Silicon wafer cleaning method and manufacturing method, and method for evaluating hydrogen peroxide concentration in cleaning solution and method for managing hydrogen peroxide concentration

A cleaning method using ammonium hydroxide and hydrogen peroxide solutions effectively roughens silicon wafer surfaces, addressing transportation defects and enabling precise hydrogen peroxide concentration management, ensuring stable and high-quality wafer production.

JP7571691B2Active Publication Date: 2024-10-23SHIN ETSU HANDOTAI CO LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2021144950
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-06
Publication Date
2024-10-23
Estimated Expiration
2041-09-06

AI Technical Summary

Technical Problem

Existing silicon wafer manufacturing processes face challenges in transporting wafers due to inadequate surface roughness, leading to transportation failures during wet environments, and there is a need for accurate evaluation and management of hydrogen peroxide concentration in cleaning solutions to stabilize roughening behavior.

Method used

A cleaning method using an aqueous solution with ammonium hydroxide and hydrogen peroxide concentrations of 0 to 0.15 wt% to selectively roughen the front and back surfaces of silicon wafers, combined with methods to evaluate and control hydrogen peroxide concentration, ensuring stable roughening conditions.

Benefits of technology

The method enables stable roughening of silicon wafer surfaces, reducing transportation defects and allowing for accurate evaluation and management of hydrogen peroxide concentration, resulting in high-quality wafers with controlled roughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571691000002
    Figure 0007571691000002
  • Figure 0007571691000003
    Figure 0007571691000003
  • Figure 0007571691000004
    Figure 0007571691000004
Patent Text Reader

Abstract

To provide: a cleaning method capable of roughening the front and back surfaces or the back surface of a silicon wafer; a manufacturing method of a silicon wafer, capable of achieving a silicon wafer, only one surface of which is roughened; and an evaluation method and a management method of hydrogen peroxide concentration in minute amount in a cleaning solution that affects roughening behavior.SOLUTION: Provided is a cleaning method of a silicon wafer, in which the silicon wafer is roughened. The cleaning method includes: acquiring, in advance, a relationship between cleaning temperature, NH4OH concentration, H2O2 concentration, and an amount of roughening for the front and back surfaces or the back surface of a study silicon wafer that has no native oxide film and has an exposed bare surface, when the study silicon wafer is cleaned with a cleaning solution that contains ammonium hydroxide and is an aqueous solution having a hydrogen peroxide concentration of 0-0.15 wt.%; determining, based on the relationship, roughening cleaning conditions of the cleaning temperature, the NH4OH concentration and the H2O2 concentration from a desired amount of roughening; and roughening the front and back surfaces or the back surface of a silicon wafer to be roughened that has no native oxide film and has an exposed bare surface by cleaning the silicon wafer to be roughened under the determined roughening cleaning conditions.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for cleaning and manufacturing a silicon wafer capable of roughening the front and back surfaces or the back surface of a silicon wafer, and a method for evaluating and managing the hydrogen peroxide concentration in a cleaning solution. [Background technology]

[0002] The manufacturing process for silicon wafers for semiconductor devices consists of a single crystal manufacturing process in which a single crystal ingot is grown using the Czochralski (CZ) method or similar, and a wafer processing process in which this single crystal ingot is sliced ​​and processed to a mirror finish. In order to add value, the process may also include an annealing process in which heat treatment is performed and an epitaxial growth process in which an epitaxial layer is formed.

[0003] The process of processing the wafer into a mirror-like finish consists of the DSP (double-sided polishing) process and the subsequent CMP (single-sided polishing) process. More specifically, from the perspective of particle quality and transportation, DSP processed wafers are not dried, but are cleaned as necessary, and then stored underwater before being transported to the CMP process. Therefore, in the CMP process, the wafers stored underwater must be chucked by a robot or similar device and transported to the CMP device. Similarly, after CMP processing, wafers wet with abrasives or pure water must be chucked and transported to the cleaning process as necessary.

[0004] In this way, in the wafer processing process, it is essential to transport the wafer in a wet environment, not a dry one. In particular, in such a wet environment, when a wafer adsorbed by a chuck is to be detached, the wafer may not be detached even if the chuck is released, causing a transport failure. This is thought to be caused by the roughness of the wafer surface to be chucked. If the roughness of the wafer surface to be chucked is too good, the contact area with the chuck increases, making it difficult to detach the wafer even if the chuck is released. On the other hand, if the roughness of the wafer surface is poor, the contact area decreases, making it easy to detach the wafer. In general, the chucked surface is prone to forming chuck marks to some extent, which reduces the quality, and therefore the chuck surface is often the back surface of the silicon wafer. Therefore, from the viewpoint of reducing transport failure, it is better to have a rough back surface of the silicon wafer, and a method for manufacturing such a wafer is required.

[0005] A common method for cleaning silicon wafers is called RCA cleaning, which is a method that combines SC1 (Standard Cleaning 1), SC2 (Standard Cleaning 2), and DHF (Diluted Hydrofluoric Acid) cleaning depending on the purpose. The SC1 cleaning is a cleaning method in which ammonia water and hydrogen peroxide water are mixed in a given ratio, and the silicon wafer surface is etched with an alkaline cleaning solution to lift off adhering particles, and then the electrostatic repulsion between the silicon wafer and the particles is used to remove the particles while suppressing their re-adhesion to the silicon wafer. SC2 cleaning is a cleaning method in which metal impurities on the silicon wafer surface are dissolved and removed using a cleaning solution in which hydrochloric acid and hydrogen peroxide water are mixed in a given ratio. DHF cleaning is a cleaning method in which chemical oxide films on the silicon wafer surface are removed using dilute hydrofluoric acid. Ozone water cleaning, which has a strong oxidizing power, may also be used to remove organic matter adhering to the silicon wafer surface and to form chemical oxide films on the silicon wafer surface after DHF cleaning. Silicon wafers are cleaned by combining these cleaning methods depending on the purpose. Among these, SC1 cleaning involves etching, and it is generally known that the wafer surface roughness increases after SC1 cleaning.

[0006] Additionally, methods for evaluating the surface roughness of a wafer can use the Sa (three-dimensional calculated average height) value obtained by AFM (Atomic Force Microscopy) or the Haze value obtained by a particle counter as indicators. Haze is expressed as cloudiness and is widely used as an indicator of the roughness of silicon surfaces, with a high haze level indicating a rough wafer surface. Haze inspection using a particle counter has a very high throughput and can inspect the entire surface of a wafer.

