Method for cleaning silicon wafers and method for manufacturing silicon wafers with native oxide film
By adjusting surface roughness through varied SC1 cleaning conditions and subsequent hydrofluoric acid and ozone water treatments, the method achieves precise control over natural oxide film thickness on silicon wafers, addressing the reproducibility issues in existing technologies.
Patent Information
- Application Number
- JP2021186095
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-11-16
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-11-16
AI Technical Summary
Existing methods struggle to accurately control the thickness of natural oxide films on silicon wafers with high reproducibility, as surface roughness formed during polishing and cleaning processes significantly influences film thickness, and existing correlations are not applicable to modern silicon wafer surface roughness ranges.
A method involving multiple test wafers with varied SC1 cleaning conditions to form different surface roughness levels, followed by hydrofluoric acid removal of the SC1 oxide film and formation of a natural oxide film using oxidizing solutions like ozone water, to establish a correlation between surface roughness and film thickness, allowing precise control of natural oxide film thickness.
Enables accurate and reproducible control of natural oxide film thickness by adjusting surface roughness, particularly in the 60 to 90/μm spatial frequency band, using easily adjustable cleaning conditions like SC1 chemical concentration, temperature, and time.
Smart Images

Figure 0007571710000002 
Figure 0007571710000003 
Figure 0007571710000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for cleaning a silicon wafer and a method for producing a silicon wafer with a native oxide film. [Background technology]
[0002] In the manufacturing process of single crystal silicon wafers for semiconductor devices, their main surfaces are polished. In addition, a cleaning process is carried out to remove abrasives and metal impurities that have adhered to the silicon wafer surface during the polishing process. A cleaning method called RCA cleaning is used in this cleaning process.
[0003] This RCA cleaning is a cleaning method that combines SC1 (Standard Cleaning 1), SC2 (Standard Cleaning 2), and DHF (Diluted Hydrofluoric Acid) cleaning depending on the purpose. SC1 cleaning is a cleaning method that uses an alkaline cleaning solution made by mixing ammonia water and hydrogen peroxide water at a desired ratio, and lifts off particles attached to the silicon wafer surface by etching it, and removes particles while suppressing reattachment to the silicon wafer by utilizing the electrostatic repulsion between the silicon wafer and the particles. SC2 cleaning is a cleaning method that uses a cleaning solution made by mixing hydrochloric acid and hydrogen peroxide water at a desired ratio to dissolve and remove metal impurities from the silicon wafer surface. DHF cleaning is a cleaning method that removes the natural oxide film on the silicon wafer surface using dilute hydrofluoric acid. In addition, ozone water cleaning, which has a strong oxidizing power, may also be used to remove organic matter attached to the silicon wafer surface and form a natural oxide film on the silicon wafer surface after DHF cleaning. The surface quality of silicon wafers after cleaning, such as particle removal and surface roughness, is important, and a combination of these cleaning processes is used depending on the purpose.
[0004] Semiconductor elements such as MOS (Metal Oxide Semiconductor) capacitors and transistors are formed on the surface of semiconductor silicon wafers. Insulating films such as gate oxide films formed on these semiconductor elements are used under high electric field strength, and silicon oxide films, which are easy to form, are often used as these insulating films.
[0005] One method for evaluating the thickness of oxide films on silicon wafers is to use an ellipsometer. An ellipsometer is a device that measures the phase difference (Δdelta) and amplitude ratio (Ψpsi) by irradiating polarized light onto a substrate sample and measuring the change in the polarization state between the incident light and the reflected light. For example, in the case of a silicon oxide film on a silicon wafer, the polarization state of the incident light changes as it is reflected by the silicon oxide film on the top surface and the interface between the silicon oxide film and the silicon wafer. There are two types of ellipsometers: a single-wavelength type that uses a laser as a light source and a spectral type that uses a white light source containing many wavelength components. The single-wavelength type measures delta and psi for a specific wavelength (e.g. 633 nm), while the spectral type can measure delta and psi for each wavelength, and it is known that the spectral type, which has a large amount of information, can evaluate the film thickness more accurately.
[0006] As mentioned above, the information obtained by the measurement of the ellipsometer is the phase difference and the amplitude ratio, and the film thickness cannot be calculated directly. To calculate the film thickness, a model corresponding to the substrate sample is created, and the delta and psi theoretically obtained from this model are compared with the delta and psi obtained by the measurement of the ellipsometer. The model is created by setting conditions according to the physical properties of the sample, and the items of the conditions to be set include the material of the substrate and the film, the film thickness of each film layer, and the optical constants of the substrate and the film. In addition, a known reference corresponding to the sample, a required dispersion equation showing the wavelength dependency of the dielectric constant and having multiple parameters, etc. are usually used to set each item.
[0007] Furthermore, a process is carried out to change the parameters of the dispersion equation and the thickness of each film layer of the model so that the degree of difference between the two is minimized in the above comparison (also called fitting). The difference between the two is usually calculated using the least squares method, and when it is determined that the result obtained by the least squares method has become small to a certain extent by fitting, the refractive index and extinction coefficient of the film are calculated from the parameter values of the dispersion equation at that time, and the film thickness at that time is specified as the film thickness of the film possessed by the sample, thereby making it possible to calculate the film thickness. Note that model creation and fitting are generally performed manually or automatically using a computer based on a required program.
[0008] When unevenness (also called roughness) exists on the sample surface, the concept of effective medium approximation may be used (for example, Patent Document 1, etc.). This method improves the calculation results of the least squares method by defining roughness and voids as one flat layer. In addition, the effective medium approximation may be applied not only to cases where roughness exists on the film surface of the sample, but also to interface layers when roughness exists at the interface between the substrate and the film or at the interface between film layers. Furthermore, the effective medium approximation may be used to reduce the value of the refractive index as a technique in analysis, regardless of the existence of roughness. Naturally, the use of the effective medium approximation changes the calculation results of the least squares method, and as a result, the value of the film thickness also changes, so the operator needs to determine whether to use the effective medium approximation from, for example, the calculation results of the least squares method.
