Defect Inspection Method

The method forms a 1 to 4 nm thick silicon nitride film on substrates to enlarge and detect smaller defects, overcoming sensitivity loss from haze and roughness, allowing detection of defects smaller than 10.6 nm.

JP7571854B1Active Publication Date: 2024-10-23SHIN ETSU HANDOTAI CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023206511
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-12-06
Publication Date
2024-10-23
Estimated Expiration
2043-12-06

AI Technical Summary

Technical Problem

Conventional methods for defect inspection on substrates, such as semiconductor substrates, fail to detect protruding defects smaller than 10.6 nm due to the lens effect and haze caused by the formation of CVD films, which deteriorate detection sensitivity.

Method used

A defect inspection method involving the formation of a silicon nitride film with a thickness of 1 to 4 nm on the substrate, followed by detection using a surface inspection device, to estimate the size of protruding defects by enlarging them and suppressing haze and roughness deterioration.

Benefits of technology

Enables the detection of smaller protruding defects than the minimum sensitivity of current particle counters by forming a thin silicon nitride film, maintaining high sensitivity without significant haze or roughness deterioration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571854000001_ABST
    Figure 0007571854000001_ABST
Patent Text Reader

Abstract

A defect inspection method capable of estimating the size of smaller protrusion-like defects is provided. [Solution] This defect inspection method includes a silicon nitride film formation step of forming a silicon nitride film having a thickness of 1 to 4 nm on a substrate in order to increase the detection size of a protrusion-like defect present on the surface of the substrate; a detection step of detecting, after the silicon nitride film formation step, the size of a protrusion portion enlarged and formed on the surface of the silicon nitride film above the protrusion-like defect using a surface inspection device; and a defect size estimation step of estimating the size of the protrusion-like defect before the formation of the silicon nitride film from the size of the protrusion portion detected in the detection step and a predetermined relationship between the film thickness of the silicon nitride film and the amount of increase in the detection size.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for inspecting a substrate for defects. [Background technology]

[0002] Since defects present on the surface of a substrate, such as a semiconductor substrate, can cause device failure, the reduction and evaluation of defects have become more important with the recent advancement of miniaturization due to the sophistication of devices. Defects present on the surface of a substrate are mainly detected by a particle counter, which is known as a representative surface inspection device. A particle counter inspects the substrate surface by irradiating light onto the substrate surface and detecting scattered light caused by protruding defects (also called particles) present on the substrate surface. The intensity of the scattered light varies depending on the size, shape, composition, etc. of the particle, and for example, the larger the particle, the greater the scattered light intensity. In addition, the particle counter can calculate the detection size based on the scattered light intensity and the scattered light intensity for each size of standard particle. In other words, the greater the scattered light intensity, the greater the detection size. In order to detect particles with a small detection size, it is necessary to perform measurements using the particle counter for a long time. In addition, in the case of particles with very small scattered light intensity, they cannot be detected because they cannot be distinguished from scattered light caused by the roughness (haze) of the substrate surface.

[0003] Patent Document 1 discloses that in order to detect minute particles that cannot be directly detected by a particle counter, a silicon nitride film (hereinafter also simply referred to as a nitride film) is formed to make the size of the particles larger than that of the original particles.

[0004] In this technology, the formation of a nitride film causes the nitride film to rise with tiny particles acting as nuclei, so by measuring the substrate with a particle counter after the nitride film is formed, it is possible to measure particles with high sensitivity. The film thickness in this case is determined as follows: Film Thickness ≧ (Inspection Equipment Detection Sensitivity - Defect Size) × Safety Factor, with the safety factor being 100% or more. Here, detection sensitivity is also called measurement sensitivity. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-212009 A Summary of the Invention [Problem to be solved by the invention]

[0006] When depositing a CVD film such as a nitride film on a substrate, if there is a convex protrusion on the substrate, the CVD film will be deposited around the protrusion, increasing the size of the convex protrusion. In particular, since nitride film has a high refractive index, it can be detected by making the size larger.

[0007] This phenomenon is called the lens effect, and is a common phenomenon, but since CVD films are not formed uniformly, the roughness after the CVD film is formed is generally worse than the roughness of the substrate before the CVD film is formed. Therefore, forming a thick CVD film causes the haze caused by the roughness to worsen, and the detection sensitivity of the particle counter decreases.