[0007] Patent Document 1 describes a method of cleaning silicon wafers with a diluted aqueous solution of ammonium hydroxide, hydrogen peroxide, and water having a composition in the range of 1:1:5 to 1:1:2000, and forming native oxide films of different thicknesses. In Patent Document 2, OH ionized from ammonium hydroxide is used in SC1 cleaning. -It has been reported that when the concentration of is high, direct etching of Si occurs preferentially, and the wafer surface roughness increases. Patent Documents 3 to 6 also disclose techniques relating to cleaning of semiconductor substrates such as silicon wafers.

[0008] In addition, when the SC1 cleaning solution is used at high temperatures, the concentration of ammonium hydroxide and hydrogen peroxide decreases due to decomposition and evaporation reactions. Therefore, it is desirable to monitor the concentration of the solution and adjust it to keep it constant. Methods for evaluating the concentration of the SC1 cleaning solution include concentration measurement methods using absorbance and refractive index, which are known to be highly accurate, but the concentration range is limited. It is currently difficult to evaluate the concentration of low-concentration chemicals in particular. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 7-66195 [Patent Document 2] JP 2011-82372 A [Patent Document 3] Japanese Patent Application Publication No. 7-240394 [Patent Document 4] Japanese Patent Application Publication No. 10-242107 [Patent Document 5] Japanese Patent Application Publication No. 11-121419 [Patent Document 6] Special Publication No. 2012-523706 Summary of the Invention [Problem to be solved by the invention]

[0010] As described above, a silicon wafer having a rough back surface to be chucked is required to reduce transport defects during processing. The present invention has been made to solve the above problem, and aims to provide a cleaning method capable of roughening the front and back surfaces or the back surface of a silicon wafer, a manufacturing method for a silicon wafer capable of obtaining a silicon wafer having only one surface selectively roughened, and a method for evaluating and managing the concentration of a trace amount of hydrogen peroxide in a cleaning solution that affects the roughening behavior. [Means for solving the problem]

[0011] In order to achieve the above object, the present invention provides a cleaning method for roughening a silicon wafer, comprising the steps of: A silicon wafer for investigation having an exposed bare surface free of a native oxide film is roughened by cleaning the silicon wafer with a cleaning solution that contains ammonium hydroxide and has a hydrogen peroxide concentration of 0 to 0.15 wt %. The roughening amount of the front and back surfaces or the back surface of the silicon wafer for investigation; The temperature of the cleaning liquid; and a concentration of ammonium hydroxide in the cleaning solution; and a cleaning solution concentration investigation step of acquiring a correlation with the hydrogen peroxide concentration in the cleaning solution in advance; a roughening cleaning condition determining step of determining roughening cleaning conditions, including a temperature of the cleaning solution, an ammonium hydroxide concentration and a hydrogen peroxide concentration in the cleaning solution, from a desired roughening amount based on the correlation obtained in the cleaning solution concentration investigating step; and a roughening cleaning step of roughening the front and back surfaces or the back surface of the silicon wafer to be roughened by cleaning the silicon wafer to be roughened, the bare surface of which is exposed and free from a native oxide film, under the roughening cleaning conditions determined in the roughening cleaning condition determination step.

[0012] Such a silicon wafer cleaning method makes it possible to manufacture a wafer whose front and back surfaces or the back surface are roughened to a desired degree. Furthermore, by investigating the dependency of the hydrogen peroxide concentration on the degree of roughening, more suitable roughening cleaning conditions can be selected. In particular, the roughening cleaning conditions can be selected so as to reduce the variation in the degree of roughening.

[0013] At this time, in the cleaning solution concentration investigation step, The haze value of the test silicon wafer is obtained by a particle counter before and after the cleaning, and the increase in the haze value after the cleaning can be regarded as the amount of roughening.

[0014] Such a method makes it possible to monitor the roughening behavior and the amount of roughening simply and with good throughput.

[0015] In addition, when the roughening cleaning conditions are determined in the roughening cleaning condition determination step, the hydrogen peroxide concentration is within a concentration range in which a change in the roughening amount with respect to a change in the hydrogen peroxide concentration is equal to or less than a predetermined value, and a native oxide film formed during the cleaning remains on the surface of the silicon wafer to be roughened after the cleaning in the roughening cleaning step, The roughening cleaning conditions can be determined.

[0016] With this method, even if the hydrogen peroxide concentration in the cleaning solution changes, it is possible to more stably supply wafers that have been roughened to a desired degree, and it is also possible to obtain wafers that are more sufficiently roughened.

[0017] In the step of determining the roughening cleaning conditions, the temperature of the cleaning solution may be set to 80° C. or higher.

[0018] With this method, the variation in the amount of roughening caused by the variation in the concentration of aqueous peroxide can be reduced, and roughened wafers can be supplied more stably.

[0019] The present invention also provides a method for producing a silicon wafer, characterized in that a CMP process is performed on one surface of a silicon wafer that has been cleaned by the silicon wafer cleaning method of the present invention and has roughened front and back surfaces, to obtain a silicon wafer in which only the surface opposite to the one surface is selectively roughened.

[0020] In this way, by roughening the front and back surfaces and then polishing only one of the surfaces, a wafer can be produced in which one surface is in a good surface condition and only the surface opposite to the one surface is selectively roughened.

[0021] The present invention also provides a method for producing a silicon wafer, characterized in that only the back surface of the silicon wafer is cleaned and roughened in a sheet-by-sheet manner by the method for cleaning a silicon wafer of the present invention.

[0022] In this manner, a wafer having a roughened back surface only can be produced.

[0023] The present invention also provides a method for evaluating a hydrogen peroxide concentration in a cleaning solution, comprising the steps of: The amount of roughening of the front and back surfaces or the back surface of the silicon wafer for investigation, which has a native oxide film and is roughened by cleaning the silicon wafer for investigation with a cleaning solution that is an aqueous solution containing ammonium hydroxide and having a hydrogen peroxide concentration of 0 to 0.15 wt %, and The temperature of the cleaning liquid; and a concentration of ammonium hydroxide in the cleaning solution; and a cleaning solution concentration investigation step of acquiring a correlation with the hydrogen peroxide concentration in the cleaning solution in advance; Based on the correlation obtained in the cleaning solution concentration investigation step, A silicon wafer having a native oxide film is roughened by cleaning the silicon wafer with a cleaning solution to be evaluated, which is an aqueous solution containing at least ammonium hydroxide, to obtain a roughening amount on the front and back surfaces or the back surface of the silicon wafer; The temperature of the cleaning solution to be evaluated; and and the concentration of ammonium hydroxide in the cleaning solution to be evaluated. and evaluating the hydrogen peroxide concentration in the cleaning solution to be evaluated.

