ORTHOPEDIC IMPLANTS HAVING GALLIUM-CONTAINING HYDROXYAPATITE COATINGS - Patent application
A gallium-substituted hydroxyapatite coating addresses the issues of non-uniform degradation and adhesion in orthopedic implants by providing a crystalline, uniformly degrading, and biocompatible solution that enhances osteoinductivity and reduces inflammation.
Patent Information
- Application Number
- JP2023031717
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-03-28
- Filing Date
- 2023-03-02
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2038-03-27
AI Technical Summary
Existing methods for coating orthopedic implants with hydroxyapatite result in non-uniform degradation, particle formation, and poor adhesion, leading to inflammation and wear issues, particularly in porous structures.
A gallium-substituted hydroxyapatite coating is applied using a solution deposition process that incorporates gallium ions into the hydroxyapatite lattice, resulting in a crystalline coating with controlled degradation and uniform dissolution over several weeks, enhancing biocompatibility and adhesion.
The gallium-substituted hydroxyapatite coating provides uniform degradation without particle formation, improves osteoinductivity, and enhances adhesion to orthopedic implants, reducing inflammation and wear, while being rapidly formed with controlled microstructure and composition.
Smart Images

Figure 0007571177000010 
Figure 0007571177000011 
Figure 0007571177000012
Abstract
Description
[Technical field]
[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) Cross-reference is made to co-pending U.S. patent application Ser. No. 15 / 472,189, entitled "ORTHOPEDIC IMPLANT HAVING A CRYSTALLINE CALCIUM PHOSPHATE COATING AND METHODS FOR MAKING THE SAME" (Attorney Docket No. 265280-259106, DSP5297USNP), which is incorporated herein by reference.
[0002] FIELD OF THEINVENTION The present invention relates generally to gallium-containing hydroxyapatite coatings, and more specifically to orthopedic implants having solution-deposited gallium-substituted hydroxyapatite coatings and methods of making same. [Background technology]
[0003] Bone repair often involves the use of orthopedic implants to replace missing bone or to support the bone during the healing process. Typically, it is desirable to coat such orthopedic implants with osteoinductive materials to promote bone growth or biological fixation.
[0004] Hydroxyapatite (HA) is a naturally occurring mineral found in bones and teeth. Studies have shown that HA is osteoinductive, and for this reason orthopedic implants are coated with HA. Various processes are known for coating implants with HA. One process used to coat implants is plasma spraying. In this process, HA powder is delivered to a hot torch using a carrier gas. The HA powder is partially melted and impacts the substrate at high velocity where it is rapidly cooled to room temperature. This process results in a mixture of HA, other calcium phosphate phases, and amorphous calcium phosphate. These phases have a large difference in solubility in vivo. As a result, plasma sprayed hydroxyapatite (PSHA) films do not dissolve or degrade uniformly in vivo. This heterogeneous degradation can result in particles in the vicinity of the implant, which can trigger an inflammatory cascade leading to osteolysis. The particles can further penetrate into the articular surface, resulting in increased wear. Finally, this process is a "line of sight" process, and therefore is not well suited for coating the porous structure of cementless implants. The PSHA process or post-treatment methods can be applied to result in highly crystalline coatings that have long absorption times in vivo, an attribute that raises concerns about the delamination of relatively thick and stable coatings over time.
[0005] Other methods to produce HA coatings for biological fixation include physical methods such as sputtering, evaporation, and chemical vapor deposition. These physical methods do not reproduce the nanocrystallinity and large surface area of biological apatite, and the resulting coatings may not dissolve uniformly and may release particles.
[0006] Solution (or suspension) methods of producing HA coatings have also been attempted. For example, Zitelli, Joseph P. and Higham, Paul (2000) "A Novel Method For Solution Deposition of Hydroxyapatite Onto Three Dimensionally Porous Metallic Surfaces: Peri-Apatite HA" describes a process that involves making a slurry or finely divided HA particles into which the implant is placed and coated by deposition of the slurry particles. A large surface area microcrystalline coating is produced, but the adhesion to the substrate is poor.
[0007] Electrochemically assisted solution deposition has also been developed. In this process, a voltage exceeding that required to hydrolyze water is applied to the implant while it is suspended in an aqueous solution. This process results in the deposition of calcium phosphate on the implant surface. Typically, the deposited film is a mixture of calcium phosphate (CaP) phases and requires post-treatment to convert the film to a pure HA phase. Poor adhesion is also a concern with these films. Finally, it is difficult to control the electrochemical current on porous implants with irregular grains, making this process difficult to scale up.
[0008] Biomimetic processes have also been developed. These processes employ solutions that mimic body fluid concentrations and are typically performed near body temperature. These processes can produce bone-like apatite, but require days or weeks to produce films several micrometers thick. Attempts to increase the speed associated with such methods result in complications in reproducible pH control, deposition rate, and growth rate compared to crystal growth on the implant surface. Films formed at high speeds have been found to contain amorphous material. Furthermore, because the deposition rate is not controlled, it is difficult to achieve the target coating weight or thickness.
[0009] Previous attempts have been made to add gallium (Ga) to apatite coatings, but previous methods have not been successful in doping Ga ions into the hydroxyapatite lattice to substitute for specific calcium sites.
[0010] As discussed above, hydroxyapatite coatings can be applied to orthopedic implants to enhance osteoinductivity using methods that are either rapid but result in coatings with certain undesirable or unpredictable properties, or that result in a more desirable product but can take several days to form. Summary of the Invention [Problem to be solved by the invention]
[0011] What is needed is a conformal calcium phosphate coating that has a microstructure that can be rapidly formed and that has the property of degrading uniformly over a period of weeks without producing particles. [Means for solving the problem]
[0012] Some embodiments of the present invention are described in the items listed below. 1. An orthopedic implant comprising a metal surface and a hydroxyapatite layer deposited on at least a portion of the metal surface, the hydroxyapatite layer including gallium ions therein, the hydroxyapatite layer being crystalline. 2. An orthopedic implant comprising a metal surface and a hydroxyapatite layer deposited on at least a portion of the metal surface, the hydroxyapatite layer including gallium ions therein, the hydroxyapatite layer having an average crystallite size in the
[0001] direction of less than about 75 nm. 3. An orthopedic implant comprising a metal surface and a hydroxyapatite layer deposited on at least a portion of the metal surface, the hydroxyapatite layer comprising gallium ions therein, the hydroxyapatite layer, when subjected to XRD, producing a (002) XRD peak and a (112) XRD peak, the (002) XRD peak having an intensity between 1.5 and 10 times that of the (112) XRD peak. 4. An orthopedic implant comprising a metal surface and a hydroxyapatite layer deposited on at least a portion of the metal surface, the hydroxyapatite layer including gallium ions therein, the hydroxyapatite layer dissolving continuously in vitro for more than two hours. 5. An orthopedic implant comprising a metal surface and a hydroxyapatite layer deposited on at least a portion of the metal surface, wherein the hydroxyapatite layer includes gallium ions therein, and wherein the hydroxyapatite layer is substantially free of carbonate as measured by infrared spectroscopy. 6. The orthopedic implant of any one of the preceding claims, wherein gallium ions are substituted into the crystal lattice of the hydroxyapatite layer. 7. The orthopedic implant of any one of the preceding claims, wherein the hydroxyapatite layer, when subjected to XRD, produces a (002) XRD peak that is shifted by about 0.001° 2θ to about 0.1° 2θ compared to the (002) XRD peak of crystalline hydroxyapatite that does not contain gallium. 8. The orthopedic implant of any one of the preceding claims, wherein the hydroxyapatite layer, when subjected to XRD, produces a (002) XRD peak corresponding to a d-spacing shift of about 0.001 Å to about 0.05 Å compared to the (002) XRD peak of crystalline hydroxyapatite without gallium. 9. The orthopedic implant according to any one of the preceding claims, wherein the gallium ions comprise from about 0.01% to about 5% by weight of the hydroxyapatite layer. 10. An orthopedic implant according to any one of the preceding claims, wherein the hydroxyapatite layer has an average crystallite size in the
[0001] direction of less than about 75 nm. 11. An orthopedic implant according to any one of the preceding claims, wherein the hydroxyapatite layer has an average crystallite size in the
[0001] direction of about 10 to about 75 nm. 12. An orthopedic implant according to any one of the preceding claims, wherein the hydroxyapatite layer has an average crystallite size in the
[0001] direction of about 20 to about 70 nm. 13. The orthopedic implant of any one of the preceding claims, wherein the hydroxyapatite layer, upon XRD, produces a (002) XRD peak and a (112) XRD peak, the (002) XRD peak having an intensity 1.5 to 10 times that of the (112) XRD peak. 14. The orthopedic implant of any one of the preceding claims, wherein the hydroxyapatite layer, upon XRD, produces a (002) XRD peak and a (112) XRD peak, the (002) XRD peak having an intensity 2 to 5 times that of the (112) XRD peak. 15. The orthopedic implant according to any one of the preceding claims, wherein the hydroxyapatite layer dissolves in vitro over a period of 2 hours or more. 16. The orthopedic implant according to any one of the preceding claims, wherein the hydroxyapatite layer dissolves in vitro over a period of 5 hours or more. 17. The orthopedic implant according to any one of the preceding claims, wherein the hydroxyapatite layer dissolves in vitro over a period of 24 hours or more. 18. An orthopedic implant according to any one of the preceding claims, wherein the hydroxyapatite layer is resorbed in vivo within 6 weeks. 19. The orthopedic implant of any one of the preceding claims, wherein the hydroxyapatite layer comprises from about 0% to about 5% by weight of carbonate. 20. The orthopedic implant of any one of the preceding claims, wherein the hydroxyapatite layer is substantially free of carbonate as measured by infrared spectroscopy. 21. An orthopedic implant according to any one of the preceding claims, wherein the hydroxyapatite layer is in contact with a metal surface. 22. The orthopedic implant of any one of the preceding claims, wherein the metal surface comprises a metal oxide. 23. The orthopedic implant of any one of the preceding claims, wherein the metal surface comprises titanium. 24. The orthopedic implant of any one of the preceding claims, wherein the metal surface comprises a cobalt chromium alloy. 25. An orthopedic implant according to any one of the preceding claims, wherein the metal surface comprises titanium oxide. 26. An orthopedic implant according to any one of the preceding claims, wherein the metal surface comprises titanate. 27. An orthopedic implant as described in any one of the preceding claims, wherein the metal surface comprises sodium titanate. 28. The orthopedic implant of any one of the preceding claims, wherein the metal surface comprises a porous metal oxide surface. 29. An orthopedic implant according to any one of the preceding claims, wherein the metal surface is a titanium surface treated with a hydroxide. 30. The orthopedic implant of paragraph 29, wherein the hydroxide has a concentration of 1M or greater. 31. The orthopedic implant of paragraph 29 or paragraph 30, wherein the hydroxide has a concentration of 2M or more. 32. An orthopedic implant according to any one of paragraphs 29 to 31, wherein the hydroxide is sodium hydroxide. 33. An orthopedic implant according to any one of paragraphs 29 to 32, wherein the hydroxide is potassium hydroxide. 34. An orthopedic implant according to any one of claims 29 to 33, wherein the titanium surface is not heat treated after being treated with hydroxide. 35. An orthopedic implant as described in any one of the previous claims, wherein the metal surface has a thickness of greater than about 50 nm. 36. An orthopedic implant according to any one of the preceding claims, wherein the metal surface has a thickness of from about 50 nm to about 1 μm. 37. An orthopedic implant according to any one of the preceding claims, wherein the metal surface has a thickness of about 50 nm to about 100 nm. 38. The orthopedic implant of any one of the preceding claims, wherein the hydroxyapatite layer has a crystallinity of greater than about 90%. 39. The orthopedic implant of any one of the preceding claims, wherein the hydroxyapatite layer has a crystallinity of about 70% to about 100% by weight. 40. The orthopedic implant of any one of the preceding claims, wherein the hydroxyapatite layer has a phase purity of greater than 90% crystalline hydroxyapatite. 41. The orthopedic implant of any one of the preceding claims, wherein the hydroxyapatite layer has a shear strength of about 20 MPa to about 80 MPa as measured according to ASTM F1044. 42. The orthopedic implant of any one of the preceding claims, wherein the hydroxyapatite layer has a tensile strength of about 50 MPa to about 100 MPa as measured according to ASTM F1147. 43. An orthopedic implant according to any one of the preceding claims, wherein the hydroxyapatite layer is transparent or translucent in the absence of a colorant. 44. An orthopedic implant according to any one of the preceding claims, wherein the Ca / P ratio of the hydroxyapatite layer is 1-2. 45. The hydroxyapatite layer is about 15 m 2 / g~about 200m 2 3. The orthopedic implant of any preceding claim, having a surface area of 0.1 μm / g. 46. An orthopedic implant according to any one of the preceding claims, wherein the hydroxyapatite layer does not release particles under physiological conditions. 47. An orthopedic implant according to any one of the preceding claims, wherein the hydroxyapatite layer is a calcium-deficient hydroxyapatite layer. 48. An orthopedic implant according to any preceding claim, wherein the gallium is distributed throughout the hydroxyapatite layer. 49. A method of treating a patient, the method comprising administering to the patient an orthopedic implant as described in any one of the preceding claims.
