrombin converts fibrinogen, a soluble plasma protein, into fibrin, an insoluble protein, and simultaneously converts factor XIII into factor XIIIa. This conversion of factors stabilizes fibrin and causes cross-linking of fibrin monomers to generate a stable clot.
[0006] During surgery, it is important to maintain a delicate balance between bleeding and clotting to ensure a continuous flow of blood to the tissues at the surgical site without excessive blood loss in order to optimize surgical success and patient outcomes. Continuous bleeding from the widely distributed small capillaries or small venules during surgery can obscure the surgical field, prolong the operation time, increase the risk of physiological complications, and expose the patient to risks associated with blood transfusions.
[0007] Surgeons have many options for controlling bleeding, including mechanical and thermal techniques and devices, as well as medications and topical agents.
[0008] One of the earliest topical hemostatic agents was cotton in the form of gauze sponges. Such materials thicken blood and clotting products by physical adsorption, but are not absorbable by the body, and upon removal, clots may become dislodged, leading to further bleeding. Since then, absorbable topical hemostatic agents have been developed and have become useful adjunctive therapies when traditional methods of hemostasis are ineffective or impractical. Topical hemostatic agents can be applied directly to the bleeding site and prevent continuous uninterrupted bleeding. Hemostasis using topical agents also avoids the adverse effects of systemic hemostatic agents, such as "unwanted" clots. Furthermore, in surgical procedures where the amount of blood loss is unpredictable, topical hemostasis can be used sparingly when blood loss is minimal and in larger doses during severe bleeding.
[0009] Many topical hemostatic agents are currently available for use in surgery. These can be divided into two categories: those that exert their mode of action on the coagulation cascade in a biologically active manner, and those that act passively through contact activation and promotion of platelet aggregation. Passive topical hemostatic agents include collagen, cellulose, and gelatin, while active agents include thrombin and products in which thrombin is combined with a passive agent to produce an overall active product.
[0010] US Patent Application Publication No. 2003 / 0064109 describes a dry hemostatic powder prepared by a method including the steps of providing an aqueous solution containing gelatin in combination with at least one rehydration aid; drying the solution to form a solid; grinding the solid to form a powder; cross-linking the powder; removing at least 50% (w / w) of the rehydration aid; and drying the cross-linked gelatin to form a powder. The rehydration aid may include at least one material selected from the group consisting of polyethylene glycol (PEG), polyvinylpyrrolidone (PVP) and dextran.
[0011] WO 2010 / 059280 describes an anhydrous fibrous sheet comprising a first component of a fibrous polymer containing electrophilic or nucleophilic groups and a second component capable of crosslinking with the first component to form a crosslinked hydrogel adherent to biological tissue when the sheet is exposed to an aqueous medium in contact with biological tissue; a) the second component is a fibrous polymer having the same or different backbone structure as the fibrous polymer of the first component, and containing electrophilic groups when the first component contains nucleophilic groups, or containing nucleophilic groups when the first component contains electrophilic groups; b) the second component is a coating on the fibrous polymer of the first component, said coating containing electrophilic groups if the first component contains nucleophilic groups, or containing nucleophilic groups if the first component contains electrophilic groups; or c) describes an anhydrous fibrous sheet in which the second component is a dry powder dispersed and entrapped within the interstices of the fibrous polymer of the first component, said powder containing electrophilic groups if the first component contains nucleophilic groups, or containing nucleophilic groups if the first component contains electrophilic groups.
[0012] US Patent Application Publication No. 2012 / 0021058 describes a method for making a hemostatic composition comprising the steps of: a) providing a dry granular preparation of a biocompatible polymer; and b) coating the granules in said dry granular preparation with a preparation of a coagulation inducer, such as a thrombin solution. The biocompatible polymer may be selected from gelatin, soluble collagen, albumin, hemoglobin, fibrinogen, fibrin, casein, fibronectin, elastin, keratin, laminin, and derivatives or combinations thereof.
[0013] US Patent Application Publication No. 2013 / 0316974 describes a hemostatic material comprising compressed ORC powder, the particles having an average aspect ratio of about 1 to about 18. The hemostatic material may further comprise an additive selected from polysaccharides, calcium salts, anti-infective agents, hemostatic promoters, gelatin, and collagen.
[0014] US Patent Application Publication No. 2016 / 0271228 discloses a hemostatic composition comprising: A particulate form of a hemostatic biocompatible polymer selected from the group consisting of proteins, polysaccharides, biological polymers, non-biological polymers, and derivatives and combinations thereof, wherein the particulate form of the hemostatic biocompatible polymer is present as granular particles having a median diameter range of 50 to 700 μm; one hydrophilic crosslinking agent comprising electrophilic reactive groups, the electrophilic reactive groups retain their reactivity until the composition is exposed to a patient's blood, the electrophilic reactive groups being configured to crosslink with the patient's blood proteins to form a gel having sealing and hemostatic properties; and A binder that does not react with the electrophilic reactive groups of one hydrophilic crosslinker wherein the hemostatic composition is in a paste form.
[0015] US Patent Application Publication No. 2012 / 057628 describes a kit for producing a biocompatible crosslinked polymer, the kit comprising an electrophilically activated polyoxazoline (EL-POx), the EL-POX comprising m electrophilic groups, the nucleophilic crosslinker comprising n nucleophilic groups, the m electrophilic groups capable of reacting with the n nucleophilic groups to form covalent bonds, where m>2, n>2 and m+n>5, and at least one of the m electrophilic groups is a pendant electrophilic group.
[0016] WO 2016 / 056901 describes an adhesive hemostatic product selected from a coated mesh, a coated foam or a coated powder, the hemostatic product comprising: a porous solid substrate having a porosity of at least 5 vol.% and comprising an exterior surface comprising a nucleophilic polymer containing reactive nucleophilic groups; and An adherent coating covering at least a portion of a solid substrate, said coating comprising an electrophilically activated polyoxazoline (EL-POx), said EL-POx containing an average of at least one reactive electrophilic group. This application describes an adhesive hemostatic product comprising:
[0017] [Summary of the Invention] The present inventors have developed a hemostatic powder that can be advantageously used to control bleeding during surgical procedures, even on anticoagulated blood.
[0018] The hemostatic powder of the present invention comprises at least 10 wt.% particle aggregates, said particle aggregates having a diameter in the range of 1 to 500 μm; an electrophilic polyoxazoline particle comprising an electrophilic polyoxazoline carrying at least three reactive electrophilic groups capable of reacting with amine groups in blood under the formation of covalent bonds; Nucleophilic polymer particles containing a water-soluble nucleophilic polymer bearing at least three reactive nucleophilic groups capable of reacting in the presence of water with the reactive electrophilic groups of an electrophilic polyoxazoline under formation of a covalent bond between the electrophilic polyoxazoline and the nucleophilic polymer. Includes.
[0019] When applied to the bleeding site, the hemostatic powder of the present invention turns into a gel and simultaneously binds to proteins present in the blood and surrounding tissue. The superior bleeding stopping ability of the hemostatic powder is due to the induction of highly active blood clotting and the formation of a strong gelled clot that adheres to tissue. The hemostatic powder can be easily distributed throughout the bleeding site. If necessary, additional powder can be added, as this will form a new layer of gelled clot that sticks to the underlying layer of gelled clot.
[0020] Although the inventors do not wish to be bound by theory, it is believed that when the hemostatic powder comes into contact with blood, the electrophilic polyoxazoline particles containing the electrophilic polyoxazoline rapidly dissolve and simultaneously react with the proteins in the blood and the reactive nucleophilic groups of the water-soluble nucleophilic polymer in the nucleophilic polymer particles. As a result, a layer of gelled clot is formed. The dissolved electrophilic polyoxazoline also reacts with the proteins in the tissue surrounding the bleeding site, thereby anchoring the layer of gelled clot to the tissue and sealing the bleeding area.
[0021] Compared to particles comprising a molecular mixture of electrophilic polyoxazoline and water-soluble nucleophilic polymer, the particle aggregates of the present invention offer the advantage of providing better sealing properties, which is believed to be due to the fact that when the particle aggregates come into contact with blood, the electrophilic polyoxazoline reacts with the water-soluble nucleophilic polymer at a relatively slow rate, thereby allowing the electrophilic polyoxazoline to react not only with the water-soluble nucleophilic polymer, but also with proteins in the blood and tissue at the bleeding site.
[0022] Compared to powder mixtures consisting of particles of electrophilic polyoxazoline and particles of water-soluble nucleophilic polymer, the particle aggregates of the present invention offer the advantage that a more homogeneous and strong gel is formed. It is believed that when the particle aggregates come into contact in blood, a very homogeneous dispersion of the electrophilic polyoxazoline and the water-soluble nucleophilic polymer is formed, and when the polymer components dissolve therein and begin to react, a homogeneous and strong gel is formed.
[0023] The present invention also provides (a) an electrophilic polyoxazoline particle comprising an electrophilic polyoxazoline bearing at least three reactive electrophilic groups capable of reacting with amine groups in blood under the formation of a covalent bond; and (b) nucleophilic polymer particles containing a water-soluble nucleophilic polymer bearing at least three reactive nucleophilic groups capable of reacting with the reactive electrophilic groups of the electrophilic polyoxazoline under formation of a covalent bond between the electrophilic polyoxazoline and the nucleophilic polymer. The present invention provides a method for preparing a hemostatic particle aggregate of the present invention, the method comprising the step of combining 100 parts by weight of electrophilic polyoxazoline particles and 10 to 1000 parts by weight of nucleophilic polymer particles in the presence of a non-aqueous granulation liquid.
[0024] The inventors have unexpectedly discovered that by using a non-aqueous granulation liquid in which the electrophilic polyoxazoline is insoluble and the nucleophilic polymer is somewhat soluble, the electrophilic polyoxazoline and the water-soluble nucleophilic polymer can be combined into a single particle with minimal cross-linking reaction therebetween and minimal decomposition of the electrophilic polyoxazoline. Although the inventors do not wish to be bound by theory, it is believed that the use of a non-aqueous granulation liquid in which the electrophilic polyoxazoline is insoluble ensures that no cross-linking reaction occurs between the electrophilic polyoxazoline and the nucleophilic polymer during granulation. Furthermore, in this manner, the decomposition (hydrolysis) of the electrophilic polyoxazoline is minimized. In contrast to the electrophilic polyoxazoline, a portion of the nucleophilic polymer dissolves in the non-aqueous granulation liquid, thereby forming a viscous mass that can hold the electrophilic polyoxazoline particles and the nucleophilic polymer particles together.
[0025] a cohesive fibrous support structure comprising three-dimensional interconnected void spaces; and The hemostatic powder of the present invention dispersed within the interstitial spaces There is further provided a biocompatible, flexible hemostatic sheet comprising:
[0026] [Detailed Description of the Invention] Accordingly, a first aspect of the present invention provides a hemostatic powder comprising at least 10 wt.% particle agglomerates, said particle agglomerates having a diameter in the range of 1 to 500 μm, an electrophilic polyoxazoline particle comprising an electrophilic polyoxazoline carrying at least three reactive electrophilic groups capable of reacting with amine groups in blood under the formation of covalent bonds; Nucleophilic polymer particles containing a water-soluble nucleophilic polymer bearing at least three reactive nucleophilic groups capable of reacting in the presence of water with the reactive electrophilic groups of an electrophilic polyoxazoline under formation of a covalent bond between the electrophilic polyoxazoline and the nucleophilic polymer. The present invention relates to a hemostatic powder comprising:
[0027] As used herein, the term "particle agglomerate" refers to a granule that includes two or more types of particles that are all bonded together.
[0028] The term "polyoxazoline" as used herein refers to poly(N-acylalkyleneimine) or poly(aroylalkyleneimine), further referred to as POx. An example of POx is poly(2-ethyl-2-oxazoline). The term "polyoxazoline" also encompasses copolymers of POx.
[0029] The term "water-soluble nucleophilic polymer" as used herein refers to a nucleophilic polymer that has a water solubility of at least 50 g / L in demineralized water at 20° C. with a pH ranging from 3 to 7. Chitosan is an example of a water-soluble nucleophilic polymer. Chitosan is soluble in water with a pH <6. To determine the water solubility of the nucleophilic polymer at various pHs, the pH of the demineralized water is adjusted using hydrochloric acid.
[0030] The term "collagen" as used herein refers to the major structural protein in the extracellular space of various connective tissues in the body of animals. Collagen forms a characteristic triple helix of three polypeptide chains. Depending on the degree of mineralization, collagen tissues can be either strong (bone) or flexible (tendon) or have a gradient from strong to flexible (cartilage). Unless otherwise indicated, the term "collagen" also encompasses denatured collagens other than gelatin (e.g., cross-linked collagens).