[0009] Patent Document 2 describes that the thickness of a native oxide film on a silicon wafer measured by an ellipsometer varies depending on the surface roughness. Specifically, the rougher the surface, the thicker the film thickness, and discloses a method for quantitatively evaluating surface roughness based on the correlation between surface roughness and the thickness of the native oxide film.
[0010] Atomic Force Microscope (AFM) is also known as a method for evaluating the surface roughness on silicon wafers. Arithmetic mean heights such as Ra and Sa are often used as indexes of surface roughness. Ra is the arithmetic mean height in a reference length, which is a two-dimensional roughness index, and Sa is a parameter that extends Ra to a surface, which is a three-dimensional roughness index. As a method for evaluating roughness in more detail, conversion to the spatial frequency domain by spectrum analysis can also be performed. This method can extract a specific wavelength component from the measured surface profile, and is expressed, for example, by a specific spatial wavelength and a parameter related to the amplitude intensity at that wavelength, such as PSD (Power Spectrum Density). In this way, by performing PSD analysis, the spatial frequency of the dominantly formed roughness can be identified. In addition, the haze value obtained by a particle counter using a laser scattering method can be used as an index of roughness. Haze is expressed as a so-called cloudiness, and is widely used as an index of roughness on silicon surfaces. A high haze level indicates that the wafer surface is rough.
[0011] A dense silicon oxide film with high insulating properties is produced by thermally oxidizing silicon wafers, but because silicon wafers shipped with the silicon wafers have a native oxide film formed during cleaning, thermal oxidation is often performed on silicon wafers with a native oxide film formed thereon, in order to prevent particle adhesion, etc. In this case, it is known that the thickness of the thermal oxide film is affected by the film quality (thickness and structure) of the native oxide film before thermal oxidation.
[0012] In recent years, with the miniaturization and multi-layering of semiconductor integrated circuits, there is a demand for further thinning of various films, including insulating films constituting elements. This thinning requires the formation of extremely thin insulating films, i.e., silicon oxide films, uniformly and reproducibly within a surface or between substrates. To achieve this, it is necessary to control the quality of the natural oxide film at the time of shipment of silicon wafers, particularly the film thickness, which affects the quality of the silicon oxide film. In general, if the natural oxide film is thick, the thickness of the thermal oxide film will also be thick. If you want to make the thermal oxide film thinner, it is better to have a thin natural oxide film, and if you want to make the thermal oxide film thicker, it is better to have a thick natural oxide film. Therefore, in recent years, there has been a particular demand for controlling the thickness of the natural oxide film with good reproducibility within a certain range.
[0013] Patent Document 3 describes the relationship between silicon wafers cleaned under various conditions and the thickness of the oxide film after thermal oxidation. Specifically, it discloses that increasing the NH4OH concentration in the SC1 cleaning solution increases the amount of OH groups contained in the native oxide film, resulting in a thicker film after thermal oxidation, and that a method of controlling the film thickness after thermal oxidation is disclosed by using the correlation between the composition (film quality) of the native oxide film and the film thickness after thermal oxidation. [Prior art documents] [Patent documents]
[0014] [Patent Document 1] JP 2005-283502 A [Patent Document 2] Japanese Patent Application Publication No. 6-163662 [Patent Document 3] Patent No. 6791453 Summary of the Invention [Problem to be solved by the invention]
[0015] As mentioned above, it is necessary to control the thickness of the native oxide film and thermal oxide film on silicon wafers. In general, in the manufacturing process of silicon wafers, the surface roughness of the wafer is formed by polishing and the subsequent cleaning. For cleaning the wafer after polishing, SC1 cleaning, hydrofluoric acid cleaning, and ozone water cleaning are used, but it is known that the surface becomes rough mainly by SC1 cleaning, which has an etching effect.
[0016] Patent Document 3 describes the surface roughness Ra after SC1 cleaning or ozone water cleaning, and the value is about 0.06 to 0.12 nm. Such Ra values are the roughness values of silicon wafers that have been used in recent years.
[0017] Patent Document 2 discloses that the surface roughness of a wafer affects the thickness of a native oxide film measured by an ellipsometer. In this case, the surface roughness value is 0.22 to 2.05 nm in terms of the AFM Ra value, which is very high compared to the above-mentioned surface roughness value of 0.06 to 0.12 nm.
[0018] In addition, the thickness of the natural oxide film is generally known to be about 1 nm, but in Patent Document 2, when the Ra value is 0.22 nm, the thickness of the natural oxide film is 0.097 nm, when the Ra value is 1.23 nm, the thickness of the natural oxide film is 1.586 nm, and when the Ra value is 2.05 nm, the thickness of the natural oxide film is 3.313 nm, all of which are far from about 1 nm. Thus, the surface roughness and the thickness of the natural oxide film in Patent Document 2 are significantly different from the surface roughness and the thickness of the natural oxide film of silicon wafers used in recent years. The reason for this is considered to be that the invention described in Patent Document 2 uses a mixed solution of hydrofluoric acid and nitric acid, which is not used in normal silicon wafer cleaning solutions, to intentionally roughen the surface. That is, it is difficult to discuss the roughness and the thickness of the natural oxide film in the range of Ra of 0.06 to 0.12 nm, for example, using the correlation disclosed in Patent Document 2, and it is presumed that it can be applied exclusively to very rough surfaces, such as those with an Ra value exceeding 1 nm.
[0019] Here, when focusing on the AFM Ra value and the thickness of the thermal oxide film obtained by spectroscopic ellipsometry when the NH4OH concentration in SC1 cleaning is varied as described in Patent Document 3, it is found that the higher the NH4OH concentration, the higher the AFM Ra value and the thicker the thermal oxide film tends to be (Figure 9 of Patent Document 3). Patent Document 3 discloses that the composition (film quality) of the natural oxide film (chemical oxide film) formed in the cleaning process, for example, the amount of OH groups measured by the ATR (Attenuated Total Reflectance)-FT (Fourier Transform)-IR (Infrared Spectroscopy) method, is correlated with the thickness of the thermal oxide film, and describes that the higher the NH4OH concentration, the greater the amount of OH groups, resulting in a thicker thermal oxide film.