[0013] Further, some embodiments of the present invention are described in the items listed below. 1. An osteoinductive composition comprising hydroxyapatite, wherein the hydroxyapatite includes gallium ions therein, and wherein the hydroxyapatite is crystalline. 2. An osteoinductive composition comprising hydroxyapatite, wherein the hydroxyapatite has an average crystallite size in the
[0001] direction of less than about 75 nm. 3. An osteoinductive composition comprising hydroxyapatite, wherein, when subjected to XRD, the hydroxyapatite produces a (002) XRD peak and a (112) XRD peak, and the (002) XRD peak has an intensity 1.5 to 10 times that of the (112) XRD peak. 4. An osteoinductive composition comprising hydroxyapatite, the hydroxyapatite containing gallium ions therein, the hydroxyapatite dissolving continuously in vitro for more than 2 hours. 5. An osteoinductive composition comprising hydroxyapatite, the hydroxyapatite including gallium ions therein, the hydroxyapatite being substantially free of carbonate as measured by infrared spectroscopy. 6. The osteoinductive composition according to any one of the preceding claims, wherein gallium ions are substituted into the crystal lattice of hydroxyapatite. 7. The osteoinductive composition according to any one of the preceding claims, wherein the hydroxyapatite, when subjected to XRD, produces a (002) XRD peak that is shifted by about 0.001° 2θ to about 0.1° 2θ compared to the (002) XRD peak of crystalline hydroxyapatite that does not contain gallium. 8. The osteoinductive composition of any one of the preceding claims, wherein the hydroxyapatite, when subjected to XRD, produces a (002) XRD peak corresponding to a d-spacing shift of about 0.001 Å to about 0.05 Å compared to the (002) XRD peak of crystalline hydroxyapatite that does not contain gallium. 9. The osteoinductive composition according to any one of the preceding claims, wherein the gallium ions are contained in an amount of about 0.01% to about 5% by weight of the hydroxyapatite. 10. The osteoinductive composition of any one of the preceding claims, wherein the hydroxyapatite has an average crystallite size in the
[0001] direction of less than about 75 nm. 11. The bone-inducing composition according to any one of the preceding claims, wherein the hydroxyapatite has an average crystallite size in the
[0001] direction of about 10 nm to about 75 nm. 12. The bone-inducing composition according to any one of the preceding claims, wherein the hydroxyapatite has an average crystallite size in the
[0001] direction of about 20 nm to about 70 nm. 13. The bone-inducing composition according to any one of the preceding claims, wherein, when hydroxyapatite is subjected to XRD, it produces a (002) XRD peak and a (112) XRD peak, and the (002) XRD peak has an intensity 1.5 to 10 times that of the (112) XRD peak. 14. The osteoinductive composition according to any one of the preceding claims, wherein, when subjected to XRD, the hydroxyapatite produces a (002) XRD peak and a (112) XRD peak, and the (002) XRD peak has an intensity 2 to 5 times that of the (112) XRD peak. 15. The osteoinductive composition according to any one of the preceding claims, wherein the hydroxyapatite dissolves in vitro over a period of 2 hours or more. 16. The osteoinductive composition according to any one of the preceding claims, wherein the hydroxyapatite dissolves in vitro over a period of 5 hours or more. 17. The osteoinductive composition according to any one of the preceding claims, wherein the hydroxyapatite dissolves in vitro over a period of 24 hours or more. 18. The bone-inducing composition according to any one of the preceding claims, wherein the hydroxyapatite is resorbed in vivo within 6 weeks. 19. The osteoinductive composition of any one of the preceding claims, wherein the hydroxyapatite comprises from about 0% to about 5% by weight of carbonate. 20. The osteoinductive composition of any preceding claim, wherein the hydroxyapatite is substantially free of carbonate as measured by infrared spectroscopy. 21. An osteoinductive composition according to any one of the preceding claims, wherein the hydroxyapatite is in contact with a metal surface. 22. The osteoinductive composition of paragraph 21, wherein the metal surface comprises a metal oxide. 23. The osteoinductive composition of paragraph 21 or 22, wherein the metal surface comprises titanium. 24. The osteoinductive composition of paragraph 21 or paragraph 23, wherein the metal surface comprises a cobalt chromium alloy. 25. The bone-inducing composition according to any one of paragraphs 21 to 24, wherein the metal surface comprises titanium oxide. 26. The osteoinductive composition of any one of paragraphs 21 to 25, wherein the metal surface comprises titanate. 27. The bone-inducing composition of any one of paragraphs 21 to 26, wherein the metal surface comprises sodium titanate. 28. The osteoinductive composition of any one of paragraphs 21 to 27, wherein the metal surface comprises a porous metal oxide surface. 29. An osteoinductive composition according to any one of claims 21 to 28, wherein the metal surface is a titanium surface treated with a hydroxide. 30. The osteoinductive composition according to paragraph 29, wherein the hydroxide has a concentration of 1M or more. 31. The osteoinductive composition of paragraph 29 or paragraph 30, wherein the hydroxide has a concentration of 2M or more. 32. The bone-inducing composition according to any one of paragraphs 29 to 31, wherein the hydroxide is sodium hydroxide. 33. The bone-inducing composition according to any one of paragraphs 29 to 32, wherein the hydroxide is potassium hydroxide. 34. An osteoinductive composition according to any one of claims 29 to 33, wherein the titanium surface is not heat-treated after being treated with hydroxide. 35. An osteoinductive composition according to any one of paragraphs 29 to 34, wherein the metal surface has a thickness of greater than about 50 nm. 36. An osteoinductive composition according to any one of paragraphs 29 to 35, wherein the metal surface has a thickness of about 50 nm to about 1 μm. 37. An osteoinductive composition according to any one of paragraphs 29 to 36, wherein the metal surface has a thickness of about 50 nm to about 100 nm. 38. The osteoinductive composition of any one of the preceding claims, wherein the hydroxyapatite has a crystallinity of greater than about 90%. 39. The osteoinductive composition according to any one of the preceding claims, wherein the hydroxyapatite has a crystallinity of about 70% to about 100% by weight. 40. The osteoinductive composition of any one of the preceding claims, wherein the hydroxyapatite has a phase purity of greater than 90% crystalline hydroxyapatite. 41. The osteoinductive composition according to any one of the preceding claims, wherein the hydroxyapatite has a shear strength of about 20 MPa to about 80 MPa as measured according to ASTM F1044. 42. The osteoinductive composition according to any one of the preceding claims, wherein the hydroxyapatite has a tensile strength of about 50 MPa to about 100 MPa as measured according to ASTM F1147. 43. An osteoinductive composition according to any one of the preceding claims, wherein the hydroxyapatite is transparent or translucent in the absence of a colorant. 44. The osteoinductive composition according to any one of the preceding claims, wherein the Ca / P ratio of the hydroxyapatite is 1-2. 45. Hydroxyapatite is about 15m 2 / g~about 200m 2 The osteoinductive composition according to any one of the preceding claims, having a surface area of 1 / g. 46. The osteoinductive composition according to any one of the preceding claims, wherein the hydroxyapatite does not release particles under physiological conditions. 47. The osteoinductive composition of any preceding claim, wherein the hydroxyapatite comprises calcium-deficient hydroxyapatite. 48. An osteoinductive composition according to any one of the preceding claims, wherein the gallium is distributed throughout the hydroxyapatite.
[0014] Further, some embodiments of the present invention are described in the items listed below. 1. A method of forming a hydroxyapatite coating, the method comprising the steps of contacting a metal surface with a supersaturated solution containing calcium ions, phosphate ions, and gallium ions, and reducing the amount of air contacting the supersaturated solution during the coating process. 2. A method of forming a hydroxyapatite coating, the method comprising contacting a metal surface with a supersaturated solution comprising calcium ions, phosphate ions, and gallium ions, wherein the pH of the solution fluctuates less than 0.1 pH units / hour during the contacting step. 3. A method of forming a hydroxyapatite coating, the method comprising contacting a metal surface with a supersaturated solution comprising calcium ions, phosphate ions, and gallium ions, wherein hydroxyapatite is formed on the metal surface at a rate of between 0.05 μm / h and 1.5 μm / h. 4. A method of forming a hydroxyapatite coating, the method comprising the steps of mixing a first solution containing gallium ions and phosphate ions with a second solution containing calcium ions to form a supersaturated solution, and contacting a metal surface with the supersaturated solution. 5. The method of any one of the preceding claims, wherein the metal surface is a metal oxide surface. 6. The method of any one of the preceding claims, wherein a hydroxyapatite coating is formed on an orthopedic implant that includes a metal surface. 7. The method of any one of the preceding claims, further comprising the step of reducing the amount of air that contacts the supersaturated solution during the coating step. 8. The method of any one of the preceding claims, wherein during the contacting step, the pH of the supersaturated solution fluctuates by less than 0.1 pH units / hour. 9. The method of any one of the preceding claims, further comprising the step of decreasing the pH by a predetermined value that is less than 0.15 pH units during the contacting step. 10. The method according to any one of the preceding claims, wherein hydroxyapatite is formed on the metal surface at a rate of 0.05 μm / h to 1 μm / h. 11. The method according to any one of the preceding claims, wherein the hydroxyapatite is calcium-deficient hydroxyapatite. 12. The method according to any one of the preceding claims, wherein the pH of the supersaturated solution is from about 7.5 to about 7.9. 13. The method according to any one of the preceding claims, wherein the calcium concentration of the supersaturated solution is about 1.4 mM to about 1.8 mM. 14. The method according to any one of the preceding claims, wherein the phosphate concentration of the supersaturated solution is from about 2 mM to about 2.3 mM. 15. The method according to any one of the preceding claims, wherein the gallium concentration of the supersaturated solution is from about 0.01 mM to about 1.0 mM. 16. The method according to any one of the preceding claims, wherein the Gibbs free energy change associated with the hydroxyapatite coating formation step is from about 8 kJ / mol to about 8.4 kJ / mol at the start of the contacting step. 17. The coating has a rate per unit surface area of approximately 0.015 mg / hr mm 2 ~Approx. 0.05mg / hr mm 2 20. The method of any one of the preceding claims, wherein the 18. The method according to any one of the preceding claims, further comprising the step of removing the metal surface from the supersaturated solution after about 0.5 hours to about 12 hours. 19. The method of claim 18, further comprising the step of contacting the metal surface with an additional amount of the supersaturated solution that was not in contact with the metal surface after the removing step. 20. The method according to any one of the preceding claims, wherein the temperature of the supersaturated solution is about 45°C to about 50°C. 21. The method according to any one of the preceding claims, wherein the temperature of the supersaturated solution is about 46.5°C to 47.5°C. 22. The method of any one of the preceding claims, wherein the supersaturated solution further comprises a salt and a buffer. 23. The method of claim 22, wherein the salt is sodium chloride and the buffer is tris(hydroxymethyl)aminomethane. 24. The method of any one of the preceding claims, further comprising the step of agitating the supersaturated solution during the contacting step. 25. The method according to any one of the preceding claims, wherein heterogeneous crystal growth occurs at the metal surface and homogeneous crystal growth does not occur. 26. The method according to any one of the preceding claims, further comprising the step of forming a titanium layer on the implant body to form a metallic surface. 27. The method of any one of the preceding claims, further comprising the step of activating the metal surface by contacting the metal surface with a base. 28. The method of claim 27, wherein the base is hydroxide anion. 29. The method of any one of the preceding claims, wherein the metal surface comprises a titanium dioxide surface. 30. The method of any one of the preceding claims, wherein the metal surface comprises an activated metal surface. 31. The method of any one of the preceding claims, wherein the metal surface comprises titanate. 32. The method according to any one of the preceding claims, wherein the process occurs under inert atmospheric conditions. 33. The method according to any one of the preceding claims, wherein the process occurs under an argon atmosphere. 34. The method according to any one of the preceding claims, wherein the calcium solution and the phosphate solution are mixed at about 15°C to about 35°C. 35. The method of any one of the preceding claims, wherein the hydroxyapatite coating is not further treated to enhance crystallinity after the contacting step. 36. The method according to any one of the preceding claims, wherein the method is validated with respect to the amount of calcium phosphate coating on the metal surface. 37. The method of any one of the preceding claims, wherein the hydroxyapatite coating is formed primarily by heterogeneous nucleation, whereby the supersaturated solution remains free of visible turbidity during the contacting step. 38. The method of any one of the preceding claims, wherein the hydroxyapatite coating is formed at a substantially continuous rate throughout the contacting step. 39. The method according to any one of the preceding claims, further comprising the step of determining the amount of hydroxyapatite coating based on the amount of calcium ions and phosphate ions. 40. The method according to any one of the preceding claims, wherein at least two deposition sequences are employed. 41. The method of any one of the preceding claims, further comprising the step of determining the amount of hydroxyapatite coating based on the pH of the supersaturated solution. 42. The method of any one of the preceding claims, further comprising the step of determining the amount of hydroxyapatite coating based on the duration of the contacting step. 43. The method according to any one of the preceding claims, wherein during the contacting step, the pH of the supersaturated solution fluctuates by about 0.01 to about 0.1 pH units / hour. 44. The coating adheres at a rate of approximately 0.005 mg / hr mm 2 ~Approx. 0.015mg / hr mm 2 20. The method of any one of the preceding claims, wherein the 45. The method according to any one of the preceding claims, wherein the initial pH of the supersaturated solution is about 7.5 to about 7.9, and the temperature of the supersaturated solution is about 38°C to about 60°C. 46. The method of any preceding claim, further comprising the step of heating the coating in a phosphate solution to reduce surface cracking. 47. The method of any preceding claim, further comprising contacting the coating with a supercritical fluid to reduce surface cracking. 48. An osteoinductive composition formed by the method of any one of the preceding claims. 49. An orthopedic implant comprising an osteoinductive composition formed by the method of any one of the preceding claims.
[0015] The above and other objects, features and advantages of the present invention will become apparent from the following description and accompanying drawings. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a graph showing the properties of hydroxyapatite coatings formed on crystalline and amorphous titanium dioxide (TiO2) coated substrates having thicknesses ranging from 50 nm to 500 nm. [Diagram 2] FIG. 2 is a scanning electron microscope (SEM) image of a 200 nm thick amorphous TiO2 coating after treatment with hydroxide. [Diagram 3] SEM image of a 200 nm thick crystalline TiO2 coating that was not treated with hydroxide. [Figure 4] FIG. 11 is a grazing angle X-ray diffraction (XRD) spectral overlay showing the spectra of a 200 nm thick amorphous TiO2 coating with and without hydroxide treatment, and a 500 nm thick amorphous TiO2 coating with and without hydroxide treatment. [Diagram 5] 1 is a grazing angle XRD spectral overlay showing spectra of a 200 nm thick crystalline TiO2 coating with and without hydroxide treatment, and a 500 nm thick crystalline TiO2 coating with and without hydroxide treatment. [Figure 6] SEM image of a titanium layer electrocoated onto a CoCrMo core. [Figure 7] 1 is an image of the full-scale coating vessel. [Figure 8] 1 is a SEM image of the SoDHA coating at 15,000x magnification. [Figure 9A] 1 is a SEM image of the SoDHA coating at 100x magnification. [Figure 9B] 1 is a SEM image of the SoDHA coating at 400x magnification. [Figure 10] 1 is a graph showing the relationship between pH and the weight of hydroxyapatite precipitate over the course of each deposition process. [Figure 11] 1 is a graph showing deposition rates at various surface areas for a solution deposited hydroxyapatite (SoDHA) process. [Figure 12] 8 is a graph showing the Ca / P ratios of five samples produced by the SoDHA process in the full-scale deposition system shown in FIG. [Figure 13]13 is a graph showing the crystallinity of hydroxyapatite in the five samples illustrated in FIG. 12. [Figure 14] 13 is a graph showing the percentage of crystalline hydroxyapatite in materials formed by the SoDHA process for the five samples illustrated in FIG. 12. [Figure 15] 13 is a graph showing the tensile strength of hydroxyapatite in the five samples illustrated in FIG. 12. [Figure 16] 13 is a graph showing the shear strength of hydroxyapatite in the five samples illustrated in FIG. 12. [Figure 17] 1 shows the hip stem coupon tool used in the XRD characterization studies described herein. [Figure 18] Figure 1 shows overlaid XRD scans of gallium substituted SoDHA HA disks coated from 0 wt% to 20 wt% Ga solution conditions. [Figure 19] The overlaid XRD scans in Figure 18 are shown from 25° to 27° 2θ. [Figure 20] The %Ga of gallium-substituted SoDHA HA disks formed under 0 wt% to 20 wt% Ga solution conditions is shown. [Figure 21] Figure 2 shows the Fourier transform infrared spectroscopy (FTIR) spectrum of SoDHA-G HA shavings powder. [Figure 22] 1 is a graph showing the dissolution rates of gallium substituted SoDHA HA samples. [Diagram 23] 1 is a graph showing the dissolution rate of National Institute of Standards and Technology (NIST) standard HA samples. [Figure 24] 1 shows a DSC trace of SoDHA shavings powder, showing no discernible exothermic peaks upon heating. [Diagram 25] 1 shows bone ingrowth of implants with SoDHA coating and gallium substituted SoDHA coating in a dog model. [Figure 26A]400x magnification SEM image of air-dried gallium-substituted SoDHA coating without post-treatment. [Figure 26B] 13 is an SEM image of scCO2-dried gallium substituted SoDHA coating at 400x magnification. [Figure 27] 400x magnification SEM image of oven-dried gallium-substituted SoDHA coating. [Figure 28A] SEM image at 800x magnification of gallium substituted SoDHA coating after hydrothermal treatment at 70°C for 2 hours in phosphate-Ga stock solution. [Figure 28B] SEM image at 1000x magnification of gallium substituted SoDHA coating after hydrothermal treatment at 70°C for 2 hours in phosphate-Ga syrup solution. [Figure 29A] SEM image at 501x magnification of gallium substituted SoDHA coating after hydrothermal treatment at 90°C for 1 hour in phosphate-Ga stock solution. [Figure 29B] SEM image at 500x magnification of gallium substituted SoDHA coating after hydrothermal treatment at 90°C for 1 hour in phosphate-Ga syrup solution. [Figure 30A] SEM image at 500x magnification of gallium substituted SoDHA coating after hydrothermal treatment at 90°C for 2 hours in phosphate-Ga stock solution. [Figure 30B] SEM image at 500x magnification of gallium substituted SoDHA coating after hydrothermal treatment at 90°C for 2 hours in phosphate-Ga syrup solution. [Diagram 31] 1 shows overlaid XRD scans of a SoDHA coating with no post-treatment, a gallium-substituted SoDHA coating with no post-treatment, and a hydrothermally treated gallium-substituted SoDHA coating. [Figure 32A] Representative images illustrating crack density quantification are shown. [Figure 32B] Representative images illustrating crack density quantification are shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] While the invention is susceptible to various modifications and alternative forms, specific embodiments thereof have been shown by way of example in the drawings and are herein described in detail, it being understood, however, that it is not intended to limit the invention to the particular forms disclosed, but on the contrary, the intention is to cover all modifications, equivalents and alternatives falling within the spirit and scope of the invention as defined in the appended claims.
[0018] The present invention relates to calcium phosphate coated orthopedic implants, such as those coated with gallium substituted hydroxyapatite (HA), and methods for making the same. Without wishing to be bound by theory, it is believed that the presence of gallium in the coating allows for enhanced biocompatibility compared to conventional hydroxyapatite coatings. In the present invention, gallium ions (Ga +3 ) is incorporated or doped into the hydroxyapatite (HA) lattice, allowing for localized, controlled release of this therapeutic ion as the HA coating is absorbed over a period of weeks in vivo. Gallium accumulates in newly formed bone to aid in new bone formation, can downregulate inflammation, and possesses antibacterial properties. The gallium-substituted HA coatings described herein can be used in multifunctional coatings to enhance bone formation capabilities and promote antibacterial effects at the implantation site.
