Method for producing thermosetting resin composition and method for producing electronic component device

The method addresses the challenge of uniform dispersion of small inorganic fillers by controlling solvent removal and kneading temperatures, achieving high filling rates and improved resin composition properties.

JP7571549B2Active Publication Date: 2024-10-23RESONAC CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021002321
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-08
Publication Date
2024-10-23
Estimated Expiration
2041-01-08

AI Technical Summary

Technical Problem

Existing methods for manufacturing thermosetting resin compositions struggle with uniform dispersion of inorganic fillers due to their small particle sizes, leading to difficulties in achieving high filling rates, especially when using low cut point fillers, which can result in uneven distribution and increased viscosity.

Method used

A method involving controlled solvent removal and kneading processes at specific temperatures to reduce viscosity and apply sufficient shearing force, ensuring uniform dispersion of inorganic fillers, including steps such as desolvation and kneading with a curing accelerator at temperatures below the reaction threshold to prevent gelation.

Benefits of technology

The method enables high filling of inorganic fillers in thermosetting resin compositions, improving uniformity and reducing viscosity, thereby enhancing the properties of the final resin composition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571549000001
    Figure 0007571549000001
  • Figure 0007571549000002
    Figure 0007571549000002
  • Figure 0007571549000003
    Figure 0007571549000003
Patent Text Reader

Abstract

To provide a method for producing a thermosetting resin composition which allows an inorganic filler to be highly loaded.SOLUTION: The method for producing a thermosetting resin composition includes: a desolvation step of removing a solvent at a first desolvation temperature from a first mixture containing a thermosetting resin, a curing agent, and a slurry containing an inorganic filler and the solvent to obtain a second mixture; and a kneading step of adding a curing accelerator to the second mixture and kneading the second mixture having the curing accelerator added thereto at a first kneading temperature lower than the first desolvation temperature.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing a thermosetting resin composition and a method for producing an electronic component device. [Background technology]

[0002] In recent years, in order to reduce the cost, size, thickness, weight, performance, and functionality of electronic device devices, there has been a trend toward finer wiring, multi-layering, and more pins for elements, as well as smaller and thinner packages, resulting in higher density packaging. As a result, electronic device devices that are roughly the same size as elements such as ICs (Integrated Circuits), i.e., CSPs (Chip Size Packages), have come into widespread use. Furthermore, SiPs (System in Packages) that incorporate multiple elements in a single package have been developed.

[0003] As a sealing material for sealing elements of electronic component devices, a thermosetting resin composition containing a thermosetting resin, a curing agent, and an inorganic filler is widely used in terms of productivity, cost, etc. As the density and functionality of elements mounted on electronic component devices become higher, the bump-chip distance in CSPs or the distance between elements in SiPs becomes narrower. Therefore, the cut point of inorganic fillers is becoming smaller. However, as the cut point becomes smaller, the specific surface area of ​​the inorganic filler increases, making uniform dispersion difficult, and as a result, high loading of the inorganic filler has become an issue.

[0004] As an example of a method for producing a thermosetting resin composition, there is disclosed a method for producing an epoxy resin molding material for semiconductor encapsulation, which is characterized by mixing all of the raw materials including an epoxy resin, a curing agent, and an inorganic filler in a solvent, dissolving them to obtain a mixed solution, and then removing the solvent (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2011-252041 A [Patent Document 2] JP 2011-252042 A Summary of the Invention [Problem to be solved by the invention]

[0006] The manufacturing method described in Patent Document 1 or 2 is a method in which raw materials are made into a mixed and molten state in order to remove metallic foreign matter in an epoxy resin molding material for semiconductor encapsulation. However, in the manufacturing method described in Patent Document 1 or 2, it is difficult to apply a strong shear force to the mixed and molten material, and it may be difficult to uniformly disperse an inorganic filler with a low cut point. One aspect of the present disclosure has been made in consideration of the above-described conventional circumstances, and aims to provide a method for producing a thermosetting resin composition that enables high filling of an inorganic filler, and a method for producing an electronic component device using the thermosetting resin composition obtained by this production method. [Means for solving the problem]

[0007] Specific means for achieving the above object are as follows. <1> a desolvation step of removing the solvent from a first mixture containing a thermosetting resin, a curing agent, an inorganic filler, and a slurry containing a solvent at a first desolvation temperature to obtain a second mixture; a kneading step of adding a curing accelerator to the second mixture and kneading the second mixture to which the curing accelerator has been added at a first kneading temperature that is lower than the first desolvation temperature; A method for producing a thermosetting resin composition comprising the steps of: <2> a desolvation step of removing the solvent from a third mixture containing one of a thermosetting resin and a curing agent, and a slurry containing an inorganic filler and a solvent at a second desolvation temperature, and then adding the other of the thermosetting resin and the curing agent, or adding the other of the thermosetting resin and the curing agent while removing the solvent at the second desolvation temperature from a third mixture containing one of a thermosetting resin and a curing agent, and a slurry containing an inorganic filler and a solvent, to obtain a fourth mixture; a kneading step of adding a hardening accelerator to the fourth mixture and kneading the fourth mixture to which the hardening accelerator has been added at a second kneading temperature that is lower than the second desolvation temperature; A method for producing a thermosetting resin composition comprising the steps of: <3> The first kneading temperature is equal to or lower than a temperature at which the reaction rate of the second mixture to which the curing accelerator has been added is 40% as measured by differential scanning calorimetry. <1> A method for producing the thermosetting resin composition according to claim 1. <4> The second kneading temperature is equal to or lower than a temperature at which the reaction rate of the fourth mixture to which the curing accelerator has been added is 40% as measured by differential scanning calorimetry. <2> A method for producing the thermosetting resin composition according to claim 1. <5> The solvent removal step and the kneading step are carried out continuously. <1> ~ <4> 13. A method for producing the thermosetting resin composition according to claim 12. <6> The solvent removal step is carried out in a batch manner. <1> ~ <4> 13. A method for producing the thermosetting resin composition according to claim 12. <7> The first desolvation temperature or the second desolvation temperature is higher than the melting point or the softening point of the thermosetting resin. <1> ~ <6> 13. A method for producing the thermosetting resin composition according to claim 12. <8> The slurry further comprises a coupling agent. <1> ~ <7> 13. A method for producing the thermosetting resin composition according to claim 12. <9> The top cut diameter of the inorganic filler is 10 μm or less. <1> ~ <8> 13. A method for producing the thermosetting resin composition according to claim 12. <10> The boiling point of the solvent is 50°C to 200°C. <1> ~ <9> 13. A method for producing the thermosetting resin composition according to claim 12. <11> The solid content ratio of the inorganic filler in the slurry is 40% by mass to 90% by mass. <1> ~ <10> 13. A method for producing the thermosetting resin composition according to claim 12. <12> The solid content ratio of the first mixture or the third mixture is 30% by mass to 90% by mass. <1> ~ <11> 13. A method for producing the thermosetting resin composition according to claim 12. <13> <1> ~ <12> 13. A method for producing an electronic component device, comprising a step of encapsulating an element with a thermosetting resin composition obtained by the method for producing a thermosetting resin composition according to any one of claims 1 to 12. Effect of the Invention

[0008] According to one aspect of the present disclosure, it is possible to provide a method for producing a thermosetting resin composition that allows high filling of an inorganic filler, and a method for producing an electronic component device using the thermosetting resin composition obtained by this production method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the embodiments for carrying out the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments. In the following embodiments, the components (including element steps, etc.) are not essential unless otherwise specified. The same applies to the numerical values ​​and their ranges, and do not limit the present disclosure.

[0010] In the present disclosure, the term "step" includes not only a step that is independent of other steps, but also a step that cannot be clearly distinguished from other steps as long as the purpose of the step is achieved. In the present disclosure, a numerical range indicated using "~" includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples. In the present disclosure, each component may contain multiple types of corresponding substances. When multiple types of substances corresponding to each component are present in the composition, the content or amount of each component means the total content or amount of the multiple substances present in the composition, unless otherwise specified. In the present disclosure, the particles corresponding to each component may include multiple types of particles. When multiple types of particles corresponding to each component are present in the composition, the particle size of each component means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified. In the present disclosure, the term "solid content" refers to the remaining components after removing volatile components such as solvents from a mixture, a slurry, or a thermosetting resin composition.

[0011] <Method for producing thermosetting resin composition> A method for producing a thermosetting resin composition according to a first embodiment of the present disclosure includes a desolvation step of removing the solvent from a first mixture containing a thermosetting resin, a curing agent, and a slurry containing an inorganic filler and a solvent at a first desolvation temperature to obtain a second mixture, and a kneading step of adding a curing accelerator to the second mixture and kneading the second mixture to which the curing accelerator has been added at a first kneading temperature that is lower than the first desolvation temperature. Further, the method for producing a thermosetting resin composition according to the second embodiment of the present disclosure includes a desolvation step of removing the solvent from a third mixture containing one of a thermosetting resin and a curing agent, and a slurry containing an inorganic filler and a solvent at a second desolvation temperature, and then adding the other of the thermosetting resin and the curing agent, or removing the solvent from a third mixture containing one of a thermosetting resin and a curing agent, and a slurry containing an inorganic filler and a solvent at a second desolvation temperature while adding the other of the thermosetting resin and the curing agent to obtain a fourth mixture, and a kneading step of adding a curing accelerator to the fourth mixture and kneading the fourth mixture to which the curing accelerator has been added at a second kneading temperature that is lower than the second desolvation temperature. Hereinafter, the method for producing a thermosetting resin composition according to the first embodiment and the method for producing a thermosetting resin composition according to the second embodiment may be collectively referred to as the production method of the present disclosure. In addition, the method for producing a thermosetting resin composition according to the first embodiment may be referred to as a first production method, and the method for producing a thermosetting resin composition according to the second embodiment may be referred to as a second production method. The first desolvation temperature and the second desolvation temperature may be collectively referred to as a specific desolvation temperature, and the first kneading temperature and the second kneading temperature may be collectively referred to as a specific kneading temperature.

