High-strength hot-dip galvanized steel sheet with excellent surface quality and electric resistance spot weldability, and its manufacturing method
By controlling the hardness ratio between the surface and interior layers of galvanized steel sheets through precise manufacturing processes, the issues of liquid metal embrittlement and surface oxide formation are mitigated, improving the spot weldability and quality of high-strength galvanized steel sheets.
Patent Information
- Application Number
- JP2022536982
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-20
- Filing Date
- 2020-12-18
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-12-18
AI Technical Summary
High-strength galvanized steel sheets face issues with spot weldability due to liquid metal embrittlement and surface oxide formation, which compromise the strength and quality of the welds.
A galvanized steel sheet with controlled hardness ratio between the surface layer and interior, achieved through specific manufacturing processes including reheating, rolling, pickling, and annealing, to reduce the likelihood of microcracks and improve plating quality.
The controlled hardness ratio significantly reduces the occurrence of liquid metal embrittlement and surface oxides, enhancing the spot weldability and surface quality of high-strength galvanized steel sheets.
Smart Images

Figure 0007571140000005 
Figure 0007571140000001 
Figure 0007571140000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a high-strength hot-dip galvanized steel sheet having excellent surface quality and electric resistance spot weldability, and a method for producing the same. [Background technology]
[0002] Due to issues such as environmental pollution, regulations on automobile exhaust gas and fuel efficiency are becoming stricter day by day. Therefore, there is a strong demand for reducing fuel consumption by reducing the weight of automobile steel sheets, and various types of high-strength steel sheets with high strength per unit thickness have been developed and are commercially available.
[0003] High-strength steel usually means steel having a strength of 490 MPa or more, but is not necessarily limited to this, and examples of this include transformation induced plasticity (TRIP) steel, twin induced plasticity (TWIP) steel, dual phase (DP) steel, and complex phase (CP) steel.
[0004] Meanwhile, automotive steel is supplied in the form of plated steel sheets, the surface of which is plated to ensure corrosion resistance. Among these, zinc-plated steel sheets (GI steel sheets) or galvannealed steel sheets (GA) are widely used as materials for automobiles, as they have high corrosion resistance due to the sacrificial corrosion protection properties of zinc.
[0005] However, when the surface of a high-strength steel sheet is plated with zinc, there is a problem that the spot weldability is weakened. That is, since high-strength steel has high tensile strength and high yield strength, it is difficult to eliminate the tensile stress generated during welding through baking deformation, and there is a high possibility of microcracks occurring on the surface. When welding is performed on a high-strength galvanized steel sheet, zinc, which has a low melting point, penetrates into the microcracks of the steel sheet, resulting in a phenomenon called liquid metal embrittlement (LME), which can cause the steel sheet to break in a fatigue environment, and this acts as a major obstacle to increasing the strength of the steel sheet.
[0006] In addition, alloying elements such as Si, Al, and Mn, which are contained in large quantities in high-strength steel sheets, diffuse to the steel sheet surface during the manufacturing process and form surface oxides. This can result in a significant decrease in the wettability of zinc, leading to unplated areas and other deterioration in surface quality. Summary of the Invention [Problem to be solved by the invention]
[0007] According to one aspect of the present invention, there is provided a hot-dip galvanized steel sheet having excellent surface quality and spot weldability, and a manufacturing method thereof.
[0008] The object of the present invention is not limited to the above-mentioned contents. A person having ordinary skill in the art to which the present invention pertains will have no difficulty in understanding further object of the present invention from the entire contents of the specification of the present invention. [Means for solving the problem]
[0009] A galvanized steel sheet according to one aspect of the present invention includes a base steel sheet and a zinc-based plating layer formed on a surface of the base steel sheet, and the ratio (a / b) of hardness (a) of a surface layer of the base steel sheet to hardness (b) of an internal portion of the base steel sheet may be less than 0.95.
[0010] A method for producing a galvanized steel sheet according to another aspect of the present invention includes the steps of heating a steel slab to a temperature of 950 to 1350°C; hot rolling the steel slab under conditions of a finish rolling start temperature of 900 to 1150°C and a finish rolling end temperature of 850 to 1050°C to obtain a hot rolled steel sheet; coiling the hot rolled steel sheet at a temperature of 590 to 750°C; pickling the hot rolled steel sheet at a sheet passing speed of 180 to 250 mpm; cold rolling the hot rolled steel sheet at a rolling reduction of 35 to 60% to obtain a cold rolled steel sheet; recrystallization annealing the cold rolled steel sheet at 650 to 900°C in an atmosphere with a dew point of -10 to 30°C; and hot-dip galvanizing the annealed cold rolled steel sheet. Effect of the Invention
[0011] As described above, in one embodiment of the present invention, by controlling the hardness of the surface layer of the steel sheet to a lower value than the hardness of the interior, it is possible to reduce the possibility of cracks occurring even if tensile stress is applied during spot welding, and therefore it is possible to significantly reduce the liquid metal embrittlement (LME) phenomenon that occurs when the hot-dip galvanized layer penetrates along the cracks. In addition, one embodiment of the present invention can reduce the formation of oxides on the steel sheet surface, which has the effect of suppressing deterioration of plating quality. [Brief description of the drawings]
[0012] [Figure 1] 1 is a cross-sectional photograph of a steel plate test piece for measuring the hardness of a surface layer portion and an internal region. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below with reference to several embodiments.