[0024] Such a method for evaluating the concentration of hydrogen peroxide in a cleaning liquid makes it possible to accurately evaluate the concentration of minute amounts of hydrogen peroxide that affect the roughening behavior.

[0025] The present invention also provides a method for managing a hydrogen peroxide concentration in a cleaning solution, comprising the steps of: The concentration of hydrogen peroxide in the cleaning solution to be evaluated is evaluated by the method for evaluating the concentration of hydrogen peroxide in a cleaning solution of the present invention; The present invention provides a method for controlling the concentration of hydrogen peroxide in a cleaning solution, which comprises adjusting the concentration of hydrogen peroxide in the cleaning solution after the evaluation based on the evaluation results.

[0026] According to such a method for controlling the hydrogen peroxide concentration in the cleaning liquid, the hydrogen peroxide concentration can be controlled with high accuracy, and roughening can be performed stably. Effect of the Invention

[0027] The method for cleaning a silicon wafer of the present invention can roughen the front and back surfaces or the back surface of a silicon wafer. Furthermore, the method for producing a silicon wafer of the present invention can produce a wafer in which one surface is in a good surface condition and only the surface opposite to the one surface is selectively roughened. Furthermore, the method for evaluating and controlling the concentration of hydrogen peroxide in a cleaning solution of the present invention makes it possible to accurately evaluate and control the concentration of a trace amount of hydrogen peroxide in a cleaning solution used in roughening cleaning. [Brief description of the drawings]

[0028] [Figure 1] 1 is a flowchart showing an example of a method for cleaning a silicon wafer according to the present invention. [Diagram 2] This figure shows a relationship diagram indicating the amount of haze increase, the number of LLS, and the surface condition after cleaning a bare silicon wafer with various liquid compositions, and also shows SEM images of levels 5 and 9. [Diagram 3] 1 is a graph showing an increase in haze with respect to H2O2 concentration at three levels of NH4OH concentration when the cleaning solution temperature is 80° C. [Figure 4] 1 is a graph showing the amount of haze increase versus H2O2 concentration when the cleaning solution temperature is 45° C. or 60° C. [Diagram 5]1 is a graph showing an increase in haze with respect to cleaning time after cleaning at a cleaning temperature of 80° C. using a cleaning solution having an NH4OH concentration of 0.03 wt % and an H2O2 concentration of 0.05 wt %. [Figure 6] 1 is a flowchart showing an example of a method for evaluating and managing the hydrogen peroxide concentration in a cleaning solution of the present invention. [Figure 7] This is a graph showing the amount of haze increase versus H2O2 concentration when the cleaning solution temperature is 80°C and the NH4OH concentration in the cleaning solution is 0.03 wt%, and is a graph showing the results (correlation) of the cleaning solution concentration investigation step S11 carried out in the examples. [Figure 8] 1 is a graph showing the amount of haze increase versus H2O2 concentration when the cleaning solution temperature is 80° C. and there are two levels of NH4OH concentration, and also showing the results (correlation) of the cleaning solution concentration investigation step S1 carried out in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] Hereinafter, the present invention will be described in detail with reference to the drawings as an example of an embodiment, but the present invention is not limited thereto. First, the method and mechanism of the roughening phenomenon in the present invention will be described. In Fig. 2, a post-DSP wafer with an exposed bare surface was cleaned with SC1 composition (liquid composition NH4OH:H2O2:H2O) at different cleaning temperatures and cleaning times (denoted as level 1 to level 12), and the haze value, which is an index of roughness, was obtained using a particle counter, and the difference from the haze value obtained before cleaning was shown. The increase in the haze value after cleaning (hereinafter also referred to as the haze increase amount) is an example of the amount of roughening. The higher this value, the more rough the surface is. Also shown are the results of surface observation by SEM (Scanning Electronic Microscopy) for Ref without roughening treatment and levels 5 and 9.

[0030] The chemicals used were 28% by mass ammonia water (NH4OH) and 30% by mass hydrogen peroxide water (H2O2), each of which was expressed as a percentage by mass (wt%). Note that mass% is the concentration expressed as a percentage of the mass ratio of the cleaning solution and the solutes (ammonium hydroxide, hydrogen peroxide) contained in it, and is also expressed as wt%.

[0031] It can be seen that the haze value increases significantly in levels 5, 6, 8, 9, and 12. Furthermore, looking at the SEM images, uneven shapes are observed in levels 5 and 9, but no such uneven shapes are observed in the Ref. From the above, it can be seen that the surfaces of these levels are significantly roughened and have become rough. On the other hand, in standards 3, 4, and 11, the increase was about 0.8 to 0.9 ppm, but the increase, i.e., the degree of roughening, was small and could not be said to be roughening. Furthermore, the number of LLS (Localized Light Scatter) defects was very high, and the defect quality had significantly deteriorated. Since the surface condition after cleaning was water-repellent, it is believed that the bare surface was exposed during cleaning, and etching of Si progressed significantly, resulting in the formation of etch pits. In the remaining standards, the surface condition was hydrophilic, but the increase in haze was also slight.

[0032] The roughening mechanism will be explained in detail. In SC1 cleaning, hydrogen peroxide acts as an oxidizing agent, oxidizing silicon and forming SiO2 (a natural oxide film, hereafter also referred to as simply an oxide film). Ammonium hydroxide is ionized to form OH - This OH - The SiO2 on the wafer surface is etched by this. In a typical chemical (cleaning) composition (e.g. NH4OH:H2O2:H2O = 1:1:10), an oxide film is always present on the wafer during cleaning, the bare surface (Si) is not exposed, and the thickness of the oxide film formed is always about 1 nm, regardless of the cleaning time. This is known to be due to the balance between the oxidation rate and the etching rate. In other words, in a chemical with a certain concentration or more of H2O2, the oxidation rate of Si by H2O2 is faster than that of OH. -This means that the etching rate of SiO2 by OH is faster than that of SiO2 by OH. Therefore, the silicon is not exposed and the oxide film is always present on the wafer. In other words, when the concentration of H2O2 becomes lower than a certain level, the oxide film is always present on the wafer. - The etching rate by H2O2 is faster than the oxidation rate of Si by H2O2, so the oxidation cannot keep up and OH - In this case, the silicon is exposed after cleaning, resulting in a water-repellent surface.