[0012] According to the manufacturing method of the present disclosure, it is possible to increase the loading of the inorganic filler. Although the reason is not clear, it is presumed as follows. The solvent contained in the first or third mixture acts as a dispersion medium to reduce the viscosity of the first or third mixture, thereby suppressing the generation of shear heat when preparing the first or third mixture or when removing the solvent from the first or third mixture while stirring at a specific desolvation temperature. In conventional methods for producing thermosetting resin compositions that do not use a solvent as a dispersion medium, it is difficult to reduce the cohesive force of the inorganic filler, and particularly when an inorganic filler with a low cut point is used, large shear heat may be generated, causing gelation of the thermosetting resin composition. In the manufacturing method of the present disclosure, a solvent is used when obtaining the first or third mixture, and therefore, compared to conventional manufacturing methods that do not use a solvent, a rise in temperature of the first or third mixture is suppressed, and it becomes possible to apply a sufficient shear force to the first or third mixture in the solvent removal step without worrying about gelation of the thermosetting resin composition. By applying a sufficient shear force to the first or third mixture, the inorganic filler in the thermosetting resin composition is more likely to be uniformly dispersed. In addition, by setting the specific desolvation temperature to be higher than the specific kneading temperature, the viscosity of the first or third mixture can be further reduced in the desolvation step, making it easier to stir the first or third mixture and making it easier to disperse the inorganic filler in the thermosetting resin composition more uniformly. Furthermore, by setting the specific kneading temperature lower than the specific desolvation temperature, it is possible to suppress the progress of the curing reaction between the thermosetting resin and the curing agent caused by the curing accelerator in the kneading process, thereby reducing the risk of gelling of the thermosetting resin composition. From the above, it is presumed that the dispersibility of the inorganic filler is further improved, and as a result, it becomes possible to highly pack the inorganic filler into the thermosetting resin composition.

[0013] In the present disclosure, the "kneading temperature" refers to the temperature of the heating section of a kneading device when the mixture is kneaded by the kneading device. In the present disclosure, the "desolvation temperature" refers to the temperature of the heating part of an apparatus for heating a mixture used when removing a solvent from the mixture. For example, when the desolvation step is performed in a batch manner using a vacuum dryer, the temperature of the heating part of the container that contains the mixture is taken as the desolvation temperature. On the other hand, when the desolvation step is performed using a kneading device, the temperature of the heating part of the kneading device is taken as the desolvation temperature. In this disclosure, both "mixing" and "kneading" refer to mixing a mixture. Mixing relatively low-viscosity materials, such as powders or powders and solvents, without applying shear is called "mixing", while dispersing and mixing simultaneously by applying shear to molten resin or a molten resin with a relatively low solvent content and high viscosity is called "kneading". The content of the solvent in the mixture for distinguishing between "mixing" and "kneading" is not strictly determined as a specific value.

[0014] Hereinafter, each step constituting the manufacturing method of the present disclosure and steps used as necessary will be described.

[0015] (Preparation of the mixture) In the first manufacturing method, a first mixture containing a thermosetting resin, a curing agent, and a slurry containing an inorganic filler and a solvent is used in the solvent removal step. The first mixture may contain other components such as a stress relaxation agent and an ion exchanger as necessary. The first mixture is obtained by mixing a slurry containing a thermosetting resin, a curing agent, an inorganic filler, and a solvent, and other components such as a stress relaxation agent and an ion exchanger that are used as necessary, using a mixer such as a stirrer or a planetary mixer, an ultrasonic disperser, a wet disperser such as a jet mill, etc. The mixing conditions for preparing the first mixture are appropriately set depending on the types of components contained in the first mixture, the ratio of the components, etc. In the first manufacturing method, in the solvent removal step, a composite mixture obtained by mixing a mixture containing a thermosetting resin, a slurry containing an inorganic filler, and a solvent, and a mixture containing a curing agent, a slurry containing an inorganic filler, and a solvent may be used as the first mixture. The composite mixture is obtained in the same manner as the first mixture.

[0016] In the second manufacturing method, a third mixture containing one of a thermosetting resin and a curing agent, and a slurry containing an inorganic filler and a solvent is used. The third mixture may contain other components such as a stress relaxation agent and an ion exchanger as necessary. The third mixture may also contain the other of the thermosetting resin and the curing agent. When the third mixture contains the other of the thermosetting resin and the curing agent, a part of the thermosetting resin or the curing agent contained in the thermosetting resin composition manufactured by the second manufacturing method is added to the third mixture. The third mixture is obtained in the same manner as the first mixture.

[0017] From the viewpoint of liquid transportability in the solvent removal step, the solid content ratio of the first or third mixture is preferably 30% by mass to 90% by mass, more preferably 40% by mass to 85% by mass, and even more preferably 50% by mass to 80% by mass.

[0018] (Solvent removal process) In the first production method, in the desolvation step, the solvent is removed from the first mixture at a first desolvation temperature to obtain a second mixture. When removing the solvent from the first mixture, the solvent may be removed while the first mixture is being mixed. The method for removing the solvent from the first mixture is not particularly limited, and examples thereof include a method of heating the first mixture, a method of placing the first mixture in a reduced pressure environment, a method of heating the first mixture while placing it in a reduced pressure environment, and the like. When the first mixture is placed in a reduced pressure environment, a known vacuum dryer may be used. At that time, the first mixture may be stirred. When the solvent is removed while mixing the first mixture, a known kneading device may be used, such as a screw-type kneader, a single-screw kneader, a twin-screw kneader, or a multi-screw kneader having three or more screws, or a roll mill, such as a two-roll mill or a three-roll mill. The stirring blade of the screw mixer may be supported at the base and the tip, or only at the base. From the viewpoint of improving mixing performance and productivity, it is preferable that the stirring blade is supported only at the base. Among these, a screw type kneader, which is an example of a closed system kneading device that allows removal of the solvent by reducing pressure, is preferred, and a twin-screw kneader is more preferred from the viewpoint of easy control of shear force. In addition, in order to add the hardening accelerator to the second mixture and subsequently further knead the second mixture to which the hardening accelerator has been added at the first kneading temperature, it is preferable to use a screw kneader as the kneading device.

[0019] In the second manufacturing method, in the desolvation step, the solvent is removed from a third mixture containing one of a thermosetting resin and a curing agent, and a slurry containing an inorganic filler and a solvent, at a second desolvation temperature, and then the other of the thermosetting resin and the curing agent is added, or the other of the thermosetting resin and the curing agent is added while removing the solvent at the second desolvation temperature from a third mixture containing one of a thermosetting resin and a curing agent, and a slurry containing an inorganic filler and a solvent, to obtain a fourth mixture. In the second manufacturing method, the method for obtaining the fourth mixture is not particularly limited, and the fourth mixture may be obtained by the same method as in the first manufacturing method. For example, a vacuum dryer may be used when removing the solvent from the third mixture at the second desolvation temperature. Also, a screw-type kneader may be used when adding the other of the thermosetting resin and the curing agent while removing the solvent from the third mixture at the second desolvation temperature. In addition, from the viewpoint of easily performing the operation of adding the other of the thermosetting resin and the curing agent to the third mixture, it is preferable to use a screw type kneader. When the solvent removal step in the second production method is performed using a screw type kneader, the other of the thermosetting resin and the curing agent may be added to the third mixture by a side feed.

[0020] The specific desolvation temperature is not particularly limited, and is preferably a temperature higher than the melting point or softening point of the thermosetting resin from the viewpoint of suppressing uneven distribution of the thermosetting resin. When two or more types of thermosetting resins are used in combination, the specific desolvation temperature is preferably a temperature higher than the melting point or softening point of the thermosetting resin having the highest melting point or softening point. The specific desolvation temperature is preferably a temperature 1° C. to 90° C. higher than the melting point or softening point of the thermosetting resin (when multiple types of thermosetting resins are used in combination, the thermosetting resin with the highest melting point or softening point), more preferably a temperature 1° C. to 70° C. higher, and even more preferably a temperature 1° C. to 60° C. higher. By carrying out the desolvation treatment using, for example, a screw kneader at such a temperature, the thermosetting resin can be melted and fluidity can be maintained, and therefore stirring and mixing can be performed well. In one embodiment, the specific desolvation temperature is preferably 30°C to 200°C, more preferably 50°C to 180°C, and even more preferably 80°C to 160°C.

[0021] When a screw type kneader is used as the kneading device, it is preferable to reduce the pressure inside the screw type kneader to remove the solvent. When a screw type kneader is used as the kneading device, from the viewpoint of distilling off the solvent, the pressure inside the screw type kneader is preferably 0.001 MPa to 0.08 MPa, more preferably 0.003 MPa to 0.06 MPa, and even more preferably 0.005 MPa to 0.05 MPa.

[0022] (Kneading process) In the manufacturing method disclosed herein, a curing accelerator is added to the second or fourth mixture obtained in the desolvation step, and the second or fourth mixture to which the curing accelerator has been added is kneaded at a specific kneading temperature that is lower than the specific desolvation temperature to obtain a kneaded product. The temperature of the second or fourth mixture when the curing accelerator is added to the second or fourth mixture is preferably lower than the specific desolvation temperature, from the viewpoint of suppressing the progress of the curing reaction between the thermosetting resin and the curing agent.

[0023] The specific kneading temperature is not particularly limited as long as it is lower than the specific desolvation temperature. From the viewpoint of suppressing gelation of the kneaded product in the kneading step, the specific kneading temperature is preferably set so that the reaction rate at the specific kneading temperature calculated based on differential scanning calorimetry for the second or fourth mixture to which the hardening accelerator has been added is small, and is preferably set to a temperature or lower at which the reaction rate is 40%, more preferably a temperature or lower at which the reaction rate is 30%, and even more preferably a temperature or lower at which the reaction rate is 20%. In the present disclosure, the reaction rate at a given temperature can be measured by the following method. For a sample obtained by adding a curing accelerator to the second or fourth mixture, a DSC chart is measured under conditions of a temperature rise rate of 10°C / min from 50°C. Next, the area from the rise temperature of the exothermic peak observed in the obtained DSC chart to the temperature set as the predetermined temperature and the total exothermic area of ​​the exothermic peaks are calculated. The area from the rise temperature of the exothermic peak to the predetermined temperature is divided by the total exothermic area and multiplied by 100 to obtain the reaction rate at the predetermined temperature.

[0024] In one embodiment, the specific kneading temperature is preferably 1° C. to 100° C. lower than the specific desolvation temperature, more preferably 10° C. to 90° C. lower, and even more preferably 20° C. to 85° C. lower. In one embodiment, the specific kneading temperature is preferably from 50°C to 150°C, more preferably from 60°C to 140°C, and even more preferably from 70°C to 120°C.

[0025] The method of adding the hardening accelerator to the second or fourth mixture is not particularly limited. When a screw-type kneader is used as the kneading device, it is preferable to knead the first or third mixture at a specific desolvation temperature to obtain the second or fourth mixture, and then add the hardening accelerator to the second or fourth mixture by side feeding. When the curing accelerator is added to the second or fourth mixture by side feeding, the curing accelerator may be added directly to the second or fourth mixture, or the curing accelerator may be mixed with the curing agent, inorganic filler, etc. to prepare a master batch, and the master batch may be added to the second or fourth mixture. To improve the accuracy of the amount of curing accelerator added, it is preferable to add the master batch to the second or fourth mixture.

[0026] When the masterbatch is added to the second or fourth mixture, the ratio of the masterbatch to the thermosetting resin composition obtained as a kneaded product in the kneading step is desirably 50 mass % or less. In one embodiment, the ratio of the masterbatch in the thermosetting resin composition obtained as a kneaded product is preferably less than 50% by mass, more preferably less than 30% by mass, and even more preferably less than 25% by mass. If it is 50% by mass or less, the mixing property after adding the masterbatch to the second or fourth mixture tends to be improved. The ratio of the masterbatch may be 5% by mass or more.

