Method for recovering valuable materials from lithium-ion secondary batteries

A multi-step process with heat treatment, classification, and dual magnetic separation enhances cobalt and nickel recovery from lithium ion batteries with low grades, addressing the inefficiencies of existing methods by achieving high recovery rates.

JP7571367B2Active Publication Date: 2024-10-23DOWA ECO SYST CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023179529
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-10-25
Filing Date
2023-10-18
Publication Date
2024-10-23
Estimated Expiration
2043-10-18

AI Technical Summary

Technical Problem

Existing methods for recovering cobalt and nickel from lithium ion secondary batteries with low cobalt and nickel grades result in low recovery rates due to the formation of agglomerates and small particle sizes, making them non-magnetic in wet magnetic separation processes.

Method used

A multi-step process involving heat treatment, classification, and dual magnetic separation stages with specific parameters to enhance the recovery of cobalt and nickel, including a first classification at 600 μm to 2,400 μm, a second classification at 25 μm to 1,700 μm, and high-gradient wet magnetic separation with controlled magnetic flux densities to recover these metals effectively.

Benefits of technology

The method achieves a high recovery rate of cobalt and nickel even when their grades are low, improving the overall efficiency of material recovery from lithium ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571367000003
    Figure 0007571367000003
  • Figure 0007571367000004
    Figure 0007571367000004
  • Figure 0007571367000005
    Figure 0007571367000005
Patent Text Reader

Abstract

To provide a method for recovering valuable materials from lithium ion secondary batteries, capable of achieving a high recovery rate of cobalt and nickel even if the grade of cobalt and nickel in a magnetic separation object is low.SOLUTION: A method for recovering valuable materials from lithium ion secondary batteries includes: a heat treatment step in which a heat treated material is obtained by subjecting the lithium ion secondary batteries to heat treatment; a first classification step in which a coarse grain product 1 and a fine grain product are obtained by classifying a crushed material that is obtained by crushing the heat treated material; a second classification step in which a coarse grain product 2 and a microfine grain product are obtained by classifying a ground material, which is obtained by grinding the fine grain product, at a classification point that is smaller than the classification point in the first classification step; a first magnetic separation step in which a magnetically attracted material 1 and a magnetically non-attracted material 1 are obtained by magnetically separating the microfine grain product obtained in the second classification step; a second magnetic separation step in which a magnetically attracted material 2 and a magnetically non-attracted material 2 are obtained by magnetically separating the magnetically non-attracted material 1 obtained in the first magnetic separation step; and a recovery step in which valuable materials are recovered from the magnetically attracted material 1 and the magnetically attracted material 2.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for recovering valuable materials from lithium ion secondary batteries. [Background technology]

[0002] Lithium-ion secondary batteries are lighter, have a higher capacity, and have a higher electromotive force than conventional lead-acid batteries and nickel-cadmium secondary batteries, and are used as secondary batteries in personal computers, electric vehicles, portable devices, etc. For example, valuable materials such as cobalt and nickel are mixed in the positive electrode of a lithium-ion secondary battery to form lithium cobalt oxide (LiCoO 2 ), ternary cathode material (LiNi x Co y Mn z O 2 It is used as (x+y+z=1) etc.

[0003] Since the use of lithium-ion secondary batteries is expected to continue to expand in the future, from the viewpoint of resource recycling, it is desirable to recover valuable materials such as lithium from lithium-ion secondary batteries that are discarded due to defective products generated during the manufacturing process, devices used, or the end of the battery life, etc. When recovering valuable materials such as lithium from lithium-ion secondary batteries, it is important to separate and recover the various metals or impurities used in the lithium-ion secondary batteries in order to increase the value of the recovered materials.

[0004] As a method for recovering valuable materials such as cobalt and nickel from crushed products of heat-treated lithium-ion secondary batteries, for example, a method for recovering valuable materials from lithium-ion secondary batteries has been proposed, in which the heat-treated products obtained by heat-treating lithium-ion secondary batteries are crushed and classified to obtain fine particles, and then the fine particles are subjected to wet magnetic separation (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6948481 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the method for recovering valuable materials described in Patent Document 1 above was unable to achieve a high recovery rate when the cobalt and nickel grades were low. That is, in a fine product (hereinafter sometimes referred to as "black mass") with low cobalt and nickel grades (the combined value of cobalt and nickel grades is 30% or less), the formation of agglomerates of cobalt metal particles and nickel metal particles is difficult to progress, and since the average particle size of these particles is small, they become non-magnetic in the wet magnetic separation process, resulting in loss.

[0007] The present invention aims to solve the various problems in the past and to achieve the following objectives: That is, the present invention aims to provide a method for recovering valuable materials from lithium-ion secondary batteries, which can achieve a high recovery rate of cobalt and nickel even when the cobalt and nickel contents in the magnetic separation target are low. [Means for solving the problem]

[0008] The means for solving the above problems are as follows. <1> a heat treatment step of heat-treating the lithium ion secondary battery to obtain a heat-treated product; A first classification step of crushing the heat-treated product and classifying the crushed product to obtain a coarse product 1 and a fine product; A second classification step in which the pulverized product obtained by pulverizing the fine product is classified at a classification point smaller than the classification point of the first classification step to obtain a coarse product 2 and a fine product; a first magnetic separation step in which the fine product obtained in the second classification step is magnetically separated to obtain magnetic materials 1 and non-magnetic materials 1; a second magnetic separation step in which the non-magnetic materials 1 obtained in the first magnetic separation step are magnetically separated to obtain magnetic materials 2 and non-magnetic materials 2; a recovery step of recovering valuable materials from the magnetic materials 1 and 2; The present invention relates to a method for recovering valuable materials from a lithium ion secondary battery, the method comprising the steps of: <2> The first classification step is performed at a classification point of 600 μm or more and 2,400 μm or less. <1> This is a method for recovering valuable materials from the lithium ion secondary battery described in the above. <3> The second classification step is performed at a classification point of 25 μm or more and 1,700 μm or less. <1> or <2> This is a method for recovering valuable materials from the lithium ion secondary battery described in the above. <4> The magnetic flux density of the magnetic separation in the first magnetic separation step is 0.1T End 0.3T is less than The magnetic flux density of the magnetic separation in the second magnetic separation step is 0.3T End 2T The above-mentioned <1> ~ <3> 13. A method for recovering valuable materials from the lithium ion secondary battery according to claim 12. <5> The total content of cobalt and nickel in the non-magnetic material 1 is 30 mass% or less. <1> ~ <4> 13. A method for recovering valuable materials from the lithium ion secondary battery according to claim 12. <6> At least one of cobalt and nickel contained in the non-magnetic material 1 has a number average particle size of 50 μm or less. <1> ~ <5> 13. A method for recovering valuable materials from the lithium ion secondary battery according to claim 12. <7> At least one of the first magnetic separation step and the second magnetic separation step is performed by wet magnetic separation; <1> ~ <6> 13. A method for recovering valuable materials from the lithium ion secondary battery according to claim 12. <8> The second magnetic separation step is performed by wet magnetic separation, using a high gradient wet magnetic separation method. <7> This is a method for recovering valuable materials from the lithium ion secondary battery described in the above. <9> The second magnetic separation step is performed by wet magnetic separation, and the non-magnetic material slurry is introduced into a rotating drum having a magnet. <8> This is a method for recovering valuable materials from the lithium ion secondary battery described in the above. <10> The second magnetic separation step is performed by wet magnetic separation, and a magnet is placed at the 3 o'clock position on the drum, a non-magnetic material 1 slurry is added from the 12 o'clock to 2 o'clock position on the drum, and the drum is rotated counterclockwise to use a drum-type wet magnetic separation method. <8> ~ <9> 13. A method for recovering valuable materials from the lithium ion secondary battery according to claim 12. <11> The second magnetic separation step is carried out by adding a dispersant to the non-magnetic material 1 obtained in the first magnetic separation step. <8> ~ <10> 13. A method for recovering valuable materials from the lithium ion secondary battery according to claim 12. <12> In the recovery step, the magnetic materials 1 and 2 are washed and subjected to solid-liquid separation to recover valuable materials. <1> ~ <11> 13. A method for recovering valuable materials from the lithium ion secondary battery according to claim 12. <13> Copper is recovered from the coarse product 2. <1> ~ <12> 13. A method for recovering valuable materials from the lithium ion secondary battery according to claim 12. Effect of the Invention