[0008] However, Patent Document 1 focuses only on the increase in defect size due to the formation of a CVD film, and does not take into consideration the decrease in sensitivity due to haze.

[0009] In addition, if we focus only on the increase in defect size due to the formation of a CVD film, the particle size is expected to increase to 19 nm, the general measurement sensitivity, by forming a 50 nm CVD film only for particles that were larger than 12 nm before the CVD film was formed. In other words, particles smaller than 12 nm cannot be detected by forming a 50 nm CVD film.

[0010] In recent years, the performance of particle counters has improved, making it possible to measure particles smaller than 12 nm without forming a CVD film. The minimum size detection sensitivity of this highly sensitive particle counter is 10.6 nm. In this case, if a CVD film is formed using conventional methods, the effect of haze can actually cause the detection sensitivity to deteriorate. For this reason, when measuring minute protruding defects with a highly sensitive particle counter, it is more sensitive to measure without forming a nitride film, and the limit (minimum sensitivity) is 10.6 nm.

[0011] As devices become more sophisticated and miniaturized in the future, it will be desirable to be able to inspect even smaller protrusion defects; however, there has traditionally been a problem in that there is no inspection method capable of detecting protrusion defects smaller than 10.6 nm.

[0012] The present invention has been made to solve the above problems, and has an object to provide a defect inspection method capable of estimating the size of smaller protrusion-like defects. [Means for solving the problem]

[0013] In order to solve the above problems, the defect inspection method of the present invention includes a silicon nitride film formation step of forming a silicon nitride film having a thickness of 1 to 4 nm on a substrate in order to increase the detectable size of protrusion-like defects present on the surface of the substrate; a detection step of detecting, after the silicon nitride film forming step, a size of a protrusion portion enlarged and formed on a surface of the silicon nitride film above the protrusion defect by a surface inspection device; a defect size estimation step of estimating a size of the protrusion defect before the formation of the silicon nitride film based on a size of the protrusion detected in the detection step and a preset relationship between a film thickness of the silicon nitride film and an amount of enlargement of the detected size; The defect inspection method includes the steps of:

[0014] With this defect inspection method, by forming a silicon nitride film with a thickness of 1 to 4 nm, it is possible to form an enlarged protrusion on the surface of the silicon nitride film above the protrusion-like defect, and it is also possible to suppress the deterioration of roughness due to the formation of the silicon nitride film and the deterioration of haze caused by the roughness, so that the size of smaller protrusion-like defects can be estimated based on the size of the detected protrusion.

[0015] In the defect inspection method of the present invention, it is preferable that in the silicon nitride film forming step, the silicon nitride film is formed at a temperature of 500° C. or higher and 580° C. or lower.

[0016] Within this temperature range, a silicon nitride film can be formed in which the deterioration of haze is further suppressed.

[0017] In addition, in the defect inspection method of the present invention, it is preferable that the predetermined relationship between the film thickness of the silicon nitride film and the amount of increase in the detection size is set based on the amount of change in the detection size before and after the formation of the silicon nitride film detected in advance on another substrate.

[0018] Within an appropriate film thickness range (1 to 4 nm), there is a correlation between the detection size before and after the formation of the silicon nitride film, and the larger the film thickness, the larger the detection size after the formation of the silicon nitride film (i.e., the larger the amount of expansion). Therefore, it is easy to set the relationship between the film thickness and the amount of expansion of the detection size based on the amount of change in the detection size before and after the formation of the silicon nitride film, which is previously obtained on another substrate. Therefore, the size of the protrusion defect before the formation of the silicon nitride film can be easily estimated from the size of the protrusion detected after the formation of the silicon nitride film and the previously set relationship between the film thickness of the silicon nitride film and the amount of expansion of the detection size.

[0019] In the defect inspection method of the present invention, in the detection step, it is preferable that the measurement sensitivity during detection by the surface inspection device is higher than 19 nm.

[0020] With this level of measurement sensitivity, it is possible to detect the size of small protrusions that cannot be detected with the 19 nm measurement sensitivity of typical surface inspection devices, and based on the size of these detected protrusions, the size of even smaller protrusion-like defects can be estimated.