[0020] However, as mentioned above, the results can be interpreted as a correlation between the Ra value obtained by AFM measurement and the film thickness after thermal oxidation obtained by an ellipsometer. Thus, there is no publicly known document that describes the effect of the surface roughness of the wafer formed in the manufacturing process of silicon wafers used in recent years on the thickness of the native oxide film and the thermal oxide film obtained by an ellipsometer. If the wafer surface roughness formed in the manufacturing process of silicon wafers, such as an Ra value of 0.06 to 0.12 nm, is one of the factors that affect the thickness of the oxide film, it can be considered to be an important quality in controlling the thickness of the native oxide film and the thermal oxide film, just like the composition (film quality) of the native oxide film described above. In addition, if the thickness of the native oxide film formed after cleaning can be controlled by appropriately adjusting the surface roughness of the wafer, it is considered to be useful.
[0021] Therefore, the present invention has been made to solve the above problems, and an object of the present invention is to provide a method for cleaning silicon wafers that can control the thickness of a native oxide film with good accuracy and reproducibility by adjusting the surface roughness of the wafer. [Means for solving the problem]
[0022] The present invention has been made to achieve the above object, and is a method for cleaning a silicon wafer, the method comprising the steps of: preparing a plurality of test silicon wafers in advance; performing SC1 cleaning on the test silicon wafers under different SC1 cleaning conditions to fabricate the test silicon wafers having a plurality of levels of surface roughness different from each other; an SC1 oxide film removal step for the test silicon wafers in which the SC1 oxide film formed in the SC1 cleaning step for the test silicon wafers is completely removed by cleaning with hydrofluoric acid; a native oxide film formation step for the test silicon wafers in which the test silicon wafers from which the SC1 oxide film has been removed are cleaned with a cleaning solution having oxidizing power to form a native oxide film; a correlation acquisition step for acquiring a correlation between the surface roughness of the test silicon wafers formed by the SC1 cleaning and the thickness of the native oxide film formed in the natural oxide film formation step for the test silicon wafers; The present invention provides a silicon wafer cleaning method that controls the thickness of a natural oxide film formed on a silicon wafer by cleaning, comprising: an SC1 cleaning condition determination step of determining a surface roughness to be formed on the silicon wafer on which a natural oxide film is to be formed based on the correlation acquired in the correlation acquisition step so as to achieve a predetermined thickness, and determining SC1 cleaning conditions that will result in the determined surface roughness; an SC1 cleaning step of performing SC1 cleaning on the silicon wafer on which a natural oxide film is to be formed under the SC1 cleaning conditions determined in the SC1 cleaning condition determination step; an SC1 oxide film removal step of the silicon wafer on which a natural oxide film is to be formed, cleaning the silicon wafer on which a natural oxide film is to be formed after the SC1 cleaning step with hydrofluoric acid to completely remove the SC1 oxide film formed by the SC1 cleaning; and an oxide film formation step of the silicon wafer on which a natural oxide film is to be formed, from which the SC1 oxide film has been removed, using a cleaning solution having oxidizing power to form a natural oxide film.
[0023] According to such a method for cleaning a silicon wafer, the thickness of the native oxide film can be controlled with high accuracy and reproducibility by utilizing the correlation between the surface roughness of the wafer and the thickness of the native oxide film.
[0024] In this case, the SC1 cleaning conditions may be one or more of the SC1 chemical concentration, cleaning temperature, and cleaning time in the silicon wafer cleaning method.
[0025] These are conditions that are easily changed in practical operation, so that the cleaning conditions can be easily set.
[0026] In this case, the surface roughness can be a roughness component having a spatial frequency of 60 to 90 / μm.
[0027] Since such roughness components have a large effect on the thickness of the oxide film, it is possible to perform more accurate and stable evaluation and control of the film thickness.
[0028] In this case, the index of surface roughness can be the haze value of a particle counter.
[0029] Haze values can be easily obtained using a particle counter, resulting in extremely high throughput and enabling cleaning conditions to be set quickly and easily.
[0030] In this case, the index of surface roughness can be the average value of the power spectrum density with a spatial frequency of 60 to 90 / μm.
[0031] This allows the roughness to be evaluated in detail, enabling more accurate and stable evaluation and control of film thickness.
[0032] In this case, the cleaning liquid having an oxidizing power may be ozone water or hydrogen peroxide water.
[0033] Ozone water and hydrogen peroxide water have a strong oxidizing power, and can uniformly oxidize the wafer surface, making it possible to easily and stably form an oxide film.
[0034] In this case, the method for cleaning a silicon wafer according to the present invention can be used as a method for producing a silicon wafer with a native oxide film.
[0035] This makes it possible to manufacture silicon wafers with a native oxide film while controlling the film thickness with high accuracy and reproducibility. Effect of the Invention
[0036] As described above, according to the method for cleaning silicon wafers of the present invention, by utilizing the correlation between the surface roughness of the wafer and the thickness of the native oxide film, it is possible to control the thickness of the native oxide film with good accuracy and reproducibility. [Brief description of the drawings]
[0037] [Figure 1] 1 is a flowchart showing an example of a method for cleaning a silicon wafer according to the present invention. [Diagram 2] 1 shows a flowchart relating to an investigation of the relationship between the surface roughness of a silicon wafer and the thickness of an oxide film. [Diagram 3] FIG. 3 is a graph showing the relationship between the surface roughness (haze) of silicon wafers subjected to the roughening treatment of FIG. 2 by CMP and SC1 cleaning, and the native oxide film and the 5 nm oxide film. [Figure 4] FIG. 3 is a graph showing the relationship between the surface roughness (haze) of silicon wafers subjected to the roughening treatment of FIG. 2 by single-wafer cleaning, and the native oxide film and the 5 nm oxide film. [Diagram 5] This is a graph showing the relationship between the cleaning time and the thickness of the haze and native oxide film when the roughening treatment in FIG. 2 was performed with a liquid composition of NH4OH:H2O2:H2O=1:1:10, a cleaning temperature of 80° C., and cleaning times of 0, 3, 6, and 12 minutes. [Figure 6] The AFM measurement results and PSD curves of each sample are shown. [Figure 7] FIG. 13 is a diagram showing the relationship between the SC1 cleaning conditions and the thickness of the native oxide film of the sample after cleaning with hydrofluoric acid and cleaning with ozone water. [Figure 8] FIG. 13 is a diagram showing the relationship between the amount of haze increase and the thickness of the native oxide film for each sample. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0038] The present invention will be described in detail below, but the present invention is not limited thereto.