[0033] It can be seen that the chemical composition of the roughened level here has a lower H2O2 ratio than NH4OH, for example NH4OH:H2O2:H2O = 1:0.4:1000 in level 5. Therefore, when a bare silicon wafer is cleaned with such a chemical, since the surface state after cleaning is hydrophilic, an oxidation reaction first proceeds and an oxide film is formed, but since the oxidation rate is slow, etching of SiO2 becomes relatively dominant, and etching of Si proceeds in the places where SiO2 is etched and Si is locally exposed, leading to roughening.

[0034] Thus, the roughening phenomenon in the present invention progresses when the balance between the oxidation reaction and the etching reaction is within a certain range. In order to stably progress the roughening, cleaning must be performed with a solution composition and chemical concentration that stabilizes these reactions.

[0035] Taking these factors into consideration, the cleaning method of the present invention will be described. FIG. 1 is a flow chart showing an example of the method for cleaning a silicon wafer according to the present invention. (Step S1: Cleaning solution concentration investigation step) In S1 of FIG. 1, a cleaning solution concentration investigation step is performed as a preliminary test to select the roughening cleaning conditions under which the roughening phenomenon proceeds stably. That is, this is a step of acquiring in advance the correlation between the roughening amount, the temperature of the cleaning solution, the ammonium hydroxide concentration in the cleaning solution, and the hydrogen peroxide concentration in the cleaning solution. Here, the above-mentioned roughening amount refers to the roughening amount of the front and back surfaces (or the back surface) roughened by cleaning a silicon wafer for investigation (without a native oxide film and with an exposed bare surface) with a cleaning solution (an aqueous solution containing ammonium hydroxide and with a hydrogen peroxide concentration of 0 to 0.15 wt%), and can be, for example, the above-mentioned haze increase amount. The haze increase amount is preferable because it allows the roughening behavior and roughening amount to be monitored easily and with good throughput. As an example of the cleaning liquid, when the hydrogen peroxide concentration is 0 wt%, it can be an aqueous solution containing ammonium hydroxide, and when the hydrogen peroxide concentration is not 0 wt%, it can be an aqueous solution containing ammonium hydroxide and hydrogen peroxide.

[0036] The cleaning solution concentration checking step will be described below with a more specific example. Figure 3 shows the increase in haze before and after cleaning when the H2O2 concentration was changed to three levels of NH4OH concentration: 0.03, 0.13, and 0.25wt% and a bare silicon wafer without a native oxide film was cleaned at 80℃ for 3 minutes. When the NH4OH concentration was 0.03wt%, the surface condition after cleaning is also shown (◯ is a water-repellent surface, ● is a hydrophilic surface).

[0037] For example, when the NH4OH concentration is 0.03 wt%, it can be seen that the amount of haze increase varies depending on the H2O2 concentration. When the H2O2 concentration is 0 wt% or 0.007 wt%, the amount of haze increase is small. This is because the H2O2 concentration is too low, so the oxidation rate is too slow and only the etching effect on the Si occurs. This coincides with the fact that the surface state after cleaning is water-repellent (bare Si surface exposed) only at the low H2O2 concentration level. As mentioned above, in the case of a hydrophobic surface, etching of silicon becomes prominent and the LLS quality (LLS number) deteriorates, so it is desirable to proceed with roughening within the range that results in a hydrophilic surface. When the H2O2 concentration was between 0.019wt% and 0.078wt%, the surface condition was hydrophilic, with a large increase in haze and roughening progressing. From 0.09wt% onwards, the surface was hydrophilic, but the increase in haze became smaller. This is because the H2O2 concentration was too high, so the oxidation rate of silicon was significantly faster than the etching rate, and the etching effect was relatively weak.

[0038] It is preferable to carry out this cleaning solution concentration investigation process at multiple levels of NH4OH concentration and cleaning temperature. As shown in the figure, the haze increase amount increases with increasing NH4OH concentration, so when setting the desired haze increase amount (amount of deterioration) in step S2 described later, it is easier to select the roughening cleaning conditions if there are investigation results at multiple levels.

[0039] Furthermore, as a result of research by the present inventors, when the H2O2 concentration was greater than 0.15 wt%, even if the NH4OH concentration was increased within a practical range, the oxidation rate became faster and roughening did not progress, so in step S1, the H2O2 concentration is set to 0 to 0.15 wt% or less, as described above.

[0040] (Step S2: Roughening cleaning conditions determination step) Next, a roughening cleaning condition determination step S2 is performed based on the result of S1. That is, this is a step of determining the roughening cleaning conditions, such as the temperature of the cleaning solution, the concentration of ammonium hydroxide in the cleaning solution, and the concentration of hydrogen peroxide in the cleaning solution, from the desired amount of roughening (amount of haze increase) based on the correlation in S1. The desired haze increase amount can be determined on a case-by-case basis.

[0041] In this step, the object is to select roughening cleaning conditions under which the variation in the amount of haze increase relative to the variation in the H2O2 concentration is stable, based on the correlation obtained in S1. In FIG. 3, when the NH4OH concentration is 0.03 wt%, the variation of the haze increase is small and stable in the range of 0.032 to 0.078 wt%. In this case, for example, by setting the H2O2 concentration to 0.05 wt%, even if the H2O2 concentration in the cleaning solution fluctuates unintentionally, the variation of the haze increase is relatively small and stable with respect to the fluctuation, so that the desired haze increase is not significantly deviated from, and roughening can be progressed more stably with the desired haze increase. In this way, the H2O2 concentration selected as one of the roughening cleaning conditions is preferably determined from a range of H2O2 concentrations in which the variation of the haze increase with respect to the variation of the H2O2 concentration is within a relatively small value (predetermined value). This predetermined value can be appropriately set from a value equal to or greater than 0 according to the required accuracy, etc.

[0042] Next, when we look at the cases where the NH4OH concentration is 0.13wt% and 0.25wt%, we can determine that when the H2O2 concentration is low, the oxidation rate is slow, etching becomes dominant, and the increase in haze fluctuates greatly, making it unstable. Therefore, it is not recommended to roughen the surface in this range. The higher the NH4OH concentration, the faster the etching rate becomes, which is probably why the fluctuations are greater than with 0.03wt%. However, as the H2O2 concentration increases, it can be seen that there is a H2O2 concentration range in which the amount of haze increase is stable, just as in the case of 0.03 wt%. Since the H2O2 concentration range required for the amount of haze increase to be stable changes depending on the NH4OH concentration, it is possible to proceed with more stable roughening by determining the appropriate H2O2 concentration range in advance.