[0009] According to the present invention, it is possible to solve the above-mentioned problems in the conventional art and achieve the above-mentioned object, thereby providing a method for recovering valuables from lithium-ion secondary batteries that can achieve a high recovery rate of cobalt and nickel even when the cobalt and nickel contents in the magnetic separation subject are low. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a diagram showing an example of a process flow in the method of the present invention for recovering valuable materials from a lithium ion secondary battery. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a drum type wet magnetic separation device. [Diagram 3] FIG. 3 is a schematic diagram showing another example of a drum type wet magnetic separation device. [Figure 4] FIG. 4 is a photograph showing an example of a matrix inlet in a high gradient type wet magnetic separation device. [Diagram 5]FIG. 5 is a photograph showing an example of a matrix storage container in a high gradient type wet magnetic separation device. [Figure 6A] FIG. 6A is a diagram showing an example of a horizontal matrix. [Figure 6B] FIG. 6B is a diagram showing an example of a vertical matrix. [Figure 7] FIG. 7 is a diagram showing an example of a matrix member in which three horizontal matrices and four vertical matrices are alternately stacked. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] (Method for recovering valuable materials from lithium-ion secondary batteries) The method for recovering valuable materials from a lithium ion secondary battery of the present invention includes a heat treatment step, a first classification step, a second classification step, a first magnetic separation step, a second magnetic separation step, and a recovery step, and may further include other steps as necessary.

[0012] In the present invention, by performing a second magnetic separation step after performing a first magnetic separation step, cobalt and nickel that were lost as non-magnetic matter in the first magnetic separation step can be recovered as magnetic matter in the second magnetic separation step, and a high recovery rate of cobalt and nickel can be realized. In particular, even if the combined value of the cobalt and nickel grades of the non-magnetized matter 1 obtained in the first magnetic separation step is 30 mass% or less, or even if the number average particle size of at least one of the cobalt and nickel contained in the non-magnetized matter 1 obtained in the first magnetic separation step is 50 μm or less, a high recovery rate of cobalt and nickel can be realized.

[0013] The method for recovering valuable materials from lithium ion secondary batteries of the present invention is a method for recovering valuable materials from a lithium ion secondary battery, which is a target object. Here, valuables refer to things that can be traded without being discarded, and examples of such things include various metals. Examples of valuables in lithium-ion secondary batteries include copper (Cu), aluminum (Al), lithium (Li), cobalt (Co), nickel (Ni), iron (Fe), and carbon (C). Among these, cobalt (Co) and nickel (Ni) are preferred.

[0014] <Lithium-ion secondary battery> The lithium ion secondary battery that is the target is not particularly limited and can be appropriately selected depending on the purpose. Examples include defective lithium ion secondary batteries generated during the manufacturing process of lithium ion secondary batteries, lithium ion secondary batteries that are discarded due to a defect in the equipment they are used in or the end of the life of the equipment, and used lithium ion secondary batteries that are discarded due to the end of the life of the equipment.

[0015] The shape, structure, size, and material of the lithium ion secondary battery are not particularly limited and can be appropriately selected depending on the purpose. The shape of the lithium ion secondary battery is not particularly limited and can be appropriately selected depending on the purpose. Examples of the shape include laminate type, cylindrical type, button type, coin type, square type, and flat type. The form of the lithium ion secondary battery is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a battery cell, a battery module, and a battery pack. Here, the battery module means a battery cell, which is a unit battery, connected and assembled into one housing. The battery pack means a battery module that has a plurality of battery modules assembled into one housing. The battery pack may also include a controller or a cooling device.

[0016] Examples of the lithium ion secondary battery include a battery including a positive electrode, a negative electrode, a separator, an electrolytic solution containing an electrolyte and an organic solvent, and an outer container that is a battery case that contains the positive electrode, the negative electrode, the separator, and the electrolytic solution. The lithium ion secondary battery may be in a state in which the positive electrode and the negative electrode have fallen off.

[0017] -Positive electrode- The positive electrode is not particularly limited as long as it has a positive electrode active material containing at least one of cobalt and nickel, and can be appropriately selected depending on the purpose. The shape of the positive electrode is not particularly limited and can be appropriately selected depending on the purpose. For example, the shape may be a flat plate or a sheet.

[0018] --Positive electrode current collector-- The shape, structure, size, material, etc. of the positive electrode current collector are not particularly limited and may be appropriately selected depending on the purpose. The positive electrode current collector may be in the form of, for example, a foil. Examples of the material for the positive electrode current collector include stainless steel, nickel, aluminum, copper, titanium, tantalum, etc. Among these, aluminum is preferable.

[0019] The positive electrode material is not particularly limited and can be appropriately selected depending on the purpose. For example, a positive electrode material containing at least a positive electrode active material containing lithium and, if necessary, a conductive agent and a binder resin can be mentioned. There are no particular limitations on the positive electrode active material as long as it contains at least one of cobalt and nickel, and it can be appropriately selected depending on the purpose. As the positive electrode active material, for example, lithium manganese oxide (LiMn 2 O 4 ), lithium cobalt oxide (LiCoO 2 ), ternary and NCM systems, LiNi x Co y Mn z O 2(x+y+z=1), LiNi, also known as NCA x Co y Al z (x+y+z=1), lithium iron phosphate (LiFePO 4 ), lithium cobalt nickel oxide (LiCo 1 / 2 Ni 1 / 2 O 2 ), lithium titanate (Li 2 TiO 3 ) As the positive electrode active material, these materials may be used in combination. The conductive agent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the conductive agent include carbon black, graphite, carbon fiber, and metal carbides. The binder resin is not particularly limited and can be appropriately selected depending on the purpose. Examples of the binder resin include homopolymers or copolymers of vinylidene fluoride, tetrafluoroethylene, acrylonitrile, ethylene oxide, and the like, and styrene-butadiene rubber.

[0020] -Negative electrode- The negative electrode is not particularly limited as long as it has a negative electrode active material, and can be appropriately selected depending on the purpose. The shape of the negative electrode is not particularly limited and can be appropriately selected depending on the purpose. For example, the shape may be a flat plate or a sheet.

[0021] --Negative electrode current collector-- The negative electrode current collector is not particularly limited in shape, structure, size, material, etc., and can be appropriately selected depending on the purpose. The negative electrode current collector may be in the form of, for example, a foil. Examples of the material for the negative electrode current collector include stainless steel, nickel, aluminum, copper, titanium, tantalum, etc. Among these, copper is preferable.