[0021] In the defect inspection method of the present invention, it is preferable that the size of the protrusion defect before the silicon nitride film is formed is less than 10.6 nm.

[0022] Such protrusion defects of less than 10.6 nm are smaller than the minimum sensitivity of the latest particle counters, which are typical surface inspection devices, and therefore the size of the protrusion defects could not be estimated using conventional methods. However, the above-described means of the present invention make it possible to estimate the size of even smaller protrusion defects. Effect of the Invention

[0023] According to the defect inspection method of the present invention, by forming a silicon nitride film having a thickness of 1 to 4 nm, it is possible to enlarge and form a protrusion on the surface of the silicon nitride film on the protrusion defect, and it is also possible to suppress the deterioration of roughness due to the formation of the silicon nitride film and the deterioration of haze due to the roughness, so that it is possible to estimate the size of a smaller protrusion defect based on the size of the detected protrusion. Specifically, it is possible to detect even a protrusion defect smaller than the minimum sensitivity (10.6 nm) of the latest particle counter, which is a representative surface inspection device. [Brief description of the drawings]

[0024] [Figure 1] 2 is a flowchart showing an example of a defect inspection method according to the present invention. [Diagram 2] This is an LPD map before and after forming a silicon nitride film with a thickness of 50 nm. [Diagram 3] This is an LPD map before and after forming a silicon nitride film with a thickness of 50 nm. [Figure 4] This is an LPD map comparing the difference in film thickness and measurement sensitivity. [Diagram 5] These are LPD maps before and after the formation of a 4 nm thick silicon nitride film. [Figure 6] 1 is a graph showing the change in defect size before and after the formation of a silicon nitride film having a thickness of 4 nm. [Figure 7] 1 is a graph showing particle size distribution after forming a silicon nitride film having a thickness of 4 nm. [Figure 8] 1 is a graph showing the change in defect size before and after the formation of silicon nitride films having thicknesses of 6 nm and 9.5 nm. [Figure 9] 1 is a graph showing the change in defect size before and after the formation of a silicon nitride film having a thickness of 0.4 nm. [Figure 10] The LPD maps are before and after the formation of a silicon nitride film with a thickness of 1.2 nm. [Figure 11] 1 is a graph showing the change in defect size before and after the formation of a silicon nitride film having a thickness of 1.2 nm. [Figure 12] 1 is a graph showing particle size distribution after forming a silicon nitride film having a thickness of 1.2 nm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] The present invention will be described in detail below, but the present invention is not limited thereto.

[0026] As described above, there has been a demand for providing a defect inspection method capable of detecting smaller protrusion defects.

[0027] The inventors of the present invention have conducted extensive research into the above-mentioned problems, and have focused on finding a method for measuring minute protrusion-like defects with higher sensitivity by utilizing the lens effect caused by the formation of a nitride film, even when measuring with a highly sensitive particle counter.

[0028] First, it has been known that when particles are coated with a CVD film such as a silicon nitride film, the size of the particles increases and they become easier to detect, and this should enable high-sensitivity measurement. Since the deterioration of haze caused by CVD causes the sensitivity to drop after the formation of the CVD film, we thought that high sensitivity could be achieved by using a thin-film CVD that enlarges small defects slightly without causing haze deterioration. Currently, the minimum sensitivity of particle counters is about 10 nm, and the scattered light intensity used for detection is very weak, so it is very difficult to improve the particle counter to increase the sensitivity by several nm from 10 nm size. However, in the research by the inventors, by forming a nitride film of several nm, the particles are coated with a coating of several nm and enlarged, and finally it became possible to detect defects several nm smaller than 10 nm.

[0029] Looking back, with conventional methods, for defects approximately 12 nm or larger in size, the effect of larger particles was greater than the deterioration in sensitivity due to haze caused by the formation of a CVD film, and so high sensitivity was achieved by forming a CVD film. However, for defects approximately 10 nm in size, the increase in size due to the formation of a CVD film was small, and it is thought that the deterioration in haze actually made the defects less visible. In this study, thin-film CVD was used to increase the size of defects below 10 nm while minimizing the deterioration of haze, making it possible to detect defects smaller than the sensitivity of the latest particle counters.

[0030] Thus, the present inventors have discovered a method capable of measuring minute protrusion defects with higher sensitivity, and have completed the present invention.

