Resin composition, resin film with carrier using same, resin substrate, prepreg, metal-clad laminate, printed wiring board, and semiconductor device
The resin composition with cyclic urea compound addresses the limitations of Patent Document 1 by improving flame retardancy and dielectric properties, ensuring effective insulation and reliability in circuit boards.
Patent Information
- Application Number
- JP2020144707
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-28
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-08-28
Smart Images

Figure 0007571423000010 
Figure 0007571423000011 
Figure 0007571423000012
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, and a resin film with a carrier, a resin substrate, a prepreg, a metal-clad laminate, a printed wiring board, and a semiconductor device using the same. [Background technology]
[0002] Various developments have been made so far regarding resin compositions used for printed wiring boards. For example, the technology described in Patent Document 1 is known as this type of technology. Patent Document 1 describes a polyphenylene ether resin composition containing a modified polyphenylene ether copolymer, a crosslinking curing agent, and an inorganic filler (Table 1 of Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-113543 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, as a result of investigations conducted by the present inventors, it was found that the resin composition described in Patent Document 1 above still has room for improvement in terms of high flame retardancy and low dielectric properties. [Means for solving the problem]
[0005] In the resin composition of Patent Document 1, a general phosphorus-based flame retardant is used from the viewpoint of improving flame retardancy. However, when a phosphorus-based flame retardant is used, there is a risk that phosphoric acid may be eluted from a member using the resin composition, which may cause wiring corrosion or the like, thereby raising concerns about a decrease in the insulation reliability of a printed wiring board.
[0006] In view of the above circumstances, the present inventors have investigated flame retardants that can replace phosphorus-based flame retardants and have found that by using an appropriate nitrogen-based flame retardant, it is possible to obtain a desired flame retardancy while suppressing phosphoric acid elution. As a result of further intensive research based on this knowledge, it was found that by using a cyclic urea compound as a nitrogen-based flame retardant, it is possible to improve the flame retardancy of the cured product of a resin composition for circuit boards while reducing its dielectric tangent, and thus the present invention was completed.
[0007] According to the present invention, A resin composition for a circuit board, Polyphenylene ether, a crosslinking agent reactive with the polyphenylene ether; A filler material; A cyclic urea compound, A resin composition is provided.
[0008] Further, according to the present invention, A carrier substrate; There is provided a resin film with a carrier, comprising: a resin film formed on the carrier base material and made of the above-mentioned resin composition.
[0009] Further, according to the present invention, There is provided a resin substrate having an insulating layer made of a cured product of the above-mentioned resin composition.
[0010] Further, according to the present invention, A prepreg is provided which comprises a fibrous substrate in the above resin composition.
[0011] Further, according to the present invention, There is provided a metal-clad laminate comprising a resin film made of the above resin composition, the above resin substrate, or the above prepreg, and a metal layer disposed on at least one surface of the resin film.
[0012] Further, according to the present invention, A printed wiring board is provided, in which a circuit layer is formed on the surface of the metal-clad laminate.
[0013] Further, according to the present invention, The above printed wiring board; and a semiconductor element mounted on a circuit layer of the printed wiring board or embedded in the printed wiring board. Effect of the Invention
[0014] According to the present invention, there are provided a resin composition having excellent flame retardancy and low dielectric properties, and a resin film with a carrier, a resin substrate, a prepreg, a metal-clad laminate, a printed wiring board, and a semiconductor device using the same. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a cross-sectional view showing an example of the configuration of a resin film with a carrier in the present embodiment. [Diagram 2] 1 is a cross-sectional view showing an example of a configuration of a printed wiring board according to an embodiment of the present invention. [Diagram 3] 1 is a cross-sectional view showing an example of the configuration of a semiconductor device according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given similar reference numerals and their explanations will be omitted as appropriate. Also, the drawings are schematic diagrams and do not correspond to the actual dimensional ratios.
[0017] The resin composition of the present embodiment will be outlined.
[0018] The resin composition of the present embodiment contains polyphenylene ether, a crosslinking agent reactive with the polyphenylene ether, a filler, and a cyclic urea compound. Such a resin composition is a resin composition for circuit boards, which is used to form a member that constitutes at least a part of a circuit board.
[0019] According to the findings of the present inventors, it has been found that by using a cyclic urea compound as a nitrogen-based flame retardant in a resin composition containing polyphenylene ether, a crosslinking agent, and a filler, it is possible to improve the flame retardancy and low dielectric properties of the cured product of the flame-retardant resin composition.
[0020] Although the detailed mechanism is unclear, it is believed that the above-mentioned cyclic urea compounds are moderately compatible with polymer components such as polyphenylene ether, remain without volatilizing even in high temperature environments, and have a relatively large amount of residual components containing nitrogen atoms, which increases the flame retardancy of the cured product of a resin composition to which they are added and reduces the dielectric tangent at relatively high frequencies.
[0021] In this embodiment, examples of the insulating layer in the printed wiring board include insulating members that constitute the printed wiring board, such as a core layer, a build-up layer (interlayer insulating layer), and a solder resist layer.
[0022] Examples of the printed wiring board include a printed wiring board having a core layer, a build-up layer (interlayer insulating layer), and a solder resist layer, a printed wiring board not having a core layer, a coreless substrate used in a panel package process (PLP), and an MIS (Molded Interconnect Substrate) substrate.
[0023] The cured resin film made of the resin composition of the present embodiment can be suitably used for build-up layers, such as build-up layers in printed wiring boards having no core layer, build-up layers in coreless boards used in PLP, build-up layers in MIS boards, etc. In addition, in a large-area printed wiring board used to collectively produce a plurality of semiconductor packages, the cured resin film can be used for build-up layers constituting the printed wiring board, and can also be applied to build-up layers constituting the printed wiring board in a system to which a large current is supplied.
[0024] Each component of the resin composition of the present embodiment will be described in detail below.
[0025] (Polyphenylene ether) The resin composition contains polyphenylene ether, which makes it possible to realize an insulating layer having a low dielectric constant and a low dielectric loss tangent, thereby providing a circuit board having excellent high frequency characteristics. The polyphenylene ether is not particularly limited as long as it contains, in the molecule, one or more functional groups capable of undergoing a crosslinking reaction with a crosslinking agent.
[0026] An example of the polyphenylene ether may include one or more polymers having a structural unit represented by the following general formula (1).
[0027] [ka]
[0028] In the above general formula (1), R1, R2, R3, and R4 may be the same or different and represent any one selected from the group consisting of a hydrogen atom, a halogen atom, an optionally substituted alkyl group, an optionally substituted alkenyl group, an optionally substituted alkynyl group, an optionally substituted aryl group, an optionally substituted aralkyl group, and an optionally substituted alkoxy group.