[0022] The negative electrode active material is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include carbon materials such as graphite and hard carbon, titanate, silicon, etc. Furthermore, the negative electrode active material may be a combination of these materials.

[0023] The positive electrode current collector and the negative electrode current collector have a laminate structure, and the laminate is not particularly limited and can be appropriately selected depending on the purpose.

[0024] -Outer packaging- The material for the exterior container (casing) of the lithium ion secondary battery is not particularly limited and can be appropriately selected depending on the purpose. Examples of the material include aluminum, iron, stainless steel, and resin (plastic).

[0025] Hereinafter, each step in the method for recovering valuable materials from a lithium ion secondary battery of the present invention will be described in detail.

[0026] <Heat treatment process> The heat treatment step is a step of heat treating the lithium ion secondary battery to obtain a heat-treated product. The heat-treated product means a product obtained by heat treating the lithium ion secondary battery. The method of performing the heat treatment in the heat treatment step is not particularly limited and can be appropriately selected depending on the purpose. For example, the heat treatment can be performed by heating the object in a known roasting furnace. The roasting furnace is not particularly limited and can be appropriately selected depending on the purpose. Examples of the roasting furnace include batch furnaces such as rotary kilns, fluidized bed furnaces, tunnel furnaces and muffle furnaces, cupola furnaces, and stoker furnaces.

[0027] The atmosphere used for the heat treatment is not particularly limited and can be appropriately selected depending on the purpose. Examples of the atmosphere include air, an inert atmosphere, a reducing atmosphere, and a low-oxygen atmosphere. The atmospheric atmosphere (air atmosphere) means an atmosphere using atmospheric air (air) containing about 21% by volume of oxygen and about 78% by volume of nitrogen. The inert atmosphere can be, for example, an atmosphere made of nitrogen or argon. The reducing atmosphere is, for example, a mixture of CO, H in an inert atmosphere such as nitrogen or argon. 2 , H 2 S, SO 2 It refers to an atmosphere that includes the following: A low-oxygen atmosphere means an atmosphere in which the oxygen concentration is 11% by volume or less.

[0028] The conditions for heat treating (heating) the object to be heat-treated (heat treatment conditions) are not particularly limited as long as the conditions are such that each component part of the object can be separated and crushed in the crushing and classification process described below, and can be appropriately selected depending on the purpose. Here, examples of the heat treatment conditions include the heat treatment temperature and the heat treatment time.

[0029] The heat treatment temperature means the temperature of the lithium ion secondary battery that is the object of the heat treatment. The heat treatment temperature can be measured by inserting a thermometer such as a couple or a thermistor into the object during the heat treatment.

[0030] The temperature in the heat treatment (heat treatment temperature) is preferably 400°C or higher and 1,080°C or lower, more preferably 660°C or higher and 1,080°C or lower, and particularly preferably 750°C or higher and 900°C or lower. By setting the heat treatment temperature at 400°C or higher, the cobalt oxide and nickel oxide contained in the positive electrode active material are reduced to metal. In addition, these metals can be grown to a particle size that is easy to magnetically attract in the subsequent magnetic separation. This particle size growth is more likely to occur the higher the heat treatment temperature is. In addition, by setting the heat treatment temperature at 660°C or higher, it is possible to melt the aluminum that constitutes the exterior case of the LIB pack or cell and separate and recover it from the other members. In addition, by setting the heat treatment temperature at 750°C or higher, the Li(Ni / Co / Mn)O in the positive electrode active material can be reduced. 2 or LiPF in the electrolyte 6 The lithium in 2 CO 3 ), lithium oxide (Li2 0) can be made into a form that is soluble in aqueous solutions and can be leached into the dispersion medium during the slurry process. In addition, it is preferable that the exterior container of the lithium ion secondary battery is made of a material having a melting point higher than the heat treatment temperature. When a material having a melting point lower than the heat treatment temperature is used for the outer container of the lithium ion secondary battery, the heat treatment is preferably performed in a low-oxygen atmosphere with an oxygen concentration of 11% by volume or less, or at least in such a way that the oxygen concentration inside the lithium ion secondary battery (particularly the positive electrode current collector and the negative electrode current collector arranged in the outer container of the lithium ion secondary battery) during roasting becomes 11% by volume or less.

[0031] In addition, as a method for realizing a low-oxygen atmosphere, for example, the positive electrode or negative electrode of the lithium ion secondary battery may be housed in an oxygen-shielding container and heat-treated. There is no particular limitation on the material of the oxygen-shielding container as long as it has a melting point equal to or higher than the heat treatment temperature, and it can be appropriately selected according to the purpose. For example, when the heat treatment temperature is 800° C., iron, stainless steel, and the like having a melting point higher than this heat treatment temperature can be used. In order to release the gas pressure of the gas generated by the combustion of the electrolyte solution in the lithium ion secondary battery or the laminate, it is preferable to provide an opening in the oxygen shielding container. The opening area is preferably 12.5% ​​or less of the surface area of ​​the outer container in which the opening is provided. It is more preferable that the opening area is 6.3% or less of the surface area of ​​the outer container in which the opening is provided. There are no particular limitations on the shape, size, and location of the opening, and it can be appropriately selected depending on the purpose. The heat treatment time of the lithium ion secondary battery is not particularly limited and can be appropriately selected according to the purpose, but is preferably 1 minute to 10 hours, more preferably 1 minute to 3 hours. The heat treatment time may be a heat treatment time that reaches a desired temperature at which cobalt and nickel are metallized, and the holding time may be a time that ensures the metallization. If the heat treatment time is within the preferred range, it is advantageous in terms of the cost required for the heat treatment. Therefore, it is preferable to carry out the heat treatment at 400° C. or higher and 1,080° C. or lower for one hour or longer.

[0032] <First classification process> The first classification step is a step in which the heat-treated product is crushed and the crushed product obtained is classified to obtain a coarse product 1 and a fine product. The crushing treatment of the heat-treated product is not particularly limited as long as it is a treatment that can crush the heat-treated product to obtain a crushed product, and can be appropriately selected depending on the purpose. In addition, the crushed product means the product obtained by crushing the heat-treated product. As the crushing treatment, for example, it is preferable to crush the heat-treated product by impact to obtain crushed products. In addition, if the outer container of the lithium ion secondary battery does not melt during the heat treatment, it is more preferable to pre-crush the heat-treated product by cutting it with a cutter before applying an impact to the heat-treated product.

[0033] Examples of the method of crushing by impact include a method of throwing the heat-treated material with a rotating striking plate and striking it against a collision plate to give an impact, and a method of hitting the heat-treated material with a rotating striker (beater), which can be performed, for example, by a hammer crusher. Another method of crushing by impact may be a method of hitting the heat-treated material with ceramic balls, which can be performed, for example, by a ball mill. Crushing by impact can also be performed, for example, by using a biaxial crusher with a short blade width and blade length for crushing by compression. Further, examples of the method for crushing the material by impact include a method in which the heat-treated material is struck and impacted by two rotating chains, and this can be carried out, for example, by a chain mill.

[0034] Crushing the heat-treated material by impact promotes crushing of the positive electrode current collector (e.g., aluminum (Al)), but the negative electrode current collector (e.g., copper (Cu)), whose form has not changed significantly, exists in a form such as a foil. Therefore, in the crushing process, the negative electrode current collector is merely cut, and thus it is possible to obtain crushed material in a state in which valuable materials derived from the positive electrode current collector (e.g., aluminum) and valuable materials derived from the negative electrode current collector (e.g., copper (Cu)) can be efficiently separated in the first classification step (classification process).