[0014] It should be noted that the concept of galvanized steel sheet in the present invention includes not only galvanized steel sheet (GI steel sheet) but also galvannealed steel sheet (GA) and all plated steel sheets in which a zinc-based plating layer containing mainly zinc is formed. "Mainly containing zinc" means that zinc has the highest ratio among the elements contained in the plating layer. However, in galvannealed steel sheet, the ratio of iron may be higher than that of zinc, and the present invention can include steel sheets in which the ratio of zinc is the highest among the remaining components excluding iron.
[0015] The inventors of the present invention focused on the fact that liquid metal embrittlement (LME) that occurs during welding is caused by microcracks that develop on the surface of the steel sheet, and conducted research into means for suppressing surface microcracks. They discovered that to achieve this, it is necessary to soften the steel sheet surface, and thus arrived at the present invention.
[0016] Normally, high-strength steels can contain large amounts of elements such as carbon (C), manganese (Mn), and silicon (Si) to ensure the hardening ability and austenite stability of the steel, but these elements play a role in increasing the sensitivity of the steel to cracks. Therefore, steels containing large amounts of these elements easily develop microcracks, which ultimately cause liquid metal embrittlement during welding.
[0017] According to the research results of the present inventors, the reason why microcracks easily occur is that the hardness of a steel sheet is roughly proportional to its strength, and a steel sheet with high hardness has a high susceptibility to cracks. Therefore, the present inventors have found that the overall hardness can be maintained at a high level to ensure the strength of the steel sheet, while the hardness of only the surface layer, where cracks are generated and start to propagate, can be reduced to reduce the susceptibility to cracks, and have arrived at the present invention.
[0018] Therefore, according to one embodiment of the present invention, there can be provided a hot-dip galvanized steel sheet including a base steel sheet and a zinc-based coating layer formed on the surface of the base steel sheet, in which a ratio (a / b) of the hardness (a) of the surface layer to the hardness (b) of the inner part is controlled to be less than 0.95. Here, the surface layer means a region from the surface of the steel sheet to a depth of 20 μm, and the inner part means a region with a depth of 30 to 100 μm. The hardness of each region can be an average value of values measured at the same interval in the depth direction. In one embodiment of the present invention, the ratio (a / b) of the hardness (a) of the surface layer to the hardness (b) of the inner part can be determined by measuring the hardness at 5 μm intervals from the surface to a depth of 5 to 100 μm by applying a nanoindentation Vickers hardness tester with a load of 5 g at 5 μm intervals, and the average value of the hardness measurements at points corresponding to the depth of the surface layer and the inner part can be determined as the hardness value of the corresponding region.
[0019] In this case, even if the steel material has high strength, the possibility of cracks occurring due to stress acting on the surface can be significantly reduced. According to one embodiment of the present invention, the ratio (a / b) may be less than 0.90, in another embodiment, the ratio (a / b) may be less than 0.85, and in another embodiment, the ratio (a / b) may be less than 0.80.
[0020] Since the lower the hardness of the surface layer, the more advantageous it is, the lower limit of the ratio (a / b) of the hardness (a) of the surface layer to the hardness (b) of the interior is not particularly limited. However, when considering a common method for efficiently reducing the hardness of the surface layer without significantly affecting the strength of the steel sheet, the ratio (a / b) may be set to 0.2 or more.
[0021] The ratio (a / b) of the hardness of the surface layer to the hardness of the inside may be a value measured at any position in the width direction of the steel plate, for example, a value measured at the center in the width direction may be used as a reference. However, according to one embodiment of the present invention, the hardness of the surface layer may have a higher value at the edge portion in the width direction, and the ratio (a / b) may have a higher value, so the ratio (a / b) may be a value measured at the edge portion in the width direction. In this case, the edge portion means both ends of the steel plate, but if there is a problem with the soundness of the test piece, such as contamination occurring at the above-mentioned points, it may mean a point 1 mm inward in the width direction from the end portion.
[0022] The steel sheet targeted by the present invention is not limited to any particular type, so long as it is a high-strength steel sheet having a strength of 490 MPa or more. However, although not necessarily limited thereto, the steel sheet targeted by the present invention may have a composition including, by weight percentage, C: 0.05-1.5%, Si: 2.0% or less, Mn: 1.0-30%, S-Al (acid-soluble aluminum): 3% or less, Cr: 2.5% or less, Mo: 1% or less, B: 0.005% or less, Nb: 0.2% or less, Ti: 0.2% or less, V: 0.2% or less, Sb+Sn+Bi: 0.1% or less, and N: 0.01% or less. The remaining components are iron and other impurities, and further elements that may be contained in steel but are not listed above may be included in the steel in a total amount of 1.0% or less. In the present invention, the content of each component element is expressed by weight unless otherwise specified. The above-mentioned composition means the bulk composition of the steel plate, that is, the composition at a 1 / 4 point in the steel plate thickness (the same applies hereinafter).
[0023] In some embodiments of the present invention, the high-strength steel plate may be a TRIP steel, etc. These steels may have the following compositions when classified in detail.