[0043] In addition, the higher the NH4OH concentration, the greater the haze increase, so the desired roughness (haze increase) can be formed by adjusting the NH4OH concentration. For example, if you want to obtain a wafer with a haze increase of 5 ppm, you can select the roughening cleaning conditions of NH4OH concentration 0.03 wt%, H2O2 concentration 0.05 wt%, 80°C, and 3 min. On the other hand, if you want to obtain a wafer with a haze increase of 30 ppm, you can select the roughening cleaning conditions of NH4OH concentration 0.25 wt%, H2O2 concentration 0.07 wt%, 80°C, and 3 min. In this way, by understanding the fluctuation of the haze increase with respect to the H2O2 concentration, you can select the roughening cleaning conditions that will progress the roughening more stably.

[0044] In addition, in this step S2, if the roughening cleaning conditions are determined so that the natural oxide film formed during cleaning in step S3 remains on the surface of the silicon wafer to be roughened after cleaning in step S3 described later, the degree of roughening can be made even more sufficient, which is preferable. A hydrophilic surface can also be obtained, and the deterioration of the LLS number can also be prevented.

[0045] Next, the effect of the temperature of the cleaning solution (cleaning temperature) will be described. Figure 4 shows the variation in haze increase when cleaning is performed at 45°C and 60°C with NH4OH concentrations of 0.03wt% and 0.25wt%, for a cleaning time of 3min. Although there are conditions where the haze increase increases for all three levels, the H2O2 concentration range where the haze increase is stable is narrower than that of Figure 3 for 80°C. Therefore, it can be interpreted that it is easier to select more stable roughening cleaning conditions by performing the cleaning solution concentration investigation process S1 or by selecting in the roughening cleaning condition determination process S2 at a cleaning temperature of 80°C or higher. The reason for this is thought to be that the oxidation action of hydrogen peroxide is more stable at higher temperatures. There is no particular upper limit for the cleaning temperature, but for example, 90°C is sufficient.

[0046] However, it does not necessarily have to be 80°C or higher; there are regions where the amount of haze increase is large even at temperatures below 60°C, so it is possible to advance roughening. For example, by shortening the chemical life, it is possible to suppress variations in the amount of haze increase caused by fluctuations in the H2O2 concentration in the cleaning solution.

[0047] Next, the effect of cleaning time will be described. FIG. 5 shows the increase in haze when cleaning was performed with a cleaning solution having an NH4OH concentration of 0.03 wt% and an H2O2 concentration of 0.05 wt%, at a cleaning temperature of 80°C, and for cleaning times of 30, 60, 180, and 360 seconds. It can be seen that the longer the cleaning time, the greater the increase in haze. Therefore, the degree of roughening can be adjusted by adjusting the NH4OH concentration, H2O2 concentration, cleaning temperature, and even the cleaning time. As described above, the NH4OH concentration can be adjusted, or the cleaning time can be adjusted to control the degree of roughening, and these can be used appropriately as needed. In this way, it is also possible to obtain the correlation in S1 and determine the roughening cleaning conditions in S2 by further considering the cleaning time.

[0048] (Step S3: Roughening and cleaning step) Next, in the roughening cleaning step S3, the bare surface of the silicon wafer to be roughened, which has no natural oxide film, is cleaned under the roughening cleaning conditions determined in S2. This cleaning step roughens the front and back surfaces (or the back surface) of the silicon wafer to be roughened. In this way, by carrying out the steps S1 and S2 described above and then S3, it is possible to reliably obtain a roughened wafer with the desired haze increase amount described above. Moreover, in particular, the wafer can be produced with a stable degree of roughening without deviating significantly from the desired haze increase amount (i.e., the variation in the haze increase amount is small).

[0049] Next, the cleaning method for carrying out the cleaning of the present invention will be described. Currently, most wafer cleaning methods use liquids such as chemicals and pure water, and are called wet cleaning. The main methods are the batch method, which cleans many wafers at once, and the single-wafer method, which processes wafers one by one. In the batch method, both the front and back sides of the wafer are immersed in the chemicals due to the configuration of the device, so the front and back sides are roughened when the cleaning of the present invention is carried out. In contrast, in the single-wafer method, the chemicals are sprayed on the wafer while it is rotating, so only one side of the wafer can be cleaned. According to the inventors' investigation, the present invention can roughen the wafer using either the batch method or the single-wafer method. The method can be selected appropriately taking into consideration the wafer manufacturing process.

[0050] As described above, to produce a wafer with only a rough back surface, in the case of a single wafer method, only the back surface needs to be cleaned, whereas in the case of a batch method, both the front and back surfaces are roughened. Therefore, as in the silicon wafer manufacturing method of the present invention, it is desirable to improve the quality of the front surface side in particular by a polishing process after cleaning by the cleaning method of the present invention. For example, by performing the silicon wafer cleaning method of the present invention in a batch-type cleaning machine to roughen both the front and back surfaces of a silicon wafer, and then performing single-sided polishing such as CMP processing on one side (i.e., the front side), it is possible to produce a wafer in which only the side opposite to the one side (i.e., the back side) is selectively roughened. Such a wafer will not cause chucking failure even in a wet environment, enabling stable manufacturing.

[0051] Next, a method for evaluating and controlling the concentration of hydrogen peroxide in the cleaning solution used for roughening in the above-mentioned cleaning method of the present invention will be described. As described above, the roughening behavior of the present invention strongly depends on the hydrogen peroxide concentration, so roughening can be progressed more stably by controlling the hydrogen peroxide concentration. A method for evaluating the chemical concentration of a general SC1 cleaning solution is a concentration measurement method using absorbance or refractive index, which is known to be highly accurate. However, when the present inventors measured the concentration of a cleaning solution containing, for example, 0.25 wt% NH4OH and 0.07 wt% H2O2 for roughening cleaning using a concentration meter using an absorbance method, the NH4OH concentration was measured to be 0.24 wt%, but the H2O2 concentration was below the detection limit and could not be measured.

