Semiconductor Device
The semiconductor device addresses heat dissipation inefficiencies by varying diamond crystal grain density and size in the diamond layer to enhance heat radiation while preserving semiconductor integrity.
Patent Information
- Application Number
- JP2020082006
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-07
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-05-07
AI Technical Summary
Existing semiconductor devices using nitride semiconductors face inefficiencies in heat dissipation due to the use of diamond layers that either damage the semiconductor or inhibit heat conduction through insulating films.
A semiconductor device with a diamond layer composed of a plurality of diamond crystal grains, where the number density and average grain size are strategically varied across surfaces to enhance heat radiation without damaging the semiconductor, utilizing a manufacturing process that minimizes exposure to hydrogen gas.
The solution enables efficient heat radiation and maintains the semiconductor's characteristics by forming a diamond layer with higher diamond crystal grain density and smaller grain size on one surface, reducing sheet resistance and preventing semiconductor damage.
Smart Images

Figure 0007571390000001 
Figure 0007571390000002 
Figure 0007571390000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a semiconductor device. [Background technology]
[0002] Nitride semiconductors have characteristics such as a high saturation electron velocity and a wide band gap, and their application to high-voltage and high-power semiconductor devices is being considered. For example, the band gap of GaN, a nitride semiconductor, is 3.4 eV, which is larger than the band gap of Si (1.1 eV) and the band gap of GaAs (1.4 eV), and has a high breakdown electric field strength. Therefore, nitride semiconductors such as GaN are extremely promising materials for semiconductor devices for power supplies that operate at high voltages and obtain high power. As semiconductor devices using nitride semiconductors, many reports have been made on field effect transistors, particularly high electron mobility transistors (HEMTs).
[0003] In such a HEMT using a nitride semiconductor, a high voltage is applied and a large current flows, so that heat is generated in a large amount, and therefore efficient heat dissipation is required. For example, a technique is known in which a diamond layer is deposited using a chemical vapor deposition (CVD) method. Specifically, a technique is known in which diamond synthesized using a CVD method is bonded to the back surface of a substrate on which a semiconductor device that generates a large amount of heat, such as a laser diode, or a semiconductor device using a nitride semiconductor such as gallium nitride (GaN) is provided (for example, Patent Document 1). In addition, a technique is known in which an insulating film such as TiC or AlC is formed on the front surface of a substrate on which a similar semiconductor device is provided, and then a diamond layer is laminated (for example, Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2016-539510 [Patent Document 2] JP 2007-157829 A [Non-patent literature]
[0005] [Non-Patent Document 1] Diamond Relat. Mater. 10, 744 (2001) [Non-Patent Document 2] Appl. Phys. Lett. 111, 041901 (2017) Summary of the Invention [Problem to be solved by the invention]
[0006] However, as described in Patent Document 1, providing diamond on the back surface of the substrate does not provide efficient heat dissipation, and as described in Patent Document 2, when an insulating film is formed on the front surface of the substrate and a diamond layer is then formed on the insulating film, heat conduction is inhibited in the insulating film, and efficient heat dissipation is not achieved.