[0035] The crushing time in the crushing process is not particularly limited and can be appropriately selected depending on the purpose, but the crushing time per 1 kg of lithium ion secondary batteries is preferably from 1 second to 30 minutes, more preferably from 2 seconds to 10 minutes, and particularly preferably from 3 seconds to 5 minutes.

[0036] The first classification step includes a process of obtaining a coarse-grained product 1 and a fine-grained product by crushing the heat-treated product and classifying the crushed product obtained at a classification point of 600 μm or more and 2,400 μm or less, and it is preferable to classify the product at a classification point of 850 μm or more and 1,700 μm or less. The first classification step is not particularly limited as long as it can classify the crushed material to obtain a coarse product 1 (a product that passes through the sieve) and a fine product (a product that passes through the sieve), and can be appropriately selected depending on the purpose.

[0037] The classification method is not particularly limited and can be appropriately selected depending on the purpose, and can be performed using, for example, a vibrating sieve, a multi-stage vibrating sieve, a cyclone, a JIS Z8801 standard sieve, a wet vibrating table, an air table, etc. By classification, copper (Cu), iron (Fe), etc. can be separated into the coarse product 1, and lithium, cobalt, nickel, or carbon can be concentrated in the fine product. The particle size of the classification (classification point, sieve opening) is set to a classification point of 600 μm or more and 2,400 μm or less, in order to separate copper (Cu), iron (Fe), aluminum (Al), etc. into the coarse product 1 and concentrate carbon (C), lithium (Li), cobalt (Co), nickel (Ni), manganese (Mn), etc. into the fine product.

[0038] Furthermore, when using a sieve as a classification method, by placing, for example, stainless steel balls or alumina balls on the sieve as a crushing promoter and performing classification, small crushed pieces adhering to larger crushed pieces can be separated from the larger crushed pieces more efficiently, and the quality of the recovered metal can be further improved. As described above, in the first classification step, the crushing process can be carried out simultaneously with the classification process. For example, the heat-treated product obtained in the heat treatment step can be crushed while the crushed product is classified into a coarse product 1 and a fine product, as a crushing / classification step (crushing / classification). If the ratio of fine products is low in the first classification step (classification treatment), the coarse product 1 can be returned to the step of crushing the heat-treated material. This can improve the recovery rate of valuable materials other than Fe and Cu.

[0039] <Second classification process> The second classification process is a process for obtaining a coarse product 2 and a fine product by crushing the fine product obtained in the first classification process and classifying the crushed product obtained at a classification point smaller than the classification point of the first classification process. The grinding process is not particularly limited as long as it can grind a fine product to obtain ground products of a predetermined size, and can be appropriately selected depending on the purpose. Examples of the grinding process include media-agitation type grinders (attritors, bead mills, tower mills) that use media such as iron balls, roller mills, jet mills, high-speed rotary grinders (hammer mills, pin mills), and container-driven mills (rotary mills, vibration mills, planetary mills).

[0040] The pulverization may be either wet or dry, and can be appropriately selected depending on the purpose, but wet pulverization is preferable. Wet pulverization can suppress the decrease in the recovery rate of cobalt (Co) and nickel (Ni) due to dust generation in each process, and does not require a means to prevent dust from scattering into the surrounding atmosphere. When wet pulverization is performed, it is preferable to perform a slurrying process in which the fine product obtained after the first classification process is immersed in water to obtain a slurry-like liquid (fine product slurry). The slurrying process is not particularly limited as long as it is a process that can disperse the fine product recovered in the first classification process in water to obtain a slurry (suspension) by immersing (soaking or placing) the fine product in water, and can be appropriately selected depending on the purpose. The particle size (90% particle size) of the pulverized product is preferably 1,000 μm or less, more preferably 750 μm or less, and particularly preferably 500 μm or less. The 90% particle size is, for example, the particle size that is 90% in the particle size cumulative distribution obtained by measurement using a laser diffraction scattering type particle size distribution measuring device. The number average particle size of at least one or both of the cobalt and nickel contained in the pulverized material is preferably 100 μm or less, more preferably 75 μm or less, and particularly preferably 50 μm or less. The number average particle size is, for example, an average value calculated by measuring the particle sizes of 100 cobalt particles and 100 nickel particles in total by observation with an electron microscope. A smaller 90% particle size or number-average particle size promotes the liberation of cobalt and nickel from other components, and can improve the quality of cobalt and nickel in the magnetized material 1 and the magnetized material 2 recovered in the first magnetic separation step and the second magnetic separation step. Even when the 90% particle size or number-average particle size is small, the recovery rates of cobalt and nickel in the first magnetic separation step and the second magnetic separation step can be increased, so that further recovery steps such as a third magnetic separation step may be provided as necessary.

[0041] The dispersion medium for forming a slurry of the fine granular product is not particularly limited and can be appropriately selected depending on the purpose. Examples of the dispersion medium include industrial water, tap water, ion-exchanged water, ultrafiltered water, reverse osmosis water, distilled water, and other pure water and ultrapure water.

[0042] Here, the slurrying treatment is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a method of simply putting the fine-grained product in water, a method of putting the fine-grained product in water and stirring, a method of putting the fine-grained product in water and gently stirring while applying ultrasonic waves, a method of adding water to the fine-grained product, etc. Among these, the method of putting the fine-grained product in water and stirring is preferred, and the method of putting the fine-grained product in water and gently stirring while applying ultrasonic waves is more preferred.

[0043] The solid-liquid ratio in the slurrying process (the concentration (mass ratio) of the fine product relative to the water) is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1% by mass or more and 50% by mass or less, and more preferably 5% by mass or more and 20% by mass or less. If the solid-liquid ratio is less than 1% by mass, cobalt and nickel that would normally be recovered as magnetized matter will not be recovered by the magnetic separator and will be lost to non-magnetized matter, which is likely to reduce the recovery rate of cobalt and nickel. If the solid-liquid ratio exceeds 50% by mass, the amount of impurities caught in the magnetized matter will increase, and the cobalt and nickel grades may decrease. The stirring speed of the water in the slurrying treatment is not particularly limited and can be appropriately selected depending on the purpose, and can be, for example, 200 rpm. The leaching time in the slurrying treatment is not particularly limited and can be appropriately selected depending on the purpose, and can be, for example, 1 hour.

[0044] In the second classification step, the pulverized material obtained in the pulverization process is classified at a classification point smaller than the classification point in the first classification step and not less than 75 μm and not more than 1,200 μm, thereby obtaining a coarse product 2 and a fine product. For example, when the pulverized material obtained by the pulverization process is subjected to a second classification step using a JIS Z8801 standard sieve with a classification point of 500 μm, the product that passes over the sieve of the standard sieve with a classification point of 500 μm is the coarse product 2, and the product that passes under the sieve is the fine product. Copper can be concentrated and recovered from the coarse product 2.

[0045] The classification point used in the second classification step is preferably 25 μm to 1,700 μm, more preferably 75 μm to 1,200 μm, even more preferably 75 μm to 850 μm, and particularly preferably 106 μm to 600 μm. If the classification point exceeds 1,700 μm, copper may be mixed into the fine product, and the cobalt and nickel grades may decrease, while if the classification point is below 25 μm, the pulverization energy required to recover cobalt and nickel into the fine product may become excessive.