[0031] That is, the defect inspection method of the present invention is a defect inspection method including: a silicon nitride film formation step of forming a silicon nitride film having a thickness of 1 to 4 nm on a substrate in order to increase the detection size of a protrusion-like defect present on the surface of the substrate; a detection step of detecting, after the silicon nitride film formation step, the size of a protrusion portion enlarged and formed on the surface of the silicon nitride film above the protrusion-like defect using a surface inspection device; and a defect size estimation step of estimating the size of the protrusion-like defect before the formation of the silicon nitride film from the size of the protrusion portion detected in the detection step and the relationship between a preset film thickness of the silicon nitride film and the amount of increase in the detection size.

[0032] Hereinafter, the present invention will be described in detail with reference to the drawings as an example of an embodiment, but the present invention is not limited thereto.

[0033] FIG. 1 is a flow chart showing an example of a defect inspection method according to the present invention.

[0034] <Step S1: Silicon nitride film formation process> Step S1 is a process of forming a silicon nitride film having a thickness of 1 to 4 nm on a substrate in order to increase the detectable size of protrusion defects present on the surface of the substrate.

[0035] By deliberately making the film thickness 1 to 4 nm instead of the conventional thickness of several tens of nm, it is possible to form enlarged protrusions on the surface of the silicon nitride film on the protrusion-like defects, and also to suppress the deterioration of roughness due to the formation of the silicon nitride film and the deterioration of haze caused by the roughness.

[0036] Here, the silicon nitride film is preferably formed at a temperature in the range of 500° C. to 580° C. If the temperature is within this range, a silicon nitride film can be formed in which the deterioration of haze is further suppressed.

[0037] <Step S2: Detection process> Step S2 is a step of detecting the size of the enlarged protrusion formed on the surface of the silicon nitride film above the protrusion defect by a surface inspection device after the silicon nitride film forming step of step S1.

[0038] The particle counter used as the surface inspection device is not particularly limited as long as it can detect defects (in this case, protrusions) and measure the number and size of defects. For example, a conventional commercially available particle counter such as SP7 manufactured by KLA-Tencor can be used. Using such a particle counter, an LPD (Light Point Defect) map, i.e., the distribution of defects within the wafer surface, is obtained.

[0039] By acquiring such an LPD map, it is possible to measure the number of defects (and their position coordinates (simply referred to as coordinates)) present on the wafer surface. At the same time, by adjusting the detection sensitivity and setting the level of the defect size to be detected, it is possible to measure the number of defects of a given size present on the surface, along with their respective position coordinates. The detection sensitivity can be adjusted on an as-needed basis according to the desired defect size. The detection sensitivity can be set, for example, to the general 19 nm or 10.6 nm, which is the highest sensitivity of SP7. The defect size can be measured from the size of the LPD.

[0040] In addition, as described below, by performing measurements after forming the nitride film and comparing based on the coordinates of each defect on the wafer surface at each measurement, various data regarding the number of defects can be obtained, along with information on the size of each defect, such as the number of defects detected in the measurement before forming the nitride film, the number of defects detected in the measurement after forming the nitride film at the same position as in the measurement before forming the nitride film, the number of defects detected in the measurement before forming the nitride film but not at the same position in the measurement after forming the nitride film, and the number of defects newly detected in the measurement after forming the nitride film.

[0041] In the detection process of step S2, it is preferable to set the measurement sensitivity during detection by the surface inspection device to be higher than 19 nm. With such measurement sensitivity, it is possible to detect the size of small protrusions that cannot be detected with the measurement sensitivity of 19 nm of a general surface inspection device, and it is possible to estimate and measure the size of smaller protrusion-like defects based on the size of the detected protrusions.

[0042] Furthermore, it is preferable that the size of the protrusion defect before the formation of the silicon nitride film is less than 10.6 nm. Since such a protrusion defect less than 10.6 nm is smaller than 10.6 nm, which is the minimum sensitivity of the latest particle counters, the size of the protrusion defect could not be measured by conventional methods, but in the embodiment of the present invention, the size of even a smaller protrusion defect can be estimated and measured.