[0039] As described above, there has been a demand for a method for cleaning silicon wafers that can control the thickness of a native oxide film with high accuracy and reproducibility by adjusting the wafer surface roughness. In order to solve this problem, the present inventors have focused on the relationship between the roughness formed in the manufacturing process of silicon wafers, specifically the roughness formed in the polishing process and the cleaning process, and the thickness of a native oxide film and a thermal oxide film measured by an ellipsometer, and have conducted extensive research. As a result, they have found that when the average value of the power spectrum density (intensity) of a certain frequency band is equal to or greater than a predetermined value, the thickness of the oxide film becomes thick, and that the thickness of the native oxide film can be controlled by adjusting this specific roughness component, and have completed the present invention.
[0040] That is, the present inventors have discovered a method for cleaning a silicon wafer, comprising: an SC1 cleaning step for preparing a plurality of test silicon wafers in advance, and performing SC1 cleaning on the test silicon wafers under different SC1 cleaning conditions to fabricate the test silicon wafers with a plurality of levels of surface roughness different from each other; an SC1 oxide film removal step for the test silicon wafers, in which an SC1 oxide film formed in the SC1 cleaning step for the test silicon wafers is completely removed by cleaning with hydrofluoric acid; a native oxide film formation step for the test silicon wafers, in which the test silicon wafers from which the SC1 oxide film has been removed are cleaned with a cleaning solution having oxidizing power to form a native oxide film; a correlation acquisition step for acquiring a correlation between the surface roughness of the test silicon wafers formed by the SC1 cleaning and the thickness of the native oxide film formed in the native oxide film formation step for the test silicon wafers; The inventors have found that a method for cleaning a silicon wafer, which controls the thickness of a natural oxide film formed on a silicon wafer by cleaning, includes a step of determining a surface roughness to be formed on the silicon wafer on which a natural oxide film is to be formed based on the correlation, and determining SC1 cleaning conditions which will result in the determined surface roughness, a step of performing SC1 cleaning on the silicon wafer on which a natural oxide film is to be formed under the SC1 cleaning conditions determined in the SC1 cleaning condition determining step, a step of cleaning the silicon wafer on which a natural oxide film is to be formed after the SC1 cleaning step with hydrofluoric acid to completely remove the SC1 oxide film formed by the SC1 cleaning, and a step of forming a natural oxide film on the silicon wafer on which a natural oxide film is to be formed by cleaning the silicon wafer on which the SC1 oxide film has been removed using a cleaning solution having oxidizing power, thereby enabling the thickness of a natural oxide film to be controlled with good accuracy and reproducibility, and have completed the present invention.
[0041] The following description will be given with reference to the drawings.
[0042] First, we will discuss the relationship between various surface roughnesses formed in the manufacturing process of silicon wafers and the thickness of oxide films. Figure 2 is the investigation flow chart. We prepared silicon wafers by changing the CMP processing conditions and SC1 cleaning conditions, and then performed CMP processing or SC1 cleaning as a roughening process to form roughness, to prepare multiple levels of silicon wafers. Next, the oxide film was completely removed by hydrofluoric acid cleaning in a batch cleaning machine, and then an oxide film was formed by cleaning with ozone water. In both levels, the oxide film formed by the SC1 cleaning of the roughening process was completely removed by hydrofluoric acid cleaning, and the oxide film was formed by the subsequent ozone water, so it can be interpreted that the oxide film was formed by the same method on multiple levels of silicon wafers. After that, we performed haze measurement using a particle counter, and then thermally oxidized some wafers with a target thickness of 5 nm, and evaluated the thickness of the natural oxide film and the oxide film formed with a target thickness of 5 nm using spectroscopic ellipsometry.
[0043] Figure 3 is a graph showing the relationship between the surface roughness (haze) of silicon wafers that were roughened using CMP and SC1 cleaning as shown in Figure 2, and the thickness of the native oxide film and the oxide film aimed for a thickness of 5 nm. At the CMP level (■), the thickness of the native oxide film and the oxide film aimed for a thickness of 5 nm were the same even when the haze value exceeded 10 ppm, but at the SC1 cleaning level (●), there was a tendency for both the native oxide film and the oxide film aimed for a thickness of 5 nm to become thicker as the haze increased. Since the oxide film was formed under the same conditions, it was assumed that the film thickness would be the same, as with the CMP level, but this was not the case with the SC1 cleaning level.
[0044] Furthermore, Figure 4 shows the relationship between the surface roughness (haze) of silicon wafers and the thickness of the native oxide film and the oxide film aimed at 5 nm, when the roughening treatment in Figure 2 was performed by single-wafer cleaning combined with hydrofluoric acid and ozone water cleaning. In addition, the hydrofluoric acid cleaning and ozone water cleaning after the roughening treatment were also performed by single-wafer method instead of batch method. In this case, since the oxide film formation method is different from the batch method of ozone water, it is not possible to compare the film thickness of the above-mentioned SC1 and CMP levels with the single-wafer cleaning level, but the influence of haze within the single-wafer cleaning level can be discussed. As a result, the single-wafer cleaning level was the same as the CMP level, and the thickness of the native oxide film and the oxide film aimed at 5 nm was the same even if the haze changed. To summarize the above results, it was newly discovered that the roughness formed by CMP and single-wafer cleaning does not affect the thickness of the oxide film, and the surface roughness of the substrate formed by SC1 cleaning has an effect of making the oxide film thicker.