[0027] (Post-processing) In the manufacturing method of the present disclosure, the thermosetting resin composition obtained as a kneaded product may be cooled and pulverized to obtain a powdered thermosetting resin composition. The thermosetting resin composition obtained through kneading may be molded into a granular, tablet, pellet, or granular shape (cylindrical granules, etc.). The pulverization method or molding method of the thermosetting resin composition is not particularly limited, and a conventionally known method may be used.

[0028] In the production method of the present disclosure, the desolvation step and the kneading step may be carried out continuously. Also, in the production method of the present disclosure, the desolvation step may be carried out in a batch manner. When the desolvation step and the kneading step are carried out continuously, it is preferable to use a screw type kneader for carrying out the desolvation step and the kneading step. When using a screw type kneader, the desolvation step and the kneading step can be carried out continuously by carrying out the kneading step successively after the desolvation step. When the desolvation step is carried out in a batch manner, the second or fourth mixture obtained in the desolvation step may be cooled and pulverized to a powder form, and the curing accelerator may be added to the powder form of the second or fourth mixture and kneaded with a screw kneader to obtain a thermosetting resin composition. In this case, the method of adding the curing accelerator to the second or fourth mixture is not particularly limited, and a mixture of the second or fourth mixture and the curing accelerator may be kneaded with a screw kneader, or the curing accelerator may be added to the second or fourth mixture by a side feed.

[0029] Next, the various components used in the manufacturing method of the present disclosure will be described in detail.

[0030] (thermosetting resin) The thermosetting resin composition produced by the production method of the present disclosure contains a thermosetting resin. The type of thermosetting resin is not particularly limited, and examples thereof include epoxy resin, phenol resin, urea resin, thiol resin, melamine resin, urethane resin, silicone resin, maleimide resin, and unsaturated polyester resin. In the present disclosure, a resin that exhibits both thermoplastic and thermosetting properties, such as an acrylic resin containing an epoxy group, is included in the term "thermosetting resin." The thermosetting resin may be solid or liquid at room temperature and normal pressure (e.g., 25°C and atmospheric pressure), and is preferably solid. The thermosetting resin may be used alone or in combination of two or more types.

[0031] The thermosetting resin preferably includes an epoxy resin. The type of epoxy resin is not particularly limited as long as it has two or more epoxy groups in one molecule. Specifically, the novolac type epoxy resins are obtained by epoxidizing a novolac resin obtained by condensing or co-condensing at least one phenolic compound selected from the group consisting of phenolic compounds such as phenol, cresol, xylenol, resorcin, catechol, bisphenol A, bisphenol F, and naphthol compounds such as α-naphthol, β-naphthol, and dihydroxynaphthalene with an aliphatic aldehyde compound such as formaldehyde, acetaldehyde, and propionaldehyde under an acidic catalyst (phenol novolac type epoxy resin, orthocresol novolac type epoxy resin, etc.); the triphenylmethane type epoxy resins are obtained by epoxidizing a triphenylmethane type phenolic resin obtained by condensing or co-condensing the above phenolic compound with an aromatic aldehyde compound such as benzaldehyde or salicylaldehyde under an acidic catalyst; and the novolac resins are obtained by co-condensing the above phenolic compound and naphthol compound with an aldehyde compound under an acidic catalyst (triphenylmethane type epoxy resins). diphenylmethane type epoxy resins which are diglycidyl ethers of bisphenol A, bisphenol F, etc.; biphenyl type epoxy resins which are diglycidyl ethers of alkyl-substituted or unsubstituted biphenols; stilbene type epoxy resins which are diglycidyl ethers of stilbene-based phenolic compounds; sulfur-containing type epoxy resins which are diglycidyl ethers of bisphenol S, etc.; epoxy resins which are glycidyl ethers of alcohols such as butanediol, polyethylene glycol, and polypropylene glycol; glycidyl ester type epoxy resins which are glycidyl esters of polyvalent carboxylic acid compounds such as phthalic acid, isophthalic acid, and tetrahydrophthalic acid; glycidylamine type epoxy resins in which active hydrogen bonded to nitrogen atoms of aniline, diaminodiphenylmethane, isocyanuric acid, etc. is substituted with a glycidyl group; dicyclopentadiene type epoxy resins which are epoxidized co-condensation resins of dicyclopentadiene and phenolic compounds;Alicyclic epoxy resins such as vinylcyclohexene diepoxide, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, and 2-(3,4-epoxy)cyclohexyl-5,5-spiro(3,4-epoxy)cyclohexane-m-dioxane, which are epoxy-modified epoxy resins in which the olefin bonds in the molecule have been epoxidized; paraxylylene-modified epoxy resins, which are glycidyl ethers of paraxylylene-modified phenolic resins; metaxylylene-modified epoxy resins, which are glycidyl ethers of metaxylylene-modified phenolic resins; terpene-modified epoxy resins, which are glycidyl ethers of terpene-modified phenolic resins; and dicyclopentadiene-modified phenolic resins, which are glycidyl ethers of dicyclopentadiene-modified phenolic resins. Examples of the epoxy resin include pentadiene-modified epoxy resins; cyclopentadiene-modified epoxy resins which are glycidyl ethers of cyclopentadiene-modified phenolic resins; polycyclic aromatic ring-modified epoxy resins which are glycidyl ethers of polycyclic aromatic ring-modified phenolic resins; naphthalene-type epoxy resins which are glycidyl ethers of naphthalene ring-containing phenolic resins; halogenated phenol novolac-type epoxy resins; hydroquinone-type epoxy resins; trimethylolpropane-type epoxy resins; linear aliphatic epoxy resins obtained by oxidizing olefin bonds with peracids such as peracetic acid; aralkyl-type epoxy resins obtained by epoxidizing aralkyl-type phenolic resins such as phenol aralkyl resins and naphthol aralkyl resins; and the like. Further examples of the epoxy resin include epoxidized silicone resins and aminophenol-type epoxy resins which are glycidyl ethers of aminophenol. These epoxy resins may be used alone or in combination of two or more.

[0032] Among the above epoxy resins, from the viewpoint of the balance between heat resistance and fluidity, epoxy resins selected from the group consisting of biphenyl type epoxy resins, stilbene type epoxy resins, diphenylmethane type epoxy resins, sulfur atom-containing type epoxy resins, novolac type epoxy resins, dicyclopentadiene type epoxy resins, triphenylmethane type epoxy resins, copolymer type epoxy resins and aralkyl type epoxy resins (these are referred to as "specific epoxy resins"). The specific epoxy resins may be used alone or in combination of two or more.

[0033] When the epoxy resin contains a specific epoxy resin, from the viewpoint of exhibiting the performance of the specific epoxy resin, the content thereof is preferably 30% by mass or more, and more preferably 50% by mass or more, of the entire epoxy resin.

[0034] Among the specific epoxy resins, from the viewpoint of fluidity, biphenyl type epoxy resins, stilbene type epoxy resins, diphenylmethane type epoxy resins, or sulfur atom-containing type epoxy resins are more preferable, and from the viewpoint of heat resistance, dicyclopentadiene type epoxy resins, triphenylmethane type epoxy resins, or aralkyl type epoxy resins are preferable. Specific examples of preferable epoxy resins are shown below.

[0035] The biphenyl type epoxy resin is not particularly limited as long as it is an epoxy resin having a biphenyl skeleton. For example, an epoxy resin represented by the following general formula (II) is preferred. Among the epoxy resins represented by the following general formula (II), R 8 In the above, the oxygen atoms are substituted at the 4 and 4' positions, and the 3, 3', 5 and 5' positions are methyl groups. 8 YX-4000H (Mitsubishi Chemical Corporation, product name) where R is a hydrogen atom, 8 4,4'-bis(2,3-epoxypropoxy)biphenyl, where R is a hydrogen atom; 8 When is a hydrogen atom and R 8 The oxygen atom is substituted at the 4 and 4' positions, and the 3, 3', 5, and 5' positions are methyl groups. 8is a hydrogen atom, YL-6121H (product name, Mitsubishi Chemical Corporation) and the like are commercially available.

[0036] [ka]

[0037] In formula (II), R 8 represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aromatic group having 4 to 18 carbon atoms, and may be the same or different. n is an average value and represents a number from 0 to 10.

[0038] The stilbene type epoxy resin is not particularly limited as long as it is an epoxy resin having a stilbene skeleton. For example, an epoxy resin represented by the following general formula (III) is preferred. Among the epoxy resins represented by the following general formula (III), R 9 In the above, the oxygen atoms are substituted at the 4 and 4' positions, and the 3, 3', 5 and 5' positions are methyl groups. 9 is a hydrogen atom, and R 10 are all hydrogen atoms, and R 9 Three of the 3, 3', 5, and 5' positions are methyl groups, one is a t-butyl group, and the remaining R 9 is a hydrogen atom, and R 10 and mixtures of those in which all of the above are hydrogen atoms.

[0039] [ka]

[0040] In formula (III), R 9 and R 10 represents a hydrogen atom or a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. n is an average value and represents a number from 0 to 10.

[0041] The diphenylmethane type epoxy resin is not particularly limited as long as it is an epoxy resin having a diphenylmethane skeleton. For example, an epoxy resin represented by the following general formula (IV) is preferable. Among the epoxy resins represented by the following general formula (IV), R 11 are all hydrogen atoms, and R 12 In the above, the oxygen atoms are substituted at the 4 and 4' positions, and the 3, 3', 5 and 5' positions are methyl groups. 12 YSLV-80XY (product name, Nippon Steel Chemical & Material Co., Ltd.), in which R is a hydrogen atom, is commercially available.

[0042] [ka]

[0043] In formula (IV), R 11 and R 12 represents a hydrogen atom or a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. n is an average value and represents a number from 0 to 10.

[0044] The sulfur-containing epoxy resin is not particularly limited as long as it is an epoxy resin containing a sulfur atom. For example, an epoxy resin represented by the following general formula (V) is included. Among the epoxy resins represented by the following general formula (V), R 13 In the above, when the oxygen atom is substituted at the 4 and 4' positions, the 3 and 3' positions are t-butyl groups, the 6 and 6' positions are methyl groups, and the remaining R 13 YSLV-120TE (product name, Nippon Steel Chemical & Material Co., Ltd.), in which R is a hydrogen atom, is commercially available.

[0045] [ka]

[0046] In formula (V), R 13represents a hydrogen atom or a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. n is an average value and represents a number from 0 to 10.