[0024] Steel composition 1: C: 0.05-0.30% (preferably 0.10-0.25%), Si: 0.5-2.5% (preferably 1.0-1.8%), Mn: 1.5-4.0% (preferably 2.0-3.0%), S-Al: 1.0% or less (preferably 0.05% or less), Cr: 2.0% or less (preferably 1.0% or less), Mo: 0.2% or less (preferably 0.1% or less), B: 0.005% or less (preferably 0.004% or less), Nb: 0.1% or less (preferably 0.05% or less), Ti: 0.1% or less (preferably 0.001-0.05%), Sb+Sn+Bi: 0.05% or less, N: 0.01% or less, balance Fe and unavoidable impurities. In some cases, elements not listed above but that may be contained in the steel may be further included up to a total of 1.0% or less.
[0025] Steel composition 2: C: 0.05 to 0.30% (preferably 0.10 to 0.2%), Si: 0.5% or less (preferably 0.3% or less), Mn: 4.0 to 10.0% (preferably 5.0 to 9.0%), S-Al: 0.05% or less (preferably 0.001 to 0.04%), Cr: 2.0% or less (preferably 1.0% or less), Mo: 0.5% or less (preferably 0.1 to 0.35%), B: 0.005% or less (preferably 0.004% or less), Nb: 0.1% or less (preferably 0.05% or less), Ti: 0.15% or less (preferably 0.001 to 0.1%), Sb+Sn+Bi: 0.05% or less, N: 0.01% or less, the balance being Fe and inevitable impurities. In some cases, elements not listed above but which may be contained in the steel may further be contained up to a total content of 1.0% or less.
[0026] Furthermore, when the lower limit of the content of each of the above-mentioned component elements is not specified, this means that the element may be regarded as an optional element, and the content may be 0%.
[0027] Although not necessarily limited thereto, the thickness of the base steel sheet according to one embodiment of the present invention may be 1.0 to 2.0 mm.
[0028] Furthermore, the plated steel sheet according to one embodiment of the present invention can have improved surface quality by containing, in the surface layer portion of the base steel sheet, internal oxides containing at least one of Si, Mn, Al, and Fe. That is, the presence of the above oxides in the surface layer portion can suppress the formation of oxides on the steel sheet surface, and as a result, wettability between the base steel sheet and the plating solution during plating can be ensured, and good plating performance can be obtained.
[0029] According to one embodiment of the present invention, the surface of the steel sheet may include one or more plating layers, and the plating layer may be a zinc-based plating layer including GI (Galvanized) or GA (Galva-annealed), etc. As described above, in the present invention, the ratio of the hardness of the surface layer to the hardness of the interior is controlled within an appropriate range, so that even if a zinc-based plating layer is formed on the surface of the steel sheet, the problem of liquid phase metal embrittlement occurring during spot welding can be suppressed.
[0030] According to one embodiment of the present invention, when the zinc-based plating layer is a GA layer, the degree of alloying (meaning the content of Fe in the plating layer) can be controlled to 8 to 13 wt%, preferably 10 to 12 wt%. If the degree of alloying is insufficient, the zinc in the zinc-based plating layer may penetrate into microcracks, causing liquid metal embrittlement, while if the degree of alloying is excessively high, problems such as powder ring may occur.
[0031] The coating weight of the zinc-based coating layer is 30 to 70 g / m 2 If the coating weight is too low, it is difficult to obtain sufficient corrosion resistance, whereas if the coating weight is too high, problems of increased production costs and liquid phase metal embrittlement may occur, so it is controlled within the above-mentioned range. A more preferable range of the coating weight is 40 to 60 g / m 2This plating weight means the amount of the plating layer attached to the final product, and in the case where the plating layer is a GA layer, the plating weight increases due to alloying, so that its weight may decrease slightly before alloying, and since it varies depending on the degree of alloying, it is not necessarily limited to this, but the plating weight before alloying (i.e., the amount of plating attached from the plating bath) may be a value that is about 10% less than that.
[0032] Hereinafter, one embodiment of the method for producing the steel sheet of the present invention will be described. However, it should be noted that the steel sheet of the present invention does not necessarily have to be produced according to the embodiment described below, and the embodiment described below is one preferred method for producing the steel sheet of the present invention.
[0033] First, a hot-rolled steel sheet can be manufactured by reheating a steel slab having the above-mentioned composition, hot-rolling it through rough rolling and finish rolling, and then ROT (Run Out Table) cooling and coiling. The manufactured steel sheet can then be pickled and cold-rolled, and the obtained cold-rolled steel sheet can be annealed and plated. There are no particular limitations on the hot-rolling conditions such as ROT cooling, but in one embodiment of the present invention, the slab heating temperature, finish rolling start and end temperatures, coiling temperature, heating conditions of the edge of the coiled coil, pickling conditions, cold rolling conditions, annealing conditions, plating conditions, etc. can be limited as follows.
[0034] Slab heating temperature: 950~1,300℃ Slab heating is performed to heat the material before hot rolling to ensure rollability. During slab reheating, the surface layer of the slab combines with oxygen in the furnace to form scale, which is an oxide. When the scale is formed, it also reacts with the carbon in the steel, causing a decarburization reaction that forms carbon monoxide gas, and the higher the slab reheating temperature, the greater the amount of decarburization. If the slab reheating temperature is too high, an excessive decarburization layer is formed, which causes the material of the final product to soften, while if it is too low, hot rollability cannot be ensured, edge cracks may occur, and the hardness of the surface layer cannot be sufficiently reduced, resulting in insufficient LME improvement.