[0031] The term "gelatin" as used herein refers to a mixture of peptides and proteins produced by partial hydrolysis of collagen extracted from the skin, bones and connective tissues of animals such as domestic cattle, chickens, pigs and fish. During hydrolysis, the natural molecular bonds between the individual collagen strands are broken down into a form that is more easily reconstituted. The term "gelatin" as used herein also encompasses modified gelatins such as cross-linked gelatin and reduced cross-linked gelatin.
[0032] The term "reduced cross-linked gelatin" as used herein refers to partially hydrolyzed cross-linked gelatin. Partial hydrolysis of peptide bonds in cross-linked gelatin can be achieved, for example, by alkaline treatment. Hydrolysis of cross-linked gelatin increases the density of free carboxyl and free amine groups, increasing its water solubility.
[0033] The term "hemostatic sheet" as used herein, unless otherwise indicated, refers to a sheet capable of stopping bleeding from damaged tissue. The hemostatic sheets of the present invention may achieve hemostasis by turning blood into a gel and / or forming a seal to close the wound site.
[0034] The term "water-resistant" as used herein in relation to a fibrous carrier structure means that the structure is not water-soluble and does not disintegrate or form a colloidal dispersion in water at neutral pH conditions (pH 7) and a temperature of 37°C.
[0035] The term "interstitial space" as used herein refers to void ("empty") space within the fibrous carrier structure. The interstitial space within the fibrous carrier structure allows for the introduction of hemostatic powder into the structure. Blood and other bodily fluids can also enter the interstitial space, thereby allowing the hemostatic powder to exert its hemostatic effect and / or provide adhesion of tissue to the hemostatic sheet.
[0036] The term "protein" as used herein includes cross-linked and hydrolyzed proteins unless otherwise indicated. Similarly, unless otherwise indicated, when a particular protein species, such as gelatin or collagen, is referred to, hydrolyzed and cross-linked versions of that protein species are also included.
[0037] The particle aggregate diameter distribution of electrophilic polyoxazoline particles and nucleophilic polymer particles of the hemostatic powder may be determined by laser diffraction, preferably using a Malvern Mastersizer 2000 in combination with a Stainless Steel Sample Dispersion Unit. The sample dispersion unit is filled with approximately 120 ml of cyclohexane and the unit is allowed to stabilize for 5-10 minutes at a stirring speed of 1800 rpm, after which a background measurement (blank measurement) is taken. The sample tube is shaken and rotated horizontally 20 times. Approximately 50 mg is then dispersed in the sample dispersion unit containing cyclohexane. Once the sample is introduced into the dispersion unit, the sample is stirred at 1800 rpm for 1 minute 30 seconds to ensure that all particles are properly dispersed, after which measurements are taken. No sonication is performed on the dispersed particles. The mean particle size is determined by D[4,3], the volume weighted mean diameter (ΣniDi 4 ) / (ΣniDi 3 )
[0038] In addition to particle aggregates comprising electrophilic polyoxazoline particles and nucleophilic polymer particles, the hemostatic powder of the present invention may contain other particulate components, for example biocompatible (bio)polymers such as gelfoam or starch. Preferably, the hemostatic powder contains at least 30 wt.%, more preferably at least 60 wt.%, and most preferably at least 80 wt.% particle aggregates.
[0039] The particle agglomerates in the hemostatic powder preferably contain at least 10 wt.%, more preferably at least 25 wt.%, and most preferably at least 40 wt.% electrophilic polyoxazoline.
[0040] The nucleophilic polymer is preferably contained in the particle agglomerates at a concentration of at least 10 wt.%, more preferably at least 12 wt.%, and most preferably at least 30 wt.%.
[0041] The combination of the electrophilic polyoxazoline and the nucleophilic polymer typically constitutes at least 10 wt.% of the particle agglomerate. More preferably, the combination of the two polymers constitutes at least 50 wt.%, and most preferably at least 75 wt.% of the particle agglomerate.
[0042] In addition to the electrophilic polyoxazoline and the nucleophilic polymer, the particle aggregate may contain one or more other components, such as polysaccharides. Examples of polysaccharides that may be utilized include amylose, maltodextrin, amylopectin, starch, dextran, hyaluronic acid, heparin, chondroitin sulfate, dermatan sulfate, heparan sulfate, keratan sulfate, dextran sulfate, pentosan polysulfate, alginate, and combinations thereof. Typically, the amount of polysaccharide in the particle aggregate does not exceed 50 wt.%. When polysaccharides are contained in the particle aggregate, the combination of electrophilic polyoxazoline, nucleophilic polymer, and polysaccharide preferably constitutes at least 60 wt.% of the particle aggregate, more preferably at least 80 wt.%, and most preferably at least 90 wt.%.
[0043] According to another advantageous embodiment, the particle agglomerate contains a dry buffer system. Preferably, the buffer system has a buffer pH in the range of 7 to 11, more preferably in the range of 8 to 10. Preferably, the buffer system has a buffer pH of at least 10 mmol.l -1 .pH -1 More preferably, the buffer capacity is at least 25 mmol.l -1 .pH -1 and most preferably the buffer capacity is at least 50 mmol.l -1 .pH -1 Examples of biocompatible buffer systems that may be utilized with the particle aggregates include sodium phosphate / sodium carbonate buffer, sodium borate decahydrate buffer, Tris-buffered protein, HEPES-buffered saline, and sodium bicarbonate / carbonate buffer.
[0044] As described below, the particle agglomerates of the present invention may be prepared without the use of a granulation binder, i.e., a component utilized during granulation to provide adhesion between the electrophilic polyoxazoline particles and the nucleophilic polymer particles. Thus, in a preferred embodiment, the particle agglomerates do not contain a granulation binder.
[0045] The hemostatic powder of the present invention preferably contains at least 10 wt.% particle agglomerates having diameters in the range of 1 to 200 μm, more preferably at least 10 wt.% particle agglomerates having diameters in the range of 1 to 100 μm, and most preferably at least 10 wt.% particle agglomerates having diameters in the range of 1 to 75 μm.
[0046] The hemostatic powder preferably has a volume weighted mean diameter (D[4,3], (Σn i D 4 ) / (ΣniD 3 )).
[0047] Particle aggregates in the hemostatic powder preferably have a D[4,3] in the range of 10-200 μm, more preferably in the range of 15-100 μm, and most preferably in the range of 30-60 μm.
[0048] The electrophilic polyoxazoline particles in the particle agglomerates preferably have a volume weighted average diameter (D[4,3]) in the range of 1 to 100 μm, more preferably in the range of 50 to 50 μm, and most preferably in the range of 10 to 40 μm.
[0049] The nucleophilic polymer particles in the particle agglomerates preferably have a volume weighted average diameter (D[4,3]) in the range of 10 to 300 μm, more preferably in the range of 15 to 200 μm, and most preferably in the range of 20 to 100 μm.
[0050] The electrophilic polyoxazoline particles preferably contain at least 30 wt.%, more preferably at least 50 wt.%, and most preferably at least 80 wt.% electrophilic polyoxazoline.
[0051] The electrophilic polyoxazoline preferably has a solubility in distilled water at 20° C. of at least 100 g / L, more preferably at least 300 g / L.
[0052] The electrophilic polyoxazoline preferably has a solubility in isopropyl alcohol at 20° C. of less than 10 mg / L, more preferably less than 5 mg / L, and most preferably less than 1 mg / L.
[0053] The electrophilic polyoxazoline preferably has a molecular weight of at least 2 kDa, more preferably from 5 to 200 kDa, most preferably from 10 to 100 kDa.
[0054] As previously described herein, the inventors have found a method to combine electrophilic polyoxazoline and water-soluble nucleophilic polymer into a single particle with minimal crosslinking reaction therebetween and minimal degradation of the electrophilic polyoxazoline.Thus, in a highly preferred embodiment of the present invention, the electrophilic polyoxazoline in the particle agglomerate has a polydispersity index (PDI) of less than 2.0, more preferably less than 1.8, and most preferably less than 1.5.
[0055] The electrophilic polyoxazoline preferably contains at least 4 reactive electrophilic groups, more preferably at least 8 reactive electrophilic groups, even more preferably at least 16 reactive electrophilic groups, and most preferably at least 32 reactive electrophilic groups.
[0056] The electrophilic polyoxazoline typically bears an average of at least 10, more preferably at least 20, reactive electrophilic groups.
[0057] The electrophilic polyoxazoline has repeating units of the following formula (I): (CHR 1 ) m NCOR 2 (In the formula, R 2 and R 1 each of which is H, optionally substituted C 1~22 alkyl, optionally substituted cycloalkyl, optionally substituted aralkyl, and optionally substituted aryl, and m is 2 or 3. It is preferred that the polyoxazoline is derived from a polyoxazoline represented by the formula:
[0058] Preferably, R in formula (I) 1 and R 2 H and C 1~8 Alkyl, even more preferably H and C 1~4 R is selected from alkyl. 1 is most preferably H. The integer m in formula (I) is preferably equal to 2.
[0059] According to a preferred embodiment, the polyoxazoline is a polymer, even more preferably a homopolymer of 2-alkyl-2-oxazoline, said 2-alkyl-2-oxazoline being selected from 2-methyl-2-oxazoline, 2-ethyl-2-oxazoline, 2-propyl-2-oxazoline, 2-butyl-2-oxazoline and combinations thereof. Preferably, the polyoxazoline is a homopolymer of 2-propyl-2-oxazoline or 2-ethyl-oxazoline. Most preferably, the polyoxazoline is a homopolymer of 2-ethyl-oxazoline.
[0060] According to certain preferred embodiments, the electrophilic polyoxazoline comprises at least 20 oxazoline units, more preferably at least 30 oxazoline units, and most preferably at least 80 oxazoline units. The electrophilic polyoxazoline preferably comprises an average of at least 0.05 reactive electrophilic groups per oxazoline residue. Even more preferably, the electrophilic polyoxazoline comprises an average of at least 0.1 reactive electrophilic groups per oxazoline residue. Most preferably, the electrophilic polyoxazoline comprises an average of 0.12 to 0.5 reactive electrophilic groups per oxazoline residue.
[0061] The polyoxazoline may carry reactive electrophilic groups at its side chains (pendant reactive electrophilic groups), at its termini or both. The electrophilic polyoxazoline utilized according to the present invention advantageously contains one or more pendant reactive electrophilic groups. Typically, the electrophilic polyoxazoline contains 0.03-0.5 pendant reactive electrophilic groups per monomer, more preferably 0.04-0.35 pendant reactive electrophilic groups per monomer, even more preferably 0.05-0.25 pendant reactive electrophilic groups per monomer.
[0062] According to a preferred embodiment, the reactive electrophilic groups of the electrophilic polyoxazoline are selected from carboxylate esters, sulfonate esters, phosphonate esters, pentafluorophenyl esters, p-nitrophenyl esters, p-nitrothiophenyl esters, acid halide groups, anhydrides, ketones, aldehydes, isocyanates, thioisocyanates, isocyano, epoxides, activated hydroxyl groups, olefins, glycidyl ethers, carboxyls, succinimidyl esters, sulfosuccinimidyl esters, maleimides (maleimidyl), ethenesulfonyl, imidoesters, acetoacetates, haloacetals, orthopyridyl disulfides, dihydroxyphenyl derivatives, vinyls, acrylates, acrylamides, iodoacetamides, and combinations thereof. More preferably, the reactive electrophilic group is selected from carboxylate esters, sulfonate esters, phosphonate esters, pentafluorophenyl esters, p-nitrophenyl esters, p-nitrothiophenyl esters, acid halide groups, anhyinidrides, ketones, aldehydes, isocyanates, thioisocyanates, isocyano, epoxides, activated hydroxyl groups, glycidyl ethers, carboxyls, succinimidyl esters, sulfosuccinimidyl esters, imido esters, dihydroxyphenyl derivatives, and combinations thereof. Even more preferably, the reactive electrophilic group is selected from haloacetals, orthopyridyl disulfides, maleimides, vinyl sulfones, dihydroxyphenyl derivatives, vinyls, acrylates, acrylamides, iodoacetamides, succinimidyl esters, and combinations thereof. Most preferably, the reactive electrophilic group is selected from maleimides, vinyls, acrylates, acrylamides, succinimidyl esters, sulfosuccinimidyl esters, and combinations thereof.
[0063] Examples of succinimidyl esters which may be utilized include succinimidyl glutarate, succinimidyl propionate, succinimidyl succinamide, succinimidyl carbonate, disuccinimidyl suberate, bis(sulfosuccinimidyl)suberate, dithiobis(succinimidyl propionate), bis(2-succinimidooxycarbonyloxy)ethyl sulfone, 3,3'-dithiobis(sulfosuccinimidyl-propionate), succinimidyl carbamate, sulfosuccinimidyl(4-iodoacetyl)acetate, and the like. sulfosuccinimidyl esters, ...