[0047] The novolac type epoxy resin is not particularly limited as long as it is an epoxy resin obtained by epoxidizing a novolac type phenolic resin. For example, an epoxy resin obtained by epoxidizing a novolac type phenolic resin such as a phenol novolac resin, a cresol novolac resin, or a naphthol novolac resin using a method such as glycidyl etherification is preferred, and an epoxy resin represented by the following general formula (VI) is more preferred. Among the epoxy resins represented by the following general formula (VI), R 14 are all hydrogen atoms, and R 15 is a methyl group, and i=1; ESCN-190 and ESCN-195 (product names, Sumitomo Chemical Co., Ltd.); 14 N-770 and N-775 (trade names, DIC Corporation) in which all of R 14 are all hydrogen atoms, the part where i = 0 and the part where i = 1, R 15 -CH(CH 3 YDAN-1000-10C (product name, Nippon Steel Chemical & Material Co., Ltd.), a styrene-modified phenol novolac type epoxy resin having a moiety of R 14 are all hydrogen atoms, i=1, and R 15 is a methyl group and i=2, R 15 Benzyl group-modified cresol novolac epoxy resins, in which one moiety is a methyl group and the other is a benzyl group, are commercially available.

[0048] [ka]

[0049] In formula (VI), R 14 R represents a hydrogen atom or a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. 15represents a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. Each i independently represents an integer of 0 to 3. n is an average value and represents a number of 0 to 10.

[0050] The dicyclopentadiene type epoxy resin is not particularly limited as long as it is an epoxy resin obtained by epoxidizing a compound having a dicyclopentadiene skeleton as a raw material. For example, an epoxy resin represented by the following general formula (VII) is preferable. Among the epoxy resins represented by the following general formula (VII), HP-7200 (DIC Corporation, trade name) where i=0 is available as a commercially available product.

[0051] [ka]

[0052] In formula (VII), R 16 represents a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. Each i independently represents an integer of 0 to 3. n is an average value and represents a number of 0 to 10.

[0053] The triphenylmethane type epoxy resin is not particularly limited as long as it is an epoxy resin made from a compound having a triphenylmethane skeleton. For example, an epoxy resin obtained by glycidyl etherification of a triphenylmethane type phenolic resin obtained from an aromatic aldehyde compound and a phenolic compound is preferred, and an epoxy resin represented by the following general formula (VIII) is more preferred. Among the epoxy resins represented by the following general formula (VIII), 1032H60 (Mitsubishi Chemical Corporation, product name) and EPPN-502H (Nippon Kayaku Co., Ltd., product name), in which i is 0 and k is 0, are commercially available.

[0054] [ka]

[0055] In formula (VIII), R 17 and R 18represents a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. Each i independently represents an integer of 0 to 3, and each k independently represents an integer of 0 to 4. n is an average value and represents a number of 0 to 10.

[0056] The copolymerized epoxy resin obtained by epoxidizing a novolac resin obtained from a naphthol compound, a phenol compound, and an aldehyde compound is not particularly limited as long as it is an epoxy resin made from a compound having a naphthol skeleton and a compound having a phenol skeleton as raw materials. For example, an epoxy resin obtained by glycidyl etherification of a novolac type phenol resin using a compound having a naphthol skeleton and a compound having a phenol skeleton is preferred, and an epoxy resin represented by the following general formula (IX) is more preferred. Among the epoxy resins represented by the following general formula (IX), R 21 is a methyl group, i is 1, j is 0, and k is 0, and NC-7300 (trade name, Nippon Kayaku Co., Ltd.) is available as a commercially available product.

[0057] [ka]

[0058] In formula (IX), R 19 ~R 21 represents a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. Each i is independently an integer of 0 to 3, each j is independently an integer of 0 to 2, and each k is independently an integer of 0 to 4. Each l and m is an average value and a number of 0 to 10, and (l+m) is a number of 0 to 10. The terminal of the epoxy resin represented by formula (IX) is either one of the following formulas (IX-1) or (IX-2). In formulas (IX-1) and (IX-2), R 19 ~R 21 The definitions of i, j and k are as follows: 19 ~R 21 The definitions of i, j and k are the same as those of i, j and k. n is 1 (when bonding via a methylene group) or 0 (when bonding not via a methylene group).

[0059] [ka]

[0060] The epoxy resin represented by the above general formula (IX) may be a random copolymer containing l structural units and m structural units randomly, an alternating copolymer containing them alternately, a copolymer containing them regularly, a block copolymer containing them in a block form, etc. Any one of these may be used alone, or two or more may be used in combination.

[0061] Another preferred copolymer epoxy resin is Epiclon HP-5000 (trade name, DIC Corporation), a methoxynaphthalene-cresol formaldehyde co-condensation epoxy resin containing the following two structural units in a random, alternating or block order: In the following general formula, n and m are each an average value and a number from 0 to 10, and (n+m) is a number from 0 to 10, preferably n and m are each an average value and a number from 1 to 9, and (n+m) is a number from 2 to 10.

[0062] [ka]

[0063] The aralkyl type epoxy resin is not particularly limited as long as it is an epoxy resin made from a phenolic resin synthesized from at least one selected from the group consisting of phenolic compounds such as phenol, cresol, and naphthol compounds such as naphthol and dimethylnaphthol, and dimethoxyparaxylene, bis(methoxymethyl)biphenyl, or a derivative thereof. For example, an epoxy resin obtained by glycidyl etherification of a phenolic resin synthesized from at least one selected from the group consisting of phenolic compounds such as phenol, cresol, and naphthol compounds such as naphthol and dimethylnaphthol, and dimethoxyparaxylene, bis(methoxymethyl)biphenyl, or a derivative thereof is preferred, and an epoxy resin represented by the following general formulas (X) and (XI) is more preferred.

[0064] Among the epoxy resins represented by the following general formula (X), i is 0 and R 38 is a hydrogen atom, i is 0, and R 38 is a hydrogen atom and all R 8 CER-3000 (product name, Nippon Kayaku Co., Ltd.), which is a mixture of epoxy resins in which l is a hydrogen atom and epoxy resins in which k is a hydrogen atom at a mass ratio of 80:20, is commercially available. Furthermore, among the epoxy resins represented by the following general formula (XI), ESN-175 (product name, Nippon Steel Chemical & Material Co., Ltd.), in which l is 0, j is 0, and k is 0, is commercially available.

[0065] [ka]

[0066] In formulae (X) and (XI), R 38 R represents a hydrogen atom or a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. 37 , R 39 ~R 41 represents a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. Each i is independently an integer of 0 to 3, each j is independently an integer of 0 to 2, each k is independently an integer of 0 to 4, and each 1 is independently an integer of 0 to 4. Each n is an average value and is independently a number of 0 to 10.

[0067] R in the above general formulas (II) to (XI) 8 ~R 21 and R 37 ~R 41 With respect to the above, the term "may all be the same or different" means, for example, that 8 to 88 R 8 This means that all of the R may be the same or different. 9 ~R 21 and R 37 ~R 41In addition, the numbers of each element in the formula may all be the same or different. 8 ~R 21 and R 37 ~R 41 may be the same or different. For example, R 9 and R 10 may be the same or different. In addition, the monovalent organic group having 1 to 18 carbon atoms in the general formulas (III) to (XI) is preferably an alkyl group or an aryl group.

[0068] In the above general formulas (II) to (XI), n is an average value, and each is preferably independently in the range of 0 to 10. When n is 10 or less, the melt viscosity of the resin component does not become too high, and the viscosity of the thermosetting resin composition during melt molding decreases, and the occurrence of filling defects, deformation of bonding wires (gold wires connecting elements and leads), etc. tends to be suppressed. It is more preferable to set n in the range of 0 to 4.

[0069] Specific examples of preferred epoxy resins that can be used in the thermosetting resin composition have been described above in accordance with the general formulas (II) to (XI). More specific preferred epoxy resins include 4,4'-bis(2,3-epoxypropoxy)-3,3',5,5'-tetramethylbiphenyl from the viewpoint of heat resistance, and 4,4'-bis(2,3-epoxypropoxy)-biphenyl from the viewpoints of moldability and heat resistance.

[0070] The epoxy equivalent of the epoxy resin is not particularly limited. From the viewpoint of the balance of various properties such as moldability, heat resistance, and electrical reliability, the epoxy equivalent of the epoxy resin is preferably 60 g / eq to 1000 g / eq, and more preferably 80 g / eq to 500 g / eq.

[0071] The epoxy resin may be liquid or solid. When the epoxy resin is solid, the softening point or melting point of the epoxy resin is not particularly limited. From the viewpoints of moldability and heat resistance, it is preferably 40°C to 180°C, and from the viewpoint of handling during preparation of the thermosetting resin composition, it is more preferably 50°C to 130°C. In the present disclosure, the softening point refers to a value measured by the ring and ball method of JIS K 7234:1986. In the present disclosure, the melting point refers to a value measured in accordance with the visual observation method of JIS K 0064:1992.

[0072] From the viewpoints of strength, fluidity, heat resistance, moldability, etc., the content of the epoxy resin in the thermosetting resin composition is preferably 0.5% by mass to 60% by mass, and more preferably 2% by mass to 50% by mass.

[0073] (hardening agent) The thermosetting resin composition produced by the production method of the present disclosure contains a curing agent. The type of the curing agent is not particularly limited, and is not particularly limited as long as it is a compound that undergoes a curing reaction with the thermosetting resin used in combination. For example, curing agents used in combination with an epoxy resin include phenol-based curing agents, amine-based curing agents, acid anhydride-based curing agents, polymercaptan-based curing agents, polyaminoamide-based curing agents, isocyanate-based curing agents, and blocked isocyanate-based curing agents. The curing agent may be used alone or in combination of two or more. The curing agent may be solid or liquid at room temperature and normal pressure (for example, 25°C, atmospheric pressure), and is preferably solid. When the thermosetting resin is an epoxy resin, the curing agent is preferably a phenol-based curing agent or an amine-based curing agent from the viewpoint of heat resistance. Examples of phenol-based curing agents include phenol resins and polyhydric phenol compounds having two or more phenolic hydroxyl groups in one molecule.Specific examples of the phenol-based curing agent include polyhydric phenol compounds such as resorcin, catechol, bisphenol A, bisphenol F, and substituted or unsubstituted biphenol; novolac-type phenol resins obtained by condensing or co-condensing at least one phenolic compound selected from the group consisting of phenolic compounds such as phenol, cresol, xylenol, resorcin, catechol, bisphenol A, bisphenol F, phenylphenol, and aminophenol, and naphthol compounds such as α-naphthol, β-naphthol, and dihydroxynaphthalene, with aldehyde compounds such as formaldehyde, acetaldehyde, and propionaldehyde, under an acid catalyst; phenolic compounds synthesized from the above-mentioned phenolic compounds and dimethoxyparaxylene, bis(methoxymethyl)biphenyl, and the like; Examples of the phenolic curing agent include aralkyl-type phenolic resins such as nol aralkyl resins and naphthol aralkyl resins; paraxylylene and / or metaxylylene modified phenolic resins; melamine modified phenolic resins; terpene modified phenolic resins; dicyclopentadiene-type phenolic resins and dicyclopentadiene-type naphthol resins synthesized by copolymerization of the above phenolic compounds and dicyclopentadiene; cyclopentadiene modified phenolic resins; polycyclic aromatic ring modified phenolic resins; biphenyl type phenolic resins; triphenylmethane type phenolic resins obtained by condensing or co-condensing the above phenolic compounds with aromatic aldehyde compounds such as benzaldehyde and salicylaldehyde under an acid catalyst; and phenolic resins obtained by copolymerizing two or more of these. These phenolic curing agents may be used alone or in combination of two or more.