[0007] For this reason, there is a demand for a semiconductor device that can dissipate heat efficiently. [Means for solving the problem]
[0008] According to one aspect of this embodiment, there is provided a semiconductor laminated structure, a gate electrode, a source electrode and a drain electrode formed on the semiconductor laminated structure, and a diamond layer formed on the semiconductor laminated structure, the diamond layer having a first surface on the semiconductor laminated structure side and a second surface opposite to the first surface, the diamond layer being composed of a plurality of diamond crystal grains, the diamond layer covering the gate electrode, the source electrode and the drain electrode, the number density of the plurality of diamond crystal grains on the first surface being higher than the number density on the second surface, and the average grain size of the plurality of diamond crystal grains on the first surface being 1 μm or less. the plurality of diamond grains has an average grain size at the second surface of greater than 1 μm, the plurality of diamond grains including a first diamond grain having a third surface that forms a portion of the first surface and a fourth surface that forms a portion of the second surface. A semiconductor device having the above structure is provided. Effect of the Invention
[0009] According to the present disclosure, heat can be dissipated efficiently. [Brief description of the drawings]
[0010] [Figure 1] 1 is a structural diagram of a semiconductor device according to a first embodiment. [Diagram 2] 1 is a process diagram (1) of the method for manufacturing a semiconductor device according to the first embodiment. [Diagram 3] 4 is a process diagram (2) of the method for manufacturing the semiconductor device according to the first embodiment. FIG. [Figure 4] 4 is a process diagram (3) of the method for manufacturing the semiconductor device according to the first embodiment. FIG. [Diagram 5] FIG. 4 is a process diagram (4) of the method for manufacturing the semiconductor device according to the first embodiment. [Figure 6] FIG. 1 is an explanatory diagram of sheet resistance in a semiconductor device. [Figure 7] FIG. 1 is a structural diagram of a semiconductor device used to measure sheet resistance (1). [Figure 8] FIG. 2 is a structural diagram of the semiconductor device used to measure the sheet resistance (2). [Figure 9] 1 is a SEM image of a cross section of a diamond layer. [Figure 10] 1 is an SEM image of the top surface of the diamond layer. [Figure 11] This is an SEM image of the top surface at the early stage of crystal growth. [Figure 12] 11 is a structural diagram of a semiconductor device according to a second embodiment. FIG. [Figure 13] 11 is a structural diagram of a semiconductor device according to a third embodiment. FIG. [Figure 14] FIG. 13 is a diagram showing a discrete package according to a fourth embodiment. [Figure 15] FIG. 13 is a wiring diagram showing a PFC circuit according to a fifth embodiment. [Figure 16] FIG. 13 is a wiring diagram showing a power supply device according to a sixth embodiment. [Figure 17] FIG. 13 is a wiring diagram showing an amplifier according to a seventh embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. In this specification and the drawings, components having substantially the same functional configurations are denoted by the same reference numerals, and redundant description may be omitted.
[0012] (First embodiment) Diamond is one of the materials with high thermal conductivity. It is considered that by providing a diamond layer with high thermal conductivity on a substrate including a heat generating body such as a semiconductor device, the heat generated in the substrate can be dissipated through the diamond layer. However, when a diamond layer is formed on the surface of a substrate on which a semiconductor device using a nitride semiconductor such as GaN is provided by a CVD method, the hydrogen gas used in forming the diamond layer causes Ga to be desorbed from the nitride semiconductor such as GaN, damaging the nitride semiconductor, changing the characteristics of the semiconductor device, and making it impossible to obtain good characteristics.
[0013] For this reason, it is possible to form an insulating film as a protective film on the nitride semiconductor, and then form a diamond layer on the formed insulating film. However, in order to prevent damage to the nitride semiconductor when forming the diamond layer, a certain thickness of the insulating film is required. However, since the thermal conductivity of the insulating film is lower than that of diamond, heat dissipation is not efficient. In addition, if the insulating film is made thin in order to efficiently dissipate heat through the diamond layer, the insulating film is also etched by the hydrogen gas used when stacking diamond, and the nitride semiconductor is damaged, which may prevent the semiconductor device from obtaining good characteristics.
[0014] [Semiconductor Device] Next, a semiconductor device according to a first embodiment will be described with reference to Fig. 1. In the semiconductor device 100 according to the first embodiment, nitride semiconductor layers such as a nucleation layer 11, a buffer layer 12, an electron transit layer 21, and an electron supply layer 22 are formed on a substrate 10 by a metal organic vapor phase epitaxy (MOVPE) method. The nitride semiconductor layers such as the nucleation layer 11, the buffer layer 12, the electron transit layer 21, and the electron supply layer 22 are included in a nitride semiconductor stacked structure 20. In this embodiment, a case where the nitride semiconductor layers are formed by an MOCVD method will be described, but they may be formed by a molecular beam epitaxy (MBE) method.
[0015] In the electron transit layer 21, a 2DEG 21a is generated near the interface between the electron transit layer 21 and the electron supply layer 22. In addition, a gate electrode 31, a source electrode 32, and a drain electrode 33 are formed on the electron supply layer 22. Note that a cap layer (not shown) may be formed on the electron supply layer 22, and the gate electrode 31, the source electrode 32, and the drain electrode 33 may be formed on the cap layer.