[0064] Examples of dihydroxyphenyl derivatives that may be utilized include dihydroxyphenylalanine, 3,4-dihydroxyphenylalanine (DOPA), dopamine, 3,4-dihydroxyhydroccinamic acid (DOHA), norepinephrine, epinephrine, and catechol.
[0065] The water-soluble nucleophilic polymer contained in the nucleophilic polymer particles preferably has a solubility of at least 100 g / L, more preferably at least 150 g / L, and most preferably at least 200 g / L in demineralized water at 20° C. and a pH in the range of 3 to 7. In the present invention, when the electrophilic polyoxazoline releases an acidic substance when reacting with a blood component, tissue, and / or nucleophilic polymer, a nucleophilic polymer that is soluble at an acidic pH can be suitably used. This applies, for example, to the case where the electrophilic polyoxazoline contains an N-hydroxysuccinimide group.
[0066] The nucleophilic polymer particles preferably contain at least 30 wt.%, more preferably at least 50 wt.%, and most preferably at least 80 wt.% nucleophilic polymer.
[0067] According to a particularly preferred embodiment, the water-soluble nucleophilic polymer utilized in the aggregate particles dissolves relatively slowly in water. As previously described herein, it is believed that when the electrophilic polyoxazoline reacts with the water-soluble nucleophilic polymer at a relatively slow rate, the electrophilic polyoxazoline may also react with proteins in blood and tissues at the bleeding site. By utilizing a water-soluble nucleophilic polymer that dissolves relatively slowly, the dissolved electrophilic polyoxazoline has the opportunity to react with the (slow) water-soluble nucleophilic polymer as well as with proteins in blood and tissues, thereby creating a strong homogeneous sealing gel.
[0068] Water-soluble nucleophilic polymers with high molecular weight tend to dissolve relatively slowly in water. Therefore, in a highly preferred embodiment, the water-soluble nucleophilic polymer contained in the nucleophilic polymer particles has a molecular weight of at least 3 kDa, more preferably at least 10 kDa, and most preferably 20 to 3,000 kDa.
[0069] The nucleophilic polymer preferably contains at least 4 reactive nucleophilic groups, more preferably at least 8 reactive nucleophilic groups, and most preferably at least 10. Most preferably, these reactive nucleophilic groups are amine groups, most preferably primary amine groups.
[0070] Examples of water-soluble nucleophilic polymers suitable for use in the nucleophilic polymer particles include proteins, chitosan, nucleophilic polyoxazolines, nucleophilic polyethylene glycols, polyethyleneimines, and combinations thereof. More preferably, the nucleophilic polymer is selected from gelatin, collagen, chitosan, nucleophilic polyoxazolines, and combinations thereof.
[0071] According to a particularly advantageous embodiment, the nucleophilic polymer particles utilized by the present invention allow hemostasis by accelerating the clotting process. Collagen can activate the intrinsic pathway of the clotting cascade. Collagen has a large surface area that acts as a matrix for platelet activation, clotting and clot formation. Gelatin particles have the ability to restrict blood flow and provide a matrix for clot formation. Thus, in a highly preferred embodiment, the nucleophilic polymer is selected from gelatin, collagen and combinations thereof. Most preferably, the nucleophilic polymer is gelatin, even more preferably cross-linked gelatin.
[0072] The crosslinked gelatin has a molecular weight preferably in the range of 30 to 3,000 kDa, more preferably in the range of 400 to 2,000 kDa, and most preferably in the range of 500 to 1,500 kDa.
[0073] The average primary amine content of crosslinked gelatin is 5 × 10 per μg of reduced crosslinked gelatin. -4 ~2×10 -2 μmol, more preferably 1.0×10 -3 ~1.0×10 -2 μmol of primary amine.
[0074] According to another advantageous embodiment, the nucleophilic polymer is a nucleophilic polyethylene glycol (PEG). Preferably, the nucleophilic PEG contains at least 3, more preferably at least 5 and most preferably 8 reactive nucleophilic groups.
[0075] According to a further preferred embodiment, the nucleophilic polymer is chitosan. Chitosan is a biodegradable, non-toxic complex carbohydrate derivative of chitin (poly-N-acetyl-D-glucosamine), a naturally occurring substance. Chitosan is the deacetylated form of chitin. The chitosan applied according to the invention preferably has a degree of deacetylation higher than 70%. The chitosan utilized according to the invention has a molecular weight of at least 5 kDa, more preferably between 10 and 10,000 kDa.
[0076] According to another highly advantageous embodiment, the nucleophilic polymer is a nucleophilic polyoxazoline. Preferably, the nucleophilic polyoxazoline contains at least 3, more preferably at least 5, most preferably 8 to 20 reactive nucleophilic groups.
[0077] Compared to naturally occurring nucleophilic biopolymers such as gelatin, collagen and chitosan, the use of synthetic nucleophilic polymers such as nucleophilic polyoxazolines and nucleophilic PEGs offers the advantage that particle aggregates containing these synthetic nucleophilic polymers exhibit more predictable (reproducible) hemostatic properties.
[0078] The reactive nucleophilic groups of the water-soluble nucleophilic polymer are preferably selected from amine groups, thiol groups, and combinations thereof.
[0079] According to a preferred embodiment, the water-soluble nucleophilic polymer contains two or more amine groups and the reactive electrophilic groups in the electrophilic polyoxazoline are selected from carboxylate esters, sulfonate esters, phosphonate esters, pentafluorophenyl esters, p-nitrophenyl esters, p-nitrothiophenyl esters, acid halide groups, anhydrides, ketones, aldehydes, isocyanates, thioisocyanates, isocyano, epoxides, activated hydroxyl groups, glycidyl ethers, carboxyls, succinimidyl esters, sulfosuccinimidyl esters, imido esters, dihydroxyphenyl derivatives and combinations thereof.
[0080] According to another preferred embodiment, the water-soluble nucleophilic polymer contains two or more thiol groups, and the reactive electrophilic groups of the electrophilic polyoxazoline are selected from haloacetals, orthopyridyl disulfides, maleimides, vinyl sulfones, dihydroxyphenyl derivatives, vinyls, acrylates, acrylamides, iodoacetamides, succinimidyl esters, sulfosuccinimidyl esters, and combinations thereof. More preferably, the reactive electrophilic groups are selected from succinimidyl esters, sulfosuccinimidyl esters, haloacetals, maleimides or dihydroxyphenyl derivatives, and combinations thereof. Most preferably, the reactive electrophilic groups are selected from maleimides or dihydroxyphenyl derivatives, and combinations thereof.
[0081] According to a particularly preferred embodiment, the ratio between the total number of reactive electrophilic groups provided by the electrophilic polyoxazoline and the total number of reactive nucleophilic groups provided by the nucleophilic polymer is in the range of 1:1.5 to 1.5:1, more preferably in the range of 1:1.2 to 1.2:1, most preferably in the range of 1:1.1 to 1.1:1.
[0082] The present inventors have unexpectedly discovered that particle aggregates that exhibit excellent adhesion to organs such as the spleen and kidneys are obtained when the particle aggregates contain 1-20 wt.%, more preferably 2.5-15 wt.%, and most preferably 5-10 wt.% of a non-reactive non-ionic polymer that does not contain reactive electrophilic or reactive nucleophilic groups.
[0083] In a highly preferred embodiment, the agglomerated particles are coated with a non-reactive non-ionic polymer.
[0084] The non-reactive nonionic polymer preferably has a melting point in the range of 40 to 70° C., more preferably in the range of 45 to 65° C., and most preferably in the range of 50 to 60° C. Here, the melting point refers to the temperature at which the polymer completely melts.
[0085] Examples of non-reactive non-ionic polymers suitable for use in the aggregate particles of the present invention include poloxamers, polyethylene glycols, and combinations thereof. Poloxamers are non-ionic triblock copolymers composed of a central hydrophobic chain of polyoxypropylene (poly(propylene oxide)) flanked by two hydrophilic chains of polyoxyethylene (poly(ethylene oxide)), and are represented by the formula (I): [ka] (In the formula, a is an integer of 10 to 110, and b is an integer of 20 to 60.) When a is 80 and b is 27, the polymer is known as poloxamer 188. Other known poloxamers useful in the present invention are poloxamer 237 (a=64 and b=37), poloxamer 338 (a=141 and b=44), and poloxamer 407 (a=101 and b=56). Additional poloxamers that are known and may be useful in the present invention include poloxamer 108, poloxamer 182, poloxamer 183, poloxamer 212, poloxamer 217, poloxamer 238, poloxamer 288, poloxamer 331, poloxamer 338, and poloxamer 335.
[0086] According to a particularly preferred embodiment, the non-reactive non-ionic polymer is a poloxamer, even more preferably a poloxamer with an average molecular mass between 2,000 and 18,000, most preferably a poloxamer with an average molecular mass between 7,000 and 10,000.
[0087] The poloxamer applied to the particle aggregates is preferably a solid at room temperature.
[0088] In another advantageous embodiment, the hemostatic powder of the present invention is bioresorbable, allowing the powder to be used in abdominal surgery.
[0089] Another aspect of the present invention is a method for producing a (a) an electrophilic polyoxazoline particle comprising an electrophilic polyoxazoline bearing at least three reactive electrophilic groups capable of reacting with amine groups in blood under the formation of a covalent bond; and (b) nucleophilic polymer particles containing a water-soluble nucleophilic polymer bearing at least three reactive nucleophilic groups capable of reacting with the reactive electrophilic groups of the electrophilic polyoxazoline under formation of a covalent bond between the electrophilic polyoxazoline and the nucleophilic polymer. The present invention relates to a method for preparing a hemostatic particle aggregate of claim 1, said method comprising the step of combining 100 parts by weight of electrophilic polyoxazoline particles and 10-1000 parts by weight of nucleophilic polymer particles in the presence of a non-aqueous granulation liquid.
[0090] The electrophilic polyoxazoline particles utilized in the method of the present invention are preferably the same as the electrophilic polymer particles previously described herein.Similarly, the nucleophilic polymer particles utilized are the same as the nucleophilic polymer particles previously described herein.
[0091] According to a preferred embodiment, both the electrophilic polyoxazoline particles and the nucleophilic polymer particles utilized in the method of the present invention have a moisture content of less than 2 wt.%, more preferably less than 1 wt.%. To achieve such low moisture content, it may be necessary to dry the polymer particles prior to granulation.
[0092] The electrophilic polyoxazoline preferably has a solubility in the non-aqueous granulation liquid at 20° C. of less than 1 mg / L, more preferably less than 0.5 mg / L, even more preferably less than 0.2 mg / L, and most preferably less than 0.1 mg / L.
[0093] The nucleophilic polymer preferably has a solubility in the non-aqueous granulation liquid at 20° C. of at least 5 mg / L, more preferably at least 10 mg / L, even more preferably from 20 to 200 mg / L, and most preferably from 40 to 150 mg / L.
[0094] In a preferred embodiment, the method comprises combining 100 parts by weight of electrophilic polyoxazoline particles with 20 to 400 parts by weight, more preferably 50 to 200 parts by weight, of nucleophilic polymer particles in the presence of a non-aqueous granulation liquid.
[0095] The amount of non-aqueous granulation liquid utilized in the process of the present invention is preferably in the range of 0.5-5% by weight of the combined electrophilic polyoxazoline particles and nucleophilic polymer particles used in the process, more preferably the amount of non-aqueous granulation liquid utilized is in the range of 1-4%, most preferably 1.5-3% by weight of the combined electrophilic polyoxazoline particles and nucleophilic polymer particles used in the process.
[0096] According to a particularly preferred embodiment, the method comprises the steps of wetting electrophilic polyoxazoline particles with a non-aqueous granulation liquid and then combining the wetted polyoxazoline particles with nucleophilic polymer particles. This particular embodiment offers the advantage of producing a granulation that is very homogeneous in terms of particle size and composition.
[0097] The electrophilic polyoxazoline particles used in preparing the powder blend preferably have a volume weighted average diameter (D[4,3]) in the range of 1 to 100 μm, more preferably in the range of 50 to 50 μm, and most preferably in the range of 10 to 40 μm.
[0098] The volume weighted mean diameter (D[4,3]) of the nucleophilic polymer particles used to prepare the powder blend is preferably in the range of 10 to 300 μm, more preferably in the range of 15 to 200 μm, and most preferably in the range of 20 to 100 μm.
[0099] The agglomerated powder obtained by the method of the present invention preferably has a volume weighted mean diameter (D[4,3]) in the range of 12 to 1000 μm, more preferably in the range of 20 to 500 μm, and most preferably in the range of 30 to 300 μm.