[0074] Among the phenol-based curing agents, from the viewpoint of heat resistance, at least one selected from the group consisting of aralkyl-type phenolic resins, dicyclopentadiene-type phenolic resins, triphenylmethane-type phenolic resins, copolymerized phenolic resins of triphenylmethane-type phenolic resins and aralkyl-type phenolic resins, and novolac-type phenolic resins (these are referred to as "specific phenol-based curing agents"). The specific phenol-based curing agents may be used alone or in combination of two or more.

[0075] When the phenol-based curing agent contains a specific phenol-based curing agent, from the viewpoint of fully exerting the performance thereof, the content of the specific phenol-based curing agent is preferably 30 mass% or more, and more preferably 50 mass% or more, of the entire phenol-based curing agent.

[0076] Examples of the aralkyl type phenolic resin include phenol aralkyl resins and naphthol aralkyl resins synthesized from a phenolic compound and dimethoxy-para-xylene, bis(methoxymethyl)biphenyl, etc. The aralkyl type phenolic resin may be further copolymerized with other phenolic resins. Examples of the copolymerized aralkyl type phenolic resin include a copolymerized phenolic resin of a triphenylmethane type phenolic resin and an aralkyl type phenolic resin, a copolymerized phenolic resin of a salicylaldehyde type phenolic resin and an aralkyl type phenolic resin, and a copolymerized phenolic resin of a novolac type phenolic resin and an aralkyl type phenolic resin.

[0077] The aralkyl type phenolic resin is not particularly limited as long as it is a phenolic resin synthesized from at least one selected from the group consisting of phenolic compounds and naphthol compounds, and dimethoxy-para-xylene, bis(methoxymethyl)biphenyl or a derivative thereof. For example, phenolic resins represented by the following general formulas (XII) to (XIV) are preferred.

[0078] [ka]

[0079] In formulas (XII) to (XIV), R 23 R represents a hydrogen atom or a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. 22 , R 24 , R 25 and R 28 R represents a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. 26 and R 27 represents a hydroxyl group or a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. Each i is independently an integer of 0 to 3, each j is independently an integer of 0 to 2, each k is independently an integer of 0 to 4, and each p is independently an integer of 0 to 4. Each n is an average value and is independently a number of 0 to 10.

[0080] Among the phenolic resins represented by the above general formula (XII), i is 0 and R 23 MEH-7851 (product name, Meiwa Kasei Co., Ltd.), in which all are hydrogen atoms, is commercially available.

[0081] Among the phenolic resins represented by the above general formula (XIII), XL-225, XLC (Mitsui Chemicals, Inc., product name), MEH-7800 (Meiwa Chemical Industry Co., Ltd., product name), etc., in which i is 0 and k is 0, are commercially available.

[0082] Among the phenolic resins represented by the above general formula (XIV), SN-170 (trade name, Nippon Steel Chemical & Material Co., Ltd.), in which j is 0, k is 0, and p is 0, and SN-170 (trade name, Nippon Steel Chemical & Material Co., Ltd.), in which j is 0, k is 1, and R 27 is a hydroxyl group and p is 0, and SN-395 (product name, Nippon Steel Chemical & Material Co., Ltd.) is available as a commercially available product.

[0083] The dicyclopentadiene type phenolic resin is not particularly limited as long as it is a phenolic resin obtained from a compound having a dicyclopentadiene skeleton. For example, a phenolic resin represented by the following general formula (XV) is preferable. Among the phenolic resins represented by the following general formula (XV), a phenolic resin in which i is 0 is commercially available.

[0084] [ka]

[0085] In formula (XV), R 29 represents a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. Each i independently represents an integer of 0 to 3. n is an average value and represents a number of 0 to 10.

[0086] The triphenylmethane type phenolic resin is not particularly limited as long as it is a phenolic resin obtained from an aromatic aldehyde compound as a raw material. For example, a phenolic resin represented by the following general formula (XVI) is preferable.

[0087] Among the phenol resins represented by the following general formula (XVI), MEH-7500 (product name, Meiwa Kasei Co., Ltd.), in which i is 0 and k is 0, is commercially available.

[0088] [ka]

[0089] In formula (XVI), R 30 and R 31 represents a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. Each i is independently an integer of 0 to 3, and each k is independently an integer of 0 to 4. n is an average value and is a number of 0 to 10.

[0090] The copolymerized phenolic resin of triphenylmethane type phenolic resin and aralkyl type phenolic resin is not particularly limited as long as it is a copolymerized phenolic resin of aralkyl type phenolic resin and phenolic resin obtained from a compound having a benzaldehyde skeleton as a raw material. For example, a phenolic resin represented by the following general formula (XVII) is preferable.

[0091] Among the phenolic resins represented by the following general formula (XVII), HE-510 (trade name, Air Water Chemical Co., Ltd.), in which i is 0, k is 0, and q is 0, is commercially available.

[0092] [ka]

[0093] In formula (XVII), R 32 ~R 34 represents a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. Each i is independently an integer of 0 to 3, each k is independently an integer of 0 to 4, and each q is independently an integer of 0 to 5. Each l and m is an average value and independently a number of 0 to 11, provided that the sum of l and m is a number of 1 to 11.

[0094] The novolac type phenolic resin is not particularly limited as long as it is a phenolic resin obtained by condensing or co-condensing at least one phenolic compound selected from the group consisting of phenolic compounds and naphthol compounds with an aldehyde compound under an acid catalyst. For example, a phenolic resin represented by the following general formula (XVIII) is preferred.

[0095] Among the phenolic resins represented by the following general formula (XVIII), i is 0 and R 35 are commercially available products such as Tamanor 758 and 759 (trade names, Arakawa Chemical Industries, Ltd.) and H-4 (trade name, Meiwa Chemical Industry Co., Ltd.).

[0096] [ka]

[0097] In formula (XVIII), R 35 R represents a hydrogen atom or a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. 36 represents a monovalent organic group having 1 to 18 carbon atoms, and may be the same or different. Each i independently represents an integer of 0 to 3. n is an average value and represents a number of 0 to 10.

[0098] R in the above general formulas (XII) to (XVIII) 22 ~R 36 The description of "may be the same or different" means, for example, that i R 22 This means that all of the R's may be the same or different from each other. 23 ~R 36 In addition, the numbers of each of the groups in the formula may all be the same or different from each other. 22 ~R 36 may be the same or different. For example, R 22 and R 23 may be the same or different, and R 30 and R 31 may be the same or different.

[0099] In the above general formulas (XII) to (XVIII), n is preferably in the range of 0 to 10. If it is 10 or less, the melt viscosity of the resin component does not become too high, and the viscosity of the thermosetting resin composition during melt molding also becomes low, making it difficult for filling defects, deformation of bonding wires (gold wires connecting elements and leads), etc. to occur. The average n in one molecule is preferably set in the range of 0 to 4.

[0100] Specific examples of the amine-based curing agent include aliphatic amine compounds such as diethylenetriamine, triethylenetetramine, n-propylamine, 2-hydroxyethylaminopropylamine, cyclohexylamine, and 4,4'-diamino-dicyclohexylmethane, aromatic amine compounds such as diethyltoluenediamine, 3,3'-diethyl-4,4'-diaminodiphenylmethane, dimethylthiotoluenediamine, and 2-methylaniline, imidazole compounds such as imidazole, 2-methylimidazole, 2-ethylimidazole, and 2-isopropylimidazole, imidazoline compounds such as imidazoline, 2-methylimidazoline, and 2-ethylimidazoline, etc. Among these, aromatic amine compounds are preferred from the viewpoint of storage stability, and diethyltoluenediamine, 3,3'-diethyl-4,4'-diaminodiphenylmethane, and dimethylthiotoluenediamine are more preferred.

[0101] The functional group equivalent of the curing agent (hydroxyl group equivalent in the case of a phenolic curing agent, active hydrogen equivalent in the case of an amine curing agent) is not particularly limited. From the viewpoint of the balance of various properties such as moldability, heat resistance, and electrical reliability, it is preferably 10 g / eq to 1000 g / eq, and more preferably 30 g / eq to 500 g / eq. The hydroxyl equivalent in the case of a phenolic curing agent is a value calculated based on the hydroxyl value measured in accordance with JIS K0070: 1992. The active hydrogen equivalent in the case of an amine curing agent is a value calculated based on the amine value measured in accordance with JIS K7237: 1995.

[0102] When the curing agent is solid, the softening point or melting point is not particularly limited, but is preferably 40° C. to 180° C. from the viewpoints of moldability and heat resistance, and more preferably 50° C. to 130° C. from the viewpoint of handleability during production of the thermosetting resin composition.

[0103] When the thermosetting resin is an epoxy resin, the equivalent ratio of the epoxy resin to the curing agent (molar number of epoxy groups in the resin / molar number of active hydrogens in the curing agent) is not particularly limited, but from the viewpoint of keeping the unreacted amounts of each to a minimum, it is, for example, preferably 0.7 to 1.6, more preferably 0.8 to 1.4, and even more preferably 0.9 to 1.2.

[0104] (slurry) In the manufacturing method of the present disclosure, a slurry containing an inorganic filler and a solvent is used. The slurry is obtained by mixing the inorganic filler, the solvent, and the coupling agent, dispersant, etc., which are used as necessary, using a mixer such as a stirrer, a planetary mixer, etc., or a wet disperser such as an ultrasonic disperser or a jet mill, etc. The mixing conditions for preparing the slurry are appropriately set depending on the types of components contained in the slurry, the ratio of the components, etc. The inorganic filler contained in the slurry may be subjected to a wet sieving process. The wet sieving process tends to be more likely to make the top cut diameter, which will be described later, smaller than the dry sieving process.

[0105] The solid content ratio of the inorganic filler in the slurry is preferably 40% by mass to 90% by mass, more preferably 50% by mass to 85% by mass, and even more preferably 60% by mass to 80% by mass, from the viewpoint of suppressing sedimentation.