[0016] The substrate 10 is made of silicon carbide (SiC), sapphire (Al 2 O 3 ), silicon (Si), GaN, zinc oxide (ZnO), etc. are used. The nucleation layer 11 is formed of AlN having a thickness of, for example, 160 nm, and the buffer layer is formed of AlGaN having a thickness of, for example, 500 nm, in which the Al composition ratio is gradually changed as the film is formed.
[0017] The electron transit layer 21 is made of i-GaN with a thickness of about 1 μm. The electron supply layer 22 is made of Al 0.2 Ga 0.8 The electron supply layer 22 is made of N. The electron supply layer 22 may be made of InAlN or InAlGaN.
[0018] A diamond layer 50 is formed on the semiconductor laminate structure 20. The diamond layer 50 has a first surface 50A on the semiconductor laminate structure 20 side and a second surface 50B opposite to the first surface 50A, and is composed of a plurality of diamond crystal grains 51. The diamond layer 50 has a thickness of, for example, 1 μm or more.
[0019] The plurality of diamond crystal grains 51 includes a first diamond crystal grain 61 and a second diamond crystal grain 62. The first diamond crystal grain 61 includes a third face 61A that constitutes a part of the first face 50A and a fourth face 61B that constitutes a part of the second face 50B. The second diamond crystal grain 62 is smaller in height than the first diamond crystal grain 61 and includes a face 62A that constitutes a part of the first face 50A, but does not include a face that constitutes a part of the second face 50B. The plurality of diamond crystal grains 51 may include another diamond crystal grain that is located above the second diamond crystal grain 62, is smaller in height than the first diamond crystal grain 61, and does not include a face that constitutes a part of either the first face 50A or the second face 50B.
[0020] The number density of the plurality of diamond crystal grains 51 on the first surface 50A is higher than the number density on the second surface 50B. For example, the number density of the plurality of diamond crystal grains 51 on the first surface 50A is 1×10 8 cm -2 The number density of the plurality of diamond crystal grains 51 on the second surface 50B is 1×10 8 cm -2 The number density of the plurality of diamond crystal grains 51 on the first surface 50A is, for example, 1×10 8 cm -2 More than 1×10 12 cm -2 It may be the following.
[0021] The average grain size of the plurality of diamond crystal grains 51 on the first surface 50A is 1 μm or less. The average grain size of the plurality of diamond crystal grains 51 on the first surface 50A may be, for example, 5 nm or more and 1 μm or less. The average grain size of the plurality of diamond crystal grains 51 on the first surface 50A is preferably 5 nm or more and 100 nm or less, and more preferably 5 nm or more and 20 nm or less.
[0022] The average grain size of the plurality of diamond crystal grains 51 on the second surface 50B is greater than 1 μm.
[0023] In the semiconductor device 100 of the first embodiment, the diamond layer 50 is provided so as to be in direct contact with the semiconductor laminate structure 20, so that heat generated in the channel including the 2DEG 21a during operation of the semiconductor device 100 can be efficiently dissipated.
[0024] The thermal conductivity of a diamond layer formed from diamonds having a small average grain size of about 5 nm is about 10 W / m·K. In contrast, the thermal conductivity of a diamond layer formed from diamonds having a large average grain size of more than 1 μm is about 2000 W / m·K. For this reason, it is preferable that the second diamond grains 62 are provided in a thin layer shape. For example, as will be described later, it is preferable that the second diamond grains 62 are formed in a layer shape as thin as possible when the first diamond grains 61 are formed, within a range that does not damage the semiconductor laminate structure 20.
[0025] Diamond crystal grains with a small average grain size can be formed at a lower temperature than diamond crystal grains with a large average grain size, and in some cases can be formed without being exposed to radical hydrogen, etc. Therefore, by providing a plurality of diamond crystal grains with a small average grain size on the semiconductor laminate structure 20 and growing diamond crystal grains with a large average grain size from some of these diamond crystal grains, the diamond layer 50 can be formed without damaging the semiconductor laminate structure 20. This makes it possible to suppress the deterioration of the characteristics of the semiconductor device 100 when forming the diamond layer 50.