[0043] <Step S3: Defect size estimation process> Step S3 is a step of estimating the size of the protrusion defect before the formation of the silicon nitride film from the size of the protrusion detected in the detection step of step S2 and the relationship between the preset film thickness of the silicon nitride film and the amount of enlargement of the detected size.

[0044] The preset relationship between the thickness of the silicon nitride film and the amount of increase in the detection size is preferably set based on the amount of change in the detection size before and after the formation of the silicon nitride film, which is detected in advance on another substrate.

[0045] Within an appropriate film thickness range (1 to 4 nm), there is a correlation between the detection size before and after the formation of the silicon nitride film, and the larger the film thickness, the larger the detection size after the formation of the silicon nitride film (i.e., the larger the amount of expansion). Therefore, it is easy to set the relationship between the film thickness and the amount of expansion of the detection size based on the amount of change in the detection size before and after the formation of the silicon nitride film, which is previously obtained on another substrate. Therefore, the size of the protrusion defect before the formation of the silicon nitride film can be easily estimated from the size of the protrusion detected after the formation of the silicon nitride film and the previously set relationship between the film thickness of the silicon nitride film and the amount of expansion of the detection size.

[0046] Next, the size of a small protrusion defect is estimated based on one example of the above-mentioned defect inspection method, and an attempt is made to compare the size with the estimation result obtained by a conventional method.

[0047] First, as a conventional method, Patent Document 1 forms a nitride film several tens of nm thick to enlarge particles. Following this example, Fig. 2 shows an example in which a 50 nm thick nitride film is formed at 750°C. Here, Fig. 2 shows LPD maps before and after the formation of a 50 nm thick silicon nitride film, with Fig. 2(a) showing the results of measuring particles before nitridation with a detection sensitivity of 15 nm, and Fig. 2(b) showing the results of measuring particles after nitridation with a detection sensitivity of 19 nm.

[0048] In this case, the formation of the nitride film caused the particle size to increase, and in the measurement after nitridation with a detection sensitivity of 19 nm, new defects were detected in addition to the defects detected before nitridation with a detection sensitivity of 15 nm. In other words, the formation of the nitride film detected smaller defects.

[0049] On the other hand, when a nitride film is formed, the particle size increases, but at the same time the haze also worsens, and when a 50 nm film is formed, the detection sensitivity for the minimum size after film formation is 19 nm. When the detection sensitivity is 18 nm, particles cannot be measured due to the effect of haze.

[0050] As a result of the above experiment, it was found that the particles that expanded to 19 nm in size by forming a 50 nm nitride film were those with an original size of about 12 nm. In other words, particles smaller than 12 nm before nitridation do not expand in size to 19 nm or more even if a 50 nm nitride film is formed, so they will not be detected after nitridation by a particle counter with a maximum sensitivity of 19 nm.

[0051] The maximum sensitivity of modern particle counters is around 10 nm, so defects smaller than 12 nm can be measured with the latest particle counters without forming a nitride film. However, if a nitride film is formed, the effect of haze means that the defects cannot be measured.

[0052] Figure 3 shows LPD maps before and after the formation of a 50 nm thick silicon nitride film. Figure 3(a) shows the measurement result with a detection sensitivity of 12.5 nm before nitridation, Figure 3(b) shows the measurement result with a detection sensitivity of 10.6 nm before nitridation, and Figure 3(c) shows the measurement result with a detection sensitivity of 19 nm after nitridation.

[0053] Comparing the number of defects before and after the formation of the nitride film, the number of defects with a detection sensitivity of 10.6 nm before the formation of the nitride film is far greater than the number of defects with a detection sensitivity of 19 nm after the formation of a 50 nm nitride film. Also, comparing a detection sensitivity of 12.5 nm before the formation of the nitride film with a detection sensitivity of 19 nm after the formation of the nitride film, the difference is only that the number of defects with a detection sensitivity of 12.5 nm before the formation of the nitride film is slightly smaller, so it is estimated that a detection sensitivity of about 12 nm before the formation of the nitride film is equivalent to a detection sensitivity of 19 nm after the formation of the nitride film.

[0054] In order to increase the detection sensitivity of particles after the nitride film is formed, it is necessary to make the defects larger during the nitride film formation and to suppress the deterioration of haze caused by nitridation. As a result of extensive research into how to achieve this, it was found that the above objective can be achieved by making the nitride film thinner. Specifically, the film thickness needs to be 1nm to 4nm.