[0106] -Inorganic filler- The slurry contains an inorganic filler. The type of inorganic filler is not particularly limited. Specifically, inorganic materials such as spherical silica, crystalline silica, glass, alumina, calcium carbonate, zirconium silicate, calcium silicate, silicon nitride, aluminum nitride, boron nitride, aluminum nitride, boehmite, beryllia, magnesium oxide, zirconia, zircon, fosterite, steatite, spinel, mullite, titania, talc, clay, mica, and titanates can be mentioned. Inorganic fillers having a flame retardant effect may be used. Examples of inorganic fillers having a flame retardant effect include aluminum hydroxide, magnesium hydroxide, composite metal hydroxides such as composite hydroxides of magnesium and zinc, and zinc borate. Among them, spherical silica is preferred from the viewpoint of reducing the linear expansion coefficient, and alumina is preferred from the viewpoint of high thermal conductivity. The inorganic fillers may be used alone or in combination of two or more types. Examples of the state of the inorganic filler include powder, beads obtained by sphering powder, and fibers.

[0107] The top cut diameter of the inorganic filler is not particularly limited. From the viewpoint of filling into narrow gaps of 30 μm or less, the top cut diameter of the inorganic filler is preferably 10 μm or less, more preferably 7 μm or less, even more preferably 6 μm or less, and particularly preferably 5 μm or less. From the viewpoint of suppressing the increase in viscosity of the thermosetting resin composition, the top cut diameter of the inorganic filler may be 1 μm or more. In the present disclosure, the top cut diameter of an inorganic filler refers to the particle size value at which the volume cumulative distribution curve is drawn from the small diameter side using a laser diffraction scattering particle size distribution measuring device, and the volume integrated value is 90% by volume.

[0108] The average particle size of the inorganic filler is not particularly limited. For example, the volume average particle size is preferably 10 μm or less, more preferably 0.1 μm to 10 μm, even more preferably 0.1 μm to 8 μm, and particularly preferably 0.2 μm to 6 μm. When the volume average particle size is 10 μm or less, the filling ability into narrow gaps tends to be improved. Also, when the volume average particle size is 0.1 μm or more, the increase in viscosity of the thermosetting resin composition tends to be further suppressed. The volume average particle diameter of the inorganic filler can be measured as the volume average particle diameter (D50) by a laser diffraction scattering particle size distribution measuring device.

[0109] From the viewpoint of flowability of the thermosetting resin composition, the particle shape of the inorganic filler is preferably spherical rather than angular, and the particle size distribution of the inorganic filler is preferably distributed over a wide range.

[0110] The content of the inorganic filler in the thermosetting resin composition is not particularly limited. From the viewpoint of fluidity and strength, it is preferably 30% by volume to 95% by volume of the entire thermosetting resin composition, more preferably 35% by volume to 90% by volume, and even more preferably 40% by volume to 80% by volume. When the content of the inorganic filler is 30% by volume or more of the entire thermosetting resin composition, the properties such as the thermal expansion coefficient, thermal conductivity, and elastic modulus of the cured product tend to be further improved. When the content of the inorganic filler is 95% by volume or less of the entire thermosetting resin composition, the increase in viscosity of the thermosetting resin composition is suppressed, and the fluidity is further improved, tending to improve the moldability.

[0111] -solvent- The slurry contains a solvent. The type of the solvent is not particularly limited, and is appropriately selected from those that can be easily removed from the first or third mixture in the solvent removal step. The solvent contained in the first or third mixture may or may not dissolve either the thermosetting resin or the curing agent.

[0112] The boiling point of the solvent at normal pressure is preferably 50°C to 200°C, more preferably 60°C to 180°C, even more preferably 70°C to 160°C, particularly preferably 70°C to 140°C, and extremely preferably 70°C to 130°C, since the solvent can be easily removed from the first or third mixture.

[0113] Specific examples of the solvent include methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), toluene, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone (CHN), etc. Among these, MIBK, CHN, or MEK is preferred. The solvent may be used alone or in combination of two or more kinds.

[0114] -Coupling agent- The slurry may further contain a coupling agent. The type of the coupling agent is not particularly limited, and a known coupling agent can be used. Examples of the coupling agent include a silane coupling agent and a titanium coupling agent. The coupling agent may be used alone or in combination of two or more types.

[0115] Specific examples of the silane coupling agent include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-ureidopropyltriethoxysilane, octenyltrimethoxysilane, glycidoxyoctyltrimethoxysilane, and methacryloxyoctyltrimethoxysilane.

[0116] Examples of titanium coupling agents include isopropyl triisostearoyl titanate, isopropyl tris(dioctyl pyrophosphate) titanate, isopropyl tri(N-aminoethyl-aminoethyl) titanate, tetraoctyl bis(ditridecyl phosphite) titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl phosphite) titanate, bis(dioctyl pyrophosphate)oxyacetate titanate, bis(dioctyl pyrophosphate)ethylene titanate, isopropyl trioctanoyl titanate, isopropyl dimethacryl isostearoyl titanate, isopropyl tridodecyl benzenesulfonyl titanate, isopropyl isostearoyl diacryl titanate, isopropyl tri(dioctyl phosphate) titanate, isopropyl tricumyl phenyl titanate, and tetraisopropyl bis(dioctyl phosphite) titanate.

[0117] When the slurry contains a coupling agent, the content of the coupling agent is preferably 0.001 to 10 parts by mass, more preferably 0.01 to 8 parts by mass, and even more preferably 0.05 to 5 parts by mass, relative to 100 parts by mass of the inorganic filler, from the viewpoint of adhesion at the interface between the thermosetting resin and the inorganic filler.

[0118] By including a coupling agent in the slurry, the inorganic filler can be surface-treated more uniformly with the coupling agent than in the dry treatment method, and therefore the flowability of the thermosetting resin composition produced by the production method of the present disclosure is further improved.

[0119] (Cure accelerator) The thermosetting resin composition produced by the production method of the present disclosure contains a curing accelerator. The type of the curing accelerator is not particularly limited and can be selected depending on the type of thermosetting resin, the desired properties of the thermosetting resin composition, and the like.

[0120] Specifically, diazabicycloalkenes such as 1,5-diazabicyclo[4.3.0]nonene-5 (DBN) and 1,8-diazabicyclo[5.4.0]undecene-7 (DBU), cyclic amidine compounds such as 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, and 2-heptadecylimidazole, derivatives of the cyclic amidine compounds, phenol novolak salts of the cyclic amidine compounds or their derivatives, and combinations of these compounds with maleic anhydride, 1,4-benzoquinone, 2,5-toluquinone, 1,4-naphthoquinone, 2,3-dimethylbenzoquinone, 2,6-dimethylbenzoquinone, 2,3-dimethoxy-5-methyl-1,4-benzoquinone, 2,3-dimethoxy-1,4-benzoquinone, and phenyl-1,4-benzoquinone, diazof compounds having intramolecular polarization obtained by adding a compound having a π bond, such as phenylmethane; cyclic amidinium compounds such as the tetraphenylborate salt of DBU, the tetraphenylborate salt of DBN, the tetraphenylborate salt of 2-ethyl-4-methylimidazole, and the tetraphenylborate salt of N-methylmorpholine; tertiary amine compounds such as pyridine, triethylamine, triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol; derivatives of the above tertiary amine compounds; ammonium salt compounds such as tetra-n-butylammonium acetate, tetra-n-butylammonium phosphate, tetraethylammonium acetate, tetra-n-hexylammonium benzoate, and tetrapropylammonium hydroxide;organic phosphines such as primary phosphines, e.g., ethylphosphine, phenylphosphine, etc.; secondary phosphines, e.g., dimethylphosphine, diphenylphosphine, etc.; and tertiary phosphines, e.g., triphenylphosphine, diphenyl(p-tolyl)phosphine, tris(alkylphenyl)phosphine, tris(alkoxyphenyl)phosphine, tris(alkylalkoxyphenyl)phosphine, tris(dialkylphenyl)phosphine, tris(trialkylphenyl)phosphine, tris(tetraalkylphenyl)phosphine, tris(dialkoxyphenyl)phosphine, tris(trialkoxyphenyl)phosphine, tris(tetraalkoxyphenyl)phosphine, trialkylphosphine, dialkylarylphosphine, alkyldiarylphosphine, trinaphthylphosphine, tris(benzyl)phosphine; phosphine compounds, e.g., complexes of the organic phosphines and organic borons; and complexes of the organic phosphines or the phosphine compounds with maleic anhydride, 1,4-benzoquinone, 2,5-toluquinone, 1,4-naphthoquinone, 2,3-dimethylbenzoquinone, compounds having intramolecular polarization obtained by adding a compound having a π bond, such as quinone compounds, such as 2,6-dimethylbenzoquinone, 2,3-dimethoxy-5-methyl-1,4-benzoquinone, 2,3-dimethoxy-1,4-benzoquinone, phenyl-1,4-benzoquinone, and anthraquinone, and diazophenylmethane; compounds having intramolecular polarization obtained by adding a compound having a π bond, such as the organic phosphines or the phosphine compounds, and 4-bromophenol, 3-bromophenol, 2-bromophenol, 4-chlorophenol, 3-chlorophenol, 2-chlorophenol, and 4-iodophenol; a compound having intramolecular polarization, which is obtained by reacting a halogenated phenol compound such as phenol, 3-iodophenol, 2-iodophenol, 4-bromo-2-methylphenol, 4-bromo-3-methylphenol, 4-bromo-2,6-dimethylphenol, 4-bromo-3,5-dimethylphenol, 4-bromo-2,6-di-t-butylphenol, 4-chloro-1-naphthol, 1-bromo-2-naphthol, 6-bromo-2-naphthol, or 4-bromo-4'-hydroxybiphenyl, followed by a dehydrohalogenation process;Examples of the tetra-substituted phosphonium include tetra-substituted phosphonium compounds such as tetraphenylphosphonium, tetraphenylborate salts of tetra-substituted phosphonium such as tetraphenylphosphonium tetra-p-tolylborate, and salts of tetra-substituted phosphonium with phenolic compounds; phosphobetaine compounds; and adducts of phosphonium compounds with silane compounds. For example, examples of a curing accelerator that is particularly suitable when an epoxy resin is used as the thermosetting resin include triphenylphosphine and an adduct of triphenylphosphine and a quinone compound. Furthermore, for example, when an epoxy resin is used as the thermosetting resin, examples of curing accelerators that enable low-temperature curing include an adduct of tributylphosphine and 1,4-benzoquinone, dimethylaminopyridine, 2-ethyl-4-methylimidazole, 2-methylimidazole, and 1-benzyl-2-methylimidazole. The curing accelerators may be used alone or in combination of two or more.

[0121] The content of the curing accelerator in the thermosetting resin composition is preferably 0.1 mass % to 8 mass %, more preferably 0.3 mass % to 6 mass %, and even more preferably 0.5 mass % to 5 mass %, based on the total amount of the thermosetting resin and the curing agent.