[0046] The classification treatment in the second classification step is not particularly limited and can be appropriately selected depending on the purpose. Examples include a vibrating sieve, a multistage vibrating sieve, a cyclone, a JIS Z8801 standard sieve, a wet vibrating table, and an air table. The second classification step is not particularly limited and can be appropriately selected depending on the purpose, but is preferably performed in a wet manner. When performing wet classification, the ground slurry obtained by the wet grinding process may be supplied as it is, or the ground slurry may be diluted by adding a dispersion medium (water) to adjust the solid-liquid ratio. In addition, when the second classification step is performed in a wet manner and a vibrating sieve or a multi-stage vibrating sieve is used, the dispersion medium (water) is showered from the top of the sieve to suppress aggregation of the pulverized material during classification, and good classification results can be obtained. In addition, the phase angle of the weight of the vibrating sieve is preferably 30° to 90°, more preferably 40° to 80°, and particularly preferably 50° to 70°. By setting this phase angle, excessive discharge of the pulverized material or the product after classification outside the sieve device (too short a residence time on the sieve) can be prevented, and good classification results can be obtained.

[0047] <First magnetic separation process> The first magnetic separation step is a step in which the fine product obtained in the second classification step is magnetically separated to obtain magnetic materials 1 and non-magnetic materials 1.

[0048] The magnetized object 1 refers to an object that can be attracted to a magnetic source (such as a magnet or electromagnet) by the magnetic force generated by the magnetic source, generating an attractive force between the magnetic object 1 and the magnetic source. Examples of the magnetized object 1 include ferromagnetic metals. Examples of the ferromagnetic metals include iron (Fe), nickel (Ni), and cobalt (Co). The non-magnetic object 1 means an object that is not attracted to the magnetic source by the magnetic force generated by the magnetic source. There is no particular limitation on the non-magnetic object, and it can be selected according to the purpose. Examples of the non-magnetic metal object include paramagnetic or semimagnetic metals. Examples of the paramagnetic or semimagnetic metals include aluminum (Al), manganese (Mn), gold (Au), silver (Ag), and copper (Cu).

[0049] The first magnetic separation step may be either dry magnetic separation or wet magnetic separation, but wet magnetic separation is preferred for the following reasons. When the fine product obtained in the second classification step is magnetically separated, for example, if the magnetic separation is performed in a dry manner, the particles may aggregate due to moisture adhering between the particles, and the metal particles derived from the negative electrode current collector and the negative electrode active material fine particles, which are contained in the fine product at 10% or more, and the cobalt particles and nickel particles may not be sufficiently separated. For this reason, in the present invention, it is preferable to perform wet magnetic separation to separate the material derived from the negative electrode active material and the metal derived from the negative electrode current collector into a non-magnetized material slurry, and recover the cobalt and nickel as the magnetized material 1.

[0050] In the wet magnetic separation, the fine product slurry obtained in the second wet classification step may be fed as is, or the fine product slurry may be concentrated or diluted by solid-liquid separation such as sedimentation to adjust the solid-liquid ratio. Also, the fine product slurry may be diluted with water to adjust the solid-liquid ratio. The solid-liquid ratio (concentration (mass ratio) of the fine product to water) of the slurry supplied to the wet magnetic separation is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 5% by mass or more and 67% by mass or less, and more preferably 10% by mass or more and 40% by mass or less. If the solid-liquid ratio is less than 5% by mass, the recovery rate of cobalt and nickel as magnetic substances in the wet magnetic separator may decrease. If the solid-liquid ratio exceeds 67% by mass, problems such as pump blockage during slurry supply are likely to occur, and the separation performance of cobalt and nickel (magnetic substances) and non-magnetic substances such as carbon may decrease. The method of supplying the slurry is not particularly limited and can be appropriately selected depending on the purpose, but the slurry in the tank may be supplied by a pump while being stirred.

[0051] The first magnetic separation step is not particularly limited and can be performed using a known magnetic separator (magnetic separator), for example, a drum type magnetic separator, a high gradient type magnetic separator, etc. Among these, a drum type magnetic separator is preferred.

[0052] The magnetic flux density for magnetic separation in the first magnetic separation step is not particularly limited and can be appropriately selected depending on the purpose. 0.05T End 0.9T The following are preferred: 0.075T End 0.6T The following is more preferred: 0.1T End 0.3T More preferably, 0.1T End 0.2T The following is particularly preferred: 0.05T If the magnetic flux density is less than 100%, it is difficult to magnetically attract the fine particles of cobalt and nickel, and the recovery rate of the magnetic particles of cobalt and nickel is likely to decrease. 0.9T If the concentration exceeds this range, the recovery rate of impurities other than cobalt and nickel in the magnetized material 1 increases, and the grades of cobalt and nickel in the magnetized material 1 may decrease. Examples of drum-type wet magnetic separation methods in the first magnetic separation step include (1) a method in which a magnet is placed at the 6 o'clock position on a drum as shown in FIG. 2, a slurry of non-magnetic material 1 is added from the 3 o'clock position (side) and the drum is rotated clockwise, and (2) a method in which a magnet is placed near the 3 o'clock position on a drum as shown in FIG. 3, a slurry of non-magnetic material 1 is added from the 12 o'clock to 2 o'clock position (top) of the drum and the drum is rotated counterclockwise. Among these, (1) the drum type wet magnetic separation method shown in FIG. 2 is preferred because it can produce high-quality magnetic products of cobalt and nickel.

[0053] <Second magnetic separation process> The second magnetic separation step is a step of magnetically separating the non-magnetic material 1 obtained in the first magnetic separation step to obtain magnetic material 2 and non-magnetic material 2. In the case where collected dust generated during the transportation of the fine product obtained in the first classification step is collected, the collected dust can also be subjected to magnetic separation in the second magnetic separation step.

[0054] The combined content of cobalt and nickel contained in the non-magnetic matter 1 obtained in the first magnetic separation step is preferably 30% or less, more preferably 20% or less, and particularly preferably 15% or less. Even the non-magnetic material 1 having a combined cobalt and nickel content of 30% or less can be recovered as a magnetic material in the second magnetic separation step, thereby improving the recovery rate of cobalt and nickel. However, it is a well-known fact that the higher the grades of cobalt and nickel in the non-magnetic material, the easier it is to recover cobalt and nickel in the magnetic material. The number average particle size of at least one of the cobalt and nickel contained in the non-magnetic material 1 obtained in the first magnetic separation step is preferably 50 μm or less, more preferably 35 μm or less, and particularly preferably 25 μm or less. The number average particle size is, for example, an average value calculated by measuring the particle sizes of a total of 100 cobalt particles and nickel particles by electron microscope observation. The smaller the number average particle size, the more the liberation of cobalt and nickel from other components is promoted, and the cobalt and nickel quality of the magnetic material 2 recovered in the second magnetic separation step can be improved. Note that, since the recovery rate of cobalt and nickel in the second magnetic separation step can be increased, a further recovery step such as a third magnetic separation step may be provided as necessary. Even cobalt particles and nickel particles having a number-average particle size of 50 μm or less can be recovered as magnetic matter in the second magnetic separation step, thereby improving the recovery rate of cobalt and nickel in the entire process.

[0055] The second magnetic separation step is not particularly limited, and can be performed using a known magnetic separator (magnetic separator), for example, a drum type magnetic separator, a high gradient type magnetic separator, or the like.