[0055] It was found that it is more preferable to lower the temperature at which the nitride film is formed. Specifically, it is more preferable to set the nitride film formation temperature at 500°C to 580°C. EXAMPLES

[0056] The present invention will be described in more detail below by showing examples of the present invention, but the present invention is not limited to these.

[0057] (Example 1, Comparative Example 1) The difference in detection sensitivity of defects due to nitride film formation was compared between a case where a nitride film was formed on a substrate with a diameter of 300 mm at a nitride film thickness of 50 nm and a nitride film formation temperature of 750°C (Comparative Example 1) and a case where a nitride film was formed at a nitride film thickness of 4 nm and a nitride film formation temperature of 630°C (Example 1).

[0058] The particle counter was a KLA-Tencor SP7xp (maximum sensitivity is 10.6 nm). The nitride film was a Si3N4 film formed from SiH2Cl2 and NH3. The measurement sensitivity of the SP7xp before the nitride film formation was 10.6 nm.

[0059] Below is a comparison of defect maps before and after the nitride film formation. Figure 4 is an LPD map comparing the difference between film thickness and measurement sensitivity. The top row is Comparative Example 1, and the bottom row is Example 1, and the horizontal direction shows the results before and after nitridation and the difference in detection sensitivity (also called measurement sensitivity).

[0060] Comparative Example 1 When a 50 nm nitride film was formed, the number of defects was smaller with a detection sensitivity of 19 nm after the nitride film was formed than with a detection sensitivity of 10.6 nm before the nitride film was formed, indicating that the formation of the nitride film reduced the detection sensitivity.

[0061] Furthermore, when measurements were performed after the nitride film was formed with a detection sensitivity of 15 nm, overflow occurred and measurements were not possible due to the deterioration of haze caused by the nitride film formation.

[0062] Example 1 By thinning the film thickness to 4 nm (nitride film formation temperature is 630°C), it became possible to measure up to a measurement sensitivity of 15 nm after nitridation, and at the same time, a new defect flow pattern was visible near the 6 o'clock (downward) position on the substrate surface.

[0063] With a 4 nm nitride film, measurements with a detection sensitivity of 13 nm were not possible due to overflow caused by worsening haze. Even with the formation of a thin nitride film, the haze on the substrate surface worsened, making it impossible to perform high-sensitivity measurements with a detection sensitivity of 10.6 nm, which was possible before the nitride film was formed.

[0064] Regarding the flow pattern of the defect in the 6 o'clock direction (downward) of the paper surface that occurred at a detection sensitivity of 15 nm, this substrate was contaminated from the comb part of the substrate transport box, and it is believed that the contamination caused minute particles with a size of 10.6 nm or less to adhere, and the subsequent formation of a nitride film caused the protrusions to grow in size, making them detectable. In other words, by making the nitride film thin, which is a necessary condition, it was found that the deterioration of haze was suppressed, and even when measuring with a highly sensitive particle counter with a maximum sensitivity of 10.6 nm, the formation of the nitride film made it possible to measure with a higher sensitivity than 10.6 nm (i.e., it was possible to estimate the size of smaller protrusion-like defects).

[0065] Next, we will explain how particle size changes with the formation of the nitride film. In this study, high-sensitivity measurement was achieved by detecting defects after the nitride film was formed, even though they were not detected before. We will show a method for estimating the original particle size before the nitride film was formed from the detected size after the nitride film was formed.

[0066] Below we compare the positions of particles detected before and after the formation of a nitride film. Figure 5 shows the LPD maps before and after the formation of a 4nm-thick silicon nitride film. Figure 5 shows the results of measurements with a measurement sensitivity of 10.6nm before the nitride film was formed, and measurements with a measurement sensitivity of 14nm after a 4nm nitride film was formed at 580℃, and we can see that there are a large number of defects that are now newly detected after the nitride film is formed.

[0067] The triangular points in the figure are defects that were commonly seen before and after the deposition of the nitride film. When we investigated the change in size of these defects before and after the formation of the nitride film, the results are shown in Figure 6. Figure 6 is a graph of the change in defect size before and after the formation of a 4 nm thick silicon nitride film. An average size increase of 5.9 nm was observed. However, not all defects increased by 5.9 nm; some increased by more than 10 nm, and others showed little change, but using this relationship it is possible to estimate the approximate original size.