[0122] (Coloring agent) The thermosetting resin composition produced by the production method of the present disclosure may contain a colorant. Examples of colorants include known colorants such as carbon black, black titanium oxide, organic dyes, organic pigments, red lead, and red iron oxide. The content of the colorant can be appropriately selected depending on the purpose, etc. The colorants may be used alone or in combination of two or more.

[0123] When the thermosetting resin composition contains a colorant, the content thereof is preferably from 0.01% by mass to 5% by mass, and more preferably from 0.05% by mass to 3% by mass. When the thermosetting resin composition contains a colorant, the colorant may be added to the first or third mixture.

[0124] (Ion exchanger) The thermosetting resin composition produced by the production method of the present disclosure may contain an ion exchanger. In particular, from the viewpoint of improving the moisture resistance and high-temperature storage characteristics of the semiconductor device, it is preferable to contain an ion exchanger. The ion exchanger is not particularly limited, and conventionally known ones can be used. Specifically, for example, hydrotalcite compounds and hydrous oxides of at least one element selected from the group consisting of magnesium, aluminum, titanium, zirconium, and bismuth can be mentioned. The ion exchanger may be used alone or in combination of two or more. Among them, hydrotalcite represented by the following general formula (A) is preferable.

[0125] Mg (1-X) Al X (OH) 2 (CO 3 ) X / 2 ·mH 2 O ……(A) (0 < X ≦ 0.5, m is a positive number)

[0126] When the thermosetting resin composition contains an ion exchanger, its content is not particularly limited as long as it is sufficient to capture ions such as halogen ions. For example, it is preferably 0.1 part by mass to 30 parts by mass, and more preferably 1 part by mass to 5 parts by mass with respect to 100 parts by mass of the thermosetting resin. When the thermosetting resin composition contains an ion exchanger, the ion exchanger may be added to the first or third mixture.

[0127] (Release agent) The thermosetting resin composition produced by the production method of the present disclosure may contain a release agent from the viewpoint of obtaining good releasability from the mold during molding. The release agent is not particularly limited, and a conventionally known one may be used. Specific examples include carnauba wax, higher fatty acids such as montanic acid and stearic acid, higher fatty acid metal salts, ester waxes such as montanic acid esters, polyolefin waxes such as oxidized polyethylene and non-oxidized polyethylene, etc. The release agent may be used alone or in combination of two or more types.

[0128] When the thermosetting resin composition contains a release agent, the content is preferably 0.01 to 15 parts by mass, more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the thermosetting resin. When the amount of the release agent is 0.01 parts by mass or more relative to 100 parts by mass of the thermosetting resin, sufficient releasability tends to be obtained. When the amount of the release agent is 15 parts by mass or less relative to 100 parts by mass of the thermosetting resin, better adhesion tends to be obtained. When the thermosetting resin composition contains a release agent, the release agent may be added to the first or third mixture.

[0129] (Flame retardant) The thermosetting resin composition produced by the production method of the present disclosure may contain a flame retardant. The flame retardant is not particularly limited, and a conventionally known one may be used. Specific examples include organic or inorganic compounds containing halogen atoms, antimony atoms, nitrogen atoms, or phosphorus atoms, metal hydroxides, etc. The flame retardant may be used alone or in combination of two or more types.

[0130] When the thermosetting resin composition contains a flame retardant, the content is not particularly limited as long as it is a sufficient amount to obtain the desired flame retardant effect. For example, the content is preferably 1 to 30 parts by mass, more preferably 2 to 20 parts by mass, per 100 parts by mass of the thermosetting resin. When the thermosetting resin composition contains a flame retardant, the flame retardant may be added to the first or third mixture.

[0131] (Stress reliever) The thermosetting resin composition produced by the production method of the present disclosure may contain a stress relaxation agent such as silicone oil or silicone rubber particles. By containing a stress relaxation agent in the thermosetting resin composition, it is possible to further reduce the warpage deformation of the package and the occurrence of package cracks. Examples of the stress relaxation agent include known stress relaxation agents (flexible agents) that are generally used. Specifically, examples of the stress relaxation agent include thermoplastic elastomers such as silicone-based, styrene-based, olefin-based, urethane-based, polyester-based, polyether-based, polyamide-based, and polybutadiene-based elastomers, NR (natural rubber), NBR (acrylonitrile-butadiene rubber), acrylic rubber, urethane rubber, and silicone powder, and rubber particles having a core-shell structure such as methyl methacrylate-styrene-butadiene copolymer (MBS), methyl methacrylate-silicone copolymer, and methyl methacrylate-butyl acrylate copolymer. The stress relaxation agent may be used alone or in combination of two or more types. Among them, silicone-based stress relaxation agents are preferred. Examples of the silicone-based stress relaxation agent include those having an epoxy group, those having an amino group, and those modified with polyether.

[0132] When the thermosetting resin composition contains a stress relaxation agent, the content thereof is preferably 0.1 to 30 parts by mass, and more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the thermosetting resin. When the thermosetting resin composition contains a stress relaxation agent, the stress relaxation agent may be added to the first or third mixture. When a stress relief agent is used, the stress relief agent may be added to the first or third mixture in the form of a slurry similar to the inorganic filler. When a stress relaxation agent is used, the solid content ratio of the stress relaxation agent in the slurry is preferably 0.1 mass % to 50 mass % from the viewpoint of moldability, more preferably 0.2 mass % to 30 mass %, and even more preferably 0.5 mass % to 20 mass %. As the solvent for dispersing the stress relaxation agent, the same solvent as that used for the slurry of the inorganic filler can be used.

[0133] (solvent) The thermosetting resin composition produced by the production method of the present disclosure may contain a solvent. When the thermosetting resin composition contains a solvent, the flowability during molding tends to be improved. When the thermosetting resin composition contains a solvent, the content of the solvent in the entire thermosetting resin composition is preferably 0.1% by mass to 2% by mass, and more preferably 0.1% by mass to 0.5% by mass. When the content of the solvent in the entire thermosetting resin composition is 2% by mass or less, blocking of the thermosetting resin composition is unlikely to occur, and the thermosetting resin composition tends to be easily supplied to a molding machine such as a press. When the content of the solvent in the entire thermosetting resin composition is 0.1% by mass or more, the flowability during molding tends to be further improved. The solvent contained in the thermosetting resin composition may be a residual solvent contained in the slurry. The solvent contained in the thermosetting resin composition may be referred to as a "residual solvent amount." The content of the solvent is calculated based on the change in mass before and after heating the thermosetting resin composition at 175° C. for one hour.

[0134] (Physical Properties of Thermosetting Resin Composition) The viscosity of the thermosetting resin composition is not particularly limited. It is preferable to adjust the viscosity to a desired value depending on the molding method, the composition of the thermosetting resin composition, etc. When the thermosetting resin composition is used for sealing material applications, it is preferable to adjust the viscosity of the thermosetting resin composition depending on the tendency of wire sweep during molding. For example, when the thermosetting resin composition is used as an encapsulant, from the viewpoint of reducing wire sweep, etc., the viscosity of the thermosetting resin composition is preferably 200 Pa·s or less at 175° C., more preferably 150 Pa·s or less, even more preferably 100 Pa·s or less, particularly preferably 70 Pa·s or less, and extremely preferably 50 Pa·s or less. The lower limit of the viscosity of the thermosetting resin composition is not particularly limited, and may be, for example, 2 Pa·s or more at 175° C. The viscosity of the thermosetting resin composition can be measured by a Koka type flow tester (for example, manufactured by Shimadzu Corporation).

[0135] (Uses of thermosetting resin composition) The use of the thermosetting resin composition produced by the production method of the present disclosure is not particularly limited, and can be used in various mounting techniques, for example, as a sealant for electronic component devices. The thermosetting resin composition of the present disclosure can also be used in various applications in which it is desirable for the resin composition to have good fluidity and curability, such as resin molded bodies for various modules, resin molded bodies for motors, resin molded bodies mounted on vehicles, and sealants for electronic circuit protection materials.

[0136] <Electronic component device manufacturing method> The method for producing an electronic component device according to the present disclosure includes a step of encapsulating an element with the thermosetting resin composition obtained by the production method according to the present disclosure described above.

[0137] Examples of electronic component devices include devices obtained by mounting elements (active elements such as semiconductor chips, transistors, diodes, and thyristors, and passive elements such as capacitors, resistors, and coils) on a support member such as a lead frame, a pre-wired tape carrier, a wiring board, glass, a silicon wafer, or an organic substrate, and then sealing the resulting element portion with a thermosetting resin composition. More specifically, typical resin-sealed ICs such as DIP (Dual Inline Package), PLCC (Plastic Leaded Chip Carrier), QFP (Quad Flat Package), SOP (Small Outline Package), SOJ (Small Outline J-lead package), TSOP (Thin Small Outline Package), and TQFP (Thin Quad Flat Package) have a structure in which an element is fixed on a lead frame, terminal parts of the element such as bonding pads and lead parts are connected by wire bonding, bumps, or the like, and then sealed by transfer molding or the like using a thermosetting resin composition; TCP (Tape Carrier Package) has a structure in which an element connected to a tape carrier by bumps is sealed with a thermosetting resin composition; and COB (Chip On Board) has a structure in which an element connected to wiring formed on a support member by wire bonding, flip chip bonding, solder, or the like, is sealed with a thermosetting resin composition. Examples of suitable printed wiring boards include a BGA (Ball Grid Array), CSP, MCP (Multi Chip Package), and SiP, which have a structure in which an element is mounted on the surface of a support member having terminals for connecting a wiring board formed on the back side thereof, the element is connected to wiring formed on the support member by bump or wire bonding, and the element is then sealed with a thermosetting resin composition.The thermosetting resin composition can also be suitably used in printed wiring boards.

[0138] Methods for encapsulating electronic device components using a thermosetting resin composition include low pressure transfer molding, injection molding, compression molding, and the like.

[0139] <Thermosetting resin composition> The thermosetting resin composition of the present disclosure can be obtained by the production method of the present disclosure described above. The thermosetting resin composition may be solid or liquid at room temperature and normal pressure (for example, 25°C, atmospheric pressure), and is preferably solid. When the thermosetting resin composition is solid, the shape is not particularly limited, and examples thereof include powder, granules, tablets, pellets, and granules. When the thermosetting resin composition is in tablet or pellet form, the dimensions and mass are preferably set to be suitable for the molding conditions of the package from the viewpoint of handling. EXAMPLES

[0140] The present disclosure will be specifically described below with reference to examples, but the present disclosure is not limited to these examples.

[0141] <Preparation of Thermosetting Resin Composition> First, the following components were prepared.