[0019] The gallium-substituted hydroxyapatite coating described herein has a highly uniform microstructure. When the implant is used in the human or animal body, the gallium-substituted hydroxyapatite coating degrades uniformly over an extended period of time without releasing particles. In some embodiments, this period is six weeks or less. The coating described herein also has advantageous adhesive and / or cohesive properties, such as higher tensile strength than conventional coatings. In addition, the gallium-substituted hydroxyapatite coating described herein can be rapidly formed on a substrate by a controlled yet rapid growth process, which allows verification using process diagnostics, which allows the measurement of the total coating weight of a batch of parts without the need to measure the coating weight of the part, which results in a uniform microstructure and chemical composition of the coating.
[0020] Solution-deposited ceramic coatings may be prone to cracking during drying. This effect may be exacerbated as the coating thickness increases. In some instances, cracking may be observed in solution-deposited gallium-substituted SoDHA (SoDHA-G) coatings as they dry after formation. Without being bound by theory, compared to gallium-free SoDHA coatings, SoDHA-G coatings exhibit a greater tendency to crack, potentially as a result of the lattice strain associated with doping gallium into the hydroxyapatite lattice. Two exemplary independent methods for reducing cracking during drying described herein include (1) organic solvent exchange and supercritical solvent extraction, and (2) reprecipitation crack repair by hydrothermal treatment. It will be understood that organic solvent exchange and reprecipitation crack repair can be performed independently of each other or in combination.
[0021] Those skilled in the art will appreciate that the compositions and methods described herein improve cementless fixation of orthopedic implants for improved survival and may extend the use of cementless implants to procedures where cemented implants are the current standard of care, thereby reducing surgical time and healthcare costs.
[0022] Gallium-substituted hydroxyapatite coating The calcium phosphate coatings described herein include gallium-substituted HA. As used herein, HA includes, but is not limited to, calcium-deficient hydroxyapatite (CDHA) in which the calcium ions are substituted with gallium. In some embodiments, the HA described herein is non-stoichiometric gallium-substituted HA. Gallium-substituted HA can be represented by the formula Ca 10-x Ga x (PO4)6(OH) 2-x (CO3) x where x is about 0 to about 1, or about 0.1 to about 1. It will be understood that the formulas described herein describe stoichiometric equivalents. The HA coating has a characteristic calcium to phosphorus ratio (Ca / P ratio). The Ca / P ratio can be about 1 to about 2, about 1.2 to about 2, about 1.3 to about 2, about 1.39 to about 2, about 1 to about 1.8, about 1.2 to about 1.8, about 1.3 to about 1.8, about 1.39 to about 1.8, about 1 to about 1.7, about 1.2 to about 1.7, about 1.3 to about 1.7, about 1.39 to about 1.7, about 1 to about 1.649, about 1.2 to about 1.649, about 1.3 to about 1.649, about 1.39 to about 1.649, or about 1.5 to about 1.67. It will be appreciated that the gallium substituted HA can be modified by adjusting the calcium and phosphorus concentrations of the solution in which the HA coating may be formed.
[0023] In the gallium-substituted HA coating, a portion of the calcium ions are replaced by gallium ions, as compared to conventional HA. The bioactive gallium-substituted hydroxyapatite coatings prepared herein preferably have a molar ratio of gallium ions to calcium ions of about 1:10 to about 1:5000, about 1:10 to about 1:1500, or about 1:20 to about 1:1500. Thus, the Ca / P ratio can be varied as a function of Ga substitution into the hydroxyapatite lattice.
[0024] As described in detail below, the gallium-substituted HA coating can be formed from a supersaturated solution, which remains substantially clear during the coating process due to homogeneous nucleation in the solution. In some embodiments, the gallium-substituted HA coating does not contain carbonate, which assists in pH control during coating formation. Without being bound by theory, it is believed that deposition from a substantially clear solution with homogeneous nucleation plays a role in the gallium-substituted HA being deposited at a predictable coating rate, and the gallium-substituted HA coating having high crystallinity, homogeneous microstructure, and enhanced biocompatibility. In some embodiments, the weight percent of carbonate in the coating is from about 0% to about 25%, from about 0% to about 20%, from about 0% to about 15%, from about 0% to about 10%, from about 0% to about 5%, from about 0% to about 3%, from about 0% to about 2%, from about 0% to about 1%, from about 0% to about 0.1%, from about 0.1% to about 25%, from about 0.1% to about 20%, from about 0.1% to about 15%, from about 0.1% to about 10%, or from about 0.1% to about 5%, about 0.1% to about 3%, about 0.1% to about 2%, about 0.1% to about 1%, about 1% to about 25%, about 1% to about 20%, about 1% to about 15%, about 1% to about 10%, about 1% to about 5%, about 1% to about 3%, about 1% to about 2%, about 2% to about 25%, about 2% to about 20%, about 2% to about 15%, about 2% to about 10%, about 2% to about 5%, or about 2% to about 3%. In some embodiments, the concentration of carbonate in the coating is measured by spectroscopic methods, such as infrared spectroscopy. The coating may be substantially free of carbonate. As used herein, a "substantially carbonate-free" coating is one that has a carbonate-free peak at 1500 cm when measured by infrared spectroscopy. -1 ~1300cm -1 This refers to coatings that have no discernible carbonate peak between
[0025] The weight percent of crystalline gallium substituted HA in the coatings described herein is about 50% to about 100%, about 60% to about 100%, about 70% to about 100%, about 80% to about 100%, about 90% to about 100%, about 50% to about 99%, about 60% to about 99%, about 70% to about 99%, about 80% to about 99%, about 90% to about 99%, about 50% to about 95%, about 60% to about 95%, about 70% to about 95%, about 80% to about 95%, or about 90% to about 95%. Without wishing to be bound by theory, it is believed that the coating is formed by heterogeneous nucleation, resulting in a coating that comprises primarily crystalline gallium substituted HA or OCP.
[0026] The gallium-substituted HA component of the gallium-substituted HA coating has a high degree of crystallinity, for example as measured by differential scanning calorimetry (DSC), of greater than about 50%, greater than about 80%, greater than about 90%, greater than about 95%, greater than about 96%, greater than about 97%, between about 80% and about 99.9%, between about 90% and about 99.9%, between about 95% and about 99.9%, between about 96% and about 99.9%, or between about 97% and about 99.9%.
[0027] The gallium-substituted HA component of the coating has a high crystalline phase purity in its predominant phase, which may be greater than about 80%, greater than about 90%, greater than about 95%, greater than about 96%, greater than about 97%, about 80% to about 99.9%, about 90% to about 99.9%, about 95% to about 99.9%, about 96% to about 99.9%, or about 97% to about 99.9%. The high crystallinity and high crystalline phase purity of the gallium-substituted HA component in the gallium-substituted HA coating enhances biocompatibility and uniform degradation in vivo while avoiding particulate shedding. In some embodiments, the crystallinity is measured by differential scanning calorimetry (DSC).
[0028] The gallium-substituted HA component of the coating has low or no amorphous content. The amorphous content is less than about 20%, less than about 15%, less than about 10%, less than about 5%, less than about 4%, less than about 3%, about 0.1% to about 3%, about 0.1% to about 5%, about 0.1% to about 10%, or about 0.1% to about 20%. The amorphous content may be below the detection limit. In some embodiments, the amorphous content is measured by differential scanning calorimetry (DSC).
[0029] The crystal structure of the gallium-substituted HA coating can be characterized using X-ray spectroscopy, such as powder X-ray diffraction spectroscopy. The gallium-substituted HA coating exhibits several characteristic 2θ diffraction angles when characterized by powder X-ray diffraction. The numbers in parentheses are the Miller indices associated with each peak. The X-ray spectrum of the gallium-substituted HA coating can exhibit 2θ diffraction angles including about 26±2° (002), about 28±2° (102), about 32±2° (112), about 50±2° (213), and about 53±2° (004) or 26±0.5° (002), about 28±0.5° (102), about 32±0.5° (112), about 50±0.5° (213), and about 53±0.5° (004). X-ray spectra of gallium substituted HA coatings may exhibit 2θ diffraction angles including about 26±1° (002), about 28±1° (102), about 32±1° (112), about 50±1° (213), and about 53±1° (004). X-ray spectra of gallium substituted HA coatings may exhibit 2θ diffraction angles including about 25.58±0.1°, about 28.13±0.1°, about 31.75±0.1°, 32.17±0.1°, about 49±0.1°, and about 53±0.1°. It will be understood that the diffraction angles stated herein may systematically shift due to instrumental variations.
[0030] The XRD spectrum of a gallium substituted HA coating has characteristic relative intensities. As used herein, the relative intensity of a peak in an XRD spectrum refers to the peak intensity divided by the intensity of the strongest peak in the spectrum. The peaks associated with the (002), (211), (112), (202), (213), and (004) directions may have relative intensities of 100%, 40-50%, 45-55%, 15-25%, 10-20%, and 15-25%, respectively. Any one of the peaks associated with the (002), (211), (112), (202), (213), and (004) directions may have relative intensities of 100%, 30-60%, 35-65%, 5-35%, 0-30%, and 5-35%, respectively. In some embodiments, the hydroxyapatite layer has an XRD intensity ratio of the (002) peak:(211) peak that is greater than about 1, greater than about 1.25, greater than about 1.5, greater than about 1.75, greater than about 2.0, greater than about 2.5, greater than about 3.0, or greater than about 3.5.
[0031] As a result of the gallium substitution, the 2θ diffraction angle of the (002) peak is shifted relative to HA coatings formed by solution deposition processes without gallium, as characterized using X-ray spectroscopy. The resulting shift in the (002) diffraction peak can be approximately about 0.25° or less, about 0.2° or less, about 0.15° or less, about 0.01° to about 0.25°, about 0.01° to about 0.2°, about 0.01° to about 0.15°, about 0.05° to about 0.25°, about 0.05° to about 0.2°, or about 0.05° to about 0.15°. The shift in the (002) diffraction peak can increase with increasing gallium ion concentration. This shift in the (002) diffraction peak 2θ is associated with a d-spacing of about 0.001 Å to about 0.05 Å, about 0.0025 Å to about 0.025 Å, or about 0.0037 Å to about 0.0226 Å.
[0032] The gallium-substituted HA coating can be further characterized using Fourier transform infrared (FTIR) spectroscopy. 3- The characteristic of this is about 1100cm -1The gallium-substituted HA coating exhibits an FTIR band at approximately 1400–1500 cm, which is characteristic of carbonates. -1 The FTIR bands are missing.
[0033] In some embodiments, the gallium-substituted HA coating is nanocrystalline. Thus, the gallium-substituted HA coating of the present disclosure provides a small crystallite size as measured by X-ray diffraction or scanning electron microscopy. The gallium-substituted hydroxyapatite has an average crystallite size in the range of about 1 nm to about 100 nm, about 5 nm to about 100 nm, about 10 nm to about 100 nm, about 15 nm to about 100 nm, about 1 nm to about 80 nm, about 5 nm to about 80 nm, about 10 nm to about 80 nm, about 15 nm to about 80 nm, or about 15 nm to about 70 nm. The average crystallite size in the (002) direction is about 60 nm to about 80 nm, about 65 nm to about 75 nm, about 66 nm to about 73 nm, or about 68 nm to about 69 nm. The average crystallite size in the (200) direction is about 10 nm to about 30 nm, about 15 nm to about 25 nm, about 16 nm to about 23 nm, or about 18 nm to about 22 nm. The average crystallite size in the (210) direction is about 40 nm to about 60 nm, about 45 nm to about 55 nm, about 46 nm to about 53 nm, or about 48 nm to about 52 nm. In some embodiments, the gallium substituted HA film has a crystallite size in at least one direction that is smaller than the wavelength of light, and the grains are bonded together without the presence of a second amorphous or crystalline phase having a different refractive index. In such embodiments, the coating is transparent or translucent.
[0034] The gallium substituted HA coatings of the present disclosure are highly porous and have a large surface area, approximately 5 m 2 / g~about 100m 2 / g, approx. 10m 2 / g ~ approx. 75m 2 / g, approx. 10m 2 / g~about 50m 2 / g, approx. 10m 2 / g~about 200m 2 / g, approx. 10m 2 / g~about 150m 2 / g, approx. 10m2 / g~about 100m 2 / g, approx. 50m 2 / g~about 200m 2 / g, approx. 50m 2 / g~about 150m 2 / g, approx. 50m 2 / g~about 100m 2 / g, or about 15m 2 / g ~ approx. 35m 2 / g. This surface area can be determined using the Brunauer-Emmett-Teller (BET) method. This surface area can provide significant improvements in the adsorption of therapeutic agents onto these coatings, as described in more detail below. This increased loading capacity can be utilized to modulate the dosage and delayed release of therapeutic agents, thereby enhancing therapeutic efficacy.
[0035] Without wishing to be bound by theory, another advantage of gallium substituted HA crystallite size reduction is that it allows for refinement of the surface nanomorphology of the implant surface, which may enhance blood-borne fibrinogen adsorption after implantation. This increases platelet adhesion and activation, which are initiators of the inflammatory cascade and healing process. Nanomorphology has also been shown to increase the adhesive strength of the fibrin clot (or extracellular matrix) to the implant surface, thereby ensuring integrity during new bone formation and wound contraction throughout the healing process.
[0036] The coatings described herein may release calcium and / or gallium in vitro at a substantially sustained rate, or at a sustained rate over an extended period of time, as measured with a calcium electrode as described in ASTM F1926. As used herein, a substantially sustained rate is a rate that varies less than 20% per hour. As used herein, a sustained rate is a rate that varies less than 5% per hour. The coating may release calcium at a substantially sustained rate for at least about 5 hours, at least about 10 hours, at least about 15 hours, at least about 20 hours, about 5 hours to about 100 hours, about 5 hours to about 50 hours, about 5 hours to about 30 hours, about 5 hours to about 25 hours, about 10 hours to about 100 hours, about 10 hours to about 50 hours, about 10 hours to about 30 hours, about 10 hours to about 25 hours, about 15 hours to about 100 hours, about 15 hours to about 50 hours, about 15 hours to about 30 hours, or about 15 hours to about 25 hours. The coating may release calcium at a sustained rate for at least about 5 hours, at least about 10 hours, at least about 15 hours, at least about 20 hours, about 5 hours to about 100 hours, about 5 hours to about 50 hours, about 5 hours to about 30 hours, about 5 hours to about 25 hours, about 10 hours to about 100 hours, about 10 hours to about 50 hours, about 10 hours to about 30 hours, about 10 hours to about 25 hours, about 15 hours to about 100 hours, about 15 hours to about 50 hours, about 15 hours to about 30 hours, or about 15 hours to about 25 hours.
[0037] The gallium substituted HA coatings described herein may have higher adhesion and higher cohesion to the substrate than previously described coatings. Adhesion and cohesion may be quantified by measuring peak stress values in tension and shear. The coatings described herein may extend outward from the surface of the orthopedic implant. As used herein, shear stress is the component of stress parallel to the bulk surface, and tensile stress is the component of stress away from the bulk surface.
[0038] The peak shear stress of the gallium substituted HA coating, as measured by ASTM F1044, can be from about 10 MPa to about 150 MPa, from about 10 MPa to about 100 MPa, from about 10 MPa to about 75 MPa, from about 10 MPa to about 65 MPa, or from about 28.2 MPa to about 63.6 MPa. The peak tensile stress, when measured by ASTM F1147, can be about 25 MPa to about 120 MPa, about 40 MPa to about 120 MPa, about 50 MPa to about 120 MPa, about 60 MPa to about 120 MPa, about 68 MPa to about 120 MPa, 25 MPa to about 100 MPa, about 40 MPa to about 100 MPa, about 50 MPa to about 100 MPa, about 60 MPa to about 100 MPa, about 68 MPa to about 100 MPa, 25 MPa to about 95 MPa, about 40 MPa to about 95 MPa, about 50 MPa to about 95 MPa, about 60 MPa to about 95 MPa, about 68 MPa to about 95 MPa, 25 MPa to about 90 MPa, about 40 MPa to about 90 MPa, about 50 MPa to about 90 MPa, about 60 MPa to about 90 MPa, or about 68 MPa to about 90 MPa.