[0056] The magnetic flux density for magnetic separation in the second magnetic separation step is not particularly limited and can be appropriately selected depending on the purpose. 0.3T End 2T The following are preferred: 0.4T End 1.8T The following is more preferred: 0.6T End 1.2T The following is particularly preferred: 0.3T If the magnetic flux density is less than 100%, it is difficult to magnetically attract the fine particles of cobalt and nickel, and the recovery rate of the magnetic particles of cobalt and nickel is likely to decrease. 2T If the concentration exceeds this range, the recovery rate of impurities other than cobalt and nickel in the magnetized material 2 increases, and the grades of cobalt and nickel in the magnetized material 2 may decrease.

[0057] The second magnetic separation step may be either dry magnetic separation or wet magnetic separation, but wet magnetic separation is preferred. The second magnetic separation step is carried out by wet magnetic separation, preferably using a high gradient wet magnetic separation method, which may be repeated two or more times. In the high gradient wet magnetic separation method, it is preferable to use a matrix in order to increase the change in magnetic flux density. As the matrix, for example, a horizontal iron matrix shown in FIG. 6A (line width: 2 mm, thickness: 4 mm, 200 mm wide × 50 mm long) and a vertical iron matrix shown in FIG. 6B (maximum length of diamond: 22 mm, minimum length of diamond: 10 mm, thickness: 4 mm, 200 mm wide × 50 mm long) can be used, and a matrix member shown in FIG. 7 (200 mm wide × 50 mm long × 28 mm thick) can be used, which is made by stacking and bundling three horizontal matrices of FIG. 6A and four vertical matrices of FIG. 6B alternately.

[0058] The second magnetic separation step is carried out by wet magnetic separation, preferably using a drum type wet magnetic separation method. The drum type wet magnetic separation method in the second magnetic separation step may be, for example, a method in which a non-magnetic material slurry is poured into a rotating drum having a magnet. The direction of rotation is not particularly limited and may be appropriately selected depending on the purpose, and may be either clockwise or counterclockwise. The position of the magnet on the drum is not particularly limited and can be appropriately selected depending on the purpose. For example, the magnet may be at the same position as the non-magnetic material slurry is charged, or at a position different from the non-magnetic material slurry is charged. Specific examples of drum-type wet magnetic separation methods in the second magnetic separation step include, for example, (1) a method in which a magnet is placed at the 6 o'clock position on a drum as shown in Figure 2, a slurry of non-magnetic material 1 is added from the 3 o'clock position (side) and the drum is rotated clockwise, and (2) a method in which a magnet is placed near the 3 o'clock position on a drum as shown in Figure 3, a slurry of non-magnetic material 1 is added from the 12 o'clock to 2 o'clock position (top) of the drum and the drum is rotated counterclockwise. Among these, the drum type wet magnetic separation method shown in (2) Fig. 3 is preferred because it provides a high recovery rate of cobalt and nickel. In the method shown in (2) Fig. 3, the magnetized materials attracted to the magnet are carried in the 9 o'clock direction by the rotation of the drum and are recovered, and the non-magnetized material slurry 2 flows on the drum surface in the 3 o'clock to 6 o'clock directions and is discharged from the 6 o'clock direction.

[0059] The second magnetic separation step can be carried out by adding a dispersant to the slurry of non-magnetized material 1 obtained in the first magnetic separation step. By adding a dispersant to the slurry of non-magnetized material 1, the magnetic separation efficiency of the second magnetic separation step can be improved. The dispersant is not particularly limited and can be appropriately selected depending on the purpose. For example, dispersants used in the fields of dyes, pigments, agricultural chemicals, and inorganic substances can be used. Examples of dispersants include condensates of aromatic sulfonic acid and formalin, and anionic surfactants whose main component is a special carboxylic acid type polymer surfactant (for example, the "Demol" series of surfactants manufactured by Kao Corporation).

[0060] In addition, additional magnetic separation may be performed on the magnetized object 1 and / or the magnetized object 2, and additional magnetic separation may be performed on the non-magnetized object 1 and / or the non-magnetized object 2.

[0061] The combined value of the cobalt and nickel grades in the magnetic material obtained by wet magnetic separation is preferably concentrated to 1.3 times or more, and more preferably 1.5 times or more, of the combined value of the cobalt and nickel grades in the fine product.

[0062] <Recovery process> The recovery step is a step of recovering valuable materials from the magnetized materials 1 and 2. In the recovery step, valuable materials are recovered by performing solid-liquid separation on the magnetized materials 1 and 2. The magnetized materials 1 and 2 may be washed before the solid-liquid separation. Washing can reduce the grade of impurities such as fluorine contained in the magnetized materials. The washing water used for washing is not particularly limited and can be appropriately selected depending on the purpose. Examples of the washing water include industrial water, tap water, ion-exchanged water, ultrafiltered water, reverse osmosis water, distilled water, and other pure water and ultrapure water. Since the magnetized materials 1 and 2 recovered in the first and second magnetic separation steps contain moisture, the moisture may be removed by performing solid-liquid separation using filter paper, a filter press, or a centrifuge, or by air drying or by heating and drying in a dryer.

[0063] <Other processes> The other steps are not particularly limited and can be appropriately selected depending on the purpose. For example, a drying step, a purification step, etc. can be mentioned.

[0064] <Example of embodiment> Here, an example of an embodiment of the method for recovering valuable materials from a lithium ion secondary battery of the present invention will be described with reference to the drawings. Fig. 1 is a diagram showing an example of a process flow in the embodiment of the method for recovering valuable materials from a lithium ion secondary battery of the present invention.

[0065] First, a heat treatment (heat treatment step) is performed on a discarded lithium ion secondary battery (LIB; Lithium Ion Battery) to obtain a heat-treated product (heat treatment step). Next, the crushed product obtained by crushing the heat-treated product is classified at a classification point of 600 μm to 2,400 μm to obtain a coarse product 1 and a fine product (first classification step). Here, copper (Cu), aluminum (Al), iron (Fe), etc. can be separated from the coarse product 1.

[0066] The fine product is then soaked in water to obtain a fine product slurry, during which lithium (lithium oxide or lithium carbonate) is leached into the water and residues containing nickel (Ni) and cobalt (Co) are formed in the fine product slurry.

[0067] The resulting fine product slurry is then wet milled to obtain a milled product slurry. Next, the obtained pulverized product slurry is wet classified at a classification point of 25 μm or more and 1,700 μm or less to obtain a coarse product slurry 2 and a fine product slurry (second classification step).

[0068] Next, the resulting fine product slurry is magnetically separated to obtain a magnetic material 1 and a non-magnetic material slurry 1 (first magnetic separation step). Next, the obtained non-magnetized material slurry 1 is magnetically separated to obtain magnetized materials 2 and non-magnetized material slurry 2 (second magnetic separation step). The obtained magnetized materials 1 and 2 are subjected to solid-liquid separation to recover nickel (Ni) and cobalt (Co). In addition, the non-magnetized material slurry 2 is subjected to solid-liquid separation to recover carbon and copper. EXAMPLES

[0069] Examples of the present invention will be described below, but the present invention is not limited to these examples.