[0045] Here, we will explain the results of an additional investigation into the SC1 cleaning level. SC1 cleaning for roughening treatment was performed in batch cleaning with a liquid composition of NH4OH:H2O2:H2O = 1:1:10, a cleaning temperature of 80°C, and cleaning times of 3, 6, and 12 minutes. The oxide film was completely removed by hydrofluoric acid cleaning, and then cleaning with ozone water was performed. Figure 5 shows the thickness and haze value of the native oxide film after this. The native oxide film thickness without cleaning time (0 minutes), which serves as the reference, was 1.207 nm, while the thickness was 1.258 nm with a cleaning time of 3 minutes, 1.258 nm with a cleaning time of 6 minutes, and 1.261 nm with a cleaning time of 12 minutes. The difference between the average film thickness of 1.259 nm with cleaning times of 3, 6, and 12 minutes and the film thickness of 1.207 nm without cleaning (cleaning time of 0 minutes) is 0.052 nm, so the amount of film thickening caused by the SC1 cleaning for roughening treatment is considered to be about 0.052 nm. Haze tended to increase with increasing cleaning time, whereas the amount of film thickening was similar for cleaning times of 3, 6, and 12 minutes. Considering this, it is believed that the specific roughness components formed in SC1 cleaning affect the film thickening behavior, and the film thicknesses were similar for times 3, 6, and 12 minutes because the roughness components involved in the film thickness (thickening) were similar.
[0046] To verify these results, the surface roughness of wafers with typical CMP, SC1 cleaning, and single-wafer cleaning levels was evaluated using an AFM (atomic force microscope). The observation field was 1 μm x 1 μm, and in addition to the three-dimensional arithmetic mean height Sa, a PSD curve was obtained from the spectral analysis of the surface profile data. Figure 6 shows the AFM measurement results and PSD curves for each sample.
[0047] First, we will look at the CMP level. In terms of CMP level, we evaluated the level with the smallest haze value (CMP-1) and the highest level (CMP-2) in Figure 3. In CMP-2, the power spectrum density (intensity) in the low frequency band (1-10 / μm) was extremely high, and roughness on the low frequency side was predominant. The AFM image also showed a large undulating image, which matched the results. As mentioned above, the roughness formed by CMP does not affect the thickness of the oxide film, so it can be said that this low frequency component does not affect the thickness of the oxide film.
[0048] Next, we focus on the SC1 cleaning level. For the SC1 cleaning level, three levels of solution composition NH4OH:H2O2:H2O = 1:1:10, cleaning temperature and cleaning time were evaluated: 60℃ / 3min, 80℃ / 3min, and 80℃ / 12min. These are the levels at which an oxide film would be thicker by the same thickness if it were formed using the same method. As shown in Figure 6, the roughness in the high frequency band (10-100 / μm) is dominant in all three levels compared to CMP-2, which coincides with the fine granular roughness obtained in the AFM image. Therefore, it can be said that the roughness components (spatial frequency band) formed by CMP and SC1 cleaning are significantly different.
[0049] Finally, we focus on the single-wafer cleaning level. In the single-wafer cleaning level, the level with the smallest haze value (single-wafer cleaning-1) and the level with the largest haze value (single-wafer cleaning-2) were evaluated in Figure 4. The power spectrum density (intensity) of the single-wafer cleaning level was about halfway between CMP and SC1 cleaning in the high frequency band (10 to 100 / μm).
[0050] We consider these roughness evaluation results and their influence on the oxide film thickness. In particular, while the Sa value for both SC1 cleaning at -80°C / 3min and single-wafer cleaning at -2 is 0.108 nm, the oxide film thickness is thicker with SC1 cleaning at -80°C / 3min, but not with single-wafer cleaning at -2. Looking at the PSD curves for both, the power spectrum density (intensity) in the low frequency band (1-10 / μm) is equivalent, whereas the power spectrum density (intensity) in the high frequency band (especially 50 / μm or more) is greater with SC1 cleaning at -80°C / 3min than with single-wafer cleaning at -2. Therefore, although there is no significant difference between the two in the AFM images, the PSD curves indicate that roughness in the high frequency band is more dominant with SC1 cleaning at -80°C / 3min. Furthermore, considering that the three SC1 cleaning levels shown in the figure (60°C / 3 min, 80°C / 3 min, 80°C / 12 min) all result in the same thickness (approximately 0.05 nm), it can be seen that the power spectrum density (intensity) in the spatial frequency band of 60-90 / μm is equivalent for all three levels, and is higher than single wafer cleaning-2. Therefore, it has become clear that the roughness component in the 60-90 / μm range is the roughness component that affects the thickness of the native oxide film and the oxide film targeted at 5 nm. By evaluating and controlling the surface roughness of such roughness components, it is possible to control the film thickness more accurately and stably.
[0051] In addition, the power spectrum density (intensity) for spatial frequency bands of 50 / μm or less is within the three levels of SC1 cleaning. 80℃ / 12min > 80℃ / 3min > 60℃ / 3min The relationship between the magnitudes of the Sa values is as follows: 80℃ / 12min > 80℃ / 3min > 60℃ / 3min This also coincides with the Sa value in this case, which is dominated by roughness information on the low-frequency side where intensity is high. This is thought to be the reason for the difference in oxide film thickness, even though the above-mentioned single wafer cleaning-2 and SC1 cleaning-80°C / 3min have the same Sa value of 0.108 nm.