[0029] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, etc. Preferred are a chlorine atom and a bromine atom.
[0030] The "alkyl group" in the above-mentioned optionally substituted alkyl group is, for example, a linear or branched alkyl group having a carbon number of 1 or more and 6 or less, preferably a carbon number of 1 or more and 3 or less. More specific examples include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, and the like, and a methyl group or an ethyl group is more preferable.
[0031] Examples of the "alkenyl group" in the optionally substituted alkenyl group include ethenyl, 1-propenyl, 2-propenyl, 3-butenyl, pentenyl, and hexenyl groups, with ethenyl and 1-propenyl groups being more preferred.
[0032] Examples of the "alkynyl group" in the above-mentioned optionally substituted alkynyl group include an ethynyl group, a 1-propynyl group, a 2-propynyl (propargyl) group, a 3-butynyl group, a pentynyl group, and a hexynyl group, and are more preferably an ethynyl group, a 1-propynyl group, or a 2-propynyl (propargyl) group.
[0033] Examples of the "aryl group" in the above-mentioned optionally substituted aryl group include a phenyl group, a naphthyl group, etc., and a phenyl group is more preferable.
[0034] Examples of the "aralkyl group" in the optionally substituted aralkyl group include a benzyl group, a phenethyl group, a 2-methylbenzyl group, a 4-methylbenzyl group, an α-methylbenzyl group, a 2-vinylphenethyl group, a 4-vinylphenethyl group, and the like, with a benzyl group being more preferable.
[0035] The "alkoxy group" in the above-mentioned alkoxy group which may be substituted is, for example, a linear or branched alkoxy group having a carbon number of 1 to 6, preferably a carbon number of 1 to 3. Examples include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, a sec-butoxy group, a tert-butoxy group, a pentyloxy group, a hexyloxy group, etc., and a methoxy group or an ethoxy group is more preferable.
[0036] When the above alkyl groups, aryl groups, alkenyl groups, alkynyl groups, aralkyl groups and alkoxy groups are substituted, they may have one or more substituents. Examples of such a substituent include halogen atoms (e.g., fluorine atom, chlorine atom, bromine atom), alkyl groups having 1 to 6 carbon atoms (e.g., methyl group, ethyl group, propyl group, isopropyl group, butyl group, isobutyl group, sec-butyl group, tert-butyl group, pentyl group, hexyl group), aryl groups (e.g., phenyl group, naphthyl group), alkenyl groups (e.g., ethenyl group, 1-propenyl group, 2-propenyl group), alkynyl groups (e.g., ethynyl group, 1-propynyl group, 2-propynyl group), aralkyl groups (e.g., benzyl group, phenethyl group), alkoxy groups (e.g., methoxy group, ethoxy group), and the like.
[0037] The polyphenylene ether may have a structural unit represented by the following general formula (1a).
[0038] [ka]
[0039] In the above general formula (1a), R 11 ,R 12 ,R 13 ,R 14 ,R 15 ,R 16 ,R 17 ,R 18 may be the same or different and are a hydrogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group. -A- is a linear, branched or cyclic divalent hydrocarbon group having 20 or less carbon atoms.
[0040] The polyphenylene ether may include modified polyphenylene ether functionalized in part or in whole with an ethylenically unsaturated group such as a vinylbenzyl group, an epoxy group, an amino group, a hydroxyl group, a mercapto group, a carboxyl group, a silyl group, or the like.
[0041] In addition, it is preferable that the polyphenylene ether has a hydroxy group, an epoxy group, or an ethylenically unsaturated group at both ends. Examples of the ethylenically unsaturated group include alkenyl groups such as ethenyl, allyl, methacrylic, propenyl, butenyl, hexenyl, and octenyl, cycloalkenyl groups such as cyclopentenyl and cyclohexenyl, and alkenylaryl groups such as vinylbenzyl and vinylnaphthyl. In addition, both ends may be the same functional group or different functional groups.
[0042] The weight average molecular weight of the polyphenylene ether is preferably 500 to 5000, more preferably 1000 to 4000. By making the weight average molecular weight of the polyphenylene ether equal to or greater than the lower limit, the flexibility of the resulting resin layer can be improved. On the other hand, by making the weight average molecular weight of component (A) equal to or less than the upper limit, the solubility in chemical solutions can be improved.
[0043] The content of polyphenylene ether is 2 to 30% by weight, preferably 2.5 to 25% by weight, and more preferably 3 to 20% by weight, based on 100% by weight of the solid content of the resin composition. By making it equal to or more than the lower limit, low dielectric properties can be realized. By making it equal to or less than the upper limit, resin residue can be suppressed.
[0044] In this embodiment, the solid content of the resin composition refers to the non-volatile content in the resin composition, and refers to the remainder excluding volatile components such as water, solvent, etc. When a solvent is included, the content relative to the total solid content of the resin composition refers to the content relative to the total solid content (100% by weight) of the resin composition excluding the solvent.
[0045] (Crosslinking agent) The resin composition includes a crosslinking agent that reacts with the polyphenylene ether. The crosslinking agent may include at least one of an addition polymerization type and a radical polymerization type.
[0046] The crosslinking agent includes at least one or more selected from the group consisting of maleimide compounds, cyanate ester resins, phenolic resins, epoxy resins, and compounds having two or more carbon-carbon unsaturated double bonds in one molecule.
[0047] The maleimide compound, cyanate ester resin, phenol resin, and epoxy resin can form crosslinks between functional groups contained in these molecules and functional groups of the polyphenylene ether.
[0048] For example, a maleimide compound may be used in combination with a polyphenylene ether having an ethylenically unsaturated group at both ends and / or in -A- in general formula (1a). Also, at least one of a cyanate ester resin, a phenol resin and an epoxy resin may be used in combination with a polyphenylene ether having hydroxy groups at both ends and / or in -A- in general formula (1a).
[0049] The maleimide group of the maleimide compound has a planar structure of a five-membered ring, and the double bond of the maleimide group is highly polar and easily interacts with molecules, so that it exhibits strong intermolecular interactions with the maleimide group, benzene ring, other compounds having a planar structure, etc., and can suppress molecular motion. Therefore, by including a maleimide compound in the resin composition, the linear expansion coefficient of the obtained insulating layer can be reduced, the glass transition temperature can be improved, and further, the heat resistance can be improved.