[0070] Example 1 -Heat treatment process- The waste lithium-ion secondary batteries (approximately 300 kg) to be treated were subjected to heat treatment using a batch-type burner furnace manufactured by Ecosystem Akita Co., Ltd. as a heat treatment device at a heat treatment temperature of 750°C (heated from 20°C to 750°C over 15 minutes, and then held for 3 hours) in an atmospheric condition, to obtain a heat-treated product.

[0071] -Crushing process- Next, the heat-treated lithium ion secondary batteries were crushed using a chain mill (Crossflow Shredder S-1000, manufactured by Sato Iron Works Co., Ltd.) as a crushing device under conditions of 50 Hz (chain tip speed: approximately 60 m / sec) and a residence time of 50 seconds to obtain crushed lithium ion secondary batteries.

[0072] -First classification process- Next, the crushed lithium-ion secondary battery material was sieved using a vibrating sieve (diameter 200 mm, manufactured by Tokyo Screen Co., Ltd.) with sieve openings of 1.2 mm. After sieving, the 1.2 mm over-sieve product (coarse product 1) and under-sieve product (fine product) were collected. The cobalt content of the fine product (black mass) was 6.2%, the nickel content was 13.5%, and the combined content was 19.7%.

[0073] -Slurry process- The resulting fine product (62.5 kg) was immersed in 250 L of water and subjected to a slurry treatment under conditions of a solid-liquid ratio of 25%, a stirring speed of 400 rpm, and a leaching time of 1 hour to obtain a fine product slurry.

[0074] -Wet grinding process- The obtained fine product slurry and 10 kg of grinding media (iron balls) were fed into a media stirring grinder (Tower Mill NE008, manufactured by Nippon Eirich Co., Ltd.) in 20 batches, and wet-ground for 30 minutes at a rotation speed of 716 rpm (circumferential speed 3 m / sec) per batch.

[0075] -The second classification process- Next, the obtained fine product slurry was wet classified using JIS Z8801 standard sieves with sieve classification points (openings) of 500 μm and 250 μm, and the product that passed through the 500 μm sieve (coarse product 2) and the product that passed through the 250 μm sieve (fine product slurry) were collected. Note that the intermediate product that was generated on the 250 μm sieve was returned to the previous wet grinding process and repeatedly ground until all of it passed through the 250 μm sieve.

[0076] -First magnetic separation process- The obtained fine product slurry (slurry concentration 15 mass%) was subjected to a magnetic flux density test using a drum type wet magnetic separator (manufactured by Eriez Magnetics Co., Ltd., model: WD L-8 lab model) shown in FIG. 0.15T The first magnetic separation step was carried out at a drum rotation speed of 40 rpm, and magnetized matter 1 and non-magnetized matter slurry 1 were recovered. The drum-type wet magnetic separation device shown in FIG. 2 is a device in which a magnet is placed at the 6 o'clock position on the drum, a slurry of non-magnetic material 1 is added from the 3 o'clock position (side) of the drum, and magnetic separation is performed while the drum is rotated clockwise. For the obtained non-magnetized material slurry 1, the particle sizes of a total of 100 cobalt particles and nickel particles were measured by electron microscope observation, and the number average particle size was found to be 10 μm. The cobalt grade of the non-magnetized material 1 contained in the non-magnetized material slurry 1 was 3.4%, the nickel grade was 8.2%, and the combined grade was 11.6%.

[0077] -Second magnetic separation process- The non-magnetic material slurry 1 (slurry concentration: 30 mass%) obtained in the first magnetic separation step was subjected to a magnetic flux density test using a drum-type wet magnetic separator (manufactured by Eriez Magnetics Co., Ltd., model: WD REX 1.5φ×12W) shown in FIG. 0.6T The second magnetic separation step was carried out at a drum rotation speed of 5 rpm, and magnetized matter 2 and non-magnetized matter slurry 2 were recovered. The drum-type wet magnetic separation device shown in FIG. 2 is a device in which a magnet is placed at the 6 o'clock position on the drum, a slurry of non-magnetic material 1 is added from the 3 o'clock position (side) of the drum, and magnetic separation is performed while the drum is rotated clockwise.

[0078] Next, the cobalt and nickel grades, as well as the recovery rates of cobalt and nickel, were measured as follows. The results are shown in Tables 1 and 2.

[0079] <Measurement of cobalt and nickel content> The masses of the obtained coarse product 2, fine product, magnetized material 1, non-magnetized material 1, and magnetized material 2 were measured using an electromagnetic balance (product name: GX-8K, manufactured by A&D Corporation) after drying at 105°C for 1 hour.The fine product, magnetized material 1, non-magnetized material 1, and magnetized material 2 were then heated and dissolved in aqua regia and analyzed using a high-frequency inductively coupled plasma optical emission spectrometer (SPECTROGREEN FMX46, manufactured by Hitachi High-Tech Science Corporation) to determine the cobalt and nickel grades.

[0080] <Calculation of recovery rate of cobalt and nickel> The total amounts of cobalt and nickel contained in coarse product 2, magnetized material 1, non-magnetized material 1, and magnetized material 2 were set to 100%, respectively, and the recovery rates of cobalt and nickel recovered in magnetized material 1 and magnetized material 2 were calculated.