[0026] [Method of manufacturing a semiconductor device] Next, a method for manufacturing the semiconductor device 100 according to the first embodiment will be described.
[0027] First, as shown in FIG. 2, a semiconductor laminated structure 20 including a nucleation layer 11, a buffer layer 12, an electron transit layer 21, an electron supply layer 22, etc. is formed on a substrate 10 by a crystal growth method such as MOVPE or molecular beam epitaxy (MBE). When the semiconductor laminated structure 20 including the nucleation layer 11, the buffer layer 12, the electron transit layer 21, the electron supply layer 22, etc. is formed by MOVPE, a mixed gas of trimethylaluminum gas, trimethylgallium gas, and ammonia gas is used as a source gas. The film is formed by adjusting the supply and flow rate of trimethylaluminum gas as an Al source and trimethylgallium gas as a Ga source according to the composition of the nitride semiconductor layer to be formed. The flow rate of the ammonia gas supplied is 100 ccm to 10 LM. Furthermore, the pressure in the chamber when forming the semiconductor laminated structure 20 is about 7 kPa (50 Torr) to about 40 kPa (300 Torr), and the film formation temperature is 1000° C. to 1200° C. When the electron supply layer 22 is formed of InAlGaN, the pressure in the chamber is about 7 kPa (50 Torr) to about 27 kPa (200 Torr), and the film formation temperature is 650° C. to 800° C. Trimethylindium gas can be used when growing a semiconductor layer containing In.
[0028] Next, as shown in FIG. 3, a gate electrode 31, a source electrode 32, and a drain electrode 33 are formed on the semiconductor laminate structure 20.
[0029] Next, as shown in FIG. 4, a diamond layer 70 consisting of a plurality of nanodiamond particles 71 is formed on the semiconductor laminated structure 20, the gate electrode 31, the source electrode 32, and the drain electrode 33. The nanodiamond particles 71 are an example of diamond particles. Specifically, the diamond layer 70 is formed by attaching a plurality of nanodiamond particles 71 onto the semiconductor laminated structure 20, etc. For example, the electron supply layer 22, etc. is immersed in an aqueous solution in which a plurality of nanodiamond particles 71 are dispersed, and the nanodiamond particles 71 are attached onto the semiconductor laminated structure 20, etc., to form the diamond layer 70. For example, the average particle size of the nanodiamond particles 71 is 5 nm or more and 1 μm or less, and the number density of the nanodiamond particles 71 on the surface of the diamond layer 70 facing the semiconductor laminated structure 20 is 1×10 8 cm -2 ~1×10 12 cm -2 Another method for forming the diamond layer 70 is the bias enhanced nucleation (BEN) method. However, the method of attaching the nanodiamond particles 71 dispersed in an aqueous solution or the like to the surface of the semiconductor laminated structure 20 or the like as described above is preferable because it causes less damage to the semiconductor laminated structure 20.
[0030] Next, as shown in FIG. 5, the diamond layer 50 is formed by growing diamond crystal grains using the nanodiamond particles 71 as growth nuclei by the CVD method, and is composed of a plurality of diamond crystal grains 51. A mixture of methane gas and hydrogen gas is used as the raw material gas. Depending on the growth conditions, oxygen gas or nitrogen gas may be supplied into the CVD chamber. The ratio of methane gas to hydrogen gas is about 0.05% by volume to 10% by volume. The growth pressure is about 0.5 kPa to 100 kPa, and the growth temperature is about 350°C to 1200°C. The crystal growth is anisotropic, and during the formation of the diamond layer 50, some diamond crystal grains come into contact with each other, and the growth of the diamond crystal grains located between them is hindered. The diamond crystal grains that can grow without being hindered by other diamond crystal grains become the first diamond crystal grains 61, and the diamond crystal grains whose growth is hindered by the first diamond crystal grains 61 become the second diamond crystal grains 62. As described above, the plurality of diamond crystal grains 51 may include another diamond crystal grain that is located above the second diamond crystal grain 62, has a smaller height than the first diamond crystal grain 61, and does not have a surface that forms part of either the first surface 50A or the second surface 50B.
[0031] In this manner, the semiconductor device 100 according to the first embodiment can be manufactured.