[0100] The non-aqueous granulation liquid utilized in the wet granulation contains at least 60 wt.% of an organic solvent selected from isopropyl alcohol, ethanol, methanol, diethyl ether, heptane, hexane, pentane, cyclohexane, dichloromethane, acetone, and mixtures thereof. More preferably, the non-aqueous granulation liquid contains at least 60 wt.%, and most preferably at least 85 wt.%, of an organic solvent selected from isopropyl alcohol, ethanol, and mixtures thereof. Even more preferably, the non-aqueous granulation liquid contains at least 60 wt.%, and most preferably at least 85 wt.%, of isopropyl alcohol.
[0101] The non-aqueous granulation liquid preferably contains no more than 1 wt.% water, more preferably no more than 0.1 wt.% water.
[0102] The method of the present invention provides the advantage that it is not necessary to use a granulation binder.Therefore, in a preferred embodiment of the method, no granulation binder is used.According to a particularly preferred embodiment, the only materials used in the preparation method are electrophilic polyoxazoline particles, nucleophilic polymer particles and non-aqueous granulation liquid.
[0103] The particle aggregates of the present invention can be advantageously applied within a hemostatic sheet to improve its hemostatic properties. Thus, a further aspect of the present invention is a cohesive fibrous support structure comprising three-dimensional interconnected void spaces; and Dispersed within the interstitial spaces is a hemostatic powder as previously described herein. The present invention relates to a biocompatible, flexible hemostatic sheet comprising:
[0104] According to a particularly preferred embodiment, the adhesive fibrous carrier structure is water resistant.
[0105] The electrophilic polyoxazoline in the hemostatic powder distributed throughout the fibrous carrier structure dissolves rapidly when the sheet comes into contact with blood or other aqueous body fluids that can penetrate the interstitial spaces. Thus, as soon as the sheet is applied to the wound site, rapid covalent crosslinking occurs between the electrophilic polyoxazoline on the one hand, and the nucleophilic polymer in the nucleophilic polymer particles, blood proteins and tissue on the other hand, resulting in the formation of a gel that seals the wound surface and stops bleeding, as well as strong adhesion of the hemostatic sheet to the tissue. The chitosan applied according to the present invention preferably has a deacetylation degree of 70% or more. The water-resistant fibrous carrier structure provides mechanical strength during and after application and prevents excessive swelling.
[0106] The electrophilic polyoxazoline and nucleophilic polymer are contained within a single particle, ensuring that these two reactive components can be homogenously distributed throughout the hemostatic sheet, that separation will not occur during shipping and handling, and that the components can react with each other instantly when the particle aggregates come into contact with blood.
[0107] According to particularly preferred embodiments, the hemostatic sheets of the present invention are bioabsorbable, i.e., the carrier structure, particle aggregates, and any other components of the hemostatic sheet are eventually absorbed by the body. Absorption of the carrier structure and particle aggregates typically requires chemical degradation (e.g., hydrolysis) of the polymers contained therein. Complete bioabsorption of the hemostatic sheet by the human body is typically achieved in 1-10 weeks, preferably 2-8 weeks.
[0108] The hemostatic sheet of the present invention typically has an uncompressed average thickness of 0.5 to 25 mm, more preferably in the range of 1 to 10 mm, and most preferably in the range of 1.5 to 5 mm.
[0109] The dimensions of the hemostatic sheet are preferably at least 2 cm at the top and bottom of the sheet. 2 , more preferably at least 10 cm 2 , most preferably 25-50 cm 2Typically the sheets are rectangular in shape, with a length of 25-200 mm and a width of 25-200 mm.
[0110] The hemostatic sheet is preferably 200 mg / cm 3 less than 150 mg / cm 3 less than 10-100 mg / cm 3 It has an uncompressed density of
[0111] The hemostatic sheets of the present invention are preferably essentially anhydrous. Typically, the hemostatic sheets have a moisture content of 5 wt.% or less, more preferably 2 wt.% or less, and most preferably 1 wt.% or less.
[0112] The water absorption capacity of the hemostatic sheet is preferably at least 50%, more preferably in the range of 100% to 800%, and most preferably in the range of 200% to 500%.
[0113] The hemostatic sheets of the present invention are preferably sterile.
[0114] The use of a fibrous carrier structure in the hemostatic sheet of the present invention offers the advantage that the hemostatic powder can be distributed homogeneously throughout the carrier structure without difficulty, which is much more difficult to achieve with, for example, a foam carrier structure.
[0115] The fibers of the fibrous carrier structure preferably have an average diameter of 1 to 500 μm, more preferably 2 to 300 μm, most preferably 5 to 200 μm. The average diameter of the fibers can be suitably determined using a microscope.
[0116] Typically, at least 50 wt.%, more preferably at least 80 wt.%, of the fibers of the fibrous support structure have a diameter of from 1 to 300 μm and a length of at least 1 mm.
[0117] Preferably, at least 50 wt.%, more preferably at least 80 wt.%, of the fibers of the fibrous support structure have an aspect ratio (ratio of length to diameter) of at least 1000.
[0118] The fibrous carrier structure utilized by the present invention is preferably a felt, woven or knitted structure. Most preferably, the fibrous carrier structure is a felt structure, where the term "felt structure" refers to a structure produced by matting fibers and pressing them together to form a cohesive material.
[0119] The fibrous carrier structure comprises at least 50 wt.%, more preferably at least 80 wt.%, and most preferably at least 90 wt.%, fibers containing gelatin, collagen, cellulose, modified cellulose, carboxymethyl dextran, PLGA, sodium hyaluronate / carboxymethyl cellulose, polyvinyl alcohol, chitosan, or combinations thereof.
[0120] In an embodiment of the invention, the fibrous support structure does not comprise oxidized regenerated cellulose.
[0121] Preferred fibrous support structures have an air permeability of at least 0.1 L / min×cm 2 , more preferably at least 0.5 L / min×cm 2 The air permeability is determined according to EN ISO 9237:1995 (Determination of the air permeability of textile fabrics).
[0122] The fibers in the fibrous carrier structure may be produced by methods known in the art, such as electrospinning, electroblown spinning, and high-speed rotary atomizer spinning. The production of fibrous carrier structures by high-speed rotary atomizer spinning is described in US Patent Application Publication No. 2015 / 0010612. Commercially available hemostatic fibrous sheets can also be used as the fibrous carrier structure.
[0123] The hemostatic powder is preferably present in the hemostatic sheet of the present invention in an amount of 5-90% by weight of the fibrous carrier structure, more preferably 10-80% by weight, even more preferably 20-75% by weight, and most preferably 50-70% by weight.
[0124] The present invention is further illustrated by the following non-limiting examples. EXAMPLES
[0125] Generally, whenever residual moisture after drying (i.e. residual water in the dry powder, granulation and / or cohesive fibrous carrier structure) is not specified, the level will be below 2.0% w / w.
[0126] (Preparation of NHS-POx) NHS side chain activated poly[2-(ethyl / hydroxy-ethyl-amido-ethyl / NHS-ester-ethyl-ester-ethyl-amido-ethyl)-2-oxazoline] terpolymer containing 20% NHS ester groups (=EL-POx, 20% NHS) was synthesized as follows: Poly[2-(ethyl / methoxy-carbonyl-ethyl)-2-oxazoline] copolymer (DP=+ / -100) was synthesized by CROP using 60% 2-ethyl-2-oxazoline (EtOx) and 40% 2-methoxycarbonyl-ethyl-2-oxazoline (MestOx). 1 Secondly, the polymer containing 40% 2-methoxycarbonyl-ethyl groups was reacted with ethanolamine to give a statistical copolymer containing 40% 2-hydroxy-ethyl-amido-ethyl groups ( 1 H-NMR) was then used to obtain a copolymer with half of the 2-hydroxy-ethyl-amido-ethyl groups reacted with succinic anhydride, 1A terpolymer with 60% 2-ethyl, 20% 2-hydroxy-ethyl-amido-ethyl and 20% 2-carboxy-ethyl-ester-ethyl-amido-ethyl groups was obtained by H-NMR. Finally, the 2-carboxy-ethyl-ester-ethyl-amido-ethyl groups were activated by N-hydroxysuccinimide (NHS) and diisopropylcarbodiimide (DIC) to obtain EL-POx, 20% NHS. 1 According to H-NMR, NHS-POx contained 20% NHS-ester groups. NHS-POx was dissolved in water between 2 and 8 °C (60 g in 300 mL) and lyophilized by cooling at minus 80 °C for 30 min. The lyophilized powder so obtained was dried in a Rotavap at 40 °C until the moisture content was less than 0.8% w / w as determined by Karl Fischer titration. This dry (white) powder was ground using a ball mill (Retch MM400) to an average particle size of ≤40 μm (D[4,3]) and vacuum sealed in alu-alu bags.
[0127] (Staining of NHS-POx powder) 20 g of NHS-POx powder was dissolved in water and mixed with 50 mg of Brilliant Blue FCF (Sigma Aldrich) using a high-speed disperser (Ultra-Turrax, IKA). Immediately after mixing (2 min), the solution was frozen at -78 °C and then freeze-dried overnight. The so-obtained freeze-dried powder was dried in a Rotavap at 40 °C until the residual moisture content was less than 0.8% w / w as determined by Karl Fischer titration. The dry (blue) powder was then ground using a ball mill (Retch MM400) to a blue-stained NHS-POx powder with an average particle size of 40 μm or less (D[4,3]) and vacuum-sealed in an alu-alu bag.
[0128] (Effect of NHS-POx crosslinking on PDI (polydispersity index)) An 80 μg / mL solution of 2,2'-(ethylenedioxy)-bis-(ethylamine) (EDEA, Aldrich, Mw 148.2) was prepared in a mixture of dichloromethane (DCM) and isopropanol (IPA) by dissolving 80 mg of EDEA in 10 mL of DCM / IPA 95:5 (v / v). This solution was diluted 10-fold with DCM / IPA 95:5 (v / v) and 26.8 μL of the EDEA solution was added to 100 μL of a 0.5 g / mL solution of NHS-POx in DCM / IPA 95:5 (v / v), corresponding to 0.05 mol % amine groups relative to NHS groups. Immediately after the addition of the EDEA solution, the reaction mixture was thoroughly mixed using a vortex mixer. The reaction mixture was agitated at 40 °C for 3 h and all volatiles were removed by rotary evaporation under reduced pressure.
[0129] The dried samples were reconstituted in N,N-dimethylacetamide containing 50 mM lithium chloride, the mobile phase for size exclusion chromatography (SEC). SEC was measured against poly(methyl methacrylate) standards. The M n , M w and PDI were determined. The PDI was greater than 2.5. A 0.5 g / mL solution of NHS-POx in DCM / IPA 95:5 (v / v) without the addition of EDEA gave a PDI of 1.5 after the same SEC procedure, indicating that the crosslinking of only 0.05 mol % of the NHS groups already significantly increases the PDI of the polymer.
[0130] (Preparation of NU-POx) Polyoxazolines containing ethyl and amine groups in the alkyl side chains were synthesized by CROP of EtOx and MestOx followed by amidation of the methyl ester side chains with ethylenediamine to give poly(2-ethyl / aminoethylamidoethyl-2-oxazoline) copolymers (NU-POx). 1By H-NMR, NU-POx contained 10% NH2. NU-POx was dissolved in water between 2 and 8 °C (60 g in 300 mL) and freeze-dried by cooling at -80 °C for 30 min. The freeze-dried powder so obtained was dried in a Rotavap at 40 °C until the moisture content was less than 0.8% w / w as determined by Karl Fischer titration. The dried powder was ground in a benchtop grinder until the average particle size was less than 100 μm (D[4,3]) and vacuum sealed in alu-alu bags.
[0131] (Preparation of reactive NHS-POx / NU-POx granules) Blue or white (undyed) NHS-POx powder was wetted with isopropyl alcohol (IPA) in a high shear mixer until a homogenous snow-like powder containing approximately 1-2% w / w IPA was obtained. After this, NU-POx powder was added and mixed. The wetted blue NHS-POx powder was mixed with NU-POx powder in a molar ratio of 1:0.6, the molar ratio referring to the ratio of the number of NHS groups provided by NHS-POx to the number of amine groups provided by NU-POx. The wetted undyed NHS-POx powder was also mixed with NU-POx powder in other molar ratios (1:0.8; 1:1 and 1:1.2).
[0132] After mixing, 1 The wet granulation was dried under reduced pressure until the IPA content was less than 0.1% w / w as determined by H-NMR. The dried granulation was milled using a ball mill (Retch MM400) to an average particle size of 50 μm or less (D[4,3]) and vacuum sealed in alu-alu bags.