[0035] Finish rolling start temperature: 900~1,150℃ If the finish rolling start temperature is too high, the surface hot rolling scale may develop excessively, increasing the occurrence of surface defects due to the scale in the final product, so the upper limit is limited to 1,150° C. Also, if the finish rolling start temperature is less than 900° C., the stiffness of the bar increases with the decrease in temperature, and there is a possibility that the hot rolling properties may be significantly reduced, so the finish rolling start temperature can be limited to the above range.
[0036] Finish rolling temperature: 850~1,050℃ If the finish rolling end temperature exceeds 1,050°C, the scale removed by descaling will be excessively formed again on the surface during finish rolling, increasing the number of surface defects. If the finish rolling end temperature is less than 850°C, the hot rolling properties will deteriorate, so the finish rolling end temperature can be limited to the above-mentioned range.
[0037] Winding temperature: 590~750℃ The hot-rolled steel sheet is then wound into a coil and stored, and the wound steel sheet undergoes a slow cooling process. Through this process, hardening elements contained in the surface layer of the steel sheet are removed, but if the coiling temperature of the hot-rolled steel sheet is too low, the coil is slowly cooled at a temperature lower than the temperature required for the oxidation and removal of these elements, making it difficult to obtain a sufficient effect.
[0038] Heating the edge of hot rolled coil: 600-800℃ for 5-24 hours In one embodiment of the present invention, the edge of the hot rolled coil may be heated to adjust the ratio (a / b) of the hardness (a) of the surface layer of the edge to the hardness (b) of the inside. Heating the edge of the hot rolled coil means heating both ends in the width direction of the coiled coil, i.e., the edge, and the edge is heated first to a temperature suitable for oxidation. That is, in one embodiment of the present invention, the hardness of the surface layer can be reduced by removing carbon and other dissolved hardening elements (Si, Mn, Al) from the surface of the steel sheet, and this process can be performed by internally oxidizing the surface of the steel sheet. However, while the inside of the coiled coil is maintained at a high temperature, the edge is cooled relatively quickly, and therefore the time that the edge is maintained at a temperature suitable for internal oxidation is shorter than that of the edge. Therefore, decarburization or removal of hardening elements is not actively performed in the edge compared to the center in the width direction. Heating the edge can be used as one method for removing hardening elements in the edge.
[0039] That is, when the edge portion is heated, the edge portion is heated first, in contrast to the case of cooling after coiling, and therefore the temperature of the edge portion in the width direction is maintained to be suitable for internal oxidation, but as a result, the thickness of the internal oxidation layer of the edge portion increases. For this purpose, the heating temperature of the edge portion needs to be 600°C or more (based on the temperature of the edge portion of the steel sheet). However, if the temperature is too high, excessive scale is formed on the edge portion during heating or porous highly oxidized scale (hematite) is formed, which may deteriorate the surface condition after pickling, so the temperature of the edge portion is preferably 800°C or less. A more preferable heating temperature of the edge portion is 600 to 750°C.
[0040] In addition, in order to eliminate the non-uniformity of the ferrite fraction in the region within 20 μm of the steel sheet surface between the edge and center in the width direction that occurs during coiling, the heating time of the edge must be 5 hours or more. However, if the heating time of the edge is too long, there is a possibility that excessive scale will be formed or even the hardness of the inside will decrease. Therefore, it is preferable that the heating time of the edge is 24 hours or less.
[0041] According to one embodiment of the present invention, the edge portion can be heated by a combustion heating method using air-fuel ratio adjustment. That is, the oxygen fraction in the atmosphere changes due to air-fuel ratio adjustment, and the higher the oxygen partial pressure, the higher the oxygen concentration in contact with the surface layer of the steel sheet, which may increase decarburization and internal oxidation. Although not necessarily limited thereto, in one embodiment of the present invention, the atmosphere can be controlled to a nitrogen atmosphere containing 1 to 2% oxygen by air-fuel ratio adjustment. Since a person having ordinary knowledge in the technical field to which the present invention pertains can control the oxygen fraction by air-fuel ratio adjustment without any special difficulty, a separate description will not be given here.
[0042] Pickling treatment: Carried out at a strip speed of 180 to 250 mpm The hot-rolled steel sheet that has undergone the above-mentioned process is subjected to pickling treatment in a hydrochloric acid bath in order to remove hot-rolled scale. During pickling, the hydrochloric acid concentration of the hydrochloric acid bath is in the range of 10-30%, and the pickling speed is 180-250 mpm. If the pickling speed exceeds 250 mpm, the scale on the surface of the hot-rolled steel sheet may not be completely removed, and if the pickling speed is lower than 180 mpm, the surface layer of the base steel may be corroded by hydrochloric acid, so the pickling speed is 180 mpm or higher.
[0043] Cold rolling: reduction rate 35-60% After pickling, cold rolling is performed. The cold rolling reduction is in the range of 35 to 60%. If the cold rolling reduction is less than 35%, there is no particular problem, but the driving force for recrystallization during annealing is insufficient, which may make it difficult to sufficiently control the microstructure. If the cold rolling reduction exceeds 60%, the thickness of the soft layer secured during hot rolling becomes thin, making it difficult to sufficiently reduce the hardness within a region within 20 μm of the steel sheet surface after annealing.