[0050] The maleimide compound is preferably a bismaleimide compound having at least two maleimide groups in the molecule. Examples of maleimide compounds having at least two maleimide groups in the molecule include compounds having two maleimide groups in the molecule, such as 4,4'-diphenylmethane bismaleimide, m-phenylene bismaleimide, p-phenylene bismaleimide, 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, bis-(3-ethyl-5-methyl-4-maleimidophenyl)methane, 4-methyl-1,3-phenylene bismaleimide, N,N'-ethylene dimaleimide, N,N'-hexamethylene dimaleimide, bis(4-maleimidophenyl)ether, bis(4-maleimidophenyl)sulfone, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethane bismaleimide, and bisphenol A diphenyl ether bismaleimide; and polymaleimide compounds having three or more maleimide groups in the molecule, such as polyphenylmethane maleimide. One of these may be used alone, or two or more of them may be used in combination.
[0051] The bismaleimide compound may include, for example, a compound represented by the following general formula (10): These may be used alone or in combination of two or more kinds.
[0052] [ka] (In the above general formula (10), n1 is an integer of 0 to 10, each X1 is independently an alkylene group having 1 to 10 carbon atoms, a group represented by the following formula (10a), a group represented by the following formula (10b), a group represented by the formula "-SO2-", a group represented by the formula "-CO-", an oxygen atom or a single bond, each R1 is independently a hydrocarbon group having 1 to 6 carbon atoms or a phenyl group, each a is independently an integer of 0 to 4, and each b is independently an integer of 0 to 3.)
[0053] [ka] In formula (10a), Y is a hydrocarbon group having an aromatic ring and having 6 to 30 carbon atoms, and n2 is an integer of 0 or more.
[0054] [ka]
[0055] The bismaleimide compound may include a bismaleimide having a biphenylaralkyl skeleton, such as the compound shown in general formula (10) above, in which X1 has the above (10b).
[0056] The cyanate ester resin is not particularly limited, but can be obtained, for example, by reacting a halogenated cyanide compound with a phenol or naphthol, and optionally prepolymerizing it by a method such as heating. Also, a commercially available product thus prepared can be used.
[0057] Examples of the cyanate ester resin include bisphenol cyanate ester resins such as novolac type cyanate ester resins, bisphenol A type cyanate ester resins, bisphenol E type cyanate ester resins, and tetramethyl bisphenol F type cyanate ester resins; naphthol aralkyl type cyanate ester resins obtained by reacting naphthol aralkyl type phenol resins with cyanogen halides; dicyclopentadiene type cyanate ester resins; and biphenyl alkyl type cyanate ester resins. Among these, it is preferable to have a bisphenol A skeleton or a novolac skeleton, and specifically, bisphenol A type cyanate ester resins, novolac type cyanate ester resins, and naphthol aralkyl type cyanate ester resins are preferable, and novolac type cyanate ester resins are more preferable. Among these, by using bisphenol A type cyanate ester resins, a good low dielectric tangent can be obtained. The reason for this is that bisphenol A type cyanate ester resin has few crosslinking points, so that when a triazine ring is formed, unreacted cyanate groups are unlikely to remain, and it becomes easier to maintain good dielectric properties.
[0058] Examples of the phenol resin include novolac-type phenol resins such as phenol novolac resin, cresol novolac resin, bisphenol A novolac resin, and triazine skeleton-containing phenol novolac resin; aralkyl-type phenol resins such as biphenyl aralkyl-type phenol resin; and resol-type phenol resins such as unmodified resol phenol resin and oil-modified resol phenol resin modified with tung oil, linseed oil, walnut oil, etc.
[0059] Examples of epoxy resins include bisphenol type epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol E type epoxy resin, bisphenol S type epoxy resin, bisphenol M type epoxy resin (4,4'-(1,3-phenylenediisopridiene) bisphenol type epoxy resin), bisphenol P type epoxy resin (4,4'-(1,4-phenylenediisopridiene) bisphenol type epoxy resin), and bisphenol Z type epoxy resin (4,4'-cyclohexydiene bisphenol type epoxy resin); phenol novolac type epoxy resin, cresol novolac type epoxy resin, tetraphenol group ethane type novolac type epoxy resin, and the like. Examples of epoxy resins that can be used include novolac-type epoxy resins such as xylylene-type epoxy resins and novolac-type epoxy resins having a condensed ring aromatic hydrocarbon structure; biphenyl-type epoxy resins; aralkyl-type epoxy resins such as xylylene-type epoxy resins and biphenylaralkyl-type epoxy resins; naphthalene-type epoxy resins such as naphthylene ether-type epoxy resins, naphthol-type epoxy resins, naphthalene diol-type epoxy resins, difunctional to tetrafunctional naphthalene-type epoxy resins, binaphthyl-type epoxy resins, and naphthalenearalkyl-type epoxy resins; anthracene-type epoxy resins; phenoxy-type epoxy resins; dicyclopentadiene-type epoxy resins; norbornene-type epoxy resins; adamantane-type epoxy resins; and fluorene-type epoxy resins.
[0060] The compound having two or more carbon-carbon unsaturated double bonds in one molecule has a melting point of 30° C. or less and is compatible with polyphenylene ether.
[0061] An example of the compound having two or more carbon-carbon unsaturated double bonds in one molecule may include a compound represented by the following general formula (2): These may be used alone or in combination of two or more kinds.
[0062] [ka]
[0063] In the above formula (2), m represents an integer of 1 to 3, n represents 0 or 1, and R 1 ~R 3 each independently represents a hydrogen atom or an alkyl group. X represents an arylene group, a dicyclopentadienyl group, or an isocyanurate group. Y represents a group represented by the following (2a) or (2b).
[0064] [ka]
[0065] Examples of compounds having two or more carbon-carbon unsaturated double bonds in one molecule include trialkenyl isocyanurate compounds such as triallyl isocyanurate (TAIC), polyfunctional methacrylate compounds having two or more methacrylic groups in the molecule, polyfunctional acrylate compounds having two or more acrylic groups in the molecule, and vinylbenzyl compounds such as styrene and divinylbenzene having a vinylbenzyl group in the molecule. Among these, preferred are trialkenyl isocyanurate compounds, polyfunctional acrylate compounds, polyfunctional methacrylate compounds, and divinylbenzene compounds.
[0066] In addition, a compound having two or more carbon-carbon unsaturated double bonds in the molecule and a compound having one carbon-carbon unsaturated double bond in the molecule may be used in combination. Specific examples of the compound having one carbon-carbon unsaturated double bond in the molecule include compounds having one vinyl group in the molecule (monovinyl compounds).