[0133] The particle size distribution of the granules thus obtained was approximately 90 vol.% < 90 μm, 50 vol.% < 45 μm and 10 vol.% < 15 μm.
[0134] 1The NHS-POX / NU-POx granules (1:1) were analyzed using H-NMR spectroscopy. 25 mg of granules were dissolved in trifluoroacetic acid (0.20 mL) by sonication for 20 min. After complete dissolution of the granules, the sample was diluted with deuterated dimethyl sulfoxide (DMSO-d6) (0.80 mL) containing maleic acid (2.5 mg / mL) as an internal standard and transferred to an NMR tube. 1 H-NMR spectra were recorded. From the spectra obtained, the amount of NHS bound to NHS-POx can be calculated, along with the molar ratio of NHS and amine groups present in the granulate. The amount of NHS bound to NHS-POx in the granulate is comparable to the amount of NHS bound to the NHS-POx starting material, indicating that no collapse or cross-linking occurs during granulation.
[0135] Total polymer recovery in the NMR samples, i.e., the combination of NHS-POx and NU-POx, was determined using known amounts of an internal standard (maleic acid) and recorded NMR spectra of different concentrations of NHS-POx and NU-POx. 1 The total polymer recovery was determined using a calibration curve generated from the H-NMR spectrum and was determined to be 99 percent, indicating that no insoluble crosslinked material was formed.
[0136] The NHS-POX / NU-POx granules (1:1) were further analyzed by size exclusion chromatography. 20 mg of the granules were treated with acetic anhydride (1.00 mL) at 50° C. for 1 h. Methanol (2.00 mL) was then added and the mixture was stirred at 50° C. for an additional 1 h. An aliquot (0.75 mL) was taken and all volatiles were removed under reduced pressure. The sample was dissolved in N,N-dimethylacetamide (2.50 mL) containing 50 mM lithium chloride, the eluent for SEC analysis. SEC was measured against poly(methyl methacrylate) standards and the M was calculated from the resulting size exclusion chromatogram. n , M wand PDI were determined. The PDI was below 1.5, indicating that no cross-linking occurred during granulation. Analytical validation of this size exclusion chromatography method showed that intentional cross-linking of NHS-POx and NU-POx at a level of 0.05 mol% increased the PDI to above 2.5.
[0137] Preparation of NHS-POx / NU-POx mixtures by co-lyophilization Co-lyophilized NHS-POx / NU-POx powder was prepared as follows: 2.4 g NU-POx was dissolved in 40 mL glacial acetic acid. After complete dissolution of the polymer, 2.0 g NHS-POx was added and the sample was sonicated for 30 min. The solution was flash frozen in liquid nitrogen and lyophilized. The resulting viscous solid was further dried under reduced pressure (<1 kPa) and vacuum sealed in an alu-alu bag. The co-lyophilized NHS-POx / NU-POx samples were not soluble in either trifluoroacetic acid or acetic anhydride due to the high degree of cross-linking between NHS-POx and NU-POx. 1 It could not be analysed by 1 H-NMR spectroscopy and size exclusion chromatography.
[0138] (Preparation of NHS-POx / NU-POx mixtures by dry blending) NHS-POx / NU-POx mixtures were prepared as follows: 2 g of NHS-POx and 2 g of NU-POx were dry mixed by tumble mixing for 30 min. The resulting powder was dried under reduced pressure (<1 kPa) and vacuum sealed in an alu-alu bag.
[0139] 1 The powder was analyzed using H-NMR spectroscopy. 25 mg of powder was dissolved in trifluoroacetic acid (0.20 mL) by sonication for 20 min. After complete dissolution of the powder, the sample was diluted with deuterated dimethyl sulfoxide (DMSO-d6) (0.80 mL) containing maleic acid (2.5 mg / mL) as an internal standard and transferred to an NMR tube. 1H-NMR spectrum was recorded, from which the amount of unreacted NHS was calculated to be 99 percent compared to NHS-POx.
[0140] Total polymer recovery in the NMR samples, i.e., the combination of NHS-POx and NU-POx, was determined using known amounts of an internal standard (maleic acid) and recorded NMR spectra of different concentrations of NHS-POx and NU-POx. 1 The total polymer recovery was determined using a calibration curve generated from the H-NMR spectrum and was determined to be 101 percent, indicating that no insoluble crosslinked material was formed.
[0141] The powder was further analyzed by size exclusion chromatography. 20 mg of powder was treated with acetic anhydride (1.00 mL) at 50° C. for 1 h. Methanol (2.00 mL) was then added and the mixture was stirred at 50° C. for an additional 1 h. An aliquot (0.75 mL) was taken and all volatiles were removed under reduced pressure. The sample was dissolved in N,N-dimethylacetamide (2.50 mL) containing 50 mM lithium chloride, the eluent for SEC analysis. SEC was measured against poly(methyl methacrylate) standards and the M was calculated from the resulting size exclusion chromatogram. n , M w and PDI was determined. The PDI was below 1.5, indicating that no crosslinking occurred during dry mixing.
[0142] (Preparation of NHS-POx / NU-POx (sequestering) granules) Lyophilization produced the following powders: [Phosphate powder] 42.66 g of sodium phosphate dibasic dihydrate and 26.56 g of sodium phosphate monobasic monohydrate were dissolved in 170 mL of ultrapure water. After complete dissolution, the pH was adjusted to 7 by adding 62 mL of 0.1 molar aqueous sodium hydroxide solution. The solution was frozen in liquid nitrogen and lyophilized. The resulting powder was dried under reduced pressure and vacuum sealed in an alu-alu bag. [Carbonate powder] A 1:1 mole / mole mixture of sodium carbonate and sodium bicarbonate was prepared by dissolving 25.31 g of sodium carbonate and 20.06 g of sodium bicarbonate in 350 mL of ultrapure water. The solution was flash frozen in liquid nitrogen and lyophilized. The resulting powder was dried under reduced pressure and vacuum sealed in an alu-alu bag. [NHS-POx / citric acid powder] 3.08 g of citric acid was dissolved in 10 mL of ultrapure water. The solution was cooled between 2 and 8 °C. Then, 7.00 g of NHS-POx was added and dissolved using a high-speed dispersing device (Ultra-Turrax, IKA). Immediately after mixing (2 min), the solution was flash frozen in liquid nitrogen and lyophilized overnight. The resulting powder was dried under reduced pressure and vacuum sealed in an alu-alu bag. [NU-POx / carbonate powder] Next, carbonate-containing NU-POx powder was produced as follows: 9.60 g of NU-POx and 0.80 g of carbonate powder were dissolved in 40 mL of ultrapure water. The solution was flash frozen using liquid nitrogen and lyophilized. The resulting powder was dried under reduced pressure and vacuum sealed in an alu-alu bag.
[0143] NHS-POx / NU-POx (sequestered) granulation was prepared as follows: 6.50 g NHS-POx / citric acid powder and 5.50 g phosphate powder were mixed in a high shear mixer. After obtaining a homogenous mixture, 0.40 mL IPA was added slowly with continued mixing until a homogenous snow-like powder was formed. Then, 5.41 g NU-POx / carbonate powder was added and mixing was stopped when a homogenous granulation was formed. The granulation was dried under vacuum until the IPA content was less than 0.1% w / w. The dried granulation was ground in a coffee grinder until the average particle size was 100 μm or less (D[4,3]) and vacuum sealed in an alu-alu bag.
[0144] (Preparation of reactive NHS-POx / NU-POx / P188 granules) The reactive NHS-POx / NU-POx granules described above were coated with Pluronic P188. Reactive NHS-POx / NU-POx granules coated with 2.5% w / w P188 were prepared by heating the NHS-POx / NU-POx granules with P188 powder in a high shear mixer at 65°C for 10 minutes and then cooling to ambient conditions. The coated granules were milled using a ball mill (Retch MM400) to an average particle size of 40 μm or less (D[4,3]) and vacuum sealed in alu-alu bags.
[0145] The particle size distribution of the granules thus obtained was approximately 90 vol.% < 80 μm, 50 vol.% < 40 μm, and 10 vol.% < 10 μm.
[0146] 1 The NHS-POx / NU-POx / P188 granules were analyzed using H-NMR spectroscopy. 25 mg of powder was dissolved in trifluoroacetic acid (0.20 mL) by sonication for 20 min. After complete dissolution of the granules, the sample was diluted with deuterated dimethyl sulfoxide (DMSO-d6) (0.80 mL) and transferred to an NMR tube. 1 H-NMR spectrum was recorded, from which the amount of unreacted NHS was calculated to be 98 percent compared to NHS-POx.
[0147] The NHS-POx / NU-POx / P188 granules were further analyzed by size exclusion chromatography. 20 mg of granules were treated with acetic anhydride (1.00 mL) at 50° C. for 1 h. Methanol (2.00 mL) was then added and the mixture was stirred at 50° C. for an additional 1 h. An aliquot (0.75 mL) was taken and all volatiles were removed under reduced pressure. The sample was dissolved in N,N-dimethylacetamide (2.50 mL) containing 50 mM lithium chloride, the eluent for SEC analysis. SEC was measured against poly(methyl methacrylate) standards and the M was calculated from the resulting size exclusion chromatogram. n , M w and PDI were determined. The PDI was less than 1.5, indicating that no cross-linking occurred during granulation.
[0148] (Preparation of reduced cross-linked gelatin (RXL)) Reduced cross-linked gelatin (RXL) was prepared according to three procedures: 12 g of gelatin powder (Gelita-SPON®, Gelita Medical GmbH) was dissolved in 350 mL of 0.1 molar aqueous sodium hydroxide solution by stirring at 40° C. for 2 hours. After obtaining a clear solution, the mixture was cooled to ambient temperature and the pH was adjusted to 7 by adding 32.5 mL of 1.0 molar aqueous hydrochloric acid solution. The solution was flash frozen using liquid nitrogen and freeze-dried. The powder was then ground in a coffee grinder, dried under reduced pressure and vacuum-sealed in an alu-alu bag. Hereafter, this reduced cross-linked gelatin is referred to as RXL-LS (low salt). 12 g of gelatin powder (Gelita-SPON®, Gelita Medical GmbH) was dissolved in 360 mL of 1.0 molar aqueous sodium hydroxide solution by stirring for 10 min at 40° C. The resulting clear solution was cooled to ambient temperature and the pH was reduced to 7 by adding 30 mL of concentrated hydrochloric acid solution (37% w / w). The solution was flash frozen using liquid nitrogen and freeze-dried. The powder was then ground in a coffee grinder, dried under reduced pressure, and vacuum-sealed in an alu-alu bag. Hereafter, this reduced cross-linked gelatin is referred to as RXL-HS (high salt). 12 g of gelatin powder (Gelita-SPON®, Gelita Medical GmbH) was dissolved in 350 mL of 0.1 molar aqueous sodium hydroxide solution by stirring at 40° C. for 2 hours. After obtaining a clear solution, the mixture was cooled to ambient temperature and the pH was adjusted to 7 by adding 32.5 mL of 1.0 molar aqueous hydrochloric acid. 400 mL of methanol was then added to the solution and the solution was placed in a −20° C. freezer for 16 hours to cause precipitation of RXL, which was isolated by decanting the liquid phase. RXL was washed three times with 100 mL portions of methanol and then dried under vacuum. The crude product was dissolved in 200 mL of ultrapure water, flash frozen in liquid nitrogen and lyophilized. The powder was ground in a coffee grinder, dried under reduced pressure and vacuum sealed in an alu-alu bag. Hereafter, this reduced cross-linked gelatin is referred to as RXL (salt-free).
[0149] Preparation of reactive NHS-POx / RXL granules (no salt, low salt and high salt) Reactive NHS-POx / RXL granules were prepared as follows: 5 g of blue NHS-POx powder was wetted with IPA in a high shear mixer until a homogenous snow-like powder containing approximately 1-2% w / w IPA was obtained. After this, 5 g of RXL, RXL-LS or RXL-HS powder was added and mixed. After mixing, 1 The wet granulation was dried under reduced pressure until the IPA content was less than 0.1% w / w as determined by H-NMR. The dried granulation was ground in a coffee grinder to an average particle size of 90 μm or less (D[4,3]) and vacuum sealed in alu-alu bags.
[0150] The particle size distribution of the granules thus obtained was approximately 90 vol.% < 190 μm, 50 vol.% < 60 μm and 10 vol.% < 15 μm.
[0151] Granules containing RXL 1The dispersion was analyzed by H-NMR spectroscopy. For this purpose, 1.0 mL of deuterated chloroform (CDCl3) containing 5% (v / v) acetic acid was added to 25 mg of the granulation. The NHS-POx was selectively extracted by ultrasonicating the sample for 20 min. The dispersion was passed through a 0.22 μm filter and transferred to an NMR tube. 1 H-NMR spectrum was recorded, from which the amount of unreacted NHS was calculated to be 98 percent compared to NHS-POx.