[0039] The gallium substituted HA coating may have an average thickness of about 1 μm to about 50 μm, about 1 μm to about 25 μm, about 1 μm to about 20 μm, about 1 μm to about 15 μm, about 1 μm to about 10 μm, about 1 μm to about 8 μm, about 3 μm to about 50 μm, about 3 μm to about 25 μm, about 3 μm to about 20 μm, about 3 μm to about 15 μm, about 3 μm to about 10 μm, about 3 μm to about 8 μm, about 5 μm to about 50 μm, about 5 μm to about 25 μm, about 5 μm to about 20 μm, about 5 μm to about 15 μm, about 5 μm to about 10 μm, about 5 μm to about 8 μm, or about 7 μm when measured from the surface of the orthopedic implant to the bonding surface of about 150 nm or more.
[0040] When a porous ingrowth surface such as Porocoat or Gription is applied, the gallium substituted HA coating can be applied at a concentration of about 1 to about 100 mg / cm 2 , about 1 to about 75mg / cm 2 , about 1 to about 50mg / cm 2 , about 1 to about 25mg / cm 2 , about 1 to about 12mg / cm 2 , about 5~100mg / cm 2, about 5~75mg / cm 2 , about 5~50mg / cm 2 , about 5~25mg / cm 2 , about 5~12mg / cm 2 , about 7~15mg / cm 2 , about 7~14mg / cm 2 , about 7~12mg / cm 2 , about 9~15mg / cm 2 , about 9~14mg / cm 2 , about 9~12mg / cm 2 , about 9~11mg / cm 2 , about 9~12mg / cm 2 , or about 8 to about 12 mg / cm 2 The surface area of the material may be 0.1 to 0.5 mm.
[0041] When an orthopedic implant coated with the gallium-substituted HA coating described herein is used in a patient or animal (e.g., a dog), the rate of absorption in vivo is such that the gallium-substituted HA coating is absorbed within about 3 to about 15 weeks, about 4 to about 15 weeks, about 5 to about 15 weeks, about 6 to about 15 weeks, about 3 to about 14 weeks, about 4 to about 14 weeks, about 5 to about 14 weeks, about 6 to about 14 weeks, about 3 to about 12 weeks, about 4 to about 12 weeks, about 5 to about 12 weeks, about 6 to about 12 weeks, about 1 to about 6 weeks, or less than about 6 weeks.
[0042] In some embodiments, the gallium substituted HA coating further comprises one or more additional therapeutic agents. The coating may carry additional materials for improved osteoconductivity and / or delivery of anti-inflammatory materials.
[0043] The therapeutic agent may include proteins, fats, (lipo)polysaccharides, growth factors, cytostatic agents, hormone antibiotics, anti-infective agents, anti-allergic agents, anti-inflammatory agents, progesterone agents, humoral agents, antipyretics, and nutritional agents. The therapeutic agent may be an osteoconductive substance, an osteoinductive substance, or a substance that is both osteoconductive and osteoinductive.
[0044] metal surface The calcium phosphate layer described herein is disposed near the surface of an orthopedic implant. The surface may be a metal surface, such as a titanium or CoCr alloy surface, or a titanium dioxide (TiO2) surface. In some embodiments, the outer surface of the metal layer is amorphous and the remainder of the metal layer is crystalline. In other embodiments, the entire metal layer is crystalline. For example, the interface between the surface and the calcium phosphate coating may include an activated layer from which the calcium phosphate coating may nucleate and grow outwardly. It will be appreciated that the entire surface may be coated with HA, or alternatively, the surface may be masked and selected portions of the surface may be coated with HA.
[0045] The surface may be an activated metal surface. For example, when the metal surface is a titanium surface, the surface is activated to form a titanate outer surface, which promotes nucleation and increases adhesion between the titanium surface and the calcium phosphate coating. As described in detail below, the activation of the titanium surface also promotes controlled crystal growth of a calcium phosphate layer resulting therefrom without further heat treatment. In some embodiments, the native oxide, or an oxide produced by a passivation process, is converted to a titanate by hydroxide treatment. In some embodiments, the titanate is sodium titanate. Alternatively, crystalline TiO2 can be applied to the implant core. Such a crystalline film induces nucleation without further treatment. In some embodiments, the implant surface is made of something other than a titanium alloy. In this case, activation can be achieved by depositing a nm-scale crystalline TiOx film on the implant surface. Alternatively, a thin amorphous TiOx layer can be deposited and the amorphous film converted to a titanate by hydroxide treatment. Further methods of activation include forming surfaces that contain COOH, NH2, or other charged moieties, as will be apparent to those skilled in the art.
[0046] In some embodiments, the entire core of the implant is titanium. In other embodiments, the titanium is coated onto at least a portion of the implant core, which is further coated with a calcium phosphate coating as described herein. The implant core and / or surface may comprise materials such as CoCrMo or PEEK.
[0047] Alternatively, the implant may comprise any suitable material, such as silicon-based, ceramic-based, or polymer-based materials. Other contemplated materials include cobalt, chromium, iron, tantalum, niobium, zirconium, and their alloys (e.g., titanium and tantalum alloys), as well as cobalt, cobalt-chromium alloys, and stainless steel. The implant may comprise a biocompatible polymer, natural or synthetic, such as polyethylene (e.g., ultra-high molecular weight polyethylene or polyethylene oxide), polypropylene, polytetrafluoroethylene, polyglycolic acid, polylactic acid, other polysaccharides, and copolymers of any of the foregoing (e.g., copolymers of polylactic acid and polyglycolic acid), including tissue engineering scaffolds made of synthetic polymers (e.g., polyHEMA) and biological macromolecules (e.g., collagen and chondroitin sulfate).
[0048] The metal or metal oxide layer may have a thickness of at least about 25 nm, at least about 30 nm, at least about 35 nm, at least about 40 nm, at least about 45 nm, at least about 50 nm, at least about 60 nm, at least about 70 nm, at least about 80 nm, at least about 90 nm, or at least about 100 nm. In some embodiments, the layer may have a thickness of about 25 nm to about 125 nm, about 30 nm to about 125 nm, about 35 nm to about 125 nm, about 40 nm to about 125 nm, about 45 nm to about 125 nm, about 50 nm to about 125 nm, about 25 nm to about 100 nm, about 30 nm to about 100 nm, about 35 nm to about 100 nm, about 40 nm to about 100 nm, about 45 nm to about 100 nm, or about 50 nm to about 100 nm. Films less than 100 nm may not exhibit interference colors after hydroxide treatment. The preferred layer thickness can be determined based on the desired color profile of the orthopedic implant.
[0049] The crystalline structure of the titanium surface can be characterized using X-ray spectroscopy, such as powder X-ray diffraction. The titanium surface exhibits several characteristic 2θ diffraction angles when characterized by powder X-ray diffraction. The X-ray spectrum of the titanium film exhibits 2θ diffraction angles of about 26°, about 28°, about 32°, about 49°, and about 53°.
[0050] The metal surface can be modified before being coated with the HA coating. For example, the metal surface can be modified with respect to surface roughness to promote adhesion of the apatite coating to the biocompatible substrate. Possible methods for modifying the roughness of the metal surface include acid etching or grit blasting.
[0051] Titanium oxide formation and activation As mentioned above, titanium oxide layers can be formed on orthopedic prostheses. The preferred process for forming the TiO2 layer is one that produces a film that is conformal (non-line of sight) and strongly adheres to the core. Atomic layer deposition has been shown to produce both amorphous and crystalline films with good adhesion and uniform thickness. Sol-gel processing and electrodeposition of TiO2 films can also be utilized.
[0052] After a surface is formed or otherwise made available, surface activation can be performed to promote nucleation and calcium phosphate growth. The titanium oxide surface can be activated by applying basic conditions. In some embodiments, the titanium surface is treated with a hydroxide source, such as sodium hydroxide. The hydroxide treatment creates a porous titanate surface on the metal, which promotes nucleation and calcium phosphate growth.
[0053] Gallium-substituted solution-deposited hydroxyapatite (SoDHA-G) process The gallium-substituted hydroxyapatite coatings described herein are formed on the activated surface by deposition from a supersaturated solution. At a sufficiently optimized supersaturation value, stable nuclei are formed and grow from the activated surface, resulting in the calcium phosphate coatings described herein. Without being bound by theory, it is believed that this growth occurs primarily by a heterogeneous nucleation mechanism, rather than a homogeneous mechanism, under the conditions described in detail below. This process results in a gallium-substituted hydroxyapatite product, such as the coatings described above.
[0054] A calcium solution and a phosphate / gallium solution are prepared and adjusted to the desired concentration by dilution. The calcium solution and the phosphate / gallium solution are mixed to produce a supersaturated solution with respect to hydroxyapatite. An orthopedic implant precursor having an activated surface is contacted with the supersaturated solution to produce a gallium-substituted hydroxyapatite coating formation at a reproducible rate under solution conditions that do not produce turbidity. In some embodiments, the substrate has a crystalline TiO2 film surface, which is not necessarily activated. In some embodiments, the substrate has an amorphous film surface that has been treated with a base, such as a hydroxide. It is contemplated that the implant can be masked to allow deposition only on selected portions of the implant.
[0055] The turbidity of the solution can be determined using an optical sensor that evaluates the ultraviolet range. Utilizing an Optek AS16F probe sensor operating at 430 nm, turbidity due to homogeneous nucleation in the solution was detected. Without wishing to be bound by theory, it is believed that coating at a controlled rate occurs primarily due to heterogeneous nucleation.
[0056] The degree of supersaturation of the coating solution depends on the activity of the calcium, phosphate, and gallium ions in the solution and the pH of the solution. Activity further depends on the concentration, speciation, and ionic strength of the solution. The calcium and phosphate stock solutions are mixed to provide a supersaturated solution with respect to the desired calcium phosphate product. Contacting an orthopedic implant having an activated surface with the supersaturated solution results in the formation of a gallium-substituted hydroxyapatite coating at a rapid and reproducible rate.
[0057] The implant is coated in a solution that is supersaturated with respect to the HA phase. In some embodiments, the supersaturated solution includes Ga(NO3)3, Ca(NO3), K2HPO4, KH2PO4, NaCl, and tris(hydroxymethyl)aminomethane (TRIS) buffer. HPO42- / - The ratio of H2PO4 can be selected to achieve the target solution pH. As will be appreciated by those skilled in the art, other counterions besides NO3 and K can also be utilized. Calcium and phosphate / gallium concentrates are available at specified concentrations which can be diluted to working concentrations and then mixed to produce the final supersaturated solution.
[0058] The solution used to form HA contains calcium cations at a concentration of about 0.5 to about 1.5 mM, about 0.6 to about 1.5 mM, about 0.7 to about 1.5 mM, about 0.5 to about 1.3 mM, about 0.6 to about 1.3 mM, about 0.7 to about 1.3 mM, about 0.5 to about 1.1 mM, about 0.6 to about 1.1 mM, about 0.7 to about 1.1 mM, about 0.5 to about 1.05 mM, about 0.6 to about 1.05 mM, about 0.7 to about 1.05 mM, or about 0.62 to about 1.05 mM. In some embodiments, the calcium ion is Ca 2+ It is.
[0059] The solution used to form HA contains phosphate anion at a concentration of about 0.75 mM to about 1.75 mM, about 1.0 mM to about 1.75 mM, about 1.25 mM to about 1.75 mM, about 0.75 mM to about 1.5 mM, about 1.0 mM to about 1.5 mM, about 1.25 mM to about 1.5 mM, about 0.75 mM to about 1.35 mM, about 1.0 mM to about 1.35 mM, about 1.25 mM to about 1.35 mM, about 0.75 mM to about 1.3 mM, about 1.0 mM to about 1.3 mM, or about 1.25 mM to about 1.3 mM. In some embodiments, the phosphate anion is PO4 3- , HPO4 2- , H2PO4 - , or a combination thereof.
[0060] The phosphate solution used to form HA contains gallium cations at a concentration of about 0.01 mM to about 0.4 mM, about 0.01 mM to about 0.3 mM, about 0.01 mM to about 0.2 mM, about 0.01 mM to about 0.1 mM, about 0.01 mM to about 0.4 mM, about 0.05 mM to about 0.3 mM, about 0.05 mM to about 0.2 mM, or about 0.05 mM to about 0.1 mM. In some embodiments, the gallium ion is Ga 3+ In some embodiments, the source of gallium is Ga(NO3)3.
[0061] The solutions used to form gallium substituted HA are about 7.5 to about 8, about 7.55 to about 8, about 7.6 to about 8, about 7.65 to about 8, about 7.5 to about 7.9, about 7.55 to about 7.9, about 7.6 to about 7.9, about 7.65 to about 7.9, 7.5 to about 7.85, about 7.55 to about 7.85, about 7.6 to about 7.85, about 7.65 to about 7.85, The coating solution has a pH of 7.5 to about 7.8, about 7.55 to about 7.8, about 7.6 to about 7.8, about 7.65 to about 7.8, 7.5 to about 7.75, about 7.55 to about 7.75, about 7.6 to about 7.75, about 7.65 to about 7.75, 7.5 to about 7.7, about 7.55 to about 7.7, about 7.6 to about 7.7, about 7.65 to about 7.7, or about 7.684. This pH may be the initial pH of the coating process for a given coating iteration. This pH may be the pH when the solution is at 25°C.
[0062] In some embodiments, a buffer is included in the supersaturated solution to stabilize the pH. In some embodiments, the buffer is a tris(hydroxymethyl)aminomethane (Tris) buffer. The concentration of Tris is about 1 mM to about 10 mM, about 2 mM to about 10 mM, about 3 mM to about 10 mM, about 1 mM to about 8 mM, about 2 mM to about 8 mM, about 3 mM to about 8 mM, about 1 mM to about 6 mM, about 2 mM to about 6 mM, about 3 mM to about 6 mM, or about 5 mM.
[0063] To increase the ionic strength, the supersaturated solution may contain a salt. In some embodiments, the salt is sodium chloride. The concentration of the salt is about 100 mM to about 200 mM, about 100 mM to about 175 mM, about 100 mM to about 160 mM, 125 mM to about 200 mM, about 125 mM to about 175 mM, about 125 mM to about 160 mM, 140 mM to about 200 mM, about 140 mM to about 175 mM, or about 140 mM to about 160 mM.
[0064] The temperature of the solution during the coating process is about 40° C. to about 50° C., 42° C. to about 50° C., 44° C. to about 50° C., 46° C. to about 50° C., about 40° C. to about 48° C., 42° C. to about 48° C., 44° C. to about 48° C., 46° C. to about 48° C., 46.5° C. to about 47.5° C., or about 47° C. The implant may be maintained within 0.5° C. of the process temperature.
[0065] HA is a poorly soluble salt, sp is 10 -120 Since the nucleation temperature is on the order of magnitude of 0.01 to 0.01, the "metastability zone" in which controlled heterogeneous nucleation can occur is very narrow. Surprisingly, this range was found to exist, which allows a relatively stable supersaturated solution to deposit crystalline gallium-substituted HA on the activated surface of an orthopedic implant in a controlled manner. In identifying this range, it was observed that low supersaturation concentrations result in slow nucleation rates, while high supersaturation concentrations result in uncontrolled rapid nucleation rates and growth, resulting in heterogeneous growth on the substrate. Without wishing to be bound by theory, it is believed that coating under conditions of extreme supersaturation occurs primarily by homogeneous nucleation and growth.
[0066] Various conditions can enhance solution stability: in some embodiments, the solutions are mixed at room temperature rather than at the temperature at which the deposition process occurs; in some embodiments, a calcium stock solution is added to a phosphate stock solution that includes NaCl and Tris; in some embodiments, the temperature of the stock solution does not fall below room temperature; in some embodiments, the solution is contained in a container with smooth walls rather than rough walls.