[0052] Therefore, the inventors of the present invention have conducted extensive research into whether the H2O2 concentration can be evaluated and controlled by utilizing the above-mentioned roughening behavior. Figure 6 shows the flow of the method for evaluating and controlling the hydrogen peroxide concentration in a cleaning solution of the present invention. (Step S11: Cleaning solution concentration investigation step) First, as in the cleaning solution concentration investigation step S11, this is a step in which correlations are obtained for a silicon wafer under investigation (having a native oxide film) between the amount of roughening (e.g., the amount of haze increase), the temperature of the cleaning solution (an aqueous solution containing ammonium hydroxide and having a hydrogen peroxide concentration of 0 to 0.15 wt%), the ammonium hydroxide concentration in the cleaning solution, and the hydrogen peroxide concentration in the cleaning solution. As an example of the above cleaning liquid, when the hydrogen peroxide concentration is 0 wt%, it can be an aqueous solution containing ammonium hydroxide, and when the hydrogen peroxide concentration is not 0 wt%, it can be an aqueous solution containing ammonium hydroxide and hydrogen peroxide (SC1 cleaning liquid).

[0053] Here, unlike the cleaning solution concentration investigation step S1 in the above-described silicon wafer cleaning method of the present invention (wherein a silicon wafer having no native oxide film is used as the investigation silicon wafer), the reason why a wafer having a native oxide film is used in this cleaning solution concentration investigation step S11 in the method for evaluating the hydrogen peroxide concentration in a cleaning solution of the present invention is as follows. In the cleaning method, the variation in the amount of roughening relative to the change in the amount of hydrogen peroxide is particularly small, and in order to obtain a stable region, a sample without a native oxide film was used so that the trend shown in Figure 3 could be obtained, but in this case, conversely speaking, it is not possible to uniquely determine the hydrogen peroxide concentration corresponding to the amount of roughening. On the other hand, when a native oxide film is present, as described later, the amount of roughening tends to decrease as the hydrogen peroxide concentration increases, and the hydrogen peroxide concentration can be uniquely determined from the amount of roughening.

[0054] The cleaning solution concentration checking step will be described below with a more specific example. First, a silicon wafer to be examined having a native oxide film is prepared, and the haze value is obtained using a particle counter before cleaning in order to calculate the amount of haze increase. The method for forming the natural oxide film includes general SC1 cleaning and ozone water cleaning. There are no particular limitations on these cleaning methods as long as the natural oxide film is formed after cleaning. The mixture ratio (volume ratio) of the SC1 cleaning liquid is, for example, NH4OH:H2O2:H2O=1:1:10, the temperature is preferably 30 to 80°C, and the cleaning time is preferably 90 to 360 seconds. The concentration of the ozone water is preferably in the range of 3 to 25 ppm, the temperature is preferably 10 to 30°C, and the cleaning time is preferably 60 to 360 seconds.

[0055] Next, the aforementioned cleaning solution is prepared at various temperatures, and the NH4OH concentration or H2O2 concentration is varied (and the cleaning time is also varied as necessary) to clean the silicon wafers to be investigated that have a native oxide film thereon, roughening the front and back surfaces (or the back surface), and then the haze value is obtained using a particle counter. Figure 7 shows the haze increase versus H2O2 concentration when the cleaning temperature is 80°C, the cleaning time is 3 minutes, and the NH4OH concentration in the cleaning solution is 0.03 wt%. The trend is different from that of the bare surface (e.g., Figure 3), and it can be seen that the higher the H2O2 concentration, the smaller the haze increase. In this way, the correlation between cleaning temperature, NH4OH concentration, H2O2 concentration, and haze increase is obtained in advance. As a result of research by the inventors, when the H2O2 concentration is more than 0.15wt%, the haze increase amount is close to 0, making it difficult to use it as an index. On the other hand, the present invention is an evaluation method for cleaning solutions with H2O2 concentrations of 0.15wt% or less, and can accurately evaluate the H2O2 concentration even in such a small amount.

[0056] (Step S12: Hydrogen peroxide concentration evaluation step) Next, as in the hydrogen peroxide concentration evaluation step of S12, a silicon wafer having a native oxide film similar to that in S11 is washed with the evaluation target cleaning solution (aqueous solution containing at least ammonium hydroxide) for which the H2O2 concentration is to be measured, at a predetermined cleaning temperature (and further, a predetermined cleaning time) in the correlation obtained in S11, and the haze increase amount is obtained. Note that the NH4OH concentration may be measured by a conventional method, for example, and obtained in advance. In particular, it is convenient to preset the cleaning temperature (and cleaning time) and perform steps S11 and S12 at the same cleaning temperature (and cleaning time). Next, based on the correlation obtained in S11, the H2O2 concentration can be evaluated from the haze increase amount, cleaning temperature (and cleaning time), and NH4OH concentration obtained above.

[0057] (Step S13: Hydrogen peroxide concentration management step) Furthermore, as in the hydrogen peroxide concentration control step S13, the hydrogen peroxide concentration in the cleaning liquid can be adjusted according to the evaluation results obtained in S12. For example, after first cleaning for a predetermined time using a cleaning solution formulated to have an NH4OH concentration of 0.03 wt% and an H2O2 concentration of 0.05 wt%, if the H2O2 concentration is evaluated using the evaluation method of the present invention and judged to be 0.04 wt%, hydrogen peroxide solution can be injected so that the H2O2 concentration becomes 0.05 wt%. Conversely, if the concentration is judged to be 0.06 wt%, pure water can be injected so that the H2O2 concentration becomes 0.05 wt%. By carrying out such a management method, the life of the chemical solution can be extended and a roughened wafer with a stable increase in haze can be manufactured. In this manner, the concentration of H2O2 in the cleaning solution, which is as small as 0 to 0.15 wt%, can be accurately evaluated and controlled, and it is therefore possible to stably manufacture desired roughened wafers. EXAMPLES

[0058] The present invention will be further described below with reference to examples. However, these examples are presented for illustrative purposes and should not be construed as limiting. Example 1 As shown in the cleaning method of the present invention in FIG. 1, first, a preliminary test S1 was carried out to investigate the concentration of the cleaning solution. The haze value of the bare silicon wafer (survey silicon wafer) without the native oxide film after DSP processing was obtained using a particle counter SP3 manufactured by KLA. Next, 28 mass% ammonia water (NH4OH) and, if necessary, 30 mass% hydrogen peroxide water (H2O2) were used to prepare two levels of cleaning solution with a cleaning solution temperature of 80°C and NH4OH concentrations of 0.03wt% and 0.25wt%, and the H2O2 concentration was changed within the range of 0 to 0.15w%. After cleaning the bare silicon wafer for 3 minutes, the haze value was obtained using SP3, and the increase in haze, which is an index of the amount of roughening, was calculated from the difference before and after cleaning. FIG. 8 shows the correlation between the haze increase, NH4OH concentration, and H2O2 concentration when the cleaning temperature was 80°C.