[0044] The above-mentioned cold rolling process may be followed by a process of annealing the steel sheet. During the annealing process of the steel sheet, the hardness in a region within 20 μm of the steel sheet surface (surface layer) may change significantly. Therefore, in one embodiment of the present invention, the annealing process may be controlled under conditions that appropriately control the hardness in a region within 20 μm of the steel sheet surface. Among these, the sheet threading speed and the dew point in the annealing furnace may be controlled under the following conditions.
[0045] Threading speed: 40~130mpm In order to ensure sufficient productivity, the threading speed of the cold rolled steel sheet needs to be 40 mpm or more. However, if the threading speed is too fast, it may be disadvantageous in terms of ensuring the quality of the material. Therefore, in one embodiment of the present invention, the upper limit of the threading speed can be set to 130 mpm.
[0046] Dew point control in annealing furnace: Controlled within the range of -10 to 30°C at 650 to 900°C In order to obtain a hardness value of the surface layer in an appropriate range, it is advantageous to control the dew point in the annealing furnace. If the dew point is too low, surface oxidation may occur instead of internal oxidation, and oxides such as Si and Mn may be formed on the surface. These oxides have a negative effect on plating. Therefore, the dew point needs to be controlled to -10°C or higher. Conversely, if the dew point is too high, oxidation of Fe may occur, so the dew point needs to be controlled to 30°C or lower. In this way, the temperature for controlling the dew point may be 650°C or higher, which is a temperature at which sufficient internal oxidation effects are observed. However, if the temperature is too high, not only will surface oxides such as Si be formed to hinder oxygen from diffusing inward, but excessive austenite may be generated during heating of the crack zone, reducing the diffusion rate of carbon, thereby reducing the level of internal oxidation, and the size of the austenite in the crack zone may grow excessively, causing material softening. In addition, since there is a possibility of causing problems such as generating a load on the annealing furnace, shortening the life of the equipment, and increasing the process cost, the temperature for controlling the dew point may be 900°C or lower.
[0047] At this time, the dew point is the amount of humid nitrogen (N 2 +H 2 O) can be added to the annealing furnace.
[0048] Hydrogen concentration in the annealing furnace: 5 to 10 Vol% The atmosphere inside the annealing furnace is maintained as a reducing atmosphere by adding 5-10 vol% hydrogen to nitrogen gas. If the hydrogen concentration inside the annealing furnace is less than 5 vol%, the reducing ability decreases, causing excessive formation of surface oxides, which leads to inferior surface quality and plating adhesion, and the surface oxides inhibit the reaction between oxygen and carbon in the steel, resulting in a decrease in the amount of decarburization and a low level of LME improvement. Although no particular problems arise when the hydrogen concentration is high, the hydrogen concentration is limited due to the increase in costs caused by the increase in the amount of hydrogen gas used and the risk of explosion inside the furnace caused by the increase in hydrogen concentration.
[0049] The steel sheet annealed according to the above-mentioned process may be cooled through a slow cooling and a rapid cooling step.
[0050] Temperature of the annealing zone: 550-750℃ The slow cooling zone is a zone where the cooling rate is 3 to 5°C / s, and if the temperature of the slow cooling zone exceeds 750°C, soft ferrite is excessively formed during slow cooling, resulting in a decrease in tensile strength, and conversely, if the temperature of the slow cooling zone is less than 550°C, bainite is excessively formed or martensite is formed, resulting in an excessive increase in tensile strength and a decrease in elongation. Therefore, the temperature of the slow cooling zone can be limited to the above-mentioned range.
[0051] Quenching zone temperature: 270~550℃ The quenching zone is a section where the cooling rate is 12 to 20°C / s. If the temperature of the quenching zone exceeds 550°C, an appropriate level of martensite is formed during quenching, resulting in insufficient tensile strength. If the temperature of the quenching zone is less than 270°C, too much martensite is formed, which may result in insufficient elongation.
[0052] The steel sheet annealed by the above process is immediately immersed in a galvanizing bath to perform hot-dip galvanizing. If the steel sheet is cooled, the process may further include a step of heating the steel sheet. The heating temperature must be higher than the drawing temperature of the steel sheet described below, and may be higher than the temperature of the galvanizing bath in some cases.
[0053] Temperature of steel plate in galvanizing bath: 420~500℃ If the drawing temperature of the steel sheet in the coating bath is low, the wettability at the contact interface between the steel sheet and the liquid zinc is not sufficiently ensured, so it must be maintained at 420°C or higher. If the temperature is too high, the reaction between the steel sheet and the liquid zinc is excessive, resulting in the formation of a Zetta phase, which is an Fe-Zn alloy phase, at the interface, reducing the adhesion of the coating layer, and causing excessive dissolution of Fe elements from the steel sheet in the coating bath, resulting in the formation of dross in the coating bath. Therefore, the drawing temperature of the steel sheet can be limited to 500°C or lower.
[0054] Al concentration in plating bath: 0.10-0.25% The Al concentration in the plating bath must be maintained at an appropriate level to ensure the wettability of the plating layer and the fluidity of the plating bath. By controlling the Al concentration to 0.10-0.15% for GA and 0.2-0.25% for GI, the formation of dross in the plating bath can be maintained at an appropriate level, ensuring the quality and performance of the plating surface.
[0055] The hot-dip galvanized steel sheet plated by the above-mentioned process may then be subjected to an alloying heat treatment process, if necessary. The preferred conditions for the alloying heat treatment are as follows.