[0052] To summarize the above results, it is believed that the oxide film will become thicker if the average value of the power spectrum density (intensity), which is the roughness component in the spatial frequency band of 60 to 90 / μm, is above a threshold value. Here, the average value of the power spectrum density (intensity) in the range of 60 to 90 / μm for the three levels of SC1 cleaning was calculated to be 0.16 nm for SC1 cleaning at -60°C / 3 min. 3 , 0.18 nm after SC1 cleaning at -80℃ / 3 min 3 , SC1 cleaning -80℃ / 12min: 0.17nm 3 On the other hand, the average value for single wafer cleaning-2, where the oxide film does not become thick, was 0.11 nm. 3 Therefore, the average value of the power spectrum density (intensity) of 60 to 90 / μm was 0.15 nm. 3 is considered to be the threshold value, and 0.15 nm 3 It can be determined that the thickness of the silicon oxide film on the silicon wafer where the average value of the above power spectrum density (intensity) exists is affected by the surface roughness of the wafer, and includes the thickness caused by the surface roughness of the substrate.
[0053] From the above findings, it can be interpreted that the surface roughness of a specific wafer is a factor that affects the thickness of an oxide film (film thickness influencing factor). Here, the factors that affect the thickness of a native oxide film and a thermal oxide film include, for example, the structure of a native oxide film (chemical oxide film) described in Patent Document 3 and the surface roughness of a silicon wafer described above.
[0054] Here, we consider the surface roughness of the wafer after SC1 cleaning and the structure of the native oxide film. First, SC1 cleaning is a cleaning in which the reaction of oxidizing Si by hydrogen peroxide and the reaction of etching the oxidized SiO2 are always progressing, and the oxidation and etching behavior changes depending on the cleaning conditions, such as the chemical concentration, cleaning temperature, and cleaning time. In addition, under general conditions, the etching reaction of SiO2 is rate-limiting, so the surface is always covered with a native oxide film. Since the thickness of the native oxide film after SC1 cleaning varies depending on the balance between the oxidation and etching reactions, it is necessary to control the oxidation and etching reactions in order to control the thickness of the native oxide film after SC1 cleaning. This oxidation and etching behavior affects both the structure of the native oxide film as described in Patent Document 3 in addition to the wafer surface roughness. In other words, it can be said that both of these two factors must be controlled in order to control the thickness of the native oxide film after SC1 cleaning and the film thickness after thermal oxidation. In other words, it shows that when a slight unintended change in the cleaning conditions occurs, the film thickness of the native oxide film fluctuates greatly. In particular, the structure of the native oxide film greatly affects the film thickness after thermal oxidation, so it is an important quality when controlling the film thickness after thermal oxidation.
[0055] Here, in addition to SC1 cleaning, there are other methods for forming a natural oxide film on the wafer surface, such as ozone water and hydrogen peroxide water. These do not cause an etching reaction, and only an oxidation reaction proceeds. Ozone water in particular has a very strong oxidizing power, so it can form an oxide film with better control than SC1 cleaning.
[0056] Therefore, the present inventors have studied whether the thickness of the native oxide film can be controlled by limiting the variation factor of the native oxide film to only the wafer surface roughness. That is, the target wafer on which the native oxide film is to be formed is subjected to SC1 cleaning, and roughness is formed in the range of spatial frequency band 60-90 / μm to thicken the thickness of the native oxide film. After that, for example, hydrofluoric acid cleaning is performed to completely peel off the native oxide film formed by the SC1 cleaning, and then the native oxide film is formed using a cleaning solution having an oxidizing power, such as ozone water without etching. It was thought that this would limit the variation factor to the wafer surface roughness and control the thickness of the native oxide film.
[0057] [Silicon wafer cleaning method] Based on the above, the method for cleaning a silicon wafer according to the present invention will be described in detail below. FIG. 1 is a flow chart showing an example of the method for cleaning a silicon wafer according to the present invention. First, a test silicon wafer is used to obtain a correlation between the surface roughness of the silicon wafer after SC1 cleaning and the thickness of the native oxide film. Then, using this correlation, the surface roughness of the silicon wafer on which the native oxide film is to be formed is determined, and the silicon wafer is SC1 cleaned under SC1 cleaning conditions according to the determined surface roughness of the silicon wafer to form a predetermined surface roughness, and after removing the SC1 oxide film, a native oxide film is formed. The method for cleaning a silicon wafer according to the present invention will be described in detail below.
[0058] (Test silicon wafer) First, a plurality of test silicon wafers for obtaining the correlation are prepared (S1 in FIG. 1). There is no restriction on the conductive type and diameter of the silicon wafer. As for the surface roughness, it is preferable that the surface roughness of the test silicon wafer and the silicon wafer on which the native oxide film is formed, which will be described later, is 0.5 nm or less in terms of Sa value. This is because the oxide film thickness calculated by spectroscopic ellipsometry in such a range is about 1 nm, and is more suitable for evaluating the thickness of the native oxide film of silicon wafers used in recent years. Generally, the Sa value of the front surface of a silicon wafer after CMP is 0.1 nm or less, and the Sa value of the back surface (DSP surface) is about 0.2 to 0.4 nm. Therefore, any wafer after CMP processing, which is at least followed by DSP (double-sided polishing) processing, can be suitably used in the silicon wafer cleaning method according to the present invention.
[0059] (SC1 cleaning process for test silicon wafers) Next, SC1 cleaning is performed on the prepared test silicon wafers under different cleaning conditions (S2 in FIG. 1). As cleaning conditions, it is desirable to change at least one of the following: the SC1 chemical concentration, the cleaning temperature, and the cleaning time. These are conditions that are easy to change in practical operation, and the cleaning conditions can be easily set. For example, the chemical concentration may be adjusted in the range of NH4OH:H2O2:H2O=1:1:5 to 1:1:100. For example, the cleaning temperature may be adjusted in the range of 30 to 90°C. For example, the cleaning time may be adjusted in the range of 0.5 to 10 min. One or more of the above conditions can be set, but it is preferable to set more cleaning conditions, and it is also possible to set three or more of the above conditions. By performing SC1 cleaning in this way, roughness is formed on the surface of the wafer, and an oxide film is formed at the same time.