[0067] Surprisingly, it was possible to identify a range of supersaturated solution concentrations, or Gibbs free energies, that would allow for controlled gallium-substituted HA crystal growth in a desirable time frame. The solutions used in the gallium-substituted SoDHA process have a dG of about 7 kJ / mol to about 9 kJ / mol, 7 kJ / mol to about 8.8 kJ / mol, 7 kJ / mol to about 8.6 kJ / mol, 7 kJ / mol to about 9.4 kJ / mol, 7 kJ / mol to about 8.2 kJ / mol, 7.2 kJ / mol to about 9 kJ / mol, 7.2 kJ / mol to about 8.8 kJ / mol, 7.2 kJ / mol to about 8.6 kJ / mol, 7.2 kJ / mol to about 9.4 kJ / mol, 7.2 kJ / mol to about 8.2 kJ / mol, 7.4 kJ / mol to about 9 kJ / mol, 7.4 kJ / mol to about 8.8 kJ / mol, 7.4 kJ / mol to about 8.6 ... mol to about 9.4 kJ / mol, 7.4 kJ / mol to about 8.2 kJ / mol, 7.6 kJ / mol to about 9 kJ / mol, 7.6 kJ / mol to about 8.8 kJ / mol, 7.6 kJ / mol to about 8.6 kJ / mol, 7.6 kJ / mol to about 9.4 kJ / mol, 7.6 kJ / mol to about 8.2 kJ / mol, 7.8 kJ / mol to about 9 kJ / mol, 7.8 kJ / mol to about 8.8 kJ / mol, 7.8 kJ / mol to about 8.6 kJ / mol, 7.8 kJ / mol to about 9.4 kJ / mol, 7.8 kJ / mol to about 8.2 kJ / mol, about 8.0 kJ / mol to about 8.4 kJ / mol, about 8 kJ / mol, about 8.2 kJ / mol, or about 8.4 kJ / mol.
[0068] The dG for gallium-free HA formation and the relative supersaturation of the solutions for gallium-free HA for the SoDHA HA process are listed in Table 1. These representative values are not intended to be limiting as possible values with the methods disclosed herein.
[0069] [Table 1]
[0070] As described in detail below, the gallium-substituted hydroxyapatite coating can be formed from a supersaturated solution that remains substantially clear during the coating process due to homogeneous nucleation in the solution. Without wishing to be bound by theory, it is believed that deposition from a substantially clear solution due to homogeneous nucleation plays a role in the gallium-substituted hydroxyapatite coating being deposited with high crystallinity, homogeneous microstructure, and enhanced biocompatibility at predictable coating rates.
[0071] Gallium-substituted HA is a poorly soluble salt with a very narrow "metastable zone" within which controlled heterogeneous nucleation can occur. Surprisingly, it has been possible to identify a range of supersaturation levels and temperatures that allow for controlled heterogeneous nucleation and growth of gallium-substituted hydroxyapatite crystals in a desired time frame. At these supersaturation values, stable nuclei are formed and grow from the active surface, resulting in the gallium-substituted hydroxyapatite coatings described herein.
[0072] The gallium substituted SoDHA process further includes agitating the solution while in contact with the substrate. Too little agitation during mixing of the stock solution can destabilize the solution. High shear agitation during mixing of the stock solution can destabilize the solution. Agitation can be achieved by stirring.
[0073] This process includes reducing the amount of air in contact with the supersaturated solution. In some embodiments, this process can be carried out under inert atmosphere conditions, such as an argon or nitrogen atmosphere. The inert atmosphere limits the dissolution of carbon dioxide into the supersaturated solution, which can change the pH without causing CaP deposition and prevent the use of pH as an internal process monitor. Under such conditions, the resulting gallium-substituted hydroxyapatite coating is substantially carbonate-free.
[0074] This process occurs at a controlled, yet relatively rapid, coating rate. The coating rate can be described in terms of coating mass or coating thickness. For a given number of implants in the coating solution, implants with a large specific surface area (e.g., those coated with porous metallic ingrowth structures) will yield a higher coating weight. However, the coating thickness is largely independent of the specific surface area of the implant. Finally, the coating rate based on mass and the coating rate based on thickness are functions of the total surface area / volume of the coating solution, as can be seen in Figure 11.
[0075] This process is carried out in a range of thicknesses from about 0.01 μm / h to about 10 μm / h, from about 0.01 μm / h to about 5 μm / h, from about 0.01 μm / h to about 4 μm / h, from about 0.01 μm / h to about 3 μm / h, from about 0.01 μm / h to about 2 μm / h, from about 0.01 μm / h to about 1 μm / h, from about 0.1 μm / h to about 10 μm / h, from about 0.1 μm / h to about 5 μm / h, from about 0.1 μm / h to about 4 The gallium substituted HA is deposited at a rate of increasing at about a rate of about 0.1 μm / h, about 0.1 μm / h to about 3 μm / h, about 0.1 μm / h to about 2 μm / h, about 0.1 μm / h to about 1 μm / h, about 0.5 μm / h to about 10 μm / h, about 0.5 μm / h to about 5 μm / h, about 0.5 μm / h to about 4 μm / h, about 0.5 μm / h to about 3 μm / h, about 0.5 μm / h to about 2 μm / h, or about 0.5 μm / h to about 1 μm / h.
[0076] This process produces a rate of approximately 0.005 mg / hr mm 2 ~ approx. 0.09 mg / hr mm 2 , about 0.005mg / hr·mm 2 ~Approx. 0.025mg / hr mm 2 , 0.005mg / hr mm 2 ~Approx. 0.0225mg / hr·mm 2 , 0.005mg / hr mm 2 ~ approx. 0.02 mg / hr mm 2 , 0.005mg / hr mm 2~Approx. 0.0175mg / hr mm 2 , about 0.005mg / hr·mm 2 ~Approx. 0.015mg / hr mm 2 , about 0.0075mg / hr·mm 2 ~ approx. 0.09 mg / hr mm 2 , about 0.0075mg / hr·mm 2 ~Approx. 0.025mg / hr mm 2 , 0.0075mg / hr mm 2 ~Approx. 0.0225mg / hr·mm 2 , 0.0075mg / hr mm 2 ~ approx. 0.02 mg / hr mm 2 , 0.0075mg / hr mm 2 ~Approx. 0.0175mg / hr mm 2 , about 0.0075mg / hr·mm 2 ~Approx. 0.015mg / hr mm 2 , about 0.025mg / hr·mm 2 ~ approx. 0.09 mg / hr mm 2 , about 0.01 mg / hr mm 2 ~Approx. 0.025mg / hr mm 2 , 0.01 mg / hr mm 2 ~Approx. 0.0225mg / hr·mm 2 , 0.01 mg / hr mm 2 ~ approx. 0.02 mg / hr mm 2 , 0.01 mg / hr mm 2 ~Approx. 0.0175mg / hr mm 2 , or approximately 0.01 mg / hr mm 2 ~Approx. 0.025mg / hr mm 2 The HA is deposited on the Gription at a rate of 0.1 μm.
[0077] The coating process can be a "constant composition" or a "variable composition" process.
[0078] In a constant composition process, reactants consumed by the deposition of gallium-substituted hydroxyapatite on the implant are replenished to the deposition solution almost continuously throughout the coating process. The addition of reagents is performed based on the drop in pH corresponding to the precipitation of gallium-substituted hydroxyapatite from the solution. Thus, the amount of process reagent replenished into the deposition solution is a proxy for the amount of gallium-substituted hydroxyapatite deposited on the implant. Without being bound by theory, when gallium is not included in HA, the formula for calculating the composition of the "titrant" (the solution replenished to the deposition solution in response to the change in pH caused by the precipitation of CDHA) can be as follows: TCaNO3 = (Nb)(W CaNO3 )+(10-x)Ceff ·TP=(Nb)(W PO4 )+6 Ceff TNaCl = (Nb)(W NaCl )-(20-2x)Ceff TKOH = (Nb) (W KOH )+(14-2x)Ceff where Ceff is equal to the moles of CaP precipitated per liter of titrant added, x is the nonstoichiometric coefficient of CDHA, Nb=the number of burets adding titrant to the solution, and W is the concentration of reactant in the supersaturated solution.
[0079] In the variable composition process, rather than maintaining a constant high driving force as achieved by the constant composition process, the chemical driving force of deposition is allowed to drop from the initial condition by an amount that maintains a high driving force range. When a lower driving force limit is reached due to depletion of a certain percentage of the coating reagent by precipitation of CaP from the solution, the coating solution is discarded and new coating solution is added to the deposition process vessel. One embodiment of the variable composition process utilizes a quantitative relationship between the change in solution pH and the amount and composition of gallium-substituted hydroxyapatite that precipitates from the coating solution. This relationship can be used to determine when the coating solution should be discarded and replaced with fresh solution, and to determine the predetermined process endpoint when the gallium-substituted hydroxyapatite coating weight has been reached. The amount of buffer is selected to reduce the pH reduction associated with gallium-substituted hydroxyapatite precipitation, while at the same time allowing the pH change to be used for internal process diagnostics. In some embodiments, the pH measurement can be performed intermittently rather than continuously. The coating rate increases with fewer deposition sequences and with more coating sequences. In some embodiments, the coating solution is carbonate-free, which can be useful for using pH as a process monitor or control during coating formation.
[0080] Without wishing to be bound by theory, it is believed that in the absence of gallium, the reaction proceeds according to the stoichiometry shown in Table 2.
[0081] [Table 2]
[0082] Precipitation of calcium phosphate is accompanied by a decrease in calcium and phosphate concentrations and a decrease in pH, as shown in Table 2. These changes in concentration and pH reduce the degree of supersaturation as the reaction proceeds, and are accompanied by a slowing of the deposition rate.
[0083] The relationship between pH and amount of precipitate can be extended to different solution volumes and can be used as a process monitor to ensure that a predictable amount of precipitate is formed.
[0084] The pH of the supersaturated solution can be monitored to determine the extent of coating that has occurred. In some embodiments, the substrate is contacted with the solution until one or more of the calcium concentration, phosphate concentration, and pH are reduced to a predetermined level.
[0085] The nucleation rate, growth rate, and relative driving force of gallium-substituted SoDHA change as gallium-substituted HA is precipitated, but a process was developed that minimizes the change in these values as the deposition proceeds. The process used to coat the implant was a variable composition process. As used herein, a variable composition process refers to a process in which thermodynamic variables are allowed to change over the course of the process. In the variable composition process described herein, the implant may be coated with multiple solution batches, allowing ion concentrations and pH to drop only to a predetermined level during each repeated procedure. To reduce the degree of concentration change, multiple successive depositions were used, with each deposition sequence involving contacting the orthopedic implant with a new solution. pH changes associated with deposition may be reduced by buffering the solution with a buffer (e.g., TRIS buffer).
[0086] In some embodiments, three deposition sequences were performed. For a three-sequence deposition process, the concentration change during each deposition sequence is reduced by two-thirds compared to a single deposition sequence. In some embodiments, only one deposition sequence is performed. In some embodiments, two or three deposition sequences are performed. 1-10, 2-10, 3-10, 1-5, 2-5, or 3-5 deposition sequences may be performed. In some embodiments, the number of deposition sequences employed depends on the ratio of the implant surface area to the volume of the coating vessel. A larger implant surface area / volume ratio may result in more coating sequences and shorter sequences. A smaller surface area / volume ratio may result in fewer sequences and longer duration per sequence. A combination of pH buffering and solution renewal may help minimize changes in thermodynamic driving forces and ensure that the same calcium phosphate phase is created throughout the deposition process.
[0087] The total contact time with the solution deposition composition according to the method of the present invention is typically about 30 minutes or more. The total contact time is preferably about 8 hours or less. More preferably, the biocompatible substrate is subjected to multiple sequence contact times of about 1 minute to about 2 hours, about 1 minute to about 1 hour, about 1 minute to about 30 minutes, about 5 minutes to about 2 hours, about 5 minutes to about 1 hour, about 5 minutes to about 30 minutes, about 2 hours or less, about 1 hour or less, or about 30 minutes or less. In general, longer total contact times and shorter coating sequences result in thicker bioactive hydroxyapatite coatings. Additionally, the contact time depends on the number of bioactive substrates being coated at any one time.
[0088] In some embodiments, the relationship between precipitate weight and pH change is used to monitor the progress of the SoDHA-G process. In additional embodiments, the relationship between precipitate weight and calcium and / or phosphate concentration changes may be used to monitor the progress of the SoDHA-G process. In other embodiments, the process is carried out for a predetermined amount of time and pH, and calcium and phosphate concentrations are not monitored.
[0089] In some embodiments, a supercritical fluid may be employed to dry the SoDHA-G coating. This process involves replacing the water contained in the coating with an organic solvent, followed by extraction with a supercritical fluid. After the formation of the SoDHA-G coating, an organic solvent exchange is performed by immersing the coated article in an organic solvent for a period of time. After replacement of the organic solvent in the coating, the coated article is placed in a container, into which a supercritical fluid is introduced. The container is then depressurized to atmospheric pressure while maintaining a temperature above the critical temperature of the supercritical fluid. In this way, the supercritical fluid is depressurized directly from the supercritical state to gas, thereby avoiding the formation of liquid capillary forces that may cause cracking.
[0090] In some embodiments, the organic solvent is an alcohol. For example, the organic solvent is methanol, ethanol, or isopropanol. In some embodiments, the supercritical fluid is supercritical CO2 (scCO2).
[0091] Additionally, in some embodiments, the SoDHA-G coating can be subjected to hydrothermal reprecipitation conditions. After formation of the SoDHA-G coating, the coating can be heated in a gallium phosphate solution. This hydrothermal treatment can be performed at temperatures ranging from about 50°C to about 350°C, about 60°C to about 350°C, about 70°C to about 350°C, about 80°C to about 350°C, about 50°C to about 150°C, about 60°C to about 150°C, about 70°C to about 150°C, about 80°C to about 150°C, about 50°C to about 99°C, about 60°C to about 99°C, about 70°C to about 99°C, about 80°C to about 99°C, about 50°C to about 95 ... The reaction may be carried out at a temperature of from about 30° C. to about 95° C., from about 70° C. to about 95° C., from about 80° C. to about 95° C., from about 50° C. to about 90° C., from about 60° C. to about 90° C., from about 70° C. to about 90° C., from about 80° C. to about 90° C., from about 50° C. to about 85° C., from about 60° C. to about 85° C., from about 70° C. to about 85° C., from about 80° C. to about 85° C., from about 50° C. to about 80° C., from about 60° C. to about 80° C., or from about 70° C. to about 80° C. The coating may be heated for about 15 minutes to about 24 hours, about 15 minutes to about 4 hours, about 15 minutes to about 3 hours, about 15 minutes to about 2 hours, about 30 minutes to about 24 hours, about 30 minutes to about 4 hours, about 30 minutes to about 3 hours, about 30 minutes to about 2 hours, about 1 hour to about 24 hours, about 1 hour to about 4 hours, about 1 hour to about 3 hours, about 1 hour to about 2 hours, or about 2 hours.
[0092] The methods described herein maximize the amount of material grown on the substrate and minimize the amount of caking on the surface by uniformly precipitating the material in suspension. In addition, these methods provide controlled and predictable deposition rates, produce films with high adhesion and cohesion, and produce uniform microstructures that degrade uniformly without releasing particles. The predictable deposition rates allow the target film thickness to be easily achieved. The methods also provide suitable coatings for porous structures and are suitable for a variety of implant geometries.
[0093] definition As used herein, the relative supersaturation (S) of the product is calculated according to the formula S=[IAP / K sp ] 1 / v where IAP is the ionic activity of the product and K spis the solubility constant of the product and v is the number of ions in the formula of the product.
[0094] As used herein, the Gibbs free energy change (dG) associated with a phase change is expressed by the formula dG=RT / v * ln[IAP / K sp ], where R is the universal gas constant, T is the absolute temperature, and K sp is the solubility constant of the product and v is the number of ions in the formula of the product.
[0095] As used herein, relative supersaturation S is defined as (IAP / Ksp) 1 / v is equal to.
[0096] As used herein, homogeneous precipitation or homogeneous nucleation refers to the nucleation of a solid phase from a supersaturated solution without the involvement of foreign surfaces, resulting in a turbid, supersaturated coating solution.
[0097] As used herein, heterogeneous precipitation or heterogeneous nucleation refers to the nucleation of a solid phase on an impurity phase from a supersaturated solution that is substantially clear during the deposition process.
[0098] As used herein, "octacalcium phosphate" or "OCP" refers to a calcium phosphate having the formula Ca8(HPO4)2(PO4)4.
[0099] As used herein, supersaturation refers to a solution in which a solute is concentrated beyond equilibrium. When the concentration exceeds the saturation point, the solution is said to be supersaturated.