[0032] However, if the density of nanodiamonds on the semiconductor laminate structure 20 is low, the surface of the semiconductor laminate structure 20 is exposed to hydrogen gas for a long time during the crystal growth using the nanodiamonds as nuclei. 8 cm -2 ~1×10 12 cm -2A diamond layer 70 is formed, which is composed of nanodiamond particles 71 with a high number density, and substantially covers the surface of the semiconductor laminate structure 20. This makes it possible to prevent the semiconductor laminate structure 20 from being exposed to hydrogen gas, prevent damage to the semiconductor laminate structure 20, and suppress deterioration of the characteristics of the manufactured semiconductor device 100. Note that, for the sake of convenience of explanation, gaps exist between the nanodiamond particles 71 in FIG. 4, but the nanodiamond particles 71 having an average particle size of 5 nm or more and 1 μm or less are arranged in a number of 1×10 8 cm -2 ~1×10 12 cm -2 When the nanodiamond particles 71 are arranged at a density of 1000 or more, adjacent nanodiamond particles 71 come into contact with each other. Also, some nanodiamond particles 71 may overlap each other in the stacking direction of the semiconductor stacked structure 20.
[0033] FIG. 6 shows the sheet resistance of each semiconductor device. The semiconductor device 6A is a semiconductor device in which no diamond layer is formed on the semiconductor laminate structure 20, etc., as shown in FIG. 7. The semiconductor device 6B is a semiconductor device 100 according to the first embodiment, in which a diamond layer 50 is formed, as shown in FIG. 1. The semiconductor device 6C is a semiconductor device in which a diamond layer 950 is formed, which is composed of a plurality of diamond crystal grains 81 as large as the first diamond crystal grains 61, as shown in FIG. 8. In this semiconductor device 6C, the diamond crystal grains 81 are grown on the semiconductor laminate structure 20 by the CVD method, without providing nanodiamond grains with a small average grain size, to form the diamond layer 950.
[0034] 6, in the semiconductor device 100 according to the first embodiment shown in the semiconductor device 6B, the sheet resistance of the semiconductor stack 20 is similar to that of the semiconductor device 6A, and an increase in the sheet resistance is suppressed. From this, it can be confirmed that in the semiconductor device 100 according to the first embodiment, even if the diamond layer 50 is formed, no damage accompanying the formation of the diamond layer 50 occurs in the semiconductor stack 20.
[0035] The semiconductor device 6C has a significantly high sheet resistance. This is because the semiconductor laminate structure 20 is exposed to hydrogen gas for a long time when the diamond layer 950 is formed, and the semiconductor laminate structure 20 is damaged by, for example, desorption of Ga. An increase in sheet resistance leads to an increase in on-resistance.
[0036] FIG. 9 is a cross-sectional scanning electron microscope (SEM) image of a diamond layer 50 including a first diamond crystal grain 61 and a second diamond crystal grain 62 formed on a nitride semiconductor layer, and FIG. 10 is an SEM image of the diamond layer 50 indicated by an arrow in FIG. 9 viewed from above. In the formation of the diamond layer 50 shown in FIG. 9 and FIG. 10, after the diamond layer 70 is formed, crystal growth is performed for about 7 hours. The thickness of this diamond layer 50 is about 2.5 μm. As shown in FIG. 9 and FIG. 10, it is confirmed that the average grain size on the second surface 50B of the multiple diamond crystal grains 51 constituting the diamond layer 50 is more than 1 μm.
[0037] Fig. 11 is a cross-sectional SEM image of the diamond layer 70 after the diamond layer 70 is formed and the diamond is grown for about 10 minutes. The nanodiamond particles 71 constituting the diamond layer 70 have an average grain size of about 10 nm and cannot be confirmed by SEM, but by growing the diamond for 10 minutes, the diamond grains become larger and can be confirmed by SEM. As shown in Fig. 11, the diamond grains in this state are small, with an average grain size of about 50 nm to 100 nm, but by growing the diamond for a long period of time, diamond grains with an average grain size of more than 1 μm can be obtained, as shown in Fig. 10.