[0056] Alloying (GA) temperature: 480~560℃ If the temperature is less than 480°C, the amount of Fe diffusion is small and the degree of alloying is insufficient, which may result in poor plating properties. If the temperature is more than 560°C, problems with powdering may occur due to excessive alloying, and the material may deteriorate due to the ferrite transformation of retained austenite. Therefore, the alloying temperature is set within the above-mentioned range. EXAMPLES
[0057] The present invention will be described in more detail with reference to the following examples. However, it should be noted that the following examples are merely for illustrating and embodying the present invention, and are not intended to limit the scope of the present invention, since the scope of the present invention is determined by the matters described in the claims and matters reasonably inferred therefrom.
[0058] (Example) A steel slab having the composition shown in Table 1 below (the remaining components not shown in the table are Fe and inevitable impurities. In the table, B and N are shown in ppm units, and the remaining components are shown in weight percent units) was heated to 1230°C, and hot-rolled with finish rolling start and end temperatures of 980°C and 895°C, respectively, and then the hot-rolled coil was heated at the edge, cold-rolled, pickled with a 19.2% by volume hydrochloric acid solution, and cold-rolled. The obtained cold-rolled steel sheet was annealed in an annealing furnace, slowly cooled at 4.2°C / s in a 620°C slow cooling zone, and quenched at 17°C / s in a 315°C rapid cooling zone to obtain an annealed steel sheet. Thereafter, the obtained steel sheet was heated to 470°C, and GA was immersed in a 0.13% Al plating bath, and GI was immersed in a 456°C zinc-based plating bath containing 0.24% by weight Al, to perform hot-dip galvanization. The obtained hot-dip galvanized steel sheet was subjected to an alloying (GA) heat treatment at 520°C as required to finally obtain an alloyed hot-dip galvanized steel sheet.
[0059] In all the examples, the temperature of the steel sheet drawn into the hot dip galvanizing bath was 475° C. Other conditions for each example are as shown in Table 2.
[0060] [Table 1]
[0061] [Table 2]
[0062] The properties of the hot-dip galvanized steel sheets manufactured by the above-mentioned process were measured, and the occurrence of liquid metal embrittlement (LME) during spot welding was observed, and the results are shown in Table 3. The steel sheets were cut in the width direction, and spot welding was performed along each cut edge. The spot welding current was applied twice, and a hold time of one cycle was maintained after energization. Spot welding was performed in two-type triple layer. The following materials were stacked in the order of evaluation material--evaluation material--GA 980DP 1.4t material (having a composition of 0.12 wt% C, 0.1 wt% Si, and 2.2 wt% Mn) and spot welding was performed. During spot welding, a new electrode was welded to the soft material 15 times, and the electrode was worn down, and the upper limit current at which expulsion occurs in the material to be spot welded was measured. After measuring the upper limit current, spot welding was performed 8 times for each welding current at currents 0.5 and 1.0kA lower than the upper limit current, and the cross section of the spot weld was precisely machined by electric discharge machining, epoxy mounted and polished, and the crack length was measured using an optical microscope. The magnification for optical microscope observation was set to 100x, and if no cracks were found at that magnification, it was determined that liquid metal embrittlement had not occurred, and if cracks were found, their length was measured using image analysis software. B-type cracks occurring at the shoulder of the spot weld were 100μm or less, and if no C-type cracks were found, it was determined to be good.
[0063] The ratio (a / b) of the hardness (a) of the surface layer of the steel plate to the hardness (b) of the internal portion can be the average value of the values measured at the same interval in the depth direction, as shown in Fig. 1. In one embodiment of the present invention, the hardness is measured by applying a load of 5 g to a nanoindentation Vickers hardness tester at 5 µm intervals from the surface of a portion 1 mm away from the edge of the steel plate to a depth of 5 to 100 µm, and the average values of the hardness measurements at the points corresponding to the depths of the surface layer and the internal portion are taken as the hardness (a) of the surface layer and the hardness (b) of the internal portion, respectively, and the ratio (a / b) between them is taken as the hardness (a) of the surface layer and the hardness (b) of the internal portion.
[0064] Tensile strength was measured by preparing C-direction samples according to JIS-5 standard and conducting tensile tests. The degree of alloying and the amount of plating attached were measured using a wet dissolution method using a hydrochloric acid solution. For sealer adhesion, automotive structural adhesive D-type was applied to the plating surface, and the steel sheet was bent 90 degrees to check whether the plating fell off. For powdering, the plating material was bent 90 degrees, tape was applied to the bent area, and then peeled off to check how many mm of the plating layer fell off onto the tape. If the length of the plating layer peeled off from the tape exceeded 10 mm, it was deemed defective. For flaking, the sample was processed into an inverted U-shape, and it was checked whether the plating layer fell off at the processed area. For GI steel sheets, a sealer bending test (SBT) was conducted to check whether the plating layer peeled off and adhered to the surface where the sealer fell off when the steel sheet was bent 90 degrees with automotive structural adhesive applied to the surface. The surface quality was checked by visually checking for defects such as unplated steel sheets, and if defects such as unplated steel sheets were visible during visual inspection, the sheets were judged to be defective.
[0065] [Table 3] JPEG0007571140000004.jpg195169
[0066] Inventive Examples 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10, the steel composition and manufacturing conditions satisfied the conditions of the present invention, and the tensile strength, coating quality, coating weight, and length of spot weld LME cracks were also good.