[0068] The particle size distribution after nitridation in this case is shown in Figure 7. Many of the defects that occurred after the nitride film was formed but not before, indicated by the square symbols on the defect map in Figure 5, are in the 14 nm range, and Figure 7 also shows that most of the defects are 14 nm. Considering that they were not detected before nitridation when measured with a detection sensitivity of 10.6 nm, and that the average size had increased by about 5.9 nm, it can be estimated that the defects, which were approximately 9 to 10.6 nm in size before the nitride film was formed, had increased in size to 14 nm due to the nitride film.

[0069] Comparative Example 2 Next, Figure 8 shows the change in defect size before and after the formation of a 6 nm nitride film at 610°C and a 9.5 nm nitride film at 600°C. Figure 8(a) shows that the formation of a 6 nm nitride film resulted in an average increase in size of 7.4 nm, while Figure 8(b) shows that the formation of a 9.5 nm nitride film resulted in an average increase in size of 14 nm, but there was a large variance in the amount of increase in size for each defect, and it was found that it was difficult to estimate the original size before the nitride film was formed from the size detected after the nitride film was formed. (The measurement sensitivity of the SP7xp after the nitride film was formed in this case was 15 nm.)

[0070] Comparative Example 3 Next, the change in size when a thin nitride film with a thickness of 0.4 nm is formed is shown in Figure 9. When a nitride film with a thickness of 0.4 nm was formed at 500°C (the nitride film was formed in a shorter time than when a 1.2 nm film was formed), no change in size was observed before and after the nitride film was formed. In this case, a measurement sensitivity of 10.6 nm up was possible even after the nitride film was formed, but since the size did not increase, the result was that high sensitivity cannot be expected even if a nitride film was formed.

[0071] Example 2 Therefore, a nitride film with a thickness of 1.2 nm, which is intermediate between Comparative Example 2 and Comparative Example 3, was formed at 500°C. Measurements with a measurement sensitivity of 10.6 nm were possible even after the nitride film was formed, and new defects were detected as shown in the LPD map in Figure 10. As shown in the defect size change graph in Figure 11, it was estimated that the defect was enlarged by 1.5 nm due to the nitride film formation, and the variation in the amount of size increase was small. Therefore, it can be estimated that the original size of the newly generated defects was 9 to 10.6 nm. Figure 12 is a graph showing the particle size distribution after the formation of a silicon nitride film with a thickness of 1.2 nm, and many small size particles are seen.

[0072] The film thicknesses, SP7 measurement sizes before and after the nitride film formation, and size increase amounts for the above examples shown in Examples 1 and 2 and Comparative Examples 2 and 3 are summarized in Table 1, arranged in ascending order of film thickness. Additionally, the size before nitridation was estimated under each condition.

[0073] [Table 1]

[0074] Of these, for a film thickness of 0.4 nm (Comparative Example 3), the variation in the amount of size increase is small, but the size of protrusion defects less than 10.6 nm cannot be estimated. For film thicknesses of 6 nm and 9.5 nm (both Comparative Example 2), the variation in the amount of size increase is large, so even if an attempt is made to estimate the size before nitridation, the accuracy is poor and it is not possible to correctly estimate the size of protrusion defects less than 10.6 nm.

[0075] The film thicknesses of 1.2 nm (Example 2) and 4 nm (Example 1) showed little variation in the amount of size increase, and the size of protrusion defects less than 10.6 nm could be estimated. The estimated sizes before nitridation were 9.1 nm and 8.1 nm, respectively, and it was found that it was possible to estimate the size of protrusion defects smaller than the minimum sensitivity (10.6 nm) of the latest particle counter. Table 1 above summarizes the results of Examples 1 and 2 and Comparative Examples 1 to 3.