[0152] The recovery of NHS-POx in the NMR samples was evaluated using trimethylsilane as an internal standard as well as different concentrations of NHS-POx. 1 The total NHS-POx recovery was determined using a calibration curve generated from H-NMR spectra. The total NHS-POx recovery was determined to be 100 percent, indicating that no insoluble cross-linked material was formed.
[0153] The NHS-POx / RXL granulations were further analyzed by size exclusion chromatography. 1 An aliquot (0.15 mL) was removed from the solution used for H-NMR spectroscopy. This solution was diluted with N,N-dimethylacetamide (1.00 mL) containing 50 mM lithium chloride, the eluent for the SEC analysis. The SEC was run against poly(methyl methacrylate) standards, and the M n , M w and PDI was determined. The PDI was below 1.5, again indicating that no cross-linking occurred during granulation.
[0154] Preparation of NHS-POx / RXL mixtures by co-lyophilization Co-lyophilized NHS-POx / RXL powder was prepared as follows: 2.5 g of RXL powder was dissolved in 200 mL of ultrapure water. The pH was adjusted to 4.5 by adding acetic acid and the solution was cooled to 4° C. Then, 2.5 g of NHS-POx was added and dissolved by high shear stirring. Immediately after complete dissolution of NHS-POx, the solution was flash frozen in liquid nitrogen and lyophilized. The resulting powder was dried under reduced pressure and vacuum sealed in an alu-alu bag.
[0155] Co-lyophilized NHS-POx / RXL powder 1 The NHS-POx were analyzed by H-NMR spectroscopy. For this purpose, 1.0 mL of deuterated chloroform (CDCl3) containing 5% (v / v) acetic acid was added to 25 mg of the granulation. The NHS-POx were selectively extracted by ultrasonicating the sample for 20 min. The dispersion was passed through a 0.22 μm filter and transferred to an NMR tube. 1 H-NMR spectrum was recorded, from which the amount of unreacted NHS was calculated to be 93 percent compared to NHS-POx.
[0156] The recovery of NHS-POx in the NMR samples was evaluated using trimethylsilane as an internal standard as well as different concentrations of NHS-POx. 1 The total NHS-POx recovery was determined using a calibration curve generated from H-NMR spectra and was determined to be 81 percent, indicating that some insoluble cross-linked material was formed.
[0157] The NHS-POx / RXL powder was further analyzed by size exclusion chromatography. 1 An aliquot (0.15 mL) was removed from the solution used for H-NMR spectroscopy. This solution was diluted with N,N-dimethylacetamide (1.00 mL) containing 50 mM lithium chloride, the eluent for the SEC analysis. The SEC was run against poly(methyl methacrylate) standards, and the M n , M w and PDI were determined. The PDI was 3.3, indicating that cross-linking occurred during the co-lyophilization of both components.
[0158] (Preparation of NHS-POx / RXL mixtures by dry blending) The NHS-POx / RXL mixture was prepared as follows: 2 g of RXL powder and 2 g of NHS-POx were dry mixed by tumble mixing for 30 minutes. The resulting powder was dried under reduced pressure and vacuum sealed in an alu-alu bag.
[0159] Powder 1 The NHS-POx were analyzed by H-NMR spectroscopy. For this purpose, 1.0 mL of deuterated chloroform (CDCl3) containing 5% (v / v) acetic acid was added to 25 mg of the granulation. The NHS-POx were selectively extracted by ultrasonicating the sample for 20 min. The dispersion was passed through a 0.22 μm filter and transferred to an NMR tube. 1 H-NMR spectrum was recorded, from which the amount of unreacted NHS was calculated to be 100 percent compared to NHS-POx.
[0160] The recovery of NHS-POx in the NMR samples was evaluated using trimethylsilane as an internal standard as well as different concentrations of NHS-POx. 1 The total NHS-POx recovery was determined using a calibration curve generated from H-NMR spectra and was determined to be 104 percent, indicating that no insoluble cross-linked material was formed.
[0161] The NHS-POX / RXL powder was further analyzed by size exclusion chromatography. 1 An aliquot (0.15 mL) was removed from the solution used for H-NMR spectroscopy. This solution was diluted with N,N-dimethylacetamide (1.00 mL) containing 50 mM lithium chloride, the eluent for the SEC analysis. The SEC was run against poly(methyl methacrylate) standards, and the M n , M w and PDI was determined. The PDI was below 1.5, indicating that no crosslinking occurred during dry mixing.
[0162] Preparation of Reactive NHS-POx / RXL Granules Containing Carbonate First, a 1:1 mole / mole mixture of sodium carbonate and sodium bicarbonate was prepared by dissolving 25.31 g of sodium carbonate and 20.06 g of sodium bicarbonate in 350 mL of ultrapure water. The solution was flash frozen in liquid nitrogen and lyophilized. The resulting powder was dried under reduced pressure and vacuum sealed in an alu-alu bag.
[0163] NHS-POx / RXL / carbonate granules were prepared as follows: 5g of RXL-LS or RXL-HS was mixed with 0.178g of sodium carbonate / bicarbonate using a high shear mixer. 5g of blue NHS-POx containing approximately 1-2% w / w IPA was then added and mixed until a homogenous powder was obtained. After mixing, 1 The wet granulation was dried under reduced pressure until the IPA content was less than 0.1% w / w as determined by H-NMR. The dried granulation was ground in a coffee grinder to an average particle size of 100 μm or less (D[4,3]) and vacuum sealed in alu-alu bags.
[0164] (Preparation of reactive NHS-POx / NH2-PEG granules) NHS-POx (6.9 g) was wetted with IPA in a high shear mixer until a homogenous snow-like powder containing about 1-2% w / w IPA was obtained, followed by the addition of 8.1 g of Amine-PEG-amine, 2-arm, MW2k (ex-Creative PEGWorks) (molar ratio 1:1.16, the molar ratio referring to the ratio of the number of NHS groups provided by NHS-POx to the number of amine groups provided by PEG-amine). 1 The formed granulation was dried under reduced pressure until the IPA content was less than 0.1% w / w as determined by H-NMR. The dried granulation was ground in a coffee grinder to an average particle size of 100 μm or less (D[4,3]) and vacuum sealed in alu-alu bags.
[0165] 1The NHS-POX / NH2-PEG granules were analyzed using H-NMR spectroscopy. 25 mg of granules were dissolved in trifluoroacetic acid (0.20 mL) by sonication for 20 min. After complete dissolution of the granules, the sample was diluted with deuterated dimethyl sulfoxide (DMSO-d6) (0.80 mL) and transferred to an NMR tube. 1 H-NMR spectrum was recorded, from which the amount of unreacted NHS was calculated to be 97 percent compared to NHS-POx.
[0166] The NHS-POX / NH2-PEG granules were further analyzed by size exclusion chromatography. 20 mg of the granules were treated with acetic anhydride (1.00 mL) at 50° C. for 1 h. Methanol (2.00 mL) was then added and the mixture was stirred at 50° C. for an additional 1 h. An aliquot (0.75 mL) was taken and all volatiles were removed under reduced pressure. The sample was dissolved in N,N-dimethylacetamide (2.50 mL) containing 50 mM lithium chloride, the eluent for SEC analysis. SEC was measured against poly(methyl methacrylate) standards and the M was determined from the resulting size exclusion chromatogram. n , M w and PDI were determined. The PDI was less than 1.5, indicating that no cross-linking occurred during granulation.
[0167] (Preparation of Starch / NHS-POx / NU-POx Granules) Lyophilization produced the following starch powders: [NHS-POx / starch powder] 2.79 g of starch (Arista™ AH, BARD) was dispersed in 50 mL of ultrapure water using a high shear mixer. The dispersion was cooled to between 2 and 8° C. and 0.71 g of NHS-POx was added and dissolved using a high shear mixer. Immediately after dissolution of NHS-POx, the solution was flash frozen using liquid nitrogen and lyophilized. The resulting powder was dried under reduced pressure and vacuum sealed in alu-alu bags. [NU-POx / starch powder] 1.45 g of starch (Arysta™ AH, BARD) was dispersed in 30 mL of ultrapure water using a high shear mixer. Then, 0.36 g of NU-POx was added and dissolved. After complete dissolution of NU-POx, the dispersion was flash frozen using liquid nitrogen and lyophilized. The resulting powder was dried under reduced pressure and vacuum sealed in an alu-alu bag. [NU-POx / starch / sodium carbonate powder] 2.25 g of starch (Arysta™ AH, BARD) was dispersed in 50 mL of ultrapure water using a high shear mixer. Then, 0.58 g of NU-POx and 0.25 g of sodium carbonate were added and dissolved. After complete dissolution of NU-POx, the dispersion was flash frozen using liquid nitrogen and lyophilized. The resulting powder was dried under reduced pressure and vacuum sealed in an alu-alu bag.
[0168] Two granulations were prepared from these three powders. Starch / NHS-POx / NU-POx granulations were prepared as follows: [Starch granules 1] 1.41 g of NHS-POx / starch powder, 1.68 g of NU-POx / starch powder and 0.20 mL of IPA were mixed using a pestle and mortar. After obtaining a homogenous granulation, the residual IPA was removed under reduced pressure until the IPA content was less than 0.1% w / w. The dried granulation was ground using a coffee grinder until the average particle size was 100 μm or less (D[4,3]) and vacuum sealed in an alu-alu bag. [Starch granules 2] 1.20 g of NHS-POx / starch powder, 1.45 g of NU-POx / starch / sodium carbonate powder 3 and 0.15 mL of IPA were mixed using a pestle and mortar. After formation of a homogenous granulation, the residual IPA was removed under reduced pressure until the IPA content was less than 0.1% w / w. The dried granulation was ground using a coffee grinder until the average particle size was 100 μm or less (D[4,3]) and vacuum sealed in an alu-alu bag.
[0169] (Preparation of reactive NHS-POx / Gelita Spon granules) 7.01 g of pre-dried gelatin powder (Gelita-SPON®, formerly Gelita Medical GmbH) with a moisture content of less than 0.2% w / w was dispersed in dichloromethane (200 mL) using a high shear mixer operating at 20,000 rpm for 20 min. NHS-POx (7.02 g) was then added and stirring was continued for 5 min. NHS-POx did not dissolve. All volatiles were removed from the suspension under reduced pressure. The resulting powder was ground using a coffee grinder until the average particle size was ≤95 μm (D[4,3]), vacuum sealed in an alu-alu bag, further dried under reduced pressure and vacuum sealed in an alu-alu bag.
[0170] The particle size distribution of the granules thus obtained was approximately 90 vol.% < 190 μm, 50 vol.% < 80 μm and 10 vol.% < 15 μm.
[0171] Granulated material 1 The NHS-POx were analyzed by H-NMR spectroscopy. For this purpose, 1.0 mL of deuterated chloroform (CDCl3) containing 5% (v / v) acetic acid was added to 25 mg of the granulation. The NHS-POx were selectively extracted by ultrasonicating the sample for 20 min. The dispersion was passed through a 0.22 μm filter and transferred to an NMR tube. 1 H-NMR spectrum was recorded, from which the amount of unreacted NHS was calculated to be 97 percent compared to NHS-POx.
[0172] The granulation was further analyzed by size exclusion chromatography (SEC) analysis. An aliquot (0.15 mL) of the filtered NHS-POx extract described above was diluted with N,N-dimethylacetamide (1.00 mL) containing 50 mM lithium chloride, the eluent for SEC analysis. The sample was analyzed by SEC against a poly(methyl methacrylate) standard with a PDI of 1.45, indicating that no crosslinking had occurred.
[0173] (Preparation of reactive NHS-POx / chitosan granules) Reactive NHS-POx / chitosan granules were prepared as follows: 5 g of NHS-POx powder was wetted with IPA in a high shear mixer until a homogenous snow-like powder containing approximately 1-2% w / w IPA was obtained. After this, 5 g of chitosan powder (Shanghai Waseta International, DAC degree 85%) was added and mixed. After mixing, the wet granulation was 1 The dried material was dried under reduced pressure until the IPA content was less than 0.1% w / w as determined by H-NMR. The dried granules were ground in a coffee grinder until the average particle size was 200 μm or less (D[4,3]) and vacuum sealed in alu-alu bags.
[0174] The particle size distribution of the granules thus obtained was approximately 90 vol.% < 350 μm, 50 vol.% < 180 μm and 10 vol.% < 60 μm.