[0081] Example 2 In Example 1, the non-magnetized material slurry 1 (slurry concentration: 30 mass%) obtained in the first magnetic separation step was subjected to a magnetic flux density of 1.000 g / m2 using a drum-type wet magnetic separator (manufactured by Eriez Magnetics Co., Ltd., model: WD REX 1.5φ×12W) shown in FIG. 0.6T Cobalt and nickel were recovered in the same manner as in Example 1, except that the second magnetic separation step was carried out at a drum rotation speed of 5 rpm. The drum-type wet magnetic separation device shown in Figure 3 is an apparatus in which a magnet is placed at the 3 o'clock position on the drum, a slurry of non-magnetic material 1 is added from the 12 o'clock to 2 o'clock direction (top) of the drum, and magnetic separation is performed while the drum is rotated counterclockwise. Next, the cobalt grade and nickel grade, and the recovery rates of cobalt and nickel were measured in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0082] Example 3 In Example 1, the non-magnetized material slurry 1 (slurry concentration: 30 mass%) obtained in the first magnetic separation step was subjected to a magnetic flux density of 1.000 g / m2 using a drum-type wet magnetic separator (manufactured by Eriez Magnetics Co., Ltd., model: WD REX 1.5φ×12W) shown in FIG. 0.6T Cobalt and nickel were recovered in the same manner as in Example 1, except that the second magnetic separation step was carried out at a drum rotation speed of 20 rpm. The drum-type wet magnetic separation device shown in Figure 3 is an apparatus in which a magnet is placed at the 3 o'clock position on the drum, a slurry of non-magnetic material 1 is added from the 12 o'clock to 2 o'clock direction (top) of the drum, and magnetic separation is performed while the drum is rotated counterclockwise. Next, the cobalt grade and nickel grade, and the recovery rates of cobalt and nickel were measured in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0083] Example 4 In Example 1, the non-magnetized material slurry 1 (slurry concentration: 15 mass%) obtained in the first magnetic separation step was subjected to a magnetic flux density of 1.5 mm using a drum-type wet magnetic separator (manufactured by Nippon Eriez Magnetics Co., Ltd., model: WM REX1.5φ×12W) shown in FIG. 0.6T Cobalt and nickel were recovered in the same manner as in Example 1, except that the second magnetic separation step was carried out at a drum rotation speed of 5 rpm. Next, the cobalt grade and nickel grade, and the recovery rates of cobalt and nickel were measured in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0084] Example 5 In Example 1, the non-magnetized material slurry 1 (slurry concentration: 15 mass%) obtained in the first magnetic separation step was subjected to a magnetic flux density of 1.5 mm using a drum-type wet magnetic separator (manufactured by Nippon Eriez Magnetics Co., Ltd., model: WM REX1.5φ×12W) shown in FIG. 0.6T Cobalt and nickel were recovered in the same manner as in Example 1, except that the second magnetic separation step was carried out at a drum rotation speed of 20 rpm. Next, the cobalt grade and nickel grade, and the recovery rates of cobalt and nickel were measured in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0085] Example 6 In Example 1, the non-magnetized material slurry 1 (slurry concentration: 15 mass%) obtained in the first magnetic separation step was subjected to a high gradient wet magnetic separation device (manufactured by Nippon Eriez Magnetics Co., Ltd., model: L-4) to obtain an air-core magnetic flux density of 0.3T Cobalt and nickel were recovered in the same manner as in Example 1, except that the second magnetic separation step was carried out. The high gradient wet magnetic separation device used was a matrix member (200 mm wide × 50 mm long × 28 mm thick) shown in FIG. 7, which was made by stacking and bundling three horizontal iron matrices (line width: 2 mm, thickness: 4 mm, 200 mm wide × 50 mm long) shown in FIG. 6A and four vertical iron matrices (maximum diamond length: 22 mm, minimum diamond length: 10 mm, thickness: 4 mm, 200 mm wide × 50 mm long) shown in FIG. 6B alternately, and placing them in the container shown in FIG. 5 and attaching them to the matrix inlet shown in FIG. 4. Next, the cobalt grade and nickel grade, and the recovery rates of cobalt and nickel were measured in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0086] Example 7 In Example 6, the non-magnetized material slurry 1 (slurry concentration: 15 mass%) obtained in the first magnetic separation step was subjected to a high gradient wet magnetic separation device (manufactured by Nippon Eriez Magnetics Co., Ltd., model: L-4) to obtain an air-core magnetic flux density of 0.6T Cobalt and nickel were recovered in the same manner as in Example 6, except that the second magnetic separation step was carried out. Next, the cobalt grade and nickel grade, and the recovery rates of cobalt and nickel were measured in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0087] Example 8 In Example 6, the non-magnetized material slurry 1 (slurry concentration: 15 mass%) obtained in the first magnetic separation step was subjected to a high gradient wet magnetic separation device (manufactured by Nippon Eriez Magnetics Co., Ltd., model: L-4) to obtain an air-core magnetic flux density of 1.2T Cobalt and nickel were recovered in the same manner as in Example 6, except that the second magnetic separation step was carried out. Next, the cobalt grade and nickel grade, and the recovery rates of cobalt and nickel were measured in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0088] Example 9 In Example 1, a drum-type wet magnetic separator (manufactured by Eriez Magnetics Corporation, model: WM REX 1.5φ×12W) shown in FIG. 2 was used, and the magnetic flux density was 0.6T Cobalt and nickel were recovered in the same manner as in Example 1, except that the first magnetic separation step was carried out at a drum rotation speed of 40 rpm. Next, the cobalt grade and nickel grade, and the recovery rates of cobalt and nickel were measured in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0089] Comparative Example 1 Cobalt and nickel were recovered in the same manner as in Example 1, except that the second magnetic separation step was not carried out. Next, the cobalt grade and nickel grade, and the recovery rates of cobalt and nickel were measured in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0090] [Table 1] [Table 2]

[0091] The results in Tables 1 and 2 show that even when the cobalt and nickel contents of the fine product slurry, which is the subject of magnetic separation, are low, in Examples 1 to 8, cobalt and nickel can be recovered at a high recovery rate by performing a second magnetic separation after the first magnetic separation.

Claims

1. a heat treatment step of heat-treating the lithium ion secondary battery to obtain a heat-treated product; A first classification step of crushing the heat-treated product and classifying the crushed product to obtain a coarse product 1 and a fine product; A second classification step in which the pulverized product obtained by pulverizing the fine product is classified at a classification point smaller than the classification point of the first classification step to obtain a coarse product 2 and a fine product; a first magnetic separation step in which the fine product obtained in the second classification step is magnetically separated to obtain magnetic materials 1 and non-magnetic materials 1; a second magnetic separation step in which the non-magnetic materials 1 obtained in the first magnetic separation step are magnetically separated to obtain magnetic materials 2 and non-magnetic materials 2; a recovery step of recovering valuable materials from the magnetic materials 1 and 2; Including, The second magnetic separation step is carried out by wet magnetic separation, using a drum type magnetic separation method or a high gradient type magnetic separation method. A method for recovering valuable materials from a lithium ion secondary battery.

2. The method for recovering valuable materials from a lithium ion secondary battery according to claim 1 , wherein the first classification step is performed at a classification point of 600 μm or more and 2,400 μm or less.

3. The method for recovering valuable materials from a lithium ion secondary battery according to claim 1 or 2, wherein the second classification step is performed at a classification point of 25 μm or more and 1,700 μm or less.

4. The magnetic flux density of the magnetic separation in the first magnetic separation step is 0.1 T or more and less than 0.3 T, 3. The method for recovering valuable materials from a lithium ion secondary battery according to claim 1, wherein a magnetic flux density in the magnetic separation in the second magnetic separation step is 0.3 T or more and 2 T or less.

5. 3. The method for recovering valuable materials from a lithium ion secondary battery according to claim 1, wherein the combined content of cobalt and nickel in the non-magnetic material 1 is 30 mass% or less.

6. 3. The method for recovering valuable materials from a lithium ion secondary battery according to claim 1, wherein at least one of cobalt and nickel contained in the non-magnetic material 1 has a number average particle size of 50 μm or less.

7. The method for recovering valuable materials from a lithium ion secondary battery according to claim 1 or 2, wherein the first magnetic separation step is performed by wet magnetic separation.

8. A method for recovering valuable materials from a lithium-ion secondary battery as described in claim 1, wherein the second magnetic separation step is performed by wet magnetic separation, and a non-magnetic material slurry is fed into a rotating drum having a magnet.

9. A method for recovering valuable materials from a lithium-ion secondary battery as described in claim 1, wherein the second magnetic separation step is performed by wet magnetic separation, a magnet is placed at the 3 o'clock position on the drum, a non-magnetic material 1 slurry is added from the 12 o'clock to 2 o'clock direction on the drum, and the drum is rotated counterclockwise using a drum-type wet magnetic separation method.

10. A method for recovering valuable materials from a lithium ion secondary battery as described in claim 1, wherein the second magnetic separation process is carried out by adding a dispersant to the non-magnetic material 1 obtained in the first magnetic separation process.

11. A method for recovering valuable materials from a lithium ion secondary battery as described in claim 1 or 2, wherein in the recovery process, the magnetized material 1 and the magnetized material 2 are washed and subjected to solid-liquid separation to recover valuable materials.

12. A method for recovering valuables from a lithium ion secondary battery as described in claim 1 or 2, comprising recovering copper from the coarse product 2.

Citation Information

Patent Citations

  • Method for recovering valuables from lithium ion secondary battery

    JP2015219948A

  • Method for collecting valuable substance from used lithium ion battery

    JP2017174517A

  • How to collect valuables

    JP6948481B2

  • Separation method for valuable resources

    WO2021157483A1

  • Method for recovering valuable substance