[0076] Furthermore, a size increase of 5.9 nm can be achieved by forming a nitride film with a thickness of 4 nm (Example 1), and a size increase of 1.5 nm can be achieved by forming a nitride film with a thickness of 1.2 nm (Example 2). If this is applied to the case where the safety factor is 100% in the formula of film thickness ≧ (inspection device detection sensitivity-defect size) × safety factor in the above-mentioned Patent Document 1, in the case of the inspection device detection sensitivity of Example 1 being 14 nm and the original defect size being 8.1 nm, the nitride film thickness must be > 5.9 nm, which does not include the actual film thickness of 4 nm in Example 1. Similarly, in the case of the inspection device detection sensitivity of Example 2 being 10.6 nm and the original defect size being 9.1 nm, the nitride film thickness must be > 1.5 nm, which does not include the actual film thickness of 1.2 nm in Example 2. In other words, the scope of Patent Document 1 does not include the present Examples 1 and 2.

[0077] In this way, when inspecting protrusion defects, the present invention forms a thinner silicon nitride film (thickness 1 to 4 nm) that differs from the range of Patent Document 1, thereby making it possible to suppress variations due to deterioration of roughness and haze caused by roughness, and to estimate the size of protrusion defects that are smaller than the minimum sensitivity (10.6 nm) of the latest particle counters.

[0078] The present invention includes the following aspects. [1]: a silicon nitride film forming step of forming a silicon nitride film having a thickness of 1 to 4 nm on the substrate in order to increase the detection size of protrusion-like defects present on the surface of the substrate; a detection step of detecting, after the silicon nitride film forming step, a size of a protrusion portion enlarged and formed on a surface of the silicon nitride film above the protrusion defect by a surface inspection device; a defect size estimation step of estimating a size of the protrusion defect before the formation of the silicon nitride film based on a size of the protrusion detected in the detection step and a preset relationship between a film thickness of the silicon nitride film and an amount of enlargement of the detected size; A defect inspection method comprising: [2]: The defect inspection method according to the above-mentioned [1], characterized in that in the silicon nitride film formation step, the formation temperature of the silicon nitride film is 500°C or higher and 580°C or lower. [3]: The defect inspection method according to the above-mentioned [1] or [2], characterized in that the predetermined relationship between the thickness of the silicon nitride film and the amount of increase in the detection size is set based on the amount of change in the detection size before and after the formation of the silicon nitride film detected in advance on another substrate. [4]: A defect inspection method according to any one of [1] to [3] above, characterized in that in the detection step, the measurement sensitivity during detection by the surface inspection device is set to be higher than 19 nm. [5]: The defect inspection method according to any one of [1] to [4] above, characterized in that the size of the protrusion defect before the formation of the silicon nitride film is less than 10.6 nm.

[0079] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and any configuration that is substantially the same as the technical idea described in the claims of the present invention and that provides similar effects is included in the technical scope of the present invention. [Explanation of symbols]

[0080] S1, S2, S3... steps.

Claims

1. a silicon nitride film forming step of forming a silicon nitride film having a thickness of 1 to 4 nm on the substrate in order to increase the detection size of protrusion-like defects present on the surface of the substrate; a detection step of detecting, after the silicon nitride film forming step, a size of a protrusion portion enlarged and formed on a surface of the silicon nitride film above the protrusion defect by a surface inspection device; a defect size estimation step of estimating a size of the protrusion defect before the formation of the silicon nitride film based on a size of the protrusion detected in the detection step and a preset relationship between a film thickness of the silicon nitride film and an amount of enlargement of the detected size; A defect inspection method comprising:

2. 2. The defect inspection method according to claim 1, wherein in said silicon nitride film forming step, the silicon nitride film is formed at a temperature of 500° C. or more and 580° C. or less.

3. 3. The defect inspection method according to claim 1, wherein the predetermined relationship between the thickness of the silicon nitride film and the amount of increase in the detection size is set based on the amount of change in the detection size before and after the formation of the silicon nitride film, which is detected in advance on another substrate.

4. 3. The defect inspection method according to claim 1, wherein in said detection step, a measurement sensitivity during detection by said surface inspection device is set to be higher than 19 nm.

5. 3. The defect inspection method according to claim 1, wherein the size of the protrusion defect before the silicon nitride film is formed is less than 10.6 nm.

Citation Information

Patent Citations

  • Method for measurig fine particle on silicon wafer surface

    JP2001257243A

  • Evaluation method of semiconductor wafer

    JP2006303134A

  • Defect inspection method

    JP2016212009A

  • Specifying method for kind of defect of silicon single-crystal wafer

    JP2023061116A