[0059] Next, the roughening cleaning condition determination step S2 was carried out. The objective was to fabricate wafers with two levels of haze increase: 10 ppm and 30 ppm. The roughening cleaning conditions that would obtain these haze increases were determined from the correlation in Figure 8 obtained in S1. For 10 ppm, when the NH4OH concentration is 0.03 wt%, it can be seen that there is a stable range where the haze increase is about 5 to 6 ppm when the H2O2 concentration is in the range of about 0.03 to 0.08 wt%. Therefore, in the next step S3, the cleaning solution used for the silicon wafer to be roughened has an NH4OH concentration of 0.03 wt%, an H2O2 concentration of 0.05 wt% within the range of 0.03 to 0.08 wt%, and a cleaning temperature of 80°C. Regarding the cleaning time, there is a positive correlation between the haze increase and the cleaning time, and considering that the haze increase is 5 to 6 ppm in 3 minutes, the cleaning time was set to 6 minutes, which is twice the 3 minutes. With this setting, a haze increase of about 10 ppm is expected.

[0060] Regarding 30 ppm, when the NH4OH concentration is 0.25 wt%, the haze increase is stable at about 30 ppm when the H2O2 concentration is in the range of 0.05 to 0.09 wt%. For this reason, the cleaning solution was set to NH4OH concentration of 0.25 wt%, H2O2 concentration of 0.07 wt% within the range of 0.05 to 0.09 wt%, and the cleaning temperature was set to 80°C. The cleaning time was set to 3 minutes, as with S1, since the haze increase was 30 ppm in 3 minutes.

[0061] Next, the roughening cleaning step S3 was carried out. Under the two roughening cleaning conditions determined in S2, aiming for a haze increase of 10 ppm and 30 ppm, five bare silicon wafers (silicon wafers to be roughened) without a natural oxide film after DSP processing were cleaned in a batch cleaning machine for each level to roughen both sides, and the haze value was obtained in SP3 to calculate the haze increase. The average haze increase of the wafers aiming for 10 ppm was 10.7 ppm, and the average haze increase of the wafers aiming for 30 ppm was 31.2 ppm, and it was possible to produce wafers with roughness equivalent to the target haze increase. In addition, the LLS quality was good, being 1 pcs for the wafers aiming for 10 ppm and 0 pcs for the wafers aiming for 30 ppm.

[0062] For each wafer with a roughened surface and a target haze increase of 10 ppm and 30 ppm, CMP processing was performed on the front surface with a removal allowance of 500 nm. The number of LLSs was evaluated using KLA's SP5 / 19nmUp after CMP processing, and the results were 12 pcs for the 10 ppm target and 9 pcs for the 30 ppm target, which was equivalent to Level 1 of the comparative example described below and was of good quality. After that, a transport test was conducted 200 times in which the back side of each wafer stored underwater was chucked and the wafer was unchucked on the stage of the polishing machine. In both cases, the wafers were transported without any defects all 200 times.

[0063] Example 2 Next, based on the evaluation method of the present invention shown in FIG. 6, an evaluation was made of the hydrogen peroxide concentration in the cleaning solution for stably carrying out roughening cleaning. Based on the results of S2 and S3 in Example 1, the hydrogen peroxide concentration of a cleaning solution with an NH4OH concentration of 0.03 wt%, an H2O2 concentration of 0.05 wt%, and a temperature of 80° C. was evaluated so that the haze increase amount was 10 ppm. First, as in the cleaning solution concentration investigation process in S11, the correlation between the cleaning temperature (80°C), NH4OH concentration (0.03 wt%), H2O2 concentration, and the roughening amount was obtained. Specifically, first, a silicon wafer was cleaned for 3 min at 80°C with a cleaning solution of NH4OH:H2O2:H2O = 1:1:10 to prepare a wafer with a native oxide film (silicon wafer for investigation), and the haze value was obtained using SP3. Next, the silicon wafer with a native oxide film was cleaned for 3 min with a cleaning solution of 0.03 wt% NH4OH and 80°C cleaning temperature, with different H2O2 concentrations. The haze value of the wafer after cleaning was obtained using SP3, and the haze increase was calculated. The results were the same as those in Figure 7. That is, for example, when the H2O2 concentration was 0.05 wt%, it was 41 ppm, and when it was 0.02 wt%, it was 181 ppm, and a correlation was obtained in which the amount of roughening (i.e., the amount of haze increase) decreased with increasing H2O2 concentration.

[0064] Next, the hydrogen peroxide concentration evaluation step S12 was carried out. First, 200 silicon wafers were cleaned with this cleaning solution to produce silicon wafers with roughened surfaces on both sides. In order to evaluate the hydrogen peroxide concentration in the cleaning solution (evaluation target cleaning solution) after cleaning 200 wafers, the haze value was acquired by cleaning a wafer with a native oxide film, and the haze value was acquired by SP3, and the haze increase was calculated. As a result, the haze increase was 60 ppm. Referring to the correlation in Figure 7, the H2O2 concentration in the cleaning solution being evaluated was found to be approximately 0.04wt%. Since the target H2O2 concentration before cleaning 200 wafers was 0.05wt%, it was determined that the concentration had decreased by approximately 0.01wt%. This was probably due to the chemicals adhering to the wafers after cleaning 200 wafers, or carryover from the pure water (rinse) tank.

[0065] Next, in the hydrogen peroxide concentration control step S13, H2O2 was added to the cleaning solution to achieve the target H2O2 concentration of 0.05 wt%. After that, for confirmation, we cleaned a wafer with a native oxide film that had a haze value, then acquired the haze value with SP3 and calculated the amount of haze increase. As a result, it was found to be 40 ppm, and from the correlation, H2O2 was found to be about 0.05 wt%, and it was confirmed that the H2O2 concentration was as targeted.

[0066] From the above results, it is understood that the cleaning method of the present invention can sufficiently roughen the front and back surfaces (especially the back surface) of a silicon wafer to provide a roughness suitable for adsorption by a chuck. Furthermore, it is understood that the method of evaluating and controlling the hydrogen peroxide concentration in a cleaning solution of the present invention can evaluate and control the concentration of minute amounts of hydrogen peroxide, which was previously difficult to achieve.