[0142] (thermosetting resin) Epoxy resin 1: NC-3000 (product name, Nippon Kayaku Co., Ltd., aralkyl type epoxy resin with epoxy equivalent of 265g / eq to 285g / eq and softening point of 53℃ to 63℃) Epoxy resin 2: jER YX-4000H (product name, Mitsubishi Chemical Corporation, biphenyl type epoxy resin with epoxy equivalent of 180g / eq to 192g / eq and melting point of 105°C) Epoxy resin 3: EPPN501HY (trade name, Nippon Kayaku Co., Ltd., triphenylmethane type epoxy resin with epoxy equivalent of 163g / eq to 175g / eq and softening point of 57℃ to 63℃)

[0143] (hardening agent) Hardener 1: MEHC-7851 (product name, Meiwa Kasei Co., Ltd., aralkyl-type phenolic resin with hydroxyl equivalent of 205 g / eq, softening point 60°C to 70°C) Hardener 2: MEHC-7800 (product name, Meiwa Kasei Co., Ltd., aralkyl-type phenolic resin with hydroxyl equivalent of 170g / eq, softening point 60℃~70℃)

[0144] (Coupling Agent) Coupling agent: N-phenyl-3-aminopropyltrimethoxysilane

[0145] (Inorganic filler) Slurry 1: Methyl isobutyl ketone solution of spherical silica with a volume average particle size of 1.5 μm (top cut diameter 5 μm), solid content 70 mass% (treated with N-phenyl-3-aminopropyltrimethoxysilane) Slurry 2: Methyl isobutyl ketone solution of spherical silica with a volume average particle size of 0.3 μm (top cut diameter 5 μm), solid content 60 mass% (treated with N-phenyl-3-aminopropyltrimethoxysilane) Inorganic filler: Spherical silica with a volume average particle size of 0.8 μm (top cut diameter 20 μm) (no surface treatment)

[0146] (Cure accelerator) -Cure accelerator: Phosphorus-based cure accelerator

[0147] (Other additives) Release agent: Hoechst wax (Hoechst) Colorant: Carbon black ·MIBK: Methyl isobutyl ketone CHN: Cyclohexanone MEK: Methyl ethyl ketone

[0148] The thermosetting resin compositions of Examples 1 to 9 were prepared by the following method (referred to as "production method A"). The main feed components shown in Table 1 were mixed in a container and stirred with a stirrer for 1 hour. The obtained mixture corresponds to the first mixture. Then, using a twin-screw kneader (extruder), the mixture was melt-kneaded for about 5 minutes at the desolvation temperature in Table 1 under reduced pressure of 0.02 MPa. The mixture after melt-kneading corresponds to the second mixture. Subsequently, the auxiliary feed components were added from the opening and melt-kneaded for about 2 minutes at the kneading temperature in Table 1. The molten material was cooled with a press roll through which cold water at 10°C was circulated, and the sheet-like product was pulverized to prepare a powdered thermosetting resin composition. In production method A, the desolvation step and the kneading step are performed continuously.

[0149] The thermosetting resin composition of Example 10 was prepared by the following method (referred to as "production method B"). The main supply components shown in Table 1 were mixed in a container and stirred with a stirrer for 1 hour. The resulting mixture corresponds to the first mixture. The solvent was distilled off at 140°C for 2 hours under a reduced pressure of 0.02 MPa using a vacuum dryer. The resulting mixture corresponds to the second mixture. The melt was cooled and the resulting resin composition was pulverized to prepare a powdered thermosetting resin composition to which no curing accelerator was added. Subsequently, the thermosetting resin composition to which no curing accelerator was added was kneaded using a twin-screw kneader (extruder). At this time, the auxiliary supply components were added from the opening and melt-kneaded for about 2 minutes at the kneading temperature in Table 1. The melt was cooled with a press roll through which cold water at 10°C was circulated, and the sheet-like product was pulverized to prepare a powdered thermosetting resin composition. In production method B, the desolvation step is performed in a batch manner.

[0150] The thermosetting resin compositions of Comparative Examples 1 to 3 were produced by the following method (referred to as "production method C"). All of the components shown in Table 2 were mixed in a container and stirred with a stirrer for 1 hour. Then, using a twin-screw kneader (extruder), the mixture was melt-kneaded for about 5 minutes at the first kneading temperature in Table 2 under reduced pressure of 0.02 MPa. Subsequently, the mixture was melt-kneaded for about 2 minutes at the second kneading temperature. The molten material was cooled with a press roll through which cold water at 10°C was circulated, and the sheet-like material was pulverized to prepare a powdered thermosetting resin composition.

[0151] The thermosetting resin composition of Comparative Example 4 was produced by the following method (referred to as "production method D"). All of the components shown in Table 2 were mixed in a container and stirred with a stirrer for 1 hour. Then, the solvent was distilled off at 140°C for 2 hours under a reduced pressure of 0.02 MPa using a vacuum dryer. The resulting molten product was cooled and pulverized to prepare a powdered thermosetting resin composition.

[0152] <Evaluation of Thermosetting Resin Composition> The prepared thermosetting resin compositions were evaluated by the following various tests. The evaluation results are shown in Tables 1 and 2. Unless otherwise specified, the thermosetting resin compositions were molded using a transfer molding machine under the conditions of a mold temperature of 180°C, a molding pressure of 6.9 MPa, and a curing time of 90 seconds. In addition, post-curing was performed at 175°C for 6 hours, if necessary.

[0153] [Spiral Flow] Using a spiral flow measurement mold conforming to EMMI-1-66, the thermosetting resin composition was molded under the above conditions, and the flow distance (cm) was determined.

[0154] [Agglomeration of inorganic fillers] The appearance of the molded product of the thermosetting resin composition using the transfer molding machine was visually observed, and the presence or absence of aggregation of the inorganic filler (hereinafter, sometimes referred to as filler aggregation) was evaluated. Cases where filler aggregation was observed were rated as "A," and cases where filler aggregation was not observed were rated as "B."

[0155] [Gel time] Measurement was carried out at a temperature of 175° C. using a Curelastometer manufactured by JSR Trading Co., Ltd. for 3 g of the thermosetting resin composition, and the time until the torque curve rose was taken as the gel time (GT, seconds).

[0156] [Residual Solvent Amount] 5 g of the thermosetting resin composition was treated at 175°C for 1 hour using an explosion-proof dryer, and the amount of residual solvent was calculated using formula 1. From the viewpoint of the occurrence of voids after molding, a residual solvent amount of 0.5 mass% or less was rated as "A", a residual solvent amount of more than 0.5 mass% but less than 2 mass% was rated as "B", and a residual solvent amount of more than 2 mass% was rated as "C". Residual solvent amount (mass%) = ((mass before heat treatment - mass after heat treatment) / mass before heat treatment) x 100

[0157] [Table 1]

[0158] [Table 2]

[0159] In Tables 1 and 2, "non-volatile components" refers to the mass content of non-volatile components when the main feed components are added to a container, and corresponds to the solid content ratio of the mixture. In Tables 1 and 2, "filler content" refers to the volume content of inorganic filler contained in the thermosetting resin composition.

[0160] As is clear from the evaluation results in Tables 1 and 2, when the filler content was 70 volume % or more, the properties of the thermosetting resin composition obtained by the manufacturing method of the Example were superior to the properties of the thermosetting resin composition obtained by the manufacturing method of the Comparative Example. From this, it can be seen that the manufacturing method of the Example enables high loading of inorganic filler without deteriorating the properties of the thermosetting resin composition compared to the manufacturing method of the Comparative Example.

Claims

1. a desolvation step of removing the solvent from a first mixture containing a thermosetting resin, a curing agent, an inorganic filler, and a slurry containing a solvent at a first desolvation temperature to obtain a second mixture; a kneading step of adding a curing accelerator to the second mixture and kneading the second mixture to which the curing accelerator has been added at a first kneading temperature that is lower than the first desolvation temperature; A method for producing a thermosetting resin composition comprising the steps of:

2. 2. The method for producing a thermosetting resin composition according to claim 1, wherein the first kneading temperature is equal to or lower than a temperature at which a reaction rate of the second mixture to which the curing accelerator has been added is 40% as measured by differential scanning calorimetry.

3. 3. The method for producing a thermosetting resin composition according to claim 1, wherein the first desolvation temperature is higher than a melting point or a softening point of the thermosetting resin.

4. The method for producing a thermosetting resin composition according to any one of claims 1 to 3, wherein the solid content ratio of the first mixture is 30% by mass to 90% by mass.

5. a desolvation step of removing the solvent from a third mixture containing one of a thermosetting resin and a curing agent, and a slurry containing an inorganic filler and a solvent at a second desolvation temperature, and then adding the other of the thermosetting resin and the curing agent, or adding the other of the thermosetting resin and the curing agent while removing the solvent at the second desolvation temperature from a third mixture containing one of a thermosetting resin and a curing agent, and a slurry containing an inorganic filler and a solvent, to obtain a fourth mixture; a kneading step of adding a hardening accelerator to the fourth mixture and kneading the fourth mixture to which the hardening accelerator has been added at a second kneading temperature that is lower than the second desolvation temperature; A method for producing a thermosetting resin composition comprising the steps of:

6. 6. The method for producing a thermosetting resin composition according to claim 5, wherein the second kneading temperature is equal to or lower than a temperature at which a reaction rate of the fourth mixture to which the curing accelerator has been added is 40% as measured by differential scanning calorimetry.

7. A method for producing a thermosetting resin composition described in claim 5 or claim 6, wherein the second desolvation temperature is higher than the melting point or softening point of the thermosetting resin.

8. A method for producing a thermosetting resin composition described in any one of claims 5 to 7, wherein the solid content ratio of the third mixture is 30 mass% to 90 mass%.

9. The method for producing a thermosetting resin composition according to any one of claims 1 to 8, wherein the solvent removing step and the kneading step are carried out continuously.

10. The method for producing a thermosetting resin composition according to any one of claims 1 to 8, wherein the solvent removal step is carried out in a batch manner.

11. The method for producing a thermosetting resin composition according to any one of claims 1 to 10, wherein the slurry further contains a coupling agent.

12. The method for producing a thermosetting resin composition according to any one of claims 1 to 11, wherein the inorganic filler has a top cut diameter of 10 µm or less.

13. The method for producing a thermosetting resin composition according to any one of claims 1 to 12, wherein the boiling point of the solvent is 50°C to 200°C.

14. The method for producing a thermosetting resin composition according to any one of claims 1 to 13, wherein a solid content ratio of the inorganic filler in the slurry is 40% by mass to 90% by mass.

15. A method for producing an electronic component device, comprising a step of encapsulating an element with a thermosetting resin composition obtained by the method for producing a thermosetting resin composition according to any one of claims 1 to 14.

Citation Information

Patent Citations

  • Liquid crystal sealant and liquid crystal display cell using the same

    JP2008088350A

  • Method for producing epoxy resin molding material for sealing semiconductor, and resin-sealed semiconductor device

    JP2011252041A

  • Method for producing epoxy resin molding material for sealing semiconductor, and resin-sealed semiconductor device

    JP2011252042A

  • Liquid curable resin composition and application thereof