[0067] The content of the crosslinking agent is, for example, 10 to 70% by weight, preferably 15 to 60% by weight, and more preferably 20 to 50% by weight, based on 100% by weight of the solid content of the resin composition. By making the content equal to or more than the lower limit, low dielectric properties can be realized. By making the content equal to or less than the upper limit, resin residue can be suppressed.
[0068] The content of at least one of the maleimide compound, the cyanate ester resin, the phenolic resin, and the epoxy resin is, for example, 10 to 50% by weight, preferably 11 to 40% by weight, and more preferably 12 to 30% by weight, based on 100% by weight of the solid content of the resin composition. By making it equal to or more than the lower limit, low dielectric properties can be realized. By making it equal to or less than the upper limit, resin residue can be suppressed.
[0069] The content of the compound having two or more carbon-carbon unsaturated double bonds in the molecule is, for example, 10 to 50% by weight, preferably 11 to 40% by weight, and more preferably 12 to 30% by weight, based on 100% by weight of the solid content of the resin composition. By making it equal to or more than the lower limit, low dielectric properties can be realized. By making it equal to or less than the upper limit, resin residue can be suppressed.
[0070] (Reaction initiator) The resin composition may contain a reaction initiator as necessary. The reaction initiator is not particularly limited as long as it can promote the reaction between the polyphenylene ether and the crosslinking agent. The reaction initiator can promote the polymerization reaction of the radical polymerization type crosslinking agent.
[0071] As the reaction initiator, an organic peroxide, a dihalogen, an azo compound, a combination of an oxidizing agent and a reducing agent, or the like is used.
[0072] Examples of the reaction initiator include organic peroxides such as α,α'-bis(t-butylperoxy-m-isopropyl)benzene, 2,5-dimethyl-2,5-di(t-butylperoxy)-3-hexyne, benzoyl peroxide, 3,3',5,5'-tetramethyl-1,4-diphenoquinone, chloranil, 2,4,6-tri-t-butylphenoxyl, t-butylperoxyisopropyl monocarbonate, and azobisisobutyronitrile. In addition, a carboxylate metal salt or the like can be used in combination as necessary. By doing so, the curing reaction can be further accelerated. Among these, α,α'-bis(t-butylperoxy-m-isopropyl)benzene is preferably used. Since α,α'-bis(t-butylperoxy-m-isopropyl)benzene has a relatively high reaction initiation temperature, it can suppress the promotion of the curing reaction at the time when curing is not required, such as when drying the prepreg, and can suppress the deterioration of the storage stability of the polyphenylene ether resin composition. Furthermore, since α,α'-bis(t-butylperoxy-m-isopropyl)benzene has low volatility, it does not volatilize during drying or storage of the prepreg, and has good stability. The reaction initiator may be used alone or in combination of two or more kinds.
[0073] The content of the reaction initiator is 0.2 to 5% by weight, preferably 0.25 to 3% by weight, and more preferably 0.3 to 2% by weight, based on 100% by weight of the solid content of the resin composition. By making it equal to or more than the lower limit, low dielectric properties can be realized. By making it equal to or less than the upper limit, resin residue can be suppressed.
[0074] (filling material) The resin composition includes a filler. The filler includes at least one of an organic filler and an inorganic filler. From the viewpoint of obtaining an appropriate elastic modulus and a low dielectric tangent, an inorganic filler may be used.
[0075] Examples of inorganic fillers include silicates such as talc, calcined clay, uncalcined clay, mica, and glass; oxides such as titanium oxide, alumina, boehmite, silica, and fused silica; carbonates such as calcium carbonate, magnesium carbonate, and hydrotalcite; hydroxides such as aluminum hydroxide, magnesium hydroxide, and calcium hydroxide; sulfates or sulfites such as barium sulfate, calcium sulfate, and calcium sulfite; borates such as zinc borate, barium metaborate, aluminum borate, calcium borate, and sodium borate; nitrides such as aluminum nitride, boron nitride, silicon nitride, and carbon nitride; and titanates such as strontium titanate and barium titanate. Among these, talc, alumina, glass, silica, mica, aluminum hydroxide, and magnesium hydroxide are preferable, and from the viewpoint of achieving both an elastic modulus, a low dielectric tangent, and a reduction in resin residue, silica is more preferable. Among these, one type may be used alone, or two or more types may be used in combination.
[0076] The average particle diameter of the inorganic filler is preferably 0.01 μm or more, more preferably 0.05 μm or more. When the average particle diameter of component (C) is equal to or more than the above lower limit, the viscosity of the varnish can be suppressed from increasing, and the workability during the preparation of the insulating layer can be improved. In addition, the average particle diameter of the inorganic filler is preferably 5.0 μm or less, more preferably 2.0 μm or less, and even more preferably 1.0 μm or less. When the average particle diameter of component (C) is equal to or less than the above upper limit, the phenomenon of precipitation of component (C) in the varnish can be suppressed, and a more uniform resin layer can be obtained. In addition, when the circuit dimension L / S of the printed wiring board is less than 20 μm / 20 μm, the influence on the insulation between the wirings can be suppressed.
[0077] The average particle diameter of the inorganic filler is determined by, for example, measuring the particle size distribution of the particles on a volume basis using a laser diffraction particle size distribution measuring device (HORIBA, LA-500) and calculating the median diameter (D 50 ) can be used as the average particle size.
[0078] The inorganic filler may be one having a monodisperse average particle size, or one having a polydisperse average particle size. Furthermore, one or more types of monodisperse and / or polydisperse average particle sizes may be used in combination.
[0079] As the inorganic filler, silica particles are preferred, with silica particles having an average particle size of 5.0 μm or less being preferred, silica particles having an average particle size of 0.1 μm to 4.0 μm being more preferred, and silica particles having an average particle size of 0.2 μm to 2.0 μm being even more preferred, which can further improve the filling property of component (C).
[0080] The content of the filler is 45 to 70% by weight, preferably 48 to 68% by weight, and more preferably 50 to 65% by weight, based on 100% by weight of the solid content of the resin composition. By making the content equal to or more than the lower limit, low dielectric properties and good elastic modulus can be realized. By making the content equal to or less than the upper limit, the handleability of the composition can be improved. The content of the inorganic filler may be in the same range as the above-mentioned range of the content of the filler.
[0081] (Cyclic urea compounds) The resin composition contains a cyclic urea compound. The cyclic urea compound is a compound having at least one urea unit -NHCONH- as a ring constituent unit. The ring may be, for example, a single ring, two or more condensed rings, or a condensed ring with an aromatic hydrocarbon ring. The oxygen atom in the urea unit may be replaced with a sulfur atom.