[0038] Second embodiment Next, the semiconductor device according to the second embodiment will be described. In the semiconductor device 200 according to the second embodiment, as shown in FIG. 12, an insulating film 140 is formed on the semiconductor laminated structure 20, and a diamond layer 50 is formed on the insulating film 140. The thickness of the insulating film 140 is, for example, 0.5 nm or more and 10 nm or less. From the viewpoint of thermal conduction, it is preferable that the insulating film 140 is not formed. On the other hand, in order to further suppress the damage that the semiconductor laminated structure 20 receives during the crystal growth of diamond, the insulating film 140 may be formed on the semiconductor laminated structure 20, and the diamond layer 50 may be formed on the insulating film 140.
[0039] The insulating film 140 may be made of silicon nitride (SiN), SiO 2 (silicon oxide), AlN (aluminum nitride), Al 2 O 3 (aluminum oxide), HfO 2 (Hafnium oxide), etc.
[0040] The other configurations are similar to those of the first embodiment.
[0041] Third embodiment Next, the semiconductor device according to the third embodiment will be described. In the semiconductor device 300 according to the third embodiment, as shown in FIG. 13, a diamond layer 50 is formed on the semiconductor laminate structure 20 formed on one surface 10a of the substrate 10, and a back surface diamond layer 250 is formed on the other surface 10b. This makes it possible to obtain a higher heat dissipation effect. The back surface diamond layer 250 is an example of a second diamond layer.
[0042] The back surface diamond layer 250 formed on the other surface 10b, which is the back surface of the substrate 10, may be polycrystalline or single crystalline. The back surface diamond layer 250 may be formed by forming growth nuclei and growing crystals, similar to the diamond layer 50. As the back surface diamond layer 250, a single crystal diamond or a polycrystalline diamond may be bonded to the surface 10b. The thickness of the back surface diamond layer 250 is preferably 1 μm or more, and more preferably 2.5 μm.
[0043] The other configurations are similar to those of the first embodiment.
[0044] (Fourth embodiment) Next, a fourth embodiment will be described. The fourth embodiment relates to a discrete package of a HEMT. Fig. 14 is a diagram showing the discrete package according to the fourth embodiment.
[0045] In the fourth embodiment, as shown in FIG. 14, the back surface of a semiconductor device 1210 having a structure similar to any one of the first to third embodiments is fixed to a land (die pad) 1233 using a die attaching agent 1234 such as solder. A wire 1235d such as an Al wire is connected to a drain pad 1226d to which a drain electrode 108 is connected, and the other end of the wire 1235d is connected to a drain lead 1232d integrated with the land 1233. A wire 1235s such as an Al wire is connected to a source pad 1226s connected to a source electrode 107, and the other end of the wire 1235s is connected to a source lead 1232s independent from the land 1233. A wire 1235g such as an Al wire is connected to a gate pad 1226g connected to a gate electrode 109, and the other end of the wire 1235g is connected to a gate lead 1232g independent from the land 1233. The land 1233, the semiconductor device 1210, and the like are packaged in a mold resin 1231 so that a part of the gate lead 1232g, a part of the drain lead 1232d, and a part of the source lead 1232s protrude.
[0046] Such a discrete package can be manufactured, for example, as follows. First, the semiconductor device 1210 is fixed to the land 1233 of the lead frame using a die attaching agent 1234 such as solder. Next, by bonding using wires 1235g, 1235d, and 1235s, the gate pad 1226g is connected to the gate lead 1232g of the lead frame, the drain pad 1226d is connected to the drain lead 1232d of the lead frame, and the source pad 1226s is connected to the source lead 1232s of the lead frame. After that, sealing is performed using the molding resin 1231 by the transfer molding method. Then, the lead frame is separated.
[0047] Fifth embodiment Next, a fifth embodiment will be described. The fifth embodiment relates to a PFC (Power Factor Correction) circuit equipped with a HEMT. Fig. 15 is a wiring diagram showing a PFC circuit according to the fifth embodiment.