[0067] In Comparative Examples 2 and 7, the coiling temperature during the hot rolling process does not meet the range proposed by the present invention. In Comparative Example 2, the hot rolling coiling temperature is lower than the range proposed by the present invention, and the amount of decarburization occurring during hot rolling is insufficient, so the ratio (a / b) of the hardness (a) of the surface layer of the steel sheet to the hardness (b) of the inside is 95% (0.95) or more, and the LME cracks do not meet the standard. Comparative Example 7 was produced at a hot rolling coiling temperature higher than the hot rolling coiling temperature proposed by the present invention, and the amount of decarburization occurring during the hot rolling process was sufficient, and the LME characteristics were good, but the hot rolling scale was excessively generated, and the scale was not completely removed during pickling, resulting in non-plating and poor surface quality, so that plating peeling occurred during flaking evaluation, and the powder ring properties were poor due to uneven alloying. The hot rolling coiling temperature was excessively high, and the hot rolling material softened and did not recover even after annealing, so the tensile strength was inferior.
[0068] In Comparative Example 15, the heating temperature of the edge portion exceeded the range proposed in the present invention, and overoxidation occurred at the edge portion during the heat treatment process, resulting in the formation of red hematite on the surface scale and an excessively deep thickness. During the pickling process after hot rolling, the edge portion was excessively pickled, resulting in an increase in surface roughness, and the surface shape after plating was non-uniform, resulting in defects such as the surface color being different from that of the center, and the powder ring property was poor due to non-uniform alloying. Excessive decarburization occurred during the heat treatment process, and although the hardness reduction rate met the standard and LME met the standard, the material quality was inferior.
[0069] In Comparative Example 8, the heating temperature of the edge portion was controlled to be lower than the range of the present invention. As a result, the hardness ratio (a / b) during hot rolling could not be sufficiently reduced, and the evaluation criteria for LME cracks during spot welding were not met.
[0070] In Comparative Example 13, the heating temperature of the edge part was within the range of the present invention, but the heating time exceeded the time, and overoxidation occurred at the edge part during the heat treatment process, the surface scale formed red hematite, and the penetration thickness of the scale was also excessive. As the edge part was excessively pickled in the pickling process after hot rolling, the surface roughness increased, the surface shape after plating was non-uniform, and the surface color was different from the center, resulting in defects in non-uniform color, and the powder ring property was poor due to non-uniform alloying.
[0071] In Comparative Example 5, the heating temperature of the edge portion was within the range of the present invention, but the heating time of the edge portion was lower than the range of the present invention. As a result, a sufficient hot-rolled decarburized layer was not formed, and the standard for the LME crack evaluation of spot welding was not met, resulting in a poor result.
[0072] In Comparative Examples 1 and 14, the pickling speed does not satisfy the range proposed by the present invention. In Comparative Example 1, the pickling speed was lower than the standard, and as the pickling speed became excessively long, the decarburized layer formed during hot rolling was dissolved and removed in the acid solution, and the ratio (a / b) of the hardness (a) of the surface layer of the steel sheet to the hardness (b) of the interior was higher than the standard, so LME cracks occurred. As the oxide grain boundaries inside the hot rolling were corroded by the acid solution, the grain boundary integrity was reduced, and peeling occurred during the flaking test. In Comparative Example 14, the pickling speed was higher than the standard, so the hot rolling scale was not completely removed and remained on the steel sheet surface, resulting in poor surface quality, and the powder ring property was poor due to the non-uniformity of the GA alloying degree.
[0073] In Comparative Example 10, the temperature of the crack zone in the annealing furnace exceeded the range proposed by the present invention. As the annealing temperature became excessive, the amount of external oxidation increased, and sufficient internal oxidation was not formed, so the ratio (a / b) of the hardness (a) of the surface layer of the steel sheet to the hardness (b) of the internal layer was 95% or more, and the LME crack did not meet the standard, resulting in poor spot weldability. In addition, austenite was excessively formed and grew in the crack zone, and the material did not meet the standard, resulting in poor quality.
[0074] In Comparative Example 12, the temperature of the crack zone in the annealing furnace was lower than the range proposed by the present invention. Since the annealing temperature was low and the oxidation reaction between the steam and the steel sheet was insufficient, the internal oxidation was not sufficiently formed, the ratio (a / b) of the hardness (a) of the surface layer of the steel sheet to the hardness (b) of the interior was high, and the LME crack did not meet the standard, so the spot weldability was poor. In addition, recrystallization was not sufficiently performed during annealing, and the target fine structure was not formed, so the material did not meet the standard, so it was poor.
[0075] In Comparative Example 6, the dew point in the furnace during annealing was lower than the range presented in the present invention. Even if a sufficient internal oxidation layer was generated over the entire width during the hot rolling heating process, the dew point was not high enough during the annealing process after cold rolling, so the decarburized layer was not sufficiently formed, and the ratio (a / b) of the hardness (a) of the surface layer of the steel sheet to the hardness (b) of the inside was 95% or more, and as a result, the length of the LME crack in the spot weld did not meet the standard. In the case of GI material, the dew point was low, so sufficient internal oxidation could not be generated, and excessive surface oxide was generated, resulting in poor surface quality and SBT peeling.