[0082] The cyclic urea compound may include one or more selected from the group consisting of cyclic monoureido, cyclic diureido, and cyclic thioureas.
[0083] Examples of cyclic monoureides that can be used include alkylene ureas such as methylene urea, ethylene urea, and crotonylidene urea (CDU); alkenylene ureas such as vinylene urea and cytosine; alkynylene ureas; arylene ureas such as imesatin; ureides of dicarboxylic acids such as parabanic acid, dimethylparabanic acid, barbituric acid, 5,5-diethylbarbituric acid, dilituric acid, dialuric acid, alloxan, alloxanic acid, isocyanuric acid, and uramyl; ureides of β-aldehyde acids such as uracil, 5-methyluracil (thymine), dihydrouracil, urazole, and benzoyl urea; ureides of α-oxy acids such as hydantoin, 5,5-dimethylhydantoin, 1,1-methylenebis(5,5-dimethylhydantoin), and allantoin; and derivatives thereof. These may be used alone or in combination of two or more.
[0084] Examples of the cyclic diureides include uric acid, 3-methyluric acid, pseudouric acid, acetylene urea (glycoluril), diureides of α-oxy acids, diurea, diureides of dicarboxylic acids, and derivatives thereof. These may be used alone or in combination of two or more.
[0085] Examples of cyclic thioureas include ethylenethiourea, thiobarbituric acid, dithiourazole, thiohydantoin, and dithiohydantoin.
[0086] The cyclic urea compound and the cyclic diureide also include salts. The salt is not particularly limited as long as it can form a salt with the cyclic urea, and examples thereof include salts with at least one selected from sulfuric acid, sulfonic acid, boric acid, non-condensed phosphoric acid, organic phosphoric acid, polyphosphoric acid, and other oxygen acids, triazine compounds, and metals. These may be used alone or in combination of two or more.
[0087] Among the cyclic urea compounds, from the viewpoints of flame retardancy and physical properties when applied to an encapsulant, cyclic diureides having two urea units as ring constituent units are preferred, acetylene urea, uric acid, and derivatives thereof are more preferred, and from the viewpoint of further improving flame retardancy, acetylene urea and uric acid are even more preferred.
[0088] The cyclic urea compound may be in a powder form, which can improve dispersibility and compatibility.
[0089] The cyclic urea compound may contain, for example, a compound having a melting point of 250° C. or higher, preferably a melting point of 280° C. or higher, more preferably a melting point of 300° C. or higher, which can improve flame retardancy.
[0090] The lower limit of the content of the cyclic urea compound is, for example, preferably 1.0% by mass or more, more preferably 2.0% by mass or more, and even more preferably 3.5% by mass or more, based on 100% by mass of the solid content of the resin composition. This can improve the flame retardancy of the insulating layer while reducing the dielectric constant and dielectric loss tangent. In addition, the linear expansion coefficient can be reduced. On the other hand, the upper limit of the content of the cyclic urea compound is, for example, preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less, based on 100% by mass of the solid content of the resin composition. This allows for a balance of various physical properties such as copper peel strength. In addition, when the resin composition is in the form of a varnish, the deterioration of its coatability can be suppressed.
[0091] The resin composition of the present embodiment may contain other additives, if necessary, in addition to the above components. Examples of other additives include curing accelerators, silane coupling agents, tackifiers, surfactants, thermoplastic resins, pigments, dyes, defoamers, leveling agents, UV absorbers, foaming agents, antioxidants, heat stabilizers, antistatic agents, other flame retardants, ion traps, lubricants, dispersants, etc. These may be used alone or in combination of two or more kinds, as long as the object of the present invention is not impaired. The resin composition may be configured so as not to contain a phosphorus-based flame retardant.
[0092] The characteristics of the resin composition of this embodiment will be described.
[0093] The dielectric loss tangent of the cured product of the resin composition measured at 25° C. and 1 GHz is, for example, 0.0050 or less, preferably 0.0040 or less, and more preferably 0.0030 or less, thereby realizing an insulating layer with excellent low dielectric properties.
[0094] The dielectric constant of the cured product of the resin composition measured at 25° C. and 1 GHz is, for example, 3.90 or less, preferably 3.80 or less, and more preferably 3.70 or less, thereby realizing an insulating layer with excellent low dielectric properties.
[0095] The dielectric loss tangent of the cured product of the resin composition measured at 25° C. and 10 GHz is, for example, 0.0080 or less, preferably 0.0060 or less, and more preferably 0.0040 or less, thereby realizing an insulating layer with excellent low dielectric properties.
[0096] The resin composition of the present embodiment may be a varnish-like composition containing a solvent, or may be a film-like composition. For example, a film-like composition can be obtained by applying a varnish-like resin composition to a coating film obtained by performing a solvent removal treatment, thereby obtaining a film-like composition.
[0097] Examples of the solvent include organic solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, toluene, ethyl acetate, cyclohexane, heptane, cyclohexane, cyclohexanone, tetrahydrofuran, dimethylformamide, dimethylacetamide, dimethylsulfoxide, ethylene glycol, cellosolves, carbitols, anisole, and N-methylpyrrolidone. These may be used alone or in combination of two or more.
[0098] When the resin composition is in the form of a varnish, the solid content of the resin composition may be, for example, 30% by weight or more and 80% by weight or less, more preferably 40% by weight or more and 70% by weight or less, which results in a resin composition with excellent workability and film-forming properties.
[0099] The varnish-like resin composition can be prepared by dissolving, mixing, and stirring the above-mentioned components in a solvent using various mixers such as those used in an ultrasonic dispersion system, a high-pressure collision dispersion system, a high-speed rotation dispersion system, a bead mill system, a high-speed shear dispersion system, and a rotation-revolution dispersion system.
[0100] Furthermore, the use form of the resin composition of the present embodiment is not particularly limited, but examples thereof include a resin film made of the above-mentioned resin composition, a resin film with a carrier in which the above-mentioned resin film is provided on a carrier substrate, a resin substrate having an insulating layer made of a cured product of the above-mentioned resin composition, a prepreg obtained by impregnating a fiber substrate with the above-mentioned resin composition, a metal-clad laminate having a metal layer disposed on one surface of these, a resin substrate having an insulating layer made of a cured product of the above-mentioned resin composition, and a printed wiring board in which a circuit layer is formed on the surface of the above-mentioned metal-clad laminate.