[0100] As used herein, referring to dissolution studies, in vitro refers to in a Tris buffered saline solution at pH 7.4 as described in ASTM F1926. EXAMPLES
[0101] Example 1 - Activation of CoCr by atomic layer deposition of TiO2 films TiO2 films were prepared by atomic layer deposition on CoCr grit-blasted surfaces by Beneq (Helsinki, Finland). The films were made from TiCl4 and H2O precursors. Amorphous films were made at 90°C and crystalline (anatase + rutile) films at 200°C. The films were hydroxide activated (4 hours, 5M NaOH, 60°C) according to the method described in Example 3. Amorphous films of 500, 200, 100, and 50 nm (500A, 200A, 100A, and 50A) and crystalline films of 500 and 200 nm (500°C, 200°C) were evaluated for their ability to form hydroxyapatite coatings by the SoDHA method using the nominal concentrations detailed in Examples 5 and 6.
[0102] The HA coating weights for the samples ranged from about 6 mg to about 8 mg, as shown in Figure 1. Both amorphous and crystalline films were capable of nucleating HA after activation with strong base. Coating experiments showed that deposition occurred as deposited crystalline TiO2, but at a lower rate than observed for NaOH etched amorphous or crystalline TiO2.
[0103] Scanning electron microscope (SEM) images of 200 nm thick activated amorphous films before HA coating are shown in Figure 2. SEM images of 200 nm thick activated crystalline films before HA coating are shown in Figure 3. Characteristic titanate morphology was evident in the amorphous films. Films prepared with thicknesses greater than 100 nm showed interference colors after hydroxide treatment.
[0104] Grazing angle X-ray diffraction (XRD) spectra were obtained for 200 nm and 500 nm thick amorphous and crystalline titanium coatings before and after activation with NaOH. The XRD spectrum of the amorphous film is shown in Figure 4. The XRD spectrum of the crystalline film is shown in Figure 5.
[0105] Example 2 - Electrochemical formation of TiO2 films on CoCr alloys An electrolyte solution of 0.05 M TiCl4 and 0.25 M H2O2 in methanol / water (3 / 1% by volume) mixed solvent was prepared. The pH of this solution was fixed between 0.9 and 1.0. All chemicals were ACS grade. To prepare the electrolyte solution, TiCl4 was slowly added to the solvent followed by H2O2. During the addition of H2O2, a rapid color change from clear to deep orange was observed, indicating the formation of a peroxo complex. After preparation and pH measurement, the electrolyte was stored at about 4°C and the pH was adjusted as required. Electrodeposition was carried out at constant current up to the desired charge density. The temperature was fixed at 0°C by a cryostat. A home-made Labview program (controlling a Xantrex XDC 300-20 power supply) was constructed to record voltage-time curves while controlling the current charge density. The applied charge density was 2.5 C / cm 2 ~40CC / cm 2 The current density was fixed in the range of -50mA / cm 2 ~-50mA / cm 2 It changed between.
[0106] Good film homogeneity was obtained with a 0.05 M TiCl4, 0.5 M H2O2 solution (pH = 0.97) in a methanol / water (3 / 1 vol.%) mixed solvent. Good growth occurred at -1.1 V, 1 h, and 60 °C. Figure 6 shows an SEM image of a titanium coating electrodeposited under these conditions on a CoCrMo substrate.
[0107] Example 3: Activation of the titanium surface Ti6-4 disks, 2.5 centimeters (1 inch) in diameter, coated with a DePuy Gription porous metal coating, were cleaned and activated using the following process: The disks were placed in a container of reverse osmosis (RO) water and alkaline detergent and cleaned with an ultrasonic generator for 2×15 minutes. The disks were then placed in a container of RO water only and cleaned with an ultrasonic generator for 2×15 minutes. Four disks were placed in a 500 mL beaker and 200 mL of 5M NaOH was added. The disks were placed in a secondary containment vessel and a loose cap was placed on the beaker. The temperature of the beaker was set to 60° C. and held for 4 hours. The disks were removed from the beaker and rinsed with RO water using an ultrasonic generator for 4×15 minutes. The disks were placed in a 60° C. oven and dried overnight. No effect of heat treatment of this activation layer on the tendency to promote CaP nucleation and growth was observed in the methods disclosed herein. The examples reported below were carried out without heat treatment of the activated surface. Coating experiments showed that deposition occurred as crystalline titanium, but at a lower rate than observed for NaOH etched amorphous titanium.
[0108] Example 4: Preparation of stock solutions Concentrated and stock solutions for HA coating of 2.5 centimeter (1 inch) diameter disks in 1 L containers were prepared by the following steps.
[0109] A 36 mM Ca solution was prepared. A clean 2 liter bottle was obtained and a magnetic stir bar was placed in the bottle. 8.50194 g of Ca(NO3) was weighed out and placed in the 2 liter bottle. The bottle was purged with argon for 3-5 minutes. 1000 ml of deionized (DI) water (electrical resistance ≥ 18 MΩ) was added to the bottle. The bottle was placed on a stir plate and the contents were stirred until the Ca(NO3) was completely dissolved. The solution was filtered using a 0.22 μm cell culture vacuum filter (Corning, funnel volume 1000 mL; receiver: 90 mm; pore size: 0.22 μm; PES, No.: 431098).
[0110] 40 mM phosphate (P i A clean 2 liter bottle was obtained and a magnetic stir bar was placed in the bottle. 5.444g of KH2PO4 was weighed out and placed in the 2 liter bottle. 19.0387g of Tris and 273.675g of NaCl were weighed out and added to the bottle. The bottle was purged with argon for 3-5 minutes. 898.1mL of 18MΩ or higher DI water was added. Using a manual pipette, 5.8mL of 6N HCl was added to the bottle. The bottle was placed on a stir plate and stirred until the Tris, NaCl, and KH2PO4 were completely dissolved. The final volume of the solution was 1L and the pH of the solution was approximately 8.23 at 25°C. If necessary, the pH can be adjusted to this value using HCl or NaOH. The solution was filtered using a 0.22 μm cell culture vacuum filter (Corning, funnel volume 1000 mL; receiver: 90 mm; pore size: 0.22 μm; PES, No.: 431098).
[0111] 495.3 mL of 2.0787 mM Ca stock solution was prepared. The previously prepared 36 mM calcium solution was placed on a stir plate and stirred for 5 minutes. A clean 1 liter bottle was purged with argon. 28.6 mL of the 36 mM calcium solution was added using a pipette. 466.7 mL of DI water >18 MΩ was added.
[0112] 500mL of 2.5690mM P i A stock solution was prepared. The previously prepared 40 mM phosphate solution was placed on a stir plate and stirred for 5 minutes. A clean 1 liter bottle was purged with argon. 32.112 mL of 40 mM phosphate solution was added using a pipette. 467.888 mL of DI water >18 MΩ was added.
[0113] A 1.7792 mM Ca solution was prepared. The previously prepared 36 mM calcium solution was placed on a stir plate and stirred for 5 minutes. A clean 1 liter bottle was purged with argon. The 36 mM calcium solution was mixed with 18 MΩ DI water to obtain the desired concentration.
[0114] 500mL of 2.2262mM P i A solution was prepared. The previously prepared 40 mM phosphate solution was placed on a stir plate and stirred for 5 minutes. A clean 1 liter bottle was purged with argon. The 40 mM phosphate solution was mixed with 18 MΩ DI water to obtain the desired concentration.
[0115] Gallium / phosphate stock solutions were prepared. First, approximately 2 L of 1.2730 mM phosphate stock solution was prepared by diluting the 40 mM phosphate concentrate as described above. This solution was set aside. Next, a clean 2 L bottle was obtained. Based on the desired wt% Ga of the GaNO3 / phosphate solution, GaNO3 hydrate was weighed out on a balance and this was placed in a second empty clean 2 L bottle. Approximately 200-300 mL of phosphate stock solution was added to the 2 L bottle containing the GaNO3. The bottle containing GaNO3 and 200-300 mL of phosphate stock solution was capped. A cloudy solution was formed by shaking the bottle. This solution was transferred to a clean 500 mL volumetric flask. Phosphate stock solution was added until the volumetric flask's fill line was reached. The contents of the volumetric flask were transferred back into the 2 L bottle that previously contained the solution. The volumetric flask was filled two more times with phosphate stock solution, each time adding this stock solution to the 2 L bottle containing the GaNO3. Another 50 mL of the phosphate stock solution was measured into a graduated cylinder and added to the GaNO3 solution. The 2 L bottle containing this solution was capped and shaken again to double check that all solids had dissolved to form a GaNO3 / phosphate solution.
[0116] Gallium / phosphate salts were prepared with ratios ranging from 5 to 20 wt% Ga. After mixing, the pH was adjusted to 8.3–8.4 by adding microliters of 6N NaOH.
[0117] Example 5: HA coating by solution deposition in a 1 L vessel A 2.5 centimeter (1 inch) diameter porous metal coated titanium coupon was coated. A cover for the 1 L jacket vessel was provided to allow for argon blanket gas during the deposition process. 500 mL of 2.569 mM phosphate stock solution prepared according to Example 4 was added to the 1 L jacket vessel and the vessel was placed on a stir bar plate. The stir bar was operated at 200 rpm. 495.3 mL of 2.0787 mM Ca stock solution prepared according to Example 4 was then poured into the vessel. Due to the volume increase associated with NaCl dilution, the total volume was 1 L at 25° C. The pH of the solution was 7.68 and the calculated dG was 8.242. The relative SS of HA was 22.15 at the beginning of the coating process. A heated water bath was circulated through the jacket vessel to warm the solution to 47° C. The temperature was controlled within 0.5° C. The temperature sensor was calibrated with a NIST traceable RTD. The etched (activated) disk was placed in a fixture so that it was suspended in a 1 L jacketed vessel.
[0118] After coating, the disks were transferred to the first container of DI water and soaked for 1 minute. The disks were then transferred from the first container of DI water to the second container of DI water and soaked for 1 minute. The disks were then transferred from the second container of DI water to the third container of DI water and soaked for 1 minute. After soaking, the disks were transferred to a 6-well tray and dried in a 60°C oven for 60 minutes.
[0119] This process was repeated three times, using fresh solution each time. Each sequence was controlled at a fixed dpH. For larger implant SA / V ratios, shorter coating sequences can be used more frequently. For lower SA / V ratios, fewer sequences with longer duration per sequence can be used. The 941 mm 2 With an SA / V ratio equal to 1000 / L, a total coating time of 5.73 h, 2.35 coating sequences, and a duration per sequence of 2.44 h were used.
[0120] After coating, the disks were transferred to the first container of DI water and soaked for 1 minute. The disks were then transferred from the first container of DI water to the second container of DI water and soaked for 1 minute. The disks were then transferred from the second container of DI water to the third container of DI water and soaked for 1 minute. After soaking, the disks were transferred to a 6-well tray and dried in a 60°C oven for 60 minutes.
[0121] Example 6: Full-scale process validation The nominal process shown in Example 5 was repeated using a "full-scale" system as shown in Figure 7. This full-scale system is designed to coat up to 40 cups or 16 hip stems in one coating run in one or more coating sequences. A series of coating runs were performed at nominal scale and above and below process limits utilizing both standard DePuy TriLock BPS hip stems or hip stems modified to accept 2.5 centimeter (1 inch) diameter coupons (as shown in Figure 17). Process limits were defined as ±2% for Ca and phosphate concentrations and ±0.06 pH units. Coatings were characterized in a variety of ways as described in the Examples.
[0122] Example 7: Use of dpH as a process monitor The pH and precipitate mass were monitored for the SoDHA process described in Example 5 at nominal values, the SoDHA process described in Example 5 at nominal values without Tris, and the SoDHA process described in Example 5 at nominal values with 5 mM Tris. The relationship between pH and precipitate mass can be extended to different solution volumes and buffer strengths using, for example, solution thermodynamics software "Chemist" version 1.0.3 available from Micromath Scientific Software (9202 Litzsinger Road, Saint Louis, Missouri 63144). This relationship between pH change and precipitate mass can be used as a process monitor to confirm that the target precipitate mass is formed. A spreadsheet calculator was constructed based on the relationships summarized in Table 2 to calculate reactant concentrations and activities as a function of the amount of precipitated CaP phase. CaP phases that can be modeled by this calculator include stoichiometric HA, stoichiometric OCP, non-stoichiometric CDHA, and mixtures of HA or CDHA with OCP. For each increment of precipitated CaP phase, the reduced reactant concentrations are entered into Chemist, which calculates the system pH based on the buffer type and level of analysis. Figure 10 shows a plot of predicted pH versus experimental value as a function of total mg of CaP, which is comprised of the following formula: 1) Formula Ca 10-x (PO4) 6-x (HPO4) x (OH) 2-x where x=1.0 or less, a) No TRIS buffer b) With 5mM TRIS buffer 2) A mixture of 80% OCP and 20% CDHA, where x=1.5, with 5 mM TRIS.
[0123] The experimental values for this plot are taken from Example 5.
[0124] Example 8: Characterization of HA coatings Figure 8 shows a scanning electron microscope (SEM) image of a SoDHA HA coated flat titanium disk at a magnification of 15,000x. Figures 9A and 9B show scanning electron microscope (SEM) images of the SoDHA HA coated porous ingrowth structure (Gription) at a magnification of 100x and 400x, respectively. It can be seen that the HA coating was continuous across the disk surface.
[0125] FIG. 11 shows the relationship between deposition rate (mg / hr) and various surface areas (mm 2 ) shows the effect of substrate having a surface area of 100 nm or less. Materials were nominally HA coated in a full-scale deposition system using the nominal conditions described in Example 5. It can be seen that as the surface area increases, the coating rate decreases. This trend can be used to estimate the coating time for a given substrate based on the surface area.
[0126] The density of bulk HA and OCP is approximately 3.1 g / cm 3 A deposition of 7 mg of HA on a flat coupon, nominally prepared according to Example 5, yields a surface area of 5.07 cm 2 , has a thickness of about 7 micrometers, which gives a practical density of about 1.97 g / cm 3 , corresponding to a porosity of approximately 36%.
[0127] Example 9: Characterization of the full-scale process Coatings prepared by the full scale system process according to Example 5 at nominal and process limits met the following properties: Coating weight: 0.08-0.12mg / mm2 per projected surface area 2 Crystalline HA% by Rietveld analysis: over 70% % Amorphous Calcium Phosphate: Below detection limit by DSC (described in Example 11).
[0128] XRD crystallite size parameters: 1 / β (200) 1.63 +- 0.13 1 / β (002) 4.15+-0.10 1 / β (210)1.5+-0.10
[0129] Tensile adhesion measured by ASTM F1147 (grit blasted flat surface): >68MPa, Ca / P ratio: 1.39-1.65
[0130] Figures 12-16 summarize data obtained from full-scale systems evaluated at nominal and process limit conditions. In all cases, error bars are equal to 3 standard deviations of the data.
[0131] Figure 12 shows the Ca / P ratio of HA-coated materials prepared by deposition in a full-scale system according to Example 6 at nominal and process limits. The Ca / P ratio is determined by wet chemical methods. "NIST" refers to the National Institute of Standards and Technology standard hydroxyapatite.
[0132] Figure 13 shows the coating crystallinity measured by XRD for HA-coated materials prepared by deposition in a full-scale system according to Example 6 at nominal and process limits. Crystallinity was measured based on the area under selected diffraction peaks on the coating and compared to the area under the same peaks of highly crystalline NIST standards. The remainder of the material, not reported, was not amorphous, as seen in PSHA deposition. Crystallinity values less than 100% reflect the fine grain size of the film, indicating the fact that the grain boundaries are disrupted, and do not contribute significantly to the diffraction peak area. Amorphous content is measured by DSC.
[0133] Figure 14 shows the percentage of HA as crystalline material out of all crystalline material in HA coated substrates prepared by deposition in a full scale system according to Example 6, in other words a measure of the phase purity of the film.
[0134] FIG. 15 shows the tensile adhesion, measured by ASTM F1147, of HA films prepared by deposition in a full-scale system according to Example 6.
[0135] FIG. 16 shows the shear adhesion, measured by ASTM F1044, of HA films prepared by deposition in a full-scale system according to Example 6.
[0136] Example 10 - Differential Scanning Calorimetry (DSC) Differential scanning calorimetry (DSC) has been previously studied to directly observe and quantitatively measure the thermal recrystallization of the amorphous calcium phosphate phase in plasma sprayed hydroxyapatite materials. It has been reported that the amorphous calcium phosphate recrystallizes through a series of exothermic reactions that occur at various temperatures (within the range of 500°C to 750°C) with different intensities depending on the changes in the plasma spray parameters (e.g., plasma power, feed rate, coating thickness, etc.). The reactions are seen in an exothermic peak at about 500-550°C (crystallization of the hydroxyl-rich amorphous regions in the material), an exothermic peak at about 600-650°C (diffusion of hydroxyl ions to the hydroxyl-depleted regions), and an exothermic peak at about 720-750°C (crystallization of the oxyapatite phase).