[0067] (Comparative Example) Bare silicon wafers without any natural oxide film after DSP processing were prepared and subjected to haze evaluation using SP3. Next, cleaning was performed using a batch cleaning machine under the six levels of conditions (liquid composition, cleaning temperature, cleaning time) shown in Table 1. 28% by mass ammonia water (NH4OH) and 30% by mass hydrogen peroxide water (H2O2) were used to prepare the cleaning liquid. After cleaning, the wafers were evaluated using SP3 to obtain the haze value and calculate the amount of haze increase.

[0068] For all levels in Table 1, the amount of haze increase was 1 ppm or less, which was smaller than the 10 ppm and 30 ppm in Example 1, and therefore it was determined that no roughening was occurred. After performing CMP processing with a removal amount of 500 nm on wafers of level 1 and level 5, the number of LLS was evaluated using SP5 / 19 nmUP, resulting in 10 pcs for level 1 and 342 pcs for level 5. The LLS level for level 1 was equivalent to that of Example 1, but it is believed that the LLS quality of level 5 deteriorated because etching prevailed during the roughening cleaning process and etch pits formed remained in the CMP process. Next, chuck tests similar to those in Example 1 were performed 200 times on wafers of levels 1 and 5. Defects in which the wafer did not detach from the chuck occurred four times for level 1 and three times for level 5. In addition, the H2O2 concentration of the cleaning solution of level 5 was measured using an absorbance type concentration meter, but it was below the detection limit and could not be evaluated.

[0069] [Table 1]

[0070] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and any configuration that is substantially the same as the technical idea described in the claims of the present invention and that provides similar effects is included in the technical scope of the present invention.

Claims

1. A cleaning method for roughening a silicon wafer, comprising the steps of: A silicon wafer for investigation having an exposed bare surface free of a native oxide film is roughened by cleaning the silicon wafer with a cleaning solution that is an aqueous solution containing ammonium hydroxide and having a hydrogen peroxide concentration of 0 to 0.15 wt %, thereby obtaining a roughening amount of the front and back surfaces or the back surface of the silicon wafer for investigation; The temperature of the cleaning liquid; and a concentration of ammonium hydroxide in the cleaning solution; and a cleaning solution concentration investigation step of acquiring a correlation with the hydrogen peroxide concentration in the cleaning solution in advance; a roughening cleaning condition determining step of determining roughening cleaning conditions, including a temperature of the cleaning solution, an ammonium hydroxide concentration and a hydrogen peroxide concentration in the cleaning solution, from a desired roughening amount based on the correlation obtained in the cleaning solution concentration investigating step; and a roughening cleaning step of roughening a silicon wafer to be roughened, the bare surface of which is exposed and free from a native oxide film, by cleaning the silicon wafer to be roughened under the roughening cleaning conditions determined in the roughening cleaning condition determination step, thereby roughening the front and back surfaces or the back surface of the silicon wafer to be roughened.

2. In the cleaning solution concentration investigation step, 2. The method for cleaning a silicon wafer according to claim 1, wherein a haze value of the test silicon wafer is obtained by a particle counter before and after the cleaning, and an increase in the haze value after the cleaning is defined as the amount of roughening.

3. When the roughening cleaning conditions are determined in the roughening cleaning condition determination step, the hydrogen peroxide concentration is within a concentration range in which a change in the roughening amount with respect to a change in the hydrogen peroxide concentration is equal to or less than a predetermined value, and a native oxide film formed during the cleaning remains on the surface of the silicon wafer to be roughened after the cleaning in the roughening cleaning step, 3. The method for cleaning a silicon wafer according to claim 1, further comprising determining the roughening cleaning conditions.

4. 4. The method for cleaning a silicon wafer according to claim 1, wherein the temperature of the cleaning solution is set to 80° C. or higher in the roughening cleaning condition determination step.

5. 5. A method for producing a silicon wafer, comprising the steps of: performing CMP processing on one surface of a silicon wafer that has been cleaned by the method for cleaning a silicon wafer according to any one of claims 1 to 4 and has roughened front and back surfaces; and obtaining a silicon wafer in which only the surface opposite to the one surface is selectively roughened.

6. A method for producing a silicon wafer, comprising the steps of: obtaining a silicon wafer having only its back surface cleaned and roughened in a sheet-by-sheet manner by the method for cleaning a silicon wafer according to any one of claims 1 to 4.

7. 1. A method for assessing a hydrogen peroxide concentration in a cleaning solution, comprising: A roughening amount of the front and back surfaces or the back surface of the silicon wafer for investigation, which has a native oxide film and is roughened by cleaning the silicon wafer for investigation with a cleaning solution that is an aqueous solution containing ammonium hydroxide and having a hydrogen peroxide concentration of 0 to 0.15 wt %, and The temperature of the cleaning liquid; and a concentration of ammonium hydroxide in the cleaning solution; and a cleaning solution concentration investigation step of acquiring a correlation with the hydrogen peroxide concentration in the cleaning solution in advance; Based on the correlation obtained in the cleaning solution concentration investigation step, A silicon wafer having a native oxide film is roughened by cleaning the silicon wafer with a cleaning solution to be evaluated, which is an aqueous solution containing at least ammonium hydroxide, and the roughening amount of the front and back surfaces or the back surface of the silicon wafer; The temperature of the cleaning solution to be evaluated; and and the concentration of ammonium hydroxide in the cleaning solution to be evaluated. and evaluating the hydrogen peroxide concentration in the cleaning solution to be evaluated.

8. A method for managing a hydrogen peroxide concentration in a cleaning solution, comprising: The method for evaluating a hydrogen peroxide concentration in a cleaning solution according to claim 7 is used to evaluate the hydrogen peroxide concentration in the cleaning solution to be evaluated; A method for controlling the concentration of hydrogen peroxide in a cleaning solution, comprising adjusting the concentration of hydrogen peroxide in the cleaning solution after the evaluation based on the evaluation results.

Citation Information

Patent Citations

  • Deposition of oxide on surface of silicon wafer

    JP1995066195A

  • Surface cleaning method of semiconductor wafer

    JP1995240394A

  • Method for washing semiconductor device

    JP1996017775A

  • Cleansing liquid, its formulation and production, cleansing, and production of semiconductor substrate

    JP1998183185A

  • Improved method of cleaning microelectronics circuit board

    JP1998242107A