[0101] (Resin film with carrier) FIG. 1 is a cross-sectional view showing an example of the configuration of a resin film 100 with a carrier in this embodiment. 1, the carrier-attached resin film 100 of the present embodiment can include a carrier substrate 12 and a resin film 10 made of the above-mentioned resin composition provided on the carrier substrate 12. This can improve the handleability of the resin film 10.
[0102] The resin film 100 with a carrier may be in a roll shape that can be wound up, or in a leaf shape (sheet shape) such as a rectangular shape.
[0103] The carrier substrate 12 may be, for example, a polymer film or a metal foil. Examples of polymer films include, but are not limited to, polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate and polybutylene terephthalate, polycarbonates, release papers such as silicone sheets, and heat-resistant thermoplastic resin sheets such as fluorine-based resins and polyimide resins. The metal foil is not particularly limited, but examples thereof include copper and / or copper-based alloys, aluminum and / or aluminum-based alloys, iron and / or iron-based alloys, silver and / or silver-based alloys, gold and / or gold-based alloys, zinc and / or zinc-based alloys, nickel and / or nickel-based alloys, and tin and / or tin-based alloys. Among these, a sheet made of polyethylene terephthalate is most preferable because it is inexpensive and the peel strength can be easily adjusted. This makes it easy to peel off the sheet from the resin film 100 with the carrier with a moderate strength.
[0104] The lower limit of the thickness of the resin film 10 is not particularly limited, but may be, for example, 1 μm or more, 3 μm or more, or 5 μm or more. This can increase the mechanical strength of the resin film 10. On the other hand, the upper limit of the thickness of the resin film 10 is not particularly limited, but may be, for example, 500 μm or less, 300 μm or less, or 100 μm or less. This can reduce the thickness of the semiconductor device.
[0105] The thickness of the carrier base 12 is not particularly limited, but may be, for example, 10 to 100 μm, or 10 to 70 μm, which is preferable because it allows for good handling when producing the carrier-attached resin film 100.
[0106] The resin film 100 with a carrier may be a single layer or a multilayer, and may contain one or more types of resin films 10. When the resin sheet is a multilayer, it may be composed of the same type or different types. In addition, the resin film 100 with a carrier may have a protective film on the outermost layer side on the resin film 10.
[0107] In this embodiment, the method for forming the carrier-attached resin film 100 is not particularly limited, but for example, a method can be used in which a varnish-like resin composition is applied onto the carrier substrate 12 using various coater devices to form a coating film, and then the coating film is appropriately dried to remove the solvent.
[0108] The resin film of this embodiment can be obtained by forming the above-mentioned resin composition in a varnish form into a film. For example, the resin film of this embodiment can be obtained by removing the solvent from a coating film obtained by applying the resin composition in a varnish form. In such a resin film, the solvent content can be 5% by weight or less based on the entire resin film. In this embodiment, the step of removing the solvent may be carried out under conditions of, for example, 100°C to 150°C and 1 minute to 5 minutes. This makes it possible to sufficiently remove the solvent while suppressing the progress of curing of the resin film containing a thermosetting resin.
[0109] (Resin substrate) The resin substrate of the present embodiment includes an insulating layer made of the cured product of the above-mentioned resin composition. Such a resin substrate can be used as a coreless substrate that does not contain glass fibers for a printed wiring board.
[0110] (Prepreg) The prepreg of the present embodiment contains a fiber base material in the above-mentioned resin composition. The prepreg can be formed, for example, by impregnating a fiber base material with a resin composition. Prepregs can be used as semi-cured sheet-like materials. Sheet-like materials with such structures have excellent properties such as dielectric properties and mechanical and electrical connection reliability under high temperature and humidity, and are suitable for producing insulating layers for printed wiring boards.
[0111] The method for impregnating the resin composition into the fiber substrate is not particularly limited, but examples thereof include a method of dissolving the resin composition in a solvent to prepare a resin varnish and immersing the fiber substrate in the resin varnish, a method of applying the resin varnish to the fiber substrate using various coaters, a method of spraying the resin varnish onto the fiber substrate using a sprayer, and a method of laminating both sides of the fiber substrate with the resin film made of the resin composition.
[0112] The fiber substrate is not particularly limited, but includes glass fiber substrates such as glass woven fabric and glass nonwoven fabric; polyamide resin fibers such as polyamide resin fibers, aromatic polyamide resin fibers, and wholly aromatic polyamide resin fibers; polyester resin fibers such as polyester resin fibers, aromatic polyester resin fibers, and wholly aromatic polyester resin fibers; synthetic fiber substrates composed of woven or nonwoven fabrics mainly composed of either polyimide resin fibers or fluororesin fibers; paper substrates mainly composed of kraft paper, cotton linter paper, or mixed paper of linter and kraft pulp; and the like. Any of these can be used. Among these, glass fiber substrates are preferred. This allows for the production of a resin substrate with low water absorption, high strength, and low thermal expansion.
[0113] The thickness of the fiber base material is not particularly limited, but is preferably 5 μm to 150 μm, more preferably 10 μm to 100 μm, and even more preferably 12 μm to 90 μm. By using a fiber base material having such a thickness, the handleability during the production of the prepreg can be further improved. When the thickness of the fiber substrate is equal to or less than the upper limit, the impregnation of the resin composition in the fiber substrate is improved, and the occurrence of strand voids and deterioration of insulation reliability can be suppressed. In addition, the formation of through holes by carbon dioxide, UV, excimer, or other lasers can be facilitated. In addition, when the thickness of the fiber substrate is equal to or more than the lower limit, the strength of the fiber substrate and prepreg can be improved. As a result, the handling property can be improved, the preparation of prepreg can be facilitated, and warping of the substrate can be suppressed.
[0114] As the above-mentioned glass fiber substrate, for example, a glass fiber substrate formed of one or more types of glass selected from E glass, S glass, D glass, T glass, NE glass, UT glass, L glass, HP glass and quartz glass is suitably used.
[0115] In this embodiment, the prepreg can be used to form, for example, an insulating layer in a core layer or a build-up layer in a printed wiring board. When the prepreg is used to form an insulating layer in a core layer of a printed wiring board, for example, two or more prepregs can be stacked and the resulting laminate can be heat-cured to form an insulating layer for the core layer.
[0116] (Metal-clad laminate) The metal-clad laminate of the present embodiment has a structure in which a metal layer is disposed on at least one surface of the resin film made of the resin composition, the resin substrate, or the prepreg.