[0060] In general, oxide films formed by cleaning are collectively called natural oxide films or chemical oxide films. In this specification, however, in order to distinguish between different types of oxide films, an oxide film formed by SC1 cleaning is called an "SC1 oxide film," and an oxide film formed by cleaning using a cleaning solution other than SC1 cleaning that has oxidizing power is called a "natural oxide film."
[0061] (SC1 oxide film removal process for test silicon wafers) Next, the test silicon wafer after SC1 cleaning is cleaned with hydrofluoric acid to completely remove the SC1 oxide film (S3 in Fig. 1). As long as the SC1 oxide film can be completely removed, there are no limitations on the hydrofluoric acid cleaning conditions. For example, the hydrofluoric acid concentration is 0.3 to 5.0 wt%, the temperature is 10 to 30°C, and the cleaning time is 60 to 360 seconds.
[0062] (Natural oxide film formation process for test silicon wafers) Next, the test silicon wafer from which the SC1 oxide film has been removed is cleaned using a cleaning solution having an oxidizing power to form a native oxide film (S4 in FIG. 1). As the cleaning solution having an oxidizing power, ozone water or hydrogen peroxide water is preferable, and ozone water having a stronger oxidizing power is more preferable. Ozone water or hydrogen peroxide water has a strong oxidizing power, and can uniformly oxidize the wafer surface, and can easily and stably form an oxide film. For example, the concentration of the ozone water used can be in the range of 3 to 25 ppm, the temperature can be 10 to 30° C., and the cleaning time can be 60 to 360 seconds. Also, for example, the concentration of the hydrogen peroxide water used can be 0.2 to 5.0 wt%, the temperature can be 30 to 90° C., and the cleaning time can be 60 to 360 seconds. When a batch-type cleaning machine is used, a series of these cleaning steps can be performed in one batch to reduce the labor.
[0063] (Correlation acquisition process) Next, the correlation between the surface roughness of the test silicon wafer on which the oxide film is formed and the thickness of the native oxide film is obtained (S5 in FIG. 1). The thickness of the native oxide film may be measured by a known measurement method, for example, by spectroscopic ellipsometry. The simplest index of surface roughness is to obtain the Haze value using a particle counter. When using the Haze value, the roughness can be accurately reflected by using the difference (Haze increase amount, ΔHaze) before and after cleaning. Alternatively, a roughness index such as Sa may be used by AFM, or a PSD curve may be obtained from the spectrum analysis of the AFM profile data, and the average value of the power spectrum density (intensity) in the spatial frequency band of 60 to 90 / μm may be used. Note that the roughness evaluation may be performed after the SC1 cleaning and before the correlation acquisition step, and may be performed before the hydrofluoric acid cleaning, or may be performed after the SC1 cleaning, hydrofluoric acid cleaning, or cleaning with a cleaning solution having an oxidizing power. This is because the surface roughness components that affect the thickness of the oxide film are almost unchanged by the hydrofluoric acid cleaning and cleaning with an oxidizing power.
[0064] Figure 7 shows the thickness of the native oxide film under each cleaning condition when SC1 cleaning was performed with a chemical concentration of NH4OH:H2O2:H2O = 1:1:10, cleaning temperatures of 40, 50, 55, and 60°C, cleaning times of 3 and 6 minutes, followed by hydrofluoric acid cleaning and ozone water cleaning. For both cleaning times of 3 and 6 minutes, the higher the cleaning temperature, the thicker the film tended to be. This is because the higher the cleaning temperature, the more roughness components in the spatial frequency band of 60 to 90 / μm mentioned above are formed. The haze value of the particle counter reflects the roughness in this range of 60 to 90 / μm, so the haze value can be used as an index.
[0065] Figure 8 shows the relationship between the haze increase and film thickness before and after cleaning for a cleaning time of 3 minutes. As shown here, there is a good correlation between the haze increase and film thickness. In this way, the correlation between surface roughness and the film thickness of the native oxide film can be obtained.
[0066] Next, using this correlation, the silicon wafer on which the native oxide film is to be formed (S6 in FIG. 1) is cleaned to form a native oxide film of the desired thickness.
[0067] (SC1 cleaning condition determination process) In the SC1 cleaning condition determination process (S7 in Fig. 1), first, the thickness of the native oxide film to be formed is set. Next, the necessary surface roughness is estimated and determined from the correlation, and the SC1 cleaning conditions that will result in the determined surface roughness are determined. In this specific example, the target film thickness is set to 1.310 nm. From the correlation in Fig. 8, the haze increase amount corresponding to the film thickness of 1.310 nm is 0.020 ppm. Also, from the correlation in Fig. 7, it can be seen that in order to form this roughness of 0.020 ppm, cleaning should be performed with a liquid composition of NH4OH:H2O2:H2O=1:1:10, a cleaning temperature of 55°C, and a cleaning time of 3 minutes. These cleaning conditions were determined as the SC1 cleaning conditions.
[0068] (SC1 cleaning process for silicon wafers subject to native oxide film formation) Next, the silicon wafer on which the native oxide film is to be formed is subjected to SC1 cleaning under the determined cleaning conditions (S8 in FIG. 1).
[0069] (SC1 oxide film removal process for silicon wafers with native oxide film) Next, the silicon wafer on which the native oxide film is to be formed is cleaned with hydrofluoric acid to completely remove the SC1 oxide film formed by the SC1 cleaning (S9 in FIG. 1).
[0070] (Oxide film formation process for silicon wafers on which natural oxide films are to be formed) Next, the silicon wafers on which the natural oxide film is to be formed, from which the SC1 oxide film has been completely removed, are cleaned with a cleaning solution having the same oxidizing power as that used when the natural oxide film was formed on the test silicon wafer (the oxide film formation process for the test silicon wafer), to form a natural oxide film (S10 in Fig. 1). In a specific example, the natural oxide film was formed by cleaning with ozone water. When the natural oxide film on the silicon wafer after cleaning with ozone water was evaluated by spectroscopic ellipsometry, it was found to be approximately 1.312 nm, which indicates that a natural oxide film equivalent to the set value of 1.310 nm can be formed.