[0175] Granulated material 1 The NHS-POx were analyzed by H-NMR spectroscopy. For this purpose, 1.0 mL of deuterated chloroform (CDCl3) containing 5% (v / v) acetic acid was added to 25 mg of the granulation. The NHS-POx were selectively extracted by ultrasonicating the sample for 20 min. The dispersion was passed through a 0.22 μm filter and transferred to an NMR tube. 1 H-NMR spectrum was recorded, from which the amount of unreacted NHS was calculated to be 95 percent compared to NHS-POx.
[0176] The recovery of NHS-POx in the NMR samples was evaluated using trimethylsilane as an internal standard as well as different concentrations of NHS-POx. 1 The total NHS-POx recovery was determined using a calibration curve generated from H-NMR spectra. The total NHS-POx recovery was measured to be 103 percent, indicating that no insoluble cross-linked material was formed.
[0177] The NHS-POX / chitosan granules were further analyzed by size exclusion chromatography. 1An aliquot (0.15 mL) was removed from the solution used for H-NMR spectroscopy. This solution was diluted with N,N-dimethylacetamide (1.00 mL) containing 50 mM lithium chloride, the eluent for the SEC analysis. The SEC was run against poly(methyl methacrylate) standards, and the M n , M w and PDI were determined. The PDI was less than 1.5, indicating that no cross-linking occurred during granulation.
[0178] Preparation of NHS-POx / chitosan mixtures by co-lyophilization Co-lyophilized NHS-POx / chitosan powder was prepared as follows: 2.5 g of chitosan powder (Shanghai Waseta International, DAC degree 85%) was dissolved in 200 mL of 0.2% v / v acetic acid solution in ultrapure water. The pH was adjusted to 4.5 by adding acetic acid and the solution was cooled to 4°C. Then, 2.5 g of NHS-POx was added and dissolved by high shear stirring. Immediately after complete dissolution of NHS-POx, the solution was flash frozen in liquid nitrogen and lyophilized. The resulting powder was dried under reduced pressure and vacuum sealed in alu-alu bags.
[0179] Granulated material 1 The NHS-POx were analyzed by H-NMR spectroscopy. For this purpose, 1.0 mL of deuterated chloroform (CDCl3) containing 5% (v / v) acetic acid was added to 25 mg of the granulation. The NHS-POx were selectively extracted by ultrasonicating the sample for 20 min. The dispersion was passed through a 0.22 μm filter and transferred to an NMR tube. 1 H-NMR spectrum was recorded, from which the amount of unreacted NHS was calculated to be 12 percent compared to NHS-POx, implying that crosslinking and / or hydrolysis had occurred.
[0180] The recovery of NHS-POx in the NMR samples was evaluated using trimethylsilane as an internal standard as well as different concentrations of NHS-POx. 1The total NHS-POx recovery was determined using a calibration curve generated from the H-NMR spectrum and was determined to be 11 percent (consistent with the NMR results), indicating that an insoluble cross-linked material was formed.
[0181] The NHS-POX / chitosan granulations were further analyzed by size exclusion chromatography. 1 An aliquot (0.15 mL) was removed from the solution used for H-NMR spectroscopy. This solution was diluted with N,N-dimethylacetamide (1.00 mL) containing 50 mM lithium chloride, the eluent for the SEC analysis. The SEC was run against poly(methyl methacrylate) standards, and the M n , M w and the PDI was determined. The PDI was determined to be 5.4, indicating that crosslinking had occurred.
[0182] (Preparation of NHS-POx / Chitosan Mixtures by Dry Blending) The NHS-POx / chitosan mixture was prepared as follows: 2 g of chitosan powder (Shanghai Waseta International, DAC degree 85%) and 2 g of NHS-POx were dry mixed by tumble mixing for 30 min. The resulting powder was dried under reduced pressure and vacuum sealed in an alu-alu bag.
[0183] Powder 1 The NHS-POx were analyzed by H-NMR spectroscopy. For this purpose, 1.0 mL of deuterated chloroform (CDCl3) containing 5% (v / v) acetic acid was added to 25 mg of the granulation. The NHS-POx were selectively extracted by ultrasonicating the sample for 20 min. The dispersion was passed through a 0.22 μm filter and transferred to an NMR tube. 1 H-NMR spectrum was recorded, from which the amount of unreacted NHS was calculated to be 99 percent compared to NHS-POx.
[0184] The recovery of NHS-POx in the NMR samples was evaluated using trimethylsilane as an internal standard as well as different concentrations of NHS-POx. 1The total NHS-POx recovery was determined using a calibration curve generated from H-NMR spectra and was determined to be 96 percent, indicating that no insoluble cross-linked material was formed.
[0185] The NHS-POX / chitosan powder was further analyzed by size exclusion chromatography. 1 An aliquot (0.15 mL) was removed from the solution used for H-NMR spectroscopy. This solution was diluted with N,N-dimethylacetamide (1.00 mL) containing 50 mM lithium chloride, the eluent for the SEC analysis. The SEC was run against poly(methyl methacrylate) standards, and the M n , M w and PDI was determined. The PDI was below 1.5, indicating that no crosslinking occurred during dry mixing.
[0186] (Adhesive fibrous carrier structure) The following commercially available hemostatic products were selected for use as fibrous carrier structures in the preparation of tissue adhesive sheets according to the present invention: Gelita Tuft-It®: A cohesive fibrous carrier structure consisting of eight layers of reduced cross-linked gelfoam fibers. The eight layers, each about 2 mm thick, have dimensions of 50 mm x 75 mm. The moisture content of Gelita Tuft-It® is 15% or less. The product was dried in a vacuum oven at 40°C for several hours to reduce the moisture content to 2.0% w / w or less (determined by gravimetry) before impregnating the agglomerated particles.
[0187] (Bleeding experiment) Hemostatic efficacy was assessed using standardized ex-vivo and in-vivo porcine bleeding models. All models used heparin to prolong clotting times, increasing the activated clotting time (ACT) by approximately 2-3 fold.
[0188] Ex-vivo model: A live ex-vivo porcine model with a fresh liver perfused with fresh heparinized blood from the slaughterhouse to mimic the actual in-vivo environment as closely as possible. The liver is attached to a perfusion machine that maintains oxygenation, blood pH, temperature and blood pressure within the biologic boundaries. Two livers and 10 liters of heparinized blood (5000 units / L) are collected at the slaughterhouse. The livers are shipped on ice and the blood at ambient temperature. Within 2 hours of collection, the livers are inspected for lesions and closed with gloves and cyanoacrylate glue. Perfusion parameters: flow rate 600 ml / min, pressure 10-12 mmHg, temperature 37°C (+ / - 1°C), carbogen 0.25 liters per minute. A circular bleeding wound (8 mm diameter) is created on the liver surface using a flat round rotary scraping tool, with a rubber onlay so that the depth of the punched bleeding area is always 3 mm. Once the liver is properly perfused (check color and temperature), test the sample according to the following procedure: cut the sample to the appropriate size (2.7 x 2.7 cm); turn on the camera; check the number of sites with the camera; punch an 8 mm biopsy; cut and remove the biopsy; remove blood from the bleeding site with gauze (2x); collect blood with pre-weighed gauze for 30 seconds; score the bleeding (by 2 investigators); pour hemostatic powder into the bleeding site and distribute the powder evenly using a stainless steel spatula; observe for 5 minutes (check and score for adhesion and coagulation) and repeat after 30 minutes.
[0189] In vivo model: A standardized combination penetrating splenic rupture is induced in anesthetized pigs (domestic pig, male, weight range: 40 kg, adult). A midline laparotomy is performed to access the spleen and other organs. A scalpel is used to create n=3 (S1...S3) subcapsular standardized lesions (10 mm x 10 mm). The hemostatic product is applied with gentle pressure by pre-moistened gauze (saline) and held down for 1 min. After application of the product, the time to hemostasis (TTH) is assessed. A TTH equal to zero means that hemostasis is already achieved after 1 min of pressure.
[0190] Granulation scoring system: Coagulation ++++ Achieved immediately after application +++ Achieved within <10 seconds of application ++ Achieved within <30 seconds of application + Achieved within 3 minutes of application - Not achieved
[0191] Granulation scoring system: adhesion 10 minutes after application ++++ Very strong adhesion (hardly any solidified granulation can be removed) +++ Strong adhesion (solidified granulation is difficult to remove) ++ Strong adhesion (solidified granulation can be removed) + Moderate adhesion (solidified granulation is easily removed) + / - Mild adhesion (clotted granulation is removed by blood flow) - Not achieved
[0192] Patch scoring system: Clotting ++++ Achieved immediately after tamponade +++ Achieved <10 seconds after tamponade ++ Achieved <30 seconds after tamponade + Achieved within 3 minutes of tamponade Achieved after + / - 3 minutes, apply second tamponade - Not achieved
[0193] Patch scoring system: 10 minutes after application ++++ Very strong adhesion (patch breaks upon removal) +++ Strong adhesion (patch breaks when removed) ++ Strong adhesion (patch can be removed without damage) + Moderate adhesion (patch can be removed without damage) + / - Mild adhesion (patch can be removed without damage) - Not achieved
[0194] [Example 1] The hemostatic properties of the different reactive granules were evaluated in the ex vivo and in vivo bleeding tests described above, and the results are summarized in Tables 1 and 2.
[0195] [Table 1] [Table 2]
[0196] [Example 2] Impregnation of the support structure with particle agglomerates A Gelita Tuft-It® patch (50×75 mm, approx. 0.71 g) was impregnated with blue-dyed NHS-POx / NU-POx (1:0.6) granulation using mechanical shaking. A paint shaker (VIBA PRO V from Collomix GmbH) was used to introduce the powder (approx. 0.75 g) into the patch. The holder of the array containing the carrier structure was clamped to the machine. The array was vibrated vertically.
[0197] The impregnated samples were placed on a PMMA plate and placed in an oven, where the samples were subjected to different heat treatments. To evaluate the powder adhesion, the samples were moved twice on the white PMMA plate. The results were considered as stuck if no blue powder was released. The results are shown in Table 3.
[0198] [Table 3]
[0199] NHS-POx / NU-POx granules are hygroscopic. At ambient temperature and below 40% relative humidity (RH), fibrous support structures can be reproducibly impregnated within 30 minutes of exposure. However, when impregnation is performed at, for example, 75% RH and 25° C., the granules become viscous within minutes, resulting in non-reproducible and inhomogeneous impregnation characteristics.
[0200] [Example 3] A hemostatic patch (Gelita Tuft-It®; 50×75 mm, approximately 0.7 g) was impregnated with reactive NHS-POx / NU-POx (1:0.6) granulation as described above. One gram of the granulation was distributed throughout the patch as described in Example 2. The hemostatic patch was then loaded into an alu-alu pouch containing 1 g of silica and vacuum sealed.
[0201] The patches were cut into 2 cm x 2 cm pieces and tested in triplicate in an ex vivo liver perfusion model. The time to hemostasis (TTH) was 0 (after 1 min of compression) and no rebleeding was observed during the 30 min observation period. The patches were also found to have high flexibility and bending properties.
[0202] Furthermore, the patch was evaluated in an in vivo porcine heparinization model. The patch was found to have very good clotting and adhesion properties. Active bleeding was efficiently stopped in the resection of different organs: spleen, liver and kidney. A summary of the results is shown in Table 3.
[0203] [Table 4]
[0204] [Example 4] A hemostatic patch (Gelita Tuft-It®; 50×75 mm, approximately 0.7 g) was impregnated with NHS-POx / NU-POx / P188 2.5%. One gram of granulation was distributed throughout the patch as described in Example 2. The hemostatic patch was then loaded into an alu-alu pouch containing 1 g of silica and vacuum sealed.
[0205] The patch was evaluated in an in vivo porcine heparinization model. The patch was found to have very good clotting and sufficient adhesive properties. The reduced adhesive properties allowed the patch to be removed in one piece, in contrast to an identical patch without P188. Active bleeding was efficiently stopped in the resection of different organs: spleen, liver and kidney. A summary of the results is shown in Table 4.
[0206] [Table 5]
[0207] [Example 5] Gelita Tuft-It® (50×75 mm, approximately 0.7 g) was impregnated with different reactive polymer powders. The hemostatic properties of the so obtained patches were tested in ex-vivo and in-vivo porcine bleeding models as previously described herein.
[0208] A pneumatic shaking device was used to impregnate the fibrous carrier structure with 1.4 g of powder. The fibrous carrier sheet was vibrated vertically. A long stroke engine (NTK 25 AL L, ex Netter Vibration GmbH) was operated at 6 bar, 11 Hz and an amplitude of 30 mm. Four cycles of 15 seconds were used to disperse the powder on the sheet. The granulation was distributed over the entire thickness of the sheet. The distribution over the entire surface of the sheet was also homogenous.
[0209] Seven different reactive granulations were tested. These granulations contained NHS-POx in combination with a water-soluble nucleophilic polymer. The preparation of these granulations has been previously described herein.