[0048] The PFC circuit 1250 includes a switch element (transistor) 1251, a diode 1252, a choke coil 1253, capacitors 1254 and 1255, a diode bridge 1256, and an AC power supply (AC) 1257. The drain electrode of the switch element 1251 is connected to the anode terminal of the diode 1252 and one terminal of the choke coil 1253. The source electrode of the switch element 1251 is connected to one terminal of the capacitor 1254 and one terminal of the capacitor 1255. The other terminal of the capacitor 1254 is connected to the other terminal of the choke coil 1253. The other terminal of the capacitor 1255 is connected to the cathode terminal of the diode 1252. A gate driver is connected to the gate electrode of the switch element 1251. The AC 1257 is connected between both terminals of the capacitor 1254 via the diode bridge 1256. A direct current power supply (DC) is connected between both terminals of the capacitor 1255. In this embodiment, a semiconductor device having the same structure as any one of the first to third embodiments is used for the switch element 1251.
[0049] When manufacturing the PFC circuit 1250, the switch element 1251 is connected to the diode 1252 and the choke coil 1253, etc., using, for example, solder or the like.
[0050] Sixth embodiment Next, a sixth embodiment will be described. The sixth embodiment relates to a power supply device equipped with a HEMT, suitable for a server power supply. Fig. 16 is a wiring diagram showing the power supply device according to the sixth embodiment.
[0051] The power supply device is provided with a high-voltage primary circuit 1261 , a low-voltage secondary circuit 1262 , and a transformer 1263 disposed between the primary circuit 1261 and the secondary circuit 1262 .
[0052] The primary side circuit 1261 is provided with a PFC circuit 1250 according to the fifth embodiment, and an inverter circuit, for example, a full-bridge inverter circuit 1260, connected between both terminals of a capacitor 1255 of the PFC circuit 1250. The full-bridge inverter circuit 1260 is provided with a plurality of (four in this case) switch elements 1264a, 1264b, 1264c, and 1264d.
[0053] The secondary side circuit 1262 is provided with a plurality of (three in this case) switch elements 1265a, 1265b, and 1265c.
[0054] In this embodiment, a semiconductor device having a structure similar to that of any one of the first to third embodiments is used for the switch element 1251 of the PFC circuit 1250 constituting the primary side circuit 1261, and the switch elements 1264a, 1264b, 1264c, and 1264d of the full bridge inverter circuit 1260. On the other hand, a normal MIS type FET (field effect transistor) using silicon is used for the switch elements 1265a, 1265b, and 1265c of the secondary side circuit 1262.
[0055] Seventh embodiment Next, a seventh embodiment will be described. The seventh embodiment relates to an amplifier including a HEMT. Fig. 17 is a wiring diagram showing the amplifier according to the seventh embodiment.
[0056] The amplifier includes a digital predistortion circuit 1271, mixers 1272a and 1272b, and a power amplifier 1273.
[0057] The digital predistortion circuit 1271 compensates for nonlinear distortion of the input signal. The mixer 1272a mixes the input signal, the nonlinear distortion of which has been compensated for, with an AC signal. The power amplifier 1273 includes a semiconductor device having a structure similar to that of any one of the first to third embodiments, and amplifies the input signal mixed with the AC signal. In this embodiment, for example, by switching a switch, the output side signal can be mixed with the AC signal by the mixer 1272b and sent to the digital predistortion circuit 1271. This amplifier can be used as a high-frequency amplifier or a high-output amplifier. The high-frequency amplifier can be used, for example, in a transmitting / receiving device for a mobile phone base station, a radar device, and a microwave generating device.
[0058] Although preferred embodiments have been described above in detail, the present invention is not limited to the above-described embodiments, and various modifications and substitutions can be made to the above-described embodiments without departing from the scope of the claims.
[0059] Various aspects of the present disclosure are summarized below as appendices.