[0137] In this example, DSC is used to observe any phase transformations (e.g., recrystallization) that may occur in the hydroxyapatite / calcium phosphate material as a result of impurities and / or amorphous phases upon heating to 725°C.
[0138] Solution deposited SoDHA HA powders prepared according to Example 5 were milled from flat Ti64 proof coupons. Each powder material was tested a minimum of three times using DSC. Peak areas and peak positions (550-710 °C) were measured for all powder samples using Pyris DSC analysis software, and the resulting recrystallization energies (J / g) were calculated.
[0139] A DSC analysis of the SoDHA powder ground from the coated Ti proof coupon is shown in Figure 24. It shows no discernible exothermic peak upon heating.
[0140] The DSC heating curves generated for the SoDHA turnings powder showed no exothermic peaks in the region of interest, i.e., 550°C to 710°C, indicating that there was very little, if any, glassy amorphous phase. Based on the DSC curves, there was less than 2 wt% glassy amorphous material in the tested SoDHA powder. Also, the SoDHA powder analyzed using DSC was gray in color after testing, indicating that a small amount of titanium was removed from the substrate during turning and was oxidized during the DSC test.
[0141] Example 11: First Gallium-Substituted SoDHA Coating Trial Gallium doping studies began by adding gallium ions to the calcium stock solution. The process described in Example 6 was repeated using a gallium / calcium solution instead of a calcium solution. This method destabilized the deposition process, and the gallium found in the films formed by this method was present as a separate phase. Turbidity was observed at various time intervals after the addition of gallium nitrate to the calcium stock solution. This reflected poor coating efficiency, and the gallium detected in the coatings made by this method was present as separate gallium containing particles. A significant amount of loosely bound calcium phosphate precipitate formed on the surface of the desired SoDHA coating.
[0142] Example 12: Gallium-substituted SoDHA coating The process described in Example 6 was repeated, except that the phosphate solution was replaced with a gallium / phosphate solution. 500 mL of calcium solution was added to the gallium / phosphate solution. The pH at the start of the experiment was typically 7.68-7.8.
[0143] Surprisingly, the addition of gallium to a stock solution containing phosphate, TRIS, and NaCl resulted in the incorporation of gallium into the HA lattice. This incorporation is demonstrated by data showing gallium dose-dependent shifts in lattice parameters, crystallite size, and BET surface area, as detailed in Example 9. Gallium-substituted SoDHA coating trials have shown that the addition of Ga salt (Ga(NO3)3) to a Tris-buffered phosphate (Pi) stock solution produced coating efficiencies that allowed for heterogeneous coating of test articles without solution turbidity.
[0144] This process was repeated using a "full-scale" system in the coating vessel shown in Figure 7. In the full-scale system, 40 cups were placed in 64 L of supersaturated solution.
[0145] Example 13: XRD characterization of Ga-substituted HA coatings In this example, gallium substituted HA coatings prepared by deposition in a full-scale system according to Example 12 were characterized by XRD.
[0146] Six coated disks, representing 0 wt %, 5 wt %, 10 wt %, 15 wt % and 20 wt % Ga in the HA lattice added to the coating solution, were analyzed by X-ray diffraction (XRD) spectroscopy.
[0147] The gallium-substituted HA shavings were analyzed by powder XRD (and associated Rietveld and FWHM analyses). Care must be taken when shaving the coated HA material down to the Ti substrate to avoid Ti contamination in the powder. As the amount of powder was relatively small (4-9 mg) for each coated flat substrate, six substrates were shaved to obtain approximately 15-20 mg of gallium-substituted HA powder. XRD scans of the coated gallium-substituted HA disks were measured with the background, which was then calculated and removed using Panalytical X'Pert software.
[0148] The XRD plot overlay is shown in Figure 18, which shows that the gallium substituted HA coating is phase pure within the detection limits of the X-ray instrument (no XRD peaks associated with second phases are observed) and that the HA coating is highly textured in the 001 crystallographic direction.
[0149] For the 20 wt% gallium sample, Table 3 shows the 2θ° values along with the relative intensity of various peaks measured using XRD on the gallium substituted HA sample. The background was calculated and removed using Panalytical X'Pert software. The relative intensity of each peak was calculated as a percentage of the most intense peak in the scan. Note that not all peaks published in the NIST SRM data are observed in the coated gallium substituted HA coating because the coating has a preferred orientation. Also note that the 100% intensity peak in the randomly oriented HA powder is the (211) peak at 31.70° 2θ, while the 100% intensity peak observed in the coated gallium substituted HA disk is the (002) peak at approximately 25.95° 2θ. The increased intensity of the (002) peak indicates crystals that are highly oriented in the 001 direction.
[0150] [Table 3]
[0151] As shown in Figure 18, a reduction in the HA crystalline phase content was observed with increasing Ga wt%. This can be seen from the decrease in peak intensity in the XRD traces as the Ga wt% increases. It can also be seen that as Ga increases in the gallium substituted SoDHA coatings, a regular shift of the (002) peak is observed at higher 2θ angles (corresponding to a decrease in d-spacing). Table 4 shows the average HA(002) peak positions measured for coated disks formed with solutions of various gallium concentrations. The gradual decrease in lattice d-spacing is due to the larger Ca2+ Instead of the Ga ion (0.99 Å), 3+ This is consistent with the ion (0.62 Å) substituting the CA1 lattice site in the hyaluronan lattice.
[0152] [Table 4]
[0153] Analysis of the (002) peak shift confirms the observations of the coated disks, i.e., the (002) d-spacing decreases with increasing Ga weight % in the SoDHA coating, which is consistent with the increasing Ga substitution of Ca1 sites in the HA lattice. These data indicate that gallium has been successfully substituted into the hydroxyapatite lattice.
[0154] Example 14 - Additional Gallium-Substituted HA Coating Results The weight percent of gallium in the SoDHA lattice was measured for gallium substituted HA coatings formed from solutions having 5 wt%, 10 wt%, and 20 wt% gallium nitrate according to Example 12. The results are shown in FIG.
[0155] The results presented in Table 5 show the crystalline hydroxyapatite, amorphous, and disordered crystalline component contents in gallium-substituted hydroxyapatite samples formed from solutions with various Ga contents according to Example 12.
[0156] [Table 5]
[0157] As shown in Table 6, FWHM analysis shows that the average crystallite size in the (200), (002) and (210) directions is significantly reduced when Ga is introduced into the HA lattice. The average crystallite sizes in the (200), (002) and (210) directions are shown in Table 7. It can be seen that the crystallite size in the (200) direction is too small to measure after 10 wt% Ga addition. Without being bound by theory, it is believed that the reduction in crystallite size in the HA coating is the main reason for the decrease in the calculated crystallinity by Rietveld analysis due to the peak broadening associated with very small crystallite sizes.
[0158] [Table 6]
[0159] [Table 7]
[0160] Example 15 - FTIR characterization An FTIR spectrum was obtained of the gallium substituted SoDHA HA formed in Example 12 and is shown in FIG.
[0161] Example 16 - Dissolution The dissolution rates of the gallium substituted SoDHA coating formed in Example 12 and the NIST hydroxyapatite reference material were measured. This was measured by placing the samples in a Tris buffered saline solution at pH 7.4 and measuring the change in calcium concentration. Figure 22 shows the dissolution results for the gallium substituted SoDHA coating and Figure 23 shows the dissolution results for the NIST standard. While the NIST sample stopped releasing calcium after less than 2 hours, the gallium substituted SoDHA sample released calcium over more than 20 hours with no clear dissolution plateau.
[0162] Example 17 - Dog Study The purpose of this preclinical study was to measure the bone response to gallium-doped hydroxyapatite coatings on orthopedic implants. Implants were placed in either in-line or gap junctions in the trabecular bone of dogs. Tissues were harvested 6 weeks after surgery. Outcome measurements were implant fixation (measured by mechanical destructive testing), bone surface growth and bone ingrowth (measured by backscatter scanning electron microscopy and histology), and new bone fill within the gap (measured by histology). Destructive histology was included as a secondary method to report the tissue response around the implant and to quantify the % remaining gallium-substituted HA coating.
[0163] Implants were placed into cylindrical defects created in the cancellous bone of large, skeletally mature, mixed bred hound dogs. Dogs were chosen as the model for the study because canine bone structure is very similar to human bone. The implant sites selected for this study provide a large cancellous bone volume. A total of five dogs participated in the study. Five laboratory-bred hound dogs (22-27 kg) were used in the study. Skeletal maturity was confirmed by radiographic evidence of growth plate closure. The dogs were acclimated for a period of at least two weeks prior to surgery. The experimental animals were housed in a single facility for the entire duration of the study. The five dogs appeared healthy on arrival, and preoperative examination by the attending veterinarian revealed no obvious abnormalities.
[0164] The effect of these coatings on implant fixation was evaluated in both 1 mm gap and in-line or precision joints, which represent the range of implant-to-host osteosynthesis scenarios encountered in total joint arthroplasty in humans. Four defects per animal were created in the cancellous bone to create side-by-side areas of in-line and radial 1 mm gap joints between the porous coated surface of the 6 mm diameter implant and the host bone. These defects were created bilaterally in the proximal humerus, distal femur, and proximal tibia. Two additional defects per animal were created in the cancellous bone distal to the first defect in both humeri to place a single implant with a 1 mm radial gap joint. This was done because of the limited number of anatomical sites suitable for side-by-side implant placement in this model.
[0165] The following test articles were used: Gription™ implants with SoDHA HA coating (HA version of SoDHA coating) - 10mm and 11mm in length, 6mm diameter (in-line implant) or 8mm diameter (1mm gap implant).
[0166] Gription™ with Gallium-substituted SoDHA HA coating (Gallium-substituted HA version of the SoDHA coating) - 10mm and 11mm long, 6mm diameter (in-line implant) or 8mm diameter (1mm gap implant).
[0167] All experimental procedures in this study were reviewed and approved by the local institutional animal care and use committee (protocol no. 2008A0083-R2, approved June 23, 2014). Animals in this study were handled and maintained in accordance with the requirements of the Animal Welfare Act.
[0168] Dogs were housed in cages with approximately 24 square feet of floor space and equipped with a stainless steel runway. The floor was elevated with a removable vinyl-coated expanded mesh floor for sanitation. Cages were hosed down at least once daily, and more frequently as needed, to prevent the accumulation of feces. Animals remained within the cage during daily cleanings, and measures were taken to keep animals dry. All cleaning or disinfecting agents used in the enclosure were designated USDA "food safe" and approved for use by the attending veterinarian.
[0169] Sanitation of cages and holding rooms was performed every 2-6 weeks (frequency based on biological monitoring) using a pressure washer or other approved agent. Animals were removed from their cages during sanitation procedures to prevent exposure to hot water or disinfectant solutions. If a disinfectant solution was used, all surfaces in the cages and rooms were thoroughly rinsed.
[0170] Dogs were fed appropriate amounts for body weight and activity level according to USDA and National Research Council regulations. All food was presented in stainless steel bowls. All animals not scheduled for surgical procedures were fed at least once daily. Animals scheduled for surgical procedures were fasted for 12-24 hours prior to surgery. There were no known contaminants that would be deemed to interfere with the validity of this study.
[0171] Animals in this study had free access to fresh, clean water. There were no known contaminants that would be considered to interfere with the validity of the study.
[0172] The animals received acepromazine (0.05 mg / kg IM) as a preoperative tranquilizer, and general anesthesia was induced with an intravenous injection of ketamine hydrochloride and diazepam. The dogs were intubated and anesthesia was maintained with inhalation of a mixture of isoflurane in oxygen. The surgical surface was assessed by monitoring pulse, heart rate, respiration, and reflexes (eye, pinch). An intravenous catheter was placed in the brachiocephalic vein and perioperative antibiotics (cefazolin) were administered. Maintenance doses of sterile isotonic fluid (LRS or similar) were administered throughout the procedure. All four limbs were prepped for surgery in sequence and the hair was clipped (forelimbs from elbow to proximal scapula, hind limbs from knee to hip). After initial skin preparation with surgical antiseptic, the dogs were transferred to the operating room and placed in a lateral decubitus position. The top front and back limbs were suspended from an IV stand by tape and the lateral aspects of the humerus and femur were scrubbed with a combination of surgical antiseptic (povidone-iodine or chlorhexidine) and alcohol. The surgical site was isolated with a sterile drape and an adhesive antimicrobial incise drape (Ioban 2, available from 3M, St. Paul, Minn.). Small incisions (<20 mm in length) were made on the lateral aspect of the proximal humerus and the distal lateral aspect of the femur to expose the metaphyseal region of both bones. A drill was used to place the guidewire and fluoroscopy was used to ensure that the guidewire was pointing into the trabecular bone at a 90 degree angle to the cortical surface. A tubular drill bit was then used to drill a hole 6 mm in diameter and 20 mm in total length. The proximal half of the drill hole was further enlarged with a drill to a final diameter of 8 mm. The same procedure was used on both the humerus and femur. A total of four implants were placed. A 6 mm implant was inserted into each defect and completely impacted into the distal half of the drill hole using a custom impactor. An 8 mm implant (6 mm core diameter implant with 8 mm washers on each end) was then placed into the drill hole and fully seated. Thus, each bone defect contained one implant in-line bonded at the implant-bone interface and one implant with a 1 mm circumferential gap between the gallium-substituted HA coated implant and the surrounding bone. After placement of the humeral and femoral implants, the skin incision was closed with subcuticular absorbable sutures (Monocryl, PDS II or similar) and the repair was reinforced with skin staples.The wound was covered with adhesive dressing, the dog was turned over, the skin was scrubbed, and the implants were placed in exactly the same procedure as described for the first side. After placement of the humeral and femoral implants, the skin on the medial aspect of the right and left tibia was scrubbed with a combination of surgical antiseptic (povidone-iodine or chlorhexidine) and alcohol. The surgical site was isolated with a sterile drape and an adhesive antimicrobial incise drape (Ioban 2, available from 3M, St. Paul, Minn.). A small incision (<20 mm in length) was made in the metaphysis of the medial tibia. A guidewire was placed as before, and a single drill hole (6 mm in diameter, 10 mm in length) was made in the cancellous bone perpendicular to the medial tibial cortex. A 6 mm implant was placed in the in-line junction, and the subcutaneous and skin were closed as described before. After surgery, the dog was closely monitored until it recovered from anesthesia. Once the dog's swallowing reflex had returned, the endotracheal tube was removed. At this point, intravenous catheters were removed if present. Postoperative pain management included an opiate painkiller (buprenorphine) every 6-12 hours for 3 days after surgery. A nonsteroidal anti-inflammatory drug (carprofen or meloxicam) was administered the first postoperative morning and continued for 7-10 days after surgery. Dogs were monitored by study team members at least twice daily, and staples were removed 10-14 days after surgery.
[0173] At the designated time points, dogs were euthanized by intravenous overdose of sodium pentobarbital and death was confirmed by cessation of cardiorespiratory activity. The left and right proximal humeri, distal femora, and proximal tibia surgical sites were exposed, photographed, and sectioned with a necropsy saw to preserve the integrity of the implant and surrounding bone. Close-up radiographs were taken in two planes to examine the bone response around each implant. Bone specimens were examined by micro-CT (30 μm resolution) and then shipped on ice to DePuy Synthes Joint Replacement (Warsaw, Indiana) by next-day arrival mail. After receipt at the Warsaw office, specimens were sectioned perpendicular to the implant axis, one half was used for mechanical testing at DePuy Synthes, and the other half was returned to Ohio State University in 70% alcohol for decalcified histology.
[0174] Example 18 - Histological Results Decalcified histology was performed on fixed specimens of the implant-bone interface processed with a Technovit 7200 and cut perpendicular to the implant axis with a diamond band saw. A custom-aligned jig was used to ensure precision of implant placement and cutting. Two sections were prepared from each implant. Each section was milled to a final thickness of 100–150 μm, polished, and the surface was stained with Goldner trichrome. The nature and degree of bone contact, fibrous tissue formation, and periprosthetic inflammation were described.