[0210] The granulations tested are listed below: NHS-POx / Jerita Spon NHS-POx / RXL (high salt) Carbonate-containing NHS-POx / RXL (high salinity) NHS-POx / RXL (low salinity) NHS-POx / NH2-PEG
[0211] The different combinations of fibrous support structures and reactive polymer powders that were tested are shown in Table 5.
[0212] [Table 6]
[0213] The results obtained with these patches in ex-vivo and in-vivo porcine bleeding models are summarized in Table 6.
[0214] [Table 7]
[0215] [Comparative example A] 7.03 g of NHS-POx was dispersed in 50 mL dichloromethane (DCM). A cloudy mixture was formed and IPA (4 mL) was slowly added to obtain a clear solution. 7.00 g of pre-dried gelatin (Gelita-SPON®, Gelita Medical GmbH) was dispersed in DCM / IPA (150 mL / 12 mL) at room temperature for 20 min using a high shear mixer operating at 20,000 rpm. The prepared NHS-POx solution was added and the dispersion was stirred at 20,000 rpm for 5 min. Afterwards, all volatiles were removed under reduced pressure. The formed granulation was ground using a coffee grinder, dried under reduced pressure and vacuum sealed in an alu-alu bag.
[0216] Granulated material 1 H-NMR spectroscopy and size exclusion chromatography were used to analyze the gelatin / NHS-POx granules. The results so obtained showed that NHS-POx was not present in the gelatin / NHS-POx granules, indicating that complete cross-linking between NHS-POx and gelatin had occurred.
[0217] [Example 6] Experiments were conducted to determine the effect of NU-POx content of reactive NHS-POx / NU-POx granulations on the in-vivo performance of hemostatic patches.
[0218] (Impregnation method) Hemostatic patches (Gelita Tuft-It®; 50×75 mm, approximately 0.7 g) were impregnated with reactive NHS-POx / NU-POx granules prepared by acetone granulation in molar ratios of 1:0.10, 1:0.20, and 1:0.40, the molar ratio referring to the ratio of the number of NHS groups provided by NHS-POx to the number of amine groups provided by NU-POx. The same hemostatic patches were also impregnated with reactive NHS-POx powder.
[0219] Using a Fibroline SL-Preg lab machine, 1 gram of granulation / powder was distributed throughout the patch. The hemostatic patch was then cemented, dried, loaded into an alu-alu pouch containing 1 gram of silica, and vacuum sealed.
[0220] 〔machine〕 The Fibroline SL-Preg laboratory machine moves particles between electrodes by applying voltages of up to 40 kV at frequencies of up to 200 Hz for periods of up to 60 seconds. The two electrode plates are approximately 50 x 40 cm in size. The upper plate is grounded.
[0221] The following standard settings were used: 40 kV, 100 Hz, 20 s.
[0222] 〔array〕 After attaching the 3D printed PMMA array to the lower electrode plate, the powder was poured into the array by gravity. A scraping carton or metal spatula was used to fill the array with reactive polymer powder. The array was 50 x 75 x 4 mm and contained 22 x 33 = 726 square wells (inner dimensions of each well: 2 x 2 x 2 mm). The total volume of the 726 wells was approximately 5.8 mL.
[0223] [Spacer] A spacer mask was placed on top of the array. The use of a spacer allows the particles to move up and down when subjected to an alternating electric field. If a spacer is not used, it limits penetration into and distribution through the carrier. In the case of the Tuft-IT this was a 3mm mask. This gives an electrode distance of 3+4mm=7mm.
[0224] The in vivo performance of hemostatic patches containing NHS-POx:NU-POx granules (0, 10, 20 and 40 percent of amine groups from NU-POx, percentages calculated based on the number of NHS groups provided by NHS-POx) or NHS-POx powder was evaluated in a non-heparinized in-vivo porcine model. Details of the tested patches are shown in Table 7.
[0225] [Table 8]
[0226] (In vivo test) Studies were performed on adult female domestic pigs (40-50 kg). No anticoagulant was applied. Patch performance was tested on both the spleen and liver. The spleen or liver were located and exposed as necessary over the course of the study period, and their natural moisture was maintained by covering them with saline-soaked sponges.
[0227] Different types of damage created: Liver: abrasion, biopsy punch and excision wound Spleen: resection wound
[0228] Appropriately sized portions of liver parenchyma were abraded / punched to induce moderate to severe bleeding. Liver abrasions were made with a scalpel and a 1x1 cm2 template, and circular punches were made using an 8 mm circular biopsy punch. Liver and spleen resection wounds were made using a surgical knife.
[0229] Patches were applied immediately after tissue excision or scarification: Biopsy punch and 2 x 2 cm pieces for scraping Complete 7.5 x 5 cm patch for excision wound
[0230] The test patch was applied to the bleeding tissue and gently pressed by applying pressure using gauze pre-moistened with saline solution. Tamponade was applied initially for a 10 second period, followed by a 30 second interval, up to a total of 5 minutes.
[0231] An unimpregnated Tuft-IT patch was used as a reference (referred to as Tuft-IT).
[0232] The results of the in vivo studies are summarized in Table 8.
[0233] [Table 9]
[0234] Patches 1-4 showed very strong tissue adhesion, whereas only mild adhesion was observed for the Tuft-IT patch.
[0235] Patches 1 and 2 showed very little swelling after application, while patches 3-4 showed more significant, but still acceptable, swelling.
[0236] [Example 7] Hemostatic patches (Gelita Tuft-It®; 50×75 mm, approximately 0.7 g) were impregnated with either a solution of NHS-POx, NHS-POx powder, or NHS-POx / NU-POx granules. The NHS-POx / NU-POx granules used were made by acetone granulation at a molar ratio of 1:0.20 (see Example 8).
[0237] A spray solution containing NHS-POx was prepared by dissolving NHS-POx in a 1:1 mixture of isopropyl alcohol and dichloromethane (200 g / L). Using a laboratory glass sprayer and pressurized air, 5 mL of this spray solution was impregnated into the patches in one spray cycle. The total amount of NHS-POx delivered in this manner was 1 gram per patch. After impregnation, the patches were dried in an oven at 40° C. for 2 hours and then stored in a desiccator for 2 days before being loaded into an alu-alu pouch containing 1 g of silica and vacuum sealed.
[0238] Additionally, using the procedure described in Example 8, patches were impregnated with 1 gram of NHS-POx powder or 1 gram of NHS-POx / NU-POx granulation.
[0239] The performance of the so-prepared patches was tested in triplicate in an ex vivo liver perfusion model under mild (<20 mL / min) and severe bleeding (>50 mL / min) conditions. A circular bleeding wound (8 mm diameter) was created on the liver surface using a flat round rotary scraping tool, and a rubber onlay was used to ensure that the punched bleeding area was always 3 mm deep. The results are shown in Table 9.
[0240] [Table 10]
[0241] [Example 8] Hemostatic powder was prepared by mixing NHS-POx / NU-POx granules with hemostatic starch powder (Arysta™ AH, formerly BARD). The NHS-POx / NU-POx granules used were made by acetone granulation at a molar ratio of 1:0.20 (see Example 8).
[0242] The NHS-POx / NU-POx granulation was mixed with starch powder in a pestle and mortar in 80 / 20 and 90 / 10 w / w ratios.
[0243] The gel forming ability of these powder blends, pure starch powder and pure NHS-POx / NU-POx granules was evaluated as follows: The test tube was loaded with 20 mg of powder sample. 250 μL of heparinized sheep blood was added and the mixture was immediately mixed for 10 seconds using a vortex mixer. After 2 minutes, the test tube was placed upside down to determine if a gel had formed. If a gel had formed, 1 mL of water was added to the gel and after 30 minutes it was determined whether the gel remained intact. The results are shown in Table 10.
[0244] [Table 11]
Claims
1. 1. A hemostatic powder comprising at least 10 wt. % particle aggregates, the particle agglomerates have diameters in the range of 1 to 500 μm; The particle agglomerates are (a) an electrophilic polyoxazoline particle comprising an electrophilic polyoxazoline bearing at least three reactive electrophilic groups, the at least three reactive electrophilic groups being capable of reacting with amine groups in blood to form covalent bonds; and (b) nucleophilic polymer particles comprising a water-soluble nucleophilic polymer bearing at least three reactive nucleophilic groups, said at least three reactive nucleophilic groups being capable of reacting in the presence of water with said reactive electrophilic groups of said electrophilic polyoxazoline to form a covalent bond between said electrophilic polyoxazoline and said nucleophilic polymer. Including, A hemostatic powder, wherein a portion of said electrophilic polyoxazoline particles and said nucleophilic polymer particles in said particle agglomerates are crosslinked.
2. 2. The hemostatic powder of claim 1, wherein said nucleophilic polymer is selected from proteins, chitosan, nucleophilic polyoxazolines, nucleophilic polyethylene glycols, polyethyleneimines, and combinations thereof.
3. 3. The hemostatic powder of claim 2, wherein said nucleophilic polymer is selected from gelatin, collagen, and combinations thereof.
4. 4. The hemostatic powder of claim 3, wherein said nucleophilic polymer is gelatin.
5. The hemostatic powder described in claim 3, wherein the nucleophilic polymer is reduced cross-linked gelatin.
6. 3. The hemostatic powder of claim 2, wherein said nucleophilic polymer is a nucleophilic polyoxazoline.
7. 3. The hemostatic powder of claim 2, wherein said nucleophilic polymer is chitosan.
8. 8. The hemostatic powder of any one of claims 1 to 7, wherein said electrophilic polyoxazoline contains at least 8 reactive electrophilic groups.
9. 9. The hemostatic powder of any one of claims 1 to 8, wherein the reactive electrophilic groups of the electrophilic polyoxazoline are selected from carboxylate esters, sulfonate esters, phosphonate esters, pentafluorophenyl esters, p-nitrophenyl esters, p-nitrothiophenyl esters, acid halide groups, anhydrides, ketones, aldehydes, isocyanates, thioisocyanates, isocyano, epoxides, activated hydroxyl groups, olefins, glycidyl ethers, carboxyls, succinimidyl esters, sulfosuccinimidyl esters, maleimides (maleimidyl), ethenesulfonyl, imidoesters, acetoacetates, haloacetals, orthopyridyl disulfides, dihydroxyphenyl derivatives, vinyls, acrylates, acrylamides, iodoacetamides, and combinations thereof.
10. 10. The hemostatic powder of any one of claims 1 to 9, wherein said particle agglomerates contain at least 10 wt.% of said electrophilic polyoxazoline and at least 10 wt.% of said nucleophilic polymer.
11. 11. The hemostatic powder of any one of claims 1 to 10, wherein the combination of said electrophilic polyoxazoline and said nucleophilic polymer comprises at least 50 wt.% of said particle aggregates.
12. 12. The hemostatic powder of any one of claims 1 to 11, wherein the ratio between the total number of reactive electrophilic groups provided by said electrophilic polyoxazoline and the total number of reactive nucleophilic groups provided by said nucleophilic polymer is in the range of 1:1.5 to 1.5:
1.
13. (a) an electrophilic polyoxazoline particle comprising an electrophilic polyoxazoline bearing at least three reactive electrophilic groups, the at least three reactive electrophilic groups being capable of reacting with amine groups in blood to form covalent bonds; (b) a method of preparing a hemostatic particle aggregate with a nucleophilic polymer particle comprising a water-soluble nucleophilic polymer bearing at least three reactive nucleophilic groups, said at least three reactive nucleophilic groups being capable of reacting with said reactive electrophilic groups of said electrophilic polyoxazoline to form a covalent bond between said electrophilic polyoxazoline and said nucleophilic polymer, comprising: the method comprising combining 100 parts by weight of the electrophilic polyoxazoline particles and 10 to 1000 parts by weight of the nucleophilic polymer particles in the presence of a non-aqueous granulation liquid; In the hemostatic particle aggregate, a portion of the electrophilic polyoxazoline particles and the nucleophilic polymer particles are crosslinked; The method of claim 1, wherein the non-aqueous granulation liquid comprises at least 60 wt.% of an organic solvent selected from isopropyl alcohol, ethanol, methanol, diethyl ether, heptane, hexane, pentane, cyclohexane, dichloromethane, acetone, and mixtures thereof.
14. 14. The method of claim 13, comprising wetting the electrophilic polyoxazoline particles with the non-aqueous granulation liquid and then combining the wetted electrophilic polyoxazoline particles with the nucleophilic polymer particles.
Citation Information
Patent Citations
hemostatic components
JP2014533988A
Crosslinked polymers and medical products derived from nucleophilically activated polyoxazolines
JP2015511507A
Hemostatic compositions
US20130129710A1