[0060] (Appendix 1) A semiconductor laminate structure; a diamond layer formed on the semiconductor laminated structure, having a first surface on the semiconductor laminated structure side and a second surface opposite to the first surface, the diamond layer being made up of a plurality of diamond crystal grains; having a number density of the plurality of diamond grains on the first surface is higher than a number density of the plurality of diamond grains on the second surface; 13. A semiconductor device comprising: a first surface of the plurality of diamond crystal grains having an average grain size of 1 μm or less. (Appendix 2) The number density of the plurality of diamond grains on the first surface is 1×10 8 cm -2 The semiconductor device according to claim 1, characterized in that: (Appendix 3) 3. The semiconductor device according to claim 1, wherein the average grain size of the plurality of diamond crystal grains on the first surface is 5 nm or more and 100 nm or less. (Appendix 4) 4. The semiconductor device according to claim 1, wherein the average grain size of the plurality of diamond crystal grains on the first surface is 5 nm or more and 20 nm or less. (Appendix 5) 5. The semiconductor device according to claim 1, wherein the diamond layer has a thickness of 1 μm or more. (Appendix 6) A substrate having the semiconductor laminate structure formed on one surface thereof; a second diamond layer in contact with the other face of the substrate; and 6. The semiconductor device according to claim 1, further comprising: (Appendix 7) 7. The semiconductor device according to claim 1, further comprising an insulating film formed between the semiconductor multilayer structure and the diamond layer. (Appendix 8) The semiconductor device according to claim 7, wherein the insulating film has a thickness of 0.5 nm or more and 10 nm or less. (Appendix 9) The semiconductor laminate structure includes: an electron transit layer formed of a nitride semiconductor; an electron supply layer formed of a nitride semiconductor on the electron transport layer; having 9. The semiconductor device according to claim 1, further comprising a gate electrode, a source electrode, and a drain electrode formed on the electron supply layer. (Appendix 10) forming a diamond layer on a semiconductor laminated structure, the diamond layer having a first surface on the semiconductor laminated structure side and a second surface opposite to the first surface, the diamond layer being made up of a plurality of diamond crystal grains; The step of forming the diamond layer comprises: providing a plurality of diamond particles having an average particle size of 1 μm or less on the semiconductor laminate structure; growing a crystal using some of the diamond particles as growth nuclei; 1. A method for manufacturing a semiconductor device comprising the steps of: (Appendix 11) 10. An amplifier comprising the semiconductor device according to any one of claims 1 to 9. (Appendix 12) A power supply device comprising the semiconductor device according to any one of claims 1 to 9. [Explanation of symbols]
[0061] 10: Substrate 20: Semiconductor laminate structure 50: Diamond layer 50A: Side 1 50B: 2nd side 51: Diamond grain 61: First diamond grain 61A:Side 3 61B:Side 4 62: Second diamond grain 62A: Surface 70: Diamond layer 71: Nano diamond particles 81: Diamond grain 100, 200, 300: Semiconductor device 140: Insulating film 250: Diamond layer on the back
Claims
1. A semiconductor laminate structure; a gate electrode, a source electrode, and a drain electrode formed on the semiconductor laminate structure; a diamond layer formed on the semiconductor laminated structure, having a first surface on the semiconductor laminated structure side and a second surface opposite to the first surface, the diamond layer being made up of a plurality of diamond crystal grains; having the diamond layer covers the gate electrode, the source electrode and the drain electrode; a number density of the plurality of diamond grains on the first surface is higher than a number density of the plurality of diamond grains on the second surface; the average grain size of the plurality of diamond grains at the first surface is 1 μm or less; the average grain size of the plurality of diamond grains at the second face is greater than 1 μm; the plurality of diamond grains includes a first diamond grain; The first diamond grains are A third surface that constitutes a part of the first surface; A fourth surface that constitutes a part of the second surface; A semiconductor device comprising:
2. The number density of the plurality of diamond grains on the first surface is 1×10 8 cm -2 2. The semiconductor device according to claim 1, wherein:
3. A substrate having the semiconductor laminate structure formed on one surface thereof; a second diamond layer in contact with the other face of the substrate; 3. The semiconductor device according to claim 1, further comprising:
4. 4. The semiconductor device according to claim 1, further comprising an insulating film formed between said semiconductor laminate structure and said diamond layer.
5. The semiconductor laminate structure includes: an electron transit layer formed of a nitride semiconductor; an electron supply layer formed of a nitride semiconductor on the electron transport layer; 5. The semiconductor device according to claim 1, further comprising:
Citation Information
Patent Citations
Diamond film for cutting tool
JP1993148089A
Forming method of diamond coating film
JP1993339730A
Vapor synthesized diamond and its production
JP1998081586A
Semiconductor device
JP2007157829A
Semiconductor device
JP2016096318A