[0071] [Manufacturing method for silicon wafers with native oxide film] By using the silicon wafer cleaning method according to the present invention, it is possible to manufacture silicon wafers with a native oxide film while controlling the film thickness with high precision. EXAMPLES
[0072] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto.
[0073] (Example) As test silicon wafers, several silicon wafers that had been subjected to CMP polishing and single-wafer cleaning were prepared. First, the haze value before SC1 cleaning was obtained using a KLA particle counter SP3. Next, SC1 cleaning, hydrofluoric acid cleaning, and ozone water cleaning were performed using a batch cleaning machine under the cleaning conditions described below. The SC1 cleaning conditions were a liquid composition of NH4OH:H2O2:H2O=1:1:10, a cleaning time of 3 min, and cleaning temperatures of 40, 50, 55, and 60°C. The hydrofluoric acid cleaning was performed with a concentration of 0.5 wt%, a cleaning temperature of 25°C, and a cleaning time of 3 min, and the ozone water cleaning was performed with a concentration of 20 ppm, a cleaning temperature of 25°C, and a cleaning time of 3 min. Next, the haze of the test silicon wafers after cleaning was evaluated using SP3. After that, the thickness of the native oxide film was evaluated using a JA Woollam spectroscopic ellipsometer M-2000V. The results are shown in Table 1. The higher the cleaning temperature, the greater the increase in haze and the thicker the film tended to be, and a correlation was obtained between roughness and film thickness.
[0074] [Table 1]
[0075] Next, the target thickness of the native oxide film formed on the silicon wafer was set to 1.330 nm. Using the obtained correlation, the increase in haze when the target thickness was 1.330 nm was approximately 0.028 ppm, and since the cleaning conditions of a cleaning temperature of 60°C and a cleaning time of 3 min were suitable for forming this surface roughness, the SC1 cleaning conditions were determined to be a liquid composition of NH4OH:H2O2:H2O=1:1:10, a cleaning temperature of 60°C and a cleaning time of 3 min.
[0076] Next, the target silicon wafer was SC1 cleaned at the determined cleaning temperature of 60°C / cleaning time of 3 min, and then cleaned with hydrofluoric acid and ozone water under the same conditions as when the above correlation was obtained. After that, the native oxide film after cleaning was evaluated with M-2000V, and the thickness was found to be 1.332 nm, which was confirmed to be equivalent to the target set value of 1.330 nm. Thus, according to the embodiment of the present invention, the thickness of the native oxide film could be controlled by using the relationship between the surface roughness and the thickness of the native oxide film.
[0077] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.
Claims
1. A method for cleaning a silicon wafer, comprising the steps of: a SC1 cleaning step of preparing a plurality of test silicon wafers in advance and performing SC1 cleaning of the test silicon wafers under different SC1 cleaning conditions to produce the test silicon wafers having a plurality of levels of different surface roughness; an SC1 oxide film removing step of completely removing the SC1 oxide film formed in the SC1 cleaning step of the test silicon wafer by hydrofluoric acid cleaning; a native oxide film forming step of cleaning the test silicon wafer from which the SC1 oxide film has been removed using a cleaning solution having an oxidizing power to form a native oxide film on the test silicon wafer; a correlation acquisition step of acquiring a correlation between a surface roughness of the test silicon wafer formed by the SC1 cleaning and a thickness of a native oxide film formed in a native oxide film formation step of the test silicon wafer; a SC1 cleaning condition determination step of determining a surface roughness to be formed on a silicon wafer on which a native oxide film is to be formed, based on the correlation obtained in the correlation obtaining step, so that a native oxide film formed on the silicon wafer by cleaning the silicon wafer with the cleaning solution having an oxidizing power has a predetermined thickness, and determining SC1 cleaning conditions that will result in the determined surface roughness; an SC1 cleaning step of the silicon wafer on which the native oxide film is to be formed, the SC1 cleaning step being performed on the silicon wafer on which the native oxide film is to be formed under the SC1 cleaning conditions determined in the SC1 cleaning condition determination step; an SC1 oxide film removal step of the silicon wafer on which the native oxide film is to be formed, which is subjected to hydrofluoric acid cleaning after the SC1 cleaning step, to completely remove the SC1 oxide film formed by the SC1 cleaning; and an oxide film formation step for the silicon wafer as the target for natural oxide film formation, in which the silicon wafer as the target for natural oxide film formation, from which the SC1 oxide film has been removed, is cleaned with the cleaning solution having oxidizing power to form a natural oxide film, thereby controlling the thickness of the natural oxide film formed on the silicon wafer by cleaning.
2. 2. The method for cleaning silicon wafers according to claim 1, wherein the SC1 cleaning conditions are at least one of an SC1 chemical concentration, a cleaning temperature, and a cleaning time.
3. 3. The method for cleaning a silicon wafer according to claim 1, wherein the surface roughness is a roughness component having a spatial frequency of 60 to 90 / μm.
4. 4. The method for cleaning a silicon wafer according to claim 1, wherein the index of surface roughness is a haze value measured by a particle counter.
5. 4. The method for cleaning a silicon wafer according to claim 1, wherein the index of surface roughness is an average value of power spectrum density having a spatial frequency of 60 to 90 / μm.
6. 6. The method for cleaning a silicon wafer according to claim 1, wherein the cleaning liquid having an oxidizing power is ozone water or hydrogen peroxide water.
7. 7. A method for producing a silicon wafer with a native oxide film, comprising producing a silicon wafer with a native oxide film by the method for cleaning a silicon wafer according to claim 1.
Citation Information
Patent Citations
Method for measuring surface roughness of semiconductor substrate
JP1994163662A
Method for analyzing sample
JP2005283502A
Method for forming thermal oxide film on semiconductor substrate
JP6791453B1
Method for manufacturing gate oxide film on semiconductor wafer by wet process
KR1020090044812A
Method of growing uniform oxide layer and method of cleaning substrate
KR1020110036990A