[0175] The embedded blocks containing the implant-bone interface were polished, coated with graphite, and examined using a backscattered SEM. Grey-scale images were taken around the entire circumference of the implant, and the fractional percentage of bone apposition on the implant surface and bone ingrowth within the implant surface were measured using semi-automated image analysis (Bioquant Osteo II). The linear extent (%) of the remaining HA coating on the implant surface was measured.
[0176] Histomorphometric analysis was performed on each slide blinded to the treatment. Low magnification digital images were taken of each section, including each implant interstitial space and additional amounts of surrounding tissue. Static histomorphometric analysis was performed to determine the % bone ingrowth to the implant surface, % bone within the porous coating, and % bone within the interstitial area. In-growth was measured as % total void. Additional parameters evaluated included average coating thickness. Results averaged over the various specimens for SoDHA HA and gallium-substituted SoDHA HA interstitial implants are shown in Table 8. Data showing the benefit of Ga addition to bone ingrowth are also shown in the graph of FIG. 25.
[0177] [Table 8]
[0178] Histological data shows that the Gription™ SoDHA-Gallium implant performs significantly (>2-fold) better than both Gription™ SoDHA implants on the proximal humerus. Based on the absence of inflammation, particles, and radiolucency around the implant, there are no adverse reactions to the implants or test HA coatings detected at any of the implant sites 6 weeks after implantation.
[0179] Example 19 - Organic Solvent Exchange and Supercritical CO2 Solvent Extraction After forming the SoDHA-G coating as described in Example 12, the coated Gription™ and grit blasted flat coupons were rinsed with DI water. The remaining aqueous solvent was exchanged with ethanol three times in a soaking process. The soaking times performed in the study were 1 hour and 20 hours. After the organic solvent exchange with ethanol, the coupons were placed on a rack and inserted into a 100 mL stainless steel container. The coupons were covered with ethanol and the upper end cap of the container was closed. The CO2 flow was from the top of the container to the bottom. The container was pressurized to 10 MPa (100 bar) with liquid CO2 and the liquid ethanol was replaced with liquid CO2 at room temperature with a gaseous CO2 flow rate of about 2 liters / min. The replacement time was about 1 / 2 hour. After the ethanol was replaced, the container was heated to 38°C and dried with supercritical CO2 at a gas flow rate of 5 liters / min for 4 hours. After the allotted drying time of 4 hours, the vessel was depressurized to atmospheric pressure while maintaining the temperature above the CO2 critical temperature of 32° C. This depressurization was accomplished with a gas flow rate of approximately 1 liter / min and took approximately ½ hour.
[0180] The surface morphology of treated (Figure 26A) and untreated (Figure 26B) films was examined by scanning electron microscopy. The scCO2 treatment significantly reduced cracking of the SoDHA-G coating compared to normal drying.
[0181] Example 20 - Reprecipitation of SoDHA-G by hot water treatment The SoDHA-G coated coupons prepared according to Example 12 were quickly transferred from the DI water into a vial containing 15 mL of 40 mM phosphate-Ga(Pi) syrup solution prepared according to Example 4 or 15 mL of 2.2262 mM phosphate-Ga(Pi) stock solution prepared according to Example 4. The vial was sealed with a cap. The hot water treatment of the SoDHA-G films was carried out at 70° C. or 90° C. for 2 hours. After the hot water treatment, the SoDHA-G coated coupons were rinsed with excess DI water for 1 minute and dried in an oven at 60° C. for 1 hour.
[0182] The surface morphology of SoDHA-G and hydrothermally treated SoDHA-G (SoDHA-G-HT) films was examined by scanning electron microscopy (FE-SEM, Quanta 600 F). Scanning electron microscopy images of SoDHA-G are shown in FIG. 27. Scanning electron microscopy images of SoDHA-G-HT hydrothermally treated at 70° C. for 2 h for films treated with phosphate-Ga stock solution and phosphate-Ga syrup solution are shown in FIG. 28A and FIG. 28B, respectively. Scanning electron microscopy images of SoDHA-G-HT hydrothermally treated at 90° C. for 1 h for films treated with phosphate-Ga stock solution and phosphate-Ga syrup solution are shown in FIG. 29A and FIG. 29B, respectively. Scanning electron microscopy images of SoDHA-G-HT hydrothermally treated at 90° C. for 2 h for films treated with phosphate-Ga stock solution and phosphate-Ga syrup solution are shown in FIG. 30A and FIG. 30B, respectively. Figures 26-30B reveal the improvement of cracking by optimizing the temperature and time of hydrothermal treatment. X-ray diffraction measurements (Philips Analytical) identified the phase composition of SoDHA and SoDHA-HT films using Cu Kα radiation at 45 kV and 40 mA. As shown in Figure 31, X-ray diffraction patterns of SoDHA, SoDHA-G, and SoDHA-G HT (hydrothermally treated in Pi-Ga stock solution at 90 °C for 2 h) were collected from 4° to 60° (2θ) at 0.02° intervals and 0.01° / s. The XRD results show that the (002) peak of hydroxyapatite does not shift after hydrothermal treatment, indicating no measurable Ga loss from the lattice.
[0183] Five SoDHA-G coated Gription™ coupons prepared according to Example 12 were quickly transferred from the DI water into a vial containing 250 mL of 2.2262 mM phosphate-Ga(Pi) stock solution prepared according to Example 4. Ten SoDHA-G coated Gription™ coupons prepared according to Example 12 were quickly transferred from the DI water into a vial containing 250 mL of 40 mM phosphate-Ga(Pi) syrup solution prepared according to Example 4. The vial was sealed with a cap. The hot water treatment of the SoDHA-G film was carried out at 90° C. for 2 hours. After the hot water treatment, the SoDHA-G coated Gription™ coupons were rinsed with excess DI water for 1 minute and dried in an oven at 60° C. for 1 hour.
[0184] The hydrothermally treated coatings and the coatings that were dried normally (without hydrothermal treatment) were dissolved in 0.1 M hydrochloric acid, and the solutions were analyzed for gallium by inductively coupled plasma (ICP) atomic emission spectrometry. The gallium contents of the coatings without thermal treatment and those treated with the phosphate-Ga stock solution were 2.58 and 2.71 wt%, respectively. However, unexpectedly, the gallium content of the coatings hydrothermally treated with the phosphate-Ga syrup solution increased to 5.67 wt%, revealing that hydrothermal treatment with a highly concentrated gallium-containing solution was an effective method to increase the gallium content of hydroxyapatite coatings.
[0185] Example 21 - Crack quantification The crack-improving effect of post-treatment according to Examples 19 and 20 was quantified using image analysis. This was done by measuring the number of crack intersections on a given horizontal grid. Images were taken with an mFEI Quanta 600 F SEM at 1000x magnification, which was analyzed using Axio Vision software (AxioVision SE64, release 4.9.1.0, sold by Carl Zeiss Microscopy GmbH) and 25 horizontal grid lines (193.5 μm long and 6 μm apart vertically) were placed across most of the image. The intersections of the cracks and grid lines in the image were then manually marked. The intersections were manually selected by the operator to eliminate software-induced errors. The number of intersections in a given area was used as a quantitative measurement of the degree of surface cracking of the SoDHA-G coating. A representative image illustrating this method is shown in FIG. 32.
[0186] The SoDHA-G coating on the grit blasted coupons subjected to normal drying at 60°C and no post-treatment step had more than 600 nodes, while the hot water treated SoDHA-G coating had 200-400 crack nodes. The SoDHA-G with optimized hot water treatment parameters had minimal cracking, with less than 200 nodes. The number of crack nodes and node density for representative normal drying and post-treated coatings are shown in Table 9.
[0187] [Table 9]
[0188] While the invention has been illustrated and described in detail in the drawings and foregoing description, it is understood that such illustration and description is merely illustrative in nature and should not be regarded as restrictive, that merely representative embodiments have been shown and described, and that all changes and modifications that come within the spirit of the invention are desired to be protected.
[0189] There are several advantages of the present invention based on the various structures of the gallium-substituted HA coatings described herein. It is noted that each alternative embodiment of the coating of the present invention may not have all of the features described, but still benefit from at least some of the advantages of such features. Those skilled in the art will be readily able to independently implement calcium phosphate coatings incorporating one or more features of the present invention that are within the spirit and scope of the present invention as defined in the claims.
[0190] [Embodiment] (1) An orthopedic implant comprising a metal surface and a hydroxyapatite layer deposited on at least a portion of said metal surface, said hydroxyapatite layer including gallium ions therein, said hydroxyapatite layer being crystalline. (2) The orthopedic implant of claim 1, wherein the hydroxyapatite layer, when subjected to XRD, produces a (002) XRD peak that is shifted by about 0.001° 2θ to about 0.5° 2θ relative to the (002) XRD peak of crystalline hydroxyapatite without gallium. (3) The orthopedic implant of claim 1, wherein the hydroxyapatite layer, when subjected to XRD, produces a (002) XRD peak corresponding to a d-spacing shift of about 0.001 Å to about 0.05 Å relative to the (002) XRD peak of crystalline hydroxyapatite without gallium. (4) The orthopedic implant of claim 1, wherein the hydroxyapatite layer has an average crystallite size of less than about 75 nm. (5) The orthopedic implant of claim 1, wherein the hydroxyapatite layer has an average crystallite size in the
[0001] direction of less than about 75 nm.
[0191] (6) The orthopedic implant of claim 1, wherein the hydroxyapatite layer, upon XRD, produces a (002) XRD peak and a (112) XRD peak, the (002) XRD peak having an intensity 1.5 to 10 times that of the (112) XRD peak. (7) The orthopedic implant of embodiment 1, wherein the hydroxyapatite layer continuously dissolves in vitro over a period of more than 24 hours. (8) The orthopedic implant of claim 1, wherein the hydroxyapatite layer comprises about 0% to about 5% by weight of carbonate. (9) The orthopedic implant of claim 1, wherein the gallium ions comprise about 0.01% to about 10% by weight of the hydroxyapatite layer. (10) The orthopedic implant of claim 1, wherein the hydroxyapatite layer is in contact with the metal surface.
[0192] 11. The orthopedic implant of claim 10, wherein the metal surface comprises titanate. (12) The orthopedic implant of claim 11, wherein the metal surface comprises sodium titanate. (13) The orthopedic implant of claim 1, wherein the metal surface is a hydroxide-treated titanium surface. (14) The orthopedic implant of claim 1, wherein the hydroxyapatite layer has a crystallinity of about 70% to about 100% by weight. (15) The orthopedic implant of claim 1, wherein the hydroxyapatite layer has a phase purity of crystalline hydroxyapatite of greater than 90%.
[0193] (16) The hydroxyapatite layer is about 15 m 2 / g~about 200m 2 2. The orthopedic implant of embodiment 1, having a surface area of 1.0 μm / g. (17) An osteoinductive composition comprising hydroxyapatite, the hydroxyapatite including gallium ions therein, the hydroxyapatite being crystalline, and the hydroxyapatite, upon XRD, producing a (002) XRD peak that is shifted by about 0.001° 2θ to about 2° 2θ compared to the (002) XRD peak of crystalline hydroxyapatite not containing gallium. (18) The osteoinductive composition of embodiment 17, wherein the hydroxyapatite has an average crystallite size in the
[0001] direction of less than about 75 nm. (19) A method for forming a hydroxyapatite coating, said method comprising the step of contacting a metal surface with a supersaturated solution comprising calcium ions, phosphate ions, and gallium ions, wherein the pH of the solution fluctuates by less than 0.2 pH units / hour during said contacting step. 20. The method of claim 19, further comprising mixing a first solution comprising gallium ions and phosphate ions with a second solution comprising calcium ions to form a supersaturated solution; and contacting a metal surface with the supersaturated solution.
[0194] 21. The method of claim 19, wherein the hydroxyapatite coating is formed primarily by heterogeneous nucleation, whereby the supersaturated solution remains free of visible turbidity during the contacting step. (22) The method of embodiment 19, wherein at least two deposition sequences are employed. (23) The hydroxyapatite coating has a rate per unit surface area of about 0.01 mg / hr mm 2 ~Approx. 0.03mg / hr mm 2 20. The method of embodiment 19, wherein the compound is formed from (24) The method according to embodiment 19, wherein the initial pH of the supersaturated solution is about 7.5 to about 7.9, and the initial temperature of the supersaturated solution is about 38° C. to about 60° C. 25. The method of claim 19, wherein the metal surface is a metal oxide surface.
[0195] (26) The method according to embodiment 19, wherein the calcium concentration of the supersaturated solution is about 1.4 mM to about 1.8 mM. (27) The method according to embodiment 19, wherein the phosphate concentration of the supersaturated solution is from about 2 mM to about 2.3 mM. 28. The method of claim 19, further comprising removing the metal surface from the supersaturated solution after about 0.5 hours to about 12 hours. 29. The method of claim 19, further comprising heating the coating in a phosphate solution to reduce surface cracking. 30. The method of claim 19, further comprising heating the coating in a gallium-containing solution to increase the gallium content of the coating to up to 15% by weight.
[0196] 31. The method of claim 19, further comprising contacting the coating with a supercritical fluid to reduce surface cracking.
Claims
1. 1. An orthopedic implant comprising: a metal surface; and a hydroxyapatite layer deposited on at least a portion of said metal surface, said hydroxyapatite layer including gallium ions therein; The orthopedic implant, wherein the hydroxyapatite layer, upon XRD, produces a (002) XRD peak and a (112) XRD peak, the (002) XRD peak having an intensity between 1.5 and 10 times that of the (112) XRD peak.
2. 2. The orthopedic implant of claim 1, wherein the hydroxyapatite layer, when subjected to XRD, produces a (002) XRD peak that is shifted by about 0.001 degrees 2θ to about 0.5 degrees 2θ compared to the (002) XRD peak of crystalline hydroxyapatite without gallium.
3. 10. The orthopedic implant of claim 1, wherein the hydroxyapatite layer, when subjected to XRD, produces a short lattice d-spacing of the (002) XRD peak, corresponding to a d-spacing shift of about 0.001 Å to about 0.05 Å compared to the lattice d-spacing of the (002) XRD peak of crystalline hydroxyapatite without gallium.
4. The orthopedic implant of claim 1, wherein the hydroxyapatite layer, upon XRD, produces a short (002) XRD peak lattice d-spacing that corresponds to a d-spacing shift of about 0.001 Å to 0.0158 Å compared to the lattice d-spacing of the (002) XRD peak of crystalline hydroxyapatite that does not contain gallium.
5. The orthopedic implant of claim 1, wherein the hydroxyapatite layer, upon XRD, produces a short (002) XRD peak lattice d-spacing that corresponds to a d-spacing shift of 0.0015 Å to about 0.0158 Å compared to the lattice d-spacing of the (002) XRD peak of crystalline hydroxyapatite that does not contain gallium.
6. The orthopedic implant of claim 1, wherein the hydroxyapatite layer, upon XRD, produces a lattice d-spacing of the (002) XRD peak of 3.4348 Å to 3.4491 Å.
7. The orthopedic implant of claim 1 , wherein the hydroxyapatite layer has an average crystallite size of less than about 75 nm.
8. 2. The orthopedic implant of claim 1, wherein the hydroxyapatite layer has an average crystallite size in the [001] direction of less than about 75 nm.
9. 10. The orthopedic implant of claim 1, wherein the hydroxyapatite layer continuously dissolves in vitro for greater than 24 hours.
10. The orthopedic implant of claim 1 , wherein the hydroxyapatite layer comprises from about 0% to about 5% by weight carbonate.
11. The orthopedic implant of claim 1 , wherein the gallium ions comprise from about 0.01% to about 10% by weight of the hydroxyapatite layer.
12. The orthopedic implant of claim 1 , wherein the hydroxyapatite layer is in contact with the metal surface.
13. The orthopedic implant of claim 12 , wherein the metal surface comprises a titanate.
14. The orthopedic implant of claim 13 , wherein the metal surface comprises sodium titanate.
15. The orthopaedic implant of claim 1 , wherein the metal surface is a hydroxide treated titanium surface.
16. The orthopedic implant of claim 1 , wherein the hydroxyapatite layer is crystalline.
17. 10. The orthopedic implant of claim 1, wherein the hydroxyapatite layer has a phase purity of greater than 90% crystalline hydroxyapatite.
18. The hydroxyapatite layer is about 15 m 2 / g ~ approx. 200m 2 13. The orthopedic implant of claim 1 having a surface area of 1 / g.
Citation Information
Patent Citations
Orthopedic implant having crystalline gallium-containing hydroxyapatite coating and methods for producing the same