[0117] A method for producing a metal-clad laminate using a prepreg is, for example, as follows. A metal foil is placed on both the upper and lower sides or one side of the outer side of a prepreg or a laminate of two or more prepregs, and these are bonded under high vacuum conditions using a laminator or Becquerel device, or a metal foil is placed on both the upper and lower sides or one side of the outer side of the prepreg as is. When two or more prepregs are laminated, a metal foil is placed on both the upper and lower sides or one side of the outermost side of the laminated prepregs. Next, the laminate of the prepreg and the metal foil is heated and pressurized to obtain a metal-clad laminate. Here, it is preferable to continue pressing until the end of cooling during the heating and pressurizing. The above-mentioned metal-clad laminate manufacturing method may employ a method of hot-press molding using the above-mentioned resin film or the above-mentioned resin substrate instead of the above-mentioned prepreg.
[0118] Examples of the metals constituting the metal foil include copper, copper-based alloys, aluminum, aluminum-based alloys, silver, silver-based alloys, gold, gold-based alloys, zinc, zinc-based alloys, nickel, nickel-based alloys, tin, tin-based alloys, iron, iron-based alloys, Fe-Ni-based alloys such as Kovar (trade name), 42 alloy, Invar, and Super Invar, W, and Mo. Among these, the metal constituting the metal foil 105 is preferably copper or a copper alloy, because it has excellent conductivity, is easy to form a circuit by etching, and is inexpensive. That is, the metal foil 105 is preferably a copper foil. As the metal foil, a metal foil with a carrier or the like can also be used. The thickness of the metal foil is preferably 0.5 μm or more and 20 μm or less, and more preferably 1.5 μm or more and 18 μm or less.
[0119] (Printed wiring board) The printed wiring board of the present embodiment may include the above-mentioned metal-clad laminate having a circuit layer formed on the surface thereof. Specifically, the printed wiring board may include an insulating layer composed of a cured product of the resin composition, a cured product of the resin film, the resin substrate, and a cured product of the prepreg, and a circuit pattern (circuit layer) formed on the insulating layer.
[0120] An example of a printed wiring board 300 according to the present embodiment will be described with reference to FIG. 2 includes an insulating layer 301 (core layer) and a metal layer 303 (circuit layer) formed on the insulating layer 301. This printed wiring board 300 may have a multilayer circuit structure in which a plurality of circuit layers are stacked with an interlayer insulating layer interposed therebetween. The printed wiring board 300 may further include an insulating layer 401 (solder resist layer).
[0121] In the printed wiring board 300, the core layer and the interlayer insulating layer are composed of any one of the cured product of the resin composition, the cured product of the resin film, the resin substrate, and the insulating layer composed of the cured product of the prepreg.
[0122] Furthermore, the printed wiring board 300 may be a single-sided printed wiring board, a double-sided printed wiring board, or a multi-layer printed wiring board. A double-sided printed wiring board is a printed wiring board in which metal layers 303 are laminated on both sides of an insulating layer 301. A multi-layer printed wiring board may be a printed wiring board in which two or more build-up layers are laminated on an insulating layer 301, which is a core layer, by a plated through-hole method, a build-up method, or the like.
[0123] In this embodiment, the metal layer 303 may be, for example, a circuit pattern or an electrode pad. The metal layer 303 may have a metal laminate structure of, for example, the metal foil 105 and the electrolytic metal plating layer 309.
[0124] The metal layer 303 is formed by, for example, a SAP (semi-additive process) method on the surface of the metal foil 105 that has been treated with a chemical solution or plasma, or an insulating layer (for example, the insulating layer 301) made of a cured product of the resin film of this embodiment. For example, after applying an electroless metal plating film 308 onto the metal foil 105 or the insulating layers 301, 305, non-circuit forming portions are protected with a plating resist, an electrolytic metal plating layer 309 is formed by electrolytic plating, and the plating resist is removed and the electrolytic metal plating layer 309 is patterned by flash etching, thereby forming the metal layer 303.
[0125] In this embodiment, the via hole 307 may be either a through hole or a non-through hole as long as it is a hole for electrically connecting layers. The via hole 307 may be formed by embedding a metal. The embedded metal may have a structure covered with an electroless metal plating film 308.
[0126] Moreover, the printed wiring board 300 of the present embodiment may be a resin board that does not contain glass fibers. For example, the insulating layer 301, which is the core layer, may be configured not to contain glass fibers. Even in a semiconductor package using such a resin board, the linear expansion coefficient of the cured resin film can be reduced, so that package warpage can be sufficiently suppressed.
[0127] (Semiconductor Package) Next, a description will be given of the semiconductor device 400 of this embodiment. The semiconductor device 400 of this embodiment can include a printed wiring board 300 and a semiconductor element 407 mounted on a circuit layer of the printed wiring board 300 or embedded in the printed wiring board 300 . The semiconductor element 407 may be, for example, a light emitting diode (LED).
[0128] For example, a semiconductor device 400 shown in FIG. 3 has a structure in which a semiconductor element 407 is mounted on a circuit layer (metal layer 303) of a printed wiring board 300. The semiconductor package may have a flip-chip structure in which the semiconductor element 407 is electrically connected to the printed wiring board 300 via the solder bumps 410 and the metal layer 303 .
[0129] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES
[0130] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.
[0131] <Preparation of Resin Composition> Raw material components such as polyphenylene ether, crosslinking agent, filler, nitrogen-based flame retardant, and reaction initiator were dissolved or dispersed in the solid content ratio shown in Table 1 below, and the non-volatile content was adjusted to 70 mass % with methyl ethyl ketone. The resin varnish was prepared by stirring using a high-speed stirrer.
[0132] The information on the raw material ingredients in Table 1 is shown below. (Filling material) · Silica particles 1 (manufactured by Admatechs Co., Ltd., SC4050-KNT, average particle size: 1.1 μm) (Silane coupling agent) · Silane coupling agent 1: Vinyltrimethoxysilane (manufactured by Shin-Etsu Silicone Co., Ltd., KBM-1003) (Polyphenylene ether) · Polyphenylene ether 1: Polyphenylene ether resin having methacrylate groups at both ends (manufactured by SABIC Japan Co., Ltd., SA9000, weight-average molecular weight Mw = 1,700) (Adhesion promoter) · Adhesion promoter 1: Coumarone resin (manufactured by Nippon Paint Chemical Co., Ltd., V-120S) · Adhesion promoter 2: Vinyl group-containing polybutadiene (manufactured by Nippon Soda Co., Ltd., B-1000) (Crosslinking agent) · Maleimide compound 1: Bismaleimide having a biphenylaralkyl skeleton (manufactured by Nippon Kayaku Co., Ltd., MIR-3000-70T) · Compound 1 having two or more carbon-carbon unsaturated double bonds in one molecule: Triallyl isocyanurate (manufactured by Mitsubishi Chemical Corporation, TAIC) (Surfactant) · Surfactant 1: Acrylic surfactant (manufactured by BYK-Chemie GmbH, BYK-361N) (Reaction initiator) · Organic peroxide 1: 1,3-Bis(butylperoxyisopropyl)benzene (manufactured by NOF Corporation, Perbutyl P) (Cyclic urea compound) · Cyclic diureide 1: Uric acid (manufactured by Tokyo Chemical Industry Co., Ltd., powder, melting point: >300 °C)
[0133]
Table 1
[0134] Regarding the obtained resin composition (resin varnish), evaluations were conducted on the following items.