[0076] In Comparative Example 18, the range of the dew point in the annealing furnace exceeded the range proposed by the present invention. As the dew point became excessively high, the decarburization reaction occurred sufficiently, and although the LME was satisfied, the material deteriorated due to excessive internal oxidation, and the standard was not met. The excessive dew point also increased the amount of surface oxide generated, and as a result of SBT, plating peeling occurred.
[0077] In Comparative Example 3, the hydrogen concentration in the annealing furnace was less than 5 Vol%, and the composition of the reducing atmosphere in the annealing furnace was insufficient. Excessive surface oxide formation caused non-plating, resulting in poor surface quality and SBT plating peeling. In addition, the excessive oxides made it difficult for carbon and oxygen in the steel to come into physical contact, and the reduction in hardness of the surface layer was insufficient, so the LME cracks did not meet the standard.
[0078] In Comparative Examples 4 and 11, the sheet passing speed in the annealing furnace is outside the range proposed by the present invention. In Comparative Example 4, the sheet passing speed was higher than the range proposed by the present invention. Since the time required for reaction with the humid nitrogen in the annealing furnace was not secured and the decarburization level was insufficient, the ratio (a / b) of the hardness (a) of the surface layer to the hardness (b) of the inner layer was 95% or more, the LME crack did not meet the standard, and sufficient recrystallization time could not be secured in the annealing furnace, resulting in inferior material properties (tensile strength). In Comparative Example 11, the sheet passing speed was lower than the range proposed by the present invention, and although a sufficient decarburized layer was secured in the annealing furnace and LME was satisfied, the material properties (tensile strength) were inferior due to the formation of an excessive decarburized layer.
[0079] Through the results of these examples, the advantageous effects of various embodiments of the present invention can be confirmed.
Claims
1. Base steel sheet and A zinc-plated steel sheet including a zinc-based plating layer formed on a surface of the base steel sheet, the ratio (a / b) of the Vickers hardness (a) of the surface layer portion of the base steel sheet to the Vickers hardness (b) of the interior portion is less than 0.95; The ratio (a / b) is based on the value measured at the edge portion in the width direction, The tensile strength is 978 MPa or more, A zinc-plated steel sheet in which, when the plated product is bent 90 degrees, a tape is adhered to the bent portion and then peeled off, the length of the plated layer peeled off from the tape is 10 mm or less.
2. The coating weight of the zinc-based plating layer is 30 to 70 g / m 2 The galvanized steel sheet according to claim 1 ,
3. 3. The galvanized steel sheet according to claim 1, wherein the base steel sheet contains, in mass%, C: 0.05 to 1.5%, Si: 2.0% or less, Mn: 1.0 to 30%, S-Al (acid-soluble aluminum): 3% or less, Cr: 2.5% or less, Mo: 1% or less, B: 0.005% or less, Nb: 0.2% or less, Ti: 0.2% or less, V: 0.2% or less, Sb+Sn+Bi: 0.1% or less, and N: 0.01% or less, with the remaining components being iron and other unavoidable impurities.
4. The galvanized steel sheet according to claim 3, wherein the base steel sheet has a thickness of 1.0 to 2.0 mm.
5. The galvanized steel sheet according to claim 1 or 2, wherein the surface layer portion contains an inner oxide containing at least one of Si, Mn, Al, and Fe.
6. heating the steel slab to a temperature of 950-1350°C; A step of hot rolling the steel slab under the conditions of a finish rolling start temperature of 900 to 1,150°C and a finish rolling end temperature of 850 to 1,050°C to obtain a hot rolled steel sheet; coiling the hot-rolled steel sheet at a temperature of 590 to 750°C; heating the edge portion of the hot-rolled steel sheet at 600 to 800° C. for 5 to 24 hours; pickling the hot-rolled steel sheet at a threading speed of 180 to 250 mpm; cold rolling the hot-rolled steel sheet at a rolling reduction of 35 to 60% to obtain a cold-rolled steel sheet; recrystallization annealing the cold-rolled steel sheet in an atmosphere at 650 to 900° C. and a dew point of −10 to 30° C.; Slowly cooling the annealed steel sheet to a temperature of 550 to 750° C. at a cooling rate of 3 to 5° C. / s; quenching the slowly cooled steel sheet to 270 to 550° C. at a cooling rate of 12 to 20° C. / s; and hot-dip galvanizing the quenched cold-rolled steel sheet; The ratio (a / b) of the Vickers hardness (a) of the surface layer of the produced zinc-plated steel sheet to the Vickers hardness (b) of the interior layer is less than 0.95; A method for producing a galvanized steel sheet, wherein the tensile strength is 978 MPa or more.
7. The recrystallization annealing step is performed using hydrogen (H 2 The method for producing a galvanized steel sheet according to claim 6, wherein the heating is performed in a wet nitrogen gas atmosphere containing 5 to 10 volume % of
8. The method for producing a galvanized steel sheet according to claim 6, wherein a sheet passing speed during the recrystallization annealing is 40 to 130 mpm.
9. The method for producing a galvanized steel sheet according to any one of claims 6 to 8, further comprising a step of alloying the plated steel sheet at a temperature of 480 to 560°C.
Citation Information
Patent Citations
Pickling method for hot rolled steel sheet
JP1986279311A
Method for pickling hot rolled steel sheet
JP1987063687A
High strength galvanized steel sheet and method for manufacturing the same
JP2014009399A
High strength steel sheet excellent in acid resistance and manufacturing method therefor