[0135] <UL94V test> (Preparation of prepreg) The obtained resin varnish was applied to a woven glass fabric (cloth type #1078, E glass, basis weight 47.5 g / m 2 ) was impregnated using a coating device and then dried for 4 minutes using a hot air dryer at 150°C to obtain a prepreg with a thickness of 80 μm. The obtained prepreg was heated at 255° C. for 2 hours to be cured, and a resin plate (test piece) having a thickness of 80 μm was obtained. The obtained test pieces were cut to 127 mm x 12.7 mm, and then measured in accordance with the UL-94 vertical test. The number of test pieces that burned completely was counted out of the five pieces.
[0136] (Preparation of copper-clad laminates) Ultra-thin copper foil (Mitsui Mining & Smelting, Microthin FL, 1.5 μm) was laminated on both sides of the prepreg obtained above (preparation of prepreg), and heated and pressurized for 2 hours at a pressure of 3 MPa and a temperature of 225° C. to obtain a laminate with metal foil. The thickness of the core layer (portion consisting of the resin substrate) of the obtained laminate with metal foil was 0.080 mm.
[0137] <Copper peel strength> A 30 μm thick copper plating film was formed by electroplating on a metal foil laminate, and the copper peel strength (kN / m) was measured when the copper plating film was peeled off at 90 degrees in accordance with JIS C6481.
[0138] <Dielectric constant, dielectric loss tangent> The copper foil of the metal foil-attached laminate was removed by etching, and the dielectric loss tangent (Df) at frequencies of 1 GHz and 10 GHz was measured by the cavity resonator method.
[0139] <Elasticity modulus> The laminate with metal foil was etched to remove the copper, and the elastic modulus (GPa) was measured at a frequency of 1 GHz and a temperature of 250°C using a dynamic viscoelasticity device in accordance with JISC-6481 (DMA method).
[0140] <Coefficient of Linear Expansion (CTE)> The laminate with metal foil was etched to remove the copper, and a 4 mm x 20 mm test piece was prepared. This was used as a sample to measure the linear expansion coefficient (ppm / °C) in the ranges of 50°C to 100°C and 50°C to 150°C in the second cycle using a TMA (thermal mechanical analysis) device (TA Instruments, Q400) under conditions of a heating rate of 5°C / min, a temperature range of 30 to 300°C, 10°C / min, and a load of 5g.
[0141] The resin compositions of Examples 1 and 2 showed excellent results in terms of high flame retardancy and low dielectric properties, since the number of burned pieces was small and the dielectric loss tangent at 10 GHz was small, compared with Comparative Example 1. Such resin compositions of the examples can be suitably used for members constituting circuit boards. [Explanation of symbols]
[0142] 10 Resin Film 12 Carrier substrate 100 Resin film with carrier 105 Metal foil 300 Printed Wiring Board 301 Insulating layer 303 Metal layer 307 Beer Hall 308 Electroless metal plating film 309 Electrolytic metal plating layer 400 Semiconductor equipment 401 Insulating layer 407 Semiconductor Devices 410 Solder Bump
Claims
1. A resin composition for a circuit board, Polyphenylene ether, a crosslinking agent reactive with the polyphenylene ether; A filler material; A cyclic urea compound, The resin composition, wherein the cyclic urea compound contains a cyclic diureide.
2. The resin composition according to claim 1, The resin composition, wherein the polyphenylene ether contains a polymer having a structural unit represented by the following general formula (1): [Formula 1] (In the above general formula (1), R 1 , R 2 , R 3 , R 4 may be the same or different and represent any one selected from the group consisting of a hydrogen atom, a halogen atom, an optionally substituted alkyl group, an optionally substituted alkenyl group, an optionally substituted alkynyl group, an optionally substituted aryl group, an optionally substituted aralkyl group, and an optionally substituted alkoxy group.
3. The resin composition according to claim 1 or 2, The resin composition, wherein the crosslinking agent comprises at least one selected from the group consisting of a maleimide compound, a cyanate ester resin, a phenolic resin, an epoxy resin, and a compound having two or more carbon-carbon unsaturated double bonds in one molecule.
4. The resin composition according to any one of claims 1 to 3, A resin composition comprising a reaction initiator.
5. The resin composition according to claim 4, The resin composition, wherein the reaction initiator comprises an organic peroxide.
6. The resin composition according to any one of claims 1 to 5, A resin composition, wherein a cured product of the resin composition has a dielectric loss tangent of 0.0050 or less, as measured at 25°C and 1 GHz.
7. The resin composition according to any one of claims 1 to 6, A resin composition, wherein a cured product of the resin composition has a dielectric loss tangent of 0.0080 or less, as measured at 25°C and 10 GHz.
8. A carrier substrate; A resin film with a carrier, comprising: a resin film formed on the carrier base material and made of the resin composition according to any one of claims 1 to 7.
9. A resin substrate comprising an insulating layer formed of a cured product of the resin composition according to any one of claims 1 to 7.
10. A prepreg comprising a fiber base material in the resin composition according to any one of claims 1 to 7.
11. A metal-clad laminate comprising a resin film made of the resin composition according to any one of claims 1 to 7, a resin substrate according to claim 9, or a prepreg according to claim 10, and a metal layer disposed on at least one surface of the resin film.
12. A printed wiring board comprising the metal-clad laminate according to claim 11 and a circuit layer formed on a surface of the metal-clad laminate.
13. The printed wiring board according to claim 12; a semiconductor element mounted on a circuit layer of the printed wiring board or embedded in the printed wiring board.
Citation Information
Patent Citations
Nannenseigoseijushisoseibutsu
JP1976066329A
Polyphenylene ether resin composition, prepreg, metal-clad laminate and printed wiring board
JP2016113543A
Resin composition and crosslinked body of the same
JP2018095786A
Epoxy resin composition, and cured product of the same
JP2020122034A
Flame-retardant resin composition
WO2004061008A1